Adhesive composition, separator, non-aqueous secondary battery, and method for manufacturing the adhesive composition
The adhesive composition for non-aqueous secondary batteries, comprising (meth)acrylic acid ester monomers and an acetate-free dispersant, addresses the issue of discoloration, enhancing adhesion and lithium ion permeability while reducing powder shedding and blocking.
Patent Information
- Application Number
- JP2025256184
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-12-16
- Publication Date
- 2026-11-19
- Estimated Expiration
- 2045-12-16
AI Technical Summary
Adhesives used in non-aqueous secondary batteries, such as those described in Patent Document 1, are prone to discoloration.
An adhesive composition comprising polymer particles with (meth)acrylic acid ester monomers and a dispersant without an acetate group is used to suppress discoloration, which includes components like alkyl (meth)acrylates, hydroxyl-containing (meth)acrylic acid esters, and a dispersant such as polyvinylpyrrolidone.
The adhesive composition effectively suppresses discoloration, improving adhesion and lithium ion permeability while maintaining resistance to powder shedding and blocking.
Smart Images

Figure 0007953944000001
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to an adhesive composition, a separator, a non-aqueous secondary battery, and a method for producing the adhesive composition. BACKGROUND ART
[0002] Adhesives are important compositions that have a wide range of uses. For example, in the manufacturing process of non-aqueous secondary batteries such as lithium batteries, adhesives are also used to bond separators and electrodes together. For this reason, various compositions have been developed. For example, an adhesive composition that is a vinyl acetate resin emulsion using a PVA-based resin obtained by partially saponifying an aliphatic polyvinyl ester as a protective colloid is known to achieve both excellent adhesiveness and film-forming property (Patent Document 1). PRIOR ART DOCUMENTS PATENT DOCUMENTS
[0003] PATENT DOCUMENT 1 Japanese Unexamined Patent Application Publication No. 2001-302709 SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION
[0004] However, when the adhesive described in Patent Document 1 is used, the adhesive after coating may undergo discoloration.
[0005] The present invention aims to suppress discoloration of the adhesive. MEANS FOR SOLVING THE PROBLEMS
[0006] To achieve the object of the present invention, an adhesive composition according to one embodiment has the following configuration. That is, the adhesive composition comprises polymer particles and a dispersant having no acetate group, wherein the polymer particles contain a (meth)acrylate ester monomer as a constituent unit. EFFECTS OF THE INVENTION
[0007] This invention provides an adhesive composition that suppresses discoloration of the adhesive. [Modes for carrying out the invention]
[0008] The embodiments will be described in detail below. Note that the following embodiments do not limit the invention as defined in the claims, and not all combinations of features described in the embodiments are essential to the invention. Two or more of the features described in the embodiments may be combined in any way.
[0009] [Adhesive composition] An adhesive composition according to one embodiment of the present invention comprises polymer particles and a dispersant that does not have an acetate group. The adhesive composition may optionally further comprise a dispersion medium such as water. When the adhesive composition comprises a dispersion medium, the form of the adhesive composition may be a slurry.
[0010] <Polymer particles> Polymer particles according to one embodiment of the present invention include (meth)acrylic acid ester monomers as constituent units. For example, polymer particles according to one embodiment of the present invention are (meth)acrylic resin particles obtained by polymerizing monomer components that include at least (meth)acrylic acid ester as polymerizable monomers, and have constituent units derived from at least (meth)acrylic acid ester.
[0011] In this specification, the term "(meth)acrylic" includes both the meanings of "acrylic" and "methacrylic," and similarly, the term "(meth)acrylate" includes both the meanings of "acrylate" and "methacrylate." Also, in this specification, the numerical range A to B means A or greater and B or less, unless otherwise specified.
[0012] The (meth)acrylic resin particles (polymer particles) may be a polymer (homopolymer) obtained by polymerizing one type of polymerizable monomer ((meth)acrylic acid ester), or they may be copolymer particles obtained by copolymerizing two or more polymerizable monomers containing (meth)acrylic acid ester. The polymer particles are preferably copolymer particles.
[0013] ((meth)acrylic acid ester) Examples of (meth)acrylic acid esters include alkyl (meth)acrylates, hydroxyl-containing (meth)acrylic acid esters, crosslinkable (meth)acrylic acid esters, alkoxyalkyl (meth)acrylates, aralkyl (meth)acrylates, and aryl (meth)acrylates, as well as other (meth)acrylic acid esters. One or more of these (meth)acrylic acid esters can be used. Among these, it is preferable that the monomer components constituting the (meth)acrylic resin particles (polymer particles) contain at least an alkyl (meth)acrylate.
[0014] ((meth)acrylate alkyl ester) Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, sec-butyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl Examples include alkyl (meth)acrylates having linear or branched alkyl groups such as syl(meth)acrylate, n-undecyl(meth)acrylate, n-dodecyl(meth)acrylate, n-tridecyl(meth)acrylate, n-tetradecyl(meth)acrylate, cetyl(meth)acrylate, stearyl(meth)acrylate, and behenyl(meth)acrylate; and alicyclic alkyl (meth)acrylates such as cyclohexyl(meth)acrylate, 4-tert-butylcyclohexyl(meth)acrylate, isobornyl(meth)acrylate, dicyclopentanyl(meth)acrylate, and dicyclopentenyl(meth)acrylate. One or more of these alkyl (meth)acrylates can be used. Among these, alkyl (meth)acrylates having linear or branched alkyl groups with 1 to 18 (more preferably 1 to 12) carbon atoms are preferred.
[0015] The content of alkyl (meth)acrylate per 100 parts by mass of the total components constituting the polymer particles is preferably 10 to 100 parts by mass, more preferably 20 to 100 parts by mass, and even more preferably 30 to 100 parts by mass.
[0016] ((meth)acrylic acid ester containing a hydroxyl group) Hydroxylated (meth)acrylic acid esters are, for example, esters of (meth)acrylic acid with a compound having two or more hydroxyl groups. Examples of hydroxylated (meth)acrylic acid esters include hydroxyalkyl (meth)acrylic acid esters. Examples of hydroxyalkyl (meth)acrylic acid esters include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. Other examples of (meth)acrylic acid esters having hydroxyl groups include polyalkylene glycol (meth)acrylates such as polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, and methoxypolyethylene glycol mono(meth)acrylate. Among these, hydroxyalkyl (meth)acrylates having 5 to 20 (more preferably 5 to 15) carbon atoms are preferred.
[0017] (Cross-linkable (meth)acrylic acid ester) As the (meth)acrylic acid ester, it is also possible to use a crosslinkable (meth)acrylic acid ester that can function as a crosslinking agent. The crosslinkable (meth)acrylic acid ester can be a monomer having two or more polymerizable unsaturated bonds. For example, the crosslinkable (meth)acrylic acid ester may be a bifunctional or polyfunctional acrylate having two or more (meth)acryloyl groups. Examples of crosslinkable (meth)acrylic acid esters include 2-hydroxy-3-acryloyloxypropyl (meth)acrylate, ethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and dipropylene glycol di(meth)acrylate. Examples include difunctional (meth)acrylates such as chol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, and glycerin di(meth)acrylate; polyfunctional (meth)acrylates such as pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate; allyl (meth)acrylate; divinylbenzene; and diallyl phthalate. Examples of crosslinkable (meth)acrylic acid esters include silane coupling agents such as 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, and 3-acryloxypropyltrimethoxysilane.
[0018] ((meth)acrylate alkoxyalkyl ester) Examples of the alkoxyalkyl (meth)acrylate include 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, ethoxyethoxyethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, and the like.
[0019] (Aralkyl (meth)acrylate) Examples of the aralkyl (meth)acrylate include benzyl (meth)acrylate, 2-phenylethyl (meth)acrylate, methylbenzyl (meth)acrylate, naphthylmethyl (meth)acrylate, and the like.
[0020] (Aryl (meth)acrylate) Examples of the aryl (meth)acrylate include phenyl (meth)acrylate, 4-hydroxyphenyl (meth)acrylate, tolyl (meth)acrylate, naphthyl (meth)acrylate, and the like.
[0021] (Other (meth)acrylates) Other (meth)acrylic acid esters include alkyl (meth)acrylic acid esters having halogen atoms such as 2-chloroethyl (meth)acrylate, trifluoroethyl (meth)acrylate, 2-(perfluorobutyl)ethyl (meth)acrylate, and perfluorooctylethyl (meth)acrylate; (meth)acrylic acid esters having amino groups such as 2-(dimethylamino)ethyl (meth)acrylate, 2-(diethylamino)ethyl (meth)acrylate, and 3-(dimethylamino)propyl (meth)acrylate; (meth)acrylic acid esters having carboxyl groups such as carboxyethyl (meth)acrylate and carboxypentyl (meth)acrylate; glycidyl (meth)acrylate, glycerin mono(meth)acrylate, and 2-methylglycidyl (meth)acrylate. Examples include (meth)acrylic acid esters and derivatives thereof having epoxy groups such as 3,4-epoxycyclohexylmethyl (meth)acrylate; (meth)acrylates having sulfonic acid groups such as 2-sulfoethyl (meth)acrylate and 3-sulfopropyl (meth)acrylate; (meth)acrylates having phosphate groups such as 2-(phosphonooxy)ethyl (meth)acrylate; (meth)acrylates having isocyanate groups such as 2-isocyanatoethyl (meth)acrylate; heterocyclic (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate; alkyl or allyl group-terminated polyalkylene glycol mono(meth)acrylates such as methoxypolyethylene glycol (meth)acrylate and phenoxypolyethylene glycol (meth)acrylate.
[0022] The total content of (meth)acrylic acid ester relative to 100 parts by mass of the total components constituting the polymer particles is preferably 20 to 100 parts by mass, more preferably 70 to 100 parts by mass, and even more preferably 90 to 100 parts by mass.
[0023] The polymer particles according to one embodiment may contain aromatic vinyl monomers, cyano group-containing monomers, acid group-containing monomers, hydroxyl group-containing monomers, or crosslinkable monomers as constituent units. The polymer particles may also contain these monomers separately from (meth)acrylic acid ester monomers. Furthermore, the polymer particles may contain (meth)acrylic acid ester monomers as these monomers.
[0024] (Aromatic vinyl monomer) Aromatic vinyl monomers can be monomers in which an aromatic group is bonded to a polymerizable double bond. Examples of aromatic vinyl monomers include styrene-based monomers such as styrene, α-methylstyrene, o-,m-, or p-methylstyrene, o-,m-, or p-ethylstyrene, 4-tert-butylstyrene, o-,m-, or p-hydroxystyrene, o-,m-, or p-methoxystyrene, o-,m-, or p-ethoxystyrene, o-,m-, or p-chlorostyrene, o-,m-, or p-bromostyrene, o-,m-, or p-fluorostyrene, and o-,m-, or p-chloromethylstyrene. One or more of these can be used. Among these, styrene is preferred.
[0025] The aromatic vinyl monomer has preferably 8 to 20 carbon atoms, more preferably 8 to 15 carbon atoms. The content of aromatic vinyl monomer relative to 100 parts by mass of the total components constituting the polymer particles is, for example, 0 to 80 parts by mass, preferably 50 to 75 parts by mass.
[0026] In one embodiment, the polymer particles contain both (meth)acrylic acid monomers and aromatic vinyl monomers as constituent units. The total content of (meth)acrylic acid monomers and aromatic vinyl monomers per 100 parts by mass of the total components constituting the polymer particles is, for example, 50 to 100 parts by mass, preferably 70 to 100 parts by mass, more preferably 90 to 100 parts by mass, and even more preferably 95 to 100 parts by mass.
[0027] In one embodiment, the polymer particles contain both an alkyl (meth)acrylate monomer and an aromatic vinyl monomer as constituent units. The total content of the alkyl (meth)acrylate monomer and the aromatic vinyl monomer relative to 100 parts by mass of the total components constituting the polymer particles is, for example, 50 to 100 parts by mass, preferably 70 to 100 parts by mass, more preferably 90 to 100 parts by mass, and even more preferably 95 to 100 parts by mass.
[0028] (Cyano group-containing monomer) Cyano group-containing monomers can be, for example, unsaturated monomers having a cyano group, such as acrylonitrile and methacrylonitrile. One or more of these can be used.
[0029] (Acid group-containing monomer) Acid group-containing monomers are monomers having a polymerizable double bond and an acid group. Examples of acid group-containing monomers include unsaturated carboxylic acid monomers. In this specification, unsaturated carboxylic acid monomers include unsaturated carboxylic acids, as well as their anhydrides and monoesters. Examples of unsaturated carboxylic acid monomers include unsaturated carboxylic acids such as (meth)acrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, and citraconic acid; anhydrides of unsaturated carboxylic acids such as maleic anhydride and itaconic anhydride; and monoesters of polyunsaturated carboxylic acids such as monomethyl maleate, monobutyl maleate, monomethyl itaconic acid, and monobutyl itaconic acid. One or more of these unsaturated carboxylic acid monomers can be used. Among these, (meth)acrylic acid is more preferred.
[0030] The number of carbon atoms in the acid group-containing monomer is preferably 3 to 10, more preferably 3 to 5. The content of the acid group-containing monomer relative to 100 parts by mass of the total components constituting the polymer particles is preferably 0.1 to 10 parts by mass, more preferably 1 to 5 parts by mass.
[0031] (Hydroxyl group-containing monomer) A hydroxyl group-containing monomer is a monomer having a polymerizable double bond and a hydroxyl group. Examples of hydroxyl group-containing monomers include (meth)acrylic acid esters having the hydroxyl group mentioned above. As another example, the polymer particles may contain unsaturated alcohols such as vinyl alcohol or allyl alcohol as constituent components. One or more monomers can be used as the hydroxyl group-containing monomer.
[0032] The number of carbon atoms in the hydroxyl group-containing monomer is preferably 5 to 30, more preferably 5 to 15. The content of the hydroxyl group-containing (meth)acrylic acid ester per 100 parts by mass of the total components constituting the polymer particles is preferably 0.1 to 10 parts by mass, more preferably 1 to 5 parts by mass.
[0033] (Cross-linkable monomer) A crosslinkable monomer is a monomer having a polymerizable double bond and a crosslinkable group. A crosslinkable monomer may be, for example, a monomer having two or more polymerizable unsaturated bonds, or a monomer having a polymerizable unsaturated bond and a crosslinkable group such as an alkoxysilyl group. Examples of crosslinkable monomers include the crosslinkable (meth)acrylic acid esters mentioned above. Other examples include monomers having multiple unsaturated bonds, such as divinylbenzene, trivinylbenzene, diallyl phthalate, diallyl isocyanurate, triallyl isocyanurate, divinyl ether, and trivinyl ether. One or more types of monomers can be used as the crosslinkable monomer.
[0034] The number of carbon atoms in the crosslinkable monomer is preferably 5 to 30, more preferably 5 to 15. The content of the crosslinkable monomer relative to 100 parts by mass of the total components constituting the polymer particles is preferably 0.1 to 10 parts by mass, more preferably 1 to 5 parts by mass.
[0035] (Other polymerizable monomers) The (meth)acrylic resin particles (polymer particles) may be resin particles obtained by polymerizing monomer components that include the (meth)acrylic acid ester and other polymerizable monomers copolymerizable with the (meth)acrylic acid ester. In this case, the (meth)acrylic resin particles may have structural units derived from the (meth)acrylic acid ester and structural units derived from other polymerizable monomers copolymerizable with the (meth)acrylic acid ester.
[0036] Polymer particles according to one embodiment may contain one or more other polymerizable monomers as constituent units. Examples of other polymerizable monomers include the aromatic vinyl monomers, cyano group-containing monomers, acid group-containing monomers, hydroxyl group-containing monomers, or crosslinkable monomers other than (meth)acrylic acid esters. Other polymerizable monomers include unsaturated monomers having nitrogen atoms, vinyl halogenated monomers, vinyl ether monomers, vinyl ester monomers, unsaturated monomers having epoxy groups, and unsaturated monomers having sulfonic acid groups. Polymer particles according to one embodiment may contain one or more of the above monomers as constituent units.
[0037] Examples of unsaturated monomers containing a nitrogen atom include, in addition to cyano group-containing monomers, (meth)acrylamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-methylol(meth)acrylamide, N-butoxymethyl(meth)acrylamide, N-[2-dimethylaminoethyl](meth)acrylamide, N-[3-dimethylaminopropyl Examples include acrylamide monomers such as (meth)acrylamide, diacetoneacrylamide, 4-acryloylmorpholine, and 4-methacryloylmorpholine; acetamide monomers having a vinyl group such as N-vinylacetamide and N-vinyl-N-methylacetamide; and nitrogen-containing heterocyclic compounds having a vinyl group such as N-vinyl-2-pyrrolidone, 4-vinylpyridine, 1-vinylimidazole, 2-vinyl-2-oxazoline, and 2-isopropenyl-2-oxazoline.
[0038] Examples of vinyl halogenated monomers include vinyl chloride and vinyl fluoride.
[0039] Examples of vinyl ether monomers include methyl vinyl ether, ethyl vinyl ether, isobutyl vinyl ether, phenyl vinyl ether, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, and diethylene glycol monovinyl ether.
[0040] Examples of vinyl ester monomers include vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caprylate, vinyl laurate, vinyl stearate, and vinyl versatate.
[0041] Examples of unsaturated monomers having an epoxy group include allyl glycidyl ether.
[0042] Examples of unsaturated monomers having a sulfonic acid group include vinyl sulfonic acid, styrene sulfonic acid, allyl sulfonic acid, methallyl sulfonic acid, and 2-(meth)acrylamide-2-methylpropanesulfonic acid.
[0043] (Physical properties) The following describes the physical properties of polymer particles.
[0044] (Average particle size D50) From the viewpoint of improving resistance to powder shedding and blocking, the average particle size D50 of the polymer particles is preferably 1.4 μm to 10.0 μm, more preferably 1.5 μm to 7.0 μm, and even more preferably 2.5 μm to 5.0 μm. Here, the average particle size D50 is the particle size that accounts for 50% of the cumulative volume-based particle size distribution measured by laser diffraction-scattering, and is measured in accordance with JIS Z8819-2:2019.
[0045] (Glass transition temperature Tg) From the viewpoint of improving adhesion and lithium ion permeability, the glass transition temperature Tg of polymer particles is preferably 0°C to 100°C, and more preferably 20°C to 75°C. The glass transition temperature Tg of polymer particles is calculated using Fox's formula based on the glass transition temperature when each structural unit contained in the polymer is considered a homopolymer. The specific method for calculating the glass transition temperature Tg of polymer particles is to use Fox's formula 1 / Tg = Σ(Xi / Tgi) from the glass transition temperature Tgi of the homopolymer of each structural unit Mi (i=1,2,3...) and the mass fraction Xi of structural unit Mi in the copolymer (ΣXi (total structural units) = 1).
[0046] <Dispersant> The dispersant used in the present invention is a substance intended to prevent the re-aggregation and sedimentation of polymer particles in an aqueous medium. Furthermore, the dispersant may have the effect of easily redispersing polymer particles by stirring even if they have settled. In one embodiment, the dispersant is a water-soluble polymer. The water-soluble polymer may, for example, have hydrophilic functional groups in its side chains. In one embodiment, the water-soluble polymer has a solubility of 0.1 g / 1 mL or more in water at 25°C. The water-soluble polymer may include synthetic polymers, semi-synthetic polymers, and natural polymers.
[0047] The semi-synthetic polymer includes, for example, cellulose derivatives (carboxymethylcellulose or its salts (such as sodium carboxymethylcellulose), hydroxyethylcellulose, etc.) and starch derivatives (such as oxidized starch, modified starch, etc.). Among these, cellulose derivatives are preferred, and sodium carboxymethylcellulose is more preferred, but the polymer is not limited to these. One or more of these can be used.
[0048] Natural polymers include, for example, polysaccharides (such as starch, mannan, pectin, xanthan gum, gellan gum, dextran, pullulan, agar, or alginic acid) or proteins (such as glue or gelatin). To obtain better dispersibility, polysaccharides derived from microbial fermentation, such as xanthan gum, gellan gum, dextran, and pullulan, are preferred as natural polymers, but are not limited to these. One or more of these can be used.
[0049] Synthetic polymers include, for example, N-vinylamide polymers. N-vinylamide polymers are polymers of N-vinylamide compounds. N-vinylamide polymers may be, for example, polyvinylpyrrolidone, poly(N-vinylacetamide), or poly(N-vinylformamide). Another example of synthetic polymers is acrylic acid-based water-soluble polymers. Acrylic acid-based water-soluble polymers include homopolymers or copolymers with acrylic acid as a monomer, and salts thereof. Examples of acrylic acid-based water-soluble polymers include polyacrylic acid, copolymers with acrylic acid as a monomer, and sodium polyacrylate. Yet another example of synthetic polymers is acrylamide-based water-soluble polymers. Acrylamide-based water-soluble polymers include homopolymers or copolymers with acrylamide as a monomer, and salts thereof. Examples of acrylamide-based water-soluble polymers include polyacrylamide, acrylamide-acrylic acid copolymers, and salts thereof. Yet another example of synthetic polymers is polyethyleneimine and polyethylene oxide.
[0050] The dispersant preferably comprises at least one of a cellulose derivative and an N-vinylamide polymer. From the viewpoint of improving dust resistance and adhesion, the content of the dispersant is preferably 1.5 to 19.5 parts by mass, more preferably 2 to 18 parts by mass, even more preferably 3 to 15 parts by mass, and even more preferably 5 to 12 parts by mass, per 100 parts by mass of the total components constituting the polymer particles.
[0051] From the viewpoint of suppressing discoloration of the adhesive, the synthetic polymer is preferably an N-vinylamide polymer. In one embodiment, the N-vinylamide polymer is polyvinylpyrrolidone. Polyvinylpyrrolidone (hereinafter also referred to as PVP) is a polymer of N-vinyl-2-pyrrolidone and can be produced by known methods. Discoloration of the adhesive can be suppressed by using PVP as a dispersant. In one embodiment, the film-forming properties of the adhesive composition are improved by using PVP as a dispersant. Furthermore, the side chains having a highly polar lactam structure can impart high adhesion to a variety of substrates. Moreover, because PVP has a hydrophobic polyethylene backbone and a hydrophilic lactam structure in its structure, it has emulsifying dispersibility and functions as a protective colloid for polymer particles after the polymerization reaction.
[0052] In one embodiment, the weight-average molecular weight of PVP is preferably 5,000 to 500,000, and more preferably 30,000 to 300,000. Setting the weight-average molecular weight to 30,000 or more improves its effect as a protective colloid, while setting it to 300,000 or less allows the viscosity of the pre-emulsion before polymerization to be made more manageable.
[0053] The PVP content is preferably 2 to 18 parts by mass, and more preferably 4 to 12 parts by mass, per 100 parts by mass of monomers constituting the polymer particles. By using PVP within this range, dust resistance and adhesion can be improved.
[0054] In this embodiment, the adhesive composition comprises a dispersant that does not have an acetate group. An example of a dispersant having an acetate group is polyvinyl alcohol (hereinafter also referred to as PVA). PVA is generally obtained by partially saponifying polyvinyl acetate. That is, PVA has a hydrophilic hydroxyl group (-OH) and a hydrophobic acetate group (-CH3COO) in the side chains of its structure. According to the inventors' research, using a dispersant having an acetate group makes the adhesive more prone to discoloration. The inventors believe that the reaction between the highly reactive acetate group and other components leads to discoloration of the adhesive. For example, the reaction between the acetate group of PVA and electrolytes such as LiPF6 in electrolytes sometimes used in non-aqueous secondary batteries may lead to discoloration of the adhesive.
[0055] <Additives> The adhesive composition according to the present invention may contain additives. Additives according to one embodiment include chain transfer agents and / or surfactants. (Chain transfer agent) In one embodiment, the adhesive composition may include a chain transfer agent as an additive to adjust the degree of polymerization. Examples of chain transfer agents include n-dodecyl mercaptan, 2-mercaptoethanol, n-butyl mercaptan, trichloromercaptan, isopropyl alcohol, and at least one selected from this group can be used.
[0056] (Surfactants) In one embodiment, the adhesive composition may contain a surfactant as an additive. Examples of surfactants that can be used include anionic surfactants such as sodium dodecylsulfonate and sodium dodecyl sulfate, nonionic surfactants such as polyoxyethylene nonylphenyl ether and sorbitan monolaurate, or cationic surfactants such as ocdadecylamine acetate. In one embodiment, the surfactant is anionic surfactant, preferably sodium dodecylsulfonate.
[0057] (Other additives) Other additives that the adhesive composition may contain are not particularly limited, but include, for example, known additives. Examples of known additives include non-conductive particles, surface tension modifiers, viscosity modifiers, reinforcing materials, and electrolyte additives. These components may be used individually or in combination of two or more in any ratio.
[0058] <Method for manufacturing adhesive composition> In one embodiment, a method for producing an adhesive composition containing polymer particles includes the step of generating polymer particles by adding a polymerization initiator to an emulsion containing a monomer raw material containing a (meth)acrylic acid ester monomer and a dispersant that does not have an acetate group, and carrying out a polymerization reaction.
[0059] The adhesive composition according to this embodiment can be prepared by known methods. For example, it can be prepared by emulsion polymerization or suspension polymerization using an emulsion solution containing a monomer raw material containing a (meth)acrylic acid ester monomer and a dispersant that does not contain an acetate group.
[0060] (Polymerization initiator) The polymerization initiator is not particularly limited, and conventionally known ones can be used. For example, polymerization initiators commonly used in radical polymerization, such as those listed below, can be used as appropriate.
[0061] Examples of polymerization initiators include persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate; and oils such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and 2-phenylazo-4-methoxy-2,4-dimethylvaleronitrile. Soluble azo compounds; 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis{2-methyl-N-[2-(1-hydroxyethyl)]propionamide}, 2,2'-azobis{2-methyl-N-[2-(1-hydroxybutyl)]propionamide}, 2,2'-azobis[2-(5-methyl-2-imidazoline-2-yl) 2,2'-Azobis[2-(2-imidazolin-2-yl)propane] and its salts, 2,2'-Azobis[2-(3,4,5,6-tetrahydropyrimidine-2-yl)propane] and its salts, 2,2'-Azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} and its salts, 2,2'-Azobis(2-methylpropionamidine) and its salts, Examples include water-soluble azo compounds such as 2,2'-azobis(2-methylpropyneamidine) and its salts, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] and its salts; and organic peroxides such as benzoyl peroxide, cumene hydroperoxide, t-butyl hydroperoxide, t-butyl peroxy-2-ethylhexanoate, and t-butyl peroxyisobutyrate. These may be used individually or in combination of two or more.
[0062] <Uses of adhesive compositions> In one embodiment, the adhesive composition is an adhesive composition for bonding battery components of a non-aqueous secondary battery. Here, "between battery components" refers to, for example, between a separator and a negative electrode, or between a separator and a positive electrode.
[0063] <Separator for non-aqueous secondary batteries> In one embodiment, the separator of a non-aqueous secondary battery comprises a substrate and at least an adhesive layer containing the above-described adhesive composition, provided on at least one surface of the substrate. The separator may further comprise components other than the adhesive layer on the substrate. The separator is a battery component that isolates the positive electrode and the negative electrode in a non-aqueous secondary battery to prevent a short circuit between the positive electrode and the negative electrode.
[0064] (base material) Examples of substrates include those containing organic materials. A substrate containing organic materials is a porous member made of organic materials. Examples of substrates containing organic materials include microporous membranes or nonwoven fabrics containing polyethylene, polyolefin resins such as polypropylene, or aromatic polyamide resins. From the viewpoint of superior strength, polyethylene microporous membranes or nonwoven fabrics are preferred as substrates. The thickness of the substrate is not particularly limited, but is preferably 5 to 30 μm, more preferably 5 to 20 μm, and even more preferably 5 to 18 μm. Furthermore, the substrate may also include an inorganic filler layer.
[0065] Inorganic fillers are electrochemically stable materials in the operating environment of non-aqueous secondary batteries. Examples of inorganic fillers include oxide particles such as aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, BaTiO3, ZrO, and alumina-silica composite oxide; nitride particles such as aluminum nitride and boron nitride; covalent crystalline particles such as silicon and diamond; sparingly soluble ionic crystalline particles such as barium sulfate, calcium fluoride, and barium fluoride; and clay microparticles such as talc and montmorillonite. These particles may be subjected to elemental substitution, surface treatment, or solid solution treatment as needed, and may be used individually or in combination of two or more types. Among these, oxide particles are preferred from the viewpoint of stability in the electrolyte and potential stability.
[0066] (Application method) The following methods (1) to (3) can be used to form an adhesive layer on the substrate described above. That is, (1) A method of applying an adhesive composition to the surface of a substrate and drying it; (2) A method of immersing a substrate in an adhesive composition and then drying it; and (3) A method of applying an adhesive composition onto a release substrate, drying it to produce an adhesive layer, and transferring the obtained adhesive layer to the surface of a substrate. Among these methods, method (1) is preferred because it allows for easy control of the thickness of the adhesive layer.
[0067] More specifically, method (1) includes a step of applying an adhesive composition onto a substrate (application step) and a step of forming an adhesive layer by drying the adhesive composition applied onto the substrate (adhesive layer formation step). Depending on the structure of the non-aqueous secondary battery to be manufactured, the adhesive layer may be formed on only one side of the substrate or on both sides of the substrate.
[0068] (coating process) In the coating process, methods for applying the adhesive composition onto the substrate include, for example, the doctor blade method, the reverse roll method, the direct roll method, the gravure method, the extrusion method, and the brush coating method.
[0069] (Adhesive layer formation process) In the adhesive layer formation process, methods for drying the adhesive composition on the substrate include, for example, drying with warm air, hot air, or low-humidity air, vacuum drying, or drying by irradiation with infrared rays or electron beams. The drying conditions are not particularly limited, but the drying temperature is preferably 30 to 150°C.
[0070] <Non-aqueous secondary battery> In one embodiment, a non-aqueous secondary battery comprises a separator on which an adhesive layer made of an adhesive composition is provided on at least one surface.
[0071] Non-aqueous secondary batteries include, for example, lithium-ion secondary batteries. Lithium-ion secondary batteries are small, lightweight, and have high energy density, and are capable of repeated charging and discharging. Due to these excellent characteristics, lithium-ion batteries are used in a wide range of applications. Non-aqueous secondary batteries may comprise the separator, battery components (positive electrode, negative electrode), and electrolyte mentioned above. [Examples]
[0072] The abbreviations and definitions of the evaluation items in Table 1 are as follows: ST: Styrene BA: n-butyl acrylate 2EHA:2-Ethylhexylacrylate MMA: Methyl methacrylate CHMA: Cyclohexyl acrylate AN: Acrylonitrile MAAC: Methacrylic acid 2HEMA:2-hydroxyethyl methacrylate EDMA: Ethylene glycol dimethacrylate Dust shedding resistance: See Test 1 below. Blocking resistance: See Test 2 below. Adhesion: See Test 3 below. Lithium ion permeability: See Test 4 below. Adhesive discoloration: See Test 5 below.
[0073] [Table 1]
[0074] <Preparation of seed particle A1> Seed particles A1 were prepared as follows: In an emulsifying container, 68.6 parts of deionized water, 56.0 parts of styrene (ST) as monomer raw materials, 13.0 parts of 2-ethylhexyl acrylate (2-EHA), 31.0 parts of methyl methacrylate (MMA), 1.5 parts of 2-hydroxyethyl methacrylate (2-HEMA) as a hydroxyl group-containing monomer, 0.5 parts of sodium dodecylbenzenesulfonate as a surfactant, 6.7 parts of 30% polyvinylpyrrolidone aqueous solution (product name: Pitzcol K-30L, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) as a dispersant, and 3.6 parts of 5% potassium persulfate aqueous solution as a polymerization initiator were added and stirred to obtain a monomer emulsion.
[0075] Next, 68.4 parts of deionized water were charged into a reaction apparatus equipped with a stirrer, reflux condenser, thermometer, dropping device, and nitrogen gas inlet tube. The internal temperature was heated to 80°C while stirring, and 4.4 parts of 5% potassium persulfate aqueous solution were added. Polymerization was carried out for 2 hours while adding the monomer emulsion dropwise at the same temperature. After the dropwise addition of the monomer emulsion was completed, the reaction was carried out for another 2 hours while maintaining the internal temperature at 80°C, and then the internal temperature was cooled to room temperature to obtain seed particles A1 containing polyvinylpyrrolidone. The physical properties were pH 2.0, viscosity 35 mPa·s / 25°C, solid content 41.0%, average particle size D50 of 0.5 μm, and the glass transition temperature calculated using the Fox formula was 65°C.
[0076] <Preparation of Seed Particle A2> Seed particles A2 were prepared as follows: In an emulsifying container, 91.8 parts of deionized water, 75.0 parts of styrene (ST) and 25.0 parts of 2-ethylhexyl acrylate (2-EHA) as monomer raw materials, 1.5 parts of 2-hydroxyethyl methacrylate (2-HEMA) as a hydroxyl group-containing monomer, 0.3 parts of sodium dodecylbenzenesulfonate as a surfactant, 16.0 parts of 30% polyvinylpyrrolidone aqueous solution (product name: Pitzcol K-30L, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) as a dispersant, and 2.0 parts of t-butyl peroxy-2-ethylhexanoate (product name: Perbutyl O, manufactured by NOF Corporation) as a polymerization initiator were added and stirred to obtain a monomer emulsion.
[0077] Next, 141.3 parts of deionized water and 36.8 parts of seed particles A1 were charged into a reaction apparatus equipped with a stirrer, reflux condenser, thermometer, dropping device, and nitrogen gas inlet tube, and the internal temperature was heated to 60°C while stirring. At the same temperature, the monomer emulsion was charged into the reaction vessel, and the polymerization reaction was carried out for 2 hours starting when the internal temperature rose to 85°C. After 2 hours, the reaction was carried out for another 2 hours while maintaining the internal temperature at 85°C, and then the internal temperature was cooled to room temperature to obtain seed particles A2 containing polyvinylpyrrolidone. The physical properties were pH 3.3, viscosity 110 mPa·s / 25°C, solid content 31.0%, average particle size D50 of 1.0 μm, and the glass transition temperature calculated using the Fox formula was 39°C.
[0078] <Examples 1, 2, 3, 9, 10-13 and Comparative Examples 1, 2> In an emulsifying container, the types and amounts of each component shown in Table 1, 97.3 parts of ion-exchanged water, and 2.0 parts of t-butylperoxy-2-ethylhexanoate (trade name: Perbutyl O, manufactured by NOF Corporation) as a polymerization initiator were added and stirred to obtain a monomer emulsion. Table 1 shows the solid content in parts of each component contained in the monomer emulsion. In each example and comparative example, a 30% polyvinylpyrrolidone aqueous solution (trade name: Pitzcol K-30L, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) was used as polyvinylpyrrolidone. The trade name CMC Daicel 1180 (manufactured by Daicel Mirise Co., Ltd.) was used as carboxymethylcellulose sodium. The trade name Aron A-210 (manufactured by Toagosei Co., Ltd.) was used as polyacrylate. The inventors prepared polyacrylamide. The trade name KELZAN M (manufactured by Sansho Co., Ltd.) was used as xanthan gum. For the polyvinyl alcohol used, we used the product name J-POVAL JP-05 (manufactured by Nippon Vinegar Vinegar POVAL Co., Ltd.).
[0079] Next, 127.9 parts of deionized water and 1.2 parts of seed particles A1 were charged into a reaction apparatus equipped with a stirrer, reflux condenser, thermometer, dropping device, and nitrogen gas inlet tube, and the internal temperature was heated to 60°C while stirring. At the same temperature, the monomer emulsion was charged into the reaction vessel, and the polymerization reaction was carried out for 2 hours starting when the internal temperature rose to 85°C. After 2 hours, the reaction was carried out for another 2 hours while maintaining the internal temperature at 85°C, and then the internal temperature was cooled to room temperature to obtain adhesive compositions corresponding to each example and comparative example. Table 1 shows the glass transition temperature and average particle size D50 of the polymer particles contained in the adhesive compositions for each example and comparative example, calculated using the Fox formula. Other physical properties were pH 4.0, viscosity 30 mPa·s / 25°C, and solid content 31.0%.
[0080] <Examples 4, 5> A monomer emulsion was obtained in the same manner as in Example 1, except that the types and amounts of each component shown in Table 1 were used, and 88.2 parts of deionized water were used.
[0081] Next, 139.1 parts of deionized water were charged into a reaction apparatus equipped with a stirrer, reflux condenser, thermometer, dropping device, and nitrogen gas inlet tube, and the internal temperature was heated to 60°C while stirring. At the same temperature, the monomer emulsion was charged into the reaction vessel, and the polymerization reaction was carried out for 2 hours starting when the internal temperature rose to 85°C. After 2 hours, the reaction was carried out for another 2 hours while maintaining the internal temperature at 85°C, and then the internal temperature was cooled to room temperature to obtain the adhesive composition. The physical properties were pH 3.5, viscosity 60 mPa·s / 25°C, and solid content 31.0%.
[0082] <Example 6> A monomer emulsion was obtained in the same manner as in Example 1, except that the types and amounts of each component shown in Table 1 and 96.9 parts of deionized water were used. Furthermore, an adhesive composition was obtained by carrying out a polymerization reaction in the same manner as in Example 1, except that 130.1 parts of deionized water and 9.8 parts of seed particles A1 were used. The physical properties were pH 3.5, viscosity 80 mPa·s / 25℃, and solid content 31.0%.
[0083] <Example 7> A monomer emulsion was obtained in the same manner as in Example 1, except that the types and amounts of each component shown in Table 1 were used, and 86.5 parts of deionized water were used.
[0084] Next, 137.0 parts of deionized water and 1.5 parts of seed particles A2 were charged into a reaction apparatus equipped with a stirrer, reflux condenser, thermometer, dropping device, and nitrogen gas inlet tube, and the internal temperature was heated to 60°C while stirring. At the same temperature, the monomer emulsion was charged into the reaction vessel, and the polymerization reaction was carried out for 3 hours starting when the internal temperature rose to 75°C. After 3 hours, the internal temperature was raised to 85°C, and the reaction was carried out for a further 2 hours, after which the internal temperature was cooled to room temperature to obtain the adhesive composition. The physical properties were pH 3.3, viscosity 20 mPa·s / 25°C, and solid content 31.0%.
[0085] <Example 8> A monomer emulsion was obtained in the same manner as in Example 1, except that the types and amounts of each component shown in Table 1 and 83.7 parts of deionized water were used. Furthermore, an adhesive composition was obtained by carrying out a polymerization reaction in the same manner as in Example 7, except that 139.4 parts of deionized water and 0.5 parts of seed particles A2 were used, and the polymerization reaction was carried out for 4 hours. The physical properties were pH 3.1, viscosity 15 mPa·s / 25℃, and solid content 31.0%.
[0086] <Testing Method> The following tests 1 to 5 were conducted using the adhesive compositions of Examples 1 to 13 and Comparative Examples 1 and 2 (hereinafter also referred to as adhesives).
[0087] (Test 1: Evaluation of resistance to dust shedding) A bar coater was used to apply 1.0 g / m² of adhesive to a single-layer polyethylene separator (SC12-S3, manufactured by GELLEC). 2 The adhesive was applied to a dry state and dried at 40°C. After drying, a load of 200±50g was applied with a finger and rubbed for more than 20cm. The amount of adhesive detached from the separator was used to evaluate the dust resistance. A: Adhesive detachment is less than 25% by visual inspection. B: Approximately 25-50% of the adhesive has detached visually. C: Adhesive detachment is visible to the naked eye at 51% or more.
[0088] (Test 2: Evaluation of blocking resistance) A bar coater was used to apply 1.0 g / m² of adhesive to a separator (SC18-D6, manufactured by GELLEC) equipped with an inorganic filler layer. 2 The adhesive was applied to a dry state and dried at 40°C. The adhesive-coated surfaces were joined together and heat-pressed at 60°C x 6 MPa for 30 seconds. The heat-pressed samples were then cut into 25 mm wide strips, and the 180° peel strength was measured using a peel tester at a speed of 300 mm / min. Blocking resistance was evaluated according to the following criteria. A: Peel strength is less than 5.0 N / m B: Peel strength of 5.0~10.0 N / m C: Peel strength of 10.1N or higher
[0089] (Test 3: Evaluation of Adhesion) A bar coater was used to apply 1.0 g / m² of adhesive to a separator (SC18-D6, manufactured by GELLEC) equipped with an inorganic filler layer. 2 The adhesive was applied to a dry surface and dried at 40°C. The adhesive-coated surface and the negative electrode sheet surface, which had been prepared in-house, were joined together and heat-pressed at 60°C × 6 MPa for 30 seconds. The heat-pressed sample was cut into 25 mm wide strips, and the 180° peel strength was measured using a peel tester at a speed of 300 mm / min. The adhesion was evaluated according to the following criteria. A: Peel strength of 10.1 N / m or more B: Peel strength of 5.0~10.0 N / m C: Peel strength less than 5.0N
[0090] (Test 4: Evaluation of lithium ion permeability) A bar coater was used to apply 1.0 g / m² of adhesive to a separator (SC18-D6, manufactured by GELLEC) equipped with an inorganic filler layer. 2 The sample was applied to a dry state and dried at 40°C. The rate of increase in air permeability was calculated from the Gaurle value (seconds / 100ml) measured using a Gaurle tester, and lithium ion permeability was evaluated according to the following criteria. A: Air permeability increase rate is less than 25% B: Air permeability increase rate of 25-50% C: Air permeability increase rate of 51% or more
[0091] (Test 5: Discoloration of the adhesive) A bar coater was used to apply 1.0 g / m² of adhesive to a separator (SC18-D6, manufactured by GELLEC) equipped with an inorganic filler layer. 2 The adhesive was applied to a dry surface and dried at 40°C. The separator was cut into 20mm x 20mm squares and immersed in 10mL of non-aqueous electrolyte containing LiPF6. It was left in a 60°C atmosphere for 24 hours, and the presence or absence of discoloration on the adhesive-coated surface was visually evaluated. For this test, a non-aqueous electrolyte was used, prepared by dissolving LiPF6 in a 1 mol / L solution in a mixture of organic solvents: ethylene carbonate (EC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). A: Does not discolor. B: Slightly discolored C: Clearly discolored to a reddish-brown.
[0092] <Test Results> Referring to Table 1, the test results for Examples 1-13 and Comparative Examples 1 and 2 will be described.
[0093] In Examples 1-13, no discoloration of the adhesive was observed, as shown in Test 5. Furthermore, in Examples 1-13, as shown in the results of Tests 1-4, excellent results were obtained in all aspects: dust resistance, blocking resistance, adhesion, and lithium ion permeability, with a good balance between these. In addition, there was no sedimentation of polymer particles, or if sedimentation occurred, the polymer particles could be redispersed by stirring.
[0094] In particular, increasing the average particle size D50 improved blocking resistance. According to the inventors' studies, setting D50 to 1.4 μm or more significantly improved blocking resistance. Furthermore, setting D50 to 3.0 μm or more, or 6.0 μm or more, further improved blocking resistance. On the other hand, decreasing the average particle size D50 improved dust shedding resistance. According to the inventors' studies, setting D50 to 10.0 μm or less significantly improved blocking resistance.
[0095] Furthermore, raising the glass transition temperature resulted in improved lithium ion permeability. According to the inventors' studies, setting the glass transition temperature to 0°C or higher significantly improved lithium ion permeability. Raising the glass transition temperature to 30°C or higher further improved lithium ion permeability. On the other hand, lowering the glass transition temperature improved adhesion. According to the inventors' studies, setting the glass transition temperature to 100°C or lower significantly improved adhesion.
[0096] Furthermore, increasing the dispersant content improved dust resistance. According to the inventors' studies, dust resistance was particularly improved when the dispersant content was 1.4 parts by mass or more per 100 parts by mass of the total components constituting the polymer particles. Additionally, decreasing the dispersant content improved adhesion. According to the inventors' studies, adhesion was particularly improved when the dispersant content was 18 parts by mass or less per 100 parts by mass of the total components constituting the polymer particles, and further improved when it was 10 parts by mass or less.
[0097] Furthermore, the use of a dispersant prevented the sedimentation of polymer particles, or if sedimentation occurred, it could be easily redispersed by stirring.
[0098] On the other hand, in Comparative Example 1, the adhesive clearly changed color to a reddish-brown. In Comparative Example 2, the polymer particles settled and aggregated, and did not redisperse even after stirring, making it impossible to conduct the test.
[0099] A comparison of Examples 1-10 with Comparative Example 1 confirmed that discoloration of the adhesive can be suppressed by using a dispersant that does not contain acetate groups. Although the reason why the adhesive did not discolor in Examples 1-10 is not clear, the inventors speculate that in Comparative Example 1, the discoloration occurred because polyvinyl alcohol was used as the dispersant, and the acetate groups in the polyvinyl alcohol have high reactivity and reacted with the surrounding compounds.
[0100] A comparison of Examples 1-10 with Comparative Example 2 confirmed that the presence of a dispersant in the adhesive composition can suppress the sedimentation and aggregation of polymer particles.
[0101] As described above, the present invention has the remarkable effect of providing an adhesive composition that can suppress discoloration.
[0102] The invention is not limited to the embodiments described above, and various modifications and changes are possible within the scope of the invention.
Claims
1. Polymer particles and A dispersant is provided, The polymer particles include (meth)acrylic acid ester monomers, or (meth)acrylic acid ester monomers and aromatic vinyl monomers as constituent units. The total content of the (meth)acrylic acid ester monomer and the aromatic vinyl monomer relative to 100 parts by mass of the monomer constituting the polymer particles is 95 parts by mass or more and 100 parts by mass or less. The dispersant is an N-vinylamide polymer that does not have an acetate group. The dispersant is contained in an amount of 1.5 parts by mass or more and 18 parts by mass or less per 100 parts by mass of monomers constituting the polymer particles. The glass transition temperature of the polymer particles is 0°C or higher and 100°C or lower. The average particle size D50 of the polymer particles is 1.5 μm or more and 10.0 μm or less. Adhesive composition.
2. The adhesive composition according to claim 1, wherein the dispersant is polyvinylpyrrolidone.
3. The adhesive composition according to claim 1, wherein the aromatic vinyl monomer is styrene.
4. The adhesive composition according to claim 1, wherein the polymer particles include a cyano group-containing monomer, an acid group-containing monomer, a hydroxyl group-containing monomer, or a crosslinkable monomer as constituent units.
5. An adhesive composition according to any one of claims 1 to 4, for bonding between battery components of a non-aqueous secondary battery.
6. Substrate and A separator comprising an adhesive layer provided on at least one surface of the substrate, The adhesive layer comprises the adhesive composition described in any one of claims 1 to 4. Separator.
7. A non-aqueous secondary battery comprising the separator described in claim 6.
8. A method for producing an adhesive composition containing polymer particles, The process includes a step of generating polymer particles by carrying out a polymerization reaction in an emulsion containing a (meth)acrylic acid ester monomer, or a monomer raw material containing a (meth)acrylic acid ester monomer and an aromatic vinyl monomer, and a dispersant. The total content of the (meth)acrylic acid ester monomer and the aromatic vinyl monomer relative to 100 parts by mass of the monomer constituting the polymer particles is 95 parts by mass or more and 100 parts by mass or less. The dispersant is an N-vinylamide polymer that does not have an acetate group. The emulsified liquid contains 1.5 to 18 parts by mass of the dispersant with respect to 100 parts by mass of the monomer constituting the polymer particles. The glass transition temperature of the polymer particles is 0°C or higher and 100°C or lower. The average particle size D50 of the polymer particles is 1.5 μm or more and 10.0 μm or less. Manufacturing method.
Citation Information
Patent Citations
Lithium ion battery diaphragm and lithium ion battery
CN118867579A
Composite material, preparation method thereof, isolating membrane, pole piece, battery and electric device
CN120271942A
Polymer, method for preparing polymer, separator, battery, and electric device
CN120289702A
Chemical composition containing copolymer and protective colloid and redispersible in water-base medium,its water-base polymer composition,and its production and use
JP1996239539A
Process for preparing vinyl-acetate resin emulsion
JP2001302709A