Uncrosslinked fluororubber composition, sealant manufactured using the same, and method for manufacturing the same.
By integrating an organic resin filler with fluororubber and ionic liquid, the uncrosslinked fluororubber composition addresses mechanical property deficiencies and plasma-induced dust issues, ensuring effective performance in semiconductor manufacturing.
Patent Information
- Application Number
- JP2023527501
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-08
- Filing Date
- 2022-02-28
- Publication Date
- 2026-11-19
- Estimated Expiration
- 2042-02-28
AI Technical Summary
Existing uncrosslinked fluororubber compositions compounded with ionic liquids lack sufficient mechanical properties due to the liquid form of the ionic liquids, and they generate dust when exposed to plasma atmospheres in semiconductor manufacturing environments.
Incorporating an organic resin filler, such as a phenolic resin, into the uncrosslinked fluororubber composition, along with a fluororubber and ionic liquid, enhances mechanical properties and suppresses dust generation during plasma exposure.
The crosslinked fluororubber composition achieves high mechanical properties and minimal dust generation, meeting performance criteria for semiconductor manufacturing applications.
Smart Images

Figure 0007954141000001
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to an uncrosslinked fluororubber composition, a sealing material produced using the same, and a method for producing the same. BACKGROUND ART
[0002] For example, it is known to use a rubber composition containing a fluororubber and an ionic liquid as a rubber material for sealing materials. Patent Document 1 discloses a rubber material for sealing materials containing an uncrosslinked crosslinkable fluororubber, an ionic liquid, and a crosslinking agent. Patent Document 2 discloses that a rubber composition containing a partially fluorinated elastomer rubber and an ionic liquid is used for forming a sealing material. PRIOR ART DOCUMENTS PATENT DOCUMENTS
[0003] PATENT DOCUMENT 1 JP 2019-85475 A PATENT DOCUMENT 2 JP 2019-116629 A SUMMARY OF THE INVENTION
[0004] The present invention relates to Based on JIS K6253-3:2012, the hardness measured using a Type A durometer as the instantaneous value when the pressure plate is in contact with the test specimen is A70 or higher and A95 or lower; based on JIS K6251:2017, the tensile strength measured using a dumbbell-shaped No. 3 test specimen is 10 MPa or higher, the elongation is 100% or higher, and the tensile stress at 100% elongation is 4.6 MPa or higher and 10 MPa or lower; based on JIS K6262:2013, the compression set measured using a test specimen made by cutting an AS-214 O-ring in half, with a test temperature of 200°C and a test time of 72 hours, is 35% or lower; and based on JIS K6271-1:2015, the volume resistivity measured using the double-ring electrode method with an applied voltage of 500V is 1.0 × 10⁻⁶ 13 It is less than or equal to Ω·cm, and O 2 Gas and CF 4 An uncrosslinked fluororubber composition before crosslinking is obtained in which a crosslinked fluororubber composition is obtained in which the mass loss rate calculated from the mass before and after exposure for 30 minutes to a plasma generated using a mixed gas of gases mixed in a volume ratio of 50:1 under conditions of frequency 2.45 GHz, pressure 100 Pa and output 1500 W is 3% or less, the crosslinked fluororubber composition is obtained, comprising a rubber component mainly composed of a fluororubber, an ionic liquid, an organic resin filler other than a perfluoro resin, and dry-process silica having a hydrophobized surface, wherein the organic resin filler comprises a phenol resin filler nothing.
[0005] The present invention is a sealing material formed of a crosslinked fluororubber composition obtained by crosslinking the rubber component of the uncrosslinked fluororubber composition of the present invention.
[0006] The present invention is a method for producing a sealing material, comprising forming the uncrosslinked fluororubber composition of the present invention into a shape of a sealing material and crosslinking the rubber component. [Modes for carrying out the invention]
[0007] The embodiments will be described in detail below.
[0008] The uncrosslinked fluororubber composition according to this embodiment contains a rubber component mainly composed of fluororubber, an ionic liquid, and an organic resin filler other than perfluororesin (hereinafter referred to as "organic resin filler A"). This uncrosslinked fluororubber composition can be used as a rubber material for various rubber products, and can be suitably used as a sealing material such as O-rings, and particularly as a rubber material for sealing materials used in semiconductor manufacturing equipment. Here, "perfluororesin" in this application refers to a polymer in which all monovalent atoms bonded to carbon atoms constituting the main chain are fluorine atoms. Examples of such perfluororesins include polytetrafluoroethylene (PTFE), a copolymer of tetrafluoroethylene (TFE) and hexafluoropropylene (HFP) (FEP), etc.
[0009] However, in uncrosslinked fluororubber compositions in which ionic liquids are compounded with fluororubber, there is a problem in that sufficient mechanical properties cannot be obtained in the crosslinked fluororubber composition obtained by crosslinking the ionic liquid, because the ionic liquid is in liquid form.
[0010] In contrast, the uncrosslinked fluororubber composition according to the above embodiment has fluororubber as the main component of the rubber component and contains an ionic liquid, but also contains organic resin filler A, and due to the reinforcing effect of the organic resin filler A, sufficient mechanical properties of the crosslinked fluororubber composition can be obtained. Furthermore, because it contains organic resin filler A, when used as a rubber material for sealing materials used in semiconductor manufacturing equipment, dust generation can be suppressed even when the sealing material is exposed to a plasma atmosphere.
[0011] Here, the fluororubber content in the rubber component is 50% by mass or more, and from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition, it is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 100% by mass. In addition to fluororubber, the rubber component may also contain nitrile rubber, silicone rubber, ethylene propylene rubber, etc.
[0012] Examples of fluororubbers include copolymers of vinylidene fluoride (VDF) and hexafluoropropylene (HFP) (binary FKM), copolymers of vinylidene fluoride (VDF), hexafluoropropylene (HFP), and tetrafluoroethylene (TFE) (ternary FKM), copolymers of tetrafluoroethylene (TFE) and propylene (Pr) (FEP), copolymers of vinylidene fluoride (VDF), propylene (Pr), and tetrafluoroethylene (TFE), and copolymers of ethylene (E) and tetrafluoroethylene (T). Examples include copolymers of ethylene (E) with perfluoroethylene (TFE) (ETFE), copolymers of ethylene (E) with tetrafluoroethylene (TFE) and perfluoromethyl vinyl ether (PMVE), copolymers of vinylidene fluoride (VDF) with tetrafluoroethylene (TFE) and perfluoromethyl vinyl ether (PMVE), copolymers of tetrafluoroethylene (TFE) with perfluoromethyl vinyl ether (PMVE) (FFKM), and copolymers of vinylidene fluoride (VDF) with perfluoromethyl vinyl ether (PMVE). The fluororubber preferably contains one or more of these, and from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition, it is more preferable to include vinylidene fluoride-based fluororubber such as binary FKM or ternary FKM, and from the viewpoint of obtaining excellent plasma resistance even when the seal material is exposed to a plasma atmosphere when the uncrosslinked fluororubber composition is used as a rubber material for seal materials used in semiconductor manufacturing equipment, it is even more preferable to include ternary FKM.
[0013] In this application, "ionic liquid" refers to a liquid that is a salt composed of cations and anions and has a melting point of 100°C or lower.
[0014] Examples of cations in ionic liquids include imidazolium cations, pyridinium cations, pyrrolidinium cations, and ammonium cations. Examples of imidazolium cations include 1-ethyl-3-methylimidazolium cation, 1-methyl-3-methylimidazolium cation, 1-butyl-3-methylimidazolium cation, 1-hexyl-3-methylimidazolium cation, 1-octyl-3-methylimidazolium cation, 1-methyl-2,3-dimethylimidazolium cation, 1-butyl-2,3-dimethylimidazolium cation, 1-hexyl-2,3-dimethylimidazolium cation, and 1-octyl-2,3-dimethylimidazolium cation. Examples of pyridinium-based cations include 1-octyl-4-methylpyridinium cation, 1-methylpyridinium cation, 1-butylpyridinium cation, and 1-hexylpyridinium cation. Examples of pyrrolidinium-based cations include 1-ethyl-1-methylpyrrolidinium cation. Examples of ammonium-based cations include tributylmethylammonium cation. It is preferable that the cation of the ionic liquid contains one or more of these.
[0015] Examples of anions in the ionic liquid include bisfluorosulfonylimide anions, fluorinated sulfonic acid anions, fluorinated carboxylic acid anions, thiocyanate anions, dicyanamide anions, and tetracyanoborate anions. Examples of bisfluorosulfonylimide anions include bisfluorosulfonylimide anions, bistrifluoromethanesulfonylimide anions, and bistrifluorobutanesulfonylimide anions. Examples of fluorinated sulfonic acid anions include tetrafluoroborate anions, hexafluoroborate anions, and trifluoromethanesulfonate anions. Examples of fluorinated carboxylic acid anions include trifluoroacetate anions. The anions in the ionic liquid preferably contain one or more of these, and from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition, it is more preferable to include those having a fluorine atom, such as bisfluorosulfonylimide anions, fluorinated sulfonic acid anions, and fluorinated carboxylic acid anions.
[0016] The ionic liquid preferably contains a combination of one or more of these cations and one or more of these anions, and more preferably contains 1-butyl-3-methylimidazolium-bistrifluoromethanesulfonylimide, 1-ethyl-1-methylpyrrolidinium-bistrifluoromethanesulfonylimide, or tributylmethylammonium-bistrifluoromethanesulfonylimide, from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition.
[0017] The ionic liquid content P in the uncrosslinked fluororubber composition according to the embodiment is preferably 0.1 parts by mass or more and 10 parts by mass or less, more preferably 0.2 parts by mass or more and 5 parts by mass or less, and even more preferably 0.5 parts by mass or more and 1.5 parts by mass or less, per 100 parts by mass of the rubber component, from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition.
[0018] Examples of organic resin filler A include phenolic resin fillers, polyether ether ketone (PEEK) resin fillers, polyvinylidene fluoride (PVDF) resin fillers, and other fluororesin fillers besides perfluororesins. It is preferable that organic resin filler A contains one or more of these.
[0019] Organic resin filler A preferably contains a phenolic resin filler, from the viewpoint of obtaining sufficient mechanical properties for the crosslinked fluororubber composition and promoting crosslinking of the uncrosslinked fluororubber composition. From the same viewpoint, it is preferable that this phenolic resin is neither resol-type nor novolac-type. Furthermore, from the same viewpoint, it is preferable that the phenolic resin has a methylol group in its molecule.
[0020] Organic resin filler A preferably contains a fluororesin filler other than perfluororesin, and more preferably contains a PVDF resin filler, from the viewpoint of suppressing dust generation even when the sealing material is exposed to a plasma atmosphere when the uncrosslinked fluororubber composition is used as a rubber material for sealing materials used in semiconductor manufacturing equipment.
[0021] From the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition, the average particle size of the organic resin filler A is preferably 0.5 μm to 20 μm, more preferably 1 μm to 10 μm, and even more preferably 1.2 μm to 2 μm.
[0022] When the uncrosslinked fluororubber composition according to the embodiment contains fillers other than the organic resin filler A, the content Q of the organic resin filler A is preferably 0.5 to 30 parts by mass, more preferably 1 to 20 parts by mass, and still more preferably 1 to 10 parts by mass, based on 100 parts by mass of the rubber component, from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition. When no filler other than the organic resin filler A is contained, the content is preferably 1 to 50 parts by mass, more preferably 2 to 40 parts by mass, and still more preferably 3 to 30 parts by mass, based on 100 parts by mass of the rubber component.
[0023] When the organic resin filler A contains a fluororesin filler other than perfluororesin, the content of the fluororesin filler other than perfluororesin in the uncrosslinked fluororubber composition according to the embodiment is based on 100 parts by mass of the rubber component, from the viewpoint that when the uncrosslinked fluororubber composition is used as a rubber material for a sealing material used in semiconductor manufacturing equipment, dust generation can be suppressed even if the sealing material is exposed to a plasma atmosphere, the content is preferably 1 to 25 parts by mass, more preferably 2 to 10 parts by mass, and still more preferably 3 to 7 parts by mass.
[0024] When the uncrosslinked fluororubber composition according to the embodiment contains fillers other than the organic resin filler A, the content Q of the organic resin filler A is preferably equal to or higher than the content P of the ionic liquid, from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition. In this case, the ratio (Q / P) of the content Q of the organic resin filler A to the content P of the ionic liquid in the uncrosslinked fluororubber composition is preferably 1 to 15, more preferably 1.5 to 10, from the same viewpoint. When no filler other than the organic resin filler A is contained, the content Q of the organic resin filler A is preferably larger than the content P of the ionic liquid from the same viewpoint. In this case, the ratio (Q / P) of the content Q of the organic resin filler A to the content P of the ionic liquid in the uncrosslinked fluororubber composition is preferably 5 to 40, more preferably 10 to 30, from the same viewpoint.
[0025] From the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition, the uncrosslinked fluororubber composition according to the embodiment preferably further contains silica as a filler. Examples of the silica include dry process silica such as fumed silica, and wet process silica such as precipitated silica. The surface of the silica may be subjected to a hydrophobic treatment with organochlorosilane, organoalkoxysilane, hexaorganodisilazane, organosiloxane oligomer or the like. The silica preferably contains one or more of these, and from the same viewpoint, more preferably contains dry process silica whose surface is hydrophobized with organochlorosilane, and further preferably contains fumed silica whose surface is hydrophobized with dimethyldichlorosilane.
[0026] When silica is contained as a filler in the uncrosslinked fluororubber composition according to the embodiment, the mechanical properties of the crosslinked fluororubber composition can be effectively enhanced even if the content of silica is small. Further, when the uncrosslinked fluororubber composition is used as a rubber material for a sealing material employed in semiconductor manufacturing apparatuses, silica does not generate dust even when the sealing material is exposed to a plasma atmosphere. On the other hand, the combined use of silica with an ionic liquid may inhibit the crosslinking of the uncrosslinked fluororubber composition. However, if a phenol resin filler is used as the organic resin filler A, the crosslinking of the uncrosslinked fluororubber composition can be promoted as described above, so that the inhibition of crosslinking can be suppressed. For this reason, when the uncrosslinked fluororubber composition contains silica as a filler, it preferably also contains a phenol resin filler as the organic resin filler A.
[0027] When the organic resin filler A contains a fluororesin filler other than perfluororesin, the uncrosslinked fluororubber composition according to the embodiment can obtain sufficiently high mechanical properties of the crosslinked fluororubber composition, and thus preferably does not contain silica. However, even in this case, the uncrosslinked fluororubber composition may contain silica.
[0028] The silica content R in the uncrosslinked fluororubber composition according to the embodiment is preferably 1 to 20 parts by mass, more preferably 5 to 15 parts by mass, per 100 parts by mass of the rubber component, from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition.
[0029] In the uncrosslinked fluororubber composition according to the embodiment, the silica content R is preferably greater than the ionic liquid content P, from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition. From the same viewpoint, the ratio of the silica content R to the ionic liquid content P (R / P) in the uncrosslinked fluororubber composition is preferably 3 to 20, more preferably 5 to 15.
[0030] In the uncrosslinked fluororubber composition according to the embodiment, the silica content R is preferably equal to or greater than the organic resin filler A content Q, from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition. From the same viewpoint, the ratio of the silica content R to the organic resin filler A content Q (R / Q) in the uncrosslinked fluororubber composition is preferably 1 to 15, more preferably 1 to 3.
[0031] The uncrosslinked fluororubber composition according to the embodiment may further contain a crosslinking agent. Examples of crosslinking agents include organic peroxides, polyols, polyamines, and triazines. From the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition, it is preferable that the crosslinking agent includes an organic peroxide.
[0032] Examples of organic peroxides include dialkyl peroxides such as dicumyl peroxide, 1,3-di(t-butylperoxy)diisopropylbenzene, 1,4-di(t-butylperoxy)diisopropylbenzene, t-butylcumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, and 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane-3; peroxyketals such as 1,1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, and n-butyl-4,4-di(t-butylperoxy)valerate; and peroxyesters such as 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-hexylperoxybenzoate, and t-butylperoxybenzoate. The organic peroxide preferably contains one or more of these, and more preferably contains 2,5-dimethyl-2,5-di(t-butylperoxy)hexane from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition.
[0033] The content X of the organic peroxide crosslinking agent in the uncrosslinked fluororubber composition according to the embodiment is preferably 0.5 parts by mass or more and 5 parts by mass or less, more preferably 0.5 parts by mass or more and 4 parts by mass or less, and even more preferably 1 part by mass or more and 2 parts by mass or less, per 100 parts by mass of the rubber component, from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition.
[0034] If the uncrosslinked fluororubber composition according to the embodiment contains an organic peroxide as a crosslinking agent, it may further contain a crosslinking aid. Examples of crosslinking aids include allyl crosslinking aids such as triallyl isocyanurate, diallyl fumarate, diallyl phthalate, tetraallyl oxyethane, and trimethallyl isocyanurate; maleimide crosslinking aids such as N,N'-m-phenylenebismaleimide, maleimide, and phenylmaleimide; methacrylate crosslinking aids such as trimethylolpropane trimethacrylate, ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, and polyethylene glycol dimethacrylate; and 1,2-polybutadiene. The crosslinking aid preferably contains one or more of these, and from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition, it is more preferable to include an allyl crosslinking aid, and even more preferable to include triallyl isocyanurate.
[0035] The content Y of the crosslinking aid in the uncrosslinked fluororubber composition according to the embodiment is preferably 1 to 10 parts by mass, more preferably 2 to 8 parts by mass, and even more preferably 2 to 6 parts by mass, per 100 parts by mass of the rubber component, from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition.
[0036] In the uncrosslinked fluororubber composition according to the embodiment, the content Y of the crosslinking aid is preferably greater than the content X of the organic peroxide, from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition. From the same viewpoint, the ratio of the content Y of the crosslinking aid to the content X of the organic peroxide (Y / X) in the uncrosslinked fluororubber composition is preferably 1 or more and 10 or less, more preferably 1.5 or more and 4 or less.
[0037] The uncrosslinked fluororubber composition according to the embodiment may contain other rubber compounding agents as needed. However, when used as a rubber material for sealing materials used in semiconductor manufacturing equipment, it is preferable that the uncrosslinked fluororubber composition does not contain conductive fillers such as carbon black, conductive carbon, or metal oxides, from the viewpoint of preventing dust generation when the sealing material is exposed to a plasma atmosphere.
[0038] The uncrosslinked fluororubber composition according to this embodiment can be obtained by adding a rubber component mainly composed of fluororubber to a rubber kneader such as an open roll or Banbury mixer and kneading it, and then adding various rubber compounding agents including an ionic liquid and organic resin filler A and kneading them together.
[0039] By using the uncrosslinked fluororubber composition according to the above embodiment, and crosslinking the rubber component, a sealing material used in semiconductor manufacturing equipment can be manufactured, for example.
[0040] In a sealing material manufactured using the uncrosslinked fluororubber composition according to the embodiment, the hardness Hs of the crosslinked fluororubber composition forming it is preferably A50 or higher and A95 or lower. This hardness Hs is measured using a Type A durometer in accordance with JIS K6253-3:2012, as the instantaneous value when the pressure plate is in contact with the test piece.
[0041] The tensile strength Tb of the cross-linked fluororubber composition forming the sealant is preferably 10 MPa or higher. The elongation Eb is preferably 100% or higher. The tensile stress S100 at 100% elongation is preferably 1 MPa or higher and 10 MPa or lower. These tensile strength Tb, elongation Eb, and tensile stress S100 at 100% elongation are measured using a dumbbell-shaped No. 3 test specimen in accordance with JIS K6251:2017.
[0042] The compression set of the crosslinked fluororubber composition forming the sealing material is preferably 40% or less, more preferably 35% or less, and even more preferably 30% or less. This compression set is measured in accordance with JIS K6262:2013, using a sample of an AS-214 O-ring cut in half, at a test temperature of 200°C and a test time of 72 hours.
[0043] The volume resistivity of the crosslinked fluororubber composition forming the sealant is preferably 1.0 × 10⁻⁶. 13 Ω·cm or less, more preferably 1.0 × 10⁻⁶ 12 It is less than or equal to Ω·cm. This volume resistivity is measured using the double-ring electrode method with an applied voltage of 500V, in accordance with JIS K6271-1:2015.
[0044] The mass loss rate (plasma resistance) of the cross-linked fluororubber composition forming the sealing material due to plasma irradiation is preferably 3% or less, more preferably 2.5% or less. This mass loss rate is calculated based on the following formula by exposing the cross-linked fluororubber composition to plasma generated for 30 minutes using a mixed gas of O2 gas and CF4 gas in a volume ratio of 50:1, at a frequency of 2.45 GHz, a pressure of 100 Pa, and an output of 1500 W, and measuring the mass before and after the exposure. Mass reduction rate (%) = {(mass before exposure - mass after exposure) / mass before exposure} × 100
[0045] Next, an example of a method for manufacturing a seal material is described, which involves using an uncrosslinked fluororubber composition according to the embodiment, forming it into a seal material shape, and crosslinking the rubber component.
[0046] First, a predetermined amount of the uncrosslinked fluororubber composition according to the embodiment is taken and filled into a cavity in the shape of a seal material formed in a mold. Then, the mold is clamped to form the uncrosslinked fluororubber composition into the shape of a seal material.
[0047] Next, a mold is placed between heating plates, and the uncrosslinked fluororubber composition formed into a sealing material shape is subjected to press molding by heating and pressurizing at a predetermined temperature (e.g., 160°C to 170°C) and a predetermined pressure (e.g., 10 MPa to 20 MPa) for a predetermined time (e.g., 5 to 30 minutes) to cause primary crosslinking of the rubber components and obtain a primary crosslinked product (primary crosslinking step).
[0048] Then, after demolding the primary crosslinked material from the mold, it is placed in an oven and subjected to annealing, in which the primary crosslinked material is heated at a higher temperature (e.g., 190°C to 210°C) than in the primary crosslinking step and for a long period of time (e.g., 3 to 5 hours) to cause secondary crosslinking of the rubber components, thereby obtaining a secondary crosslinked material (secondary crosslinking step).
[0049] The method for manufacturing the sealant consists of a primary crosslinking step and a secondary crosslinking step, and the secondary crosslinked product may be used as the sealant as is. However, from the viewpoint of obtaining sufficient mechanical properties of the crosslinked fluororubber composition, the method for manufacturing the sealant may further include a radiation crosslinking step in addition to the primary and secondary crosslinking steps, in which radiation is irradiated to crosslink the rubber components. In this case, from the same viewpoint, it is preferable to irradiate the secondary crosslinked product with radiation in the radiation crosslinking step, that is, to perform the radiation crosslinking step after the secondary crosslinking step. Examples of radiation include alpha rays, beta rays, gamma rays, electron beams, ions, etc. Of these, electron beams or gamma rays are preferred. The radiation dose is, for example, 10 kGy or more and 100 kGy or less. [Examples]
[0050] (Uncrosslinked fluororubber composition) The following is Example 1 4, Reference examples 1~7 Uncrosslinked fluororubber compositions of Comparative Examples 1 to 5 were prepared. Their respective compositions are also shown in Table 1.
[0051] <Example 1> Example 1 was an uncrosslinked fluororubber composition prepared by kneading 100 parts by mass of ternary FKM (Technoflon P959, manufactured by Solvay Specialty Polymers Japan) as the rubber component, with 1 part by mass of the ionic liquid 1-butyl-3-methylimidazolium bistrifluoromethanesulfonylimide (BMIN111, manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.), 1 part by mass of phenolic resin filler (Bellpearl R100, manufactured by Air Water Bellpearl Co., Ltd., average particle size 1.5 μm), 10 parts by mass of hydrophobized fumed silica (Aerosil R976S, manufactured by Nippon Aerosil Co., Ltd.) treated with dimethyldichlorosilane, 1.5 parts by mass of the organic peroxide 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (Perhexa 25B, manufactured by NOF Corporation), and 4 parts by mass of the crosslinking aid triallyl isocyanurate (TAIC, manufactured by Mitsubishi Chemical Corporation).
[0052] <Example 2> Example 2 was an uncrosslinked fluororubber composition prepared in the same manner as in Example 1, except that the amount of phenolic resin filler was 5 parts by mass per 100 parts by mass of rubber component.
[0053] <Example 3> Example 3 was an uncrosslinked fluororubber composition prepared in the same manner as in Example 2, except that 1-ethyl-1-methylpyrrolidinium bistrifluoromethanesulfonylimide (P12N111, manufactured by Mitsubishi Materials Electronics Chemicals Co., Ltd.) was used as the ionic liquid.
[0054] <Example 4> Example 4 was an uncrosslinked fluororubber composition prepared in the same manner as in Example 2, except that tributylmethylammonium bistrifluoromethanesulfonylimide (FC-4400, manufactured by 3M Corporation) was used as the ionic liquid.
[0055] < Reference example 1 > An uncrosslinked fluororubber composition prepared in the same manner as in Example 2, except that hydrophilic fumed silica (Aerosil 200, manufactured by Nippon Aerosil Co., Ltd.) that has not been hydrophobized was used. Reference example 1That's what I decided.
[0056] < Reference example 2 > An uncrosslinked fluororubber composition prepared in the same manner as in Example 1, except that fumed silica was not included and the amount of phenol resin filler was 25 parts by mass per 100 parts by mass of rubber component. Reference example 2 That's what I decided.
[0057] < Reference example 3 > An uncrosslinked fluororubber composition was prepared in the same manner as in Example 1, except that phenolic resin filler and fumed silica were not included, and 25 parts by mass of PVDF resin filler (Kyner MG15, manufactured by Arkema, average particle size 10 μm) were added per 100 parts by mass of rubber component. Reference example 3 That's what I decided.
[0058] < Reference example 4 > An uncrosslinked fluororubber composition was prepared in the same manner as in Example 1, except that phenolic resin filler and fumed silica were not included, and 25 parts by mass of PEEK resin filler (Vestakeep 2000UFP10, manufactured by Daicel Evonik, average particle size 10 μm) was added per 100 parts by mass of rubber component. Reference example 4 That's what I decided.
[0059] < Reference example 5 > An uncrosslinked fluororubber composition prepared in the same manner as in Example 1, except that fumed silica was not included and the amount of phenol resin filler was 5 parts by mass per 100 parts by mass of rubber component. Reference example 5 That's what I decided.
[0060] < Reference example 6 > Except for the fact that PVDF resin filler is added in a ratio of 5 parts by mass per 100 parts by mass of rubber component, without the addition of phenolic resin filler. Reference example 5 An uncrosslinked fluororubber composition prepared in the same manner Reference example 6 That's what I decided.
[0061] < Reference example 7 > Except for the fact that PEEK resin filler is added in an amount of 5 parts by mass per 100 parts by mass of rubber component, without the addition of phenolic resin filler. Reference example 5 An uncrosslinked fluororubber composition prepared in the same manner Reference example 7 That's what I decided.
[0062] <Comparative Example 1> Comparative Example 1 was an uncrosslinked fluororubber composition prepared in the same manner as in Example 1, except that it did not contain phenolic resin filler and fumed silica.
[0063] <Comparative Example 2> A comparative example was prepared in the same manner as in Example 1, except that it did not contain an ionic liquid and a phenolic resin filler. 2 That's what I decided.
[0064] <Comparative Example 3> Comparative Example 3 was prepared in the same manner as in Example 1, except that it did not contain phenolic resin filler and fumed silica, and instead contained 25 parts by mass of PTFE resin filler (Lubron L-5, manufactured by Daikin Corporation, average particle size 5 to 7 μm) per 100 parts by mass of rubber component.
[0065] <Comparative Example 4> Comparative Example 4 was an uncrosslinked fluororubber composition prepared in the same manner as in Example 1, except that it did not contain phenolic resin filler and fumed silica, and instead contained 25 parts by mass of carbon black (Thermax N990, manufactured by Cancarb) per 100 parts by mass of rubber component.
[0066] <Comparative Example 5> Except for the fact that PTFE resin filler is added in a ratio of 5 parts by mass per 100 parts by mass of rubber component, without the addition of phenolic resin filler. Reference example 5 A non-crosslinked fluororubber composition prepared in the same manner was designated as Comparative Example 5.
[0067] [Table 1]
[0068] Furthermore, an uncrosslinked fluororubber composition similar to that in Example 1 was prepared, except that it did not contain a phenolic resin filler, and an uncrosslinked fluororubber composition similar to that in Example 1 was prepared, except that it did not contain a phenolic resin filler and the amount of ionic liquid was 0.1 parts by mass per 100 parts by mass of rubber component. However, no crosslinked products were obtained from these compositions.
[0069] (Test method and results) Test specimens of the crosslinked fluororubber composition, obtained by crosslinking the above-mentioned uncrosslinked fluororubber composition, were prepared and used to conduct the following tests. The results are shown in Table 1.
[0070] <Hardness> Example 1 to 4. Reference examples 1 to 7 From each of the uncrosslinked fluororubber compositions of Comparative Examples 1 to 5, 6 mm thick sheet-like crosslinked fluororubber composition test specimens were prepared, and the hardness Hs was measured using a Type A durometer in accordance with JIS K6253-3:2012, as the instantaneous value when the pressure plate was in contact with the test specimen.
[0071] <Tensile properties> Example 1 to 4. Reference examples 1 to 7 Dumbbell-shaped test specimens of crosslinked fluororubber compositions were prepared from each of the uncrosslinked fluororubber compositions of Comparative Examples 1 to 5, and the tensile strength Tb, elongation Eb, and tensile stress S100 at 100% elongation were measured according to JIS K6251:2017.
[0072] <Compression set> Example 1 to 4. Reference examples 1 to 7 AS-214 O-rings were prepared from the crosslinked fluororubber compositions of each of the uncrosslinked fluororubber compositions of Comparative Examples 1 to 5, and the O-rings were cut in half to be used as samples. The compression set CS was measured according to JIS K6262:2013, with a test temperature of 200°C and a test time of 72 hours.
[0073] <Volume resistivity> Example 1 to 4. Reference examples 1 to 7 Test specimens (100 × 100 × t2 mm sheets) of the crosslinked fluororubber compositions were prepared from each of the uncrosslinked fluororubber compositions of Comparative Examples 1 to 5, and the volume resistivity was measured by the double-ring electrode method with an applied voltage of 500 V, in accordance with JIS K6271-1:2015.
[0074] <Plasma resistance> Example 1 to 4. Reference examples 1 to 7 AS-214 O-rings formed from crosslinked fluororubber compositions were prepared from each of the uncrosslinked fluororubber compositions of Comparative Examples 1 to 5 and used as samples. These samples were then placed in a plasma exposure device (manufactured by Shinko Seiki Co., Ltd.) and exposed to plasma generated for 30 minutes using a mixed gas of O2 gas and CF4 gas in a 50:1 volume ratio, at a frequency of 2.45 GHz, a pressure of 100 Pa, and an output of 1500 W. The presence or absence of dust generation was visually confirmed. The mass loss rate was calculated from the mass before and after the procedure based on the following formula. Mass reduction rate (%) = {(mass before exposure - mass after exposure) / mass before exposure} × 100
[0075] Example 1 to 4. Reference examples 1 to 7 In comparative examples 1 to 5, 5 parts by mass of PVDF resin filler were blended with 100 parts by mass of three-dimensional FKM rubber component. Reference example 6 This option showed the smallest mass loss rate and superior plasma resistance. [Industrial applicability]
[0076] The present invention is useful in the technical field of uncrosslinked fluororubber compositions, sealing materials manufactured using them, and methods for manufacturing the same.
Claims
1. The hardness measured using a Type A durometer based on JIS K6253-3:2012, as an instantaneous value when the pressure plate is in contact with the test piece, is A70 or more and A95 or less; the tensile strength measured using a dumbbell-shaped No. 3 test piece based on JIS K6251:2017, is 10 MPa or more, the elongation is 100% or more, and the tensile stress at 100% elongation is 4.6 MPa or more and 10 MPa or less; the compression set measured using a test piece made by cutting an AS-214 O-ring in half, with a test temperature of 200°C and a test time of 72 hours, based on JIS K6262:2013, is 35% or less; and the volume resistivity measured using the double-ring electrode method with an applied voltage of 500V, based on JIS K6271-1:2015, is 1.0 × 10¹³ Ω·cm or less, and O₂ gas and CF₄ An uncrosslinked fluororubber composition before crosslinking is obtained in which a crosslinked fluororubber composition is obtained in which the mass loss rate calculated from the mass before and after exposure for 30 minutes to a plasma generated using a mixed gas obtained by mixing gases in a volume ratio of 50:1 under the conditions of frequency 2.45 GHz, pressure 100 Pa and output 1500 W is 3% or less, the mass loss rate calculated from the mass before and after exposure, the crosslinked fluororubber composition is 3% or less, It contains a rubber component mainly composed of fluororubber, an ionic liquid, an organic resin filler other than perfluororesin, and dry-process silica with a hydrophobic surface treatment. The organic resin filler is an uncrosslinked fluororubber composition containing a phenolic resin filler.
2. In the uncrosslinked fluororubber composition described in claim 1, The aforementioned fluororubber is an uncrosslinked fluororubber composition containing vinylidene fluoride-based fluororubber.
3. In the uncrosslinked fluororubber composition described in claim 2, The aforementioned fluororubber is an uncrosslinked fluororubber composition comprising a copolymer of vinylidene fluoride, hexafluoropropylene, and tetrafluoroethylene.
4. In an uncrosslinked fluororubber composition according to any one of claims 1 to 3, An uncrosslinked fluororubber composition in which the anions of the ionic liquid have fluorine atoms.
5. In an uncrosslinked fluororubber composition according to any one of claims 1 to 4, An uncrosslinked fluororubber composition in which the cation of the ionic liquid contains one or more of the following: imidazolium-based cations, pyridinium-based cations, pyrrolidinium-based cations, and ammonium-based cations.
6. In an uncrosslinked fluororubber composition according to any one of claims 1 to 5, An uncrosslinked fluororubber composition wherein the average particle size of the organic resin filler is 0.5 μm or more and 20 μm or less.
7. In an uncrosslinked fluororubber composition according to any one of claims 1 to 6, An uncrosslinked fluororubber composition in which the content of the organic resin filler is 0.5 parts by mass or more and 30 parts by mass or less per 100 parts by mass of the rubber component.
8. In an uncrosslinked fluororubber composition according to any one of claims 1 to 7, An uncrosslinked fluororubber composition in which the surface of the dry-process silica is hydrophobized with dimethyldichlorosilane.
9. In an uncrosslinked fluororubber composition according to any one of claims 1 to 8, An uncrosslinked fluororubber composition in which the content of the dry-process silica is 1 part by mass or more and 20 parts by mass or less per 100 parts by mass of the rubber component.
10. In an uncrosslinked fluororubber composition according to any one of claims 1 to 9, An uncrosslinked fluororubber composition in which the content of the dry-process silica is greater than the content of the ionic liquid.
11. In the uncrosslinked fluororubber composition described in claim 10, An uncrosslinked fluororubber composition in which the mass ratio of the content of the dry-process silica to the content of the ionic liquid is 3 or more and 20 or less.
12. In an uncrosslinked fluororubber composition according to any one of claims 1 to 11, An uncrosslinked fluororubber composition in which the content of the dry-process silica is equal to or greater than the content of the organic resin filler.
13. In the uncrosslinked fluororubber composition described in claim 12, An uncrosslinked fluororubber composition in which the mass ratio of the dry-process silica content to the organic resin filler content is 1 or more and 15 or less.
14. In an uncrosslinked fluororubber composition according to any one of claims 1 to 13, An uncrosslinked fluororubber composition further containing an organic peroxide as a crosslinking agent.
15. In the uncrosslinked fluororubber composition described in claim 14, An uncrosslinked fluororubber composition further containing a crosslinking aid.
16. A sealing material formed from a crosslinked fluororubber composition in which the rubber component of the uncrosslinked fluororubber composition described in any one of claims 1 to 15 is crosslinked.
17. In the sealing material described in claim 16, A sealing material used in semiconductor manufacturing equipment.
18. A method for producing a seal material by forming an uncrosslinked fluororubber composition according to any one of claims 1 to 15 into a seal material shape and crosslinking the rubber component.
Citation Information
Patent Citations
Sealant rubber material and sealant including the same
JP2019085475A
Partially fluorinated elastomers and methods of making and using the same
JP2019116629A
Fluorine-containing elastomer composition with excellent plasma-aging prevention effect and shaped article made thereof
WO2004094527A1