Resin composition and molded article
A resin composition combining polycarbonate resin, an alkali metal salt, and a fibril-forming fluoropolymer enhances flame retardancy by promoting controlled carbonization, addressing the need for shortened afterflame times in polycarbonate resin compositions.
Patent Information
- Application Number
- JP2022050543
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-25
- Publication Date
- 2026-11-19
- Estimated Expiration
- 2042-03-25
AI Technical Summary
There is a need for polycarbonate resin compositions with further improved flame retardancy, particularly in terms of shortened afterflame time.
A resin composition is formulated by blending polycarbonate resin with an alkali metal salt and a fluoropolymer having fibril-forming ability, where the polycarbonate resin includes specific luminescence characteristics and molecular properties to enhance flame retardancy.
The composition achieves a further shortened afterflame time in molded articles, with improved flame retardancy through controlled oxidative degradation and carbonization processes.
Smart Images

Figure 0007954002000001 
Figure 0007954002000002 
Figure 0007954002000003
Abstract
Description
[Technical Field]
[0001] This invention relates to resin compositions and molded articles, and more particularly to resin compositions containing polycarbonate resin. [Background technology]
[0002] Polycarbonate resin is a general-purpose engineering plastic that excels in transparency, mechanical strength, electrical properties, heat resistance, and dimensional stability, and is therefore used in a wide range of fields, including electrical and electronic equipment components, office automation equipment, machine parts, vehicle parts, building materials, various containers, and leisure goods and general merchandise. Resin compositions containing polycarbonate resin (hereinafter sometimes referred to as "polycarbonate resin compositions") are often required to be flame-retardant, and various polycarbonate resin compositions with excellent flame retardancy have been investigated (Patent Document 1, Patent Document 2, etc.). [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2021-187863 [Patent Document 2] Japanese Patent Publication No. 2021-155499 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] As mentioned above, various polycarbonate resin compositions with excellent flame retardancy are known, but with the increasing demand for polycarbonate resin compositions, there is a need for even more novel polycarbonate resin compositions with superior flame retardancy. In particular, there is a demand for polycarbonate resin compositions with shortened afterflame time. The present invention aims to solve the above problems and to provide a resin composition containing a polycarbonate resin, wherein the afterflame time is further shortened, and a molded article formed from the resin composition. [Means for solving the problem]
[0005] Based on the above problems, the inventors conducted research and found that the above problems can be solved by blending a predetermined polycarbonate resin in a flame-retardant polycarbonate resin composition containing a polycarbonate resin, an alkali metal salt, and a fluoropolymer having fibril-forming ability. Specifically, the above problem was solved by the following means. <1> (A) 100 parts by mass of polycarbonate resin, (B) 0.005 to 1 part by mass of alkali metal salt, and (C) 0.01 to 3 parts by mass of fibril-forming fluoropolymer, wherein (A) polycarbonate resin comprises polycarbonate resin (A-1) and polycarbonate resin (A-2), the proportion of polycarbonate resin (A-2) in 100 parts by mass of polycarbonate resin (A) is 10 to 99 parts by mass, and the cumulative luminescence amount of polycarbonate resin (A-1) when measured by chemiluminescence is 1.0 × 10⁻¹⁴ 6 The cps is less than the ratio of the maximum luminescence at low temperature to the maximum luminescence at high temperature when the polycarbonate resin (A-2) is measured by chemiluminescence, where (maximum luminescence at low temperature) / (maximum luminescence at high temperature) is between 0.14 and 2.30, and the integrated luminescence measured by chemiluminescence is 1.0 × 10⁻¹⁰. 6 ~7.5×10 6 A resin composition that is a CPS. <2> The ratio of the maximum luminescence at low temperature to the maximum luminescence at high temperature when the polycarbonate resin (A-1) is measured by chemiluminescence is less than 0.14. <1> The resin composition described above. <3> The 5% mass loss temperature of the polycarbonate resin (A-2) is 480°C or higher and less than 512°C. <1> or <2> The resin composition described above. <4> The aforementioned polycarbonate resin (A-2) is derived from a molded product formed from polycarbonate resin. <1> ~ <3> A resin composition as described in any one of the following. A molded article formed from the resin composition according to any one of claims <5> to <1>.
Effects of the Invention
[0006] According to the present invention, it has become possible to provide a resin composition containing a polycarbonate resin with a further shortened afterflame time, and a molded article formed from the resin composition.
Modes for Carrying Out the Invention
[0007] Hereinafter, modes for carrying out the present invention (hereinafter simply referred to as "the present embodiment") will be described in detail. The following present embodiment is an exemplification for illustrating the present invention, and the present invention is not limited only to the present embodiment. In the present specification, the symbol "~" is used to mean that the numerical values stated before and after the symbol are included as the lower limit and upper limit values. In the present specification, various physical property values and characteristic values are those at 23°C, unless otherwise specified. When the measurement methods and the like described in the standards indicated in the present specification differ depending on the year, they shall be based on the standards as of January 1, 2022, unless otherwise specified.
[0008] The resin composition of the present embodiment comprises, relative to 100 parts by mass of (A) a polycarbonate resin, 0.005 to 1 part by mass of (B) an alkali metal salt, and 0.01 to 3 parts by mass of (C) a fluoropolymer having fibril-forming ability, wherein the (A) polycarbonate resin includes a polycarbonate resin (A-1) and a polycarbonate resin (A-2), the proportion of the polycarbonate resin (A-2) in 100 parts by mass of the (A) polycarbonate resin is 10 to 99 parts by mass, and the integrated luminescence amount of the polycarbonate resin (A-1) measured by temperature elevation using the chemiluminescence method is 1.0×10 6less than cps, and the ratio of the maximum luminescence amount on the low temperature side to the maximum luminescence amount on the high temperature side, (maximum luminescence amount on the low temperature side) / (maximum luminescence amount on the high temperature side), when the polycarbonate resin (A-2) is measured by raising the temperature with a chemiluminescence method, is 0.14 or more and 2.30 or less, and the integrated luminescence amount when measured by raising the temperature with a chemiluminescence method is 1.0×10 6 ~7.5×10 6 cps. Thus, in a flame-retardant polycarbonate resin composition comprising a polycarbonate resin, an alkali metal salt, and a fluoropolymer having fibril-forming ability, the flame retardancy can be further improved by blending the polycarbonate resin (A-2) in addition to the polycarbonate resin (A-1). In particular, the afterflame time of the obtained molded article can be further shortened. The reason for this is presumed to be as follows. That is, when an alkali metal salt is used as a flame retardant, intermolecular transesterification and isomerization rearrangement reactions of the polycarbonate resin occur during combustion of the molded article, and the polycarbonate resin is branched to promote carbonization, which is considered to contribute to extinguishing the fire. In the present embodiment, by using the polycarbonate resin (A-2), which is a polycarbonate resin in which the progress of oxidative degradation and decomposition has proceeded to some extent, in combination, moderate branching of the polycarbonate resin proceeds, carbonization is promoted, and it is presumed that the afterflame time could be shortened. On the other hand, if the progress of oxidative degradation and decomposition is too large, it is presumed that the decomposition of the polycarbonate resin is excessively promoted by the alkali metal salt, resulting in a longer afterflame time. Hereinafter, the details of the present invention will be described.
[0009] <(A) Polycarbonate Resin> The resin composition of the present embodiment contains (A) a polycarbonate resin. In the present embodiment, (A) the polycarbonate resin is usually the main component. In the resin composition of the present embodiment, (A) the polycarbonate resin includes a polycarbonate resin (A-1) and a polycarbonate resin (A-2).
[0010] <<Polycarbonate Resin (A-1)>> The resin composition of the present embodiment contains a polycarbonate resin (A-1) having an integrated luminescence amount of 1.0×10 when measured by temperature elevation using a chemiluminescence method 6 cps or less. The integrated luminescence amount of the polycarbonate resin (A-1) when measured by temperature elevation using a chemiluminescence method is preferably 9.0×10 5 cps or less, more preferably 8.0×10 5 cps or less. The lower limit of the integrated luminescence amount of the polycarbonate resin (A-1) when measured by temperature elevation using a chemiluminescence method is not particularly limited, and is, for example, 1.0×10 5 cps or more. The polycarbonate resin (A-1) preferably has a ratio of the maximum luminescence amount on the low temperature side to the maximum luminescence amount on the high temperature side, (maximum luminescence amount on the low temperature side) / (maximum luminescence amount on the high temperature side), of less than 0.14 when measured by temperature elevation using a chemiluminescence method. The lower limit of the (maximum luminescence amount on the low temperature side) / (maximum luminescence amount on the high temperature side) is not particularly limited, but is preferably 0.01 or more.
[0011] When a Raman spectrum of the polycarbonate resin (A-1) is measured with a laser beam having a wavelength of 532 nm at an exposure time of 1.0 second, 4 exposure times, and a laser output of 1.6 mW, the intensity at 2000 cm -1 is preferably less than 500 cps, more preferably less than 450 cps, still more preferably 400 cps or less, even more preferably 300 cps or less, and still even more preferably 200 cps or less. By setting the intensity to the upper limit value or less, the flame retardancy tends to be further improved. In addition, when the Raman spectrum is measured, the intensity at 2000 cm -1 The lower limit of the intensity is not particularly limited, but 10 cps or more is practical. In this embodiment, the 5% mass loss temperature of the polycarbonate resin (A-1) is preferably above 510°C, more preferably above 511°C, and even more preferably above 512°C. Alternatively, the 5% mass loss temperature of the polycarbonate resin (A-1) may be, for example, 550°C or lower.
[0012] The cumulative luminescence measured by the chemiluminescence method as temperature rise, the ratio of the maximum luminescence on the low-temperature side to the maximum luminescence on the high-temperature side when measured by the chemiluminescence method as temperature rise, and the 2000 cm⁻¹ measurement of the Raman spectrum. -1 The strength and the 5% mass loss temperature are measured according to the examples described below.
[0013] The cumulative luminescence measured by the chemiluminescence method as temperature rise, the ratio of the maximum luminescence on the low-temperature side to the maximum luminescence on the high-temperature side when measured by the chemiluminescence method as temperature rise, and the 2000 cm⁻¹ measurement of the Raman spectrum. -1 Virgin polycarbonate resin is an example of a polycarbonate resin that meets the required strength. Commercially available products such as the polycarbonate resins shown in Examples A7 to A9 described later are virgin polycarbonate resins. Furthermore, it is preferable that such polycarbonate resin (A-1) satisfies the above-mentioned 5% mass loss temperature.
[0014] Specifically, the polycarbonate resin (A-1) is not particularly limited as long as it contains a carbonate ester bond-containing -[OR-OC(=O)]- unit in the molecular main chain (where R is an organic group, preferably a hydrocarbon group, more preferably an aliphatic group, an aromatic group, or a group containing both an aliphatic and an aromatic group, and furthermore, a linear or branched structure). In this embodiment, the polycarbonate resin is preferably an aromatic polycarbonate resin, and more preferably a polycarbonate resin having a bisphenol skeleton. By using such a polycarbonate resin, better heat resistance and toughness can be achieved. In this embodiment, the polycarbonate resin having a bisphenol skeleton preferably has 90 mol% or more of its total constituent units having a bisphenol skeleton, and more preferably has 90 mol% or more of its total constituent units derived from bisphenol A.
[0015] Furthermore, the viscosity-average molecular weight (Mv) of the polycarbonate resin is preferably 10,000 or more, more preferably 12,000 or more, and even more preferably 15,000 or more. Setting it above the lower limit tends to further improve the durability of the resulting molded product. The upper limit of the viscosity-average molecular weight (Mv) of the polycarbonate resin is preferably 50,000 or less, more preferably 40,000 or less, and even more preferably 30,000 or less. Setting it below the upper limit tends to further improve the moldability of the molded product. The viscosity-average molecular weight (Mv) is calculated using methylene chloride as the solvent, determining the intrinsic viscosity [η] (unit: dL / g) at 25°C using an Ubbelohde viscometer, and then using Schnell's viscosity formula, i.e., η = 1.23 × 10⁻⁶ -4 ×Mv 0.83 It means a value calculated from ,. When using two or more types of polycarbonate resin, the viscosity-average molecular weight of the mixture shall be used.
[0016] The method for producing polycarbonate resin is not particularly limited, and resins produced by conventionally known methods such as the phosgene method (interfacial polymerization) or the melting method (transesterification) can be used. Furthermore, when using the melting method, polycarbonate resins with adjusted amounts of OH groups at the end groups can be used.
[0017] In addition to the above, further details of polycarbonate resin can be found in paragraphs 0013 to 0041 of Japanese Patent Publication No. 2021-084942 and paragraphs 0030 to 0035 of Japanese Patent Publication No. 2021-119211, and this information is incorporated herein by reference.
[0018] <<Polycarbonate resin (A-2)>> The resin composition of this embodiment has a ratio of (maximum light emission at low temperature) / (maximum light emission at high temperature), which is the ratio of the maximum light emission at low temperature to the maximum light emission at high temperature when measured by chemiluminescence, of 0.14 to 2.30, and the integrated light emission when measured by chemiluminescence is 1.0 × 10⁻⁶. 6 ~7.5×10 6 It contains polycarbonate resin (A-2), which is a CPS (component-forming compound). It is presumed that by including such polycarbonate resin (A-2), appropriate branching of the polycarbonate resin occurs, carbonization is promoted, and flame retardancy is improved.
[0019] The ratio of (maximum light emission on the low temperature side) to (maximum light emission on the high temperature side) of the polycarbonate resin (A-2) is preferably 0.17 or higher, more preferably 0.20 or higher, even more preferably 0.25 or higher, even more preferably 0.30 or higher, and even more preferably 0.35 or higher. Setting it above the lower limit improves the flame retardancy of the resulting molded product. Furthermore, the ratio of (maximum light emission on the low temperature side) to (maximum light emission on the high temperature side) of the polycarbonate resin (A-2) is preferably 2.25 or lower, more preferably 2.00 or lower, even more preferably 1.50 or lower, even more preferably 1.30 or lower, even more preferably 1.15 or lower, even more preferably 1.00 or lower, especially more preferably 0.90 or lower, and even more especially preferably 0.80 or lower. Setting it below the upper limit tends to further improve flame retardancy.
[0020] The cumulative luminescence measured by chemiluminescence for the aforementioned polycarbonate resin (A-2) was 1.0 × 10⁻⁶. 6 Preferably, it is cps or higher, 1.1 × 10 6 It is more preferable that it be cps or higher, and 1.5 × 10 6 It is even more preferable that it be cps or higher, and 2.0 × 10 6 It may be greater than or equal to cps, such as 4.0 × 10 cps 6 It may be greater than the above. By setting it above the lower limit, the flame retardancy tends to improve further. Also, the cumulative luminescence when the polycarbonate resin (A-2) is measured by chemiluminescence as it rises in temperature is 7.4 × 10⁻⁶. 6 Preferably, it is less than or equal to cps, and 7.3 × 10 6 It is more preferable that it be less than or equal to cps, and 7.2 × 10 6 It is even more preferable that it be less than or equal to cps, 7.1 × 10 6 It is even more preferable that it be less than or equal to cps, 7.0 × 10 6 It is even more preferable that the value be below the cps. By keeping it below the aforementioned upper limit, the flame retardancy tends to improve further.
[0021] The Raman spectrum was measured at 2000 cm² using a 532 nm wavelength laser beam on the aforementioned polycarbonate resin (A-2) with an exposure time of 1.0 second, 4 exposures, and a laser output of 1.6 mW. -1 The intensity at 500 cps is preferably 500 cps or more, more preferably 600 cps or more, even more preferably 700 cps or more, even more preferably 800 cps or more, even more preferably 1000 cps or more, and may also be 2000 cps or more. Furthermore, the Raman spectrum of the polycarbonate resin (A-2) measured at 2000 cm² is also preferable. -1 The strength is preferably 50,000 cps or less, and may be 30,000 cps or less. Setting it below the upper limit and above the lower limit tends to further improve the flame retardancy of the resulting molded product.
[0022] In this embodiment, the 5% mass loss temperature of the polycarbonate resin (A-2) is preferably 480°C or higher, more preferably 485°C or higher, even more preferably 490°C or higher, even more preferably 496°C or higher, even more preferably 500°C or higher, and may also be 501°C or higher. Furthermore, the 5% mass loss temperature of the polycarbonate resin (A-2) is preferably less than 512°C, more preferably 511°C or lower, and even more preferably 510°C or lower. By setting the temperature within this range, the decomposition of the polycarbonate resin proceeds somewhat faster. As a result, it carbonizes somewhat faster and is more likely to form char, improving flame retardancy. If the decomposition of the polycarbonate resin is too fast, it will burn before char can form.
[0023] The cumulative luminescence measured by the chemiluminescence method as temperature rise, the ratio of the maximum luminescence on the low-temperature side to the maximum luminescence on the high-temperature side when measured by the chemiluminescence method as temperature rise, and the 2000 cm⁻¹ measurement of the Raman spectrum. -1 The strength and the 5% mass loss temperature are measured according to the examples described below.
[0024] The cumulative luminescence measured by the chemiluminescence method as temperature rise, the ratio of the maximum luminescence on the low-temperature side to the maximum luminescence on the high-temperature side when measured by the chemiluminescence method as temperature rise, and the 2000 cm⁻¹ measurement of the Raman spectrum. -1 Examples of polycarbonate resins that satisfy the strength at and at least one of the above 5% mass loss temperature include polycarbonate resins derived from molded articles formed from polycarbonate resins. Polycarbonate resin derived from molded products made from polycarbonate resin refers to virgin polycarbonate resin that has undergone some kind of molding process, and includes recycled polycarbonate resin, defective polycarbonate resin molded products, and scraps from the manufacture of polycarbonate resin molded products. Molded products include injection molded products, extruded products, and molded products formed by other manufacturing methods. Examples of recycled polycarbonate resin include that obtained through material recycling, where collected used polycarbonate resin molded products are crushed, alkaline-washed, and reused as fibers, as well as those obtained through chemical recycling (chemical decomposition method) and mechanical recycling. Chemical recycling involves chemically decomposing collected used polycarbonate resin molded products to return them to their raw material level and then resynthesizing the polycarbonate resin. Mechanical recycling, on the other hand, is a method that makes it possible to remove dirt from polycarbonate resin molded products more reliably than material recycling by performing alkaline cleaning more rigorously than in the aforementioned material recycling, or by vacuum drying at high temperatures. For example, recycled polycarbonate resin can be obtained from used polycarbonate resin molded products by removing foreign matter, crushing and washing them, and then pelletizing them using an extruder. Examples of used polycarbonate resin molded products include discs, sheets (including films), meter covers, headlamp lenses, and water bottles, with meter covers, sheets, or headlamp lenses being preferred.
[0025] The polycarbonate resin (A-2) is not particularly limited as long as it contains a -[OR-OC(=O)]- unit containing a carbonate ester bond in its molecular main chain (where R is an organic group, preferably a hydrocarbon group, more preferably an aliphatic group, an aromatic group, or a group containing both an aliphatic and an aromatic group, and furthermore, a linear or branched structure). In this embodiment, the polycarbonate resin is preferably an aromatic polycarbonate resin, and more preferably a polycarbonate resin having a bisphenol skeleton. By using such a polycarbonate resin, better heat resistance and toughness can be achieved. In this embodiment, the polycarbonate resin having a bisphenol skeleton preferably has 90 mol% or more of its total constituent units having a bisphenol skeleton, and more preferably has 90 mol% or more of its total constituent units derived from bisphenol A.
[0026] <<Blend form of polycarbonate resin (A-1) and (A-2)>> In this embodiment, the proportion of polycarbonate resin (A-2) in 100 parts by mass of polycarbonate resin (A) is 10 parts by mass or more, and may be 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 35 parts by mass or more, 40 parts by mass or more, 45 parts by mass or more, or 50 parts by mass or more. Also in this embodiment, the proportion of polycarbonate resin (A-2) in 100 parts by mass of polycarbonate resin (A) is 99 parts by mass or less, preferably 95 parts by mass or less, and may be 90 parts by mass or less, 85 parts by mass or less, or 80 parts by mass or less. Setting it below the above upper limit tends to further improve flame retardancy. The resin composition of this embodiment may contain only one type of polycarbonate resin (A-1) and one type of polycarbonate resin (A-2), or it may contain two or more types. When two or more types are included, it is preferable that the total amount is within the above range.
[0027] In this embodiment, the proportion of polycarbonate resin (A-1) and polycarbonate resin (A-2) in the (A) polycarbonate resin contained in the resin composition is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 97% by mass or more, and even more preferably 99% by mass or more. Furthermore, in the resin composition of this embodiment, the content of (A) polycarbonate resin is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 97% by mass or more, when the resin composition does not contain a reinforcing material. Furthermore, in the resin composition of this embodiment, the content of (A) polycarbonate resin is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 97% by mass or more, of the components excluding the reinforcing material in the resin composition when the resin composition contains a reinforcing material.
[0028] <(B) Alkali metal salts> The resin composition of this embodiment contains (B) an alkali metal salt. By including an alkali metal salt (alkali metal salt-based flame retardant), a molded product with excellent flame retardancy can be obtained. (B) The alkali metal salt is usually an alkali metal salt of an organic acid. (B) Examples of alkali metal salts include metal sulfonic acid salts, metal carboxylate salts, metal borate salts, and metal phosphate salts, but metal sulfonic acid salts are preferred from the viewpoint of thermal stability.
[0029] Examples of metals that make up alkali metal salts include lithium (Li), sodium (Na), potassium (K), rubidium (Rb), and cesium (Cs), among which sodium, potassium, and cesium are preferred, and sodium and potassium are more preferred.
[0030] Examples of preferred alkali metal sulfonic acid salts include alkali metal salts of fluorine-containing aliphatic sulfonic acids or aromatic sulfonic acids. Specific examples of preferred alkali metal salts of fluorine-containing aliphatic sulfonic acids having at least one CF bond in the molecule, such as potassium perfluorobutanesulfonate, lithium perfluorobutanesulfonate, sodium perfluorobutanesulfonate, cesium perfluorobutanesulfonate, potassium trifluoromethanesulfonate, lithium trifluoromethanesulfonate, sodium trifluoromethanesulfonate, and cesium trifluoromethanesulfonate; dipotassium diphenylsulfon-3,3'-disulfonate, potassium diphenylsulfon-3-sulfonate, sodium benzenesulfonate, and sodium (poly)styrenesulfonate. Examples include alkali metal salts of aromatic sulfonic acids having at least one aromatic group in their molecule, such as sodium p-toluenesulfonate, sodium (branched) dodecylbenzenesulfonate, sodium trichlorobenzenesulfonate, potassium benzenesulfonate, potassium styrenesulfonate, potassium (poly)styrenesulfonate, potassium p-toluenesulfonate, potassium (branched) dodecylbenzenesulfonate, potassium trichlorobenzenesulfonate, cesium benzenesulfonate, cesium (poly)styrenesulfonate, cesium p-toluenesulfonate, cesium (branched) dodecylbenzenesulfonate, and cesium trichlorobenzenesulfonate.
[0031] For other alkali metal salts, refer to paragraphs 0069 to 0078 of Japanese Patent Publication No. 2015-117298, which are incorporated herein by reference.
[0032] The content of (B) alkali metal salt in the resin composition of this embodiment is 0.005 parts by mass or more, preferably 0.008 parts by mass or more, more preferably 0.01 parts by mass or more, even more preferably 0.03 parts by mass or more, and even more preferably 0.05 parts by mass or more, per 100 parts by mass of (A) polycarbonate resin. Setting it above the lower limit promotes the formation of a carbonized layer during combustion of the polycarbonate resin, thereby further enhancing flame retardancy. Furthermore, the content of (B) alkali metal salt is 1 part by mass or less, preferably 0.8 parts by mass or less, more preferably 0.5 parts by mass or less, even more preferably 0.3 parts by mass or less, even more preferably 0.2 parts by mass or less, and even more preferably 0.15 parts by mass or less, per 100 parts by mass of (A) polycarbonate resin. Setting it below the upper limit tends to result in a more effective flame retardant effect despite a reduction in the amount of flame retardant. The resin composition of this embodiment may contain only one alkali metal salt (B), or it may contain two or more. When it contains two or more, it is preferable that the total amount is within the above range.
[0033] The resin composition of this embodiment may or may not contain (B) a flame retardant other than an alkali metal salt. Examples of (B) flame retardants other than alkali metal salts include phosphorus-based flame retardants and halogen-based flame retardants. An example of the resin composition of this embodiment is that it substantially does not contain any flame retardants other than (B) alkali metal salts. Substantially does not contain any flame retardants other than (B) alkali metal salts among the flame retardants contained in the resin composition. salt This means that the content is 10% by mass or less, preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less.
[0034] <(C) Fluoropolymer having fibril-forming ability> The resin composition of this embodiment includes a fluoropolymer having fibril-forming ability. Fluoropolymers with fibril-forming ability are drip-preventing agents that readily disperse in resin compositions and tend to bond with other polymers to form fibrous structures; they are fluorine-based resins with fibril-forming ability. The fluoropolymer having fibril-forming ability preferably has an extremely high molecular weight of 1 million to 10 million, and tends to bond with other fluoropolymers to form fibers when subjected to external forces such as shear force. Preferred fluoropolymers include tetrafluoroethylene (TFE) resin, perfluoroalkoxy (PFA) resin, and fluoroethylene propylene (FEP) resin, with polytetrafluoroethylene being particularly preferred.
[0035] Examples of fluoropolymers that have fibril-forming ability include Teflon® 6J manufactured by Mitsui DuPont Fluorochemicals and Polyflon manufactured by Daikin Industries, Ltd.
[0036] It is also preferable to use the fluoropolymer in the form of an aqueous dispersion. This dispersion is an aqueous dispersion prepared by adding a surfactant to a fluoropolymer latex, which is usually obtained by emulsion polymerization, and then concentrating and stabilizing it. The fluoropolymer content in the aqueous dispersion is preferably 20 to 80% by mass, and particularly preferably 30 to 70% by mass. Examples of aqueous dispersions of polytetrafluoroethylene include Teflon® 30J manufactured by Mitsui DuPont Fluorochemicals, Fluon D-1 manufactured by Daikin Industries, and polytetrafluoroethylene polymers having a multilayer structure formed by polymerizing vinyl monomers, such as Metabren A-3800 manufactured by Mitsubishi Rayon.
[0037] Furthermore, the fluoropolymer having fibril-forming ability preferably has a primary particle diameter in the range of 0.05 to 1.0 μm, and more preferably 0.1 to 0.5 μm. In the resin composition, the fluoropolymer mainly takes the form of fibrils with a thickness of 0.5 microns or less, and it is preferable that the fibrils exist in a network structure and / or a branched structure.
[0038] The content of (C) fibril-forming fluoropolymer in the resin composition of this embodiment is 0.01 parts by mass or more, preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.07 parts by mass or more, and even more preferably 0.1 parts by mass or more, per 100 parts by mass of (A) polycarbonate resin. Setting it above the lower limit tends to effectively exhibit a drip prevention effect. Furthermore, the content of (C) fibril-forming fluoropolymer is 3 parts by mass or less, preferably 2.5 parts by mass or less, more preferably 2.0 parts by mass or less, even more preferably 1.0 part by mass or less, even more preferably 0.7 parts by mass or less, and even more preferably 0.5 parts by mass or less, per 100 parts by mass of (A) polycarbonate resin. Setting it below the upper limit tends to improve the mechanical strength of the resulting molded product and improve its appearance. The resin composition of this embodiment may contain only one type of fluoropolymer having fibril-forming ability, or it may contain two or more types. When two or more types are included, it is preferable that the total amount is within the above range.
[0039] <Elastomer> The resin composition of this embodiment may also preferably contain an elastomer. As the elastomer, a copolymer obtained by graft copolymerizing a rubber component with a monomer component copolymerizable thereto is preferred. The method for producing such a graft copolymer may be any of the following methods: bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc., and the copolymerization method may be single-stage grafting or multi-stage grafting.
[0040] The above rubber components typically have a glass transition temperature of 0°C or lower, preferably -20°C or lower, and more preferably -30°C or lower. Specific examples of rubber components include polybutadiene rubber, polyisoprene rubber, polyalkyl acrylate rubber such as polybutyl acrylate, poly(2-ethylhexyl acrylate), and butyl acrylate-2-ethylhexyl acrylate copolymer, silicone rubber such as organopolysiloxane rubber, butadiene-acrylic composite rubber, IPN-type composite rubber consisting of organopolysiloxane rubber and polyalkyl acrylate rubber, styrene-butadiene rubber, ethylene-α-olefin rubber such as ethylene-propylene rubber, ethylene-butene rubber, and ethylene-octene rubber, ethylene-acrylic rubber, and fluororubber. These may be used individually or in combination of two or more. Among these, polybutadiene rubber, polyalkyl acrylate rubber, IPN-type composite rubber consisting of organopolysiloxane rubber and polyalkyl acrylate rubber, and styrene-butadiene rubber are preferred in terms of mechanical properties and surface appearance.
[0041] Specific examples of monomer components that can be graft copolymerized with rubber components include aromatic vinyl compounds, vinyl cyanide compounds, (meth)acrylic acid ester compounds, epoxy group-containing (meth)acrylic acid ester compounds such as glycidyl (meth)acrylate; maleimide compounds such as maleimide, N-methylmaleimide, and N-phenylmaleimide; and α,β-unsaturated carboxylic acid compounds such as maleic acid, phthalic acid, and itaconic acid, and their anhydrides (e.g., maleic anhydride). These monomer components may be used individually or in combination of two or more. Among these, aromatic vinyl compounds, vinyl cyanide compounds, (meth)acrylic acid ester compounds, and (meth)acrylic acid compounds are preferred in terms of mechanical properties and surface appearance, and (meth)acrylic acid ester compounds are more preferred. Specific examples of (meth)acrylic acid ester compounds include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, and octyl (meth)acrylate.
[0042] In this embodiment, the elastomer used is preferably of the core / shell type graft copolymer type from the viewpoint of impact resistance and surface appearance. Among these, a core / shell type graft copolymer is preferred, comprising a core layer made of at least one rubber component selected from polybutadiene-containing rubber, polybutyl acrylate-containing rubber, and IPN-type composite rubber consisting of organopolysiloxane rubber and polyalkyl acrylate rubber, and a shell layer formed by copolymerizing (meth)acrylic acid ester around it, with a core / shell type elastomer using butadiene-based rubber as the core being particularly preferred. In the above core / shell type graft copolymer, it is preferable that the rubber component is contained in 40% by mass or more, and more preferably 60% by mass or more. Furthermore, it is preferable that the (meth)acrylic acid component is contained in 10% by mass or more.
[0043] Preferred specific examples of these core / shell type graft copolymers include acrylonitrile-butadiene-styrene copolymer (ABS), methyl methacrylate-butadiene-styrene copolymer (MBS), methyl methacrylate-acrylonitrile-butadiene-styrene copolymer (MABS), methyl methacrylate-butadiene copolymer (MB), methyl methacrylate-acrylic rubber copolymer (MA), methyl methacrylate-acrylic rubber-styrene copolymer (MAS), methyl methacrylate-acrylic butadiene rubber copolymer, methyl methacrylate-acrylic butadiene rubber-styrene copolymer, and methyl methacrylate-(acrylic silicone IPN rubber) copolymer. Such rubbery polymers may be used individually or in combination of two or more. In addition to the above, as elastomers, those described in paragraphs 0068 to 0079 of Japanese Patent Publication No. 2019-123809 may be used, and this content is incorporated herein by reference.
[0044] If the resin composition of this embodiment contains an elastomer, its content is preferably 0.5 parts by mass or more, more preferably 1.0 part by mass or more, and even more preferably 1.5 parts by mass or more, per 100 parts by mass of (A) polycarbonate resin. Setting it above the lower limit tends to improve the impact resistance of the resulting molded product. Furthermore, the upper limit of the elastomer content is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, even more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, per 100 parts by mass of (A) polycarbonate resin. Setting it below the upper limit tends to improve the surface hardness, heat resistance, rigidity, etc., of the resulting molded product. The resin composition of this embodiment may contain only one type of elastomer, or it may contain two or more types. When it contains two or more types, it is preferable that the total amount is within the above range.
[0045] <Epoxy compounds> The resin composition of this embodiment may also preferably contain an epoxy compound. By including an epoxy compound, a molded product with superior mechanical strength can be obtained. Any epoxy compound that has one or more epoxy groups in one molecule is acceptable, and typically glycidyl compounds, which are reaction products of alcohols, phenols, or carboxylic acids with epichlorohydrin, or compounds in which olefinic double bonds have been epoxidized can be used. Examples of epoxy compounds include novolac-type epoxy compounds, bisphenol A-type epoxy compounds, bisphenol F-type epoxy compounds, alicyclic epoxy compounds, glycidyl ethers, glycidyl esters, epoxidized butadiene polymers, and resorcinol-type epoxy compounds.
[0046] Examples of novolac-type epoxy compounds include phenol novolac-type epoxy compounds and cresol novolac-type epoxy compounds. Examples of bisphenol A type epoxy compounds include bisphenol A-diglycidyl ether and hydrogenated bisphenol A-diglycidyl ether, while examples of bisphenol F type epoxy compounds include bisphenol F-diglycidyl ether and hydrogenated bisphenol F-diglycidyl ether.
[0047] Examples of alicyclic epoxy compounds include vinylcyclohexene dioxide, dicyclopentadiene oxide, 3,4-epoxycyclohexyl-3,4-cyclohexyl carboxylate, bis(3,4-epoxycyclohexylmethyl) adipate, vinylcyclohexene diepoxide, and 3,4-epoxycyclohexyl glycidyl ether.
[0048] Specific examples of glycidyl ethers include monoglycidyl ethers such as methyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, decyl glycidyl ether, stearyl glycidyl ether, phenyl glycidyl ether, butylphenyl glycidyl ether, and allyl glycidyl ether; and diglycidyl ethers such as neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, glycerin diglycidyl ether, propylene glycol diglycidyl ether, and bisphenol A diglycidyl ether.
[0049] Examples of glycidyl esters include monoglycidyl esters such as glycidyl benzoate and glycidyl sorbate; and diglycidyl esters such as diglycidyl adipic acid, diglycidyl terephthalate, and diglycidyl orthophthalate.
[0050] Examples of epoxidized butadiene polymers include epoxidized polybutadiene, epoxidized styrene-butadiene copolymers, and epoxidized hydrogenated styrene-butadiene copolymers. Examples of resorcinol-type epoxy compounds include resorcinol diglycidyl ether.
[0051] Furthermore, the epoxy compound may be a copolymer in which a glycidyl group-containing compound is one of the components. For example, a copolymer of a glycidyl ester of an α,β-unsaturated acid and one or more monomers selected from the group consisting of α-olefins, acrylic acid, acrylic acid esters, methacrylic acid, and methacrylic acid esters is used.
[0052] As for the epoxy compound, epoxy compounds with an epoxy equivalent of 50 to 10,000 g / eq and a weight-average molecular weight of 8,000 or less are preferred.
[0053] The epoxy compound content is preferably 0.001 parts by mass or more, more preferably 0.005 parts by mass or more, even more preferably 0.01 parts by mass or more, and preferably 2 parts by mass or less, more preferably 1 part by mass or less, even more preferably 0.5 parts by mass or less, and particularly preferably 0.1 parts by mass or less, per 100 parts by mass of polycarbonate resin (A). The resin composition of this embodiment may contain only one epoxy compound or two or more epoxy compounds. When two or more epoxy compounds are included, it is preferable that the total amount is within the above range.
[0054] <Stabilizer> Examples of stabilizers include heat stabilizers and antioxidants. Other examples of stabilizers include phenolic, amine, phosphorus, and thioether-based stabilizers. In this embodiment, in particular, phosphorus-based heat stabilizers and / or phenolic antioxidants are preferred.
[0055] Any known phosphorus-based heat stabilizer can be used. Specific examples include phosphorus oxoacids such as phosphoric acid, phosphonic acid, phosphorous acid, phosphinic acid, and polyphosphate; acidic pyrophosphate metal salts such as sodium acidic pyrophosphate, potassium acidic pyrophosphate, and calcium acidic pyrophosphate; phosphates of Group 1 or Group 2B metals such as potassium phosphate, sodium phosphate, cesium phosphate, and zinc phosphate; and organic phosphate compounds, organic phosphite compounds, and organic phosphonite compounds, with organic phosphite compounds being particularly preferred.
[0056] Examples of organic phosphite compounds include triphenyl phosphite, tris(mononylphenyl) phosphite, tris(mononyl / dinonylphenyl) phosphite, tris(2,4-di-tert-butylphenyl) phosphite, monooctyldiphenyl phosphite, dioctylmonophenyl phosphite, monodecyldiphenyl phosphite, didecylmonophenyl phosphite, tridecyl phosphite, trilauryl phosphite, tristearyl phosphite, and 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite. Examples of such organic phosphite compounds include, for example, "ADEKA Stab (registered trademark; hereinafter the same) 1178," "ADEKA Stab 2112," and "ADEKA Stab HP-10" manufactured by ADEKA Corporation, "JP-351," "JP-360," and "JP-3CP" manufactured by Johoku Chemical Industry Co., Ltd., and "Irgaphos (registered trademark; hereinafter the same) 168" manufactured by BASF.
[0057] As a phenolic antioxidant, a hindered phenolic antioxidant is preferably used. Specific examples of hindered phenol antioxidants include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphate, 4,6-bis(octyl) Examples include ruthiomethyl)-o-cresol, ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazine-2-ylamino)phenol, and 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate.
[0058] Among these, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred. Specific examples of such hindered phenol antioxidants include, for example, BASF's "Irganox (registered trademark; hereinafter the same) 1010" and "Irganox 1076," and ADEKA's "ADEKA Stab AO-50" and "ADEKA Stab AO-60."
[0059] The stabilizer content in the resin composition of this embodiment is typically 0.001 parts by mass or more, preferably 0.005 parts by mass or more, more preferably 0.01 parts by mass or more, and typically 1 part by mass or less, preferably 0.5 parts by mass or less, more preferably 0.3 parts by mass or less, per 100 parts by mass of (A) polycarbonate resin. By setting the stabilizer content within the above range, the effect of adding the stabilizer is more effectively exhibited. The resin composition of this embodiment may contain only one stabilizer or two or more stabilizers. When two or more stabilizers are included, it is preferable that the total amount is within the above range.
[0060] <Release agent> The resin composition of this embodiment may contain a mold release agent. Examples of release agents include aliphatic carboxylic acids, salts of aliphatic carboxylic acids, esters of aliphatic carboxylic acids and alcohols, aliphatic hydrocarbon compounds with a number average molecular weight of 200 to 15,000, polysiloxane-based silicone oils, ketone waxes, and light amides. Aliphatic carboxylic acids, salts of aliphatic carboxylic acids, and esters of aliphatic carboxylic acids and alcohols are preferred, and salts of aliphatic carboxylic acids are more preferred. Details of the release agent can be found in paragraphs 0055 to 0061 of Japanese Patent Publication No. 2018-095706 and paragraphs 0106 to 0115 of Japanese Patent Publication No. 2015-117298, and this information is incorporated herein by reference. If the resin composition of this embodiment contains a release agent, its content is preferably 0.05 to 3% by mass, more preferably 0.1 to 0.8% by mass, and even more preferably 0.1 to 0.6% by mass. The resin composition of this embodiment may contain only one type of release agent, or it may contain two or more types. When it contains two or more types, it is preferable that the total amount is within the above range.
[0061] <Other ingredients> The resin composition of this embodiment may contain other components as needed, as long as they do not significantly impair the desired physical properties. Examples of other components include reinforcing materials, thermoplastic resins other than polycarbonate resin, and various resin additives. For reinforcing materials, refer to paragraphs 0107 to 0115 of Japanese Patent Publication No. 2014-136710, which are incorporated herein by reference. Examples of resin additives include colorants (dyes, pigments), antistatic agents, antifogging agents, antiblocking agents, flow improvers, plasticizers, dispersants, and antibacterial agents. The resin additive may contain only one type, or two or more types in any combination and ratio. As for resin additives, reference can also be given to paragraphs 0117 to 0128 of Japanese Patent Publication No. 2015-117298, which are incorporated herein by reference.
[0062] <Physical properties of resin compositions> The resin composition of this embodiment is preferably highly flame-retardant. Specifically, it is preferable that the resin composition of this embodiment achieves V-0 when molded to a thickness of 1.5 mm and tested in accordance with UL94. Furthermore, when the resin composition of this embodiment is molded to a thickness of 1.5 mm and tested in accordance with UL94, the total afterflame time is preferably 50 seconds or less, more preferably 30 seconds or less, even more preferably 25 seconds or less, and most preferably 24 seconds or less.
[0063] <Manufacturing of resin compositions> There are no limitations on the manufacturing method of the resin composition of this embodiment, and a wide range of known methods for manufacturing resin compositions can be used. For example, a method may be used in which (A) polycarbonate resin, (B) alkali metal salt, and (C) fluoropolymer having fibril-forming ability, as well as other components that may be added as needed, are pre-mixed using various mixers such as a tumbler or Henschel mixer, and then melt-kneaded using a mixer such as a Banbury mixer, roll, braver, single-screw extruder, twin-screw extruder, or kneader. The melt-kneading temperature is not particularly limited, but is usually in the range of 240 to 320°C.
[0064] <Molded products> The molded article of this embodiment is formed from the resin composition of this embodiment. The resin composition described above (for example, pellets) is molded into a molded article by various molding methods. There are no particular restrictions on the shape of the molded article, and it can be appropriately selected according to the use and purpose of the molded article. Examples include film-shaped, rod-shaped, cylindrical, annular, circular, elliptical, polygonal, irregularly shaped, hollow, frame-shaped, box-shaped, panel-shaped, button-shaped, etc.
[0065] The method for molding the molded product is not particularly limited, and conventionally known molding methods can be employed. Examples include injection molding, injection compression molding, extrusion molding, shape extrusion, transfer molding, hollow molding, gas-assisted hollow molding, blow molding, extrusion blow molding, IMC (in-mold coating) molding, rotational molding, multilayer molding, two-color molding, insert molding, sandwich molding, foam molding, and pressure molding. In particular, the resin composition of this embodiment is suitable for molded products obtained by injection molding, injection compression molding, and extrusion molding. However, it goes without saying that the resin composition of this embodiment is not limited to molded products obtained by these methods.
[0066] The molded product of this embodiment is widely used in applications where flame retardancy is required. Specifically, it is preferably used in electrical and electronic equipment / components, office automation equipment / components, information terminal equipment / components, machine parts, home appliances, vehicle parts, building materials, various containers, leisure goods and miscellaneous items, lighting equipment, and the like. [Examples]
[0067] The present invention will be described in more detail below with reference to examples. The materials, amounts used, proportions, processing content, and processing procedures shown in the following examples can be modified as appropriate, as long as they do not depart from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments used in the examples are difficult to obtain due to discontinuation or other reasons, measurements can be taken using other instruments with equivalent performance.
[0068] 1. Raw materials Regarding the polycarbonate resin, A1 uses recycled material derived from discs, A2 and A3 use recycled material derived from seats and meter covers, A4 and A10 use recycled material derived from headlamp lenses, and A5, A6, and A11 use recycled material derived from water bottles. Polycarbonate resins A7 to A9 were made from commercially available virgin polycarbonate resins as listed below.
[0069] [Table 1]
[0070] <Integrated luminescence and (maximum luminescence at low temperature) / (maximum luminescence at high temperature) when measured by chemiluminescence during temperature increase> The cumulative luminescence amount when measuring polycarbonate resin by chemiluminescence and the ratio of the maximum luminescence amount at low temperature to the maximum luminescence amount at high temperature, (maximum luminescence amount at low temperature) / (maximum luminescence amount at high temperature), were measured as follows.
[0071] Approximately 200 mg of the sample (polycarbonate resin) was placed in a chemiluminescence analyzer. Under a nitrogen atmosphere with a nitrogen flow rate of 50 mL / min, the temperature was raised from 50°C to 350°C at a heating rate of 20°C / min, and the amount of luminescence (unit: cps) was measured every second. The cumulative luminescence (cumulative luminescence measured by chemiluminescence during temperature increase) from 0 seconds to 810 seconds (unit: cps) was measured. The maximum luminescence between 0 and 500 seconds was defined as the "maximum luminescence on the low-temperature side," and the maximum luminescence between 500 seconds and 810 seconds was defined as the "maximum luminescence on the high-temperature side." The formula (maximum luminescence on the low-temperature side) / (maximum luminescence on the high-temperature side) was then calculated. However, if the maximum luminescence occurred at 810 seconds on the high-temperature side, the peak closest to 810 seconds before that point was used as the maximum luminescence. The chemiluminescence measurement system used was the CLA-FS4 (main unit) and CLS-SH0 (sample chamber) manufactured by Tohoku Electronics Industry Co., Ltd. The results are shown in Table 2 below.
[0072] <5% mass loss temperature> The 5% mass loss temperature was calculated using a thermogravimetric analyzer under the following conditions: measurement range 40-600°C, heating rate 10°C / min, nitrogen atmosphere at 200 mL / min, and sample volume 5 mg. The thermogravimetric analyzer used was the "NEXTA(registered trademark) STA200RV" manufactured by Hitachi High-Tech Science Corporation. The results are shown in Table 2 below.
[0073] <2000cm -1 Raman spectral intensity > When measuring the Raman spectrum at 2000 cm⁻¹ using a 532 nm wavelength laser, with an exposure time of 1.0 second, 4 exposures, and a laser output of 1.6 mW, the result was... -1 The intensity was measured. The measurement was taken with the focus on the surface of the pellet. A Thermo Fisher Scientific DXR II was used to measure the intensity of the Raman spectra. The results are shown in Table 2 below.
[0074] [Table 2]
[0075] Other ingredients are listed in Table 3 below. [Table 3]
[0076] Examples 1-23, Comparative Examples 1-13 <Preparation of resin pellets> Each component listed in Tables 1-3 was blended in the proportions shown in Tables 5-10 (each component is in parts by mass) and mixed in a tumbler for 20 minutes. This mixture was supplied to a Japan Steel Works extruder (TEX30HSST) and kneaded under the conditions of a screw rotation speed of 220 rpm, a discharge rate of 30 kg / hour, and a barrel temperature of 260-270°C, and extruded into strands. This was cooled with water and pelletized using a pelletizer.
[0077] <Manufacturing of combustion test specimens> The obtained pellets were dried at 120°C for 5 hours, and then injection molded using an injection molding machine (Sumitomo Heavy Industries, Ltd. "SE100DUHP") under conditions of a set temperature of 280°C and a mold temperature of 80°C to obtain a molded specimen (UL specimen) with a length of 127 mm, a width of 12.7 mm, and a wall thickness of 1.5 mm. The obtained UL specimen was subjected to a vertical combustion test in accordance with UL94, and the flammability results were ranked from best to worst as V-0, V-1, and V-2.
[0078] <Evaluation of flame retardancy> The UL test specimens prepared as described above were conditioned for 48 hours in a constant temperature chamber at 23°C and 50% humidity, and then their flame retardancy was evaluated according to the UL94 test (combustion test for plastic materials for equipment components). The results are shown in Tables 5 to 10. This test evaluates flame retardancy based on the afterflame time and drip rate after a burner flame is applied to a vertically held test specimen for 10 seconds, according to the following criteria.
[0079] [Table 4]
[0080] Afterflame time is the length of time that the UL test specimen continues to burn with flame after the burner is removed. The cotton ignition test by drip is a test to determine whether the marker cotton, located approximately 300 mm from the bottom of the UL test specimen, is ignited by the dripping material from the specimen. If even one of the five samples fails to meet the above criteria, it will be marked as NR (not rated) and V-2 will not be satisfied.
[0081] [Table 5]
[0082] [Table 6]
[0083] [Table 7]
[0084] [Table 8]
[0085] [Table 9]
[0086] [Table 10]
[0087] As is clear from the above results, the ratio of the maximum luminescence at the low temperature side to the maximum luminescence at the high temperature side when measured by chemiluminescence, i.e., (maximum luminescence at low temperature side) / (maximum luminescence at high temperature side), is between 0.14 and 2.30, and the integrated luminescence measured by chemiluminescence when measured by chemiluminescence is 1.0 × 10⁻⁶. 6 ~7.5×10 6When polycarbonate resin (A-2), which is a cps (comparative example), was not included (Comparative Examples 1, 2, 3, 5-13), the total afterflame time increased. Furthermore, when the alkali metal salt content was high (Comparative Example 4), the total afterflame time increased even further. In addition, despite the inclusion of a large amount of flame retardant, the flame retardancy decreased to V-1.
Claims
1. (A) Per 100 parts by mass of polycarbonate resin, (B) 0.005 to 1 part by mass of alkali metal salt, (C) 0.01 to 3 parts by mass of a fluoropolymer having fibril-forming ability, It contains 0.001 to 2 parts by mass of epoxy compound, The aforementioned (A) polycarbonate resin comprises polycarbonate resin (A-1) and polycarbonate resin (A-2), The proportion of polycarbonate resin (A-2) in 100 parts by mass of polycarbonate resin (A) is 10 to 99 parts by mass. The polycarbonate resin (A-1) was heated from 50°C to 350°C at a heating rate of 20°C / min under a nitrogen atmosphere with a nitrogen flow rate of 50 mL / min, and the integrated luminescence measured by chemiluminescence was 1.0 × 10⁻¹⁴. 6 It is less than cps, Under the conditions that the polycarbonate resin (A-2) was heated from 50°C to 350°C at a heating rate of 20°C / min in a nitrogen atmosphere with a nitrogen flow rate of 50 mL / min, the ratio of the maximum luminescence at the low temperature side to the maximum luminescence at the high temperature side, (maximum luminescence at low temperature side) / (maximum luminescence at high temperature side), measured by chemiluminescence, was 0.14 or more and 2.30 or less, and the integrated luminescence measured by chemiluminescence was 1.0 × 10⁻¹⁴. 6 ~7.5 x 10 6 It is a CPS, The alkali metal salts (B) include potassium perfluorobutanesulfonate, lithium perfluorobutanesulfonate, sodium perfluorobutanesulfonate, cesium perfluorobutanesulfonate, potassium trifluoromethanesulfonate, lithium trifluoromethanesulfonate, sodium trifluoromethanesulfonate, cesium trifluoromethanesulfonate, dipotassium diphenylsulfonate-3,3'-disulfonate, potassium diphenylsulfonate-3,6,5 At least one selected from the group consisting of cesium, sodium (branched) dodecylbenzenesulfonate, sodium trichlorobenzenesulfonate, potassium benzenesulfonate, potassium styrenesulfonate, potassium (poly)styrenesulfonate, potassium p-toluenesulfonate, potassium (branched) dodecylbenzenesulfonate, potassium trichlorobenzenesulfonate, cesium benzenesulfonate, cesium (poly)styrenesulfonate, cesium p-toluenesulfonate, cesium (branched) dodecylbenzenesulfonate, and cesium trichlorobenzenesulfonate. A resin composition, The content of flame retardants other than alkali metal salts in (B) above is 1% by mass or less of the content of alkali metal salts. The polycarbonate resin (A-1) is such that 90 mol% or more of its total constituent units are derived from bisphenol, and is a virgin polycarbonate resin. The aforementioned polycarbonate resin (A-2) is a material recycled product of used polycarbonate resin molded products, in which 90 mol% or more of the total constituent units are derived from bisphenol A. The epoxy compound is 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate. Resin composition.
2. Under the conditions that the polycarbonate resin (A-1) was heated from 50°C to 350°C at a heating rate of 20°C / min in a nitrogen atmosphere with a nitrogen flow rate of 50 mL / min, the ratio of the maximum luminescence emission at the low temperature to the maximum luminescence emission at the high temperature, (maximum luminescence emission at low temperature) / (maximum luminescence emission at high temperature), measured by chemiluminescence, was less than 0.
14. The resin composition according to claim 1.
3. The resin composition according to claim 1 or 2, wherein the 5% mass loss temperature of the polycarbonate resin (A-2), measured under conditions of a nitrogen atmosphere of 200 mL / min, a heating rate of 10°C / min, and a measurement range of 40 to 600°C, is 480°C or higher and less than 512°C.
4. The resin composition according to any one of claims 1 to 3, wherein the polycarbonate resin (A-2) is derived from a molded article formed from the polycarbonate resin.
5. A molded article formed from the resin composition according to any one of claims 1 to 4.
Citation Information
Patent Citations
Polycarbonate based laser direct structuring compounds with post-consumer recycled plastics
EP3640954A1
Flame-retardant polycarbonate resin composition and resin molded article produced by molding the same
JP2007254561A
Resin composition
JP2009114364A
Aromatic polycarbonate resin composition and molded product thereof
JP2010202746A
Resin composition and molding
JP2021155499A