Sodium ion electrochemical element

The sodium-ion electrochemical element addresses lithium-ion battery limitations by using abundant resources and innovative materials, enabling high-current discharge and charge over a wide temperature range with a significantly longer lifespan.

JP7953899B2Active Publication Date: 2026-11-19IELECTROLYTE CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022197792
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2026-11-19
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

Existing lithium-ion batteries face challenges in achieving high-current discharge and charge capabilities over a wide temperature range, are resource-constrained due to lithium scarcity, and have limited lifespan compared to lead-acid batteries, necessitating a more sustainable and efficient alternative.

Method used

A sodium-ion electrochemical element with a carbon-coated metal foil, amorphous carbon negative electrode, and specific electrolytes and separators, utilizing abundant resources like sodium, iron, and manganese, to enable high-current discharge and charge, extended temperature operation, and longer lifespan.

Benefits of technology

The sodium-ion battery operates at -40°C to 100°C, discharges at 30ItA or higher, charges at 50ItA or higher, and has a lifespan twice that of conventional lithium-ion and lead-acid batteries, suitable for automotive and industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007953899000001
    Figure 0007953899000001
  • Figure 0007953899000002
    Figure 0007953899000002
  • Figure 0007953899000003
    Figure 0007953899000003
Patent Text Reader

Abstract

To provide a sodium ion electrochemical element such as a battery or ion capacitor that is capable of larger current charging and discharging, has a longer life, and can be used over a wider temperature range than a lithium ion battery that is used as an alternative to a lead battery for an engine starter.SOLUTION: An electrochemical element in which an ionic conductor is interposed between a positive electrode in which a sodium-containing positive electrode material is formed on the surface of a metal foil and a negative electrode in which a negative electrode material is formed on the surface of the metal foil. The metal foil constituting the positive electrode is a carbon-coated metal foil, the sodium-containing positive electrode material contains an alkaline neutralizer, and the negative electrode material contains an amorphous carbon material in which fluorine atoms and carboxyl groups are introduced.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a sodium-ion electrochemical element such as a sodium-ion secondary battery or a sodium-ion capacitor. [Background technology]

[0002] Lithium-ion secondary batteries, which utilize materials capable of intercalating and releasing lithium ions, have been introduced to the market as consumer-grade batteries for mobile devices such as cell phones. In recent years, these lithium-ion secondary batteries have been adopted for use as power sources in vehicles such as hybrid cars and electric vehicles. Furthermore, in Europe and other regions, considering the lead pollution caused by lead-acid batteries, lithium-ion batteries have been adopted and are already in use as a power source to replace lead-acid batteries used in engine starters for idle stop systems in vehicles. In addition, while sealed lead-acid batteries have traditionally been widely used for power supply in backup and standby use for social infrastructure and various industrial power sources, there is a growing trend to replace them with lithium-ion batteries.

[0003] Regarding lithium-ion batteries, those capable of discharging a large current of approximately 20 ItA at around -30°C, enabling engine operation, and capable of high-current regenerative charging of 30 ItA or more during braking have already appeared. Furthermore, with the aim of expanding the usable temperature range and obtaining even higher current discharge capacity and regenerative charging, studies are being conducted to reduce battery resistance and prevent the deposition of metallic lithium through intercalation reactions at the negative electrode of Li ions. Regarding the reduction of electrical resistance, it has been proposed to reduce the thickness of the positive and negative electrode plates, to reduce electrode resistance by coating carbon on the aluminum current collector foil, to reduce resistance by increasing the conductive material within the electrodes, to reduce resistance by controlling the thickness and pore size of the separator, or to reduce resistance by improving the welding method of the positive and negative electrode terminals within the battery. On the other hand, regarding the prevention of metallic lithium deposition, it has been proposed to reduce the particle size of the positive and negative electrode active materials to increase the reaction area and reduce the apparent charge and discharge current density, or to change the negative electrode active material from graphite to amorphous carbon material, or to change to lithium titanate. However, while these studies make high-current charging and discharging possible, realizing a lithium-ion battery that can be used in a temperature range of -40°C to 100°C and has the capability for high-current discharge of 30 ItA or more, as well as high-current regeneration of 50 ItA or more, has been difficult. Furthermore, the rapid increase in demand for EVs and other vehicles has led to a sharp increase in electricity demand due to the resulting shortage of natural gas and coal, and the rising prices of resources such as lithium for cathodes and electrolytes, rare metals for cathodes, and raw coke for graphite raw materials for anodes have become scarce, raising concerns about the stable supply of lithium-ion batteries.

[0004] Therefore, in order to address concerns about material supply, sodium-ion batteries using abundant sodium resources are being considered (see, for example, Patent Document 1). Patent Document 1 discloses a technology for using carbon materials as the negative electrode of a sodium battery. Graphite has poor compatibility with sodium ion insertion, and therefore reversible charging and discharging reactions using graphite are difficult to achieve. Unlike graphite, which has been used as a carbon-based negative electrode active material in lithium-ion batteries until now, technologies are being considered to improve battery characteristics by optimizing the carbon / oxygen atom ratio, BET surface area, and true density of the carbon material to enhance its compatibility with sodium ion insertion and removal. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] International Publication No. 2017 / 056991 [Overview of the Initiative] [Problems that the invention aims to solve]

[0006] However, while the above technology achieves the battery characteristics required for lithium-ion batteries, namely discharge capacity, cycle characteristics, and storage characteristics, it does not surpass the characteristics of conventional lithium-ion batteries. In particular, it has been shown that unnecessary sodium consumption can be suppressed by changing the carbon / oxygen atom ratio, but many of the factors related to sodium consumption are traps caused by crystal water and functional groups other than CF, and the above technology has not considered how to control these factors.

[0007] This invention addresses the need for a battery or ion capacitor that offers a longer lifespan even in standby use than lead-acid batteries or lithium-ion batteries. It aims to provide a sodium-ion electrochemical element, such as a battery or ion capacitor, that can charge and discharge at even higher currents than lithium-ion batteries used as alternatives to lead-acid batteries for engine starters, has a longer lifespan, and operates over a wider temperature range. In particular, this invention aims to provide a sodium-ion secondary battery or sodium-ion capacitor or other electrochemical element that operates within a temperature range of -40°C to 100°C, can discharge at 30 ItA or higher, and can be charged at 50 ItA or higher. [Means for solving the problem]

[0008] To achieve the above objective, the sodium ion electrochemical element of the present invention is an electrochemical element in which an ion conductor is interposed between a positive electrode, in which a sodium-containing positive electrode material is formed on the surface of a metal foil, and a negative electrode, in which a negative electrode material is formed on the surface of a metal foil. The metal foil constituting the positive electrode is a carbon-coated metal foil. The sodium-containing cathode material contains an alkali neutralizing agent. The aforementioned negative electrode material includes an amorphous carbon material, The amorphous carbon material is characterized by having fluorine atoms and carboxyl groups introduced into it.

[0009] In the sodium ion electrochemical element of the present invention, the ion conductor comprises an electrolyte and a separator, and it is preferable that the electrolyte contains at least one selected from sodium hexafluorophosphate (NaPF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium tetrafluoroborate (NaBF4), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), and sodium trifluoromethylsulfonylimide (NaFTI) as the electrolyte.

[0010] In the sodium ion electrochemical element of the present invention, the separator is preferably selected from a nonwoven fabric made of fibers having heat resistance of 200°C or higher and having at least one hydrophilic group and oxide ceramic on its surface, a resin film having a ceramic selected from group 3 element oxides and group 4 element oxides on its surface, a resin film with a polyamide resin as the main chain, and a resin film with a polyimide resin as the main chain.

[0011] In the sodium ion electrochemical element of the present invention, the ion conductor comprises a solid electrolyte or a gel-like polymer electrolyte, and the solid electrolyte or gel-like polymer electrolyte contains fibers, wherein the fibers are preferably at least one selected from cellulose fibers, olefin resin fibers, and polyethylene terephthalate resin fibers.

[0012] In the sodium ion electrochemical element of the present invention, the sodium-containing cathode material is a transition metal sodium layered oxide whose main components are Ni, Fe, and Mn, a sodium-containing polyanionic compound, a sodium-containing sulfide, a sodium-containing cyanide, a sodium-containing layered oxide, and Na2Mn as the cathode active material. X O Y It is preferable that the compound contains at least one selected from (X+Y=1) and Prussian blue-based Na2Mn[Fe(CN)6] in which a transition metal ion is bridged to a cyano group.

[0013] In the sodium ion electrochemical element of the present invention, the sodium-containing cathode material preferably contains a binder, and the binder preferably contains polyvinylidene fluoride in which a functional group selected from a carboxyl group, a carbonyl group, an imide group, and an amide group is substituted with terminal groups of the vinylidene main chain.

[0014] The sodium-ion electrochemical element of the present invention is preferably a sodium-ion secondary battery or a sodium-ion capacitor. [Effects of the Invention]

[0015] The electrochemical device such as the sodium-ion secondary battery or sodium-ion capacitor of the present invention operates at -40°C to 100°C, is capable of discharging at 30ItA or higher and charging at 50ItA or higher, and furthermore has a service life approximately twice that of the conventional lead-acid batteries and lithium-ion batteries for automotive engine starters, as well as the lead-acid batteries and lithium-ion batteries for power supplies of electrical components for electric vehicles. Furthermore, it is also significant as an industrial power supply by leveraging its long-life performance even as a stationary power supply backup power supply for standby use. [Mode for Carrying Out the Invention]

[0016] Hereinafter, embodiments of the present invention will be described in detail, but the scope of the present invention is not restricted by these descriptions, and appropriate modifications and implementations can be made for configurations other than the following examples within the range that does not impair the gist of the present invention. Unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more and B or less". In addition, "mass" and "weight", and "mass%" and "weight%" are treated as synonyms.

[0017] In the sodium-ion electrochemical device of the present invention, the positive electrode is formed by forming a sodium-containing positive electrode material containing an alkali neutralizer on the surface of a carbon-coated metal foil. As with lithium-ion batteries, aluminum foil can be used as the current collector for the positive electrode, but in order to prevent dissolution by an alkaline solution and improve the conductivity of the positive electrode plate, a metal foil such as aluminum with a carbon coating treatment applied to its surface is used in the present invention. In addition, the negative electrode is formed by forming a negative electrode material containing an amorphous carbon material into which fluorine atoms and carboxyl groups are introduced on the surface of a metal foil. An ionic conductor is interposed between the positive electrode and the negative electrode.

[0018] The positive electrode active material used in the aforementioned sodium-containing positive electrode material is strongly alkaline. Therefore, in order to prevent the dissolution of the carbon-coated metal foil, such as aluminum, which is the current collector, the sodium-containing positive electrode material contains an alkali neutralizing agent. As the alkali neutralizing agent, inorganic materials such as chlorine compounds, sulfuric acid compounds, carbonate compounds, boron compounds such as boric anhydride and polyboric acid, or organic acids such as oxalic acid derivatives, phosphoric acid derivatives, acetic acid derivatives, maleic acid derivatives, and alginic acid derivatives can be used.

[0019] The sodium-containing cathode material preferably contains a binder that bonds the current collector foil and the active material. The binder preferably contains polyvinylidene fluoride in which a functional group selected from carboxyl groups, carbonyl groups, imide groups, and amide groups is substituted at the terminal groups of the vinylidene main chain. As a binder for the cathode, polyvinylidene fluoride is used as the basic resin, but in alkaline solutions, gelation occurs due to polyene formation, so it is useful to use a material in which a part of the vinylidene chain is substituted with a carbonyl group, a carboxyl group, or an amide group.

[0020] The aforementioned sodium-containing cathode material minimizes the use of rare metal elements that were previously used in conventional lithium-ion batteries. The cathode active material capable of intercalating and releasing sodium ions includes transition metal sodium layered oxides whose main components are Ni, Fe, and Mn, sodium-containing polyanionic compounds such as NaFePO4, sodium-containing sulfides, sodium-containing cyanides, sodium-containing layered oxides such as ammonium sulfate sodium iron sulfate Na2Fe2(SO4)3, and NaMO2(M:Fe,Ni,Mn, etc.), and Na2Mn X O Y It is preferable that the compound contains at least one selected from (X+Y=1) and Prussian blue-based Na2Mn[Fe(CN)6] in which a transition metal ion is bridged to a cyano group.

[0021] To address the common hydrate removal and alkali resistance requirements of each material system, temperature control and F2 / O2 gas substitution are performed during material preparation. Additionally, coatings of metal oxides such as alumina, which do not form compounds with sodium ions, may be applied to the surface of the positive electrode active material. When using Fe or Mn cyanide hydrates such as Prussian blue or Prussian white as sodium-containing cyanides, they may be used as is, or compounds from which a predetermined amount of crystal water has been removed may be used. Since crystal water within the crystal lattice of Prussian hydrate compounds inhibits the ion movement of sodium ions within crystal vacancies, temperature-controlled removal of crystal water during the compound preparation process or substitution reaction of crystal water with fluorine atoms using F2 / O2 gas are effective.

[0022] The negative electrode is formed by creating a negative electrode material containing an amorphous carbon material on the surface of a metal foil into which fluorine atoms and carboxyl groups have been introduced. If a material is used in which functional groups such as carboxyl groups are chemically modified on the carbon material at the entrances and exits of the carbon layers and cluster structure where sodium ions are absorbed and released, the initial charge-discharge efficiency is improved, as is the mobility of sodium ions during the battery's lifespan. Unlike lithium-ion batteries, aluminum foil can be used as the current collector foil for the negative electrode due to the noble potential of the negative electrode and the fact that sodium ions do not alloy with aluminum. Similar to the positive electrode, a carbon-coated metal foil can be used for the negative electrode.

[0023] The ion conductor may be in the form of an electrolyte and a separator, or a gel-like polymer electrolyte which is a solid electrolyte or a semi-solid electrolyte may be used.

[0024] When using an electrolyte solution, it is preferable that the supporting electrolyte contains at least one selected from sodium hexafluorophosphate (NaPF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium tetrafluoroborate (NaBF4), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), and sodium trifluoromethylsulfonylimide (NaFTI), and it is also preferable to use a mixture of these. The total concentration of the supporting electrolyte is preferably 1.0 to 1.3 mol.

[0025] As the solvent for the electrolyte, it is preferable to combine cyclic carbonates containing unsaturated bonds, such as propylene carbonate (PC) and ethylene carbonate (EC), or fluorides that do not contain unsaturated bonds, such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC), or fluoride such as ethylene fluoride (FEC), in a formulation that does not freeze at -40°C. With these solvent systems, the usable temperature limit is 90°C on the higher end. Furthermore, to further improve the high-temperature cycle life or the self-discharge characteristics during storage, propane saltonate may be used as the solvent and bis(oxalate) boron compounds as the solute. However, if a solid ion-conducting electrolyte (solid electrolyte) or gel-like polymer is used without a separator, or if an ionic liquid solvent such as 1-ethyl-3 methylimidazolium or bis(fluorosulfonyl)imide is used even with a separator, it can be used at -40°C to 100°C.

[0026] The separator is preferably selected from a nonwoven fabric made of fibers having heat resistance of 200°C or higher and having at least one of hydrophilic groups and oxide ceramics on its surface, a resin film having a ceramic selected from group 3 element oxides and group 4 element oxides on its surface, a resin film with a polyamide resin as the main chain, and a resin film with a polyimide resin as the main chain. Examples of the hydrophilic groups include -OH and -COO-. As the resin film, it is preferable to use a three-layer resin film of PP / PE / PP in which a ceramic such as group 3 and 4 element oxides is coated on the surface to a thickness of several microns or less. Alumina and silica can be suitably used as the ceramic present on the surface of the resin film.

[0027] As the solid electrolyte, sulfur-based NaGePS, NaSiPSCl, or oxide-based NaAlTi(PO4)2 can be used. As the gel-like polymer electrolyte, ion-conducting resins such as PEO or PVDF can be used.

[0028] The solid electrolyte or gel-like polymer electrolyte contains fibers, and it is preferable that the fibers are at least one selected from cellulose fibers, olefin resin fibers, and polyethylene terephthalate resin fibers. When using a solid electrolyte or gel-like polymer electrolyte, porous spaces (so-called voids) may be generated at the interface with the positive and negative electrode active materials or within the intervening electrolyte due to the expansion and contraction of the positive and negative electrode active materials during charging and discharging. When such voids are generated, the diffusion of lithium ions within the solid and the movement between solids between the positive and negative electrodes becomes impossible, inhibiting the charge-discharge reaction and shortening the lifespan of the electrochemical element. Mixing the fibers into the solid electrolyte or gel-like polymer electrolyte is preferable because it can suppress the generation of voids and lead to a longer lifespan.

[0029] The sodium-ion electrochemical element of this invention benefits from the abundance of sodium resources. The positive electrode material can be manufactured from abundant resources such as iron and manganese, and the negative electrode material, being an amorphous carbon material (hard carbon material), can be produced from resin resources. Therefore, compared to lithium-ion batteries, it is possible to use materials that are not subject to resource depletion concerns, resulting in lower-cost secondary batteries and capacitors. Furthermore, since lead is not used, pollution concerns are avoided.

[0030] The sodium-ion electrochemical element of the present invention is preferably a sodium-ion secondary battery or a sodium-ion capacitor. It is applicable not only to the so-called conventional secondary battery structure or ion capacitor structure in which positive and negative electrode plates face each other via a separator, but also to a bipolar structure in which the positive electrode active material and the negative electrode active material are integrated on both sides via a current collector. [Examples]

[0031] The present invention will be described in more detail based on examples and comparative examples, but the present invention is not limited thereto.

[0032] The prototype method for the embodiment of this patent is shown below.

[0033] Na of transition metal layered sodium oxide x Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 was used as the positive electrode active material, and acetylene black and carbon nanotubes with a diameter of 100-150 nm were mixed with the positive electrode as conductive materials, and alginic acid as an alkaline neutralizing agent, all in powder form. The mixing ratio was adjusted to 89 parts by weight of the positive electrode active material, 3.5 parts by weight of acetylene black, 1.0 part by weight of carbon nanotubes, and 2.5 parts by weight of alginic acid. To this, 4 parts by weight of modified polyvinylidene fluoride (in which the terminal functional groups of the polymer were replaced with amide groups, etc.) was added as a binder to prevent gelation. N-methylpyrrolidone was added as a dispersion solvent, and the mixture was kneaded to prepare a positive electrode mixture (positive electrode slurry).

[0034] The above positive electrode slurry was applied to both sides of a 25 μm thick carbon-coated aluminum foil in a dry state at 195 g / m 2 coating weight per side, followed by drying. Thereafter, pressing and cutting were performed to obtain a positive electrode for a sodium secondary battery. After the positive electrode slurry was applied to both sides of the carbon-coated aluminum foil and dried, the total thickness of the positive electrode plate after pressing was 140 μm.

[0035] The negative electrode of the sodium ion secondary battery of the present patent was produced by the following method. 96 parts by weight of amorphous carbon material particles as the main material and 1 part by weight of acetylene black were added, and 3 parts by weight of a binder SBR / CMC emulsion solution was added to prepare a slurry. Next, the slurry was applied to a 25 μm thick aluminum foil at 99 g / m per one side 2 to perform double-side coating, followed by drying. Subsequently, pressing was performed to adjust the total thickness of the negative electrode plate to 224 μm, followed by cutting to obtain a negative electrode plate. It is also useful to use a carbon-coated foil.

[0036] As the raw material for the amorphous carbon, a non-graphitizable thermosetting resin is mainly used, and it is generally produced by carbonizing the resin at 800 to 1400°C. Due to being amorphous, the structure has many defects, and a large number of residual oxygen atoms are present in those portions. Those portions and crystal sites contain H2O molecules as crystal water, and in particular, it is not easy to remove the latter H2O molecules by heat treatment. Conventionally, amorphous carbon has a problem that the initial Coulombic efficiency (ICE) is lowered due to this crystal water. Irreversible Na caused by crystal water in SEI formation and defects, and residual oxygen atoms + occlusion is considered to be the cause. Improving ICE without reducing the mobility of working metal ions at defects or crystal sites is an important technical point when an amorphous material is used as a negative electrode material for a secondary battery. For that purpose, it is necessary to remove H2O of crystal water and residual oxygen atoms, and further devise the design of functional groups left at those sites. Accordingly, in the present invention, the amorphous carbon material was produced by the method described below. The amorphous carbon material was reacted in a reaction vessel at a temperature from room temperature to 50°C or lower under a fluorine pressure of 0.5 kPa to 20 kPa for 10 minutes to 48 hours, and subsequently, the partial pressure ratio P of fluorine to oxygenF2 / P O2 The processes for values ​​0.1 to 10 were to be carried out at the same temperature and reaction time. The atomic radius of fluorine is 64 pm (pm=10). -12 Fluorine has a small molecular weight (m) after hydrogen (53pm), and if there is sufficient space, it can easily diffuse to the reaction site. The introduced fluorine first carries out a dehydration reaction as shown in equation (1). This reaction removes H2O molecules contained in defects and crystal water. In addition, the HF produced in equation (1) functions as a Lewis acid, generating a fluorine-graphite intercalation compound as shown in equation (2). When a fluorine-graphite intercalation compound is formed in the graphene layer of amorphous carbon, the conductivity of the material may increase. TIFF0007953899000001.tif13170 At the same time, as shown in equation (3), fluorine appropriately replaces the residual oxygen atom sites in amorphous carbon with CF bonds, thereby removing the residual oxygen atoms. The CO bond sites between residual oxygen atoms and C have low adsorption energy and are unstable, and are easily replaced by CF bonds (D. Sun et al, “Engineering the trap effect of residual oxygen atoms and effects in hard carbon anode towards high initial Coulombic efficiency”, Nano Energy, 64,103937(2019)). When CF bonds are formed on the surface of a defect, the bond energy increases, and the adsorption energy of that site increases. Therefore, Na at the CF site + Adsorption of Na becomes difficult, and during charging and discharging, + The absorption and release of the substance are reversible. Next, the partial pressure ratio P of fluorine to oxygen due to the O2 produced in equations (1) and (2) and the additionally added O2 is calculated. F2 / P O2 The process was performed with a coefficient of 0.1 to 10 to introduce -COOH groups to the carbon atoms in the defective and crystalline regions, as shown in equation (4). TIFF0007953899000003.tif8170-H of the COOH group + is Na +Because ion exchange is easily performed, Na in the crystalline region + This allows for control over the decrease in mobility. This method has enabled improvement in ICE (Integrated Heat and Discharge) performance during initial charging and discharging.

[0037] [Example 1] Example 1 is a sodium-ion battery that utilizes all of the technologies described in this patent for the positive electrode plate, negative electrode plate, electrolyte, and separator. Using the positive and negative electrode plates prepared as described above, a 20 μm thick nonwoven cellulose fiber fabric was interposed as a separator to create a 3.2V-600mAh aluminum laminate film pack type sodium-ion battery with 6 positive electrodes and 7 negative electrodes. For the electrolyte, a solution of PC, EC, DEC, and DMC solvents was mixed in a volume ratio of PC / EC / DEC / DMC = 1 / 2 / 4 / 3, to which 0.6 mol / L of sodium hexafluorophosphate (NaPF6) and 0.6 mol / L of sodium bisfluorosulfonyliimide (NaFSI) were dissolved as supporting electrolytes, and 1 wt% of FEC was added.

[0038] [Comparative Example 1] On the other hand, Comparative Example 1 was a 3.4V-600mAh lithium-ion battery made using commercially available materials for engine starters. Comparative Example 1 is a lithium-ion battery in which the positive electrode plate is composed of LiFePO4, a conductive material, and a PVDF binder, and the negative electrode is made of artificial graphite.

[0039] [Example 2] A sodium-ion battery was prepared in the same manner as in Example 1, except that only sodium bisfluorosulfonylimide (NaFSI) was used as the supporting electrolyte, and the amount added was 1.2 mol / L.

[0040] [Example 3] A sodium-ion battery was fabricated in the same manner as in Example 1, except that a 20 μm thick polyethylene film was used as the separator.

[0041] The performance targets for the sodium-ion battery of the present invention were met by conducting discharge tests at -30°C and above, and charging tests at above 50ItA, and the results of the performance tests for each battery were compared.

[0042] [DCIR value evaluation] After the initial charge and capacity confirmation of the obtained batteries, the discharge and charge DCIR (Direct Current Internal Resistance) values ​​were measured at a state of charge (SOC) of 50%. The measurement method involved adjusting the batteries to a 50% SOC state at room temperature for each measurement. Discharging was performed from an open circuit state with currents of 1 ItA, 5 ItA, and 10 ItA, and the battery voltage was measured at 10 seconds. The voltage drop from the open circuit voltage at each discharge was plotted against each current, and the slope of the graph, which was linearized using the least squares method, was taken as the discharge DCIR value at 10 seconds. Conversely, for charging, the charge DCIR value at 10 seconds was calculated from a graph plotting the increase in charge voltage from the open circuit voltage against each charging current when charging a battery adjusted to a 50% SOC state with the same current. Table 1 shows the measurement results for the discharge DCIR value and charge DCIR value at 10 seconds.

[0043] [Table 1]

[0044] It can be seen that the sodium-ion battery of Example 1 has a significantly lower resistance value than the battery of Comparative Example 1. Furthermore, the lithium-ion battery of Comparative Example 1 has a higher DCIR value compared to the sodium-ion batteries of Examples 1 to 3. It can be seen that the lithium-ion battery of Comparative Example 1 has a higher DCIR value on the charging side than on the discharging side, which is a different trend from the batteries of Examples 1, 2, and 3. This is thought to indicate that the reaction overpotential for charge acceptance on the negative electrode side of the sodium-ion battery is low, resulting in fewer side reactions and reactions such as deposition of metallic lithium as in Comparative Example 1, and that metal deposition reactions on the amorphous negative electrode material of the sodium-ion battery are less likely to occur.

[0045] [Evaluation of discharge duration at low temperatures] At -30°C, the discharge duration to 2.0V was measured for each battery capacity at currents of 20ItA and 30ItA. The results are shown in Table 2.

[0046] [Table 2]

[0047] Table 2 shows that the sodium-ion battery of Example 1 can discharge for a sufficient duration at both 20ItA and 30ItA, and can be used as a substitute for lead-acid batteries (discharge duration of 15-16 seconds at 20ItA) in idle stop systems at -30°C. Furthermore, the specifications of the sodium-ion batteries of Examples 2 and 3 show improved low-temperature discharge characteristics compared to lithium-ion batteries, although not as good as those of Example 1. However, while the lithium-ion battery of Comparative Example 1 can start the engine at -20°C, it was found that it cannot operate as a substitute battery at the low temperature of -30°C.

[0048] [Evaluation of regenerative charging capacity (fast charging efficiency)] To compare regenerative charging capabilities, the discharge capacity up to 2.0V at a constant current of 1 ItA was confirmed. Then, constant current charging up to 4.0V was performed at current values ​​of 30 ItA, 50 ItA, and 80 ItA, respectively. The ratio of regenerative recovery charge capacity to 1 ItA discharge capacity was calculated as the charging efficiency, and this efficiency was used to compare regenerative charging capabilities. The results are shown in Table 3.

[0049] [Table 3]

[0050] Table 3 shows that the sodium-ion battery of the present invention in Example 1 can be ultra-rapidly charged in less than 1 minute (80 ItA) at room temperature. Compared to the lithium-ion battery of Comparative Example 1, this is due to the fact that the electrochemical reaction resistance at the negative electrode of the sodium-ion battery of the present invention is lower, and the solvation diameter during sodium ion movement is smaller than that during lithium ion movement, resulting in lower diffusion resistance of sodium ions in the electrolyte between the positive and negative electrodes. Furthermore, it is thought that sodium ions undergo a smooth desorption reaction from between the positive electrode active material layers through solid diffusion from within the positive electrode active material. On the other hand, at the negative electrode, while the lithium-ion battery of Comparative Example 1 undergoes reactions requiring relatively high voltage, such as the insertion of lithium ions between graphite layers, the sodium-ion battery of Example 1 undergoes ion insertion reactions into the amorphous-specific cluster structure. In the lithium-ion battery of Comparative Example 1, the intercalation rate at the negative electrode graphite surface, which receives lithium ions, was slow, resulting in diffusion-limited rate of change within the solid and polarization. As a result, the charging voltage reached 4.0V prematurely, leading to a decrease in charging efficiency. On the other hand, in the sodium-ion batteries of Examples 2 and 3, although the positive and negative electrodes were the same as in Example 1, in Example 2, the diffusion capacity was lower due to the difference in the supporting electrolyte. Similarly, in Example 3, polarization occurred due to insufficient liquid retention capacity of the separator, resulting in an absolute shortage at the electrode interface. Therefore, the charging efficiency was lower compared to Example 1.

[0051] [Charge life test] Each battery underwent a trickle charge life test at 45°C with a voltage of 4.0V to evaluate its performance as a stationary battery. Life determination was based on the number of months of trickle charging until 60% of the initial capacity was maintained. This test also served as an accelerated life test using the Arrhenius law at 25°C, with the acceleration being six times faster than the 45°C test, and the lifespan was determined based on the 25°C test. The results are shown in Table 4.

[0052] [Table 4]

[0053] Table 4 shows that the stationary lifespan of the sodium-ion battery of the present invention in Example 1 was determined to be 24 months at 45°C and 12 years at 25°C. The lithium-ion battery in Comparative Example 1 was determined to have a lifespan of 10 months and 5 years, suggesting that metal deposition at the lithium-ion negative electrode is the problem. The sodium-ion batteries of Examples 2 and 3 are inferior to those of Example 1 of the present invention, but their superior trickle life characteristics compared to the lithium-ion battery of Comparative Example 1 are evidence of this. Thus, it has been found that the sodium-ion battery of the present invention can be applied not only to battery applications with excellent rapid charging characteristics for in-vehicle use such as EVs, but also to stationary battery applications for industrial standby use.

[0054] Furthermore, although this embodiment only describes the application of sodium ion secondary batteries as electrochemical elements, it is also applicable to other electrochemical elements such as ion capacitors and flame-retardant safety batteries using ionic liquids. Although not described in this embodiment, the effects were also advantageous when using polyanion compound systems, sulfur compound systems, and even Prussian cyanide hydrate compound cathodes other than transition metal layered oxide cathodes, similar to those in Embodiment 1. [Industrial applicability]

[0055] The electrochemical elements such as the sodium-ion secondary battery or sodium-ion capacitor of the present invention can discharge 30 ItA or more over a wide temperature range of -40°C to 100°C, making them suitable for use as a lead-acid battery replacement for idle stop systems. Furthermore, the sodium-ion battery of the present invention has superior performance to lithium-ion batteries with a similar configuration, and is capable of rapid regenerative charging of 50 ItA or more, surpassing the performance of lead-acid batteries and lithium-ion batteries. Therefore, according to the present invention, it is possible to develop industrial batteries for vehicles and other applications that can operate at low temperatures not only as a power source for idle stop systems but also as a power source for electrical components in HEVs, PHEVs, and EVs, and can extend the electric driving range through regenerative capabilities without increasing battery capacity, volume, or weight, thereby improving fuel efficiency. In addition, the sodium-ion battery of the present invention has superior lifespan characteristics as a standby-use battery for industrial infrastructure compared to lithium-ion batteries, having a lifespan equivalent to lead-acid batteries in that field, while also being lightweight, significantly reducing the installation area, free from lead pollution problems, and without resource problems for large industrial batteries. Furthermore, although the sodium-ion battery and sodium-ion capacitor of the present invention have a smaller capacity than conventional lithium-ion batteries, they are lighter, capable of equivalent charging and discharging, and have a long lifespan suitable for cycle charging and discharging. Therefore, they have been shown to be superior as power sources for cyclical use in industrial drones for pesticide spraying and transportation.

[0056] The embodiments disclosed herein should be considered in all respects to be illustrative and not restrictive. The scope of this invention is indicated by the claims rather than by the foregoing description, and all modifications within the meaning and scope equivalent to the claims are intended to be included.

Claims

1. An electrochemical element comprising a positive electrode having a sodium-containing positive electrode material formed on the surface of a metal foil, and a negative electrode having a negative electrode material formed on the surface of a metal foil, with an ion conductor interposed between them, The metal foil constituting the positive electrode is a carbon-coated metal foil. The sodium-containing cathode material contains an alkali neutralizing agent. The aforementioned negative electrode material includes an amorphous carbon material, A sodium ion electrochemical element characterized in that fluorine atoms and carboxyl groups are introduced into the amorphous carbon material.

2. The ionic conductor comprises an electrolyte and a separator. The electrolyte in the aforementioned solution is sodium hexafluoride phosphate (NaPF) as the electrolyte. 6 ), sodium bis(fluorosulfonyl)imide (NaFSI), sodium tetrafluoroborate (NaBF 4 The sodium ion electrochemical element according to claim 1, comprising at least one selected from sodium bis(trifluoromethanesulfonyl)imide (NaTFSI) and sodium trifluoromethylsulfonylimide (NaFTI).

3. The sodium ion electrochemical element according to claim 2, wherein the separator is selected from a nonwoven fabric made of fibers having heat resistance of 200°C or higher and having at least one of hydrophilic groups and oxide ceramics on its surface, a resin film having a ceramic selected from group 3 element oxides and group 4 element oxides on its surface, a resin film with a polyamide resin as the main chain, and a resin film with a polyimide resin as the main chain.

4. The ionic conductor comprises a solid electrolyte or a gel-like polymer electrolyte. The solid electrolyte or the gel-like polymer electrolyte contains fibers, The sodium ion electrochemical element according to claim 1, wherein the fiber is at least one selected from cellulose fiber, olefin resin fiber, and polyethylene terephthalate resin fiber.

5. The sodium-containing cathode material includes, as a cathode active material, transition metal sodium layered oxides whose main components are Ni, Fe, and Mn, sodium-containing polyanionic compounds, sodium-containing sulfides, sodium-containing cyanides, sodium-containing layered oxides, and Na 2 Mn X O Y (X + Y = 1), and Prussian blue-based sodium in which a transition metal ion is bridged to the cyano group. 2 Mn[Fe(CN)] 6 A sodium ion electrochemical element according to any one of claims 1 to 4, comprising at least one selected from ].

6. The sodium-containing cathode material includes a binder, The sodium ion electrochemical element according to any one of claims 1 to 4, wherein the binder comprises polyvinylidene fluoride in which a functional group selected from a carboxyl group, a carbonyl group, an imide group, and an amide group is substituted at the terminal groups of the vinylidene main chain.

7. A sodium-ion electrochemical element according to any one of claims 1 to 4, which is a sodium-ion secondary battery or a sodium-ion capacitor.

Citation Information

Patent Citations

  • Preparation method and application of biomass-derived oxygen-rich hard carbon material

    CN110255527A

  • Non-aqueous electrolyte composition

    JP2022538380A

  • Partially and fully surface-enabled metal ion-exchanging energy storage devices

    US20120171574A1

  • Positive electrode for sodium ion secondary cell, and sodium ion secondary cell

    WO2016021405A1

  • Sodium-ion secondary battery negative electrode carbonaceous material and sodium-ion secondary battery using thereof

    WO2017056991A1