Epoxy adhesive with impact resistance, stress resistance, and weldability.
A novel epoxy adhesive formulation with rubber particles and polyurethane reinforcing agents ensures strong adhesion and impact resistance on both steel and aluminum substrates, addressing the limitations of existing adhesives in high-temperature/humid conditions and substrate compatibility.
Patent Information
- Application Number
- JP2023553944
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-05
- Filing Date
- 2022-03-04
- Publication Date
- 2026-11-19
- Estimated Expiration
- 2042-03-04
AI Technical Summary
Existing epoxy adhesives fail to provide impact resistance and stress resistance in high-temperature/humid conditions, especially when uncured, and are not suitable for bonding both steel and aluminum substrates efficiently.
A liquid epoxy adhesive formulation comprising epoxy resin, rubber particles, polyurethane reinforcing agents, latent curing agents, and accelerators, along with optional additives, which can be cured to achieve strong adhesion and impact resistance on both steel and aluminum substrates even after exposure to high-temperature/humid conditions.
The adhesive maintains cured adhesive strength and impact resistance on both steel and aluminum substrates, even when uncured, and reduces the need for multiple adhesives, enhancing manufacturing adaptability and durability.
Smart Images

Figure 0007953802000015 
Figure 0007953802000016 
Figure 0007953802000017
Abstract
Description
[Technical Field]
[0001] The present invention relates to a liquid epoxy adhesive that is weldable in an uncured state and provides cured adhesion with impact resistance and stress resistance, an adhesive assembly obtained by curing the liquid epoxy adhesive in contact with one or more substrates, a method for manufacturing these liquid epoxy adhesives, a method for bonding substrates, and a product including the adhesive assembly. [Background technology]
[0002] Epoxy adhesives are used in manufacturing to bond metals to other metals or materials, and may be used in conjunction with spot welding techniques. Automotive original equipment manufacturers (OEMs) require impact-resistant structural adhesive compositions with cured adhesion and adhesion resistance suitable for use in vehicle assembly. Furthermore, automotive OEMs want to expand processing capabilities by improving the moisture resistance of uncured adhesives applied to surfaces, ensuring that the subsequently cured adhesive does not lose its adhesive strength and adhesion resistance performance. Cured structural adhesives must exhibit high strength and toughness after exposure to high-temperature / humid conditions in the uncured state in order to enable shipment of uncured assemblies. Therefore, there is a need for a single-package adhesive composition that exhibits improved uncured moisture resistance, indicated by environmental stress resistance to aluminum, particularly impact resistance at -40°C after low bake curing conditions, and high T peel strength and impact wedge peel strength in the cured state after exposure to high-temperature / humid conditions in the uncured state. New and improved adhesives that meet these requirements are always needed. This disclosure addresses at least some of these needs. [Overview of the Initiative] [Means for solving the problem]
[0003] The applicants have discovered that unexpectedly improved liquid adhesive formulations can be prepared by mixing an epoxy resin, rubber particles (preferably having a core-shell structure and / or an average particle size of less than 500 nm), an end-capped polyurethane reinforcing agent, at least one latent curing agent that can be activated by heating, and at least one accelerator different from the curing agent, as well as at least one additive selected from the group consisting of a carboxyl-terminated butadiene acrylonitrile-epoxy adduct, at least one plasticizer (e.g., sulfonic acid ester plasticizers, phosphate ester plasticizers), and a softener. Optionally, such compositions also contain flame retardants, chelate-modified epoxy resins, auxiliary impact resistance modifiers / reinforcers, fillers, optionally surface-modified thixotropic agents (e.g., fumed silica, mixed mineral phyllosilicates), or other auxiliary agents. When this adhesive is applied to a substrate or carrier and heated to cure, the adhesive yields a product that can form an adhesion with improved T peel strength and impact wedge peel strength in the cured state, even after exposure to high-temperature humid conditions in the uncured state. A particular advantage of some embodiments is that a single formulation exhibits good adhesion to both steel and aluminum substrates. This ability to adhere to both types of metals improves manufacturing adaptability in the vehicle factory and reduces the number of adhesives required at the pump station to just one.
[0004] This disclosure relates to a novel composition of a liquid epoxy adhesive that, upon curing, provides impact-resistant and stress-resistant cured adhesion useful for bonding substrates (e.g., metal substrates); an adhesive assembly obtained by applying an uncured adhesive to one or both of the substrates to be bonded, bringing the substrates into contact so that the adhesive is positioned between the substrates to be joined, and curing the adhesive; and a product comprising a method for producing the liquid epoxy adhesive, a method for bonding substrates, and the adhesive assembly. The epoxy adhesive composition retains its cured adhesive strength even if the uncured liquid epoxy composition is exposed to moisture before curing. In some embodiments, the composition is weldable in the uncured state. Throughout this disclosure, various embodiments of the invention, encompassing the following, are described:
[0005] Embodiment 1 (a) at least one epoxy resin; (b) One or more carboxyl-terminated butadiene homopolymers or butadiene acrylonitrile copolymers (CTBNs); (c) Rubber particles, preferably core-shell rubber particles and / or particles with a size of 500 nm or less; (d) One or more block-type polyurethane reinforcers; (e) preferably at least one thermally activated latent curing agent comprising DICY; (f) At least one accelerator different from the curing agent; A liquid epoxy adhesive composition comprising, A liquid epoxy adhesive composition comprising one or more block-type polyurethane reinforcing agents, each containing at least one asymmetric end-cap polyurethane.
[0006] The epoxy adhesive may further contain other additives such as flame retardants, polyetheramine softeners, fillers, coupling agents, plasticizers, diluents, fillers, pigments and dyes, thixotropic agents, leavening agents, flow control agents, adhesion promoters and antioxidants. In certain aspects of this embodiment, the liquid epoxy adhesive composition does not contain formaldehyde.
[0007] Embodiment 2 The liquid epoxy adhesive composition of Embodiment 1 is further characterized in that the aforementioned components are or contain the following: (a) one or more diglycidyl ethers of bisphenol A (DGEBA) epoxy resin or bisphenol F (DGEBF) epoxy resin, preferably in an amount ranging from 20% to 60% by weight; (b) Preferably, one or more carboxyl-terminated butadiene acrylonitrile copolymers (CTBNs) present in an amount ranging from 1% to 8% by weight; (c) Core-shell rubber (CSR) particles preferably present in a range of 5% to 30% by weight; (d) preferably one or more block-type polyurethane reinforcing agents present in an amount ranging from 5% to 20% by weight; (e) Preferably one or more dicyandiamides (DICY) present in an amount ranging from 2% to 6% by weight; (f) One or more urea accelerators, preferably present in an amount ranging from 0.5% to 2.0% by weight; (g) One or more fillers, preferably in an amount ranging from 0% to 20% by weight; (h) preferably one or more phenol novolac epoxy present in an amount ranging from 0% to 20% by weight; (i) one or more flame retardants preferably present in an amount ranging from 0% to 35% by weight; (j) preferably one or more polyetheramine-based softeners present in an amount ranging from 0% to 12% by weight; and (k) Preferably one or more plasticizers present in the range of 0% to 5% by weight; The weight percentage of each component is relative to the total weight of the composition, and the total amount of components does not exceed 100% by weight.
[0008] Embodiment 3 A liquid epoxy adhesive composition of Embodiment 1 or 2, wherein one or more diglycidyl ethers of bisphenol A (DGEBA) epoxy resin or bisphenol F (DGEBF) epoxy resin are present in amounts of 20% to 25% by weight, 25% to 30% by weight, 30% to 35% by weight, 35% to 40% by weight, 40% to 45% by weight, 45% to 50% by weight, 50% to 55% by weight, 55% to 60% by weight, or any combination of two or more of the aforementioned ranges, for example, 25% to 55% by weight, or any of the aforementioned values, based on the total weight of the composition.
[0009] Embodiment 4 (b) One or more carboxyl-terminated butadiene acrylonitriles (CTBNs) in amounts of 1% to 1.1% by weight, 1.1% to 1.2% by weight, 1.2% to 1.3% by weight, 1.3% to 1.4% by weight, 1.4% to 1.5% by weight, 1.5% to 1.6% by weight, 1.6% to 1.7% by weight, 1.7% to 1.8% by weight, 1.8% to 1.9% by weight, 1.9% to 2% by weight, 2% to 2.5% by weight, and 2.5% to 3% by weight, relative to the total weight of the composition. A liquid epoxy adhesive composition according to any one of Embodiments 1 to 3, existing in the range of %, 3% to 3.5% by weight, 3.5% to 4% by weight, 4% to 4.5% by weight, 4.5% to 5% by weight, 5% to 5.5% by weight, 5.5% to 6% by weight, 6% to 6.5% by weight, 6.5% to 7% by weight, 7% to 7.5% by weight, 7.5% to 8% by weight, or any combination of two or more of the aforementioned ranges, for example, 1.3% to 1.6% by weight, or any of the aforementioned values.
[0010] Embodiment 5 (c) Core-shell rubber (CSR) particles are present in amounts of 5% to 6% by weight, 6% to 7% by weight, 7% to 8% by weight, 8% to 9% by weight, 9% to 10% by weight, 10% to 11% by weight, 11% to 12% by weight, 12% to 13% by weight, 13% to 14% by weight, 14% to 15% by weight, 15% to 16% by weight, 16% to 17% by weight, 17% to 18% by weight, 18% to 19% by weight, 19% to 20% by weight, and 2% by weight. A liquid epoxy adhesive composition according to any one of Embodiments 1 to 4, existing in the range of 0% to 21% by weight, 21% to 22% by weight, 22% to 23% by weight, 23% to 24% by weight, 24% to 25% by weight, 25% to 26% by weight, 26% to 27% by weight, 27% to 28% by weight, 28% to 29% by weight, 29% to 30% by weight, or any combination of two or more of the aforementioned ranges, for example, 10% to 15% by weight, or any of the aforementioned values.
[0011] Embodiment 6 (d) A liquid epoxy adhesive composition of any one of Embodiments 1 to 5, wherein one or more block-type polyurethane reinforcing agents are present in an amount of 5% to 6% by weight, 6% to 7% by weight, 7% to 8% by weight, 8% to 9% by weight, 9% to 10% by weight, 10% to 11% by weight, 11% to 12% by weight, 12% to 13% by weight, 13% to 14% by weight, 14% to 15% by weight, 15% to 16% by weight, 16% to 17% by weight, 17% to 18% by weight, 18% to 19% by weight, 19% to 20% by weight, or any combination of two or more of the above ranges, for example, 5% to 7% by weight, or any of the above values.
[0012] Embodiment 7 (e) A liquid epoxy adhesive composition of any one of Embodiments 1 to 6, wherein at least one heat-activated latent curing agent comprises DICY, and one or more dicyandiamides (DICY) are present in amounts of 2% to 2.5% by weight, 2.5% to 3% by weight, 3% to 3.5% by weight, 3.5% to 4% by weight, 4% to 4.5% by weight, 4.5% to 5% by weight, 5% to 5.5% by weight, or any combination of two or more of the aforementioned ranges, for example, 3% to 4% by weight, or any of the aforementioned values, based on the total weight of the composition.
[0013] Embodiment 8 (f) at least one accelerator different from the curing agent; for example, one or more urea-based accelerators, such as substituted urea accelerators, present in an amount of 0.5 wt% to 0.6 wt%, 0.6 wt% to 0.7 wt%, 0.7 wt% to 0.8 wt%, 0.8 wt% to 0.9 wt%, 0.9 wt% to 1.0 wt%, 1.0 wt% to 1.1 wt%, 1.1 wt% to 1.2 wt%, 1.2 wt% to 1.3 wt%, 1.3 wt% to 1.4 wt%, 1.4 wt% to 1.5 wt%, 1.5 wt% to 1.6 wt%, 1.6 wt% to 1.7 wt%, 1.7 wt% to 1.8 wt%, 1.8 wt% to 1.9 wt%, 1.9 wt% to 2.0 wt%, 2.0 wt% to 2.1 wt%, 2.1 wt% to 2.2 wt%, 2.2 wt% to 2.4 wt%, 2.4 wt% to 2.5 wt%, or any combination of two or more of the aforementioned ranges, such as 0.5 wt% to 1 wt%, or in any range of the aforementioned values, relative to the total weight of the composition, the liquid epoxy adhesive composition according to any one of Embodiments 1 to 7.
[0014] Embodiment 9 (g) one or more fillers present in an amount of 1 wt% to 2 wt%, 2 wt% to 3 wt%, 3 wt% to 4 wt%, 4 wt% to 5 wt%, 5 wt% to 6 wt%, 6 wt% to 7 wt%, 7 wt% to 8 wt%, 8 wt% to 9 wt%, 9 wt% to 10 wt%, 10 wt% to 11 wt%, 11 wt% to 12 wt%, 12 wt% to 13 wt%, 13 wt% to 14 wt%, 14 wt% to 15 wt%, 15 wt% to 16 wt%, 16 wt% to 17 wt%, 17 wt% to 18 wt%, 18 wt% to 19 wt%, 19 wt% to 20 wt%, or any combination of two or more of the aforementioned ranges, such as 5 wt% to 17 wt%, or in any range of the aforementioned values, relative to the total weight of the composition, the liquid epoxy adhesive composition according to any one of Embodiments 1 to 8. The filler may be one or more organic fillers, one or more inorganic fillers, or a combination of one or more organic fillers and one or more inorganic fillers.
[0015] Embodiment 10 (h) The liquid epoxy adhesive composition according to any one of Embodiments 1 to 9, wherein the one or more phenol novolac epoxies are present in an amount of 1 wt% to 1.5 wt%, 1.5 wt% to 2 wt%, 2 wt% to 2.5 wt%, 2.5 wt% to 3 wt%, 3 wt% to 3.5 wt%, 3.5 wt% to 4 wt%, 4 wt% to 4.5 wt%, 4.5 wt% to 5 wt%, 5 wt% to 5.5 wt%, 5.5 wt% to 6 wt%, 6 wt% to 6.5 wt%, 6.5 wt% to 7 wt%, 7 wt% to 7.5 wt%, 7.5 wt% to 8 wt%, 8 wt% to 8.5 wt%, 8.5 wt% to 9 wt%, 9 wt% to 9.5 wt%, 9.5 wt% to 10 wt%, 10 wt% to 12 wt%, 12 wt% to 14 wt%, 14 wt% to 16 wt%, 16 wt% to 20 wt%, or any combination of two or more of the aforementioned ranges, for example 4.5 wt% to 6.5 wt%, or 4.5 wt% to 9 wt%, or in any range of the aforementioned values, relative to the total weight of the composition.
[0016] Embodiment 11 (i) The liquid epoxy adhesive composition according to any one of Embodiments 1 to 10, wherein the one or more flame retardants are present in an amount of 0 wt% to 1 wt%, 1 wt% to 2 wt%, 2 wt% to 3 wt%, 3 wt% to 4 wt%, 4 wt% to 5 wt%, 5 wt% to 6 wt%, 6 wt% to 7 wt%, 7 wt% to 8 wt%, 8 wt% to 9 wt%, 9 wt% to 10 wt%, 10 wt% to 11 wt%, 11 wt% to 12 wt%, 12 wt% to 13 wt%, 13 wt% to 14 wt%, 14 wt% to 15 wt%, 15 wt% to 16 wt%, 16 wt% to 17 wt%, 17 wt% to 18 wt%, 18 wt% to 19 wt%, 19 wt% to 20 wt%, 20 wt% to 22 wt%, 22 wt% to 24 wt%, 24 wt% to 26 wt%, 26 wt% to 28 wt%, 28 wt% to 30 wt%, 30 wt% to 35 wt%, or any combination of two or more of the aforementioned ranges, for example 2 wt% to 16 wt%, or in any range of the aforementioned values, relative to the total weight of the composition.
[0017] Embodiment 12 (j) One or more polyetheramine-based softeners in amounts of 0% to 1% by weight, 1% to 1.5% by weight, 1.5% to 2% by weight, 2% to 2.5% by weight, 2.5% to 3% by weight, 3% to 3.5% by weight, 3.5% to 4% by weight, 4% to 4.5% by weight, 4.5% to 5% by weight, 5% to 5.5% by weight, 5.5% to 6% by weight, 6% to 6.5% by weight, 6.5% to 7% by weight, 7% to 7.5% by weight, A liquid epoxy adhesive composition according to any one of Embodiments 1 to 11, existing in the range of 7.5% to 8% by weight, 8% to 8.5% by weight, 8.5% to 9% by weight, 9% to 9.5% by weight, 9.5% to 10% by weight, 10% to 10.5% by weight, 10.5% to 11% by weight, 11% to 11.5% by weight, 11.5% to 12% by weight, or any combination of two or more of the aforementioned ranges, for example, 1.5% to 10% by weight, or any of the aforementioned values.
[0018] Embodiment 13 (k) One liquid epoxy adhesive composition according to any one of Embodiments 1 to 12, wherein one or more plasticizers are present in the range of 0% to 1% by weight, 1% to 1.5% by weight, 1.5% to 2% by weight, 2% to 2.5% by weight, 2.5% to 3% by weight, 3% to 3.5% by weight, 3.5% to 4% by weight, 4% to 4.5% by weight, 4.5% to 5% by weight, or any combination of two or more of the above ranges, for example, 0% to 2% by weight, or any of the above values.
[0019] Embodiment 14 A liquid epoxy adhesive composition according to any one of Embodiments 1 to 13, wherein one or more diglycidyl ethers of bisphenol A (DGEBA) epoxy resin or bisphenol F (DGEBF) epoxy resin comprise one or more diglycidyl ethers of bisphenol A (DGEBA) epoxy resin. In other embodiments of this embodiment, one or more diglycidyl ethers comprise one or more diglycidyl ethers of bisphenol F (DGEBF) epoxy resin. In some embodiments of this embodiment, the diglycidyl ether comprises at least one liquid (at 23°C) diglycidyl ether of bisphenol A, bisphenol F, or both bisphenol A and bisphenol F. Such epoxy resins may further comprise at least one solid (at 23°C) diglycidyl ether of bisphenol A and / or bisphenol F. Such epoxy resin mixtures may contain up to 5% monohydrolyzed species present as impurities in one or more of the constituent resins.
[0020] Embodiment 15 A liquid epoxy adhesive composition according to any one of Embodiments 1 to 14, wherein one or more diglycidyl ethers of bisphenol A (DGEBA) epoxy resin have an epoxy equivalent weight (EEW) in the range of 180 to 195, preferably 185 to 192, where EEW = molecular weight of epoxy resin / number of epoxy groups.
[0021] Embodiment 16 A liquid epoxy adhesive composition according to any one of Embodiments 1 to 15, wherein one or more phenol novolac epoxys have an EEW in the range of 165 to 185, preferably 172 to 179.
[0022] Embodiment 17 A liquid epoxy adhesive composition according to any one of Embodiments 1 to 16, comprising one or more carboxyl-terminated butadiene acrylonitrile (CTBN) copolymers of butadiene and nitrile monomers, preferably comprising or consisting of acrylonitrile. The specific properties of butadiene acrylonitrile are described elsewhere and incorporated herein as separate embodiments of this embodiment, but in a preferred embodiment, the CTBN composition has acrylonitrile in the range of about 22 to 30% by weight, more preferably 26%.
[0023] Embodiment 18 A liquid epoxy adhesive composition according to any one of Embodiments 1 to 17, wherein DGEBF is added to one or more carboxyl-terminated butadiene acrylonitrile (CTBN) groups.
[0024] Embodiment 19 Core-shell rubber (CSR) particles: (a) Dispersed in a unimodal or bimodal manner; (b) Having an average particle size within the range enclosed by 50 nm, 75 nm, 100 nm, 125 nm, 150 nm, 175 nm, 200 nm, 250 nm, or 500 nm, or any two of the aforementioned values; (c) having a core consisting of or comprising polybutadiene, butadiene / styrene copolymer, or acrylic polymer or copolymer; and / or (d) Dispersed in DGEBA epoxy resin, A liquid epoxy adhesive composition according to any one of Embodiments 1 to 18.
[0025] Each of these various descriptions of CSR particles (characteristics, composition, and size) is described elsewhere in this disclosure, so as to be considered an independent aspect of this embodiment.
[0026] Embodiment 20 A liquid epoxy adhesive composition according to any one of Embodiments 1 to 19, wherein one or more blocked polyurethane reinforcing agents comprise a polyalkylene glycol segment. In a preferred embodiment of this embodiment, the polyalkylene glycol segment independently comprises polyethylene glycol, polypropylene glycol, or polybutylene glycol (or polytetramethylene glycol (poly-THF or PTMEG)) having equivalent molecular weights in the range of 2000 to 5000 Daltons. PTMEG bonding is preferred. In another, even more preferred embodiment of this embodiment, the polyurethane reinforcing agent also comprises a polyalkylene (extensioner) segment, preferably the polyalkylene glycol segment having end caps. 1~10 Alkylene bond, preferably C 6~8 It is adjacent to the alkylene bond and bonded to it by a urethane group.
[0027] In a more preferred embodiment of this design, one or more block-type polyurethane reinforcing agents are end-capped at both ends of the structure, with at least one adjacent C1-10 alkylene bond being end-capped. The two end-caps of the reinforcing agent may be the same or different. By selecting a combination of different end-caps, the block dissociation temperature can be adjusted. In some aspects of this design, the block dissociation temperature of the reinforcing agent is then selected to be in the range defined by 135°C-140°C, 140°C-145°C, 145°C-150°C, 150°C-160°C, 160°C-165°C, or any two or more of the aforementioned ranges, for example, in the range of 140°C-150°C.
[0028] In some aspects of this embodiment, at least one end cap is a bisphenol (e.g., bisphenol A) group. Huntsman's DY965 is one commercially available sample of such a reinforcing agent, in which the end cap contains bisphenol.
[0029] In some cases, the end capping may be the same at both ends of the molecule, and end capping by one or more bisphenol (e.g., bisphenol A) groups may be permitted, but blocking groups that provide a lower block dissociation temperature are also permitted and, in some cases, have been observed to be preferable. In some aspects of this embodiment, such end capping agents include optionally substituted phenols (or hydroxyheteroaryl analogs), amines, methacrylates, acetoxys, oximes, and / or pyrazoles.
[0030] In some aspects of this embodiment, end capping may be asymmetric, meaning that the ends of the polyurethane molecule may be blocked with different functional groups, such as optionally substituted phenols, amines, methacrylates, acetoxys, oximes, and / or pyrazoles. An example of substitution on phenol is C containing 1, 2, 3, or 4 conjugated and / or unconjugated alkenylene bonds. 12~24 The pendant functional group may be included.
[0031] For example, in an independent aspect of this embodiment, adjacent C 1-10 At least one alkylene bond is at least one C 12-24 The end caps are monophenols containing pendant functional groups, and at least one C 12-24 The pendant functional group contains one, two, three, or four conjugated and / or unconjugated alkenylene bonds. Again, the use of substituted monophenols is preferred in that it appears to provide a lower curing temperature than bisphenol end caps.
[0032] Another independent aspect of this embodiment is an enhancement agent in which at least one end cap contains methyl ethyl ketoxime, 2,4-dimethyl-3-pentanone oxime or 2,6-dimethyl-4-heptanone oxime, diethyl malonate, 3,5-dimethylpyrazole, 1,2,4-triazole, or a mixture of diisopropylamine and 1,2,4-triazole, or a combination thereof.
[0033] Embodiment 21 A liquid epoxy adhesive composition according to any one of Embodiments 1 to 20, comprising at least one heat-activated latent curing agent DICY; and one or more dicyandiamides (DICY) which are finely powdered dicyandiamide (cyanoguanidine). In certain aspects of this embodiment, the finely powdered dicyandiamide is not completely soluble in the liquid epoxy adhesive composition. In certain aspects of this embodiment, at least 98% of the finely powdered dicyandiamide has a particle size of 40 microns or less. In other aspects, at least 98% of the finely powdered dicyandiamide has a particle size of 10 microns or less. In other aspects, at least 98% of the finely powdered dicyandiamide has a particle size of 6 microns or less.
[0034] Embodiment 22 A liquid epoxy adhesive composition according to any one of Embodiments 1 to 21, comprising one or more flame retardants. In certain aspects of this embodiment, the flame retardant is one or more of any combination of aluminum trihydrate (ATH), ammonium polyphosphate, melamine, melamine polyphosphate, phosphonic acid esters (e.g., diethyl bis(hydroxyethyl)aminomethylphosphonate, halogen-free phosphonic acid esters, or unsubstituted mono, di, or tributylated phenyl phosphates), or comprising these. In certain aspects of this embodiment, the flame retardant is liquid, the composition does not contain a solid flame retardant, and optionally ATH may be present as a filler.
[0035] Embodiment 23 A liquid epoxy adhesive composition according to any one of Embodiments 1 to 22, wherein one or more fillers include one or more naturally occurring clays such as calcium carbonate, calcium oxide, calcium silicate, aluminosilicate, organic affinity phyllosilicate, bentonite, wollastonite or kaolin glass, silica, mica, talc, microspheres (polymer or glass beads) or hollow glass microspheres, shredded or pulverized fibers (e.g., carbon, glass, or aramid), pigments, zeolites (natural or synthetic), or thermoplastic fillers.
[0036] Embodiment 24 A liquid epoxy adhesive composition of any one of Embodiments 1 to 23, wherein at least one accelerator, distinct from the curing agent, comprises one or more accelerators including urea, guanidine other than cyanoguanidine, or a substituted urea accelerator; preferably a substituted urea accelerator, more preferably a micronized substituted urea accelerator. In certain aspects of this embodiment, the substituted urea accelerator is a substituted urea and / or crosslinked diurea (each urea is substituted with 1, 2, 3, or 4 alkyl groups and / or aromatic groups). In some aspects of this embodiment, one or more accelerators preferably include a substituted urea, optionally alkyl-substituted ureas including dimethylurea, e.g., 1,1-dimethylurea and / or 1,3-dimethylurea, as described elsewhere herein and incorporated herein. In some aspects of this embodiment, the accelerator is activated in a temperature range that is 100°C to 120°C, 120°C to 140°C, 140°C to 160°C, or 160°C to 180°C, or a combination of two or more of these ranges. In certain aspects of this embodiment, the substituted urea accelerator is activated at a temperature above the block dissociation temperature of polyurethane, preferably at a temperature of at least about 160°C, suitable for low-temperature curing in an E-coat oven. In some aspects of this embodiment, the liquid epoxy adhesive composition comprises at least two accelerators.
[0037] Embodiment 25 A liquid epoxy adhesive composition according to any one of Embodiments 1 to 24, wherein one or more polyetheramine-based softeners are polyalkylene glycols containing amine endcaps, and one or more polyetheramine-based softeners are present as DGEBA adducts. The polyetheramine is preferably an end-capped polypropylene glycol characterized by repeating oxypropylene units in the backbone. The polypropylene glycol has a weight-average molecular weight in the range of about 1000 to 3000 daltons, preferably 1500 to 2500 daltons, and more preferably about 2000 daltons. Such materials are commercially available as Jeff Famin® D-2000 polyetheramine.
[0038] Embodiment 26 A liquid epoxy adhesive composition according to any one of Embodiments 1 to 25, comprising one or more plasticizers, which are tricresil phosphate or contain tricresil phosphate. In certain aspects of this embodiment, the plasticizer is selected from the group consisting of triphenyl phosphate, tricresil phosphate, and phenylcresil esters of pentadecylsulfonic acid.
[0039] Embodiment 27 A method for manufacturing a composite article, comprising the steps of bringing one of the liquid epoxy adhesive compositions of Embodiments 1 to 26 into contact with a surface, and temporarily adhering an uncured epoxy to that surface. In a particular aspect of this embodiment, at least two surfaces are in contact with the composition, and the surfaces are arranged such that the uncured epoxy is located between them.
[0040] Embodiment 28 A cured epoxy adhesive layer prepared by thermally curing one of the liquid epoxy adhesive compositions of Embodiments 1 to 27 on a substrate. In a particular aspect of this embodiment, the cured epoxy adhesive layer has a nominal thickness in the range of 0.25 to 0.5 mm, preferably about 0.25 mm.
[0041] Embodiment 29 (a) a cured epoxy adhesive layer of Embodiment 28, cured at a temperature of 160°C for 10 minutes; or (b) a cured epoxy adhesive layer of 205°C for 30 minutes. The time refers to the total time the adhesive is at the specified curing temperature. The epoxy adhesive layer may be cured at other temperatures determined by the curing of the paint over the parameters, e.g., in the ranges of 150-210, 160-205, 165-200, and other temperatures within the range described. The curing time of 10-30 minutes encompasses other curing times within the range described. Other combinations of temperature and time may be used as known in the art. The adhesive may be cured at higher temperatures and longer curing times, provided that the curing conditions do not interfere with other purposes of the invention with respect to the performance of the cured adhesive.
[0042] Embodiment 30 A cured epoxy adhesive layer of Embodiment 28 or 29, wherein the substrate is cold-rolled steel (CRS), electro-galvanized steel (EZG), hot-dip galvanized steel (HDG), or treated aluminum. In certain aspects of this embodiment, the substrate (also called the adherend) has a thickness in the range of 0.7 mm to 2.0 mm.
[0043] Embodiment 31 Any one of the cured epoxy adhesive layers from Embodiments 28 to 30 exhibits a 100% cohesive failure mode in delamination of cold-rolled steel (CRS), electro-galvanized steel (EZG), hot-dip galvanized steel (HDG), and / or treated aluminum when tested under the T delamination conditions of ASTM D1876-08(2015)e1 or according to the wedge impact method of ISO 11343.2019.
[0044] Embodiment 32 (a) Between two 0.8 mm thick cold-rolled steel sheets, sufficient adhesive force is provided between the sheets to exhibit a peel strength of at least 10, 11, 12, 13, 14, or 15 N / mm at room temperature after curing at 160°C for 10 minutes; and / or (b) Between two 0.8 mm thick cold-rolled steel sheets, curing at 205°C for 30 minutes provides sufficient adhesion between the sheets to exhibit a T peel strength of at least 10, 11, 12, 13, 14, or 15 N / mm at room temperature; and / or (c) When hardened between two 0.8 mm thick cold-rolled steel sheets at 160°C for 10 minutes, it exhibits cutting resistance [impact wedge peel strength] under impact loads of at least 20, 22, 24, 26, 28, 30, or 32 N / mm when tested at -40°C using the wedge impact method of ISO 11343.2019; and / or (d) When two 0.8 mm thick cold-rolled steel sheets are cured at 205°C for 30 minutes, they exhibit cutting resistance under impact loads of at least 20, 22, 24, 26, 28, 30, or 32 N / mm when tested at -40°C using the wedge impact method of ISO 11343.2019; and / or (e) Between two 2.0 mm thick 5754 aluminum plates, sufficient adhesive force is provided between the plates to exhibit a peel strength of at least 10, 11, 12, 13, 14, or 15 N / mm at room temperature after curing at 160°C for 10 minutes; and / or (f) Between two 2.0 mm thick 5754 aluminum plates, when cured at 205°C for 30 minutes, sufficient adhesive strength is provided between the plates to exhibit a peel strength of at least 10, 11, 12, 13, 14, or 15 N / mm at room temperature and / or (g) When cured between two 2.0 mm thick cold-rolled steel sheets at 160°C for 30 minutes, it exhibits cutting resistance under impact loads of at least 24, 26, 28, 30, 32, 34, 36, or 38 N / mm when tested at -40°C using the wedge impact method of ISO 11343.2019; any one of the cured epoxy adhesive layers of embodiments 28 to 31. Specific aspects of this embodiment are provided in the examples and incorporated herein.
[0045] Embodiment 33 A cured epoxy adhesive layer of any one of embodiments 28 to 32 having sufficient resistance to withstand a standardized stress resistance test. In some aspects of this embodiment, the stress resistance test includes subjecting the cured epoxy adhesive layer to at least 22 cycles carried out according to FLTM BV101-07 (as described elsewhere herein) or an equivalent. In other aspects of this embodiment, a cured epoxy adhesive layer cured at 160°C for 10 minutes can withstand at least 25, 30, 35, 40, or 45 cycles of environmental aging according to FLTM BV101-07, which is incorporated herein by reference for teaching the criteria and method of this test.
[0046] Embodiment 34 An uncured epoxy adhesive layer of Embodiment 27, comprising a flame retardant that is sufficiently flame-retardant to meet the following conditions: (a) FLTM BV114-01 for steel substrates; and / or (b) FLTM BV062-01 for aluminum substrates.
[0047] Embodiment 35 A product comprising a liquid epoxy adhesive composition of any one of Embodiments 1 to 26 applied, or a cured epoxy adhesive layer of any one of Embodiments 28 to 33. In certain aspects of this embodiment, the product is an automobile, a home appliance, or a part thereof.
[0048] Embodiment 36 A method for preparing one of the liquid epoxy adhesive compositions of Embodiments 1 to 26, comprising the steps of: 1) mixing liquid components; 2) mixing solid components, excluding the curing agent and accelerator, with the mixture at a temperature below the activation energy of the final desired composition; and 3) incorporating the curing agent and accelerator into the mixture.
[0049] Embodiment 37 A method for manufacturing an adhesive assembly, comprising the steps of: applying one of the compositions of Embodiments 1 to 26 to a first surface; bringing at least one second surface into contact with the composition on the first surface; and curing the composition by bringing the first surface and the second surface into contact to produce an adhesive assembly. In certain aspects of this embodiment, one or more of the first and second surfaces are contaminated with at least one oily substance, and the composition further comprises at least one chelate-modified epoxy resin. In other aspects of this embodiment, the adhesive assembly is prepared by thermocuring a liquid epoxy adhesive composition in a temperature range of 140°C to 220°C, and upon curing, exhibits a 100% cohesive failure mode of the adhesive assembly in peeling of cold-rolled steel (CRS), electro-galvanized steel (EZG), hot-dip galvanized steel (HDG), and / or treated aluminum when tested under the T peeling conditions of ASTM D1876-08(2015)e1 or according to the wedge impact method of ISO11343.2019.
[0050] Embodiment 38 A product comprising any one of the liquid epoxy adhesive compositions of Embodiments 1 to 26, applied to at least one surface of the product and either uncured or cured on at least one surface of the product. The product is preferably an automobile or a part thereof.
[0051] The disclosure also includes the use of these liquid epoxy adhesive compositions in forming an adhesive surface including a corresponding cured epoxy adhesive layer, methods for using them for this purpose, and cured epoxy adhesive layers prepared by thermally curing the liquid epoxy adhesive composition between substrates.
[0052] The recommended thickness of the cured adhesive layer is provided along with the conditions for curing the adhesive composition. Exemplary curing conditions include curing at 160°C for 10 minutes or at 200°C for 30 minutes. Typical substrates include, but are not limited to, cold-rolled steel (CRS), electro-galvanized steel (EZG), hot-dip galvanized steel (HDG), or treated aluminum.
[0053] Upon curing, the adhesive provides excellent adhesion between such surfaces. In some embodiments, the cured adhesive layer exhibits a 100% cohesive failure mode in peeling cold-rolled steel (CRS), electro-galvanized steel (EZG), hot-dip galvanized steel (HDG), and / or treated aluminum when tested under the T peeling conditions of ASTM D1876. The T peeling strength is at least 10, 11, 12, 13, 14, or 15 N / mm. When tested using the wedge impact method of ISO 11343.2019 at -40°C, it exhibits cutting resistance under impact loads of at least 20, 22, 24, 26, 28, 30, or 32 N / mm.
[0054] This disclosure also includes products comprising one or more of the cured epoxy adhesive layers described herein.
[0055] Some of the many advantages of the currently disclosed composition include the following: (1) Excellent adhesion properties and impact wedge peel strength on steel and aluminum substrates, especially at -40°C, while maintaining excellent uncured open bead moisture resistance (conventional reinforced epoxy polymers tend to exhibit brittle fracture under high strain rate impact events); (2) The use of polyurethane reinforcing agents improves adhesion to steel and aluminum and moisture resistance compared to currently available materials; (3) The long-term resistance of aluminum treated under harsh high-temperature / humid aging conditions is improved; (4) The adhesion strength, impact wedge peel strength, and failure mode to the treated aluminum are improved; and / or (5) The flame resistance of the uncured weld is enhanced, and at the same time, it is easier to pass aluminum welding tests, and it exhibits good impact wedge peel strength at temperatures above -40°C after curing under the "low bake" curing conditions used in the automotive E-coat process. [Brief explanation of the drawing]
[0056] [Figure 1] Figures 1A and 1B show the differential scanning calorimetry (DSC) results for Comparative Example 1 and Example 2. Figure 1A shows the heat flow rate as a function of temperature. Figure 1B shows the thermogram corresponding to the "low bake" curing condition. [Figure 2] Figure 2 shows the isothermal thermogravimetric analysis (TGA) curves for phosphorus flame retardants Phos.1, Phos.2, and Phos.3. [Modes for carrying out the invention]
[0057] This disclosure can be more readily understood by referring to the following description in conjunction with the attached abstract, drawings, and examples, all of which form part of this disclosure. These components, identified by their trade names, are independent embodiments of the referenced materials. Similarly, unless otherwise noted, any description of possible mechanisms or modes of action, or reasons for improvement, is for illustrative purposes only, and the disclosure herein is not bound by the correctness of such suggested mechanisms or modes of action, or reasons for improvement. Throughout this text, it is recognized that the description refers to compositions and methods of manufacturing and using those compositions. That is, whereever this disclosure describes or claims features or embodiments relating to a composition or a method of manufacturing or using a composition, it is understood that such description or claim is intended to extend those features or embodiments to embodiments in their respective contexts (i.e., compositions, manufacturing methods, and methods of use).
[0058] Liquid epoxy adhesive composition The specific embodiments described herein include liquid epoxy adhesive compositions comprising: (a) at least one epoxy resin; (b) One or more carboxyl-terminated butadiene acrylonitriles (CTBNs); (c) Rubber particles, preferably core-shell rubber (CSR) particles, most preferably nanoscale core-shell rubber particles, meaning that at least one dimension of the particles is less than 100 nm. The particle size distribution may vary in the specific embodiments described herein; (d) One or more block-type polyurethane reinforcers; (e) At least one thermally activated latent curing agent comprising DICY; (f) At least one accelerator different from the curing agent; Here, one or more block-type polyurethane reinforcers include at least one asymmetrically end-capped polyurethane.
[0059] In a particular embodiment, a liquid epoxy adhesive composition: (a) one or more diglycidyl ethers of bisphenol A (DGEBA) epoxy resin or bisphenol F (DGEBF) epoxy resin, preferably in an amount ranging from 20% to 60% by weight; (b) Preferably, one or more carboxyl-terminated butadiene homopolymers or butadiene acrylonitrile copolymers (CTBNs) present in an amount ranging from 1% to 8% by weight; (c) Core-shell rubber (CSR) particles preferably present in a range of 5% to 30% by weight; (d) preferably one or more block-type polyurethane reinforcing agents present in an amount ranging from 5% to 20% by weight; (e) Preferably one or more dicyandiamides (DICY) present in an amount ranging from 2% to 6% by weight; (f) One or more urea accelerators, preferably present in an amount ranging from 0.5% to 2.0% by weight; (g) One or more fillers, preferably in an amount ranging from 0% to 20% by weight; (h) preferably one or more phenol novolac epoxy present in an amount ranging from 0% to 20% by weight; (i) one or more flame retardants preferably present in an amount ranging from 0% to 35% by weight; (j) preferably one or more polyetheramine-based softeners present in an amount ranging from 0% to 12% by weight; and (k) preferably one or more plasticizers present in the range of 0% to 5% by weight; The weight percentage of each component is relative to the total weight of the composition, and the total amount of components does not exceed 100% by weight.
[0060] Each of these ranges is considered independently, and exemplary independent and partial ranges for each of these components are described elsewhere in this specification.
[0061] epoxy resin In general, a number of polyepoxides having at least about two 12-epoxy groups per molecule are suitable as epoxy resins for the compositions of the present invention. The polyepoxides may be saturated, unsaturated, cyclic or acyclic, aliphatic, alicyclic, aromatic or heterocyclic polyepoxide compounds. Examples of suitable polyepoxides include polyglycidyl ethers prepared by reacting epichlorohydrin or epibromohydrin with a polyphenol in the presence of an alkali. Suitable polyphenols include, for example, resorcinol, pyrocatechol, hydroquinone, bisphenol A (bis(4-hydroxyphenyl)-2,2-propane), bisphenol F (bis(4-hydroxyphenyl)methane), bis(4-hydroxyphenyl)-1,1-isobutane, 4,4'-dihydroxybenzophenone, and bis(4-hydroxyphenyl)-1,1-ethane. Other suitable polyphenols as a base for polyglycidyl ethers are known condensation products of phenol with novolac resin-type formaldehyde or acetaldehyde. Particularly preferred are liquid epoxy resins derived from the reaction of bisphenol A or bisphenol F with epichlorohydrin. Epoxy resins that are liquid at room temperature generally have an epoxy equivalent of 150 to about 480. In preferred embodiments of the liquid epoxy adhesive composition, one or more diglycidyl ethers of bisphenol A (DGEBA) epoxy resin or bisphenol F (DGEBF) epoxy resin may be present individually or together. In certain embodiments, one or both of these resins have an epoxy equivalent (EEW) in the range of 155 to 400, 160 to 300, 165 to 200, 170 to 250, or 180 to 200, preferably 185 to 195, where EEW = molecular weight of the epoxy resin / number of epoxy groups. Suitable commercially available polyphenol polyglycidyl ether products include diglycidyl ethers of bisphenol A resin (including 300 and 600 series resins), such as those sold by Orin under the trade name DER®.Other aliphatic epoxy diluents / flexiblers in the DER® 700 series may also be incorporated to reduce viscosity (i.e., as diluents), increase flexibility / elongation, and improve adhesion.
[0062] Carboxylate-terminated butadiene acrylonitrile (CTBN) In addition, or instead, in the adhesive composition, one or more carboxyl-terminated butadiene acrylonitriles (CTBNs) may comprise a copolymer of butadiene and a nitrile monomer, preferably acrylonitrile, or a homopolymer of butadiene. A higher acrylonitrile content is preferred, in the range of 22-30% by weight based on the weight of the CTBN, and in some preferred embodiments, the CTBN composition contains about 26% by weight of acrylonitrile. The increased solubility is thought to delay the onset of phase separation (kinetics) during curing, resulting in smaller particle size and increased fracture toughness.
[0063] These carboxyl-terminated butadiene acrylonitriles (CTBNs) may contain, on average, about 1.5, more preferably about 1.8, up to about 2.5, and more preferably about 2.2 terminal epoxide-reactive carboxyl groups per molecule. The molecular weight (Mn) of the butadiene acrylonitrile copolymer is preferably about 2000 to about 6000, more preferably about 3000 to about 5000. Suitable carboxyl-functionalized butadienes and butadiene / acrylonitrile copolymers are commercially available from Huntsman under the trade names Hiker® and Hypro®. In certain preferred embodiments, a portion of one or more carboxyl-terminated butadiene acrylonitriles (CTBNs) may be adsorbed with DGEBA or DGEBF. See suitable adducts commercially available from Huntsman under the trade name Hypox®. These adducts may be dissolved or dispersed in a novolac epoxy resin to enhance solubility. In a preferred embodiment, CTBN is a CTBN-DGEBF adduct in a novolac epoxy resin.
[0064] Core-shell rubber (CSR) particles Core-shell rubber (CSR) particles, as measured by differential scanning calorimetry (DSC), generally have a structure in which a core made of a polymer material having elastomer or rubber-like properties (i.e., a glass transition temperature of less than about 0°C, e.g., less than about -30°C) is surrounded by a shell made of a non-elastomer polymer material (i.e., a thermoplastic or thermosetting / crosslinked polymer having a glass transition temperature higher than ambient temperature, e.g., higher than about 50°C). The rubber core may constitute 50-90%, particularly 50-85%, of the weight of the core-shell rubber particles.
[0065] In some embodiments, the CSR particles have an average particle size of less than about 500 nm. In yet other embodiments, the CSR particles have an average particle size greater than about 500 nm, for example, an average particle size of about 0.03 to about 2 microns, or about 0.05 to about 1 micron. Preferably, the rubber particles have an average diameter of less than about 500 nm. In other embodiments, the average particle size is less than about 200 nm. For example, the rubber particles may have an average diameter in the range of about 25 to about 200 nm, or about 50 to about 150 nm. The core-shell rubber particles may have a number-average particle size (diameter) of 10 to 300 nanometers, particularly 75 to 250 nanometers, as measured by transmission electron spectroscopy.
[0066] The core may consist of a diene homopolymer or a copolymer of monomers including one or more ethylenically unsaturated monomers such as butadiene, isoprene, vinyl aromatic monomers, (meth)acrylonitrile, (meth)acrylate, etc. Polybutadiene core particles are preferred. Other suitable rubbery core polymers include polybutyl acrylate or polysiloxane elastomers (e.g., polydimethylsiloxane).
[0067] The shell may consist of a polymer or copolymer of one or more monomers having a sufficiently high glass transition temperature, such as (meth)acrylates (e.g., methyl methacrylate), vinyl aromatic monomers (e.g., styrene), vinyl cyanide (e.g., acrylonitrile), unsaturated acids and anhydrides (e.g., acrylic acid), and (meth)acrylamide; acrylates, particularly poly(methyl methacrylate), are preferred. The shell polymer or copolymer may be crosslinked and / or have one or more different types of functional groups (e.g., carboxylic acid or epoxy groups) that can interact with other components of the adhesive. In one embodiment, the shell polymer may be polymerized from at least one lower alkyl methacrylate, such as methyl, ethyl, or t-butyl methacrylate. Up to 40% by weight of the shell polymer can be formed from other monovinylidene monomers such as styrene, vinyl acetate, vinyl chloride, methyl acrylate, ethyl acrylate, butyl acrylate, etc. The shell polymer may be a homopolymer of any of such lower alkyl methacrylate monomers. The molecular weight (Mn) of the grafted shell polymer is generally between 20,000 and 500,000. The rubber particles may consist of two or more layers (for example, a central core rubbery material may be surrounded by different rubbery materials, and then surrounded by a shell or two shells or a hard shell, soft shell, hard shell). The shells may be grafted onto the core.
[0068] CSR particles may be prepared as a masterbatch in which rubber particles are dispersed in one or more epoxy resins such as diglycidyl ether of bisphenol A, preferably remaining as separated individual particles with little or no particle aggregation or precipitation when the masterbatch is aged by being left at room temperature. Core-shell rubber particles may be provided as a dispersion in an epoxy or phenol resin matrix. Such a dispersion may contain, for example, about 5 to about 50% by weight (about 15 to about 40% by weight) of core-shell rubber, with the remainder being an epoxy resin. The epoxy resin in such a dispersion is preferably the polyglycidyl polyphenol ether described above. The matrix material is preferably liquid at room temperature. Examples of epoxy matrices include bisphenol A, F, or S, or diglycidyl ether of bisphenol, novolac epoxy, and alicyclic epoxy. An example of a phenol resin is bisphenol A-based phenoxy. A dispersion of rubber particles having a core-shell structure in an epoxy resin matrix is commercially available from Kaneka Corporation under the trade name "ACE MX," which is described as having a polybutadiene core or a (meth)acrylate-butadiene-styrene copolymer core, with butadiene being the main component of the phase-separated particles dispersed in the epoxy resin. When core-shell rubber particles are provided in the form of such a dispersion, only the weight of the core-shell rubber particles is counted as the core-shell rubber component in this disclosure. Methods for producing masterbatches are described in European Patent No. 1,632,533, U.S. Patents No. 4,778,851 and No. 6,111,015, each of which is incorporated herein by reference in its entirety.
[0069] Examples of CSR particles suitable for use in the compositions of the present invention include: those commercially available from Rohm & Haas under the trade name PARALOID EXL2600 / 3600 series, described as styrene / methyl methacrylate copolymer graphed on a polybutadiene core, with an average particle size of 0.1 to 0.3 microns; those commercially available from Rehm or Rehm America under the trade name Degaran; those commercially available from Zeon Corporation under the trade name F351; and those in powder form commercially available from Wacker Chemie under the trade name Geniopal, described by the supplier as having a crosslinked polysiloxane core, epoxy-functionalized polymethyl methacrylate shell, and a polysiloxane content of approximately 65% by weight.
[0070] Different combinations of core-shell rubber particles can be advantageously used in the present invention. The core-shell rubber particles may differ, for example, in particle size, glass transition temperature of each core and / or shell, composition of the polymer used for each core and / or shell, functionalization of each shell, etc. Some of the core-shell particles may be supplied to the adhesive composition in the form of a masterbatch in which the particles are stably dispersed in an epoxy resin matrix, and other parts may be supplied to the adhesive composition in the form of a dry powder (i.e., without using epoxy resin or other matrix materials). For example, the adhesive composition may be prepared using both a first type of core-shell particles in the form of a dry powder having an average particle size of about 0.1 to about 0.5 microns, and a second type of core-shell particles having an average particle size of about 25 to about 200 nm, stably dispersed in a matrix of liquid bisphenol A diglycidyl ether at a concentration of about 5 to about 50% by weight. The weight ratio of the first type to the second type of core-shell rubber particles may be, for example, about 1.5:1 to about 0.3:1.
[0071] Alternatively, or in conjunction with CSR, the composition may include rubber particles that do not have a shell encapsulating a central core. In such embodiments, the chemical composition of the rubber particles may be essentially uniform throughout each particle, or their outer surface may be modified by irradiation or chemical treatment to aid in dispersion in or adhesion to the matrix. A polymer suitable for use in the preparation of shell-less rubber particles may be selected from any of the polymers described above as suitable for use as the core of core-shell rubber particles. The polymer may contain functional groups such as carboxylate groups and hydroxyl groups, and may have linear, branched, crosslinked, random copolymer or block copolymer structures. Examples of commercially available rubber particles include acrylonitrile / butadiene copolymer, butadiene / styrene / 2-vinylpyridine copolymer; hydroxy-terminated polydimethylsiloxane; and similar elastomer solid rubbers. These particles may optionally be surface-modified to generate polar groups (carboxylic acid or hydroxyl groups) and / or doped with small amounts of inorganic material such as calcium carbonate or silica, as is known in the art. If the rubber particles do not have a core-shell structure, it is desirable that the rubber particles have an average diameter of approximately 750 nm, 500 nm, or less than 200 nm. For example, the rubber particles may have an average diameter in the range of approximately 25 to 200 nm, or approximately 50 to 150 nm.
[0072] In some preferred embodiments of the adhesive composition, core-shell rubber (CSR) particles may be characterized by one or more of the following features: (a) the CSR particles are dispersed in a unimodal or bimodal manner and are capable of maximum concentration; the degree of dispersion of the CSR particles may be defined by any suitable means, including sedimentation or visual or automated transmission electron microscope (TEM) imaging; (b) the average particle size of the CSR particles is within the range bounded by 50 nm, 75 nm, 100 nm, 125 nm, 150 nm, 175 nm, 200 nm, 250 nm, or 500 nm, or any two of the aforementioned values; in yet another embodiment, the rubber particles have a core-shell structure and an average particle size greater than about 500 nm; (c) the CSR particles consist of, or have a core made of, polybutadiene, butadiene / styrene copolymer, or acrylic polymer or copolymer; and / or (d) the CSR particles are dispersed in a DGEBA epoxy resin.
[0073] In the disclosed compositions, the use of these core-shell rubbers enables strengthening of the formulation regardless of the temperature used to cure the formulation. That is, because of the formulation's inherent two-phase separation by the core-shell rubber (in contrast to liquid rubbers that are miscible, partially miscible, or immiscible in the formulation and solidify at a different temperature than the formulation), the phase separation in the formulation is often observed to be essentially uniform, thus minimizing the destruction of the matrix properties. Furthermore, because it is substantially uniformly dispersed, predictable strengthening can be achieved (in terms of temperature neutrality toward curing).
[0074] Blocked polyurethane reinforcing agent In addition, or alternatively, the adhesive composition comprises one or more blocked polyurethane reinforcing agents containing polyalkylene glycol segments. The blocked polyurethane reinforcing agents improve adhesion to the intended substrate under static and dynamic peeling conditions.
[0075] In a preferred embodiment, the polyalkylene glycol segment independently comprises polyethylene glycol, polypropylene glycol, or polybutylene glycol (or polytetramethylene glycol (poly-THF or PTMEG)) having equivalent molecular weights in the range of 2000 to 5000 daltons. PTMEG bonding is preferred. In another, even more preferred embodiment, the polyurethane reinforcing agent also comprises a polyalkylene (extensioner) segment, preferably the polyalkylene glycol segment having end caps. 1~10 Alkylene bond, preferably C 6~8 They are adjacent by alkylene bonds and bonded to them by urethane groups.
[0076] Other elastomer “reinforcers” having capped isocyanate groups that may also be suitable for the compositions disclosed herein include, for example, U.S. Patent No. 5,202,390, U.S. Patent No. 5,278,257, International Publication No. 2005 / 118734, International Publication No. 2007 / 003650, International Publication No. 2012 / 091842, U.S. Published Patent Application No. 2005 / 0070634, U.S. Published Patent Application No. 200 It is described in 5 / 0209401, U.S. Published Patent Application 2006 / 0276601, European Patent No. 0308664, European Patent No. 1498441, European Patent No. 1728825, European Patent No. 1896517, European Patent No. 1916269, European Patent No. 1916270, European Patent No. 1916272, and European Patent No. 1916285. These elastomer reinforcing agents (2) are generally described as reaction products of amine or hydroxyl-terminated rubber and polyisocyanate, forming isocyanate-terminated prepolymers, optionally extending the chain of the prepolymer, and subsequently capping the isocyanate groups with capping groups such as: a) aliphatic, aromatic, alicyclic, aromaticaliphatic and / or heteroaromatic monoamines having one primary or secondary amino group; b) phenol compounds such as monophenols, polyphenols, and aminophenols; c) benzyl alcohols which may be substituted with one or more alkyl groups on the aromatic ring; d) hydroxy-functional acrylate or methacrylate compounds; e) thiol compounds such as alkylthiols with 6 to 16 carbon atoms in the alkyl group, including dodecanethiol; f) alkylamide compounds having at least one amine hydrogen such as acetamide and N-alkylacetamide; and g) ketoximes.
[0077] In the compositions of the present invention, one or more block polyurethane reinforcing agents are preferably end-capped at both ends of the structure. The two end-capping groups of the block polyurethane reinforcing agent may be the same or different. By selecting different combinations of end caps, the block dissociation temperature can be adjusted. In some embodiments, end caps are then selected to provide a block dissociation temperature of 135°C to 140°C, 140°C to 145°C, 145°C to 150°C, 150°C to 160°C, 160°C to 165°C, or any two or more of the aforementioned ranges, for example, 140°C to 150°C.
[0078] Huntsman's DY965 is a commercially available example of such a blocked polyurethane reinforcing agent, containing bisphenol in both end caps. In some cases, end capping with one or more bisphenol (e.g., bisphenol A) groups may be acceptable, but the inventors have found that the use of one or more blocking groups that provide a lower block dissociation temperature is preferred. Such end capping agents include optionally substituted phenols (or hydroxyheteroaryl analogs), amines, methacrylics, acetoxys, oximes, and / or pyrazoles (see Johannes Karl Fink, High Performance Polymers (2nd edition), 2014; https: / / www.sciencedirect.com / topics / engineering / blocked-isocyanate). For example, an aliphatic poly(isocyanate) blocked with equimolar amounts of diisopropylamine and diethyl malonate is known to have a crosslinking temperature of 130°C. Triazole-blocked isocyanates are typically stable at 130–140°C.
[0079] In some embodiments, the blocked polyurethane reinforcing agent has at least one end cap derived from methyl ethyl ketone oxime, 2,4-dimethyl-3-pentanone oxime, or 2,6-dimethyl-4-heptanone oxime, diethyl malonate, 3,5-dimethylpyrazole, 1,2,4-triazole, or a mixture of diisopropylamine and 1,2,4-triazole, or a combination thereof.
[0080] For example, C containing 1, 2, 3, or 4 conjugated and / or non-conjugated alkenylene bonds 12-24 Hydrophobic end cap substituents, such as pendant functional groups, also appear to ensure additional benefits. Accordingly, in another embodiment, any substituent of phenol (or hydroxyheteroaryl analog), amine, methacryl, acetoxy, oxime, and / or pyrazole includes such a pendant functional group.
[0081] In other embodiments, adjacent C 1-10 The alkylene bond is end-capped with at least one monophenol comprising at least one C 12-24 pendant functional group, and the at least one C 12-24 The pendant functional group contains 1, 2, 3, or 4 conjugated and / or non-conjugated alkenylene bonds. Again, the use of substituted monophenols is preferred compared to bisphenols in that it is believed to provide lower curing temperatures than bisphenol end caps.
[0082] Thermally activated latent curing agent The compositions of the present invention are preferably one-component or single-component compositions that cure at high temperatures, containing one or more curing agents capable of achieving crosslinking or curing of adhesive components when the adhesive is heated to the activation temperature of the curing agent and / or blocking reactant. To ensure good storage stability of single-component liquid epoxy adhesives, it is desirable that the latent curing agent has low solubility in epoxy resin at room temperature. To allow for easy dissolution near the activation temperature, a solid, finely ground curing agent is preferred, and dicyandiamide (DICY) is particularly suitable. In certain embodiments, one or more dicyandiamides (DICY) in the liquid epoxy adhesive composition are micronized dicyandiamide (cyanoguanidine). Since DICY is insoluble in epoxy resin before melting, the use of micronized dicyandiamide is preferred to ensure the reactivity of DICY with epoxy during and after melting. In certain embodiments, at least 98% of the micronized dicyandiamide has a particle size of 40 microns or less. In other embodiments, at least 98% of the micronized dicyandiamide has a particle size of 10 microns or less. In other embodiments, at least 98% of the pulverized dicyandiamide has a particle size of 6 microns or less. Such materials are commercially available from Alzchem under the trade name Diehard®.
[0083] One or more accelerators different from latent curing agents The liquid epoxy adhesive composition contains one or more accelerators. In certain embodiments, one or more accelerators are urea, guanidine, or substituted ureas, or include these, with substituted urea accelerators being preferred. In other embodiments, one or more accelerators are micronized, preferably micronized substituted ureas. In certain embodiments, the substituted urea is urea or crosslinked diurea substituted with 1, 2, 3, or 4 alkyl groups. In some embodiments, the urea-based accelerator is optionally aryl-substituted 1,1-dialkyl-3-arylurea. The (substituted urea) accelerator is preferably activated at a temperature above the block dissociation temperature of the urethane, but this is not required. In some embodiments, the accelerator is activated in a temperature range of 100°C to 120°C, 120°C to 140°C, 140°C to 160°C, or 160°C to 180°C, or a combination of two or more of these ranges. The Diehard® UR series and Omicure® U series are commercially available from Alzchem and Huntsman, respectively. The former is reported to be activated in the temperature range of 120°C to 140°C, and the literature characterizes UR700 as a substituted urea. Omicure® U-52M is commercially available from Huntsman and is reported to have a 4,4'-methylenebis-(phenyldimethylurea) structure. Both of these materials are useful in these liquid epoxy adhesive compositions, and the use of either (or both) of these compositions constitutes individual embodiments of this disclosure.
[0084] In some embodiments, the liquid epoxy adhesive composition comprises at least two accelerators, each activated at a different temperature. When two accelerators are present, it is preferable that the first is activated when heated to a temperature in the range of 60 to 120°C (having an activation temperature), and the second is activated when heated to a temperature in the range of at least 140°C.
[0085] Filler Liquid epoxy adhesive compositions contain solid fillers, which are organic or inorganic materials, to give the composition structural integrity before curing. Such fillers are known to those skilled in the art. In certain embodiments, one or more fillers include one or more naturally occurring clays such as calcium carbonate, calcium oxide, calcium silicate, aluminosilicate, organic affinity phyllosilicate, bentonite, wollastonite, or kaolin glass, silica, mica, talc, microspheres, or hollow glass microspheres (HGM), shredded or pulverized fibers (e.g., carbon, glass, or aramid), pigments, zeolites (natural or synthetic), or thermoplastic fillers. Calcium silicate and calcium oxide are preferred. Fillers having low aspect ratios (e.g., less than about 1) and / or very high aspect ratios (e.g., shredded or pulverized fibers) are also preferred.
[0086] Phenolic novolac epoxy In addition, or instead, the adhesive composition preferably includes one or more phenol novolac epoxys. These polyfunctional epoxy resins are typically produced from phenol novolac resins and epichlorohydrins. Upon curing, a cured material is formed having a mesh structure with a high crosslinking density. They also exhibit excellent heat resistance and chemical resistance. In the liquid epoxy adhesive compositions described herein, the phenol novolac epoxy preferably has an EEW in the range of 165 to 185, more preferably 172 to 179. Suitable epoxy novolac resins include those sold under the trade name DEN®, which encompass the 300 and 400 series epoxies commercially available from Olin.
[0087] Flame retardant The liquid epoxy adhesive composition may optionally contain one or more flame retardants. One or more flame retardants may be solid, liquid, or a combination thereof. In certain embodiments, the flame retardant is one or more of the following: aluminum trihydrate (ATH) (which may also be classified as a filler, but is classified as a flame retardant for counting purposes if present), ammonium polyphosphate, melamine, melamine polyphosphate, phosphonic acid esters (e.g., diethylbis(hydroxyethyl)aminomethylphosphonate (commercially available as phyllo(registered trademark) 6-phosphonic acid ester), halogen-free phosphate esters (commercially available as phyllo(registered trademark) HF-9), or any combination of unsubstituted mono, di, or tributylated phenyl phosphates (e.g., Emerald Innovation NH1 is a low-viscosity liquid flame retardant designed for use in flexible polyurethane foams and is said to contain a mixture of dibutylated phenyl phosphate and triphenyl phosphate, and is commercially available) or a combination thereof.
[0088] In the compositions of the present invention, a liquid flame retardant, particularly one having higher thermal stability, is preferred. In addition, or instead, a mixture comprising unsubstituted mono, di, and / or tributylated phenyl phosphate is preferred.
[0089] Furthermore, the disclosure includes examples of compositions consistent with these descriptions that have flame resistance in an uncured state, resisting ignition and flame propagation during welding via uncured adhesives.
[0090] Polyetheramine-based softeners The liquid epoxy adhesive composition may optionally contain one or more blunting agents. The inclusion of these blunting agents is thought to contribute to the improvements observed in the compositions described herein, particularly to adhesion to steel and aluminum, and to the impact wedge peel strength after "overbake" or "highbake" curing conditions of automotive E-coats and after exposure of uncured open beads to moisture. In one embodiment, one or more blunting agents may include a polyetheramine blunting agent having a polyalkylene glycol backbone, further comprising amine endcaps, such as diamines and triamines bonded to a polyether backbone based typically ethylene oxide (EO), propylene oxide (PO), or a mixture of such compounds. In some embodiments, one or more polyetheramine blunting agents exist as DGEBA adducts. The polyetheramine is preferably an end-capped polypropylene glycol characterized by repeating oxypropylene units in the backbone in a number sufficient to provide a weight-average molecular weight in the range of about 1000 to 3000 daltons, more preferably about 2000 daltons. Such materials are commercially available from Huntsman as Jefffamin® polyetheramine.
[0091] Other ingredients These liquid epoxy adhesive compositions may optionally contain additional components, such as additives including adhesion promoters; plasticizers such as tricresyl phosphate; diluents, such as epoxy-compatible chemically inert hydrocarbon resins; fillers; colorants, such as pigments and dyes; thixotropic agents, such as surface-treated fumed silica and mixed mineral thixotropes; coupling agents, such as silane coupling agents including γ-glycidoxypropyltrimethoxysilane coupling agents; swelling agents, flow control agents, and antioxidants. In certain embodiments, the liquid epoxy adhesive composition is formaldehyde-free.
[0092] Preferred adhesion promoters can be selected from reaction products of materials that enhance adhesion to metal substrates, such as chelate-modified epoxy resins, epoxy resins, and compounds containing chelate functional groups (chelate ligands). Chelate functional groups are functional groups of compounds that have multiple coordinations capable of chelating with metal ions within the molecule, and include phosphorus-containing acid groups (e.g., -PO(OH)2), carboxyl groups (-CO2H), sulfur-containing acid groups (e.g., -SO3H), amino groups, and hydroxyl groups (especially adjacent hydroxyl groups within an aromatic ring). Chelate ligands include ethylenediamine, bipyridine, ethylenediaminetetraacetic acid, phenanthroline, porphyrin, and crown ethers. A suitable commercially available chelate-modified epoxy resin is EP-49-10N manufactured by Adeka Corporation.
[0093] Method for manufacturing liquid epoxy adhesive composition Methods for producing liquid epoxy adhesive compositions are described herein. In certain embodiments of these embodiments, the method involves mixing the corresponding components at a temperature below the activation energy of the final desired composition. In certain embodiments, this temperature is within the range of about 20°C to about 40°C, about 40°C to about 60°C, about 60°C to about 80°C, or any combination of two or more of the aforementioned ranges.
[0094] Generally, it is most convenient to pre-mix components that exist as liquids at ambient temperature before adding components that exist as solids at ambient temperature, although the order of mixing is not considered important. One exemplary method is described in the examples.
[0095] Method of using liquid epoxy adhesive composition One particularly preferred application of the adhesives according to the present invention is a method for forming structural bonds in vehicle structures, such as metal-to-metal interfaces, including the joining of hem flanges and body panels, using a process that combines welding, spot welding, and adhesive bonding, for example. The use of liquid epoxy adhesive compositions in forming a bonding surface including a corresponding cured epoxy adhesive layer is considered an independent embodiment of the present disclosure, as is the method of using them for this purpose.
[0096] Liquid epoxy adhesive compositions can be applied to substrates by any convenient technique. Preferably, the composition is pumpable and can be applied cold or, if desired, warmed, preferably only to a temperature where the latent curing agent has not yet activated. It can be applied manually and / or robotically, for example, using a jet spray method or an extruder. The composition can be applied by extruding it in a bead shape from a robot or by mechanical or manual application means, and can also be applied using vortex or flow techniques. Vortex and flow techniques utilize devices well known in the art, such as pumps, control systems, dosing guns, remote dosing devices and application guns. The adhesive may be applied to one or both of the substrates to be joined. Once the liquid epoxy adhesive composition is applied, the substrates are brought into contact so that the adhesive is located at the bond line between the substrates. The substrates are brought into contact so that the adhesive is located between the substrates to be bonded together. The adhesive composition is then heated to a temperature at which the thermosetting or latent curing agent begins to cure the epoxy resin composition, forming an adhesive assembly containing the cured epoxy adhesive located between the substrates and bonded to the substrates.
[0097] In some embodiments, the adhesive is formulated to function as a hot melt; that is, an adhesive that is solid at room temperature but can be converted into a pumpable or flowable material when heated to a temperature above room temperature. In another embodiment, the composition of the present invention is formulated so that it can be flowed or pumped into the work site at or slightly above ambient temperature, since in most applications it is preferable that the adhesive is not heated to a certain temperature, at which point the latent curing agent is not yet activated. The molten composition may be applied directly to the substrate surface or poured into a space separate from the substrates to be joined, such as in hem-flanging operations. In yet another embodiment, the composition is formulated so that the curing process proceeds in two or more stages (partial curing at a first temperature, and complete curing at a second, higher temperature) (for example, by including finely divided thermoplastics or by using multiple curing agents having different activation temperatures). The two parts are preferably bonded immediately after the deposition of the adhesive mass, thereby temporarily bonding the two parts to each other.
[0098] Preferably, the resulting bond already possesses sufficient strength so that, for example, when metal plates that have been temporarily bonded to each other are treated in a washing bath for degreasing purposes and then in a phosphate treatment bath, the uncured adhesive is not easily washed away.
[0099] The composition is preferably cured in an oven at a temperature significantly higher than the temperature at which the composition was applied to the parts to be bonded, and at a temperature above the temperature at which the curing agent and / or accelerator and / or latent expanding agent (if present) is activated (i.e., in the case of a curing agent, the lowest temperature at which the curing agent becomes reactive with the other components of the adhesive; in the case of an expanding agent, the lowest temperature at which the expanding agent causes the adhesive to foam or expand). The epoxy adhesive is cured by heating it to 140°C or higher. Preferably, the temperature is about 220°C or lower, more preferably about 180°C or lower. The time required for complete curing varies somewhat with temperature, but is generally at least 5 minutes, more generally 15 to 120 minutes. Curing is preferably carried out at a temperature above 150°C, for example 160 to 220°C, for about 10 to about 120 minutes.
[0100] Epoxy adhesives can be used to bond a variety of substrates, including wood, metal, coated metal, aluminum, various plastics and filled plastic substrates, fiberglass, and the like. The substrates to be joined with the adhesive may be the same or different. It is preferably used for joining metal parts, particularly steel sheets such as cold-rolled steel sheets. These may be, for example, electro-galvanized, hot-dip galvanized, and / or zinc / nickel plated steel sheets. The composition is particularly useful for bonding substrates having surfaces contaminated with oily substances, because good adhesion is achieved despite such contamination.
[0101] After curing, the adhesive composition according to the present invention may be used as a casting resin in the electrical or electronics industry, or as a die-attach adhesive for bonding components to printed circuit boards in electronic equipment. A further possible application of this composition is as a matrix material for composite materials such as fiber-reinforced composites. One particularly preferred application of the adhesive according to the present invention is the formation of structural bonds in vehicle structures such as hem flanges.
[0102] In preferred embodiments, epoxy adhesives are used to bond parts of automobiles or other vehicles. Such parts can be steel, coated steel, galvanized steel, aluminum, coated aluminum, plastics, and filled plastic substrates. Particularly interesting applications include bonding vehicle frame components to each other or to other parts of the vehicle. Frame components are often metals such as cold-rolled steel, galvanized metal, and aluminum. Components bonded to the frame components may be the metals described above, or other metals, plastics, composite materials, etc. Assembled automobile frame components are usually coated with coating materials (such as paint) that require baking and curing. Coatings are usually baked at temperatures between 140°C and over 200°C, for example, 177-204°C for 10-20 minutes. In such cases, it is often convenient to apply epoxy adhesive to the frame components, then apply the coating, and allow the epoxy adhesive to cure simultaneously with the baking and curing of the coating.
[0103] In some embodiments, the epoxy adhesive does not cure immediately after application. During this delay before curing, the epoxy adhesive may be exposed to moist air at a temperature of up to approximately 40°C.
[0104] In some cases (such as "open bead" applications), the adhesive may be applied to one substrate and left uncovered and exposed to ambient air for a certain period before the second substrate comes into contact with the adhesive. "Open bead" applications can occur in manufacturing environments. For example, adhesive may be applied to one substrate at or near the end of a business day or business week, but the next step of assembling the substrates may not occur until work resumes on the next business day.
[0105] In other cases (such as the "closed bead" case), the second substrate is brought into contact with the adhesive, but the adhesive is left uncured and exposed to ambient air until later. In this case, the process of bonding the substrates is carried out, but this occurs in a manufacturing environment where the resulting assembly is not cured until later. The uncured assembly may be stored and / or transported, for example, before curing. In such cases, the uncured adhesive may be exposed to humid air for several hours to several months.
[0106] The adhesive of the present invention is resistant to exposure of open and closed beads to moist air, and the peel resistance and other properties of the cured adhesive are maintained.
[0107] Adhesive assembly including a cured epoxy adhesive layer The disclosed embodiments include a cured epoxy adhesive layer prepared by thermal curing the liquid epoxy adhesive composition described herein on a substrate, which preferably bonds two or more substrates together to form an adhesive assembly. In preferred embodiments, the cured epoxy adhesive layer has a nominal thickness in the range of 0.25 to 0.5 mm, preferably about 0.25 mm.
[0108] These cured epoxy adhesive layers are obtained by curing a liquid epoxy adhesive composition at a temperature in the range of 140°C to over 200°C, although in certain embodiments the liquid composition was cured (a) at a temperature of 160°C for 10 minutes; or (b) at a temperature of 205°C for 30 minutes.
[0109] Again, as previously stated, the cured epoxy adhesive layer is bonded to substrates containing cold-rolled steel (CRS), electro-galvanized steel (EZG), hot-dip galvanized steel (HDG), or treated aluminum. The cured epoxy adhesive layer exhibits excellent adhesion to these substrates. In some embodiments, the cured epoxy adhesive layer exhibits 100% cohesive failure mode in delamination of cold-rolled steel (CRS), electro-galvanized steel (EZG), hot-dip galvanized steel (HDG), and / or treated aluminum when tested under the T delamination conditions of ASTM D1876-08(2015)e1 or based on the wedge impact method of ISO11343.2019. These results demonstrate that 100% cohesive failure mode can be achieved without relying on high concentrations of fillers.
[0110] The adhesive compositions described herein exhibit high T-type peel strength after exposure to high-temperature humid conditions in an uncured state. These compositions also provide excellent impact properties at -40°C under low-temperature and high-temperature bake-curing conditions. As illustrated in the examples, the cured epoxy adhesive layer is: (a) Between two 0.8 mm thick cold-rolled steel sheets, sufficient adhesive force is provided between the sheets to exhibit a peel strength of at least 10, 11, 12, 13, 14, or 15 N / mm at room temperature after curing at 160°C for 10 minutes; and / or (b) Between two 0.8 mm thick cold-rolled steel sheets, curing at 205°C for 30 minutes provides sufficient adhesion between the sheets to exhibit a T peel strength of at least 10, 11, 12, 13, 14, or 15 N / mm at room temperature; and / or (c) When hardened between two 0.8 mm thick cold-rolled steel sheets at 160°C for 10 minutes, it exhibits cutting resistance [impact wedge peel strength] under impact loads of at least 20, 22, 24, 26, 28, 30, or 32 N / mm when tested at -40°C using the wedge impact method of ISO 11343.2019; and / or (d) When two 0.8 mm thick cold-rolled steel sheets are cured at 205°C for 30 minutes, they exhibit cutting resistance under impact loads of at least 20, 22, 24, 26, 28, 30, or 32 N / mm when tested at -40°C using the wedge impact method of ISO 11343.2019; and / or (e) Between two 2.0 mm thick 5754 aluminum plates, sufficient adhesive force is provided between the plates to exhibit a peel strength of at least 10, 11, 12, 13, 14, or 15 N / mm at room temperature after curing at 160°C for 10 minutes; and / or (f) When cured at 205°C for 30 minutes between two 2.0 mm thick 5754 aluminum plates, sufficient adhesive strength is provided between the plates to exhibit a peel strength of at least 10, 11, 12, 13, 14, or 15 N / mm at room temperature.
[0111] The cured structural adhesive also exhibits good stress resistance to aluminum in high-temperature / humid environments, and in some embodiments, for example, it has the ability to withstand a constant compressive shear load of 7.68 MPa while reaching environmental aging of more than 22 cycles in accordance with Ford BV101-07 "Stress resistance test of adhesive lap shear bond" (described elsewhere in this specification), with no paper fragments failing under both low-temperature and high-temperature bake-curing conditions. In other embodiments, a cured epoxy adhesive layer cured at 160°C for 10 minutes can withstand at least 25, 30, 35, 40, or 45 cycles of environmental aging according to FLTM BV101-07.
[0112] This disclosure encompasses all products comprising any applied (not fully cured) liquid (pre-cured or partially cured) epoxy adhesive composition and any cured epoxy adhesive layer bonded thereto. In certain embodiments, the product is an automobile, a home appliance, or a component thereof.
[0113] term In this disclosure, the singular forms "a," "an," and "the" include multiple references, and unless the context explicitly indicates otherwise, references to a particular number include at least that particular value. Thus, for example, a reference to "material" is a reference to at least one such material and / or equivalent known to those skilled in the art.
[0114] When a value is expressed as an approximation using the descriptor "approximately," it will be understood that the particular value may form another embodiment. In general, the use of the term "approximately" indicates an approximation that may vary depending on the desired properties to be obtained by the disclosed subject matter, and should be interpreted in the specific context in which it is used, based on its function. Those skilled in the art will be able to interpret this as an everyday matter. Where present, all ranges are inclusive and combinable. That is, a reference to a value specified in a range encompasses all values within that range.
[0115] For clarity, it should be understood that certain features of the Disclosure described herein in relation to separate embodiments may be provided in combination in a single embodiment. That is, unless otherwise clearly incompatible or specifically excluded, individual embodiments are considered to be able to be combined with other embodiments, and such combinations constitute a different embodiment. Conversely, for brevity, various features of the Disclosure described in relation to a single embodiment may be provided individually or in any subcombination. Finally, certain embodiments may be described as part of a series of steps or as part of a more general structure, but each of the steps may also be considered an independent embodiment that can be combined with other steps.
[0116] The transitional terms “contains,” “essentially consists of,” and “consist of” are intended to imply the meanings commonly accepted in patent dictionaries. In the case of these embodiments provided by the term “essentially consists of,” the basic and novel features are the ease of operation of the method or composition / system for providing a composition exhibiting the claimed functional features using only the enumerated components.
[0117] Where a list is presented, please understand that, unless otherwise stated, each element of that list, and all combinations of that list, are distinct embodiments. For example, a list of embodiments presented as "A, B, or C" is to be interpreted as including embodiments of "A," "B," "C," "A or B," "A or C," "B or C," or "A, B, or C" as distinct embodiments.
[0118] Unless otherwise specified, the percentage of composition is given as a weight percentage relative to the weight of the material or composition.
[0119] The following examples are intended to supplement, rather than replace, the previous description. [Examples]
[0120] The following examples provide experimental methods used for the manufacture and characterization of liquid epoxy adhesives, as well as their variations and performance. While each example disclosed herein is intended to provide a specific individual embodiment of a composition, preparation method, and use, none of the examples should be considered to limit the more general embodiments described herein.
[0121] In the following embodiments, efforts have been made to ensure the accuracy of the numerical values (quantities, temperatures, etc.) used, but some degree of experimental error and deviation should be taken into consideration. Unless otherwise specified, temperatures are in Celsius, and pressures are atmospheric pressure or close to it.
[0122] Examples of mixed conditions: Bisphenol diglycidyl ether (e.g., DGEBA and / or DGEBF) epoxy resin; epoxy novolac resin (poly[(phenylglycidyl ether)-co-formaldehyde]); diluent; core-shell rubber particles dispersed in DGEBA and / or DGEBF; chelate-modified glycidyl resin; carboxyl-terminated butadiene acrylonitrile (CTBN) to which DGEBA and / or DGEBF has been added and dissolved in the novolac epoxy resin; polyurethane reinforcing agent; γ-glycidoxypropyltrimethoxysilane coupling agent; and plasticizer were mixed in a Thinky cup up to 100 g and mixed under vacuum on a Thinky mixer at 2,000 rpm for 1.5 minutes. After mixing the lipid components, solid fillers and thixotropes were added to the mixture as follows: calcium oxide (CaO); pigment; surface-functionalized hydrophobic fumed silica thixotrope; and surface-functionalized mixed mineral thixotrope. The mixture was then mixed at atmospheric pressure, followed by vacuum mixing at 8.0 kPa at 2,000 rpm for 1.5 minutes. Additional desired auxiliary agents and additives were blended into the mixture. Subsequently, a 1K curing agent package containing dicyandiamide (DICY) and an accelerator was added to the batch, mixed at atmospheric pressure, followed by vacuum mixing at 8.0 kPa at 2,000 rpm for 1.5 minutes. Care was taken to ensure that the batch was not heated to a temperature above 55.0°C.
[0123] test Unless otherwise specified, T peel tests were performed under the T peel conditions of ASTM D1876-08(2015)e1. The CRS specimens were 0.8 mm thick and coated with Ferrocote 6130 lubricant, while the Al specimens were 2.0 mm thick and coated with DC290 lubricant. Before applying lubricant to one side, the metal specimens were cleaned with 2-propanol and wiped with a paper towel. The adhesive composition was then applied to the lubricated surface of the specimens. During the curing cycle, the two specimens were held together using metal clips, typically at temperatures well above ambient temperature. The specimen / adhesive assemblies were cured as described below. For the T peel test, the specimens had an overlay of 75 mm and a width of 20 mm, and were pulled at a speed of 127 mm / min using an Instron tester. The peel strength was calculated using the average load at the plateau.
[0124] A test specimen for impact peeling testing, having the ISO 11343 test shape (30 mm overlay, 20 mm width), was subjected to an impact load of 90 J at a drop velocity of 2 m / s. The impact peeling strength was measured using an Instron Dyna-Up 9250HV impact tester with the average impact load on a plateau.
[0125] Example 1: Curing of polyurethane reinforcing agent, Part 1: The effect of various reinforcing agents on the resistance of uncured adhesives to moisture exposure of open beads was investigated. Test compositions 1-6 were prepared according to the components listed in Table 1 below, using exemplary mixing conditions.
[0126] [Table 1]
[0127] Both reinforcing agents PU1 and PU2 were characterized by containing a polytetramethylene glycol (PTMEG) backbone. PU1 was described by the manufacturer as a bisphenol-terminated polyurethane. PU2 was a polyurethane asymmetrically end-capped with oxime and hydrophobic monophenol functional groups. PU2 exhibited a significantly lower block dissociation temperature than PU1 and had at least one end cap that was more hydrophobic than the bisphenol end cap of PU1.
[0128] Using compositions 1 to 6, the effect of each reinforcing agent on the moisture resistance of the uncured open bead was measured as follows: As described above, each composition was applied as an open bead of adhesive onto cold-rolled steel (CRS) specimens prepared for the T peel test. Each specimen with the adhesive open bead was left uncovered and exposed to ambient air at 35°C and 85% relative humidity for the periods shown in Table 2 below. Next, a second substrate was brought into contact with the adhesive and cured at 205°C for 30 minutes, and the T peel strength was tested according to ASTM D1876-08(2015)e1. The test results are shown in Table 2 for the initial T peel strength at T0 (corresponding to no humidity aging), as well as for various humidity exposure times after T24, T72, and T168 hours of exposure followed by T peel tests.
[0129] [Table 2]
[0130] These results indicate that PU2 showed higher T peel strength compared to PU1 after initial and uncured open bead exposure to moisture. Interestingly, each reinforcing agent investigated showed increased T peel strength after the uncured open bead was exposed to moisture.
[0131] Example 1: Curing of polyurethane reinforcing agent, Part 2: Next, PU2 was directly compared to PU1 in a more complex structural adhesive composition with a block polyurethane concentration of 9.58% by weight. Examples PU1 and PU2 were prepared according to the components listed in Table 3 below, using exemplary mixing conditions.
[0132] [Table 3]
[0133] T peel tests were performed using the compositions listed in Table 3, applied to CRS pre-lubricated with Ferrokote 6130 oil and Al 5754-A951 pre-lubricated with DC290, in accordance with ASTM D1876-08(2015)e1. These compositions were applied to CRS and cured at a high bake temperature of 205°C for 30 minutes or at a "low bake" temperature of 160°C for 10 minutes, followed by an impact test at -40°C to perform a low-temperature impact peel test (ISO11343).
[0134] [Table 4]
[0135] These results indicate that PU2 exhibited a 67.9% improvement in T-peel strength on cold-rolled steel (CRS) compared to PU1. Furthermore, while PU1 showed complete adhesive failure on both steel and aluminum substrates, PU2 showed thin-film failure, indicating improved adhesion compared to PU1. It was also found that PU2 provided comparable impact properties at -40°C, typically when using a combination of block polyurethane, core-shell rubber, and a CTBN-based reinforcing agent. In this case, both PU1 and PU2 showed a good failure mode after dynamic impact at -40°C. Similar to the CTBN reinforcing chemical reaction, the PU phase separated during the curing of the epoxy network via a reaction-induced phase separation (RIPS) mechanism. Thermodynamically, the phase separation of PU is favorable because the mixing free energy between the epoxy resin and PU increases as the curing reaction progresses. Such a RIPS mechanism forms nano- and / or micron-scale spherical, rubbery reinforcing adducts, activating cavitation, void growth, and matrix shear, resulting in a reinforcing mechanism prior to crack growth. These strengthening mechanisms occur under both static and dynamic failure conditions.
[0136] Example 2 With PU2 remaining as the polyurethane reinforcing agent, additional Comparative Examples 1-3 and the adhesive compositions of Example 2 were prepared according to Table 5 below, and the effects of various accelerators and amounts of PU2 on the adhesion and impact properties of uncured open beads before and after exposure to moisture were tested.
[0137] [Table 5]
[0138] Comparative Examples 1-3 and Example 2 were subjected to impact peel (N / mm) and T peel (N / mm) tests according to Example 1, unless otherwise specified below. The CRS substrate was 0.8 mm thick, and the aluminum substrate was 2.0 mm thick. These and additional tests and results are shown in Tables 6 and 7.
[0139] [Table 6]
[0140] Surprisingly, as shown in Table 6, Example 2 exhibited high T-peel strength on both steel and aluminum substrates, correspondingly showing a 100% cohesive failure mode. Achieving good adhesion to both steel and aluminum substrates, along with excellent impact properties over a wide curing range, with a single formulation is extremely difficult. Typically, different adhesive compositions are used to bond steel and aluminum substrates. For example, Betamate® 4601 is a highly elastic epoxy adhesive used for bonding Al substrates (International Publication No. 2018 / 048655). In further testing according to ASTM D1876-08(2015)e1, Example 2 also showed a cohesive failure mode and good T-peel strength on electroplated (EZG) and hot-dip galvanized (HDG) steels, respectively.
[0141] The data in Table 6 show that alkyl-substituted urea accelerators provided structural adhesives with higher T peel strength on both steel and aluminum substrates compared to aromatic-substituted ureas. This occurred regardless of the concentration of novolac epoxy resin or polyurethane reinforcing agent, which tended to provide harder adhesives with lower modulus (see Comparative Examples 2 and 3).
[0142] These examples also demonstrate adhesive compositions that minimize "foaming" due to the presence of moisture absorbed when uncured open beads are exposed to moisture. Foaming appeared to decrease in relation to the concentrations of CaO and blocked polyurethane in the composition. Surprisingly, Example 2 provided an adhesive with an impact peel strength value of >20 N / mm at -40°C after 72 hours of exposure of the uncured open bead to moisture. Typically, North American automotive OEMs require an impact peel strength of >15 N / mm when the adhesive is not exposed to moisture before curing and tested at a test temperature of -40°C. Example 2 demonstrated excellent moisture resistance under both static and dynamic peel conditions.
[0143] Furthermore, the adhesion and impact wedge peel data in Table 6 indicate that Example 2 showed improved adhesion to aluminum, which may be at least partially due to the combination of core-shell rubber (CSR), carboxyl-terminated butadiene-acrylonitrile (CTBN), and polyurethane (PU) reinforcing agents, in addition to the use of alkyl-substituted urea accelerators.
[0144] Comparative Examples 1-3 and Example 2 underwent stress resistance testing on aluminum test substrates as follows, based on Ford BV101-07 "Stress Resistance Test of Adhesive Wrap Shear Bonding": Six Al5754-A951 wrap shear test specimens were cleaned with acetone, and pairs of specimens were bonded with a 12.7 mm adhesive overlap, a 25.4 mm adhesive width, and a 0.25 mm adhesive thickness, secured with stainless steel bolts and fiberglass washers. Unless otherwise specified, the adhesive was cured at 205°C for 30 minutes before testing. Curing at 160°C for 10 minutes is considered a "low bake" state. A series of bonded test specimens were connected to a fixture and a load of 2400 N was applied. The loaded specimens and assemblies were immersed in a 5 wt% NaCl solution at pH 7 according to a predetermined cycle. Each tube containing the specimens was circulated daily during working hours; otherwise, the tubes were left under the following humidity conditions (e.g., weekends and holidays). Each exposure cycle consists of 15 ± 1 minute in a 5 wt% NaCl solution, followed by 105 ± 5 minutes of vertical drop-drying under ambient laboratory conditions, and then 22 hours at 50 ± 2°C and 90 ± 5% relative humidity. Typically, the test is performed for at least 22 cycles. The results are shown in Table 7.
[0145] [Table 7]
[0146] The stress resistance of Comparative Examples 1-3 and Example 2 on aluminum indicates that adhesives cured under low bake conditions have comparable resistance; however, under high bake conditions of 205°C for 30 minutes, Example 2 undergoes considerably more cycles before the first test specimen breaks compared to Comparative Example 1.
[0147] Figure 1 shows the differential scanning calorimetry (DSC) results for Comparative Example 1 and Example 2. Figure 1A shows the heat flow rate as a function of temperature. Figure 1B shows the thermogram corresponding to the "low bake" curing condition. The differential scanning calorimetry (DSC) results shown in Figures 1A and 1B tend to indicate that alkyl-substituted urea accelerators participate in the reaction more effectively than aromatic-substituted urea accelerators. Specifically, the thermogram in Figure 1A shows sharper exothermic reactions occurring in a lower temperature range compared to accelerators that are activated at higher temperatures. The thermogram corresponding to the "low bake" curing condition in Figure 1B shows that alkyl-substituted urea accelerators promote the conversion of more available epoxy rings during the curing cycle, especially under low-temperature curing conditions, compared to bulkier aromatic-substituted urea accelerators, thereby ensuring that the structural adhesive cures properly in the OEM E-coat oven despite the inherent temperature fluctuations of the oven and the entire vehicle component. The alkyl substitution accelerator provided a broader curing range, enabling proper formation of a thermosetting network for adhesion and facilitating efficient reaction phase separation of the reinforcing agent during curing, resulting in good impact wedge peel strength at -40°C. The dynamic mechanical analysis (DMA) results, shown in Table 8, support the DSC results.
[0148] Formulations corresponding to Comparative Examples 1, 2, and 3 in Table 5; and formulations corresponding to Example 2 in Table 5, Examples 3 and 4 in Table 9, and Example 5 in Table 12 were prepared, and separate samples were cured under low bake conditions (160°C for 10 minutes) or high bake conditions (205°C for 30 minutes). The samples were subjected to dynamic mechanical analysis, and the results are shown in Table 8 below.
[0149] [Table 8]
[0150] Surprisingly, the DMA results in Table 8 show that, after high bake curing conditions, the alkyl-substituted urea accelerator resulted in a cured composition with a lower modulus of elasticity in the rubbery plateau. Compared to Comparative Example 1, Example 2 was observed to exhibit more stress-resistant cycles before failure after overbake curing. This is likely because the adhesive was able to more efficiently distribute the load at the overlapping edges where undercutting of the adhesive bond is likely to occur.
[0151] Examples 3 and 4 Further impact and stress resistance examples shown in Table 9 were prepared and tested using the test plans described for Examples 1 and 2, unless otherwise noted. Example 3 contains increased amounts of silicate filler and thixotrope, and Example 4 has an additional component of polyetheramine-DGEBA adduct. The corresponding test data are shown in Tables 10 and 11.
[0152] [Table 9]
[0153] Examples 3 and 4 underwent impact peel (N / mm) and T peel (N / mm) tests according to Example 1, unless otherwise specified below. The CRS substrates had the thicknesses shown in the table, and the aluminum substrate was 2.0 mm thick.
[0154] [Table 10]
[0155] Examples 3 and 4 underwent stress resistance testing on aluminum test substrates according to Ford BV101-07, as described above for Example 2. Unless otherwise specified, the adhesive was cured at 205°C for 30 minutes before testing. The aluminum substrate used for testing was 5754-A951-DC290. The results of the stress resistance cycle are shown in Table 11.
[0156] [Table 11]
[0157] The test results in Table 11 show that the incorporation of calcium metasilicate in Example 3 improved the stress resistance properties compared to Example 2. This may be due to improved adhesion by increasing the shear modulus of the interface adhesive (see Dolzal, Influence of Mechanical Properties of Polymer Matrix on Fiber-Matrix Interface Shear Strength, Materials Science and Engineering: A, 126, 1990). Here, a similar adhesion mechanism to that of epoxy adhesives bonded to inorganic surfaces such as carbon fibers may be at work, with needle-shaped calcium metasilicate increasing the shear modulus of the interface from the aluminum / epoxy interface by approximately 5 to 5,000 angstroms. However, the incorporation of fillers may reduce the impact wedge-release properties of the structural adhesive, especially at low temperatures, e.g., -40°C.
[0158] As shown in the test results of Example 4, the introduction of the polyetheramine-DGEBA adduct improved the impact wedge peel strength and failure mode in CRS and aluminum after overbake curing conditions compared to Example 3. Furthermore, the impact wedge peel strength after exposure of the uncured open bead to moisture increased by 44.9% after the introduction of the polyetheramine-DGEBA adduct, even after a 10.7% reduction in CSR content. Thus, the good moisture resistance shown in Example 2 was maintained, while the stress resistance in the "first cycle to fracture" after overbake curing increased by 36%.
[0159] Examples 5-11 In some embodiments, an uncured adhesive composition may be applied to a workpiece, and then, for example, before curing in an E-coat oven, the workpiece may be spot-welded to another metal substrate during the assembly of an automotive body-in-white (BIW) structure, such that the spot welds pass through the uncured adhesive. Therefore, it is desirable that the adhesive composition includes a flame retardant that imparts flame resistance to the adhesive in its uncured state without adversely affecting other performance properties of the adhesive.
[0160] The impact-resistant adhesive compositions of Examples 5-11 were prepared using the components listed in Table 12 below and tested to investigate the effect of various flame retardant (FR) chemicals on the flame resistance of the uncured weld. In Table 12, the FRs are solid: ATH; melamine polyphosphate and melamine; and liquid: Phos.1, Phos.2 and Phos.3.
[0161] The thickness of the bond line was controlled using glass beads (GB). GB may be mixed directly into the liquid adhesive, or it may be introduced during sample preparation, as is known to be done by applying it to the uncured layer before bonding the substrates.
[0162] [Table 12]
[0163] The compositions of Examples 5-11 underwent the following weld flammability performance test: a layer of uncured adhesive was formed between two cleaned metal panels, and a series of 34 welds were performed at specific spatial intervals using medium-frequency DC. This test was repeated for a total of 170 welds across five specimens. The panels were observed during welding to check for ignition of the adhesive. A "pass" rating was given if (a) the structural adhesive ignited in four or fewer welds out of 170, and (b) any combustion that occurred spontaneously extinguished within 30 seconds, in accordance with FLTM BV114-01 for steel substrates and / or FLTM BV062-01 for aluminum substrates. The results are shown in Table 13.
[0164] For adhesives that passed the weld flammability test, impact resistance, adhesion, and stress resistance were also measured. As shown in Table 13, the applicants have developed flame-retardant liquid adhesive compositions that pass uncured flammability and weldability tests, provide improved flame retardancy suitable for welding, and maintain impact, adhesion, and stress resistance.
[0165] [Table 13]
[0166] The results in Tables 12 and 13 indicate that melamine and ATH, which are solid FRs, can be incorporated into structural adhesives, but that high concentrations of these solid FR particles are required to pass weld flammability tests. However, high concentrations of solid FR materials tend to embrittle the cured adhesive composition, resulting in reduced impact wedge peel strength at -40°C, decreased fracture toughness, and particularly reduced adhesive strength at -40°C.
[0167] It was discovered that specific combinations of liquid phosphate-containing flame retardants, such as mono, di, and tributylated phenyl phosphates and triphenyl phosphates, and low concentrations of solid flame retardants, such as ammonium polyphosphate, melamine, and ATH, suppressed flame rise and propagation during welding flammability tests (see Example 9). Even more surprisingly, the applicants found that incorporating a blend of phenyl isobutylated phosphate and triphenyl phosphate with 7.9% phosphorus into a composition in an amount of less than 3% by weight (other than 0) (see Example 11) effectively mitigated "flame rise" and rapidly extinguished flames during welding flammability tests.
[0168] Therefore, the compositions of the present invention may be manufactured using or without solid flame retardants. Solid flame retardants are advantageous because they have been shown to reduce adhesive fracture toughness, peel strength, and impact strength. Also, a lower solid filler content increases elongation; for example, Example 11 had an elongation of 12.3 ± 1.8% (ASTM D638). Finally, the low viscosity of adhesives without high concentrations of solid flame retardant fillers made it easier to pass acceptance welding tests on aluminum.
[0169] Thermogravimetric analysis (TGA) was used to study the mechanism of phosphorus-containing flame retardants investigated in this study. Figure 2 shows the isothermal thermogravimetric analysis (TGA) curves for phosphorus-based flame retardants Phos.1, Phos.2, and Phos.3 used in the formulations listed in Tables 12 and 13. The TGA curves show that Phos.3, used in Example 11, exhibited higher thermal stability compared to Phos.1 and 2, which had higher phosphorus concentrations but failed the weld flammability test. Thus, phosphorus concentration alone could not govern the flame resistance of the weld. The thermal stability of the flame retardant played a role in suppressing flame rise and extinguishing the fire throughout the weld flammability test.
[0170] Examples 12-17 and Comparative Example 4 Examples 12-17 and Comparative Example 4 were prepared according to Table 14 below, using modified formulations that separated the rubber effect from various polyurethane reinforcing agents and their amounts by omitting the rubber reinforcing agent. The compositions were tested for T peel strength (n / mm) on HDG and aluminum substrates according to ASTM D1876-08(2015)e1, and the test results are also shown in Table 14. PU1 improved T peel strength on aluminum, but adhesive failure occurred on HDG. PU2 exhibited a cohesive failure mode on both aluminum and HDG substrates, resulting in a satisfactory improvement in T peel strength for both.
[0171] [Table 14]
[0172] As will be understood by those skilled in the art, many modifications and variations of the present invention are possible in light of these teachings, all of which are intended herein. All references cited herein are incorporated herein by reference, at least in relation to their teachings in the context in which they are presented.
Claims
1. (a) At least one bisphenol A diglycidyl ether (DGEBA) epoxy resin or / or bisphenol F diglycidyl ether (DGEBF) epoxy resin present in an amount ranging from 20% to 60% by weight; (b) One or more carboxyl-terminated butadiene homopolymers or butadiene acrylonitrile copolymers (CTBNs) present in an amount ranging from 1% to 8% by weight; (c) Core-shell rubber (CSR) particles present in a range of 5% to 30% by weight; (d) One or more polytetramethylene glycol (PTMEG) backbone-containing asymmetric end-capped polyurethane reinforcers present in an amount ranging from 5% to 20% by weight; (e) At least one thermally activated latent curing agent comprising dicyandiamide (DICY) present in an amount ranging from 2% to 6% by weight; (f) at least one accelerator different from the curing agent, present in an amount ranging from 0.5% by weight to 2.0% by weight, wherein the accelerator is an alkyl-substituted urea accelerator; and (j) One or more polyetheramine-based softeners present in an amount ranging from 1% to 12% by weight; A liquid epoxy adhesive composition comprising, A liquid epoxy adhesive composition in which the weight percentage of each component is relative to the total weight of the composition.
2. (a) One or more bisphenol A diglycidyl ether (DGEBA) epoxy resins and / or bisphenol F diglycidyl ether (DGEBF) epoxy resins present in an amount ranging from 20% by weight to 60% by weight; (b) One or more carboxyl-terminated butadiene acrylonitrile copolymers (CTBNs) present in an amount ranging from 1% to 8% by weight; (c) Core-shell rubber (CSR) particles present in a range of 5% to 30% by weight; (d) One or more polytetramethylene glycol (PTMEG) backbone-containing asymmetric end-capped polyurethane reinforcers present in an amount ranging from 5% to 20% by weight; (e) A thermally activated latent curing agent which is one or more dicyandiamides (DICY) present in an amount ranging from 2% to 6% by weight; (f) One or more alkyl-substituted urea promoters present in an amount ranging from 0.5% to 2.0% by weight; (g) One or more fillers present in an amount ranging from 0% to 20% by weight; (h) One or more phenol novolac epoxy present in an amount ranging from 0% to 20% by weight; (i) One or more flame retardants present in an amount ranging from 0% by weight to 35% by weight; (j) A polyetheramine-based softener containing one or more polyetheramine-DGEBA adducts present in an amount ranging from 1% to 12% by weight; and (k) One or more plasticizers present in an amount ranging from 0% by weight to 5% by weight; Includes, The liquid epoxy adhesive composition according to claim 1, wherein the weight percentage of each component is relative to the total weight of the composition.
3. The liquid epoxy adhesive composition according to claim 2, wherein one or more bisphenol A diglycidyl ether (DGEBA) epoxy resins and / or bisphenol F diglycidyl ether (DGEBF) epoxy resins have an epoxy equivalent weight (EEW) in the range of 180 to 195, where EEW = molecular weight of the epoxy resin / number of epoxy groups.
4. A liquid epoxy adhesive composition according to claim 1 or 2, wherein bisphenol F diglycidyl ether (DGEBF) is added to one or more carboxyl-terminated butadiene acrylonitrile (CTBN).
5. The core-shell rubber (CSR) particles are: (a) Having a unimodal or bimodal particle size distribution; (b) Having a number-average particle size in the range of 50 nm to 500 nm as measured by transmission electron spectroscopy; (c) having a core that is essentially composed of or made of polybutadiene, butadiene / styrene copolymer, or acrylic polymer or copolymer; and / or (d) The liquid epoxy adhesive composition according to claim 1 or 2, wherein component (a) is dispersed in bisphenol A diglycidyl ether (DGEBA epoxy resin).
6. The liquid epoxy adhesive composition according to claim 1 or 2, wherein one or more dicyandiamides (DICY) include finely powdered dicyandiamide.
7. The liquid epoxy adhesive composition according to claim 1 or 2, comprising one or more flame retardants and one or more combinations of aluminum trihydrate (ATH), ammonium polyphosphate, melamine, melamine polyphosphate, phosphonic acid esters, aminomethylphosphonic acid esters, halogen-free phosphate esters, or unsubstituted mono, di, or tributylated phenyl phosphates.
8. The liquid epoxy adhesive composition according to claim 2, wherein one or more fillers comprise one or more of the following: calcium carbonate, calcium oxide, calcium silicate, aluminosilicate, organic affinity phyllosilicate, naturally occurring clay, wollastonite or kaolin glass, silica, mica, talc, microspheres, or hollow glass microspheres, shredded or pulverized fibers, pigments, zeolites (natural or synthetic), or thermoplastic fillers.
9. The liquid epoxy adhesive composition according to claim 2, wherein the (j) polyetheramine-based softener has a weight-average molecular weight in the range of 1,000 to 3,000.
10. At a temperature below the activation energy of the final desired composition, 1) A step of mixing liquid components, 2) A step of mixing the solid components excluding the hardener and accelerator with the combination of step 1), and 3) A step of incorporating the hardening agent and accelerator into the mixture. A method for preparing the liquid epoxy adhesive composition according to claim 1 or 2, comprising the above.
11. A step of applying the liquid epoxy adhesive composition according to claim 1 or 2 to a first surface, A step of bringing at least one second surface into contact with a composition on the first surface, and A step of curing the composition by bringing it into contact with the first surface and the second surface to prepare an adhesive assembly. A method for manufacturing an adhesive assembly, including the method described above.
12. The method according to claim 11, wherein one or more of the first surface and the second surface are contaminated with at least one oily substance, and the liquid epoxy adhesive composition further comprises at least one chelate-modified epoxy resin.
13. The method according to claim 11, wherein the curing step includes thermal curing of the liquid epoxy adhesive composition at a temperature in the range of 140°C to 220°C.
14. A product comprising an adhesive assembly having two surfaces bonded together with a cured liquid epoxy adhesive composition according to claim 1 or 2, wherein the adhesive assembly exhibits a 100% cohesive failure mode in delamination of cold-rolled steel (CRS), electro-galvanized steel (EZG), hot-dip galvanized steel (HDG), and / or treated aluminum when tested under the T delamination conditions of ASTM D1876-08 (2015)e1 or according to the wedge impact method of ISO 11343.2019.
15. A product comprising the liquid epoxy adhesive composition according to claim 1 or 2, applied to at least one surface of the product and in an uncured state, or cured on at least one surface of the product.
16. The liquid epoxy adhesive composition according to claim 1, wherein the (c) core-shell rubber (CSR) particles have a number-average particle size of 500 nm or less as measured by transmission electron spectroscopy.
17. The liquid epoxy adhesive composition according to claim 1 or 2, wherein the alkyl-substituted urea accelerator (f) is a finely powdered urea having 1 to 4 alkyl groups, or a methylene crosslinked bis(phenylurea) N-substituted with 1 to 4 alkyl groups, and the accelerator is activated in a temperature range of 100°C to 180°C.
Citation Information
Patent Citations
Epoxy resin adhesive composition
JP1993065391A
Reinforced epoxy adhesive composition
JP2008542484A
Capped polyurethane prepolymer and thermosetting epoxy resin composition
JP2010507706A
Polymer fine particle-containing curable resin composition improved in storage stability and adhesion
JP2016199739A
Curable epoxy resin composition and laminate using the same
JP2020132833A