Method for manufacturing bismuth ion filtration membranes and its applications

Bismuth ion filtration membranes address the inefficiencies of costly bactericidal materials by producing effective, cost-reduced air filters with enhanced bactericidal and photocatalytic capabilities, generating safe oxygen ions.

JP7953947B2Active Publication Date: 2026-11-19WORK TOGETHER MARKETING CONSULTANT LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2025508946
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-08-18
Filing Date
2023-09-28
Publication Date
2026-11-19
Estimated Expiration
2043-09-28

AI Technical Summary

Technical Problem

Existing bactericidal materials like silver and platinum ions are costly and inefficient, while commercially available air purifiers generate excessive ozone and hydroxyl groups, necessitating a more economical and effective alternative.

Method used

A method for producing bismuth ion filtration membranes involving pretreatment, embedding bismuth ions into a nonwoven fabric substrate, and post-processing to enhance bactericidal and photocatalytic effects, generating over 3 million negative oxygen ions without electrodes.

Benefits of technology

The bismuth ion filtration membranes achieve long-term antibacterial properties and reduced costs by 10 times compared to silver ions, with enhanced photocatalytic bactericidal effects and safe oxygen ion generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007953947000001
    Figure 0007953947000001
  • Figure 0007953947000002
    Figure 0007953947000002
Patent Text Reader

Abstract

In the manufacturing method of a bismuth ion filtration membrane and its application, the manufacturing method includes the steps of: putting a filtration membrane substrate into a washing machine, adding a non-ionic chelating agent solution and water, treating for 1 to 2 hours, and dehydrating after the treatment to obtain a filtration membrane substrate A; putting the filtration membrane substrate A and a chelating bismuth ion solution into a reactor, adding a non-ionic chelating agent solution to react, and obtaining a filtration membrane substrate embedded with bismuth ions after the reaction is complete; and dehydrating and drying the filtration membrane substrate embedded with bismuth ions to obtain a bismuth ion filtration membrane.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention pertains to the technical field of filtration membrane production, and specifically relates to a method for producing a bismuth ion filtration membrane and applications thereof.

BACKGROUND ART

[0002] In recent years, as the prevalence of epidemics has become rather severe, different ionic bactericidal materials have come to be used in masks and air filters, and in addition to silver ions that have been utilized hitherto, developments have also been seen in materials such as platinum and gold. Empirically, it has been found that platinum ions have better and more stable bactericidal functions than silver ions, and also generate a relatively large amount of negative oxygen ions on masks. Therefore, it can be said that platinum ions have higher advantages than silver ions. However, unfortunately, platinum has a relatively high price and cost, and the production material cost reaches as much as 10 times that of silver, so it can be said to be inferior in cost performance. In addition, since platinum is produced using gold ions, the price becomes even higher.

[0003] In applications, we have found that bismuth ions exert a reinforcing effect on other metal ions. In particular, during the recent pandemic of novel coronavirus, bismuth plays a very important role in its application to bactericidal and disinfectant materials. Bismuth not only reinforces the bactericidal and virus-inactivating capabilities of ions, but also enables cost reduction and efficacy improvement, while also providing additional beneficial effects. For example, as a very obvious point, silver ions are capable of sterilization and disinfection, but their price and cost are high. In addition, platinum ions have superior bactericidal properties, but their cost is even higher than that of silver. Therefore, under the circumstance of poor cost performance, when bismuth ions were added, the performance of silver and platinum materials was greatly improved, which further reduced the usage cost of precious metals. Furthermore, tests showed that similar sterilization capabilities could reduce the cost of precious metals by 5 to 10 times. In addition, bismuth ions possess an additional sterilization ability: photocatalytic effect. Under photocatalytic conditions, bismuth can enhance micro-EMC reactions, enabling sterilization within a distance of 1 to 3 feet. This represents a significant added value and improves the functional practicality of the material.

[0004] It is known that the most effective commercially available positive and negative electrode air purifiers generate around 10,000 negative oxygen ions, but because these are generated by electrodes, there is a risk that the generated ozone and hydroxyl groups may exceed the standard. Furthermore, naturally, commercially available air purifiers typically generate around 2,000 to 6,000 negative oxygen ions. However, bismuth ion filtration membranes can generate over 3 million negative oxygen ions without the need for electrodes, making them an extremely economical and environmentally friendly application material. [Overview of the project] [Problems that the invention aims to solve]

[0005] In response to the shortcomings of the prior art, the present invention provides a method for manufacturing a bismuth-in filtration membrane and its applications. [Means for solving the problem]

[0006] To achieve the above objectives, the present invention provides the following technical means.

[0007] The method for producing a bismuth ion filtration membrane includes the following steps.

[0008] (1) Pretreatment of filtration membrane substrate: The filtration membrane substrate is placed in a washing machine, a nonionic chelating agent solution and water are added, and the substrate is immersed and stirred. After the treatment is complete, it is dewatered to obtain filtration membrane substrate A.

[0009] (2) Embedding of bismuth ions: The filtration membrane substrate A obtained in step (1) and the chelating bismuth ion solution are placed in the reaction vessel, and the nonionic chelating agent solution is added and the reaction is carried out. After the reaction is complete, the filtration membrane substrate with embedded bismuth ions is obtained.

[0010] (3) Post-processing: The filtration membrane substrate embedded with bismuth ions obtained in step (2) is subjected to dehydration and drying to obtain a bismuth ion filtration membrane.

[0011] Preferably, the filtration membrane substrate in step (1) is a nonwoven fabric, the nonionic chelating agent is EDTA ammonium, and the concentration of the nonionic chelating agent solution is 1 mol / L.

[0012] Preferably, the immersion and stirring time in step (1) is 1 to 2 hours.

[0013] Preferably, the mass ratio of the filtration membrane substrate to water in step (1) is 4 to 8:50, and the mass ratio of the nonionic chelating agent solution to water is 1:100 to 1000.

[0014] Preferably, the method for preparing the chelating bismuth ion solution in step (2) includes the following steps:

[0015] S1: Scale graphite is placed in an H2O2 / H2SO4 solution, stirred at room temperature for 10 minutes, then filtered and washed, and calcined in a nitrogen gas atmosphere at 500-600°C for 10-20 minutes to obtain pre-treated scale graphite. Subsequently, the pre-treated scale graphite is added to an ethanol aqueous solution in a volume ratio of 1:1, ultrasonically treated for 8-12 hours under stirring conditions, and sheet graphite is obtained after vacuum drying.

[0016] S2 : step S1 Add 50 parts by weight of sheet graphite to 920 parts by weight of deionized water, then add 10 parts by weight of chitosan to adjust the pH to 2-3. Then, stir at 40-50°C and allow the reaction to proceed for 4-6 hours, and after the reaction is complete, add 20 parts by weightChelating bismuth is added. The mixture is allowed to react at 60 to 70°C for 3 to 4 hours, and after the reaction is completed, the chelating bismuth ion solution is obtained.

[0017] Preferably, the nonionic chelating agent in the step (2) is ammonium EDTA, and the concentration of the nonionic chelating agent solution is 1 mol / L. Further, the mass ratio of the filtration membrane substrate A to the chelating bismuth ion solution is 4 to 8:50, and the mass ratio of the nonionic chelating agent solution to the chelating bismuth ion solution is 1:100 to 1000.

[0018] Preferably, the reaction temperature in the step (2) is 30 to 40°C, the reaction time is 10 to 30 min, the reaction gas pressure is 0.1 to 0.15 MPa, and the pH is 6 to 7.

[0019] Preferably, the drying temperature in the step (3) is 60 to 90°C, and the drying time is 4 to 8 h.

[0020] The present invention further protects the bismuth ion filtration membrane produced by the aforementioned production method.

[0021] The present invention further protects the application of the aforementioned bismuth ion filtration membrane in masks and air filters.

Effects of the Invention

[0022] Compared with the prior art, the present invention has the following beneficial effects.

[0023] (1) The present invention proposes for the first time the application of bismuth ions to masks and air filters. The masks and filtration membranes produced with bismuth ions were capable of generating an effect of more than 3 million oxygen anions in test results. The specific numerical value depended on the concentration of bismuth ions used during production.

[0024] (2) In the bismuth ion filtration membrane produced by the present invention, graphite with a favorable layered crystal structure is obtained by subjecting flake graphite to oxidation, acidification and ultrasonic treatment. Moreover, increasing the oxygen-containing functional groups on the graphite surface is beneficial to the progress of the subsequent reaction .So Then, the sheet-like graphite is reacted with chitosan to support chitosan on the graphite surface. Since chitosan contains a large amount of active groups such as amino groups and carboxyl groups, it can react with the oxidized graphite to improve the bonding strength between chitosan and graphite. In addition, since chitosan has good adsorptivity, firstly, it is possible to increase the subsequent loading amount of bismuth ions, thereby increasing the content of bismuth ions in the graphite. Secondly, by improving the bonding force between the graphite and the filtration membrane base material to make the graphite containing bismuth ions less likely to peel off, the produced filtration membrane can have long-term antibacterial properties.

[0025] (3) For the bismuth ion filtration membrane produced by the present invention, bismuth ions are introduced into flake graphite through a chemical reaction, and then the flake graphite is introduced into the filtration membrane base material. Thereby, the photocatalytic effect of bismuth ions can exert a bactericidal effect within a distance of 1 to 3 feet. Moreover, the structure of bismuth ions can also increase the negative oxygen ions generated during air filtration. Producing filtration membranes and masks using bismuth ions can obtain the material with the best cost performance, and the cost can be reduced by 10 times compared with silver ions, which is economical and practical.

Modes for Carrying Out the Invention

[0026] Hereinafter, the technical solutions of the present invention will be described clearly and concisely in combination with specific examples of the present invention. It is needless to say that the described examples are only a part of the examples of the present invention, not all of them. Furthermore, all other examples obtained by a person of ordinary skill in the art based on the embodiments of the present invention without creative efforts shall fall within the protection scope of the present invention.

[0027] All raw materials in the embodiments of the present invention can be obtained from commercially available sources, and among them, the nonionic chelating agent (EDTA ammonium) Chelating bismuth It can be purchased from the Yatian Group. Chelating bismuth The bismuth ion concentration in the sample was set to 5%.

[0028] Example 1

[0029] The method for manufacturing a bismuth ion filtration membrane included the following steps:

[0030] (1) Pretreatment of filtration membrane substrate: 4 kg of nonwoven fabric was placed in a washing machine, 50 kg of water and 500 mL of 1 mol / L EDTA diammonium were added, and the fabric was immersed and stirred for 1 hour. After the treatment was completed, it was dewatered to obtain filtration membrane substrate A.

[0031] (2) Embedding of bismuth ions: The filtration membrane substrate A (4 kg) obtained in step (1) and 50 kg of chelater bismuth ion solution were placed in a reaction vessel, and 500 g of 1 mol / L EDTA ammonium was added to adjust the pH to 6 and the reaction gas pressure to 0.1 MPa. The reaction was then carried out at 30°C for 10 minutes, and after the reaction was complete, a filtration membrane substrate with embedded bismuth ions was obtained.

[0032] (3) Post-processing: After dehydrating the bismuth ion-embedded filtration membrane substrate obtained in step (2), it was dried at 70°C for 6 hours to obtain a bismuth ion filtration membrane.

[0033] The method for preparing the chelating bismuth ion solution included the following steps:

[0034] S1: Scale graphite was placed in an H2O2 / H2SO4 solution (with a volume ratio of H2O2 / H2SO4 of 1:3, a mass concentration of H2O2 of 30%, and a concentration of H2SO4 of 98%) and stirred at room temperature for 10 minutes. Next, the solution was filtered and washed, and then calcined at 500°C for 20 minutes under a nitrogen gas atmosphere to obtain pre-treated scale graphite. Subsequently, the pre-treated scale graphite was added to an ethanol aqueous solution in a volume ratio of 1:1, sonicated for 10 hours under stirring conditions, and then vacuum dried to obtain sheet graphite.

[0035] S2: 50g of sheet graphite from step S1 was added to 920g of deionized water, then 10g of chitosan was added to adjust the pH to 2.5. The reaction was then stirred at 45°C for 5 hours, and after the reaction was complete, 20g of... Chelating bismuth This was added. The mixture was reacted at 65°C for 3.5 hours, and after the reaction was complete, the chelated bismuth ion solution was obtained.

[0036] Example 2

[0037] The method for manufacturing a bismuth ion filtration membrane included the following steps:

[0038] (1) Pretreatment of filtration membrane substrate: 5 kg of nonwoven fabric was placed in a washing machine, 50 kg of water and 500 mL of 1 mol / L EDTA diammonium were added, and the fabric was immersed and stirred for 1.5 hours. After the treatment was completed, it was dewatered to obtain filtration membrane substrate A.

[0039] (2) Embedding of bismuth ions: The filtration membrane substrate A (5 kg) obtained in step (1) and 50 kg of chelater bismuth ion solution were placed in a reaction vessel, and 500 g of 1 mol / L EDTA ammonium was added to adjust the pH to 6.5 and the reaction gas pressure to 0.1 MPa. The reaction was then carried out at 40°C for 10 minutes, and after the reaction was complete, a filtration membrane substrate with embedded bismuth ions was obtained.

[0040] (3) Post-processing: After dewatering the bismuth ion-embedded filtration membrane substrate obtained in step (2), it was dried at 80°C for 6 hours to obtain a bismuth ion filtration membrane.

[0041] The method for preparing the chelating bismuth ion solution included the following steps:

[0042] S1: Scale graphite in H2O2 / H2SO4 solution (volume ratio of H2O2 / H2SO4 is 1:3) (The mass concentration of H2O2 was set to 30%, and the concentration of H2SO4 to 98%). The mixture was then stirred at room temperature for 10 minutes. Next, it was filtered and washed, and then subjected to a nitrogen gas atmosphere and 550°C. Pre-treated scale graphite was obtained by calcining at °C for 15 minutes. Subsequently, the pre-treated scale graphite was added to an ethanol aqueous solution in a volume ratio of 1:1, and ultrasonic treatment was performed for 10 hours under stirring conditions. After vacuum drying, sheet graphite was obtained.

[0043] S2: 50g of sheet graphite from step S1 was added to 920g of deionized water, then 10g of chitosan was added to adjust the pH to 2.5. The reaction was then stirred at 45°C for 5 hours, and after the reaction was complete, 20g of... Chelating bismuth This was added. The mixture was reacted at 65°C for 3.5 hours, and after the reaction was complete, the chelated bismuth ion solution was obtained.

[0044] Example 3

[0045] The method for manufacturing a bismuth ion filtration membrane included the following steps:

[0046] (1) Pretreatment of filtration membrane substrate: 6 kg of nonwoven fabric was placed in a washing machine, 50 kg of water and 500 mL of 1 mol / L EDTA diammonium were added, and the fabric was immersed and stirred for 1 hour. After the treatment was completed, it was dewatered to obtain filtration membrane substrate A.

[0047] (2) Embedding of bismuth ions: The filtration membrane substrate A (6 kg) obtained in step (1) and 50 kg of chelater bismuth ion solution were placed in a reaction vessel, and 500 g of 1 mol / L EDTA ammonium was added to adjust the pH to 7 and the reaction gas pressure to 0.15 MPa. The reaction was then carried out at 40°C for 20 minutes, and after the reaction was complete, a filtration membrane substrate with embedded bismuth ions was obtained.

[0048] (3) Post-processing: After dehydrating the bismuth ion-embedded filtration membrane substrate obtained in step (2), it was dried at 60°C for 7 hours to obtain a bismuth ion filtration membrane.

[0049] The method for preparing the chelating bismuth ion solution included the following steps:

[0050] S1: Scale graphite in H2O2 / H2SO4 solution (volume ratio of H2O2 / H2SO4 is 1:3) (The mass concentration of H2O2 was set to 30%, and the concentration of H2SO4 to 98%). The mixture was then stirred at room temperature for 10 minutes. Next, it was filtered and washed, and then subjected to a nitrogen gas atmosphere and 550°C. Pre-treated scale graphite was obtained by calcining at °C for 20 minutes. Subsequently, the pre-treated scale graphite was added to an ethanol aqueous solution in a volume ratio of 1:1, and ultrasonic treatment was performed for 8 hours under stirring conditions. After vacuum drying, sheet graphite was obtained.

[0051] S2: 50g of sheet graphite from step S1 was added to 920g of deionized water, then 10g of chitosan was added to adjust the pH to 2. The reaction was then stirred at 40°C for 6 hours, and after the reaction was complete, 20g of... Chelating bismuth This was added. The mixture was reacted at 60°C for 4 hours, and after the reaction was complete, the chelated bismuth ion solution was obtained.

[0052] Example 4

[0053] The method for manufacturing a bismuth ion filtration membrane included the following steps:

[0054] (1) Pretreatment of filtration membrane substrate: 8 kg of nonwoven fabric was placed in a washing machine, 50 kg of water and 500 mL of 1 mol / L EDTA diammonium were added, and the fabric was immersed and stirred for 2 hours. After the treatment was completed, it was dewatered to obtain filtration membrane substrate A.

[0055] (2) Embedding of bismuth ions: The 8 kg of filtration membrane substrate A obtained in step (1) and 50 kg of chelater bismuth ion solution were placed in a reaction vessel, and 500 g of 1 mol / L EDTA diammonium was added to adjust the pH to 7 and the reaction gas pressure to 0.15 MPa. The reaction was then carried out at 40°C for 30 minutes, and after the reaction was complete, a filtration membrane substrate with embedded bismuth ions was obtained.

[0056] (3) Post-processing: After dewatering the bismuth ion-embedded filtration membrane substrate obtained in step (2), it was dried at 90°C for 6 hours to obtain a bismuth ion filtration membrane.

[0057] The method for preparing the chelating bismuth ion solution included the following steps:

[0058] S1: Scale graphite in H2O2 / H2SO4 solution (volume ratio of H2O2 / H2SO4 is 1:3) (The mass concentration of H2O2 was set to 30%, and the concentration of H2SO4 to 98%). The mixture was then stirred at room temperature for 10 minutes. Next, it was filtered and washed, and then subjected to a nitrogen gas atmosphere and 600°C. Pre-treated scale graphite was obtained by calcining at °C for 10 minutes. Subsequently, the pre-treated scale graphite was added to an ethanol aqueous solution in a volume ratio of 1:1, and ultrasonic treatment was performed for 12 hours under stirring conditions. After vacuum drying, sheet graphite was obtained.

[0059] S2: 50 parts by weight of sheet graphite from step S1 were added to 920 parts by weight of deionized water, then 10 parts by weight of chitosan was added to adjust the pH to 3. The reaction was then stirred at 50°C for 4 hours, and after the reaction was complete, 20 g of... Chelating bismuth This was added. The mixture was reacted at 70°C for 3 hours, and after the reaction was complete, the chelated bismuth ion solution was obtained.

[0060] Comparative Example 1

[0061] The method for manufacturing a bismuth ion filtration membrane included the following steps:

[0062] (1) Pretreatment of filtration membrane substrate: 4 kg of nonwoven fabric was placed in a washing machine, 50 kg of water and 500 mL of 1 mol / L EDTA diammonium were added, and the fabric was immersed and stirred for 1 hour. After the treatment was completed, it was dewatered to obtain filtration membrane substrate A.

[0063] (2) Embedding of bismuth ions: The filtration membrane substrate A (4 kg) obtained in step (1) and 50 kg of chelater bismuth ion solution were placed in a reaction vessel, and 500 g of 1 mol / L EDTA ammonium was added to adjust the pH to 6 and the reaction gas pressure to 0.1 MPa. The reaction was then carried out at 30°C for 10 minutes, and after the reaction was complete, a filtration membrane substrate with embedded bismuth ions was obtained.

[0064] (3) Post-processing: After dehydrating the bismuth ion-embedded filtration membrane substrate obtained in step (2), it was dried at 70°C for 6 hours to obtain a bismuth ion filtration membrane.

[0065] The method for preparing the chelating bismuth ion solution included the following steps:

[0066] 50g of scale graphite is added to 930g of deionized water, then 20g of Chelating bismuth This was added. The mixture was reacted at 65°C for 3.5 hours, and after the reaction was complete, the chelated bismuth ion solution was obtained.

[0067] Example 1~ 4 Antimicrobial tests were conducted on the bismuth ion filtration membranes manufactured in Comparative Example 1. The test standard was GB / T 23763-2009. The test results are shown in Table 1 below.

[0068] [Table 1]

[0069] Example 1~ 4 Masks were fabricated using the filtration membranes produced in Comparative Example 1, and then the masks underwent antimicrobial performance testing. Following GB / T 20944.3-2008 "Antimicrobial Performance Testing" and standards, the masks were washed 50 times and then tested for antimicrobial performance. The test results are shown in Table 2.

[0070] [Table 2]

[0071] While embodiments of the present invention have been presented and described, those skilled in the art will understand that various changes, modifications, substitutions, and variations can be made to these embodiments without departing from the principles and spirit of the invention. Therefore, the scope of the present invention is limited by the appended claims and their equivalents.

Claims

1. A method for producing a bismuth ion filtration membrane, (1) Pretreatment of filtration membrane substrate: The filtration membrane substrate is placed in a washing machine, EDTA ammonium solution and water are added, and immersion and stirring treatment is performed. After the treatment is completed, it is dewatered to obtain filtration membrane substrate A. (2) Embedding of bismuth ions: The filtration membrane substrate A obtained in step (1) and the chelating bismuth ion solution are placed in a reaction vessel, and then the EDTA ammonium solution is added and the reaction is carried out. After the reaction is complete, a filtration membrane substrate with embedded bismuth ions is obtained. (3) Post-processing: The filtration membrane substrate with bismuth ions embedded obtained in step (2) is subjected to dehydration and drying to obtain a bismuth ion filtration membrane. Includes, The method for preparing the chelating bismuth ion solution in step (2) is as follows: S1: Scale-like graphite H 2 O 2 / H 2 SO 4 The process involves adding the material to a solution, stirring for 10 minutes at room temperature, then filtering and washing, calcining in a nitrogen gas atmosphere at 500-600°C for 10-20 minutes to obtain pre-treated scale graphite, then adding the pre-treated scale graphite to a 1:1 volume-ratio ethanol aqueous solution, ultrasonically treating under stirring conditions for 8-12 hours, and obtaining sheet graphite after vacuum drying. S2: Steps include adding 50 parts by weight of sheet graphite from step S1 to 920 parts by weight of deionized water, then adding 10 parts by weight of chitosan to adjust the pH to 2-3, stirring at 40-50°C for 4-6 hours, adding 20 parts by weight of chelating bismuth after the reaction is complete, reacting at 60-70°C for 3-4 hours, and obtaining the chelating bismuth ion solution after the reaction is complete. A method characterized by including the following.

2. The method for producing a bismuth ion filtration membrane according to claim 1, characterized in that the filtration membrane substrate in step (1) is a nonwoven fabric and the concentration of the EDTA ammonium solution is 1 mol / L.

3. The method for producing a bismuth ion filtration membrane according to claim 1, characterized in that the immersion and stirring treatment time in step (1) is 1 to 2 hours.

4. The method for producing a bismuth ion filtration membrane according to claim 1, characterized in that the mass ratio of the filtration membrane substrate to water in step (1) is 4 to 8:50, and the mass ratio of the EDTA ammonium solution to water is 1:100 to 1000.

5. The method for producing a bismuth ion filtration membrane according to claim 1, characterized in that the concentration of the EDTA ammonium solution in step (2) is 1 mol / L.

6. The method for producing a bismuth ion filter membrane according to claim 1, characterized in that the mass ratio of the filter membrane substrate A to the chelating bismuth ion solution in step (2) is 4 to 8:50, and the mass ratio of the EDTA ammonium solution to the chelating bismuth ion solution is 1:100 to 1000.

7. The method for producing a bismuth ion filtration membrane according to claim 1, characterized in that the reaction temperature in step (2) is 30 to 40°C, the reaction time is 10 to 30 min, the reaction gas pressure is 0.1 to 0.15 MPa, and the pH is 6 to 7.

8. The method for producing a bismuth ion filtration membrane according to claim 1, characterized in that the drying temperature in step (3) is 60 to 90°C and the drying time is 4 to 8 hours.

Citation Information

Patent Citations

  • Preparation method for activated carbon non-woven fabric loaded with monoclinic phase bismuth vanadate

    CN103962121A

  • Anti-coronavirus non-woven fabric, preparation method thereof and mask comprising anti-coronavirus non-woven fabric

    CN114855448A

  • Functional filter

    JP2017205692A

  • Photocatalytic air purification and disinfection compositions and systems

    JP2023520822A