Suspension for thermal spray coating
The suspension with a low fine fraction ratio forms large spray particles to naturally produce dense, defect-free coatings, addressing the issue of cylindrical defects in existing methods and enhancing coating quality without additional equipment.
Patent Information
- Application Number
- JP2023561618
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-07
- Filing Date
- 2022-04-06
- Publication Date
- 2026-11-19
- Estimated Expiration
- 2042-04-06
AI Technical Summary
Existing suspension plasma spraying methods produce cylindrical defects and require additional equipment like air cross jets or water shrouds to achieve defect-free, dense coatings, increasing cost and labor.
A suspension with a fine fraction ratio (FFR) of 0.5 or less, comprising solid ceramic particles with a particle size distribution of 2-10 μm and a density of 3.0 to 7.0 g/cm³, which naturally forms large spray particles with high inertia, reducing the formation of defects and the need for additional equipment.
Produces dense, defect-free coatings with smooth surfaces, enhancing corrosion, erosion, and scratch resistance without additional equipment, improving deposition efficiency and reducing thermal stress.
Smart Images

Figure 0007954161000002 
Figure 0007954161000003 
Figure 0007954161000004
Abstract
Description
[Technical Field]
[0001] This invention relates to a suspension for thermal spraying. [Background technology]
[0002] Suspension spraying, such as suspension plasma spraying, is an emerging technique for creating coatings.
[0003] Using a suspension as a raw material for thermal spraying typically allows for the use of fine particles with an average size (d50) of less than 10 μm, offering many advantages compared to conventional thermal spraying using solid raw materials such as powders. Suspension spraying allows for lower surface roughness and coating porosity, and enables the creation of smaller pore sizes. Furthermore, suspension spraying with small particles is beneficial for pneumatic thermal spraying systems.
[0004] Depending on the properties of the suspension (e.g., viscosity, surface tension, particle size, solid load), cylindrical and dense coatings can be formed by suspension spraying. In addition, coatings with a thickness of several micrometers can be obtained using suspension materials. Smooth and dense coatings are of particular interest for abrasion-resistant, corrosion-resistant, and electrical insulation applications.
[0005] A preferred suspension spraying method for producing dense coatings is suspension plasma spraying (SPS). In suspension plasma spraying, a suspension is introduced into a spray jet of high-temperature, high-velocity plasma gas, where it is atomized into smaller droplets. The liquid then vaporizes, simultaneously causing the original solid particles to aggregate and increase in size. These spray particles are melted by the high-temperature plasma gas and accelerated toward the surface to be coated. Upon impact with the low-temperature, solid surface, the spray particles are flattened into what are commonly called splats, which then cool and solidify, forming the sprayed coating.
[0006] The general principles of suspension plasma spraying of dense ceramic coatings are disclosed in U.S. Patent No. 5,609,921, U.S. Patent No. 6,579,573, and U.S. Patent Application Publication No. 2006 / 0222777.
[0007] VanEvery et al. (Journal of Thermal Spray Technology, Vol. 20(4), Nos. 817-828 (2011)) investigated the effect of suspension droplet size and deposited particle size on coating microstructure. Small deposited particles with low inertia follow the gas jet near the substrate and are deposited at collision angles not perpendicular to the substrate surface, forming cylindrical structures (defects). In contrast, large deposited particles with high inertia maintain their trajectories and collide with the coating surface at angles close to 90°, forming dense microstructure. Typically, starting with the same suspension droplet size, small deposited particles are formed when the suspension is low concentration and contains small solid particles, while large deposited particles are formed when the suspension is high concentration and contains large or small particles.
[0008] Further background information on coating formation is disclosed in L. Pawlowski, Surface & Coatings Technology, Vol. 203(19), pp. 2807-2829 (2009). Curry et al. (Coatings, Vol. 5, pp. 338-356 (2015)) disclose that the droplet size of a suspension is controlled by the properties of the suspension, particularly viscosity, surface tension, and density (solid load) of the suspension. Further prior art is disclosed in Journal of Thermal Spray Technology, Vol. 20(Nos. 1-2), pp. 170-185 (2011) by Kitamura et al., U.S. Patent Application No. 2019 / 0242001(A1), and in Journal of Thermal Spray Technology, Vol. 28, pp. 1579-1605 (2019) by Aghasibeig et al.
[0009] Commercially available suspensions are ethanol-based for the production of cylindrical coatings or aqueous-based for the production of dense coatings. Mixtures of ethanol and water have also been reported, but are not widely used in this industry.
[0010] In the latest technologies, suspensions for wear-resistant coatings typically contain approximately 25-40% by weight of chromia, alumina, or titania in an aqueous liquid. For applications requiring a smooth and dense coating, these suspensions increase the formation of cylindrical defects (Kiilakoski et al., Journal of Thermal Spray Technology, Vol. 28, pp. 1933-1944 (2019)). These defects may be referred to as "nodules."
[0011] For example, a defect-free coating can only be produced when fine particles are removed from the spray jet using additional equipment, such as an air cross jet (Kiilakoski et al., Journal of Thermal Spray Technology, Vol. 28, pp. 1933-1944 (2019)) or a water shroud (U.S. Patent No. 10,279,365). Such additional equipment is undesirable due to the increased cost and labor involved.
[0012] Further prior art related to the technology of this disclosure is disclosed in U.S. Patent Application Publication No. 2020 / 0048752; "Suspension and coating characterization of high velocity suspension flame sprayed (HVSFS) mixed titanium oxide-titanium carbide coatings" by Forg et al., Surf.CoatingsTech., Vol. 371, pp. 90-96 (2019); "An investigation of the dispersion of YSZ, SDC, and mixtures of YSZ / DSC powders in aqueous suspensions for application in suspension plasma spraying" by Arevalo et al., Surf.CoatingsTech., Vol. 205, pp. 5218-5227 (2011); and European Patent No. 3,778,981. [Overview of the Initiative]
[0013] The object of the present invention is to provide a suspension spraying suspension that overcomes the shortcomings of the latest technology and can produce a dense, defect-free coating without using further technical measures such as air cross jets or water shrouds.
[0014] This objective is addressed by a suspension comprising solid ceramic particles and a solvent, characterized in that the fine fraction ratio (FFR) of the suspension is 0.5 or less. According to the present invention, the fine fraction ratio is -When determined from the particle size distribution, the volume fraction of solid ceramic particles with a particle size of 1.0 μm or less, - Mass fraction of solid ceramic particles in suspension and It is defined as the ratio of, The density of the solid ceramic particles is 3.0 to 7.0 g / cm³. 3 And, Solid ceramic particles are based on volume d50 It has a particle size distribution in the range of 2 μm to 10 μm.
[0015] Accordingly, the present invention takes into account the different particle size distributions of particles in a suspension and the particle aggregation process in the spray jet during a suspension spray, and defines a critical ratio between the fine content and the solid concentration in the suspension in the particle size distribution of the solid content of the suspension. The fine fraction ratio defines the minimum standard for the suspension composition to form spray particles large enough to naturally produce a dense, lumpy coating structure.
[0016] The present invention is particularly useful for producing corrosion-resistant, erosion-resistant, and / or scratch-resistant coatings that have a dense microstructure and a smooth surface.
[0017] The ability to reduce particles is inherent to the suspension formulation. Low FFR reduces the formation of fine particles in the spray jet, thereby preventing the formation of cylindrical defects. No further technical equipment such as an air cross jet or water shroud is required to remove fine particles from the spray jet.
[0018] The suspension described in this invention, which has a low FFR, can reduce the spray distance. This is because larger spray particles in the spray jet have higher inertia. Increasing the spray distance reduces the thermal load on the coating and prevents cracks caused by thermal stress. Furthermore, deposition efficiency is automatically increased because more material reaches the substrate when there is no need to remove fine particles from the spray jet by further means. [Brief explanation of the drawing]
[0019] [Figure 1A]The SEM BSE image of the polished cross-section of the coating obtained in Example 1 is shown, which exhibits a dense microstructure free of cracks and defects, and a smooth surface (magnification: 170×, accelerating voltage: 15.0 kV, working distance, WD: 10.2 mm). [Figure 1B] The SEM BSE image of the same cross-section is continuously shown (magnification: 170×, accelerating voltage: 15.0 kV, WD: 10.1 mm). [Figure 2] The SEM BSE image of the polished cross-section of the coating obtained in Example 2 is shown, which exhibits a dense microstructure free of cracks and defects, and a smooth surface (magnification: 60×, accelerating voltage: 15.0 kV, WD: 10.1 mm). [Figure 3] The SEM BSE image of the polished cross-section of the coating obtained in Example 3 is shown, which exhibits a dense microstructure free of cracks and defects, and a smooth surface (magnification: 60×, accelerating voltage: 15.0 kV, WD: 11.8 mm). [Figure 4A] The SEM BSE image of the cross-section of the coating obtained in Comparative Example 1A is shown, which shows a bimodal coating structure with an uneven (rough) surface (Figure 4A: magnification: 1000×, accelerating voltage: 15.0 kV, WD: 11.5 mm). [Figure 4B] The SEM BSE image of the cross-section of the coating obtained in Comparative Example 1A is shown, which shows a bimodal coating structure with an uneven (rough) surface (Figure 4B: magnification: 1000×, accelerating voltage: 15.0 kV, WD: 11.5 mm). [Figure 4C] The SEM BSE image of the cross-section of the coating obtained in Comparative Example 1A is shown, which shows a bimodal coating structure with an uneven (rough) surface (Figure 4C: magnification: 1000×, accelerating voltage: 15.0 kV, WD: 10.0 mm). [Figure 4D] The SEM BSE image of the cross-section of the coating obtained in Comparative Example 1A is shown, which shows a bimodal coating structure with an uneven (rough) surface (Figure 4D: magnification: 1000×, accelerating voltage: 15.0 kV, WD: 9.8 mm). [Figure 5]The image shows an SEM BSE image of a polished cross section of the obtained coating, prepared in the same manner as described in Example 1B, representing an overall flat surface with a granular morphology and scattered surface irregularities, formed by a single column (magnification: 500x, acceleration voltage: 15.0kV, WD: 10.2mm). [Modes for carrying out the invention]
[0020] In a first aspect, the present invention provides a suspension for thermal spraying comprising solid ceramic particles and a solvent, characterized in that the fineness fraction ratio of the suspension is 0.5 or less, where the fineness fraction ratio is defined as the ratio of the volume fraction of solid ceramic particles with a particle size of 1.0 μm or less, as determined from the particle size distribution, to the mass fraction of solid ceramic particles in the suspension, and the density of the solid ceramic particles is 3.0 to 7.0 g / cm³. 3 Therefore, the solid ceramic particles are based on volume d 50 It has a particle size distribution in the range of 2 μm to 10 μm.
[0021] In a second aspect, the present invention provides the use of the suspension for suspension thermal spraying.
[0022] The following disclosures apply similarly to the first and second embodiments.
[0023] As used herein, the term “suspension spraying” refers to the use of a suspension as a raw material in a spraying process including plasma spraying (such as atmospheric plasma spraying and low-pressure plasma spraying), fast oxygen fuel spraying, fast air fuel spraying, flame spraying, cold spraying, laser spraying, or laser cladding. Preferably, the suspensions described in the present invention are used in suspension plasma spraying, low-pressure plasma spraying, and fast oxygen fuel spraying, and most preferably in suspension plasma spraying, specifically atmospheric suspension plasma spraying.
[0024] For the purposes of this specification and the claims, the fine fraction ratio (FFR) is given by formula (1):
number
[0025] According to the present invention, the fine fraction ratio is 0.5 or less. Preferably, the fine fraction ratio is 0.4 or less.
[0026] The FFR proposed herein has a density of preferably 3.0 to 7.0 g / cm³. 3 , more preferably 4.9 to 6.6 g / cm³ 3 It is preferable to apply this to solid ceramic particles.
[0027] As used herein, the term "volume fraction" refers to the ratio of the total volume of solid ceramic particles with a particle size of 1.0 μm or less to the total volume of all solid ceramic particles in a suspension. The volume fraction is expressed in volume percent.
[0028] The term "mass fraction of solid ceramic particles in a suspension" refers to the ratio of the total mass of all ceramic particles in the suspension to the total mass of the suspension (i.e., the sum of the masses of all components in the suspension). The mass fraction is given in weight percent.
[0029] The volume fraction of particles with a particle size of 1.0 μm or less is determined from the particle size distribution obtained by particle size analysis. In this invention, the particle size distribution is determined using laser diffraction particle analysis, preferably a "Microtrac" particle analyzer.
[0030] In these particle analyzers, the laser beam is scattered by the particles in the sample, and the angle of light scattering is inversely proportional to the particle size. The particle size distribution is typically determined by intervals ("boxes").
[0031] According to the present invention, in order to obtain a dense coating, it is particularly preferable to minimize the volume fraction of particles with a particle size of 1 μm or less. To determine the volume fraction of these particles from the particle size distribution, measurements from a particle analyzer as close to 1.0 μm as possible are obtained. The value at 1.0 μm is then determined by linear interpolation if the analyzer does not provide data for intervals precisely divided at 1.0 μm.
[0032] In this invention, the particle size distribution is determined using a Microtrac S3500 or Microtrac X100 instrument utilizing the Fraunhofer analysis mode (measurement mode: full-range analysis of absorbed particles (FRA)). The term "full-range analysis" refers to the determination of particle size over the entire measurement range of the instrument, and the term "absorbed particles" refers to particles that do not transmit light.
[0033] The Microtrac S3500 and X100 instruments determine the particle volume fraction in the range of 0.972 μm to 1.06 μm, with the value closest to 1.0 μm being used.
[0034] Other instruments exhibiting comparable sensitivity and measurement range to the Microtrac S3500 and X100 instruments, particularly comparable lower limits for detectable particle size and comparable sensitivity in the small size region, may be used to determine the particle size distribution described in the present invention. Those skilled in the art will know of suitable instruments available on the market.
[0035] In preferred embodiments, the volume fraction of solid ceramic particles with a particle size of 1.0 μm or less is 20% or more. The present invention is essentially beneficial in the case of suspensions having a certain amount of small particle size particles. Therefore, the present invention particularly provides teachings on the maximum amount of small particle size particles that must be contained in the suspension if small particle size particles are present.
[0036] In a more preferred embodiment, the volume fraction of solid ceramic particles having a particle size of 1.0 μm or less is less than 30 volume%, preferably less than 25 volume%.
[0037] In preferred embodiments, the solid ceramic particles of the suspension of the present invention exhibit a particle size distribution having d50 values in the range of 4.0 μm to 5.0 μm. The d50 value should be understood as the "average particle size" and is determined from the particle size distribution. The d50 value is known as the median diameter, i.e., the median of the particle size distribution, and these are determined from a volume-based representation (dv50) or a number-based representation (dn50). In this application, the d50 value refers to a volume-based representation, i.e., the particle size at 50 volume percent of the cumulative distribution (for example, a d50 of 2.0 μm means that 50 volume percent of particles have a diameter smaller than 2.0 μm).
[0038] In one embodiment, the solid ceramic particles contain or consist of a transition metal, a rare earth metal, or at least one oxide of a metal from Group 13 or Group 14 of the periodic table.
[0039] As used herein, the term “transition metal” refers to a transition metal element or a mixture thereof, i.e., two or more transition metal elements. According to IUPAC, a transition metal is an element whose atom has an incomplete d subshell or which can produce a cation having an incomplete d subshell. However, for the purposes of this specification and the claims, the term “transition metal” includes only the elements of Groups 4 through 11 of the periodic table and Zn.
[0040] As used herein, the term "rare earth metals" refers to a group of 17 chemically similar metallic elements, including lanthanides, yttrium, and scandium. Lanthanides are defined as a set of elements with atomic numbers 57–71, all of which exist in nature except for promethium (Extractive Metallurgy of Rare Earths, CK Gupta, N. Krishnamurthy, CRC).
[0041] If the solid ceramic particles contain or are derived from an oxide of a transition metal, the oxide is preferably chromium(III) oxide (chromia, Cr2O3) or titanium oxide (titania, TiO2O3). xx is preferably 1.6 to 2, more preferably 1.6 to 1.9, or 2, which is i.e., TiO2.
[0042] The solid ceramic particles may also contain or be composed of oxides of rare earth metals such as yttrium oxide (yttria, Y2O3).
[0043] If the solid ceramic particles contain or are composed of metal oxides of Group 13 of the periodic table, the oxide is preferably aluminum oxide (alumina, Al2O3).
[0044] If the solid ceramic particles contain or are composed of metal oxides of Group 14 of the periodic table, the oxide is preferably a silicate mineral containing silicon dioxide (silica, SiO2), such as aluminum silicate (3Al2O3·2SiO2) like mullite.
[0045] In a particularly preferred embodiment, the solid ceramic particles are chromium(III) oxide (Cr2O3), aluminum oxide (Al2O3), yttrium oxide (Y2O3), and titanium oxide (TiO2O3). x The material is selected from the group consisting of (where x is preferably in the range of 1.6 to 2) and mixtures and / or composite materials thereof.
[0046] According to a preferred embodiment, the mass fraction of solid ceramic particles in the suspension is at least 60% by weight, preferably at least 70% by weight, and more preferably at least 75% by weight. The mass fraction of solid ceramic particles in the suspension may also be at least 80% by weight or more.
[0047] According to the present invention, the solvent may include water, an organic solvent, or a mixture thereof, or consist of these. The organic solvent may be selected from the group consisting of alcohols, ketones, esters, glycols, glycol ethers, glycol ether esters, hydrocarbons, or any combination thereof.
[0048] Preferably, the solvent contains or consists of water, preferably deionized water. The solvent may also contain an antifreeze agent. Antifreeze agents are particularly useful when the solvent consists mainly of water or entirely of water. The solvent consists mainly of water if water constitutes at least 60% by weight, preferably at least 70% by weight, or 75% by weight, or 80% by weight, or 85% by weight, or 90% by weight or more of the solvent.
[0049] Antifreezing agents ensure that suspensions remain liquid and stable at temperatures below 0°C. This is beneficial for the transport and storage of suspensions. Preferably, the suspension remains liquid at at least -10°C. Antifreezing agents may be selected from the group of glycols and alcohols. Preferably, the antifreezing agent is ethylene glycol. The antifreezing agent may also be ethanol or isopropanol.
[0050] According to certain embodiments of the present invention, the solvent consists of a mixture of water and ethylene glycol. Preferably, the weight ratio of water to ethylene glycol is in the range of 1:10 (w / w) to 1:1 (w / w). For example, the solvent may consist of 70% to 80% by weight of water and 30% to 20% by weight of ethylene glycol.
[0051] In one embodiment, the suspension described in the present invention further comprises a dispersant. The dispersant may be any compound suitable for stabilizing the suspension for thermal spraying. The dispersant ensures that the particles remain well dispersed and do not form large aggregates or precipitates. For example, the dispersant may be a salt and inorganic salt of a polymer or an organic molecule. Those skilled in the art know of dispersants suitable for various solid ceramic particles.
[0052] Examples of suitable dispersants are 2-amino-2-methylpropanol (AMP 90™ and AMP 95™), ammonium polycarboxylate, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid (MEEA), polyacrylic acid, polyethyleneimine, sodium metaphosphate, sodium tetraborate, triethanolamine, TRITON X-100™, Lopon® 888, sodium bicarbonate and citric acid. For example, particularly preferred dispersants for Cr₂O₃ are 2-amino-2-methyl-1-propanol and ammonium polycarboxylate. Suitable dispersants for Al₂O₃ are 2-amino-2-methyl-1-propanol or 2-[2-(2-methoxyethoxy)ethoxy]acetic acid (MEEA).
[0053] However, the present invention is not limited to this exemplary list of dispersants.
[0054] The concentration of the dispersant is selected depending on the concentration of the solid ceramic particles in the suspension, so as to provide a homogeneous and stable suspension and reduce the viscosity. The concentration of the dispersant may be in the range of 0.1 wt% to 10 wt%, preferably 0.5 to 5 wt%, even more preferably 1 to 3 wt%, relative to the content of the solid ceramic particles, for example 1 wt%.
[0055] The suspension according to the present invention may optionally further contain a binder.
[0056] Preferably, the viscosity of the suspension according to the present invention is, at a shear rate of 100 to 1000 s -1 , less than 50 mPa*s, preferably less than 40 mPa*s, even more preferably less than 30 mPa*s. Usually, the viscosity is measured at room temperature, which refers to a range of 23 to 25°C. Preferably, the viscosity is measured at a shear rate of 1000 s -1 . More preferably, the viscosity is measured, for example, with an Anton Paar Physica MCR 301 rotational rheometer equipped with a plate-plate system.
[0057] Low viscosity is preferable for the suspension thermal spraying process.
[0058] The suspension described in the present invention is particularly suitable for producing coatings having a dense microstructure and a smooth surface by suspension spraying, preferably suspension plasma spraying. As understood herein, “dense microstructure” is characterized by low porosity (i.e., less than 10%, preferably less than 5%), where the pore diameter of the smallest pores is less than 20 μm, preferably less than 10 μm. In addition, the dense coating is preferably free from cracks of 50 μm or more, preferably 10 μm or more. Those skilled in the art know the suitable spraying parameters for obtaining a dense coating.
[0059] These coatings are preferably used to protect the coated material from corrosion, erosion, and / or abrasion.
[0060] According to the present invention, a dense coating can be manufactured on any suitable substrate, such as metals, ceramics, polymers, ceramic matrix composites, alloys, and mixtures or composites thereof. For example, the substrate may be made of aluminum, iron, or steel, and preferably stainless steel.
[0061] The suspension according to the present invention can be prepared by dispersing solid ceramic raw materials in the solvent described herein and grinding the suspension until a desired average particle size (d50) is obtained. Grinding is optionally carried out in the presence of a dispersant described herein. After this, the suspension is diluted to a desired solid concentration.
[0062] The present invention will be described in more detail below by the following examples and comparative examples, but will not be limited thereto. [Examples]
[0063] Example 1 Commercially available Cr2O3 powder (10.192 kg) with an average particle size (d50) of 4.3 was used as the raw material for the suspension. The purity of the Cr2O3 was over 99% by weight. The particle size of the powder was measured in the measurement chamber using a Microtrac S3500 with 5 drops of 5% by weight TSPP dispersant (tetrabasic sodium pyrophosphate). The following parameters were used: analysis mode: Fraunhofer, measurement mode: "FRA" (full-range analysis), particle permeability: absorbance mode, refractive index of water 1.33, flow rate 50%, and internal ultrasonic power 30 watts for 40 seconds.
[0064] The raw materials were dispersed in 2.548 kg of deionized water at a solid concentration of 80 wt%. To reduce the viscosity of the raw material suspension, 102 g of the dispersant Lopon® 888 (BK Giulini GmbH, Germany) was added to enable a strong dispersion process. This corresponds to 1 wt% relative to the oxide content. The mixture was stirred for 15 minutes. The oxide material was ground using a WAB Dyno-Mill Multilab high-energy ball mill. Grinding was carried out to obtain a well-dispersed suspension free of aggregates. A 1 mm diameter grinding ball was used. The Cr2O3 suspension thus produced contained 79.54 wt% solid and 0.79 wt% dispersant Lopon® 888.
[0065] To avoid particle sedimentation, the suspension was stirred from start to finish. The density of the suspension was 2.8 g / ccm and was measured using a graduated cylinder and scale. The viscosity of the suspension, measured with a rheometer MCR301 (Anton Paar, Austria), was in the range of 23-24 mPas at a shear rate of 100 1 / s. The final PSD (particle size distribution) was d10: 0.24 μm, d50: 3.99 μm, and d90: 8.82 μm. A sample for particle size measurement was prepared by diluting 10 ml of the suspension with 10 ml of deionized water and manually mixing it with 5 drops of 5 wt% TSPP dispersant (tetrabasic sodium pyrophosphate) for 1 minute. A few drops of the sample thus prepared were used for measurement. The instrument used was a Microtrac S3500. Before starting the measurement, an additional 5 drops of 5 wt% TSPP dispersant were added to the measurement chamber. The following parameters were used: Analysis mode: Fraunhofer, Measurement mode: "FRA" (Full Range Analysis), Particle permeability: Absorption mode, Refractive index of water 1.33, Flow rate 70%, and internal ultrasonic power 35 watts for 50 seconds. The volume fraction of particles smaller than 1.0 μm was 21.76 volume%. The calculated FFR was 0.27.
[0066] This suspension was used as a raw material in a suspension plasma spraying process. The suspension was supplied to a spray torch (Axial III®, Northwest Mettech) using a suspension feeder (NanoFeeder®, Northwest Mettech) at a supply rate of 30 ml / min. The spray torch was operated with an argon-nitrogen-hydrogen plasma gas composition at a flow rate of 220 standard liters per minute at an output setting of 23-25 kJ / l. The coating was deposited on a grid-blasted stainless steel coupon with a diameter of 25 mm and a thickness of 5 mm, at a spray distance of 140 mm (from the torch nozzle exit to the substrate surface). The sample was mounted on equipment that rotated around a vertical axis at 106 rotations / min. The spray torch was moved 14 times in a linear and perpendicular direction on the rotating substrate to reach the desired coating thickness. Two air jets with 5 bar compressed air were mounted parallel to the torch, and one air jet with 5 bar compressed air was mounted facing the coating sample to maintain the coating surface temperature below 250°C during coating deposition.
[0067] As shown in the SEM BSE images (Figures 1A and 1B), a coating was obtained with a dense, crack- and defect-free cross-section and a smooth surface. SEM BSE images were taken of the polished cross-section of the coating. The coating cross-section was embedded in epoxy resin, then smoothed with silicon carbide abrasive paper, and polished with a diamond suspension until the surface finish was completed with mirror polishing.
[0068] Example 2 Commercially available Cr2O3 powder (20.0 kg) with an average particle size (d50) of 4.3 μm was used as the raw material for the suspension. The measurement was the same as that described in Example 1. The purity of the Cr2O3 was over 99% by weight.
[0069] The raw materials were dispersed in 5.236 kg of water / monoethylene glycol mixture at a solid concentration of 79.3 wt%. The mixture was prepared by mixing 4.0 kg (76.4 wt%) of deionized water and 1.236 kg (23.6 wt%) of ethylene glycol (99%, Donau Chem GmbH, Austria). To reduce the viscosity of the raw material suspension, 200 g of the dispersant Lopon® 888 (BK Giulini GmbH, Germany) was added to enable a strong dispersion process. This corresponds to 1 wt% of the oxide content. The oxide material was wet-milled in a WAB Dyno-Mill Multilab high-energy ball mill. Milling was performed to obtain a well-dispersed suspension free of aggregates. A 1 mm diameter milling ball was used. After milling, the suspension was pumped through a 40 μm sieve to remove coarse particulate impurities. To prevent large losses of the suspension, 300 ml of water / MEG mixture was pumped through the mill. These liquids were combined and mixed with the suspension.
[0070] The Cr2O3 suspension thus prepared contained a solid concentration of 78.7% by weight and 0.79% by weight of the dispersant Lopon® 888. The suspension was stirred from start to finish to avoid particle sedimentation. The final PSDs were d10: 0.23 μm, d50: 3.66 μm, and d90: 7.93 μm. The measurements were the same as those described in Example 1. The volume fraction of particles smaller than 1.0 μm was 24.25% by volume. The calculated FFR was 0.31.
[0071] This suspension was used as a raw material in a suspension plasma spraying process. The suspension was supplied to a spray torch (Axial III, Northwest Mettech) using a suspension feeder (NanoFeeder®, Northwest Mettech) at a supply rate of 30 ml / min. The spray torch was operated with an argon-nitrogen-hydrogen plasma gas composition at a flow rate of 220 standard liters per minute at an output setting of 23-25 kJ / l. The coating was deposited onto a grid-blasted 50 × 30 × 5 mm stainless steel plate at a spray distance of 160 mm (from the torch nozzle exit to the substrate surface). The sample was mounted on equipment that rotated around a vertical axis at 106 rotations / min. The spray torch was moved 96 times in a linear and perpendicular direction on the rotating substrate to reach the desired coating thickness. Two air jets with 5 bar compressed air were mounted parallel to the torch, and one air jet with 5 bar compressed air was mounted facing the coating sample to maintain the coating surface temperature below 250°C during coating deposition.
[0072] As shown in the SEM BSE image of the polished cross section prepared using the same method as described in Example 1 (Figure 2), a coating was obtained with a dense cross section free of cracks and defects, and a smooth surface.
[0073] Example 3 Commercially available Y2O3 powder (4.56 kg) with an average particle size (d50) of 2.4 μm was used as the raw material for the suspension. The measurement was the same as that described in Example 1. The purity of the Y2O3 was over 99% by weight.
[0074] The following steps in the suspension process: 1. The raw materials were dispersed in 1.97 kg of monoethylene glycol / MEG by slowly adding the powder while stirring the MEG. 2. After stirring for 30 minutes, 1.03 kg of 1-hexanol was added to the mixture and stirred for a further 30 minutes. 3. To reduce the viscosity of the suspension to less than 50 mPas at a shear rate of 100 * 1 / s, an additional 69 g of the dispersant MEEA (2-(2-methoxyethoxy)ethoxyacetic acid) (Amri Global) was added. The suspension was stirred for a further 30 minutes.
[0075] The Y2O3 suspension thus prepared contained 60.4 wt% solid and 0.90 wt% dispersant MEEA. The density of the suspension was 1.9 g / ccm and was measured using a graduated cylinder and scale. The viscosity of the suspension, measured with a rheometer MCR301 (Anton Paar, Austria), ranged from 34 to 38 mPas at a shear rate of 100 1 / s. The final PSD (particle size distribution) was d10: 0.52 μm, d50: 2.35 μm, and d90: 5.64 μm. The measurements were the same as those described in Example 1. The volume fraction of particles smaller than 1.0 μm was 25.05 vol%. The calculated FFR was 0.41.
[0076] This suspension was used as a raw material in a suspension plasma spraying process. The suspension was supplied to a spray torch (Axial III®, Northwest Mettech) using a suspension feeder (NanoFeeder®, Northwest Mettech) at a supply rate of 30 ml / min. The spray torch was operated with an argon-nitrogen-hydrogen plasma gas composition at a flow rate of 220 standard liters per minute at an output setting of 14.2 kJ / l. The coating was deposited on a grid-blasted alumina coupon measuring 30 × 50 mm and 4 mm thick, with a spray distance of 115 mm (from the torch nozzle exit to the substrate surface). The sample was mounted on equipment that rotated around a vertical axis at 318 revolutions / min. The spray torch was moved 160 times in a linear and perpendicular direction on the rotating substrate to reach the desired coating thickness. Two air jets with 4.1 bar compressed air were mounted parallel to the torch, and one air jet with 4.1 bar compressed air was mounted facing the coating sample to maintain the coating surface temperature below 250°C during coating deposition.
[0077] As shown in the SEM BSE image of the polished cross section prepared using the same method as described in Example 1 (Figure 3), a coating was obtained with a dense cross section free of cracks and defects, and a smooth surface.
[0078] Comparative Example 1 Commercially available Cr2O3 powder (2.3 kg) with an average particle size (d50) of 1.08 μm was used as the raw material for the suspension. The particle size of the powder was measured in a measurement chamber using a Microtrac X100 with 5 drops of 5 wt% TSPP dispersant (tetrabasic sodium pyrophosphate). The following parameters were used: refractive index of water 1.33, flow rate 70%, and internal ultrasonic power of 35 watts for 50 seconds.
[0079] The purity of Cr2O3 was over 99% by weight.
[0080] The raw materials were dispersed in a water / monoethylene glycol mixture to a solid concentration of 43.7 wt%. A mixture was prepared by mixing 1.978 kg (66.7 wt%) of deionized water with 0.989 kg (33.3 wt%) of ethylene glycol (99%, Donau Chem GmbH, Austria). To reduce the viscosity of the raw material suspension, 23 g of the dispersant AMP 90® (BK Giulini GmbH, Germany) was added to enable a strong dispersion process. AMP 90® contains 2-amino-2-methylpropanol and 10 wt% water. The dispersant was added at an amount of 1 wt% relative to the oxide content and stirred for 20 minutes using a dissolver disc. The 4.6 kg Cr2O3 suspension thus prepared with a measured solid concentration of 43.5 wt% was used in the dilution step. To obtain a 40 wt% suspension, 0.4 kg of deionized water was added while stirring. To avoid particle sedimentation, the suspension was stirred from start to finish. The resulting suspension had a solid concentration of 40.05% by weight and a dispersant concentration of AMP 90® of 0.4% by weight.
[0081] The viscosity of the suspension, measured with a rheometer MCR301 (Anton Paar, Austria), was in the range of 3–4 mPas at a shear rate of 100 1 / s. Final PSD (particle size distribution) measurements were performed using a Microtrac S3500 and the parameters from Example 1. The final PSD (particle size distribution) was d10: 0.16 μm, d50: 0.86 μm, and d90: 2.54 μm. The volume fraction of particles smaller than 1.0 μm was 52.4 volume%. The calculated FFR was 1.31.
[0082] Comparative Example 1A This suspension was used as a raw material in a suspension plasma spraying process. The suspension was supplied to a spray torch (Axial III, Northwest Mettech) using a suspension feeder (NanoFeeder®, Northwest Mettech) at a supply rate of 30 ml / min. The spray torch was operated with an argon-nitrogen-hydrogen plasma gas composition at a flow rate of 220 standard liters per minute at an output setting of 23-25 kJ / l. The coating was deposited on a grid-blasted steel pipe with a diameter of 108 mm and a wall thickness of 4 mm, over a spray distance of 160 mm (from the torch nozzle exit to the substrate surface). The pipe was rotated 382 times / min around a horizontal axis. The spray torch was moved 30 times in a straight horizontal direction on the rotating pipe to reach the desired coating thickness. Two air jets with 5 bar compressed air were mounted parallel to the torch, and one air jet with 5 bar compressed air was mounted facing the pipe surface to keep the coating surface below 250°C during coating deposition.
[0083] SEM analysis of the polished cross-section of the obtained coating, prepared using the same method as described in Example 1, revealed a bimodal coating structure with an uneven (rough) surface (Figures 4A to 4D).
[0084] Comparative example 1B The same suspension was used as the raw material in a suspension plasma spraying process. The suspension was supplied to a spray torch (Axial III®, Northwest Mettech) using a suspension feeder (NanoFeeder®, Northwest Mettech) at a supply rate of 45 ml / min. The spray torch was operated with an argon-nitrogen-hydrogen plasma gas composition at a flow rate of 220 standard liters per minute at an output setting of 23-25 kJ / l. The coating was deposited on a grid-blasted stainless steel coupon with a diameter of 25 mm and a thickness of 5 mm at a spray distance of 120 mm (from the torch nozzle exit to the substrate surface). The sample was mounted on equipment that rotated around a vertical axis at 106 rotations / min. The spray torch was moved 60 times in a linear and vertical direction on the rotating substrate to reach the desired coating thickness. Two air jets with 5 bar compressed air were mounted parallel to the torch, and one air jet with 5 bar compressed air was mounted facing the coating sample to maintain the coating surface temperature below 300°C during coating deposition.
[0085] SEM analysis of the polished cross-section of the coating prepared using the same method as described in Example 1 shows an overall flat surface formed by a single column, with surface irregularities present in a granular, sporadic manner (Figure 5).
[0086] Comparative Example 2 Commercially available Cr2O3 powder (5.0 kg) with an average particle size (d50) of 4.3 μm was used as the raw material for the suspension. The measurement was the same as that described in Example 1. The purity of the Cr2O3 was over 99% by weight.
[0087] The raw materials were dispersed in 1.25 kg of water / monoethylene glycol mixture at a solid concentration of 80 wt%. A mixture was prepared by mixing 0.955 kg (76.4 wt%) of deionized water and 0.295 kg (23.6 wt%) of monoethylene glycol (99%, Donau Chem GmbH, Austria). To reduce the viscosity of the raw material suspension, 50 g of the dispersant Lopon® 888 (BK Giulini GmbH, Germany) was added to enable the grinding process. The dispersant was added at an amount of 1 wt% relative to the oxide content. The oxide material was wet-ground using a WAB Dyno-Mill Multilab high-energy ball mill. Grinding was performed to obtain a well-dispersed suspension free of aggregates. Grinding balls manufactured by YSZ were used. After grinding, the suspension was pumped through a 40 μm sieve to remove coarse particulate impurities. To prevent large losses of the suspension, 500 ml of water / MEG mixture was pumped through the mill. This liquid was combined and mixed with the suspension. The Cr2O3 suspension prepared in this manner had a solid concentration of 78.25% by weight. To avoid particle sedimentation, the suspension was stirred from start to finish. The density of the suspension was 2.6 g / ccm, measured using a graduated cylinder and scale. The solid concentration of the suspension was diluted to 40.05% by weight by adding 6.2 kg of the water / MEG mixture described above. The viscosity of the suspension, measured with a rheometer MCR301 (Anton Paar, Austria), was in the range of 2-3 mPas at a shear rate of 100 1 / s. The final PSD (particle size distribution) was d10: 0.22 μm, d50: 3.90 μm, and d90: 8.81 μm. The measurements were the same as those described in Example 1. The volume fraction of particles smaller than 1.0 μm was 23.63 vol%. The calculated FFR was 0.59.
[0088] This suspension was used as a raw material in a suspension plasma spraying process. The suspension was supplied to a spray torch (Axial III®, Northwest Mettech) using a suspension feeder (NanoFeeder®, Northwest Mettech) at a supply rate of 45 ml / min. The spray torch was operated with an argon-nitrogen-hydrogen plasma gas composition at a flow rate of 220 standard liters per minute at an output setting of 23-25 kJ / l. The coating was deposited on a grid-blasted stainless steel coupon with a diameter of 25 mm and a thickness of 5 mm, at a spray distance of 120 mm (from the torch nozzle exit to the substrate surface). The sample was mounted on equipment that rotated around a vertical axis at 106 rotations / min. The spray torch was moved 40 times in a linear and vertical direction on the rotating substrate to reach the desired coating thickness. Two air jets with 5 bar compressed air were mounted parallel to the torch, and one air jet with 5 bar compressed air was mounted facing the coating sample to maintain the coating surface temperature below 300°C during coating deposition.
[0089] Sufficient SEM BSE images of the coating cross-section could not be obtained. The various aspects or embodiments that may be included in the present invention are summarized below. [1]. A suspension for thermal spraying comprising solid ceramic particles and a solvent, characterized in that the fine fraction ratio of the suspension is 0.5 or less, and the fine fraction ratio is -When determined from the particle size distribution obtained from particle size analysis using laser diffraction particle analysis, the volume fraction of solid ceramic particles with a particle size of 1.0 μm or less is, - Mass fraction of solid ceramic particles in suspension and It is defined as the ratio of, The density of the solid ceramic particles is 3.0 to 7.0 g / cm³. 3 And, The solid ceramic particles, based on volume d 50 A suspension having a particle size distribution in the range of 2 μm to 10 μm. [2]. The suspension according to item 1, wherein the volume fraction of the solid ceramic particles having a particle size of 1.0 μm or less is 20% or more. [3]. The density of the solid ceramic particles is 4.9 to 6.6 g / cm³. 3 The suspension described in item 1 or 2 above. [4]. The solid ceramic particles are Cr 2 O 3 、Al 2 O 3 、Y 2 O 3 , TiO x A suspension according to any one of items 1 to 3 above, selected from the group consisting of (wherein x is preferably in the range of 1.6 to 2) and mixtures and / or composite materials thereof. [5]. The suspension according to any one of items 1 to 4 above, wherein the volume fraction of the solid ceramic particles having a particle size of 1.0 μm or less is less than 30 volume%, preferably less than 25 volume%. [6]. The solid ceramic particles have a size in the range of 4 μm to 5 μm. 50 A suspension according to any one of the above items 1 to 5, having a particle size distribution that includes the value. [7]. The suspension according to any one of items 1 to 6 above, wherein the solvent contains water or consists of water. [8]. The suspension according to any one of items 1 to 7 above, wherein the solvent contains an antifreeze. [9]. The suspension according to item 8 above, wherein the antifreeze agent contains or comprises a glycol (preferably ethylene glycol) or an alcohol (preferably ethanol or isopropanol).
[10] . The suspension according to any one of items 1 to 9 above, wherein the solvent consists of a mixture of water and ethylene glycol, and the weight ratio of water to ethylene glycol is in the range of 1:10 (w / w) to 1:1 (w / w).
[11] . A suspension according to any one of the above items 1 to 10, further comprising a dispersant.
[12] . The suspension according to any one of items 1 to 11, wherein the mass fraction of the solid ceramic particles in the suspension is at least 60% by weight, at least 70% by weight, preferably at least 75% by weight.
[13] . The suspension according to any one of the above items 1 to 12, wherein the fine fraction ratio is 0.4 or less, preferably 0.35 or less.
[14] . The suspension according to any one of items 1 to 13, wherein, when measured as described herein, the viscosity of the suspension is less than 50 mPa*s, preferably less than 40 mPa*s, and more preferably less than 30 mPa*s.
[15] . Use of the suspension described in any one of items 1 to 14 above for suspension spraying, preferably suspension plasma spraying.
[16] . The use described in item 15 above for manufacturing a coating on a substrate, wherein the substrate is selected from the group consisting of metals, ceramics, polymers, alloys and mixtures thereof.
Claims
1. A suspension for thermal spraying comprising solid ceramic particles and a solvent, characterized in that the fine fraction ratio of the suspension is 0.5 or less, and the fine fraction ratio is - When determined from the particle size distribution obtained from particle size analysis using laser diffraction particle analysis, the volume fraction of solid ceramic particles with a particle size of 1.0 μm or less relative to the total volume of all solid ceramic particles in the suspension, - Mass fraction of solid ceramic particles in suspension and It is defined as the ratio of, The density of the solid ceramic particles is 3.0 to 7.0 g / cm³. 3 And, The solid ceramic particles, based on volume d 50 The particle size distribution has values in the range of 2 μm to 10 μm. The mass fraction of the solid ceramic particles in the suspension is at least 60% by weight. The fine fraction ratio (FFR) is given by the following formula (1): FFR = (Volume fraction of solid ceramic particles with a particle size of 1.0 μm or less) / (Mass fraction of solid ceramic particles in the suspension) ... (1) A suspension calculated according to the following.
2. The suspension according to claim 1, wherein the volume fraction of the solid ceramic particles having a particle size of 1.0 μm or less is 20% or more.
3. The density of the solid ceramic particles is 4.9 to 6.6 g / cm³. 3 The suspension according to claim 1 or 2.
4. The solid ceramic particles are selected from the group consisting of Cr 2 O 3 , Al 2 O 3 , Y 2 O 3 , TiO x and mixtures and / or composites thereof, the suspension according to claim 1 or 2.
5. The suspension according to claim 4, wherein x is in the range of 1.6 to 2.
6. The suspension according to claim 1 or 2, wherein the volume fraction of the solid ceramic particles having a particle size of 1.0 μm or less is less than 30 volume percent.
7. The suspension according to claim 6, wherein the volume fraction of the solid ceramic particles having a particle size of 1.0 μm or less is less than 25 volume percent.
8. The solid ceramic particles have a size in the range of 4 μm to 5 μm. 50 The suspension according to claim 1 or 2, having a particle size distribution including the value.
9. The suspension according to claim 1 or 2, wherein the solvent contains water or consists of water.
10. The suspension according to claim 1 or 2, wherein the solvent contains an antifreeze agent.
11. The suspension according to claim 10, wherein the antifreeze agent contains or comprises glycol or alcohol.
12. The suspension according to claim 11, wherein the antifreeze contains or comprises ethylene glycol.
13. The suspension according to claim 11, wherein the antifreeze agent contains or comprises ethanol or isopropanol.
14. The suspension according to claim 1 or 2, further comprising a dispersant.
15. The suspension according to claim 1 or 2, wherein the mass fraction of the solid ceramic particles in the suspension is at least 70% by weight.
16. The suspension according to claim 1 or 2, wherein the mass fraction of the solid ceramic particles in the suspension is at least 75% by weight.
17. The suspension according to claim 1 or 2, wherein the fine fraction ratio is 0.4 or less.
18. At room temperature in the range of 23-25°C, 100-1000 seconds -1 The suspension according to claim 1 or 2, wherein the viscosity of the suspension is less than 50 mPa*s when measured at a shear rate.
19. The suspension according to claim 18, wherein the viscosity of the suspension is less than 40 mPa*s.
20. The suspension according to claim 19, wherein the viscosity of the suspension is less than 30 mPa*s.
21. Use of the suspension according to claim 1 or 2 for suspension thermal spraying.
22. Use of the suspension according to claim 21 for suspension plasma spraying.
23. An use according to claim 21 for manufacturing a coating on a substrate, wherein the substrate is selected from the group consisting of metals, ceramics, polymers, alloys and mixtures thereof.
Citation Information
Patent Citations
Film conveying guide roll
JP1982062035A
Powder for flame spray and flame spray material
JP2016138309A
Slurry for spray, and formation method of spray coating
JP2018154895A
SiC SPUTTERING TARGET
JP2019039070A
Slurry for spray
JP2019178389A