Structured films and optical articles containing structured films
Structured films with engineered structures and adhesive layers facilitate large-scale production of nanostructured articles for optical metasurfaces, overcoming inefficiencies of traditional lithography by enabling efficient, scalable manufacturing and effective bonding to waveguides.
Patent Information
- Application Number
- JP2023536852
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-18
- Filing Date
- 2021-12-15
- Publication Date
- 2026-11-19
- Estimated Expiration
- 2041-12-15
AI Technical Summary
Existing methods for creating nanostructured articles, such as optical metasurfaces, require complex lithography patterning processes that are inefficient for large-scale production and may not achieve the desired surface relief gratings effectively.
The development of structured films that can be applied to substrates without traditional lithography patterning, allowing for larger dimensions and continuous roll-to-roll manufacturing, featuring engineered structures with controlled refractive index differences and adhesive layers for bonding to waveguides, and including peelable or dynamic separation layers for easy substrate removal.
Enables efficient, large-scale production of nanostructured articles with embedded surface relief gratings on waveguides, facilitating optical applications like incoupling, outcoupling, and optical distribution without the limitations of conventional lithography, while maintaining structural integrity and adhesion.
Smart Images

Figure 0007954144000002 
Figure 0007954144000003 
Figure 0007954144000004
Abstract
Description
[Background technology]
[0001] Structured articles, such as nanostructured articles, are useful for a variety of applications, including optical applications such as optical metasurface applications. [Overview of the Initiative]
[0002] This specification generally relates to structured films and optical articles containing structured films.
[0003] In some aspects of this specification, optical articles are provided. The optical article includes a waveguide and a structured film. The structured film includes a polymer substrate, an etch-stop layer disposed on the polymer substrate, a structured layer including a plurality of engineered structures disposed on the side of the etch-stop layer opposite to the polymer substrate, a planar backfill layer disposed on the plurality of engineered structures having a surface roughness Ra and defining a substantially flat main surface of the planar backfill layer, and an adhesive layer disposed on the substantially flat main surface of the planar backfill layer for bonding the structured film to the waveguide. The difference in refractive index between the planar backfill layer and the structured layer is at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm. The adhesive layer has an average thickness ta and Ra <ta<(1 / 4)W1である。
[0004] In some aspects of the present specification, a structured film is provided. The structured film includes a polymer substrate, an etch stop layer disposed on the polymer substrate, a structured layer comprising a plurality of fabricated structures disposed on a side of the etch stop layer opposite to the polymer substrate, a planarizing backfill layer disposed over the plurality of fabricated structures, the planarizing backfill layer defining a substantially planar major surface of the planarizing backfill layer having a surface roughness Ra, and an adhesive layer disposed on the substantially planar major surface of the planarizing backfill layer. The fabricated structures can be tilted relative to the etch stop layer. A difference in refractive index between the planarizing backfill layer and the structured layer is at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm. The adhesive layer has an average thickness ta, where Ra < ta < (1 / 4)W1.
[0005] In some aspects of the present specification, an optical article is provided that includes a waveguide and a structured film disposed on a major surface of the waveguide. The structured film includes an etch stop layer, a structured layer disposed on the etch stop layer and comprising a plurality of fabricated structures, a planarizing backfill layer disposed over the plurality of fabricated structures, the planarizing backfill layer defining a substantially unstructured major surface of the planarizing backfill layer having a surface roughness Ra, and an adhesive layer disposed on the substantially unstructured major surface of the planarizing backfill layer. A difference in refractive index between the planarizing backfill layer and the structured layer is at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm. The adhesive layer bonds the structured film to the major surface of the waveguide and has an average thickness ta where Ra < ta < (1 / 4)W1. The fabricated structures can be tilted relative to the etch stop layer.
[0006] In several aspects of the present specification, a structured film is provided. The structured film includes a polymer substrate, an etch stop layer, a dynamic separation layer disposed between the polymer substrate and the etch stop layer, a structured layer disposed on a side of the etch stop layer opposite to the dynamic separation layer and comprising a plurality of fabricated structures, a planarization backfill layer disposed over the plurality of fabricated structures, the planarization backfill layer defining a substantially flat major surface of the planarization backfill layer having a surface roughness Ra, and an adhesive layer disposed on the substantially flat major surface of the planarization backfill layer. The difference in refractive index between the planarization backfill layer and the structured layer is at least 0.25 for at least a first wavelength W1 within the range of 400 nm to 2500 nm. The adhesive layer has an average thickness ta, and satisfies Ra < ta < (1 / 4)W1. The dynamic separation layer is adapted to facilitate separation of the polymer substrate and the etch stop layer upon activation.
[0007] These and other aspects will be apparent from the following detailed description. However, in no event shall this brief summary be construed as limiting the subject matter of the claims. [Brief Description of the Drawings]
[0008]
Figure 1
Figure 2
Figure 3
Figure 4A
Figure 4B
Figure 5A
Figure 5B
Figure 5C
Figure 6A
Figure 6B
Figure 6C
Figure 7A
Figure 7B
Figure 7C
Figure 8
[0009] In the following description, reference is made to the accompanying drawings, which form a part of this specification and in which various embodiments are shown by way of example. The drawings are not necessarily to scale. It is to be understood that other embodiments are contemplated and may be practiced without departing from the scope or spirit of the present disclosure. The following detailed description is therefore not to be interpreted in a limiting sense.
[0010] Nanostructured articles can be formed by patterning functional materials. Patterning of functional materials can be performed by depositing a uniform layer of the functional material onto a substrate (e.g., a waveguide) and then forming a pattern on the material using a lithography patterning process. Other methods for forming nanostructured articles are described, for example, in International Publication No. 2020 / 095258 (Van Lengerich et al.) and International Publication No. 2020 / 097319 (Wolk et al.).
[0011] According to several embodiments of this specification, structured films are provided that can be used to apply structures (e.g., nanostructures) onto substrates without the series of steps used in typical lithography patterning processes. The structured films may be substantially larger than, for example, semiconductor wafer formats used in conventional nanoimprint lithography (NIL) batch processes, or display glass substrates typically used in large NIL or roll-to-plate NIL. In some embodiments, the structured films have maximum dimensions exceeding, for example, 100 mm, 200 mm, 300 mm, 450 mm, or 600 nm. In some embodiments, the structured films have maximum dimensions exceeding, for example, 4 m, or 5 m, or 10 m, or 50 m, or 100 m. The structured films can be manufactured in a continuous roll-to-roll process. In some embodiments, rolls of structured films are provided. In some embodiments, the rolls are converted into sheets.
[0012] For example, the structured film may include a low refractive index layer that separates the structured layer from the polymer substrate, or the polymer substrate contained in the structured film may be removed after the structured film has been applied to the waveguide. The structured film may be designed to produce an equivalent of a surface relief grating (SRG) or optical metasurface on the waveguide without a series of lithography patterning steps used in a typical SRG patterning process.
[0013] FIGS. 1 to 3 are each schematic cross-sectional views of optical articles 100, 200, and 300. In some embodiments, the optical article 100 (respectively, 200, 300) includes a waveguide 190 and a structured film 150 (respectively, 250, 350). The structured film 150 (respectively, 250, 350) comprises: a polymer substrate 130; an etch stop layer 137 disposed on the polymer substrate 130; a structured layer 110 (respectively, 210, 310) including a plurality of fabricated structures 129 (respectively, 229, 329) disposed on a side of the etch stop layer 137 opposite to the polymer substrate 130; a planarization backfill layer 115 (respectively, 215, 315) disposed over the plurality of fabricated structures 129 (respectively, 229, 329) to define a substantially flat major surface 121 (respectively, 221, 321), the planarization backfill layer 115 (respectively, 215, 315) having a surface roughness Ra (see, for example, FIGS. 7A to 7C); and an adhesive layer 140 disposed on the substantially flat major surface 121 (respectively, 221, 321) of the planarization backfill layer 115 (respectively, 215, 315) for bonding the structured film to the waveguide 190. The difference in refractive index between the planarization backfill layer 115 (respectively, 215, 315) and the structured layer may be at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm or in other ranges described elsewhere herein. The adhesive layer 140 has an average thickness ta, where Ra < ta < (1 / 4)W1. The surface roughness Ra is the mean deviation surface roughness. The surface roughness Ra can be determined, for example, in accordance with the ISO 4287:1997 standard.
[0014] The main surfaces 121 (221, 321, respectively) can be considered substantially planar if any deviation from planarity on a transverse length scale (e.g., xy-plane) substantially greater than the average height t2 (e.g., 100 times t2 or 1000 times t2) is substantially less than the average height t2 (e.g., less than 20%, 10%, 5%, or 3% of the average height t2). In some embodiments, a substantially planarized surface has a planarization amount (P) greater than 50%, more preferably greater than 75%, and most preferably greater than 90%, given by P = (1 - (a1 / a2)) × 100%, where a1 is the relief height of the surface layer (e.g., the planarized backfill layer) and a2 is the feature height of the features covered by the surface layer, which are further disclosed in P. Chiniwalla, IEEE Trans.Adv.Packaging 24(1), 2001, 41.
[0015] The adhesive layer 140 can have an average thickness in a range suitable for a given application. In some embodiments, the average thickness ta of the layer 140 is less than 250 nm, or less than 200 nm, or less than 150 nm, or less than 100 nm, or less than 75 nm, or less than 50 nm, or less than 40 nm, or less than 30 nm. In some such embodiments, or in other embodiments, the average thickness ta is at least 5 nm, or at least 10 nm, or at least 15 nm. In some embodiments, the average thickness ta is selected to be less than 1 / 4 of the wavelength of interest. For example, for visible light, the average thickness may preferably be less than 100 nm or substantially less than 100 nm (e.g., less than 50 nm), while for near-infrared light, the average thickness may be, for example, up to 250 nm, or even greater if longer wavelengths are of interest. Having a thickness of less than 1 / 4 of the wavelength of interest allows, for example, the resulting structure formed on one or more unstructured layers to couple to evanescent waves in the waveguide. This makes it possible to use the resulting structure, for example, as a surface relief grating (SRG). When used herein, an SRG includes a case where the grating is embedded in a material having a different refractive index. This structure can be used, for example, for optical incoupling and / or outcoupling (to, for example, an augmented reality waveguide element). Alternatively or in addition, the resulting structure may be used, for example, as an optical distribution element, orthogonal pupil expander, or redirection element for exit pupil dilation in an augmented reality waveguide element. Exemplary examples of the use of SRGs in image-preserving waveguides can be found, for example, in International Publication No. 2019 / 195186 (Peroz et al.).
[0016] Layer 140 may be a polymer adhesive layer or a monomer adhesive layer, and / or an optically transparent adhesive layer. Suitable optically transparent adhesives include, for example, those available from Norland Products, Inc. (Cranbury, NJ). Other suitable adhesives include thermosetting materials, such as those available from Dow Chemical Company (Midland, MI) under the trade name CYCLOTENE. Still other suitable adhesives include thermally activated adhesives, such as those available from KRATON Polymers (Huston, TX) under the trade name KRATON. Suitable adhesive layers, including thin adhesive layers (for example, less than 50 nm thick), are described, for example, in U.S. Patents 7,521,727 (Khanarian et al.), 7,53,419 (Camras et al.), 6,709,883 (Yang et al.), and 6,682,950 (Yang et al.).
[0017] The polymer substrate 130 may be, for example, a polyethylene terephthalate (PET) film or a polycarbonate film, and may be dimensionally stabilized (e.g., heat-set). Other suitable materials for the polymer substrate 130 include, for example, other polyesters or copolyesters, polyurethanes, polymethyl methacrylates, polystyrenes, polyimides, polyethylene naphthalates, polypropylenes, and cyclic olefin copolymers. In some embodiments, the polymer substrate has a low birefringence (the maximum in-plane difference in refractive index at a first wavelength W1 multiplied by the thickness of the layer). In some embodiments, the retardance is less than 50 nm, or less than 10 nm, or less than 5 nm, or less than 1 nm.
[0018] Waveguide 190 may be, for example, a glass waveguide or a polymer (e.g., polymethyl methacrylate) waveguide. In some embodiments, waveguide 190 is, for example, an image-preserving waveguide (e.g., a waveguide such that when light containing an image (e.g., light from a display) propagates along the waveguide and is then extracted from the waveguide, the extracted light retains the image). In some embodiments, the waveguide combiner includes a waveguide and a structured film that defines an optical metasurface input and / or output coupler. Waveguide combiners are described, for example, in Kress, “Optical waveguide combiners for AR headsets: features and limitations”, Proc.SPIE 11062, Digital Optical Technologies 2019, 110620J (16 July 2019); doi:10.1117 / 12.2527680.
[0019] In some embodiments, the fabricated structure 129 has length and width in orthogonal directions (e.g., x and y directions), each direction being orthogonal to the thickness direction (z direction). In some embodiments, multiple fabricated structures 129 (229, 329, respectively) are multiple nanostructures or comprise multiple nanostructures. A nanostructure is a structure having at least two orthogonal dimensions (e.g., at least two of height, length, and width) in the range of about 1 nm to about 1000 nm. A fabricated structure is a structure intentionally fabricated with a predetermined geometric shape (e.g., predetermined length, width, and height). Some typical shapes of fabricated structures (e.g., fabricated nanostructures) include, but are not limited to, rectangular, triangular, and trapezoidal prisms, fins, cylindrical and truncated conical pillars, and other such shapes. In some embodiments, the fabricated structure has an average aspect ratio (height divided by length or width or maximum transverse dimension (orthogonal to height)) of, for example, at least 0.1, or at least 0.2, or at least 0.5, or at least 1, or at least 2, or at least 5, or at least 10. The fabricated structure can be arranged in a regular or irregular (e.g., a pseudo-random distribution where the structure appears randomly placed but is produced from an underlying deterministic process) pitch, orientation, and / or shape, which may depend on the functionality and manufacturability of the application.
[0020] In some embodiments, the planar backfill layers 115 (215, 315, respectively) include a residual layer 142 (242, 342, respectively) between the adhesive layer 140 and the structuring layer 110 (210, 320, respectively). The residual layer can be described as the portion of the backfill layer above the top of the structure (in the positive z-direction) of the structuring layer. In some embodiments, the ratio of the average (unweighted average) thickness t1 of the residual layer 142 to the average height t2 of the multiple fabricated structures is less than 1, or less than 0.5, or less than 0.3, or less than 0.25. In some embodiments, t1 / t2 is, for example, in the range of 0.001 to 0.5. In some embodiments, the maximum thickness (t1+t2) of the planar backfill layer is less than or equal to 2 times, or less than or equal to 1.5 times, or less than or equal to 1.3 times the average height t2 of the multiple fabricated structures. In some embodiments, the thickness of the residual layer 142 is less than 100 nm, less than 50 nm, less than 30 nm, less than 20 nm, or less than 10 nm.
[0021] A primary surface 121 (221, 321, respectively) can be considered substantially unstructured if any structures that may exist on its surface have a height substantially smaller than the average height t2 (e.g., less than 20%, 10%, 5%, or 3% of the average height t2). A primary surface 121 (221, 321, respectively) can be considered substantially planar if any deviation from planarity on a transverse length scale (e.g., the xy-plane) substantially larger than the average height t2 (e.g., 100 times t2 or 1000 times t2) is substantially smaller than the average height t2 (e.g., less than 20%, 10%, 5%, or 3% of the average height t2).
[0022] In some embodiments, the polymer substrate 130 is peelably attached to the etch-stop layer 137 and removed after the structured film is bonded to the waveguide (see, for example, Figures 4A to 6C). Alternatively, in some embodiments, after the structured film is bonded to the waveguide, the polymer substrate 130 is removed by dissolving the layer in acid. In either case, after the polymer substrate 130 has been removed, the etch-stop layer 137 may optionally be removed, for example, by reactive ion etching.
[0023] The two layers are detachably attached to each other if there is little or no damage to either layer and they can be separated from each other (for example, if the damage is small enough that it is not easily visible to the naked eye of a person with standard vision). The detachability of the first and second layers includes the case where a third layer is placed between the first and second layers and the third layer is adapted to facilitate the separation of the first and second layers (for example, the third layer may be adapted to split or separate from at least one of the first and second layers). The third layer may be adapted to facilitate the separation of the first and second layers only after activation of the third layer (for example, by irradiation, chemical activation, or thermal activation). For example, the third layer may be a dynamic separation layer. A dynamic separation layer is a layer that can be changed from a first state to at least a second state (for example, by activating the separation layer by irradiation), the layer providing higher adhesion to at least one adjacent layer in the first state and lower adhesion to at least one adjacent layer in the second state. For example, a dynamic separation layer may be a photo-induced stress-mode delamination layer (for example, a polymer layer that can be crosslinked or further crosslinked upon irradiation such that increased crosslinking generates stress that promotes delamination from adjacent layers), and / or a photothermal conversion (LTHC) layer.
[0024] The structured film can be configured such that the polymer substrate 130 adheres peelably to the etch-stop layer 137 by including a splitting layer between the polymer substrate 130 and the etch-stop layer 137, or by including a dynamic separation layer between the polymer substrate 130 and the etch-stop layer 137 and activating the dynamic separation layer (e.g., by irradiation). The splitting layer may be, for example, a static separation layer which may be a low surface energy layer, or a layer which is co-extruded with the polymer substrate 130 and weakly adhered to the polymer substrate 130 (e.g., separation layer 160' shown in Figure 5A in some embodiments), as generally described in, for example, U.S. Patent No. 9,415,561 (Lindquist et al.). The dynamic separation layer (e.g., LTHC layer) may include a plurality of sub-layers. Suitable dynamic separation layers include light-absorbing optical cavities defined by a thin (e.g., 10-30 nm) metal (e.g., aluminum, titanium, or chromium) layer separated by a polymer layer such as a carbon black nanocomposite, a thin light-absorbing metal (e.g., aluminum, titanium, or chromium) layer, and an acrylate layer. The dynamic separation layer can be formed from, for example, 3M Light-To-Heat Conversion Release Coating (LTHC) Ink (available from 3M Company (St. Paul, MN)). Other suitable dynamic separation layers include, for example, the LTHC layers described in U.S. Patent No. 7,977,864 (Bellmann et al.) and U.S. Patent No. 7,670,450 (Lamansky et al.).
[0025] In some embodiments, an additional layer 160 is placed between the etch-stop layer 137 and the polymer substrate 130. This is schematically shown in Figure 2 for a structured film 250, which may correspond to the structured film 150 except for the additional layer 160. Similarly, an additional layer 160 may be optionally included between the etch-stop layer 137 and the polymer substrate 130 of the structured film 350 in Figure 3. The additional layer 160 may be, for example, a low refractive index layer, or a splitting or separation layer. In some embodiments, the additional layer 160 is a dynamic separation layer (e.g., a photothermal conversion (LTHC) layer) placed between the etch-stop layer 137 and the polymer substrate 130. In some such embodiments, an additional polymer layer is placed between the etch-stop layer 137 and the layer 160 (see, for example, Figures 5B-5C). In some embodiments, a dynamic separation layer is included, and a low refractive index layer is included between the dynamic separation layer and the etch-stop layer 137. In some embodiments, the dynamic separation layer 160 is adapted to facilitate the separation of the polymer substrate and the etch-stop layer upon activation. Activation can be carried out, for example, by irradiation. Suitable radiation may include one or more wavelengths, including visible light, infrared light, or ultraviolet light, from a laser, lamp, or other radiation source. Useful radiation conditions are described, for example, in U.S. Patent No. 7,977,864 (Bellmann et al.).
[0026] Figures 4A to 5C schematically illustrate various methods for removing the polymer substrate 130. In Figures 4A to 4B, optical articles 100' and 100'' may correspond to, for example, optical article 100. Optical article 100' is configured such that the polymer substrate 130 is peelably attached to the etch-stop layer 137. In this embodiment and several other embodiments, there is a dividing interface between the polymer substrate 130 and the etch-stop layer 137, which may result from a surface treatment applied to the polymer substrate 130 before the etch-stop layer 137 is applied to the polymer substrate 130. Optical article 100'' is configured such that the etch-stop layer 137 is peelably attached to layers 110 and 115. In this embodiment and several other embodiments, there is a dividing interface between the etch-stop layer 137 and layers 110 and 115, which may result from a surface treatment applied to the etch-stop layer 137 before layer 110' (see Figure 7A) is placed on the etch-stop layer 137.
[0027] In Figures 5A to 5C, optical articles 200' and 200'' may correspond to, for example, optical article 200. In Figure 5A, the polymer substrate is peelably attached to a separation layer 160', which may be a static separation layer (e.g., co-extruded with the polymer substrate 130) or a dynamic separation layer. In this embodiment and several other embodiments, a separation interface exists between the polymer substrate 130 and the separation layer 160', which may result from co-extrusion of the polymer substrate 130 and the separation layer 160', as generally described, for example, in U.S. Patent No. 9,415,561 (Lindquist et al.). In Figure 5B, a dynamic separation layer 160'' is positioned between the polymer substrate 130 and the etch-stop layer 137. An additional substrate layer 132 is positioned between the dynamic separation layer 160'' and the etch-stop layer 137. The additional substrate layer 132 may be, for example, a low refractive index layer (having a refractive index in the range described elsewhere in this specification for low refractive index layers). The dynamic separation layer 160'' can be adapted to be peelably attached to the additional substrate layer 132 upon activation. In this embodiment and several other embodiments, upon activation, a separation interface exists between the dynamic separation layer 160'' and the additional substrate layer 132, as schematically shown in Figure 5C.
[0028] In some embodiments, the structured film 250 includes a polymer substrate 130, an etch-stop layer 137, a dynamic separation layer 160 disposed between the polymer substrate and the etch-stop layer, a structured layer 210 including a plurality of processed structures 229 disposed on the side of the etch-stop layer 137 opposite to the dynamic separation layer 160, a planar backfill layer 215 disposed on the plurality of processed structures 229, having a surface roughness Ra and defining a substantially flat main surface 221 of the planar backfill layer 215, and an adhesive layer 140 having an average thickness ta disposed on the substantially flat main surface 221 of the planar backfill layer 215. In some embodiments, the dynamic separation layer is adapted to facilitate separation of the polymer substrate 130 and the etch-stop layer 137 upon activation (e.g., by irradiation). For example, the dynamic separation layer 160 may be adapted to peel off from the etch stop layer 137 upon activation (e.g., by irradiation), or the dynamic separation layer 160 may be adapted to peel off from an additional layer (see, for example, Figure 5C) positioned between the etch stop layer 137 and the dynamic separation layer upon activation. In some embodiments, the refractive index difference between the planarizing backfill layer 215 and the structuring layer 210 is at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm or other ranges described elsewhere herein. In some embodiments, Ra <ta<(1 / 4)W1である。
[0029] In some embodiments, it is desirable to retain the polymer substrate 130 within the structured film. However, in some cases, it is desirable to have a layer having a lower refractive index than the polymer substrate 130 (e.g., air or a low refractive index cladding layer) adjacent to the etch-stop layer 137. Such a layer may be included to improve light confinement in the planarization backfill and structured layer. In some embodiments, the additional layer 160 is a low refractive index unstructured layer. Suitable low refractive index layers include, for example, nanoporous coatings, xerogels and aerogels, perfluoropolyethers, TEFLON, CYTOP materials, hexafluoropropylene oxide (HFPO), or fluorenol methacrylate. Useful low refractive index layers are described, for example, in U.S. Patent No. 8,808,811 (B. Kolb et al.). In some embodiments, the additional layer 160 is a fluoropolymer layer. The low refractive index layer may have a refractive index in the range of, for example, 1.1 to 1.45, or 1.15 to 1.4, or 1.2 to 1.35 for at least a first wavelength W1. In some embodiments, the low refractive index layer has a thickness of, for example, at least 50 nm, or at least 100 nm, or at least twice t2, or at least five times t2. In some such embodiments, or in other embodiments, the low refractive index layer has a thickness of, for example, 10 micrometers or less, or 5 micrometers or less. In some embodiments, the structured film 250 includes an unstructured layer 160 disposed between the etch-stop layer 137 and the polymer substrate 130, wherein the refractive index difference between the planarizing backfill layer 215 and the unstructured layer 160 is at least 0.2, or at least 0.25, with respect to at least a first wavelength W1.
[0030] In some embodiments, the processed structures 129 or 229 are inclined with respect to the etch-stop layer 137. Figure 3 is a schematic cross-sectional view of an article 300 having a structured film 350 having processed structures 329 inclined with respect to the etch-stop layer 137. In some embodiments, the structured film 350 includes a polymer substrate 130, an etch-stop layer 137 disposed on the polymer substrate 130, a structured layer 310 comprising a plurality of processed structures 329 disposed on the side of the etch-stop layer 137 opposite to the polymer substrate 130, wherein the processed structures 329 are inclined with respect to the etch-stop layer 137, a planar backfill layer 315 disposed on the plurality of processed structures 329 and defining a substantially flat main surface 321 having a surface roughness Ra, and an adhesive layer 140 having an average thickness ta disposed on the substantially flat main surface of the planar backfill layer. In some embodiments, the refractive index difference between the planarizing backfill layer 315 and the structured layer 310 is at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm or other ranges described elsewhere herein. In some embodiments, Ra <ta<(1 / 4)W1である。
[0031] A machined structure is inclined if a line passing through the center of the top (facing away from the etch-stop layer 137) and bottom (facing the etch-stop layer 137) of the structure forms an angle with respect to the etch-stop layer 137 within the range of 5 to 85 degrees. In the case of upper and lower facets, the center can be the centroid of the upper and lower parts of the structure. For example, a machined structure 329 can be said to be inclined if a line 341 passing through the centroid of facet 343 of the machined structure facing the etch-stop layer 137 and the centroid of the opposite facet 346 facing away from the etch-stop layer 137, or, in the case of a pointed machined structure, a line 341 passing through that point, forms an angle θ0 with respect to the etch-stop layer 137 within the range of 5 to 85 degrees. An inclined engineered structure may have opposing side walls that form angles θ1 and θ2 with respect to the etch-stop layer 137. Angles θ1 and θ2 are exterior angles (angles on the outside of the structure 329). The angles θ0 and / or θ1 may be, for example, at least 45 degrees or at least 50 degrees, and / or, for example, 85 degrees or less, or 80 degrees or less, or 75 degrees or less. In some embodiments, the angles θ0 and / or θ1 are, for example, in the range of 45 to 85 degrees or 50 to 80 degrees. The angle θ2 may be about 180 degrees minus θ1, or may be different. In some embodiments, the angle θ2 is, for example, in the range of 95 degrees to 135 degrees. In some embodiments, for at least a majority (or at least 60%, or at least 80%, or at least 90%) of the machined structures, each machined structure has a side wall defining an outer angle θ1 in the range of 45 to 85 degrees relative to the etch stop layer 137. The structured layer 310 may optionally include non-inclined structures in addition to the inclined machined structures 329. In some embodiments, at least 60%, or at least 80%, or at least 90% of all processed structures defined within the structured layer 310 are inclined relative to the etch stop layer 137.
[0032] In some embodiments, the polymer substrate 130 is removed after the structured film 150, 250, or 350 is bonded to the waveguide. Figures 6A to 6C are schematic cross-sectional views of exemplary articles that can be formed by bonding the structured film to the waveguide 190 and then removing the polymer substrate 130. Figure 6A schematically shows a structured film 351 that can be formed from structured film 350 by removing the polymer substrate 130. Similarly, structured films can be obtained from structured films 150 and 250 by removing the polymer substrate 130 and, optionally, an additional layer 160 of structured film 250.
[0033] In some embodiments, the optical article 301 (or 301', 301'' shown in Figures 6B to 6C) includes a waveguide 190 and a structured film 351 disposed on the main surface 191 of the waveguide 190. The structured film 351 includes an etch stop layer 137, a structured layer 310 disposed on the etch stop layer 137 and comprising a plurality of processed structures 329, the processed structures 329 being inclined with respect to the etch stop layer 137, a planar backfill layer 315 disposed on the plurality of processed structures 329 and having a surface roughness Ra, defining a substantially unstructured main surface 321 of the planar backfill layer 325, and an adhesive layer 140 disposed on the substantially unstructured main surface 321 of the planar backfill layer 315, the adhesive layer 140 bonding the structured film 351 to the main surface 191 of the waveguide 190 and having an average thickness ta. In some embodiments, the refractive index difference between the planarizing backfill layer 315 and the structured layer 310 is at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm or other ranges described elsewhere herein. In some embodiments, Ra <ta<(1 / 4)W1である。
[0034] In some embodiments, the structured layers 110, 210, or 310 include a plurality of sublayers. For example, the structured layers can be formed by etching an unstructured layer, as further described elsewhere in this specification, and the unstructured layers can include a stack of sublayers such that the resulting fabricated structure has sublayers. Figure 6B is a schematic cross-sectional view of an article 301' including a structured film 351' bonded to a waveguide 190 according to some embodiments. The structured film 351' includes structured layers 310a, 310b, with a first sublayer 310a positioned on a second sublayer 310b.
[0035] In some embodiments, the multiple processed structures 129, 229, or 329 include structures having at least two different heights. For example, structures having at least two different heights can be formed by etching through an etch-resist layer having structures having at least two different heights. For example, referring to Figures 7A to 7C, the mask layer 131 can be omitted, and the etch-resist layers 125, 225, or 325 can be multi-level resist layers, and the pattern transfer process can provide multi-level patterns to previously unstructured layers 110', 210', or 310', respectively. Figure 6C is a schematic cross-sectional view of an article 301'' including a structured film 351'' bonded to a waveguide 190 according to some embodiments. The structured film 351'' includes a structured layer 310'' which includes structures 329a and 329b having different heights. In some embodiments, the structured layer 310'' includes multiple sublayers, where the higher structure 329a includes more sublayers than the shorter sublayer 329b. For example, the upper sublayer of structure 329b, rather than structure 329a, may be removed by etching.
[0036] Figures 7A to 7C schematically illustrate the processes for producing structured films 150, 250, and 350, respectively. The input film (e.g., a roll of film) includes a polymer substrate 130, an etch stop layer 137 disposed on the polymer substrate 130, unstructured layers 110' (210', 310', respectively) disposed on the unstructured layers, and a mask layer 131 disposed on the unstructured layers. In step A (A', A'', respectively), etch resist layers 125 (225, 325, respectively) are disposed on the mask layer 131. The etch resist layers may be formed by replication from tools as further described elsewhere in this specification. The mask layer 131 may be optionally omitted (e.g., if a relatively low aspect ratio structure is desired, or if a multi-level structured layer is desired), in which case the etch resist layer can function as an etch mask for etching to the unstructured layers. In step B (B' and B'', respectively), breakthrough etching is performed, followed by etching of the mask layer 131. Reactive ion etching (RIE) can be used for either etching step. In step C (C' and C'', respectively), etching continues until the etch-resist layer 125 (225 and 325, respectively) is removed. In step D (D' and D'', respectively), the etching conditions are changed (e.g., to oxygen RIE) and the unstructured layer 110' (210' and 310', respectively) is etched until the vias reach the etch-stop layer 137. In step D' in Figure 7C, directional etching (e.g., directional RIE) is performed at a tilt angle to form a gradient structure. Forming a gradient structure by etching at a tilt angle is described, for example, in U.S. Patent No. 10,670,862 (Vallius et al.) and U.S. Patent Application Publication No. 2016 / 0033784 (Levola et al.). In step E (E', E'', respectively), etching is continued until the mask layer 131 is removed. The structured layers 110 (210, 310, respectively), in combination with the exposed portion of the mask layer, can define the main surfaces 111 (211, 311, respectively) facing away from the polymer substrate 130.In process F (F', F'', respectively), the vias are backfilled with a planar backfill (e.g., by atomic layer deposition). The planar backfill may have a main surface 116 (216, 316, respectively) facing and substantially conforming to the main surface 111 (211, 311, respectively) (e.g., deviating from conformation by only 20% or less or 10% or less of t2). The planar backfill has a desired roughness Ra, with troughs or valleys corresponding to the underlying vias. 0 It may have a roughness greater than Ra. In some embodiments, the surface roughness is Ra <Ra 0 To reduce this, process G (G', G'', respectively) is performed. In some embodiments, Ra is less than about 30 nm, or less than about 20 nm, or less than about 10 nm, or less than about 5 nm, or less than about 2 nm, or less than about 1 nm, or less than about 0.5 nm. In some such embodiments, or in other embodiments, Ra 0 -Ra is greater than 10 nm, greater than 20 nm, greater than 40 nm, or greater than 80 nm. In some embodiments, smoothing of rough surfaces is carried out by chemical mechanical planarization (e.g., using an abrasive together with a corrosive chemical slurry), as generally described in, for example, U.S. Patent No. 6,623,355 (McClain et al.) and U.S. Patent No. 9,200,180 (Banerjee et al.). In some embodiments, smoothing of rough surfaces is carried out by a combination of mechanical polishing and dry etching, as generally described in, for example, U.S. Patent No. 6,858,537 (Brewer). In step H (H, H', respectively), an adhesive layer 140 is applied to the planarized backfill layer 115 (215, 315, respectively). For some applications (e.g., visible optics applications), a surface roughness of less than 5 nm, less than 2 nm, less than 1 nm, or less than 0.5 nm may be preferred. In some embodiments, a removable liner is applied to the adhesive layer 140 before covering and / or storing the structured film with a sheet.
[0037] The etching process in Figures 7A to 7C may also be a plasma etching process. When high aspect ratio structures are desired, ion-assisted plasma treatment is conveniently used. Methods for achieving anisotropic etching include reactive ion etching (RIE), high-density ion source treatment, or a combination of high-density ion source treatment and RIE. High-density plasma can be generated by inductive radio frequency or microwave coupling, or by a helicon ion source. Linear high-density plasma sources are particularly advantageous for forming high aspect ratio features. By combining high-density plasma with RIE, ion generation (by the high-density plasma) can be decoupled from ion energy (by the RIE bias voltage).
[0038] The RIE method involves etching the portion of the main surface not protected by a masking layer to form a structure (e.g., a nanostructure) on the substrate. In some embodiments, this method can be performed using a continuous roll-to-roll process referred to as "cylindrical reactive ion etching" (cylindrical RIE). Cylindrical RIE utilizes a rotating cylindrical electrode to provide anisotropically etched nanostructures on the surface of a substrate of an article. Generally, cylindrical RIE can be described as follows: A rotatable cylindrical electrode ("drum electrode") powered by radio frequency coupling and a grounded counter electrode are provided inside a vacuum vessel. The counter electrode may include the vacuum vessel itself. Etchant gas is supplied into the vacuum vessel, and a plasma is ignited and maintained between the drum electrode and the grounded counter electrode.
[0039] Next, a continuous substrate containing a patterned masking layer can be wrapped around the drum, and the substrate can be etched in the direction normal to the plane of the substrate. By controlling the exposure time of the substrate, a predetermined etching depth can be obtained for the resulting nanostructure. This process can be carried out at an operating pressure of about 1 to 10 milliliters. A cylindrical RIE is described, for example, in U.S. Patent No. 8,460,568 (David et al.).
[0040] When multiple materials are present, the chemicals in the plasma environment can be controlled to achieve etching selectivity. Oxygen, and mixtures of oxygen and fluorinated gases, are used to etch carbon-containing materials such as polymers, diamond-like carbon, and diamond. The concentration of fluorine in the plasma can be selected to optimize etching rate and selectivity. Typically, using small amounts of fluorinated gas can dramatically increase the etching rate of hydrocarbon polymers by as much as 300%.
[0041] Silicate materials (silicon dioxide, SiO₂) x To etch materials such as diamond-like glass, silicon nitride, silicon carbide, silicon oxycarbide, polysiloxane, and silsesquioxane (SSQ) resins, mixtures of fluorocarbons, such as CF4, C2F6, and / or C3F8, are used in combination with oxygen. The etching selectivity of siliceous materials and hydrocarbon polymers can be finely tuned by obtaining the etching profiles of these materials as a function of the F / O atomic ratio in the plasma feed gas mixture. Oxygen-rich conditions provide excellent selectivity for etching hydrocarbon polymers and diamond-like carbon (DLC) while using siliceous materials as masking layers. In contrast, fluorine-rich conditions provide excellent selectivity for etching siliceous materials while using hydrocarbon polymer-based masking materials.
[0042] Fluorinated plasma chemicals can be used to etch other masking materials, such as tungsten, whose fluorides are volatile. Chlorine-containing gas mixtures can be used to etch materials whose chlorides are volatile, such as aluminum and titanium. Oxides, nitrides, and carbides of these etchable metals can also be etched using chlorine-based chemicals. Silicon nitride, aluminum nitride, and titanium oxide are high refractive index materials that can be etched with chlorine chemicals.
[0043] Various layers (e.g., mask layer 131, etch-stop layer 137, layers 110', 210', 310', backfill layers 115, 215, 315, or adhesive layer 140) can be deposited using various deposition methods, taking into account the type of material and layer thickness. Suitable deposition methods include, for example, chemical vapor deposition (CVD), sputter coating, physical vapor deposition (PVD), atomic layer deposition (ALD), or combinations thereof. Thin layers or films can be coated on flat or structured surfaces using coating methods known in the art, such as slot die coating, slide coating, curtain coating, knife coating, blade coating, dip coating, and spin coating. Slot die coating equipment is described, for example, in U.S. Patent No. 5,639,305 (Brown et al.) and No. 7,591,903 (Maier et al.). Spin coaters are described, for example, in U.S. Patent No. 6,033,728 (Kikuchi et al.).
[0044] The planar backfill layer (e.g., 115, 215, 315) can be formed from any suitable material. Preferably, the planar backfill layer is formed from a material having a refractive index at least 0.2, at least 0.25, at least 0.3, or at least 0.35 higher than the refractive index of the structured layer (e.g., 115, 215, 315) for at least a first wavelength W1. Suitable materials for the backfill layer include, for example, zirconia or titania-filled acrylate resins which may be deposited by coating; metal oxides, nitrides, and oxynitrides, for example, including oxides, nitrides, and oxynitrides of Si, Ti, Zr, Hf, Nb, Ta, or Ce which may be vapor-deposited; and parylene which may be applied by coating. Since silicon is a metalloid, silicon oxides, silicon nitrides, and silicon oxynitrides are considered to be metal oxides, metal nitrides, and metal oxynitrides, respectively. In some cases, titania (TiO2) may be preferred for optical applications involving visible light, and silicon or other metal oxides may be used for applications involving near-infrared light. The structured layer can be formed from any of the low refractive index materials described elsewhere in this specification. The structured layer may be, for example, a fluoropolymer layer. In some embodiments, the structured layer comprises a fluoropolymer, and the planarizing backfill layer comprises a metal oxide, nitride, or oxynitride. In some embodiments, for at least a first wavelength W1, the structured layer has a refractive index of 1.4 or less, and the planarizing backfill layer has a refractive index of at least 1.65 or at least 1.7.
[0045] In some embodiments, the target wavelength is in the visible or near-infrared range. Therefore, the first wavelength W1 may be in the range of 400 nm to 2500 nm. In some embodiments, the visible wavelength is the primary target. Therefore, the first wavelength W1 may be in the range of 400 nm to 700 nm. In some embodiments, the near-infrared wavelength is the primary target. Therefore, the first wavelength W1 may be, for example, in the range of 700 nm to 2500 nm, or 800 nm to 2000 nm. Some specific near-infrared wavelengths that may be targeted depending on the application include, for example, 850 nm, 905 nm, 940 nm, 1060 nm, 1330 nm, and 1550 nm.
[0046] In some embodiments, the etch-resist layer 125, 225, or 325 comprises a silicone-containing polymer. In some embodiments, the etch-resist layer comprises a siloxane, silicone, or silsesquioxane. In some embodiments, the etch-resist layer comprises a crosslinked acrylate. A suitable etch-resist layer is described, for example, in U.S. Patent No. 5,811,183 (Shaw et al.). The etch-resist layer may have a total thickness in the range of, for example, 50 nm to 500 nm.
[0047] The etch-resist layers 125, 225, or 325 can be formed using different pattern printing, transfer, tiling, copying, or replication techniques, which may include, for example, a master mold fabricated by photolithography, electron beam lithography, grayscale lithography, two-photon lithography, nanoimprint lithography, or microcontact printing (μCP). Replication techniques (e.g., nanoreplication) may include, for example, casting and curing a resin onto a structured surface of a tool. Suitable casting and curing methods, as well as resins suitable for use in such methods, are described, for example, in U.S. Patent No. 5,175,030 (Lu et al.), No. 5,183,597 (Lu), and U.S. Patent Application Publication No. 2012 / 0064296 (Walker, Jr. et al.). Other useful methods and / or materials for forming an etch-resist layer are described, for example, in U.S. Patent No. 8,658,248 (Anderson et al.), No. 5,811,183 (Shaw et al.), and No. 6,045,864 (Lyons et al.). Structured tools may be fabricated using any preferred fabrication method, such as photolithography or electron beam lithography, to prepare a tooling master, a metal copy thereof, a polymer copy of either the tooling master or its metal copy, a polymer copy of such a polymer copy, a directly written tool or any copy thereof, a copy of a structured liner or any copy thereof. Preferred manufacturing methods are described, for example, in International Publication No. 2009 / 002637 (Zhang et al.), and U.S. Patent Application Publications No. 2007 / 0065636 (Merrill et al.) and No. 2014 / 0193612 (Yu et al.), and U.S. Patent No. 8,460,568 (David et al.). The tools may be manufactured, for example, by diamond turning. Exemplary diamond turning systems and methods are described, for example, in U.S. Patents No. 7,350,442 (Ehnes et al.), No. 7,328,638 (Gardiner et al.), and No. 6,322,236 (Campbell et al.).An example of patterning a subwavelength grating can be found in Chun-Wei Liu, Jiwang Yan, Shih-Chieh Lin, "Diamond turning of high-precision roll-to-roll imprinting molds for fabricating subwavelength gratings," Opt. Eng. 55(6), 064105 (2016), doi:10.1117 / 1.OE.55.6.064105.).
[0048] The mask layer 131 can be made of any material that has suitable etch selectivity with respect to the layer 110', 210', or 310'. In some embodiments, the mask layer 131 is or includes a metal or a silicon-containing metal oxide. Examples include chromium (Cr), aluminum (Al), copper (Cu), titanium (Ti), tungsten (W), germanium (Ge), iridium (Ir), platinum (Pt), ruthenium (Ru), osmium (Os), rhenium (Re), alloys thereof, or silicon-containing oxides thereof. In some embodiments, the mask layer 131 is SiO2, Si x O y N z (x=1, y=1~2, z=0~1), or Si x Al y O z (x=1, y=0~1, z=1~2). Useful oxides are described, for example, in U.S. Patent Application Publication No. 2015 / 0214405 (Nachtigal et al.). Useful materials include, for example, titanium nitride (TiN), aluminum oxide (Al2O3), aluminum and chromium (Al / Cr) metal alloys, Si x C y H z (x=1, y=1~4, z=1~4), or Si x C y N z H n (x=1, y=1~4, z=0~1, n=1~4), Si x N y (x=1, y=0~1), SiOx (x=1~2), SiH x (x=1~4) are examples. Other suitable materials include, for example, diamond-like glass as described in U.S. Patent No. 8,034,452 (Padiyath et al.). The mask layer 131 may also be called a hard mask layer.
[0049] The etch stop layer 137 can be made from any material having suitable etching selectivity for layers 110', 210', or 310'. In some embodiments, the etch stop layer 137 may be a metal (e.g., Cr, Al, Ti, Zr, Ta, Hf, Nb, Ce, or an alloy thereof), a metal oxide (e.g., Al2O3 or Si x Al y O z (For example, x=1, y=0~1, z=1~2) an oxide of any of these metals; or Si x O y N z (For example, x=1, y=1~2, z=0~1), or metal nitrides (for example, nitrides of any of these metals, or Si x O y Nz), or including them. In some embodiments, the etch stop layer 137 is, for example, indium tin oxide, tin oxide, or alumina (Al2O3), or includes them. Useful materials include, for example, Si x C y H z (For example, x=1, y=1~4, z=1~4), Si x C y N z H n (For example, x=1, y=1~4, z=0~1, n=1~4), Si x N y (For example, x=1, y=0~1), SiO x (For example, x=1~2), Si x O y N z (For example, x=1, y=1~2, z=0~1), or SiH xExamples include x=1 to 4. Other suitable materials include, for example, diamond-like glass. In some embodiments, the etch stop layer 137 is optically transparent, which can be understood as meaning that the etch stop layer has an average light transmittance of at least 60% for substantially perpendicular incident light in the wavelength range of 400 nm to 700 nm.
[0050] The average thickness of the mask layer 131 and / or the etch stop layer 137 may be in the range of, for example, about 1 nm to about 200 nm, or about 2 nm to about 50 nm, or about 2.5 nm to about 10 nm. The mask layer 131 may have an average thickness of, for example, less than 50 nm, or less than 25 nm, and / or greater than 5 nm. The etch stop layer 137 may have an average thickness of, for example, less than 25 nm, and / or greater than 2 nm.
[0051] The etch stop layer 137 can be selected from a material having a desired light transmittance at the target wavelength for a suitable thickness. In some embodiments, the etch stop layer 137 has a light transmittance of at least 60%, or at least 70%, for substantially perpendicularly incident light for at least a first wavelength W1. In some embodiments, the structured layer is formed from one or more unstructured layers (for example, any of layers 110', 210', and 310' may be a single layer or may include multiple sublayers). In some embodiments, one or more unstructured layers have a light transmittance of at least 60%, or at least 70%, for substantially perpendicularly incident light for at least a first wavelength W1.
[0052] Figure 8 is a schematic cross-sectional view showing one or more unstructured layers 777, incident light 773, and transmitted light 774. The incident light 773 is incident substantially perpendicularly (e.g., within 20 degrees, 10 degrees, or 5 degrees from the perpendicular) to one or more unstructured layers 777, which may be a single layer (e.g., corresponding to any one of layers 131, 137, 110', 210', or 310', or an unstructured layer formed from the material of any of layers 115, 215, or 315 and having a thickness of t1+t2) or a stack of layers (e.g., corresponding to layers 131, 137, and 110', 210', or 310'). The incident light 773 is schematically represented as having a wavelength λ in the range λ1 to λ2. The range λ1 to λ2 may be, for example, 400 nm to 2500 nm, or 400 nm to 700 nm, or 700 nm to 2500 nm. The wavelength λ may be a single wavelength (e.g., a first wavelength W1) or a wavelength range (e.g., 400 nm to 700 nm). In some embodiments, one or more unstructured layers 777 may have a light transmittance for substantially perpendicularly incident light of at least 60%, or at least 70%, or at least 80% for at least a first wavelength W1. In some embodiments, one or more unstructured layers 777 may have an average light transmittance (unweighted average of light transmittance over a given wavelength range) for substantially perpendicularly incident light of at least 50%, or at least 60%, or at least 70%, or at least 80% for the wavelength range of 400 nm to 2500 nm or 400 nm to 700 nm.
[0053] In some embodiments, a wafer master (e.g., a semiconductor wafer substrate, typically silicon or silicon dioxide on silicon, with nanopatterns etched onto its surface) is used when fabricating structured films that can be used to apply nanostructures to waveguides. The wafer master can be generated using standard mastering techniques, such as electron beam lithography or immersion lithography. The master pattern can then be copied into a series of process intermediates, which may include polymer copies (imprint resist on a wafer), polymer stamps (imprint resist on a polymer), tiled polymer mothers (tiled wafer patterns on a large glass substrate), electroformed nickel shims, and welded nickel sleeves. The welded nickel sleeves can be used, for example, in a continuous casting and curing (e.g., nanoreplication) process to manufacture structured films. The wafer pattern may be used in a single-element layout or may be combined with other patterns from other wafers to form a composite layout. Each element may be transported through the process as a single element and then combined during the lamination process, or, for example, all but one may be synthesized in a tiled polymer mother process and produced as a single synthesized film roll. The remaining element may be laminated, for example, on the opposite side of the waveguide and not synthesized with the other elements.
[0054] In some embodiments, a synthesis method is used in which individual nanopatterns are synthesized in an intermediate such as a tiled polymer mother, which is used to fabricate synthetic shims, sleeves, and films. A liner on the structured film may be laser kiss-cut to expose the adhesive in the structured region of the film (e.g., the optical coupler region), and the entire film can be laminated to a waveguide. This path is useful, for example, when all couplers are on the same side of the waveguide. In some embodiments, a single-element method is used in which individual nanopatterns are transported from the wafer to the film as single elements. In this case, the number of films may be the same as the number of wafers. Elements from each film may be prepared as described elsewhere in this specification and synthesized during lamination. In some embodiments, a combination of the synthesis method and the single-element method is used, in which the synthesis method applies some, rather than all, of the individual nanopatterns to one side of the waveguide, and in the single-element method, the remaining individual nanopatterns are applied to the opposite side of the waveguide.
[0055] The laminated waveguide can be laser-cut, for example, around the bonded coupling region to remove weeds. In some embodiments, the resulting laminate represents the finished optical article. In other embodiments, the laminate is processed in a further separate process to produce the final optical article. In some embodiments, the waveguide may be fragmented into, for example, multiple near-to-eye (NTE) augmented reality (AR) waveguides.
[0056] Examples Structured film articles were prepared using nano-replication, solvent coating, plasma etching, vacuum thin-film deposition, and lamination methods. The resulting structures are optical articles having a nanostructured optical functional layer (titanium dioxide) bonded to a receptor substrate such as a polished glass sheet.
[0057] These examples are for illustrative purposes only and are not intended to limit the scope of the invention. All parts, percentages, ratios, etc., in the examples and elsewhere in this specification are by weight unless otherwise indicated. The solvents and other reagents used were obtained from Sigma-Aldrich Chemical Company (St. Louis, Missouri) unless otherwise indicated. [Table 1]
[0058] Preparation example Preparation example 1 (PE1) First, an acrylate solution was prepared by adding 75 wt% PHOTOMER 6210 to 25 wt% SR238 and 0.5% TPO to form a first acrylate mixture. A second acrylate mixture was obtained by manually mixing 93 wt% of the first acrylate mixture with 7 wt% HFPO-UA. Then, an acrylate solution was formed by manually combining 14 wt% of the second acrylate mixture with 43 wt% PGME and 43 wt% MEK.
[0059] Preparation example 2 (PE2) An adhesion promoter solution was prepared by adding 0.3 wt% of compound 01 to 99.7 wt% of MEK and 0.003 wt% of TPO-L.
[0060] Preparation example 3 (resin D) An acrylate resin mixture prepared by mixing PHOTOMER 6210, SR238, SR351, and TPO in a weight ratio of 60 / 20 / 20 / 0.5.
[0061] Preparation example 4 (base material 01) A substrate having a peelable layer is produced by adding a second evaporator and a curing system positioned between a plasma pretreatment station and a first sputtering system, and by coating an evaporator described in U.S. Patent No. 8,658,248 (Anderson and Ramos) onto an ST505 film on a roll-to-roll vacuum coater similar to the coater described in U.S. Patent Application Publication No. 20100316852 (Condo et al.).
[0062] ST505 films for coating were prepared by treating the ST505 film with nitrogen plasma to improve adhesion to the metal layer. The film was treated with nitrogen plasma operating at 120 W using a titanium cathode at a web speed of 9.8 meters / min, while the back side of the film was kept in contact with a coating drum cooled to 0°C.
[0063] A 90% / 10% Si / Al stripping layer is deposited on the prepared ST505 substrate in line with the previous plasma treatment step. A 7nm thick layer of SiAl alloy is deposited on the substrate using a conventional AC sputtering process operating at 16kW power with Ar gas. The SiAl-coated PET substrate is then unwound.
[0064] An acrylate transfer layer SR833 containing less than 1% by weight of compound 1 is applied to the release layer by ultrasonic atomization and flash evaporation. The liquid monomer flow rate to the evaporator is 0.67 mL / min. The nitrogen gas flow rate is 100 standard cubic centimeters per minute (SCCM), and the evaporator temperature is set to 500°F (260°C). The process drum temperature is 14°F (-10°C). Subsequently, this monomer coating is cured immediately downstream by an electron beam curing gun operating at 7.0 kV and 10.0 mA to obtain an acrylate layer with a thickness of 180 nm.
[0065] Preparation example 5 (FPI) Pentafluorobenzoylmethoxyphenylphosphine oxide is synthesized under vacuum and yellow ambient light in a flame-dried three-necked round-bottom flask equipped with a thermocouple, magnetic stirring rod, and liquid addition funnel. Dry nitrogen is packed into the round-bottom flask, and 9.92 g (58.3 mmol) of dimethoxyphenylphosphine is added.
[0066] Add 13.44 g (58.3 mmol) of pentafluorobenzoyl chloride to a liquid addition funnel and connect the reaction apparatus to a vacuum. Cool the round-bottom flask in a dry ice / isopropanol bath and add the pentafluorobenzoyl chloride dropwise at a rate sufficient to maintain the reaction temperature below 15°C. During this time, the reaction mixture will become a bright yellow-orange oil with a pourable viscosity. Collect the pentafluorobenzoyl methoxyphenylphosphine oxide in quantitative yield and store in a brown glass jar.
[0067] Preparation example 6 (HFPO-FCA) In a 500 mL round-bottom flask equipped with a stirring bar and septum, 120 g (0.0663 mol, 1810 MW) of HFPO oligomer acrylate (Mn = 2000 g / mol, prepared according to the synthesis method generally described in U.S. Patent No. 9,718,961 (Corveleyn et al.)) and 120 g of 1,1,1-trifluorotoluene, pre-dried as a 50% solid solution on a 4 angstrom molecular sieve in a bottle with a septum cap, are added under nitrogen gas. Next, 1.42 g (1.46 mL, 0.007366 mol, 193.32 number-average molecular weight) of N-methyl-3-aminopropyltrimethoxysilane is added, and the reaction mixture is stirred at room temperature (RT) for 2 hours. At this point, aliquots are evaluated by 1H Fourier transform nuclear magnetic resonance spectroscopy (FT-NMR) in D8-tetrahydrofuran / Freon 113. Next, the reaction mixture is concentrated in a rotary evaporator at 2 Torre and 57°C for approximately 30 minutes, and then bottled under nitrogen.
[0068] Virtual Example 1 Optical articles are prepared using the following process.
[0069] Step 1. Nano-replicating the template layer. A nanostructured tooling film is prepared by die-coating resin D onto a polycarbonate film. The coated film is pressed onto a nanostructured nickel surface attached to a steel roller controlled at 60°C using a rubber-coated roller at a speed of 15.2 meters / minute. The nanostructured nickel surface consists of 12 6mm × 6mm patterned regions with features ranging in size from 75nm to 500nm. The patterned regions consist of a multi-pitch pattern with pitches of 150nm, 200nm, and 250nm, and feature widths of half the pitch (75nm, 100nm, and 125nm).
[0070] The features are arranged in a square grid such that the pitch varies along both axes, resulting in a repeating cell of 9 units, each containing rectangles for all combinations of the widths described above. In this repeating cell, the 150nm pitch section has 27 features, the 200nm pitch section has 20 features, and the 250nm pitch section has 16 features. The feature height is approximately 200nm, and the sidewall angle is approximately 4 degrees.
[0071] The coating thickness of resin D on the film is sufficient to completely wet the nickel surface and form rolling beads of resin when the coated film is pressed onto the nanostructured nickel surface. The film is exposed to radiation from two Fusion UV lamp systems (trademarked "F600" from Fusion UV Systems, Gaithersburg, MD), both equipped with D valves operating at 142 W / cm, while in contact with the nanostructured nickel surface. After peeling the film from the nanostructured nickel surface, the nanostructured side of the film is exposed again to radiation from the Fusion UV lamp systems.
[0072] Step 2: Peeling process A silicon-containing release film layer assembled by the method described in U.S. Patent No. 6,696,157 (David et al.) and No. 8,664,323 (Iyer et al.), and U.S. Patent Application Publication No. 2013 / 0229378 (Iyer et al.) is applied to a nanostructured tooling film in a parallel-plate capacitively coupled plasma reactor. The chamber is 1.7 m 2 (18.3ft 2 It has a central cylindrical powered electrode with a surface area of ).
[0073] The nanostructured tooling film is placed on a powered electrode, and the reactor chamber is pumped down to a base pressure of less than 1.3 Pa (2 milliliters). O2 gas is introduced into the chamber at a flow rate of 1000 SCCM. The process is carried out using plasma-enhanced CVD by coupling radio frequency (RF) power to the reactor at a frequency of 13.56 MHz and an applied power of 2000 watts. The processing time is controlled by moving the nanostructured tooling film through the reaction area at a speed of 9.1 meters / min (30 feet / min), resulting in an exposure time of approximately 10 seconds. After deposition is complete, the RF power is switched off and the gas is evacuated from the reactor.
[0074] Following the first treatment, a second plasma treatment is performed in the same reactor without returning the chamber to atmospheric pressure. HMDSO gas is flowed into the chamber at approximately 1750 SCCM to achieve a pressure of 9 milliliters. Subsequently, 13.56 MHz RF power is coupled to the reactor with an applied power of 1000 W. The film is then transported through the reaction area at a speed of 9.1 meters / min (30 feet / min), resulting in an exposure time of approximately 10 seconds. At the end of this treatment time, the RF power and gas supply are stopped, the chamber is returned to atmospheric pressure, and the delaminated nanostructured tooling film is removed from the chamber.
[0075] Step 3: Pattern transfer film A pattern transfer film is prepared by depositing an etch stop layer and a pattern transfer layer onto an 11.5-inch wide ST505 PET substrate film by reactive sputtering and organic vapor deposition in a system similar to those described in U.S. Patent No. 5,440,446 (Shaw et al.) and No. 7,018,713 (Padiyath et al.). The substrate film is coated in a roll-to-tall (R2R) format. In a first pass through this system, the substrate film is treated with nitrogen plasma from a non-equilibrium dc magnetron cathode with a titanium target at a power of 50 W and a nitrogen flow rate of 100 SCCM.
[0076] Immediately after plasma treatment of the film, approximately 12 nm of SiAlO x The base etch stop layer is sputter-deposited onto a plasma-treated surface. A pair of rotating cathodes are controlled using a 40kHz AC power supply. Each cathode houses a 90% / 10% Si / Al sputtering target (obtained from Soleras Advanced Coatings ETS (Biddeford, ME)). During sputter deposition, a voltage signal from the power supply is used as input to a proportional-integral-derivative control loop to maintain a predetermined oxygen flow to each cathode. The sputtering conditions are 16kW AC power, 9.75 m / min (32 ft / min) line speed, and a gas mixture containing 350 SCCM of argon and 223 SCCM of oxygen at a sputtering pressure of 2.6 milliliters.
[0077] Next, using the organic vapor deposition system and method described in U.S. Patent No. 8,658,248 (Anderson et al.), SiAlO xThe surface is coated with a layer of 90% HFPO-FCA / 9% HFPO / 1% FPI (wt%) to a thickness of approximately 100 nm. The line speed is maintained at 3.81 m / min (12.5 ft / min) while the back of the film is in contact with a coating drum cooled to 0°C. Before coating, the monomer is degassed under vacuum to a pressure of 20 milliliters. This liquid is pumped to an ultrasonic atomizer at a liquid flow rate of 1.0 mL / min using a syringe pump, and nitrogen gas at a flow rate of 10 SCCM is supplied to the atomizer. The liquid is flash-deposited at 250°C, and SiAlO x It is supplied to the surface. The vapor stream is condensed on the film surface and cured by UV irradiation using a low-pressure mercury arc lamp.
[0078] Using the same method as described for the base etch stop layer, approximately 12 nm thick SiAlO was applied to the HFPO-FCA / HFPO / FPI surface. x The upper etch stop layer is deposited.
[0079] Step 4: Adhesion promoter A PE2 adhesion promoter solution was coated onto the pattern transfer film prepared in step 3 using slot die coating. A Harvard syringe pump was used at 3 SCCM to pump the solution through the slot die onto the film moving at a speed of 6 meters / minute. The film was then moved into a 65°C oven for 1.5 minutes, cured using a Fusion H valve, and subsequently wound up.
[0080] Step 5: Resist Transfer The nanostructured tooling film, peeled from step 2, is slot-die coated with acrylate solution PE1 at a rate of 3 meters / min. The solution is coated in a 10.16 cm width and pumped at a rate of 1.05 SCCM using a Harvard syringe pump. The coating is partially cured at a distance of 1.5 meters from the solution application area using a 405 nm UV-LED system powered at 40 volts and 0.2 amps. The coating has a UV-visible emission of approximately 0.005 W / cm².2 It receives irradiance from.
[0081] Next, the film is dried under ambient conditions for 3 minutes and then placed in the nip. In the nip, the pattern transfer film from step 4 (along with the base etch stop, transfer layer, top etch stop, and adhesion promoter) is laminated with the PE 1 coated, release-treated template film.
[0082] The nip consists of a 90-duro hardness rubber roll and a steel roll set to 37°C. The nip is engaged by two Bimba air cylinders pressed at 0.28 MPa.
[0083] The coated PE1 acrylate solution is cured using a Fusion H valve, and the first acrylate mixture is separated from the peeled template film, leaving the cured PE1 coating on the transfer film over the entire 6mm x 6mm patterned area. The web tension is set to approximately 0.0057 N / m.
[0084] Step 6: Etching of the transfer layer An etched pattern transfer film is prepared by etching the patterned transfer film from step 5 according to a method for reactive ion etching.
[0085] Reactive ion etching is performed on the patterned film in the same reactor chamber used to deposit the release layer in step 2. After placing the patterned transfer film on a powered electrode, the reactor chamber is pumped down to a base pressure of less than 1.3 Pa (1 milliliter). A mixture of PF-5060 and oxygen gas is flowed into the chamber at flow rates of 100 SCCM and 50 SCCM, respectively. Subsequently, 13.56 MHz RF power is coupled to the reactor with an applied power of 7500 W. The film is then transported through the reaction area at a speed of 1.2 meters / min (4 feet / min) to transfer the pattern to the upper etch-stop layer, resulting in an exposure time of approximately 75 seconds.
[0086] Once the first etching process is complete, the RF power is switched off and the gas is discharged from the reactor. Following the first etching, a second reactive ion etching process is performed in the same reactor without returning the chamber to atmospheric pressure. Oxygen is flowed into the chamber at a flow rate of 275 SCCM. Subsequently, 13.56 MHz RF power is coupled to the reactor with an applied power of 7500 W.
[0087] Next, the patterned transfer film is transported through the reaction area at a speed of 7.6 meters / minute (25 feet / minute), resulting in an exposure time of approximately 12 seconds. At the end of this processing time, the RF power and gas supply are shut off, and the chamber is returned to atmospheric pressure.
[0088] Additional information regarding materials and processes for continuous reactive ion etching via nanostructured masks, as well as further details regarding the reactor periphery, can be found in U.S. Patent No. 8,460,568 (David et al.).
[0089] Step 7: TiO2 backfill A backfilled nanostructured film is formed by depositing TiO2 onto the etched pattern transfer film from step 6. The TiO2 backfill layer is formed from a titanium tetra(isopropoxide) (TTIP) precursor using a space atomic layer deposition (ALD) process. Planar coating is performed in a space R2R ALD machine as described in International Publication No. 2017 / 172531 (Lyons et al.). TiO2 is deposited using TTIP heated to 80°C with a plasma discharge (approximately 0.50 mA / cm2) in an environment of 300 SCCM of N2 push gas and 1.1 Torr N2 and 0.3 Torr CO2. The ALD chamber is heated to 100°C.
[0090] The film is moved through the ALD chamber in multiple passes at a speed of 30.48 meters / min (100 feet / min). Each ALD cycle involves one precursor exposure and one plasma exposure, and 72 ALD cycles per chamber pass. The film is moved through the ALD chamber in 10 to 50 passes to obtain a TiO2 layer of sufficient thickness to fill the etched nanostructures within the transfer film, covering the top of the nanostructured regions of the transfer film and forming a plane.
[0091] Step 8: Solution coating of the adhesive layer An adhesive layer is formed on the surface of the TiO2 backfill nanostructured film from step 7 by slot die coating of the adhesive coating solution in a roll-to-roll process. The adhesive coating solution is prepared by diluting a certain amount of FG1901 G with sufficient cyclohexane to produce a solution containing 0.33 wt% total solids. This solution is coated onto the film from step 5 at a rate and flow rate that forms a wet coating thickness of approximately 9 micrometers. The coated web is moved approximately 2.4 m (8 feet) before entering a 9.1 m (30 feet) conventional air flotation dryer with all three zones set to 80°C (176°F). After drying, the thickness of the adhesive coating is approximately 30 nanometers.
[0092] Step 9: Lamination onto the glass substrate The optical article is formed by laminating a nanostructured film coated with adhesive from step 8 onto a glass substrate. A suitable glass substrate is an Eagle XG glass wafer with a thickness of 1.1 mm and a diameter of 76.2 mm, having a surface roughness of less than 1 nm RMS. The adhesive side of the structured film is placed on one surface of the glass wafer, and the film is laminated onto the glass substrate by passing it through an HL-100 Hot Roll Laminator (ChemInstruments, West Chester Township, OH) set to 80 psi, 40 cm / min, and 115°C.
[0093] Virtual Example 2 Complete steps 1-7 as in the virtual example 1.
[0094] Step 7a: Thinning of TiO2 backfill The TiO2 backfill nanostructured film constructed in step 7 is subjected to reactive ion etching to reduce the thickness of the planarized ALD TiO2 layer. Reactive ion etching is performed on the film in the same reactor chamber used to deposit the peeling layer in step 2 of hypothetical example 1. After placing the patterned transfer film on the powered electrode, the reactor chamber is pumped down to a base pressure of less than 1.3 Pa (1 milliliter). Nitrogen trifluoride is introduced into the chamber at a flow rate of 1000 SCCM. Subsequently, 13.56 MHz RF power is coupled to the reactor at an applied power of 7500 W. The film is then transported through the reaction area to achieve a planar removal rate of 100 nm per minute of exposure time. The exposure time is selected to leave a thin planar layer of TiO2 on the nanostructured film such that the residual layer is less than 50 nm thick.
[0095] Steps 8 and 9 are repeated in the same manner as in the 1st example.
[0096] Virtual Example 3 The optical article is prepared as described in Virtual Example 1 or Virtual Example 2, except that in step 1, the nanostructured tooling film is prepared on a substrate 01 instead of polycarbonate.
[0097] After step 9, 90% / 10% of the Si / Al layer of substrate 01 is weakened by exposure to UV light through the ST505 film. After UV exposure, the ST505 substrate is removed by peeling it off the structure, thereby leaving the structure attached to the glass wafer.
[0098] Terms such as “about” will be understood by those skilled in the art in the context in which they are used and described herein. Where the use of “about” in relation to the size, quantity, and physical properties of a feature is not otherwise obvious to those skilled in the art in the context in which it is used and described herein, “about” will be understood to mean within 10 percent of a particular value. A quantity given as about or approximately of a particular value may be exactly that particular value. For example, where it is not otherwise obvious to those skilled in the art in the context in which it is used and described herein, a quantity having a value of about 1 means that the quantity has a value between 0.9 and 1.1, and that the value may also be 1.
[0099] All references, patents, or patent applications cited above are incorporated herein by reference in their entirety. In the event of any inconsistency or contradiction between any part of the incorporated references and this application, the information in the foregoing description shall prevail.
[0100] Unless otherwise indicated, the descriptions of elements in the drawings should be understood to apply equally to the corresponding elements in other drawings. While specific embodiments are illustrated and described herein, it will be understood by those skilled in the art that these specific embodiments may be replaced by various alternative and / or equivalent embodiments without departing from the scope of this disclosure. This application is intended to encompass all adaptations, modifications, or combinations of the specific embodiments discussed herein. Therefore, this disclosure is intended to be limited only by the claims and their equivalents. Exemplary embodiments are described below. [Item 1] a waveguide, and a structured film, comprising: a polymer substrate, an etch stop layer disposed on the polymer substrate, a structured layer comprising a plurality of fabricated structures disposed on a side of the etch stop layer opposite to the polymer substrate, a planarizing backfill layer disposed over the plurality of fabricated structures, defining a substantially flat major surface of the planarizing backfill layer having a surface roughness Ra, wherein a difference in refractive index between the planarizing backfill layer and the structured layer is at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm, and an adhesive layer disposed on the substantially flat major surface of the planarizing backfill layer, for bonding the structured film to the waveguide, the adhesive layer having an average thickness ta satisfying Ra < ta < (1 / 4)W1; An optical article comprising: [Item 2] The optical article according to Item 1, wherein the structured film further comprises an unstructured layer disposed between the etch stop layer and the polymer substrate, and a difference in refractive index between the planarizing backfill layer and the unstructured layer is at least 0.2 for at least the first wavelength W1. [Item 3] The optical article according to Item 1 or 2, wherein the fabricated structures are inclined relative to the etch stop layer. [Item 4] The optical article according to any one of Items 1 to 3, further comprising a dynamic separation layer disposed between the etch stop layer and the polymer substrate. [Item 5] The optical article according to any one of Items 1 to 4, wherein the average thickness ta is less than 250 nm. [Item 6] The optical article according to any one of Items 1 to 4, wherein the average thickness ta is less than 100 nm. [Item 7] The optical article according to any one of Items 1 to 6, wherein the plurality of fabricated structures comprises a plurality of nanostructures. [Item 8] a polymer substrate, an etch stop layer disposed on the polymer substrate, a structured layer comprising a plurality of fabricated structures disposed on a side of the etch stop layer opposite to the polymer substrate, wherein the fabricated structures are inclined relative to the etch stop layer. a planarization backfill layer disposed over the plurality of fabricated structures, defining a substantially flat major surface of the planarization backfill layer having a surface roughness Ra, wherein the difference in refractive index between the planarization backfill layer and the structured layer is at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm; an adhesive layer disposed on the substantially flat major surface of the planarization backfill layer, the adhesive layer having an average thickness ta that satisfies Ra<ta<(1 / 4)W1; A structured film comprising: [Item 9] The structured film according to Item 8, wherein for at least a majority of the fabricated structures, each fabricated structure comprises sidewalls defining an exterior angle relative to the etch stop layer in the range of 45 to 85 degrees. [Item 10] The structured film according to Item 8 or 9, wherein the structured layer comprises a fluoropolymer, and the planarization backfill layer comprises a metal oxide, nitride, or oxynitride. [Item 11] The structured film according to any one of Items 8 to 10, wherein the first wavelength W1 is in the range of 400 nm to 700 nm. [Item 12] a waveguide; a structured film disposed on a major surface of the waveguide, the structured film comprising: an etch stop layer; a structured layer disposed on the etch stop layer and comprising a plurality of fabricated structures, wherein the fabricated structures are inclined relative to the etch stop layer; a planarization backfill layer disposed over the plurality of fabricated structures, defining a substantially unstructured major surface of the planarization backfill layer having a surface roughness Ra, wherein the difference in refractive index between the planarization backfill layer and the structured layer is at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm; and an adhesive layer disposed on the substantially unstructured major surface of the planarization backfill layer, the adhesive layer bonding the structured film to the major surface of the waveguide and having an average thickness ta that satisfies Ra<ta<(1 / 4)W1; An optical article comprising: [Item 13] The optical article according to Item 12, wherein the surface roughness Ra is less than 20 nm. [Item 14] a polymer substrate; an etch stop layer; a dynamic separation layer disposed between the polymer substrate and the etch stop layer. a structured layer comprising a plurality of processed structures disposed on a side of the etch stop layer opposite to the dynamic separation layer; a planarizing backfill layer disposed over the plurality of processed structures, the planarizing backfill layer defining a substantially flat main surface thereof having a surface roughness Ra, wherein a difference in refractive index between the planarizing backfill layer and the structured layer is at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm; and an adhesive layer disposed on the substantially flat main surface of the planarizing backfill layer and having an average thickness ta satisfying Ra < ta < (1 / 4)W1, the structured film. The structured film, wherein the dynamic separation layer is adapted to facilitate separation between the polymer substrate and the etch stop layer upon activation. [Item 15] The structured film according to Item 14, wherein the dynamic separation layer is adapted to peel off from the etch stop layer upon activation.
Claims
1. Waveguides and A structured film, Polymer substrate and An etch stop layer disposed on the polymer substrate, A structured layer comprising a plurality of processed structures disposed on the side of the etch stop layer opposite to the polymer substrate, A planar backfill layer disposed on the plurality of processed structures, having a surface roughness Ra, defining a substantially flat main surface of the planar backfill layer, and the difference in refractive index between the planar backfill layer and the structured layer being at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm, A structured film comprising: an adhesive layer disposed on the substantially flat main surface of the planarized backfill layer and for bonding the structured film to the waveguide, the adhesive layer having an average thickness ta such that Ra < ta < (1 / 4)W1; Equipped with, An optical article in which the structured film is laminated to the waveguide by the adhesive layer, and light is coupled between the waveguide and the structured layer through the adhesive layer.
2. The optical article according to claim 1, wherein the structured film further comprises an unstructured layer disposed between the etch-stop layer and the polymer substrate, the unstructured layer does not include a plurality of processing structures, and the difference in refractive index between the planarized backfill layer and the unstructured layer is at least 0.2 with respect to the first wavelength W1.
3. The optical article according to claim 1, wherein the processed structure is inclined with respect to the etch stop layer.
4. The optical article according to any one of claims 1 to 3, further comprising a dynamic separation layer disposed between the etch stop layer and the polymer substrate.
5. The optical article according to any one of claims 1 to 3, wherein the average thickness ta is less than 250 nm.
6. The optical article according to any one of claims 1 to 3, wherein the average thickness ta is less than 100 nm.
7. The optical article according to any one of claims 1 to 3, wherein the plurality of processed structures include a plurality of nanostructures.
8. Polymer substrate and An etch stop layer disposed on the polymer substrate, A structured layer comprising a plurality of processed structures arranged on the side of the etch-stop layer opposite to the polymer substrate, wherein the processed structures are inclined with respect to the etch-stop layer, and A planar backfill layer disposed on the plurality of processed structures, having a surface roughness Ra, defining a substantially flat main surface of the planar backfill layer, and the difference in refractive index between the planar backfill layer and the structured layer being at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm, An adhesive layer having an average thickness ta such that Ra < ta < (1 / 4)W1 is disposed on the substantially flat main surface of the planarized backfill layer, A structured film comprising, A structured film in which the structured film is laminated to a substrate with the adhesive layer, thereby enabling light to bond between the substrate and the structured layer through the adhesive layer.
9. The structured film according to claim 8, wherein at least a majority of the processed structures include a side wall that defines an outer angle with respect to the etch stop layer in the range of 45 to 85 degrees.
10. The structured film according to claim 8, wherein the structured layer comprises a fluoropolymer, and the planar backfill layer comprises a metal oxide, nitride, or oxynitride.
11. The structured film according to any one of claims 8 to 10, wherein the first wavelength W1 is in the range of 400 nm to 700 nm.
12. Waveguides and A structured film disposed on the main surface of the waveguide, Etching stop layer, A structured layer disposed on the etch stop layer and comprising a plurality of processed structures, wherein the processed structures are inclined with respect to the etch stop layer, A planar backfill layer disposed on the plurality of processed structures, having a surface roughness Ra, defining a substantially unstructured main surface of the planar backfill layer, and the difference in refractive index between the planar backfill layer and the structured layer being at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm, A structured film comprising: an adhesive layer disposed on the substantially unstructured main surface of the planarized backfill layer, the adhesive layer bonding the structured film to the main surface of the waveguide, and having an average thickness ta such that Ra < ta < (1 / 4)W1; Equipped with, An optical article in which the structured film is laminated to the waveguide by the adhesive layer, and light is coupled between the waveguide and the structured layer through the adhesive layer.
13. The optical article according to claim 12, wherein the surface roughness Ra is less than 20 nm.
14. Polymer substrate and Etching stop layer, A dynamic separation layer disposed between the polymer substrate and the etch stop layer, A structured layer including a plurality of processed structures arranged on the side of the etch stop layer opposite to the dynamic separation layer, A planar backfill layer disposed on the plurality of processed structures, having a surface roughness Ra, defining a substantially flat main surface of the planar backfill layer, and the difference in refractive index between the planar backfill layer and the structured layer being at least 0.25 for at least a first wavelength W1 in the range of 400 nm to 2500 nm, A structured film comprising: an adhesive layer disposed on the substantially flat main surface of the planarized backfill layer, having an average thickness ta such that Ra < ta < (1 / 4)W1, The dynamic separation layer is a structured film adapted to promote the separation of the polymer substrate and the etch stop layer upon activation, A structured film in which the structured film is laminated to a substrate with the adhesive layer, thereby enabling light to bond between the substrate and the structured layer through the adhesive layer.
15. The structured film according to claim 14, wherein the dynamic separation layer is adapted to peel off from the etch stop layer upon activation.
Citation Information
Patent Citations
Thermal transfer of microstructured layers
JP2003515461A
Method for fabricating a photonic circuit with active and passive structures
JP2015527608A
Laminated transfer film forming an antireflection structure
JP2017508640A
Display System
US20160234485A1
Waveguide for head-up display, including reflective output coupling structure