Method for manufacturing a rotationally molded body and rotationally molded body
The method of dry blending thermoplastic resin with functional fine particles and rotational molding addresses the uneven distribution issue, resulting in enhanced inner surface properties like conductivity or antibacterial effects.
Patent Information
- Application Number
- JP2020138967
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-19
- Publication Date
- 2026-11-19
- Estimated Expiration
- 2040-08-19
AI Technical Summary
Existing rotational molding methods result in uneven distribution of additives on the outer surface of molded articles, which is undesirable for enhancing properties like electrical conductivity on the inner surface of containers.
A method involving dry blending of thermoplastic resin powder with functional fine particles followed by rotational molding, ensuring additives are predominantly distributed on the inner surface.
The method enables easy manufacturing of molded articles with additives predominantly on the inner surface, enhancing properties such as conductivity or antibacterial effects on the inner surface.
Smart Images

Figure 0007953878000003 
Figure 0007953878000004 
Figure 0007953878000005
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for producing a rotationally molded article, a rotationally molded article, and a molding material for rotational molding. In particular, the present disclosure relates to a method for producing a rotationally molded article that includes a dry blending step and a rotational molding step, a rotationally molded article of a molding material containing a thermoplastic resin and functional fine particles, and a molding material for rotational molding that includes a dry blend mixture.
Background Art
[0002] As a method for manufacturing hollow products such as containers and tanks, a rotational molding method is used. In the rotational molding method, a mold charged with a molding material is heated while being rotated, so that the molten molding material adheres to the mold surface and is gradually deposited, thereby producing a molded article. The rotationally molded article formed by depositing the molding material in this manner has an outer surface that is the surface in contact with the mold surface, and an inner surface that is the surface on the opposite side of the material forming the molded article with respect to the outer surface.
[0003] In rotational molding, when particles such as metal and carbon are contained in the molded article as additives, it is known that in addition to uniformly dispersing the additives in the molded article, the additives can be unevenly distributed on the outer surface side of the molded article by the centrifugal force of rotational molding (see Patent Document 1).
Prior Art Documents
Patent Documents
[0004]
Patent Document 1
Summary of Invention
Problems to be Solved by the Invention
[0005] However, in containers and the like, it is often required to enhance properties such as electrical conductivity on the inner surface, for example, to reduce adhesion of contents to the inner surface of the container. For this purpose, it is required to make additives more unevenly distributed on the inner surface side than on the outer surface side of the molded article.
[0006] The object of this disclosure is to provide a method for easily manufacturing molded articles in which additives are unevenly distributed on the inner surface. [Means for solving the problem]
[0007] A method for manufacturing a rotationally molded article according to one aspect of the present disclosure comprises the steps of: dry blending a thermoplastic resin powder and functional fine particles to obtain a molding material; and rotationally molding the molding material.
[0008] A rotationally molded article according to one aspect of the present disclosure is a rotationally molded article of a molding material comprising a thermoplastic resin and functional fine particles. This rotationally molded article has an inner surface and an outer surface. The ratio of functional fine particles to the thermoplastic resin is greater in the surface layer of the inner surface than in the surface layer of the outer surface.
[0009] A rotationally molded article according to one aspect of the present disclosure is a rotationally molded article of a molding material comprising a thermoplastic resin and functional fine particles. This rotationally molded article has an inner surface and an outer surface. The properties derived from the functional fine particles are higher on the inner surface than on the outer surface.
[0010] A molding material for rotational molding according to one aspect of the present disclosure includes a dry blend mixture of thermoplastic resin powder and functional fine particles. [Effects of the Invention]
[0011] This disclosure provides a method for easily manufacturing molded articles in which additives are predominantly located on the inner surface. [Brief explanation of the drawing]
[0012] [Figure 1] Figure 1 is a schematic perspective view showing an example of a rotationally molded body according to one embodiment of the present disclosure. [Figure 2] Figure 2 is a schematic horizontal cross-sectional view of the same rotationally molded body. [Figure 3] Figure 3 is an optical microscope image of a portion of the same rotationally molded body. DETAILED DESCRIPTION OF EMBODIMENTS
[0013] 1. Overview The method for producing a rotational molded article of the present embodiment includes a step of dry-blending thermoplastic resin powder and functional fine particles to obtain a molding material (hereinafter also referred to as the dry blending step), and a step of rotationally molding the aforementioned molding material (hereinafter also referred to as the rotational molding step).
[0014] According to the production method of the present embodiment, it is possible to easily produce a molded article in which the functional fine particles as an additive are unevenly distributed on the inner surface side by performing dry blending and rotational molding. The reason why a molded article in which functional fine particles are unevenly distributed on the inner surface side is obtained by the production method of the present embodiment is not necessarily clear, but can be inferred as follows, for example. By adopting rotational molding as the molding method for the molded article, and using a dry blend mixture of thermoplastic resin powder and functional fine particles as the molding material used for rotational molding, unlike the case where a kneaded product of thermoplastic resin and functional fine particles or the like is used as the molding material, the functional fine particles are not immediately and uniformly dispersed in the thermoplastic resin during the molding process. On the outer surface side that first comes into contact with the mold where the molded article is formed, the ratio of the functional fine particles to the thermoplastic resin is small, but it is considered that this ratio increases as the molding proceeds toward the inner surface side. As a result, a molded article in which the functional fine particles are unevenly distributed on the inner surface side of the molded article is formed.
[0015] 2. Details Hereinafter, the method for producing the rotational molded article of the present embodiment, the rotational molded article obtained by this production method, and the molding material for rotational molding used in this production method will be described in detail.
[0016] <Method for Producing Rotational Molded Article> As described above, the production method of the present embodiment includes a dry blending step and a rotational molding step. Each step will be described below.
[0017] [Dry Blending Step] In this process, a thermoplastic resin powder and functional fine particles are dry-blended to obtain a molding material. The term "dry-blending" refers to directly mixing two or more types of materials without melting them and without using a medium such as a solvent, to perform mixing (dry mixing).
[0018] (Thermoplastic resin powder) Examples of the thermoplastic resin include polyolefins such as polyethylene, polypropylene, and copolymers of ethylene and α-olefins such as 1-butene and 1-octene; vinyl resins such as polyvinyl acetate, polyvinyl chloride, and polyvinyl alcohol; polyamides such as polyamide 66 and polyamide 6; polyimide; polyphenylene sulfide; polyoxymethylene; polyesters such as polyethylene terephthalate and polybutylene terephthalate; polystyrene; styrene copolymers such as polyacrylonitrile-butadiene-styrene copolymer; polycarbonate; polyether ether ketone; acrylic resins such as polymethyl methacrylate; and fluororesins.
[0019] In the present embodiment, the thermoplastic resin preferably contains one or more resins selected from the group consisting of polyethylene, acrylonitrile-butadiene-styrene copolymer, and acrylic resins, and particularly preferably contains polyethylene. Polyethylene is lightweight, hardly generates toxic gas even when incinerated, is easy to recycle, and is excellent in oil resistance, chemical resistance, and impact strength. Examples of the polyethylene include linear low-density polyethylene, side chain branched low-density polyethylene, medium-density polyethylene, and high-density polyethylene.
[0020] The fluidity (MFR: Melt Flow Rate) of the thermoplastic resin specified in JIS-K7210 is preferably 2.5 g / 10min or more. In this case, the fluidity of the molten molding material can be ensured during molding, and the surface shape of the rotational molded article can be further improved. The upper limit value of the MFR of the thermoplastic resin is not particularly limited, and is, for example, 50 g / 10min.
[0021] Examples of thermoplastic resin powder shapes include spherical, egg-shaped, spindle-shaped, hollow, amorphous, chain-like, needle-shaped, cylindrical, rod-shaped, flattened, flaky, leaf-shaped, tubular, and sheet-like forms.
[0022] The particle size of the thermoplastic resin powder is preferably 100 μm to 1500 μm, more preferably 300 μm to 1300 μm, and even more preferably 500 μm to 1000 μm. The particle size of the powder is the median diameter measured, for example, with a particle size distribution analyzer (SALD-2300, manufactured by Shimadzu Corporation).
[0023] Thermoplastic resin powder can be obtained, for example, by grinding thermoplastic resin pellets. The grinding method is not particularly limited, but known grinding methods such as mechanical grinding or cryogenic grinding can be used. The thermoplastic resin may be new, recycled, or a mixture of these.
[0024] (Functional fine particles) "Functional microparticles" refer to microparticles added to a molded article to impart or improve its functionality, such as conductivity or antibacterial properties. It is preferable that the functional microparticles have a melting point of 60°C or higher, or have no melting point. By using such functional microparticles, they can be more unevenly distributed towards the inner surface of the molded article.
[0025] Examples of functional microparticles include conductive microparticles, insulating microparticles, thermally conductive microparticles, heat-insulating microparticles, sound-absorbing microparticles, electromagnetic wave-absorbing microparticles, flame-retardant microparticles, coloring microparticles, reinforcing microparticles, antibacterial microparticles, and antifouling microparticles.
[0026] Examples of conductive nanoparticles include carbon particles such as carbon black, carbon nanotubes, fullerenes, and graphite; metal particles such as gold, silver, copper, nickel, chromium, palladium, rhodium, ruthenium, indium, aluminum, tungsten, molybdenum, platinum, copper-nickel alloys, silver-palladium alloys, copper-tin alloys, silver-copper alloys, copper-manganese alloys, and those whose surfaces are coated with silver, etc.; and conductive oxide particles such as silver oxide, indium oxide, tin oxide, zinc oxide, ruthenium oxide, titanium oxide, antimony-containing tin oxide, and tin-containing indium oxide.
[0027] Examples of insulating fine particles include inorganic particles such as glass, silica, alumina, titania, clay, zeolite, silicon nitride, boron nitride, and calcium oxide; and resin particles such as acrylic resin, polyamide resin, and polyacetal resin.
[0028] Examples of thermally conductive fine particles include metal particles such as gold, silver, copper, iron, nickel, tin, aluminum, cobalt, indium, and their alloys; metal oxide particles such as aluminum oxide, magnesium oxide, and titanium oxide; metal nitride particles such as boron nitride and aluminum nitride; carbon particles such as graphite and diamond; and metal-coated particles in which a metal layer is coated onto resin particles.
[0029] Examples of insulating fine particles include inorganic or organic hollow fillers, beads, and particles such as silica.
[0030] Examples of sound-absorbing particles include barium sulfate, silica, shirasu balloons, and vermiculite.
[0031] Examples of electromagnetic wave absorbing nanoparticles include carbonyl iron and various ferrites (manganese-zinc, nickel-zinc, nickel-zinc-copper, copper-zinc, magnesium-manganese, copper-magnesium-manganese, neodymium-iron-boron, etc.).
[0032] Examples of flame-retardant fine particles include red phosphorus-based compound particles, phosphazene compound particles, melamine-based resin particles, and titanium dioxide-silicon dioxide composite particles.
[0033] Examples of colored microparticles include pigments, colored aggregates, colored resin particles, and colored gel particles.
[0034] Examples of reinforcing microparticles include ceramic particles such as zirconia, barium titanate, and hydroxyapatite; metal oxide particles such as aluminum oxide; and diamond particles.
[0035] Examples of antimicrobial microparticles include particles containing metallic elements such as silver, copper, zinc, gold, titanium, cobalt, tungsten, tin, bismuth, chromium, nickel, and thallium; known antimicrobial compounds such as silver ions; or particles on which photocatalysts such as titanium dioxide have been micronized or supported.
[0036] Examples of antifouling microparticles include inorganic copper compound particles such as copper compounds and cuprous oxide compounds; and particles on which known antifouling compounds have been micronized or supported.
[0037] In this embodiment, it is preferable that the antibacterial microparticles include at least one selected from the group consisting of conductive microparticles and antibacterial microparticles.
[0038] Examples of functional microparticle shapes include spherical, egg-shaped, spindle-shaped, hollow, amorphous, chain-like, needle-shaped, cylindrical, rod-shaped, flattened, scale-like, leaf-shaped, tubular, and sheet-like shapes.
[0039] The average particle size of the functional fine particles is preferably 0.01 μm or larger, and more preferably 0.03 μm or larger. In this case, the functional fine particles can be more unevenly distributed on the inner surface of the molded body. The average particle size is preferably 100 μm or smaller, and more preferably 10 μm or smaller. In this case, the uneven distribution of the functional fine particles can be made more uniform. The particle size of the functional fine particles is the median diameter measured, for example, with a particle size distribution analyzer (SALD-2300, manufactured by Shimadzu Corporation). The functional fine particles may be primary particles aggregated together to form secondary particles or structures.
[0040] (Dry blending method) A dry blend mixture, which is a molding material for rotational molding, is obtained by dry blending thermoplastic resin powder and functional fine particles. The dry blending method is not particularly limited and can be performed using a closed mixer such as a tumbler mixer, ribbon mixer, Nauter mixer, or Ribocone mixer. The temperature during dry blending is usually above room temperature and below 60°C. The dry blending time is usually between 1 minute and 6 hours, preferably between 5 minutes and 3 hours, more preferably between 10 minutes and 2 hours, and particularly preferably between 20 minutes and 60 minutes.
[0041] The ratio of functional fine particles to 100 parts by mass of thermoplastic resin powder is preferably 0.01 parts by mass or more. In this case, the properties on the inner surface of the molded article can be further improved. This ratio is more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, and particularly preferably 0.15 parts by mass or more. The ratio of functional fine particles is preferably 1 part by mass or less. In this case, the peeling of functional fine particles from the inner surface of the molded article can be further reduced. This ratio is more preferably 0.7 parts by mass or less, even more preferably 0.4 parts by mass or less, and particularly preferably 0.3 parts by mass or less.
[0042] To the extent that the effects of this disclosure are not impaired, other components other than the thermoplastic resin powder and functional fine particles may be mixed with at least one of the thermoplastic resin powder and functional fine particles before dry blending, or during dry blending. The other components may be in particulate form, liquid form, etc. Examples of other components include ultraviolet absorbers, stabilizers, antioxidants, compatibilizers, dispersants, and release agents.
[0043] The dry-blended mixture of thermoplastic resin and functional fine particles obtained in the dry-blending process can be suitably used as a molding material for rotational molding.
[0044] [Rotational molding process] In this process, the molding material obtained in the dry blending process (hereinafter also referred to as molding material (X)) is rotationally molded.
[0045] In this process, first, the molding material (X) is placed into the mold. Next, the mold is heated while rotating. As the temperature of the mold rises, the molding material (X) melts. The molten molding material (X) adheres to the surface of the mold and gradually accumulates. After heating the mold for a certain period of time, the mold is cooled and the molded body is removed from the mold. In this way, a rotationally molded body of the molding material (X) is obtained.
[0046] In this embodiment, the mold temperature during rotational molding is set appropriately according to the type of thermoplastic resin, but is preferably 150°C to 300°C, and more preferably 180°C to 280°C. In this embodiment, the heating time during rotational molding is preferably 5 minutes to 60 minutes, and more preferably 10 minutes to 35 minutes. Examples of heating methods in rotational molding include direct flame, hot air circulation oven, and media circulation.
[0047] In this embodiment, molded bodies of various shapes and dimensions, such as containers, tanks, cases, and boxes, can be manufactured depending on the shape of the mold. The rotation method in rotational molding may be single-axis rotation, double-axis rotation, or a method that combines single-axis rotation with oscillating motion, depending on the shape of the rotationally molded body to be manufactured.
[0048] Figure 1 shows an example of a rotationally molded body obtained by the manufacturing method of this embodiment. Figure 2 is a horizontal cross-sectional view of the container, which is the rotationally molded body 1 of Figure 1. The rotationally molded body 1 has an inner surface 2 and an outer surface 3. In the rotationally molded body 1 obtained by the manufacturing method of this embodiment, the side facing the mold for rotational molding becomes the outer surface 3, and the side opposite the mold becomes the inner surface 2.
[0049] The wall thickness of the rotationally molded body 1 is preferably 0.5 mm or more and 30 mm or less, more preferably 1 mm or more and 20 mm or less, even more preferably 2 mm or more and 10 mm or less, and particularly preferably 3 mm or more and 8 mm or less.
[0050] In the rotationally molded body 1, the functional fine particles are predominantly located on the inner surface. That is, in the rotationally molded body 1, the ratio of functional fine particles to thermoplastic resin is greater on the surface of the inner surface 2 than on the surface of the outer surface 3. The surface layer refers to the area near the surface of the rotationally molded body 1, such as the inner surface 2 and the outer surface 3, for example, the area from the surface of the rotationally molded body 1 to a depth of 100 μm, preferably the area from the surface to a depth of 10 μm.
[0051] In the rotationally molded body 1, the ratio of functional fine particles to the thermoplastic resin (hereinafter also referred to as ratio (Y)) is preferably 1.1 times or more, more preferably 1.5 times or more, even more preferably 2 times or more, and particularly preferably 3 times or more. The upper limit of this ratio is not particularly limited, but for example, it is 10 times.
[0052] Due to the aforementioned uneven distribution of functional microparticles, in the rotationally molded body 1, the properties derived from the functional microparticles are higher on the inner surface 2 than on the outer surface 3. These properties include, for example, conductivity for conductive microparticles and antibacterial properties for antibacterial microparticles.
[0053] In the rotationally molded body 1, the multiple of the characteristic value on the inner surface (characteristic value on inner surface 2 / characteristic value on outer surface 3) to the characteristic value on the outer surface 3 (hereinafter also referred to as characteristic value (Z)) is preferably 2 times or more, more preferably 5 times or more, even more preferably 10 times or more, and particularly preferably 100 times or more. The upper limit of this multiple is not particularly limited, but for example 10 10 It is double.
[0054] When the functional microparticles are conductive microparticles, the surface resistivity corresponding to the conductivity on the surface of the rotationally molded body 1 is 1 × 10⁻⁶ on the inner surface 2. 12 It is preferable that the resistivity is Ω or less. In this case, the adhesion of the contents of the rotationally molded body 1 to the inner surface 2 can be further suppressed. The surface resistivity of the inner surface 2 is 1 × 10⁻⁶ 10 It is more preferable that it be less than or equal to Ω, and 1 × 10 9 It is even more preferable that it be less than or equal to Ω, 1 × 10 8 It is particularly preferable that the value be less than or equal to Ω. The lower limit of the surface resistivity is not particularly limited, but for example, 1 × 10⁻⁶ 5 It is Ω. The surface resistivity on the outer surface 3 is 1 × 10⁻⁶. 13 It is preferable that the surface resistivity is greater than or equal to Ω. The surface resistivity is a value measured by a method in accordance with JIS-K6911:2006.
[0055] When the functional microparticles are antimicrobial microparticles, the antimicrobial activity value on the surface of the rotationally molded body 1 is preferably 2.0 or higher on the inner surface 2. In this case, the increase in the number of viable bacteria on the inner surface of the rotationally molded body 1 can be further suppressed. The antimicrobial activity value is more preferably 2.5 or higher, even more preferably 3.0 or higher, and particularly preferably 4.0 or higher. The upper limit of the antimicrobial activity value is not particularly limited, but for example it is 8.0. The antimicrobial activity value on the outer surface 3 is, for example, 1.0 or higher and less than 2.0. The antimicrobial activity value is a value measured by a method in accordance with JIS-Z2801:2012.
[0056] In this embodiment, the rotationally molded body, by using the manufacturing method described above, has functional fine particles predominantly located on the inner surface, and the properties derived from the functional fine particles are higher on the inner surface than on the outer surface. [Examples]
[0057] 1. Manufacturing of containers containing conductive fine particles [Example 1] (Dry blending process) 100 parts by mass of polyethylene powder and 0.2 parts by mass of conductive fine particles of carbon black (manufactured by Tokyo Ink Co., Ltd., product number PM-905H-BLK) were dry blended using a ribbon mixer to obtain a dry blend mixture, which was designated as molding material A.
[0058] (Rotational molding process) The molding material A obtained in the dry blending process was placed inside the mold of a rotational molding machine, and a hollow cylindrical container with a wall thickness of 4.5 mm was manufactured by rotational molding. The heating temperature was set to 250°C to 300°C, and the heating time was set to 15 minutes.
[0059] [Comparative Example 1] Molding material B was obtained by mixing 100 parts by mass of polyethylene pellets with 0.2 parts by mass of carbon black (manufactured by Tokyo Ink Co., Ltd., product number PM-905H-BLK), kneading the mixture in an extruder, and then grinding it in a fine grinder. Using this molding material B, containers of the same shape and dimensions were manufactured under the same rotational molding conditions as in Example 1.
[0060] (Measurement of surface resistivity) To evaluate the conductivity of the inner and outer surfaces of the rotationally molded body, the surface resistivity of the inner and outer surfaces was measured according to JIS-K6911:2006 (General Test Methods for Thermosetting Plastics) under conditions of a test voltage of 500V or 5V and a charging time of 1 minute. The measurement results are shown in Table 1.
[0061] [Table 1]
[0062] From the results in Table 1, the surface resistivity of the comparative example was similar on both the inner and outer surfaces, whereas the surface resistivity of the example was 10 times higher on the outer surface than on the inner surface. 8 This means that in the rotationally molded body of this embodiment, the inner surface has higher conductivity than the outer surface.
[0063] (Structural analysis of rotationally molded bodies) A sample prepared by cutting out a portion of the inner and outer surfaces of the rotationally molded body obtained in Example 1 was observed under an optical microscope at 40x magnification, and the structure of the rotationally molded body was analyzed. The micrograph is shown in Figure 3. In the sample in Figure 3, the right side is the outer surface, and the left side is the inner surface. On the outer surface (right side), the ratio of carbon black (black) to polyethylene (colorless) is small, while on the inner surface (left side), the ratio of carbon black to polyethylene is large. This is thought to be related to the fact that it was manufactured by rotational molding. Furthermore, the polyethylene and carbon black are not uniformly mixed; much of the carbon black exists in the gaps between multiple regions caused by the polyethylene powder, and the rotationally molded body forms a structure that includes areas with a locally high proportion of carbon black. This is thought to be related to the fact that it was manufactured using a dry blend mixture of polyethylene and carbon black.
[0064] 2. Manufacturing of containers containing antimicrobial particulate matter [Example 2] (Dry blending process) 100 parts by mass of polyethylene powder and 0.5 parts by mass of an antibacterial agent (manufactured by Fuji Chemical Co., Ltd., product name Bactekiller, product number BM-102JG), which is an antibacterial fine particle, were placed together in a tumbler mixer and dry blended to obtain a dry blend mixture, which was used as molding material C.
[0065] (Rotational molding process) The molding material C obtained in the dry blending process was placed inside the mold of a rotational molding machine and molded by rotational molding to produce a hollow, rectangular prism-shaped container with a wall thickness of 3.0 mm. The heating temperature was set to 280°C and the heating time to 14 minutes.
[0066] [Comparative Example 2] Molding material E was obtained by mixing 100 parts by mass of polyethylene pellets with 0.5 parts by mass of an antibacterial agent (manufactured by Fuji Chemical Co., Ltd., product name Bactekiller, product number BM-102JG), which is an antibacterial fine particle, kneading the mixture in an extruder, and then grinding it in a pulverizer. Using this molding material E, containers of the same shape and dimensions were manufactured under the same rotational molding conditions as in Example 1.
[0067] (Measurement of antibacterial activity) To evaluate the antibacterial properties of the inner and outer surfaces of rotationally molded bodies, the antibacterial activity values of the inner and outer surfaces were measured for Staphylococcus aureus using a method compliant with JIS-Z2801:2012 (Antibacterial processed products - Antibacterial test methods and antibacterial effects). Specifically, a bacterial solution prepared with 1 / 500 ordinary broth was dropped onto the surface of a test piece, sealed tightly with a film, and stored at 35°C. Subsequently, the number of viable bacteria in the bacterial solution on the test piece was measured. The antibacterial activity value was calculated using the following formula. Antimicrobial activity value = (Common logarithm of the number of viable bacteria after 24 hours in the untreated test piece) - (Common logarithm of the number of viable bacteria after 24 hours in the test piece)
[0068] [Table 2]
[0069] The results in Table 2 show that the antibacterial activity values of the comparative example were similar on both the inner and outer surfaces, whereas the antibacterial activity value of the example was 1.0 higher on the inner surface than on the outer surface. This indicates that in the rotationally molded body of this embodiment, the inner surface has higher antibacterial properties than the outer surface. [Explanation of Symbols]
[0070] 1 Rotational molded body 2. Inner self 3 External surface
Claims
1. A process to obtain a molding material by dry blending a thermoplastic resin powder having a particle size of 100 μm or more and 1500 μm or less with conductive fine particles having an average particle size of 0.01 μm or more and 10 μm or less, A step of rotationally molding the aforementioned molding material and A method for manufacturing a rotationally molded body comprising: The rotationally molded body has an inner surface and an outer surface, The conductivity value on the inner surface is 2 times or more than the conductivity value on the outer surface. 10 A method for manufacturing a rotationally molded body that is less than twice the original size.
2. A rotationally molded body of a molding material comprising a thermoplastic resin and conductive fine particles, The molding material comprises a dry blend mixture of the thermoplastic resin powder and the conductive fine particles having an average particle size of 0.01 μm or more and 10 μm or less. Having both an inner and outer aspect, A rotationally molded body in which the mass ratio of conductive fine particles to the thermoplastic resin is 1.1 times or more and 10 times greater in the inner surface layer than in the outer surface layer.
3. A rotationally molded body of a molding material comprising a thermoplastic resin and conductive fine particles, The molding material comprises a dry blend mixture of the thermoplastic resin powder and the conductive fine particles having an average particle size of 0.01 μm or more and 10 μm or less. Having both an inner and outer aspect, The conductivity, which is a property derived from the conductive fine particles, is at least twice as high on the inner surface as on the outer surface. 10 Rotationally molded bodies that are more than twice as expensive.
4. A rotationally molded article of a molding material comprising a thermoplastic resin and antimicrobial fine particles, Having both an inner and outer aspect, A rotationally molded body in which the antibacterial properties derived from the antibacterial fine particles are higher on the inner surface than on the outer surface.
Citation Information
Patent Citations
Rotational molding method of electroconductive plastic
JP1985239216A
Preparation of conductive resin molded piece
JP1986084214A
Plastic product and its production
JP1993140331A
Ethylene-based polymer powder for rotational molding and rotationally molded container
JP2008024769A
Electromagnetic wave shield sleeve
JP2013157445A