Method for manufacturing precious metal solutions
The method of using oxygen and ozone to leach gold or silver in a cyanide solution prioritizes metal extraction over cyanide decomposition, addressing the environmental challenges of toxic wastewater by enhancing extraction efficiency and simplifying handling and detoxification processes.
Patent Information
- Application Number
- JP2023181620
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-10-23
- Publication Date
- 2026-11-19
- Estimated Expiration
- 2043-10-23
AI Technical Summary
The wastewater generated during the refining and leaching of precious metals, particularly gold and silver, contains high levels of cyanide compounds, posing significant environmental and handling challenges due to its toxicity and requiring complex detoxification processes.
A method involving the use of an oxidizing agent containing oxygen and ozone to leach gold or silver into a cyanide solution, with an excess oxidizing agent to facilitate both metal extraction and cyanide decomposition, utilizing a controlled bubble diameter and stirring mechanism to prioritize metal leaching over cyanide decomposition.
This approach enhances the efficiency of precious metal extraction while minimizing cyanide residue, simplifying the handling and detoxification of waste liquids, thereby reducing environmental impact and operational complexity.
Smart Images

Figure 0007954131000001 
Figure 0007954131000002 
Figure 0007954131000003
Abstract
Description
[Technical Field]
[0001] This invention relates to a method for producing a precious metal solution. [Background technology]
[0002] Conventionally, complexing agents such as cyanide compounds have been used as leaching agents in the refining, leaching, and recovery of precious metals. As shown in Patent Document 1 below, it is common to use oxidizing agents such as oxygen and hydrogen peroxide when leaching precious metal solutions. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Special Publication No. 01-52456 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] The wastewater generated during the refining and leaching processes of precious metals, as described above, has a significant environmental impact and often requires strict detoxification treatment. When the precious metal is gold or silver, the wastewater may contain large amounts of components such as cyanide compounds, which require strict control not only from an environmental perspective but also from the perspective of toxic and hazardous substances. Therefore, since the handling of the wastewater, including storage and transportation, is inherently difficult, there is a need to simplify its handling.
[0005] One aspect of the present invention is to provide a method for producing a precious metal solution that facilitates the handling of waste liquid. [Means for solving the problem]
[0006] One aspect of the present invention provides a method for producing a precious metal solution as described in [1] to [9] below. Each embodiment is as follows: [1] The process comprises supplying an oxidizing agent containing oxygen and ozone and an object containing gold or silver to a liquid containing a cyanide compound which is a complexing agent, thereby leaching the gold into the liquid. A method for producing a precious metal solution, wherein in the step described above, an excess of the oxidizing agent exceeding the amount necessary for the leaching of the gold or silver is supplied to the liquid. [2] The method for producing a gold solution according to [1], wherein the substance is in powder form. [3] The method for producing a precious metal solution according to [1], wherein the object is the gold foil. [4] The method for producing a precious metal solution according to [1], wherein the object is used as the anode in the step, a cathode is provided in the liquid, and a partition wall is provided to separate the anode and the cathode, and electrolysis is carried out. [5] A method for producing a precious metal solution according to any one of [1] to [4], wherein in the step, the ratio of the amount of ozone consumed due to the leaching of gold or silver to the amount of ozone consumed due to the decomposition reaction of the cyanide compound decreases over time. [6] The method for producing a precious metal solution according to any one of [1] to [5], wherein in the step, the average leaching rate of the gold or silver is 20 g / (L·h) or more relative to the total amount of liquid. [7] A method for producing a precious metal solution according to any one of [1] to [6], wherein a stirrer is provided in the container containing the object and the liquid, and the supply unit for the oxidizing agent to the container is located directly below the stirrer. [8] A method for producing a precious metal solution according to any one of [1] to [7], wherein in the step, the ozone is supplied to the liquid as bubbles. [9] The method for producing a noble metal solution according to [8], wherein the diameter of the bubbles supplied to the liquid in the step is greater than 250 μm. [Effects of the Invention]
[0007] According to one aspect of the present invention, it is possible to provide a method for producing a precious metal solution that facilitates the handling of waste liquid. [Brief explanation of the drawing]
[0008] [Figure 1] Figure 1 is a schematic diagram of the precious metal solution manufacturing apparatus according to the embodiment. [Figure 2] Figure 2(a) shows the change in the amount of gold leached over time for Experimental Examples 1 and 2, and Figure 2(b) shows the change in the amount of gold leached over time for Experimental Examples 2 to 4. [Figure 3] Figure 3(a) shows the change in potassium cyanide concentration over time for Experimental Examples 1 and 2, and Figure 3(b) shows the change in potassium cyanide concentration over time for Experimental Examples 2 to 4. [Modes for carrying out the invention]
[0009] Preferred embodiments of the present invention will be described below with reference to the drawings. However, the present invention is not limited to these examples, and is intended to include all modifications within the meaning and scope of the claims, as indicated by the claims. In the following description, the same elements in the drawings are denoted by the same reference numerals, and redundant descriptions are omitted.
[0010] Figure 1 is a schematic diagram of the precious metal solution manufacturing apparatus according to this embodiment. As shown in Figure 1, the manufacturing apparatus 100 is an apparatus for producing a precious metal solution by leaching a precious metal, such as gold or silver, into a liquid (precious metal leaching treatment). In this embodiment, the manufacturing apparatus 100 is an apparatus for producing a gold solution by leaching gold, a type of precious metal, into a liquid (gold leaching treatment) from an object containing gold. Note that the precious metals in this specification are not limited to gold or silver.
[0011] An object containing precious metals is either pure precious metal or a solid containing precious metal. An object containing precious metals may also contain recycled materials. Such recycled materials include, for example, industrial scrap containing precious metal plating, jewelry containing precious metals, and concentrates of factory wastewater containing precious metals. The above recycled materials may also be high-purity precious metals obtained by pre-treating the aforementioned industrial scrap, jewelry, concentrates, etc. Hereinafter, precious metals derived from recycled materials will also be simply referred to as recycled precious metals. For example, when an object containing gold is used as in this embodiment, the object is either pure gold or a solid containing gold, and may also contain recycled materials. Such recycled materials include, for example, industrial scrap containing gold plating, jewelry containing gold, and concentrates of factory wastewater containing gold. Hereinafter, gold derived from recycled materials will also be simply referred to as recycled gold. Similarly, silver derived from recycled materials will also be simply referred to as recycled silver.
[0012] Part or all of the object containing a noble metal dissolves during the production of the noble metal solution. In the present embodiment, part or all of the object containing gold dissolves during the production of the gold solution. The shape of the object containing a noble metal is not particularly limited, and examples thereof include a plate shape (foil shape), a rod shape, and a powder shape. Alternatively, the object containing a noble metal may be a laminate including a noble metal film and a base material. In the present embodiment, from the viewpoint of the leaching rate of the noble metal and the like, the object containing a noble metal is in a powder form, a granular form, or the like. The powder form follows the so-called definition of powder, but is not limited to this definition. The powdery object may be, for example, an aggregate of solids having an average particle diameter in the range of 0.1 μm or more and 100 μm or less. From the viewpoint of dispersibility, the average particle diameter may be 0.1 μm or more and 10 μm or less. The granular object is, for example, an object having an average particle diameter of 300 μm or more and 2000 μm or less. The object containing a noble metal may be in a state where a powder form and other forms are mixed. For example, the object containing a noble metal may include both a powdery noble metal and a foil-shaped noble metal. The noble metal solution is an aqueous noble metal solution that serves as a raw material for a noble metal plating solution and the like. When the noble metal solution is a gold solution, the gold solution contains, for example, an anionic gold complex. For example, by purifying the gold solution taken out from the production apparatus 100 in a subsequent step, a gold solution from which impurities have been removed, a gold-containing compound, and the like can be obtained. Each of the gold solution and the silver solution obtained according to one embodiment of the present invention can have a low impurity concentration derived from a complexing agent. Therefore, purification in the subsequent step for each of the gold solution and the silver solution can be simplified.
[0013] The production apparatus 100 may be a batch type apparatus or a continuous type apparatus. In the present embodiment, the production apparatus 100 includes a reaction tank 1, a constant temperature tank 2, a temperature control unit 3, an oxygen supply unit 4, an ozone generator 5, a bubble generation device 6, an ozone concentration meter 7, and an ozone treatment tower 8.
[0014] Reaction tank 1 is a member for leaching a noble metal from a noble metal-containing object into a liquid. For example, the noble metal is leached from the object into the liquid by supplying the noble metal-containing object, a complexing agent, and an oxidizing agent to the liquid accommodated in reaction tank 1. The complexing agent is an agent for complexing the noble metal, and is, for example, a cyanide compound. The cyanide compound is potassium cyanide, calcium cyanide, sodium cyanide, or the like. The oxidizing agent is for oxidizing the noble metal, and is, for example, oxygen, aqueous hydrogen peroxide, ozone, or the like. From the viewpoint of carrying out both the oxidation performance, and the excess cyanide decomposition treatment and the noble metal leaching treatment into the liquid, which will be described later, at least ozone may be contained in the oxidizing agent in reaction tank 1. In the present embodiment, the oxidizing agent is a gas containing oxygen and ozone.
[0015] An excess oxidizing agent (in particular, at least excess ozone) exceeding the amount required for leaching the noble metal is supplied into reaction tank 1. Thereby, both the treatment of leaching the noble metal into the liquid and the cyanide decomposition treatment described later can be efficiently completed. The excess oxidizing agent exceeding the amount required for leaching the noble metal is, for example, 5 times or more and 1000 times or less the molar equivalent of the oxidizing agent used for leaching the noble metal, but is not limited thereto. The excess oxidizing agent may be 10 times or more of the above molar equivalent, 20 times or more, 500 times or less, or 100 times or less. Alternatively, even after the noble metal leaching treatment is completed or nearly completed, the supply of the oxidizing agent is maintained for, for example, at least 10 minutes or more, 30 minutes or more, or 60 minutes or more, so that an excess oxidizing agent exceeding the amount required for leaching the noble metal is supplied into reaction tank 1. Here, the completion timing of the noble metal leaching treatment may be the time point at which the increase in the concentration of the noble metal in the liquid or the weight reduction of the noble metal-containing object is within 1.0% per 30 minutes. In addition, the timing at which the leaching treatment is nearly completed may be the time point at which the concentration increase or the weight reduction is within 3.0% per 30 minutes.
[0016] When the precious metal is gold, a cyanide compound is used as the complexing agent, and ozone is used as the oxidizing agent, the leaching of gold into the liquid (i.e., the formation of a gold complex) is carried out by a chemical reaction according to the following chemical formula 1. This chemical reaction is a three-phase gold complexing reaction carried out in a mixed phase of solid (i.e., gold), liquid (i.e., water in which the complexing agent is dissolved), and gas (i.e., ozone). If oxygen is supplied to the reaction vessel 1 in addition to ozone, or if some of the ozone in the reaction vessel 1 is converted into oxygen, the chemical reaction shown in the following chemical formula 2 may also occur. Note that when the precious metal is silver, the chemical reaction in the following chemical formulas 1 and 2 may occur by substituting "Au" with "Ag". Chemical formula 1:2Au+4CN - +O3+H2O→2[Au(CN)2] - +O2+2OH - Chemical formula 2:4Au+8CN - +O2+2H2O→4[Au(CN)2] - +4OH -
[0017] Although not all are shown in the diagram, the reaction vessel 1 includes, for example, a main container for holding liquids, complexing agents, and objects containing precious metals; a material supply unit for supplying liquids, complexing agents, and objects containing precious metals into the main container; a stirrer for stirring the liquids in the main container; an oxidizing agent supply unit for supplying ozone into the main container; a liquid recovery unit for feeding back the liquid in the main container to the foam generator 6; a gas recovery unit for recovering gases discharged outside the main container; and a discharge unit for discharging the precious metal solution from the main container. The reaction vessel 1 may also have a power supply, electrodes, etc. for performing electrolysis.
[0018] The material supply unit has, for example, a first part that supplies a liquid in which a complexing agent is pre-dissolved and which is connected to the foam generator 6, and a second part that supplies an object containing a precious metal. The agitator has at least an agitator that agitates the liquid in the main container. As the agitator, for example, a propeller type, paddle type, or rotor type may be used, or a turbine type such as a pitched turbine type or a disc turbine type may be used. From the viewpoint of agitating not only the liquid but also an object containing a precious metal, a bladeless agitator that can easily obtain a choke-up effect of the object may be used. From the viewpoint of the dispersibility of the oxidizing agent in the liquid, the oxidizing agent supply unit may be located directly below the agitator. The oxidizing agent supply unit may be located directly below the agitator of the agitator. In this embodiment, when the oxidizing agent supply unit can overlap at least a part of the agitator in a plan view, the oxidizing agent supply unit is interpreted as being located directly below the agitator. The liquid recovery unit has a part that supplies the liquid in the main container to the foam generator 6. The liquid recovered by the liquid recovery unit is returned to the reaction tank 1 via the material supply unit (circulated). Therefore, the liquid supplied from the material supply unit to the reaction tank 1 may contain dissolved precious metals. The liquid recovery unit may be equipped with a filter or the like to prevent the recovery of solids such as objects containing precious metals. The gas recovery unit has, for example, a part that supplies the recovered gas to the ozone treatment tower 8. The discharge unit may discharge only the precious metal solution, or it may discharge the precious metal solution in addition to substances that do not dissolve in the precious metal solution. If the manufacturing apparatus 100 is a continuous type, the discharge unit may have a part that discharges the supernatant liquid of the precious metal solution.
[0019] The liquid containing cyanide is a poisonous and deleterious substance. For this reason, when cyanide remains in the precious metal solution, it is necessary to perform detoxification treatment on the waste liquid (cyanide liquid) obtained by recovering the precious metal from the precious metal solution. As a method for detoxifying cyanide liquid, decomposition of cyanide using ozone can be mentioned. In the present embodiment, in the reaction tank 1, both the leaching treatment of the precious metal into the liquid and the decomposition treatment such as reduction treatment or detoxification treatment of excess cyanide are performed. The treatment method of cyanide liquid (liquid phase) using ozone (gas phase) is performed, for example, by chemical reactions according to the following chemical formulae 3 and 4. For example, when the concentration of cyanide ions in the reaction tank 1 becomes 0.2 mol / L or less, 0.15 mol / L or less, or 0.1 mol / L or less, it can be determined that the decomposition treatment of excess cyanide is completed. From the viewpoint of preventing precipitation of the precious metal, the above decomposition treatment may be performed such that the cyanide ions in the reaction tank 1 become 0.10 times, 0.075 times, or 0.05 times the molar equivalent required for leaching of the precious metal. Ozone supply, stirring, and the like may be set so that the chemical reaction represented by the above chemical formula 1 takes precedence over the chemical reactions represented by the following chemical formulae 3 and 4. Chemical formula 3: CN - +O3→OCN - +O2 Chemical formula 4: 2OCN - +3O3+2H + →2CO2+N2+H2O+3O2
[0020] The constant temperature bath 2 is a member that maintains the temperature of the liquid in the reaction tank 1 within a predetermined range. The temperature control unit 3 is a member (a heater, a chilling unit, etc.) that adjusts the temperature of the liquid (for example, water) contained in the constant temperature bath 2. In one example, the temperature of the liquid in the reaction tank 1 is maintained at 30°C or higher or 40°C or higher and 70°C or lower or 60°C or lower by the constant temperature bath 2 and the temperature control unit 3. Although the manufacturing apparatus 100 includes the constant temperature bath 2 and the temperature control unit 3, the present invention is not limited to this. An apparatus that maintains the temperature of the liquid in the reaction tank 1 within a predetermined range may be included in the manufacturing apparatus 100 instead of the constant temperature bath 2 and the temperature control unit 3.
[0021] The oxygen supply unit 4 is a component that supplies oxygen to the ozone generator 5, and is, for example, an oxygen cylinder. A flow meter FM is installed in the path (for example, a pipe) connecting the oxygen supply unit 4 and the ozone generator 5 to measure the flow rate of oxygen supplied from the oxygen supply unit 4 to the ozone generator 5. The presence of the flow meter FM makes it possible to efficiently replace the oxygen supply unit 4, etc.
[0022] The ozone generator 5 is a device that converts oxygen supplied from the oxygen supply unit 4 into ozone. The ozone generated by the ozone generator 5 is supplied to the foam generator 6. In this embodiment, the ozone is supplied not only to the foam generator 6 but also to the ozone concentration meter 7. This makes it easy to check the ozone concentration generated by the ozone generator 5.
[0023] The bubble generator 6 is a device that supplies ozone supplied from the ozone generator 5 as bubbles into the liquid recovered from the liquid recovery unit. The liquid discharged from the bubble generator 6 is supplied to the reaction tank 1 via the first part of the material supply unit. Therefore, the liquid supplied to the reaction tank 1 via the first part contains foamy ozone (bubble ozone). Thus, in this embodiment, at least a portion of the ozone exists in the liquid (i.e., water) in the reaction tank 1 as bubbles. The bubbles contain at least one of ozone and oxygen. That is, bubbles 1 may contain both ozone and oxygen. The bubbles may also be called, for example, microbubbles, nanobubbles, etc. The diameter of the bubbles supplied from the bubble generator 6 into the reaction vessel 1 corresponds, for example, to the diameter of the bubbles when ozone-containing gas is supplied into the liquid from the ozone generator 5, and is between 0.1 μm and 3000 μm, between 1.0 μm and 1000 μm, or between 10 μm and 250 μm. In this embodiment, from the viewpoint of prioritizing the chemical reaction shown in chemical formula 1 over the chemical reactions shown in chemical formulas 3 and 4, the diameter may be greater than 50 μm, greater than 100 μm, or greater than 250 μm. From this viewpoint, bubbles with a diameter of 500 μm or more may be supplied into the reaction vessel 1, or bubbles with a diameter of 1000 μm or more may be supplied into the reaction vessel 1. On the other hand, if the object containing the precious metal is in the form of a plate, the diameter may be 100 μm or less. The control of the diameter can be done by conventionally known methods. For example, the diameter of the bubbles can be controlled by providing a foaming filter in the bubble introduction section. The diameter may vary depending on the pore size, material, wettability with liquid, and other characteristics of the foaming filter.
[0024] As mentioned above, in order to prioritize the leaching of precious metals (three-phase chemical reaction) over the decomposition of cyanide (two-phase chemical reaction) in reaction vessel 1, it is necessary to increase the opportunities for contact between bubbles in reaction vessel 1 and objects containing precious metals. Specific examples include appropriately selecting the diameter of the bubbles, the introduction position of the bubbles, and the shape of the objects containing precious metals. The smaller the diameter of the bubbles, the greater the opportunity for contact between the bubbles supplied to reaction vessel 1 and objects containing precious metals, while simultaneously allowing them to easily dissolve into the liquid phase immediately after introduction, thus promoting cyanide decomposition. On the other hand, the larger the diameter of the bubbles, the lower the diffusivity of the bubbles in reaction vessel 1, and the slower the rate of gold leaching. For this reason, the diameter of the bubbles in reaction vessel 1 may be adjusted by, for example, introducing large bubbles into reaction vessel 1 and then disintegrating those large bubbles within the reaction vessel 1. For example, bubbles can be disintegrated by a stirrer or objects containing precious metals within reaction vessel 1. In one example, bubbles with a diameter of 100 μm to 300 μm are introduced into reaction vessel 1, and these bubbles are broken down to a diameter of less than 100 μm within reaction vessel 1. By adjusting the diameter of the bubbles in this way, the decomposition of cyanide is made less likely to proceed, and the efficiency of utilizing the complexing agent for the leaching of precious metals can be improved.
[0025] Whether the cyanide decomposition treatment or the precious metal leaching treatment takes priority may be influenced, for example, by the form of the object containing the precious metal. For this reason, the form of the object containing the precious metal may be determined in addition to the diameter of the bubbles. Furthermore, from the viewpoint of prioritizing the precious metal leaching treatment while also ensuring the reaction rate of said leaching treatment, the specific surface area of at least one of the object containing the precious metal and the bubbles may be increased. For example, if the diameter of the bubbles is large (for example, if the diameter of the bubbles is 250 μm or more and 3000 μm or less), the object containing the precious metal may have a fine shape such as powder. On the other hand, if the diameter of the ozone is small (for example, if the diameter of the bubbles is 0.1 μm or more and less than 250 μm), the object containing the precious metal may have a coarse shape such as foil or plate. Not limited to the above, as long as the gold leaching treatment takes priority, the diameter of the bubbles may be reduced and the object containing the precious metal may have a fine shape in order to increase the opportunity for contact between the bubbles and the object containing the precious metal. The progress of the precious metal leaching treatment and the cyanide decomposition treatment can be calculated based on the weight change of the object containing the precious metal, the concentration of the complex in reaction vessel 1, and the concentration of the cyanide compound. For example, if the leaching rate of the precious metal in reaction vessel 1 is 20 g / (L·h) relative to the total liquid volume, it can be said that there are many opportunities for contact between the bubbles and the precious metal, and that the leaching treatment of the precious metal is prioritized. If the above leaching rate is 24 g / (L·h) or more, or 26 g / (L·h) or more, relative to the total liquid volume, it can be said that the leaching treatment of gold is well prioritized.
[0026] The ozone concentration meter 7 is a device that measures the concentration of ozone generated by the ozone generator 5 and the concentration of ozone in the gas discharged from the reaction vessel 1. Adjustments to the ozone generator 5 are made according to the measurement results of the ozone concentration meter 7. The ozone treatment tower 8 is a device that treats the ozone discharged from the ozone concentration meter 7.
[0027] Next, an example of a method for producing a gold solution using the manufacturing apparatus 100 according to this embodiment will be described. In this example of a manufacturing method, a batch method is employed.
[0028] First, a liquid is supplied into reaction vessel 1. At this time, the liquid supplied into reaction vessel 1 is water in which the complexing agent is pre-dissolved, but is not limited to this. Oxygen is also supplied from the oxygen supply unit 4 to the ozone generator 5, generating ozone. This ozone and the liquid recovered from reaction vessel 1 are supplied to the bubble generator 6, and bubbles (oxidizing agent) containing the ozone are supplied to the liquid. Then, the liquid containing the bubbles is supplied into reaction vessel 1. In addition, an object containing gold is supplied into reaction vessel 1. As a result, the complexing agent, the oxidizing agent containing ozone, and the object containing gold are supplied to the liquid, and the leaching of gold into the liquid (for example, a chemical reaction according to the chemical formula 1 above) is carried out. This produces a gold solution in reaction vessel 1. At this point, an excess amount of oxidizing agent (especially ozone) exceeding the amount necessary for gold leaching is supplied into reaction vessel 1. For example, ozone is supplied into reaction vessel 1 for about 15 minutes to 120 minutes relative to the scheduled completion time of the gold leaching process. This completes the leaching of gold. The same applies to other precious metals (e.g., silver), but the ratio of ozone consumption associated with gold leaching to ozone consumption associated with cyanide compound decomposition decreases over time. In addition, after the production of the gold solution, a decomposition treatment of excess cyanide (e.g., a chemical reaction according to chemical formulas 3 and 4 above) is also carried out. Therefore, in addition to the production of the gold solution, the decomposition treatment of excess cyanide can also be carried out within reaction vessel 1. Furthermore, the decomposition treatment of excess cyanide may be carried out outside reaction vessel 1. For example, if gold is always present in reaction vessel 1, or if the supply of gold-containing material and the discharge of the produced gold solution are carried out continuously, the gold solution, which is the supernatant liquid discharged from reaction vessel 1, can be subjected to the above decomposition treatment outside reaction vessel 1.
[0029] After the gold solution is produced, the gold solution is recovered from reaction vessel 1. If any residue remains in reaction vessel 1, it is discharged separately from the gold solution. After these steps, the gold solution is discharged. If the complexing agent is not dissolved in the liquid, the complexing agent is supplied to reaction vessel 1 in addition to the above-mentioned substance.
[0030] Furthermore, gold may be recovered again as a solid from the recovered gold solution. In one example, a gold cyanide compound is produced by a known method of purification. For example, the gold cyanide compound is crystallized from the recovered gold solution. The waste liquid generated during purification and other processes is treated by an appropriate method. Since the excess cyanide in the gold solution has been reduced beforehand, the treatment of the waste liquid can also be made more efficient.
[0031] Next, the effects and benefits of the method for producing the precious metal solution according to this embodiment, as described above, will be explained.
[0032] In the method for producing a precious metal solution using the manufacturing apparatus 100 according to this embodiment, gold is leached into the liquid by supplying an oxidizing agent containing oxygen and ozone, and a gold-containing object, to a liquid containing a cyanide compound, which is a complexing agent, into the reaction vessel 1. Because the oxidizing agent contains ozone, its oxidizing power is strong, which promotes the leaching of gold into the liquid. In addition, since ozone is easily decomposed, the environmental burden of the oxidizing agent can be reduced. As shown in the chemical formulas 3 and 4 above, when ozone and cyanide coexist, cyanide is decomposed by ozone. However, the inventors have found that when a cyanide compound, ozone, and a gold-containing object coexist in a liquid, the leaching of gold into the liquid tends to take precedence over the decomposition of cyanide by ozone. According to this embodiment, the reduction of the complexing agent due to the side reaction between the complexing agent and the oxidizing agent can be suppressed. Therefore, according to this embodiment, the utilization efficiency of the cyanide compound is less likely to decrease, and the increase in the total amount of cyanide compound used can be suppressed. In addition, an excess amount of oxidizing agent exceeding the amount necessary for gold leaching is supplied to the reaction vessel 1. This allows for the decomposition of excess cyanide within reaction vessel 1 after the gold leaching treatment is complete. Therefore, the handling of waste liquids generated during further processing of the precious metal solution, such as storage and transportation, can be facilitated.
[0033] In this embodiment, the gold-containing object may be in powder form. In this case, the gold contained in the object is more readily chemically reactive with the complexing agent and the oxidizing agent, thereby improving the gold leaching efficiency.
[0034] In this embodiment, an oxidizing agent containing ozone is supplied to the liquid as bubbles controlled to a predetermined diameter. This allows for control over the balance of ozone consumption between the gold leaching process and the cyanide decomposition process.
[0035] In this embodiment, the average leaching rate of gold may be 20 g / (L·h) or more relative to the total volume of liquid. In this case, the gold leaching reaction is prioritized, allowing for efficient utilization of the cyanide compound.
[0036] In this embodiment, the main container containing the gold-containing object and the liquid is equipped with a stirrer, and the supply unit for the oxidizing agent to the main container may be located directly below the stirrer. In this case, the oxidizing agent supplied as bubbles is more easily broken down by the stirrer. In addition, the gold-containing object is dispersed in the liquid by the stirrer, making it easier for the oxidizing agent (especially ozone) to come into contact with the gold. This improves the efficiency of gold leaching in the reaction vessel 1.
[0037] In this embodiment, the diameter of the bubbles supplied to the liquid may be larger than 250 μm. In this case, the bubbles do not easily dissolve into the liquid phase immediately after being introduced into the liquid, making it less likely for the cyanide decomposition reaction to occur.
[0038] In this embodiment, the diameter of the bubbles supplied to the liquid may be 250 μm or less. In this case, the leaching rate of gold can be improved.
[0039] The above embodiments illustrate one aspect of the present invention. Therefore, the present invention can be modified as appropriate without being limited to the above embodiments. For example, in the above embodiments, the precious metal solution is produced using the manufacturing apparatus shown in Figure 1, but it is not limited thereto.
[0040] In the above embodiment, the object containing the precious metal is in powder form, but is not limited to this. The object containing the precious metal may also be a foil containing the precious metal, a plate containing the precious metal, a laminate containing a precious metal film and a substrate, etc.
[0041] In the above embodiment, the precious metal is leached from the liquid by a catalytic chemical reaction between the complexing agent, the oxidizing agent, and the precious metal, but the embodiment is not limited to this. For example, an object containing the precious metal may be used as the anode, a cathode may be placed in the liquid, and a partition separating the anode and the cathode may be placed inside, and electrolysis may be carried out. In this case, an insoluble electrode may be used as the cathode, and an ion exchange membrane may be used as the partition, which is a component that prevents the redeposition of the precious metal to the cathode. The shape of the anode may be, for example, a plate or a rod.
[0042] In the above embodiment, the manufacturing apparatus includes a foam generator, but is not limited thereto. For example, the manufacturing apparatus may supply a gas containing ozone generated by an ozone generator to a reaction vessel. In this case, a foaming filter or the like may be provided at the supply port of the reaction vessel where the gas is supplied. Furthermore, the manufacturing apparatus includes an ozone concentration meter and an ozone treatment tower, but is not limited thereto. The ozone concentration meter and ozone treatment tower may be included in an oxidizing agent device or the like, located downstream of the manufacturing apparatus. [Examples]
[0043] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0044] (Experimental Example 1) A titanium beaker (Ti beaker) was filled with 3 liters of water, potassium cyanide (manufactured by Nippon Soda Co., Ltd., 453 g), and gold (manufactured by Asahi Pritec Co., Ltd., powdered recycled gold, particle size: 2-10 μm, purity: 95% or higher, 600 g). The gold was pre-processed into powder form before being placed in the Ti beaker. In the Ti beaker, the amount of potassium cyanide was 1.14 relative to the molar equivalent of gold. Subsequently, a silent discharge ozone generator (manufactured by Ebara Corporation, OZSD-3000D) was used to supply a gas containing oxygen and ozone into the Ti beaker at a rate of 0.2 L / min (ozone concentration: 0.6 g / hr). During this time, the liquid temperature in the Ti beaker was maintained at 49°C using a constant temperature bath. The gas supplied into the Ti beaker formed bubbles, and the diameter of these bubbles was 500 μm. Then, while supplying the aforementioned bubbles into the Ti beaker, the contents of the Ti beaker were stirred for 7 hours using a stirrer (IKA Japan KK, propeller-type mechanically controlled stirrer) set to 840 rpm. At this point, 800 ml of water was added to the Ti beaker 4 hours after stirring but within 7 hours. The gold concentration of the gold solution produced was 171 g / L, the KCN concentration was 6.1 g / L, and the remaining gold was 3.7 g. From this, it was determined that 87.0 mass% of the total potassium cyanide was consumed for gold leaching. Of the remaining portion (13.0 mass%), 8.3 mass% was decomposed by ozone, etc., and 4.7 mass% remained in the solution. The average gold leaching rate was 28 g / (L·hr) relative to the amount of liquid used (total liquid volume).
[0045] (Experimental Example 2) The gold solution was prepared using the same method as in Experimental Example 1, except that a polypropylene jug was used instead of a Ti beaker, the liquid temperature in the jug was maintained at 50°C, and 800 ml of water was added to the jug after stirring. The gold concentration of the gold solution was 164 g / L, the KCN concentration was 7.8 g / L, and the remaining gold amounted to 13.2 g. From the above, 85.6 mass% of the total potassium cyanide was consumed for gold leaching. Of the remaining amount (14.4 mass%), 8.4 mass% was decomposed by ozone, etc., and 6.0 mass% remained in the solution. The average gold leaching rate was 28 g / (L·hr) relative to the amount of liquid used (total liquid volume).
[0046] (Experimental Example 3) The gold solution was prepared using the same method as in Experimental Example 1, except that a polypropylene jug was used instead of a Ti beaker, the liquid temperature in the jug was maintained at 52°C, 800 ml of water was supplied to the jug after stirring, and gas was supplied to the jug at a rate of 0.3 g / hr. The gold concentration of the gold solution was 173 g / L, the KCN concentration was 5.2 g / L, and the remaining gold was 2.3 g. From the above, 87.2 mass% of the total potassium cyanide was consumed for gold leaching. Of the remaining portion (12.8 mass%), 8.8 mass% was decomposed by ozone, etc., and 4.0 mass% remained in the solution. The average gold leaching rate was 28 g / (L·hr) relative to the amount of liquid used (total liquid volume).
[0047] (Experimental Example 4) The gold solution was prepared using the same method as in Experimental Example 1, except that a polypropylene jug was used instead of a Ti beaker, the liquid temperature in the jug was maintained at 50°C, a commercially available disk turbine was used as a stirrer with a rotation speed of 851 rpm, and no water was supplied after stirring began. In Experimental Example 4, the bubbles were well dissipated and made into fine particles (at introduction: 500 μm in diameter, after dissipation: less than 10 μm in diameter). On the other hand, the gold remained at the bottom of the jug and was not sufficiently stirred. As a result, gold leaching hardly progressed, and only a certain amount of cyanide decomposition was observed. For this reason, in Experimental Example 4, the production of the gold solution was stopped 2 hours after stirring began.
[0048] Figure 2(a) shows the changes in the amount of gold leached over time for Experimental Examples 1 and 2. Figure 2(b) shows the changes in the amount of gold leached over time for Experimental Examples 2 to 4. In both Figures 2(a) and (b), the horizontal axis represents the stirring time and the vertical axis represents the amount of gold leached. In Figure 2(a), graph 11 shows the changes for Experimental Example 1, and graph 12 shows the changes for Experimental Example 2. In Figure 2(b), graph 13 shows the changes for Experimental Example 3, and graph 14 shows the changes for Experimental Example 4.
[0049] Figure 3(a) shows the change in potassium cyanide concentration over time for Experimental Examples 1 and 2. Figure 3(b) shows the change in potassium cyanide concentration over time for Experimental Examples 2 to 4. In both Figures 3(a) and (b), the horizontal axis represents stirring time, and the vertical axis represents potassium cyanide concentration. In Figure 3(a), graph 21 shows the change for Experimental Example 1, and graph 22 shows the change for Experimental Example 2. In Figure 3(b), graph 23 shows the change for Experimental Example 3, and graph 24 shows the change for Experimental Example 4.
[0050] As shown in Figures 2(a) and (b), in Experimental Examples 1-3, gold leaching was almost complete after approximately 6 hours of stirring. On the other hand, in Experimental Example 4, almost no gold leaching occurred. This is presumed to be mainly due to the gold not being stirred while in liquid. Furthermore, as shown in Experimental Example 3, no difference was observed in the average gold leaching rate or the amount of gold leached when the gas supply amount was 0.3 g / L or higher. In addition, as shown in Figures 3(a) and (b), in Experimental Examples 1-4, the concentration of potassium cyanide decreased even after gold leaching was almost complete. From the above, it is presumed that when gold is present in a liquid, gold leaching takes precedence over cyanide decomposition. Furthermore, cyanide decomposition occurs by continuing to supply gas (ozone) after gold leaching is complete.
[0051] (Experimental Example 5) A polypropylene jug was filled with 3 liters of water, 405 g of potassium cyanide (manufactured by Nippon Soda Co., Ltd.), 600 g of powdered gold (manufactured by Asahi Pritec Co., Ltd., recycled powdered gold, particle size: 2-10 μm, purity: 95% or higher), and 1.3 liters of water. Next, a silent discharge ozone generator (manufactured by Ebara Corporation, OZSD-3000D) was used to supply a gas containing oxygen and ozone into the jug at a rate of 0.2 L / min (ozone concentration: 0.3 g / hr). During this time, the liquid temperature inside the jug was maintained at 51°C using a constant temperature bath. A PTFE filter with a diameter of φ10 μm was placed at the gas supply port of the jug. Then, while supplying ozone into the jug, the contents of the jug were stirred for 7 hours using a stirrer (manufactured by IKA Japan KK, propeller-type mechanically controlled stirrer) set to 844 rpm. After stirring the liquid, 800 ml of water was added to the jug. The gold concentration of the resulting gold solution was 63 g / L, and 219.5 g of gold remained. This indicates that 35.8% by mass of the total potassium cyanide was consumed for gold leaching. Of the remaining portion (64.2% by mass), 9.5% by mass was decomposed by ozone, etc., leaving 54.7% by mass in the solution. The consumption rate of potassium cyanide was 40%, and the average gold leaching rate was 12 g / (L·hr). In Experiment 5, the diameter of the bubbles supplied to the jug exceeded 3000 μm. In Experiment 5, although some disintegration occurred after the bubbles were introduced, it is presumed that the gold leaching rate was slow and cyanide decomposition occurred preferentially due to insufficient contact between the bubbles and the gold.
[0052] (The effect of the presence or absence of ozone on oxidizing agents) In a 500ml Ti beaker, 300ml of water was mixed with potassium cyanide (manufactured by Nippon Soda Co., Ltd., 30g) and gold (manufactured by Asahi Pritec Co., Ltd., powdered recycled gold, particle size: 2-10μm, purity: 95% or higher, 78g). Subsequently, a silent discharge ozone generator (manufactured by Ebara Corporation, OZSD-3000D) was used to supply a mixed gas consisting of oxygen and ozone, acting as an oxidizing agent, into the beaker at a flow rate of 0.2L / min and an ozone introduction rate of 0.6g / h. At this time, the diameter of the bubbles formed when the gas was introduced into the liquid was between 1000μm and 1500μm. The liquid in the beaker was also stirred using a hot stirrer (manufactured by IKA Japan KK, "C-MAG HS7") while maintaining the liquid temperature at 42-45°C. Gold leaching was ongoing, and the average gold leaching rate after 4 hours was 29.6 g / (L·h). On the other hand, under the same conditions as above, except that ozone was not included as an oxidizing agent and oxygen gas was supplied to the beaker at a flow rate of 0.2 ml / min, the average gold leaching rate was 9.7 g / (L·h) relative to the amount of liquid used (total liquid volume).
[0053] (Gold leaching ability for each oxidizing agent) Here, in order to minimize fluctuations in elution conditions due to changes in the surface area of the gold, a 15cm x 10cm gold plate was prepared as the elution sample. Next, this sample was immersed in a sodium cyanide solution (10L, pH: 11, sodium cyanide added: 7.6g / L) adjusted to a temperature between 27°C and 37°C. At this time, the immersion surface of the gold plate was 10cm x 10cm (exposed area: 200cm²). 2The gold plate was masked with tape to achieve the desired result. Then, a mixed gas, oxygen gas, air, or hydrogen peroxide solution was supplied to the sodium cyanide solution as an oxidizing agent. The mixed gas was obtained by supplying oxygen gas (flow rate: 1.0 L / min) to an ozone generator. When the oxidizing agent was a mixed gas, oxygen gas, or air (oxygen concentration: 21%), the oxidizing agent was converted into microbubbles by a microbubble generator (Kansai Autome Kiki Co., Ltd., MBLL-102-S) and supplied to the sodium cyanide solution in a circulating manner for 4 hours. When the oxidizing agent was a mixed gas, the ozone input concentration was 108 g / m³. 3 The liquid flow rate was 11 L / min. When the oxidizing agent is oxygen gas or air, the oxidizing agent input concentration is 1.0 L / min and the liquid flow rate is 11 L / min. When the oxidizing agent is hydrogen peroxide, the oxidizing agent concentration is adjusted to 40 mmol / L, and the oxidizing agent is initially supplied to the sodium cyanide solution all at once. The concentration of hydrogen peroxide is 80 g / m³ based on the ozone concentration. 3 It corresponds to this.
[0054] The gold leaching rate was evaluated by the decrease in sample thickness. When the oxidizing agent was a mixed gas, the gold leaching rate was 5.1 μm / h. When the oxidizing agent was oxygen gas, the gold leaching rate was 0.8 μm / h. When the oxidizing agent was air, the gold leaching rate was 0.9 μm / h. When the oxidizing agent was hydrogen peroxide, the gold leaching rate was 1.6 μm / h. From the above, it can be said that when a mixed gas containing ozone is used as the oxidizing agent, the gold leaching rate is higher compared to when oxygen gas, air, or hydrogen peroxide is used as the oxidizing agent. Therefore, when a mixed gas is used as the oxidizing agent, productivity can be improved even if cyanide decomposition treatment is performed in addition to gold leaching.
[0055] (Influence of the shape of the gold) The elution behavior of gold samples A to D, shown below, was compared through the experiment described below. In this comparison, in order to compare the elution rates, the reaction was observed until the concentration of gold in the solution reached a predetermined level, rather than at the point when the elution of gold was complete. Gold samples A to D were all made from the same raw material. Gold sample A…Shape: Granular, Particle size: 500μm~2000μm, 10g Gold sample B…Form: powder, particle size: 2μm~10μm, 10g Gold Sample C…Shape: Foil-like (laminated material of gold foil and SUS plate), Total thickness: 0.3mm, 15cm x 10cm, 20 pieces Gold sample D…Shape: Plate-like, 15cm x 10cm, Immersion surface: 10cm x 10cm (exposed area: 200cm²) 2 ), thickness: 0.72mm
[0056] [Experimental conditions] A stirring bar and a glass diffuser were placed in a 1L beaker and placed on a hot stirrer. The diffuser was connected to an ozone introduction tube from the top of the beaker and held at a height sufficient to allow ozone bubbles to reach the bottom of the beaker. Next, 0.8L of water, 7.6g / L of sodium cyanide, and one of the gold samples A to D were added to the beaker. Gold samples A and B were placed entirely into the beaker. Gold samples C and D were suspended and immersed in the liquid. Ozone-containing bubbles (diameter: approximately 1000 μm) were introduced into the beaker at an ozone input concentration of 0.89 g / h, and the immersion of the gold was started. At this time, the liquid in the beaker was stirred at a constant speed using the stirring bar, and the temperature of the liquid was maintained between room temperature and 37°C.
[0057] Gold sample A settled at the bottom of the beaker and was hardly flowing. The gold concentration in the liquid was 7.3 g / L after 2 hours from the start of gold immersion, 7.5 g / L after 4 hours, and 7.7 g / L after 6 hours. Even after 6 hours, gold sample A had not completely dissolved. Therefore, when using gold sample A, although a gradual increase in the gold concentration in the liquid was observed over time, equilibrium was reached in approximately 2 hours. Below, the time it took for the gold concentration in the liquid to reach 7.3 g / L was measured for each of gold samples B to D.
[0058] After the gold immersion began, gold sample B was swept up to the surface of the liquid. Furthermore, air bubbles introduced into the liquid were disintegrated upon contact with gold sample B, resulting in a bubble diameter of 50 μm or less. Using gold sample B, the gold concentration in the liquid reached 7.3 g / L before 1 hour had elapsed since the start of gold immersion. On the other hand, using either gold sample C or D, the gold concentration in the liquid did not reach 7.3 g / L even after 10 hours had elapsed since the start of gold immersion.
[0059] Comparison of gold samples A-D revealed that when gold was in powder form, the shear force of the gold itself caused the air bubbles introduced into the liquid to break down into smaller particles, leading to a preferential gold leaching reaction. On the other hand, when gold was in foil or plate form, gold leaching did not progress to the point of reaching substantial concentration equilibrium. This is presumed to be because the cyanide decomposition reaction took precedence over the gold leaching reaction, resulting in the cyanide being consumed before gold concentration equilibrium could be reached. Furthermore, when gold was granular (i.e., the gold particle size was excessively large), the gold leaching rate tended to decrease significantly over time. This tendency is presumed to be partly due to the gold not being properly lifted and cyanide decomposition proceeding preferentially. Therefore, when using gold in a form different from powder, it may be possible to further improve the reaction rate by reducing the ozone bubble diameter from the initial introduction or by using electrolytic treatment with gold as the anode. [Explanation of symbols]
[0060] 1...Reaction vessel, 2...Constant temperature bath, 3...Temperature control unit, 4...Oxygen supply unit, 5...Ozone generator, 6...Bubble generator, 7...Ozone concentration meter, 8...Ozone treatment tower, 11-14, 21-24...Graphs, 100...Manufacturing equipment.
Claims
1. The process involves supplying a liquid containing a cyanide compound, which is a complexing agent, with an oxidizing agent containing oxygen and ozone, and a recycled material which is a gold foil, thereby leaching the gold into the liquid. A method for producing a precious metal solution, wherein in the step described above, an excess of the oxidizing agent exceeding the amount necessary for the leaching of the gold is supplied to the liquid.
2. The process includes supplying an oxidizing agent containing oxygen and ozone, and an object containing gold or silver, to a liquid containing a cyanide compound, which is a complexing agent, thereby leaching the gold or silver into the liquid. In the above step, an excess of the oxidizing agent in an amount exceeding the amount necessary for the leaching of the gold or silver is supplied to the liquid. The containers in which the object and the liquid are contained are equipped with a stirrer. A method for producing a precious metal solution, wherein the supply unit for the oxidizing agent to the container is located directly below the stirrer.
3. The method for producing a precious metal solution according to claim 2, wherein in the step described above, the oxidizing agent is supplied to the liquid as bubbles.
4. The method for producing a precious metal solution according to claim 3, wherein in the step described above, the diameter of the bubbles supplied to the liquid is greater than 250 μm.
5. The method for producing a precious metal solution according to any one of claims 2 to 4, wherein the object is a gold-containing foil.
6. A method for producing a precious metal solution according to any one of claims 1 to 4, wherein in the step described above, the object is used as the anode, the cathode and a partition wall separating the anode and the cathode are placed in the liquid, and electrolysis is performed.
7. A method for producing a precious metal solution according to any one of claims 2 to 4, wherein in the step described above, the ratio of the amount of ozone consumed due to the leaching of gold or silver to the amount of ozone consumed due to the decomposition reaction of the cyanide compound decreases over time.
8. A method for producing a precious metal solution according to any one of claims 2 to 4, wherein in the step described above, the average leaching rate of the gold or silver is 20 g / (L·h) or more relative to the total amount of liquid.
Citation Information
Patent Citations
Method for removing cyanide, thiocyanate, COD and arsenic in waste liquid
CN102070264A
Gum sanitarity improving apparatus
JP1989052456A
Method for recovering noble metal
JP1990004930A
Treatment of waste water and water washings from noble metal plating using cyanide bath
JP1994336700A
Treatment of cyan-containing water
JP1997225470A