Adhesive sheet, adhesive sheet with release liner, method for manufacturing an adhesive sheet, and method for manufacturing an adhesive sheet with a release liner

The adhesive sheet with a transparent substrate and multiple adhesive layers addresses the silvering issue by preventing air pockets, ensuring clear ink visibility.

JP7954005B2Active Publication Date: 2026-11-19LINTEC CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022058631
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-03-31
Publication Date
2026-11-19
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

Conventional adhesive sheets experience a whitening phenomenon (silvering) due to air pockets forming between the adhesive layer and the ink layer, causing the ink layer to appear whitish and altering its appearance.

Method used

The adhesive sheet is structured with a transparent substrate, an ink layer on the substrate, and multiple adhesive layers in a specific order, along with a release liner, to prevent air pockets and suppress silvering.

Benefits of technology

The solution effectively prevents the occurrence of silvering, ensuring clear visibility of the ink layer without air pockets, maintaining the intended appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954005000001
    Figure 0007954005000001
  • Figure 0007954005000002
    Figure 0007954005000002
  • Figure 0007954005000003
    Figure 0007954005000003
Patent Text Reader

Abstract

To provide an adhesive sheet capable of suppressing the occurrence of silvering, an adhesive sheet with a release liner, a method for producing an adhesive sheet and a method for producing an adhesive sheet with a release liner.SOLUTION: There is provided an adhesive sheet 10 which comprises a transparent base material 11, an ink layer 12 provided on a surface of the transparent base material 11 and a first adhesive layer 13 in this order.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive sheet, an adhesive sheet with a release liner, a method for producing an adhesive sheet, and a method for producing an adhesive sheet with a release liner. Background Art

[0002] Adhesive sheets are used, which are obtained by printing characters, colors, figures, symbols, patterns and the like (hereinafter collectively referred to as "patterns and the like") on inkjet media or the like with an inkjet printer or the like for purposes such as indoor and outdoor signboards, decorations, and vehicle markings. That is, an ink layer is formed on the adhesive sheet by printing. A transparent base material is attached to protect the ink layer.

[0003] For example, Patent Document 1 discloses a printed matter production method including: an ink arranging step of ejecting a photocurable ink onto a printing surface of a medium by an inkjet method so that the average surface roughness is less than 15 μm, and irradiating the ink with light to cure the ink; and a laminating step of bonding the medium and the protective film together by adhering the adhesive layer of the protective film, which has an adhesive layer with a thickness of 18 μm or more and a base material supporting the adhesive layer, to the printing surface and the surface of the ink.

[0004] FIG. 12 is a schematic cross-sectional view showing an example of the configuration of a conventional adhesive sheet.

[0005] The adhesive sheet 100 is an adhesive sheet with a release liner 170. The adhesive sheet 100 is constructed by laminating the transparent substrate 120, the first adhesive layer 130, the ink layer 140, the base substrate 150, the second adhesive layer 160, and the release liner 170 in that order from top to bottom of the drawing. When using the sheet, the release liner 170 is peeled off to expose the second adhesive layer 160, creating the adhesive sheet 110. The second adhesive layer 160 of the adhesive sheet 110 is then applied to the desired location. In conventional adhesive sheets 100, the ink layer 140 is placed on the base substrate 150, and when the user views it from the outside, they can see the pattern of the ink layer 140 through the transparent substrate 120 and the first adhesive layer 130 (see arrow L2).

[0006] Figure 13 is a process diagram of an example of a conventional method for manufacturing an adhesive sheet 100. Figures 13A, 13B, 13C, 13D, 13E, and 13F are process diagrams showing each step of the conventional method for manufacturing an adhesive sheet 100.

[0007] First, an adhesive composition is applied to the release liner 180 to form a first adhesive layer 130. Then, a transparent substrate 120 is bonded onto the first adhesive layer 130 to obtain a laminate 100a having the transparent substrate 120, the first adhesive layer 130, and the release liner 180 in that order (see Figures 13A, 13B, etc.).

[0008] Next, an adhesive composition is applied to the release liner 170 to form a second adhesive layer 160. Then, the base material 150 is bonded onto the second adhesive layer 160 to obtain a laminate 100b having the base material 150, the second adhesive layer 160, and the release liner 170 in this order (see Figures 13C, 13D, etc.).

[0009] Furthermore, ink is applied to the surface of the base material 150 of the laminate 100b using an inkjet printer or the like to form an ink layer 140. In this way, a laminate 100c is obtained having the ink layer 140, the base material 150, the second adhesive layer 160, and the release liner 170 in this order (see Figure 13E, etc.).

[0010] Then, the release liner 180 of the laminate 100a is peeled off to expose the first adhesive layer 130, and the laminate 100a and laminate 100c are bonded together so that the first adhesive layer 130 is in contact with the ink layer 140 of the laminate 100c, thereby obtaining an adhesive sheet 100 with a release liner (see Figure 13F, etc.). [Prior art documents] [Patent Documents]

[0011] [Patent Document 1] Japanese Patent Publication No. 2019-042955 [Overview of the Initiative] [Problems that the invention aims to solve]

[0012] However, in the conventional adhesive sheet 100 shown in Figure 12, a whitening phenomenon (silvering) is likely to occur, where the ink layer 140 appears whitish. For example, if the first adhesive layer 130 in the adhesive sheet 100 cannot adequately follow the irregularities on the media surface, tiny air pockets (air pockets p) will form in the areas where it cannot follow. In this case, when a user views the sheet from the outside, they will see not only the transparent substrate 120 and the first adhesive layer 130, but also the ink layer 140, i.e., the pattern formed by the ink, through the air pockets p (see arrow L2). For this reason, if air pockets p form at the interface between the first adhesive layer 130 and the ink layer 140, the reflection of light will change, which can cause silvering. When silvering occurs, the ink layer 140, which is visible from the outside on the transparent substrate 120 side, will have a different appearance than originally intended.

[0013] The present invention has been made in view of the above circumstances, and its object is to provide an adhesive sheet, an adhesive sheet with a release liner, a method for manufacturing an adhesive sheet, and a method for manufacturing an adhesive sheet with a release liner that can suppress the occurrence of silvering. [Means for solving the problem]

[0014] As a result of diligent research to achieve the above-mentioned objectives, the inventors of the present invention have found that an adhesive sheet comprising a transparent substrate, an ink layer provided on the surface of the transparent substrate, and a first adhesive layer in this order is appropriate, and have completed the present invention.

[0015] In other words, the present invention is as follows.

[0016] <1> Transparent substrate and An ink layer provided on the surface of the transparent substrate, This is an adhesive sheet comprising a first adhesive layer and a second adhesive layer in that order. <2> The first adhesive layer further includes a base material provided on the surface opposite to the ink layer, <1> This is the adhesive sheet described in [the document]. <3> The present invention further includes a second adhesive layer provided on the surface of the substrate material opposite to the first adhesive layer, <2> This is the adhesive sheet described in [the document]. <4> A core material is provided on the surface of the second adhesive layer opposite to the substrate material, A third adhesive layer is provided on the surface of the core material opposite to the second adhesive layer, This also includes, <3> This is the adhesive sheet described in [the document]. <5> A core material is provided on the surface of the first adhesive layer opposite to the ink layer, A second adhesive layer is provided on the surface of the core material opposite to the first adhesive layer, A base material is provided on the surface of the second adhesive layer opposite to the core material, The pressure-sensitive adhesive sheet according to <1>, further comprising a third pressure-sensitive adhesive layer provided on the surface of the base substrate opposite to the second pressure-sensitive adhesive layer. <6> A pressure-sensitive adhesive sheet with a release liner, wherein the pressure-sensitive adhesive sheet according to any one of <1> to <5> further comprises a release liner provided on the outermost surface on the side opposite to the transparent substrate. <7> (1) a step of forming an ink layer by applying an ink onto the surface of a transparent substrate; and (2) a step of forming a first pressure-sensitive adhesive layer on the surface of the ink layer opposite to the transparent substrate, to obtain a pressure-sensitive adhesive sheet at least comprising the transparent substrate, the ink layer provided on the surface of the transparent substrate, and the first pressure-sensitive adhesive layer in this order. This is a method for producing a pressure-sensitive adhesive sheet. <8> In the production method according to <7>, a step of obtaining a laminate (i) comprising the transparent substrate, the ink layer provided on the surface of the transparent substrate, and the first pressure-sensitive adhesive layer in this order through the step (1) and the step (2); (3) a step of preparing a laminate (ii) comprising a base substrate, a second pressure-sensitive adhesive layer, and a release liner in this order; (4) a step of bonding the laminate (i) and the laminate (ii) such that the first pressure-sensitive adhesive layer of the laminate (i) is in contact with the base substrate of the laminate (ii), to obtain a pressure-sensitive adhesive sheet with a release liner comprising the transparent substrate, the ink layer, the first pressure-sensitive adhesive layer, the base substrate, the second pressure-sensitive adhesive layer, and the release liner in this order; This is a method for producing a pressure-sensitive adhesive sheet with a release liner, comprising the above steps. <9> In the production method according to <7>, The step (2) is a step of forming the first pressure-sensitive adhesive layer on the surface of the ink layer or the base substrate, and then bonding the ink layer and the base substrate via the first pressure-sensitive adhesive layer, to obtain a laminate (iii) comprising the transparent substrate, the ink layer, the first pressure-sensitive adhesive layer, and the base substrate in this order, further, (3) a step of applying a pressure-sensitive adhesive onto the surface of the base substrate or the release liner to form a second pressure-sensitive adhesive layer, and then bonding the base substrate of the laminate (iii) and the release liner via the second pressure-sensitive adhesive layer, to obtain a pressure-sensitive adhesive sheet with a release liner comprising the transparent substrate, the ink layer, the first pressure-sensitive adhesive layer, the base substrate, the second pressure-sensitive adhesive layer, and the release liner in this order, This is a method for producing a pressure-sensitive adhesive sheet with a release liner, comprising the above steps. <10> In the production method described in <7>, The step (2) is (2-1) a step of preparing a laminate (iv) comprising a base substrate, a second pressure-sensitive adhesive layer, and a release liner in this order, (2-2) forming the first pressure-sensitive adhesive layer on the surface of the ink layer or the base substrate, and then bonding the ink layer and the base substrate of the laminate (iv) via the first pressure-sensitive adhesive layer, to obtain a pressure-sensitive adhesive sheet with a release liner comprising the transparent substrate, the ink layer, the first pressure-sensitive adhesive layer, the base substrate, the second pressure-sensitive adhesive layer, and the release liner in this order, This is a method for producing a pressure-sensitive adhesive sheet with a release liner, comprising the above steps. <11> In the production method described in <7>, The step (2) is a step of forming the first pressure-sensitive adhesive layer on the surface of the ink layer or the base substrate, and then bonding the ink layer and the base substrate via the first pressure-sensitive adhesive layer, to obtain a laminate (v) comprising the transparent substrate, the ink layer, the first pressure-sensitive adhesive layer, and the base substrate in this order, further, (3) A step of preparing a laminate (vi) containing a second adhesive layer and a release liner in this order, (4) A step of obtaining an adhesive sheet with a release liner, comprising the transparent substrate, the ink layer, the first adhesive layer, the substrate, the second adhesive layer, and the release liner, in this order, by bonding the base substrate of the laminate (v) and the second adhesive layer of the laminate (vi). This is a method for manufacturing an adhesive sheet with a release liner, including the following: <12> <7> In the manufacturing method described above, The above step (2) is, (2-1) A step of preparing a laminate (vii) comprising the first adhesive layer, a substrate, a second adhesive layer, and a release liner in this order, (2-2) A step of obtaining an adhesive sheet with a release liner, comprising the transparent substrate, the ink layer, the first adhesive layer, the base substrate, the second adhesive layer, and the release liner, in this order, by bonding the ink layer and the first adhesive layer of the laminate (vii). This is a method for manufacturing an adhesive sheet with a release liner, including the following: <13> <7> In the manufacturing method described above, The above step (2) is, (2-1) A step of preparing the first adhesive layer, (2-2) A step of preparing a laminate (viii) comprising a base material, a second adhesive layer, and a release liner in this order, (2-3) A step of obtaining an adhesive sheet with a release liner, comprising the transparent substrate, the ink layer, the first adhesive layer, the base substrate, the second adhesive layer, and the release liner, in this order, by bonding the ink layer and the base substrate of the laminate (viii) via the first adhesive layer. This is a method for manufacturing an adhesive sheet with a release liner, including the following: <14> <7> In the manufacturing method described above, The (2) step is a step of forming the first adhesive layer on the surface of the ink layer or the substrate, and then bonding the ink layer and the substrate via the first adhesive layer to obtain a laminate (ix) containing the transparent substrate, the ink layer, the first adhesive layer, and the substrate in this order. moreover, (3) A step of preparing a laminate (x) comprising a second adhesive layer, a core material, a third adhesive layer, and a release liner in this order, (4) A step of obtaining an adhesive sheet with a release liner, comprising the transparent substrate, the ink layer, the first adhesive layer, the substrate, the second adhesive layer, the core material, the third adhesive layer, and the release liner, in this order, by bonding the base material of the laminate (ix) and the second adhesive layer of the laminate (x). This is a method for manufacturing an adhesive sheet with a release liner, including the following: <15> <7> In the manufacturing method described above, The above step (2) is, (2-1) A step of preparing a laminate (xi) comprising the first adhesive layer, a core material, and a second adhesive layer in this order, (2-2) A step of preparing a laminate (xii) comprising a base material, a third adhesive layer, and a release liner in this order, (2-3) A step of obtaining an adhesive sheet with a release liner, comprising the transparent substrate having the ink layer, the laminate (xi), and the laminate (xii) in the order of the transparent substrate, the ink layer, the first adhesive layer of the laminate (xi), and the second adhesive layer of the laminate (xi) and the base material of the laminate (xii), such that the ink layer and the first adhesive layer of the laminate (xi) are in contact, and the second adhesive layer of the laminate (xi) and the base material of the laminate (xii) are in contact, This is a method for manufacturing an adhesive sheet with a release liner, including the following: [Effects of the Invention]

[0017] According to the present invention, it is possible to provide an adhesive sheet, an adhesive sheet with a release liner, a method for manufacturing an adhesive sheet, and a method for manufacturing an adhesive sheet with a release liner, which can suppress the occurrence of silvering. [Brief explanation of the drawing]

[0018] [Figure 1] Figure 1 is a schematic cross-sectional view of an adhesive sheet with a release liner according to the first embodiment. [Figure 2] Figure 2 is a process diagram of an example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 2A, 2B, 2C, 2D, 2E, and 2F are process diagrams showing each step of the manufacturing method. [Figure 3] Figure 3 is a process diagram of another example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 3A, 3B, 3C, and 3D are process diagrams showing each step of the manufacturing method. [Figure 4] Figure 4 is a process diagram of another example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 4A, 4B, 4C, 4D, and 4E are process diagrams showing each step of the manufacturing method. [Figure 5] Figure 5 is a process diagram of another example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 5A, 5B, 5C, 5D, 5E, and 5F are process diagrams showing each step of the manufacturing method. [Figure 6] Figure 6 is a process diagram of another example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 6A, 6B, 6C, 6D, 6E, and 6F are process diagrams showing each step of the manufacturing method. [Figure 7] Figure 7 is a process diagram of another example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 7A, 7B, 7C, 7D, 7E, 7F, and 7G are process diagrams showing each step of the manufacturing method. [Figure 8] Figure 8 is a schematic cross-sectional view of an adhesive sheet with a release liner according to the second embodiment. [Figure 9]Figure 9 is a process diagram of an example of a method for manufacturing an adhesive sheet with a release liner according to the second embodiment, and Figures 9A, 9B, 9C, 9D, 9E, and 9F are process diagrams showing each step of the manufacturing method. [Figure 10] Figure 10 is a schematic cross-sectional view of an adhesive sheet with a release liner according to the third embodiment. [Figure 11] Figure 11 is a process diagram of an example of a method for manufacturing an adhesive sheet with a release liner according to the third embodiment, and Figures 11A, 11B, 11C, 11D, 11E, 11F, and 11G are process diagrams showing each step of the manufacturing method. [Figure 12] Figure 12 is a schematic cross-sectional view showing an example of the configuration of a conventional adhesive sheet with a release liner. [Figure 13] Figure 13 is a process diagram of an example of a conventional method for manufacturing an adhesive sheet with a release liner, and Figures 13A, 13B, 13C, 13D, 13E, and 13F are process diagrams showing each step in the conventional method for manufacturing an adhesive sheet 100. [Modes for carrying out the invention]

[0019] The following describes in detail embodiments for carrying out the present invention (hereinafter simply referred to as "this embodiment"). This embodiment is illustrative for explaining the present invention and is not intended to limit the present invention to the following content. The present invention can be implemented by modifying it as appropriate within the scope of its gist.

[0020] Furthermore, identical elements in the drawings will be given the same reference numeral, and redundant explanations will be omitted. Unless otherwise specified, positional relationships such as top, bottom, left, and right will be based on those shown in the drawings. Moreover, the dimensional ratios in the drawings are not limited to those shown.

[0021] Furthermore, in this specification, terms marked with "abbreviated" indicate the meaning of the term without the "abbreviated" designation, within the scope of common technical knowledge for those skilled in the art, and shall also include the meaning of the term without the "abbreviated" designation.

[0022] The adhesive sheet according to this embodiment is an adhesive sheet comprising, in this order, a transparent substrate, an ink layer provided on the surface of the transparent substrate, and a first adhesive layer. In the adhesive sheet according to this embodiment, by providing the ink layer on the surface of the transparent substrate, the occurrence of air pockets between the transparent substrate and the ink layer can be suppressed. This makes it possible to obtain an adhesive sheet in which the occurrence of silvering is suppressed. In this specification, "sheet" also includes what is called "tape," etc., and examples include those with a substantially long shape, but are not limited to such shapes.

[0023] And a preferred example of a method for manufacturing such an adhesive sheet is: (1) A step of forming an ink layer by applying ink to the surface of a transparent substrate, (2) The process includes the step of forming a first adhesive layer on the surface of the ink layer opposite to the transparent substrate, One method for manufacturing an adhesive sheet is to obtain an adhesive sheet that includes, in this order, a transparent substrate, an ink layer provided on the surface of the transparent substrate, and a first adhesive layer.

[0024] In this regard, for example, in conventional adhesive sheets 110 and adhesive sheets with release liners 100 as shown in Figure 12, the first adhesive layer 130 is positioned between the transparent substrate 120 and the ink layer 140. Therefore, when a user views the ink layer 140, i.e., the characters, colors, figures, symbols, patterns, etc. (hereinafter collectively referred to as "patterns, etc.") formed with ink, they view the ink layer 140 through the transparent substrate 120 and the first adhesive layer 130 (see arrow L2). However, since air pockets p are generated at the interface between the first adhesive layer 130 and the ink layer 140, the user views the ink layer 140 through the air pockets p (see arrow L2 in Figure 12). For this reason, silvering occurs in conventional adhesive sheets 110.

[0025] On the other hand, as described above, the adhesive sheet according to this embodiment suppresses the occurrence of air pockets between the transparent substrate and the ink layer. Therefore, the user can clearly see the ink layer without passing through air pockets (see arrow L1 in Figure 1). In other words, the occurrence of silvering can be suppressed.

[0026] Thus, the adhesive sheet according to this embodiment can suppress the occurrence of silvering by providing at least an ink layer on the surface of the transparent substrate. Furthermore, this embodiment can take various variations. Various configurations can be taken for the adhesive sheet. Moreover, various methods can be taken for its manufacturing. Examples of these configurations are given below.

[0027] <Adhesive sheet and adhesive sheet with release liner according to the first embodiment>

[0028] (Adhesive sheet)

[0029] Figure 1 is a schematic cross-sectional view of an adhesive sheet with a release liner according to the first embodiment.

[0030] The adhesive sheet 10 according to the first embodiment is an adhesive sheet 10 that includes, in this order, at least a transparent substrate 11, an ink layer 12 provided on the surface of the transparent substrate 11, and a first adhesive layer 13. That is, the adhesive sheet 10 includes, in this order, at least a transparent substrate 11, an ink layer 12, and a first adhesive layer 13. The adhesive sheet with a release liner 1 is an adhesive sheet 10 in which a release liner 16 is attached to the surface of the second adhesive layer 15, which is the adhesive surface, and is stored in this state. In this specification, such an adhesive sheet with a release liner may also be referred to as an "adhesive sheet".

[0031] Furthermore, it is preferable that the adhesive sheet 10 further includes a base material 14 provided on the surface of the first adhesive layer 13 opposite to the ink layer 12. That is, it is preferable that the adhesive sheet 10 includes at least the transparent base material 11, the ink layer 12, the first adhesive layer 13, and the base material 14 in this order.

[0032] Furthermore, it is more preferable that the adhesive sheet 10 further includes a second adhesive layer 15 provided on the surface of the base material 14 opposite to the first adhesive layer 13. That is, it is preferable that the adhesive sheet 10 includes at least the transparent base material 11, the ink layer 12, the first adhesive layer 13, the base material 14, and the second adhesive layer 15 in this order.

[0033] Furthermore, the adhesive sheet 10 can be an adhesive sheet with a release liner 1, which further includes a release liner 16 provided on the outermost surface opposite to the transparent substrate 11. That is, the adhesive sheet with a release liner 1 includes the adhesive sheet 10 and a release liner 16 provided on the surface of the second adhesive layer. In this case, when using it, the release liner 16 is peeled off to expose the second adhesive layer 15. Then, the adhesive surface of the second adhesive layer 15 is attached to a predetermined location on the object (the object to which the adhesive sheet 10 is to be attached).

[0034] The following describes each component.

[0035] (Transparent base material)

[0036] As the transparent substrate 11, for example, a transparent protective film can be used. The material of the transparent substrate 11 can be one or more selected from the group consisting of polyester, polyolefin, polyvinyl chloride, polyurethane, acetylcellulose butyrate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polystyrene, polycarbonate, polymethylpentene, polysulfone, polyetheretherketone, polyethersulfone, polyamide, polyetherimide, polyimide, fluororesin, acrylic resin, norbornene resin, and cycloolefin resin. Examples of polyester include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of polyolefin include polyethylene and polypropylene.

[0037] Among these, the resin is preferably at least one of polyester, polyolefin, polyvinyl chloride, polyurethane, acrylic resin, and fluororesin, from the viewpoint of transparency, economy, and adhesion to the first adhesive layer 13, and more preferably at least one of polyvinyl chloride, acrylic resin, polyurethane, and fluororesin. The resin may also be a petrochemical-derived resin using petroleum as a starting material, or a carbon-neutral plant-derived resin such as sugarcane. For example, polyester derived from biomass raw materials, polyolefin derived from biomass raw materials, polyvinyl chloride derived from biomass raw materials, etc., can also be used.

[0038] The transparent substrate 11 may further contain additives, etc. The type of additive is not particularly limited, and known additives can be selected considering the application, etc. Examples of additives include antistatic agents, antioxidants, ultraviolet absorbers, light stabilizers, softeners, fillers, refractive index adjusters, etc.

[0039] Furthermore, although not shown in the figures, the layer structure of the transparent substrate 11 is not particularly limited and may be a single-layer structure consisting of only one layer, or a multilayer structure consisting of two or more layers. For example, the transparent substrate 11 may be a two-layer structure including a first substrate layer and a second substrate layer formed on the surface of the first substrate layer. The first substrate layer may contain one of the resins described above, and the second substrate layer may contain a resin different from that of the first substrate layer.

[0040] The total light transmittance of the transparent substrate 11 is not particularly limited, but is preferably 85% or higher. This provides sufficient transparency for the adhesive sheet 10 and maintains a higher level of visibility of the ink layer 12. This total light transmittance value can be measured, for example, using a haze meter (e.g., NDH 5000 haze meter manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K 7361:1997.

[0041] The average thickness of the transparent substrate 11 is not particularly limited, but is preferably 5 μm or more and 300 μm or less. The lower limit of this average thickness is more preferably 10 μm or more, and even more preferably 15 μm or more. The upper limit of this average thickness is more preferably 200 μm or less, even more preferably 150 μm or less, and even more preferably 100 μm or less. The average thickness is measured in accordance with JIS K 7130:1999, and refers to the arithmetic mean of the thickness measured at 10 equally spaced locations using a constant-pressure thickness measuring instrument.

[0042] The transparent substrate 11 may be subjected to surface treatment such as corona treatment, for example, to improve adhesion with the first adhesive layer 13. The surface treatment method and conditions are not particularly limited, and known methods and conditions can be adopted depending on the purpose.

[0043] (Ink layer)

[0044] The ink layer 12 can use inks used in inkjet printing, such as solvent-based inks, latex-based inks, and UV-curing inks.

[0045] Examples of solvent-based inks include SS21 (manufactured by Mimaki Engineering Co., Ltd.) and TrueVIS INK (manufactured by Roland DG Corporation). Examples of latex-based inks include HP873 (manufactured by Hewlett-Packard Corporation) and LX101 (manufactured by Mimaki Engineering Co., Ltd.). Examples of UV-curing inks include UltraChrome UV ink (manufactured by Seiko Epson Corporation), LUS-170 (manufactured by Mimaki Engineering Co., Ltd.), and UVgel 460 ink (manufactured by Canon Production Printing Systems Corporation).

[0046] Furthermore, the materials that can be used for the ink are not particularly limited, and examples include acrylic resins, vinyl chloride resins, vinyl chloride / vinyl acetate copolymers, urethane resins, acrylic urethane copolymers, and the like.

[0047] One suitable example is illustrated below. As the UV-curable ink, it is preferable to use an acrylic-based ink, for example. This further improves the curability of the UV-curable ink. Furthermore, when the first adhesive layer 13 is made of a material containing an acrylic-based adhesive, the affinity between the ink layer 12 and the first adhesive layer 13 is improved, and the adhesion between the ink layer 12 and the first adhesive layer 13 can be further improved.

[0048] Examples of acrylic materials contained in acrylic inks include (meth)acrylic acid, (meth)acrylate, and polymers containing at least one of these (e.g., dimers, trimers, oligomers, prepolymers, etc.). Examples of (meth)acrylate include monofunctional (meth)acrylate and polyfunctional (meth)acrylate.

[0049] Specific examples of monofunctional (meth)acrylates include, for example, isoamyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, isomirsutyl (meth)acrylate, isostearyl (meth)acrylate, 2-ethylhexyl-diglycol (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-(meth)acryloyloxyethylhexahydrophthalic acid, butoxyethyl (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, and methoxy Examples include polyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, phenoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalic acid, t-butylcyclohexyl (meth)acrylate, and the like.

[0050] Specific examples of polyfunctional (meth)acrylates include, for example, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, dimethylol-tricyclodecane di(meth)acrylate, bisphenol A PO adduct di(meth)acrylate, hydroxypivalate neopentyl glycol di(meth)acrylate, and polytetramethylene glycol Examples include bifunctional (meth)acrylates such as chol di(meth)acrylate, polyethylene glycol diacrylate, and tripropylene glycol diacrylate; trifunctional (meth)acrylates such as trimethylolpropane tri(meth)acrylate and pentaerythritol tri(meth)acrylate; trifunctional or more (meth)acrylates such as pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, glycerin propoxytri(meth)acrylate, and pentaerythritol ethoxytetra(meth)acrylate; oligomers having a (meth)acryloyl group, including polyester acrylate oligomers, and modified products thereof. Specific examples of such modified products include, for example, ethylene oxide-modified (EO-modified) acrylates with an inserted ethylene oxide group, and propylene oxide-modified (PO-modified) acrylates with an inserted propylene oxide group.

[0051] Acrylic inks may also contain other polymerizable components (e.g., non-acrylic components (non-acrylic polymer components)) with the acrylic materials described above. "Non-acrylic components" here refers to components that do not have an acrylic structure. Examples of non-acrylic polymer components include carboxyl group-containing monomers such as acrylonitrile, styrene, styrene derivatives, itaconic acid, maleic acid, maleic anhydride, maleic acid monoalkyl esters, citraconic acid, citraconic anhydride, and citraconic acid monoalkyl esters.

[0052] For example, in the case of UV-curable ink, the ink is ejected onto at least a portion of the surface of the transparent substrate 11 by an inkjet method, and then cured by UV irradiation. This allows an ink layer 12 to be formed on the surface of the transparent substrate 11.

[0053] UV-curing inks may be used individually or in combination of two or more types.

[0054] The ink layer 12 may contain components other than those described above (other components). Examples of such components include: discharge stabilizers such as silicone; non-polymerizable solvents; various colorants such as pigments and dyes; fillers; photopolymerization initiators; near-infrared absorbers; stabilizers such as antioxidants and thermal polymerization inhibitors; surfactants such as leveling agents, defoamers, thickeners, settling inhibitors, pigment dispersants, antistatic agents, and anti-fogging agents; waxes; slip agents, etc.

[0055] The shape, size, and pattern of the ink layer 12 are not particularly limited, and any desired shape, size, etc., can be selected. Examples of the shape of the ink layer 12 include those that display characters, colors, figures, symbols, pictures, etc. (patterns, etc.). The ink layer 12 may also be, for example, a solid print layer using a single color of ink.

[0056] The thickness of the ink layer 12 is not particularly limited, but is preferably 0.5 μm or more and 100 μm or less. The lower limit of this thickness is more preferably 1 μm or more. The upper limit of this thickness is more preferably 30 μm or less.

[0057] (First adhesive layer)

[0058] The form of the first adhesive layer 13 is not particularly limited and includes solvent-type adhesives, water-based emulsion-type adhesives, hot-melt type adhesives, and the like.

[0059] Furthermore, the materials of the adhesives that can be used are not particularly limited, and examples include at least one selected from the group consisting of acrylic adhesives, rubber adhesives, urethane adhesives, polyester adhesives, and silicone adhesives.

[0060] One suitable example is given. As acrylic adhesives, for example, solvent-based acrylic adhesives, water-based emulsion-type acrylic adhesives, hot-melt type acrylic adhesives, etc., can be used. As synthetic rubber adhesives, solvent-based synthetic rubber adhesives, water-based emulsion-type synthetic rubber adhesives, hot-melt type synthetic rubber adhesives, etc., can be used.

[0061] The first adhesive layer 13 may contain a tackifying resin (sometimes referred to as "tackifier," etc.). The tackifying resin can be appropriately selected depending on the application of the adhesive sheet 10. Examples include rosin resins, terpene phenol resins, terpene resins, aromatic hydrocarbon-modified terpene resins, aliphatic petroleum resins, aromatic petroleum resins, hydrogenated petroleum resins, coumarone-indene resins, styrene resins, phenolic resins, xylene resins, and the like.

[0062] The first adhesive layer 13 may contain additives as needed. Examples of additives include softeners, heat and light stabilizers, antioxidants, and crosslinking agents. Examples of softeners include process oils, liquid rubber, and plasticizers. Examples of heat and light stabilizers include benzophenone-based stabilizers, benzotriazole-based stabilizers, and hindered amine-based stabilizers. Examples of antioxidants include anilide-based antioxidants, phenol-based antioxidants, phosphite-based antioxidants, and thioester-based antioxidants.

[0063] Furthermore, the first adhesive layer 13 is preferably transparent. The total light transmittance of the first adhesive layer 13 is not particularly limited, but is preferably 85% or higher. This provides sufficient transparency for the adhesive sheet 10 and maintains a higher level of visibility of the ink layer 12. This total light transmittance value can be measured, for example, using a haze meter (for example, the NDH 5000 haze meter manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K 7361:1997.

[0064] The thickness of the first adhesive layer 13 is not particularly limited, but is preferably 5 μm or more and 50 μm or less. The lower limit of this thickness is more preferably 10 μm or more, and even more preferably 15 μm or more. The upper limit of this thickness is more preferably 50 μm or less, even more preferably 40 μm or less, even more preferably 35 μm or less, and even more preferably 30 μm or less.

[0065] (Substrate material)

[0066] Examples of materials for the base material 14 include polyester, polyolefin, polyvinyl chloride, polyurethane, acrylic resin, synthetic paper, and paper. The layer structure of the base material 14 is not particularly limited and may be a single-layer structure consisting of only one layer, or a multilayer structure consisting of two or more layers. In the case of a multilayer structure, it may be composed only of the materials mentioned above, or other resins or metal foils may be laminated to the materials mentioned above.

[0067] Furthermore, although not shown in the figures, another ink layer may be provided on the surface of the base material 14 opposite to the first adhesive layer 13. For example, by providing another ink layer, it is possible to prevent the color or pattern of the object from showing through (color transparency). For example, in the first embodiment (see Figure 1), another ink layer is provided on the surface of the base material 14 opposite to the surface facing the first adhesive layer 13. That is, in the first embodiment, in a cross-sectional view, the layers can be laminated in the order of transparent base material 11 / ink layer 12 / first adhesive layer 13 / base material 14 / another ink layer (not shown) / second adhesive layer 15. For example, when a user views the ink layer 12 from the transparent base material 11 side of the adhesive sheet 10 in the direction of arrow L1, it is possible to prevent the color or pattern of the object from showing through (color transparency).

[0068] The thickness of the substrate material 14 is not particularly limited, but is preferably 5 μm or more and 300 μm or less. The lower limit of this thickness is more preferably 10 μm or more, and even more preferably 20 μm or more. The upper limit of this thickness is more preferably 200 μm or less, and even more preferably 100 μm or less.

[0069] (Second adhesive layer)

[0070] The second adhesive layer 15 may employ the materials and conditions described for the first adhesive layer 13. The components, shape, and size of the first adhesive layer 13 and the second adhesive layer 15 may be the same or different. The second adhesive layer 15 may or may not have high transparency. In other words, the second adhesive layer 15 may or may not be transparent. Therefore, depending on the application of the adhesive sheet 10, the second adhesive layer 15 may contain fillers, pigments, etc. For example, by including fillers and / or pigments in the adhesive layer (the second adhesive layer 15 in the first embodiment), which is the adhesive surface of the adhesive sheet 10 that adheres to the object, it is possible to prevent the color or pattern of the object from showing through (color transparency).

[0071] The thickness of the second adhesive layer 15 is not particularly limited, but is preferably 5 μm or more and 80 μm or less. The lower limit of this thickness is more preferably 10 μm or more, and even more preferably 15 μm or more. The upper limit of this thickness is more preferably 60 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, and even more preferably 30 μm or less.

[0072] (Removable liner)

[0073] The material of the release liner 16 is not particularly limited, and known materials can be used. Examples of materials for the release liner 16 include resin materials and paper. Examples of resin materials include polyester, polyolefin, polyvinyl chloride, acetylcellulose butyrate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polystyrene, polycarbonate, polymethylpentene, polysulfone, polyetheretherketone, polyethersulfone, polyetherimide, polyamide, polyimide, fluororesin, acrylic resin, norbornene resin, and cycloolefin resin. Examples of polyester include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of polyolefin include polyethylene and polypropylene. Examples of paper include synthetic paper, fine paper, kraft paper, glassine paper, and laminated paper.

[0074] The thickness of the release liner 16 is not particularly limited, but is preferably between 10 μm and 300 μm. The lower limit of the thickness is more preferably 20 μm or more. The upper limit of the thickness is more preferably 250 μm or less. This thickness is the average thickness measured in accordance with JIS K 7130:1999, and refers to, for example, the arithmetic mean of the thickness measured at 10 equally spaced locations using a constant-pressure thickness measuring instrument.

[0075] <Method for manufacturing an adhesive sheet and an adhesive sheet with a release liner according to the first embodiment>

[0076] Furthermore, as a method for manufacturing the adhesive sheet 10 and the adhesive sheet 1 with a release liner according to the first embodiment, a method of appropriately laminating each layer can be employed, but several preferred variations are exemplified below. The adhesive sheet 10 and the adhesive sheet 1 with a release liner can be manufactured, for example, by the following manufacturing method.

[0077] (See Manufacturing Method 1-1, Figure 2)

[0078] Figure 2 is a process diagram of an example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 2A, 2B, 2C, 2D, 2E, and 2F are process diagrams showing each step of the manufacturing method.

[0079] The manufacturing method shown in Figure 2 is: (1) A step of forming an ink layer 12 by applying ink to the surface of a transparent substrate 11, (2) The process includes the step of forming a first adhesive layer 13 on the surface of the ink layer 12 opposite to the transparent substrate 11. This is a method for manufacturing an adhesive sheet, which provides an adhesive sheet 10 comprising, in this order, a transparent substrate 11, an ink layer 12 provided on the surface of the transparent substrate 11, and a first adhesive layer 13.

[0080] More specifically, the manufacturing method shown in Figure 2 is as follows: The process of obtaining a laminate (i) comprising a transparent substrate 11, an ink layer 12 provided on the surface of the transparent substrate 11, and a first adhesive layer 13 in that order by the above steps (1) and (2), (3) A step of preparing a laminate (ii) comprising a base material 14, a second adhesive layer 15, and a release liner 16 in this order, (4) It is more preferable to have a manufacturing method that includes the step of bonding laminate (i) and laminate (ii) together such that the first adhesive layer 13 of laminate (i) and the base material 14 of laminate (ii) are in contact, thereby obtaining an adhesive sheet 1 with a release liner that includes a transparent base material 11, an ink layer 12, the first adhesive layer 13, the base material 14, the second adhesive layer 15, and a release liner 16 in this order. By such a manufacturing method, the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured.

[0081] The following describes each step shown in Figure 2 in detail.

[0082] First, (1) a step is performed to form an ink layer 12 by applying ink to the surface of the transparent substrate 11. This results in a laminate having the transparent substrate 11 and the ink layer 12 provided on its surface. For example, an inkjet printer can be used to apply the ink (see Figures 2A and 2B). When forming the ink layer 12 on the surface of the transparent substrate 11 with an inkjet printer, a protective adhesive film may be applied to the surface of the transparent substrate 11 opposite to the printed surface (i.e., the surface on which the ink layer 12 is formed) to protect the transparent substrate 11.

[0083] Then, (2) a step is performed to form a first adhesive layer 13 on the surface of the ink layer 12 opposite to the transparent substrate 11 (see Figures 2B and 2C).

[0084] Step (2) only requires forming a first adhesive layer 13 on the surface of the ink layer 12. In the first embodiment, the step of forming the first adhesive layer 13 in step (2) also includes (a) a step of applying an adhesive composition to the surface of the ink layer 12 to form the first adhesive layer 13, and (b) a step of applying an adhesive composition to the surface of another component (such as a base material 14 or a disposable release liner) to form the first adhesive layer 13, and then bonding the first adhesive layer 13 to the surface of the ink layer 12. For example, in the case of Figure 2, it is also possible to prepare a two-layer laminate having not only the first adhesive layer 13 but also a disposable release liner 17, and then bonding the first adhesive layer 13 and the ink layer 12 (see Figures 2B and 2C). Therefore, the first adhesive layer 13 is not necessarily limited to being prepared and used alone, but may be an adhesive layer provided on the outermost surface of any two or more laminates (see, for example, the descriptions of laminate (i) in Figure 2, laminate (iii) in Figure 3, laminate (v) in Figure 5, laminate (vii) in Figure 6, etc., which will be described later).

[0085] In the case of Figure 2, the first adhesive layer 13 can be formed by applying an adhesive composition to the surface of a disposable release liner 17 that is discarded during the manufacturing process (see Figure 2B). This release liner 17 is a disposable release liner that is discarded during the manufacturing process. A laminate (i) can be obtained by bonding the first adhesive layer 13 of a laminate (not shown) having the release liner 17 and the first adhesive layer 13 to the ink layer 12. After that, the first adhesive layer 13 can be exposed by peeling off the release liner 17.

[0086] The adhesive composition may contain the adhesive types and materials described above. Furthermore, it may contain organic solvents or water for dilution. Examples of organic solvents include alcohols (methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-methyl-1-propanol, 2-butanol, 2-methyl-2-propanol, diacetone alcohol, benzyl alcohol, etc.), ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.), ethers (diethyl ether, dioxane, tetrahydrofuran, etc.), cellosolves (methyl cellosolve, ethyl cellosolve, etc.), esters (ethyl acetate, n-butyl acetate, ethyl butyrate, n-butyl glycolate, diethylene glycol monoacetate, etc.), halogenated hydrocarbons (chloroform, dichloromethane, tetrachloroethylene, carbon tetrachloride, etc.), and hydrocarbons (n-hexane, cyclohexane, toluene, xylene, Solvesso, etc.). Furthermore, if the adhesive composition contains an organic solvent or water, it is preferable to include a step of drying the applied adhesive composition in order to form an adhesive layer (for example, the first adhesive layer 13 or the second adhesive layer 15 described later).

[0087] Specific examples of components of the adhesive composition include, for example, a composition containing at least one selected from the group consisting of acrylic adhesives, rubber adhesives, urethane adhesives, polyester adhesives, and silicone adhesives, and the solvent described above. Furthermore, the composition may also contain the additives described above (softeners, heat and light stabilizers, antioxidants, crosslinking agents, etc.) as needed.

[0088] Next, the ink layer 12 of the laminate 1a and the first adhesive layer 13 on the release liner 17 are bonded together to obtain a laminate (i) having the transparent substrate 11, the ink layer 12, the first adhesive layer 13, and the release liner 17 in this order (see Figure 2C).

[0089] Meanwhile, (3) a step is performed to prepare a laminate (ii) comprising a base material 14, a second adhesive layer 15, and a release liner 16 in this order (see Figures 2D and 2E). For example, the second adhesive layer 15 is formed by applying an adhesive composition to the surface of the release liner 16. Then, by bonding the second adhesive layer 15 to the base material 14, a laminate (ii) having the base material 14, the second adhesive layer 15, and the release liner 16 in this order is obtained.

[0090] The order of steps (1) and (2) and step (3) described above is not particularly limited, as long as it does not contradict their function, and they can be performed in any order. Therefore, it is also possible to prepare laminate (i) by steps (1) and (2), and to prepare laminate (ii) by step (3).

[0091] Then, (4) the process of bonding laminate (i) and laminate (ii) together so that the first adhesive layer 13 of laminate (i) and the base material 14 of laminate (ii) are in contact is performed to obtain an adhesive sheet 1 with a release liner that includes a transparent base material 11, an ink layer 12, the first adhesive layer 13, the base material 14, the second adhesive layer 15, and a release liner 16 in this order (see Figure 2F). For example, the first adhesive layer 13 is exposed by peeling off the disposable release liner 17 of laminate (i), and laminate (i) and laminate (ii) are laminated together so that the first adhesive layer 13 of laminate (i) and the base material 14 of laminate (ii) are in contact. This makes it possible to manufacture an adhesive sheet 1 with a release liner, which includes a transparent substrate 11, an ink layer 12, a first adhesive layer 13, a base substrate 14, a second adhesive layer 15, and a release liner 16 in this order.

[0092] As described above, when laminate (i) has a disposable release liner 17, the laminate (i) can be bonded to the substrate 14 by peeling off the release liner 17 to expose the first adhesive layer 13.

[0093] Furthermore, the manufacturing method 1-1 illustrated in Figure 2 is, A step of obtaining a laminate 1a including a transparent substrate 11 and an ink layer 12 by applying ink to the surface of a transparent substrate 11 to form an ink layer 12, A step of obtaining a laminate (i) comprising, at least in this order, a transparent substrate 11, an ink layer 12 provided on the surface of the transparent substrate 11, the first adhesive layer 13, and a disposable release liner 17, by forming a first adhesive layer 13 on the surface of the ink layer 12. A step of preparing a laminate (ii) comprising a base material 14, a second adhesive layer 15, and a release liner 16 in this order, By peeling off the disposable release liner 17 of laminate (i) and bonding laminate (i) and laminate (ii) together so that the first adhesive layer 13 and the base material 14 of laminate (ii) are in contact, the transparent substrate 11 It can also be described as a method for manufacturing an adhesive sheet with a release liner, which includes the step of obtaining an adhesive sheet with a release liner 1 comprising, in this order, an ink layer 12, a first adhesive layer 13, a base material 14, a second adhesive layer 15, and a release liner 16.

[0094] As is clear from the above, the adhesive sheet 10 and the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured by manufacturing method 1-1.

[0095] (See Manufacturing Method 1-2, Figure 3)

[0096] Figure 3 is a process diagram of another example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 3A, 3B, 3C, and 3D are process diagrams showing each step of the manufacturing method.

[0097] The manufacturing method shown in Figure 3 is: (1) A step of forming an ink layer 12 by applying ink to the surface of a transparent substrate 11, (2) The process includes the step of forming a first adhesive layer 13 on the surface of the ink layer 12 opposite to the transparent substrate 11. This is a method for manufacturing an adhesive sheet, which provides an adhesive sheet 10 comprising, in this order, a transparent substrate 11, an ink layer 12 provided on the surface of the transparent substrate 11, and a first adhesive layer 13. As mentioned above, the step of forming the first adhesive layer 13 in step (2) also includes steps such as (a) applying an adhesive composition to the surface of the ink layer 12 to form the first adhesive layer 13, and (b) applying an adhesive composition to the surface of another component (such as a base substrate 14 or a disposable release liner) to form the first adhesive layer 13, and then bonding the first adhesive layer 13 to the surface of the ink layer 12.

[0098] More specifically, the manufacturing method shown in Figure 3 is: The above step (2) is a step in which a first adhesive layer 13 is formed on the surface of the ink layer 12 or the base substrate 14, and then the ink layer 12 and the base substrate 14 are bonded together via the first adhesive layer 13 to obtain a laminate (iii) containing the transparent substrate 11, the ink layer 12, the first adhesive layer 13, and the base substrate 14 in this order. moreover, (3) It is more preferable to have a manufacturing method that includes the step of applying an adhesive composition to the surface of the base material 14 or the release liner 16 to form a second adhesive layer 15, and then bonding the base material 14 of the laminate (iii) and the release liner 16 via the second adhesive layer 15 to obtain an adhesive sheet 1 with a release liner containing the transparent base material 11, the ink layer 12, the first adhesive layer 13, the base material 14, the second adhesive layer 15, and the release liner 16 in this order. By such a manufacturing method, the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured.

[0099] Furthermore, the order of steps (1), (2), and (3) described above is not particularly limited, and they can be performed in any order, as long as it does not contradict their function.

[0100] The following describes each step shown in Figure 3 in detail.

[0101] First, (1) an ink layer 12 is formed by applying ink to the surface of the transparent substrate 11 (see Figures 3A and 3B). This results in a laminate 1a having the transparent substrate 11 and the ink layer 12 provided on its surface. The formation of the ink layer 12 can be appropriately carried out using the method described in (Manufacturing Method 1-1) above. For example, the ink layer 12 can be formed on the surface of the transparent substrate 11 using the inkjet printer described above.

[0102] Then, (2) a first adhesive layer 13 is formed on the surface of the ink layer 12 opposite to the transparent substrate 11, and then the ink layer 12 and the first adhesive layer 13 are bonded together (see Figures 3B and 3C). Specifically, this (2) step is a step in which, after forming the first adhesive layer 13 on the surface of the ink layer 12 or the substrate 14, the ink layer 12 and the substrate 14 are bonded together via the first adhesive layer 13 to obtain a laminate (iii) containing the transparent substrate 11, the ink layer 12, the first adhesive layer 13, and the substrate 14 in this order.

[0103] The method for forming the first adhesive layer 13 on the surface of the ink layer 12 or the substrate 14 can be appropriately adopted from the method described in (Manufacturing Method 1-1) above. For example, the first adhesive layer 13 can be formed by applying the above-mentioned adhesive composition to the surface of the ink layer 12 or the substrate 14.

[0104] If an adhesive composition is applied to the surface of the ink layer 12 to form a first adhesive layer 13 on the ink layer 12, a laminate (iii) can be obtained by bonding this first adhesive layer 13 to the substrate 14. Alternatively, if an adhesive composition is applied to the surface of the substrate 14 to form a first adhesive layer 13 on the substrate 14, a laminate (iii) can be obtained by bonding this first adhesive layer 13 to the ink layer 12.

[0105] The formation of the first adhesive layer 13 in step (2) can be carried out without using a disposable release liner during the manufacturing process. This is because in step (2), the first adhesive layer 13 can be formed by directly applying the adhesive composition onto the surface of the ink layer 12 or the substrate 14. Of course, the first adhesive layer 13 may also be formed using a disposable release liner. When forming the first adhesive layer 13 using a disposable release liner, the first adhesive layer 13 can be formed by applying the adhesive composition onto the surface of the release liner.

[0106] Furthermore, (3) an adhesive composition is applied to the surface of the base material 14 or the release liner 16 to form a second adhesive layer 15, and then the base material 14 of the laminate (iii) and the release liner 16 are bonded together via the second adhesive layer 15 to obtain an adhesive sheet 1 with a release liner containing the transparent base material 11, the ink layer 12, the first adhesive layer 13, the base material 14, the second adhesive layer 15, and the release liner 16 in this order. (3) By performing this step, an adhesive sheet 1 with a release liner having a release liner 16 can be manufactured.

[0107] The formation of the second adhesive layer 15 in step (3) can be carried out without using a disposable release liner during the manufacturing process. This is because in step (3), the second adhesive layer 15 can be formed by directly applying the adhesive composition onto the surface of the substrate 14 or the release liner 16. In this way, it is possible to manufacture the adhesive sheet 1 with a release liner according to the first embodiment.

[0108] Furthermore, the manufacturing method 1-2 illustrated in Figure 3 is, A step of obtaining a laminate 1a including a transparent substrate 11 and an ink layer 12 by applying ink to the surface of a transparent substrate 11 to form an ink layer 12, The process of obtaining a laminate (iii) comprising, at least in this order, a transparent substrate 11, an ink layer 12 provided on the surface of the transparent substrate 11, a first adhesive layer 13, and a base substrate 14, by further forming a first adhesive layer 13 and a base substrate 14 on the surface of the ink layer 12 in this order, A step of forming a second adhesive layer 15 on the surface of the release liner 16 to obtain a laminate (not shown) having a laminate of the second adhesive and the release liner 16, The method for manufacturing an adhesive sheet with a release liner can also be described as a step of laminating a second adhesive layer 15 to a base material 14 of a laminate (iii) to obtain an adhesive sheet with a release liner 1 comprising a transparent base material 11, an ink layer 12, a first adhesive layer 13, a base material 14, a second adhesive layer 15, and a release liner 16 in this order.

[0109] As is clear from the above, the adhesive sheet 10 and the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured by manufacturing method 1-2.

[0110] (See Manufacturing Method 1-3, Figure 4)

[0111] Figure 4 is a process diagram of another example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 4A, 4B, 4C, 4D, and 4E are process diagrams showing each step of the manufacturing method.

[0112] The manufacturing method shown in Figure 4 is: (1) A step of forming an ink layer 12 by applying ink to the surface of a transparent substrate 11, (2) The process includes the step of forming a first adhesive layer 13 on the surface of the ink layer 12 opposite to the transparent substrate 11. This is a method for manufacturing an adhesive sheet, which provides an adhesive sheet 10 comprising, in this order, a transparent substrate 11, an ink layer 12 provided on the surface of the transparent substrate 11, and a first adhesive layer 13. As mentioned above, the step of forming the first adhesive layer 13 in step (2) also includes steps such as (a) applying an adhesive composition to the surface of the ink layer 12 to form the first adhesive layer 13, and (b) applying an adhesive composition to the surface of another component (such as a base substrate 14 or a disposable release liner) to form the first adhesive layer 13, and then bonding the first adhesive layer 13 to the surface of the ink layer 12.

[0113] More specifically, the manufacturing method shown in Figure 4 is: The above step (2) is, (2-1) A step of preparing a laminate (iv) comprising a base material 14, a second adhesive layer 15, and a release liner 16 in this order, (2-2) It is more preferable to have a manufacturing method that includes the step of forming a first adhesive layer 13 on the surface of the ink layer 12 or the base substrate 14, and then bonding the ink layer 12 and the base substrate 14 of the laminate (iv) via the first adhesive layer 13 to obtain an adhesive sheet 1 with a release liner that includes the transparent substrate 11, the ink layer 12, the first adhesive layer 13, the base substrate 14, the second adhesive layer 15, and the release liner 16 in this order. By such a manufacturing method, the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured.

[0114] Furthermore, the order of steps (1), (2), (2-1), and (2-2) described above is not particularly limited, and they can be performed in any order, as long as it does not contradict their function.

[0115] The following describes each step shown in Figure 4 in detail.

[0116] First, (1) an ink layer 12 is formed by applying ink to the surface of the transparent substrate 11 (see Figures 4A and 4B). This results in a laminate 1a having the transparent substrate 11 and the ink layer 12 provided on its surface. The formation of the ink layer 12 can be appropriately carried out using the methods described above (Manufacturing Methods 1-1 to 1-2). For example, the ink layer 12 can be formed on the surface of the transparent substrate 11 using the inkjet printer described above.

[0117] Next, as step (2), first, a step is performed to prepare a laminate (iv) which includes (2-1) a base material 14, a second adhesive layer 15, and a release liner 16 in that order (see Figures 4C and 4D). The laminate (iv) can be obtained, for example, by applying an adhesive composition to the surface of the base material 14 or the release liner 16 to form the second adhesive layer 15, and then bonding the base material 14 and the release liner 16 together via the second adhesive layer 15. The application and formation of the second adhesive layer 15 can be appropriately carried out using the methods described in (Manufacturing Methods 1-1 to 1-2) above.

[0118] Then, (2-2) after forming a first adhesive layer 13 on the surface of the ink layer 12 or the base substrate 14, the ink layer 12 and the base substrate 14 of the laminate (iv) are bonded together via the first adhesive layer 13, thereby obtaining an adhesive sheet 1 with a release liner that includes the transparent substrate 11, the ink layer 12, the first adhesive layer 13, the base substrate 14, the second adhesive layer 15, and the release liner 16 in this order (see Figures 4B, 4D, and 4E). The application and formation of the first adhesive layer 13 can be appropriately carried out using the methods described above (Manufacturing Methods 1-1 to 1-2).

[0119] Furthermore, the manufacturing methods 1-3 illustrated in Figure 4 are as follows: A step of obtaining a laminate 1a including a transparent substrate 11 and an ink layer 12 by applying ink to the surface of a transparent substrate 11 to form an ink layer 12, A step of preparing a laminate (iv) comprising a base material 14, a second adhesive layer 15, and a release liner 16 in this order, The method for manufacturing an adhesive sheet with a release liner 1 can also be described as a step of forming a first adhesive layer 13 on the surface of the ink layer 12 or the base substrate 14, and then bonding the ink layer 12 and the base substrate 14 of the laminate (iv) via the first adhesive layer 13 to obtain an adhesive sheet with a release liner 1 that includes, in this order, a transparent substrate 11, an ink layer 12, a first adhesive layer 13, a base substrate 14, a second adhesive layer 15, and a release liner 16.

[0120] As is clear from the above, the adhesive sheet 10 and the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured by manufacturing methods 1-3.

[0121] (See Manufacturing Method 1-4, Figure 5)

[0122] Figure 5 is a process diagram of another example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 5A, 5B, 5C, 5D, 5E, and 5F are process diagrams showing each step of the manufacturing method.

[0123] The manufacturing method shown in Figure 5 is: (1) A step of forming an ink layer 12 by applying ink to the surface of a transparent substrate 11, (2) The process includes the step of forming a first adhesive layer 13 on the surface of the ink layer 12 opposite to the transparent substrate 11. This is a method for manufacturing an adhesive sheet, which provides an adhesive sheet 10 comprising, in this order, a transparent substrate 11, an ink layer 12 provided on the surface of the transparent substrate 11, and a first adhesive layer 13. As mentioned above, the step of forming the first adhesive layer 13 in step (2) also includes steps such as (a) applying an adhesive composition to the surface of the ink layer 12 to form the first adhesive layer 13, and (b) applying an adhesive composition to the surface of another component (such as a base substrate 14 or a disposable release liner) to form the first adhesive layer 13, and then bonding the first adhesive layer 13 to the surface of the ink layer 12.

[0124] More specifically, the manufacturing method shown in Figure 5 is: The above step (2) is a step in which a first adhesive layer 13 is formed on the surface of the ink layer 12 or the base substrate 14, and then the ink layer 12 and the base substrate 14 are bonded together via the first adhesive layer 13 to obtain a laminate (v) containing the transparent substrate 11, the ink layer 12, the first adhesive layer 13, and the base substrate 14 in this order. moreover, (3) A step of preparing a laminate (vi) containing the second adhesive layer 15 and the release liner 16 in this order, (4) It is more preferable to have a manufacturing method that includes the step of bonding the base material 14 of the laminate (v) and the second adhesive layer 15 of the laminate (vi) together to obtain an adhesive sheet 1 with a release liner that includes the transparent base material 11, the ink layer 12, the first adhesive layer 13, the base material 14, the second adhesive layer 15, and the release liner 16 in this order. By such a manufacturing method, the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured.

[0125] Furthermore, the order of steps (1), (2), (3), and (4) described above is not particularly limited, and they can be performed in any order, as long as it does not contradict their function.

[0126] The following describes each step shown in Figure 5 in detail.

[0127] First, (1) an ink layer 12 is formed by applying ink to the surface of the transparent substrate 11 (see Figures 5A and 5B). This results in a laminate 1a having the transparent substrate 11 and the ink layer 12 provided on its surface. The formation of the ink layer 12 can be appropriately carried out using the methods described above (Manufacturing Methods 1-1 to 1-3). For example, the ink layer 12 can be formed on the surface of the transparent substrate 11 using the inkjet printer described above.

[0128] Then, as step (2), a first adhesive layer 13 is formed on the surface of the ink layer 12 or the base substrate 14, and then the ink layer 12 and the base substrate 14 are bonded together via the first adhesive layer 13 to obtain a laminate (v) containing the transparent substrate 11, the ink layer 12, the first adhesive layer 13, and the base substrate 14 in this order (see Figures 5B and 5C). The coating and formation of the first adhesive layer 13 can be appropriately carried out using the methods described above (Manufacturing Methods 1-1 to 1-3).

[0129] Furthermore, (3) a step is performed to prepare a laminate (vi) which includes the second adhesive layer 15 and the release liner 16 in this order. The laminate (vi) prepared in this step only needs to include at least the second adhesive layer 15 and the release liner 16. For example, the second adhesive layer 15 can be formed by applying an adhesive composition to the surface of a disposable release liner 171 (see Figures 5D and 5E). The release liner 171 is a disposable release liner that is discarded during the manufacturing process. When laminating the laminate (vi) with the laminate (v), the second adhesive layer 15 can be exposed by peeling off the disposable release liner 171 of the laminate (vi).

[0130] Furthermore, the application and formation of the second adhesive layer 15 can be appropriately carried out using the methods described in (Manufacturing Methods 1-1 to 1-3) above. In this embodiment, the adhesive composition may be applied to the surface of the disposable release liner 171 to form the second adhesive layer 15 on that surface, and then the release liner 16 may be bonded to it to create a laminate (vi). However, it is preferable to apply the adhesive composition to the surface of the release liner 16 to form the second adhesive layer 15 on that surface, and then the disposable release liner 171 may be bonded to it to create a laminate (vi).

[0131] Then, (4) the process of obtaining an adhesive sheet 1 with a release liner, which includes a transparent substrate 11, an ink layer 12, a first adhesive layer 13, a substrate 14, a second adhesive layer 15, and a release liner 16 in this order, is performed by bonding the base substrate 14 of the laminate (v) and the second adhesive layer 15 of the laminate (vi). As described above, if the laminate (vi) has a disposable release liner 171, the release liner 171 can be peeled off to expose the second adhesive layer 15, and then the base substrate 14 and the second adhesive layer 15 can be bonded together. Furthermore, it is preferable that the peeling force between the second adhesive layer 15 and the release liner 16 is greater than the peeling force between the second adhesive layer 15 and the disposable release liner 171. Here, peeling force means the force required to peel the release liner from the adhesive layer. A greater peeling force means that it is more difficult to peel off.

[0132] Furthermore, the manufacturing methods 1-4 illustrated in Figure 5 are as follows: A step of obtaining a laminate 1a including a transparent substrate 11 and an ink layer 12 by applying ink to the surface of a transparent substrate 11 to form an ink layer 12, A step of obtaining a laminate (v) comprising a transparent substrate 11, an ink layer 12, a first adhesive layer 13, and a substrate 14 in this order, by forming a first adhesive layer 13 on the surface of the ink layer 12 or the substrate 14, and then bonding the ink layer 12 and the substrate 14 via the first adhesive layer 13. The process involves forming a second adhesive layer 15 on the surface of a disposable release liner 171 or release liner 16, and then preparing a laminate (vi) containing the disposable release liner 171, the second adhesive layer 15, and the release liner 16 in that order via the second adhesive layer 15. The method for manufacturing an adhesive sheet with a release liner 1 can also be described as including the step of peeling off the disposable release liner 171 of the laminate (vi) and bonding the base material 14 of the laminate (v) with the second adhesive layer 15 of the laminate (vi) to obtain an adhesive sheet with a release liner 1 that includes, in this order, a transparent base material 11, an ink layer 12, a first adhesive layer 13, a base material 14, a second adhesive layer 15, and a release liner 16.

[0133] As is clear from the above, the adhesive sheet 10 and the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured by manufacturing methods 1-4.

[0134] (See Manufacturing Method 1-5 and Figure 6)

[0135] Figure 6 is a process diagram of another example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 6A, 6B, 6C, 6D, 6E, and 6F are process diagrams showing each step of the manufacturing method.

[0136] The manufacturing method shown in Figure 6 is: (1) A step of forming an ink layer 12 by applying ink to the surface of a transparent substrate 11, (2) The process includes the step of forming a first adhesive layer 13 on the surface of the ink layer 12 opposite to the transparent substrate 11. This is a method for manufacturing an adhesive sheet, which provides an adhesive sheet 10 comprising, in this order, a transparent substrate 11, an ink layer 12 provided on the surface of the transparent substrate 11, and a first adhesive layer 13. As mentioned above, the step of forming the first adhesive layer 13 in step (2) also includes steps such as (a) applying an adhesive composition to the surface of the ink layer 12 to form the first adhesive layer 13, and (b) applying an adhesive composition to the surface of another component (such as a base substrate 14 or a disposable release liner) to form the first adhesive layer 13, and then bonding the first adhesive layer 13 to the surface of the ink layer 12.

[0137] More specifically, the manufacturing method shown in Figure 6 is: The above step (2) is, (2-1) A step of preparing a laminate (vii) comprising a first adhesive layer 13, a substrate 14, a second adhesive layer 15, and a release liner 16 in this order, (2-2) It is more preferable to have a manufacturing method that includes the step of bonding the ink layer 12 and the first adhesive layer 13 of the laminate (vii) to obtain an adhesive sheet 1 with a release liner, which includes the transparent substrate 11, the ink layer 12, the first adhesive layer 13, the base substrate 14, the second adhesive layer 15, and the release liner 16 in this order. By such a manufacturing method, the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured.

[0138] Furthermore, the order of steps (1), (2), (2-1), and (2-2) described above is not particularly limited, and they can be performed in any order, as long as it does not contradict their function.

[0139] The following describes each step shown in Figure 6 in detail.

[0140] First, (1) an ink layer 12 is formed by applying ink to the surface of the transparent substrate 11 (see Figures 6A and 6B). This results in a laminate 1a having the transparent substrate 11 and the ink layer 12 provided on its surface. The formation of the ink layer 12 can be appropriately carried out using the methods described above (Manufacturing Methods 1-1 to 1-4). For example, the ink layer 12 can be formed on the surface of the transparent substrate 11 using the inkjet printer described above.

[0141] Then, as step (2), first, a step is performed to prepare a laminate (vii) which includes (2-1) a first adhesive layer 13, a substrate 14, a second adhesive layer 15, and a release liner 16 in this order. The laminate (vii) prepared in this step only needs to include the first adhesive layer 13, the substrate 14, the second adhesive layer 15, and the release liner 16 in this order. The laminate (vii) may further have a disposable release liner 172 on the surface of the first adhesive layer 13, for example. In that case, for example, the first adhesive layer 13 can be formed by applying an adhesive composition to the surface of the disposable release liner 172 (see Figures 6C, 6D, and 6E). Furthermore, the methods for forming the first adhesive layer 13 and the second adhesive layer 15 can be appropriately adopted from those described in (Manufacturing Methods 1-1 to 1-4) above.

[0142] For example, first, an adhesive composition is applied to the surface of the base material 14 or the release liner 16 to form a second adhesive layer 15, and then the base material 14 and the release liner 16 are bonded together via the second adhesive layer 15 to obtain a laminate 1b containing the base material 14, the second adhesive layer 15, and the release liner 16 in that order. Subsequently, an adhesive composition is applied to the surface of a disposable release liner 172 or the base material 14 of the laminate 1b to form a first adhesive layer 13, and then the disposable release liner 172 and the base material 14 are bonded together via the first adhesive layer 13. This makes it possible to obtain a laminate (vii) containing the disposable release liner 172, the first adhesive layer 13, the base material 14, the second adhesive layer 15, and the release liner 16 in that order. The order in which the layers of the laminate (vii) shown here are bonded together is just one example, and the order of bonding is not particularly limited. For example, the second adhesive layer 15 may be formed first, followed by the first adhesive layer 13, or vice versa.

[0143] Next, (2-2) the process of bonding the ink layer 12 and the first adhesive layer 13 of the laminate (vii) is performed to obtain an adhesive sheet 1 with a release liner, which includes the transparent substrate 11, the ink layer 12, the first adhesive layer 13, the base substrate 14, the second adhesive layer 15, and the release liner 16 in this order. In this case, the adhesive sheet 1 with a release liner can be obtained by peeling off the disposable release liner 172 of the laminate (vii) to expose the first adhesive layer 13, and then attaching the first adhesive layer 13 to the ink layer 12.

[0144] According to this manufacturing method, for example, first, the user (printer, etc.) prints a predetermined pattern of their choice onto the surface of the transparent substrate 11. The user prepares the laminate (vii) in advance and peels off the disposable release liner 172 to expose the first adhesive layer 13. Then, the user simply attaches the first adhesive layer 13 to the surface of the ink layer 12 (printed surface). For example, the user only needs to obtain the already laminated laminate (vii) from the manufacturer, so there is no need to form the adhesive layers (first adhesive layer 13 and second adhesive layer 15) themselves. Therefore, the user does not need to prepare or apply the adhesive composition described above. Thus, it can be said that this is a simple and versatile method for users such as printers.

[0145] Furthermore, the manufacturing methods 1-5 illustrated in Figure 6 are, A step of obtaining a laminate 1a including a transparent substrate 11 and an ink layer 12 by applying ink to the surface of a transparent substrate 11 to form an ink layer 12, A step of preparing a laminate 1b comprising a base material 14, a second adhesive layer 15, and a release liner 16 in this order, The process involves applying an adhesive composition to the surface of a disposable release liner 172 or a substrate 14 to form a first adhesive layer 13, and then bonding the disposable release liner 172 and the substrate 14 via the first adhesive layer 13 to obtain a laminate (vii) containing, in this order, the disposable release liner 172, the first adhesive layer 13, the substrate 14, the second adhesive layer 15, and the release liner 16. The method for manufacturing an adhesive sheet with a release liner 1 can also be described as including the step of peeling off the disposable release liner 172 of the laminate (vii), bonding the ink layer 12 of the laminate 1a with the first adhesive layer 13 of the laminate (vii), thereby obtaining an adhesive sheet with a release liner 1 that includes, in this order, a transparent substrate 11, an ink layer 12, a first adhesive layer 13, a base substrate 14, a second adhesive layer 15, and a release liner 16.

[0146] As is clear from the above, the adhesive sheet 10 and the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured by manufacturing methods 1-5.

[0147] (See Manufacturing Method 1-6 and Figure 7)

[0148] Figure 7 is a process diagram of another example of a method for manufacturing an adhesive sheet with a release liner according to the first embodiment, and Figures 7A, 7B, 7C, 7D, 7E, 7F, and 7G are process diagrams showing each step of the manufacturing method.

[0149] The manufacturing method shown in Figure 7 is: (1) A step of forming an ink layer 12 by applying ink to the surface of a transparent substrate 11, (2) The process includes the step of forming a first adhesive layer 13 on the surface of the ink layer 12 opposite to the transparent substrate 11. This is a method for manufacturing an adhesive sheet, which provides an adhesive sheet 10 comprising, in this order, a transparent substrate 11, an ink layer 12 provided on the surface of the transparent substrate 11, and a first adhesive layer 13. As mentioned above, the step of forming the first adhesive layer 13 in step (2) also includes steps such as (a) applying an adhesive composition to the surface of the ink layer 12 to form the first adhesive layer 13, and (b) applying an adhesive composition to the surface of another component (such as a base substrate 14 or a disposable release liner) to form the first adhesive layer 13, and then bonding the first adhesive layer 13 to the surface of the ink layer 12.

[0150] More specifically, the manufacturing method shown in Figure 7 is: The above step (2) is, (2-1) A step of preparing the first adhesive layer 13, (2-2) A step of preparing a laminate (viii) comprising a base material 14, a second adhesive layer 15, and a release liner 16 in this order, (2-3) A step to obtain an adhesive sheet with a release liner 1, comprising a transparent substrate 11, an ink layer 12, a first adhesive layer 13, a base substrate 14, a second adhesive layer 15, and a release liner 16, in this order, by bonding the ink layer 12 and the base substrate 14 of the laminate (viii) via a first adhesive layer 13. It is more preferable to use a manufacturing method that includes [a specific component]. By such a manufacturing method, the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured.

[0151] Furthermore, the order of steps (1), (2), (2-1), (2-2), and (2-3) described above is not particularly limited, and they can be performed in any order, as long as it does not contradict their function.

[0152] The following describes each step shown in Figure 7 in detail.

[0153] First, (1) an ink layer 12 is formed by applying ink to the surface of the transparent substrate 11 (see Figures 7A and 7B). This results in a laminate 1a having the transparent substrate 11 and the ink layer 12 provided on its surface. The formation of the ink layer 12 can be appropriately carried out using the methods described above (Manufacturing Methods 1-1 to 1-5). For example, the ink layer 12 can be formed on the surface of the transparent substrate 11 using the inkjet printer described above.

[0154] Then, as step (2), first, step (2-1) of preparing the first adhesive layer 13 is performed (see Figures 7C and 7D). The method for forming the first adhesive layer 13 can be any of the methods described above (Manufacturing Methods 1-1 to 1-5). The first adhesive layer 13 prepared in this step may be a laminate 1c that includes at least a disposable release liner 143, the first adhesive layer 13, and a disposable release liner 174 in this order.

[0155] For example, by first applying an adhesive composition to the surface of a disposable release liner 173 or disposable release liner 174 to form a first adhesive layer 13, and then bonding the release liner 173 and the release liner 174 together via the first adhesive layer 13, a substrate-less double-sided tape (transfer tape) can be produced that does not have a base material (core material). This manufacturing method can be described as a method of bonding a printed transparent base material and an adhesive base sheet with this substrate-less double-sided tape.

[0156] Furthermore, (2-2) a step is performed to prepare a laminate (viii) comprising a base material 14, a second adhesive layer 15, and a release liner 16 in that order. For example, an adhesive composition is applied to the surface of the base material 14 or the release liner 16 to form a second adhesive layer 15, and then the base material 14 and the release liner 16 are bonded together via the second adhesive layer 15 to obtain a laminate (viii) comprising the base material 14, the second adhesive layer 15, and the release liner 16 in that order.

[0157] Next, (2-3) the process of bonding the ink layer 12 and the base material 14 of the laminate (viii) via the first adhesive layer 13 is performed to obtain an adhesive sheet 1 with a release liner, which includes the transparent base material 11, the ink layer 12, the first adhesive layer 13, the base material 14, the second adhesive layer 15, and the release liner 16 in this order.

[0158] For example, in step (2-1), the release liner (e.g., a disposable release liner 173) on one side of the laminate 1c (substrate-less double-sided tape) prepared is peeled off to expose one side of the first adhesive layer 13, which is then bonded to the ink layer 12. Subsequently, the release liner (e.g., a disposable release liner 174) on the other side is peeled off to expose the other side of the first adhesive layer 13, which is then bonded to the base substrate 14. In this way, the adhesive sheet 1 with a release liner according to the first embodiment can be obtained.

[0159] Furthermore, the manufacturing methods 1-6 illustrated in Figure 7 are: A step of obtaining a laminate 1a including a transparent substrate 11 and an ink layer 12 by applying ink to the surface of a transparent substrate 11 to form an ink layer 12, A step of preparing a laminate 1c comprising, in this order, a disposable release liner 173, a first adhesive layer 13, and another disposable release liner 174, A step of preparing a laminate 1b comprising a base material 14, a second adhesive layer 15, and a release liner 16 in this order, The method for manufacturing an adhesive sheet with a release liner 1 can also be described as a step of obtaining an adhesive sheet with a release liner 1 that includes, in this order, a transparent substrate 11, an ink layer 12, a first adhesive layer 13, a base substrate 14, a second adhesive layer 15, and a release liner 16, by peeling off a disposable release liner 173 from the laminate 1c, bonding the ink layer 12 of the laminate 1a to the first adhesive layer 13 of the laminate 1c, and peeling off another disposable release liner 174 from the laminate 1c, bonding the first adhesive layer 13 of the laminate 1c to the base substrate 14 of the laminate (vii).

[0160] As is clear from the above, the adhesive sheet 10 and the adhesive sheet 1 with a release liner according to the first embodiment can be suitably manufactured by manufacturing methods 1-6.

[0161] <Adhesive sheet and adhesive sheet with release liner according to the second embodiment>

[0162] (Adhesive sheet)

[0163] Figure 8 is a schematic cross-sectional view of an adhesive sheet with a release liner according to the second embodiment.

[0164] The adhesive sheet 20 according to the second embodiment is similar to the adhesive sheet 10 according to the first embodiment in that it includes, at least, a transparent substrate 21, an ink layer 22 provided on the surface of the transparent substrate 21, and a first adhesive layer 23, in that order. In other words, the adhesive sheet 20 according to the second embodiment is similar to the first embodiment in that it includes, at least, a transparent substrate 21, an ink layer 22, and a first adhesive layer 23, in that order.

[0165] Furthermore, although not shown in the figures, another ink layer may be provided on the surface of the base material 24 opposite to the side facing the first adhesive layer 23. For example, by providing another ink layer, it is possible to prevent the color or pattern of the object from showing through (color transparency). For example, in the second embodiment (see Figure 8), another ink layer is provided on the surface of the base material 24 opposite to the surface facing the first adhesive layer 23. That is, in the second embodiment, in a cross-sectional view, the layers can be laminated in the order of transparent base material 21 / ink layer 22 / first adhesive layer 23 / base material 24 / another ink layer (not shown) / second adhesive layer 25. For example, when a user views the ink layer 22 from the transparent base material 21 side of the adhesive sheet 20, it is possible to prevent the color or pattern of the object from showing through (color transparency).

[0166] Furthermore, the adhesive sheet 20 according to the second embodiment preferably further includes a core material 26 provided on the surface of the second adhesive layer 25 opposite to the substrate material 24, and a third adhesive layer 27 provided on the surface of the core material 26 opposite to the second adhesive layer 25. The adhesive sheet 20 according to the second embodiment differs from the adhesive sheet 10 according to the first embodiment in that it has at least a core material 26 and a third adhesive layer 27.

[0167] Furthermore, the adhesive sheet 20 can be an adhesive sheet with a release liner 2, which further includes a release liner 28 provided on the outermost surface opposite to the transparent substrate 21. That is, the adhesive sheet with a release liner 2 includes this adhesive sheet 20 and a release liner 28 provided on the surface of the third adhesive layer 27. In this case, when using it, the release liner 28 is peeled off to expose the third adhesive layer 27. Then, the adhesive surface of the third adhesive layer 27 is attached to a predetermined location on the object.

[0168] Unless otherwise specified, the transparent substrate 21, ink layer 22, first adhesive layer 23, second adhesive layer 25, base substrate 24, and release liner 28 can be appropriately adopted from those described in the first embodiment. The components, shape, and size of the first adhesive layer 23, second adhesive layer 25, and third adhesive layer 27 may be the same or different. However, in the second embodiment, the first adhesive layer 23 is preferably transparent. The total light transmittance of the first adhesive layer 23 is not particularly limited, but is preferably 85% or higher. This provides sufficient transparency for the adhesive sheet 10 and maintains a higher visibility of the ink layer 32. This total light transmittance value can be measured, for example, using a haze meter (e.g., NDH 5000 haze meter manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K 7361:1997. Furthermore, the second adhesive layer 25 and the third adhesive layer 27, which will be described later, located on the adhesive surface side (downward in the drawing) of the base material 24 do not have to be transparent and may contain fillers, pigments, etc.

[0169] (Third adhesive layer)

[0170] The third adhesive layer 27 can employ the materials and conditions described for the first adhesive layer 23 and the second adhesive layer 25. The third adhesive layer 27 may or may not have high transparency. In other words, the third adhesive layer 27 may or may not be transparent. Therefore, depending on the application of the adhesive sheet 20, the third adhesive layer 27 may contain fillers, pigments, etc. For example, by including fillers and / or pigments in the adhesive layer (the third adhesive layer 27 in the second embodiment), which is the adhesive surface of the adhesive sheet 20 that adheres to the object, it is possible to prevent the color or pattern of the object from showing through (color transparency).

[0171] The thickness of the third adhesive layer 27 is not particularly limited, but is preferably 5 μm or more and 80 μm or less. The lower limit of this thickness is more preferably 10 μm or more. The upper limit of this thickness is more preferably 60 μm or less, even more preferably 50 μm or less, even more preferably 40 μm or less, and even more preferably 30 μm or less.

[0172] (Core material)

[0173] The core material 26 is not particularly limited and any known material can be used. Examples of core material 26 materials include resin materials, paper, and metal foil. Examples of resin materials include polyester, polyolefin, polyvinyl chloride, acetylcellulose butyrate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polystyrene, polyamide, polyimide, fluororesin, acrylic resin, and nonwoven fabric. Examples of polyester include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of polyolefins include polyethylene and polypropylene. Examples of paper include synthetic paper, fine paper, kraft paper, glassine paper, and laminated paper. Examples of metal foils include aluminum and copper.

[0174] The thickness of the core material 26 is not particularly limited, but is preferably between 2 μm and 500 μm. The lower limit of the thickness is more preferably 10 μm or more. The upper limit of the thickness is more preferably 250 μm or less. This thickness is the average thickness measured in accordance with JIS K 7130:1999, and refers to, for example, the arithmetic mean of the thickness measured at 10 equally spaced locations using a constant-pressure thickness measuring instrument.

[0175] <Method for manufacturing an adhesive sheet and an adhesive sheet with a release liner according to the second embodiment>

[0176] Furthermore, as a method for manufacturing the adhesive sheet 20 and the adhesive sheet 2 with a release liner in the second embodiment, a method of appropriately laminating each layer can be employed, but several preferred variations are exemplified. The adhesive sheet 20 and the adhesive sheet 2 with a release liner can be manufactured, for example, by the following manufacturing method.

[0177] (See Manufacturing Method 2, Figure 9)

[0178] Figure 9 is a process diagram of an example of a method for manufacturing an adhesive sheet with a release liner according to the second embodiment, and Figures 9A, 9B, 9C, 9D, 9E, and 9F are process diagrams showing each step of the manufacturing method.

[0179] The manufacturing method shown in Figure 9 is: (1) A step of forming an ink layer 22 by applying ink to the surface of a transparent substrate 21, (2) The process includes the step of forming a first adhesive layer 23 on the surface of the ink layer 22 opposite to the transparent substrate 21. The second embodiment is a method for manufacturing an adhesive sheet, which provides an adhesive sheet 20 comprising, in this order, a transparent substrate 21, an ink layer 22 provided on the surface of the transparent substrate 21, and a first adhesive layer 23.

[0180] More specifically, the manufacturing method shown in Figure 9 is as follows: The above step (2) is a step in which a first adhesive layer 23 is formed on the surface of the ink layer 22 or the substrate 24, and then the ink layer 22 and the substrate 24 are bonded together via the first adhesive layer 23 to obtain a laminate (ix) containing the transparent substrate 21, the ink layer 22, the first adhesive layer 23, and the substrate 24 in this order. moreover, (3) A step of preparing a laminate (x) comprising a second adhesive layer 25, a core material 26, a third adhesive layer 27, and a release liner 28 in this order, (4) A step of obtaining an adhesive sheet with a release liner 2, which includes, in this order, a transparent substrate 21, an ink layer 22, a first adhesive layer 23, a substrate 24, a second adhesive layer 25, a core material 26, a third adhesive layer 27, and a release liner 28, by bonding the base substrate 24 of the laminate (ix) and the second adhesive layer 25 of the laminate (x). It is more preferable to use a manufacturing method that includes [the specified element]. By such a manufacturing method, the adhesive sheet 2 with a release liner according to the second embodiment can be suitably manufactured.

[0181] Furthermore, the order of steps (1), (2), (3), and (4) described above is not particularly limited, and they can be performed in any order, as long as it does not contradict their function.

[0182] The following describes each step shown in Figure 9 in detail.

[0183] First, (1) a step is performed to form an ink layer 22 by applying ink to the surface of the transparent substrate 21 (see Figures 9A and 9B). This obtains a laminate 2a having the transparent substrate 21 and the ink layer 22 provided on its surface. The formation of the ink layer 22 can be appropriately adopted from the method described in the first embodiment. For example, the ink layer 22 can be formed on the surface of the transparent substrate 21 using the inkjet printer described above.

[0184] Then, (2) after forming a first adhesive layer 23 on the surface of the ink layer 22 or the base substrate 24, the process is carried out to obtain a laminate (ix) containing the transparent substrate 21, the ink layer 22, the first adhesive layer 23, and the base substrate 24 in this order by bonding the ink layer 22 and the base substrate 24 via the first adhesive layer 23 (see Figure 9C).

[0185] The method for forming the first adhesive layer 23 on the surface of the ink layer 22 or the substrate 24 can be appropriately adopted from the method described in the first embodiment. For example, the first adhesive layer 23 can be formed by applying the above-mentioned adhesive composition to the surface of the ink layer 22 or the substrate 24.

[0186] If an adhesive composition is applied to the surface of the ink layer 22 to form a first adhesive layer 23 on the ink layer 22, the first adhesive layer 23 and the substrate 24 can be bonded together to obtain a laminate (ix). Alternatively, if an adhesive composition is applied to the surface of the substrate 24 to form a first adhesive layer 23 on the substrate 24, the first adhesive layer 23 and the ink layer 22 can be bonded together to obtain a laminate (ix).

[0187] Furthermore, (3) a step is performed to prepare a laminate (x) comprising the second adhesive layer 25, the core material 26, the third adhesive layer 27, and the release liner 28 in this order. The laminate (x) prepared in this step only needs to include the second adhesive layer 25, the core material 26, the third adhesive layer 27, and the release liner 28 in at least this order. The laminate (x) may further have a disposable release liner 291 on the surface of the second adhesive layer 25, for example (see Figures 9D and 9E).

[0188] For example, first, an adhesive composition is applied to the surface of the release liner 28 to form a third adhesive layer 27, and then the release liner 28 and the core material 26 are bonded together via the third adhesive layer 27. On the other hand, an adhesive composition is applied to the surface of a disposable release liner 291 to form a second adhesive layer 25. Then, by bonding the second adhesive layer 25 to the core material 26, a laminate (x) can be formed containing the disposable release liner 291, the second adhesive layer 25, the core material 26, the third adhesive layer 27, and the release liner 28 in this order. In this case, the disposable release liner 291 can be peeled off to expose the second adhesive layer 25, and the laminate (x) can be bonded to the laminate (ix). Note that the third adhesive layer 27 may be formed after the second adhesive layer 25, or vice versa.

[0189] Then, (4) the process of bonding the base material 24 of the laminate (ix) and the second adhesive layer 25 of the laminate (x) is carried out to obtain an adhesive sheet 2 with a release liner, which includes the transparent base material 21, the ink layer 22, the first adhesive layer 23, the base material 24, the second adhesive layer 25, the core material 26, the third adhesive layer 27, and the release liner 28 in this order.

[0190] For example, as described above, if the laminate (ix) has a disposable release liner 291, the release liner 2 can be peeled off and the base material 24 and the second adhesive layer 25 can be bonded together to obtain the adhesive sheet 2 with the release liner.

[0191] Furthermore, the manufacturing method 2 illustrated in Figure 9 is, A step of obtaining a laminate 2a including a transparent substrate 21 and an ink layer 22 by applying ink to the surface of a transparent substrate 21 to form an ink layer 22, A step of obtaining a laminate (ix) comprising a transparent substrate 21, an ink layer 22, a first adhesive layer 23, and a substrate 24 in this order, by forming a first adhesive layer 23 on the surface of the ink layer 22 or the substrate 24, and then bonding the ink layer 22 and the substrate 24 via the first adhesive layer 23. A step of preparing a laminate (x) comprising a disposable release liner 291, a second adhesive layer 25, a core material 26, a third adhesive layer 27, and a release liner 28 in this order, The method for manufacturing an adhesive sheet with a release liner can also be described as including the step of peeling off a disposable release liner from a laminate (x), bonding the base material 24 of the laminate (ix) with the second adhesive layer 25 of the laminate (x), thereby obtaining an adhesive sheet with a release liner 2 that includes, in this order, a transparent base material 21, an ink layer 22, a first adhesive layer 23, a base material 24, a second adhesive layer 25, a core material 26, a third adhesive layer 27, and a release liner 28.

[0192] As is clear from the above, the adhesive sheet 20 and the adhesive sheet 2 with a release liner according to the second embodiment can be suitably manufactured by manufacturing method 2.

[0193] <Adhesive sheet and adhesive sheet with release liner according to the third embodiment>

[0194] (Adhesive sheet)

[0195] Figure 10 is a schematic cross-sectional view of an adhesive sheet with a release liner according to the third embodiment.

[0196] The adhesive sheet 30 according to the third embodiment is an adhesive sheet 30 that, like the adhesive sheet 10 according to the first embodiment and the adhesive sheet 20 according to the second embodiment, includes at least a transparent substrate 31, an ink layer 32 provided on the surface of the transparent substrate 31, and a first adhesive layer 33, in this order. In other words, the adhesive sheet 30 according to the third embodiment is common with the first and second embodiments in that it includes at least a transparent substrate 31, an ink layer 32, and a first adhesive layer 33, in this order. The adhesive sheet 30 according to the third embodiment differs from the adhesive sheet 10 according to the first embodiment in that it has a core material 36 and a third adhesive layer 37. Furthermore, the adhesive sheet 30 according to the third embodiment differs from the adhesive sheet 20 according to the second embodiment in the arrangement order of the core material 36 and the base material 34.

[0197] Furthermore, although not shown in the figures, another ink layer may be provided on the surface of the base material 34 opposite to the first adhesive layer 33. For example, by providing another ink layer, it is possible to prevent the color or pattern of the object from showing through (color transparency). In the case of the third embodiment (see Figure 10), the first adhesive layer 33 is not in contact with the base material 34, but is arranged via other layers (core material 36 and second adhesive layer 35). Even in this case, it can be said that another ink layer is provided on the surface of the base material 34 opposite to the first adhesive layer 33. That is, in the third embodiment, in a cross-sectional view, the layers can be laminated in the order of transparent base material 31 / ink layer 32 / first adhesive layer 33 / core material 36 / second adhesive layer 35 / base material 34 / another ink layer (not shown) / third adhesive layer 37.

[0198] Furthermore, the adhesive sheet 30 according to the third embodiment is A core material 36 is provided on the surface of the first adhesive layer 33 opposite to the ink layer 32, A second adhesive layer 35 is provided on the surface of the core material 36 opposite to the first adhesive layer 33, The second adhesive layer 35 is provided on the surface opposite to the core material 36, and the base material 34 is provided on the surface opposite to the core material 36. Preferably, the substrate further includes a third adhesive layer 37 provided on the surface of the substrate 34 opposite to the second adhesive layer 35.

[0199] Furthermore, the adhesive sheet 30 can be an adhesive sheet with a release liner 3, which further includes a release liner 38 provided on the outermost surface opposite to the transparent substrate 31. That is, the adhesive sheet with a release liner 3 includes this adhesive sheet 30 and a release liner 38 provided on the surface of the third adhesive layer 37. In this case, when using it, the release liner 38 is peeled off to expose the third adhesive layer 37. Then, the adhesive surface of the third adhesive layer 37 is attached to a predetermined location on the object.

[0200] Unless otherwise specified, the transparent substrate 31, ink layer 32, first adhesive layer 33, second adhesive layer 35, base substrate 34, and release liner 38 can be appropriately adopted from those described in the first and second embodiments. However, in the third embodiment, the first adhesive layer 33 and the second adhesive layer 35 are preferably transparent. The total light transmittance of the first adhesive layer 33 and the second adhesive layer 35 is not particularly limited, but is preferably 85% or more for each. This provides sufficient transparency for the adhesive sheet 10 and maintains a higher visibility of the ink layer 32. This total light transmittance value can be measured, for example, using a haze meter (for example, a haze meter "NDH 5000" manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K 7361:1997.

[0201] (Core material) The core material 36 can be appropriately adapted from the one described in the second embodiment. However, in the third embodiment, it is preferable that the core material 36 has high transparency. The total light transmittance is not particularly limited, but it is preferably 85% or higher. This provides sufficient transparency for the adhesive sheet 10 and maintains a higher level of visibility of the ink layer 32. The value of this total light transmittance can be measured, for example, using a haze meter (for example, the haze meter "NDH 5000" manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K 7361:1997.

[0202] (Third adhesive layer)

[0203] The third adhesive layer 37 may appropriately adopt the features described in the second embodiment. The components, shape, and size of the first adhesive layer 33, the second adhesive layer 35, and the third adhesive layer 37 may be the same or different. The third adhesive layer 37 may or may not have high transparency. In other words, the third adhesive layer 37 may or may not be transparent. Therefore, depending on the application of the adhesive sheet 30, the third adhesive layer 37 may contain fillers, pigments, etc. For example, by including fillers and / or pigments in the adhesive layer (the third adhesive layer 37 in the third embodiment), which is the adhesive surface of the adhesive sheet 30 that adheres to the object, it is possible to prevent the color or pattern of the object from showing through (color transparency).

[0204] <Method for manufacturing an adhesive sheet and an adhesive sheet with a release liner according to the third embodiment>

[0205] Furthermore, as a method for manufacturing the adhesive sheet 30 and the adhesive sheet 3 with a release liner according to the third embodiment, a method of appropriately laminating each layer can be employed, but several preferred variations are exemplified. The adhesive sheet 30 and the adhesive sheet 3 with a release liner can be manufactured, for example, by the following manufacturing method.

[0206] (See Manufacturing Method 3, Figure 11)

[0207] Figure 11 is a process diagram of an example of a method for manufacturing an adhesive sheet with a release liner according to the third embodiment, and Figures 11A, 11B, 11C, 11D, 11E, 11F, and 11G are process diagrams showing each step of the manufacturing method.

[0208] The manufacturing method shown in Figure 11 is: (1) A step of forming an ink layer 32 by applying ink to the surface of a transparent substrate 31, (2) The process includes the step of forming a first adhesive layer 33 on the surface of the ink layer 32 opposite to the transparent substrate 31. The manufacturing method for an adhesive sheet is common to the manufacturing method according to the first and second embodiments in that it is a method for manufacturing an adhesive sheet that obtains an adhesive sheet 30 comprising, in this order, a transparent substrate 31, an ink layer 32 provided on the surface of the transparent substrate 31, and a first adhesive layer 33. It goes without saying that in the third embodiment, the step of forming the first adhesive layer 33 in step (2) also includes (a) a step of applying an adhesive composition to the surface of the ink layer 32 to form the first adhesive layer 33, and (b) a step of applying an adhesive composition to the surface of another member (such as a core material 36 or a disposable release liner) to form the first adhesive layer 33, and then bonding the first adhesive layer 33 to the surface of the ink layer 32.

[0209] More specifically, the manufacturing method shown in Figure 11 is as follows: The above step (2) is, (2-1) A step of preparing a laminate (xi) comprising a first adhesive layer 33, a core material 36, and a second adhesive layer 35 in at least this order, (2-2) A step of preparing a laminate (xii) comprising a base material 34, a third adhesive layer 37, and a release liner 38 in at least this order, (2-3) It is more preferable to provide a manufacturing method that includes the step of bonding a transparent substrate 31 having an ink layer 32, a laminate (xi), and a laminate (xii) such that the ink layer 32 is in contact with the first adhesive layer 33 of the laminate (xi), and the second adhesive layer 35 of the laminate (xi) is in contact with the base material 34 of the laminate (xii), thereby obtaining an adhesive sheet 3 with a release liner containing, in this order, a transparent substrate 31, an ink layer 32, a first adhesive layer 33, a core material 36, a second adhesive layer 35, a base material 34, a third adhesive layer 37, and a release liner 38. By such a manufacturing method, the adhesive sheet 3 with a release liner according to the third embodiment can be suitably manufactured.

[0210] Furthermore, the order of steps (1), (2), (2-1), (2-2), and (2-3) described above is not particularly limited, and they can be performed in any order, as long as it does not contradict their function.

[0211] The following describes each step shown in Figure 11 in detail.

[0212] First, (1) a step is performed to form an ink layer 32 by applying ink to the surface of the transparent substrate 31 (see Figures 11A and 11B). This results in a laminate 3a having the transparent substrate 31 and the ink layer 32 provided on its surface. The formation of the ink layer 32 can be appropriately adopted from the method described in the first embodiment. For example, the ink layer 32 can be formed on the surface of the transparent substrate 31 using the inkjet printer described above.

[0213] Then, (2-1) a step is performed to prepare a laminate (xi) which includes at least the first adhesive layer 33, the core material 36, and the second adhesive layer 35 in this order. The laminate (xi) prepared in this step only needs to include the first adhesive layer 33, the core material 36, and the second adhesive layer 35 in at least this order. The laminate (xi) may further have a disposable release liner 391 on the surface of the first adhesive layer 33, or a disposable release liner 392 on the surface of the second adhesive layer 35 (see Figures 11C and 11D).

[0214] For example, first, an adhesive composition is applied to the surface of a disposable release liner 391 to form a first adhesive layer 33, and then the release liner 391 and the core material 36 are bonded together via the first adhesive layer 33. Meanwhile, an adhesive composition is applied to the surface of a disposable release liner 392 to form a second adhesive layer 35. Then, the second adhesive layer 35 is bonded to the core material 36, thereby creating a laminate (xi) containing the release liner 391, the first adhesive layer 33, the core material 36, the second adhesive layer 35, and the release liner 392 in this order. In this case, the disposable release liner 391 can be peeled off to expose the first adhesive layer 33, which can then be bonded to the ink layer 32. Then, the release liner 392 can be peeled off to expose the second adhesive layer 35, which can then be bonded to the base material 34 of the laminate (xii). Furthermore, the second adhesive layer 35 may be formed after the first adhesive layer 33 is formed, or vice versa.

[0215] Furthermore, (2-2) a step is performed to prepare a laminate (xii) which includes at least the base material 34, the third adhesive layer 37, and the release liner 38 in this order (see Figures 11E and 11F).

[0216] For example, first, an adhesive composition is applied to the surface of the base material 34 or the release liner 38 to form a third adhesive layer 37, and then the base material 34 and the release liner 38 are bonded together via the third adhesive layer 37 to obtain a laminate (xii) containing the base material 34, the third adhesive layer 37, and the release liner 38 in that order.

[0217] Then, (2-3) the process of bonding the transparent substrate 31 having the ink layer 32, the laminate (xi), and the laminate (xii) is carried out such that the ink layer 32 and the first adhesive layer 33 of the laminate (xi) are in contact, and the second adhesive layer 35 of the laminate (xi) and the base material 34 of the laminate (xii) are in contact, thereby obtaining an adhesive sheet 3 with a release liner that includes the transparent substrate 31, the ink layer 32, the first adhesive layer 33, the core material 36, the second adhesive layer 35, the base material 34, the third adhesive layer 37, and the release liner 38 in this order (see Figure 11G).

[0218] For example, as described above, if the laminate (xi) has disposable release liners 391 and 392, the release liner 391 is peeled off and the first adhesive layer 33 and the ink layer 32 are bonded together. Alternatively, the release liner 392 is peeled off and the second adhesive layer 35 and the substrate 34 are bonded together. This makes it possible to obtain an adhesive sheet 3 with a release liner.

[0219] Furthermore, the manufacturing method 3 illustrated in Figure 11 is, A step of obtaining a laminate 3a including a transparent substrate 31 and an ink layer 32 by applying ink to the surface of a transparent substrate 31 to form an ink layer 32, A step of preparing a laminate (xi) comprising, at least in this order, a disposable release liner 391, a first adhesive layer 33, a core material 36, a second adhesive layer 35, and another disposable release liner 392, A step of preparing a laminate (xii) comprising a base material 34, a third adhesive layer 37, and a release liner 38 in at least this order, The method for manufacturing an adhesive sheet with a release liner 3 can also be described as including the step of peeling off a disposable release liner 391 from the laminate (xi) and bonding the ink layer 32 to the first adhesive layer 33 of the laminate (xi), and peeling off another disposable release liner 392 from the laminate (xi) and bonding the second adhesive layer 35 to the base material 34 of the laminate (xii), thereby obtaining an adhesive sheet with a release liner 3 containing, in this order, a transparent base material 31, an ink layer 32, a first adhesive layer 33, a core material 36, a second adhesive layer 35, a base material 34, a third adhesive layer 37, and a release liner 38.

[0220] As is clear from the above, the adhesive sheet 30 and the adhesive sheet 3 with a release liner according to the third embodiment can be suitably manufactured by manufacturing method 3.

[0221] As described above, the adhesive sheets 10, 20, 30 and the adhesive sheets 1, 2, 3 with release liners according to this embodiment can effectively suppress the occurrence of silvering and can therefore be suitably used as various decorative sheets and display sheets. Suitable examples of such decorative sheets and display sheets include sheets intended for indoor and outdoor use, such as decorative applications for the interior and exterior of buildings, decorative applications for furniture and fixtures, decorative applications for automobiles, signs, and advertisements. [Explanation of symbols]

[0222] 1, 2, 3: Adhesive sheet with release liner (adhesive sheet) 10, 20, 30: Adhesive sheets 11, 21, 31: Transparent base material 12, 22, 32: Ink layer 13, 23, 33: First adhesive layer 14, 24, 34: Substrate material 15, 25, 35: Second adhesive layer 16, 28, 38: Release Liner 17, 171, 172, 173, 174, 291, 391, 392: Disposable release liner (release liner) 26, 36: Core material 27, 37: Third pressure-sensitive adhesive layer 100: Conventional pressure-sensitive adhesive sheet with release liner (pressure-sensitive adhesive sheet) 110: Conventional pressure-sensitive adhesive sheet 120: Conventional transparent base material 130: Conventional first pressure-sensitive adhesive layer 140: Conventional ink layer 150: Conventional base substrate 160: Conventional second pressure-sensitive adhesive layer 170: Conventional release liner 180: Conventional disposable release liner (release liner) p: Air trap L1, L2: Arrows

Claims

1. A transparent substrate having a thickness of 150 μm or less and made of polyvinyl chloride, An ink layer provided on the surface of the transparent substrate, The first adhesive layer is included in this order, The aforementioned ink layer is a layer formed by ejecting UV-curable ink onto a transparent substrate using inkjet printing, and then curing the UV-curable ink by UV irradiation after ejection; it is a single layer. The ink layer is used by being attached to the substrate with the first adhesive layer side of the ink layer facing the substrate side, so that the ink layer is visible from the transparent substrate side. Adhesive sheet.

2. A base material is provided on the surface of the first adhesive layer opposite to the ink layer, Furthermore, The adhesive sheet according to claim 1.

3. The present invention further includes a second adhesive layer provided on the surface of the substrate material opposite to the first adhesive layer, The adhesive sheet according to claim 2.

4. A core material is provided on the surface of the second adhesive layer opposite to the substrate material, The core material further includes a third adhesive layer provided on the surface opposite to the second adhesive layer, The adhesive sheet according to claim 3.

5. A core material is provided on the surface of the first adhesive layer opposite to the ink layer, A second adhesive layer is provided on the surface of the core material opposite to the first adhesive layer, A base material is provided on the surface of the second adhesive layer opposite to the core material, The present invention further includes a third adhesive layer provided on the surface of the substrate material opposite to the second adhesive layer, The adhesive sheet according to claim 1.

6. The adhesive sheet according to any one of claims 1 to 5 further includes a release liner provided on the outermost surface opposite to the transparent substrate, Adhesive sheet with release liner.

7. (1) A step of forming an ink layer by ejecting an ultraviolet-curable ink onto the surface of a transparent substrate made of polyvinyl chloride having a thickness of 150 μm or less using inkjet printing, and then curing the ultraviolet-curable ink by ultraviolet irradiation after ejection. (2) The process includes forming a first adhesive layer on the surface of the ink layer opposite to the transparent substrate, An adhesive sheet is obtained that includes, in this order, at least the transparent substrate, the ink layer provided on the surface of the transparent substrate, and the first adhesive layer. A method for manufacturing an adhesive sheet, The aforementioned ink layer is a single layer, The adhesive sheet is used by being attached to the substrate with the first adhesive layer side of the ink layer facing the substrate side, so that the ink layer is visible from the transparent substrate side. A method for manufacturing adhesive sheets.

8. In the manufacturing method described in claim 7, A step of obtaining a laminate (i) comprising the transparent substrate, the ink layer provided on the surface of the transparent substrate, and the first adhesive layer in this order by the steps of (1) and (2) above, (3) A step of preparing a laminate (ii) comprising a base material, a second adhesive layer, and a release liner in this order, (4) A step of obtaining an adhesive sheet with a release liner, comprising the transparent substrate, the ink layer, the first adhesive layer, the substrate, the second adhesive layer, and the release liner, by bonding the laminate (i) and the laminate (ii) together such that the first adhesive layer of the laminate (i) and the base substrate of the laminate (ii) are in contact, A method for manufacturing an adhesive sheet with a release liner, including the method described above.

9. In the manufacturing method described in claim 7, The (2) step is a step of forming the first adhesive layer on the surface of the ink layer or the substrate, and then bonding the ink layer and the substrate via the first adhesive layer to obtain a laminate (iii) containing the transparent substrate, the ink layer, the first adhesive layer, and the substrate in this order. moreover, (3) A step of obtaining an adhesive sheet with a release liner, comprising: applying an adhesive to the surface of the base material or release liner to form a second adhesive layer, and then bonding the base material of the laminate (iii) and the release liner via the second adhesive layer, thereby comprising: the transparent substrate, the ink layer, the first adhesive layer, the base material, the second adhesive layer, and the release liner in this order; A method for manufacturing an adhesive sheet with a release liner, including the method described above.

10. In the manufacturing method described in claim 7, The above step (2) is, (2-1) A step of preparing a laminate (iv) comprising a base material, a second adhesive layer, and a release liner in this order, (2-2) A step of obtaining an adhesive sheet with a release liner, comprising the transparent substrate, the ink layer, the first adhesive layer, the substrate, the second adhesive layer, and the release liner, in this order, by forming the first adhesive layer on the surface of the ink layer or the substrate, and then bonding the ink layer and the substrate of the laminate (iv) via the first adhesive layer. A method for manufacturing an adhesive sheet with a release liner, including the method described above.

11. In the manufacturing method described in claim 7, The (2) step is a step of forming the first adhesive layer on the surface of the ink layer or the substrate, and then bonding the ink layer and the substrate via the first adhesive layer to obtain a laminate (v) containing the transparent substrate, the ink layer, the first adhesive layer, and the substrate in this order. moreover, (3) A step of preparing a laminate (vi) containing a second adhesive layer and a release liner in this order, (4) A step of obtaining an adhesive sheet with a release liner, comprising the transparent substrate, the ink layer, the first adhesive layer, the substrate, the second adhesive layer, and the release liner, in this order, by bonding the base material of the laminate (v) and the second adhesive layer of the laminate (vi). A method for manufacturing an adhesive sheet with a release liner, including the method described above.

12. In the manufacturing method described in claim 7, The above step (2) is, (2-1) A step of preparing a laminate (vii) comprising the first adhesive layer, a substrate material, a second adhesive layer, and a release liner in this order, (2-2) A step of obtaining an adhesive sheet with a release liner, comprising the transparent substrate, the ink layer, the first adhesive layer, the base substrate, the second adhesive layer, and the release liner, in this order, by bonding the ink layer and the first adhesive layer of the laminate (vii). A method for manufacturing an adhesive sheet with a release liner, including the method described above.

13. In the manufacturing method described in claim 7, The above step (2) is, (2-1) A step of preparing the first adhesive layer, (2-2) A step of preparing a laminate (viii) comprising a base material, a second adhesive layer, and a release liner in this order, (2-3) A step of obtaining an adhesive sheet with a release liner, comprising the transparent substrate, the ink layer, the first adhesive layer, the base substrate, the second adhesive layer, and the release liner, in this order, by bonding the ink layer and the base substrate of the laminate (viii) via the first adhesive layer. A method for manufacturing an adhesive sheet with a release liner, including the method described above.

14. In the manufacturing method described in claim 7, The (2) step is a step of forming the first adhesive layer on the surface of the ink layer or the substrate, and then bonding the ink layer and the substrate via the first adhesive layer to obtain a laminate (ix) containing the transparent substrate, the ink layer, the first adhesive layer, and the substrate in this order. moreover, (3) A step of preparing a laminate (x) comprising a second adhesive layer, a core material, a third adhesive layer, and a release liner in this order, (4) A step of bonding the base material of the laminate (ix) and the second adhesive layer of the laminate (x) to obtain an adhesive sheet with a release liner, which includes the transparent substrate, the ink layer, the first adhesive layer, the base material, the second adhesive layer, the core material, the third adhesive layer, and the release liner in this order. A method for manufacturing an adhesive sheet with a release liner.

15. In the manufacturing method described in claim 7, The above step (2) is, (2-1) A step of preparing a laminate (xi) comprising the first adhesive layer, the core material, and the second adhesive layer in this order, (2-2) A step of preparing a laminate (xii) comprising a base material, a third adhesive layer, and a release liner in this order, (2-3) A step of obtaining an adhesive sheet with a release liner, comprising the transparent substrate having the ink layer, the laminate (xi), and the laminate (xii) in this order, by bonding them together such that the ink layer and the first adhesive layer of the laminate (xi) are in contact, and the second adhesive layer of the laminate (xi) and the base material of the laminate (xii) are in contact. A method for manufacturing an adhesive sheet with a release liner, including the method described above.

Citation Information

Patent Citations

  • Colored adhesive tape

    JP2003292911A

  • Printed structure and method for producing printed structure

    JP2014046671A

  • Road surface / floor surface marking laminate sheet and road surface / floor surface marking sheet

    JP2015184488A

  • Adhesive sheet for decoration

    JP2017119790A

  • Rail car floor display film

    JP2018091975A