Laminates, molded articles, vehicle exterior parts, and methods for manufacturing laminates.

A laminate with a biaxially oriented polyester film structure addresses peeling and heat-induced deterioration of coating substitute films in automobile exterior components by enhancing heat resistance and adhesive strength, ensuring high-quality press-formed parts.

JP7953826B2Active Publication Date: 2026-11-19TOYOBO CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2026524281
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2024-05-29
Filing Date
2025-03-28
Publication Date
2026-11-19
Estimated Expiration
2045-03-28

AI Technical Summary

Technical Problem

The existing methods for producing automobile exterior components using a metal sheet laminated with a coating substitute film face issues such as peeling and deterioration of the coating substitute film due to heat during press molding, which affects the appearance.

Method used

A laminate structure comprising a metal plate with a biaxially oriented polyester film containing two layers, where the first layer has a higher melting point than the second layer, and a specified ratio of X-ray diffraction peak intensities is used to enhance heat resistance and adhesive strength, preventing peeling and maintaining appearance.

Benefits of technology

The laminate structure effectively reduces peeling and maintains the appearance of the coating substitute film during press-forming, enabling the production of high-quality vehicle exterior parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007953826000005
    Figure 0007953826000005
  • Figure 0007953826000006
    Figure 0007953826000006
  • Figure 0007953826000001
    Figure 0007953826000001
Patent Text Reader

Abstract

A purpose of the present invention is to provide a laminate which makes it possible to reduce or prevent the occurrence of detachment of a coating substitution film from a metal sheet, and which further makes it possible to reduce or prevent deterioration in the appearance of the coating substitution film which may occur due to heat received by the coating substitution film during press-molding of the laminate. Another purpose of the present invention is to provide a molded article. Another purpose of the present invention is to provide a vehicle exterior component. The present invention pertains to a laminate (4) including a metal sheet (5) and a coating substitution film (8) laminated on the metal sheet (5). A biaxially-aligned polyester film (81) of the coating substitution film (8) contains a polyester including an alkylene terephthalate unit. In an X-ray diffraction pattern of the laminate (4), the ratio of an integrated intensity of a diffraction peak indicating the (1-10) plane derived at least from the alkylene terephthalate unit with respect to an integrated intensity of a diffraction peak indicating the (100) plane derived at least from the alkylene terephthalate unit is 0.2-1.0.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a laminate, a molded article, a vehicle exterior component, and a method for producing the laminate. BACKGROUND ART

[0002] Automobile exterior components such as door panels, front fenders, roofs, back doors, and hoods are generally coated. Spraying paint onto metal sheets for coating, that is, spray coating, is commonly performed.

[0003] However, since the paint used in spray coating contains volatile organic compounds (VOC), spray coating imposes a large environmental load. Moreover, since spray coating is performed repeatedly, a vast space is required to carry out the spray coating.

[0004] Instead of coating a metal sheet, a method of laminating a coating substitute film on a metal sheet has been proposed (see Patent Document 1). Since the coating substitute film of Patent Document 1 includes a colored layer, the metal sheet can be decorated or protected by the coating substitute film. PRIOR ART DOCUMENTS PATENT DOCUMENTS

[0005] PATENT DOCUMENT 1 Japanese Unexamined Patent Application Publication No. 2020-192787 SUMMARY OF THE INVENTION PROBLEM TO BE SOLVED BY THE INVENTION

[0006] When producing an automobile exterior component from a metal sheet laminated with a coating substitute film, the metal sheet laminated with the coating substitute film may be subjected to press molding. The heat applied to the coating substitute film during press molding may deteriorate the appearance (i.e., visual aspect) of the coating substitute film. The coating substitute film may also peel off from the metal sheet after press molding.

[0007] The present invention aims to provide a laminate that can reduce or prevent the peeling of a paint substitute film from a metal plate, and moreover, can reduce or prevent deterioration of the appearance (i.e., looks) of the paint substitute film that may occur due to the heat the paint substitute film receives when the laminate is press-formed. The present invention also aims to provide a molded product obtained by press-forming a laminate. The present invention also aims to provide a vehicle exterior part obtained by press-forming a laminate. [Means for solving the problem]

[0008] To solve this problem, the present invention comprises the configuration described in [1] below. [1] A metal plate and The paint substitute film laminated to the metal plate and A laminate containing, The aforementioned paint substitute film includes a biaxially oriented polyester film, a coloring layer, and a surface protective layer. The biaxially oriented polyester film comprises a first layer (hereinafter sometimes referred to as "layer B") and a second layer (hereinafter sometimes referred to as "layer A"), The first layer is located between the second layer and the colored layer. The first layer contains a first polyester containing alkylene terephthalate units, The second layer contains a second polyester containing alkylene terephthalate units, The melting point of the first layer is higher than the melting point of the second layer. In the X-ray diffraction pattern of the laminate, the ratio of the integrated intensity of the diffraction peaks showing the (1-10) plane, which originate from at least the alkylene terephthalate units of the first polyester and the alkylene terephthalate units of the second polyester, to the integrated intensity of the diffraction peaks showing the (100) plane, which originate from at least the alkylene terephthalate units of the first polyester and the alkylene terephthalate units of the second polyester, is 0.2 or more and 1.0 or less, and the (1-10) plane is the following crystal plane:

number

[0009] [1] According to [1], since the paint substitute film contains a colored layer, the paint substitute film can be used to decorate or protect metal plates.

[0010] Furthermore, since the paint substitute film includes a surface protection layer, the colored layer can be protected by the surface protection layer.

[0011] Furthermore, because the melting point of the first layer is higher than that of the second layer, or conversely, the melting point of the second layer is lower than that of the first layer, it is possible to lower the lamination temperature (specifically, the heat-sealing temperature) compared to the case where the biaxially oriented polyester film consists only of the first layer.

[0012] In the laminate of [1], the ratio of the integrated intensity of the diffraction peak showing the (1-10) plane (hereinafter sometimes referred to as the "first integrated intensity") to the integrated intensity of the diffraction peak showing the (100) plane (hereinafter sometimes referred to as the "second integrated intensity") (hereinafter sometimes referred to as the "integrated intensity ratio") is specified, and the integrated intensity ratio can be positioned as an indicator of crystallinity. This will be explained using the example of biaxially oriented polyethylene terephthalate (PET) film. In biaxially oriented PET film, the (100) plane of the PET crystal structure is a crystal plane containing a benzene ring. The (100) plane is almost parallel to the plane of the biaxially oriented PET film (which can also be called the "principal plane"). On the other hand, the (1-10) plane of the PET crystal structure is a plane inclined with respect to the (100) plane, and therefore faces a wider variety of directions compared to the (100) plane. Therefore, in the X-ray diffraction pattern of a biaxially oriented PET film, the influence of the crystallinity of PET on the integrated intensity of the diffraction peak representing the (1-10) plane is smaller than the influence of the crystallinity of PET on the integrated intensity of the diffraction peak representing the (100) plane. Consequently, the smaller the ratio of the integrated intensity of the diffraction peak representing the (1-10) plane to the integrated intensity of the diffraction peak representing the (100) plane, the higher the crystallinity of PET. Thus, this ratio can be positioned as an indicator of crystallinity. This principle also holds true for the biaxially oriented polyester film of the laminate [1]. Therefore, the integrated intensity ratio (i.e., the ratio of the first integrated intensity to the second integrated intensity) can be positioned as an indicator of crystallinity.

[0013] According to the laminate of [1], the integrated intensity ratio is 1.0 or less, so the degree of crystallinity is not excessively low, and therefore the heat resistance of the biaxially oriented polyester film can be improved. Thus, it is possible to reduce or prevent the occurrence of irregularities on the surface of the biaxially oriented polyester film that may occur due to the heat received by the paint substitute film when the laminate is press-molded. As a result, it is possible to reduce or prevent deterioration of the surface shape of the paint substitute film that may occur due to that heat. Therefore, it is possible to reduce or prevent deterioration of the appearance (i.e., looks) of the paint substitute film that may occur due to that heat.

[0014] On the other hand, since the integrated intensity ratio is 0.2 or more, the crystallinity is not excessively high, and thus the adhesive strength to the metal plate is prevented from becoming excessively low. Therefore, the occurrence of peeling of the coating alternative film from the metal plate, particularly the occurrence of peeling of the coating alternative film from the metal plate after press-forming the laminate, can be reduced or prevented.

[0015] In the present invention, the following configurations [2] to

[13] are preferred. [2] The coating alternative film further comprises an adhesive layer, The adhesive layer is positioned between the biaxially oriented polyester film and the colored layer, The laminate according to [1]. [3] The laminate according to [2], wherein the thickness of the adhesive layer is 10 nm or more and 200 nm or less. [4] The laminate according to any one of [1] to [3], wherein the colored layer contains a resin and a colorant. [5] The alkylene terephthalate unit of the first polyester comprises an ethylene terephthalate unit, The alkylene terephthalate unit of the second polyester comprises an ethylene terephthalate unit, The (1-10) plane is a (1-10) plane derived from at least the ethylene terephthalate unit of the first polyester and the ethylene terephthalate unit of the second polyester, The (100) plane is a (100) plane derived from at least the ethylene terephthalate unit of the first polyester and the ethylene terephthalate unit of the second polyester, The laminate according to any one of [1] to [4]. [6] When the repeating units of the first polyester are taken as 100 mol%, the content of the ethylene terephthalate unit is 85 mol% or more, When the repeating units of the second polyester are taken as 100 mol%, the content of the ethylene terephthalate unit is 60 mol% or more, The laminate according to [5]. [7] Further comprising a protective film, The laminate according to any one of [1] to [6], wherein the metal plate, the coating substitute film, and the protective film are stacked in this order. [8] The laminate according to any one of [1] to [7], which is used for manufacturing a vehicle exterior component. [9] A molded article obtained by press-working the laminate according to any one of [1] to [8].

[10] A vehicle exterior component obtained by press-working the laminate according to any one of [1] to [8].

[11] A method for producing the laminate according to any one of [1] to [8], comprising: a step of heating the metal plate, and a step of pressure-bonding the heated metal plate to the coating substitute film or the composite film, wherein the composite film includes the coating substitute film and a protective film provided on the surface protective layer of the coating substitute film. The method for producing a laminate.

[12] The method for producing a laminate according to

[11] , further comprising a step of starting cooling within 5 seconds after the metal plate and the coating substitute film or the composite film are pressure-bonded.

[13] The plane orientation coefficient of the first layer of the coating substitute film or the composite film to be pressure-bonded to the metal plate is 0.165 or more and 0.180 or less, The plane orientation coefficient of the second layer of the coating substitute film or the composite film to be pressure-bonded to the metal plate is 0.100 or more and 0.135 or less, The method for producing a laminate according to

[11] or

[12] .

[0016] The present invention also preferably has the following configurations.

[14] The laminate, the molded article, the vehicle exterior component, or the method for producing a laminate according to any one of the preceding configurations, wherein the metal plate comprises an alloy plate.

[15] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the metal plate includes a steel plate, an aluminum alloy plate, or a magnesium alloy plate.

[16] A laminate, molded product, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the metal plate includes a steel plate that has been plated with a zinc alloy.

[17] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the thickness of the biaxially oriented polyester film is 10 μm or more, or 15 μm or more.

[18] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the thickness of the biaxially oriented polyester film is 20 μm or more, or 30 μm or more.

[19] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to either of the above configurations, wherein the thickness of the biaxially oriented polyester film is 200 μm or less, or 150 μm or less.

[20] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein the thickness of the biaxially oriented polyester film is 100 μm or less, or 75 μm or less, according to either of the above configurations. [twenty one] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein when the biaxially oriented polyester film is heat-treated at 150°C for 15 minutes, the sum of the thermal shrinkage rate in the flow direction and the thermal shrinkage rate in the width direction is 5.0% or less or 4.8% or less, according to any of the above configurations. [twenty two] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, according to any of the above configurations, wherein the sum of the thermal shrinkage rate in the flow direction and the thermal shrinkage rate in the width direction is 4.5% or less or 4.0% or less. [twenty three] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, according to any of the above configurations, wherein the sum of the thermal shrinkage rate in the flow direction and the thermal shrinkage rate in the width direction is 1.0% or more or 2.0% or more. [twenty four] A laminate, molded product, vehicle exterior part, or method for manufacturing a laminate, according to any of the above configurations, wherein the sum of the thermal shrinkage rate in the flow direction and the thermal shrinkage rate in the width direction is 3.0% or more. [twenty five] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein the difference between the melting point of the first layer and the melting point of the second layer is 20°C or more or 25°C or more, according to any of the above configurations.

[26] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein the difference between the melting point of the first layer and the melting point of the second layer is 28°C or higher or 30°C or higher, according to any of the above configurations.

[27] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein the difference between the melting point of the first layer and the melting point of the second layer is 70°C or less or 60°C or less, according to any of the above configurations.

[28] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein the difference between the melting point of the first layer and the melting point of the second layer is 50°C or less, according to any of the above configurations.

[29] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, according to any of the above configurations, wherein the ratio of the thickness of the first layer to the thickness of the second layer (i.e., thickness of the first layer / thickness of the second layer) is 1.5 or more or 2.0 or more.

[30] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the ratio (i.e., thickness of the first layer / thickness of the second layer) is 10 or less or 8 or less.

[31] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the ratio (i.e., thickness of the first layer / thickness of the second layer) is 6 or less.

[32] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the thickness of the first layer is 20 μm or more or 25 μm or more.

[33] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the thickness of the first layer is 30 μm or more.

[34] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to either of the above configurations, wherein the thickness of the first layer is 150 μm or less or 100 μm or less.

[35] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to either of the above configurations, wherein the thickness of the first layer is 75 μm or less or 50 μm or less.

[36] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the melting point of the first layer is 250°C or higher or 252°C or higher.

[37] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the melting point of the first layer is 253°C or higher.

[38] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the melting point of the first layer is 260°C or less or 258°C or less.

[39] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the surface orientation coefficient of the first layer is 0.165 or more or 0.168 or more.

[40] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the surface orientation coefficient of the first layer is 0.170 or greater.

[41] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the surface orientation coefficient of the first layer is 0.180 or less or 0.178 or less.

[42] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein when the repeating units of the first polyester are set to 100 mol%, the ethylene terephthalate units are 85 mol% or more or 90 mol% or more, according to any of the above configurations.

[43] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein when the repeating units of the first polyester are set to 100 mol%, the ethylene terephthalate units are 95 mol% or more or 97 mol% or more, according to any of the above configurations.

[44] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the first polyester is a crystalline polyester.

[45] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the first polyester is polyethylene terephthalate.

[46] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the polyethylene terephthalate is homopolyethylene terephthalate or copolymerized polyethylene terephthalate.

[47] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the first layer contains inert particles.

[48] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the first layer contains silica particles.

[49] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the thickness of the second layer is 5 μm or more or 10 μm or more.

[50] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to either of the above configurations, wherein the thickness of the second layer is 30 μm or less or 25 μm or less.

[51] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the thickness of the second layer is 20 μm or less or 15 μm or less.

[52] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the surface orientation coefficient of the second layer is 0.135 or less or 0.132 or less.

[53] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the surface orientation coefficient of the second layer is 0.130 or less.

[54] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the surface orientation coefficient of the second layer is 0.100 or more or 0.110 or more.

[55] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the surface orientation coefficient of the second layer is 0.112 or greater.

[56] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein when the repeating units of the second polyester are set to 100 mol%, the ethylene terephthalate units are 60 mol% or more or 70 mol% or more, according to any of the above configurations.

[57] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein when the repeating units of the second polyester are set to 100 mol%, the ethylene terephthalate units are 80 mol% or more or 82 mol% or more, according to any of the above configurations.

[58] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein when the repeating units of the second polyester are set to 100 mol%, the ethylene terephthalate units are 96 mol% or less or 94 mol% or less, according to any of the above configurations.

[59] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate, wherein when the repeating units of the second polyester are set to 100 mol%, the ethylene terephthalate units are 92 mol% or less or 90 mol% or less, according to any of the above configurations.

[60] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the second polyester is a crystalline polyester.

[61] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the second polyester is polyethylene terephthalate.

[62] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the polyethylene terephthalate of the second polyester is copolymerized polyethylene terephthalate.

[63] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the integrated intensity ratio is 0.9 or less or 0.8 or less.

[64] A laminate, molded article, vehicle exterior part, or method for manufacturing a laminate according to any of the above configurations, wherein the integrated intensity ratio is 0.3 or more or 0.4 or more.

[65] The method for manufacturing a laminate according to

[11] , further comprising the step of pressing the metal plate and the coating substitute film or the composite film together and then starting cooling within 3 seconds or 2 seconds.

[66] A method for manufacturing a laminate according to any of the above configurations, wherein the metal plate to which the coating substitute film or the composite film is pressed is cooled with water at 60°C or below or 45°C or below.

[67] A method for manufacturing a laminate according to any of the above configurations, wherein the metal plate to which the coating substitute film or the composite film is pressed is cooled with water at 35°C or below or 30°C or below.

[68] A method for manufacturing a laminate according to any of the above configurations, wherein the metal plate to which the coating substitute film or the composite film is pressed is immersed in a water tank to cool it. [Effects of the Invention]

[0017] According to the present invention, it is possible to reduce or prevent the occurrence of delamination of the paint substitute film from the metal plate, and moreover, it is possible to provide a laminate that can reduce or prevent deterioration of the appearance (i.e., looks) of the paint substitute film that may occur due to the heat the paint substitute film receives when the laminate is press-formed. According to the present invention, it is also possible to provide a molded product obtained by press-forming the laminate. The present invention can also provide a vehicle exterior part obtained by press-forming the laminate. [Brief explanation of the drawing]

[0018] [Figure 1] This is a schematic cross-sectional view of the laminate in this embodiment. [Figure 2] This is an example of the X-ray diffraction pattern of the laminate in this embodiment. Here, the 2θ angle is shown on the horizontal axis, and the diffracted X-ray intensity is shown on the vertical axis. In this example, the diffraction peak around 2θ = 23° represents the (1-10) plane of polyethylene terephthalate, and the diffraction peak around 2θ = 26° represents the (100) plane of polyethylene terephthalate. [Modes for carrying out the invention]

[0019] Embodiments of the present invention will be described in detail below.

[0020] <1. Laminate> As shown in Figure 1, the laminate 4 includes a metal plate 5 and a composite film 7 laminated to the metal plate 5.

[0021] In other words, the laminate 4 includes a metal plate 5 and a paint substitute film 8 laminated to the metal plate 5, and further includes a protective film 9. In the laminate 4, the metal plate 5, the paint substitute film 8, and the protective film 9 are stacked in this order.

[0022] <1.1. Metal plate> Examples of metal plates 5 include steel plates, aluminum alloy plates, and magnesium alloy plates. Among these, steel plates are preferred. Examples of steel plates include stainless steel plates. These may be pre-treated with zinc alloy plating or chromium plating. In other words, the steel plates may be surface-treated steel plates. Examples of surface-treated steel plates include tin-free steel plates and tinplate. In particular, when the laminate 4 is used to manufacture vehicle exterior parts, the metal plate 5 is preferably a steel plate with zinc alloy plating. Zinc alloy plating can improve corrosion resistance.

[0023] The thickness of the metal plate 5 may be, for example, 0.2 mm or more, 0.3 mm or more, 0.4 mm or more, or 0.6 mm or more. On the other hand, the thickness of the metal plate 5 may be, for example, 1.4 mm or less, 1.2 mm or less, 1.0 mm or less, or 0.8 mm or less. In particular, for good formability, the thickness of the metal plate 5 is preferably 0.2 mm or more and 1.4 mm or less, more preferably 0.3 mm or more and 1.2 mm or less, and even more preferably 0.3 mm or more and 1.0 mm or less. If the metal plate 5 is a steel plate with zinc alloy plating, the thickness of the metal plate 5 is preferably 0.4 mm or more and 0.8 mm or less. If the metal plate 5 is an aluminum alloy plate, the thickness of the metal plate 5 is preferably 0.6 mm or more and 1.2 mm or less.

[0024] <1.2. Composite Films> The composite film 7 includes a paint substitute film 8 and a protective film 9. In the composite film 7, the protective film 9 is provided on top of the paint substitute film 8.

[0025] <1.2.1. Paint Replacement Film> The paint-alternative film 8 includes a biaxially oriented polyester film 81, an adhesive layer 82, a coloring layer 83, and a surface protection layer (hereinafter sometimes referred to as the "hard coat layer") 84. In the paint-alternative film 8, the biaxially oriented polyester film 81, adhesive layer 82, coloring layer 83, and surface protection layer 84 are stacked in this order.

[0026] <1.2.1.1. Biaxially oriented polyester film> The biaxially oriented polyester film 81 is provided on the metal plate 5. Specifically, layer A 812 of the biaxially oriented polyester film 81 is provided on the metal plate 5.

[0027] The thickness of the biaxially oriented polyester film 81 is preferably 10 μm or more, more preferably 15 μm or more, even more preferably 20 μm or more, and even more preferably 30 μm or more. A thickness of 10 μm or more facilitates film formation and also facilitates the formation of functional layers such as the colored layer 83 and the surface protection layer 84. In addition, the handling properties of the coating substitute film 8 or composite film 7 when laminating them to the metal plate 5 are also good. On the other hand, the thickness of the biaxially oriented polyester film 81 is preferably 200 μm or less, more preferably 150 μm or less, even more preferably 125 μm or less, even more preferably 100 μm or less, and even more preferably 75 μm or less. A thickness of 200 μm or less prevents the load required for press molding of the laminate 4 from becoming excessively large.

[0028] When the biaxially oriented polyester film 81 is heat-treated at 150°C for 15 minutes, the sum of the thermal shrinkage rate in the flow direction and the thermal shrinkage rate in the width direction is preferably 5.0% or less, and more preferably 4.8% or less. The smaller this sum, the less thermal shrinkage of the biaxially oriented polyester film 81 that may occur due to the heat received by the coating substitute film 8 during lamination (specifically during heat-pressing), and therefore, the reduction in adhesive strength with the metal plate that may result from such thermal shrinkage can be suppressed. The smaller this sum, the less dimensional change of the coating substitute film 8 due to the heat generated by shear when the laminate 4 is press-formed can be reduced. In other words, the dimensional stability of the coating substitute film 8 is excellent. This sum may be, for example, 4.5% or less, 4.2% or less, or 4.0% or less. On the other hand, this sum may be 1.0% or more, 2.0% or more, or 3.0% or more. This sum can be controlled by the stretching conditions and heat-fixing treatment conditions. The thermal shrinkage rate of the biaxially oriented polyester film 81 can be determined by the following formula. Thermal shrinkage rate (%) = {(L0 - L) / L0} × 100 Here, L is the gauge length after heat treatment (specifically, heat treatment at 150°C for 15 minutes), and L0 is the gauge length before heat treatment (specifically, heat treatment at 150°C for 15 minutes).

[0029] The biaxially oriented polyester film 81 includes a B layer (i.e., the first layer) 811 and an A layer (i.e., the second layer) 812. The B layer 811 is located between the A layer 812 and the colored layer 83.

[0030] The melting point of layer B 811 (hereinafter sometimes referred to as "TmB") is higher than the melting point of layer A 812 (hereinafter sometimes referred to as "TmA"). In other words, the melting point of layer A 812 is lower than the melting point of layer B 811. This makes it possible to lower the lamination temperature (specifically, the thermocompression temperature) compared to the case where the biaxially oriented polyester film 81 consists only of layer B 811.

[0031] The difference between the melting point of layer B 811 and the melting point of layer A 812 is preferably 20°C or higher, more preferably 25°C or higher, even more preferably 28°C or higher, and even more preferably 30°C or higher. A difference of 20°C or higher reduces the deterioration of the surface shape of the biaxially oriented polyester film 81 that may occur due to the heat received by the coating substitute film 8 during lamination (specifically during heat bonding), and also reduces the viscosity of layer A 812 during lamination (specifically during heat bonding). On the other hand, the difference between the melting point of layer B 811 and the melting point of layer A 812 is preferably 70°C or lower, more preferably 60°C or lower, and even more preferably 50°C or lower. A difference of 70°C or lower results in good handling during film formation.

[0032] The ratio of the thickness of layer B 811 to the thickness of layer A 812 (i.e., thickness of layer B 811 / thickness of layer A 812) is preferably 1.5 or more, and more preferably 2.0 or more. A ratio of 1.5 or more reduces the deterioration of the appearance of the coating substitute film 8 that may occur due to the heat received by the coating substitute film 8 during lamination (specifically during heat bonding). In addition, it further reduces or prevents the deterioration of the appearance of the coating substitute film 8 that may occur due to the heat received by the coating substitute film 8 when the laminate 4 is press-molded. On the other hand, the ratio of the thickness of layer B 811 to the thickness of layer A 812 (i.e., thickness of layer B 811 / thickness of layer A 812) is preferably 10 or less, more preferably 8 or less, and even more preferably 6 or less.

[0033] The thickness of layer B 811 is preferably 20 μm or more, more preferably 25 μm or more, and even more preferably 30 μm or more. A thickness of 20 μm or more reduces the deterioration of the surface shape of the biaxially oriented polyester film 81 that may occur due to the heat received by the coating substitute film 8 during lamination (specifically during heat bonding). In addition, it further reduces or prevents deterioration of the appearance of the coating substitute film 8 that may occur due to the heat received by the coating substitute film 8 when the laminate 4 is press-molded. The thickness of layer B 811 is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 75 μm or less, and even more preferably 50 μm or less.

[0034] The melting point of layer B 811 is preferably 250°C or higher, more preferably 252°C or higher, and even more preferably 253°C or higher. On the other hand, the melting point of layer B 811 may be 260°C or lower, or 258°C or lower.

[0035] The surface orientation coefficient of layer B 811 is preferably 0.165 or higher, more preferably 0.168 or higher, and even more preferably 0.170 or higher. This is because a larger surface orientation coefficient of layer B 811 reduces the occurrence of wrinkles and bubbles that may form in the coating substitute film 8 due to the heat received by the coating substitute film 8 during lamination (specifically during heat bonding). In addition, a larger surface orientation coefficient of layer B 811 tends to increase the ability of the biaxially oriented polyester film 81 to follow the springback that occurs when the laminate 4 is press-molded. On the other hand, the surface orientation coefficient of layer B 811 is preferably 0.180 or lower, and more preferably 0.178 or lower.

[0036] Layer B 811 contains a first polyester, i.e., a first polyester resin. The intrinsic viscosity of the first polyester is preferably 0.60 or higher. A viscosity of 0.60 or higher reduces the generation of thermally degraded products derived from low molecular weight components. On the other hand, the intrinsic viscosity of the first polyester is preferably less than 0.95.

[0037] The first polyester contains repeating units that include alkylene terephthalate units. That is, the repeating units of the first polyester contain alkylene terephthalate units.

[0038] Examples of alkylene terephthalate units include ethylene terephthalate units, trimethylene terephthalate units, and polybutylene terephthalate units. Among these, ethylene terephthalate units are preferred.

[0039] When the repeating units of the first polyester are set to 100 mol%, the alkylene terephthalate units are preferably 85 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, and still more preferably 97 mol% or more.

[0040] When the repeating units of the first polyester are set to 100 mol%, the ethylene terephthalate units are preferably 85 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, and even more preferably 97 mol% or more.

[0041] The repeating units of the first polyester may include other units. Examples of other units include alkylene isophthalate units and alkylene naphthalate units. Examples of alkylene isophthalate units include ethylene isophthalate units, trimethylene isophthalate units, and polybutylene isophthalate units. Examples of alkylene naphthalate units include ethylene naphthalate units, trimethylene naphthalate units, and polybutylene naphthalate units. However, it is preferable that the repeating units of the first polyester do not include alkylene isophthalate units. It is preferable that the repeating units of the first polyester do not include alkylene naphthalate units.

[0042] The first polyester is preferably a crystalline polyester. If the first polyester is a crystalline polyester, it is possible to reduce uneven stretching of the coating substitute film 8 that may occur when the laminate 4 is press-molded. This will be explained. When the laminate 4 is press-molded, the coating substitute film 8 is partially stretched by the press molding. If the B layer 811 of the biaxially oriented polyester film 81 contains crystalline polyester, the crystallization of the crystalline polyester can progress more in the part that is stretched the most (i.e., the part with the greatest deformation) than in the surrounding area (i.e., the area around the part with the greatest deformation). Therefore, at the beginning of press molding, the coating substitute film 8 stretches easily in the part with the greatest deformation, but as press molding progresses, the part with the greatest deformation itself becomes less stretchable. As a result, the surrounding area (i.e., the area around the part with the greatest deformation) stretches. Therefore, it is possible to prevent the thickness of the part with the greatest deformation from becoming excessively thin. Hence, uneven stretching of the coating substitute film 8 can be reduced. Crystalline polyester is used in differential scanning calorimetry. In the (DSC) curve, this refers to polyester in which an endothermic peak of 0.05 J / g or more appears at a temperature higher than the temperature at which the baseline shift corresponding to the glass transition point occurs, due to crystal melting. For differential scanning calorimetry to obtain the DSC curve, a sample is scraped from layer B 811, 10 mg of the sample is heated to 290°C at 20°C / min, isothermal for 3 minutes, rapidly cooled at 200°C / min, and heated to 290°C at 10°C / min. A DSC-60 differential scanning calorimeter is used for differential scanning calorimetry.

[0043] Polyethylene terephthalate is preferred as the first polyester. Examples of polyethylene terephthalate include homo-polyethylene terephthalate and copolymerized polyethylene terephthalate. Among these, homo-polyethylene terephthalate is preferred. Homo-polyethylene terephthalate may contain diethylene glycol components that may be produced as by-products during its manufacture. On the other hand, examples of copolymerization components for obtaining copolymerized polyethylene terephthalate, particularly dicarboxylic acids, include aromatic carboxylic acids such as isophthalic acid, 2,6-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid; aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, and decanedicarboxylic acid; and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid. One or more of these can be used. Examples of copolymerization components for obtaining copolymerized polyethylene terephthalate, particularly diols, include aliphatic diols such as trimethylene glycol (propanediol), butanediol, and hexanediol; and alicyclic diols such as cyclohexanedimethanol. One or more of these can be used. Among these, isophthalic acid and sebacic acid are preferred, with isophthalic acid being more preferred.

[0044] The content of the first polyester is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 75% by mass or more, when the B layer 811 is considered to be 100% by mass. The content of the first polyester is, for example, 80% by mass or more, 90% by mass or more, or 95% by mass or more, when the B layer 811 is considered to be 100% by mass. On the other hand, the content of the first polyester is, for example, 100% by mass, 99% by mass or less, 98% by mass or less, 95% by mass or less, or 90% by mass or less, when the B layer 811 is considered to be 100% by mass.

[0045] Layer B 811 may contain additives. Examples of additives include coloring pigments, fluorescent whitening agents, inert particles, antioxidants, heat stabilizers, ultraviolet absorbers, and antistatic agents. Examples of coloring pigments include inorganic pigments and organic pigments. Inorganic pigments are preferred among these. Examples of inorganic pigments include alumina, titanium dioxide, calcium carbonate, and barium sulfate. Titanium dioxide is preferred among these when imparting opacity to layer B 811. The content of the coloring pigment may be 2% by mass or more, 4% by mass or more, or 10% by mass or more, when layer B 811 is considered to be 100% by mass. On the other hand, the content of the coloring pigment may be 50% by mass or less, 40% by mass or less, or 35% by mass or less, when layer B 811 is considered to be 100% by mass. Fluorescent whitening agents can improve whiteness.

[0046] Inert particles can improve the handling, specifically the slipperiness, of the biaxially oriented polyester film 81. Examples of inert particles include polymers or copolymers of monomers selected from polystyrene, methyl polyacrylate, ethyl polyacrylate, methyl polymethacrylate, ethyl polymethacrylate, and divinylbenzene, as well as organic materials such as polytetrafluoroethylene, polyacrylonitrile, benzoguanamine, and silicone. Inorganic materials such as silica, kaolin, talc, and graphite can also be used. Among these, inorganic materials are preferred, and silica, i.e., silica particles, are more preferred. The particle size of the inert particles is preferably 0.1 μm to 10 μm. The content of inert particles is preferably 0.002% to 0.5% by mass, when the B layer 811 is considered to be 100% by mass.

[0047] Layer A 812 adheres the metal plate 5 and layer B 811. Layer A 812 is located between the metal plate 5 and layer B 811.

[0048] The thickness of layer A 812 is preferably 5 μm or more, more preferably 8 μm or more, and even more preferably 10 μm or more. If it is 5 μm or more, it is possible to fill any irregularities that may exist on the metal plate 5, and therefore the adhesion strength with the metal plate 5 can be improved. The thickness of layer A 812 is preferably 30 μm or less, more preferably 25 μm or less, even more preferably 20 μm or less, and even more preferably 15 μm or less.

[0049] The melting point of layer A 812 is preferably 160°C or higher, more preferably 180°C or higher, and even more preferably 200°C or higher. On the other hand, the melting point of layer A 812 is preferably 250°C or lower, more preferably 240°C or lower, and even more preferably 230°C or lower.

[0050] The surface orientation coefficient of layer A 812 is preferably 0.135 or less, more preferably 0.132 or less, and even more preferably 0.130 or less. A coefficient of 0.135 or less improves the adhesion strength with the metal plate 5. On the other hand, the surface orientation coefficient of layer A 812 is preferably 0.100 or more, more preferably 0.110 or more, and even more preferably 0.112 or more.

[0051] Layer A 812 contains a second polyester, i.e., a second polyester resin. The intrinsic viscosity of the second polyester is preferably 0.60 or higher. On the other hand, the intrinsic viscosity of the first polyester is preferably less than 0.95. If it is less than 0.95, it is possible to reduce the viscosity of layer A 812 during lamination (specifically during heat bonding), and therefore, the adhesion strength to the metal plate 5 can be improved.

[0052] The second polyester contains repeating units that include alkylene terephthalate units. That is, the repeating units of the second polyester contain alkylene terephthalate units.

[0053] Examples of alkylene terephthalate units include ethylene terephthalate units, trimethylene terephthalate units, and polybutylene terephthalate units. Among these, ethylene terephthalate units are preferred.

[0054] When the repeating units of the second polyester are set to 100 mol%, the alkylene terephthalate units are preferably 60 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and even more preferably 82 mol% or more. When the repeating units of the second polyester are set to 100 mol%, the alkylene terephthalate units are preferably 96 mol% or less, more preferably 94 mol% or less, even more preferably 92 mol% or less, and even more preferably 90 mol% or less.

[0055] When the repeating units of the second polyester are set to 100 mol%, the ethylene terephthalate units are preferably 60 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and even more preferably 82 mol% or more. When the repeating units of the second polyester are set to 100 mol%, the ethylene terephthalate units are preferably 96 mol% or less, more preferably 94 mol% or less, even more preferably 92 mol% or less, and even more preferably 90 mol% or less.

[0056] It is preferable that the repeating units of the second polyester include other units. Examples of other units include alkylene isophthalate units and alkylene naphthalate units. Examples of alkylene isophthalate units include ethylene isophthalate units, trimethylene isophthalate units and polybutylene isophthalate units. Examples of alkylene naphthalate units include ethylene naphthalate units, trimethylene naphthalate units and polybutylene naphthalate units. In particular, it is preferable that the repeating units of the second polyester include alkylene isophthalate units. When the repeating units of the second polyester are set to 100 mol%, the alkylene isophthalate units are preferably 4 mol% or more, more preferably 6 mol% or more, even more preferably 8 mol% or more, and even more preferably 10 mol% or more. When the repeating units of the second polyester are set to 100 mol%, the alkylene isophthalate units are preferably 40 mol% or less, more preferably 30 mol% or less, even more preferably 20 mol% or less, and even more preferably 18 mol% or less. The repeating units of the first polyester preferably do not contain alkylene naphthalate units.

[0057] The second polyester is preferably a crystalline polyester. A crystalline polyester is a polyester that, in the differential scanning calorimetry (DSC) curve, exhibits an endothermic peak of 0.05 J / g or more at a temperature higher than the temperature at which the baseline shift corresponding to the glass transition occurs, due to crystal melting. For differential scanning calorimetry to obtain the DSC curve, a sample is scraped from layer A 812, 10 mg of the sample is heated to 290°C at 20°C / min, isothermal for 3 minutes, rapidly cooled at 200°C / min, and heated to 290°C at 10°C / min. A DSC-60 differential scanning calorimeter is used for differential scanning calorimetry.

[0058] Copolymerized polyethylene terephthalate is preferred as the second polyester. The explanation of copolymerized polyethylene terephthalate in the second polyester is omitted as it overlaps with the explanation of copolymerized polyethylene terephthalate in the first polyester. Therefore, the explanation of copolymerized polyethylene terephthalate in the first polyester can also be treated as the explanation of copolymerized polyethylene terephthalate in the second polyester.

[0059] The content of the second polyester is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, when the A layer 812 is considered to be 100% by mass. On the other hand, the content of the second polyester may be, for example, 100% by mass, 99% by mass or less, 98% by mass or less, or 95% by mass or less, when the A layer 812 is considered to be 100% by mass.

[0060] Layer A 812 may contain additives. Examples of additives include coloring pigments, fluorescent whitening agents, inert particles, antioxidants, heat stabilizers, ultraviolet absorbers, and antistatic agents.

[0061] The biaxially oriented polyester film 81 can be produced by a procedure in which an unstretched polyester film is prepared, and then the unstretched polyester film is biaxially stretched. For example, the biaxially oriented polyester film 81 can be produced by a procedure in which a molding material for forming layer B 811 (i.e., a polyester composition containing a first polyester) is supplied to a first extruder, and a molding material for forming layer A 812 (specifically, a polyester composition containing a second polyester) is supplied to a second extruder, then the molding material is guided from the first extruder to a feed block, and the molding material is guided from the second extruder to a feed block, and these molding materials are laminated in the feed block, then the unstretched polyester film (hereinafter sometimes referred to as "sheet") is melt-extruded from the die, then the unstretched polyester film is solidified in a cooling drum, the unstretched polyester film is biaxially stretched, and then heat-fixed. Alternatively, the film can be manufactured by supplying raw materials for forming layer B 811 to a first extruder and raw materials for forming layer A 812 to a second extruder, then guiding the molding material from the first extruder to a multi-manifold die and guiding the molding material from the second extruder to a multi-manifold die, laminating these molding materials in the multi-manifold die, then melt-extruding the unstretched polyester film from the multi-manifold die, then solidifying the unstretched polyester film in a cooling drum, biaxially stretching the unstretched polyester film, and heat-setting it. The biaxial stretching may be simultaneous biaxial stretching in the longitudinal and transverse directions, or sequential biaxial stretching. Sequential biaxial stretching is preferred. In sequential biaxial stretching, for example, it is preferable to stretch the sheet that has passed through the cooling roll in the flow direction, i.e., the Machine Direction (hereinafter referred to as the "MD direction"), and then stretch the sheet after stretching in the MD direction in the width direction, i.e., the Transverse Direction (hereinafter referred to as the "TD direction"). Furthermore, a surface treatment may be applied to the sheet between the first stretching (for example, stretching in the flow direction) and the second stretching (for example, stretching in the width direction). For example, an adhesive layer 82 may be formed between the first stretching and the second stretching.

[0062] Regarding extrusion, in the first extruder, it is preferable to supply the molding material for forming layer B 811, i.e., the polyester composition containing the first polyester, to the first extruder after it has been thoroughly dried, and to melt it at a temperature of ~(melting point + 50)°C of the first polyester. On the other hand, in the second extruder, it is preferable to supply the molding material for forming layer A 812, i.e., the polyester composition containing the second polyester, to the second extruder after it has been thoroughly dried, and to melt it at a temperature of ~(melting point + 50)°C of the second polyester. At least one of the molding material for forming layer B 811 and the molding material for forming layer A 812 may contain inert particles.

[0063] When biaxial stretching is sequential biaxial stretching, the unstretched polyester film can be heated and stretched in the flow direction. Examples of heating methods for the unstretched polyester film include roll heating and infrared heating. The stretching temperature in the flow direction is preferably 70°C or higher, and more preferably 80°C or higher. A temperature of 70°C or higher can reduce the occurrence of breakage. On the other hand, the stretching temperature in the flow direction is preferably 110°C or lower, and more preferably 100°C or lower. A temperature of 110°C or lower can avoid excessively low orientation.

[0064] The stretching ratio in the flow direction is preferably 3.0 times or more, and more preferably 3.5 times or more. A ratio of 3.0 times or more makes it possible to avoid excessively low orientation. In addition, it is possible to reduce or avoid the occurrence of excessive thickness unevenness, and to reduce or avoid the occurrence of excessive looseness that may occur when the biaxially oriented polyester film 81 is wound into a roll. On the other hand, the stretching ratio in the flow direction is preferably 5.0 times or less, more preferably 4.5 times or less, and even more preferably 4.0 times or less. A ratio of 5.0 times or less allows for effective enjoyment of the effect of improving thickness unevenness due to stretching. As an example of a method for stretching in the flow direction, one can cite a method in which a heated unstretched polyester film is stretched by the speed difference between rolls.

[0065] A polyester film stretched in the flow direction can be stretched in the width direction. A stretching temperature of 90°C or higher is preferable, as this reduces the occurrence of breakage. On the other hand, a stretching temperature of 130°C or lower is preferable, as this avoids excessively low orientation.

[0066] The stretching ratio in the width direction is preferably 3.0 times or more, and more preferably 3.5 times or more. A ratio of 3.0 times or more makes it possible to avoid excessively low orientation. In addition, it is possible to reduce or avoid the occurrence of excessive thickness unevenness, and to reduce or avoid the occurrence of excessive looseness that may occur when the biaxially oriented polyester film 81 is wound into a roll. On the other hand, the stretching ratio in the width direction is preferably 5.0 times or less, and more preferably 4.5 times or less. A ratio of 5.0 times or less makes it possible to effectively enjoy the effect of improving thickness unevenness due to stretching.

[0067] It is preferable to perform a heat-setting treatment after biaxial stretching. An example of a heat-setting temperature is 150°C to 230°C. The heat-setting temperature can be set according to the type of first polyester and the type of second polyester. When the first polyester is polyethylene terephthalate and the second polyester is copolymerized polyethylene terephthalate, the heat-setting temperature is preferably 225°C or lower, more preferably 222°C or lower, and even more preferably 220°C or lower. If the temperature is 225°C or lower, it is possible to avoid the degree of crystallinity of the biaxially oriented polyester film 81 before lamination becoming excessively high, and therefore, excessive relaxation of the degree of plane orientation can be avoided. On the other hand, the heat-setting temperature is preferably 205°C or higher, more preferably 210°C or higher, and even more preferably 213°C or higher. The heat-setting temperature may also be 215°C or higher. If the temperature is 205°C or higher, it is possible to avoid the degree of crystallinity of the biaxially oriented polyester film 81 before lamination becoming excessively low.

[0068] It is preferable to perform a thermal relaxation treatment in conjunction with or separately from the thermal setting treatment. In the thermal relaxation treatment, it is preferable to relax in at least one of the flow direction (i.e., MD direction) and the width direction (i.e., TD direction). In particular, relaxation in the width direction is preferable. When relaxation occurs in the width direction, the relaxation rate in the width direction is preferably 3% or more, and more preferably 4% or more. On the other hand, the relaxation rate in the width direction is preferably 8% or less, and more preferably 7% or less.

[0069] <1.2.1.2.Adhesive layer> The adhesive layer 82 is located between the biaxially oriented polyester film 81 and the colored layer 83. Specifically, the adhesive layer 82 is located between the B layer 811 of the biaxially oriented polyester film 81 and the colored layer 83. The adhesive layer 82 can improve the adhesion between the biaxially oriented polyester film 81 and the colored layer 83. Mechanisms for improving adhesion include, for example, bond formation between functional groups, reduction of interlayer interface energy, and interlayer interface mixing. The adhesive layer 82 can also be referred to as the easy-adhesion layer 82.

[0070] From the viewpoint of adhesion, the thickness of the adhesive layer 82 is preferably 10 nm or more, more preferably 15 nm or more, even more preferably 20 nm, and even more preferably 40 nm or more. On the other hand, from the viewpoint of thickness uniformity and adhesion, the thickness of the adhesive layer 82 is preferably 200 nm or less, more preferably 180 nm, even more preferably 150 nm, and even more preferably 120 nm or less.

[0071] The adhesive layer 82 contains a resin. Examples of resins include polyurethane resins, vinyl chloride / vinyl acetate copolymer resins, vinyl chloride / vinyl acetate / acrylic copolymer resins, chlorinated polypropylene resins, acrylic resins, polyester resins, polyamide resins, butyral resins, polystyrene resins, nitrocellulose resins, and cellulose acetate resins. One or more of these can be used. Among these, acrylic resins and polyester resins are preferred. Considering that heat is generated by shear during press molding of the laminate 4, and the laminate 4 may reach a temperature of about 150°C, the glass transition temperature of the resin is preferably 150°C or lower. Incidentally, it is preferable that the adhesive layer 82 does not contain polyester containing alkylene terephthalate units.

[0072] The resin preferably has at least one functional group selected from the group consisting of epoxy groups, oxazoline groups, silanol groups, and isocyanate groups. Among these, epoxy groups and oxazoline groups are preferred as functional groups because they can further improve adhesion with layer B 811.

[0073] The adhesive layer 82 can be formed on the biaxially oriented polyester film 81 by any method. For example, the adhesive layer 82 may be formed by in-line coating, where the coating is applied while the biaxially oriented polyester film 81 is being formed. Alternatively, the adhesive layer 82 may be formed by off-line coating, where the biaxially oriented polyester film 81 is formed, wound into a roll, and then unwound and coated.

[0074] <1.2.1.3. Colored layer> The colored layer 83 is located between the adhesive layer 82 and the surface protection layer 84. The colored layer 83 is provided on the adhesive layer 82. The colored layer 83 can be used to decorate or protect the metal plate 5.

[0075] The thickness of the colored layer 83 is preferably 2 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. On the other hand, the thickness of the colored layer 83 is preferably 100 μm or less, more preferably 75 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, and even more preferably 30 μm or less. The colored layer 83 may be a single layer or a multi-layer structure.

[0076] The colored layer 83 contains a coloring agent. Examples of coloring agents include pigments and dyes. Examples of pigments and dyes include carbon black (ink), iron black, titanium white, antimony white, lead yellow, titanium yellow, reddish-brown, cadmium red, ultramarine, cobalt blue, quinacridone red, isoindolinone yellow, phthalocyanine blue, aluminum, brass, titanium dioxide, and pearlescent pigments. As described above, the colored layer 83 may be a single layer or a multi-layer structure. For example, if the colored layer 83 is a two-layer structure, it may be preferable that one of the two layers contains a luminescent pigment. For example, if the colored layer 83 is a two-layer structure, it may be preferable that the layer closer to the biaxially oriented polyester film 81 contains an aluminum pigment and the layer closer to the surface protection layer 84 contains a pigment.

[0077] The coloring agent content is preferably 0.5% by mass or more, more preferably 2% by mass or more, and even more preferably 5% by mass or more, when the colored layer 83 is considered to be 100% by mass. On the other hand, the coloring agent content is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, when the colored layer 83 is considered to be 100% by mass.

[0078] It is preferable that the colored layer 83 contains a resin (hereinafter sometimes referred to as "binder resin"). Because the colored layer 83 contains a binder resin, the occurrence of cracks in the colored layer 83 can be reduced when the laminate 4 is press-molded. Examples of binder resins include acrylic resin, urethane resin, polyester resin, and PVDF (polyvinylidene fluoride). One or more of these can be used. Among these, acrylic resin is preferred. It is preferable that the colored layer 83 does not contain polyester containing alkylene terephthalate units.

[0079] The colored layer 83 can be formed on the adhesive layer 82 by any method. Coating is preferred because it allows for easy formation of the colored layer 83.

[0080] <1.2.1.4. Surface protective layer> The surface protection layer 84 is provided on the colored layer 83. The surface protection layer 84 can reduce scratches on the colored layer 83 and the biaxially oriented polyester film 81 (i.e., it can improve scratch resistance). In addition, the surface protection layer 84 may improve adhesion with the protective film 9. The surface protection layer 84 is preferably transparent. The surface protection layer 84 is preferably weather resistant. The surface protection layer 84 may also be glossy.

[0081] The thickness of the surface protection layer 84 is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. This is because the thicker the surface protection layer 84, the more it is possible to reduce scratches on the colored layer 83 and the biaxially oriented polyester film 81 (i.e., to improve scratch resistance), and also to improve chemical resistance. On the other hand, the thickness of the surface protection layer 84 is preferably 80 μm or less, more preferably 60 μm or less, and even more preferably 50 μm or less. This is because the thinner the surface protection layer 84, the more economical it is. The surface protection layer 84 may be a single layer or a multi-layer structure.

[0082] It is preferable that the surface protection layer 84 contains at least one of a thermosetting resin and a photocurable resin. In other words, it is preferable that the surface protection layer 84 is thermosetting or photocurable. Thermosetting is preferred. That is, it is preferable that the surface protection layer 84 contains a thermosetting resin. This is because the heat generated by shearing when the laminate 4 is press-molded can promote thermosetting. Examples of thermosetting resins include acrylic resin, melamine resin, and urethane resin. Acrylic resin is preferred among these. One or more of these can be used. It is preferable that the surface protection layer 84 does not contain polyester containing alkylene terephthalate units. It is preferable that the surface protection layer 84 contains a crosslinking agent. The surface protection layer 84 may also contain other additives.

[0083] The degree of curing in the surface protection layer 84 may be, for example, fully cured or incompletely cured. Here, fully cured is the state in which curing has reached its final stage. On the other hand, incompletely cured is the state in which curing has not reached its final stage. Incomplete curing is preferred because, when the laminate 4 is press-molded, the surface protection layer 84 can effectively follow the deformation of the metal plate 5. If the surface protection layer 84 contains a thermosetting resin, the degree of curing in the surface protection layer 84 is preferably incompletely thermosetting. The degree of curing can be, for example, stage B.

[0084] The surface protection layer 84 can be formed on the colored layer 83 by any method. For example, the surface protection layer 84 can be formed by coating, melt extrusion, lamination, etc. Among these, coating is preferred because it allows for easy formation of the surface protection layer 84. When forming a two-layer surface protection layer 84, that is, when coating the surface protection layer 84 with paint twice, the drying conditions for the first and second coats may be changed to adjust the degree of hardening of each layer.

[0085] <1.2.2. Protective Film> A protective film 9 is provided on the surface protective layer 84 of the paint substitute film 8. The protective film 9 prevents the paint substitute film 8 from being scratched and also prevents dirt from adhering to the paint substitute film 8.

[0086] The thickness of the protective film 9 is preferably 10 μm or more, more preferably 25 μm or more, and even more preferably 38 μm or more. A thickness of 10 μm or more provides excellent rigidity. The thickness of the protective film 9 is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 75 μm or less, and even more preferably 50 μm or less. This is because the thinner the protective film 9, the more economical it is. The protective film 9 may be a single-layer structure or a multi-layer structure.

[0087] The protective film 9 may contain a resin. Examples of resins include polyethylene resin, polyester resin, polypropylene resin, and polyvinyl chloride resin. Examples of polyester resins include homopolyester resin and copolymer polyester resin. One or more of these can be used. Among these, polyester resin is preferred because it has excellent heat resistance and can reduce uneven stretching of the paint substitute film 8. Polyethylene resin is also preferred.

[0088] Of the two surfaces of the protective film 9, the surface roughness of at least the surface in contact with the hard coat layer is preferably 1 nm or more, more preferably 3 nm or more, and even more preferably 10 nm or more. If it is 10 nm or more, the transportability of the protective film 9 is good, and therefore the handling is good. The surface roughness is preferably 1000 nm or less, more preferably 800 nm or less, and even more preferably 500 nm or less. Since the surface shape of the protective film 9 can be transferred to the surface protective layer 84, if the surface roughness is 1000 nm or less, it is possible to prevent deterioration of the appearance of the surface protective layer 84 as a result.

[0089] Preferably, at least one of the two surfaces of the protective film 9 that is in contact with the surface protective layer 84 is subjected to a delamination treatment. For example, silicone-based delaminating agents, fluorine-based delaminating agents, and long-chain aliphatic delaminating agents can be used for the delamination treatment. Among these, silicone-based delaminating agents are preferred because they are inexpensive.

[0090] The protective film 9 can be formed on the surface protective layer 84 of the paint-alternative film 8 by any method. For example, the protective film 9 can be formed by coating, melt extrusion, lamination, etc. Among these, lamination, i.e., laminating the protective film 9 onto the paint-alternative film 8, is preferred.

[0091] <1.3.Integrated intensity ratio> In laminate 4, the integrated intensity ratio (i.e., the ratio of the first integrated intensity to the second integrated intensity) is 0.2 or more and 1.0 or less. The first integrated intensity is the integrated intensity of the diffraction peak showing the (1-10) plane originating from at least the alkylene terephthalate units of the first polyester and the alkylene terephthalate units of the second polyester. The second integrated intensity is the integrated intensity of the diffraction peak showing the (100) plane originating from at least the alkylene terephthalate units of the first polyester and the alkylene terephthalate units of the second polyester. Here, the (1-10) plane is preferably the (1-10) plane of the polyethylene terephthalate crystal. Therefore, the first integrated intensity is preferably the integrated intensity of the diffraction peak showing at least the (1-10) plane of polyethylene terephthalate. On the other hand, the (100) plane is preferably the (100) plane of the polyethylene terephthalate crystal. Therefore, the second integrated intensity is preferably the integrated intensity of the diffraction peak showing at least the (100) plane of polyethylene terephthalate. An example of the X-ray diffraction pattern of the laminate 4 is shown in Figure 2.

[0092] The integrated intensity ratio can be positioned as an indicator of crystallinity. This will be explained using the example of biaxially oriented polyethylene terephthalate (PET) film. In biaxially oriented PET film, the (100) plane of the PET crystal structure is a crystal plane containing a benzene ring. The (100) plane is almost parallel to the plane of the biaxially oriented PET film (which can also be called the "principal plane"). On the other hand, the (1-10) plane of the PET crystal structure is inclined with respect to the (100) plane, and therefore faces a wider variety of directions compared to the (100) plane. Consequently, in the X-ray diffraction pattern of the biaxially oriented PET film, the influence of the crystallinity of PET on the integrated intensity of the diffraction peak representing the (1-10) plane is smaller than the influence of the crystallinity of PET on the integrated intensity of the diffraction peak representing the (100) plane. Therefore, the smaller the ratio of the integrated intensity of the diffraction peak representing the (1-10) plane to the integrated intensity of the diffraction peak representing the (100) plane, the higher the crystallinity of PET. Thus, this ratio can be positioned as an indicator of crystallinity. This principle also holds true for the biaxially oriented polyester film 81 of the laminate 4. Therefore, the integrated intensity ratio (i.e., the ratio of the first integrated intensity to the second integrated intensity) can be positioned as an indicator of crystallinity.

[0093] Since the integrated intensity ratio is 1.0 or less, the degree of crystallinity is not excessively low, and therefore the heat resistance of the biaxially oriented polyester film 81 can be improved. Thus, it is possible to reduce or prevent the occurrence of irregularities on the surface of the biaxially oriented polyester film 81 that may occur due to the heat received by the paint substitute film 8 when the laminate 4 is press-molded. As a result, it is possible to reduce or prevent deterioration of the surface shape of the paint substitute film 8 that may occur due to that heat. Therefore, it is possible to reduce or prevent deterioration of the appearance (i.e., looks) of the paint substitute film 8 that may occur due to that heat.

[0094] The integrated intensity ratio is preferably 0.9 or less. The integrated intensity ratio may also be 0.8 or less, 0.7 or less, 0.6 or less, or 0.5 or less.

[0095] On the other hand, since the integrated intensity ratio is 0.2 or higher, the degree of crystallinity is not excessively high, and therefore, excessively low adhesion to the metal plate 5 is avoided. Thus, the occurrence of delamination of the paint substitute film 8 from the metal plate 5, in particular, the occurrence of delamination of the paint substitute film 8 from the metal plate 5 after the laminate 4 has been press-formed, can be reduced or prevented.

[0096] The integrated intensity ratio is preferably 0.3 or higher. The integrated intensity ratio may also be 0.4 or higher, 0.5 or higher, 0.6 or higher, or 0.7 or higher.

[0097] The integrated intensity ratio can be controlled, for example, by the heat-fixing temperature or the lamination temperature (specifically, the thermocompression temperature). A higher heat-fixing temperature increases the crystallinity of the biaxially oriented polyester film 81 before lamination, thus lowering the integrated intensity ratio. A higher lamination temperature (specifically, the thermocompression temperature) increases the melting of the crystals, thus raising the integrated intensity ratio. The integrated intensity ratio is also affected by the type of first polyester, the type of second polyester, the stretching temperature, and the stretching ratio. If the laminate 4 includes a protective film 9, the protective film 9 is peeled off before X-ray diffraction (i.e., measurement of X-ray diffraction intensity) is performed.

[0098] <1.4. Method for Manufacturing Laminates> The manufacturing method for the laminate 4 includes a step of pressing a heated metal plate 5 and a paint substitute film 8 or composite film 7 together (hereinafter sometimes referred to as the "pressing step"). Preferably, the manufacturing method for the laminate 4 further includes a step of heating the metal plate 5 (hereinafter sometimes referred to as the "heating step") and a step of cooling the metal plate 5 to which the paint substitute film 8 or composite film 7 has been pressed (hereinafter sometimes referred to as the "cooling step"). If the metal plate 5 is in the form of a roll and the paint substitute film 8 or composite film 7 is also in the form of a roll, the laminate 4 can be manufactured using a roll-to-roll method.

[0099] <1.4.1. Process of heating the metal plate> In this step, the metal plate 5 is heated. By heating the metal plate 5, it becomes possible to heat-press the metal plate 5 onto the paint substitute film 8 or the composite film 7.

[0100] <1.4.2. Crimping Process> In this process, the heated metal plate 5 and the paint substitute film 8 or composite film 7 are pressed together. Specifically, the two are pressed together with layer A 812 of the paint substitute film 8 or layer A 812 of the composite film 7 facing the heated metal plate 5.

[0101] In this process, it is preferable that the temperature of the heated metal plate 5 is above the melting point of layer A 812. If the temperature is above the melting point of layer A 812, it is possible to melt layer A 812, and therefore the metal plate 5 and the coating substitute film 8 or composite film 7 can be heat-pressed together. The temperature of the heated metal plate 5 is more preferably above the sum of the melting point of layer A 812 and 20°C, even more preferably above the sum of the melting point of layer A 812 and 30°C, even more preferably above the sum of the melting point of layer A 812 and 35°C, and even more preferably above the sum of the melting point of layer A 812 and 40°C. Therefore, if the melting point of layer A 812 is 217°C, the temperature of the heated metal plate 5 is more preferably 237°C or higher, even more preferably 247°C or higher, even more preferably 252°C or higher, and even more preferably 257°C or higher. When the temperature of the heated metal plate 5 is equal to or greater than the sum of the melting point of layer A 812 and 20°C, it is possible to effectively reduce the viscosity of layer A 812, and therefore improve the adhesion strength to the metal plate 5.

[0102] The temperature of the heated metal plate 5 is preferably less than or equal to the sum of the melting point of layer B 811 and 10°C, more preferably less than or equal to the sum of the melting point of layer B 811 and 8°C, and even more preferably less than or equal to the sum of the melting point of layer B 811 and 7°C. Therefore, if the melting point of layer B 811 is 255°C, the temperature of the heated metal plate 5 is more preferably 265°C or less, more preferably 263°C or less, and even more preferably 262°C or less. If the temperature of the heated metal plate 5 is less than or equal to the sum of the melting point of layer B 811 and 10°C, it is possible to avoid excessive melting of the crystals of layer B 811, and therefore, it is possible to avoid an excessive decrease in the heat resistance of the biaxially oriented polyester film 81. Note that the temperature of the heated metal plate 5 may also be less than or equal to the melting point of layer B 811.

[0103] <1.4.3. Cooling process> The manufacturing method for the laminate 4 preferably includes a step of cooling the metal plate 5 to which the coating substitute film 8 or composite film 7 is pressed. Cooling can suppress recrystallization, thus preventing the degree of crystallinity of at least layer A 812 from becoming excessively high after lamination. Therefore, it is possible to prevent the adhesion strength with the metal plate 5 from becoming excessively low. Thus, the occurrence of delamination of the coating substitute film 8 from the metal plate 5, in particular, the occurrence of delamination of the coating substitute film 8 from the metal plate 5 after the laminate 4 has been press-formed, can be further reduced or prevented. As an example of a cooling method, a method of water-cooling the metal plate 5 to which the coating substitute film 8 or composite film 7 is pressed can be given. Examples of water-cooling methods include immersing the metal plate 5 to which the coating substitute film 8 or composite film 7 is pressed in a water tank, or spraying water onto the metal plate 5 to which the coating substitute film 8 or composite film 7 is pressed. Examples of the water used in the tank or the water sprayed on include tap water, well water, rainwater, and pure water. Chemicals may be added to the water. The water in the tank, or the water being sprayed, is preferably cold water. The water temperature may be, for example, 5°C or higher, or 15°C or higher. The water temperature is preferably 60°C or lower, more preferably 45°C or lower, even more preferably 35°C or lower, and still more preferably 30°C or lower.

[0104] To effectively suppress recrystallization, it is preferable to start cooling within 5 seconds of pressing the heated metal plate 5 and the coating substitute film 8 or composite film 7 together (for example, immersing the metal plate 5 with the coating substitute film 8 or composite film 7 pressed together in a water bath within 5 seconds of pressing), more preferably within 3 seconds, and even more preferably within 2 seconds.

[0105] <2. Molded products> The molded product of this embodiment can be obtained by press forming the laminate 4. Cold press forming is preferred as the press forming method. Cold press forming may be, for example, deep drawing, or stretch forming. If the surface protective layer 84 of the laminate 4 has not yet hardened, the surface protective layer 84 may be applied after press forming as needed.

[0106] The molded product can be used, for example, in vehicles, ships (e.g., motorboats), home appliances, and audio products. Vehicles are particularly preferred. Examples of vehicles include automobiles, motorcycles, railway vehicles, and airplanes. Automobiles and motorcycles are particularly preferred. When the molded product is used in a vehicle, it is preferable to use it as a vehicle exterior part. As a vehicle exterior part, an exterior panel is preferred, and an automobile exterior panel is more preferred. The molded product may also be used as a construction member or a steel plate product.

[0107] <3. Various modifications can be made to the embodiments described above.> Various modifications can be made to the embodiments described above. For example, one or more of the following modifications can be selected to modify the embodiments described above.

[0108] In the above-described embodiment, a configuration was described in which the laminate 4 includes a protective film 9. However, this embodiment is not limited to this configuration. That is, the laminate 4 does not have to include a protective film 9.

[0109] In the above-described embodiment, a configuration was described in which the coating substitute film 8 includes an adhesive layer 82. However, this embodiment is not limited to this configuration. That is, the laminate 4 does not have to include an adhesive layer 82.

[0110] In the above-described embodiment, a configuration was described in which the colored layer 83 is provided on the adhesive layer 82. However, this embodiment is not limited to this configuration. Other layers may be present between the adhesive layer 82 and the colored layer 83.

[0111] In the above-described embodiment, a configuration was described in which the surface protection layer 84 is provided on the colored layer 83. However, this embodiment is not limited to this configuration. Other layers may be present between the colored layer 83 and the surface protection layer 84.

[0112] In the above-described embodiment, a configuration was described in which the protective film 9 is provided on the surface protective layer 84. However, this embodiment is not limited to this configuration. Other layers may be present between the surface protective layer 84 and the protective film 9.

[0113] In the embodiments described above, a configuration in which the biaxially oriented polyester film 81 has a two-layer structure was described. However, this embodiment is not limited to this configuration. For example, the biaxially oriented polyester film 81 may include other layers between layer B 811 and layer A 812. The biaxially oriented polyester film 81 may include other layers between layer B 811 and the colored layer 83. [Examples]

[0114] The present invention will be described in more detail below with reference to examples and comparative examples. Hereafter, unless otherwise specified, "parts" means "parts by mass" and "%" means "percent mass".

[0115] <Measurement method or evaluation method> (A) Intrinsic viscosity 0.2 g of polyester was dissolved in 50 ml of a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (60 / 40 (mass ratio)) and measured using an Ostwald viscometer at 30°C. The unit is dL / g.

[0116] (B) Melting point (Tm) In differential scanning calorimetry of polyester, the polyester was heated and melted at 300°C for 5 minutes, and then rapidly cooled with liquid nitrogen. Using a DSC-60 differential scanning calorimeter (Shimadzu Corporation), 10 mg of the rapidly cooled polyester was heated at a rate of 20°C / min. In the resulting DSC curve, the endothermic peak temperature based on crystal melting was determined as the melting point. Here, the endothermic peak is an endothermic peak of 0.05 J / g or more associated with crystal melting, appearing at a temperature higher than the baseline shift corresponding to the glass transition point. Meanwhile, the melting point of layer A was determined using a similar method, except that a sample was scraped from layer A. Specifically, the sample scraped from layer A was heated and melted at 300°C for 5 minutes, and then rapidly cooled with liquid nitrogen. Using a DSC-60 differential scanning calorimeter (Shimadzu Corporation), 10 mg of the rapidly cooled sample was heated at 20°C / min. The endothermic peak temperature based on crystal melting was determined as the melting point in the resulting DSC curve. The melting point of layer B was determined using the same method as for layer A, except that a sample was scraped off from layer B.

[0117] (C) Thickness of each layer of the paint replacement film A sample measuring 2 mm in the flow direction and 2 cm in the width direction was cut from the paint substitute film, fixed in an embedding capsule, and then embedded in epoxy resin. The embedded sample was cut perpendicular to the width direction using a microtome (Reichert-Jung Supercut) to obtain a 50 μm thick thin film section. Using a scanning electron microscope (Hitachi 4300SE / N), the samples were observed and photographed at an accelerating voltage of 20 kV. The thickness of each layer was measured from the photographs, and the average thickness of five points was calculated for each layer.

[0118] (D) Surface orientation coefficient According to JIS K 7142-1996 Method A, the refractive index in the flow direction (Nx), the refractive index in the width direction (Ny), and the refractive index in the thickness direction (Nz) of layers A and B of a biaxially oriented polyester film without adhesive treatment were measured using an Abbe refractometer with sodium D-line as the light source. Then, the surface orientation coefficient ΔP of each layer was calculated using the following formula. Surface orientation coefficient ΔP = (Nx + Ny) / 2 - Nz

[0119] (E) Thermal shrinkage rate To determine the thermal shrinkage rate in the MD direction, five test specimens measuring 10 mm wide x 150 mm long were cut from a biaxially oriented polyester film without adhesive treatment. The length direction of these test specimens coincided with the flow direction of the biaxially oriented polyester film, i.e., the MD direction. A pair of gauge marks spaced 100 mm ± 2 mm apart were marked in the center of each test specimen. The distance between the gauge marks (i.e., the distance between the pair of gauge marks) of the test specimens before heating was measured with an accuracy of 0.1 mm. The test specimens were suspended without load in a hot air dryer (ESPEC, PHH-202) and heated at 150°C for 15 minutes. After removing the test specimens from the constant temperature bath and cooling to room temperature, the distance between the gauge marks was measured with an accuracy of 0.1 mm. The thermal shrinkage rate in the MD direction was then calculated using the following formula. Thermal shrinkage rate (%) = {(L0 - L) / L0} × 100 Here, L is the gauge length after heat treatment, and L0 is the gauge length before heat treatment. As mentioned above, the average values ​​of the five test specimens were substituted for L and L0. The thermal shrinkage rate in the TD direction was determined using the same method as for the thermal shrinkage rate in the MD direction. Specifically, five test specimens measuring 10 mm wide x 150 mm long were cut from a biaxially oriented polyester film without any adhesive treatment. The length direction of these test specimens coincided with the width direction of the biaxially oriented polyester film, i.e., the TD direction. A pair of gauge marks spaced 100 mm ± 2 mm apart were marked in the center of each test specimen. The distance between the gauge marks (i.e., the distance between the pair of gauge marks) of the test specimen before heating was measured with an accuracy of 0.1 mm. The test specimens were suspended without load in a hot air dryer (ESPEC, PHH-202) and heated at 150°C for 15 minutes. After removing the test specimens from the constant temperature bath and cooling to room temperature, the distance between the gauge marks was measured with an accuracy of 0.1 mm. Then, the thermal shrinkage rate in the TD direction was determined using the above formula.

[0120] (F) X-ray diffraction Using CuKα as the X-ray source, the X-ray diffraction intensity was measured by the multiple peak separation method under the following conditions: divergence slit 1 / 2°, scattering slit 1 / 2°, receiving slit 0.15 mm, scan speed 5° / min, and incident angle 0.1°. The sample used was a metal plate (specifically, a galvanized steel plate described later) to which an easily bonded biaxially oriented polyester film was pressed. The X-rays were directed onto the sample (i.e., the metal plate to which the easily bonded biaxially oriented polyester film was pressed) along the flow direction of the biaxially oriented polyester film. The ratio of the integrated intensity of the diffraction peak representing the (1-10) plane of polyethylene terephthalate to the integrated intensity of the diffraction peak representing the (100) plane of polyethylene terephthalate (hereinafter, this ratio may be referred to as "(1-10) plane / (100) plane") was determined. In the biaxially oriented polyester film, this (100) plane is a crystal plane containing a benzene ring. This (100) plane is approximately parallel to the plane of the biaxially oriented polyester film (which can also be called the "principal plane").

[0121] (G) Image distortion A 0.6 mm thick zinc alloy plated steel sheet (hereinafter sometimes referred to as "zinc-plated steel sheet") heated to the temperature shown in Table 1 or Table 2 was pressed against a paint substitute film. The zinc-plated steel sheet with the paint substitute film pressed onto it was immersed in a water bath 2 seconds after pressing to cool it to room temperature. A test plate measuring 180 mm in width and 180 mm in length was cut from the zinc-plated steel sheet with the paint substitute film pressed onto it. To form the test plate by drawing, a die with a drawing ratio of 1.3 was used to grip the periphery of the test plate with a load of 15 tons, and the center of the test plate was pressed at room temperature with a load of 100 tons. The drawn test plate, i.e., the molded product, was placed on the floor 50 cm horizontally away from directly below a fluorescent light fixture located 2.5 m above the floor. The molded product placed on the floor had its bottom inner surface facing upwards; specifically, the hard coat layer of the paint substitute film on the bottom inner surface of the molded product was facing the fluorescent light. The image of the fluorescent light reflected on the molded product was visually observed, and the degree of image distortion was determined according to the following criteria. Judgment A: The image of the fluorescent light shows almost no distortion. Judgment B: The image of the fluorescent light is partially distorted. Rating C: The image of the fluorescent light is distorted overall.

[0122] (H) Evaluation of adhesion after cold press forming A cross-shaped cut was made in the center of the molded product (i.e., a test plate formed by deep drawing) produced using the "image distortion" method, specifically on the inner surface of the bottom of the molded product. Specifically, an X-shaped cut was made using a utility knife on the inner surface of the bottom of the molded product, reaching not only the paint substitute film but also the galvanized steel sheet. The molded product was placed in a retort processing unit and subjected to treatment at 120°C, 0.2 MPa, and for 2 hours. The adhesion state of the paint substitute film (specifically, the adhesion state between the paint substitute film and the galvanized steel sheet) of the treated molded product was judged according to the following criteria. Judgment A: No peeling Assessment B: Partial peeling present (some whitening observed) Assessment C: Peeling present (overall whitening observed)

[0123] <Raw materials for biaxially oriented polyester film> The following resin composition was used to form layer B. Resin composition A A mixture of resins B and C was used as resin composition A. Resin B: PET resin, IV = 0.75 dL / g, melting point 255℃, 97.0 parts by mass Resin C: PET resin containing 0.036% by mass of silica particles (average particle size 1.7 μm), IV = 0.75 dL / g, melting point 255°C, 3.0 parts by mass

[0124] Resin composition D A mixture of the following resins E and F was used as resin composition D. Resin E: PET resin, IV = 0.62 dL / g, melting point 255℃, 90.0 parts by mass Resin F: PET resin containing 0.72% by mass of silica particles (average particle size 2.7 μm), IV = 0.62 dL / g, melting point 255°C, 10.0 parts by mass

[0125] Resin composition G A mixture of the following resins F and H was used as the resin composition G. Resin F: PET resin containing 0.72% by mass of silica particles (average particle size 2.7 μm), IV = 0.62 dL / g, melting point 255°C, 10 parts by mass. Resin H: Copolymer polyester resin containing 92.1 mol% ethylene terephthalate units and 7.9 mol% ethylene isophthalate units, IV = 0.62 dL / g, melting point 233°C, 90 parts by mass.

[0126] The following resins were used to form layer A. Resin I Copolymer polyester resin containing 86.0 mol% ethylene terephthalate units and 14.0 mol% ethylene isophthalate units, IV = 0.70 dL / g, melting point 217°C

[0127] Resin J Copolymer polyester resin containing 89.0 mol% ethylene terephthalate units and 11.0 mol% ethylene isophthalate units, IV = 0.63 dL / g, melting point 225°C

[0128] Resin K Copolymer polyester resin containing 80.0 mol% ethylene terephthalate units and 20.0 mol% ethylene isophthalate units, IV = 0.63 dL / g, melting point 198°C

[0129] <Example 1> Preparation of easily bonded biaxially oriented polyester film In the first extruder, the molding material for layer B (specifically, resin composition A) was melted at 280°C, and in the second extruder, the molding material for layer A (specifically, resin I) was melted at 280°C. These were then laminated in a die and extruded into a cooling drum. The unstretched sheet, solidified in the cooling drum, was stretched 3.0 times in the flow direction at 80°C, the surface of layer B was coated with an epoxy adhesive (i.e., an adhesive containing epoxy resin), and then stretched 3.5 times in the width direction at 130°C. The sheet stretched in the width direction was heat-set at 215°C, and then subjected to a 5% relaxation process in the width direction. This resulted in an easily bonded biaxially oriented polyester film with a thickness of 15 μm for layer A and a thickness of 35 μm for layer B. The thickness of the easily bonded layer in the easily bonded biaxially oriented polyester film was 30 nm. The easily bonded biaxially oriented polyester film was wound into a roll.

[0130] Production of paint substitute film A biaxially oriented polyester film treated with an easy-adhesion process was fed out, and a coating solution was applied to the easy-adhesion layer of the biaxially oriented polyester film using a comma coater. The film was then dried in a 90°C drying oven. The coating solution used was a solvent-based paint containing an acrylic urethane resin and 10% by mass of aluminum pigment, with 35% by mass of non-volatile components. This resulted in a raw material, specifically a biaxially oriented polyester film treated with an easy-adhesion process and a 20 μm thick colored layer provided on the easy-adhesion layer. The raw material was then wound into a roll. While the raw material was being fed out, the hard coat coating described later was applied to the colored layer using a comma coater so that the hard coat layer thickness was 30 μm, and then thoroughly dried in a drying oven at 90°C. A paint substitute film was obtained using this procedure. The hard coat layer constituting the paint substitute film was in a semi-cured state, i.e., not fully cured.

[0131] Hard coat paint 150 parts by mass of methyl isobutyl ketone were charged into a four-necked flask equipped with a condenser, stirrer, thermometer, and nitrogen inlet tube, and the mixture was heated while stirring under a nitrogen atmosphere. When the temperature in the flask reached 74°C, this temperature was maintained as the synthesis temperature, and a monomer solution consisting of 3 parts by mass of methyl methacrylate, 82.54 parts by mass of n-butyl methacrylate, 12.85 parts by mass of 4-hydroxybutyl acrylate, 0.61 parts by mass of methacrylic acid, 1 part by mass of Funcryl FA-711MM (manufactured by Hitachi Chemical Co., Ltd., pentamethylpiperidinyl methacrylate), and 0.1 parts by mass of azobisisobutyronitrile was added dropwise to the flask over 2 hours. Starting 1 hour after the end of monomer addition, 0.02 parts by mass of azobisisobutyronitrile were added every hour to continue the reaction until the amount of unreacted monomer in the monomer solution was 1% or less. When the amount of unreacted monomer was reduced to 1% or less, the reaction was terminated by cooling, yielding an acrylic copolymer solution with a solid content of approximately 40% by mass. To this acrylic copolymer solution, 59.9 parts by mass (solid mass) of Duranate "P301-75E" (manufactured by Asahi Kasei Chemicals, a polyisocyanate variant of hexamethylene diisocyanate) was added as a polyisocyanate compound, and then methyl isobutyl ketone was added to bring the solid content to 30% by mass, and the mixture was stirred to obtain a hard coat coating.

[0132] Fabrication of galvanized steel sheets with a paint substitute film pressed onto them. A galvanized steel sheet (specifically, a 0.6 mm thick steel sheet coated with a zinc alloy) heated to the temperatures shown in Table 1 was pressed against a paint substitute film. Two seconds after pressing, the galvanized steel sheet with the paint substitute film pressed onto it was immersed in a water bath (specifically, a water bath containing 23°C water) and cooled to room temperature. This resulted in a galvanized steel sheet with the paint substitute film pressed onto it.

[0133] Fabrication of biaxially oriented polyester film without easy-adhesion treatment A biaxially oriented polyester film without easy-adhesion treatment was prepared using the same method as a biaxially oriented polyester film with easy-adhesion treatment, except that the easy-adhesion treatment was not performed.

[0134] <Examples 2-4 and Comparative Examples 1-6 (strictly speaking, Comparative Examples 1-2 and 4-6)> Except for using the resin listed in Table 1 or Table 2 as the resin for forming layer A, adopting the film-forming conditions (stretching ratio, stretching temperature, heat-fixing temperature) listed in Table 1 or Table 2, and having the thicknesses of layer A and layer B as listed in Table 1 or Table 2, a biaxially oriented polyester film with easy-adhesion treatment, a coating substitute film, and a biaxially oriented polyester film without easy-adhesion treatment were prepared in the same manner as in Example 1. Except that the temperature at which the galvanized steel sheet was heated was as shown in Table 1 or Table 2, a galvanized steel sheet with a paint substitute film pressed onto it was prepared in the same manner as in Example 1.

[0135] <Result> The table containing the results is shown below. [Table 1] [Table 2]

[0136] In these tables, the (1-10) plane / (100) plane values ​​were determined by measuring the X-ray diffraction intensity of a galvanized steel sheet to which an easily bonded biaxially oriented polyester film was pressed as a sample. When a galvanized steel sheet with a paint substitute film pressed onto it was used as a sample, and the X-ray diffraction intensity was measured using the method described above, the (1-10) plane / (100) plane yielded the same result as when a galvanized steel sheet with an easily bonded biaxially oriented polyester film pressed onto it was used as a sample.

[0137] In Comparative Example 1, where the ratio of (1-10) planes to (100) planes was 0.12, the adhesion was rated as C. This is thought to be because the degree of crystallinity was excessively high, and therefore the adhesion to the metal plate was excessively low.

[0138] In Comparative Example 4, where the ratio of (1-10) planes to (100) planes was 0.07, the adhesion was rated as B. This is thought to be because the degree of crystallinity was excessively high, and therefore the adhesion to the metal plate was excessively low. As shown above, the adhesion of Comparative Example 4 was superior to that of Comparative Example 1. In this regard, since the thermal shrinkage rate of Comparative Example 4 was smaller than that of Comparative Example 1, it is considered that in Comparative Example 4, the thermal shrinkage when the galvanized steel sheet and the paint substitute film were pressed together was small, and therefore, the decrease in adhesive strength with the galvanized steel sheet that could be caused by thermal shrinkage was small. In addition, since the surface orientation coefficient of layer A in Comparative Example 4 was smaller than that of layer A in Comparative Example 1, it is considered that in Comparative Example 4, layer A was more fluid when the galvanized steel sheet and the paint substitute film were pressed together.

[0139] In Comparative Example 5, where the ratio of (1-10) faces to (100) faces was 0.11, the adhesion was rated as C. As shown above, the adhesion of Comparative Example 5 was inferior to that of Comparative Example 4. Since the thermal shrinkage rate of Comparative Example 5 was greater than that of Comparative Example 4, it is considered that in Comparative Example 5, the thermal shrinkage when the galvanized steel sheet and the paint substitute film were pressed together was greater, and therefore, the decrease in adhesive strength with the galvanized steel sheet due to thermal shrinkage was greater.

[0140] In Comparative Example 6, although the ratio of (1-10) sides to (100) sides was 1.48, the adhesion was rated as B. This is thought to be because the thermal shrinkage rate was exceptionally large, resulting in exceptionally large thermal shrinkage when the galvanized steel sheet and the paint substitute film were pressed together. Consequently, the decrease in adhesive strength with the galvanized steel sheet, which may be due to thermal shrinkage, was also exceptionally large.

[0141] In Comparative Example 2, where the ratio of (1-10) planes to (100) planes was 1.21, the image distortion was C. This is thought to be because the degree of crystallinity was excessively low, and therefore the heat resistance of the biaxially oriented polyester film was poor. In Comparative Example 6, where the ratio of (1-10) planes to (100) planes was 1.48, the image distortion was also C.

[0142] In Example 4, although the ratio of (1-10) planes to (100) planes was 0.32, the image distortion was B. This is thought to be because the plane orientation coefficient of layer B in Example 4 was small, causing wrinkles or bubbles to form in the paint substitute film due to the heat received by the paint substitute film when the galvanized steel sheet and the paint substitute film were pressed together (i.e., heat during lamination).

[0143] In Comparative Example 4, although the ratio of (1-10) planes to (100) planes was 0.07, the image distortion was B. This is thought to be because the plane orientation coefficient of layer B was small, causing wrinkles or bubbles to form in the coating substitute film due to the heat during lamination.

[0144] Although both Example 4 and Comparative Example 4 showed image distortion of B, the degree of distortion in Example 4 was less than that of Comparative Example 4.

[0145] In Comparative Example 5, although the ratio of (1-10) planes to (100) planes was 0.11, the image distortion was B. This is thought to be because the plane orientation coefficient of layer B was small, causing wrinkles or bubbles to form in the coating substitute film due to the heat during lamination. [Industrial applicability]

[0146] This invention can provide laminates, molded products, vehicle exterior parts, and the like, and is therefore industrially applicable. [Explanation of Symbols]

[0147] 4...Laminate, 5...Metal plate, 7...Composite film, 8...Paint substitute film, 9...Protective film, 81...Biaxially oriented polyester film, 82...Adhesive layer, 83...Coloring layer, 84...Surface protective layer, 811...B layer, 812...A layer

Claims

1. A metal plate and The paint substitute film laminated to the metal plate and A laminate containing, The aforementioned paint substitute film includes a biaxially oriented polyester film, a coloring layer, and a surface protective layer. The biaxially oriented polyester film comprises a first layer and a second layer. The first layer is located between the second layer and the colored layer. The first layer contains a first polyester containing alkylene terephthalate units, The second layer contains a second polyester containing alkylene terephthalate units, The melting point of the first layer is higher than the melting point of the second layer. In the X-ray diffraction pattern of the laminate, the ratio of the integrated intensity of the diffraction peaks representing the (1-10) plane, which originate from at least the alkylene terephthalate units of the first polyester and the alkylene terephthalate units of the second polyester, to the integrated intensity of the diffraction peaks representing the (100) plane, which originate from at least the alkylene terephthalate units of the first polyester and the alkylene terephthalate units of the second polyester, is 0.2 or more and 1.0 or less, and the (1-10) plane is the following crystal plane: [Math 1] Laminated structure.

2. The aforementioned paint substitute film further includes an adhesive layer, The adhesive layer is located between the biaxially oriented polyester film and the colored layer. The laminate according to claim 1.

3. The laminate according to claim 2, wherein the thickness of the adhesive layer is 10 nm or more and 200 nm or less.

4. The laminate according to claim 1, wherein the colored layer contains a resin and a coloring agent.

5. The alkylene terephthalate units of the first polyester include ethylene terephthalate units, The alkylene terephthalate units of the second polyester include ethylene terephthalate units, The (1-10) surface is a (1-10) surface derived from at least the ethylene terephthalate units of the first polyester and the ethylene terephthalate units of the second polyester, The (100) surface is a (100) surface derived from at least the ethylene terephthalate units of the first polyester and the ethylene terephthalate units of the second polyester. The laminate according to claim 1.

6. When the repeating units of the first polyester are set to 100 mol%, the ethylene terephthalate units are 85 mol% or more. When the repeating units of the second polyester are set to 100 mol%, the ethylene terephthalate units are 60 mol% or more. The laminate according to claim 5.

7. Includes a protective film, The laminate according to claim 1, wherein the metal plate, the coating substitute film, and the protective film are stacked in this order.

8. A laminate according to claim 1, used for manufacturing vehicle exterior parts.

9. A molded article obtained by press-forming a laminate according to any one of claims 1 to 8.

10. A vehicle exterior part obtained by press-forming a laminate according to any one of claims 1 to 8.

11. A method for manufacturing a laminate according to any one of claims 1 to 8, The process of heating the metal plate, The process includes a step of pressing the heated metal plate and the paint substitute film or composite film together, wherein the composite film includes the paint substitute film and a protective film provided on the surface protective layer of the paint substitute film. A method for manufacturing laminates.

12. The method for manufacturing a laminate according to claim 11, further comprising the step of starting cooling within 5 seconds after pressing the metal plate and the coating substitute film or the composite film together.

13. The surface orientation coefficient of the first layer of the coating substitute film or composite film pressed onto the metal plate is 0.165 or more and 0.180 or less. The surface orientation coefficient of the second layer of the coating substitute film or composite film pressed onto the metal plate is 0.100 or more and 0.135 or less. A method for manufacturing a laminate according to claim 11.

Citation Information

Patent Citations

  • Biaxially oriented laminated polyester film for molding and simultaneous decoration

    JP2009029073A

  • Biaxially oriented laminated polyester film for molding

    JP2009029074A

  • Laminated film for molding and molded article using the same

    JP2016168833A

  • Laminated film

    JP2020192787A

  • Method for producing metal member, method for producing resin member, and method for producing exterior part

    WO2019078369A1