Hollow inorganic particles, a resin composition containing the hollow inorganic particles, a semiconductor package using the resin composition, and a method for manufacturing the hollow inorganic particles.

Hollow inorganic particles with controlled properties and surface treatment address the challenge of enhancing mechanical and electrical properties while maintaining low dielectric constant and refractive index, improving resin and packaging reliability.

JP7953985B2Active Publication Date: 2026-11-19UBE NITTO KASEI CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022033556
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-03-04
Publication Date
2026-11-19
Estimated Expiration
2042-03-04

AI Technical Summary

Technical Problem

Hollow inorganic particles used to impart low dielectric properties to resin materials have low water absorption, which increases the dielectric constant, posing a challenge for achieving both mechanical and electrical property enhancement.

Method used

Development of hollow inorganic particles with a specific surface area of 50 m²/g or less, water absorption rate of 0.2 to 20%, and controlled inner and outer diameters, made from silicon compounds, and treated with a silane coupling agent to enhance water absorption while maintaining structural integrity.

Benefits of technology

The particles provide mechanical and electrical property enhancement, moisture absorption, and reduce dielectric constant and refractive index, improving resin reliability and packaging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007953985000004
    Figure 0007953985000004
  • Figure 0007953985000005
    Figure 0007953985000005
  • Figure 0007953985000001
    Figure 0007953985000001
Patent Text Reader

Abstract

To provide hollow inorganic particles which can compensate for mechanical and electrical properties of resin and can impart a certain level or higher of water absorbability.SOLUTION: Provided are hollow inorganic particles, each of which is a spherical hollow particle having one space formed therein, has a specific surface area of 50 m2 / g or less when measured by a gas adsorption method using a nitrogen gas and has a water absorption ratio of 0.2 to 20%. The hollow inorganic particles according to the present technique can be produced by: a coating step for coating core particles with a silicon compound; a core particle removal step for removing the core particles; and an alkaline heating step for heating hollow inorganic particles after the core particle removal step in an alkaline solution.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to hollow inorganic particles, a resin composition containing the hollow inorganic particles, a semiconductor package using the resin composition, and a method for producing the hollow inorganic particles. [Background technology]

[0002] Hollow inorganic particles are used in a wide range of fields, including fillers, spacers, ceramic raw materials, resin modifiers, adsorbents, electronic materials, semiconductor materials, paints, and cosmetics. In recent years, various technologies have been developed to improve the performance of hollow inorganic particles and to impart properties tailored to various applications.

[0003] For example, Patent Document 1 discloses a method for producing hollow silica particles, which involves firing at a temperature exceeding 950°C to produce hollow silica particles (A) containing air inside the particle, or core-shell type silica particles (B) containing a material that disappears upon firing to form a hollow portion, both of which exhibit a peak at a diffraction angle (2θ) corresponding to a plane spacing (d) in the range of 1 to 12 nm in powder X-ray diffraction measurements. The hollow silica particles produced by this method have an average particle diameter of 0.1 to 1 μm, with more than 80% of the particles having a particle diameter within ±30% of the average particle diameter, and a BET specific surface area of ​​30 m². 2 It is characterized by being less than / g.

[0004] Hollow inorganic particles are also used in the packaging of electronic devices. Electronic devices are sensitive to moisture, and to keep the moisture content inside the packaging low, water-absorbing materials (moisture getters) are sometimes introduced inside. In addition, when resin materials are used in packaging, fillers such as silica are commonly added to compensate for their mechanical properties.

[0005] In cases where low dielectric properties and high electrical insulation resistance are required for this resin material, it is said that using hollow inorganic particles with hollow sections as fillers is effective in compensating for these electrical properties. For these fillers, it is considered necessary to have low water absorption to prevent moisture from being brought into the packaging, but conversely, by giving them water absorption, the fillers can also be given the effect of a moisture getter material.

[0006] In other words, by imparting a certain level of water absorption capacity to the hollow inorganic particles used as fillers, it becomes possible to compensate for the mechanical and electrical properties of the resin, and furthermore, to keep the moisture content inside the packaging low, thereby improving the reliability of the packaging. [Prior art documents] [Patent Documents]

[0007] [Patent Document 1] Japanese Patent Publication No. 2009-203115 [Overview of the Initiative] [Problems that the invention aims to solve]

[0008] However, hollow inorganic particles used to impart low dielectric properties to resin materials actually have low water absorption. Conversely, increasing the water absorption of hollow inorganic particles would raise the dielectric constant of the resin material using them, which presented a problem.

[0009] Therefore, the main objective of this technology is to provide hollow inorganic particles that can complement the mechanical and electrical properties of resins and provide a certain level of water absorption performance. [Means for solving the problem]

[0010] In other words, this technology first involves a spherical hollow particle having a single space inside the particle, The specific surface area measured by gas adsorption using nitrogen gas was 50 m². 2It is less than / g We provide hollow inorganic particles with a water absorption rate of 0.2 to 20%. The average outer diameter of the hollow inorganic particles related to this technology can be set to 0.05 to 5 μm. The inner diameter / outer diameter ratio of the hollow inorganic particles related to this technology can be set to 0.55 to 0.93. The hollow inorganic particles related to this technology can be made from silicon compounds represented by the following general formula (1). [C1] JPEG0007953985000001.jpg30112 (In the formula, R 1 is a non-hydrolyzable group, and is a C1-C20 alkyl group, a C1-C20 alkyl group having a (meth)acryloyloxy group or an epoxy group, a C2-C20 alkenyl group, a C6-C20 aryl group or a C7-C20 aralkyl group, R 2 R represents an alkyl group with 1 to 6 carbon atoms, n is an integer from 0 to 3, and R 1 If there are multiple R 1 They may be the same or different, OR 2 If there are multiple ORs, each OR 2 They may be identical or different. The hollow inorganic particles related to this technology may be surface-treated with a silane coupling agent.

[0011] The hollow inorganic particles related to this technology can be used in resin compositions. The resin composition can be used in semiconductor packaging.

[0012] In this technology, the next step is a coating step in which the core particles are coated with a silicon compound, A core particle removal step to remove the core particles, An alkaline heating step is performed in which the hollow inorganic particles after the core particle removal step are heated in an alkaline solution. The present invention provides a method for producing hollow inorganic particles having the following characteristics: As the core particles used in the production method according to the present technology, particles composed of an organic polymer can be used. The core particle removing step of the production method according to the present technology may include a step of calcining at a temperature of 200°C or higher and 1200°C or lower. Effects of the Invention

[0013] According to the present invention, it is possible to provide hollow inorganic particles that can supplement the mechanical properties and electrical properties of a resin, and can impart water absorption performance of a certain level or higher. The effects described herein are not necessarily limited, and may be any of the effects described in the present specification. Brief Description of the Drawings

[0014] [Figure 1] This is a cross-sectional image view showing an example of the cross-sectional structure of the hollow inorganic particle 1 according to the present technology. [Figure 2] This is a flow chart of the method for producing the hollow inorganic particle 1 according to the present technology. Modes for Carrying Out the Invention

[0015] Hereinafter, preferred modes for carrying out the present invention will be described in detail with reference to the drawings. The embodiments described below show an example of representative embodiments of the present invention, and the scope of the present invention should not be interpreted narrowly thereby.

[0016] <1. Hollow inorganic particle 1> Figure 1 is a cross-sectional image view showing an example of the cross-sectional structure of the hollow inorganic particle 1 according to the present technology. The hollow inorganic particle 1 according to the present invention is a spherical hollow particle having one space inside the particle. That is, the hollow inorganic particle 1 according to the present technology consists of an outer shell 11 and a hollow portion 12. Hereinafter, the features of the hollow inorganic particle 1 according to the present technology will be described in detail.

[0017] The outer shell 11 of the hollow inorganic particle 1 according to the present technology has a specific surface area of 50 m2 exhibits a dense structure of / g or less, with a structure having few pores.

[0018] As a method for increasing the water absorption rate of particles, a method of making the particles porous and adsorbing water molecules into the pores is common. However, when the outer shell of hollow particles is made porous, there is a possibility that a liquid substance permeates into the interior of the hollow particles. When the liquid substance permeates into the interior, it becomes impossible to provide an air layer in the object to be kneaded, and the effects of lowering the dielectric constant and lowering the refractive index cannot be obtained.

[0019] On the other hand, although the outer shell 11 of the hollow inorganic particles 1 according to the present technology has a structure with few pores, the hollow inorganic particles 1 according to the present technology are characterized by a high water absorption rate of 0.2 to 20%, as shown in Examples described later. For this reason, it is possible to exert a moisture absorbing effect while suppressing the permeation of a liquid substance into the interior of the hollow inorganic particles 1. As a result, while being the hollow inorganic particles 1 having a moisture absorbing effect, it is also possible to provide an air layer when mixed with other materials such as a resin, and various products using the hollow inorganic particles 1 according to the present technology can also be imparted with the effect of lowering the dielectric constant and the effect of lowering the refractive index.

[0020] In the present technology, the "specific surface area" refers to a value measured by a gas adsorption method using nitrogen gas. The specific surface area of the hollow inorganic particles 1 according to the present technology is 50 m 2 / g or less is not particularly limited, but is preferably 40 m 2 / g or less, more preferably 30 m 2 / g or less, still more preferably 20 m 2 / g. The lower the specific surface area, the more the structure has fewer pores.

[0021] In this technology, "water absorption rate" refers to the weight increase rate when left standing for 48 hours at 30 degrees Celsius and 90% RH. The lower limit of the water absorption rate of the hollow inorganic particles 1 according to this technology is not particularly limited as long as it is 0.2% or more, but is preferably 0.5% or more, more preferably 1% or more, and even more preferably 2% or more. By setting the water absorption rate of the hollow inorganic particles 1 according to this technology to 0.2% or more, the hygroscopic effect is enhanced, which imparts a dielectric constant reduction effect and a refractive index reduction effect to various products using the hollow inorganic particles 1 according to this technology, and also makes it possible to keep the moisture content inside the packaging low, thereby improving the reliability of the packaging.

[0022] The upper limit of the water absorption rate of the hollow inorganic particles 1 in this technology is not particularly limited as long as it is 20% or less, but is preferably 18% or less, and more preferably 15% or less. By setting the water absorption rate of the hollow inorganic particles 1 in this technology to 20% or less, it is possible to reduce viscosity increase, dispersion problems, etc., caused by water when mixing with other materials such as resins.

[0023] The particle outer diameter L1 of the hollow inorganic particles 1 in this technology can be appropriately designed depending on the purpose. In particular, in this technology, the average particle outer diameter L1 of the hollow inorganic particles 1 is preferably 0.05 to 5 μm, more preferably 0.1 to 3 μm, and even more preferably 0.5 to 2 μm.

[0024] By setting the particle outer diameter L1 of the hollow inorganic particles 1 in this technology to 0.05 μm or more, the proportion of particles dispersed in a primary particle state without aggregation increases. Furthermore, by setting the particle outer diameter L1 of the hollow inorganic particles 1 in this technology to 5 μm or less, it becomes possible to increase the particle packing density when mixing with other materials such as resins, thereby fully achieving the desired effects such as low dielectric constant and low refractive index.

[0025] Furthermore, the inner diameter L2 and outer diameter L1 of the hollow inorganic particles 1 related to this technology can be appropriately designed according to the purpose. In particular, in this technology, it is preferable that the ratio of inner diameter L2 to outer diameter L1 be 0.55 to 0.93, more preferably 0.58 to 0.89, and even more preferably 0.63 to 0.85.

[0026] By setting the inner diameter L2 / outer diameter L1 of the hollow inorganic particle 1 in this technology to 0.55 or greater, a sufficient air layer can be created in the material being kneaded, and as a result, the desired effects such as low dielectric constant and low refractive index can be fully realized. Furthermore, by setting the inner diameter L2 / outer diameter L1 of the hollow inorganic particle 1 in this technology to 0.93 or less, it is possible to prevent the outer shell thickness from becoming thin and to improve the strength of the particles.

[0027] The CV value (coefficient of variation of particle size distribution) of the hollow inorganic particles 1 in this technology is not particularly limited as long as it does not impair the effects of this technology. In particular, in this technology, the CV value of the hollow inorganic particles 1 is preferably 20% or less, more preferably 15% or less, and even more preferably 10% or less.

[0028] When the CV value of the hollow inorganic particles 1 related to this technology is 20% or less, the proportion of particles larger than the average particle outer diameter decreases, making it a suitable material for applications where the inclusion of coarse particles is undesirable.

[0029] In this technology, the CV value is calculated using the following formula. CV value (%)={[Standard deviation of particle outer diameter (μm)] / [Average particle outer diameter (μm)]}×100

[0030] The sphericity of the hollow inorganic particles 1 in this technology is not particularly limited as long as it does not impair the effects of this technology. In particular, the sphericity of the hollow inorganic particles 1 is preferably 0.8 or higher, and more preferably 0.9 or higher.

[0031] If the sphericity of the hollow inorganic particles 1 related to this technology is 0.8 or higher, the fluidity of the particles will increase when mixed with other materials such as resins, and the increase in viscosity can be suppressed.

[0032] In this technology, sphericity is calculated using the following formula. Sphericity = [Minor diameter of particle outer diameter] / [Major diameter of particle outer diameter]

[0033] The material used to form the hollow inorganic particles 1 in this technology is not particularly limited and can be any material that can be used for general inorganic particles. In this technology, it is particularly preferable to use a silicon compound represented by the following general formula (1).

[0034] [ka] (In the formula, R 1 is a non-hydrolyzable group, and is a C1-C20 alkyl group, a C1-C20 alkyl group having a (meth)acryloyloxy group or an epoxy group, a C2-C20 alkenyl group, a C6-C20 aryl group or a C7-C20 aralkyl group, R 2 R represents an alkyl group with 1 to 6 carbon atoms, n is an integer from 0 to 3, and R 1 If there are multiple R 1 They may be the same or different, OR 2 If there are multiple ORs, each OR 2 They may be identical or different.

[0035] Here, the non-hydrolyzable group R 1 In this context, the alkyl group having 1 to 20 carbon atoms is preferably one having 1 to 10 carbon atoms, and this alkyl group may be linear, branched, or cyclic. Examples of this alkyl group include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, tert-butyl group, pentyl group, hexyl group, octyl group, cyclopentyl group, and cyclohexyl group.

[0036] R is a non-hydrolyzable group. 1In this, the C1-C20 alkyl group having a (meth)acryloyloxy group or epoxy group is preferably a C1-C10 alkyl group having the above substituent, and this alkyl group may be linear, branched, or cyclic. Examples of alkyl groups having this substituent include γ-acryloyloxypropyl group, γ-methacryloyloxypropyl group, γ-glycidoxypropyl group, and 3,4-epoxycyclohexyl group.

[0037] R is a non-hydrolyzable group. 1 In this context, the alkenyl group having 2 to 20 carbon atoms is preferably an alkenyl group having 2 to 10 carbon atoms, and this alkenyl group may be linear, branched, or cyclic. Examples of this alkenyl group include vinyl, allyl, butenyl, hexenyl, and octenyl groups.

[0038] R is a non-hydrolyzable group. 1 In this context, the aryl group having 6 to 20 carbon atoms is preferably one having 6 to 10 carbon atoms, such as a phenyl group, a tolyl group, a xylyl group, or a naphthyl group. The aralkyl group having 7 to 20 carbon atoms is preferably one having 7 to 10 carbon atoms, such as a benzyl group, a phenethyl group, a phenylpropyl group, or a naphthylmethyl group.

[0039] R is an alkyl group having 1 to 6 carbon atoms. 2 The group may be linear, branched, or cyclic, and examples include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, tert-butyl group, pentyl group, hexyl group, cyclopentyl group, and cyclohexyl group.

[0040] Examples of silicon compounds represented by the general formula (I) include methyltrimethoxysilane, methyltriethoxysilane, methyltrippropoxysilane, methyltriisopropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, butyltrimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltrippropoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-acryloyloxypropyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-mercaptopropyltrimethyl Examples include toxysilane, 3-aminopropyltrimethoxysilane, dimethyldimethoxysilane, methylphenyldimethoxysilane, dimethyldiethoxysilane, divinyldimethoxysilane, divinyldiethoxysilane, trimethylmethoxysilane, trimethylethoxysilane, trivinylmethoxysilane, trivinylethoxysilane, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetraisopropoxysilane, tetra-n-butoxysilane, tetraisobutoxysilane, tetra-sec-butoxysilane, tetra-tert-butoxysilane, etc. These can be used individually or in combination of two or more.

[0041] The hollow inorganic particles 1 related to this technology may have their surfaces treated with a resin or silane coupling agent, etc., for the purpose of improving fluidity and suppressing viscosity increase when mixed with other materials such as resins.

[0042] Specific examples of silane coupling agents include phenyltriethoxysilane, phenyltrimethoxysilane, diphenyldiethoxysilane, diphenyldimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, alkyltriethoxysilane, alkyltrimethoxysilane, dialkyldiethoxysilane, dialkyldimethoxysilane, alkyltrimethoxysilane, etc. These can be used individually or in combination of two or more.

[0043] The applications of the hollow inorganic particles 1 related to this technology, as described above, are not particularly limited and can be applied to various general applications of hollow inorganic particles 1. In particular, the hollow inorganic particles 1 related to this technology can be suitably used as particles for semiconductor packaging.

[0044] <2. Method for producing hollow inorganic particles 1> Figure 2 is a flow chart of the method for producing hollow inorganic particles 1 according to this technology. The method for producing hollow inorganic particles 1 according to this technology consists of at least a coating step S1, a core particle removal step S2, and an alkaline heating step S3. In addition, this technology can also include a core particle dispersion preparation step S4 and a drying step S5 as needed. Each step will be described in detail below in chronological order.

[0045] (1) Core particle dispersion preparation step S4 The core particle dispersion preparation step S4 is a step in which core particles and water are stirred and mixed to prepare a core particle dispersion. In the core particle dispersion preparation step S4, other additives may be added as needed.

[0046] The core particles that can be used in this technology are not particularly limited as long as they do not impair the effects of this technology, and any core particles that can be used in the general production of hollow inorganic particles can be freely selected and used. For example, particles made of organic polymers such as polymethyl methacrylate (PMMA), polymethyl polyacrylate (PMA), polystyrene (PS), polyethylene (PE), polypropylene (PP), polyurethane (PU), polyimide (PI), polyvinyl chloride (PVC), ethylene vinyl acetate copolymer (EVA), phenolic resin (PF), melamine resin (MF), epoxy resin (EP), polyester resin (PEs), and divinylbenzene polymer can be used, as well as particles in which organic compounds such as hydrocarbon compounds, ester compounds, fatty acids with 6 to 22 carbon atoms, alcohols with 6 to 22 carbon atoms, or inorganic compounds such as silicone oil are emulsions.

[0047] The core particles that can be used in this technology are preferably spherical. Furthermore, their average outer diameter can be freely designed according to the desired size of the hollow space. In particular, in this technology, the average outer diameter of the core particles is preferably 0.04 to 5.8 μm, more preferably 0.08 to 3.5 μm, and even more preferably 0.4 to 2.4 μm.

[0048] By setting the average outer diameter of the core particles to 0.04 μm or more, the proportion of particles dispersed in a primary particle state without aggregation increases. Furthermore, by setting the average outer diameter of the core particles to 5.8 μm or less, it becomes possible to increase the particle packing density when mixing with other materials such as resins, thereby fully achieving the desired effects such as low dielectric constant and low refractive index.

[0049] Depending on the purpose, any additives may be used in the core particle dispersion. Additives that can be used in the core particle dispersion are, for example, used for the purpose of dispersing the core particles in a solvent. These additives are not particularly limited as long as they do not impair the effects of this technology, and general additives can be freely selected and used. Examples of additives that can be used in the core particle dispersion include polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), hydroxyethylcellulose (HEC), polyethylene glycol (PEG), sodium dodecyl sulfate (SDS), carboxymethylcellulose (CMC), polystyrene sulfonic acid (PSS), polyvinyl sulfate (PVS), polyacrylic acid (PAA), and polymethacrylic acid (PMA).

[0050] Furthermore, the solvent and additives used in synthesizing the core particles may be used as they are. In particular, it is desirable that dispersants and emulsifiers used in the synthesis be added for the purpose of stably dispersing the core particles in the solvent. Examples of particle synthesis methods using solvents and additives include dispersion polymerization, soap-free polymerization, emulsion polymerization, swelling seed polymerization, and membrane emulsification.

[0051] Furthermore, commercially available resin particle dispersions can be used as the core particle dispersion. The dispersion medium is not particularly limited as long as it does not impair the effects of this technology, and can be freely selected and used. Examples include water, alcohols such as methanol, ketones such as methyl ethyl ketone, glycols such as ethylene glycol, and glycol ethers such as 1-methoxy-2-propanol. Among these, since water is used as the solvent during synthesis in this technology, it is desirable to select water as the dispersion medium.

[0052] (2) Coating process S1 The coating step S1 is a step in which the core particles are coated with a silicon compound. The coating step S1 includes a dispersant addition step S11, a surfactant addition step S12, a catalyst addition step S13, and a silicon compound addition step S14.

[0053] (2-1) Dispersant addition step S11 The dispersant addition step S11 is a step of adding a dispersant to the core particle dispersion prepared in the core particle dispersion preparation step S4.

[0054] The dispersants that can be used in this technology are not particularly limited as long as they do not impair the effects of this technology, and any dispersants that can be used in the general production of hollow inorganic particles can be freely selected and used. For example, nonionic surfactants such as polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), hydroxyethylcellulose (HEC), and polyethylene glycol (PEG), and anionic surfactants such as sodium dodecyl sulfate (SDS), carboxymethylcellulose (CMC), polystyrene sulfonic acid (PSS), polyvinyl sulfate (PVS), polyacrylic acid (PAA), and polymethacrylic acid (PMA) can be used. Among these, nonionic surfactants are particularly preferred in this technology, and polyvinyl alcohol (PVA) is even more preferred. The use of nonionic surfactants is preferable because they do not promote particle aggregation even when used in combination with cationic surfactants. Furthermore, polyvinyl alcohol (PVA) is even more preferred because the hydrophilic groups contained in it interact with silanol groups.

[0055] The concentration of the dispersant in the core particle dispersion after the dispersant addition step S11 is not particularly limited as long as it does not impair the effects of this technology, but it is preferably 1 g / L or higher. By keeping the concentration of the dispersant in the core particle dispersion within this range, it is possible to prevent the particles from coalescing.

[0056] (2-2) Surfactant addition step S12 The surfactant addition step S12 is a step of adding a cationic surfactant to the core particle dispersion liquid after the dispersant addition step S11. In this technology, by using a cationic surfactant, it is possible to obtain particles in which the hollow 12 is located in the center of the hollow inorganic particle and the thickness of the outer shell 11 is uniform.

[0057] Furthermore, in this technology, by performing the surfactant addition step S12 after the dispersant addition step S11, it is possible to prevent the particles from coalescing together and at the same time increase the concentration of cationic surfactant on the particle surface, thereby preventing the core particles from becoming unevenly distributed. As a result, particles can be obtained in which the hollow 12 is located in the center of the hollow inorganic particle and the thickness of the outer shell 11 is uniform.

[0058] The cationic surfactants that can be used in this technology are not particularly limited as long as they do not impair the effects of this technology, and any cationic surfactants that can be used in the general production of hollow inorganic particles can be freely selected and used. For example, cationic polymer surfactants such as polyethyleneimine (PEI) and polydiallyldimethylammonium chloride (PDDA), and cationic low molecular weight surfactants such as polyvinylamine, tetramethylammonium chloride, and cetyltrimethylammonium bromide can be used. Among these, it is particularly preferable in this technology to use polyethyleneimine (PEI) or polydiallyldimethylammonium chloride (PDDA), which are cationic polymer surfactants. By using cationic polymer surfactants, adsorption to the particle surface becomes easier, and the effect of preventing core particle unevenness is further enhanced.

[0059] The concentration of the cationic surfactant in the core particle dispersion after the surfactant addition step S12 is not particularly limited as long as it does not impair the effects of this technology, but it is preferably 0.05 to 5 g / L. By setting the concentration of the cationic surfactant in the core particle dispersion within this range, it is possible to obtain particles in which the hollow 12 is located in the center of the hollow inorganic particle and the thickness of the outer shell 11 is uniform.

[0060] (2-3) Catalyst addition step S13 The catalyst addition step S13 is a step in which a substance that will act as a catalyst for the hydrolysis condensation reaction that will proceed in the silicon compound addition step S14, which will be described later, is added to the core particle dispersion.

[0061] The catalyst addition step S13 is not limited in order, as long as it is performed before or at the same time as the hydrolysis condensation reaction of the silicon compound described later. That is, it may be performed before, after, or at the same time as the dispersant addition step S11, before, after, or at the same time as the surfactant addition step S12, or before or at the same time as the silicon compound addition step S14 described later.

[0062] The catalyst that can be used in this technology is not particularly limited as long as it does not impair the effectiveness of this technology, and any catalyst that can be used in the general production of hollow inorganic particles can be freely selected and used. For example, ammonia and at least one of amines can be used. Examples of amines include monomethylamine, dimethylamine, and monoethylamine. Among these, ammonia is particularly preferred in this technology because it is less toxic, easy to remove from particles, and inexpensive.

[0063] The amount of catalyst added in catalyst addition step S13 is not particularly limited as long as it does not impair the effectiveness of this technology, and can be freely set according to the purpose.

[0064] (2-4) Silicon compound addition step S14 In the silicon compound addition step S14, a silicon compound is added to the core particle dispersion liquid after the dispersant addition step S11 and the surfactant addition step S12. In the silicon compound addition step S14, the surface of the core particles is coated with the silicon compound as a hydrolysis condensation reaction of the silicon compound proceeds on the surface of the core particles.

[0065] The silicon compound that can be used in this technology is not particularly limited as long as it does not impair the effects of this technology, and any silicone-based compound that can be used in the general production of hollow inorganic particles can be freely selected and used. For example, it is preferable to use the silicon compound represented by the general formula (1) described above. Details of the silicon compound represented by the general formula (1) described above have been described above, so we will omit the explanation here.

[0066] The amount of silicon compound added in the silicon compound addition step S14 is not particularly limited as long as it does not impair the effects of this technology, and can be set according to the purpose of adjusting the outer shell 11 of the hollow inorganic particle 1 to a desired thickness.

[0067] In step S14, the silicon compound may be added to the core particle dispersion in the form of a solution mixed with water or an organic solvent such as methanol or ethanol. The method for preparing the silicon compound solution is not particularly limited as long as it does not impair the effects of this technology, and it can be prepared using general solution preparation methods. For example, the silicon compound solution can be prepared by stirring and mixing the silicon compound with water.

[0068] In the silicon compound addition step S14, any additive can be added separately at the same time as the silicon compound, depending on the purpose. Examples of additives that can be used include dispersants such as polyvinyl alcohol (PVA) and polyvinylpyrrolidone added in the dispersant addition step S11, cationic surfactants such as polyethyleneimine (PEI) and polydiallyldimethylammonium chloride (PDDA) added in the surfactant addition step S12, and catalysts such as ammonia and amines added in the catalyst addition step S13. These additives can also be added to the silicon compound beforehand and then used in the silicon compound addition step S14.

[0069] The method of adding the silicon compound to the core particle dispersion is not particularly limited as long as it does not impair the effects of this technology, and any addition method that can be used in the general production of hollow inorganic particles can be freely selected and used. In this technology, the drop method is particularly preferable. By using the drop method, particles with a small CV value (coefficient of variation of particle size distribution) and uniform particle size can be obtained. Furthermore, by using the drop method, hollow inorganic particles 1 with uniform outer shell thickness 11 can be obtained (there is no difference in the thickness of the outer shell 11 between particles), and for example, when the hollow inorganic particles 1 are mixed with other materials such as resin, even if external force is applied to the particles by stirring or a roll mill, they are less likely to be damaged. In addition, by using the drop method, adhesion between particles can be prevented, the particles are not destroyed during particle crushing and resin kneading, and aggregation after resin kneading can also be prevented.

[0070] Furthermore, when producing hollow inorganic particles 1 with a thin outer shell 11, it is possible to obtain hollow inorganic particles 1 with a uniform outer shell thickness by adding them all at once, without using the dropwise method.

[0071] The dropping rate of the silicon compound in step S14 can also be freely set, as long as it does not impair the effectiveness of this technology. In particular, in this technology, it is preferable to use a dropping rate such that the silicon compound addition time is 24 hours or less in order to prevent the denaturation of the silicon compound.

[0072] (3) Core particle removal process S2 This step involves removing the core particles after performing the coating step S1. Since the core particles are coated with a silicon compound after performing the coating step S1, removing the core particles in this state leaves only the outer shell 11 made of the silicon compound, thus producing hollow inorganic particles 1. Before performing the core particle removal step S2, solid-liquid separation by centrifugation, washing, drying, etc., may be performed as needed.

[0073] The method for removing core particles in the core particle removal step S2 is not particularly limited as long as it does not impair the effectiveness of this technology, and any removal method that can be used in the general production of hollow inorganic particles can be freely selected and used. For example, when using core particles with low solvent resistance, or core particles that are emulsions of organic or inorganic compounds, a method of removing the core particles with an organic solvent can be selected, and when using core particles that can be removed by heating, a method of removing the core particles by heating or calcination can be selected. In this technology, it is particularly preferable to remove the core particles by calcination. By performing calcination, the removal of core particles and the densification of the outer shell 11 layers can be performed simultaneously.

[0074] When removing core particles by firing, the firing conditions can be freely set according to the material of the core particles, etc., as long as the effectiveness of this technology is not impaired. The lower limit of the firing temperature is, for example, 200°C or higher, preferably 300°C or higher, and more preferably 400°C or higher. By setting the firing temperature to 200°C or higher, the removal rate of core particles can be improved.

[0075] Furthermore, the upper limit of the firing temperature is, for example, 1200°C or less, preferably 1100°C or less, and more preferably 1000°C or less. By setting the firing temperature to 1200°C or less, the water absorption rate of the hollow inorganic particles 1 can be improved.

[0076] Furthermore, the atmosphere inside the firing furnace may be air, but it may also be an inert atmosphere where the oxygen concentration is adjusted using an inactivated gas such as nitrogen or argon. By firing in an inert atmosphere, the core particles undergo thermal decomposition (endothermic reaction), thus suppressing heat generation. Therefore, even when firing large quantities, cracking of the 11 layers of the outer shell can be prevented, and temperature control becomes easier.

[0077] Furthermore, it is possible to combine firing in air with firing in an inactive atmosphere. For example, firing in an inactive atmosphere can be followed by firing in air. Firing in air can remove organic components contained in the particles.

[0078] (4) Alkali heating process S3 The alkaline heating step S3 is a step of heating the hollow inorganic particles 1 after the core particle removal step S2 in an alkaline solution. By performing this alkaline heating step S3, the amount of silanol groups etc. on the particle surface increases, and the water absorption rate of the hollow inorganic particles 1 can be improved. The water absorption rate can be arbitrarily adjusted by changing the pH, heating temperature and heating time.

[0079] The pH of the alkaline solution used in the alkaline heating step S3 is not particularly limited as long as it is alkaline, but for example, pH 7 to 14, preferably pH 8 to 14, and more preferably pH 9 to 14. By changing the pH, it is possible to arbitrarily adjust the water absorption rate of the hollow inorganic particles 1.

[0080] The type of alkaline solution that can be used in the alkaline heating step S3 can be freely selected as long as it does not impair the purpose or effects of this technology. Examples include aqueous solutions of alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, and aqueous solutions of ammonia and amines.

[0081] The heating temperature in the alkaline heating step S3 can be freely set as long as it does not impair the effects of this technology. The lower limit of the heating temperature is, for example, 30°C or higher, preferably 40°C or higher, and more preferably 50°C or higher. By setting the heating temperature to 30°C or higher, the water absorption rate of the hollow inorganic particles 1 can be improved.

[0082] Furthermore, the upper limit of the heating temperature is, for example, 90°C or lower, preferably 80°C or lower, and more preferably 70°C or lower. By setting the heating temperature to 90°C or lower, the aqueous solution becomes easier to handle and handling safety is increased.

[0083] The heating time in the alkaline heating step S3 can also be freely set as long as it does not impair the effects of this technology. The lower limit of the heating time is, for example, 5 minutes or more, preferably 10 minutes or more, and more preferably 15 minutes or more. By heating for 5 minutes or more, the water absorption rate of the hollow inorganic particles 1 can be improved.

[0084] Furthermore, the upper limit of the heating time is, for example, 24 hours or less, preferably 12 hours or less, and more preferably 6 hours or less. Limiting the heating time to 24 hours or less contributes to improving productivity.

[0085] By changing the heating temperature and heating time in the alkaline heating process S3, it is possible to arbitrarily adjust the water absorption rate of the hollow inorganic particles 1.

[0086] In the alkaline heating step S3, heating can be performed while stirring. Stirring can be done continuously, or multiple times with appropriate intervals in between.

[0087] (5) Drying process S5 The drying step S5 is a step in which the hollow inorganic particles 1 after the alkaline heating step S3 are dried. Before performing the drying step S5, washing may be performed to remove the alkaline aqueous solution if necessary.

[0088] The drying method in drying step S5 can be freely set to any drying method that can be used for drying inorganic particles, as long as it does not impair the effectiveness of this technology. Examples include natural drying, heat drying, forced-air drying, and reduced-pressure drying, and it is also possible to combine these methods. [Examples]

[0089] The present invention will be described in more detail below based on examples. The embodiments described below are merely examples of typical embodiments of the present invention, and this should not be interpreted as narrowing the scope of the present invention.

[0090] <Experimental Example 1> In Experimental Example 1, we investigated the differences in strength and water absorption rate due to differences in the morphology of hollow inorganic particles.

[0091] 1. Manufacturing of hollow inorganic particles <Examples 1-5> (1) Preparation of core particle dispersion As core particles, polystyrene (PSt) particles with an average particle size of 0.5 μm were mixed with a water:methanol = 1:1 solution by stirring to obtain 5000 g of a core particle dispersion with a concentration of 9 wt%.

[0092] (2) Preparation of silicon compound solution A silicon compound solution was prepared by stirring 1000 g of tetraethoxysilane (TEOS) and 1000 g of methanol at 30°C for 1 minute.

[0093] (3) Addition of dispersant 5000g of the core particle dispersion prepared in (1) was mixed with 100g of a 5wt% polyvinyl alcohol (PVA) aqueous solution and stirred at 30°C for 10 minutes.

[0094] (4) Addition of catalyst To a core particle dispersion containing PVA, 1000 g of 25% aqueous ammonia was added as a catalyst.

[0095] (5) Addition of silicon compound solution The silicon compound solution prepared in (2) was added dropwise to a core particle dispersion containing a dispersant and catalyst over a period of 3 hours. This coated the core particles with the silicon compound, thereby obtaining silicon compound coated resin particles.

[0096] (6) Separation, washing, drying The obtained silicon compound coated resin particles were separated into solid and liquid phases by centrifugation and washed three times with methanol. The washed silicon compound coated resin particles were air-dried for two days and then heat-dried at 110°C.

[0097] (7) Removal of core particles By heating dried silicon compound-coated resin particles in an electric furnace under an air atmosphere at the temperatures listed in Table 1 below for 6 hours, hollow inorganic particles were obtained from which the core particles in the silicon compound-coated resin particles had been removed.

[0098] (8) Alkaline heating The resulting hollow inorganic particles were placed in a sodium hydroxide aqueous solution adjusted to pH=12 and stirred at 60°C for 1 hour.

[0099] (9) Separation, washing, drying After heat treatment in an alkaline aqueous solution, solid-liquid separation was performed by centrifugation, and the material was washed three times with methanol. The washed hollow inorganic particles were air-dried for two days, and then further heated and dried at 110°C.

[0100] <Comparative Examples 1 and 2> After carrying out (1) to (6) of Examples 1 to 5 above, the dried silicon compound coated resin particles were heated in an electric furnace in an air atmosphere at the temperatures listed in Table 1 below for 6 hours to obtain hollow inorganic particles from which the core particles in the silicon compound coated resin particles had been removed.

[0101] <Comparative Example 3> Solid inorganic particles of silicon compounds without hollow spaces were produced using a general inorganic particle manufacturing method, and these were then heated in an electric furnace under an air atmosphere at the temperatures listed in Table 1 below for 6 hours to obtain solid inorganic particles of silicon compounds.

[0102] 2. Evaluation The average particle size, specific surface area, and water absorption rate of the manufactured hollow inorganic particles and solid inorganic particles were measured using the methods described below. Furthermore, the water vapor permeability, dielectric constant, and coefficient of linear expansion of resin samples using the manufactured hollow inorganic particles or solid inorganic particles were measured using the methods described below. As a reference example, a resin sample was prepared without using particles, and its water vapor permeability, dielectric constant, and coefficient of linear expansion were measured.

[0103] (1) Average particle size For the manufactured hollow inorganic particles and solid inorganic particles, samples were taken, and the particle sizes of 70 particles were measured using FE-SEM (JSM-6700F, JEOL Ltd.), and the average particle diameter was calculated.

[0104] (2) Specific surface area The measurement was performed using a gas adsorption method with nitrogen gas.

[0105] (3) Water absorption rate 15 g of hollow inorganic particles or solid inorganic particles dried at 150°C were placed in a constant temperature and humidity chamber at 30°C and 90% RH for 48 hours, and the water absorption rate was determined from the weight change before and after the period.

[0106] (4) Moisture permeability A resin mixture was prepared by mixing epoxy resin (jER828, manufactured by Mitsubishi Chemical Corporation), curing agent (YH306, manufactured by Mitsubishi Chemical Corporation), and 2-ethyl-4-methylimidazole in a weight ratio of 5:6:0.05. Hollow inorganic particles or solid inorganic particles were added to this mixture so that the ratio was 30% by volume, and the mixture was kneaded with a spatula. Next, the kneaded resin mixture was further processed three times using a roll mill (tabletop roll mill, manufactured by Kodaira Seisakusho) with a gap adjusted to 0.08 mm to prepare a resin mixture. The obtained resin mixture was heat-cured to prepare a 1 mm thick plate-shaped sample. The water vapor permeability of the plate-shaped sample was measured using the cup method.

[0107] (5) Dielectric constant A resin mixture was prepared by mixing epoxy resin (jER828, manufactured by Mitsubishi Chemical Corporation), curing agent (YH306, manufactured by Mitsubishi Chemical Corporation), and 2-ethyl-4-methylimidazole in a weight ratio of 5:6:0.05. Hollow inorganic particles or solid inorganic particles were added to this mixture so that the ratio was 20% by volume, and the mixture was kneaded with a spatula. Next, the kneaded resin mixture was further processed three times using a roll mill (tabletop roll mill, manufactured by Kodaira Seisakusho) with a gap adjusted to 0.08 mm to prepare a resin mixture. The obtained resin mixture was poured into a mold measuring 1.2 mm × 1.2 mm × 70 mm and heated and cured at 120°C for 6 hours to prepare a sample for dielectric constant evaluation. The obtained sample was heated and dried at 120°C for 3 hours, and then the dielectric constant was measured at a frequency of 5.8 GHz using the cavity resonator perturbation method.

[0108] (6) Coefficient of linear expansion A resin mixture was prepared by mixing epoxy resin (jER828, manufactured by Mitsubishi Chemical Corporation), curing agent (YH306, manufactured by Mitsubishi Chemical Corporation), and 2-ethyl-4-methylimidazole in a weight ratio of 5:6:0.05. Hollow inorganic particles or solid inorganic particles were added to this mixture so that the ratio was 20% by volume, and the mixture was kneaded with a spatula. Next, the kneaded resin mixture was further processed three times using a roll mill (tabletop roll mill, manufactured by Kodaira Seisakusho) with a gap adjusted to 0.08 mm to prepare a resin mixture. The obtained resin mixture was poured into a 5 mm × 5 mm × 10 mm mold and heated and cured at 120 °C for 6 hours to prepare a sample for evaluation of the coefficient of linear expansion. The coefficient of linear expansion of the obtained sample was measured between 20 and 110 °C using a thermal analyzer.

[0109] 3.Results The results are shown in Table 1 below.

[0110] [Table 1]

[0111] 4. Discussion As shown in Table 1, the hollow inorganic particles in Examples 1-5 had higher water absorption rates than the particles in Comparative Examples 1-3, yet their dielectric constant and coefficient of thermal expansion were equivalent. In other words, while it is generally understood that the dielectric constant and coefficient of thermal expansion of thermosetting resins using inorganic particles increase as their water absorption rates increase, it was found that the hollow inorganic particles related to this technology can maintain low dielectric constant and coefficient of thermal expansion of thermosetting resins using them, even with high water absorption rates.

[0112] Furthermore, as shown in Table 1, the thermosetting resins using the hollow inorganic particles in Examples 1 to 5 had lower moisture permeability compared to the thermosetting resins using the particles in Comparative Examples 1 to 3. From these results, it was found that the hollow inorganic particles related to this technology can be suitably used as a packaging material for semiconductors and the like where low humidity is desired. [Explanation of symbols]

[0113] 1: Hollow inorganic particles 11: Outer shell 12:Hollow

Claims

1. A coating step in which the core particles are coated with a silicone-based compound, A core particle removal step to remove the core particles, The hollow inorganic particles after the core particle removal step are heated to 40°C or higher in an aqueous solution of alkali metal hydroxide in an alkaline heating step, A method for producing hollow inorganic particles having the following characteristics.

2. A method for producing hollow inorganic particles according to claim 1, wherein the core particle is made of an organic polymer.

3. A method for producing hollow inorganic particles according to claim 1 or 2, wherein the core particle removal step includes a step of firing at a temperature of 200°C or higher and 1200°C or lower.

4. A method for producing a resin composition, comprising the step of kneading hollow inorganic particles produced by the manufacturing method described in any one of claims 1 to 3 with a resin.

5. A method for manufacturing a semiconductor package, comprising the step of curing a resin composition manufactured by the manufacturing method described in claim 4.

Citation Information

Patent Citations

  • Production method for spherical silica powder

    JP2003137528A

  • Hollow silica particle and its manufacturing method

    JP2009203115A

  • Hollow silica powder, method for producing the same and application thereof

    JP2011042527A

  • Hollow silica particles and method for producing the same

    JP2020079165A

  • Hollow nano-silica particle, core-shell particle, and method for producing them

    JP2020176037A