Carbon dioxide adsorbent for pressure swing method

An aluminum silicate composite with a Si/Al molar ratio of 1.0 to 1.5, synthesized from water glass and aluminum sulfate, addresses the limitations of existing adsorbents by achieving high carbon dioxide adsorption and desorption capacity at 10 to 100 kPa pressures, enabling efficient recovery and reducing production costs.

JP7953850B2Active Publication Date: 2026-11-19NATIONAL INSTITUTE OF ADVANCED INDUSTRIAL SCIENCE & TECHNOLOGY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022127770
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-08-10
Publication Date
2026-11-19
Estimated Expiration
2042-08-10

AI Technical Summary

Technical Problem

Existing carbon dioxide adsorbents for pressure swing methods have limited adsorption and desorption capacity at carbon dioxide pressures of 10 to 100 kPa, and require expensive raw materials for production.

Method used

A carbon dioxide adsorbent comprising an aluminum silicate composite with a Si/Al molar ratio of 1.0 to 1.5, synthesized using water glass and aluminum sulfate, exhibiting broad peaks around 2θ = 21, 26, 34, and 39° in X-ray powder diffraction, achieves high adsorption and desorption capacity of 4.5 wt% or more in the range of 10 to 100 kPa without requiring vacuum evacuation.

Benefits of technology

The adsorbent efficiently separates and recovers carbon dioxide from exhaust gas with a concentration of about 10 vol% by the pressure swing adsorption method, reducing production costs and eliminating the need for vacuum devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007953850000001
    Figure 0007953850000001
  • Figure 0007953850000002
    Figure 0007953850000002
Patent Text Reader

Abstract

To provide a carbon dioxide adsorbent for a pressure swing method which increases a pressure to be an atmospheric pressure or higher and adsorbs carbon dioxide contained in a combustion exhaust gas, and can desorb the carbon dioxide without lowering the pressure to the atmospheric pressure or lower by only lowering the pressure to the atmospheric pressure, in which an adsorption / desorption amount under a pressure of the carbon dioxide is within a range of 10-100 kPa is excellent, the carbon dioxide adsorbent including an aluminum silicate composite body, as an active ingredient.SOLUTION: An aluminum silicate composite body having a broad peak in the vicinity of 2θ=21, 26, 34 and 39°, in X-ray powder analysis in which an Si / Al molar ratio is 1.0-1.5 and Cu is used as an X-ray source, has excellent carbon dioxide adsorption performance having an adsorption / desorption amount under a pressure of carbon dioxide is within a range of 10-100 kPa of 4.5 wt.% or more, and is usable as an active ingredient of a carbon dioxide adsorbent in a pressure swing adsorption method.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a carbon dioxide adsorbent for pressure swing processes, and particularly relates to a carbon dioxide adsorbent containing an aluminosilicate complex as an active ingredient, which is capable of adsorbing carbon dioxide contained in combustion exhaust gas and the like by increasing the pressure to atmospheric pressure or higher, and desorbing the adsorbed carbon dioxide only by lowering the pressure, without reducing the pressure to below atmospheric pressure.

Background Art

[0002] Technologies relating to gas recovery or separation have been developed in accordance with respective purposes and applications. Among them, carbon dioxide separation and recovery technology is strongly expected to be put into practical use as an important fundamental technology supporting the next-generation industries toward carbon neutrality, and has become a critical issue for its realization.

[0003] Conventionally, as methods for recovering carbon dioxide from dry gas, porous substances such as silica gel, alumina, zeolite, activated carbon and diatomaceous earth, and adsorbents such as silica, calcium oxide, sodium oxide, potassium oxide and iron oxide have been used (Patent Documents 1 and 2).

[0004] Separation and recovery of carbon dioxide by a pressure swing adsorption (PSA) method has also been studied. The pressure swing adsorption method is a method of performing adsorption and desorption under reduced pressure at normal temperature, and most embodiments use zeolite 13X as the adsorbent (Non-Patent Document 1). Zeolite 13X has an excellent carbon dioxide adsorption amount in the range of about 0 to 1 atm. However, there has been a problem that when desorbing the adsorbed carbon dioxide, vacuum evacuation must be performed to reduce the pressure to 0.2 atm or lower.

[0005] Against the above background, in the pressure swing adsorption method, for the purpose of recovering carbon dioxide at lower cost, an adsorbent has been developed that can desorb carbon dioxide, which was adsorbed by increasing the pressure to atmospheric pressure or higher, only by lowering the pressure to atmospheric pressure without vacuum evacuation (Patent Document 3).

[0006] The adsorbent described in Patent Document 3 uses an aqueous solution of sodium orthosilicate and an aqueous solution of aluminum chloride as raw materials, mixes them so that the molar ratio of silicon to aluminum (hereinafter referred to as "Si / Al molar ratio") is 0.7 to 1.0, and is synthesized by heating at 110°C or higher. The active ingredient is a composite of a low-crystalline layered clay mineral and amorphous aluminum silicate (hereinafter referred to as "aluminum silicate composite") which has broad peaks around 2θ = 20, 26, 35, and 40° in X-ray powder diffraction. It has been shown that the adsorption and desorption amount of this aluminum silicate composite is 12 wt% or more at a pressure of 100 to 900 kPa, which is more than twice as much as the adsorption and desorption amount of the comparative example zeolite 13X (5.4 wt%) in the same pressure range.

[0007] Thus, while the aluminum silicate composite described in Patent Document 3 exhibits excellent carbon dioxide adsorption and desorption at pressures of 100 to 900 kPa in the pressure swing adsorption method, it has the drawback of requiring relatively expensive raw materials for its production.

[0008] On the other hand, as a method for inexpensively obtaining aluminum silicate composites having broad peaks around 2θ = 20, 26, 35, and 40° in X-ray powder diffraction, a method has been developed in which water glass and an aqueous solution of aluminum sulfate are mixed so that the Si / Al molar ratio is 0.7 to 1.3 and the pH at the time of mixing is 3.5 to 4.8, stirred, then alkali is added to adjust the pH to 6 to 10, followed by desalting and heat treatment at 120 to 300°C (Patent Document 4). However, the carbon dioxide adsorption and desorption performance of the obtained aluminum silicate composite in the pressure swing adsorption method has not been investigated at all. [Prior art documents] [Patent Documents]

[0009] [Patent Document 1] Japanese Patent Publication No. 2003-019435 [Patent Document 2] Japanese Patent Publication No. 2005-040753 [Patent Document 3] International Publication No. 2009 / 084632 [Patent Document 4] Japanese Patent Publication No. 2019-26487 [Non-patent literature]

[0010] [Non-Patent Document 1] Latest Adsorption Technology Handbook, Revised Third Edition, NTS Publishing (2020), pp. 141-145 [Disclosure of the Invention] [Problems that the invention aims to solve]

[0011] In carbon dioxide recovery using the pressure swing method, which involves raising the pressure to 10 atmospheres and then returning it to atmospheric pressure, if the exhaust gas has a carbon dioxide concentration of about 10 vol%, the carbon dioxide will be adsorbed and desorbed within a partial pressure range of 10 to 100 kPa. However, as mentioned above, the carbon dioxide adsorbent containing an aluminum silicate composite as an active ingredient, while having an adsorption / desorption capacity of 12 wt% or more at carbon dioxide pressures of 100 to 900 kPa, has an adsorption / desorption capacity of 4.3 wt% in the range of carbon dioxide pressures of 10 to 100 kPa (see Comparative Example 1 described later), and further improvement in adsorption / desorption capacity is desired.

[0012] The present invention has been made in view of the above circumstances, and aims to provide a carbon dioxide adsorbent for the pressure swing method that can adsorb carbon dioxide contained in combustion exhaust gas and the like by raising the pressure above atmospheric pressure, and then desorb it by simply lowering the pressure to atmospheric pressure without dropping it below atmospheric pressure, wherein the carbon dioxide adsorbent has an excellent adsorption and desorption capacity in the range of carbon dioxide pressure from 10 to 100 kPa. [Means for solving the problem]

[0013] As a result of repeated studies to achieve the above objective, the inventors have obtained a new finding that by setting the Si / Al molar ratio to 1.0 to 1.5, an aluminum silicate composite with a carbon dioxide adsorption / desorption amount of 4.5 wt% or more at a carbon dioxide pressure in the range of 10 to 100 kPa can be obtained, even when using relatively inexpensive raw materials such as water glass and aluminum sulfate.

[0014] The present invention was completed based on the aforementioned findings, and the means for solving the above problems include the following embodiments. [1] A carbon dioxide adsorbent for the pressure swing method, comprising an aluminum silicate composite as the active ingredient, having a Si / Al molar ratio of 1.0 to 1.5 and exhibiting broad peaks around 2θ = 21, 26, 34, and 39° in X-ray powder diffraction using Cu as the X-ray source. [2] The aluminum silicate composite is a carbon dioxide adsorbent for the pressure swing method of [1], wherein the adsorption and desorption amount of carbon dioxide in the range of 10 to 100 kPa is 4.5 wt% or more. [3] A carbon dioxide adsorbent for the pressure swing method according to [1] or [2], wherein the Si / Al molar ratio is 1.1 to 1.4. A method for separating and recovering carbon dioxide from exhaust gas by pressure swing adsorption using one of the pressure swing adsorbents for the pressure swing method described in [4], [1], and [3]. [Effects of the Invention]

[0015] According to the present invention, it is possible to provide a carbon dioxide adsorbent for the pressure swing method that has excellent carbon dioxide adsorption performance in the range of 10 to 100 kPa. Furthermore, by using the carbon dioxide adsorbent for the pressure swing method of the present invention, it becomes possible to efficiently separate and recover carbon dioxide from exhaust gas with a carbon dioxide concentration of about 10 vol% by the pressure swing adsorption method. [Brief explanation of the drawing]

[0016] [Figure 1] This figure shows the powder X-ray diffraction patterns of the products obtained in the examples and comparative examples, using Cu as the X-ray source. [Figure 2] Figure showing the carbon dioxide adsorption amount in the carbon dioxide adsorption isotherm of the products obtained in Examples and Comparative Examples [Mode for Carrying Out the Invention]

[0017] Hereinafter, the present invention will be described with reference to more specific embodiments of the present invention, including the best mode thereof. However, the present invention is not limited to the following embodiments, and various other embodiments are included within the scope of the technical idea described in the claims. In addition, when a numerical range or the like is expressed using "~", it means that the numerical values described as the lower limit and the upper limit are also included.

[0018] <Aluminosilicate Composite> The aluminosilicate composite, which is the active ingredient of the carbon dioxide adsorbent for pressure swing processes of the present invention, is a composite of a low-crystalline layered clay mineral and amorphous aluminosilicate, having a Si / Al molar ratio of 1.0 to 1.5 and broad peaks around 2θ = 21, 26, 34, and 39° in X-ray powder diffraction, and has excellent carbon dioxide adsorption and desorption performance with an adsorption and desorption amount of 4.5 wt% or more in the carbon dioxide pressure range of 10 to 100 kPa in the carbon dioxide adsorption isotherm.

[0019] The above-mentioned aluminosilicate composite in the present invention is a hydrated aluminum silicate whose main constituent elements are silicon (Si), aluminum (Al), oxygen (O), and hydrogen (H), and which is constructed with a large number of Si-O-Al bonds.

[0020] <Method for Producing Aluminosilicate Composite> The aluminosilicate composite of the present invention can be obtained by mixing water glass and an aqueous aluminum sulfate solution so that the Si / Al molar ratio is 1.0 to 1.5 and the pH during mixing is 3.5 to 4.8, stirring the mixture, then adding an alkali thereto to adjust the pH to 6 to 10, and performing a desalting treatment and a heat treatment at 120°C or higher and 300°C or lower.

[0021] Thus, the Si / Al molar ratio of an aluminum silicate composite can be easily determined from the ratio of silicon (Si) and aluminum (Al) sources used as raw materials during the production of the aluminum silicate composite. However, the Si / Al molar ratio of the final product, the aluminum silicate composite, can also be determined by quantitatively determining Si and Al using standard methods such as ICP emission spectrometry.

[0022] (A mixture of water glass and aluminum sulfate solution) In this invention, it is necessary to mix water glass and an aqueous aluminum sulfate solution such that the Si / Al molar ratio is in the range of 1.0 to 1.5, and preferably the lower limit of the Si / Al molar ratio is 1.1 or higher. Furthermore, it is necessary to mix the water glass and the aqueous aluminum sulfate solution so that the pH at the time of mixing is 3.5 to 4.8, and the concentrations of the water glass and the aqueous aluminum sulfate solution are adjusted accordingly. If necessary, preliminary tests may be performed to determine the properties of the water glass and the aqueous aluminum sulfate solution.

[0023] The method for mixing to achieve the predetermined range described above is not particularly limited, but it is preferable to prepare solutions of water glass and aluminum sulfate to achieve predetermined concentrations, and then mix them.

[0024] Specifically, aluminum sulfate is dissolved in pure water to prepare an aqueous solution of a predetermined concentration. Water glass is diluted with pure water and / or sodium hydroxide, or diluted with a sodium hydroxide aqueous solution whose concentration has been adjusted with pure water, so that the pH is 3.5 to 4.8 when mixed with the aluminum sulfate aqueous solution, thereby preparing a solution of a predetermined concentration.

[0025] The silicon concentration in the water glass is preferably 1 to 3000 mmol / L, and the aluminum concentration in the aluminum sulfate aqueous solution is preferably 1 to 3000 mmol / L. More preferably, a water glass with a silicon concentration of 1 to 1500 mmol / L is mixed with an aluminum sulfate aqueous solution with an aluminum concentration of 1 to 1500 mmol / L.

[0026] The aqueous solution of water glass of a predetermined concentration and the aqueous solution of aluminum sulfate of a predetermined concentration, prepared in this manner, are mixed so that the pH at the time of mixing is 3.5 to 4.8, and then stirred until a homogeneous solution is obtained.

[0027] (pH adjustment, desalination treatment, heat treatment) After stirring, the solution is adjusted to a pH of 6-10 with alkali, followed by desalting and heat treatment at a temperature between 120°C and 300°C. The final dried solid is the aluminum silicate composite.

[0028] The desalting treatment in this invention is a process of removing coexisting ions from the product obtained by pH adjustment (a solution containing amorphous aluminum silicate), and the method is not particularly limited. Preferably, it is carried out by dehydration and / or washing. Specifically, by separating the solids from the solution using centrifugation or a filter press, a considerable amount of coexisting ions can be removed as a solution containing their salts. Furthermore, in desalting treatment by centrifugation, the amount of salt from coexisting ions contained in the solids can be further reduced by adding pure water to the solids separated by centrifugation, stirring, and then centrifugation again.

[0029] In this invention, the heat treatment at 120°C to 300°C is a treatment to convert amorphous aluminum silicate into an aluminum silicate composite consisting of a low-crystallinity layered clay mineral and amorphous aluminum silicate by heating. The heating temperature depends on the treatment time, but the treatment time can be shortened by increasing the temperature. For example, by heating at 120°C, it is possible to synthesize the aluminum silicate composite in 2 days, and at 180°C, it can be synthesized in 3 hours.

[0030] Furthermore, in the present invention, the order and number of times the desalination treatment and the heat treatment steps are performed are not limited. For example, not only the desalination treatment step → heat treatment step, or the heat treatment step → desalination treatment step are included, but also the desalination treatment step → heat treatment step → desalination treatment step, etc.

[0031] <Method for separating and recovering carbon dioxide using pressure swing adsorption method> The present invention provides a method for separating and recovering carbon dioxide by pressure swing adsorption, using an aluminum silicate composite manufactured as described above as an active ingredient, i.e., a carbon dioxide adsorbent. There are no particular limitations on the apparatus used in the pressure swing adsorption method; for example, conventionally known apparatuses, such as those described in Non-Patent Document 1, can be applied.

[0032] The pressure swing adsorption method generally uses multiple adsorption towers. This is because, while one adsorption tower is adsorbing and separating carbon dioxide from exhaust gas, etc., another adsorption tower can be used to desorb carbon dioxide, allowing for continuous separation and recovery of carbon dioxide through adsorption and desorption. At least one, preferably all, of these multiple adsorption towers can be filled with the carbon dioxide adsorbent for the pressure swing method of the present invention. The size of the adsorption towers and the amount of carbon dioxide adsorbent for the pressure swing method to be filled into them can be adjusted according to the amount of exhaust gas, etc. to be treated and the carbon dioxide concentration in said exhaust gas, etc.

[0033] The carbon dioxide adsorbent for the pressure swing method of the present invention is used to adsorb carbon dioxide into an adsorption tower. This tower does not require a vacuum pump or other depressurization device to reduce the pressure inside the tower to below atmospheric pressure. Instead, carbon dioxide can be desorbed by simple means, such as connecting the inside of the tower to a normal pressure (atmospheric pressure) space. As a result, a vacuum device is not required, reducing electricity costs and maintenance costs. [Examples]

[0034] Next, the present invention will be specifically described based on examples and comparative examples, but the present invention is not limited in any way by the following examples.

[0035] (Example 1) A 100 mL solution of water glass was prepared by diluting water glass with a 20% sodium hydroxide aqueous solution to achieve a Si concentration of 1.00 mol / L. Separately, a 100 mL solution of aluminum sulfate was prepared by dissolving aluminum sulfate in pure water and diluting it with 2N sulfuric acid and pure water to achieve an Al concentration of 0.83 mol / L. Next, the aluminum sulfate aqueous solution was mixed with the water glass solution and stirred with a stirrer. At this time, the Si / Al molar ratio was 1.2, and the pH after 30 minutes of stirring was 4.0. Furthermore, 12.5 mL of 20% sodium hydroxide aqueous solution was added to this mixed solution to obtain a suspension with a pH of 7.0. The obtained suspension was centrifuged to separate the solids, and then water was added again to the separated solids and stirred, followed by another centrifugation to perform desalination. The recovered material after desalination was dispersed in pure water to a total volume of 200 mL, and then stirred for 1 hour to prepare a suspension. 70 mL of the prepared suspension was measured into a 100 mL Teflon® container, placed in a stainless steel rotary reaction vessel, and heated at 200°C for 16 hours for heat treatment. After heat treatment, dehydration was performed by centrifugation, and the resulting solid was dried at 60°C for 1 day.

[0036] (Example 2) A 100 mL solution of water glass was prepared by diluting water glass with a 20% sodium hydroxide aqueous solution to achieve a Si concentration of 1.00 mol / L. Separately, a 100 mL solution of aluminum sulfate was prepared by dissolving aluminum sulfate in pure water and diluting it with 2N sulfuric acid and pure water to achieve an Al concentration of 0.91 mol / L. Next, the aluminum sulfate aqueous solution was mixed with the water glass solution and stirred with a stirrer. At this time, the Si / Al molar ratio was 1.1, and the pH after 30 minutes of stirring was 4.0. Furthermore, 12.5 mL of a 20% sodium hydroxide aqueous solution was added to this mixed solution to obtain a suspension with a pH of 7.0. The following operations were carried out in the same manner as in Example 1 to obtain a solid.

[0037] (Example 3) A 100 mL solution of water glass was prepared by diluting water glass with a 20% sodium hydroxide aqueous solution to achieve a Si concentration of 1.00 mol / L. Separately, a 100 mL solution of aluminum sulfate was prepared by dissolving aluminum sulfate in pure water and diluting it with 2N sulfuric acid and pure water to achieve an Al concentration of 0.71 mol / L. Next, the aluminum sulfate aqueous solution was mixed with the water glass solution and stirred with a stirrer. At this time, the Si / Al molar ratio was 1.4, and the pH after 30 minutes of stirring was 4.0. Furthermore, 12.5 mL of a 20% sodium hydroxide aqueous solution was added to this mixed solution to obtain a suspension with a pH of 7.0. The following operations were carried out in the same manner as in Example 1 to obtain a solid.

[0038] (Comparative Example 1) As a comparative example, the substance shown in the above-mentioned Patent Document 3 (International Publication No. 2009 / 084632) was synthesized according to the manufacturing method of the present invention as follows. A 100 mL aqueous solution of sodium orthosilicate was prepared by diluting it with pure water to a Si concentration of 0.36 mol / L. Separately, a 100 mL aqueous solution of aluminum chloride with an Al concentration of 0.45 mol / L was prepared by dissolving aluminum chloride in pure water. Next, the sodium orthosilicate aqueous solution was mixed with the aluminum chloride aqueous solution and stirred with a stirrer. The Si / Al molar ratio at this time was 0.8, and the pH after 30 minutes of stirring was 3.6. Furthermore, 7 mL of 1N sodium hydroxide aqueous solution was added to this mixed solution to obtain a suspension with a pH of 7.0. The obtained suspension was centrifuged and desalted twice. The recovered material after desalting was dispersed in pure water to a total volume of 200 mL, and then stirred for 1 hour to prepare a suspension. 70 mL of the prepared suspension was measured into a 100 mL Teflon® container, placed in a stainless steel rotary reaction vessel, and heated at 200 °C for 16 hours to perform heat treatment. After heat treatment, dehydration was performed by centrifugal separation, and the resulting solid was dried at 60°C for one day.

[0039] (Comparative Example 2) A 100 mL solution of water glass was prepared by diluting water glass with a 20% sodium hydroxide aqueous solution to achieve a Si concentration of 1.00 mol / L. Separately, a 100 mL solution of aluminum sulfate was prepared by dissolving aluminum sulfate in pure water and diluting it with 2N sulfuric acid and pure water to achieve an Al concentration of 0.63 mol / L. Next, the aluminum sulfate aqueous solution was mixed with the water glass solution and stirred with a stirrer. At this time, the Si / Al molar ratio was 1.6, and the pH after 30 minutes of stirring was 4.0. Furthermore, 12.5 mL of a 20% sodium hydroxide aqueous solution was added to this mixed solution to obtain a suspension with a pH of 7.0. The following operations were carried out in the same manner as in Example 1 to obtain a solid.

[0040] (Comparative Example 3) A 100 mL solution of water glass was prepared by diluting water glass with a 20% sodium hydroxide aqueous solution to achieve a Si concentration of 1.00 mol / L. Separately, a 100 mL solution of aluminum sulfate was prepared by dissolving aluminum sulfate in pure water and diluting it with 2N sulfuric acid and pure water to achieve an Al concentration of 0.50 mol / L. Next, the aluminum sulfate aqueous solution was mixed with the water glass solution and stirred with a stirrer. At this time, the Si / Al molar ratio was 2.0, and the pH after 30 minutes of stirring was 4.0. Furthermore, 12.5 mL of a 20% sodium hydroxide aqueous solution was added to this mixed solution to obtain a suspension with a pH of 7.0. The following operations were carried out in the same manner as in Example 1 to obtain a solid.

[0041] The products obtained in Examples 1-3 and Comparative Examples 1-3 were measured by powder X-ray diffraction using Cu as the X-ray source. The powder X-ray diffraction patterns of the products obtained in Examples 1-3 and Comparative Examples 1-3 are shown. As shown in Figure 1, broad peaks were observed around 2θ = 20, 26, 35, and 39° in all samples, clearly indicating that they were amorphous aluminum silicate composites. The peaks observed at 20 and 35° were obtained from the reflection of the hk0 plane of the layered clay mineral, and the absence of the 00l reflection commonly seen in layered clay minerals suggests that these are low-crystallinity layered clay minerals with almost no thickness in the layering direction. The broad peaks around 2θ = 26 and 39° are characteristic peaks of amorphous aluminum silicates. From these results, it was confirmed that the materials obtained in Examples 1-3 and Comparative Examples 1-3 are aluminum silicate composites consisting of low-crystallinity layered clay minerals and amorphous aluminum silicates.

[0042] In the products obtained in Examples 1-3 and Comparative Examples 1-3, carbon dioxide adsorption was evaluated using carbon dioxide adsorption isotherms measured with Belsorp-Max manufactured by Nippon Bell Co., Ltd. Figure 2 shows the adsorption amount at the time of adsorption, with the adsorption amount at 10 kPa set to 0 wt%.

[0043] As shown in Figure 2, in Example 1 (Si / Al molar ratio 1.2), Example 2 (Si / Al molar ratio 1.1), and Example 3 (Si / Al molar ratio 1.4), the amount of carbon dioxide adsorption and desorption at 10-100 kPa was 5.0 wt% for Example 1, 4.9 wt% for Example 2, and 4.5 wt% for Example 3.

[0044] In contrast, in Comparative Example 1 (Si / Al molar ratio 0.8), Comparative Example 2 (Si / Al molar ratio 1.6), and Comparative Example 3 (Si / Al molar ratio 2.0), the amount of carbon dioxide adsorption and desorption at 10-100 kPa was 4.3 wt% for Comparative Example 1, 4.3 wt% for Comparative Example 2, and 3.7 wt% for Comparative Example 3.

[0045] The results of this embodiment showed that aluminum silicate composites with a Si / Al molar ratio of 1.0 to 1.5, exhibiting broad peaks around 2θ = 21, 26, 34, and 39° in X-ray powder diffraction using Cu as the X-ray source, have a carbon dioxide adsorption / desorption capacity of 4.5 wt% or more at carbon dioxide pressures of 10 to 100 kPa. [Industrial applicability]

[0046] The carbon dioxide adsorbent for pressure swinging of the present invention contains an aluminum silicate composite as its active ingredient, which has a carbon dioxide adsorption / desorption capacity of more than 4.5 wt% in the range of carbon dioxide pressure from 10 to 100 kPa, and is useful as an adsorbent for carbon dioxide recovery by pressure swinging adsorption. Furthermore, this aluminum silicate composite has the advantage of being able to be manufactured using inexpensive raw materials. Moreover, by using the carbon dioxide adsorbent for pressure swinging of the present invention, a pressure swinging adsorption method that does not require extreme depressurization means during carbon dioxide desorption can be used, making it possible to efficiently separate and recover carbon dioxide from exhaust gas with a carbon dioxide concentration of about 10 vol%.

Claims

1. A carbon dioxide adsorbent for the separation and recovery of carbon dioxide contained in exhaust gas by pressure swing adsorption method, A carbon dioxide adsorbent for the pressure swing method, comprising an aluminum silicate composite as the active ingredient, having a Si / Al molar ratio of 1.1 to 1.4, exhibiting broad peaks around 2θ = 21, 26, 34, and 39° in X-ray powder diffraction using Cu as the X-ray source, and possessing carbon dioxide adsorption performance of 4.5 wt% or more in carbon dioxide adsorption / desorption amounts in the range of carbon dioxide pressure from 10 to 100 kPa.

2. A method for separating and recovering carbon dioxide from exhaust gas by pressure swing adsorption using the carbon dioxide adsorbent for pressure swing method described in claim 1.

Citation Information

Patent Citations

  • Carbon dioxide absorbent and apparatus for removing carbon dioxide

    JP2003019435A

  • Carbon dioxide adsorbent

    JP2005040753A

  • Method for producing aluminum silicate complex

    JP2012012267A

  • Aluminum silicate composite and production method thereof

    JP2019026487A

  • Method of producing aluminum silicate

    JP2020055717A