Non-aqueous electrolyte and non-aqueous electrolyte battery using the non-aqueous electrolyte

A non-aqueous electrolyte with specific cyclic sulfur-containing compounds and anion-containing compounds forms a robust coating on the electrode, addressing brittle coatings and side reactions, thereby improving recovery capacity and performance in lithium-ion secondary batteries.

JP7954024B2Active Publication Date: 2026-11-19MU IONIC SOLUTIONS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022125415
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-06
Filing Date
2022-08-05
Publication Date
2026-11-19
Estimated Expiration
2042-08-05

AI Technical Summary

Technical Problem

Existing non-aqueous electrolytes for lithium-ion secondary batteries face issues with brittle negative electrode coatings, side reactions, and insufficient recovery capacity maintenance rates.

Method used

A non-aqueous electrolyte containing a specific cyclic sulfur-containing compound and one or more anion-containing compounds, such as phosphate anion-containing compounds with PF bonds and P=O bonds, anion-containing compounds with S=O bonds, or oxalate complex anion-containing compounds, is used to form a sparingly soluble and robust co-coating on the electrode, minimizing side reactions.

Benefits of technology

The electrolyte improves the recovery capacity retention rate and suppresses side reactions, enhancing the performance of non-aqueous electrolyte batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954024000001
    Figure 0007954024000001
  • Figure 0007954024000002
    Figure 0007954024000002
  • Figure 0007954024000003
    Figure 0007954024000003
Patent Text Reader

Abstract

To provide a non-aqueous electrolyte that can enhance the recovery capacity retention.SOLUTION: A non-aqueous electrolyte contains an electrolyte, a compound (A) represented by formula (I), and one or more anion-containing compounds (B) selected from the group consisting of phosphate anion-containing compounds having a P-F bond and a P=O bond, anion-containing compounds having an S=O bond, and oxalate complex anion-containing compounds. The content of the anion-containing compounds (B) in the electrolyte is from 0.001 mass% to 5 mass% inclusive.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a non-aqueous electrolyte and a non-aqueous electrolyte battery using the non-aqueous electrolyte. [Background technology]

[0002] Energy devices, such as lithium-ion secondary batteries and other non-aqueous electrolyte batteries, are being put into practical use in a wide range of applications, from power supplies for so-called consumer electronics such as mobile phones and laptop computers to on-board power supplies for automobiles. However, in recent years, the demand for higher performance in non-aqueous electrolyte batteries has been increasing, and in particular, there is a demand for improvements in various battery characteristics such as higher capacity, low-temperature operation characteristics, high-temperature storage characteristics, cycle characteristics, and overcharge safety. To date, numerous technologies have been investigated regarding the active materials of the positive and negative electrodes, as well as various battery components, including the non-aqueous electrolyte, as means of improving the high-temperature storage characteristics and cycle characteristics of non-aqueous electrolyte secondary batteries.

[0003] Patent Document 1 discloses a non-aqueous electrolyte for lithium-ion secondary batteries containing a specific vinylene carbonate compound and a specific vinylethylene sulfite, in order to provide a lithium-ion secondary battery that suppresses gas generation during continuous charging and has excellent discharge characteristics after continuous charging. Patent Document 2 discloses a non-aqueous electrolyte secondary battery that suppresses the increase in the internal resistance of the battery after high-temperature storage and also suppresses the increase in the internal resistance of the battery when the battery is used at low temperatures after high-temperature storage. The non-aqueous electrolyte contains 2% by mass or less of a specific cyclic unsaturated sultone compound and 2% by mass or less of a specific cyclic sulfite ester. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 2005-166553 [Patent Document 2] Japanese Patent Publication No. 2010-92698 [Overview of the Initiative] [Problems that the invention aims to solve]

[0005] The inventors of the present invention have found that the non-aqueous electrolytes described in Patent Documents 1 and 2 have a problem in that the negative electrode coating formed on the negative electrode is brittle, side reactions of the non-aqueous electrolyte occur on the negative electrode, and the improvement of the recovery capacity maintenance rate is insufficient.

[0006] The present invention has been made to solve the above problems, and aims to provide a non-aqueous electrolyte that can improve the recovery capacity retention rate when used in a non-aqueous electrolyte battery, and a non-aqueous electrolyte battery using the said non-aqueous electrolyte. [Means for solving the problem]

[0007] In view of the above circumstances, the inventors of the present invention conducted diligent studies and found that the above problems can be solved by using a non-aqueous electrolyte containing a specific cyclic sulfur-containing compound and one or more anion-containing compounds selected in a specific amount from the group consisting of a phosphate anion-containing compound having a PF bond and a P=O bond, an anion-containing compound having an S=O bond, and an oxalate complex anion-containing compound, and thus completed the present invention. In other words, the gist of the present invention is as follows:

[0008] [1] A non-aqueous electrolyte characterized by containing a compound (A) represented by formula (I) and one or more anion-containing compounds (B) selected from the group consisting of phosphate anion-containing compounds having PF bonds and P=O bonds, anion-containing compounds having S=O bonds, and oxalate complex anion-containing compounds, wherein the content of the anion-containing compound (B) is 0.001% by mass or more and 5% by mass or less in the electrolyte.

[0009] [ka] (In formula (I), X 1 and X 2 are each independently an oxygen atom or CH2, R 1 and R 2 are each independently a hydrogen atom, a halogen atom, or a hydrocarbon group, and n is 1 or 2. Provided that either one of R 1 and R 2 is a hydrocarbon group containing at least one carbon-carbon unsaturated bond, and when n is 2, at least one of X 1 and X 2 is CH2.)

[0010] [2] The non-aqueous electrolyte according to [1], wherein the compound (A) is a compound represented by the following formula (II).

[0011] [Chemical Formula] (In formula (II), R 1 and R 2 are the same as R 1 and R 2 in the aforementioned formula (I.) [3] R 1 and R 2 are each independently one selected from a hydrogen atom, a halogen atom, a vinyl group, or an allyl group, and either one of R 1 and R 2 is selected from a vinyl group and an allyl group, the non-aqueous electrolyte according to [1] or [2]. [4] The non-aqueous electrolyte according to any one of [1] to [3], containing the compound (A) in an amount of 0.01 mass% or more and 10 mass% or less. [5] The non-aqueous electrolyte according to any one of [1] to [4], further comprising a chain carboxylic acid ester. [6] The non-aqueous electrolyte according to [5], wherein the chain carboxylic acid ester is methyl acetate or methyl propionate. [7] The non-aqueous electrolyte according to any one of [5] or [6], wherein the content of the chain carboxylic acid ester in the non-aqueous solvent is 1 volume% or more and 70 volume% or less. [8] A non-aqueous electrolyte battery comprising a positive electrode having a positive electrode active material capable of intercepting and releasing metal ions, a negative electrode having a negative electrode active material capable of intercepting and releasing metal ions, and a non-aqueous electrolyte according to any one of [1] to [7]. [Effects of the Invention]

[0012] According to the present invention, it is possible to provide a non-aqueous electrolyte that can improve the recovery capacity retention rate when used in a non-aqueous electrolyte battery. Furthermore, it is possible to provide a non-aqueous electrolyte battery equipped with this non-aqueous electrolyte. [Modes for carrying out the invention]

[0013] [1.Non-aqueous electrolyte] The non-aqueous electrolyte of the present invention is a non-aqueous electrolyte for a non-aqueous electrolyte battery, This is a non-aqueous electrolyte characterized by containing an electrolyte, a compound (A) represented by formula (I) (hereinafter also referred to as "compound (A)"), and at least one anion-containing compound (B) (hereinafter also referred to as "anion-containing compound (B)") selected from the group consisting of phosphate anion-containing compounds having PF bonds and P=O bonds, anion-containing compounds having S=O bonds, and oxalate complex anion-containing compounds, wherein the content of the anion-containing compound (B) is 0.001% by mass or more and 5% by mass or less in the electrolyte.

[0014] The inventors speculate that the reason why the non-aqueous electrolyte having the structure of the present invention exhibits such excellent effects is as follows: During charging and discharging of the non-aqueous electrolyte battery, the carbon-carbon unsaturated bonds of compound (A), preferably those contained in aliphatic groups, react on the electrode, causing compound (A) to increase in quantity. This increased quantity of compound (A) then reacts with the anion-containing compound (B), forming a sparingly soluble and robust co-coating on the electrode containing S=O bonds and structures derived from the anion-containing compound (B). This is thought to suppress side reactions between the electrode active material and the solvent. The sparingly soluble and robust co-coating on the electrode containing S=O bonds and structures derived from the anion-containing compound (B) can significantly suppress side reactions between the electrode active material and the solvent compared to coatings made of polymers of compounds containing carbon-carbon unsaturated bonds but not S=O bonds, or coatings that do not contain structures derived from the anion-containing compound (B).

[0015] [1-1. Compound (A) represented by formula (I)]

[0016] [ka]

[0017] In formula (I), X 1 and X 2 Each is independently an oxygen atom or CH2, and R 1 and R 2 Each of these is independently a hydrogen atom, a halogen atom, or a hydrocarbon group, and n is 1 or 2. However, R 1 and R 2 Either one of them is a hydrocarbon group containing at least one carbon-carbon unsaturated bond, and when n is 2, X 1 and X 2 At least one of them is CH2.

[0018] Among these, X 1 X is an oxygen atom. 2 A sulfite ester structure where is an oxygen atom and n is 1; X 1 X is an oxygen atom. 2Preferably, the structure is a sulfonic acid ester structure where is CH2 and n is 2; X 1 X is an oxygen atom. 2 A sulfite ester structure in which is an oxygen atom and n is 1 is more preferable.

[0019] R 1 and R 2 Either of these is a hydrocarbon group containing at least one carbon-carbon unsaturated bond. Examples of hydrocarbon groups containing at least one carbon-carbon unsaturated bond include alkenyl groups with 2 to 8 carbon atoms, alkynyl groups with 2 to 8 carbon atoms, aryl groups with 4 to 12 carbon atoms, or aralkyl groups with 7 to 10 carbon atoms. The aryl and aralkyl groups include heteroaryl and heteroaralkyl groups in which any carbon atom constituting the aromatic ring is substituted with a heteroatom. 1 , R 2 When is a hydrocarbon group containing a carbon-carbon unsaturated bond, an alkenyl group having 2 to 8 carbon atoms or an alkynyl group having 2 to 8 carbon atoms is preferred, and an alkenyl group having 2 to 8 carbon atoms is more preferred. R 1 and R 2 However, in the case of saturated hydrocarbon groups, examples of hydrocarbon groups include alkyl groups having 1 to 10 carbon atoms.

[0020] Examples of alkenyl groups include vinyl, allyl, methallyl, 2-butenyl, 3-methyl-2-butenyl, 3-butenyl, 4-pentenyl, 5-hexenyl, 6-heptenyl, and 7-octenyl groups. Among these, alkenyl groups having 2 to 6 carbon atoms are preferred from the viewpoint of solubility in the electrolyte, and vinyl and allyl groups are more preferred.

[0021] Examples of alkynyl groups include ethynyl, 2-propynyl, 2-butynyl, 3-butynyl, 4-pentynyl, 5-hexynyl, 6-heptynyl, and 7-octinyl groups. Among these, alkynyl groups with 2 to 6 carbon atoms are preferred from the viewpoint of solubility in the electrolyte, and ethynyl groups are more preferred.

[0022] Examples of aryl groups include phenyl, 1-naphthyl, 2-naphthyl, 2-thienyl, 3-thienyl, 2-furyl, 3-furyl, 2-pyrrolyl, 3-pyrrolyl, and benzyl groups. Among these, aryl groups with 6 to 12 carbon atoms are preferred from the viewpoint of solubility in electrolytes, and phenyl groups are more preferred.

[0023] Examples of aralkyl groups include benzyl groups, phenethyl groups, phenylpropyl groups, phenylbutyl groups, and phenylisopropyl groups. Among these, benzyl groups and phenethyl groups are preferred from the viewpoint of electrolyte solubility, and benzyl groups are more preferred.

[0024] Examples of alkyl groups include methyl, ethyl, n-propyl, iso-propyl, n-butyl, tert-butyl, n-pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups. Among these, alkyl groups having 1 to 6 carbon atoms are preferred from the viewpoint of solubility in the electrolyte, and methyl, ethyl, and iso-propyl groups are more preferred.

[0025] R in equation (I) 1 and R 2 These may be bonded together to form a cyclic structure. Examples of cyclic structures include unsaturated carbon rings other than aromatic rings, such as cyclohexene rings and cyclopentene rings. Among these, cyclohexene rings are preferred from the viewpoint of stability in electrolytes.

[0026] Also, R 1 or R 2 If the group is a hydrocarbon group, the carbon atoms in the hydrocarbon group may be substituted with oxygen atoms, and the hydrogen atoms may be substituted with halogen atoms. Examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, or iodine atoms.

[0027] Since compound (A) tends to react and increase in volume on the electrode, in formula (I), R 1 and R 2Preferably, each is independently selected from a hydrogen atom, a halogen atom, a vinyl group, and an allyl group, R 1 and R 2 Either one of them is selected from vinyl groups and allyl groups. Among them, R 1 and R 2 A combination in which one of the elements is a vinyl group and the other is a hydrogen atom is preferred.

[0028] Among the compounds (A) represented by formula (I), X 1 X is an oxygen atom. 2 A compound represented by the following formula (II) is preferred, having a sulfite ester structure in which is an oxygen atom and n is 1.

[0029] [ka]

[0030] In formula (II), R 1 and R 2 R in equation (I) 1 and R 2 It is synonymous with [the above].

[0031] Examples of compounds represented by formula (II) include those represented by the following structural formulas.

[0032] [ka]

[0033] [ka]

[0034] [ka]

[0035] Among the compounds listed above, the compound represented by formula (II) is preferably the one represented by the following structural formula.

[0036] [ka]

[0037] Among the compounds represented by formula (II) above, compounds represented by the following structural formula are more preferably included.

[0038] [ka]

[0039] Among the compounds represented by formula (II) above, compounds represented by the following structural formula are even more preferred.

[0040] [ka]

[0041] Among the compounds represented by the above formula (II), the compounds represented by the following structural formula are particularly preferred.

[0042] [ka]

[0043] Among the compounds represented by the above formula (II), the most preferred is the compound represented by the following structural formula.

[0044] [ka]

[0045] Furthermore, specific examples of compounds represented by formula (I) other than those represented by formula (II) are shown below.

[0046] In formula (I), X 1 CH2, X 2Examples of compounds having a sulfone structure where is CH2 and n is 2 include the compounds represented by the following structural formulas.

[0047] [ka]

[0048] In formula (I), X 1 X is an oxygen atom. 2 Examples of compounds having a sulfonic acid ester structure in which is CH2 and n is 2 include the compounds represented by the following structural formulas.

[0049] [ka]

[0050] In formula (I), X 1 CH2, X 2 Examples of compounds having a sulfonic acid ester structure in which is an oxygen atom and n is 2 include the compounds represented by the following structural formulas.

[0051] [ka]

[0052] (Content of compound (A)) The content of compound (A) in the total amount (100% by mass) of the non-aqueous electrolyte is usually 0.01% by mass or more, preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and usually 10% by mass or less, preferably 8% by mass or less, more preferably 6% by mass or less, and even more preferably 4% by mass or less. If the content of compound (A) is within this range, the generation of initial gas and gas generation after high-temperature storage can be suppressed in the non-aqueous electrolyte battery. Compound (A) may be used alone or two or more may be used in any combination and ratio. The identification and measurement of the content of compound (A) are performed by nuclear magnetic resonance (NMR) spectroscopy and / or gas chromatography.

[0053] (Mass ratio of compound (A) to electrolyte) In a non-aqueous electrolyte, the mass ratio of compound (A) (total amount if there are two or more compounds) to the electrolyte content (compound (A) [g] / electrolyte [g]) is usually 0.001 or higher, preferably 0.01 or higher, more preferably 0.02 or higher, even more preferably 0.025 or higher, even more preferably 0.03 or higher, and usually 0.5 or lower, preferably 0.3 or lower, more preferably 0.2 or lower, and even more preferably 0.1 or lower. If the mass ratio is within this range, the battery characteristics, especially the recovery capacity retention rate, can be significantly improved. The principle behind this effect is not clear, but it is thought that by setting the mass ratio of compound (A) to electrolyte content within this range, side reactions of the electrolyte within the battery system are minimized.

[0054] [1-2. Anion-containing compounds (B)] The anion-containing compound (B) is selected from phosphate anion-containing compounds having PF bonds and P=O bonds, anion-containing compounds having S=O bonds, and oxalate complex anion-containing compounds. The anion-containing compound (B) may be used alone or two or more may be used in any combination and ratio. Among these, from the viewpoint of improving the recovery capacity maintenance rate, compounds containing phosphate anions having PF bonds and P=O bonds or anions having S=O bonds are preferred, and compounds containing difluorophosphate anions or fluorosulfonic acid anions are more preferred. Furthermore, from the viewpoint of suppressing the generation of high-temperature storage gases, the anion-containing compound (B) is preferably a phosphate anion-containing compound or an oxalate complex anion-containing compound having PF bonds and P=O bonds, and more preferably a difluorophosphate anion-containing compound or a boron oxalate complex anion-containing compound. Moreover, from the viewpoint of suppressing deterioration of DCR, the anion-containing compound (B) is even more preferably a phosphate anion-containing compound having PF bonds and P=O bonds.

[0055] [1-2-1. Compounds containing phosphate anions with PF bonds and P=O bonds] The phosphate anion-containing compound having a PF bond and a P=O bond is not particularly limited as long as it is an anion-containing compound derived from phosphoric acid that has a PF bond and a P=O bond in its molecule. Examples of phosphoric acid having a PF bond and a P=O bond include monofluorophosphate represented by the molecular formula H2PO3F and difluorophosphate represented by the molecular formula HPO2F2. Examples of countercations of phosphate anions having PF and P=O bonds include alkali metal cations such as lithium, sodium, and potassium, with lithium cations being particularly preferred. Examples of salts of phosphate anions having PF and P=O bonds include salts of monofluorophosphate anions such as Li2PO3F; and salts of difluorophosphate anions such as LiPO2F2, NaPO2F2, and KPO2F2. In particular, from the viewpoint of balancing the output characteristics of the battery and electrode interface protection, salts of difluorophosphate anions are preferred, and lithium difluorophosphate is more preferred.

[0056] [1-2-2. Anion-containing compounds with an S=O bond] There are no particular restrictions on the anion-containing compound having an S=O bond, as long as it is an anion-containing compound having an S=O bond in its molecule, and any compound can be used as long as it does not significantly impair the effects of the present invention. Examples of acids containing an anion having an S=O bond include fluorosulfonic acid represented by the molecular formula HSO3F, fluorosulfonylimide represented by the molecular formula HN(FSO2), fluorosulfonylmethide represented by the molecular formula HC(FSO2)3, and alkyl sulfuric acid such as CH3SO4H. In addition to alkali metal cations such as lithium, sodium, and potassium, (CH3)4N can be used as countercations for anions with an S=O bond. + (C2H5)4N + FSO3(n-C4H9)4N + Examples of quaternary ammonium cations include the above, with lithium cations being preferred. Examples of salts of anions having an S=O bond include salts of fluorosulfonic acid anions such as LiSO3F, NaSO3F, KSO3F, (CH3)4NSO3F, (C2H5)4NSO3F, and (n-C4H9)4NSO3F; salts of fluorosulfonylimide anions such as LiN(FSO2)2 and LiN(FSO2)(CF3SO2); salts of fluorosulfonylmethide anions such as LiC(FSO2)3; and salts of alkyl sulfate anions such as LiCH3SO4 and LiC2H5SO4. In particular, from the viewpoint of balancing the output characteristics of the battery and the protection of the electrode interface, a salt of fluorosulfonate anion or a salt of fluorosulfonylimide anion is preferred, a salt of fluorosulfonate anion is more preferred, and lithium fluorosulfonate is even more preferred.

[0057] [1-2-3. Compounds containing oxalate complex anions] The oxalate complex anion-containing compound used in the present invention is not particularly limited as long as it is an anion-containing compound having an oxalate complex in its molecule. An oxalate complex anion is an acid anion in which oxalic acid is coordinated to or bonded to a central atom to form a complex. Examples include boron oxalate complex anions in which oxalic acid is coordinated to or bonded to a boron atom, such as bis(oxalate)borate and difluorooxalateborate, and phosphorus oxalate complex anions in which oxalic acid is coordinated to or bonded to a phosphorus atom, such as tris(oxalate)phosphate, difluorobis(oxalate)phosphate and tetrafluorooxalatephosphate. Examples of countercations for the oxalate complex anion include alkali metal cations such as lithium, sodium, and potassium, with lithium cations being particularly preferred. Examples of salts of oxalate complex anions include salts of boron oxalate complex anions such as lithium bis(oxalate)borate and lithium difluorooxalateborate; and salts of phosphorus oxalate complex anions such as lithium tetrafluorooxalate phosphate, lithium difluorobis(oxalate)phosphate and lithium tris(oxalate)phosphate. In particular, from the viewpoint of forming a stable co-coating on the electrode surface, a salt of a boron oxalate complex anion is preferred, and lithium bis(oxalate)borate is more preferred.

[0058] (Content of anion-containing compound (B)) The content of anion-containing compound (B) in the total amount (100% by mass) of the non-aqueous electrolyte (total amount if there are two or more types) is 0.001% by mass or more, preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and 5% by mass or less, preferably 4% by mass or less, and more preferably 3.5% by mass or less. If the content of anion-containing compound (B) is within this range, the battery characteristics, especially the recovery capacity retention rate, can be significantly improved. The principle behind this effect is not clear, but it is thought that if the content of anion-containing compound (B) is within this range, side reactions of the components of the non-aqueous electrolyte on the electrode can be minimized. The identification and measurement of the content of anion-containing compound (B) are performed using nuclear magnetic resonance (NMR) spectroscopy and / or ion chromatography.

[0059] (Mass ratio of anion-containing compound (B) to compound (A)) The mass ratio of the content of anion-containing compound (B) (total amount if there are two or more types) to the content of compound (A) (anion-containing compound (B) [g] / compound (A) [g]) is usually 0.01 or higher, preferably 0.05 or higher, more preferably 0.3 or higher, and usually 100 or lower, preferably 30 or lower, more preferably 10 or lower, more preferably 8 or lower, and even more preferably 5.5 or lower. If this mass ratio is within this range, the battery characteristics, especially the recovery capacity maintenance rate, can be significantly improved. The principle behind this is not entirely clear, but it is thought that by including compound (A) and anion-containing compound (B) within this mass ratio range, side reactions of the non-aqueous electrolyte components on the electrode can be minimized.

[0060] (Mass ratio of anion-containing compound (B) to LiPF6) In a non-aqueous electrolyte, when the electrolyte contains LiPF6, the mass ratio of the anion-containing compound (B) (total amount if there are two or more types) to the LiPF6 content (anion-containing compound (B) [g] / LiPF6 [g]) is usually 0.00005 or higher, preferably 0.001 or higher, more preferably 0.01 or higher, even more preferably 0.02 or higher, and even more preferably 0.025 or higher, and usually 0.5 or lower, preferably 0.45 or lower, more preferably 0.4 or lower, and even more preferably 0.35 or lower. If the mass ratio is within this range, the battery characteristics, especially the recovery capacity retention rate, can be significantly improved. The principle behind this effect is not clear, but it is thought that by including the anion-containing compound (B) and LiPF6 within this mass ratio range, side reactions of LiPF6 within the battery system are minimized.

[0061] [1-3. Electrolytes] Examples of electrolytes for non-aqueous electrolytes include lithium salts. There are no particular restrictions on the lithium salts used, and any can be used, but examples include lithium fluoroborate salts, lithium fluorophosphate salts, lithium tungstate salts, lithium carboxylate salts, lithium sulfonate salts, lithium imide salts, lithium methide salts, lithium oxalate salts, and fluorine-containing organic lithium salts.

[0062] Among these, from the viewpoint of improving low-temperature power characteristics, high-rate charge / discharge characteristics, impedance characteristics, high-temperature storage characteristics, and cycle characteristics, LiBF4 is preferred as a lithium fluoroborate salt; LiPF6 as a lithium fluorophosphate salt; LiCH3SO3 as a lithium sulfonate salt; LiN(CF3SO2)2, LiN(C2F5SO2)2, lithium cyclic 1,2-perfluoroethanedisulfonylimide, and lithium cyclic 1,3-perfluoropropanedisulfonylimide as lithium imide salts; and LiC(CF3SO2)3, LiC(C2F5SO2)3, etc. as lithium methide salts, with LiPF6 being more preferred.

[0063] Electrolytes can be used individually or in combination of two or more in any ratio. There are no particular restrictions on the combination of two or more electrolytes, and examples include combinations of LiPF6 and LiBF4, and combinations of LiPF6 and LiN(CF3SO2)2. Among these, the combination of LiPF6 and LiBF4 is preferred.

[0064] While there are no particular restrictions on the total concentration of the electrolyte, from the viewpoint of ensuring proper electrical conductivity for battery operation and sufficient output characteristics, it is usually 8% by mass or more, preferably 8.5% by mass or more, more preferably 9% by mass or more, and usually 18% by mass or less, preferably 17% by mass or less, and more preferably 16% by mass or less, relative to the total amount of the non-aqueous electrolyte. Identification and measurement of the electrolyte content are performed using nuclear magnetic resonance (NMR) spectroscopy and / or ion chromatography.

[0065] [1-4. Non-aqueous solvents] The non-aqueous electrolyte contains a non-aqueous solvent, similar to a general non-aqueous electrolyte. There are no particular restrictions on the non-aqueous solvent as long as it dissolves the electrolyte; any known organic solvent can be used. Examples of organic solvents include, but are not limited to, saturated cyclic carbonates, linear carbonates, linear carboxylic acid esters, cyclic carboxylic acid esters, cyclic ether compounds, and sulfone compounds.

[0066] Organic solvents can be used individually or in combination of two or more in any ratio. Examples of combinations of two or more organic solvents include combinations of saturated cyclic carbonates and linear carbonates, combinations of cyclic carboxylic acid esters and linear carbonates, and combinations of saturated cyclic carbonates, linear carbonates and linear carboxylic acid esters. Among these, combinations of saturated cyclic carbonates and linear carbonates, and combinations of saturated cyclic carbonates, linear carbonates and linear carboxylic acid esters are preferred, combinations of saturated cyclic carbonates, linear carbonates and methyl acetate or methyl propionate are more preferred, and combinations of saturated cyclic carbonates, linear carbonates and methyl acetate are even more preferred.

[0067] [1-4-1. Saturated Cyclic Carbonates] Examples of saturated cyclic carbonates include those having alkylene groups with 2 to 4 carbon atoms. From the viewpoint of improving battery characteristics due to an increased degree of dissociation of metal ions, particularly lithium ions, saturated cyclic carbonates having alkylene groups with 2 to 3 carbon atoms are preferred. Specific examples of saturated cyclic carbonates include ethylene carbonate, propylene carbonate, and butylene carbonate. Among these, ethylene carbonate or propylene carbonate is preferred, and ethylene carbonate, which is less susceptible to oxidation and reduction, is more preferred. Saturated cyclic carbonates can be used individually or in combination of two or more in any ratio.

[0068] The content of saturated cyclic carbonate is not particularly limited and is arbitrary as long as it does not impair the effects of the invention according to this embodiment. The content of saturated cyclic carbonate is usually 3% by volume or more, preferably 5% by volume or more, more preferably 10% by volume or more, and usually 90% by volume or less, preferably 85% by volume or less, and more preferably 80% by volume or less, based on the total amount of non-aqueous solvent. By keeping it within this range, a decrease in electrical conductivity due to a decrease in the dielectric constant of the non-aqueous electrolyte is avoided, making it easier to achieve good high-current discharge characteristics, stability to the negative electrode, and cycle characteristics of the non-aqueous electrolyte battery, improving the oxidation-reduction resistance of the non-aqueous electrolyte and tending to improve stability during high-temperature storage. In this specification, volume percent refers to volume percent at 25°C and 1 atmosphere.

[0069] [1-4-2. Chain-like carbonates] Examples of chain-like carbonates include those having 3 to 7 carbon atoms, and chain-like carbonates having 3 to 5 carbon atoms are preferred in order to adjust the viscosity of the non-aqueous electrolyte to an appropriate range. Specific examples of chain-like carbonates include dimethyl carbonate, diethyl carbonate, di-n-propyl carbonate, diisopropyl carbonate, n-propylisopropyl carbonate, ethyl methyl carbonate, and methyl-n-propyl carbonate. Among these, one or more selected from dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate are preferred, and dimethyl carbonate, and a combination of dimethyl carbonate and ethyl methyl carbonate are more preferred. Furthermore, chain-like carbonates containing fluorine atoms (hereinafter also referred to as "fluorinated chain-like carbonates") can also be suitably used. The number of fluorine atoms in a fluorinated chain-like carbonate is not particularly limited as long as it is 1 or more, but is preferably 6 or less, and more preferably 4 or less. When a fluorinated chain-like carbonate has multiple fluorine atoms, these multiple fluorine atoms may be bonded to the same carbon or to different carbons. Examples of fluorinated chain carbonates include fluorinated dimethyl carbonate derivatives such as fluoromethylmethyl carbonate; fluorinated ethylmethyl carbonate derivatives such as 2-fluoroethylmethyl carbonate; and fluorinated diethyl carbonate derivatives such as ethyl-(2-fluoroethyl) carbonate. Chain-like carbonates can be used individually or in combination of two or more types in any ratio.

[0070] The content of chain-like carbonates is not particularly limited, but from the viewpoint of setting the viscosity of the non-aqueous electrolyte within an appropriate range, suppressing a decrease in ionic conductivity, and thereby improving the output characteristics of the non-aqueous electrolyte battery, it is usually 15% by volume or more, preferably 20% by volume or more, more preferably 25% by volume or more, and also usually 90% by volume or less, preferably 85% by volume or less, and more preferably 80% by volume or less, relative to the total amount of non-aqueous solvent in the non-aqueous electrolyte.

[0071] Furthermore, by combining specific chain-like carbonates with ethylene carbonate in specific quantities, battery performance can be significantly improved. For example, when dimethyl carbonate and ethyl methyl carbonate are selected as the specific chain carbonates, the ethylene carbonate content is typically 15% by volume or more, preferably 20% by volume or more, more preferably 25% by volume or more, and typically 45% by volume or less, preferably 40% by volume or less, and more preferably 35% by volume or less, relative to the total amount of solvent in the non-aqueous electrolyte, from the viewpoint of improving high-temperature stability and suppressing gas generation. The dimethyl carbonate content is typically 15% by volume or more, preferably 20% by volume or more, more preferably 25% by volume or more, and typically 50% by volume or less, preferably 45% by volume or less, and more preferably 40% by volume or less, relative to the total amount of non-aqueous solvent in the non-aqueous electrolyte. The ethyl methyl carbonate content is typically 20% by volume or more, preferably 30% by volume or more, and typically 50% by volume or less, and preferably 45% by volume or less, relative to the total amount of non-aqueous solvent in the non-aqueous electrolyte.

[0072] [1-4-3. Chain-like carboxylic acid esters] Examples of linear carboxylic acid esters include methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, methyl valerate, methyl isobutyrate, ethyl isobutyrate, and methyl pivalate. Among these, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, and propyl propionate are preferred from the viewpoint of improving battery characteristics, with methyl acetate and methyl propionate being more preferred. Linear carboxylic acid esters in which some of the hydrogen atoms of the above compounds are substituted with fluorine atoms (e.g., methyl trifluoroacetate, ethyl trifluoroacetate, etc.) can also be suitably used. When a chain-like carboxylic acid ester is included, its content is usually 1% by volume or more, preferably 5% by volume or more, and more preferably 15% by volume or more, relative to the total amount of the non-aqueous solvent, from the viewpoint of improving the electrical conductivity of the non-aqueous electrolyte and improving the high-current discharge characteristics of the non-aqueous electrolyte battery. Furthermore, the upper limit of its content is usually 70% by volume or less, preferably 50% by volume or less, and more preferably 40% by volume or less, from the viewpoint of keeping the viscosity of the non-aqueous electrolyte within an appropriate range, avoiding a decrease in electrical conductivity, suppressing an increase in negative electrode resistance, and keeping the high-current discharge characteristics of the non-aqueous electrolyte battery within a good range. When the content of the linear carboxylic acid ester relative to the total amount of the above non-aqueous solvent is converted on a mass basis, it is usually 0.8% by mass or more, preferably 4% by mass or more, more preferably 13% by mass or more, and usually 63% by mass or less, preferably 44% by mass or less, more preferably 35% by mass or less.

[0073] [1-3-4. Cyclic carboxylic acid esters] Examples of cyclic carboxylic acid esters include γ-butyrolactone and γ-valerolactone. Of these, γ-butyrolactone is more preferred. Cyclic carboxylic acid esters obtained by substituting some of the hydrogen atoms of the above compounds with fluorine atoms can also be suitably used. When the non-aqueous electrolyte contains a cyclic carboxylic acid ester, its content is usually 1% by volume or more, preferably 5% by volume or more, and more preferably 15% by volume or more, relative to the total amount of the non-aqueous solvent, from the viewpoint of improving the electrical conductivity of the non-aqueous electrolyte and improving the high-current discharge characteristics of the non-aqueous electrolyte battery. Furthermore, the upper limit of its content is usually 70% by volume or less, preferably 50% by volume or less, and more preferably 40% by volume or less, from the viewpoint of keeping the viscosity of the non-aqueous electrolyte within an appropriate range, avoiding a decrease in electrical conductivity, suppressing an increase in negative electrode resistance, and keeping the high-current discharge characteristics of the non-aqueous electrolyte battery within a good range.

[0074] [1-4-5. Cyclic ether compounds] Examples of cyclic ether compounds include cyclic ethers having 3 to 6 carbon atoms, such as tetrahydrofuran, 2-methyltetrahydrofuran, 3-methyltetrahydrofuran, 1,3-dioxane, 2-methyl-1,3-dioxane, 4-methyl-1,3-dioxane, and 1,4-dioxane. Some of the hydrogen atoms in these cyclic ether compounds may be substituted with fluorine atoms. Among these, tetrahydrofuran, 1,3-dioxane, and 1,4-dioxane are preferred from the viewpoint of providing high ionic conductivity.

[0075] When the non-aqueous electrolyte contains a cyclic ether compound, its content is arbitrary as long as it does not impair the effects of the present invention, but is usually 1% by volume or more, preferably 2% by volume or more, more preferably 3% by volume or more, and usually 30% by volume or less, preferably 25% by volume or less, and more preferably 20% by volume or less, relative to the total amount of non-aqueous solvent in the non-aqueous electrolyte. If the content of the cyclic ether compound is within the above range, it is easy to ensure the effect of improving the degree of dissociation of metal ions, especially lithium ions, by the cyclic ether compound and improving ionic conductivity due to the reduction in viscosity of the non-aqueous electrolyte. Furthermore, when the negative electrode active material is a carbon-based material, the phenomenon of co-insertion of chain-like ethers together with metal ions, especially lithium ions, can be suppressed, so that the input / output characteristics and charge / discharge rate characteristics can be set within an appropriate range.

[0076] [1-4-6. Sulfone compounds] The sulfone compound is not particularly limited and may be a cyclic sulfone or a linear sulfone. In the case of a cyclic sulfone, the number of carbon atoms is usually 3 to 6, preferably 3 to 5, and in the case of a linear sulfone, the number of carbon atoms is usually 2 to 6, preferably 2 to 5. Furthermore, the number of sulfonyl groups in one molecule of the sulfone compound is not particularly limited, but is usually 1 or 2. Examples of cyclic sulfones include monosulfone compounds such as trimethylene sulfones, tetramethylene sulfones, and hexamethylene sulfones; and disulfone compounds such as trimethylene disulfones, tetramethylene disulfones, and hexamethylene disulfones. Among these, tetramethylene sulfones, tetramethylene disulfones, hexamethylene sulfones, and hexamethylene disulfones are more preferred from the viewpoint of dielectric constant and viscosity, and tetramethylene sulfones (sulfolanes) are even more preferred. Sulfolanes and sulfolane derivatives are preferred as sulforanes. Sulfolane derivatives are preferred in which one or more hydrogen atoms bonded to the carbon atoms constituting the sulfolane ring are substituted with fluorine atoms, alkyl groups, or fluorine-substituted alkyl groups. Among these, 2-methylsulfolane, 3-methylsulfolane, 2-fluorosulfolane, 3-fluorosulfolane, 2,3-difluorosulfolane, 2-trifluoromethylsulfolane, and 3-trifluoromethylsulfolane are preferred because they have high ionic conductivity and high input / output properties.

[0077] Furthermore, examples of chain-like sulfones include dimethyl sulfone, ethyl methyl sulfone, diethyl sulfone, monofluoromethyl methyl sulfone, difluoromethyl methyl sulfone, trifluoromethyl methyl sulfone, and pentafluoroethyl methyl sulfone. Among these, dimethyl sulfone, ethyl methyl sulfone, and monofluoromethyl methyl sulfone are preferred because they improve the high-temperature storage stability of non-aqueous electrolytes. If the non-aqueous electrolyte contains a sulfone compound, the amount is arbitrary as long as it does not impair the effects of the present invention. However, from the viewpoint of improving high-temperature storage stability, the amount is usually 0.3% by volume or more, preferably 0.5% by volume or more, more preferably 1% by volume or more, relative to the total amount of the non-aqueous solvent in the non-aqueous electrolyte, and is usually 40% by volume or less, preferably 35% by volume or less, more preferably 30% by volume or less.

[0078] [1-5. Auxiliary Agents] The non-aqueous electrolyte of the present invention may contain various auxiliary agents, as long as they do not impair the effects of the present invention. Conventionally known auxiliary agents can be used as desired. The auxiliary agents can be used individually or in combination of two or more agents in any ratio. Examples of additives include cyclic carbonates having carbon-carbon unsaturated bonds, compounds having isocyanate groups, organic compounds having an isocyanuric acid skeleton, sulfur-containing organic compounds other than those listed above, phosphorus-containing organic compounds other than those listed above, silicon-containing compounds, aromatic compounds, organic compounds having cyano groups, carboxylic acid anhydrides, and boron-containing organic compounds other than those listed above. For example, compounds described in International Publication No. 2015 / 111676 can be cited.

[0079] The content of the auxiliary agent is not particularly limited and is arbitrary as long as it does not significantly impair the effects of the present invention, but is usually 0.001% by mass or more, preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and usually 10% by mass or less, preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less, and particularly preferably less than 1% by mass, relative to the total amount of the non-aqueous electrolyte.

[0080] [2.Nonaqueous electrolyte battery] The non-aqueous electrolyte battery of the present invention is a non-aqueous electrolyte battery comprising a positive electrode having a positive electrode active material capable of intercalating and releasing metal ions, and a negative electrode having a negative electrode active material capable of intercalating and releasing metal ions, characterized in that it comprises the non-aqueous electrolyte of the present invention. Furthermore, without departing from the spirit of the present invention, it is also possible to use a mixture of other non-aqueous electrolytes with the non-aqueous electrolyte of the present invention. Examples of non-aqueous electrolyte batteries of the present invention include polyvalent cation batteries, metal-air secondary batteries, and secondary batteries using s-block metals other than those mentioned above, with non-aqueous electrolyte secondary batteries being preferred and lithium-ion secondary batteries being more preferred.

[0081] [2-1. Non-aqueous electrolyte] As the non-aqueous electrolyte, the above-mentioned non-aqueous electrolyte is used. Furthermore, without departing from the spirit of the present invention, it is also possible to mix other non-aqueous electrolytes with the non-aqueous electrolyte of the present invention.

[0082] [2-2. Positive electrode] The positive electrode has a positive electrode active material capable of intercepting and releasing metal ions on at least a portion of the current collector surface. The positive electrode active material is preferably a positive electrode active material capable of intercepting and releasing lithium ions, and preferably contains a lithium transition metal compound.

[0083] [2-2-1. Positive electrode active material] The following describes the positive electrode active material (lithium transition metal compound) used in the positive electrode.

[0084] [2-2-1-1. Lithium transition metal compounds] Lithium transition metal compounds are compounds having a structure that allows for the removal and insertion of lithium ions. Examples include sulfides, phosphate compounds, silicate compounds, borate compounds, and lithium transition metal composite oxides. Among these, phosphate compounds or lithium transition metal composite oxides are preferred, and lithium transition metal composite oxides are more preferred. Examples of lithium transition metal composite oxides include those with a spinel structure that allows for three-dimensional diffusion, and those with a layered structure that enables two-dimensional diffusion of lithium ions.

[0085] Lithium transition metal composite oxides having a spinel structure are generally represented by the following formula (1). Li x M₂O₄(1) (In Formula (1), x satisfies 1≦x≦1.5, and M represents one or more transition metal elements.) Specific examples of the oxide represented by Formula (1) include LiMn₂O₄, LiCoMnO₄, LiNi 0.5 Mn 1.5 O₄, LiCoVO₄ and the like.

[0086] A lithium transition metal composite oxide having a layered structure is generally represented by the following compositional formula (2). Li 1+y MO₂(2) (In Formula (2), y satisfies -0.1≦y≦0.5, and M represents one or more transition metal elements.) Specific examples of the oxide represented by Formula (2) include LiCoO₂, LiNiO₂, LiNi 0.85 Co 0.10 Al 0.05 O₂, LiNi 0.80 Co 0.15 Al 0.05 O₂, LiNi 0.33 Co 0.33 Mn 0.33 O₂, Li 1.05 Ni 0.33 Co 0.33 Mn 0.33 O₂, LiNi 0.5 Co 0.2 Mn 0.3 O₂, Li 1.05 Ni 0.5 Co 0.2 Mn 0.3 O₂, LiNi 0.6 Co 0.2 Mn 0.2 O₂, LiNi 0.8 Co 0.1 Mn 0.1 O₂, LiNi 0.91 Co 0.06 Mn 0.03 O₂, LiNi 0.91 Co 0.06 Al 0.03 O₂, LiNi 0.90 Co 0.03 Al 0.07 O₂, Li 1.05 Ni0.34 Co 0.33 Mn 0.33 O2, Li 1.00 Ni 0.61 Co 0.20 Mn 0.19 Examples include O2.

[0087] Among these, lithium transition metal composite oxides having a layered structure are preferred from the viewpoint of improving battery capacity, and lithium transition metal composite oxides represented by the following formula (3) are more preferred. Li a1 Ni b1 M c1 O2(3) (In equation (3), a1, b1, and c1 are 0.90 ≤ a1 ≤ 1.10, 0.30 ≤ b1 ≤ 0.98, and 0.02 ≤ c1 ≤ 0.70, respectively, and b1 + c1 = 1. M represents at least one element selected from the group consisting of Co, Mn, Al, Mg, Zr, Fe, Ti, and Er.) In formula (3), b1 is preferably 0.40 or higher, more preferably 0.50 or higher, and particularly preferably 0.60 or higher.

[0088] In particular, from the viewpoint of structural stability of lithium transition metal composite oxides, it is preferable that the lithium transition metal composite oxide is represented by the following formula (4). Li a2 Ni b2 Co c2 M d2 O2(4) (In equation (4), a2, b2, c2, and d2 are 0.90 ≤ a2 ≤ 1.10, 0.30 ≤ b2 ≤ 0.98, 0.01 ≤ c2 ≤ 0.70, and 0.01 ≤ d2 ≤ 0.70, respectively, and b2 + c2 + d2 = 1. M represents at least one element selected from the group consisting of Mn, Al, Mg, Zr, Fe, Ti, and Er.) In formula (4) above, b2 is preferably 0.40 or higher, more preferably 0.50 or higher, and particularly preferably 0.60 or higher. Also, d2 is preferably 0.01 or higher, and more preferably 0.10 or higher. A preferred example of the lithium transition metal composite oxide represented by the above formula (4) is LiNi 0.85 Co0.10 Al 0.05 O2, LiLiLi 0.80 Co 0.15 Al 0.05 O2, LiLiLi 0.8 Co 0.1 Mn 0.1 O2, LiLiLi 0.91 Co 0.06 Mn 0.03 O2, LiLiLi 0.91 Co 0.06 Al 0.03 O2, LiLiLi 0.90 Co 0.03 Al 0.07 O2, Li 1.00 Ni 0.61 Co 0.20 Mn 0.19 O2, Li 1.05 Ni 0.34 Co 0.33 Mn 0.33 Examples include O2.

[0089] In the above formulas (1) to (3), from the viewpoint of enhancing the structural stability of the lithium transition metal composite oxide and suppressing structural degradation during repeated charging and discharging, M preferably contains Mn or Al, and Mn is more preferred. In formula (4) above, from the viewpoint of enhancing the structural stability of the lithium transition metal composite oxide and suppressing structural degradation during repeated charging and discharging, M preferably contains Mn or Al, and more preferably Mn.

[0090] [2-2-1-2. Introduction of different elements] Furthermore, lithium transition metal composite oxides may contain elements other than those included in any of the above formulas (1) to (4) (other elements).

[0091] Furthermore, there are no particular restrictions on the positive electrode active material other than lithium transition metal compounds, as long as it is a positive electrode active material capable of intercalating and releasing metal ions, known positive electrode active materials can be used.

[0092] [2-2-1-3. Surface coating] As the positive electrode, a positive electrode active material may be used in which a substance with a different composition from the positive electrode active material (surface-adhered substance) is attached to its surface. Examples of surface-adhering substances include oxides such as aluminum oxide, sulfates such as lithium sulfate, and carbonates such as lithium carbonate. These surface-adhering substances can be attached to the surface of the positive electrode active material by, for example, dissolving or suspending them in a solvent, impregnating them into the positive electrode active material, and then drying them. The amount of surface-adhering material is preferably 1 μmol / g or more, more preferably 10 μmol / g or more, and usually 1 mmol / g or less, relative to the positive electrode active material. In this specification, a positive electrode active material with the above-mentioned surface-adhered substance attached to its surface is also referred to as a "positive electrode active material."

[0093] [2-2-1-4. Blend] The positive electrode active material can be used alone or in combination of two or more materials in any ratio.

[0094] [2-2-2. Configuration and Manufacturing Method of the Positive Electrode] The positive electrode using positive electrode active material can be manufactured by conventional methods. Specifically, the positive electrode can be obtained by a coating method in which the positive electrode active material, binder, and optionally conductive material and thickener are dry-mixed to form a sheet, which is then pressed onto the positive electrode current collector, or by dissolving or dispersing these materials in a liquid medium such as an aqueous solvent or an organic solvent to form a slurry, which is then applied to the positive electrode current collector and dried to form a positive electrode active material layer on the current collector. Alternatively, for example, the above positive electrode active material may be roll-molded to form a sheet electrode, or it may be compressed to form a pellet electrode. The following describes the process of sequentially applying and drying the slurry onto the positive electrode current collector.

[0095] [2-2-2-1. Content of positive electrode active material] The content of the positive electrode active material in the positive electrode active material layer is typically between 80% by mass and 99.5% by mass.

[0096] [2-2-2-2. Electrode density] The positive electrode active material layer obtained by coating and drying is preferably compacted by hand pressing, roller pressing, or the like to increase the packing density of the positive electrode active material. The density of the positive electrode active material layer present on the current collector is typically 1.5 g / cm³. 3 More than 4.5g / cm 3 The following applies:

[0097] [2-2-2-3. Conductive materials] Any known conductive material can be used as the conductive material. Specific examples include metallic materials such as copper and nickel; graphite such as natural graphite and artificial graphite; carbon black such as acetylene black; and carbon-based materials such as amorphous carbon such as needle coke. The conductive material can be used alone or in combination of two or more materials in any ratio. The conductive material is usually contained in the positive electrode active material layer in an amount of 0.01% by mass or more and 50% by mass or less.

[0098] [2-2-2-4. Binding agent] When forming the positive electrode active material layer by a coating method, the type of binder used is not particularly limited as long as it is a material that can be dissolved or dispersed in the liquid medium for the slurry. For example, fluororesins such as polyvinyl fluoride, polyvinylidene fluoride, and polytetrafluoroethylene are preferred due to their weather resistance, chemical resistance, heat resistance, and flame retardancy; CN group-containing polymers such as polyacrylonitrile and polyvinylidene cyanide are preferred. Furthermore, mixtures of the above polymers, modified products, derivatives, random copolymers, alternating copolymers, graft copolymers, block copolymers, etc., can also be used. The binder can be used alone or in combination of two or more types in any ratio. Furthermore, when a resin is used as a binder, the weight-average molecular weight of the resin can be arbitrary as long as it does not impair the effects of the present invention, and is usually between 10,000 and 3,000,000. When the molecular weight is within this range, the strength of the electrode is improved, and the electrode can be formed suitably. The binder content in the positive electrode active material layer is typically between 0.1% by mass and 80% by mass.

[0099] [2-2-2-5. Current Collector] The material of the positive electrode current collector is not particularly limited, and any known material can be used. Specific examples include metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum, with aluminum being preferred. Examples of current collector shapes include metal foil, metal cylinder, metal coil, metal plate, metal thin film, expanded metal, punched metal, and foamed metal. Among these, metal foil or metal thin film is preferred. The metal thin film may be formed in a mesh shape as appropriate. When the shape of the positive electrode current collector is plate-shaped or film-shaped, the thickness of the current collector can be arbitrary, but is usually between 1 μm and 1 mm.

[0100] [2-2-2-6. Thickness of the positive electrode plate] The thickness of the positive electrode plate is not particularly limited, but from the viewpoint of high capacity and high output, the thickness of the positive electrode active material layer, obtained by subtracting the thickness of the current collector from the thickness of the positive electrode plate, is usually between 10 μm and 500 μm on one side of the current collector.

[0101] [2-2-2-7. Surface coating of the positive electrode plate] The positive electrode plate may be one on which a substance with a different composition from the positive electrode plate is attached to its surface, and the same substance as the surface-attached substance that may be attached to the surface of the positive electrode active material is used.

[0102] [2-3. Negative electrode] The negative electrode has negative electrode active material on at least a portion of the current collector surface. [2-3-1. Negative electrode active material] There are no particular restrictions on the negative electrode active material used in the negative electrode, as long as it is electrochemically capable of intercalating and releasing metal ions. Specific examples include (i) carbon-based materials, (ii) particles containing metal elements and / or metalloid elements that can alloy with Li, (iii) lithium-containing metal composite oxide materials, and (iv) mixtures thereof. Among these, it is preferable to use (i) carbon-based materials, (ii) particles containing metal elements and / or metalloid elements that can alloy with Li, and (v) mixtures of particles containing metal elements and / or metalloid elements that can alloy with Li and graphite particles, as these offer good cycle characteristics, safety, and excellent continuous charging characteristics. These can be used individually or in combination of two or more in any ratio.

[0103] [2-3-1-1. Carbon-based materials] (i) Examples of carbon-based materials include natural graphite, artificial graphite, amorphous carbon, carbon-coated graphite, graphite-coated graphite, and resin-coated graphite. Among these, natural graphite is preferred. Carbon-based materials can be used individually or in combination of two or more in any ratio. Examples of natural graphite include scaly graphite, flake graphite, and / or graphite particles obtained by treating these graphites, such as spheroidization or densification. Among these, spherical or ellipsoidal graphite particles obtained by spheroidization treatment are preferred from the viewpoint of particle packing properties or charge / discharge rate characteristics. The volume-average particle size (d50) of graphite particles is typically between 1 μm and 100 μm.

[0104] [2-3-1-2. Physical Properties of Carbon-Based Materials] The carbon-based material used as the negative electrode active material preferably satisfies at least one of the following physical properties and characteristics such as shape, as shown in (1) to (4), and more preferably satisfies multiple items simultaneously. (1) X-ray diffraction parameters The d-value (interlayer distance) of the lattice plane (002 plane) of carbon-based materials, as determined by X-ray diffraction using the JSPS method, is typically between 0.335 nm and 0.360 nm. Furthermore, the crystallite size (Lc) of carbon-based materials, as determined by X-ray diffraction using the JSPS method, is 1.0 nm or greater. (2) Volume-based average particle size The volume-based average particle size of carbon-based materials is the volume-based average particle size (median diameter) determined by laser diffraction and scattering, and is typically between 1 μm and 100 μm. (3) Raman R value, Raman half-width The Raman R value of carbon-based materials is measured using argon ion laser Raman spectroscopy and is typically between 0.01 and 1.5. Also, 1580 cm² of carbon-based materials -1 The Raman width at half maximum in the vicinity is not particularly restricted, but is usually 10 cm. -1 More than 100cm -1 The following applies: (4) BET specific surface area The BET specific surface area of ​​carbon-based materials is the value of the specific surface area measured using the BET method, and is typically 0.1 m². 2 ·g -1 Over 100m 2 ·g -1 The following applies: The negative electrode active material may contain two or more carbon-based materials with different properties. The properties referred to here are one or more characteristics selected from the group consisting of X-ray diffraction parameters, volume-based average particle size, Raman R value, Raman full width at half maximum, and BET specific surface area. Examples of materials containing two or more carbon-based materials with different properties include those in which the volume-based particle size distribution is not symmetrical when centered on the median diameter, those containing two or more carbon-based materials with different Raman R values, and those with different X-ray parameters.

[0105] [2-3-1-3. Materials containing metallic and / or metalloid elements that can be alloyed with Li] (ii) As the material containing a metal element and / or metalloid element alloyable with Li, any conventionally known material can be used. From the viewpoints of capacity and cycle life, the material is preferably a metal or metalloid selected from the group consisting of, for example, Sb, Si, Sn, Al, As, and Zn. When the material containing a metal element and / or metalloid element alloyable with Li contains two or more metals, the material may be an alloy material composed of an alloy of these metals. Examples of the compound containing a metal element and / or metalloid element alloyable with Li include oxides, nitrides, and carbides of metals and / or metalloids. The compound may contain two or more metal elements and / or metalloid elements alloyable with Li. Among these, metal Si (hereinafter also referred to as "Si") or a Si-containing inorganic compound is preferred from the viewpoint of high capacity. In the present specification, Si or a Si-containing inorganic compound is collectively referred to as a Si compound. Further, the compound containing a metal element and / or metalloid element alloyable with Li may already be alloyed with Li during the production of a negative electrode to be described later, and as the compound, a Si compound is preferred from the viewpoint of high capacity. Examples of the Si compound include SiO x1 (0≦x1≦2) and the like. Examples of the metal compound alloyed with Li include Li z1 Si (0<z1≦4.4), Li 2z2 SiO 2+z2 (0<z2≦2) and the like. As the Si compound, Si oxide (SiO x2 , 0<x2≦2) is preferred in that the theoretical capacity is larger than that of graphite, and amorphous Si or nano-sized Si crystals are preferred in that alkali ions such as lithium ions can easily enter and exit, and a high capacity can be obtained. When the material containing a metal element and / or metalloid element alloyable with Li is in the form of particles, the volume average particle diameter (d50) of the particles is usually 0.01 μm or more and 10 μm or less from the viewpoint of cycle life.

[0106] [2-3-1-4. Mixtures of natural graphite and materials containing alloyable metallic elements and / or metalloid elements with Li] (v) A mixture of graphite particles and a material containing a metal element and / or metalloid element that can be alloyed with Li may be a mixture in which the material containing a metal element and / or metalloid element that can be alloyed with Li and the graphite particles are mixed in the state of being independent particles, or it may be a composite in which particles containing a metal element and / or metalloid element that can be alloyed with Li are present on the surface or inside the graphite particles. The content of particles containing metallic and / or metalloid elements that can alloy with Li, relative to the total amount of graphite particles, is usually between 1% by mass and 99% by mass.

[0107] [2-3-1-5. Lithium-containing metal composite oxide materials] (iii) The lithium-containing metal composite oxide material is not particularly limited as long as it is capable of intercalating and releasing lithium ions. Specifically, from the viewpoint of high current density charge / discharge characteristics, lithium-containing metal composite oxide materials containing titanium are preferred, lithium-titanium composite oxides (hereinafter also referred to as "lithium titanium composite oxides") are more preferred, and lithium titanium composite oxides having a spinel structure are even more preferred because they significantly reduce output resistance. Furthermore, the lithium and / or titanium in the lithium-titanium composite oxide may be substituted with other metallic elements, such as at least one element selected from the group consisting of Al, Ga, Cu, and Zn. As a lithium titanium composite oxide, Li 4 / 3 Ti 5 / 3 O4, Li1Ti2O4 and Li 4 / 5 Ti 11 / 5 O4 is preferred. Also, lithium titanium composite oxides in which part of lithium and / or titanium is substituted with other elements are preferred, for example, Li 4 / 3 Ti 4 / 3 Al 1 / 3 O4 is also preferable.

[0108] [2-3-2. Negative electrode configuration and manufacturing method] The negative electrode may be manufactured using any known method, as long as it does not impair the effects of the present invention. For example, it can be manufactured by adding a binder, a liquid medium such as an aqueous solvent or an organic solvent, and optionally a thickener, a conductive material, a filler, etc., to the negative electrode active material to form a slurry, applying this slurry to a current collector, drying it, and then pressing it to form a negative electrode active material layer.

[0109] [2-3-2-1. Content of negative electrode active material] The content of the negative electrode active material in the negative electrode active material layer is typically between 80% by mass and 99.5% by mass.

[0110] [2-3-2-2. Electrode density] The negative electrode active material layer obtained by coating and drying is preferably compacted using a hand press, roller press, or the like to increase the packing density of the negative electrode active material. The electrode structure when the negative electrode active material is used as an electrode is not particularly limited, but the density of the negative electrode active material layer present on the current collector is usually 1 g / cm³. 3 More than 2.2g / cm 3 The following applies:

[0111] [2-3-2-3. Thickening agents] Thickening agents are typically used to adjust the viscosity of slurries. While not particularly limited, examples of thickening agents include carboxymethylcellulose and its salts, methylcellulose, hydroxymethylcellulose, ethylcellulose, and polyvinyl alcohol. These can be used individually or in combination of two or more in any ratio. When a thickening agent is used, the amount of the thickening agent relative to the negative electrode active material is usually between 0.1% by mass and 5% by mass.

[0112] [2-3-2-4. Binding agent] The binder used to bind the negative electrode active material can be any material that is stable with non-aqueous electrolytes or liquid media used during electrode manufacturing, and is not particularly limited. Specific examples include rubbery polymers such as styrene-butadiene rubber (SBR), isoprene rubber, butadiene rubber, fluororubber, acrylonitrile-butadiene rubber (NBR), and ethylene-propylene rubber, as well as fluorine-based polymers such as polyvinylidene fluoride, polytetrafluoroethylene, fluorinated polyvinylidene fluoride, and tetrafluoroethylene-ethylene copolymers. These can be used individually or in combination of two or more in any ratio. The binder content relative to the negative electrode active material is typically between 0.1% by mass and 20% by mass. In particular, when the binder contains a rubbery polymer such as SBR as its main component, the binder content relative to the negative electrode active material is usually between 0.1% by mass and 5% by mass. Furthermore, when the binder contains a fluorine-based polymer such as polyvinylidene fluoride as its main component, the binder content relative to the negative electrode active material is usually between 1% by mass and 15% by mass.

[0113] [2-3-2-5. Current Collector] Any known material can be used as the current collector for holding the negative electrode active material. Examples of current collectors for the negative electrode include metal materials such as aluminum, copper, nickel, stainless steel, and nickel-plated steel, but copper is particularly preferred in terms of ease of processing and cost. Examples of the negative electrode current collector shape include metal foil, metal cylinder, metal coil, metal plate, metal thin film, expanded metal, punched metal, and foamed metal. Among these, metal foil or metal thin film is preferred. The metal thin film may be formed in a mesh shape as appropriate. When the negative electrode current collector is plate-shaped or film-shaped, the thickness of the current collector can be arbitrary, but is usually between 1 μm and 1 mm.

[0114] [2-3-2-6. Thickness of the negative electrode plate] The thickness of the negative electrode (negative electrode plate) is designed to match the positive electrode (positive electrode plate) used and is not particularly limited; however, the thickness of the negative electrode active material layer, obtained by subtracting the thickness of the current collector from the thickness of the negative electrode material, is usually between 15 μm and 300 μm.

[0115] [2-3-2-7. Surface coating of the negative electrode plate] Furthermore, the negative electrode plate may also be one in which a substance with a different composition from the negative electrode active material is attached to its surface (surface-attached substance). Examples of surface-attached substances include oxides such as aluminum oxide, sulfates such as lithium sulfate, and carbonates such as lithium carbonate.

[0116] [2-4. Separator] A separator is usually placed between the positive and negative electrodes to prevent short circuits. In this case, the non-aqueous electrolyte is typically used by impregnating this separator. There are no particular restrictions on the material or shape of the separator; any known material or shape can be used as long as it does not impair the effects of the present invention.

[0117] [2-5.Battery design] [2-5-1. Electrode group] The electrode group may be either a laminated structure in which the positive electrode plate and the negative electrode plate are separated by the separator, or a structure in which the positive electrode plate and the negative electrode plate are spirally wound around the separator. The ratio of the volume of the electrode group to the internal volume of the battery (electrode group occupancy rate) is usually between 40% and 90%.

[0118] [2-5-2. Current collection structure] In the case of electrode groups with the aforementioned laminated structure, a structure formed by bundling the metal core portions of each electrode layer and welding them to a terminal is preferably used. A structure that reduces resistance by providing multiple terminals within the electrode is also preferably used. In the case of electrode groups with the aforementioned wound structure, the internal resistance can be reduced by providing multiple lead structures in both the positive and negative electrodes and bundling them to a terminal.

[0119] [2-5-3. Protective Elements] As protective elements, PTC (Positive Temperature Coefficient) elements whose resistance increases with heat generation due to excessive current, thermal fuses, thermistors, and valves (current interruption valves) that interrupt the current flowing through the circuit due to a rapid rise in internal pressure or temperature of the battery in the event of abnormal heat generation can be used. It is preferable to select the above protective elements that do not operate under normal high-current use, and it is even more preferable to design the system so that abnormal heat generation or thermal runaway does not occur even without protective elements.

[0120] [2-5-4. Exterior] Non-aqueous electrolyte batteries are typically constructed by housing the non-aqueous electrolyte, negative electrode, positive electrode, separator, etc., of the present invention within an outer casing (outer case). There are no restrictions on this outer casing; any known material can be used as long as it does not impair the effects of the present invention. The material of the outer casing can be any substance that is stable with respect to the non-aqueous electrolyte used, and is not particularly limited. However, from the viewpoint of weight reduction and cost, metals such as iron, aluminum, aluminum alloys, or laminated films are preferably used. Iron is particularly preferred due to its pressure resistance required to operate the current interruption valve. Outer cases using the above-mentioned metals include those that create a sealed structure by welding the metals together using laser welding, resistance welding, or ultrasonic welding, or those that create a crimped structure using the above-mentioned metals via a resin gasket.

[0121] [2-5-5. Shape] Furthermore, the shape of the outer case is arbitrary and can be any of the following: cylindrical, rectangular, laminated, coin-shaped, large, etc. [Examples]

[0122] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0123] The compounds used in this example are listed below. Compound (A): Vinyl ethylene sulfite

[0124] [ka]

[0125] LiPO2F2: Lithium difluorophosphate LiSO3F: Lithium fluorosulfonate LiBOB: Lithium bis(oxalate) borate VC: Vinylen carbonate PRES:1-propene-1,3-sultone VEC: Vinyl ethylene carbonate

[0126] <Examples 1-1 to 1-3, Comparative Examples 1-1 to 1-13> (Preparation of non-aqueous electrolyte) Under a dry argon atmosphere, a mixture of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate (volume ratio 3:4:3) was used to dissolve thoroughly dried LiPF6 in a non-aqueous electrolyte solution to a concentration of 1.0 mol / L (12.3 mass%). Furthermore, vinyl ethylene sulfite (VES) as compound (A) and anion-containing compound (B) were dissolved in the amounts shown in Table 1 to prepare a non-aqueous electrolyte solution. Using this non-aqueous electrolyte solution, a non-aqueous electrolyte secondary battery was prepared by the following method. Note that in Comparative Examples 1-1, 1-3, 1-5, and 1-7, compound (A) was not used, in Comparative Examples 1-1 and 1-2, anion-containing compound (B) was not used, in Comparative Examples 1-9 and 1-10, VC and PRES were used instead of anion-containing compound (B), respectively, and in Comparative Examples 1-11 to 1-13, VC, VEC, or ES were added to the electrolyte solution of Comparative Example 1-7, respectively.

[0127] (Fabrication of the positive electrode) Lithium cobalt nickel manganese oxide (Li) is used as the positive electrode active material. 1.05 Ni 0.34 Co 0.33 Mn 0.3385 parts by mass of O2, 10 parts by mass of acetylene black as a conductive material, and 5 parts by mass of polyvinylidene fluoride (PVdF) as a binder were mixed in N-methyl-2-pyrrolidone to form a slurry. This slurry was uniformly applied to a 15 μm thick aluminum foil, dried, and then roll-pressed to form the positive electrode. The density of the positive electrode active material layer in the positive electrode was 2.6 g / cm³. 3 That was the case.

[0128] (Fabrication of the negative electrode) 49 parts by mass of graphite powder as the negative electrode active material, 50 parts by mass of aqueous dispersion of sodium carboxymethylcellulose (concentration of sodium carboxymethylcellulose 1%) as a thickener, and 1 part by mass of aqueous dispersion of styrene-butadiene rubber (concentration of styrene-butadiene rubber 49% by mass) as a binder were mixed in a disperser to form a slurry. The resulting slurry was uniformly applied to a 10 μm thick copper foil, dried, and then roll-pressed to form the negative electrode. The density of the negative electrode active material layer in the negative electrode was 1.35 g / cm³. 3 That was the case.

[0129] (Manufacturing of non-aqueous electrolyte secondary batteries) The positive and negative electrodes and polyolefin separators prepared as described above were stacked in the order of negative electrode, separator, and positive electrode. The resulting battery elements were wrapped in an aluminum laminate film, injected with the aforementioned non-aqueous electrolyte, and then vacuum-sealed to produce a sheet-like non-aqueous electrolyte secondary battery.

[0130] [Evaluation of non-aqueous electrolyte secondary batteries] The non-aqueous electrolyte secondary battery prepared as described above was evaluated as follows.

[0131] (Initial charge / discharge) In a constant temperature bath at 25°C, a sheet-shaped non-aqueous electrolyte secondary battery was charged with a current equivalent to 0.025C to 3.6V, then charged with constant current-constant voltage (hereinafter also referred to as "CC-CV charging") at 0.167C to a voltage of 4.2V, and finally discharged with a constant current at 0.167C to 2.5V. Furthermore, the non-aqueous electrolyte secondary battery was stabilized by CC-CV charging to 4.1V at 0.167C and then storing it at 60°C for 12 hours. Subsequently, at 25°C, it was discharged with a constant current to 2.5V at 0.167C, and then CC-CV charged to a voltage of 4.2V at 0.167C. After that, a constant current discharge to 2.5V was performed at 0.167C, and the battery capacity at that time was taken as the initial capacity. Next, CC-CV charging was performed to 4.2V at 0.2C to complete the initial charge and discharge. Here, 1C represents the current value required to discharge the battery's standard capacity in one hour. For example, 0.025C represents 1 / 40th of that current value. The same applies to subsequent values.

[0132] (Evaluation of recovery capacity maintenance rate) Non-aqueous electrolyte secondary batteries that had completed their initial charge and discharge were left standing at 60°C for two weeks. After two weeks of standing, they were discharged at 25°C at 0.167C to 2.5V with a constant current, followed by CC-CV charging at 0.167C to a voltage of 4.2V. Subsequently, they were discharged again at 0.167C to 2.5V with a constant current, and the battery capacity at that time was defined as the recovered capacity. The recovery capacity retention rate was calculated as [(recovered capacity / initial capacity) × 100]. Table 1 shows the relative values ​​of the recovery capacity retention rate, with a non-aqueous electrolyte secondary battery (Comparative Example 1-1) that does not contain compound (A) or a specific amount of anion-containing compound (B) set to 100. A higher recovery capacity retention rate is preferable.

[0133] [Table 1]

[0134] Table 1 shows that non-aqueous electrolyte secondary batteries (Examples 1-1 to 1-3) containing compound (A) and a specific amount of anion-containing compound (B) in a non-aqueous electrolyte are, (a) A non-aqueous electrolyte secondary battery in which the non-aqueous electrolyte does not contain compound (A) and anion-containing compound (B) (Comparative Example 1-1), (b) Non-aqueous electrolyte secondary battery containing compound (A) but not containing anion-containing compound (B) (Comparative Examples 1-2) (c) Non-aqueous electrolyte secondary batteries in which the non-aqueous electrolyte does not contain compound (A) but contains anion-containing compound (B) (Comparative Examples 1-3, 1-5, and 1-7), (d) Non-aqueous electrolyte secondary batteries (Comparative Examples 1-4, 1-6, and 1-8) in which the non-aqueous electrolyte contains compound (A) and an anion-containing compound (B) in an amount exceeding a predetermined amount. (e) Non-aqueous electrolyte secondary batteries (Comparative Examples 1-9 and 1-10) in which the non-aqueous electrolyte contains materials used in the prior art in place of compound (A) and anion-containing compound (B), and (f) It can be seen that the recovery capacity maintenance rate of the non-aqueous electrolyte battery is improved compared to non-aqueous electrolyte batteries containing specific anion-containing compounds and materials used in the prior art (Comparative Examples 1-11 to 1-13). The reason why the recovery capacity retention rate of the non-aqueous electrolyte battery of the present invention has improved is thought to be that by combining compound (A) with a specific amount of anion-containing compound (B), compound (A) and anion-containing compound (B) form a sparingly soluble and strong co-coating, which efficiently suppresses side reactions on the electrode surface.

[0135] <Examples 2-1 to 2-2, Comparative Examples 2-1 to 2-5> (Preparation of non-aqueous electrolyte) Under a dry argon atmosphere, a mixture of ethylene carbonate, dimethyl carbonate, and methyl acetate (volume ratio 3:4:3) was used to dissolve thoroughly dried LiPF6 in a non-aqueous electrolyte solution to a concentration of 1.0 mol / L (12.5 mass%). Compound (A) and anion-containing compound (B) were then dissolved in the amounts shown in Table 2 to prepare a non-aqueous electrolyte solution. In Comparative Examples 2-2 to 2-4, compound (A) was not used, and in Comparative Examples 2-1 to 2-2, anion-containing compound (B) was not used. A non-aqueous electrolyte secondary battery was then prepared using this non-aqueous electrolyte solution in the same manner as in Example 1-1.

[0136] [Evaluation of non-aqueous electrolyte secondary batteries] The non-aqueous electrolyte secondary batteries prepared as described above were evaluated as follows.

[0137] (Initial charge / discharge) In a constant temperature bath at 25°C, a sheet-shaped non-aqueous electrolyte secondary battery was charged with a current equivalent to 0.025C to 3.6V, then CC-CV charged to 4.2V at 0.167C, and finally discharged with a constant current at 0.167C to 2.5V. Furthermore, the non-aqueous electrolyte secondary battery was stabilized by CC-CV charging to 4.1V at 0.167C and then storing it at 60°C for 12 hours. Subsequently, at 25°C, it was discharged with a constant current to 2.5V at 0.167C, and then CC-CV charged to a voltage of 4.2V at 0.167C. After that, a constant current discharge was performed to 2.5V at 0.167C, and the battery capacity at that time was taken as the initial capacity. Then, CC-CV charging was performed to a voltage of 4.2V at 0.167C to complete the initial charge and discharge.

[0138] (Evaluation of recovery capacity maintenance rate) The recovery volume retention rate was evaluated using the same method as in Example 1-1.

[0139] (Evaluation of high-temperature storage gas generation rate) Before initial charging and discharging, and after evaluating the recovery capacity retention rate, the volume of the non-aqueous electrolyte secondary battery was measured by immersing it in an ethanol bath at room temperature, and the change in volume was defined as the amount of gas generated during high-temperature storage.

[0140] Table 2 shows the evaluation results of the recovery capacity retention rate and the high-temperature storage gas generation rate, as follows: recovery capacity retention rate (relative value with the recovery capacity retention rate of a battery containing only compound (A) as an additive (Comparative Example 2-1) set to 100) and high-temperature storage gas generation rate (relative value with the high-temperature storage gas generation amount of a battery containing only compound (A) as an additive (Comparative Example 2-1) set to 100). A lower high-temperature storage gas generation rate is preferable.

[0141] [Table 2]

[0142] Table 2 shows that even when a portion of the chain carbonate in the non-aqueous electrolyte of a non-aqueous electrolyte secondary battery is replaced with methyl acetate, the non-aqueous electrolyte secondary batteries (Examples 2-1 to 2-2) containing compound (A) and a specific amount of anion-containing compound (B) are still in use. (a) A non-aqueous electrolyte secondary battery in which the non-aqueous electrolyte does not contain compound (A) and anion-containing compound (B) (Comparative Example 2-2), (b) A non-aqueous electrolyte secondary battery in which the non-aqueous electrolyte contains compound (A) but does not contain anion-containing compound (B) (Comparative Example 2-1), (c) Non-aqueous electrolyte secondary batteries (Comparative Examples 2-3 and 2-4) in which the non-aqueous electrolyte does not contain compound (A) but contains anion-containing compound (B), and (d) It can be seen that the recovery capacity maintenance rate of the non-aqueous electrolyte battery is improved compared to a non-aqueous electrolyte secondary battery (Comparative Example 2-5) in which the non-aqueous electrolyte contains compound (A) and an anion-containing compound (B) in an amount exceeding a predetermined amount. Furthermore, in non-aqueous electrolyte secondary batteries (Examples 2-1 to 2-2) in which the non-aqueous electrolyte contains compound (A) and a specific amount of anion-containing compound (B), similar comparisons show that the gas generation rate after high-temperature storage, which is a problem when a portion of the chain carbonate in the non-aqueous electrolyte of non-aqueous electrolyte secondary batteries is replaced with methyl acetate, is suppressed.

[0143] <Examples 3-1 to 3-2, Comparative Example 3-1> (Preparation of non-aqueous electrolyte) A non-aqueous electrolyte was prepared in the same manner as in Example 2-1, except that methyl propionate was used as the ester solvent and compound (A) and anion-containing compound (B) were used in the amounts shown in Table 3. In Comparative Example 3-1, anion-containing compound (B) was not used. A non-aqueous electrolyte secondary battery was prepared using this non-aqueous electrolyte in the same manner as in Example 1-1.

[0144] [Evaluation of non-aqueous electrolyte secondary batteries] The non-aqueous electrolyte secondary battery prepared as described above was evaluated using the same method as in Example 2-1. Table 3 shows the above evaluation results, namely the recovery capacity retention rate (a relative value with the recovery capacity retention rate of the battery containing only Compound (A) as an additive (Comparative Example 3-1) taken as 100) and the high-temperature storage gas generation rate (a relative value with the high-temperature storage gas generation amount of the battery containing only Compound (A) as an additive (Comparative Example 3-1) taken as 100).

[0145]

Table 3

[0146] It can be seen from Table 3 that even when a portion of the chain carbonate in the non-aqueous electrolytic solution of the non-aqueous electrolytic solution secondary battery is replaced with methyl propionate, the non-aqueous electrolytic solution secondary batteries (Examples 3-1 and 3-2) whose non-aqueous electrolytic solutions contain Compound (A) and a specific amount of anion-containing compound (B) have an improved recovery capacity retention rate and suppressed high-temperature storage gas generation rate, similarly to Examples 2-1 and 2-2.

[0147] <Example 4-1, Comparative Examples 4-1 to 4-3> (Preparation of non-aqueous electrolytic solution) A non-aqueous electrolytic solution was prepared in the same manner as in Example 3-1, except that methyl propionate was changed to methyl acetate, and Compound (A) and anion-containing compound (B) were used so as to achieve the contents described in Table 4. Note that Compound (A) was not used in Comparative Examples 4-2 to 4-3, and anion-containing compound (B) was not used in Comparative Examples 4-1 to 4-2. Using this non-aqueous electrolytic solution, a non-aqueous electrolytic solution secondary battery was produced in the same manner as in Example 1-1.

[0148] [Evaluation of non-aqueous electrolytic solution secondary battery] (Initial charge and discharge) Initial charge and discharge were completed in the same manner as in Example 2-1.

[0149] (Initial DCR evaluation test) After completing the initial charge and discharge, non-aqueous electrolyte secondary batteries were discharged at 25°C at 0.167C to 2.5V with a constant current, and then charged at 0.167C to 3.7V using CC-CV charging. Subsequently, constant current discharge was performed at 0.5C, 1.0C, and 1.5C for 10 seconds each, and the voltage at 10 seconds was measured. The internal resistance was determined from this current-voltage line and was defined as the initial room-temperature DC resistance (DCR). Furthermore, constant current discharge was performed for 10 seconds at -10°C at 0.25C, 0.5C, and 0.75C, and the voltage at 10 seconds was measured. The internal resistance was determined from this current-voltage line and defined as the initial low-temperature DCR.

[0150] (High-temperature storage durability test) The non-aqueous electrolyte secondary batteries that underwent initial low-temperature DCR evaluation testing were CC-CV charged to 4.2V at 0.167C at 25°C (with a 0.01C cut-off), and then stored at 60°C for two weeks to achieve high-temperature storage. After the batteries had cooled sufficiently, they were discharged to 2.5V at 25°C with a constant current of 0.167C. Subsequently, they were CC-CV charged to 4.2V at 0.167C (with a 0.01C cut-off), and then discharged again to 2.5V at 0.167C.

[0151] (Evaluation of DCR after high-temperature storage) Non-aqueous electrolyte secondary batteries that underwent high-temperature storage endurance testing were discharged at 25°C at 0.167C to 2.5V with a constant current, and then charged at 0.167C to 3.7V using CC-CV charging. Next, constant current discharge was performed at 0.5C, 1.0C, and 1.5C for 10 seconds each, and the voltage at 10 seconds was measured. The internal resistance was calculated from this current-voltage line and was used as the room temperature DCR after high-temperature storage. Furthermore, at -10°C, constant current discharge was similarly performed at 0.25C, 0.5C, and 0.75C for 10 seconds each, and the voltage at 10 seconds was measured. The internal resistance was calculated from this current-voltage line and used as the low-temperature DCR after storage, and the increase in low-temperature DCR after high-temperature storage was calculated as [low-temperature DCR after storage / initial low-temperature DCR × 100]. Table 4 shows the evaluation results described above, including the rate of increase in room temperature DCR after high-temperature storage (relative value with the room temperature DCR of a battery containing only compound (A) as an additive (Comparative Example 4-1) set to 100) and the rate of increase in low-temperature DCR after high-temperature storage (relative value with the increase in low-temperature DCR of a battery containing only compound (A) as an additive (Comparative Example 4-1) set to 100). Smaller rates of increase in room temperature DCR after high-temperature storage and low-temperature DCR after high-temperature storage are preferable.

[0152] [Table 4]

[0153] From Table 4, when a portion of the chain carbonate in the non-aqueous electrolyte of a non-aqueous electrolyte secondary battery is replaced with methyl acetate, the non-aqueous electrolyte secondary battery (Example 4-1) containing compound (A) and anion-containing compound (B) is, (a) A non-aqueous electrolyte secondary battery in which the non-aqueous electrolyte does not contain compound (A) and anion-containing compound (B) (Comparative Example 4-2), (b) A non-aqueous electrolyte secondary battery (Comparative Example 4-1) in which the non-aqueous electrolyte contains compound (A) and does not contain anion-containing compound (B), and (c) Compared to a non-aqueous electrolyte secondary battery (Comparative Example 4-3) in which the non-aqueous electrolyte does not contain compound (A) but contains anion-containing compound (B), the room temperature DCR increase rate and the low temperature DCR increase rate of the non-aqueous electrolyte battery after high-temperature storage are suppressed.

[0154] <Example 5-1, Comparative Example 5-1> (Preparation of non-aqueous electrolyte) A non-aqueous electrolyte was prepared in the same manner as in Example 3-1, except that compound (A) and anion-containing compound (B) were used in the amounts shown in Table 5. In Comparative Example 5-1, anion-containing compound (B) was not used. A non-aqueous electrolyte secondary battery was prepared using this non-aqueous electrolyte in the same manner as in Example 1-1. [Evaluation of non-aqueous electrolyte secondary batteries] The non-aqueous electrolyte secondary battery prepared as described above was evaluated using the same method as in Example 4-1. Table 5 shows the evaluation results described above, including the rate of increase in room temperature DCR after high-temperature storage (relative value with the room temperature DCR after high-temperature storage of a battery containing only compound (A) as an additive (Comparative Example 5-1) set to 100) and the rate of increase in low-temperature DCR after high-temperature storage (relative value with the low-temperature increase in DCR after high-temperature storage of a battery containing only compound (A) as an additive (Comparative Example 5-1) set to 100). Smaller rates of increase in room temperature DCR after high-temperature storage and low-temperature DCR after high-temperature storage are preferable.

[0155] [Table 5]

[0156] Table 5 shows that even when a portion of the chain carbonate in the non-aqueous electrolyte of a non-aqueous electrolyte secondary battery is replaced with methyl propionate, the non-aqueous electrolyte secondary battery (Example 5-1) containing compound (A) and anion-containing compound (B) exhibits suppressed room temperature DCR increase rates and low temperature DCR increase rates after high-temperature storage of the non-aqueous electrolyte battery, similar to Example 4-1. [Industrial applicability]

[0157] By using the non-aqueous electrolyte of the present invention as the electrolyte in a non-aqueous electrolyte battery, the recovery capacity retention rate of the non-aqueous electrolyte battery can be improved. Therefore, the non-aqueous electrolyte of the present invention can be suitably used in all fields, such as electronic devices, in which non-aqueous electrolyte batteries are used. Furthermore, the non-aqueous electrolyte of the present invention and the non-aqueous electrolyte battery using the same can be used in various known applications. Specific examples of applications include, for example, notebook computers, pen-input computers, mobile computers, e-book players, mobile phones, portable fax machines, portable copiers, portable printers, portable audio players, mini video cameras, headphone stereos, video camcorders, LCD televisions, handheld vacuum cleaners, portable CDs, MiniDiscs, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power supplies, motors, automobiles, motorcycles, mopeds, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, strobes, cameras, household backup power supplies, business backup power supplies, load leveling power supplies, and renewable energy storage power supplies.

Claims

1. A non-aqueous electrolyte comprising a compound (A) represented by formula (II), one anion-containing compound (B) selected from the group consisting of a phosphate anion-containing compound having a P-F bond and a P=O bond, and anion-containing compound having an S=O bond, and a non-aqueous solvent, wherein the content of the anion-containing compound (B) is 0.001% by mass or more and 5% by mass or less in the electrolyte. 【Chemistry 1】 (In formula (II), R 1 and R 2 Each is independently a hydrogen atom, a halogen atom, or a hydrocarbon group, however R 1 and R 2 Either one of them is a hydrocarbon group containing at least one carbon-carbon unsaturated bond.

2. In the above formula (II), R 1 and R 2 Each of these is independently a hydrogen atom, a fluorine atom, or a hydrocarbon group, and R 1 and R 2 The non-aqueous electrolyte according to claim 1, wherein either one of the members is an alkenyl group having 2 to 8 carbon atoms.

3. In the above formula (II), R 1 and R 2 either one of which is selected from a vinyl group and an allyl group, the non-aqueous electrolytic solution according to claim 2.

4. The non-aqueous electrolyte according to claim 1, wherein in formula (II), one of R1 and R2 is a vinyl group and the other is a hydrogen atom.

5. The non-aqueous electrolyte according to claim 1 or 2, containing 0.01% by mass or more and 10% by mass or less of the compound (A).

6. The non-aqueous electrolyte according to claim 1 or 2, wherein the phosphate anion-containing compound having a P-F bond and a P=O bond is a difluorophosphate anion-containing compound.

7. The non-aqueous electrolyte according to claim 6, wherein the difluorophosphate anion-containing compound is lithium difluorophosphate.

8. The non-aqueous electrolyte according to claim 1 or 2, wherein the anion-containing compound having an S=O bond is at least one selected from the group consisting of salts of fluorosulfonic acid anions and salts of fluorosulfonylimide anions.

9. The non-aqueous electrolyte according to claim 8, wherein the salt of the fluorosulfonate anion is lithium fluorosulfonate.

10. The non-aqueous electrolyte according to claim 1 or 2, wherein the mass ratio of the content of anion-containing compound (B) to the content of compound (A) (anion-containing compound (B) / compound (A)) is 0.3 or more and 5.5 or less.

11. Furthermore, the non-aqueous electrolyte according to claim 1 or 2, wherein the non-aqueous solvent contains a chain-like carboxylic acid ester.

12. The non-aqueous electrolyte according to claim 11, wherein the chain-like carboxylic acid ester is methyl acetate or methyl propionate.

13. The non-aqueous electrolyte according to claim 11, wherein the content of the chain-like carboxylic acid ester in the non-aqueous solvent is 1% by volume or more and 70% by volume or less.

14. A non-aqueous electrolyte battery comprising: a positive electrode having a positive electrode active material capable of intercalating and releasing metal ions; a negative electrode having a negative electrode active material capable of intercalating and releasing metal ions; and a non-aqueous electrolyte according to claim 1 or 2.

Citation Information

Patent Citations

  • Electrolyte additive, electrolyte and lithium ion battery

    CN111682264A

  • Nonaqueous electrolytic for lithium ion secondary battery, and the lithium ion secondary battery

    JP2005166553A

  • Electrolytic solution and battery

    JP2007273396A

  • Nonaqueous electrolyte secondary battery

    JP2010092698A

  • Lithium ion secondary battery

    JP2017139087A