resin film

A resin film with controlled thermal and humidity expansion/shrinkage properties addresses peeling issues in adhesive sheets by maintaining stable bonding under harsh environmental conditions.

JP7954019B2Active Publication Date: 2026-11-19NITTO DENKO CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022109763
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-07-07
Publication Date
2026-11-19
Estimated Expiration
2042-07-07

AI Technical Summary

Technical Problem

Conventional pressure-sensitive adhesive sheets and adhesive sheets experience peeling from adherends when exposed to high-temperature and high-humidity environments.

Method used

A resin film with a specific ratio of shrinkage rate to expansion rate in a high-temperature, high-humidity environment is used, where the ratio of thermal shrinkage rate to high-humidity expansion rate is between 0.3 to 2.5, achieved by heat-treating the raw material film while applying tensile stress.

Benefits of technology

The resin film minimizes peeling from adherends even in high-temperature, high-humidity conditions, ensuring stable bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954019000002
    Figure 0007954019000002
  • Figure 0007954019000003
    Figure 0007954019000003
  • Figure 0007954019000004
    Figure 0007954019000004
Patent Text Reader

Abstract

To provide a resin film unlikely to cause a separation from an adherend even if exposed to a high-temperature high-humidity environment in a state bonded to the adherend interposing a tackifier layer or an adhesive layer.SOLUTION: A resin film 1 is to be used with a tackifier layer or an adhesive layer laminated at least on one side thereof. In the resin film, a ratio is 0.3 to 2.5 with regard to a contraction coefficient when heated for 5 minutes at a temperature of 120°C and an expansion coefficient when stored for 30 minutes in an environment of a temperature of 85°C and a humidity of 85%RH.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin film.

Background Art

[0002] As a material for bonding members to each other, pressure-sensitive adhesive sheets or adhesive sheets using a resin film as a base material, with a pressure-sensitive adhesive layer or an adhesive layer laminated on both sides of the base material, are widely used (see, for example, Patent Document 1).

Prior Art Documents

Patent Documents

[0003]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0004] However, when conventional pressure-sensitive adhesive sheets and adhesive sheets are bonded to an adherend and then exposed to a high-temperature and high-humidity environment, peeling may occur between the sheet and the adherend in some cases.

[0005] Accordingly, an object of the present invention is to provide a resin film that hardly causes peeling from an adherend even when exposed to a high-temperature and high-humidity environment in a state of being bonded to the adherend via a pressure-sensitive adhesive layer or an adhesive layer.

Means for Solving the Problems

[0006] As a result of diligent efforts to solve the above problems, the present inventors have found that by using a resin film as the base material for adhesive sheets or bonding sheets, in which the ratio of shrinkage rate when heated to expansion rate in a high-temperature, high-humidity environment is within a specific range, it is possible to obtain an adhesive sheet or bonding sheet that is less likely to peel off from the adherend even when exposed to a high-temperature, high-humidity environment while bonded to the adherend. The present invention was completed based on these findings.

[0007] The present invention provides a resin film used by laminating an adhesive layer or bonding layer on at least one surface, wherein the ratio [former / latter] of the shrinkage rate when heated at 120°C for 5 minutes to the expansion rate when stored in an environment of 85°C and 85% RH for 30 minutes is 0.3 to 2.5.

[0008] The above resin film is preferably obtained by heat-treating the raw material film while applying tensile stress in at least one direction.

[0009] The above-mentioned resin film preferably contains as its main component one or more resins, consisting of polycarbonate resins, polyester resins, acrylic resins, cellulose resins, and cycloolefin resins.

[0010] The above-mentioned resin film is preferably used by laminating an adhesive layer on one side and laminating another resin film on the other side via the adhesive layer or bonding layer.

[0011] The above resin film preferably has a ratio [former / latter] of 1.0 to 3.0 between its expansion rate and the shrinkage rate of the other resin film when stored for 30 minutes in an environment of 85°C and 85% RH. [Effects of the Invention]

[0012] The resin film of the present invention is less likely to peel off from the adherend even when it is bonded to the adherend via an adhesive layer or bonding layer and exposed to a high-temperature, high-humidity environment. For this reason, for example, by using the resin film of the present invention as a base material for an adhesive sheet or bonding sheet, peeling off from the adhesive sheet or bonding sheet and the adherend is less likely to occur even when the adhesive sheet or bonding sheet is bonded to the adherend and exposed to a high-temperature, high-humidity environment. [Brief explanation of the drawing]

[0013] [Figure 1] A cross-sectional view showing one embodiment of an adhesive sheet or the like comprising the resin film of the present invention. [Figure 2] A cross-sectional view showing another embodiment of the present invention, such as an adhesive sheet comprising the resin film. [Figure 3] This is a cross-sectional view showing one embodiment of the method for manufacturing a resin film according to the present invention. [Figure 4] A cross-sectional view showing one use case of an adhesive sheet or the like comprising the resin film of the present invention. [Modes for carrying out the invention]

[0014] [Resin film] The resin film of the present invention is a resin film used by laminating (directly laminating) an adhesive layer or bonding layer on at least one surface. Preferably, the above resin film is used by laminating (directly laminating) an adhesive layer on at least one surface. The above resin film is used, for example, as a base material or adherend for an adhesive sheet or bonding sheet. Note that the above resin film is different from the release liner and its base material that are peeled off when the adhesive layer or bonding layer is used to bond to an adherend.

[0015] FIG. 1 and FIG. 2 show an embodiment in which the resin film of the present invention is applied as a base material of an adhesive sheet. The adhesive sheet 10 shown in FIG. 1 is a single-sided adhesive sheet comprising the resin film 1 of the present invention and an adhesive layer 21 laminated on one side of the resin film 1. The adhesive surface of the adhesive layer 21 is protected by a release liner 31.

[0016] The adhesive sheet 10 shown in FIG. 2 is a double-sided adhesive sheet comprising the resin film 1 of the present invention, an adhesive layer 21 laminated on one side of the resin film 1, and an adhesive layer 22 laminated on the other side of the resin film 1. The adhesive surface of the adhesive layer 21 is protected by a release liner 31, and the adhesive surface of the adhesive layer 22 is protected by a release liner 32.

[0017] The above resin film has a ratio [the former / the latter] of 0.3 to 2.5 between the shrinkage ratio when heated at a temperature of 120°C for 5 minutes and the expansion ratio when stored in an environment at a temperature of 85°C and a humidity of 85%RH for 30 minutes. In this specification, the shrinkage ratio when heated at a temperature of 120°C for 5 minutes may be referred to as "thermal shrinkage ratio". In addition, the expansion ratio when stored in an environment at a temperature of 85°C and a humidity of 85%RH for 30 minutes may be referred to as "high-humidity expansion ratio".

[0018] The above ratio [thermal shrinkage ratio / high-humidity expansion ratio] is 0.3 or more, preferably 0.4 or more, more preferably 0.5 or more, further preferably 0.6 or more, and particularly preferably 0.7 or more. In addition, the above ratio is 2.5 or less, preferably 2.4 or less, more preferably 2.3 or less, further preferably 2.2 or less, and particularly preferably 2.1 or less. When the above ratio is within the above range, the thermal shrinkage ratio and the high-humidity expansion ratio of the resin film are well balanced, and when the resin film is bonded to an adherend via an adhesive layer or a pressure-sensitive adhesive layer and exposed to a high-temperature and high-humidity environment, the expansion and shrinkage of the resin film are offset, resulting in less likely occurrence of dimensional change and less likely occurrence of peeling from the adherend.

[0019] The above ratio [thermal shrinkage rate / high-humidity expansion rate] is calculated by adopting the respective maximum values of the thermal shrinkage rate and the high-humidity expansion rate. For example, when the value in the machine direction (MD) among the thermal shrinkage rates of the resin film is the maximum, and the value in the transverse direction (TD) among the high-humidity expansion rates of the resin film is the maximum, the value in the MD direction is adopted as the thermal shrinkage rate, and the value in the TD direction is adopted as the high-humidity expansion rate. It is preferable that each of the above thermal shrinkage rate and the above high-humidity expansion rate is a value in a direction selected from the MD direction and the TD direction.

[0020] In the present specification, the thermal shrinkage rate X is a positive value. For each of two opposing sides of a rectangular or square resin film, two points at arbitrary distances from the midpoint toward the center are taken as two evaluation points. When the distance between the evaluation points before heating (at normal temperature) is defined as a, and the distance between the evaluation points after heating at 120°C for 5 minutes is defined as a', the thermal shrinkage rate X is calculated by the following formula (1). X[%]=(a-a') / a×100 (1)

[0021] In the present specification, the high-humidity expansion rate Y is a positive value. For each of two opposing sides of a rectangular or square resin film, two points at arbitrary distances from the midpoint toward the center are taken as two evaluation points. When the distance between the evaluation points before heating (at normal temperature) is defined as a, and the distance between the evaluation points after storage for 30 minutes in an environment at a temperature of 85°C and a humidity of 85%RH is defined as a', the high-humidity expansion rate Y is calculated by the following formula (2). Y[%]=(a'-a) / a×100 (2)

[0022] The resin film in which the above ratio [thermal shrinkage rate / high-humidity expansion rate] falls within the above range can be produced by the method for producing a resin film described later. That is, the above resin film is preferably a film obtained by subjecting a raw material film to heat treatment while applying tensile stress in at least one direction. Note that there is a circumstance that such a resin film cannot be directly specified by its structure or characteristics, or is almost impractical, except when expressed by the production process.

[0023] The above-mentioned resin film mainly contains resin. The above-mentioned resin film is formed from a composition mainly composed of resin. Examples of the above-mentioned resin film include various optical films such as plastic films, anti-reflective (AR) films, anti-glare (AG) films, polarizing plates, and phase difference plates, as well as porous materials such as cloth and nonwoven fabrics, nets, and foamed sheets. It may also be a porous film or a non-porous film.

[0024] As the above resin, known or conventional film-forming resins can be used, such as low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, ultra-low-density polyethylene, random copolymer polypropylene, block copolymer polypropylene, homopolypropylene, polybutene, polymethylpentene, ionomer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester (random, alternating) copolymer, ethylene-vinyl acetate copolymer (EVA), ethylene-propylene copolymer, cycloolefin resin, ethylene-butene copolymer, ethylene-hexene copolymer, etc. Examples include polyolefin resins; polyurethanes; polyester resins such as polyethylene terephthalate (PET), polyethylene naphthalate, and polybutylene terephthalate (PBT); polycarbonate resins; polyimide resins; polyether ether ketones; polyetherimides; polyamides such as aramids and fully aromatic polyamides; polyphenyl sulfides; fluororesins; polyvinyl chloride; polyvinylidene chloride; cellulose resins such as triacetylcellulose (TAC); silicone resins; acrylic resins such as polymethyl methacrylate (PMMA); polysulfones; polyarylates; and polyvinyl acetate. Among these, polycarbonate resins, polyester resins, acrylic resins, cellulose resins, and polyolefin resins (especially cycloolefin resins) are preferred. Note that one type of these resin may be used, or two or more types may be used.

[0025] The resin content in the above resin film is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total amount (100% by mass) of the resin film. It may also be 80% by mass or more, 90% by mass or more, or 95% by mass or more. Furthermore, the above resin film may contain other components besides resin.

[0026] The above resin film preferably has a saturated water absorption rate of 2.0% or less, more preferably less than 1.5%, even more preferably less than 1.1%, even more preferably 1.0% or less, and particularly preferably 0.8% or less. When the saturated water absorption rate is 2.0% or less, peeling from the adherend is less likely to occur when the film is bonded to the adherend via an adhesive layer or bonding agent and exposed to a high-temperature, high-humidity environment. The above saturated water absorption rate can be determined in accordance with JIS K7209.

[0027] The thickness of the resin film is not particularly limited, but is preferably 10 to 1000 μm, more preferably 50 to 800 μm, and even more preferably 70 to 500 μm.

[0028] At least one surface of the above-mentioned resin film may be subjected to surface treatments such as physical treatments like corona discharge treatment, plasma treatment, sandblasting, ozone exposure treatment, flame exposure treatment, high-voltage electric shock exposure treatment, or ionization radiation treatment; chemical treatments like chromic acid treatment; or surface treatments such as easy adhesion treatment with a coating agent (primer) in order to improve adhesion and retention with the adhesive layer. It is preferable that the surface treatment to improve adhesion is applied to the entire surface of the resin film on the side to which the adhesive layer or bonding layer is laminated.

[0029] The above-mentioned resin film is preferably used by laminating it with other resin films via an adhesive layer or bonding layer.

[0030] The ratio [former / latter] of the high-humidity expansion coefficient of the above resin film to the shrinkage coefficient of the above other resin film when stored for 30 minutes in an environment of 85°C and 85% RH is preferably 0.5 or higher, more preferably 0.9 or higher, and even more preferably 1.0 or higher. Furthermore, the above ratio is preferably 3.5 or lower, more preferably 3.0 or lower, and even more preferably 2.0 or lower. The shrinkage coefficient of the above other resin film when stored for 30 minutes in an environment of 85% RH may be referred to as the "high-humidity shrinkage coefficient." When the above ratio is within the above range, the expansion and contraction of the resin film are balanced when stored for 30 minutes in an environment of 85% RH, so that peeling is less likely to occur between each layer of the above resin film, the adhesive layer or adhesive layer, and the above other resin film.

[0031] The above high humidity shrinkage rate is not particularly limited, but is preferably 1.0% or less (e.g., 0 to 1.0%), more preferably 0.5% or less, and even more preferably 0.2% or less. In this specification, the above high humidity shrinkage rate Z is calculated by the following formula (3), where, for each of the two opposing sides of the above rectangular or square resin film, two points are set at an arbitrary distance from the midpoint toward the center, the distance between the points before heating (at room temperature) is b, and the distance between the points after storage for 30 minutes in an environment of 85°C and 85% RH is b'. The maximum value of the above high humidity shrinkage rate is used. The above high humidity shrinkage rate is preferably a value in a direction selected from the MD direction and the TD direction. Z[%]=(b-b') / b×100 (3)

[0032] The above-mentioned other resin films mainly contain resin. The above-mentioned other resin films are formed from compositions mainly composed of resin. Examples of the above-mentioned other resin films include various optical films such as plastic films, anti-reflective (AR) films, anti-glare (AG) films, polarizing plates, and phase difference plates, as well as porous materials such as cloth and nonwoven fabrics, nets, and foamed sheets. They may also be porous films or non-porous films.

[0033] As the resin mentioned above, known or conventional resins for film formation can be used, for example, those exemplified and described as resins constituting the resin film of the present invention. The resin content in the other resin film is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and may be 80% by mass or more, 90% by mass or more, or 95% by mass or more, based on the total amount (100% by mass) of the other resin film. Furthermore, the other resin film may contain other components besides resin.

[0034] When the above-mentioned resin film is used by laminating another resin film on one side via an adhesive layer or bonding layer, it is preferable that the other side has an adhesive layer or bonding layer (particularly an adhesive layer) laminated (formed). In this case, the resin film can be bonded to an adherend with the other side having the other resin film laminated on one side.

[0035] [Method for manufacturing resin film] The above-mentioned resin film can be manufactured by a method that includes a heating step in which the raw material film is heated so that the above-mentioned ratio [heat shrinkage rate / high humidity expansion rate] falls within the above-mentioned range. The method for manufacturing the above-mentioned resin film may also include other steps besides the heating step described above.

[0036] (Heating process) The raw material film is appropriately selected according to the type of resin film. The raw material film may be an unstretched film or a film stretched in at least one direction (stretched film), but an unstretched film is preferred.

[0037] In the heating process described above, it is preferable to heat the raw material film while applying tensile stress. By heating in this manner, a resin film having the above ratio [heat shrinkage rate / high humidity expansion rate] within the above range can be easily produced. In particular, by appropriately adjusting the tensile stress according to the type of raw material film, a resin film having the above ratio [heat shrinkage rate / high humidity expansion rate] within the above range can be easily produced.

[0038] The direction in which the tensile stress is applied is preferably at least one direction, more preferably two directions, and even more preferably two orthogonal directions. In particular, it is especially preferable to heat the resin film while applying tensile stress in the MD direction and / or TD direction.

[0039] The above tensile stress can be applied by known or conventional methods. For example, in the heating process described above, tensile stress may be applied by stretching in the MD direction. In a method of heating while continuously feeding the raw film using a conveyor roll, such as a roll-to-roll system, tensile stress can be applied in the MD direction by the tensile stress generated during conveyance by the conveyor roll. In addition, tensile stress may be applied in the TD direction by stretching, such as tenter stretching, while heating. Furthermore, the film may be heated while being pulled or fixed by clamping both ends in the MD direction and both ends in the TD direction with a chuck or the like, and pulling outwards in the MD direction and / or TD direction.

[0040] The above tensile stress is adjusted as appropriate depending on the type and properties of the resin in the raw film, but is preferably 10N or more, more preferably 30N or more, even more preferably 50N or more, and may also be 60N or more, 80N or more, or 100N or more. Furthermore, the above tensile stress is preferably 500N or less, more preferably 450N or less, and even more preferably 400N or less. By setting the above tensile stress within the above range, a resin film with the above ratio [heat shrinkage rate / high humidity expansion rate] within the above range can be easily produced.

[0041] When tensile stress is applied in two directions, the tensile stress in one direction (particularly the MD direction) is preferably 50 N or more, more preferably 80 N or more, and even more preferably 100 N or more. Furthermore, the tensile stress in the above-mentioned one direction (particularly the MD direction) is preferably 500 N or less, more preferably 450 N or less, and even more preferably 400 N or less. Furthermore, the tensile stress in the other direction (particularly the TD direction) is preferably 10 N or more, more preferably 30 N or more, and even more preferably 50 N or more, and may be 60 N or more, 80 N or more, or 100 N or more. Furthermore, the tensile stress in the above-mentioned other direction (particularly the TD direction) is preferably 500 N or less, more preferably 450 N or less, and even more preferably 400 N or less.

[0042] The heating temperature and heating time in the above heating process are appropriately selected according to the type of raw material film. The heating temperature is, for example, 60 to 200°C, preferably 80 to 180°C, and more preferably 100 to 160°C. The heating time is, for example, 10 seconds to 30 minutes, preferably 30 seconds to 15 minutes, and more preferably 1 minute to 10 minutes.

[0043] The above heating can be carried out by known or conventional heating methods. In particular, it is preferable to heat the raw material film by applying hot air to at least one side (preferably both sides). With such a heating method, the raw material film can be heated more uniformly.

[0044] The above heating is preferably performed when no other layers, such as adhesive or bonding layers, are laminated, and is particularly preferable to be performed on the raw film alone. In this case, a resin film in which the above ratio [heat shrinkage rate / high humidity expansion rate] is within the above range can be easily produced.

[0045] The above heating is preferably carried out while the raw material film is being transported. By heating the raw material film while transporting it, the resin film can be produced efficiently.

[0046] (Unwinding process) The above manufacturing method may include a step (unwinding step) in which the raw material film is continuously unwound in the longitudinal direction from the winding body on which the raw material film is wound, prior to the heating step. Including the unwinding step allows the raw material film to be continuously fed into an oven or the like while being transported and heated, enabling efficient production of resin film.

[0047] (Winding process) The above manufacturing method may include a winding step in which the film after the heating step is wound up while being pulled in the longitudinal direction to obtain a roll of resin film raw material. Including the above winding step allows tensile stress to be generated in the longitudinal direction (MD direction) of the film during winding, making it easy to apply tensile stress to the raw film during heating and resulting in superior production efficiency.

[0048] Figure 3 shows one embodiment of the method for manufacturing the resin film of the present invention. As shown in Figure 3, first, the raw material film 1' is unwound from the wound body 11 while being held between rolls 61 and 62 (unwinding step). If a protective film 41 is laminated to the raw material film 1', the protective film 41 is peeled off by the roll 62 before heating, and the raw material film 1' alone is continuously fed into the oven 5. Multiple hot air blowers 51 are installed inside the oven 5. The raw material film 1' is pulled and conveyed by rolls 63 and 64 located outside the exit of the oven 5. By making the rotation speed of rolls 63 and 64 faster than the rotation speed of rolls 61 and 62, tensile stress can be applied to the raw material film 1' in the MD direction. Therefore, inside the oven 5, the raw material film 1' is subjected to tensile stress, and both sides of the raw material film 1' (top and bottom surfaces) are heated by hot air blown from the hot air blowers 51 (heating step). The film discharged from oven 5 is cooled to room temperature, then held between rolls 63 and 64 and transported, while the protective film 42 is re-bonded and the film is wound up (winding process). In this way, a wound body 12 with the resin film 1 wound around it can be obtained.

[0049] [Adhesive layer or bonding layer] In this specification, an adhesive layer or bonding layer may be referred to as an "adhesive layer, etc." In this specification, "adhesion" refers to the property of two surfaces adhering tightly to each other based on the cohesive force derived from the chemical structure of the composition in response to external pressure (e.g., minute pressure), and being able to be separated if necessary. In contrast, "bonding" refers to the property of two surfaces being firmly joined together by a chemical reaction (curing) of the composition, producing a cured product, and not being intended to be separated. In this specification, an "adhesive layer" is a non-fluid, layered adhesive layer, and a "bonding layer" is a non-fluid, layered bonding layer.

[0050] The above-mentioned adhesive layer, etc., includes an adhesive layer, etc., containing a polymer capable of exhibiting tackiness and / or adhesion. The polymer may contain only one type or two or more types. Examples of the polymer include thermoplastic resins, thermosetting resins, and active energy ray curable resins. An adhesive layer, etc., containing a thermoplastic resin can exhibit tackiness that allows it to adhere to an object by external pressure, for example. An adhesive layer, etc., containing a thermosetting resin can adhere to an object by curing, for example, by heating.

[0051] The above-mentioned thermosetting resin can be either a thermosetting resin (thermosetting resin) or a resin obtained by curing the above-mentioned thermosetting resin. The above-mentioned thermosetting resin has thermosetting functional groups. The number of thermosetting functional groups in the above-mentioned thermosetting resin is preferably two or more (for example, 2 to 4). Examples of the above-mentioned thermosetting resin include phenolic resins, epoxy resins, urethane resins, melamine resins, alkyd resins, and silicone resins.

[0052] Examples of the thermoplastic resins mentioned above include polystyrene resins, vinyl acetate resins, polyester resins, polyolefin resins (polyethylene resins, polypropylene resin compositions, etc.), polyimide resins, acrylic resins, rubber (natural rubber, synthetic rubber, mixtures thereof, etc.), polyether resins, polyamide resins, and fluororesins. Among these, acrylic resins are preferred because they can impart cohesive force and appropriate flexibility to the adhesive layer, etc.

[0053] The above-mentioned adhesive layer, etc. preferably contains an acrylic resin as a base polymer. In this specification, the base polymer refers to the main component of the polymer component in the adhesive or bonding agent constituting the adhesive layer, etc., for example, the polymer component that is present in more than 50% by mass. The content ratio of the base polymer in the above-mentioned adhesive layer, etc. is preferably 60% by mass or more, and more preferably 70% by mass or more, based on 100% by mass of the total amount of the adhesive layer, etc.

[0054] The design of acrylic resins varies widely depending on the purpose, and it is preferable to appropriately select monomer species, copolymerization ratio, molecular weight, molecular weight distribution, crosslinking agent, and blending ratio according to the desired values ​​of mechanical properties such as flexibility and elastic modulus, thermal properties such as glass transition temperature, and adhesive properties such as tackiness and adhesion.

[0055] The acrylic resin is a resin that contains acrylic monomers (monomers having a (meth)acryloyl group in the molecule) as monomer components constituting the resin. That is, the acrylic resin contains constituent units derived from acrylic monomers. Preferably, the acrylic resin is a polymer that contains alkyl (meth)acrylate as a monomer component constituting the polymer. In this specification, "(meth)acrylic" means "acrylic" and / or "methacrylic" (either one or both of "acrylic" and "methacrylic"), and the same applies to other terms.

[0056] The above acrylic resin is preferably a polymer that contains the largest mass percentage of constituent units derived from (meth)acrylic acid ester. Examples of the above (meth)acrylic acid ester include hydrocarbon group-containing (meth)acrylic acid esters. Examples of the above hydrocarbon group-containing (meth)acrylic acid ester include alkyl (meth)acrylic acid esters having linear or branched aliphatic hydrocarbon groups, cycloalkyl (meth)acrylic acid esters having alicyclic hydrocarbon groups, and aryl (meth)acrylic acid esters having aromatic hydrocarbon groups. Only one type of hydrocarbon group-containing (meth)acrylic acid ester may be used, or two or more types may be used.

[0057] Examples of the above alkyl (meth)acrylate esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and methyl (meth)acrylate. Examples include isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0058] Among the alkyl (meth)acrylate esters mentioned above, alkyl (meth)acrylate esters having linear or branched aliphatic hydrocarbon groups with 1 to 20 carbon atoms (preferably 2 to 12, more preferably 4 to 10) are preferred. When the number of carbon atoms is within the above range, it is easy to adjust the glass transition temperature of the acrylic resin and to make the tackiness more appropriate.

[0059] Examples of (meth)acrylic acid esters having the above-mentioned alicyclic hydrocarbon group include (meth)acrylic acid esters having a monocyclic aliphatic hydrocarbon ring such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate; (meth)acrylic acid esters having a bicyclic aliphatic hydrocarbon ring such as isobornyl (meth)acrylate; and (meth)acrylic acid esters having three or more aliphatic hydrocarbon rings such as dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, tricyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate.

[0060] Examples of (meth)acrylic acid esters having the above-mentioned aromatic hydrocarbon group include phenyl (meth)acrylate and benzyl (meth)acrylate.

[0061] In order to appropriately exhibit the basic properties such as tackiness of the hydrocarbon group-containing (meth)acrylic acid ester in the adhesive layer, the proportion of the hydrocarbon group-containing (meth)acrylic acid ester in the total monomer components constituting the acrylic resin is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total amount (100% by mass) of the total monomer components. Furthermore, from the viewpoint of enabling copolymerization with other monomer components and obtaining the effects of those other monomer components, the above proportion may be 99.9% by mass or less, 98% by mass or less, 95% by mass or less, 90% by mass or less, or 80% by mass or less.

[0062] The above acrylic resin may contain constituent units derived from other monomer components copolymerizable with the hydrocarbon group-containing (meth)acrylic acid ester, for the purpose of modifying it to improve cohesiveness or introduce crosslinking points. Examples of the above other monomer components include polar group-containing monomers such as hydroxyl group-containing monomers, nitrogen atom-containing monomers, carboxyl group-containing monomers, acid anhydride monomers, keto group-containing monomers, alkoxysilyl group-containing monomers, glycidyl group-containing monomers, sulfonic acid group-containing monomers, and phosphate group-containing monomers. Each of the above other monomer components may be used individually or in combination of two or more.

[0063] Examples of the above-mentioned hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate.

[0064] Examples of nitrogen atom-containing monomers include amide group-containing monomers, amino group-containing monomers, cyano group-containing monomers, and monomers having a nitrogen atom-containing ring. Examples of amide group-containing monomers include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide, N-methoxymethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide. Examples of amino group-containing monomers include aminoethyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, and t-butylaminoethyl(meth)acrylate. Examples of cyano group-containing monomers include acrylonitrile and methacrylonitrile. Examples of monomers having the nitrogen atom-containing ring mentioned above include N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinylcaprolactam, and N-(meth)acryloylmorpholine.

[0065] Examples of the above carboxyl group-containing monomers include acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. Examples of the above acid anhydride monomers include maleic anhydride and itaconic anhydride.

[0066] Examples of the above-mentioned keto group-containing monomers include diacetone(meth)acrylamide, diacetone(meth)acrylate, vinyl methyl ketone, vinyl ethyl ketone, allyl acetacetate, and vinyl acetacetate.

[0067] Examples of the above-mentioned alkoxysilyl group-containing monomers include 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane.

[0068] Examples of the above-mentioned glycidyl group-containing monomers include glycidyl (meth)acrylate and methylglycidyl (meth)acrylate.

[0069] Examples of the above-mentioned sulfonic acid group-containing monomers include styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid.

[0070] Examples of the above-mentioned phosphate group-containing monomers include 2-hydroxyethyl acryloyl phosphate.

[0071] The total proportion of the polar group-containing monomers in the total monomer components (100% by mass) constituting the above acrylic resin is not particularly limited, but from the viewpoint of better exhibiting the effects of using polar group-containing monomers, it is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 5% by mass or more, and may also be 10% by mass or more, 15% by mass or more, 20% by mass or more, or 25% by mass or more. Furthermore, from the viewpoint of obtaining an adhesive layer with appropriate flexibility, the total proportion is preferably 50% by mass or less, and more preferably 40% by mass or less.

[0072] The monomer components constituting the above-mentioned acrylic resin may further include other monomers. Examples of these other monomers include vinyl ester monomers such as vinyl acetate, vinyl propionate, and vinyl laurate; aromatic vinyl compounds such as styrene, substituted styrene (α-methylstyrene, etc.), and vinyltoluene; olefin monomers such as ethylene, propylene, isoprene, butadiene, and isobutylene; chlorine-containing monomers such as vinyl chloride and vinylidene chloride; alkoxy group-containing monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; and vinyl ether monomers such as methyl vinyl ether and ethyl vinyl ether.

[0073] The proportion of the other monomers in the total amount of all monomer components constituting the above acrylic resin (100% by mass) may be, for example, 0.05% by mass or more, or 0.5% by mass or more. The above proportion may also be, for example, 20% by mass or less, 10% by mass or less, or 5% by mass or less, and may be substantially absent.

[0074] The above-mentioned acrylic resin is obtained by polymerizing a monomer component containing the above-mentioned acrylic monomer. While the polymerization method is not particularly limited, examples include solution polymerization, emulsion polymerization, bulk polymerization, thermal polymerization, and polymerization by active energy ray irradiation (active energy ray polymerization). Among these, bulk polymerization, thermal polymerization, and active energy ray polymerization are preferred in terms of transparency of the adhesive layer and cost. Furthermore, the resulting acrylic resin may be a random copolymer, block copolymer, graft copolymer, or any other type.

[0075] Various common solvents may be used in the polymerization of monomer components. Examples of such solvents include esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as toluene and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; and organic solvents such as ketones such as methyl ethyl ketone and methyl isobutyl ketone. One or more of these solvents may be used.

[0076] The polymerization initiators, chain transfer agents, emulsifiers, etc., used in the radical polymerization of monomer components are not particularly limited and can be selected and used as appropriate. The weight-average molecular weight of the acrylic resin can be controlled by the amount of polymerization initiator and chain transfer agent used and the reaction conditions, and the appropriate amounts used are adjusted according to the type of agent.

[0077] Depending on the type of polymerization reaction, various polymerization initiators can be used for the polymerization of monomer components, including thermal polymerization initiators and photopolymerization initiators (photoinitiators). One type of polymerization initiator may be used, or two or more types may be used.

[0078] The above-mentioned thermal polymerization initiators are not particularly limited, but examples include azo polymerization initiators, peroxide polymerization initiators (e.g., persulfates such as dibenzoyl peroxide, tert-butyl permaleate, potassium persulfate, benzoyl peroxide, hydrogen peroxide, etc.), substituted ethane initiators such as phenyl-substituted ethane, aromatic carbonyl compounds, redox polymerization initiators, etc. Among these, the azo polymerization initiator disclosed in Japanese Patent Application Publication No. 2002-69411 is preferred. Examples of the above-mentioned azo polymerization initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionic acid)dimethyl, and 4,4'-azobis-4-cyanovaleric acid. The amount of thermal polymerization initiator used can be the usual amount, for example, it can be selected from a range of 0.01 to 5 parts by mass, preferably 0.05 to 3 parts by mass, per 100 parts by mass of monomer component.

[0079] The above-mentioned photopolymerization initiators are not particularly limited, but examples include benzoin ether-based photopolymerization initiators, acetophenone-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, ketal-based photopolymerization initiators, and thioxanthone-based photopolymerization initiators. Other examples include acylphosphine oxide-based photopolymerization initiators and titanocene-based photopolymerization initiators. Examples of the above-mentioned benzoin ether-based photopolymerization initiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethane-1-one, and anisole methyl ether. Examples of the above acetophenone-based photopolymerization initiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexylphenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone. Examples of the above α-ketol-based photopolymerization initiators include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropan-1-one. Examples of the above aromatic sulfonyl chloride-based photopolymerization initiators include 2-naphthalenesulfonyl chloride. Examples of the above photoactive oxime-based photopolymerization initiators include 1-phenyl-1,1-propanedione-2-(O-ethoxycarbonyl)-oxime. Examples of the above benzoin-based photopolymerization initiators include benzoin. Examples of the above benzyl-based photopolymerization initiators include benzyl. Examples of the benzophenone-based photopolymerization initiators include benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, and α-hydroxycyclohexylphenyl ketone. Examples of the ketal-based photopolymerization initiators include benzyldimethyl ketal.Examples of the thioxanthone-based photopolymerization initiators include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone. Examples of the acylphosphine oxide-based photopolymerization initiators include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. Examples of the titanocene-based photopolymerization initiators include bis(η. 5 Examples include -2,4-cyclopentadiene-1-yl)bis(2,6-difluoro-3-(1H-pyrrole-1-yl)-phenyl)titanium. The amount of photopolymerization initiator used can be the usual amount, for example, it can be selected from a range of 0.01 to 5 parts by mass, preferably 0.05 to 3 parts by mass, per 100 parts by mass of monomer component.

[0080] The adhesive layer described above may contain other components besides those listed above, as needed. Examples of these other components include curing catalysts, crosslinking agents (including polyfunctional (meth)acrylates), crosslinking accelerators, polymerization initiators, tackifying resins (rosin derivatives, polyterpene resins, petroleum resins, oil-soluble phenols, etc.), oligomers, antioxidants, fillers (metal powders, organic fillers, inorganic fillers, etc.), colorants (pigments, dyes, etc.), antioxidants, plasticizers, softeners, surfactants, antistatic agents, surface lubricants, leveling agents, light stabilizers, UV absorbers, sensitizers, polymerization inhibitors, granular materials, foil-like materials, flame retardants, silane coupling agents, and ion trapping agents. Each of these other components may be used individually or in combination of two or more.

[0081] The above crosslinking agents are not particularly limited as long as they crosslink polymers, but examples include polyisocyanate compounds, epoxy compounds, polyol compounds (such as polyphenol compounds), aziridine compounds, melamine-based crosslinking agents, and polyfunctional (meth)acrylates. Examples of polyfunctional (meth)acrylates include (meth)acrylic acid esters with two or more functions, such as 1,6-hexanediol diacrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. One or more of the above crosslinking agents may be used.

[0082] The above-mentioned silane coupling agent is not particularly limited, but examples include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and N-phenyl-aminopropyltrimethoxysilane. One or more of the above-mentioned silane coupling agents may be used.

[0083] As the above-mentioned coloring agent, a black coloring agent is preferred. As the above-mentioned black coloring agent, known or conventional coloring agents (pigments, dyes, etc.) that produce black can be used, and examples include carbon black (furnace black, channel black, acetylene black, thermal black, lamp black, pine soot, etc.), graphite, copper oxide, manganese dioxide, aniline black, perylene black, titanium black, cyanine black, activated carbon, ferrite (non-magnetic ferrite, magnetic ferrite, etc.), magnetite, chromium oxide, iron oxide, molybdenum disulfide, chromium complex, anthraquinone-based coloring agents, zirconium nitride, etc. Alternatively, a coloring agent that functions as a black coloring agent by combining and blending coloring agents that produce colors other than black may be used.

[0084] When the adhesive layer, etc., contains a coloring agent, the content of the coloring agent in the adhesive layer, etc., is preferably 0.2% by mass or more, and more preferably 0.4% by mass or more, based on 100% by mass of the total amount of the adhesive layer, etc. Furthermore, the content of the coloring agent is, for example, 10% by mass or less, preferably 5% by mass or less, and more preferably 3% by mass or less. The above content can be appropriately set depending on the type of coloring agent and the desired properties.

[0085] The thickness of the adhesive layer, etc. (total thickness of the adhesive layer, etc. on one side) is not particularly limited, but is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. When the thickness is 10 μm or more, the adhesive strength and bonding strength to the adherend are superior. The thickness of the adhesive layer, etc. is, for example, 500 μm or less, preferably 300 μm or less. When the thickness is 500 μm or less, the thickness of the adhesive sheet, etc. can be made thinner. The thickness of the adhesive layers, etc. on both sides may be the same or different.

[0086] The adhesive layer described above may be in any form, for example, an emulsion type, a solvent type (solution type), an active energy ray curing type, or a hot melt type. Among these, the solvent type and the active energy ray curing type are preferred because they make it easier to obtain an adhesive layer with excellent productivity.

[0087] Examples of the active energy rays mentioned above include ionizing radiation such as alpha rays, beta rays, gamma rays, neutron rays, and electron beams, as well as ultraviolet rays, with ultraviolet rays being particularly preferred. In other words, the active energy ray-curable adhesive layer is preferably an ultraviolet-curable adhesive layer.

[0088] The above-mentioned adhesive layer, etc., can be manufactured, for example, by applying an adhesive composition or bonding agent composition for forming the adhesive layer, etc., onto a release liner and drying and curing the resulting adhesive composition layer or bonding agent composition layer, or by applying the above-mentioned adhesive composition or bonding agent composition onto a release liner and curing the resulting adhesive composition layer or bonding agent composition layer by irradiating it with active energy rays. Furthermore, if necessary, it may be further heated and dried.

[0089] [Adhesive sheets and bonding sheets] Adhesive sheets or bonding sheets can be manufactured using the resin film of the present invention as a base material. In this specification, adhesive sheets or bonding sheets may be referred to as "adhesive sheets, etc." In this specification, when "adhesive sheet" is used, tape-like materials, i.e., "adhesive tape," are also included, and the same applies to "bonding sheets." The above-mentioned adhesive sheets, etc. may be double-sided adhesive sheets, etc., where both sides are surfaces of an adhesive layer, etc., or single-sided adhesive sheets, etc., where only one side is a surface of an adhesive layer, etc.

[0090] The above-mentioned adhesive sheet, etc., is an adhesive sheet, etc., comprising a resin film of the present invention as a base material and an adhesive layer, etc., formed on at least one surface of the base material. The above-mentioned "base material (base material layer)" refers to the support, and is the part that is attached to the adherend together with the adhesive layer, etc., when the adhesive sheet, etc. is used (attached) to an adherend. The release liner that is peeled off when the adhesive sheet, etc. is used (attached) is not included in the above-mentioned base material.

[0091] When the above-mentioned adhesive sheet is a single-sided adhesive sheet, the adhesive layer provided may be either an adhesive layer or a bonding layer, but it is preferable that it be an adhesive layer.

[0092] In the case of the above-mentioned adhesive sheet, etc., if it is a double-sided adhesive sheet, the adhesive layers provided on both sides of the base material may both be adhesive layers, both be adhesive layers, or one may be an adhesive layer and the other an adhesive layer, but it is preferable that at least one is an adhesive layer. Furthermore, the adhesive layers provided on both sides of the base material in the above-mentioned adhesive sheet, etc., may be the same adhesive layer, or they may be adhesive layers with different compositions, thicknesses, physical properties, etc. The adhesive layers provided on both sides of the base material may each be a single layer, or they may be a multi-layered layer composed of the same or different layers with different compositions, thicknesses, physical properties, etc.

[0093] The thickness of the adhesive sheet, etc., is preferably 100 to 1500 μm, more preferably 120 to 1200 μm, and even more preferably 150 to 1000 μm. Note that the thickness of the adhesive sheet, etc., refers to the thickness from the adhesive surface or bonding surface to the exposed surface of the substrate in the case of a single-sided adhesive sheet, and the thickness from one adhesive surface or bonding surface to the other adhesive surface or bonding surface in the case of a double-sided adhesive sheet, i.e., the thickness of the adhesive or bonding material, and does not include the release liner.

[0094] The above-mentioned adhesive sheets, etc., may have a release liner on the surface (adhesive surface or bonding surface) of the adhesive layer, etc., until use. In the case of the above-mentioned adhesive sheets, etc., if they are double-sided adhesive sheets, each adhesive surface or bonding surface may be protected by two release liners, or they may be protected in a roll-like form (winding body) by a single release liner with both sides being release surfaces. The release liner is used as a protective material for the adhesive layer, etc., and is peeled off when it is attached to the object to be adhered to. Note that the release liner is not necessarily required.

[0095] Examples of substrates for the above-mentioned peel-off liner include polyethylene film, polypropylene film, polybutene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyethylene terephthalate film, polyethylene naphthalate film, polybutylene terephthalate film, polyurethane film, ethylene vinyl acetate film, ionomer resin film, ethylene-(meth)acrylic acid copolymer film, ethylene-(meth)acrylic acid ester copolymer film, polystyrene film, polycarbonate film, polyimide film, and fluororesin film. Crosslinked films of these are also acceptable. Furthermore, laminated films of these may also be used.

[0096] It is preferable that the release surface of the above-mentioned release liner (particularly the surface in contact with the adhesive layer, etc.) is subjected to a release treatment. Examples of release agents used in the release treatment include alkyd, silicone, fluorine, unsaturated polyester, polyolefin, and wax-based release agents.

[0097] The thickness of the release liner mentioned above is not particularly limited, but is, for example, about 20 to 150 μm.

[0098] The substrate to which the above-mentioned adhesive sheet, etc., is bonded is not particularly limited, but other resin films can be used. Furthermore, if the above-mentioned adhesive sheet, etc., is a double-sided adhesive sheet, one side may be bonded to one of the above-mentioned other resin films, and the other side may be bonded to another substrate.

[0099] Figure 4 shows one embodiment of the adhesive sheet etc. attached to an object. The adhesive sheet etc. 13 shown in Figure 4 comprises the resin film 1 of the present invention, an adhesive layer etc. (adhesive layer or adhesive layer) 23 formed on one side of the resin film 1, and an adhesive layer 24 formed on the other side of the resin film 1. Another resin film 33 is bonded to the adhesive layer etc. 23. The adhesive sheet etc. 13 to which the other resin film 33 is bonded has the adhesive layer 24 side bonded to the object 7. In this way, the other resin film 33 is fixed to the object 7 via the adhesive sheet etc. 13. By using the resin film 1 of the present invention as the base material of the adhesive sheet etc. 13, when exposed to a high temperature and high humidity environment in the state shown in Figure 4, peeling is less likely to occur between the other resin film 33 and the adhesive layer etc. 23, between the resin film 1 and the adhesive layer etc. 23, and between the resin film 1 and the adhesive layer 24.

[0100] The uses of the above-mentioned adhesive sheets are not particularly limited and can be used for any purpose. For example, they can be used in optical applications, that is, for bonding to optical components. Using the above-mentioned adhesive sheets in optical applications provides excellent reliability. For example, one side of the above-mentioned adhesive sheet can be laminated with the above-mentioned resin film, which is the adherend, via an adhesive layer, and the other side can be bonded to another adherend such as a glass substrate via an adhesive layer.

[0101] The adhesive sheets mentioned above are used, for example, in optical components of electrical and electronic equipment to attach (mount) various components or parts to predetermined locations (e.g., housing, front panel, window section, etc.). "Electrical and electronic equipment" refers to equipment that falls under at least one of either electrical equipment or electronic equipment. Examples of electrical and electronic equipment include image display devices such as liquid crystal displays, organic / inorganic electroluminescent displays, and plasma displays, as well as portable electronic devices. Examples of image display devices include image display devices in portable electronic devices, in-vehicle displays, and digital signage (electronic billboards). The image display devices may be of a so-called "rigid" or "flexible" form (structure), or they may be of a form (structure) that can be bent or folded, such as a so-called "foldable" or "rollable" form (structure).

[0102] Examples of the above-mentioned portable electronic devices include mobile phones, smartphones, tablet computers, notebook computers, various wearable devices (for example, wristwear-type devices worn on the wrist like watches, modular devices attached to a part of the body with clips or straps, eyewear-type devices including glasses (monocular and binocular types, including head-mounted types), clothing-type devices attached to shirts, socks, hats, etc. as accessories, earwear-type devices attached to the ears like earphones, etc.), digital cameras, digital video cameras, audio equipment (portable music players, IC recorders, etc.), calculators (calculators, etc.), portable game consoles, electronic dictionaries, electronic organizers, e-books, in-car information systems, portable radios, portable televisions, portable printers, portable scanners, and portable modems. In this specification, "portable" means not merely being able to carry something, but having a level of portability that allows an individual (a typical adult) to carry it relatively easily. [Examples]

[0103] The present invention will be described in more detail below with reference to examples, but the present invention is not limited in any way by these examples.

[0104] Manufacturing Example 1 [Preparation of adhesive (1)] (Preparation of acrylic prepolymer solution A) In a separable flask equipped with a thermometer, stirrer, reflux condenser, and nitrogen gas inlet tube, the following monomer components were added: 78 parts by mass of 2-ethylhexyl acrylate (2-EHA), 18 parts by mass of N-vinyl-2-pyrrolidone (NVP), 5 parts by mass of 2-hydroxyethyl acetate (HEA), 0.035 parts by mass of photopolymerization initiator (trade name "omnirad 184," manufactured by IGM Resins Italia Srl), and 0.035 parts by mass of photopolymerization initiator (trade name "omnirad 651," manufactured by IGM Resins Italia Srl). After that, nitrogen gas was introduced and nitrogen purging was performed for approximately 1 hour while stirring. Subsequently, the nitrogen was purged at 5 mW / cm². 2 Polymerization was carried out by irradiating with ultraviolet light, and the reaction rate was adjusted to 5-15% to obtain acrylic prepolymer solution A.

[0105] (Preparation of acrylic oligomer solution) 100 parts by mass of toluene, 60 parts by mass of dicyclopetanyl methacrylate (DCPMA) (trade name "FA-513M", manufactured by Hitachi Chemical Co., Ltd.), 40 parts by mass of methyl methacrylate (MMA), and 3.5 parts by mass of α-thioglycerol as a chain transfer agent were placed in a four-necked flask. The mixture was then stirred at 70°C under a nitrogen atmosphere for 1 hour, after which 0.2 parts by mass of AIBN was added as a thermal polymerization initiator, and the mixture was reacted at 70°C for 2 hours, followed by a reaction at 80°C for 2 hours. Subsequently, the reaction mixture was placed under a temperature atmosphere of 130°C, and toluene, chain transfer agent, and unreacted monomers were dried off to obtain a solid acrylic oligomer. The Tg of this acrylic oligomer was 144°C, and the Mw was 4300. 50 parts by mass of 2-ethylhexyl acrylate (2-EHA) was added to 50 parts by mass of the above acrylic oligomer and dissolved to obtain an acrylic oligomer solution.

[0106] (Preparation of adhesive (1)) To an acrylic prepolymer solution A (total amount 100 parts by mass), 17.6 parts by mass of 2-hydroxyethyl acrylate (HEA), 11.8 parts by mass of an acrylic oligomer solution, 0.088 parts by mass of a bifunctional monomer (trade name "NK Ester A-HD-N", manufactured by Shin-Nakamura Chemical Industry Co., Ltd.), and 0.353 parts by mass of a silane coupling agent (trade name "KBM-403", manufactured by Shin-Etsu Chemical Co., Ltd., 3-glycidoxypropyltrimethoxysilane) were added to obtain adhesive (1).

[0107] Manufacturing Example 2 [Preparation of adhesive (2)] (Preparation of acrylic prepolymer solution B) In a separable flask equipped with a thermometer, stirrer, reflux condenser, and nitrogen gas inlet tube, 67 parts by mass of butyl acrylate (BA), 14 parts by mass of cyclohexyl acrylate (CHA), 19 parts by mass of 4-hydroxybutyl acrylate (4-BHA), 0.09 parts by mass of photopolymerization initiator (trade name "omnirad 184," manufactured by IGM Resins Italia Srl), and 0.09 parts by mass of photopolymerization initiator (trade name "omnirad 651," manufactured by IGM Resins Italia Srl) were added as monomer components. Then, nitrogen gas was introduced and nitrogen purging was performed for approximately 1 hour while stirring. After that, the nitrogen was purged at 5 mW / cm². 2 Polymerization was carried out by irradiating with ultraviolet light, and the reaction rate was adjusted to 5-15% to obtain acrylic prepolymer solution B.

[0108] (Preparation of adhesive (2)) To an acrylic prepolymer solution B (total volume 100 parts by mass), 9 parts by mass of 2-hydroxyethyl acrylate (HEA), 8 parts by mass of 4-hydroxybutyl acrylate (4-HBA), 0.1 parts by mass of dipentaerythritol hexaacrylate (trade name "KAYARAD DPHA", manufactured by Shin-Nakamura Chemical Industry Co., Ltd.) as a polyfunctional monomer, and 0.4 parts by mass of a silane coupling agent (trade name "KBM-403", manufactured by Shin-Etsu Chemical Co., Ltd., 3-glycidoxypropyltrimethoxysilane) were added to obtain adhesive (2).

[0109] Example 1 (Production of resin film) After vacuum-drying product "DURABIO" (manufactured by Mitsubishi Chemical Corporation, polycarbonate resin) at 80°C for 5 hours, a polycarbonate resin film roll with a thickness of 180 μm (saturated water absorption rate of 1.5%) was produced using a film manufacturing apparatus equipped with a single-screw extruder (manufactured by Shibaura Machinery Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 300 mm, setting temperature: 250°C), a chill roll (setting temperature: 120~130°C), and a winding machine.

[0110] The above polycarbonate resin film raw material was heated at 120°C for 5 minutes while applying a tensile stress of 60N in the MD direction, without applying tensile stress in the TD direction, to produce the polycarbonate resin film of Example 1 (thickness 179 μm, saturated water absorption rate 1.5%).

[0111] (Preparation of double-sided adhesive sheets) Adhesive (1) was applied to a 38 μm thick release liner (product name "MRF#38", manufactured by Mitsubishi Chemical Corporation) with one side of the polyester film being the release surface, and the cumulative light intensity was 3600 mJ / cm² using a black light. 2 The material was irradiated and polymerized until it reached the desired state. After irradiation, a 25 μm thick adhesive layer (1) was created by covering the coated surface with the release side of a 38 μm thick release liner (product name "MRE#38", manufactured by Mitsubishi Chemical Corporation), in which one side of the polyester film is the release surface.

[0112] Adhesive (2) was applied to a 38 μm thick release liner (product name "MRF#38", manufactured by Mitsubishi Chemical Corporation) with one side of the polyester film being the release surface, and the cumulative light intensity was 3600 mJ / cm² using a black light. 2 The material was irradiated and polymerized until it reached the desired state. After irradiation, a 100 μm thick adhesive layer (2) was created by covering the coated surface with the release side of a 38 μm thick release liner (product name "MRE#38", manufactured by Mitsubishi Chemical Corporation), in which one side of the polyester film is the release surface.

[0113] The adhesive layer (1) was laminated to one side of the polycarbonate resin film, and the adhesive layer (2) was laminated to the other side. In this way, adhesive layers (1) and (2) were laminated on both sides of the polycarbonate resin film, and a release liner was laminated to both adhesive layers, thereby creating a double-sided adhesive sheet.

[0114] Example 2 (Production of resin film) The polycarbonate resin film raw material prepared in Example 1 was heated at 120°C for 5 minutes while applying a tensile stress of 60N in the MD direction and also applying a tensile stress of 60N on both sides in the TD direction to produce the polycarbonate resin film of Example 2 (thickness 177 μm, saturated water absorption rate 1.5%).

[0115] (Preparation of double-sided adhesive sheets) A double-sided adhesive sheet was prepared in the same manner as in Example 1, except that the polycarbonate resin film of Example 2 was used instead of the polycarbonate resin film of Example 1.

[0116] Example 3 (Production of resin film) The polycarbonate resin film raw material prepared in Example 1 was heated at 120°C for 5 minutes while applying a tensile stress of 390N in the MD direction and a tensile stress of 450N on both sides in the TD direction to produce the polycarbonate resin film of Example 3 (thickness 170 μm, saturated water absorption rate 1.5%).

[0117] (Preparation of double-sided adhesive sheets) A double-sided adhesive sheet was prepared in the same manner as in Example 1, except that the polycarbonate resin film of Example 3 was used instead of the polycarbonate resin film of Example 1.

[0118] Example 4 (Production of resin film) A polyester resin film roll (product name "Diafoil S100", manufactured by Mitsubishi Chemical Corporation, thickness 188 μm) was heated at 120°C for 5 minutes while applying tensile stress of 30 N on both sides in the TD direction, without applying tensile stress in the MD direction, to produce the polyester resin film of Example 4 (thickness 186 μm, saturated water absorption rate 0.7%).

[0119] (Preparation of double-sided adhesive sheets) A double-sided adhesive sheet was prepared in the same manner as in Example 1, except that the polyester resin film of Example 4 was used instead of the polycarbonate resin film of Example 1.

[0120] Comparative Example 1 (Preparation of double-sided adhesive sheets) A double-sided adhesive sheet was prepared in the same manner as in Example 1, except that the polycarbonate resin film raw material prepared in Example 1 was used instead of the polycarbonate resin film used in Example 1.

[0121] Comparative Example 2 (Production of resin film) The polycarbonate resin film raw material prepared in Example 1 was heated at 120°C for 5 minutes without applying tensile stress in both the MD and TD directions to produce the polycarbonate resin film of Comparative Example 2 (thickness 183 μm, saturated water absorption rate 1.5%).

[0122] (Preparation of double-sided adhesive sheets) A double-sided adhesive sheet was prepared in the same manner as in Example 1, except that the polycarbonate resin film of Comparative Example 2 was used instead of the polycarbonate resin film of Example 1.

[0123] Comparative Example 3 (Production of resin film) The polycarbonate resin film raw material prepared in Example 1 was heated at 120°C for 5 minutes while applying a tensile stress of 390N in the MD direction and a tensile stress of 600N on both sides in the TD direction to produce the polycarbonate resin film of Comparative Example 3 (thickness 166 μm, saturated water absorption rate 1.5%).

[0124] (Preparation of double-sided adhesive sheets) A double-sided adhesive sheet was prepared in the same manner as in Example 1, except that the polycarbonate resin film of Comparative Example 3 was used instead of the polycarbonate resin film of Example 1.

[0125] Comparative Example 4 (Preparation of double-sided adhesive sheets) A double-sided adhesive sheet was prepared in the same manner as in Example 1, except that a polyester resin film roll (product name "Diafoil S100", manufactured by Mitsubishi Chemical Corporation, saturated water absorption rate 0.7%) was used instead of the polycarbonate resin film used in Example 1.

[0126] <Rating> The resin films and double-sided adhesive sheets obtained in the examples and comparative examples were evaluated as follows. The results are shown in the table.

[0127] (1) Heat shrinkage rate, high humidity expansion rate For the resin film, a 100mm x 100mm test piece was cut out, and scoring points were placed 20mm from the midpoint of each of the four sides toward the center. The distance 'a' between opposite scoring points was measured in a room temperature environment of 25°C and 50% RH. For the heat shrinkage rate, the test piece was placed in an environmental testing machine set to 120°C for 5 minutes. For the high humidity expansion rate, the test piece was placed in an environmental testing machine set to 85°C and 85% RH for 30 minutes. After that, the test piece was removed from the environmental testing machine and returned to the same environment as before, room temperature of 25°C and 50% RH. The distance a' between the scoring points was then measured using a planar biaxial dimension measuring device (product name "QVA1517-PRO_AE1M(SP)", manufactured by Mitutoyo Corporation). The heat shrinkage rate was calculated in the MD direction and the TD direction respectively using the following formula (1), and the high humidity expansion rate was calculated using the following formula (2). The heat shrinkage rate X of the resin film was denoted as A, and the high-humidity expansion rate Y was denoted as B. The table shows the larger of the two values, one in the MD direction and the other in the TD direction. Heat shrinkage rate X[%]=(a-a') / a×100 (1) High humidity expansion coefficient Y[%]=(a'-a) / a×100 (2)

[0128] (2) Saturated water absorption rate Measurements were taken in accordance with JIS K7209.

[0129] (3) Peeling test The release liner was peeled off the double-sided adhesive sheet to expose the adhesive layer (1), and a triacetylcellulose (TAC) film (product name "KC4UY", manufactured by Konica Minolta, Inc.) was laminated to the exposed adhesive layer (1). Then, the release liner was peeled off the double-sided adhesive sheet to expose the adhesive layer (2), and the exposed adhesive layer (2) was laminated to an acrylic glass plate. In this way, an evaluation sample consisting of a laminated structure of [TAC film / adhesive layer (1) / resin film / adhesive layer (2) / acrylic glass plate] was prepared. The above evaluation sample was placed in an environmental testing machine set to a temperature of 85°C and a humidity of 85%RH for 30 minutes. After that, the evaluation sample was removed from the environmental testing machine and placed in a room temperature environment of 25°C and a humidity of 50%RH, and it was visually checked whether peeling had occurred between the TAC film and adhesive layer (1), between the resin film and adhesive layer (1), and between the resin film and adhesive layer (2). We evaluated the results as follows: "○" if no peeling occurred, and "×" if peeling occurred in at least one place.

[0130] (4) High humidity shrinkage rate For the TAC film, a 100mm x 100mm test piece was cut out, and scoring points were placed 20mm from the midpoint of each of the four sides toward the center. The distance b between opposite scoring points was measured in a room temperature environment of 25°C and 50% RH. The test piece was then placed in an environmental testing machine set to 85°C and 85% RH for 30 minutes. After that, the test piece was removed from the environmental testing machine and returned to the same environment as before, room temperature of 25°C and 50% RH. The distance b' between the scoring points was then measured using a planar biaxial dimension measuring device (product name "QVA1517-PRO_AE1M(SP)", manufactured by Mitutoyo Corporation). The high-humidity shrinkage rate was then calculated for both the MD and TD directions using the following formula (3). The high-humidity shrinkage rate Z of the TAC film was denoted as C. The table shows the larger of the MD and TD directions. High humidity shrinkage rate Z[%]=(b-b') / b×100 (3)

[0131] [Table 1]

[0132] As shown in Table 1, it was confirmed that no peeling occurred when a resin film with an A / B ratio within a specific range was used (Example). On the other hand, peeling occurred when the A / B ratio was low or high (Comparative Example). Furthermore, it was confirmed that no peeling occurred in the peeling test described in (3) above for a double-sided adhesive sheet obtained in the same manner as in Example 1, except that an acrylic resin film with an A / B ratio within the range of 0.3 to 2.5 was used instead of the polycarbonate resin in Example 1.

[0133] The following describes variations of the invention relating to this disclosure. [Note 1] A resin film used by laminating an adhesive layer or bonding layer on at least one surface, wherein the ratio [former / latter] of the shrinkage rate when heated at 120°C for 5 minutes to the expansion rate when stored in an environment of 85°C and 85% RH for 30 minutes is 0.3 to 2.5. [Note 2] The resin film according to Note 1, obtained by heat treatment while applying tensile stress in at least one direction. [Note 3] A resin film according to Note 1 or 2, comprising one or more resins, mainly composed of polycarbonate resin, polyester resin, acrylic resin, cellulose resin, and cycloolefin resin. [Note 4] A resin film according to any one of Notes 1 to 3, wherein an adhesive layer is laminated on one side, and another resin film is laminated on the other side via the adhesive layer or the bonding layer. [Note 5] The resin film as described in Note 4, wherein the ratio [former / latter] of the expansion rate to the shrinkage rate when the other resin film is stored in an environment of 85°C and 85%RH humidity for 30 minutes is 1.0 to 3.0. [Explanation of Symbols]

[0134] 1. The resin film of the present invention 1' Raw material film 10,13 Adhesive sheets, etc. (adhesive sheets or bonding sheets) 11,12 Coiled bodies 21,22 Adhesive layer 23. Adhesive layer, etc. (adhesive layer or bonding layer) 24 Adhesive layer 31,32 Peel-off liner 33 Other resin films 41, 42 Protective film 5. Oven 51 Hot air blower 61, 62, 63, 64 rolls 7 Adherent

Claims

1. This is a resin film used by laminating an adhesive layer on one side and laminating another resin film on the other side via the adhesive layer or bonding layer. It contains one or more resins as its main component, consisting of polycarbonate resins, polyester resins, acrylic resins, cellulose resins, and cycloolefin resins. The ratio [former / latter] of the shrinkage rate when heated at 120°C for 5 minutes to the expansion rate when stored at 85°C and 85% RH for 30 minutes is 0.3 to 2.

5. A resin film in which the ratio [former / latter] of the expansion rate to the shrinkage rate when the other resin film is stored in an environment of 85°C and 85% RH for 30 minutes is 1.0 to 3.

0.

2. The resin film according to claim 1, obtained by heat-treating a raw material film while applying tensile stress in at least one direction.

Citation Information

Patent Citations

  • Optical member

    JP2002303730A

  • Surface protection film for transparent electrical conductive film, its production method and transparent electrical conductive film having surface protenction film

    JP2004059860A

  • Transparent conductive film laminate and touch panel obtained by using the same, as well as production method of transparent conductive film

    JP2016107503A

  • Film laminate for touch panel

    JP2018116543A

  • Biaxially oriented polyester film

    JP2020063399A