Polymer composition and molded article
A tailored 4-methyl-1-pentene polymer blend with defined melting and crystallization characteristics addresses transparency and moldability issues, enabling high-quality blow-molded articles with reduced energy use.
Patent Information
- Application Number
- JP2022140183
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-06-24
- Filing Date
- 2022-09-02
- Publication Date
- 2026-11-19
- Estimated Expiration
- 2042-09-02
AI Technical Summary
Existing 4-methyl-1-pentene polymer compositions face challenges in achieving high transparency and moldability, with limitations in shape and moldability depending on molding conditions, and difficulties in blow molding due to high melting point and low melt tension.
A polymer composition comprising specific 4-methyl-1-pentene polymers with defined melting peaks, enthalpy, and crystallization time, blended in particular ratios to enhance transparency and moldability, including 15-40% 4-methyl-1-pentene copolymer (A), 40-80% copolymer (B), and 5-30% copolymer (C), optimized for blow molding.
The composition achieves superior transparency and moldability with improved blow-molding properties, allowing for the production of high-quality molded articles with reduced energy consumption and enhanced shape flexibility.
Smart Images

Figure 0007954028000001 
Figure 0007954028000002 
Figure 0007954028000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to polymer compositions and molded articles. [Background technology]
[0002] 4-methyl-1-pentene polymers, such as 4-methyl-1-pentene homopolymers or 4-methyl-1-pentene copolymers, are resins that possess superior characteristics compared to polyethylene and polypropylene, including heat resistance, transparency, lightness, steam resistance, mold release properties, gas permeability, and electrical properties. They are used in a wide range of fields, including food containers, auxiliary materials for electronic and information components, laboratory equipment, stationery, crosslinking process components, mold release films, films for electronic and information components, food packaging materials, and synthetic paper.
[0003] Traditionally, the main raw materials used for resin containers have been resins such as polyethylene, polypropylene, and polyethylene terephthalate. For example, polyethylene and polypropylene are widely used in liquid containers / bottles, fuel tanks, etc., and are generally molded by injection molding or blow molding. However, depending on the application, the transparency of these molded products may be insufficient.
[0004] On the other hand, polyethylene terephthalate is widely used mainly as a beverage container and is molded by injection blow molding (hereinafter sometimes referred to as injection blow molding). In this molding method, a molded body called a preform is created by injection molding, and then the preform is reheated and blow-molded to produce the molded body. However, although molded bodies obtained by injection blow molding of polyethylene terephthalate have excellent transparency, their heat resistance was sometimes insufficient depending on the application.
[0005] Attempts have been made to manufacture molded products using systems in which engineering plastics such as polycarbonate and polyether sulfide are added to polyethylene terephthalate to impart heat resistance. However, due to hygiene concerns related to residual monomers and cost, these methods are limited to only certain applications.
[0006] In recent years, various studies have been conducted on injection blow molded articles using polypropylene in order to obtain molded articles that overcome the heat resistance drawback of polyethylene terephthalate. However, polypropylene has several drawbacks, including the fact that handling during molding is often difficult due to the narrow molding temperature range, and that transparency is difficult to achieve when homopolypropylene is used, and heat resistance is low when random polypropylene is used, resulting in a limited number of usable polypropylene types (types, physical properties, etc.).
[0007] To address the aforementioned issues related to transparency and heat resistance, studies have been conducted on molded articles using 4-methyl-1-pentene polymers. However, because 4-methyl-1-pentene polymers have a high melting point and relatively low melt tension, obtaining molded articles from them by blow molding is often more difficult compared to other polyolefins such as polyethylene and polypropylene. For example, when attempting to mold 4-methyl-1-pentene polymers by blow molding, such as injection blow molding, the polymer often solidifies after the injection blow preform is formed, before the blow molding process can begin, making molding difficult.
[0008] As a technology to solve such problems, Patent Document 1 discloses a polymer composition containing two types of 4-methyl-1-pentene polymers, and describes a hollow molded article made from this composition that is excellent in transparency, heat resistance, toughness, and dimensional stability.
[0009] In addition, Patent Document 2 describes a 4-methyl-1-pentene copolymer composition containing a specific 4-methyl-1-pentene polymer (A) and a 4-methyl-1-pentene copolymer (B) that possesses transparency and rigidity while having high impact resistance and high heat resistance. Patent Document 3 describes that specific 4-methyl-1-pentene polymer particles can have their rigidity reduced, i.e., their flexibility improved, without impairing properties such as high stereoregularity and excellent heat resistance. [Prior art documents] [Patent Documents]
[0010] [Patent Document 1] International Publication No. 2013 / 099876 [Patent Document 2] Japanese Patent Publication No. 2018-162408 [Patent Document 3] International Publication No. 2019 / 198694 [Overview of the Initiative] [Problems that the invention aims to solve]
[0011] However, depending on the application, a molded article with even higher transparency than those obtained from the polymer compositions described in Patent Documents 1 to 3 may be desirable. Furthermore, with the compositions described in Patent Documents 2 and 3, the shape may be limited and the moldability may be insufficient depending on the molding conditions, indicating room for improvement.
[0012] The object of the present invention is to provide a polymer composition that possesses the excellent physical properties such as heat resistance of conventional 4-methyl-1-pentene polymers, while having superior transparency and moldability compared to conventional 4-methyl-1-pentene polymer compositions. [Means for solving the problem]
[0013] As a result of intensive studies conducted by the present inventors, it has been found that the above-mentioned problems can be solved by a polymer composition containing a 4-methyl-1-pentene-based polymer that satisfies specific requirements, and the present invention has been completed.
[0014] That is, the present invention includes, for example, the following matters [1] to [9].
[0015] [1] A polymer composition (X) comprising a 4-methyl-1-pentene-based polymer, which satisfies the following requirements (X-1) to (X-3). Requirement (X-1): Using a pellet-shaped composition, the endothermic curve measured by DSC in accordance with JIS K7122 has two or more melting peaks. Requirement (X-2): Among the melting peaks in the endothermic curve, the melting enthalpy ΔH1 obtained from the peak area of the melting peak having the highest peak temperature is less than 20.0 J / g. Requirement (X-3): Using the pellet-shaped composition, the half-crystallization time at 215°C measured by DSC according to the following measurement method exceeds 800 seconds or is not observed. Measurement method: Using DSC8500 manufactured by PerkinElmer Co., Ltd., the temperature is raised from 30°C to 280°C at a heating rate of 500°C / min, the temperature is maintained for 10 minutes, and then the temperature is lowered to 215°C at a cooling rate of 500°C / min, and the half-crystallization time at 215°C is measured under this state.
[0016] [2] 15 to 40% by mass of a 4-methyl-1-pentene copolymer (A) that satisfies the following requirements (A-i) and (A-ii), and 40 to 80% by mass of a 4-methyl-1-pentene copolymer (B) that satisfies the following requirements (B-i) to (B-iii), and 5 to 30% by mass of a 4-methyl-1-pentene copolymer (C) that satisfies the following requirements (C-i) to (C-iii), The polymer composition (X) according to [1], comprising the above (provided that the total amount of the copolymer (A), the copolymer (B) and the copolymer (C) is 100% by mass). Requirement (Ai): When the sum of constituent units (i) derived from 4-methyl-1-pentene and constituent units (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) is taken as 100 mol%, the content of constituent unit (i) is 97.5 mol% or more and less than 100 mol%, and the content of constituent unit (ii) is greater than 0 mol% and 2.5 mol% or less. Requirement (A-ii): Intrinsic viscosity [η] measured in decalin at 135°C. A The levels are 1.0 to 5.0 dl / g. Requirements (Bi): When the sum of constituent units (i) derived from 4-methyl-1-pentene and constituent units (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) is taken as 100 mol%, the content of constituent unit (i) is 91.0 mol% or more and less than 97.5 mol%, and the content of constituent unit (ii) is greater than 2.5 mol% and less than or equal to 9.0 mol%. Requirement (B-ii): Intrinsic viscosity [η] measured in decalin at 135°C. B The levels are 2.0 to 5.0 dl / g. Requirement (B-iii): The melting point (Tm) measured by DSC is less than 180°C. Requirement (Ci): Contains a constituent unit (i) derived from 4-methyl-1-pentene, and when the sum of constituent unit (i) and constituent unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) is taken as 100 mol%, the content of constituent unit (i) is less than 91.0 mol%, and the content of constituent unit (ii) is greater than 9.0 mol%. Requirement (C-ii): Intrinsic viscosity [η] measured in decalin at 135°C. C The levels are 2.0 to 5.0 dl / g. Requirement (C-iii): The melting point (Tm) is not observed by DSC.
[0017] [3] The polymer composition (X) described in [1] or [2], wherein the 4-methyl-1-pentene polymer contained in the polymer composition (X) is such that when the sum of the constituent units (i) derived from 4-methyl-1-pentene and the constituent units (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) is 100 mol%, the content of constituent unit (ii) is 4.0 to 10.0 mol%.
[0018] [4] A molded article comprising the polymer composition (X) described in any one of [1] to [3].
[0019] [5] The molded article described in [4], which is a blow-molded article.
[0020] [6] The molded article according to [4] or [5], wherein the molded article is a blow-molded article formed by blow-molding a preform formed by injection molding.
[0021] [7] A bottle container, the molded body described in any one of [4] to [6].
[0022] [8] Formed by stretch blow molding, A molded article according to any one of [5] to [7], wherein the product of the stretch ratio in the longitudinal direction and the stretch ratio in the transverse direction in the stretch blow molding is 1.2 to 6.0 times.
[0023] [9] A step (1) of forming a preform from a polymer composition (X) described in any one of [1] to [3], The process includes (2) stretch blow molding the preform into a blow-molded body, A method for manufacturing a blow-molded article, wherein the product of the stretch ratio in the longitudinal direction and the stretch ratio in the transverse direction in the stretch blow molding is 1.2 to 6.0 times. [Effects of the Invention]
[0024] According to the present invention, a polymer composition is provided that possesses the excellent physical properties such as heat resistance of conventional 4-methyl-1-pentene polymers, while having superior transparency and moldability compared to conventional 4-methyl-1-pentene polymer compositions. [Modes for carrying out the invention]
[0025] In this specification, unless otherwise specified, A to B means A or greater and B or less. Furthermore, in this specification, polymerization and copolymerization may be referred to as polymerization, and polymers and copolymers may be collectively referred to as polymers.
[0026] ≪Polymer composition (X)≫ The polymer composition (X) of the present invention comprises a 4-methyl-1-pentene polymer and satisfies the following requirements (X-1) to (X-3). In this specification, unless otherwise specified, the "4-methyl-1-pentene polymer" may be a homopolymer of 4-methyl-1-pentene or a 4-methyl-1-pentene copolymer obtained by polymerizing 4-methyl-1-pentene and a comonomer.
[0027] <Physical properties of polymer composition (X)> [Requirements (X-1)] A polymer composition (X) in pellet form is measured using a differential scanning calorimeter (DSC) in accordance with JIS K7122, and the endothermic curve shows two or more melting peaks. The number of melting peaks observed in the endothermic curve is preferably two or more, and more preferably two.
[0028] For example, one method for obtaining a composition that satisfies requirement (X-1) is to blend two or more types of 4-methyl-1-pentene polymers whose melting points are observed by DSC. When a polymer composition (X) that satisfies requirement (X-1) is obtained by blending multiple 4-methyl-1-pentene polymers, the polymer composition (X) has a broader compositional distribution compared to a composition that does not satisfy requirement (X-1), resulting in good compatibility among the multiple types of 4-methyl-1-pentene polymers contained in the polymer composition (X). As a result, the multiple types of 4-methyl-1-pentene polymers contained in the polymer composition (X) have similar refractive indices and are less prone to phase separation from one another, and the transparency of the molded article obtained by molding the polymer composition (X) tends to be good.
[0029] In this specification, in order to distinguish between melting peaks appearing in an endothermic curve, the melting peak with the nth highest peak temperature may be referred to as the "nth melting peak." For example, the melting peak with the highest peak temperature may be referred to as the "first melting peak," and the melting peak with the second highest peak temperature may be referred to as the "second melting peak."
[0030] The peak temperature of the first melting peak is preferably 180 to 250°C, more preferably 200 to 245°C, and even more preferably 220 to 240°C. On the other hand, the peak temperature of the second melting peak is preferably less than 180°C, more preferably 100 to 175°C, and even more preferably 100 to 170°C. When the first melting peak is within the above range, the heat resistance tends to be high. When the second melting peak is within the above range, the moldability is good, and the refractive index is close among the multiple types of 4-methyl-1-pentene polymers contained in the polymer composition (X), resulting in good compatibility and less phase separation, which tends to result in good transparency of the molded article formed from the polymer composition (X).
[0031] [Requirements (X-2)] Among the melting peaks in the aforementioned endothermic curve, the enthalpy of fusion ΔH1 obtained from the peak area of the melting peak with the highest peak temperature (first melting peak) is less than 20.0 J / g. The enthalpy of fusion ΔH1 is preferably 18.0 J / g or less, more preferably 17.5 J / g or less, and even more preferably 17.0 J / g or less. There is no particular lower limit to the enthalpy of fusion ΔH1, but it is usually 10.0 J / g or more. When the enthalpy of fusion ΔH1 is within the above range, crystallization when the polymer composition (X) is cooled is easily suppressed, so the hardness of the polymer composition (X) when cooled is softer than that of a 4-methyl-1-pentene polymer whose enthalpy of fusion ΔH1 is not within the above range. As a result, the blow moldability of the polymer composition (X) is improved.
[0032] As a method for determining the enthalpy of fusion ΔH1 from the endothermic curve, a known method for calculating peak area can be used. If the first fusion peak is a multi-peak containing multiple peak tops, the entire multi-peak is considered as a single fusion peak, the peak area is calculated, and the obtained value is taken as the enthalpy of fusion ΔH1. However, if the first fusion peak is a multi-peak containing multiple peak tops, ΔH1 is defined as the integral value of the multi-peak in the range of 180 to 250°C.
[0033] [Requirements (X-3)] Using a pellet-shaped polymer composition (X), the semi-crystallization time (Tc) at 215°C was measured by DSC using the following measurement method. 1 / 2 ) exceeds 800 seconds or is not observed. Measurement method: Using a PerkinElmer DSC8500, the temperature is raised from 30°C to 280°C at a heating rate of 500°C / min, the temperature is maintained for 10 minutes, and then the temperature is cooled down to 215°C at a cooling rate of 500°C / min. The semi-crystallization time at 215°C is then measured. The aforementioned semi-crystallization time is preferably 900 seconds or more or not observed, more preferably 1000 seconds or more or not observed, and even more preferably 1200 seconds or more or not observed. The blow-molding properties of the polymer composition (X) are improved when the semi-crystallization time of the polymer composition (X) satisfies the above conditions. For example, when blow-molding a preform molded from the polymer composition (X) by reheating it before it has completely cooled (the 1.5-stage method described later), reheating for blow-molding can be performed before the polymer composition (X) has completely crystallized. As a result, blow-molding can be performed while keeping the energy (cost) of heating relatively low. Furthermore, when blow-molding a preform molded from the polymer composition (X) by reheating it after it has completely cooled (the 2-stage method described later), the energy required for heating to plasticize the polymer composition (X) and the energy required to maintain the molten state are less than when using a 4-methyl-1-pentene polymer composition that does not satisfy requirement (X-3). As a result, blow-molding can be performed while keeping the energy (cost) of heating and heat retention relatively low.
[0034] The polymer composition (X) preferably further satisfies one or more of the following requirements (X-4) to (X-6). More preferably, the polymer composition (X) satisfies all of the following requirements (X-4) to (X-6).
[0035] [Requirements (X-4)] In polymer composition (X), when the total of the constituent units (i) derived from 4-methyl-1-pentene and the constituent units (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) is set to 100 mol%, the content of constituent unit (ii) is preferably 4.0 to 10.0 mol%, more preferably 5.0 to 9.0 mol%, and even more preferably 6.0 to 8.0 mol%. Here, if the polymer composition (X) contains multiple 4-methyl-1-pentene polymers, it is preferable that the content of the constituent unit (ii) in the polymer composition (X) is within the above range, when the sum of the constituent unit (i) in the polymer composition (X) and the constituent unit (ii) in the polymer composition (X) is 100 mol%.
[0036] If the polymer composition (X) satisfies requirement (X-4), it exhibits an excellent balance of stretchability and transparency.
[0037] The α-olefin that leads to the structural unit (ii) in the 4-methyl-1-pentene polymer contained in polymer composition (X) can be a linear α-olefin. Examples of α-olefins that lead to the structural unit (ii) include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-eicosene, and the like. Among these, linear α-olefins having 6 to 18 carbon atoms are preferred from the viewpoint of heat resistance, and linear α-olefins having 10 to 18 carbon atoms are more preferred. Specifically, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, etc. are preferred, and among these, 1-decene, 1-hexadecene, and 1-octadecene are particularly preferred. The constituent unit (ii) may be derived from only one selected from the group consisting of ethylene or α-olefins having 3 to 20 carbon atoms, or it may be derived from two or more selected from the group consisting of ethylene or α-olefins having 3 to 20 carbon atoms. When the constituent unit (ii) is derived from two or more selected from the group consisting of ethylene or α-olefins having 3 to 20 carbon atoms, the transparency of the polymer composition (X) tends to be higher when the carbon numbers of the α-olefins that derive the constituent unit (ii) are close.
[0038] [Requirements (X-5)] The intrinsic viscosity [η] of the polymer composition (X), measured in decalin at 135°C by the method described in the examples below, is preferably 2.5 to 4.5 dl / g, more preferably 2.8 to 4.2 dl / g, and even more preferably 3.0 to 4.0 dl / g. A polymer composition (X) having an intrinsic viscosity [η] within the above range exhibits excellent injection moldability in the step of forming a preform (1) and excellent stretchability in the step of stretch blow molding from the preform to a blow-molded article (2), resulting in good moldability during blow molding.
[0039] [Requirements (X-6)] The MFR (at 260°C and 5kg load) of polymer composition (X), as measured by the method described in the examples below, is preferably 5.0 to 40 g / 10 min, more preferably 10 to 35 g / 10 min, and even more preferably 15 to 30 g / 10 min. Polymer compositions (X) whose MFR (260°C, 5kg load) value falls within the above range exhibit excellent injection moldability in the step of forming a preform (1), and excellent stretchability in the step of stretch blow molding from the preform to a blow-molded article (2), resulting in good moldability during blow molding.
[0040] The polymer composition (X) is not particularly limited in composition as long as it satisfies the above requirements (X-1) to (X-3) and contains a 4-methyl-1-pentene polymer. For example, polymer composition (X) may contain specific 4-methyl-1-pentene copolymers (A), (B), and (C).
[0041] <4-methyl-1-pentene copolymer (A)> The 4-methyl-1-pentene copolymer (A) (hereinafter also referred to as "polymer (A)") preferably satisfies one or more of the following requirements (Ai) to (A-iii). More preferably, copolymer (A) satisfies requirements (Ai) and (A-ii), and even more preferably, copolymer (A) satisfies all of requirements (Ai) to (A-iii).
[0042] Copolymer (A) may contain only one type of copolymer, or it may contain two or more types of copolymers. If copolymer (A) contains two or more types of copolymers, it is preferable that each copolymer satisfies one or more of the following requirements (Ai) to (A-iii).
[0043] [Requirements (Ai)] When the sum of the content of structural unit (i) derived from 4-methyl-1-pentene and the content of structural unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms is taken as 100 mol%, the content of structural unit (i) is preferably 97.5 mol% or more and less than 100 mol%, and the content of structural unit (ii) is preferably greater than 0 mol% and 2.5 mol% or less.
[0044] In copolymer (A), the content of structural unit (i) derived from 4-methyl-1-pentene is more preferably 97.5 to 99.5 mol%, and even more preferably 97.7 to 99.0 mol%. The content of structural unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms is more preferably 0.5 to 2.5 mol%, and even more preferably 1.0 to 2.3 mol%.
[0045] In copolymer (A), if the content of structural unit (i) derived from 4-methyl-1-pentene, and the content of structural unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms are within the aforementioned range, a polymer composition with good moldability while maintaining heat resistance can be obtained. For example, if the same amount of 4-methyl-1-pentene homopolymer is used instead of copolymer (A), the moldability of the resulting composition tends to be worse compared to when copolymer (A) is used. This is presumed to be because 4-methyl-1-pentene homopolymer has a fast crystallization rate, which tends to result in poor resin elongation during molding.
[0046] The preferred α-olefin for deriving the constituent unit (ii) contained in copolymer (A) is the same as the preferred α-olefin for deriving the constituent unit (ii) contained in the 4-methyl-1-pentene polymer contained in polymer composition (X).
[0047] The α-olefins that lead to the constituent unit (ii) contained in copolymer (A) may be one type or two or more types.
[0048] Copolymer (A) may further have constituent units derived from other polymerizable compounds other than 4-methyl-1-pentene, ethylene, and α-olefins having 3 to 20 carbon atoms, to the extent that it does not impair the objectives of the present invention. Other polymerizable compounds include, for example, vinyl compounds having a cyclic structure such as styrene, vinylcyclopentene, vinylcyclohexane, vinylnorbornane; vinyl esters such as vinyl acetate; unsaturated organic acids or derivatives thereof such as maleic anhydride; conjugated dienes such as butadiene, isoprene, pentadiene, 2,3-dimethylbutadiene; 1,4-hexadiene, 1,6-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, 7-methyl-1,6-octadiene, Examples of non-conjugated polyenes include dicyclopentadiene, cyclohexadiene, dicyclooctadiene, methylenenorbornene, 5-vinylnorbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, 6-chloromethyl-5-isopropene-2-norbornene, 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, and 2-propenyl-2,2-norbornadiene.
[0049] In copolymer (A), the content of constituent units derived from other polymerizable compounds is usually 10 mol% or less, preferably 5 mol% or less, and more preferably 3 mol% or less, out of 100 mol% of the total constituent units constituting copolymer (A).
[0050] [Requirements (A-ii)] The intrinsic viscosity [η] of copolymer (A) measured in decalin at 135°C. A The amount is preferably 1.0 to 5.0 dl / g, more preferably 1.0 to 4.0 dl / g, and even more preferably 1.0 to 3.0 dl / g. [η] A This can be adjusted, for example, by the amount of hydrogen added during the polymerization process when producing copolymer (A).
[0051] [η] A Copolymer (A) within the above range exhibits good fluidity during the preparation and molding of polymer compositions. Furthermore, when combined with 4-methyl-1-pentene copolymer (B) and 4-methyl-1-pentene copolymer (C), it is thought that uniform melt-kneading is easily achieved, contributing to improved transparency and blow-molding properties.
[0052] [Requirement (A-iii)] As described in the examples below, the melting point (Tm) measured by differential scanning calorimeter (DSC) is preferably 180 to 250°C, more preferably 200 to 245°C, and even more preferably 220 to 240°C. When the melting point (Tm) measured by differential scanning calorimeter (DSC) is within the above range, the polymer composition (X) containing copolymer (A) and the molded article obtained from polymer composition (X) have good heat resistance. The melting point (Tm) value tends to depend on the stereoregularity of copolymer (A) and the content of constituent unit (ii) in copolymer (A). Therefore, the melting point (Tm) can be adjusted by using the olefin polymerization catalyst described later and by controlling the content of constituent unit (ii).
[0053] <4-methyl-1-pentene copolymer (B)> The 4-methyl-1-pentene copolymer (B) (hereinafter also referred to as "polymer (B)") preferably satisfies one or more of the following requirements (Bi) to (B-iii). More preferably, copolymer (B) satisfies all of requirements (Bi) to (B-iii).
[0054] Copolymer (B) may contain only one type of copolymer, or it may contain two or more types of copolymers. If copolymer (B) contains two or more types of copolymers, it is preferable that each copolymer satisfies one or more of the following requirements (Bi) to (B-iii).
[0055] [Requirements (Bi)] When the sum of the content of constituent unit (i) derived from 4-methyl-1-pentene and the content of constituent unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms is taken as 100 mol%, the content of constituent unit (i) is preferably 91.0 mol% or more and less than 97.5 mol%, and the content of constituent unit (ii) is preferably greater than 2.5 mol% and 9.0 mol% or less.
[0056] In copolymer (B), the content of structural unit (i) derived from 4-methyl-1-pentene is more preferably 91.5 to 96.0 mol%, and even more preferably 92.0 to 95.0 mol%. The content of structural unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms is more preferably 4.0 to 8.5 mol%, and even more preferably 5.0 to 8.0 mol%.
[0057] In copolymer (B), if the content of structural unit (i) derived from 4-methyl-1-pentene, and the content of structural unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms are within the aforementioned range, a polymer composition with good moldability can be obtained. For example, if the same amount of 4-methyl-1-pentene homopolymer is used instead of copolymer (B), the moldability of the resulting composition tends to be worse compared to when copolymer (B) is used. This is presumed to be because 4-methyl-1-pentene homopolymer has a fast crystallization rate, which tends to result in poor resin elongation during molding.
[0058] Preferred α-olefins leading to the structural unit (ii) contained in the copolymer (B) are the same as the preferred α-olefins leading to the structural unit (ii) contained in the 4-methyl-1-pentene-based polymer contained in the polymer composition (X). The α-olefin leading to the structural unit (ii) contained in the copolymer (B) may be only one type, or two or more types.
[0059] [Requirement (B-ii)] The intrinsic viscosity [η] of the copolymer (B) measured in decalin at 135°C B is preferably 2.0 to 5.0 dl / g, more preferably 3.0 to 5.0 dl / g, further preferably 3.5 to 5.0 dl / g, and particularly preferably 4.0 to 4.5 dl / g. [η] B can be adjusted, for example, by the amount of hydrogen added in the polymerization step when producing the copolymer (B).
[0060] [η] B The copolymer (B) having [η] in the above range exhibits good fluidity during preparation of the polymer composition and during molding. Further, when combined with the 4-methyl-1-pentene copolymer (A) and the 4-methyl-1-pentene copolymer (C), it is considered to contribute to the improvement of stretchability. In addition, since it is uniformly melt-kneaded, it contributes to transparency. In particular, [η] B being at or above the aforementioned lower limit value results in more excellent stretchability when molding the polymer composition (X).
[0061] [Requirement (B-iii)] The melting point (Tm) measured by a differential scanning calorimeter (DSC) according to the method described in the Examples below is preferably less than 180°C, more preferably 100 to 175°C, and further preferably 100 to 170°C. The melting point (Tm) tends to depend on the stereoregularity of copolymer (B) and the content of constituent unit (ii) in copolymer (B). Therefore, the melting point (Tm) can be adjusted by using the olefin polymerization catalyst described later and by controlling the content of constituent unit (ii).
[0062] <4-methyl-1-pentene copolymer (C)> The 4-methyl-1-pentene copolymer (C) (hereinafter also referred to as "polymer (C)") preferably satisfies one or more of the following requirements (Ci) to (C-iii). More preferably, the copolymer (C) satisfies all of the requirements (Ci) to (C-iii).
[0063] Copolymer (C) may contain only one type of copolymer, or it may contain two or more types of copolymers. If copolymer (C) contains two or more types of copolymers, it is preferable that each copolymer satisfies one or more of the following requirements (Ci) to (C-iii).
[0064] [Requirements (Ci)] The material contains a constituent unit (i) derived from 4-methyl-1-pentene, and when the sum of the content of constituent unit (i) and the content of constituent unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms is taken as 100 mol%, the content of constituent unit (i) is preferably less than 91.0 mol%, and the content of constituent unit (ii) is preferably greater than 9.0 mol%.
[0065] In copolymer (C), the content of structural unit (i) derived from 4-methyl-1-pentene is more preferably 50.0 mol% or more and less than 91.0 mol%, and even more preferably 70.0 to 90.0 mol%. The content of structural unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms is more preferably greater than 9.0 mol% and 50 mol% or less, and even more preferably 10.0 to 30.0 mol%.
[0066] In copolymer (C), if the content of structural unit (i) derived from 4-methyl-1-pentene, and the content of structural unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms are within the aforementioned range, a polymer composition with good moldability can be obtained while maintaining the properties of the 4-methyl-1-pentene polymer (e.g., heat resistance, transparency, etc.). For example, if the same amount of 4-methyl-1-pentene homopolymer is used instead of copolymer (C), the moldability of the resulting composition tends to be worse compared to when copolymer (C) is used. This is presumed to be because 4-methyl-1-pentene homopolymer has a fast crystallization rate, which tends to result in poor resin elongation during molding.
[0067] The preferred α-olefin for deriving the constituent unit (ii) contained in copolymer (C) is the same as the preferred α-olefin for deriving the constituent unit (ii) contained in the 4-methyl-1-pentene polymer contained in polymer composition (X). The α-olefins that lead to the constituent unit (ii) contained in the copolymer (C) may be one type or two or more types.
[0068] [Requirement (C-ii)] The intrinsic viscosity [η] of copolymer (C) measured in decalin at 135°C. C The amount is preferably 2.0 to 5.0 dl / g, more preferably 3.0 to 5.0 dl / g, even more preferably 3.5 to 5.0 dl / g, and particularly preferably 4.0 to 4.5 dl / g. [η] C This can be adjusted, for example, by the amount of hydrogen added during the polymerization process when producing copolymer (C).
[0069] [η] C Copolymer (C) within the above range exhibits good fluidity during the preparation and molding of polymer compositions. Furthermore, it is thought to contribute to improved stretchability when combined with 4-methyl-1-pentene copolymer (A) and 4-methyl-1-pentene copolymer (B). In particular, [η] CIf the value is above the lower limit, the stretchability of the polymer composition (X) when molding is improved.
[0070] [Requirement (C-iii)] As described in the examples below, the melting point (Tm) is not observed when measured with a differential scanning calorimeter (DSC) using the method described. When the melting point (Tm) of the copolymer (C) is not observed when measured with a differential scanning calorimeter (DSC), the polymer composition (X) containing the copolymer (C) becomes easier to stretch, and the thickness distribution of the molded article formed from the polymer composition (X) tends to become smaller.
[0071] <Methods for producing copolymer (A), copolymer (B), and copolymer (C)> Copolymer (A), copolymer (B), and copolymer (C) can all be obtained by polymerizing 4-methyl-1-pentene with a specific olefin that leads to the above-mentioned structural unit (ii), and optionally with the other monomers, in the presence of an olefin polymerization catalyst, using a known method.
[0072] Examples of olefin polymerization catalysts that can be used in the production of copolymer (A), copolymer (B), and copolymer (C) include metallocene catalysts. Preferred metallocene catalysts include those described in International Publication No. 01 / 53369, International Publication No. 01 / 27124, Japanese Patent Publication No. 3-193796, Japanese Patent Publication No. 02-41303, International Publication No. 06 / 025540, International Publication No. 2013 / 009876, International Publication No. 2014 / 050817, International Publication No. 2014 / 123212, or International Publication No. 2017 / 150265.
[0073] Furthermore, copolymers (A), (B), and (C) may be polymerized in the presence of other polymers by multi-stage polymerization. For example, copolymer (A) may be polymerized in the first stage of polymerization, copolymer (B) may be polymerized in the presence of copolymer (A), and copolymer (C) may be polymerized in the presence of copolymers (A) and (B). Similarly, copolymer (A) may be polymerized in the presence of one or more of copolymers (B) and (C), and copolymer (B) may also be polymerized in the presence of one or more of copolymers (A) and (C).
[0074] Copolymers (A), (B), and (C) may be commercially available 4-methyl-1-pentene copolymers (for example, TPX® manufactured by Mitsui Chemicals, Inc.). Copolymer (A) may be a copolymer (A) prepared by heat-treating a 4-methyl-1-pentene copolymer, which has been produced using the catalyst mentioned above, in an extruder or mixer. Alternatively, copolymer (A) may be prepared by heat-treating a commercially available 4-methyl-1-pentene copolymer (for example, TPX® manufactured by Mitsui Chemicals, Inc.) in an extruder or mixer.
[0075] <Amounts of various components blended into polymer composition (X)> The content of copolymer (A) in polymer composition (X) is preferably 15 to 40% by mass, more preferably 20 to 40% by mass, and even more preferably 24 to 36% by mass, based on the total content of copolymer (A), copolymer (B), and copolymer (C) being 100% by mass. The content of copolymer (B) in polymer composition (X) is preferably 40 to 80% by mass, more preferably 40 to 70% by mass, and even more preferably 44 to 66% by mass, based on the total content of copolymer (A), copolymer (B), and copolymer (C) being 100% by mass. The content of copolymer (C) in polymer composition (X) is preferably 5 to 30% by mass, more preferably 7 to 25% by mass, and even more preferably 9 to 25% by mass, when the total content of copolymer (A), copolymer (B), and copolymer (C) is taken as 100% by mass.
[0076] As described above, in polymer composition (X), copolymer (B) has the highest content among copolymer (A), copolymer (B), and copolymer (C). Here, as the proportion of constituent unit (ii) in polymer composition (X) increases, crystallization when polymer composition (X) is cooled tends to be suppressed. Copolymer (B) has a higher content of constituent unit (ii) than copolymer (A), and is also present in a higher amount in polymer composition (X) than copolymer (C), so the semi-crystallization time of polymer composition (X) can be controlled by the content of copolymer (B). As a result of appropriately controlling the semi-crystallization time of polymer composition (X), the blow moldability of polymer composition (X) is improved. Furthermore, by setting the content of copolymer (A), copolymer (B), and copolymer (C) in polymer composition (X) within the above range, a molded article with an excellent balance of heat resistance and rigidity can be obtained.
[0077] The total content of copolymers (A), (B), and (C) in polymer composition (X) is usually 97.0% by mass or more, preferably 98.0% by mass or more, and more preferably 99.0% by mass or more, when the mass of polymer composition (X) is taken as 100% by mass. The upper limit of the total content of copolymers (A), (B), and (C) may be 100% by mass of polymer composition (X). If the polymer composition (X) contains other components (for example, other polymer components and additives described later), the upper limit is defined by the content of the other components.
[0078] [Other polymer components] The polymer composition (X) may further contain other polymer components other than copolymer (A), copolymer (B), and copolymer (C). Examples of other polymer components include 4-methyl-1-pentene copolymers other than copolymer (A), copolymer (B), and copolymer (C).
[0079] If the polymer composition (X) contains polymer components other than copolymer (A), copolymer (B), and copolymer (C), the content of these polymer components is usually 3.0 parts by mass or less, preferably 2.0 parts by mass or less, and more preferably 1.0 part by mass or less, when the total content of copolymer (A), copolymer (B), and copolymer (C) is 100 parts by mass.
[0080] [Additives] The polymer composition (X) may contain conventionally known additives. Examples of additives include secondary antioxidants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, antiblocking agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, fillers, and hydrochloric acid absorbents. The content of additives is not particularly limited, but if the total of copolymer (A), copolymer (B), and copolymer (C) is 100 parts by mass, then each additive is usually 0 to 50 parts by mass, preferably 0 to 10 parts by mass. The polymer composition (X) may contain one or more additives.
[0081] ≪Method for producing polymer composition (X)≫ Polymer composition (X) can be obtained, for example, by mixing copolymer (A), copolymer (B), and copolymer (C) described above with other polymer components and additives as needed. Mixtures of two or more copolymers (A), copolymer (B), and copolymer (C) can also be obtained by the multi-stage polymerization method described above.
[0082] Regarding the mixing method of each component, various known methods can be employed, such as mixing each component using equipment such as a plast mill, Henschel mixer, V-blender, ribbon blender, tumbler, blender, or kneader-ruder; or, after the mixing, the resulting mixture can be further melt-kneaded using equipment such as a single-screw extruder, twin-screw extruder, kneader, or Banbury mixer, and the resulting melt-kneaded product can be granulated or pulverized.
[0083] Molded body The molded article of the present invention comprises the polymer composition (X). The molded article of the present invention is obtained by using a polymer composition (X) and subjecting it to known thermoforming methods such as extrusion molding, injection molding, inflation molding, blow molding, extrusion blow molding, injection blow molding, stretch blow molding, press molding, stamping molding, vacuum forming, calendering, filament molding, foam molding, and powder slush molding.
[0084] Since the polymer composition (X) has excellent moldability, a molded article can be suitably produced by the molding method described above. In particular, the polymer composition (X) exhibits high moldability even when subjected to injection blow molding and stretch blow molding, making it possible to obtain suitable molded articles. From this viewpoint, the molded articles of the present invention are particularly advantageous when they are obtained by blow molding, especially when they are obtained by injection blow molding or stretch blow molding.
[0085] <Blow molded product> A preferred embodiment of the molded article of the present invention is a hollow molded article obtained by blow molding, such as injection blow molding or stretch blow molding.
[0086] <Method for manufacturing blow-molded articles> A blow-molded article containing the polymer composition (X) can be produced by a commonly known blow-molding method. Blow molding is a method of forming a hollow body by first molding a preform (e.g., a parison) from resin, then sandwiching this preform between molds, injecting pressurized gas into the heated preform to make the resin adhere to the mold, and then cooling it. Methods for manufacturing this preform include injection molding and extrusion molding, and corresponding blow molding methods include injection blow molding and extrusion blow molding. In addition, there is also stretch blow molding, which includes a stretching process when injecting pressurized gas into the heated preform. For example, in biaxial stretch blow molding, a stretching rod is inserted deep into the preform to stretch it vertically, and pressurized gas is simultaneously blown in horizontally to expand it horizontally as well, thereby obtaining a biaxially stretched hollow molded body.
[0087] Furthermore, blow molding has traditionally been divided into two main methods: a two-stage method in which a preform is first molded and cooled to obtain a cold parison, and then this cold parison is reheated in the mold before pressurized gas is injected; and a direct blow molding method (one-stage method) in which a parison is molded from molten resin and then pressurized gas is immediately injected into the heated preform (hot parison). The two-stage method is efficient in that it separates the parison manufacturing process from the pressurized gas injection (blow) process, but it has problems in terms of production costs (energy loss) because it requires reheating the cold parison. On the other hand, the one-stage method is superior in that it does not have this energy loss, but it has problems in that the types of resins that can be used are limited and the shapes that can be stretch-blown are limited. Therefore, in order to achieve both production efficiency and versatility, there is a method known as the 1.5-stage method, in which, after the preform is manufactured, it is transferred to equipment for a different process than the equipment used in the preform manufacturing process, and a pressurized gas blowing process is performed on the preform while it is not completely cooled (partially heated).
[0088] When the polymer composition (X) of the present invention is used in blow molding, it can be applied to either the one-stage method or the two-stage method, but it can also be applied to the 1.5-stage method. Furthermore, it is suitable for injection blow molding, in which a pressurized gas blowing (blow) step is performed after the preform is formed by injection molding. Moreover, it is suitable for stretch blow molding, in which a stretching step is performed when the pressurized gas blowing (blow) step is performed.
[0089] A preferred example of a method for manufacturing a stretch blow-molded article is a manufacturing method that includes the steps of forming a preform from a polymer composition (X) (1) and stretch blow-molding the preform into a blow-molded article (2).
[0090] [Process (1)] First, let's explain step (1). A preform is formed by melting the polymer composition (X) and injecting this resin into a mold. The temperature when melting and injecting the polymer composition (X) is usually in the range of 260 to 320°C. The molded preform is removed from the mold, and the draft angle of the preform in the mold is preferably 2.0 to 5.0°. By making the draft angle relatively large, it becomes possible to remove the preform at a high temperature and also reduces scratches during removal. Furthermore, by making the draft angle relatively large, the preform can be easily removed from the mold, so when the 1.5-stage method is used, it becomes easier to secure the heat retained by the preform necessary for the blow process.
[0091] [Process (2)] In step (2), first, the surface temperature of the preform formed in step (1) is raised to 130-220°C, preferably 135-215°C, and more preferably 140-210°C. When the surface temperature of the preform is within this range, the preform is in a softened state and easy to blow mold. If the surface temperature of the preform is lower than this range, it is reheated as appropriate using an infrared heater or the like until the surface temperature reaches this range. The surface temperature of the preform can be measured, for example, by imaging the preform from a distance of 1m using a FLIR C5 infrared camera manufactured by FLIR Systems.
[0092] Once the surface temperature of the preform reaches the aforementioned range, stretch blow molding is performed. In stretch blow molding, first, the preform is placed in a blow molding die, and a stretching rod is inserted through the opening of the preform. The preform is then stretched in the axial direction of the stretching rod (the longitudinal direction of the preform). After the longitudinal stretching, or in parallel with the longitudinal stretching, gas is injected into the blow molding die to stretch the preform laterally (the radial direction of the preform) while simultaneously molding it into the desired shape. In this way, stretch blow molding performs biaxial stretching, which improves the strength of the molded product.
[0093] When a preform formed from a polymer composition (X) is used, the temperature at which the stretch blow molding is performed (stretch blow temperature) is typically 130 to 220°C, preferably 135 to 215°C, and more preferably 140 to 210°C. When the stretch blow temperature is within the above range, surface roughness during blow stretching due to insufficient heat can be prevented, and furthermore, appearance defects caused by uneven thickness or deformation due to thermal deformation of the preform can be prevented.
[0094] Furthermore, when a preform formed from polymer composition (X) is used, from the viewpoint of uniform stretching, the stretch ratio in the longitudinal direction by stretch blow molding is preferably 1.1 to 2.0 times, more preferably 1.1 to 1.9 times, and even more preferably 1.1 to 1.8 times. Since polymer composition (X) satisfies requirement (X-2), the melting enthalpy ΔH1 obtained from the first melting peak is relatively small, and as a result, blow molding can be performed even with a high stretch ratio in the longitudinal direction. It tends to be easy. Furthermore, since polymer composition (X) satisfies requirement (X-3), the semi-crystallization time is relatively long, and as a result, it tends to be easy to blow mold. The stretch ratio in the longitudinal direction is calculated as follows. Vertical stretching ratio = (height of bottle molded product) / (height of preform)
[0095] When a preform formed from polymer composition (X) is used, from the viewpoint of uniform stretching, the lateral stretching ratio by the stretch blow molding is preferably 1.1 to 3.5 times, more preferably 1.2 to 3.0 times, and even more preferably 1.3 to 2.8 times. Since polymer composition (X) satisfies requirement (X-2), the melting enthalpy ΔH1 obtained from the first melting peak is relatively small, and as a result, blow molding tends to be easy even at high lateral stretching ratios. Furthermore, since polymer composition (X) satisfies requirement (X-3), the semi-crystallization time is relatively long, and as a result, blow molding tends to be easy. Note that when the molded body is a bottle, the lateral stretching ratio is calculated as follows. Lateral stretching ratio = (Circumference of bottle) / (Circumference of preform)
[0096] When a preform formed from a polymer composition (X) is used, the product of the longitudinal stretching ratio and the transverse stretching ratio by stretch blow molding (total stretching ratio) is preferably 1.2 to 6.0 times, more preferably 1.5 to 5.5 times, and even more preferably 1.8 to 5.0 times.
[0097] In the present invention, the blow-molded article consisting of the polymer composition (X) only needs to be at least one layer among the components constituting the formed molded article. Specifically, for example, a blow-molded article having at least one layer of the polymer composition (X) can be obtained by injection molding a multilayer preform by co-injecting two or more resin compositions containing the polymer composition (X), followed by blow molding. A generally known apparatus can be used for the above-described molding.
[0098] <Applications of molded products> The molded articles of the present invention, like molded articles obtained from conventional compositions containing 4-methyl-1-pentene polymers, exhibit excellent heat resistance, chemical resistance, gas permeability, and food hygiene properties, and furthermore, they also exhibit excellent transparency. For this reason, the molded articles of the present invention are suitably used in applications where one or more of the following are required: heat resistance, chemical resistance, gas permeability, food hygiene properties, and transparency. For example, the molded articles of the present invention can be used in applications such as laboratory containers (experimental equipment), cell culture vessels, infant beverage containers such as baby bottles and mugs, food refill containers, fragrance containers, cosmetic containers, and gas permeable containers for ornamental plants. [Examples]
[0099] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0100] <Method for measuring the physical properties of polymers> The methods for measuring the physical properties of the polymers used in the following examples and comparative examples are as follows.
[0101] [composition] For each of the polymers used in the examples and comparative examples, the amounts of constituent unit (i) and constituent unit (ii) were determined using the following apparatus and conditions: 13The results were calculated from the 1C-NMR spectrum. Here, constituent unit (i) is a constituent unit derived from 4-methyl-1-pentene, and constituent unit (ii) is a constituent unit derived from ethylene or α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene), which are copolymer monomers with 4-methyl-1-pentene.
[0102] A JEOL Ltd. ECP500 nuclear magnetic resonance spectrometer was used, with a mixed solvent of o-dichlorobenzene / deuterated benzene (80 / 20 vol%) as the solvent, a sample concentration of 55 mg / 0.6 mL, a measurement temperature of 120°C, and the observed nucleus was 13 The measurement was performed using C (125 MHz), a single-pulse proton decoupling sequence, a pulse width of 4.7 μs (45° pulse), a repetition time of 5.5 seconds, and an accumulation count of over 10,000 times, with 27.50 ppm as the reference value for chemical shift. 13 The amounts of constituent units derived from 4-methyl-1-pentene and α-olefins were determined by 13C-NMR spectroscopy.
[0103] [Intrinsic viscosity [η]] The intrinsic viscosity [η] was measured at 135°C using decalin solvent. Specifically, approximately 20 mg of each polymer used in the examples and comparative examples was weighed out, dissolved in 15 mL of decalin, and the specific viscosity [η] was measured in an oil bath at 135°C. sp The specific viscosity η was measured. After diluting this decalin solution by adding 5 mL of decalin solvent, the specific viscosity η was measured in the same manner. sp The following was measured. This dilution procedure was repeated two more times, and when the concentration (C) was extrapolated to 0, the η was measured. sp The value of / C was determined as the intrinsic viscosity (see the formula below). [η] = lim(η) sp / C) (C→0)
[0104] [Melting point (Tm)] For each of the polymers used in the examples and comparative examples, the exothermic and endothermic curves were determined using a DSC measuring device (DSC220C) manufactured by Seiko Instruments Inc., and the temperature at which the maximum melting peak was located during heating was defined as the melting point (Tm). The measurements were performed as follows. Approximately 5 mg of the sample was placed in an aluminum pan for measurement and heated from 20°C to 280°C at a heating rate of 10°C / min. After holding at 280°C for 5 minutes, the temperature was lowered to 20°C at a cooling rate of 10°C / min, held at 20°C for 5 minutes, then heated again from 20°C to 280°C at a heating rate of 10°C / min, and lowered again to 50°C at a cooling rate of 50°C / min. The melting peak that appeared during the second heating was defined as the melting point (Tm). If there were multiple melting peaks, the value of the peak with the higher temperature was used as the melting point (Tm).
[0105] [Manufacturing Examples 1-7] Copolymers of 4-methyl-1-pentene and 1-decene (A-1), (A-2), (B-1), (C-1) to (C-3), and (C-5) were obtained by changing the proportions of 4-methyl-1-pentene, 1-decene, and hydrogen used in accordance with the polymerization method described in Comparative Example 1 (
[0158] ) of International Publication 2017 / 150265, so that the physical properties of the resulting 4-methyl-1-pentene copolymers were as shown in Tables 1 and 2.
[0106] [Manufacturing Example 8] 4-methyl-1-pentene homopolymer (CA-1) was obtained by changing the hydrogen usage ratio so that the properties of the resulting polymer were as shown in Table 1, in accordance with the polymerization method described in Example 3B of International Publication 2014 / 050817.
[0107] [Manufacturing Example 9] A copolymer (C-4) of 4-methyl-1-pentene, 1-hexadecene, 1-octadecene, and 1-octadecene was obtained by changing the proportions of 4-methyl-1-pentene, 1-hexadecene, 1-octadecene, and hydrogen, in accordance with the polymerization method described in Comparative Example 3 (
[0159] ) of International Publication 2017 / 150265, so that the physical properties of the resulting polymer would be as shown in Table 2.
[0108] [Manufacturing Example 10] A copolymer of 4-methyl-1-pentene, 1-hexadecene, 1-octadecene, and hydrogen (CA-2) was obtained by changing the proportions of 4-methyl-1-pentene, 1-hexadecene, 1-octadecene, and hydrogen used in accordance with the polymerization method described in [Synthesis Example 1] of International Publication 2013 / 099876, so that the physical properties of the resulting polymer would be as shown in Table 2.
[0109] [Manufacturing Example 11] A copolymer of 4-methyl-1-pentene and propylene (CB-1) was obtained by changing the proportions of 4-methyl-1-pentene, propylene, and hydrogen used in accordance with the polymerization method described in [Synthesis Example 2-1] of International Publication 2013 / 099876, so that the physical properties of the resulting polymer would be as shown in Table 1.
[0110] [Manufacturing Example 12] A copolymer of 4-methyl-1-pentene and propylene (CC-1) was obtained by changing the proportions of 4-methyl-1-pentene, propylene, and hydrogen used in accordance with the polymerization method described in [Synthesis Example 3] of International Publication 2013 / 099876, so that the physical properties of the resulting polymer would be as shown in Table 2.
[0111] [Table 1]
[0112] [Table 2]
[0113] <Example 1> [Preparation of polymer composition (X1)] 35 parts by mass of copolymer (A-1) obtained in Production Example 1, 45 parts by mass of copolymer (B-1) obtained in Production Example 3, and 20 parts by mass of copolymer (C-1) obtained in Production Example 4 were charged into a twin-screw extruder (PCM43, manufactured by Ikegai Co., Ltd., screw diameter: 43 mm). Then, polymer composition (X1) was obtained by melt-kneading at 280°C and a rotation speed of 200 rpm using the twin-screw extruder.
[0114] [Composition and intrinsic viscosity [η]] The polymer composition (X1) was analyzed using the same method as for determining the composition of individual copolymers blended into the polymer composition (X1), thereby determining the content of constituent unit (i) and constituent unit (ii) in all components of the 4-methyl-1-pentene polymer in the polymer composition (X1) (where the sum of the content of constituent unit (i) and constituent unit (ii) is set to 100 mol%). Furthermore, the intrinsic viscosity [η] of the polymer composition (X1) was determined using the same method as that used for the intrinsic viscosity [η] of the individual copolymers blended into the polymer composition (X1). The results are shown in Table 3.
[0115] [Melt Flow Rate (MFR)] The melt flow rate (MFR) of the polymer composition (X1) was measured according to JIS K7210 Method B, under conditions of 260°C, 340 seconds of preheating, and a 5 kg load. The results are shown in Table 3.
[0116] [Preparation of injection-molded test specimens] The polymer composition (X1) was injected into a 70-ton injection molding machine (M70B) manufactured by Meiki Seisakusho Co., Ltd. under the conditions of cylinder temperature: 280°C and mold temperature: 60°C to produce injection-molded test specimens of four different thicknesses: 0.5 mm, 2 mm, 3 mm, 3.2 mm, and 1 / 4 inch.
[0117] [Enthalpy of Melting (ΔH)] Using a DSC measuring device (DSC220C) manufactured by Seiko Instruments Inc., exothermic and endothermic curves were determined, and the melting peak area during heating was defined as the enthalpy of fusion (ΔH). The measurements were performed as follows. Approximately 5 mg of the sample was cut from a 0.5 mm thick injection-molded specimen, placed in an aluminum pan for measurement, and heated from 20°C to 280°C at a heating rate of 10°C / min. After holding at 280°C for 5 minutes, the temperature was lowered to 20°C at a cooling rate of 10°C / min, held at 20°C for 5 minutes, then heated again from 20°C to 280°C at a heating rate of 10°C / min, and lowered again to 50°C at a cooling rate of 50°C / min. The area of the melting peak that appeared during the second heating was defined as the enthalpy of melting (ΔH). If there were multiple melting peaks, the peak area for each melting peak was calculated. The results are shown in Table 3.
[0118] [Half crystallization time (Tc 1 / 2 )] Using a DSC measuring device (DSC8500) manufactured by PerkinElmer, Inc., the exothermic and endothermic curves were determined, and the semicrystallization time (Tc 1 / 2 The following measurements were taken: Approximately 5 mg of the sample was cut from a 0.5 mm thick injection-molded test piece, placed in an aluminum pan for measurement, and heated from 30°C to 280°C at a heating rate of 500°C / min. After holding at 280°C for 10 minutes, the temperature was lowered to 215°C at a cooling rate of 500°C / min, and the crystallization peak at 215°C was measured. In the measured crystallization peak, the time from the start of crystallization to the point where crystallization is half accelerated (the point when the area of the crystallization peak becomes half of the total crystallization peak area) was defined as the semi-crystallization time (Tc). 1 / 2 ) was used. If no peak appeared in the above test, the semi-crystallization time (Tc 1 / 2 The option ) was omitted. The results obtained are shown in Table 3.
[0119] [Tensile test] Using injection-molded specimens with a thickness of 2 mm, ASTM-4 dumbbell-shaped specimens were prepared in accordance with ASTM D638. Tensile tests were performed on an Instron 3380 universal tensile testing machine under the conditions of a tensile speed of 50 mm / min and a measurement temperature of 23°C, and the tensile modulus, tensile fracture stress, and tensile elongation at fracture were measured. The results are shown in Table 3.
[0120] [Izod impact test] <With notch> Using injection-molded specimens with a 3mm thick notch, Izod impact tests were conducted in accordance with ASTM D 256 using a DG-IB digital impact tester manufactured by Toyo Seiki Seisakusho Co., Ltd., with a hammer capacity of 3.92J, a swing angle of 148.9°, and a test temperature of 23°C. The Izod impact strength with the notch was measured. The results are shown in Table 3.
[0121] <No notch> Using injection-molded specimens with a thickness of 3 mm, Izod impact tests were conducted in accordance with ASTM D 4812 using a DG-IB type digital impact tester manufactured by Toyo Seiki Seisakusho Co., Ltd., with a hammer capacity of 3.92 J, a swing angle of 148.9°, and a test temperature of 23°C. The Izod impact strength without notches was measured. The results are shown in Table 3.
[0122] [flexural elasticity] Using injection-molded specimens with a thickness of 3.2 mm, bending tests were conducted in accordance with ASTM D 790 using a Shimadzu AG-X plus model under the conditions of a test speed of 1.3 mm / min and a measurement temperature of 23°C, and the flexural modulus was measured. The results are shown in Table 3.
[0123] [Heat distortion temperature test] Using injection-molded specimens with a thickness of 1 / 4 inch, a heat distortion temperature (HDT) test was conducted in accordance with ASTM D648 using an HDT measuring device manufactured by Yasuda Seiki Seisakusho Co., Ltd., under the conditions of a heating rate of 50°C per hour and a test load of 0.45 MPa, and the heat distortion temperature (HDT) was measured. The results obtained are shown in Table 3.
[0124] [Measurement of total haze, internal haze, and total light transmittance] Using injection-molded test specimens with a thickness of 2 mm, and in accordance with JIS K 7136, a haze and transmittance meter HM-150 (D65 light source) manufactured by Murakami Color Technology Laboratory Co., Ltd. was used to measure the proportion of transmitted light that deviated by 2.5° or more from the incident light due to forward scattering among the transmitted light passing through the test specimen. Total haze and total light transmittance were then determined. Internal haze was measured similarly in benzyl alcohol. The obtained results are shown in Table 3.
[0125] [Fabrication of blow-molded parts] A blow-molded body was formed using the polymer composition (X1).
[0126] <Molding 1: Stretch blow molding using mold I> (Preparation of Preform A) Using a one-step injection blow molding machine manufactured by Nissei ASB Machinery Co., Ltd., a polymer composition (X1) was processed under the conditions of cylinder temperature: 280°C and mold temperature: 40°C to produce preform A with an outer diameter of 24 mm, a height of 107 mm, and a weight of 18 g.
[0127] (Stretch blow molding of preform A) The aforementioned preform A was adjusted to a surface temperature of 140°C to 200°C and blow-molded using mold I, which produced a 330cc container (longitudinal stretch ratio of 1.7x, transverse stretch ratio of 2.4x, total stretch ratio of 4.1x), and its moldability was evaluated. Air blowing was performed in two stages, with a primary pressure of 0.4 MPa and a secondary pressure of 3.0 MPa. The surface temperature of preform A during blow molding was measured by imaging preform A from a distance of 1 m using a FLIR C5 infrared camera manufactured by FLIR Systems.
[0128] (evaluation) The evaluation was conducted according to the following criteria. The evaluation results are shown in Table 3. [Evaluation Criteria] ○: Stretch blow molding was successful. ×: Stretch blow molding was not possible.
[0129] <Example 2> In Example 2, preform A obtained from the polymer composition (X1) prepared in Example 1 was blow-molded using a different mold (mold II) than that used in Example 1.
[0130] <Molding 2: Stretch blow molding of preform A using mold II> The preform A was adjusted to a surface temperature of 140°C to 200°C and blow-molded using mold II, which was a 280cc container (longitudinal stretch ratio 1.3x, transverse stretch ratio 2.6x, total stretch ratio 3.4x), and its moldability was evaluated. Air blowing was performed in two stages, with a primary pressure of 0.4 MPa and a secondary pressure of 3.0 MPa. The surface temperature of preform A during blow molding was measured in the same manner as in molding 1 of Example 1. The results of blow molding were evaluated using the same criteria as in molding 1. The evaluation results are shown in Table 3.
[0131] <Example 3> In Example 3, a preform B was prepared from the polymer composition (X1) prepared in Example 1 and blow-molded using mold III. Details are as follows.
[0132] <Molding 3: Stretch blow molding using mold III> (Preparation of Preform B) Preform B, with an outer diameter of 18 mm, a height of 76 mm, and a weight of 18 g, was prepared by processing the polymer composition (X1) using the same apparatus and under the same conditions (cylinder temperature: 280°C, mold temperature: 40°C) as in the preparation of preform A.
[0133] (Stretch blow molding of preform B) The obtained preform B was adjusted to a surface temperature of 140°C to 200°C, and blow-molded using mold III, which was a 68cc container (longitudinal stretch ratio 1.1x, transverse stretch ratio 2.1x, total stretch ratio 2.3x), and its moldability was evaluated. Air blowing was performed in two stages, with a primary pressure of 0.4 MPa and a secondary pressure of 3.0 MPa. The surface temperature of preform B during blow molding was measured in the same manner as in molding 1 of Example 1. The results of blow molding were evaluated using the same criteria as in molding 1. The evaluation results are shown in Table 3.
[0134] <Example 4> In Example 4, a preform C was prepared from the polymer composition (X1) prepared in Example 1 and blow-molded using mold IV. Details are as follows.
[0135] <Molding 4: Stretch blow molding using mold IV> (Preparation of Preform C) Preform C, with an outer diameter of 29 mm, a height of 105 mm, and a weight of 30 g, was prepared by processing the polymer composition (X1) using the same apparatus and under the same conditions (cylinder temperature: 280°C, mold temperature: 40°C) as when preform A was prepared.
[0136] (Stretch blow molding of preform C) The obtained preform was adjusted to a surface temperature of 140°C to 200°C, and blow molding was performed using mold IV, which is a 400cc container (longitudinal stretch ratio 1.5x, transverse stretch ratio 2.5x, total stretch ratio 3.8x), and the moldability was evaluated. Air blowing was performed in two stages, with a primary pressure of 0.4 MPa and a secondary pressure of 3.0 MPa. The surface temperature of preform C during blow molding was measured in the same manner as in molding 1 of Example 1. The results of blow molding were evaluated using the same criteria as in molding 1. The evaluation results are shown in Table 3.
[0137] <Examples 5, 6, 10, and 11> Polymer composition (X) was prepared in the same manner as in Example 1, except that the proportions of copolymer (A), copolymer (B), and copolymer (C) were changed as shown in Tables 3 to 5. The physical properties of polymer composition (X), the physical properties of injection-molded polymer composition (X), and blow molding were performed in the same manner as in Example 1. The results obtained are shown in Tables 3 to 5.
[0138] <Example 7> In Example 7, preform A obtained from the polymer composition (X2) prepared in Example 6 was molded using mold II in the same manner as in molding 2. The results are shown in Table 4.
[0139] <Example 8> In Example 8, preform B obtained from the polymer composition (X2) prepared in Example 6 was molded using mold III in the same manner as in molding 3. The results are shown in Table 4.
[0140] <Example 9> In Example 9, the preform C obtained from the polymer composition (X2) prepared in Example 6 was molded using mold IV in the same manner as in molding 4. The results are shown in Table 4.
[0141] <Example 12, Comparative Examples 1 and 4> Polymer composition (X) or the composition used in the comparative example was prepared in the same manner as in Example 1, except that the amounts of copolymer (A), copolymer (B), and copolymer (C) were changed as shown in Table 5. The physical properties of polymer composition (X) or the composition used in the comparative example, as well as the physical properties of injection-molded articles of polymer composition (X) or the composition used in the comparative example, were measured in the same manner as in Example 1. Blow molding was performed in the same manner as molding 4 in Example 4. The results obtained are shown in Table 5.
[0142] <Comparative Example 2> The compositions were prepared in the same manner as in Example 1, except that the amounts of copolymer (A), copolymer (B), and copolymer (C) were changed as shown in Table 5. The physical properties of the obtained compositions and the injection-molded articles of the obtained compositions were measured in the same manner as in Example 1. Blow molding was performed in the same manner as molding 2 of Example 2. The results obtained are shown in Table 5.
[0143] <Comparative Example 3> The composition prepared in Comparative Example 2 was used for blow molding in the same manner as molding 4 in Example 4. The results obtained are shown in Table 5.
[0144] [Table 3]
[0145] [Table 4]
[0146] [Table 5]
[0147] In Examples 1-4, polymer composition (X1) was molded into four different bottle shapes using molds I-IV, and all were successfully stretch-blow molded. For the four bottle shapes, the difficulty of stretch-blow molding increased with increasing total stretch ratio, so the order of difficulty was: mold I shape > mold IV shape > mold II shape > mold III shape. In Examples 6-9, polymer composition (X2) was successfully stretch-blow molded into the four bottle shapes. Therefore, polymer composition (X1) and polymer composition (X2) exhibit excellent blow-molding properties. The polymer composition (X) used in Examples 5, 10, 11, and 12 also exhibits excellent blow-molding properties, as successful stretch-blow molding was achieved using mold I or mold IV, which have relatively high total stretch ratios. Furthermore, in all of Examples 1-12, molded articles with low internal haze and low overall haze, and high transparency, were obtained. On the other hand, Comparative Examples 1 to 3, which used compositions that did not satisfy all of requirements (X-1) to (X-3), exhibited poor blow moldability. Comparative Example 4, which did not satisfy requirement (X-3), showed relatively good moldability, but the transparency of the molded article was low.
Claims
1. The following requirements (X-1) to (X-3) must be met, 15 to 40% by mass of a 4-methyl-1-pentene copolymer (A) that satisfies the following requirements (A-i) and (A-ii), 40 to 80% by mass of a 4-methyl-1-pentene copolymer (B) that satisfies the following requirements (B-i) to (B-iii), 5 to 30% by mass of a 4-methyl-1-pentene copolymer (C) that satisfies the following requirements (C-i) to (C-iii), A polymer composition (X) containing (wherein the total of copolymer (A), copolymer (B), and copolymer (C) is 100% by mass). Requirement (X-1): The endothermic curve measured by DSC in accordance with JIS K7122 using a pellet-shaped composition has two or more melting peaks. Requirement (X-2): The enthalpy of fusion ΔH obtained from the peak area of the melting peak with the highest peak temperature among the melting peaks of the endothermic curve. 1 The value is less than 20.0 J / g. Requirement (X-3): Using a pellet-shaped composition, the semi-crystallization time at 215°C, measured by DSC using the following measurement method, exceeds 800 seconds or is not observed. Measurement method: Using a PerkinElmer DSC8500, the temperature is raised from 30°C to 280°C at a heating rate of 500°C / min, the temperature is maintained for 10 minutes, and then the temperature is cooled down to 215°C at a cooling rate of 500°C / min. The semi-crystallization time at 215°C is then measured. Requirement (A-i): When the sum of constituent units (i) derived from 4-methyl-1-pentene and constituent units (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) is taken as 100 mol%, the content of constituent unit (i) is 97.5 mol% or more and less than 100 mol%, and the content of constituent unit (ii) is greater than 0 mol% and 2.5 mol% or less. Requirement (A-ii): The intrinsic viscosity [η] A measured in decalin at 135°C is 1.0 to 5.0 dl / g. Requirement (B-i): When the sum of constituent units (i) derived from 4-methyl-1-pentene and constituent units (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) is taken as 100 mol%, the content of constituent unit (i) is 91.0 mol% or more and less than 97.5 mol%, and the content of constituent unit (ii) is greater than 2.5 mol% and less than or equal to 9.0 mol%. Requirement (B-ii): The intrinsic viscosity [η] B measured in decalin at 135°C is 2.0 to 5.0 dl / g. Requirement (B-iii): The melting point (Tm) measured by DSC is less than 180°C. Requirement (C-i): Contains constituent unit (i) derived from 4-methyl-1-pentene, and when the sum of constituent unit (i) and constituent unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene) is taken as 100 mol%, the content of constituent unit (i) is less than 91.0 mol%, and the content of constituent unit (ii) is greater than 9.0 mol%. Requirement (C-ii): The intrinsic viscosity [η] C measured in decalin at 135°C is 2.0 to 5.0 dl / g. Requirement (C-iii): The melting point (Tm) is not observed by DSC.
2. The polymer composition (X) according to claim 1, wherein when the sum of the constituent unit (i) derived from 4-methyl-1-pentene, which is included in the entire 4-methyl-1-pentene polymer in the polymer composition (X), and the constituent unit (ii) derived from ethylene and α-olefins having 3 to 20 carbon atoms (excluding 4-methyl-1-pentene), which is included in the entire 4-methyl-1-pentene polymer in the polymer composition (X), is taken as 100 mol%, the content of constituent unit (ii) is 4.0 to 10.0 mol%.
3. A molded article comprising the polymer composition (X) described in claim 1.
4. The molded article according to claim 3, which is a blow-molded article.
5. The molded article according to claim 3, which is a blow-molded article formed by blow-molding a preform formed by injection molding.
6. A molded article according to any one of claims 3 to 5, which is a bottle container.
7. Formed by stretch blow molding, The molded article according to claim 4 or 5, wherein the product of the stretch ratio in the longitudinal direction and the stretch ratio in the transverse direction in the stretch blow molding is 1.2 to 6.0 times.
8. A step (1) of forming a preform from the polymer composition (X) described in claim 1, The process (2) involves stretch blow molding the preform into a blow-molded body, Includes, A method for manufacturing a blow-molded article, wherein the product of the stretch ratio in the longitudinal direction and the stretch ratio in the transverse direction in the stretch blow molding is 1.2 to 6.0 times.
Citation Information
Patent Citations
Catalyst composition containing reversible transfer agent for forming regioregular multi-block copolymers
JP2008533275A
4-methyl-1-pentene copolymer composition
JP2018162408A
Resin composition and molded product
JP2022041965A
Polymer composition and molded article
JP2022132774A
4-methyl-1-pentene (CO)polymer composition, and film and hollow molded body, each of which is formed from 4-methyl-1-pentene (CO)polymer composition