Fluorine-containing ethylene vinyl alcohol copolymer resin compositions and mixtures and blends thereof

The fluorine-containing ethylene vinyl alcohol copolymer resin composition addresses die accumulation and screw adhesion issues in EVOH extrusion by incorporating fluorinated polymers, improving film quality and process efficiency.

JP7953992B2Active Publication Date: 2026-11-19CHANG CHUN PETROCHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020218544
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-19
Filing Date
2020-12-28
Publication Date
2026-11-19
Estimated Expiration
2040-12-28

AI Technical Summary

Technical Problem

Conventional EVOH extrusion processes face issues such as die accumulation and undesirable adhesion to the screw, leading to degraded film appearance and mechanical strength, which are not adequately addressed by existing technologies.

Method used

A fluorine-containing ethylene vinyl alcohol copolymer resin composition is developed, incorporating fluorinated polymers to improve material precipitation on the die and reduce adhesion to the screw, while minimizing gel generation and improving film appearance and transmittance.

Benefits of technology

The fluorine-containing EVOH resin composition effectively reduces adhesion and gel formation, enhancing the mechanical properties and appearance of the film, and lowers torque and melting pressure during extrusion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007953992000018
    Figure 0007953992000018
  • Figure 0007953992000019
    Figure 0007953992000019
  • Figure 0007953992000020
    Figure 0007953992000020
Patent Text Reader

Abstract

To provide a fluorine-containing ethylene vinyl alcohol copolymer resin composition, and a mixture and a blend of the same.SOLUTION: There are provided a fluorine-containing ethylene vinyl alcohol copolymer (ethylene-vinyl alcohol copolymer, EVOH) resin composition, and a mixture and a blend of the same. The fluorine-containing ethylene vinyl alcohol copolymer resin composition contains an ethylene vinyl alcohol copolymer and fluorine-based particles. A total content of fluorine ions contained in the fluorine-containing ethylene vinyl alcohol copolymer resin composition is 45 ppm to 41,000 ppm. Adhesion to inside an extruder of the EVOH is reduced, and occurrence of a gel or a gelled product in a subsequent finished product can be effectively reduced.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] (Cross-reference of related applications) The claims of this application claim priority to U.S. Patent Application No. 16 / 729,984, filed on 30 December 2019, entitled “Ethylene Vinyl Alcohol Pellets and Films thereof,” which is a continuation-in-part application and is incorporated herein by reference in its entirety. This application also claims priority to U.S. Patent Applications No. 16 / 877,555 and 16 / 877,570, filed on 19 May 2020, which are incorporated herein by reference in their entirety.

[0002] (Technical field) The present invention relates to a fluorine-containing ethylene vinyl alcohol copolymer (ethylene-vinyl alcohol, EVOH) resin composition. The fluorine-containing ethylene vinyl alcohol copolymer resin composition has particles, and in particular has fluorine-containing particles. The total fluoride ion content in the fluorine-containing EVOH resin composition is 45 ppm to 41,000 ppm. The present invention further discloses mixtures and blends containing the fluorine-containing ethylene vinyl alcohol copolymer resin composition. [Background technology]

[0003] EVOH resins are widely used in multilayer structures for preserving perishable goods. For example, EVOH resins and multilayer structures are commonly used in the food packaging industry, medical device and accessories industry, pharmaceutical industry, electronics industry, and agricultural chemicals industry. EVOH resins are typically added as a separate layer to multilayer structures and used as an oxygen barrier layer.

[0004] Extrusion processes using EVOH frequently result in die accumulation. Another common problem in EVOH extrusion processes is undesirable adhesion to the screw. These problems can degrade the appearance and mechanical strength of the film formed by EVOH. Furthermore, these problems have not yet been adequately addressed or resolved in conventional technologies.

[0005] For example, conventional methods attempt to remove EVOH adhering to the inside of machinery and other equipment by adding boron. However, if the boron ion concentration becomes excessively high, it tends to increase the current and pressure of the extruder. If the dispersion of boron ions is uneven, an excessively high amount of gel will be present in the subsequently formed film, resulting in a defective film appearance.

[0006] Therefore, there is a continued need for EVOH resins that offer better film properties and enable cost-effective manufacturing processes. [Overview of the Initiative] [Problems that the invention aims to solve]

[0007] This invention relates to a fluorinated ethylene vinyl alcohol copolymer (EVOH) resin composition, which has particles, particularly fluorinated particles, and the total fluoride ion content in the fluorinated ethylene vinyl alcohol copolymer resin composition is 45 ppm to 41,000 ppm. The fluorinated EVOH resin composition can be used in the preparation of films or multilayer structures. Since EVOH and fluorinated polymers are immiscible, it is common sense to avoid combining them. For example, the immiscibility of EVOH and fluorinated polymers can be expected to negatively affect the appearance and mechanical properties of the resulting film. [Means for solving the problem]

[0008] Due to problems arising from mismatch, the combination of EVOH and fluorinated polymers (also called fluoropolymers) has conventionally been avoided. However, the present invention has discovered that by preparing an EVOH resin composition using a fluoropolymer, the partial mismatch of the fluoropolymer improves material precipitation on the die and reduces the problem of adhesion to the screw. Furthermore, the inventors have discovered that the fluorinated EVOH resin composition of the present invention not only reduces the adhesion of EVOH to the inside of the extruder, but also effectively reduces the generation of gel or gelled material in the subsequent finished product, improves the appearance and transmittance of the formed film, and can reduce the torque and melting pressure values ​​of the extruder.

[0009] The fluorine-containing EVOH resin composition described above typically comprises an ethylene vinyl alcohol copolymer and at least one fluorine-containing fine particle, and the total fluoride ion content in the fluorine-containing EVOH resin composition may be 45 ppm to 41,000 ppm. The fluorine-containing EVOH resin composition has a surface fluoride ion content, which is preferably between 1 and 126 ppm. The ratio of the surface fluoride ion content to the total fluoride ion content of the fluorine-containing EVOH resin composition may be 0.0015 to 0.03. Furthermore, the fluorine-containing EVOH resin composition according to at least one example may further have a boron content of 50 to 250 ppm.

[0010] The fluorine-containing EVOH resin composition preferably has at least two melting points, in other words, at least a first melting point and a second melting point. The first melting point may be between about 100°C and about 140°C, and the second melting point may be between about 150°C and about 195°C.

[0011] The ethylene vinyl alcohol copolymer in the fluorine-containing EVOH resin composition according to at least one example has an ethylene content and a degree of saponification, of which the ethylene content is about 24 to about 48 moles and the degree of saponification is 99.5 moles or higher, and the fluorine-containing fine particles contain a fluorinated polymer.

[0012] The aforementioned fluorine-containing EVOH resin composition can be used to produce a mixture or a blend, that is, a mixture having the fluorine-containing EVOH resin composition or a blend having the fluorine-containing EVOH resin composition can be produced.

[0013] The mixture having the fluorine-containing EVOH resin composition comprises the fluorine-containing EVOH resin composition and a first ethylene-vinyl alcohol copolymer, wherein, calculated on the basis of 20 g of the mixture, the total fluorine ion content contained therein is 100 ppm to 11000 ppm. The ethylene content of the fluorine-containing EVOH resin composition and the ethylene content of the first ethylene-vinyl alcohol copolymer may be the same or different. The fluorine ion content on the surface of the mixture is preferably between 2 ppm and 55 ppm. The ratio of the fluorine ion content on the surface of the mixture to the total fluorine ion content is preferably 0.0019 to 0.04.

[0014] The blend having the fluorine-containing EVOH resin composition comprises the fluorine-containing EVOH resin composition, a first ethylene-vinyl alcohol copolymer and a second ethylene-vinyl alcohol copolymer, the ethylene content of the first ethylene-vinyl alcohol copolymer and the ethylene content of the second ethylene-vinyl alcohol copolymer are different, wherein, calculated on the basis of 20 g of the blend, the total fluorine ion content contained therein is 200 ppm to 2000 ppm. The ratio of the fluorine ion content on the surface of the blend to the total fluorine ion content is preferably 0.0013 to 0.045. Brief Description of the Drawings

[0015] Hereinafter, the implementation of the technology of the present invention will be described by way of example only with reference to the accompanying drawings.

[0016] [Figure 1] It is a cross-sectional view of an exemplary EVOH pellet of the present invention. [Figure 2] It is a diagram of two melting point temperatures of an exemplary EVOH pellet of the present invention. [Figure 3] It is a cross-sectional view of the EVOH pellet of the present invention being melted and flowing through an extruder.

[0017] It should be understood that each aspect of the present invention is not limited to the arrangements, means and features shown in the accompanying drawings. DESCRIPTION OF EMBODIMENTS

[0018] The present invention relates to a fluorine-containing ethylene vinyl alcohol copolymer (EVOH) resin composition. The fluorine-containing EVOH resin composition has particles dispersed therein, particularly fluorine-containing particles. The fluorine-containing EVOH resin composition can be used for the preparation of films or multilayer structures.

[0019] In one aspect, the present invention provides a fluorine-containing EVOH resin composition. The fluorine-containing EVOH resin composition may take the form of pellets, films, fibers and the like. The fluorine-containing EVOH pellets described herein refer to the form and / or shape of one or more pellets formed through granulation of the fluorine-containing EVOH resin composition. Although the present specification describes the fluorine-containing EVOH resin composition in the form of one or more fluorine-containing EVOH pellets formed through granulation, the fluorine-containing EVOH resin composition may also be processed into forms such as beads, cubes, chips, and shavings. The fluorine-containing EVOH resin composition of the present invention usually comprises an ethylene vinyl alcohol copolymer and at least one fluorine-containing particle, and the particle size of the fluorine-containing particle is 20 μm or less.

[0020] Figure 1 shows a cross-sectional view of an exemplary fluorine-containing EVOH pellet 100 of the present invention. The fluorine-containing EVOH pellet 100 is formed from EVOH, which has an ethylene content. For example, the ethylene content of EVOH may be about 24 to about 48 mole%, about 20 to about 50 mole%, about 25 to about 45 mole%, about 28 to about 42 mole%, or about 30 to about 40 mole%. The fluorine-containing EVOH resin composition 100 can be formed from two or more types of EVOH having different ethylene content. For example, the ethylene content of one of the types of EVOH may be in the range of about 20 to about 35 mole%, for example, about 24 to about 35 mole%, about 28 to about 35 mole%, about 20 to about 32 mole%, about 24 to about 32 mole%, about 28 to about 32 mole%, about 20 to about 30 mole%, or about 24 to about 30 mole%. Furthermore / or, the ethylene content of one of the EVOHs may be in the range of about 36 to about 50 mole%, for example, about 40 to about 50 moles, about 44 to about 50 moles, about 36 to about 45 moles, or about 40 to about 45 moles. However, in some preferred embodiments, the EVOH resin composition 100 is formed from a single EVOH having an ethylene content of about 24 to about 48 moles.

[0021] The fluorine content of the above-mentioned fluorine-containing EVOH resin composition 100 is related to the one or more fluorinated polymers (also referred to herein as "fluorine polymers") added, and the fluorinated polymers can form fluorine-containing fine particles 110 dispersed in the EVOH pellets 100. For example, the one or more fluorine polymers mentioned above include or can be selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene, polyhexafluoropropylene, polychlorotrifluoroethylene (PCTFE), 2-chloro-1,1,3,3,3-pentafluoropropene, dichlorodifluoroethylene, 1,1-dichlorofluoroethylene, and combinations thereof. Furthermore / or, the fluoropolymer may include copolymers derived from at least two of the following: vinylidene fluoride (VDF), hexafluoropropylene (HFP), and tetrafluoroethylene (TFE). In some examples, the fluoropolymer may include copolymers derived from two or more of the following: VDF, HFP, and TFE. For example, the EVOH resin composition 100 may include copolymers derived from VDF and HFP, copolymers derived from TFE and HFP, copolymers derived from VDF and TFE, and / or copolymers derived from VDF, HFP, and TFE. Without being limited to any particular theory, the inventors are convinced that reducing the crystal size of certain fluoropolymers can lower at least one melting point of the EVOH pellet 100.

[0022] The fluorine-containing EVOH resin composition 100 has fluorine-containing particles 110, the particles may be in the form of fine particles, and according to the International Union of Pure and Applied Chemistry (IUPAC), the definition of fine particles is 10 -7 ~10 -4 The particle size of the fine particles in the present invention is preferably such that the principal axis length across the diameter or cross-sectional area is 0.5 to about 19 μm, 1.0 to about 19 μm, or 1.2 to about 16 μm. The size of the fluorine-containing particles can be controlled by adjusting the type or variety of fluoropolymer, the amount of fluoropolymer, and the ethylene content of EVOH. If the fluorine-containing particles are spherical, whether they have the desired particle size is determined by the diameter of their cross-section. If the fluorine-containing particles are not spherical and / or the cross-sectional shape of the fluorine-containing particles is not circular (e.g., elliptical or lumpy), whether the fluorine-containing particles have the desired particle size is determined by the principal axis length of the cross-section of the fluorine-containing particles. The principal axis is defined as the axis with the longest length. In some examples, the particle size of all fluorine-containing particles 110 evaluated on the cross-section of the fluorine-containing EVOH resin composition 100 is 20 μm or less, for example, 19 μm or less, 18 μm or less, 16 μm or less, 14 μm or less, or 12 μm or less. In other words, in some examples, the particle size of the fluorine-containing particles 110 does not exceed 20 μm, for example, not exceeding 19 μm, 18 μm, 16 μm, 14 μm, or 12 μm. The particle size of the fluorine-containing particles 110 may be 0.1 μm or larger, 0.3 μm or larger, 0.5 μm or larger, or 0.7 μm or larger. For example, the fluorine-containing EVOH resin composition 100 may have fluorine-containing particles 110 with a particle size of 1.0 to about 19 μm or 1.2 to about 16 μm. In some examples, all fluorine-containing particles 110 evaluated on the cross-section of the fluorine-containing EVOH resin composition 100 are within the desired particle size range described herein. However, in some examples, the majority of the fluorine-containing particles 110 evaluated on the cross-section of the fluorine-containing EVOH resin composition 100 are within the desired particle size range. Exemplary factors that may determine whether the particle size is within a desired range may include (a) the amount of fluoropolymer, (b) the ethylene content of EVOH, (c) the type of fluoropolymer, (d) the temperature in the extruder, and (e) the screw rotation speed.

[0023] As shown in Figure 2, the fluorine-containing EVOH resin composition 100 can have at least two melting points. In some examples, one melting point in the fluorine-containing EVOH resin composition 100 (e.g., the first melting point) is about 100°C to about 140°C, for example, about 105°C to about 135°C, about 110°C to about 135°C, or about 120°C to about 130°C, of ​​which the first melting point is derived from the fluorine-containing particles. Furthermore / or, one of the melting points (e.g., the second melting point) is about 150°C to about 195°C, for example, about 158°C to about 190°C, or about 164°C to about 187°C, of ​​which the second melting point is derived from the ethylene vinyl alcohol copolymer. In some examples, the fluorine-containing EVOH resin composition 100 has at least three different melting points. In other examples, the fluorine-containing EVOH resin composition 100 has at least four, at least five, or at least six different melting points. Furthermore / or, the degree of saponification of the fluorine-containing EVOH resin composition 100 may be 90 mole% or more, preferably 95 mole% or more, preferably 97 mole% or more, and preferably 99.5 mole% or more.

[0024] The fluorine-containing EVOH resin composition 100 described above does not contain polyalkylene oxide or does not need to contain it substantially. For example, the fluorine-containing EVOH resin composition 100 may have less than 5 wt% polyalkylene oxide, for example, less than 4 wt%, less than 3 wt%, less than 2 wt%, less than 1 wt%, or less than 0.5 wt%.

[0025] The fluorine-containing EVOH resin composition 100 described above helps to more efficiently prepare the EVOH film formed thereby. For example, the fluorine-containing EVOH resin composition 100 can improve precipitation onto the die and reduce the problem of adhesion to the screw during the EVOH film manufacturing process. Suitable methods and equipment for preparing the fluorine-containing EVOH film may include methods and equipment readily understood by those skilled in the art. The inventors are confident that by using a partially miscible (and partially immiscible) fluoropolymer and preparing a fluorine-containing EVOH resin composition 100 containing fluorine-containing particles 110, some of the fluoropolymer will separate on the inner surface of the extruder, forming a coating layer 120. Figure 3 illustrates the coating layer 120 formed on the inner surface of the extruder by some of the fluoropolymer of the fluorine-containing EVOH pellets in the present invention. Furthermore, the fluorine polymer layer coating the inner wall of the extruder protects the EVOH resin flowing through the extruder, which is advantageous in preventing discoloration of the EVOH film even when the extrusion process of the fluorine-containing EVOH pellets is carried out at high temperatures.

[0026] In another embodiment, the fluorine-containing EVOH resin composition of the present invention may contain one or more of the characteristics, attributes, or properties of the EVOH resin and / or pellets discussed herein. The addition of a fluoropolymer may contribute to the screw processing of the EVOH resin composition. In particular, the adhesion of the fluoropolymer to the inner wall of the screw extruder reduces the flow resistance as the EVOH resin composition passes through the screw extruder. According to one preferred embodiment, the total fluoride ion content / concentration in the fluorine-containing EVOH resin composition provided by the present invention is 45 ppm to 41000 ppm, and the total fluoride ion content is calculated relative to the fluorine-containing EVOH resin composition. The total fluoride ion content in the fluorine-containing EVOH resin composition is 45-41000 ppm, 45-38000 ppm, 45-35000 ppm, 45-33000 ppm, 45-30000 ppm, 45-28000 ppm, 45-25000 ppm, 45-23000 ppm, 45-20000 ppm, 45-18000 ppm, 45-15000 ppm, 45-13000 ppm, 4 5~10000ppm, 45~8000ppm, 45~5000ppm, 45~3000ppm, 45~1000ppm, 45~800ppm, 45~500ppm, 45~300ppm, 45~ 100ppm, 100~41000ppm, 100~38000ppm, 100~35000ppm, 100~33000ppm, 100~30000ppm, 100~28000ppm, 100 ~25000ppm, 100~23000ppm, 100~20000ppm, 100~18000ppm, 100~15000ppm, 100~13000ppm, 100~10000ppm , 100~8000ppm, 100~5000ppm, 100~3000ppm, 100~1000ppm, 100~800ppm, 100~500ppm, 100~300ppm, 1000~4 1000ppm, 1000~38000ppm, 1000~35000ppm, 1000~33000ppm, 1000~30000ppm, 1000~28000ppm, 1000~25000 ppm, 1000~23000ppm, 1000~20000ppm, 1000~18000ppm, 1000~15000ppm, 1000~13000ppm, 1000~10000ppm,1000~8000ppm, 1000~5000ppm, 1000~3000ppm, 10000~41000ppm, 10000~38000ppm, 10000~35000ppm, 10000~33000ppm, 10 000~30000ppm, 10000~28000ppm, 10000~25000ppm, 10000~23000ppm, 10000~20000ppm, 10000~18000ppm, 10000~15000ppm The ranges of 10,000-13,000 ppm, 20,000-41,000 ppm, 20,000-38,000 ppm, 20,000-35,000 ppm, 20,000-33,000 ppm, 20,000-30,000 ppm, 20,000-28,000 ppm, 20,000-25,000 ppm, 20,000-23,000 ppm, 30,000-41,000 ppm, 30,000-38,000 ppm, 30,000-35,000 ppm, or 30,000-33,000 ppm are acceptable. Surprisingly, it was found that when the total fluoride ion content of the fluorine-containing EVOH resin composition is within the range of 45 to 41,000 ppm, the fluorine can act as a lubricant and anti-adhesion agent, reducing adhesion to dies or screws during processing and improving processability. Furthermore, in this invention, if the total fluoride ion content of the fluorine-containing EVOH resin composition 100 containing fluorine-containing particles 110 is within a desired range, the fisheye pattern generated during EVOH film formation is reduced, improving its mechanical properties and film appearance. Since the above-mentioned total fluoride content is related to the type of fluoropolymer added, the amount of fluoropolymer, the ethylene content of the EVOH, the kneading method, the boron content, etc., engineers can control the total fluoride ion content of the fluorine-containing EVOH resin composition 100 within a desired range by considering these factors.

[0027] According to one preferred embodiment, the fluoride ion content / concentration on the surface of the fluorine-containing EVOH resin composition provided by the present invention is between 1 and 126 ppm, and the fluoride ion content on the surface is calculated for the fluorine-containing EVOH resin composition. The fluoride ion content on the surface of the fluorine-containing EVOH resin composition is 1-126 ppm, 1-115 ppm, 1-100 ppm, 1-90 ppm, 1-80 ppm, 1-70 ppm, 1-60 ppm, 1-50 ppm, 1-40 ppm, 1-30 ppm, 1-20 ppm, 1-10 ppm, 5-126 ppm, 5-115 ppm, 5-100 ppm, 5-90 ppm, 5-80 ppm, 5-70 ppm, 5-60 ppm, 5-50 ppm, 5-40 ppm, 5-30 ppm, 5~20ppm, 5~10ppm, 15~126ppm, 15~115ppm, 15~100ppm, 15~90ppm, 15~80ppm, 15~70ppm, 15~60ppm, 15~50ppm, 15~40ppm, 15~30ppm , 15~20ppm, 25~126ppm, 25~115ppm, 25~100ppm, 25~90ppm, 25~80ppm, 25~70ppm, 25~60ppm, 25~50ppm, 25~40ppm, 25~30ppm, 35~12 6ppm, 35~115ppm, 35~100ppm, 35~90ppm, 35~80ppm, 35~70ppm, 35~60ppm, 35~50ppm, 35~40ppm1~126ppm, 45~115ppm, 45~100ppm, 4 5~90ppm, 45~80ppm, 45~70ppm, 45~60ppm, 45~50ppm, 55~126ppm, 55~115ppm, 55~100ppm, 55~90ppm, 55~80ppm, 55~70ppm, 55~60ppm m, 65-126 ppm, 65-115 ppm, 65-100 ppm, 65-90 ppm, 65-80 ppm, 65-70 ppm, 75-126 ppm, 75-115 ppm, 75-100 ppm, 75-90 ppm, 75-80 ppm, 85-126 ppm, 85-115 ppm, 85-100 ppm, 85-90 ppm, 95-126 ppm, 95-115 ppm, 95-100 ppm, 105-126 ppm, 105-115 ppm, or 120-126 ppm are acceptable.The term "fluoride ions on the surface" refers to the amount of fluoride compounds present near the surface of the EVOH resin pellet, and is distinct from the total fluoride ion content in the EVOH resin pellet. The surface fluoride ion content was analyzed using an ion chromatograph (Metrohm 930 Compact IC Flex / Ses / PP / Deg), and the NIEA W415.54B water anion detection method was used for the analysis. In the pretreatment, 0.5 g of sample pellet was first placed in 5 c.c. of methanol, transferred to a 60°C environment, stirred for 4 hours, filtered, the pellet was removed, 0.5 cc of the liquid was taken, the liquid was burned using an oxygen cylinder, extracted with water, and then chemically analyzed. By dissolving EVOH in a sparingly soluble methanol solution, fluoride ions on the surface were precipitated.

[0028] The fluoride ion content on the surface is influenced by a combination of factors, including the type of fluorine-containing polymer, the amount of fluorine-containing polymer added, the ethylene content, and the boron content. The actual amount of fluorine present on the surface is mainly influenced by the amount of fluorine-containing polymer added. However, differences in the fluorine-containing polymer and ethylene content also affect the various reaction levels between EVOH and the fluorine-containing polymer, resulting in different ratios of fluorine concentrations on the EVOH surface and within the EVOH pellets. Furthermore, the boron content affects the viscosity of EVOH, which not only influences the reaction time but also creates a certain degree of competition with the fluorine-containing particles, potentially causing slight reactions with EVOH and resulting in differences in surface fluorine concentration. Therefore, the fluorine content on the surface according to this invention is the result obtained by comprehensively testing the influence of factors such as the type of fluorine-containing polymer, the amount of fluorine-containing polymer added, the ethylene content, and the boron content. Those skilled in the art can adjust the above-mentioned variable elements according to routine tests to obtain the desired surface fluorine concentration.

[0029] Furthermore / or, in one preferred embodiment, the fluorine-containing EVOH resin composition provided by the present invention has a surface fluorine ion content to total fluorine ion content ratio of 0.0015 to 0.03. The ratio of fluoride ion content to total fluoride ion content on the surface of the fluorine-containing EVOH resin composition is 0.0015~0.03, 0.0015~0.028, 0.0015~0.026, 0.0015~0.024, 0.0015~0.022, 0.0015~0.02, 0.0015~0.018, 0.0015~0.016, 0.0015~0.014, 0.0015~0.012, 0.0015~0.01, 0.0015~0.007, 0.0015~0.005, 0.0015~0.003, 0.00 15~0.0025, 0.0015~0.002, 0.0015~0.0017, 0.003~0.03, 0.003~0.028, 0.003~0.026, 0.003~0.024, 0.003~0.022, 0.003~0.02, 0.003~0.018, 0.003~0.016, 0.003~0.014, 0.003~0.012, 0.003~0.01, 0.003~0.007, 0.003~0.005, 0.005~0.03, 0.005~0.028, 0.005~0.026, 0.0 0.05~0.024, 0.005~0.022, 0.005~0.02, 0.005~0.018, 0.005~0.016, 0.005~0.014, 0.005~0.012, 0.005~0.01, 0.005~0.007, 0.007~0.03, 0.007~0.028, 0.007~0.026, 0.007~0.024, 0.007~0.022, 0.007~0.02, 0.007~0.018, 0.007~0.016, 0.007~0.014, 0.007~0.012, 0.007~0 0.01, 0.009~0.03, 0.009~0.028, 0.009~0.026, 0.009~0.024, 0.009~0.022, 0.009~0.02, 0.009~0.018, 0.009~0.016, 0.009~0.014, 0.009~0.012, 0.009~0.01, 0.011~0.03, 0.011~0.028, 0.011~0.026, 0.011~0.024, 0.011~0.022, 0.011~0.02, 0.011~0.018, 0.011~0.016, 0.The ranges of 0.011~0.014, 0.011~0.012, 0.015~0.03, 0.015~0.028, 0.015~0.026, 0.015~0.024, 0.015~0.022, 0.015~0.02, 0.015~0.018, 0.015~0.016, 0.02~0.03, 0.02~0.028, 0.02~0.026, 0.02~0.024, 0.02~0.022, 0.025~0.03, 0.025~0.028, or 0.025~0.026 are acceptable. According to one aspect of the present invention, when the total fluoride ion content is high and the surface fluoride ion content is low, fluoride ions are released relatively late in the extruder, affecting the transmittance. However, when the surface fluoride ion content is at a certain level, there is no need to wait for the melting and decay of EVOH, so fluoride ions are released relatively quickly, reducing precipitation. However, if the surface fluoride ion content is excessively high, it affects the behavior of the gel during film formation. Therefore, the transmittance effect can be improved by controlling the ratio of surface fluoride ion content to total fluoride ion content within a specific range.

[0030] Under certain circumstances, the fluorine-containing EVOH resin composition may contain boron compounds and / or boric acid and / or cinnamic acid and / or alkali metals and / or conjugated polyenes and / or lubricants and / or alkaline earth metals. The above-mentioned substances can impart favorable properties to the EVOH resin composition.

[0031] Furthermore / or, according to other aspects of the present invention, the fluorine-containing EVOH resin composition may have fluorine-containing particles and a boron content of 50 to 250 ppm, the boron content being calculated relative to the final fluorine-containing EVOH resin composition. Without being limited to any particular theory, the inventors are convinced that by adding a boron compound to an EVOH resin composition having fluorine-containing particles, thereby bringing the boron content of the EVOH to 50 to 250 ppm, the tackiness of the EVOH resin composition in the extrusion process of a screw extruder is reduced or eliminated, and the uniformity of film thickness and plasticity are further improved. Under certain circumstances, such an EVOH resin composition can remove or at least partially remove EVOH resin that has tackled to the inner surface of the screw extruder during the extrusion process, thereby cleaning the screw extruder.

[0032] A typical fluorine-containing EVOH resin composition may contain an ethylene vinyl alcohol copolymer, one or more fluorine-containing particles, and a boron compound, of which the boron content of the ethylene vinyl alcohol copolymer resin composition is 50 to 250 ppm. In some situations, the boron content of the fluorine-containing EVOH resin composition, based on the total weight of the fluorine-containing EVOH resin composition, is approximately 50 to 250 ppm, approximately 50 to approximately 225 ppm, approximately 50 to approximately 200 ppm, approximately 50 to approximately 175 ppm, approximately 50 to approximately 150 ppm, approximately 50 to approximately 125 ppm, approximately 50 to approximately 100 ppm, approximately 75 to 250 ppm, approximately 75 to approximately 225 ppm, approximately 75 to approximately 200 ppm, approximately 75 to approximately 175 ppm, and approximately 75 The boron content may be approximately 150 ppm, approximately 75-125 ppm, approximately 75-100 ppm, approximately 100-250 ppm, approximately 100-225 ppm, approximately 100-200 ppm, approximately 100-175 ppm, approximately 100-150 ppm, approximately 100-125 ppm, approximately 150-250 ppm, approximately 150-225 ppm, approximately 150-200 ppm, approximately 150-175 ppm, approximately 200-250 ppm, or approximately 200-225 ppm. When the boron content of the fluorine-containing EVOH resin composition is within a certain range, the viscosity of the fluorine-containing EVOH resin composition increases, and the opportunity for the fluorine-containing EVOH resin composition to adhere to the screw is reduced, or EVOH on the screw can be removed, thereby giving the material a self-cleaning function and further improving the uniformity of the film thickness. Under certain circumstances, the fluorine-containing EVOH resin composition may contain not only 50-250 ppm of boron, but also cinnamic acid, alkali metals, conjugated polyenes, lubricants, alkaline earth metals, their salts, and / or mixtures thereof. The above-mentioned substances are commonly found in EVOH resin compositions and contribute to their superior properties. When the content of compounds having a conjugated polyene structure per unit weight in the EVOH resin composition is 1-30,000 ppm, heat discoloration is further suppressed, and thermal stability can be improved. When the content of compounds having alkali metals or alkaline earth metals per unit weight in the fluorine-containing EVOH resin composition is 1-1,000 ppm in terms of metal content, long-run moldability can be improved.Furthermore, if the lubricant content per unit weight in the fluorine-containing EVOH resin composition is 1 to 300 ppm, processability can be improved.

[0033] In one aspect of the present invention, the boron content is controlled within a specific range in the presence of a fluoropolymer. This not only improves the plasticity and processing properties of EVOH, but also further improves the appearance characteristics of the product.

[0034] Under certain circumstances, boron compounds may contain boric acid or its metal salts. Examples of metal salts include calcium borate, cobalt borate, zinc borate (zinc tetraborate, zinc metaborate, etc.), aluminum potassium borate, ammonium borate (ammonium metaborate, ammonium tetraborate, ammonium pentaborate, ammonium octaborate, etc.), cadmium borate (cadmium orthoborate, cadmium tetraborate, etc.), potassium borate (potassium metaborate, potassium tetraborate, potassium pentaborate, potassium hexaborate, potassium octaborate, etc.), silver borate (silver metaborate, silver tetraborate, etc.), copper borate (copper-diced borate, copper metaborate, copper tetraborate, etc.), sodium borate (sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate, etc.) This includes, but is not limited to, sodium octaborate, lead borate (lead metaborate, lead hexaborate, etc.), nickel borate (nickel orthoborate, nickel diborate, nickel tetraborate, nickel octaborate, etc.), barium borate (barium orthoborate, barium metaborate, barium diborate, barium tetraborate, etc.), bismuth borate, magnesium borate (magnesium orthoborate, magnesium diborate, magnesium metaborate, trimagnesium tetraborate, pentamagnesium tetraborate, etc.), manganese borate (manganese borate I, manganese metaborate, manganese tetraborate, etc.), lithium borate (lithium metaborate, lithium tetraborate, lithium pentaborate, etc.), their salts, or combinations thereof. For example, it may include borate minerals such as borax, kernite, inyoite, kotoite, suanite, and szaibelyite. Of these, it is preferable to use borax, boric acid, and sodium borate (such as sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate, and sodium octaborate).

[0035] In another embodiment, the present invention provides a mixture having a fluorine-containing EVOH resin composition, which comprises the fluorine-containing EVOH resin composition and a first ethylene vinyl alcohol copolymer, wherein, calculated from 20 g of the mixture, the total fluoride ion content contained therein is 100 ppm to 11000 ppm, and the above total fluoride ion content ranges from 100 to 11000 ppm, 100 to 10000 ppm, 100 to 8500 ppm, 200 to 8500 ppm, 200 to 7500 ppm, and 200 to 6 The ranges of 500 ppm, 500-5000 ppm, 500-4000 ppm, 500-3000 ppm, 800-3000 ppm, 800-2000 ppm, 800-1500 ppm, 800, 800-1250 ppm, 800-1000 ppm, 1100-2000 ppm, 1100-1750 ppm, 1100-1500 ppm, 1100-1250 ppm, 1400-2000 ppm, 1400-1750 ppm, 1400-1500 ppm, or 1700-2000 ppm are acceptable. The fluoride ion content on the surface of the mixture is 2-55 ppm, 2-50 ppm, 2-45 ppm, 2-40 ppm, 2-35 ppm, 2-30 ppm, 2-25 ppm, 2-20 ppm, 2-15 ppm, 2-10 ppm, 5-55 ppm, 5-50 ppm, 5-45 ppm, 5-40 ppm, 5-35 ppm, 5-30 ppm, 5-25 ppm, and 5-20 ppm. The ranges of 5-15 ppm, 5-10 ppm, 15-55 ppm, 15-50 ppm, 15-45 ppm, 15-40 ppm, 15-35 ppm, 15-30 ppm, 15-25 ppm, 15-20 ppm, 30-55 ppm, 30-50 ppm, 30-45 ppm, 30-40 ppm, 30-35 ppm, 45-55 ppm, or 45-50 ppm are acceptable.The ratio of fluoride ion content to total fluoride ion content on the surface of the mixture is preferably 0.0019 to 0.04, for example, within the range of 0.0019 to 0.04, 0.0019 to 0.035, 0.0019 to 0.03, 0.0019 to 0.025, 0.0019 to 0.02, 0.0019 to 0.015, 0.0019 to 0.01, 0.0019 to 0.005, 0.0019 to 0.004, 0.0019 to 0.003, and 0.0025 to 0.04. , 0.0025~0.035, 0.0025~0.03, 0.0025~0.025, 0.0025~0.02, 0.0025~0.015, 0.0025~0.01, 0.0025~0.005, 0.0025~0.004, 0.005~0.04, 0.005~0.035, 0.005~0.03, 0.005~0.025, 0.005~0.02, 0.005~0.015, 0.005~0.01, 0.0075~0.04, 0.0075~0 0.035, 0.0075~0.03, 0.0075~0.025, 0.0075~0.02, 0.0075~0.015, 0.0075~0.01, 0.01~0.04, 0.01~0.035, 0.01~0.03, 0.01~0.025, 0.01~0.02, 0.0125~0.04, 0.0125~0.035, 0.0125~0.03, 0.0125~0.025, 0.0125~0.02, 0.015~0.04, 0.015~0.03 5, 0.015~0.03, 0.015~0.025, 0.015~0.02, 0.0175~0.04, 0.0175~0.035, 0.0175~0.03, 0.0175~0.025, 0.02~0.04, 0.02~0.035, 0.02~0.03, 0.02~0.025, 0.0225~0.04, 0.0225~0.035, 0.0225~0.03, 0.025~0.04, 0.025~0.035 or 0.03~0.04.

[0036] The ethylene content of the fluorine-containing EVOH resin composition and the ethylene content of the first ethylene vinyl alcohol copolymer may be the same or different. According to one preferred embodiment, the present invention provides a mixture having a fluorine-containing EVOH resin composition, comprising the fluorine-containing EVOH resin composition and the first ethylene vinyl alcohol copolymer, wherein the total fluoride ion content in 20 g of the mixture is calculated to be between 100 ppm and 11,000 ppm. The ethylene content of the fluorine-containing EVOH resin composition and the ethylene content of the first ethylene vinyl alcohol copolymer may be the same. The resulting mixture of fluorine-containing EVOH resin compositions (also referred to herein as general-purpose resin) has a single ethylene content of EVOH and can be selected according to various gas barrier properties, flexibility, and permeability, but can generally be used for food packaging films, etc. According to another preferred embodiment, the present invention provides a mixture having a fluorine-containing EVOH resin composition, comprising the fluorine-containing EVOH resin composition and the first ethylene vinyl alcohol copolymer, wherein the total fluoride ion content in 20 g of the mixture is between 100 ppm and 11,000 ppm. In this mixture, the ethylene content of the fluorine-containing EVOH resin composition and the ethylene content of the first ethylene vinyl alcohol copolymer may differ. The mixture of fluorine-containing EVOH resin compositions obtained above (also referred to as thermoforming resin in this specification) is an EVOH with a low ethylene content that has good gas barrier properties due to its high hydrogen bond ratio, while an EVOH with a high ethylene content has good elasticity. By mixing two types of EVOH with different ethylene content, it is possible to achieve both gas barrier properties and elasticity simultaneously, and this mixture is often used for molded containers and packaging such as food containers or cosmetic containers. Furthermore, the mixture of fluorine-containing EVOH resin compositions may contain boron or may not contain any boron at all.

[0037] According to one embodiment of the present invention, the present invention provides a blend having a fluorine-containing EVOH resin composition, which comprises the fluorine-containing EVOH resin composition, a first ethylene vinyl alcohol copolymer, and a second ethylene vinyl alcohol copolymer. The ethylene content of the first ethylene vinyl alcohol copolymer and the ethylene content of the second ethylene vinyl alcohol copolymer are different, and the ethylene content of the fluorine-containing EVOH resin composition is the same as or different from the ethylene content of the first ethylene vinyl alcohol copolymer and the second ethylene vinyl alcohol copolymer, respectively. Based on calculations for a 20g blend, the total fluoride ion content contained therein is 200ppm to 2000ppm. The total fluoride ion content mentioned above is 200-2000 ppm, 200-1750 ppm, 200-1500 ppm, 200-1250 ppm, 200-1000 ppm, 200-750 ppm, 200-500 ppm, 500-2000 ppm, 500-1750 ppm, 500-1500 ppm, ppm, 500-1000 ppm, 500-750 ppm, 800-20 The ranges of 00 ppm, 800-1750 ppm, 800-1500 ppm, 800-1250 ppm, 800-1000 ppm, 1100-2000 ppm, 1100-1750 ppm, 1100-1500 ppm, 1100-1250 ppm, 1400-2000 ppm, 1400-1750 ppm, 1400-1500 ppm, or 1700-2000 ppm are acceptable.The ratio of fluoride ion content to total fluoride ion content on the surface of the blend is 0.0013 to 0.045, for example, within the following ranges: 0.0013 to 0.045, 0.0013 to 0.035, 0.0013 to 0.025, 0.0013 to 0.015, 0.0013 to 0.0095, 0.0013 to 0.0085, 0.0013 to 0.0075, 0.0013 to 0.0065, and 0.0013 to 0.0055. , 0.0013~0.0045, 0.0013~0.0035, 0.0013~0.0025, 0.002~0.045, 0.002~0.035, 0.002~0.025, 0.002~0.015, 0.002~0.0095, 0.002~0.0085, 0.002~0.0075, 0.002~0.0065, 0.002~0.0055, 0.002~0.0045, 0.002~0.0035, 0 0.004~0.045, 0.004~0.035, 0.004~0.025, 0.004~0.015, 0.004~0.0095, 0.004~0.0085, 0.004~0.0075, 0.004~0.0065, 0.004~0.0055, 0.006~0.045, 0.006~0.035, 0.006~0.025, 0.006~0.015, 0.006~0.0095, 0.006~0.00 The values ​​are 85, 0.006~0.0075, 0.008~0.045, 0.008~0.035, 0.008~0.025, 0.008~0.015, 0.008~0.0095, 0.01~0.045, 0.01~0.035, 0.01~0.025, 0.01~0.015, 0.015~0.045, 0.015~0.035, 0.015~0.025, 0.02~0.045, or 0.02~0.035.

[0038] According to one preferred embodiment, the present invention provides a blend having a fluorine-containing EVOH resin composition, comprising a fluorine-containing EVOH resin composition, a first ethylene vinyl alcohol copolymer, and a second ethylene vinyl alcohol copolymer, wherein the ethylene content of the first ethylene vinyl alcohol copolymer and the ethylene content of the second ethylene vinyl alcohol copolymer are different. Calculated for a 20g blend, the total fluoride ion content is 200ppm to 2000ppm, and the fluorine-containing EVOH resin composition blend may or may not contain boron. The above-described fluorine-containing EVOH resin composition blend (also referred to herein as a special resin) inherits the concept of thermoformable resin standards, with more comprehensively averaged properties of the molding material, and can subsequently be applied in embodiments such as inner liners for automobile tires or oil reservoirs. In this specification, "mixture" and "blend" both refer to a mixture formed by combining the fluorine-containing EVOH resin composition of the present invention with fluorine-free EVOH (pure EVOH). However, in order to distinguish between general-purpose resins, thermoforming resins, and special resins, in this specification, "mixture" is defined as a mixture of the fluorine-containing EVOH resin composition of the present invention with only one type of fluorine-free EVOH (pure EVOH). The ethylene content of the pure EVOH and the ethylene content of the fluorine-containing EVOH resin composition of the present invention may be the same or different, and other necessary additives may be added to the mixture, but are not limited to this specification. In this specification, "blend" is defined as a mixture formed by combining the fluorine-containing EVOH resin composition of the present invention with at least two types of fluorine-free EVOH (pure EVOH) with different ethylene content, and other necessary additives may be added, but are not limited to this specification. [Examples]

[0039] The non-limiting embodiments of the present invention provided below are primarily intended to clarify the various embodiments of the present invention and the effects achieved thereby. [Examples]

[0040] Based on the present invention, four types of fluoropolymers are prepared (Fluoropolymers A to D in Examples). Subsequently, the fluorine-containing ethylene vinyl alcohol copolymer (hereinafter referred to as "EVOH") resin composition of the present invention is prepared using Fluoropolymers A to D in Examples. Fluoropolymers A to D in Examples are prepared based on the specific methods disclosed below, but other types of fluoropolymers can also be used and added to EVOH.

[0041] Example: Fluoropolymer A An autoclave was used as a batch reactor to prepare fluoropolymer A in the example. The autoclave had an internal volume of approximately 20 L and was equipped with an electromagnetic induction stirring device. The autoclave was fully filled with nitrogen gas (N2), and then filled with reduced-pressure nitrogen gas five times.

[0042] Simultaneously with reducing the pressure inside the autoclave, 6,960 g of deoxygenated water, 3,204 g of 1,1,2-trichloro-1,2,2-trifluoroethane, and 3.5 g of methylcellulose were added to the autoclave. The viscosity of the methylcellulose was 50 cp, and it was added to the composition in the autoclave by stirring at 450 rpm as a suspension stabilizer. The composition in the autoclave was left at 52°C.

[0043] A monomer composed of 25.3 wt% vinylidene fluoride (VDF), 68.6 wt% hexafluoropropylene (HFP), and 6.1 wt% tetrafluoroethylene (TFE) was mixed into the batch as a packing gas at a rate of 10 kg / cm³. 2 The container was filled to the specified depth. Then, 45.6 g of a solution containing approximately 90 wt% 1,1,2-trichloro-1,2,2-trifluoroethane and 10 wt% diisopropyl peroxydicarbonate was added as a catalyst to initiate the polymerization reaction. Diisopropyl peroxydicarbonate was used as an initiator to start the polymerization reaction. Because the pressure decreases during the polymerization reaction, a mixed monomer containing 44.7 wt% VDF, 32.5 wt% HFP, and 22.8 wt% TFE was added to raise the pressure to 10 kg / cm². 2The temperature was raised to [temperature]. After the polymerization reaction was complete, the remaining mixed monomers were removed, and the resulting suspension was dehydrated using a centrifuge, washed with deionized water, and then vacuum-dried at 100°C to obtain 7.5 kg of Example Fluoropolymer A.

[0044] Example: Fluoropolymer B Fluoropolymer B of Example was prepared using a similar autoclave and installed according to the same method as Fluoropolymer A of Example. The autoclave was similarly filled with reduced-pressure nitrogen gas five times.

[0045] Simultaneously with reducing the pressure inside the autoclave, 7,200 g of deoxygenated water, 3,250 g of 1,1,2-trichloro-1,2,2-trifluoroethane, and 4 g of methylcellulose were added to the autoclave. The viscosity of the methylcellulose was 50 cp, and it was added to the batch in the autoclave by stirring at 500 rpm as a suspension stabilizer. The batch in the autoclave was kept at 52°C.

[0046] A monomer composed of 25 wt% VDF, 55 wt% HFP, and 20 wt% TFE was used as the packing gas, at a rate of 20 kg / cm³. 2 The container was filled to the specified depth. Then, 40 g of a solution containing approximately 85 wt% 1,1,2-trichloro-1,2,2-trifluoroethane and 15 wt% diisopropyl peroxydicarbonate was added as a catalyst to initiate the polymerization reaction. Diisopropyl peroxydicarbonate was used as an initiator to start the polymerization reaction. Because the pressure decreases during the polymerization reaction, a mixed monomer containing 40 wt% VDF, 35 wt% HFP, and 25 wt% TFE was added to increase the pressure to 20 kg / cm². 2 The temperature was raised to [temperature]. After the polymerization reaction was complete, the remaining mixed monomers were removed, and the resulting suspension was dehydrated using a centrifuge, washed with deionized water, and then vacuum-dried at 100°C to obtain 6 kg of Example Fluoropolymer B.

[0047] Example: Fluorine polymer C Fluoropolymer C was prepared using the same autoclave and induction stirring apparatus as used for the preparation of Fluoropolymer A. The autoclave was filled with nitrogen gas and 3 L of the composition was added. The composition contained deoxygenated water and 30 g of ammonium nonadecafluorodecanoate as an emulsifier. The composition in the autoclave was heated to 60°C and stirred at 380 rpm.

[0048] Subsequently, the internal pressure of the autoclave reached 20 kg / cm². 2 The autoclave was filled with a mixed gas containing approximately 70 wt% VDF and approximately 30 wt% HFP until the mixture reached a certain concentration. Next, 40 g of a solution containing approximately 80 wt% 1,1,2-trichloro-1,2,2-trifluoroethane and 20 wt% diisopropyl peroxydicarbonate was added to the autoclave using nitrogen gas. Diisopropyl peroxydicarbonate was used as an initiator to start the polymerization reaction.

[0049] During the polymerization reaction, a mixed gas of VDF (62 wt%) and HFP (38 wt%) is continuously injected to maintain the internal pressure of the autoclave at 20 kg / cm². 2 The polymerization rate decreased as the polymerization reaction progressed, so 3 hours after the start of the polymerization reaction, 30 g of a solution containing approximately 80 wt% 1,1,2-trichloro-1,2,2-trifluoroethane and 20 wt% diisopropyl peroxydicarbonate was added to the autoclave using nitrogen gas. After further polymerization of the monomer for 3 hours, the resulting suspension was dehydrated by centrifugation, washed with deionized water, and then vacuum-dried at 100°C to obtain 7.2 kg of Example Fluoropolymer C.

[0050] Example: Fluoropolymer D Fluoropolymer D of Example was prepared using an autoclave with a volume of approximately 3 L as a batch reactor. The autoclave was equipped with an electromagnetic induction stirring device. Batches of 936 g of deionized water, 0.36 g of methylcellulose, 360 g of VDF, 0.3 g of t-butyl peroxypivalate, 0.36 g of sodium pyrophosphate, 0.36 g of acidic sodium pyrophosphate, and 1.8 g of diethyl carbonate were placed in the autoclave and added. The mixture was stirred at 10°C for 30 minutes, and then heated at 45°C for 140 minutes.

[0051] The maximum pressure inside the autoclave was 6 MPa. The polymerization reaction of the monomer was completed when the pressure inside the autoclave dropped to 2.5 MPa, which occurred 15 hours after the start of heating of the monomer. After the polymerization reaction was complete, the polymer slurry was removed, dehydrated, washed with deionized water, dehydrated again, and dried at 80°C for 24 hours to obtain polyvinylidene fluoride (Example Fluorine Polymer D) with an inherent viscosity of 2.05 dl / g and a bulk density of 0.225 g / ml, with a yield of 55%. [Examples]

[0052] The following provides a non-limiting method for preparing fluorine-containing EVOH pellets formed from fluorine-containing EVOH resin compositions. Based on a method similar to that disclosed below, 16 non-limiting example EVOH resin compositions (Examples EVOH1-16) and 4 comparative example EVOH resin compositions (Comparative Examples EVOH1-4) having fluorine particles were prepared. However, the specific methods for preparing Examples EVOH1-16 and Comparative Examples EVOH1-4 generally differ from the methods disclosed below in one or more aspects.

[0053] An ethylene-vinyl acetate copolymer (hereinafter referred to as "EVAC") with an ethylene content of 29 moles was saponified to prepare an EVOH polymer with a degree of saponification of 99.5%. Next, the EVOH was dissolved in a solution containing methanol and water (in a ratio of 70:30). Subsequently, the solid content of EVOH in the solution became 41 wt%, and the solution was left at 60°C.

[0054] The methanol, water, and EVOH solution described above was granulated by underwater pelletization. Specifically, the methanol, water, and EVOH solution was sent to a supply pipe at a flow rate of 120 L / min using a pump, then to a 2.8 mm diameter suction pipe, and cut at 1500 rpm using a rotating knife. The EVOH pellets were cooled by adding water at 5°C. Next, the EVOH pellets were centrifuged to separate the EVOH particles. The separated EVOH particles were washed with water and immersed in a boric acid solution and stirred. The concentration of the boric acid solution was adjusted according to the boron content in the final fluorine-containing EVOH resin composition, and then dried to obtain EVOH pellets (in examples where boron was not added, the drying process was carried out directly).

[0055] EVOH pellets and fluoropolymers such as those in Example 1 were mixed in a fixed ratio and then fed into a twin-screw extruder. As shown in Table 1, the 13 sections (sections 1 to 13) of the twin-screw extruder had different temperatures. After mixing, strand cutting was performed at 25°C to prepare EVOH containing particles with the element fluorine (also referred to herein as "fluorine particles"). In Table 1, "EV27" refers to EVOH with an ethylene content of 27 moles, "EV29" refers to EVOH with an ethylene content of 29 moles, "EV32" refers to EVOH with an ethylene content of 32 moles, "EV38" refers to EVOH with an ethylene content of 38 moles, and "EV44" refers to EVOH with an ethylene content of 44 moles.

[0056] [Table 1] [Examples]

[0057] Films were formed using Example EVOH pellets 1-16 based on the method described below. Example EVOH pellets 1-16 and Comparative Example EVOH pellets 1-4 were fed into a single-layer T-die-cast film extruder (optical control system MEV4) to prepare the films. The thickness of each film formed using Example EVOH pellets 1-16 and Comparative Example EVOH pellets 1-4 was 20 μm. The extruder temperature was set to 220°C, and the mold (i.e., T-die) temperature was set to 230°C. The screw rotation speed was 7 rpm (rotations / minutes). [Examples]

[0058] The EVOH pellets of Examples 1-16 and Comparative Examples EVOH pellets 1-4 were evaluated, and the properties of these EVOH pellets and the films formed therefrom were determined. As described above, the EVOH pellets of Examples 1-16 were prepared based on a method similar to that described in Example 2. However, the preparation methods for EVOH pellets 1-16 differ in that the EVOH pellets prepared have different ethylene content, different fluoropolymers, different total fluoride ion content, fluoride ion content on the surface, and the ratio of fluoride ion content on the surface to total fluoride ion content. Comparative Examples EVOH pellets 1-4 were also prepared based on a method similar to that described in Example 2.

[0059] Films were formed according to the same method as described in Example 3 for Examples EVOH1-16 and Comparative Examples EVOH1-4, respectively. The films were evaluated to determine their appearance, the state of deposition on the die, and their transmittance.

[0060] Table 2 below provides an overview of some attributes of Example EVOH Pellet 1-16 and Comparative Example EVOH Pellet 1-4, namely the ethylene content of EVAC, the specific fluoropolymers contained in the fluorine-containing particles, and the fluoropolymer content. Table 3 below provides an overview of the total fluoride ion content of EVOH pellets in Example EVOH Pellet 1-16 and Comparative Example EVOH Pellet 1-4, the fluoride ion content on the surface, the ratio of fluoride ion content on the surface to the total fluoride ion content, and the properties of the films formed from Example EVOH Pellet 1-16 and Comparative Example EVOH Pellet 1-4.

[0061] [Table 2]

[0062] [Table 3]

[0063] To evaluate the total fluoride ion content of Example EVOH pellets 1-16 and Comparative Example EVOH pellets 1-4, analysis was performed using an ion chromatograph (Metrohm 930 Compact IC Flex / Ses / PP / Deg), employing the NIEA W415.54B water anion detection method. As a pretreatment, 20g of the sample was burned in an oxygen cylinder, then extracted with water, and chemical analysis was performed. Samples were randomly sampled, and after 10 samples were analyzed, the average value of the 10 tests was calculated.

[0064] To evaluate the fluorine ion content on the surfaces of the EVOH pellets 1 to 16 of the Examples and the EVOH pellets 1 to 4 of the Comparative Examples, analysis was performed using an ion chromatograph (Metrohm 930 Compact IC Flex / Ses / PP / Deg), and the NIEA W415.54B Anion Detection Method in Water was used as the test method. In the pretreatment, first, 0.5 g of sample pellets were placed in 5 c.c. of methanol, transferred to an environment at 60°C and stirred for 4 hours, followed by filtration to remove the pellets. 0.5 c.c. of the liquid was taken, the liquid was combusted using an oxygen cylinder, extracted with water, and then subjected to chemical analysis. Samples were randomly sampled, sampled and analyzed 10 times, and the average value of the 10 tests was calculated.

[0065] Regarding the boron content, each EVOH resin composition (0.1 g each) was decomposed with concentrated nitric acid in a microwave to prepare sample solutions for the Examples and Comparative Examples. Next, the sample solution was diluted with pure water to adjust the concentration to 0.75 mg / ml. Using a Thermo iCAP 7000 analyzer and an inductively coupled plasma optical emission spectrometer (ICP-OES), the boron content in the prepared solution was measured. The measured boron amount corresponds to the boron amount derived from the boron compound used.

[0066] The melting point temperatures of the Examples and Comparative Examples were measured according to the method of ISO 11357-3 (2011) using a TA-Q200 differential scanning calorimeter (abbreviated as DSC, manufactured by TA Instruments), and the first melting point temperature and the second melting point temperature obtained in the first thermal scan of the differential scanning calorimeter were used.

[0067] Regarding the appearance of the films formed from EVOH 1 to 16 of the Examples and EVOH 1 to 4 of the Comparative Examples, in a 1 m 2 range, when the number of fish eyes with a size larger than 200 μm was less than 5, it was represented by "O", and in a 1 m 2If there are 5 to 10 fisheyes larger than 200 μm within the sample, it is represented as "Δ", and 1 m 2 Within the image, if the number of fisheyes larger than 200 μm was greater than 10, it was represented by "X". The FSA-100, designed with a charged-coupled device (CCD) sensor and FSA-100 V.8 software, was used for testing the number of fisheyes.

[0068] Evaluation of processing performance The extruder system ME-25 / 5800V4 and film thickness measuring instrument FTM-200, purchased from OCS Corporation, were visually inspected. "O" indicates no adhesion on the die or screw, while "X" indicates adhesion.

[0069] Transmittance could be evaluated using the ASTM D1003 method. A 25 μm thick film was taken for measurement and analyzed using an OCS-EVOHM Gamma 12 instrument. Based on the transmittance measurement method described above, if the transmittance of the EVOH film was 90% or higher, it was represented by "O", if it was less than 90% but 85% or higher, it was represented by "Δ", and if it was 85% or lower, it was represented by "X".

[0070] The films of Examples EVOH1-16 showed no adhesion on the die, and 1m 2Within the film, there were five or fewer fisheyes larger than 200 μm. The films formed by Examples EVOH1 to 16 all showed excellent appearance and processing performance, while the films formed by Comparative Examples EVOH1 to 4 showed slightly inferior appearance and processing performance. Surprisingly, it was found that when the total fluoride ion content of the fluorine-containing EVOH resin composition is within the range of 45 to 41,000 ppm, the number of fisheyes generated during EVOH film formation decreases, improving its mechanical properties and film appearance. As shown in Table 2, Comparative Examples 1 and 2 had a total fluoride ion content exceeding the desired range described herein, indicating an excessively large number of fisheyes. Furthermore, in this invention, if the total fluoride ion content of the fluorine-containing EVOH resin composition containing fluorine-containing particles is within the desired range (between 45 and 41,000 ppm), the fluoropolymer within it can reduce adhesion to the die and screw during the processing process, improving processability. For example, the total fluoride ion content of Comparative Examples EVOH3 and 4 is lower than the desired range described herein, but the results show that they adhere to the die and screw.

[0071] For fluorine-containing EVOH resin compositions that conform to the above-mentioned total fluoride ion content, the effect of improving transmittance can be obtained by further examining the ratio of fluoride ion content to total fluoride ion content on the surface. The fluorine content on the surface of the present invention is the result of testing that comprehensively considers the effects of the type of fluorine-containing polymer, the amount of fluorine-containing polymer added, the ethylene content and boron content, etc. By controlling the ratio of fluoride ion content to total fluoride ion content on the surface within a specific range, the transmittance effect can be improved. [Examples]

[0072] The preparation of the mixture having the fluorine-containing EVOH resin composition was based on a method similar to that described in Example 2, and Examples EVOH 17-38 and Comparative Examples EVOH 5-16 were prepared, but the main differences are as follows: After preparing the fluorine-containing EVOH resin composition first, in the drying step, the first ethylene vinyl alcohol copolymer (1st EVOH was mixed and added, and a conical screw mixer (manufactured by Kyoki Machinery Industry Co., Ltd., model number: CM-2) was used to mix thoroughly until homogeneous, with an input amount of 500 kg and an operating time of 20 minutes. The ethylene content of the ethylene vinyl alcohol copolymer in the fluorine-containing EVOH resin composition and the ethylene content of the first ethylene vinyl alcohol copolymer were the same. The method for preparing the first ethylene vinyl alcohol copolymer was the same as the EVOH manufacturing process before the fluoropolymer was kneaded into the fluorine-containing EVOH resin composition. The ethylene content was set according to the values ​​in Table 4, and the boron content was adjusted according to the ethylene content of the first ethylene vinyl alcohol copolymer and calculated relative to the first ethylene vinyl alcohol copolymer. When the ethylene content was 29 mole%, the boron content was 120 ppm; when the ethylene content was 32 mole%, the boron content was 100 ppm; when the ethylene content was 38 mole%, the boron content was 90 ppm; and when the ethylene content was 44 mole%, the boron content was 70 ppm. However, in the case of Example EVOH37, since neither the fluorine-containing EVOH resin composition nor the first ethylene vinyl alcohol copolymer contains boron, the step of immersion in boric acid solution is not performed.

[0073] First, a fluorine-containing EVOH resin composition was prepared. An ethylene-vinyl acetate copolymer (hereinafter referred to as "EVAC") with an ethylene content of 29 moles was saponified to prepare an EVOH polymer with a degree of saponification of 99.5%. Next, the EVOH was dissolved in a solution containing methanol and water (in a ratio of 70:30). Subsequently, the solid content of EVOH in the solution became 41 wt%, and the solution was left at 60°C.

[0074] Granulation of the methanol, water, and EVOH solution described above was performed by underwater pellet production. Specifically, the methanol, water, and EVOH solution described above was sent to a supply pipe at a flow rate of 120 L / min using a pump, then sent to a suction pipe with a diameter of 2.8 mm, and cut with a rotating knife at 1500 rpm. The EVOH pellets were cooled by adding water at 5°C. Next, the EVOH pellets were centrifuged to separate the EVOH particles. The EVOH particles separated after washing with water were immersed in a boric acid solution and stirred. The concentration of the boric acid solution was adjusted according to the various ethylene content of the EVOH described above, and also according to the boron content in the final fluorine-containing EVOH resin composition. The solution was then dried to obtain EVOH pellets (in examples where boron was not added, the drying process was carried out directly).

[0075] EVOH pellets and fluoropolymers such as those in Example 1 were mixed in a fixed ratio and then sent to a twin-screw (or single-screw, melt-stirred) extruder. As shown in Table 1, the 13 zones (zones 1 to 13) of the twin-screw extruder had different temperatures. After mixing, strand cutting or underwater granulation was performed at 25°C to prepare EVOH containing fluorine particles.

[0076] Next, a drying process is carried out, and after the drying process, the first ethylene vinyl alcohol copolymer (1 st EVOH was added in a mixture. This prepared a mixture having a fluorine-containing EVOH resin composition.

[0077] Finally, films were prepared according to the method described in Example 3, specifically for Examples EVOH17-38 and Comparative Examples EVOH5-16.

[0078] Table 4 below summarizes several attributes of mixtures of fluorine-containing EVOH resin compositions in which the ethylene content of the first ethylene vinyl alcohol copolymer is the same (i.e., Examples EVOH 17-38 and Comparative Examples EVOH 5-16), namely, ethylene content, specific fluoropolymers and fluoropolymer content contained in the fluorine-containing EVOH pellets, total fluoride ion content of the mixture having the fluorine-containing EVOH resin composition, fluoride ion content on the surface, and the ratio of fluoride ion content on the surface to total fluoride ion content. It also summarizes the evaluation of the films of Examples EVOH 17-38 and Comparative Examples EVOH 5-16 prepared according to the method described in Example 3, and the determination of several properties such as the appearance analysis of the film (number of fish eyes), adhesion to the die or screw, and transmittance, which were measured according to the methods described in Examples 2-4.

[0079] [Table 4] JPEG0007953992000005.jpg245163JPEG0007953992000006.jpg247163JPEG00079539920 00007.jpg244162JPEG0007953992000008.jpg240161JPEG0007953992000009.jpg186161

[0080] Surprisingly, when the total fluoride ion content of the mixture of the fluorine-containing EVOH resin composition of the present invention is 100 ppm to 11000 ppm, the film does not adhere to the die and does not adhere to 1 m 2 Within the sample, it was found that there were 5 or fewer fisheyes larger than 200 μm. As shown above, no adhesion occurred on the die in any of the examples EVOH17-38, and 1 m 2 Within the sample, there were five or fewer fisheyes larger than 200 μm.

[0081] Furthermore, when the ratio of fluoride ion content to total fluoride ion content on the surface of the mixture of the fluorine-containing EVOH resin composition of the present invention was 0.0019 to 0.04, the transmittance of the film was 90% or higher in all cases. As shown above, when the ratio of fluoride ion content to total fluoride ion content on the surface of the mixture of the fluorine-containing EVOH resin composition was 0.0019 to 0.04, the transmittance was 90% or higher in all cases.

[0082] In comparative examples EVOH5-16, where the total fluoride ion content exceeds the desired range, adhesion occurs on the die, and 1m 2 There were five or more fisheyes larger than 200 μm within the film. In a mixture of fluorine-containing EVOH resin compositions in which the ratio of fluoride ion content to total fluoride ion content on the surface exceeded the desired range, the film transmittance was 90% or less. As described above, under conditions where fluorine-containing particles are present and the total fluoride ion content is within a specific range, the flow behavior of EVOH in the screw extruder is smoother, and the protection of the fluoropolymer on the inner wall of the screw extruder reduces deposition on the die and improves the appearance of the film.

[0083] Regarding the total fluoride ion content present in the mixture of fluorine-containing EVOH resin compositions, if it exceeds the desired range, the mixture of EVOH resin compositions may have an undesirable film appearance and poor processability.

[0084] The mixture of fluorine-containing EVOH resin compositions obtained in this embodiment (i.e., general-purpose resin) has a single ethylene content of EVOH and can be selected according to various gas barrier properties, flexibility, and permeability, and can be applied in forms such as food packaging films. [Examples]

[0085] The mixture having the fluorine-containing EVOH resin composition of this example is based on a method similar to that described in Example 5, and Examples EVOH 39-43 and Comparative Example EVOH 17 were prepared, but the main differences are as follows: After preparing the fluorine-containing EVOH resin composition first, in the drying step, the first ethylene vinyl alcohol copolymer (1 st EVOH was mixed and added, and thoroughly mixed until homogeneous using a conical screw mixer (Kyoki Machinery Industry Co., Ltd., model number: CM-2) with an input amount of 500 kg for a total operating time of 20 minutes. The ethylene content of the ethylene vinyl alcohol copolymer in the fluorine-containing EVOH resin composition and the ethylene content of the first ethylene vinyl alcohol copolymer were different. The method for preparing the first ethylene vinyl alcohol copolymer was the same as the EVOH manufacturing process before the fluorine polymer was kneaded into the fluorine-containing EVOH resin composition. The ethylene content was set according to the values ​​in Table 5, and the boron content was adjusted according to the ethylene content as described above. However, in the case of Example EVOH42, since neither the fluorine-containing EVOH resin composition nor the first ethylene vinyl alcohol copolymer contains boron, the step of immersion in boric acid solution was not performed.

[0086] Films were prepared according to the method described in Example 3, specifically in Examples EVOH39-43 and Comparative Example EVOH17.

[0087] Table 5 below summarizes several attributes of mixtures of fluorine-containing EVOH resin compositions where the ethylene content of the fluorine-containing EVOH resin composition differs from that of the first ethylene vinyl alcohol copolymer (i.e., Examples EVOH39-43 and Comparative Example EVOH17), namely, ethylene content, specific fluoropolymers and fluoropolymer content contained in the fluorine-containing EVOH pellets, total fluoride ion content of the mixture having the fluorine-containing EVOH resin composition, fluoride ion content on the surface, and the ratio of fluoride ion content on the surface to total fluoride ion content. It also summarizes the evaluation of the films of Examples EVOH39-43 and Comparative Example EVOH17 prepared according to the method described in Example 3, and the determination of several properties such as the appearance analysis of the film (number of fish eyes), adhesion to the die or screw, and transmittance, which were measured according to the methods described in Examples 2-4.

[0088] [Table 5] JPEG0007953992000011.jpg238161JPEG0007953992000012.jpg54161

[0089] Surprisingly, when the total fluoride ion content of the mixture of the fluorine-containing EVOH resin composition of the present invention is 100 ppm to 11000 ppm, the film does not adhere to the die and does not adhere to 1 m 2 The inventors discovered that within the material, there were 5 or fewer fisheyes larger than 200 μm. As shown above, no adhesion occurred on the die in any of the examples EVOH39 to 43, and 1 m 2 Within the sample, there were five or fewer fisheyes larger than 200 μm.

[0090] Furthermore, when the ratio of fluoride ion content to total fluoride ion content on the surface of the mixture of the fluorine-containing EVOH resin composition of the present invention was 0.0019 to 0.04, the transmittance of the film was 90% or higher in all cases. As shown above, the transmittance of the films of Examples EVOH 39 to 43 was 90% or higher in all cases.

[0091] In comparative example EVOH17, where the total fluoride ion content and the ratio of fluoride ion content on the surface to the total fluoride ion content exceeded the desired range, the transmittance was only between 85% and 90%.

[0092] The mixture of fluorine-containing EVOH resin compositions (i.e., thermoformable resin) obtained in this example is EVOH with a low ethylene content, which has good gas barrier properties due to its high hydrogen bond ratio, while EVOH with a high ethylene content has good elasticity. Therefore, by mixing two types of EVOH with different ethylene content, it is possible to achieve both gas barrier properties and elasticity simultaneously. For this reason, it can be applied in subsequent applications to molded containers and packaging such as food containers or cosmetic containers. [Examples]

[0093] The blends containing the fluorine-containing EVOH resin composition were prepared using a method similar to that described in Example 5, and Examples EVOH 44-49 and Comparative Examples EVOH 18-26 were prepared, with the main differences being as follows: After preparing the fluorine-containing EVOH resin composition, the first ethylene vinyl alcohol copolymer and the second ethylene vinyl alcohol copolymer (1 st EVOH+ 2 nd EVOH was mixed and added, and thoroughly mixed until homogeneous using a conical screw mixer (Kyoki Machinery Industry Co., Ltd., model number: CM-2) with an input amount of 500 kg for a total operating time of 20 minutes. The ethylene content of the first ethylene vinyl alcohol copolymer and the second ethylene vinyl alcohol copolymer were different. The preparation method for the first ethylene vinyl alcohol copolymer was the same as the EVOH manufacturing process before the fluoropolymer was kneaded into the fluorine-containing EVOH resin composition, with the ethylene content set according to the values ​​in Table 6, and the boron content adjusted according to the ethylene content as described above. The preparation method for the second ethylene vinyl alcohol copolymer was the same as the EVOH manufacturing process before the fluoropolymer was kneaded into the fluorine-containing EVOH resin composition, with the ethylene content set according to the values ​​in Table 6, and the boron content adjusted according to the ethylene content as described above.

[0094] Films were prepared according to the method described in Example 3, specifically in Examples EVOH44-49 and Comparative Examples EVOH18-26.

[0095] Table 6 below summarizes several attributes of the fluorine-containing EVOH resin composition blends (i.e., Examples EVOH 44-49 and Comparative Examples EVOH 18-26), namely, ethylene content, specific fluoropolymer and fluoropolymer content contained in the fluorine-containing EVOH pellets, total fluoride ion content of the blends containing the fluorine-containing EVOH resin composition, fluoride ion content on the surface, and the ratio of fluoride ion content on the surface to total fluoride ion content. It also summarizes the evaluation of the films of Examples EVOH 44-49 and Comparative Examples EVOH 18-26, prepared according to the method described in Example 3, and the determination of several properties such as the appearance analysis of the film (number of fish eyes), adhesion to the die or screw, and transmittance, which were measured according to the methods described in Examples 2-4.

[0096] [Table 6] JPEG0007953992000014.jpg245165JPEG0007953992000015.jpg244166JPEG0007953992000016.jpg244166JPEG0007953992000017.jpg153166

[0097] The inventors have found that when the total fluoride ion content of the blend of the fluorine-containing EVOH resin composition of the present invention is 200 ppm to 2000 ppm, the film does not adhere to the die and does not exceed 1 m 2 Within the sample, it was found that there were 5 or fewer fisheyes larger than 200 μm. As shown above, no adhesion occurred on the die in any of the examples EVOH44-49, and 1 m 2 Within the sample, there were five or fewer fisheyes larger than 200 μm.

[0098] Furthermore, when the ratio of fluoride ion content to total fluoride ion content on the surface of the blend of the fluorine-containing EVOH resin composition of the present invention was 0.0013 to 0.045, the transmittance of the film was 90% or higher in all cases. As shown above, the transmittance of the films of Examples EVOH 44 to 49 was 90% or higher in all cases.

[0099] In comparative examples EVOH18-26, where the total fluoride ion content exceeds the desired range, adhesion occurs on the die, and 1m 2 There were five or more fisheyes larger than 200 μm within the film. In comparative examples EVOH18-26, where the ratio of fluoride ion content on the surface to total fluoride ion content exceeded the desired range, the transmittance of the film was 90% or less.

[0100] The fluorine-containing EVOH resin composition blend (i.e., special resin) obtained in this embodiment inherits the concept of thermoforming resin standards, and the properties of the molding material are more comprehensively averaged. It can subsequently be applied in forms such as inner liners for automobile tires or oil reservoir pipes.

[0101] In summary, when an EVOH resin composition or mixture or blend containing the same has fluorine-containing particles and a total fluoride ion content within a specific range, the flow behavior of the EVOH in a screw extruder is smoother, and precipitation on the die is reduced and the film appearance is improved due to the fluorine polymer protection provided to the inner wall of the screw extruder. If the total fluoride ion content exceeds the desired range, the EVOH resin composition may have an undesirable film appearance and poor processability.

[0102] All scopes provided herein include combinations of specific scopes within an allocated scope and secondary scopes between those scopes. Furthermore, unless otherwise stated, all scopes provided herein include the scope endpoints. Therefore, scopes 1-5 specifically include 1, 2, 3, 4, and 5, as well as secondary scopes such as 2-5, 3-5, 2-3, 2-4, and 1-4.

[0103] All publications and patent applications referenced herein are incorporated herein by reference, and for all purposes, each publication or patent application is explicitly and individually indicated as being incorporated herein by reference. In the event of any inconsistency between this specification and any publication or patent application incorporated herein by reference, this specification shall prevail.

[0104] As used herein, the terms “includes,” “possesses,” and “inclusive” have an open, non-restrictive meaning. The terms “one” and “the said” should be understood to include plural and singular. The term “one or more” means “at least one” and can therefore include a single characteristic or a mixture / combined characteristic.

[0105] Except in the examples of operations or where otherwise indicated, all figures indicating the amounts of components and / or reaction conditions may in all cases be modified with the term “approximately,” meaning that the actual amount is within ±5% of the indicated figure. The terms “essentially not present” or “substantially not present” as used herein mean that a particular characteristic is present in less than approximately 2%. Any element or characteristic explicitly described herein may be negatively excluded from the claims. [Explanation of symbols]

[0106] 100 EVOH pellets 110 Fluorine-containing fine particles 120 coating layers

Claims

1. A fluorine-containing ethylene vinyl alcohol copolymer resin composition, The material comprises an ethylene vinyl alcohol copolymer and at least one fluorine-containing particle. The fluorine-containing particles include a fluorinated polymer. Of these, the ratio of fluoride ion content to total fluoride ion content on the surface of the fluorine-containing ethylene vinyl alcohol copolymer resin composition is 0.0015 to 0.

03. The total fluoride ion content was measured by pretreatment according to the NIEA W415.54B method for detecting anions in water, which involved burning 20 g of the fluorine-containing ethylene vinyl alcohol copolymer resin composition in an oxygen cylinder, extracting it with water, and then analyzing it by ion chromatography (Metrohm 930 Compact IC Flex / Ses / PP / Deg). The fluoride ion content on the surface was measured according to the NIEA W415.54B method for detecting anions in water. This involved placing 0.5 g of the fluorine-containing ethylene vinyl alcohol copolymer resin composition in 5 cc of methanol, stirring at 60°C for 4 hours, filtering to obtain a liquid from which the fluorine-containing ethylene vinyl alcohol copolymer resin composition had been removed, burning 0.5 cc of this liquid in an oxygen cylinder, extracting it with water, and then analyzing it by ion chromatography (Metrohm 930 Compact IC Flex / Ses / PP / Deg). A fluorine-containing ethylene vinyl alcohol copolymer resin composition further comprising at least two melting points, wherein the first melting point is between 100°C and 140°C, the second melting point is between 150°C and 195°C, and the boron content is further between 50 and 250 ppm.

2. A mixture having a fluorine-containing ethylene vinyl alcohol copolymer resin composition, The fluorine-containing ethylene vinyl alcohol copolymer resin composition according to claim 1, A first ethylene vinyl alcohol copolymer is included, The mixture is a mixture having a ratio of fluoride ion content on the surface of the mixture to a total fluoride ion content of 0.0019 to 0.

04.

3. The mixture according to claim 2, wherein the fluoride ion content on the surface of the mixture is between 2 and 55 ppm.

4. The mixture according to claim 2, wherein the ethylene content of the fluorine-containing ethylene vinyl alcohol copolymer resin composition is the same as or different from the ethylene content of the first ethylene vinyl alcohol copolymer.

5. A blend having a fluorine-containing ethylene vinyl alcohol copolymer resin composition, The fluorine-containing ethylene vinyl alcohol copolymer resin composition according to claim 1, First ethylene vinyl alcohol copolymer and It comprises a second ethylene vinyl alcohol copolymer, The blend has a ratio of fluoride ion content to total fluoride ion content on its surface of 0.0013 to 0.045.

Citation Information

Patent Citations

  • Saponified ethylene-vinyl acetate copolymer-based resin composition

    JP1990099546A

  • Resin composition of improved melt moldability

    JP1990208340A

  • Resin composition of improved melt moldability

    JP1990208341A

  • Method of extruding ethylene-vinyl alcohol copolymer (EVOH)

    US5460760A

  • Saponified ethylene-vinyl ester copolymer resin composition, resin tube or resin liner for composite container for high pressure gas, and high pressure gas hose or composite container

    WO2016104726A1