Release film

The release film with an aqueous coating composition enhances peelability and wettability for thin ceramic green sheets, addressing environmental and health concerns by minimizing organic solvent use and improving adhesion.

JP7953823B2Active Publication Date: 2026-11-19TOYOBO CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024574854
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-02-03
Filing Date
2024-01-26
Publication Date
2026-11-19
Estimated Expiration
2044-01-26

AI Technical Summary

Technical Problem

Conventional release films face challenges with insufficient peelability and wettability for thin ceramic green sheets, leading to defects like pinholes and uneven thickness, and pose environmental and health risks due to organic solvents used in their manufacturing.

Method used

A release film with a release layer formed by reacting and solidifying an aqueous coating composition containing specific silicone emulsions, including resins with siloxane structures and Q units, applied to a polyester film, which is stretched and heat-treated to enhance peelability and wettability, reducing organic solvent use.

Benefits of technology

The film achieves improved peelability and wettability, minimizing defects in thin ceramic green sheets while significantly reducing environmental and health impacts, and optimizing adhesion to the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007953823000001
    Figure 0007953823000001
  • Figure 0007953823000002
    Figure 0007953823000002
  • Figure 0007953823000003
    Figure 0007953823000003
Patent Text Reader

Abstract

Provided is a mold release film that makes it possible to reduce the amount of an organic solvent, exhibits both good wettability and light releasability with respect to thin ceramic green sheets, and further exhibits superior adhesion between a release layer and a base material film. The present invention is a release film having a release layer on at least one surface of a polyester film, wherein: an aqueous coating composition for forming the release layer includes a silicone emulsion; the silicon emulsion contains (a) a first resin having a siloxane structure represented by the formula (R2-SiO-R1)k (in the formula, R1 is an alkenyl group having 2-8 carbon atoms, R2 is an alkyl group having 1-4 carbon atoms or an alkenyl group having 2-8 carbon atoms, and k is 1-50), (b) a second resin containing a hydrogen moiety, and (c) a silicone having a Q unit represented by the formula SiO4 / 2; and the first resin and / or the second resin further has a siloxane structure represented by the formula (R3-SiO-Ar)m (in structural formula 2, R3 is an alkyl group having 1-4 carbon atoms, Ar is an aryl group, and m is 1-50).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a release film having a base film and a release layer, and more particularly to a release film useful as a film for various processes. [Background technology]

[0002] Conventionally, release films, which use polyester film or the like as a base material and laminate a release layer on top of it, have high heat resistance and mechanical properties and are used as process films for manufacturing adhesive sheets, cover films, ceramic green sheets, polymer electrolyte membranes, and other resin sheets. Furthermore, many release layers for release films have been proposed that are formed from silicone-containing coating compositions due to their good heat resistance and peelability (for example, Patent Documents 1 to 5).

[0003] The aforementioned release film is also used as a process film for molding ceramic green sheets, which require high smoothness for ceramic capacitors, ceramic substrates, and other applications. In recent years, with the miniaturization and increased capacitance of multilayer ceramic capacitors, there has been a trend towards thinner ceramic green sheets. Ceramic green sheets are molded by coating a slurry containing ceramic components such as barium titanate and a binder resin onto the release layer of a release film and drying it. Multilayer ceramic capacitors are manufactured by printing electrodes onto the molded ceramic green sheet, peeling it off the release film, and then laminating, pressing, firing, and applying external electrodes to the resulting electrode-equipped ceramic green sheet.

[0004] Patent documents 1 and 2 propose a release film made by a method (hereinafter referred to as "offline coating") in which a coating composition containing a polysiloxane having an unsaturated group, a polysiloxane having a hydrogen group, a platinum group metal catalyst, and an organic solvent is applied to one side of a biaxially oriented polyester, and then the coating composition is dried and cured by heat treatment to form a release layer.

[0005] Patent Document 3 proposes a release film in which a release layer is formed by applying an aqueous coating composition containing an alkenyl group-containing silicone and a silicone containing a hydrogen group and a phenyl group to one side of a polyester film, and then stretching the polyester film (hereinafter referred to as "in-line coating"). Furthermore, Patent Document 4 proposes a release film in which a release layer is formed by offline coating using a coating composition containing a silicone containing an aryl group. In addition, Patent Document 5 proposes a release film in which a release layer is formed by in-line coating using a coating composition containing a silicone having Q units. [Prior art documents] [Patent Documents]

[0006] [Patent Document 1] Japanese Patent Publication No. 2003-292894 [Patent Document 2] International Publication No. WO2017 / 200056 [Patent Document 3] Patent No. 5735278 [Patent Document 4] Patent No. 5756315 [Patent Document 5] Japanese Patent Publication No. 2021-11081 [Overview of the Initiative] [Problems that the invention aims to solve]

[0007] In recent years, with the trend towards thinner ceramic green sheets, there has been a growing demand for release films that offer easy, uniform peelability, allowing the ceramic green sheet to be removed with low force. Furthermore, there is a need for release films with good wettability to the ceramic slurry applied to the release layer. To thin ceramic green sheets, for example, it is necessary to uniformly apply a diluted, low-solids-content ceramic slurry onto the release layer using an amount of organic solvent exceeding the amount of resin. When such a ceramic slurry is applied to the release layer, the wettability of the release film to the ceramic slurry may be insufficient. This can lead to pinholes and uneven thickness in the ceramic green sheet due to slight repellency or uneven application during coating, potentially worsening the yield of multilayer ceramic capacitors.

[0008] Patent documents 1 and 2, in particular, showed insufficient peelability and wettability of thin-layer ceramic green sheets, and there was a need for a further balance between easy peelability and good wettability. Furthermore, because coating compositions mainly containing organic solvents were used, there were problems with adverse effects on the human body due to contact with organic solvents and inhalation of vapors, as well as the burden on the global environment due to the release of organic solvent vapors into the atmosphere. Furthermore, the need to make the organic solvent drying equipment explosion-proof, resulting in high initial installation costs, and the significant energy required for operation, led to high CO2 emissions and a large environmental burden, which were significant challenges.

[0009] The release film described in Patent Document 3 has a release layer formed by in-line coating, but it was not intended for use in ceramic green sheet molding, and there were particular issues with the release properties of thin ceramic green sheets. Furthermore, although a phenyl group-containing crosslinking agent is used to improve the adhesion between the substrate and the release layer, no effect of the phenyl group on the release force has been observed, making it unsuitable as a release film exhibiting easy release properties.

[0010] The release film described in Patent Document 4 has a release layer formed from an aryl group-containing siloxane and a crosslinking agent. However, the invention of Patent Document 4 had a problem of high adverse effects on the human body and large environmental load during the manufacturing process. In addition, since it has a bulky substituent such as an aryl group, the curing reaction of the release layer is less likely to proceed due to steric hindrance, and as described in the Examples, when the coating composition is cured at 135°C, the curing heat amount of the release layer becomes insufficient, which may adversely affect the releasability. In order to further advance the curing of the release layer, it is necessary to cure the release layer at a higher temperature. However, in the invention of Patent Document 4, there is a risk of thermal deformation of the base film during the manufacturing process, so production at a relatively low temperature was required.

[0011] In the release film described in Patent Document 5, a release layer that achieves both releasability and wettability is formed by in-line coating. For example, technological development related to thin-layer ceramic green sheets is constantly advancing, and there is a demand for even lighter releasability and improved adaptability to thin-layer ceramic green sheets that are further enhanced compared to the time when Patent Document 5 was filed. In addition, there is a demand for further improving the base material adhesion of the release layer, and in the release film manufacturing process and the molding process of resin sheets such as ceramic green sheets, it is required to reduce adverse effects such as heavy peeling caused by the release layer falling off from the base film.

[0012] The present invention has been made against the background of the problems of such conventional techniques. That is, the present invention can reduce organic solvents that are harmful to the human body and adversely affect the environment, and achieves both light releasability and good wettability for thin-layer resin sheets, particularly thin-layer ceramic green sheets. A further object of the present invention is to provide a release film with improved adhesion between the base film and the release layer. [Means for Solving the Problems]

[0013] As a result of intensive studies to solve the above problems, the present inventors have found that the above object can be achieved by a release film having the following configuration, and have completed the present invention.

[0014] In other words, the present invention consists of the following configuration. [1] A release film having a release layer on at least one surface of a polyester film, wherein the release layer is a layer formed by reacting and solidifying an aqueous coating composition, The aqueous coating composition contains a silicone emulsion containing the following resins: (a) A first resin having a siloxane structure represented by structural formula 1,

[0015] [ka] (In structural formula 1, R1 is an alkenyl group having 2 to 8 carbon atoms, R2 is an alkyl group having 1 to 4 carbon atoms or an alkenyl group having 2 to 8 carbon atoms, and k is 1 to 50.) (b) A second resin having siloxane bonds in the main chain and containing a hydrogen group, and SiO 4 / 2 (c) A third resin containing silicone having Q units represented by Here, the first resin and / or the second resin further have a siloxane structure represented by the following structural formula 2.

[0016] [ka] (In structural formula 2, R3 is an alkyl group having 1 to 4 carbon atoms, Ar is an aryl group, and m is between 1 and 50.) Release film. [2] The aqueous coating composition further comprises (d) a fourth resin having alkenyl groups only at the molecular terminals, The release film according to (d) the fourth resin, wherein the number average molecular weight is 1,000 or more and less than 10,000 [1]. [3] The release film according to [1] or [2], wherein the second resin in (b) has the structure shown in the following chemical formula 2.

[0017] [ka] (In chemical formula 2, l is between 1 and 50, m is between 1 and 50, and n is between 0 and 5) [4](a) The number average molecular weight of the first resin is 1000 or more and less than 30000, (b) A release film according to any of [1] to [3], wherein the number average molecular weight of the second resin is 1000 or more and less than 5000. [5] The release film according to any one of [1] to [4], wherein the release film is formed by applying the aqueous coating composition to a base film before the crystal orientation is completed, stretching it in at least one direction, and then heat-treating it to complete the crystal orientation of the base film. [6] The release film according to any one of [1] to [5], wherein the polyester film has a surface layer that is substantially free of inorganic particles, and a release layer is formed on the surface layer. [7] The release film according to any one of [1] to [6], wherein the release film is a release film for manufacturing ceramic capacitors or resin sheets. [Effects of the Invention]

[0018] The release film of the present invention can improve the peelability and wettability of the release layer, and can further suppress the occurrence of defects in thin resin sheets, especially ceramic green sheets. Furthermore, it can reduce the harmful effects on human health and the environmental impact during the manufacturing process. This method allows for the formation of a release layer that does not risk deteriorating the adhesion between the base film and the release layer. [Modes for carrying out the invention]

[0019] Because the present invention has the features described herein, it can further solve the problems described below and achieve the effects described therein. In particular, it becomes possible to further improve both the ease of peeling and good wettability of thin-layer ceramic green sheets. Furthermore, compared to coating compositions that mainly contain organic solvents, it is possible to significantly reduce or substantially eliminate the amount of organic solvents. As a result, adverse effects on the human body from contact with organic solvents or inhalation of vapors, and the burden on the global environment from the release of organic solvent vapors into the atmosphere can be greatly reduced. Furthermore, there is no need to make the organic solvent drying equipment explosion-proof, and energy consumption during operation can be reduced compared to conventional manufacturing equipment. As a result, CO2 emissions can also be reduced, thus reducing the environmental impact.

[0020] Furthermore, the present invention makes it possible to provide a release film with superior peelability compared to release films manufactured by conventional in-line coating by using a silicone emulsion containing a silicone resin of a specific structure and composition. In particular, by using a release layer containing a cured silicone having Q units, a release film with excellent peelability and wettability can be obtained. In addition, by using a release layer containing a cured silicone further containing a siloxane structure having an aryl group, the ease of peeling is improved, and a release film with excellent adhesion to the substrate can be obtained.

[0021] The present invention will be described in detail below. The present invention relates to a release film having a release layer on at least one surface of a polyester film, wherein the release layer is a layer obtained by reacting and solidifying an aqueous coating composition, and the aqueous coating composition comprises a silicone emulsion, the silicone emulsion comprising the following: (a) A first resin having a siloxane structure represented by structural formula 1,

[0022] [ka] (In structural formula 1, R1 is an alkenyl group having 2 to 8 carbon atoms, R2 is an alkyl group having 1 to 4 carbon atoms or an alkenyl group having 2 to 8 carbon atoms, and k is 1 to 50.) (b) A second resin having siloxane bonds in the main chain and containing a hydrogen group, (c)SiO 4 / 2 (c) A third resin containing silicone having Q units represented by Here, the first resin and / or the second resin further have a siloxane structure represented by the following structural formula 2.

[0023] [ka] (In structural formula 2, R3 is an alkyl group having 1 to 4 carbon atoms, Ar is an aryl group, and m is between 1 and 50.)

[0024] The present invention, having such a configuration, can achieve both easy release and good wettability of the release layer, and can provide a uniform thickness without defects to a thin resin sheet, such as a thin ceramic green sheet, and can suppress defects such as pinholes. Furthermore, the present invention can achieve the following effects. In the present invention, since an aqueous coating composition with a significantly reduced amount of organic solvent compared to conventional methods, or an aqueous coating composition that substantially does not contain organic solvent, it is possible to manufacture a release film with less harm to the human body and less environmental burden, while suppressing the generation of CO2.

[0025] Furthermore, in one embodiment, the release film of the present invention can be made into a release layer with excellent adhesion to the substrate in addition to release properties and wettability by applying an aqueous coating composition containing a silicone emulsion having a predetermined composition in an in-line coating method. More specifically, by including a silicone emulsion containing a silicone having Q units, a structure in which the siloxane bond is expanded three-dimensionally can be obtained. As a result, a crosslinking reaction can proceed between the alkenyl groups in the molecule of the silicone having Q units and the silicone having hydrogen groups, resulting in a dense crosslinked structure. This allows for a release layer with excellent solvent resistance and easy release properties. Moreover, the inclusion of Q units reduces the hydrophobicity of the surface of the release layer, resulting in a release layer with excellent wettability. Furthermore, by including a silicone emulsion containing a silicone with a siloxane structure having an aryl group, adhesion can be improved through intermolecular interactions between the substrate film and the aryl groups in the release layer. In addition, by using bulky substituents such as aryl groups, the curing reaction of the release layer can be delayed, preventing the curing reaction from progressing during the stretching of the substrate film after coating composition application, and allowing the curing reaction to proceed only after the crystal orientation is complete. By preventing the curing reaction from progressing during the stretching of the substrate film, the stress caused by the difference between the stretchability of the substrate film and the stretchability of the coating composition can be reduced, thus preventing a decrease in substrate adhesion. In particular, the above effects can be achieved more effectively by including the first resin, the second resin, and the third resin in the present invention. The present invention can improve the adhesion of the release layer to the substrate by the reaction delaying effect of the aryl group. For example, in order to improve the adhesion of the release layer to the substrate, it is preferable that the curing reaction proceeds after the stretching of the substrate film. As will be described later, it is difficult to structurally determine the orientation and distribution of resin components in the release layer, as well as the distribution of substituents on the surface of the release layer that contribute to release properties. In this invention, however, we have found that "it is desirable for the curing reaction to proceed after the stretching of the base film."

[0026] (Polyester film) The polyester used as the base film is not particularly limited, and a film-formed polyester commonly used as a base film for release films can be used. Preferably, it is a crystalline linear saturated polyester composed of an aromatic dibasic acid component and a diol component, and more preferably, polyethylene terephthalate, polyethylene-2,6-naphthalate, polybutylene terephthalate, polytrimethylene terephthalate, or copolymers mainly composed of these resin components. In particular, a polyester film formed from polyethylene terephthalate is especially preferred. The polyethylene terephthalate preferably has 90 mol% or more, more preferably 95 mol% or more of repeating units of ethylene terephthalate, and may also have small amounts of other dicarboxylic acid components and diol components copolymerized. For example, from the viewpoint of cost, it is preferable to have one made only from terephthalic acid and ethylene glycol. In addition, known additives, such as antioxidants, light stabilizers, ultraviolet absorbers, and crystallizers, may be added within a range that does not hinder the effect of the release film of the present invention. The polyester film is preferably a biaxially oriented polyester film due to reasons such as high bidirectional elastic modulus.

[0027] The intrinsic viscosity of the polyester film described above is preferably 0.50 dl / g or more and 0.70 dl / g or less, and more preferably 0.52 dl / g or more and 0.62 dl / g or less. When the intrinsic viscosity is 0.50 dl / g or more, it is preferable because breakage does not occur frequently during the stretching process. Conversely, when it is 0.70 dl / g or less, it is preferable because the cutability is good when cutting to a predetermined product width and dimensional defects do not occur. In addition, it is preferable that the raw material pellets are thoroughly vacuum-dried.

[0028] In this specification, when the term "polyester film" is used, it may mean a polyester film having surface layer A and surface layer B (a laminated film).

[0029] The method for manufacturing the polyester film in the present invention is not particularly limited, and conventional methods can be used. For example, the polyester can be melted in an extruder, extruded into a film, cooled in a rotating cooling drum to obtain an unstretched film, and then biaxially stretched to obtain the film. The biaxially oriented film can be obtained by sequentially biaxially stretching a uniaxially oriented film in the longitudinal or transverse direction in the transverse or longitudinal direction, or by simultaneously biaxially stretching an unstretched film in the longitudinal and transverse directions.

[0030] In the present invention, it is preferable that the stretching temperature during stretching of the polyester film be above the secondary transition temperature (Tg) of the polyester. It is also preferable to stretch the film by 1 to 8 times, and particularly by 2 to 6 times, in both the longitudinal and transverse directions.

[0031] The polyester film described above preferably has a thickness of 12 μm to 50 μm, more preferably 15 μm to 38 μm, and more preferably 19 μm to 33 μm. A film thickness of 12 μm or more is preferable because it does not risk deformation due to heat during film production, processing, or molding. On the other hand, a film thickness of 50 μm or less is preferable because it does not result in an excessively large amount of film being discarded after use, thus reducing the environmental burden.

[0032] The polyester film substrate described above may be a single layer or a multilayer of two or more layers. For example, the substrate film may be a polyester film having a surface layer A that substantially does not contain particles with a particle size of 1.0 μm or larger, and a surface layer B that contains particles. Preferably, surface layer A substantially does not contain inorganic particles with a particle size of 1.0 μm or larger.

[0033] In this embodiment, the surface layer A may contain particles with a particle size of less than 1.0 μm and 1 nm or larger. By substantially excluding particles with a particle size of 1.0 μm or larger, such as inorganic particles, from the surface layer A, it is possible to reduce the transfer of the particle shape in the substrate to the resin sheet, which can cause defects.

[0034] In one embodiment, by not including particles with a particle size of less than 1.0 μm in the surface layer A, it is possible to more effectively suppress defects caused by the transfer of the particle shape in the substrate to the resin sheet. In one embodiment, the polyester film substrate is preferably a laminated film having a surface layer A that is substantially free of inorganic particles on at least one side. This makes it possible to more effectively suppress defects caused by the transfer of the particle shape in the substrate to the resin sheet. For example, a surface layer A that substantially does not contain particles with a particle size of less than 1.0 μm is preferably also substantially free of particles with a particle size of 1.0 μm or larger.

[0035] In this invention, "substantially free of particles" means, for example, in the case of inorganic particles smaller than 1.0 μm, that the content of inorganic elements is 50 ppm or less, preferably 10 ppm or less, and most preferably below the detection limit, when quantified by X-ray fluorescence analysis. This is because even without actively adding particles to the film, contaminants originating from foreign substances, or dirt adhering to the raw material resin or the lines and equipment in the film manufacturing process, may peel off and become mixed into the film. Furthermore, "substantially free of particles with a particle size of 1.0 μm or larger" means that the film actively does not contain particles with a particle size of 1.0 μm or larger.

[0036] In the case of a laminated polyester film consisting of two or more layers, it is preferable that the surface opposite to surface layer A, which substantially does not contain inorganic particles, has a surface layer B that may contain inorganic particles.

[0037] In terms of the lamination structure, if the layer on the side to which the release layer is applied is called layer A, the layer on the opposite side is called layer B, and the remaining core layer is called layer C, then the layer configuration in the thickness direction can be a laminated structure such as release layer / A / B or release layer / A / C / B. Naturally, layer C may consist of multiple layers. Furthermore, the surface layer B does not need to contain inorganic particles. In that case, it is preferable to provide a coating layer containing inorganic particles and a binder on the surface layer B in order to provide slipperiness for winding the film into a roll.

[0038] In the polyester film substrate of the present invention, the surface layer B that forms the opposite side of the surface to which the release layer is applied preferably contains inorganic particles from the viewpoint of the film's slipperiness and ease of air release, and it is particularly preferable to use silica particles and / or calcium carbonate particles. The inorganic particle content is preferably 5,000 ppm to 15,000 ppm in total in the surface layer B.

[0039] In this case, the average surface roughness (Sa) of the surface layer B film is preferably in the range of 1 nm to 40 nm. More preferably, it is in the range of 5 nm to 35 nm. When the total amount of silica particles and / or calcium carbonate particles is 5000 ppm or more and Sa is 1 nm or more, when the film is wound into a roll, air can be released uniformly, resulting in a good winding shape and good flatness, making it suitable for the manufacture of ultrathin ceramic green sheets. Furthermore, when the total amount of silica particles and / or calcium carbonate particles is 15000 ppm or less and Sa is 40 nm or less, lubricant aggregation is less likely to occur and no coarse protrusions are formed, resulting in stable quality during the manufacture of ultrathin ceramic green sheets, which is preferable.

[0040] In addition to silica and / or calcium carbonate, other inert inorganic particles and / or heat-resistant organic particles can be used as particles in the above-mentioned B layer, but silica particles and / or calcium carbonate particles are more preferable from the viewpoint of transparency and cost. Other inorganic particles that can be used include alumina-silica composite oxide particles and hydroxyapatite particles. Heat-resistant organic particles include cross-linked polyacrylic particles, cross-linked polystyrene particles and benzoguanamine particles. When silica particles are used, porous colloidal silica is preferred, and when calcium carbonate particles are used, light calcium carbonate surface-treated with a polyacrylic acid-based polymer compound is preferred from the viewpoint of preventing lubricant detachment.

[0041] The average particle size of the inorganic particles added to the surface layer B is preferably 0.1 μm or more and 2.0 μm or less, and particularly preferably 0.5 μm or more and 1.0 μm or less. An average particle size of 0.1 μm or more is preferable because it provides good slipperiness for the release film. Furthermore, an average particle size of 2.0 μm or less is preferable because it does not adversely affect the smoothness of the surface of the release layer, thus preventing the formation of pinholes in the ceramic green sheet.

[0042] In the surface layer A, which is the layer on the side where the release layer is provided, it is preferable not to use recycled materials or the like in order to prevent the inclusion of inorganic particles such as lubricants, from the viewpoint of reducing pinholes.

[0043] The thickness ratio of surface layer A, which is the layer on which the release layer is provided, is preferably 20% to 50% of the total thickness of the base film. If it is 20% or more, the influence of particles contained in surface layer B and the like from inside the film is less likely to occur, and it is easier for the average surface roughness Sa to satisfy the above range, which is preferable. If it is 50% or less of the total thickness of the base film, the proportion of recycled materials used in surface layer B can be increased, which is preferable because it reduces the environmental impact.

[0044] Furthermore, from an economic standpoint, layers other than the surface layer A (surface layer B or the aforementioned intermediate layer C) can use 50% to 90% by mass of recycled film scraps or PET bottles. Even in this case, it is preferable that the type, amount, particle size, and average surface roughness (Sa) of the lubricant contained in layer B satisfy the above range.

[0045] Furthermore, to improve the adhesion of release layers applied later, or to prevent static electricity, a coating layer may be provided on the surface of surface layer A and / or surface layer B before stretching or after uniaxial stretching during the film-forming process, and surface treatments may also be applied.

[0046] In one embodiment, the surface to which the aqueous coating composition is applied to form the release layer may be subjected to surface treatment or an easy-adhesion layer to enhance adhesion with the release layer. Examples of surface treatments include plasma treatment, corona discharge treatment, ultraviolet treatment, flame treatment, and electron beam / radiation treatment. Examples of easy-adhesion layers include a layer containing the same resin as the base film, and further containing an antistatic agent, pigment, surfactant, lubricant, antiblocking agent, etc. If an adhesion-enhancing agent such as a coupling agent is added to the aqueous coating composition, the release layer can have sufficient adhesion to the base film even without providing an easy-adhesion layer or the like.

[0047] (Release layer) In the present invention, the release layer is laminated on the surface layer A of the base film. In the present invention, the release layer is a layer obtained by reacting and solidifying an aqueous coating composition, the aqueous coating composition contains a silicone emulsion, and the silicone emulsion contains the following. (a) A first resin having a siloxane structure represented by structural formula 1,

[0048] [ka] (In structural formula 1, R1 is an alkenyl group having 2 to 8 carbon atoms, R2 is an alkyl group having 1 to 4 carbon atoms or an alkenyl group having 2 to 8 carbon atoms, and k is 1 to 50.) (b) A second resin having siloxane bonds in the main chain and containing a hydrogen group, (c)SiO 4 / 2 A third resin containing silicone having Q units represented by Here, the first resin and / or the second resin further have a siloxane structure represented by the following structural formula 2.

[0049] [ka] (In structural formula 2, R3 is an alkyl group having 1 to 4 carbon atoms, Ar is an aryl group, and m is between 1 and 50.)

[0050] The release layer possesses these characteristics, making it possible to provide a release film with excellent peelability and wettability, suppressing the occurrence of defects such as pinholes in resin sheets and ceramic green sheets, and enabling the formation of sheets with a uniform film thickness. Furthermore, it is possible to provide a release layer with excellent adhesion to the substrate, suppressing the detachment of the release layer during the manufacturing process of the release film and the manufacturing process of resin sheets and ceramic green sheets.

[0051] The aqueous coating composition in the present invention is a composition comprising a silicone emulsion. The silicone emulsion comprises (a) a first resin, (b) a second resin, and (c) a third resin, and in one embodiment, (d) a fourth resin. The silicone emulsion refers to a composition in which these water-insoluble resins are dispersed in water by a surfactant. The silicone emulsion contained in the aqueous coating composition may preferably consist of one type or two or more types. Furthermore, the silicone emulsion may contain only one of the selected resins (a) the first resin, (b) the second resin, (c) the third resin, and (d) the fourth resin, or it may contain two or more types, and all of (a), (b), (c), and (d) may be contained in one type of silicone emulsion.

[0052] The aqueous coating composition preferably contains substantially no organic solvents and uses water as the dispersion medium. By substantially omitting organic solvents, the stability of the silicone emulsion is improved, preventing changes in the composition of the aqueous coating composition due to emulsion breakdown, as well as aggregation and gelation of the resin in the silicone emulsion. The term "substantially free of organic solvents" means, for example, that the content is 10,000 ppm or less, preferably 5,000 ppm or less, more preferably 3,000 ppm or less, and most preferably below the detection limit, per the total weight of the aqueous coating composition. This is because even without intentionally using organic solvents, small amounts of organic solvents used in the polymerization process of the resin or the emulsification process of the emulsion may remain in the silicone emulsion.

[0053] ((a) First resin) The (a) first resin contained in the silicone emulsion preferably has the following structure.

[0054] [ka] (In structural formula 1, R1 is an alkenyl group having 2 to 8 carbon atoms, R2 is an alkyl group having 1 to 4 carbon atoms or an alkenyl group having 2 to 8 carbon atoms, and k is 1 to 50.) Having structural formula 1 allows for crosslinking reactions between the alkenyl group and the hydrogen group-containing silicone to proceed, resulting in a release layer with high crosslinking density and excellent solvent resistance, exhibiting easy peelability. Examples of alkenyl groups include vinyl, allyl, butenyl, pentenyl, and hexenyl groups, with vinyl being particularly preferred among these.

[0055] (a) As the first resin, for example, the structure represented by the following chemical formula 1 is an example.

[0056] [ka] In the above chemical formula 1, R1 is an alkenyl group having 2 to 8 carbon atoms, and R2 is an alkyl group having 1 to 4 carbon atoms or an alkenyl group having 2 to 8 carbon atoms. A vinyl group is preferred for R1, and a methyl group is preferred for R2. R2 may be the same or different; for example, a structure in which both terminal R2s are methyl groups and only the R2 in the side chain has a vinyl group is also preferred. k is a structure that contributes to the crosslinking reaction and is preferably 1 to 50. o is a structure that contributes to release properties and is preferably 1 to 500. A k of 1 or higher is preferred because the crosslinking reaction proceeds, and a k of 50 or lower is preferred because unreacted alkenyl groups are less likely to remain in the release layer, resulting in excellent release properties. A o of 1 or higher is preferred because release properties are exhibited, and a o of 500 or lower is preferred because there is no risk of the crosslinking density becoming low.

[0057] As illustrated by chemical formula 1, SiO 2 / 2 From the viewpoint of release properties, it is preferable that the silicone consists of D units represented by . Generally, silicones consisting of D units are preferable because the siloxane bonds tend to take on a helical structure, and in the case of polydimethylsiloxane, for example, both methyl groups present in the siloxane bonds are all arranged on the outside of the molecular chain, exhibiting hydrophobicity and forming a release layer with excellent release properties.

[0058] In one embodiment, the first resin contained in the silicone emulsion preferably further has the following structural formula 2.

[0059] [ka] (In structural formula 2, R3 is an alkyl group having 1 to 4 carbon atoms, Ar is an aryl group, and m is between 1 and 50.) As shown in structural formula 2, the presence of a bulky substituent, the aryl group, delays the curing reaction of the release layer, so that the curing of the release layer is completed when the crystal orientation of the base film is completed after stretching. The delayed curing reaction and the reduced curing of the release layer during stretching of the base film maintain the stretch-following ability of the coating composition, and there is no risk of a decrease in adhesion force due to the stress difference between the base film and the release layer, which is preferable. Furthermore, the resulting release layer is free from defects such as cracks that occur during stretching and has excellent peelability, which is also preferable.

[0060] As described above, structural formula 2 may be present in (a) the first resin. In another embodiment, (b) the second resin contained in the silicone emulsion described later may have the structure of structural formula 2. For example, it is preferable that (b) the second resin has an aryl group and (a) the first resin does not have an aryl group, as this makes it easier for (a) the first resin to localize on the surface side of the release layer during at least one step during stretching of the base film, drying of the coating composition, and curing, resulting in a release layer with excellent peelability.

[0061] Examples of aryl groups include phenyl, benzyl, tolyl, and xylyl groups, with phenyl being particularly preferred.

[0062] (a) The number average molecular weight of the first resin is preferably 1,000 or more and less than 30,000, more preferably 2,000 or more and less than 15,000, and even more preferably 3,000 or more and less than 10,000. When the number average molecular weight is 1,000 or more, it tends to localize on the surface of the release layer, making it easier to obtain sufficient release properties. On the other hand, when the number average molecular weight is less than 30,000, the emulsification properties of the silicone emulsion tend to be good, and uniform coating properties also tend to be good. Note that the number average molecular weight in this invention is 1 1H NMR and 29 This refers to the siloxane structure identified from the peaks observed in Si NMR, and calculated from the integral ratio of the peaks originating from each siloxane structure.

[0063] The content of the first resin in the silicone emulsion in the aqueous coating composition is preferably 5% by mass or more and 70% by mass or less, and more preferably 7% by mass or more and 60% by mass or less, when the total solid content weight in the coating composition is taken as 100. 10% by mass It is even more preferable that the amount is 55% by mass or less. If it is 5% by mass or more, the amount of (a) the first resin that exhibits release properties by localizing on the surface of the release layer is sufficient, resulting in excellent release properties, which is preferable. If it is 70% by mass or less, it is preferable because there is no risk of increased uncrosslinked components causing excessive peeling. The amount of silicone emulsion in the aqueous coating composition can be appropriately adjusted so that the amount of the first resin is within the above range. In this invention, the total solid content in the coating composition refers to the sum of the solid content of the first resin, the second resin, the third resin, and a fourth resin which may be added as needed.

[0064] ((b) Second resin) (b) The second resin, which has siloxane bonds in its main chain and contains hydrogen groups, may be any compound having siloxane bonds in its main chain, but polyorganosiloxanes having hydrogen groups at the terminals or side chains are preferred, and polydimethylsiloxanes are more preferred. The terminal silicon atoms may have hydrogen groups, but are preferably trialkylsilane structures such as trimethylsilane, and preferably have 2 to 50 hydrogen groups in one molecule. Having 2 or more hydrogen groups results in a release layer with high crosslink density when cured, exhibiting easy release properties.

[0065] In one embodiment, the second resin is exemplified by the structure shown in the following chemical formula 2.

[0066] [ka] In chemical formula 2, l is between 1 and 50, m is between 1 and 50, and n is between 0 and 5. When l is between 1 and 50, the crosslinking reaction between the alkenyl groups and hydrogen groups in the coating composition proceeds, resulting in a release layer with high crosslink density and excellent solvent resistance, which is preferable. When m is between 1 and 50, the bulky phenyl groups cause a reaction delay during the curing of the release layer, resulting in a release layer with good stretchability and excellent adhesion, which is preferable. Furthermore, the π electrons of the phenyl groups interact with the substrate film, resulting in even better adhesion, which is preferable. When n is between 0 and 5, the compatibility with (a) the first resin or (d) the fourth resin described later in the coating composition decreases, and (a) the first resin or (d) the fourth resin tends to localize on the surface side of the release layer. As a result, a release layer with excellent peelability is obtained, which is preferable.

[0067] In the present invention, (b) the number average molecular weight of the second resin is preferably 1,000 or more and less than 10,000, more preferably 1,000 or more and less than 5,000, and even more preferably 1,500 or more and less than 3,000. When the number average molecular weight is 1,000 or more, sufficient release properties are easily obtained. On the other hand, when the number average molecular weight is less than 10,000, the emulsification properties to the silicone emulsion tend to be good, and the coating uniformity also tends to be good. Furthermore, the crosslinking reaction proceeds more efficiently, the amount of residual hydrogen groups in the release layer decreases, and the release properties improve. Note that the number average molecular weight in the present invention is 1 1H NMR and 29 This refers to the siloxane structure identified from the peaks observed in Si NMR, and calculated from the integral ratio of the peaks originating from each siloxane structure.

[0068] The content of the second resin in the silicone emulsion in the aqueous coating composition is preferably 1% to 50% by mass, more preferably 3% to 40% by mass, and even more preferably 5% to 35% by mass, when the total solid content in the coating composition is taken as 100. A content of 1% or more by mass is preferable because the crosslinking reaction proceeds sufficiently. A content of 50% or less by mass is preferable because there is no risk of increased unreacted components causing severe peeling. The amount of the silicone emulsion in the aqueous coating composition can be appropriately adjusted so that the second resin falls within the above range. For example, when (b) the second resin contains an aryl group represented by Structural Formula 2, based on 100 of the total solid content in the coating composition, the content of the second resin is equal to or less than the content of (c) the third resin described later, and preferably, the content of the second resin is less than the content of (c) the third resin described later by 5 mass% or less. Satisfying such conditions is preferable because the crosslinking reaction proceeds sufficiently, and there is no risk of an increase in unreacted components that causes heavy release.

[0069] It is preferable that the structure containing the aryl group represented by Structural Formula 2 is contained in (b) the second resin rather than in (a) the first resin, because both adhesion and releasability are further enhanced. Specifically, when (b) the second resin acting as a crosslinking agent contains an aryl group, the compatibility with (a) the first resin decreases, and it is presumed that (a) tends to localize on the surface side of the release layer during stretching of the base film or during drying and curing of the coating composition, leading to improved releasability. On the other hand, in the present invention, the curing reaction by the aryl group contained in (b) the second resin acting as a crosslinking agent can be appropriately controlled, and the adhesion is also improved due to the increased interaction between the base film and the release layer. As described above, the present invention can solve the conventional problems that the curing reaction is excessively delayed, which requires time for curing the release layer, and further that the curing reaction proceeds rapidly to fail to obtain a desired release layer. In another embodiment, the structure containing the aryl group represented by Structural Formula 2 may be present in both (a) the first resin and (b) the second resin.

[0070] ((c) Third resin) The silicone emulsion in the aqueous coating composition of the present invention contains SiO 4 / 2(c) Preferably contains a third resin which includes a silicone having Q units represented by (c). The silicone emulsion containing the third resin is obtained by dispersing the silicone having the said structure in water as an emulsion or colloid. Any structure of a compound having a siloxane bond in the main chain is acceptable as the silicone having the said structure, but polyorganosiloxane having alkenyl groups in the terminals and / or side chains is preferred. Furthermore, a copolymer containing dialkylsiloxane units or alkylphenylsiloxane units is preferred because it is easy to adjust the amount of alkenyl groups in one molecule while exhibiting peelability. The terminal silicon atoms preferably have alkenyl groups, but they may also be trialkylsilane structures such as trimethylsilane.

[0071] SiO 4 / 2 Examples of silicones having the Q unit represented by the following chemical formula 3 include the structure shown below. R4 a R5 b SiO (4-a-b) / 2 ...(chemical formula 3) (In chemical formula 3, R4 is an alkenyl group having 2 to 8 carbon atoms, R5 is a monovalent saturated hydrocarbon group having 1 to 16 carbon atoms selected from alkyl or aryl groups, a is an integer between 0 and 3, and b is an integer between 0 and 3 such that a + b ≤ 3.) Here, chemical formula 3 represents a general formula, where a=0 and b=0 constitutes a Q unit, and (c) the third resin has this Q unit. Furthermore, a unit with a=1 or a=2 constitutes a siloxane structure having an alkenyl group, and a unit with b=2 constitutes a siloxane structure having only an alkyl or aryl group in its side chain, and these siloxane structures may also be present. Note that a unit with a+b=3 represents a siloxane structure having terminal groups.

[0072] Examples of C2-C8 alkenyl groups represented by R4 include vinyl, allyl, butenyl, pentenyl, and hexenyl groups, with vinyl being particularly preferred. Examples of alkyl groups represented by R5 include methyl, ethyl, propyl, and butyl groups, and examples of aryl groups include phenyl and tolyl groups. It is preferable that (c) contains a C2-C8 alkenyl group represented by R4 from the viewpoint of reactivity with the hydrogen group, and the fewer the number of carbon atoms, the less steric hindrance there is and the better the reactivity, which is preferable, with a C2 vinyl group being the most preferable. It is preferable that 50 mol% or more of the substituents of R5 are methyl groups from the viewpoint of easy peeling.

[0073] Silicones containing Q units can adopt a three-dimensionally expanded siloxane bond structure, allowing the alkenyl groups in the molecule to also exist in a three-dimensionally extended manner. Therefore, the reaction between the second resin (b), which is a silicone containing hydrogen groups, and the alkenyl groups in the molecule of (c) allows for the formation of a dense crosslinked structure, resulting in a release layer with excellent solvent resistance. Generally, the SiO contained in the release layer 2 / 2 When the proportion of D units increases, the siloxane bond is more likely to adopt a helical structure. For example, in the case of polydimethylsiloxane, both methyl groups present in the siloxane bond are all aligned on the outside of the molecular chain, resulting in hydrophobicity. On the other hand, when the proportion of Q units in the release layer increases, the helical structure of the siloxane bond formed from D units breaks down, reducing hydrophobicity. Although not specifically limited by theory, by using a release layer containing silicone with Q units, it is possible to achieve both easy release due to increased crosslinking density and reduced hydrophobicity due to the breakdown of the siloxane bond helical structure, i.e., excellent wettability.

[0074] In the silicone emulsion in the aqueous coating composition, (c) the content of the third resin is 10% by mass or more and 70% by mass or less, more preferably 15% by mass or more and 65% by mass or less, and 20% by mass or more, when the total solid content in the coating composition is taken as 100. 60% by massIt is even more preferable that the amount is 10% by mass or more, as this is preferable because the helical structure of the silicone consisting of D units contained in the release layer is disrupted by the silicone having Q units, resulting in a release layer with excellent wettability. 70% by mass The following is preferable because the silicone having Q units does not excessively disrupt the helical structure of the silicone consisting of D units contained in the release layer, resulting in a release layer with excellent release properties.

[0075] The amount of Si atoms contained in Q units is SiO 4 / 2 The Si content in the silicone having the Q unit represented by is 0.05 to 60 mol%, preferably 0.1 to 55 mol%, and more preferably 1.0 to 50 mol%, relative to the total Si atoms in the silicone. When the Si atom content in the Q unit is 0.05 mol% or more, it is preferable because it allows for a sufficiently three-dimensionally expanded siloxane bond structure, resulting in an effect of increasing crosslink density. When it is 60 mol% or less, it is preferable because it does not impart excessive wettability and risk causing excessive delamination. Furthermore, (b) from the viewpoint of forming a dense crosslinked structure through reaction with the second resin, the Si atom content in the siloxane structure having an alkenyl group is SiO 4 / 2 The amount of the total Si atoms in the silicone having Q units represented by is preferably 0.05 to 30 mol%, and more preferably 1.0 to 20 mol%.

[0076] It is preferable that the silicone having Q units is solid at room temperature. The fact that the silicone having Q units is solid at room temperature means that there are many Q units in the molecule as continuous bonds, resulting in a silicone with a rigid molecular framework and physical properties similar to glass. It is preferable to use a release layer containing such a silicone with a rigid molecular framework because the elastic modulus of the release layer is increased, making it less likely to deform when peeling off the object to be peeled, such as a ceramic green sheet, and resulting in a release layer that exhibits easy peelability.

[0077] As described above, silicones containing Q units have a rigid molecular skeleton and therefore have poor stretchability, which can lead to cracking of the coating film and a decrease in adhesion to the substrate due to stretching. However, in the present invention, a silicone emulsion containing the aryl group shown in structural formula 2 is used as the coating composition. Due to its reaction delay effect, the crosslinking reaction is less likely to proceed when the substrate film is stretched, and a release layer can be formed without adhesion or coating defects, even with a release layer containing silicone containing Q units.

[0078] (d) Fourth resin In the aqueous coating composition of the present invention, a release film can be obtained that achieves both release properties and wettability, as well as excellent adhesion to the substrate, by including (d) a fourth resin having alkenyl groups only at both ends of the silicone emulsion.

[0079] (d) Examples of the fourth resin include those shown in Chemical Formula 4 below.

[0080] [ka] In chemical formula 4, R1 is an alkenyl group having 2 to 8 carbon atoms, and p is between 1 and 300. Since p is within the above range, it is preferable because it exhibits excellent peelability. (d) Because the fourth resin has alkenyl groups only at both ends, the D units are linked in a linear structure, so the helical structure is not broken by the crosslinking reaction, and it exhibits better peelability than (a) the first resin. However, in an embodiment containing a fourth resin having alkenyl groups only at the molecular ends, the amount of alkenyl groups is less than in (a) the first resin, so the crosslinking density may decrease, but at the same time, the side chains present in the release layer have alkenyl groups. do (a) By crosslinking with the first resin, deterioration of solvent resistance can be prevented. Although not particularly limited by theory, the release film of the present invention has alkenyl groups only at both ends of the surface layer of the release layer. do (d) The fourth resin is localized and has an alkenyl group in its side chain (a) via the first resin, Q units and alkenyl groups (c) Third resinBy forming a release layer bonded to it, a release layer with excellent peelability can be achieved.

[0081] In the present invention, the number-average molecular weight of the fourth resin contained in the silicone emulsion is preferably 1,000 or more and less than 10,000, more preferably 1,000 or more and less than 5,000, and even more preferably 1,500 or more and less than 3,000. When the number-average molecular weight is 1,000 or more, sufficient release properties are easily obtained. On the other hand, when the number-average molecular weight is less than 10,000, the emulsification properties to the silicone emulsion tend to be good, and coating uniformity also tends to be good. Furthermore, the crosslinking reaction proceeds more efficiently, the amount of residual hydrogen groups in the release layer decreases, and the release properties improve. Note that the number-average molecular weight in the present invention is 1 1H NMR and 29 This refers to the siloxane structure identified from the peaks observed in Si NMR, and calculated from the integral ratio of the peaks originating from each siloxane structure.

[0082] The content of the fourth resin in the silicone emulsion in the aqueous coating composition is preferably 1% to 50% by mass, more preferably 5% to 40% by mass, and even more preferably 10% to 35% by mass, when the total solid content in the coating composition is set to 100. A content of 1% by mass or more is preferable because it can be localized on the surface of the release layer and exhibit release properties. A content of 50% by mass or less is preferable because it does not reduce the crosslinking density of the release layer and may cause excessive peeling. The amount of silicone emulsion in the aqueous coating composition can be appropriately adjusted so that the fourth resin falls within the above range.

[0083] (Other ingredients) The aqueous coating composition of the present invention preferably contains a surfactant. The inclusion of a surfactant is preferable because it provides excellent coatability when applying the coating composition to a polyester film, which is the base film, and there is no risk of coating defects such as repelling. Furthermore, it is preferable because it does not impair the stability of the emulsion present in the coating composition, there is no risk of aggregates or gels of the coating composition being mixed into the release layer, and the occurrence of unevenness and uneven coating in the release layer is suppressed.

[0084] The aqueous coating composition of the present invention must contain a platinum-based catalyst to carry out an addition reaction between a silicone having an alkenyl group and a silicone having a hydrogen group. Known platinum-based catalysts can be used, such as platinum chloride and chloroplatinic acid. Considering dispersibility in silicone, a 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum(0) complex (Karstedt catalyst) may be used as the platinum-based catalyst, and uniform dispersion can be ensured by dispersing it simultaneously when emulsifying the silicone.

[0085] The amount of platinum-based catalyst is preferably in the range of 10 to 800 ppm by weight of platinum element relative to the total amount of solid content forming the release layer. This range allows for sufficient curing of the silicone, suppresses the formation of aggregates, and yields a release film with excellent smoothness. A weight ratio of platinum element of 800 ppm or less is preferable because it accelerates the addition reaction between alkenyl groups and hydrogen groups, thus preventing the formation of silicone aggregates. The amount of platinum-based catalyst is more preferably 600 ppm or less, even more preferably 500 ppm or less, and most preferably 300 ppm or less. Furthermore, a concentration of 10 ppm or more is preferable because it allows the silicone addition reaction to proceed efficiently, resulting in sufficient curing of the release layer and exhibiting easy peelability.

[0086] The aqueous coating composition of the present invention preferably contains a reaction inhibitor to suppress the activity of the platinum-based catalyst at room temperature. The content of the reaction inhibitor is preferably 5 to 1000 ppm, more preferably 10 to 700 ppm, and preferably 20 to 500 ppm, based on the total weight of the aqueous coating composition. A content of 5 ppm or more is preferable as it provides sufficient effect in suppressing the activity of the platinum-based catalyst. A content of 1000 ppm or less is preferable as it does not pose a risk of contamination of the inside of the oven by reaction inhibitor volatilizing during heat treatment.

[0087] The aqueous coating composition of the present invention may further contain adhesion promoters, colorants, UV absorbers, particles, etc., to the extent that it does not impair the objectives of the present invention.

[0088] (Other characteristics of the release layer) In the present invention, the thickness of the release layer after drying and curing is preferably 0.001 to 0.2 μm, and more preferably 0.005 to 0.1 μm. A thickness of 0.001 μm or more is preferable because it provides a release layer with excellent peelability. A thickness of 0.2 μm or less is preferable because it eliminates the need to increase the solid content concentration or application amount of the release layer component of the aqueous coating composition, and provides excellent coatability when applied to a substrate film.

[0089] (Method of manufacturing release film) In one embodiment, the release layer is formed on at least one surface of the base film. The release layer is formed by applying an aqueous coating composition to the base film, followed by heat drying, during which the components of the aqueous coating composition react and solidify. Preferably, the release layer is formed during the film manufacturing process.

[0090] When applying an aqueous coating composition onto a substrate film, the solid content concentration is preferably 20% by mass or less, and more preferably 1% by mass or more and 10% by mass or less, based on the components in the aqueous coating composition, i.e., the solid content. When the solid content concentration of the release layer component in the aqueous coating composition is above the lower limit, the film-forming properties tend to be good. Also, when the solid content concentration is below the upper limit, the stability of the aqueous coating composition and the appearance of the release layer tend to be good. Water is preferably used as the aqueous solvent to adjust the solid content concentration.

[0091] The aqueous coating composition applied to the base film to form a release layer can be carried out at any stage, but it is preferable to carry it out during the polyester film manufacturing process, and more preferably to apply it to the polyester film before orientation crystallization is complete. After that, the film can be stretched in at least one direction and then heat-treated to complete the crystal orientation.

[0092] Here, polyester films before crystal orientation is complete include unstretched films, uniaxially oriented films in which an unstretched film is oriented in either the longitudinal direction (hereinafter sometimes referred to as the continuous film formation direction, longitudinal direction, or MD direction) or the transverse direction (hereinafter sometimes referred to as the direction perpendicular to the longitudinal direction, width direction, or TD direction), and films that have been low-magnification stretched and oriented in both the longitudinal and transverse directions (biaxially oriented films before they are finally re-stretched in the longitudinal or transverse direction to complete the orientation crystallization).

[0093] In particular, so-called in-line coating is preferred, in which an aqueous coating composition is applied to an unstretched film or a uniaxially oriented film, and then longitudinally and / or transversely stretched and heat-set. The release layer may be dried by the stretching or heat-setting process after application, and a drying process may be added as needed. Furthermore, when curing the composition using a catalyst to obtain a cured film, curing can be achieved by the stretching or heat-setting process, and a curing process may be added as needed.

[0094] Regarding the release layer in the present invention, the specifications "an aqueous coating composition is applied to an unstretched film or a uniaxially oriented film, and then longitudinally and / or transversely stretched and heat-set" and "the release layer is formed by an in-line coating method" specify the structure of the object by the manufacturing method. However, circumstances exist such as the following where it is impossible or impractical to directly specify the object by its structure or properties.

[0095] In the present invention, the aqueous coating composition that forms the release layer is presumed to undergo longitudinal and / or transverse stretching together with the coated film, causing the first resin, second resin, third resin, and optionally fourth resin contained in the silicone emulsion to become oriented and interact with each other. For example, it is presumed that during the drying process of water in the aqueous coating composition, during the stretching of the substrate film, or during the curing of the release layer, differences in compatibility and molecular weight between the first resin, the second resin, and the third resin make it easier for (a) to localize on the surface side of the release layer, thereby improving peelability. On the other hand, in the present invention, the curing reaction by the aryl group contained in the second resin (b), which acts as a crosslinking agent, can be appropriately controlled, and the adhesion between the substrate film and the release layer is also improved by increasing the interaction between them. However, it is difficult to structurally determine the orientation and distribution of resin components in the release layer, as well as the distribution of substituents on the surface of the release layer that contribute to release properties.

[0096] Furthermore, considering the measurement technology available at the time of filing the present invention, it is impossible or impractical to measure the structure or properties of the release film of the present invention and analyze and specify its physical properties based on these results. Therefore, at the time of filing the present invention, it was impossible or impractical to directly specify the object in question based on its structure or properties.

[0097] Any known coating method can be applied to the aqueous coating composition. For example, roll coating, gravure coating, roll brushing, spray coating, air knife coating, impregnation, curtain coating, etc., can be used individually or in combination.

[0098] In one embodiment, the manufacturing method of the present invention provides a method for manufacturing a release film for manufacturing a resin sheet and a multilayer ceramic capacitor.

[0099] (Resin sheet) The resin sheet in the present invention is not particularly limited as long as it is a sheet molded on the side of the release layer opposite to the substrate. Examples include a resin sheet formed by curing a resin sheet forming composition containing a resin component and a crosslinking agent, or a resin sheet formed by melt film formation or solution film formation using an organic component with film-forming properties. In one embodiment, the release film of the present invention is a release film for molding a resin sheet containing an inorganic compound. Examples of inorganic compounds include metal particles, metal oxides, and minerals, such as calcium carbonate, silica particles, aluminum particles, and barium titanate particles. Because the present invention has a highly smooth release layer, even when these inorganic compounds are included in the resin sheet, it is possible to suppress defects that may be caused by the inorganic compounds, such as damage to the resin sheet and difficulty in peeling the resin sheet from the release layer. The resin components forming the resin sheet can be appropriately selected depending on the application. In one embodiment, the resin sheet containing an inorganic compound is a ceramic green sheet. For example, the ceramic green sheet may contain barium titanate as the inorganic compound. Furthermore, the resin component may include, for example, a polyvinyl butyral resin.

[0100] (Ceramic green sheet and ceramic capacitor) Generally, a multilayer ceramic capacitor has a rectangular parallelepiped ceramic body. Inside the ceramic body, first internal electrodes and second internal electrodes are alternately arranged along the thickness direction. The first internal electrodes are exposed on the first end face of the ceramic body. A first external electrode is provided on the first end face. The first internal electrodes are electrically connected to the first external electrode at the first end face. The second internal electrodes are exposed on the second end face of the ceramic body. A second external electrode is provided on the second end face. The second internal electrodes are electrically connected to the second external electrode at the second end face.

[0101] In one embodiment, the release film of the present invention is a release film for manufacturing ceramic green sheets and is used to manufacture such multilayer ceramic capacitors. For example, using the release film for manufacturing ceramic green sheets of the present invention, a ceramic green sheet can be manufactured as follows: First, the release film of the present invention is used as a carrier film, and a ceramic slurry for forming a ceramic body is applied and dried. A conductive layer for forming a first or second internal electrode is printed on the applied and dried ceramic green sheet. A mother laminate is obtained by appropriately laminating the ceramic green sheet, the ceramic green sheet with the conductive layer for forming the first internal electrode printed on it, and the ceramic green sheet with the conductive layer for forming the second internal electrode printed on it, and pressing them. The mother laminate is divided into multiple parts to produce raw ceramic bodies. Ceramic bodies are obtained by firing the raw ceramic bodies. A multilayer ceramic capacitor can then be completed by forming the first and second external electrodes. [Examples]

[0102] The present invention will be described in more detail below using examples, but the present invention is not limited in any way by these examples. The characteristic values ​​used in the present invention were evaluated using the following method.

[0103] (Release layer thickness) After cutting the release film into triangular pieces, a 2 nm thick Pt (platinum) layer was formed on the surface of the release layer by coating. The obtained samples were fixed in a multiaxial embedding capsule and embedded using epoxy resin. Using a microtome ULTRACUT-S, the film was sliced ​​perpendicular to the plane direction to obtain ultrathin samples with a height of 50 nm. Next, the obtained ultrathin samples were placed on a grid and vapor-stained with 2% osmium acid at 60°C for 2 hours. Using the ultrathin samples after vapor staining, the film cross-section was observed with a transmission electron microscope LEM-2000 under an acceleration voltage of 100 kV, and the thickness of the release layer was measured. Measurements were performed at 10 arbitrary points, and the average value was taken as the thickness of the release layer.

[0104] (Uniformity of the release layer application) The release film obtained by winding it into a roll was unwound and cut into A4 size sheets. The number of aggregated coating defects (number per A4 sheet) was compared when the release layer surface was visually observed using fluorescent and halogen lights, and evaluated according to the following criteria. ◎: No application defects ○: 1-2 application defects △: 3-5 application defects ×: Six or more coating defects

[0105] (Adhesion to substrate) The release surface of the release film was rubbed 10 times with a thumb under a load of approximately 500 gf. To check for silicone detachment in that area, adhesive tape (manufactured by Nitto Denko Corporation, product name "No. 31B Tape") was applied, and the peeling state of the adhesive tape was checked and evaluated according to the following criteria. ○: No change in peeling when removing adhesive tape. △: Slight variation in peeling when removing adhesive tape. ×: Changes in peeling occurred when removing the adhesive tape.

[0106] (Surface free energy) For samples that had been conditioned for 24 hours under conditions of 23°C and 50% RH, the static contact angle was measured using a contact angle meter (DMo-501, manufactured by Kyowa Interface Chemical Co., Ltd.) after adding water and allowing it to stand for 30 seconds. Similarly, the static contact angles of ethylene glycol and methylene iodide were measured, and the following simultaneous equations relating to the surface tension components of the release layer were constructed using the surface tension components of each liquid listed below (the measured solutions for water, ethylene glycol, and methylene iodide are designated as 1, 2, and 3 respectively; γLD is the dispersion force component of the liquid, γLP is the polar force component of the liquid, γLH is the hydrogen bonding component of the liquid, γL is the sum of the surface tension components in the liquid, γSD is the dispersion force component of the release layer, γSP is the polar force component of the release layer, and γSH is the hydrogen bonding component of the release layer. Also, θ represents the contact angle). (γSD·γLD1) 1 / 2 +(γSP·γLP1) 1 / 2 +(γSH·γLH1) 1 / 2 =γL1(1+cosθ1) / 2 (γSD·γLD2) 1 / 2 +(γSP·γLP2) 1 / 2 +(γSH·γLH2) 1 / 2 =γL2(1+cosθ2) / 2 (γSD·γLD3) 1 / 2 +(γSP·γLP3) 1 / 2 +(γSH·γLH3) 1 / 2 =γL3(1+cosθ3) / 2 The γLD, γLP, γLH, and γL values ​​for water, ethylene glycol, and methylene iodide are shown in Table 1.

[0107] [Table 1] Next, the surface free energy γS of the release layer surface was calculated using the following formula based on the values ​​of γSD, γSP, and γSH obtained above. γS = γSD + γSP + γSH

[0108] (Ceramic sheet peelability) Slurry composition I, consisting of the materials listed below, was stirred and mixed for 10 minutes, and then dispersed using a bead mill with 0.5 mm diameter zirconia beads for 10 minutes to obtain a primary dispersion. Subsequently, slurry composition II, consisting of the materials listed below, was added to the primary dispersion in a ratio of (slurry composition I):(slurry composition II) = 3.4:1.0, and secondary dispersion was performed using a bead mill with 0.5 mm diameter zirconia beads for 10 minutes to obtain a ceramic slurry. (Slurry composition I) Toluene 22.3 parts by mass Ethanol 18.3 parts by mass Barium titanate (average particle size 100 nm) 57.5 parts by mass Homogenol L-18 (manufactured by Kao Corporation) 1.9 parts by mass (Slurry Composition II) Toluene 39.6 parts by mass Ethanol 39.6 parts by mass Dioctyl phthalate 3.3 parts by mass Polyvinyl butyral (Sekisui Chemical Co., Ltd., S-Rec BM-S) 16.3 parts by mass 1-Ethyl-3-methylimidazolium ethyl sulfate 0.5 parts by mass Next, the release surface of the obtained release film sample was coated using an applicator so that the slurry after drying was 2.0 μm thick, and dried at 60°C for 1 minute to obtain a release film with a ceramic green sheet. The obtained release film with a ceramic green sheet was destaticized using a static eliminator (Keyence Corporation, SJ-F020), and then peeled using a peel tester (Kyowa Interface Science Co., Ltd., VPA-3, load cell load 0.1N) at a peel angle of 90 degrees, peel temperature of 60°C, and peel speed of 0.3 m / min. For peeling, double-sided adhesive tape (Nitto Denko Corporation, NO.535A) was attached to a SUS plate attached to the peel tester, and the release film was fixed on top of it with the release film side adhering to the double-sided tape, and peeled by pulling the ceramic green sheet side. From the obtained measured values, the average value of the peel force for peel distances of 20 mm to 70 mm was calculated and this value was defined as the peel force. A total of 5 measurements were performed, and the average value of the peel force was adopted for evaluation. The peeling force values ​​obtained were evaluated according to the following criteria. ◎: Less than 1.0 mN / mm ○: Less than 1.5 mN / mm △: Less than 2.0 mN / mm ×: 2.0 mN / mm or higher

[0109] (Silicone emulsion: a-1) Using an emulsifying device capable of stirring the entire contents of a container (manufactured by N.P. Lab Co., Ltd., device name "Ultra Planetary Mixer"), a raw material consisting of 98% by mass of alkenyl group-containing silicone (o=125, k=4, number average molecular weight 9756) represented by chemical formula (a-1) and 2% by mass of polyoxyethylene lauryl ether (manufactured by Kao Corporation, product name "Emulgen 109P") as a surfactant was mechanically emulsified in an aqueous medium to obtain a silicone emulsion (a-1) with a solid content of 20% by mass. Furthermore, the emulsion particle size was adjusted by adjusting the stirring speed and stirring time during emulsification.

[0110] [ka]

[0111] (Silicone emulsion: a-2) Using an emulsifying device capable of stirring the entire contents of a container (manufactured by N.P. Lab Co., Ltd., device name "Ultra Planetary Mixer"), a raw material consisting of 98% by mass of alkenyl and phenyl group-containing silicone (o=115, k=4, m=5, number average molecular weight 9696) represented by chemical formula (a-2) and 2% by mass of polyoxyethylene lauryl ether (manufactured by Kao Corporation, product name "Emulgen 109P") as a surfactant was mechanically emulsified in an aqueous medium to obtain a silicone emulsion (a-2) with a solid content of 20% by mass. Furthermore, the emulsion particle size was adjusted by adjusting the stirring speed and stirring time during emulsification.

[0112] [ka]

[0113] (Silicone emulsion: b-1) Using an emulsifying device capable of stirring the entire contents of a container (manufactured by N.P. Lab Co., Ltd., device name "Ultra Planetary Mixer"), a raw material consisting of 98% by mass of hydrogen group and phenyl group-containing silicone (l=21, m=8, n=4, number average molecular weight 2806) represented by chemical formula (b-1) and 2% by mass of polyoxyethylene lauryl ether (manufactured by Kao Corporation, product name "Emulgen 109P") as a surfactant was mechanically emulsified in an aqueous medium to obtain a silicone emulsion (b-1) with a solid content of 20% by mass. Furthermore, the emulsion particle size was adjusted by adjusting the stirring speed and stirring time during emulsification.

[0114] [ka]

[0115] (Silicone emulsion: b-2) Using an emulsifying device capable of stirring the entire contents of a container (manufactured by N.P. Lab Co., Ltd., device name "Ultra Planetary Mixer"), a raw material consisting of 98% by mass of hydrogen group and phenyl group-containing silicone (l=40, n=40, number average molecular weight 5522) represented by chemical formula (b-2) and 2% by mass of polyoxyethylene lauryl ether (manufactured by Kao Corporation, product name "Emulgen 109P") as a surfactant was mechanically emulsified in an aqueous medium to obtain a silicone emulsion (b-2) with a solid content of 20% by mass. Furthermore, the emulsion particle size was adjusted by adjusting the stirring speed and stirring time during emulsification.

[0116] [ka]

[0117] (Silicone emulsion: c-1) Using an emulsifying device that can agitate the entire contents of the container (manufactured by N.P. Lab Co., Ltd., device name "Ultra Planetary Mixer"), SiO 4 / 2A raw material consisting of 98% by mass of silicone having Q units represented by SiO and 2% by mass of polyoxyethylene lauryl ether (product name "Emulgen 109P" manufactured by Kao Corporation) as a surfactant was mechanically emulsified in an aqueous medium to obtain a silicone emulsion (c-1) containing 20% ​​by mass of silicone having Q units. At this time, SiO 4 / 2 Silicones having the Q unit represented by the general formula chemical formula 3 are shown, where R4 is a vinyl group and R5 is a methyl group, and only one vinyl group is bonded to the Si atom to which the vinyl group is directly bonded, SiO 4 / 2 In the silicone having the Q unit represented by , the content of Si atoms bonded to vinyl groups relative to the total Si atoms was 5 mol%, and the content of Si atoms contained in the Q unit was 40 mol%. That is, in chemical formula 3, R4 is a vinyl group, R5 is a methyl group, and it had 5 mol% of a siloxane structure with a=1, b=1, 40 mol% of a siloxane structure with a=0, b=0, and 55 mol% of a siloxane structure with R5 being a methyl group, a=0, b=2 or 3. The emulsion particle size was adjusted by controlling the stirring speed and stirring time during emulsification. Furthermore, the number-average molecular weight was adjusted to 200,000. R4 a R5 b SiO (4-a-b) / 2 ...(chemical formula 3) (In chemical formula 3, R4 is an alkenyl group having 2 to 8 carbon atoms, R5 is a monovalent saturated hydrocarbon group having 1 to 16 carbon atoms selected from alkyl or aryl groups, a is an integer between 0 and 3, and b is an integer between 0 and 3 such that a + b ≤ 3.)

[0118] (Silicone emulsion: d-1) Using an emulsifying device capable of stirring the entire contents of a container (manufactured by N.P. Lab Co., Ltd., device name "Ultra Planetary Mixer"), a raw material consisting of 98% by mass of silicone (p=23, number average molecular weight 1888) having alkenyl groups only at both ends as shown in chemical formula (d-1) and 2% by mass of polyoxyethylene lauryl ether (manufactured by Kao Corporation, product name "Emulgen 109P") as a surfactant was mechanically emulsified in an aqueous medium to obtain a silicone emulsion (d-1) with a solid content of 20% by mass. Furthermore, the emulsion particle size was adjusted by adjusting the stirring speed and stirring time during emulsification.

[0119] [ka]

[0120] <Example 1 of manufacturing an aqueous coating composition> Aqueous coating compositions were obtained by mixing silicone emulsion (a-1), silicone emulsion (b-1), silicone emulsion (c-1), silicone emulsion (d-1), and water in the proportions shown in Table 2, so that the solid content concentration was 4% by mass. At this time, 0.02% by mass of a platinum-based catalyst (manufactured by Shin-Etsu Chemical Co., Ltd., product name: CAT-PM-10A) and 150 ppm of a crosslinking reaction inhibitor (1-ethynylcyclohexanol) were mixed with the total weight of the aqueous coating composition.

[0121] <Examples 2-8 of the production of aqueous coating compositions> An aqueous coating composition was obtained in the same manner as in Production Example 1, except that the types and ratios were mixed as shown in Table 2.

[0122] <Example 1> Polyethylene terephthalate ([η]=0.63 dl / g, Tg=78℃) containing 0.25 mass% of calcium carbonate particles with an average particle size of 0.6 μm was melted in an extruder, passed through a filter with a filtration accuracy of 10 μm, extruded from a die, and cooled in a cooling drum by conventional methods to obtain an unstretched film. Next, it was stretched 3.2 times in the longitudinal direction at 80℃, and then the aqueous coating composition obtained in Production Example 1 was uniformly applied to one surface of the polyester film using a roll coater. Next, this coated film was dried at 115℃, stretched 4.0 times in the transverse direction at 145℃, and then heat-set at 230℃ for about 10 seconds to complete the crystal orientation of the base film. After that, it was wound into a roll to obtain a roll of release film (thickness 25 μm) having the release layer shown in Table 2. The release film was unwound from the obtained release film roll and cut into A4 size samples, and the evaluations described in Table 2 were performed using these samples. The amount of aqueous coating composition applied was such that the thickness of the release layer after curing and stretching was as shown in Table 2.

[0123] <Examples 2-6> A release film was obtained in the same manner as in Example 1, except that the aqueous coating composition obtained in the manufacturing example described in Table 2 was used.

[0124] <Comparative Examples 1-2> A release film was obtained in the same manner as in Example 1, except that the aqueous coating composition obtained in the manufacturing example described in Table 2 was used.

[0125] <Reference example 1> A 25 μm thick biaxially oriented polyester film (Toyobo Co., Ltd., Toyobo Ester Film E5100) was coated with the aqueous coating composition obtained in Production Example 1 using reverse gravure printing so that the release layer thickness after drying was 0.1 μm. After drying at 135°C for 60 seconds, the film was wound into a roll to obtain a release film roll. The release film was unwound from the obtained release film roll and cut into A4 size samples, which were then used for the evaluations described in Table 2.

[0126] As shown in Table 2, in Examples 1 to 6, release films with excellent coating uniformity of the release layer, substrate adhesion, and ceramic sheet peelability were obtained. Furthermore, the surface free energy of the release layer was 17 mN / m or higher, and release films with excellent wettability of ceramic slurries were obtained. In contrast, in Comparative Example 1, a release layer was formed using an aqueous coating composition that did not contain silicone having (c)Q units, resulting in insufficient peelability of the ceramic sheet. In Comparative Example 2, a release layer was formed using an aqueous coating composition that did not contain a siloxane structure having an aryl group, resulting in poor stretchability of the coating composition and poor adhesion to the substrate. Furthermore, the peelability of the ceramic sheet was also poor. On the other hand, in Reference Example 1, the release layer was formed using an offline coating method, resulting in insufficient drying and curing heat for the aqueous coating composition. This caused deformation of the release layer when it was wound into a roll. Consequently, the uniformity of the release layer's application, adhesion to the substrate, and peelability of the ceramic sheet were poor. Furthermore, there was a large variation in the contact angle values ​​of the release layer, making it difficult to accurately measure the surface free energy.

[0127] [Table 2] [Industrial applicability]

[0128] The release film of the present invention has high peelability and wettability of the release layer, and high adhesion between the base film and the release layer, making it difficult for the release layer to detach. Therefore, it can suppress the occurrence of defects when molding thin resin sheets, especially ceramic green sheets.

Claims

1. A release film having a release layer on at least one surface of a polyester film, The aforementioned release layer is a layer formed by reacting and solidifying an aqueous coating composition. The aqueous coating composition contains a silicone emulsion containing the following resins: (a) A first resin having a siloxane structure represented by structural formula 1, 【Chemistry 1】 (In structural formula 1, R1 is an alkenyl group having 2 to 8 carbon atoms, R2 is an alkyl group having 1 to 4 carbon atoms or an alkenyl group having 2 to 8 carbon atoms, and k is 1 to 50.) (b) A second resin having siloxane bonds in the main chain and containing a hydrogen group, and SiO 4/2 (c) A third resin containing silicone having Q units represented by Here, the first resin and / or the second resin further have a siloxane structure represented by the following structural formula 2, 【Chemistry 2】 (In structural formula 2, R3 is an alkyl group having 1 to 4 carbon atoms, Ar is an aryl group, and m is between 1 and 50.) The silicone emulsion contained in the aqueous coating composition further comprises (d) a fourth resin having alkenyl groups only at the molecular ends, (d) The number average molecular weight of the fourth resin is 1,000 or more and less than 10,000. Release film.

2. The release film according to claim 1, wherein the second resin (b) has the structure shown in the following chemical formula 2. 【Transformation 3】 (In chemical formula 2, l is between 1 and 50, m is between 1 and 50, and n is between 0 and 5)

3. (a) The number average molecular weight of the first resin is 1,000 or more and less than 30,000. The release film according to claim 1, wherein the number average molecular weight of the second resin is 1,000 or more and less than 5,000.

4. The release film according to claim 1, wherein the release film is formed by applying the aqueous coating composition to a base film before crystal orientation is completed, stretching it in at least one direction, and then heat-treating it to complete the crystal orientation of the base film.

5. The release film according to claim 1, wherein the polyester film has a surface layer that is substantially free of inorganic particles, and the release layer is formed on the surface layer.

6. The release film according to claim 1, wherein the release film is a release film for manufacturing ceramic capacitors or resin sheets.

Citation Information

Patent Citations

  • Method of and apparatus for drying grain

    JP1982035278A

  • Manufacture of hydrothermally synthetic substance

    JP1982056315A

  • Polysiloxane coating material and releasing film

    JP2003292894A

  • Curable silicone releasing agent composition

    JP2005314510A

  • Release film

    JP2011509323A