Polyvalent hydroxy resins, epoxy resins, methods for producing them, epoxy resin compositions and cured products thereof

By reacting dicyclopentadiene-type phenolic resin with dicyclopentadiene and an aromatic vinyl compound, the polyvalent hydroxy resin achieves both low dielectric properties and low viscosity, enhancing the performance of epoxy resin compositions for electronic components.

JP7954162B2Active Publication Date: 2026-11-19NIPPON STEEL CHEM & MATERIAL CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023564817
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-02
Filing Date
2022-10-31
Publication Date
2026-11-19
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

Existing epoxy resins fail to achieve both low dielectric properties and low viscosity, which are essential for high-performance electronic components in the face of miniaturization and increased performance demands in information devices.

Method used

A polyvalent hydroxy resin is produced by reacting a dicyclopentadiene-type phenolic resin with dicyclopentadiene and an aromatic vinyl compound, introducing dicyclopentadiene and aromatic skeletons to the phenol ring, followed by epoxidation to create an epoxy resin with excellent dielectric properties and low viscosity.

Benefits of technology

The resulting cured products exhibit superior dielectric properties and copper foil peel strength, addressing the limitations of previous resins in achieving both low dielectric properties and low viscosity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954162000043
    Figure 0007954162000043
  • Figure 0007954162000044
    Figure 0007954162000044
  • Figure 0007954162000045
    Figure 0007954162000045
Patent Text Reader

Abstract

Provided are an epoxy resin composition that exhibits excellent low dielectric characteristics, a polyhydric hydroxy resin and / or an epoxy resin that provides the epoxy resin composition, and a method for producing those. The polyhydric hydroxy resin is characterized by being represented by general formula (1). Each R21 independently represents a hydrogen atom, a dicyclopentenyl group represented by formula (2a) or formula (2b), a group represented by formula (3a), or a group represented by formula (3b).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a polyvalent hydroxy resin or epoxy resin that exhibits excellent low viscosity and low dielectric properties, and a method for producing the same. [Background technology]

[0002] Epoxy resins are used in a wide range of applications, including paints, civil engineering adhesives, casting, electrical and electronic materials, and film materials, due to their excellent adhesive properties, flexibility, heat resistance, chemical resistance, insulation, and curing reaction. In particular, they are widely used in printed circuit board applications, a type of electrical and electronic material, by imparting flame retardancy to epoxy resins.

[0003] In recent years, information devices have become smaller and more high-performance at an accelerating pace, and consequently, materials used in the fields of semiconductors and electronic components are required to have higher performance than ever before. In particular, epoxy resin compositions used as materials for electrical and electronic components require low dielectric properties to accommodate the thinning and high-performance nature of substrates.

[0004] Until now, dicyclopentadienephenol resins with aliphatic skeletons have been used to lower the dielectric constant for laminate applications, but these have been ineffective in improving the dielectric loss tangent, and have not provided satisfactory low viscosity for increasing the amount of filler (Patent Documents 1 and 2). Furthermore, although dielectric properties have been improved by using aromatically modified dicyclopentadienephenol resins, it has not been possible to achieve both low dielectric properties and low viscosity (Patent Document 3). [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2001-240654 [Patent Document 2] Japanese Patent Application Publication No. 5-339341 [Patent Document 3] Japanese Patent Publication No. 2016-69524 [Overview of the Initiative]

[0006] Therefore, the problem that the present invention aims to solve is to provide polyvalent hydroxy resins and epoxy resins thereof that exhibit excellent dielectric loss tangent and yield cured products with good low viscosity, epoxy resin compositions using the same, and methods for producing the same.

[0007] As a result of various studies conducted by the inventors to solve the above problems, it was discovered that by reacting a dicyclopentadiene-type phenolic resin with dicyclopentadiene in a specific ratio, and then reacting it with an aromatic vinyl compound, a dicyclopentadiene skeleton derived from dicyclopentadiene and an aromatic skeleton derived from the aromatic vinyl compound can be added to the phenol ring of the dicyclopentadiene-type phenolic resin. Furthermore, it was discovered that the epoxy resin obtained when this phenolic resin is epoxidized exhibits excellent low viscosity, and when cured with a curing agent, the resulting cured product exhibits excellent low dielectric properties, thus completing the present invention. It should also be noted that the aromatic vinyl compound can be reacted with the dicyclopentadiene-type phenolic resin first, and then with dicyclopentadiene.

[0008] In other words, the present invention is a polyvalent hydroxy resin (A) characterized by being represented by the following general formula (1). [ka] Here, R1 independently represents a hydrocarbon group having 1 to 8 carbon atoms. R21 independently represents a hydrogen atom, a dicyclopentenyl group represented by formula (2a) or formula (2b), a group represented by formula (3a), or a group represented by formula (3b), of which at least two are a dicyclopentenyl group represented by formula (2a) or formula (2b) and the other is a group represented by formula (3a) or formula (3b). R3 independently represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms. R4 independently represents a hydrogen atom or a group represented by formula (3a). A1 is a residue obtained by removing two R21 groups from Formula (1), and R21 in the residue is a hydrogen atom, a dicyclopentenyl group represented by Formula (2a) or Formula (2b), or a group represented by Formula (3a). Me represents a methyl group. i is an integer of 0 to 2. n1 represents the number of repeats, and the average value thereof is a number of 0 to 5. p1 represents the number of repeats, and the average value thereof is a number of 0.01 to 3.

[0009] The aforementioned R1 is preferably a methyl group or a phenyl group, and the aforementioned i is preferably 1 or 2.

[0010] The present invention also relates to a method for producing a polyhydric hydroxy resin, characterized by reacting a polyhydric hydroxy resin (a) represented by the following general formula (4), an aromatic vinyl compound (b) represented by the following general formula (5a) and / or general formula (5b), and dicyclopentadiene.

Chemical Formula

Chemical Formula

[0011] The aforementioned production method is preferably carried out in the presence of an acid catalyst, and it is preferred to react 0.05 to 2.0 moles of the aforementioned aromatic vinyl compound (b) and 0.05 to 2.0 moles of the aforementioned dicyclopentadiene per 1 mole of phenolic hydroxyl groups of the aforementioned polyhydric hydroxy resin (a) at a reaction temperature of 50 to 200°C.

[0012] The present invention also relates to an epoxy resin characterized by being represented by the following general formula (6).

Chemical Formula

[0013] Further, the present invention is a method for producing an epoxy resin, characterized by reacting 1 to 20 moles of an epihalohydrin with 1 mole of phenolic hydroxyl groups of the above polyhydric hydroxy resin (A) in the presence of an alkali compound.

[0014] Further, the present invention is an epoxy resin composition containing an epoxy resin and a curing agent, characterized by comprising the above polyhydric hydroxy resin (A) and / or the above epoxy resin as essential components.

[0015] Further, the present invention is a cured product obtained by curing the above epoxy resin composition, and is a prepreg, a laminate, or a printed wiring board using the above epoxy resin composition.

[0016] The present invention provides a manufacturing method in which a dicyclopentadiene-type phenolic resin is reacted with dicyclopentadiene, and then further reacted with an aromatic vinyl compound, thereby adding a dicyclopentenyl group derived from dicyclopentadiene and an aromatic skeleton derived from the aromatic vinyl compound to the phenolic ring of the dicyclopentadiene-type phenolic resin. Furthermore, the cured product using the polyvalent hydroxy resin and / or epoxy resin obtained by this manufacturing method exhibits excellent dielectric properties and provides an epoxy resin composition with excellent copper foil peel strength and interlayer adhesion strength for printed circuit board applications. [Brief explanation of the drawing]

[0017] [Figure 1] This is the GPC chart for the polyvalent hydroxy resin obtained in Example 1. [Figure 2] This is the IR chart of the polyvalent hydroxy resin obtained in Example 1. [Figure 3] This is the GPC chart of the epoxy resin obtained in Example 7. [Figure 4] This is the IR chart of the epoxy resin obtained in Example 7. [Modes for carrying out the invention]

[0018] The embodiments of the present invention will be described in detail below. The polyvalent hydroxy resin (also known as phenolic resin) of the present invention is a polyvalent hydroxy resin (A) represented by the following general formula (1). [ka] This polyvalent hydroxy resin (A) is advantageously obtained by reacting a dicyclopentadiene-type polyvalent hydroxy resin (a) represented by the above general formula (4) with dicyclopentadiene in the presence of a Lewis acid, and then reacting it with an aromatic vinyl compound (b) represented by the above general formulas (5a) and (5b). Here, the polyvalent hydroxy resin (a) has a structure in which phenols are linked by dicyclopentadiene. The polyvalent hydroxy resin (A) of the present invention is a dicyclopentadiene-type polyvalent hydroxy resin (a) in which cyclopentadiene or an aromatic vinyl compound (b) is added to the phenol ring.

[0019] In general formula (1), R1 represents a hydrocarbon group having 1 to 8 carbon atoms, and is preferably an alkyl group having 1 to 8 carbon atoms, an aryl group having 6 to 8 carbon atoms, an aralkyl group having 7 to 8 carbon atoms, or an allyl group. C1-C8 alkyl groups can be linear, branched, or cyclic, and examples include methyl, ethyl, propyl, isopropyl, n-butyl, t-butyl, hexyl, cyclohexyl, and methylcyclohexyl groups. Examples of aryl groups having 6 to 8 carbon atoms include phenyl, tolyl, xylyl, and ethylphenyl groups. Examples of aralkyl groups with 7 to 8 carbon atoms include the benzyl group and the α-methylbenzyl group. Among these substituents, phenyl groups and methyl groups are preferred, with methyl groups being particularly preferred, from the viewpoint of ease of availability and reactivity when cured. The substitution site of R1 may be ortho, meta, or para, but the ortho position is preferred.

[0020] R21 independently represents a hydrogen atom, a dicyclopentenyl group represented by formula (2a) or formula (2b), or a group represented by formula (3a) or formula (3b), of which at least two are dicyclopentenyl groups represented by formula (2a) or formula (2b) and the other is a group represented by formula (3a) or formula (3b). Unlike the substituent R1, R21 does not necessarily represent only a substituent, but also a hydrogen atom.

[0021] The dicyclopentenyl group is a group derived from dicyclopentadiene and is represented by the following formula (2a) or formula (2b). [ka]

[0022] The bases represented by formula (3a) or formula (3b) are as follows: [ka] The group represented by formula (3a) is derived from the monovinyl compound represented by the following general formula (5a) among the aromatic vinyl compounds (b) that are raw materials for the polyvalent hydroxy resin (A) represented by general formula (1), and the group represented by formula (3b) is derived from the divinyl compound represented by the following general formula (5b) among the aromatic vinyl compounds (b).

[0023] [ka]

[0024] In formula (1), i is the number of substituents R1, which is 0 to 2, preferably 1 or 2, and more preferably 2.

[0025] In equation (1), n1 is a repeating number, which is a number greater than or equal to 0, and its mean value (number mean) is between 0 and 5, preferably between 1.0 and 4.0, more preferably between 1.1 and 3.0, and even more preferably between 1.2 and 2.5.

[0026] In formula (3a), R3 represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms. Examples of hydrocarbon groups having 1 to 8 carbon atoms are the same as those for R1. Like R21, R3, unlike R1 which is a substituent, does not necessarily represent only a substituent, but can also represent a hydrogen atom. When using a monovinyl compound represented by formula (5a) as a raw material for a polyvalent hydroxy resin (A) represented by general formula (1), R3 is preferably a hydrogen atom, a methyl group, or an ethyl group, with a hydrogen atom or an ethyl group being particularly preferred, from the viewpoint of ease of availability and heat resistance of the cured product. When using a divinyl compound represented by formula (5b) as a raw material, R3 may include a vinyl group. Furthermore, the substitution position of R3 may be ortho, meta, or para, but meta and para are preferred. Preferably, one of the R3 groups is an ethyl group, and the rest are hydrogen atoms.

[0027] In formula (3b), A1 is a residue obtained by removing two R21 groups from general formula (1), where R21 is either a hydrogen atom or the group represented by formula (3a). In other words, A1 is a divalent group with a structure similar to general formula (1), but it does not contain the group represented by formula (3b).

[0028] R3 in equation (3b) is equivalent to R3 in equation (3a). R4 represents a hydrogen atom or a group represented by formula (3a). Like R21 and R3, R4 differs from R1, which is a substituent, in that it does not necessarily represent only a substituent, but also a hydrogen atom. p1 is the number of repetitions, and its mean (number mean) is between 0.01 and 3, preferably between 0.1 and 2.0, more preferably between 0.2 and 1.0, and even more preferably between 0.3 and 0.8.

[0029] The weight-average molecular weight (Mw) of the polyvalent hydroxy resin (A) of the present invention is preferably 400 to 2200, more preferably 500 to 1600, even more preferably 600 to 1200, and particularly preferably 800 to 1000. The number-average molecular weight (Mn) is preferably 300 to 1500, more preferably 400 to 1000. The phenolic hydroxyl group equivalent (g / eq.) is preferably 200 to 500, more preferably 250 to 500, and even more preferably 270 to 400. In general formula (1), preferably, the area percentage of n1=0 is 20% or less, the area percentage of n1=1 is 40 to 90%, and the area percentage of n1=2 or more is 0 to 60%. The softening point is preferably 50 to 180°C, and more preferably 50 to 120°C. The polyvalent hydroxy resin (A) of the present invention exhibits low viscosity, with a melt viscosity of 0.01 to 1.0 Pa·s at 150°C. Preferably, it is 0.03 to 0.7 Pa·s, and more preferably 0.05 to 0.5 Pa·s.

[0030] The polyvalent hydroxy resin (A) of the present invention can be obtained by reacting a polyvalent hydroxy resin (a) represented by the following general formula (4) with an aromatic vinyl compound (b) represented by the following general formula (5a) and / or general formula (5b) with dicyclopentadiene represented by formula (5c). [ka] Here, R1 and i are equivalent to their definitions in general formula (1), and m is equivalent to n1 in general formula (1). [ka]

[0031] In general formula (5a), R3 represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms. Examples of hydrocarbon groups having 1 to 8 carbon atoms are the same as those for R1. From the viewpoint of availability and the heat resistance of the cured product, a hydrogen atom, a methyl group, or an ethyl group are preferred for R3, with a hydrogen atom and an ethyl group being particularly preferred. The substitution position of R3 may be ortho, meta, or para, but meta and para positions are preferred.

[0032] In general formula (5b), the substitution position of the vinyl group may be ortho, meta, or para, but meta and para are preferred, and a mixture thereof may also be used.

[0033] The aromatic vinyl compound (b) used as a raw material must be a monovinyl compound (a compound represented by general formula (5a)) and may also contain a divinyl compound (a compound represented by general formula (5b)). The higher the amount of divinyl compound, the higher the molecular weight of the polyvalent hydroxy resin (A). Therefore, the amount of divinyl compound should be adjusted while taking into account the molecular weight of the polyvalent hydroxy resin (a) used as a raw material to achieve the desired molecular weight. The monovinyl compound undergoes an addition reaction to become substituent R21 or R4 represented by formula (3a), exhibiting a dielectric property reduction effect.

[0034] Examples of monovinyl compounds include vinyl aromatic compounds such as styrene, vinylnaphthalene, vinylbiphenyl, and α-methylstyrene; nuclear alkyl-substituted vinyl aromatic compounds such as o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, o-ethylvinylbenzene, m-ethylvinylbenzene, p-ethylvinylbenzene, ethylvinylbiphenyl, and ethylvinylnaphthalene; and cyclic vinyl aromatic compounds such as indene, acenaphthylene, benzothiophene, and coumarone. Styrene and ethylvinylbenzene are preferred. These can be used individually or in combination of two or more.

[0035] Examples of divinyl compounds include divinyl aromatic compounds such as divinylbenzene, divinylnaphthalene, and divinylbiphenyl. Divinylbenzene is preferred. These can be used individually or in combination of two or more.

[0036] The proportions of monovinyl compound and divinyl compound should be such that the monovinyl compound is 15-50% by mass and the divinyl compound is 50-85% by mass relative to the total amount of vinyl compound. Preferably, the monovinyl compound is 30-50% by mass, more preferably 40-50% by mass. Preferably, the divinyl compound is 50-70% by mass, more preferably 50-60% by mass.

[0037] The polyvalent hydroxy resin (a) represented by the above general formula (4) is obtained by reacting dicyclopentadiene with a phenol represented by the following general formula (9) in the presence of a Lewis acid. [ka] Here, R1 and i are equivalent to their definitions in general formula (1).

[0038] The phenolic hydroxyl group equivalent (g / eq.) of this polyvalent hydroxy resin (a) is preferably 160 to 220, more preferably 165 to 210, and even more preferably 170 to 200. In terms of GPC content, it is preferable that the m=0 compound is within 10 area percent or less, the m=1 compound is within 50 to 90 area percent, and the m=2 or more compound is within 0 to 50 area percent.

[0039] Examples of phenols represented by general formula (9) include phenol, cresol, ethylphenol, propylphenol, isopropylphenol, n-butylphenol, t-butylphenol, hexylphenol, cyclohexylphenol, phenylphenol, tolylphenol, benzylphenol, α-methylbenzylphenol, allylphenol, dimethylphenol, diethylphenol, dipropylphenol, diisopropylphenol, di(n-butyl)phenol, di(t-butyl)phenol, dihexylphenol, dicyclohexylphenol, diphenylphenol, ditolylphenol, dibenzylphenol, bis(α-methylbenzyl)phenol, methylethylphenol, methylpropylphenol, methylisopropylphenol, methylbutylphenol, methyl-t-butylphenol, methylallylphenol, tolylphenylphenol, etc. From the viewpoint of ease of availability and reactivity when cured, phenol, cresol, phenylphenol, dimethylphenol, and diphenylphenol are preferred, and cresol and dimethylphenol are particularly preferred.

[0040] The catalyst used in this reaction is a Lewis acid, specifically boron trifluoride, boron trifluoride-phenol complex, boron trifluoride-ether complex, aluminum chloride, tin chloride, zinc chloride, iron chloride, etc., but boron trifluoride-ether complex is preferred due to its ease of handling. In the case of boron trifluoride-ether complex, the amount of catalyst used is 0.001 to 20 parts by mass, preferably 0.5 to 10 parts by mass, per 100 parts by mass of dicyclopentadiene.

[0041] The amount of dicyclopentadiene used is 0.08 to 0.80 moles, preferably 0.09 to 0.60 moles, more preferably 0.10 to 0.50 moles, even more preferably 0.10 to 0.40 moles, and particularly preferably 0.10 to 0.20 moles, per mole of phenols.

[0042] This reaction is best carried out by charging phenols and a catalyst into a reactor and adding dicyclopentadiene dropwise over 0.1 to 10 hours, preferably 0.5 to 8 hours, and more preferably 1 to 6 hours.

[0043] The reaction temperature is preferably 50 to 200°C, more preferably 100 to 180°C, and even more preferably 120 to 160°C. The reaction time is preferably 1 to 10 hours, more preferably 3 to 10 hours, and even more preferably 4 to 8 hours.

[0044] After the reaction is complete, alkalis such as sodium hydroxide, potassium hydroxide, and calcium hydroxide are added to deactivate the catalyst. Then, solvents such as aromatic hydrocarbons such as toluene and xylene, or ketones such as methyl ethyl ketone and methyl isobutyl ketone are added to dissolve the mixture. After washing with water, the solvent is recovered under reduced pressure to obtain the desired dicyclopentadienephenol resin represented by general formula (4). It is preferable to react as much of the dicyclopentadiene as possible and recover any unreacted phenolic raw materials under reduced pressure.

[0045] During the reaction, solvents such as aromatic hydrocarbons like benzene, toluene, and xylene, ketones like methyl ethyl ketone and methyl isobutyl ketone, halogenated hydrocarbons like chlorobenzene and dichlorobenzene, and ethers like ethylene glycol dimethyl ether and diethylene glycol dimethyl ether may be used as needed.

[0046] A reaction method for introducing a dicyclopentenyl group corresponding to R21 of the polyvalent hydroxy resin (A) represented by general formula (1) to the polyvalent hydroxy resin (a) represented by general formula (4) is to react the polyvalent hydroxy resin (a) with dicyclopentadiene in a predetermined ratio in the presence of a Lewis acid. The reaction ratio is 0.05 to 2.0 moles of dicyclopentadiene per mole of phenolic hydroxyl groups of the polyvalent hydroxy resin (a), more preferably 0.1 to 1.0 moles, even more preferably 0.15 to 0.80 moles, and particularly preferably 0.20 to 0.70 moles. Other reaction conditions are preferably the same as those in the production method for obtaining the polyvalent hydroxy resin (a). This reaction may be carried out immediately after the synthesis of the polyvalent hydroxy resin (a) without removing the product from the reaction system.

[0047] To confirm that a dicyclopentenyl group has been introduced into the polyvalent hydroxy resin (A), mass spectrometry and FT-IR measurement can be used. Here, the tricyclo[5.2.1.0 2,6 It can be seen that the dicyclopentenyl group, introduced as substituent (R21) of the polyvalent hydroxy resin (A) of formula (1), is not a decanediyl group. When using mass spectrometry, electrospray mass spectrometry (ESI-MS) or field desorption (FD-MS) can be employed. By subjecting a sample, in which components with different numbers of nuclei have been separated by GPC or similar methods, to mass spectrometry, it is possible to confirm the introduction of dicyclopentenyl groups. When using the FT-IR measurement method, a sample dissolved in an organic solvent such as THF is applied onto a KRS-5 cell, the organic solvent is dried, and the resulting cell with a sample thin film is measured by FT-IR, a peak derived from the C-O stretching vibration in the phenol nucleus appears at 1210 cm -1 It appears in the vicinity, and only when the dicyclopentenyl group is introduced, a peak derived from the C-H stretching vibration of the olefin moiety of the dicyclopentadiene skeleton appears at 3040 cm -1 Appears in the vicinity. The dicyclopentadiene incorporated into the main chain has no olefin moiety and thus is not detected, and only the olefin of the dicyclopentenyl group introduced as the substituent (R21) can be measured. When the line connecting the start and end of the target peak in a straight line is taken as the baseline, and the length from the peak vertex to the baseline is taken as the peak height, at 3040 cm -1 The nearby peak (A 3040 ) and 1210 cm -1 The nearby peak (A 1210 ), the introduction amount of the dicyclopentenyl group can be quantified by the ratio (A 3040 / A 1210 ). The preferred ratio (A 3040 / A 1210 ) for satisfying the target physical properties is 0.01 or more, more preferably 0.05 or more, and even more preferably 0.10 or more. The upper limit is preferably 0.7 or less, more preferably 0.60 or less. A higher ratio means that a larger number of dicyclopentadiene substituents are introduced.

[0048] As the reaction method for introducing the aromatic skeleton structure of formula (3a) or formula (3b) into the polyhydric hydroxy resin (a), it is a method of reacting the aromatic vinyl compound (b) with the polyhydric hydroxy resin (a) at a predetermined ratio. The reaction ratio is 0.05 to 2.0 mol of the aromatic vinyl compound (b) per 1 mol of the phenolic hydroxyl group of the polyhydric hydroxy resin (a), more preferably 0.1 to 1.0 mol, even more preferably 0.20 to 0.80 mol, and particularly preferably 0.30 to 0.70 mol.

[0049] The catalyst used in the reaction is an acid catalyst, specifically including mineral acids such as hydrochloric acid, sulfuric acid, and phosphoric acid; organic acids such as formic acid, oxalic acid, trifluoroacetic acid, and p-toluenesulfonic acid; Lewis acids such as zinc chloride, aluminum chloride, iron chloride, and boron trifluoride; or solid acids such as activated clay, silica-alumina, and zeolite. Among these, p-toluenesulfonic acid is preferred due to its ease of handling. In the case of p-toluenesulfonic acid, the amount of catalyst used is 0.001 to 20 parts by mass, preferably 0.5 to 10 parts by mass, per 100 parts by mass of polyvalent hydroxy resin (a).

[0050] This reaction is preferably carried out by charging a polyvalent hydroxy resin (a), a catalyst, and a solvent into a reactor, dissolving them, and then adding the aromatic vinyl compound (b) dropwise over 0.1 to 10 hours, preferably 0.5 to 8 hours, and more preferably 0.5 to 5 hours.

[0051] The reaction temperature is preferably 50 to 200°C, more preferably 100 to 180°C, and even more preferably 120 to 160°C. The reaction time is preferably 1 to 10 hours, more preferably 3 to 10 hours, and even more preferably 4 to 8 hours.

[0052] After the reaction is complete, alkalis such as sodium hydroxide, potassium hydroxide, and calcium hydroxide are added to deactivate the catalyst. Then, solvents such as aromatic hydrocarbons like toluene and xylene, or ketones like methyl ethyl ketone and methyl isobutyl ketone are added to dissolve the catalyst. After washing with water, the solvent is recovered under reduced pressure to obtain the desired phenolic resin.

[0053] The solvents used in the reaction include aromatic hydrocarbons such as benzene, toluene, and xylene; ketones such as methyl ethyl ketone and methyl isobutyl ketone; halogenated hydrocarbons such as chlorobenzene and dichlorobenzene; and ethers such as ethylene glycol dimethyl ether and diethylene glycol dimethyl ether. These solvents may be used individually or in mixtures of two or more.

[0054] The reaction to introduce a dicyclopentenyl group into the polyvalent hydroxy resin (a) and the reaction to introduce the aromatic skeleton structure of formula (3a) or formula (3b) can be carried out in any order. Due to the ease of the reaction, it is preferable to react the polyvalent hydroxy resin (a) with dicyclopentadiene first, and then with the aromatic vinyl compound (b). Alternatively, by controlling the reaction conditions between the phenols represented by general formula (9) and dicyclopentadiene, the polyvalent hydroxy resin (a1) represented by general formula (10) can be obtained without isolating the polyvalent hydroxy resin (a) represented by general formula (4), and a predetermined amount of aromatic vinyl compound (b) can be used to introduce the aromatic skeleton structure of formula (3a) or formula (3b). Furthermore, the reaction intermediate obtained by reacting the polyvalent hydroxy resin (a) with dicyclopentadiene is synonymous with the polyvalent hydroxy resin (a1). [ka] Here, R1 and i are equivalent to their definitions in general formula (1). R22 represents a hydrogen atom or a dicyclopentenyl group represented by formula (2a) or formula (2b), and at least one of them is a dicyclopentenyl group represented by formula (2a) or formula (2b). k1 represents the number of repetitions, and its average value is between 0 and 5.

[0055] Furthermore, from the viewpoint of controlling the molecular weight distribution, a predetermined amount of an aromatic vinyl compound (b) may be reacted with a polyvalent hydroxy resin (a) represented by general formula (4), and then a predetermined amount of dicyclopentadiene may be reacted. In this case, the reaction intermediate before the reaction with dicyclopentadiene is a polyvalent hydroxy resin (a2) represented by the following general formula (11). [ka] Here, R1 and i are equivalent to their definitions in general formula (1). R23 represents a hydrogen atom, a group represented by formula (3a), or a group represented by formula (3d), and at least one of them is a group represented by formula (3a) or formula (3d). R3, R4, and Me are equivalent to their definitions in equation (3b). A2 is a residue obtained by removing two R23 groups from general formula (11), where R23 is either a hydrogen atom or a group represented by formula (3a). k2 represents the number of repetitions, and its average value is between 0 and 5. p2 represents the number of repetitions, and its average value is between 0.01 and 3.

[0056] The epoxy resin of the present invention is represented by general formula (6). This epoxy resin is obtained by reacting the polyvalent hydroxy resin (A) of the present invention with an epihalohydrin such as epichlorohydrin. This reaction is carried out according to conventionally known methods.

[0057] In general formula (6), R1 and i have the same definitions as in general formula (1), and n3 has the same definition as n1 in general formula (1), although this is almost the same even in the case of raw material and product relationship. R2 independently represents a hydrogen atom, a dicyclopentenyl group, or a group represented by formula (3a) or formula (3c), of which at least two are a dicyclopentenyl group and the other is a group represented by formula (3a) or formula (3c). Unlike R1, which is a substituent, R2 does not necessarily represent only a substituent, but also a hydrogen atom.

[0058] In formula (3c), R3, R4, and Me have the same meanings as in formula (3b). p has the same meaning as p1 in formula (3b), although it is almost the same even in the case of raw material and product relationship. A is the residue obtained by removing two R2s from formula (3c), and the R2s in the residue are hydrogen atoms or the group represented by formula (3a). In other words, A is a divalent group with a structure similar to general formula (3c), but it can never be the group represented by formula (3c).

[0059] For example, epoxidation can be performed by adding an alkali metal hydroxide such as sodium hydroxide in solid or concentrated aqueous form to a mixture of phenol resin and an excess molar amount of epihalohydrin relative to the hydroxyl groups of the phenol resin, and reacting the mixture at a reaction temperature of 30 to 120°C for 0.5 to 10 hours, or by adding a quaternary ammonium salt such as tetraethylammonium chloride as a catalyst to a phenol resin and an excess molar amount of epihalohydrin, reacting the mixture at a temperature of 50 to 150°C for 1 to 5 hours, and then adding an alkali metal hydroxide such as sodium hydroxide in solid or concentrated aqueous form to the resulting polyhalohydrin ether and reacting the mixture at a temperature of 30 to 120°C for 1 to 10 hours.

[0060] In the above reaction, the amount of epihalohydrin used is 1 to 20 times the molar amount relative to the hydroxyl groups of the phenol resin, preferably 2 to 8 times. The amount of alkali metal hydroxide used is 0.85 to 1.15 times the molar amount relative to the hydroxyl groups of the phenol resin.

[0061] Since the epoxy resin obtained from these reactions contains unreacted epihalohydrins and alkali metal halides, the unreacted epihalohydrins can be removed from the reaction mixture by evaporation, and the alkali metal halides can be removed by methods such as extraction with water or filtration to obtain the desired epoxy resin.

[0062] The epoxy equivalent (g / eq.) of the epoxy resin of the present invention is preferably 200 to 4000, more preferably 250 to 2000, even more preferably 300 to 1000, and particularly preferably 350 to 500. In particular, when dicyandiamide is used as a curing agent, the epoxy equivalent is preferably 300 or more in order to prevent the precipitation of dicyandiamide crystals on the prepreg. In terms of content according to GPC, the molecular weight distribution of the raw material polyvalent hydroxy resin (A) is maintained almost as is, and in general formula (6), preferably, the n3=0 isomer is in the range of 20 area% or less, the n3=1 isomer is in the range of 40 to 90 area%, and the n3=2 or more isomers are in the range of 0 to 60 area%. The total chlorine content is preferably 2000 ppm or less, and more preferably 1500 ppm or less. The epoxy resin of the present invention exhibits low viscosity, with a melt viscosity of 0.01 to 1.0 Pa·s at 150°C. Preferably, it is 0.05 to 0.7 Pa·s, and more preferably 0.1 to 0.5 Pa·s.

[0063] An epoxy resin composition of the present invention can be obtained by using the polyvalent hydroxy resin and / or the epoxy resin of the present invention. The epoxy resin composition of the present invention comprises an epoxy resin and a curing agent as essential components. In this embodiment, part or all of the curing agent is the polyvalent hydroxy resin of the present invention, part or all of the epoxy resin is the epoxy resin of the present invention, or part or all of the curing agent is the polyvalent hydroxy resin of the present invention and part or all of the epoxy resin is the epoxy resin of the present invention.

[0064] Preferably, at least 30% by mass of the curing agent is the polyvalent hydroxy resin of the present invention, or at least 30% by mass of the epoxy resin is the epoxy resin of the present invention. More preferably, each is contained at 50% by mass or more, and even more preferably at 70% by mass. If the amount is less than this, the dielectric properties may deteriorate. In other words, if 30% by mass or more of the curing agent is the polyvalent hydroxy resin of the present invention, the epoxy resin does not need to be the epoxy resin of the present invention, and if the polyvalent hydroxy resin of the present invention is less than 30% by mass of the curing agent, it is essential that 30% by mass or more of the epoxy resin is the epoxy resin of the present invention.

[0065] As the epoxy resin used to obtain the epoxy resin composition of the present invention, one or more types of epoxy resins may be used in combination as needed.

[0066] Any conventional epoxy resin having two or more epoxy groups in its molecule can be used in combination with this product. For example, trifunctional epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, tetramethylbisphenol F type epoxy resin, hydroquinone type epoxy resin, biphenyl type epoxy resin, stilbene type epoxy resin, bisphenol fluorene type epoxy resin, bisphenol S type epoxy resin, bisthioether type epoxy resin, resorcinol type epoxy resin, biphenyl aralkylphenol type epoxy resin, naphthalenediol type epoxy resin, phenol novolac type epoxy resin, aromatic modified phenol novolac type epoxy resin, cresol novolac type epoxy resin, alkyl novolac type epoxy resin, bisphenol novolac type epoxy resin, binaphthol type epoxy resin, naphthol novolac type epoxy resin, β-naphthol aralkyl type epoxy resin, dinaphthol aralkyl type epoxy resin, α-naphthol aralkyl type epoxy resin, trisphenylmethane type epoxy resin, and tetrafunctional epoxy resins such as tetrakisphenylethane type epoxy resin. Other examples of epoxy resins include, but are not limited to, dicyclopentadiene-type epoxy resins, polyhydric alcohol polyglycidyl ethers such as 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, trimethylolethane polyglycidyl ether, and pentaerythritol polyglycidyl ether; alkylene glycol-type epoxy resins such as propylene glycol diglycidyl ether; aliphatic cyclic epoxy resins such as cyclohexanedimethanol diglycidyl ether; glycidyl esters such as dimer acid polyglycidyl esters; glycidylamine-type epoxy resins such as phenyl diglycidylamine, tol diglycidylamine, diaminodiphenylmethane tetraglycidylamine, and aminophenol-type epoxy resins; alicyclic epoxy resins such as Celoxide 2021P (manufactured by Daicel Corporation); phosphorus-containing epoxy resins; bromine-containing epoxy resins; urethane-modified epoxy resins; and oxazolidone ring-containing epoxy resins.Furthermore, these epoxy resins may be used individually or in combination of two or more types. From the viewpoint of availability, it is even more preferable to use epoxy resins represented by the following general formula (13), or dicyclopentadiene type epoxy resins other than those of the present invention, naphthalenediol type epoxy resins, phenol novolac type epoxy resins, aromatic modified phenol novolac type epoxy resins, cresol novolac type epoxy resins, α-naphthol aralkyl type epoxy resins, dicyclopentadiene type epoxy resins, phosphorus-containing epoxy resins, or oxazolidone ring-containing epoxy resins.

[0067] [ka] Here, R5 independently represents a hydrocarbon group having 1 to 8 carbon atoms, such as an alkyl group including a methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, t-butyl group, n-hexyl group, or cyclohexyl group, and may be the same or different from each other. X represents a divalent organic group, such as an alkylene group including a methylene group, ethylene group, isopropyledene group, isobutylene group, hexafluoroisopropylidene group, -CO-, -O-, -S-, -SO2-, -SS-, or an aralkylene group represented by formula (13a). R6 independently represents a hydrogen atom or a hydrocarbon group having one or more carbon atoms, for example, a methyl group, and may be the same or different from each other. Ar is a benzene ring or a naphthalene ring, and these benzene rings or naphthalene rings may have substituents such as an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an aryl group having 6 to 11 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, an aryloxy group having 6 to 11 carbon atoms, or an aralkyloxy group having 7 to 12 carbon atoms.

[0068] As a curing agent, in addition to the polyvalent hydroxy resin (A) of general formula (1), one or more commonly used curing agents such as various phenolic resins, acid anhydrides, amines, cyanate esters, activated esters, hydrazides, acidic polyesters, and aromatic cyanates may be used in combination as needed. When these curing agents are used in combination, the amount of the combined curing agent is preferably 70% by mass or less, and more preferably 50% by mass or less, of the total curing agent. If the proportion of the combined curing agent is too high, the dielectric properties of the epoxy resin composition may deteriorate.

[0069] In the epoxy resin composition of the present invention, the molar ratio of active hydrogen groups of the curing agent to 1 mole of epoxy groups of the total epoxy resin is preferably 0.2 to 1.5 moles, more preferably 0.3 to 1.4 moles, even more preferably 0.5 to 1.3 moles, and particularly preferably 0.8 to 1.2 moles. If the ratio deviates from this range, curing may be incomplete, and good cured properties may not be obtained. For example, when using a phenol resin-based curing agent or an amine-based curing agent, the active hydrogen groups are blended in approximately equimolar amounts to the epoxy groups. When using an acid anhydride-based curing agent, the acid anhydride groups are blended in an amount of 0.5 to 1.2 moles, preferably 0.6 to 1.0 moles, per mole of epoxy groups. When using the phenol resin of the present invention alone as a curing agent, it is desirable to use it in a range of 0.9 to 1.1 moles per mole of epoxy resin.

[0070] In this invention, an active hydrogen group refers to a functional group having active hydrogen that reacts with an epoxy group (including functional groups having latent active hydrogen that generates active hydrogen through hydrolysis, etc., and functional groups that exhibit equivalent curing activity). Specifically, examples include acid anhydride groups, carboxyl groups, amino groups, and phenolic hydroxyl groups. Regarding active hydrogen groups, 1 mole of carboxyl groups or phenolic hydroxyl groups is calculated as 1 mole, and 2 moles of amino groups (-NH2). Furthermore, if the active hydrogen group is not clearly defined, the active hydrogen equivalent can be determined by measurement. For example, the active hydrogen equivalent of the curing agent used can be determined by reacting a monoepoxy resin such as phenyl glycidyl ether, whose epoxy equivalent is known, with a curing agent whose active hydrogen equivalent is unknown, and measuring the amount of monoepoxy resin consumed.

[0071] Specific examples of phenolic resin curing agents that can be used in the epoxy resin composition of the present invention include bisphenol A, bisphenol F, bisphenol C, bisphenol K, bisphenol Z, bisphenol S, tetramethylbisphenol A, tetramethylbisphenol F, tetramethylbisphenol S, tetramethylbisphenol Z, tetrabromobisphenol A, dihydroxydiphenyl sulfide, 4,Bisphenols such as 4'-thiobis(3-methyl-6-t-butylphenol), dihydroxybenzenes such as catechol, resorcinol, methylresorcinol, hydroquinone, monomethylhydroquinone, dimethylhydroquinone, trimethylhydroquinone, mono-t-butylhydroquinone, and di-t-butylhydroquinone, hydroxynaphthalenes such as dihydroxynaphthalene, dihydroxymethylnaphthalene, dihydroxymethylnaphthalene, and trihydroxynaphthalene, phosphorus-containing phenol curing agents such as LC-950PM60 (manufactured by Shin-AT&C), phenol novolac resins such as Shonol BRG-555 (manufactured by Aica Kogyo Co., Ltd.), cresol novolac resins such as DC-5 (manufactured by Nippon Steel Chemical & Material Co., Ltd.), triazine skeleton-containing phenol resins, aromatically modified phenol novolac resins, bisphenol A novolac resins, and trishydroxyphenylmethane-type novolac resins such as Resitopp TPM-100 (manufactured by Gun-ei Chemical Industry Co., Ltd.) Examples include phenol compounds known as novolac phenol resins, such as lipids, phenols and / or naphthols and / or bisphenols such as naphthol novolac resins, condensates of phenols and / or naphthols and / or bisphenols with aldehydes, condensates of phenols and / or naphthols and / or bisphenols such as SN-160, SN-395, SN-485 (manufactured by Nippon Steel Chemical & Material Co., Ltd.) with xylylene glycol, condensates of phenols and / or naphthols and / or bisphenols with isopropenylacetophenone, reaction products of phenols and / or naphthols and / or bisphenols with dicyclopentadiene, reaction products of phenols and / or naphthols and / or bisphenols with divinylbenzene, reaction products of phenols and / or naphthols and / or bisphenols with terpenes, and condensates of phenols and / or naphthols and / or bisphenols with biphenyl crosslinking agents, polybutadiene-modified phenol resins, and phenol resins having spiro rings. From the viewpoint of availability, phenol novolac resins, dicyclopentadienephenol resins, trishydroxyphenylmethane-type novolac resins, aromatically modified phenol novolac resins, etc., are preferred.

[0072] Novolac phenol resin can be obtained from phenols and crosslinking agents. Examples of phenols include phenol, cresol, xylenol, butylphenol, amylphenol, nonylphenol, butylmethylphenol, trimethylphenol, and phenylphenol. Examples of naphthols include 1-naphthol and 2-naphthol. In addition, bisphenols, which were listed as phenol resin curing agents above, can be used. Examples of aldehydes used as crosslinking agents include formaldehyde, acetaldehyde, propylaldehyde, butyraldehyde, valeraldehyde, caproaldehyde, benzaldehyde, chloraldehyde, bromaldehyde, glyoxal, malonaldehyde, succinaldehyde, glutaraldehyde, adipinealdehyde, pimelinaldehyde, sebacinaldehyde, acrolein, crotonaldehyde, salicylaldehyde, phthalaldehyde, and hydroxybenzaldehyde. Examples of biphenyl-based crosslinking agents include bis(methylol)biphenyl, bis(methoxymethyl)biphenyl, bis(ethoxymethyl)biphenyl, and bis(chloromethyl)biphenyl.

[0073] Examples of acid anhydride-based curing agents include maleic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, 4-methylhexahydrophthalic anhydride, methylbicyclo[2.2.1]heptane-2,3-dicarboxylic acid anhydride, bicyclo[2.2.1]heptane-2,3-dicarboxylic acid anhydride, 1,2,3,6-tetrahydrophthalic anhydride, pyromellitic anhydride, phthalic anhydride, trimellitic anhydride, methylnadic acid, copolymers of styrene monomer and maleic anhydride, copolymers of indenes and maleic anhydride, and the like.

[0074] Examples of amine-based curing agents include, specifically, diethylenetriamine, triethylenetetramine, metaxylenediamine, isophoronediamine, diaminodiphenylmethane, diaminodiphenylsulfone, diaminodiphenyl ether, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, polyetheramines, biguanide compounds, dicyandiamide, anisidine and other aromatic amines, and amine compounds such as polyamidoamines, which are condensates of acids such as dimer acids and polyamines.

[0075] The cyanate ester compound is not particularly limited as long as it is a compound having two or more cyanate groups (cyanate ester groups) in one molecule. Examples include novolac-type cyanate ester curing agents such as phenol novolac type and alkylphenol novolac type, naphthol aralkyl-type cyanate ester curing agents, biphenylalkyl-type cyanate ester curing agents, dicyclopentadiene-type cyanate ester curing agents, bisphenol-type cyanate ester curing agents such as bisphenol A type, bisphenol F type, bisphenol E type, tetramethylbisphenol F type, and bisphenol S type, and prepolymers in which these are partially triazined. Specific examples of cyanate ester-based curing agents include, for example, bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate), bis(3-methyl-4-cyanatophenyl)methane, bis(3-ethyl-4-cyanatophenyl)methane, bis(4-cyanatophenyl)-1,1-ethane, 4,4-dicyanate-diphenyl, 2,2-bis(4-cyanatophenyl)-1,1,1,3,3,3-hexafluoropropane, 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidenediphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanato)phenylpropane, 1,1-bis(4-cyanatophenyl Examples include difunctional cyanate resins such as methane, bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanatephenyl-1-(methylethylidene))benzene, bis(4-cyanatephenyl)thioether, and bis(4-cyanatephenyl)ether; cyanate esters of trivalent phenols such as tris(4-cyanatephenyl)-1,1,1-ethane and bis(3,5-dimethyl-4-cyanatephenyl)-4-cyanatephenyl-1,1,1-ethane; polyfunctional cyanate resins derived from phenol novolacs, cresol novolacs, and phenol resins containing dicyclopentadiene structures; and prepolymers in which these cyanate resins are partially triazined. One or more of these can be used.

[0076] While there are no particular restrictions on the active ester curing agent, compounds having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are generally preferred. The active ester curing agent is preferably obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. Particularly from the viewpoint of improving heat resistance, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester curing agent obtained from a carboxylic acid compound and / or a naphthol compound is more preferred. Examples of carboxylic acid compounds include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalein, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadienyldiphenol, dicyclopentadienphenol resin (a precursor of the epoxy resin of the present invention), phenol novolac, and the like. One or more active ester curing agents can be used. As active ester curing agents, specifically, active ester curing agents containing a dicyclopentadienyldiphenol structure, active ester curing agents containing a naphthalene structure, active ester curing agents that are acetylated phenol novolacs, and active ester curing agents that are benzoylated phenol novolacs are preferred, and among these, active ester curing agents containing a dicyclopentadienyldiphenol structure, which is a precursor of the epoxy resin of the present invention, are more preferred in that they are excellent in improving peel strength.

[0077] Other curing agents include, specifically, phosphine compounds such as triphenylphosphine, phosphonium salts such as tetraphenylphosphonium bromide, imidazoles such as 2-methylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, and 1-cyanoethyl-2-methylimidazole, imidazole salts which are salts of imidazoles with trimellitic acid, isocyanuric acid, or boron, etc., quaternary ammonium salts such as trimethylammonium chloride, diazabicyclo compounds, salts of diazabicyclo compounds with phenols or phenol novolac resins, etc., complex compounds of boron trifluoride with amines or ether compounds, aromatic phosphoniums, or iodonium salts.

[0078] A curing accelerator may be used in the epoxy resin composition as needed. Examples of usable curing accelerators include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole; tertiary amines such as 4-dimethylaminopyridine, 2-(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)undecene-7; phosphines such as triphenylphosphine, tricyclohexylphosphine, and triphenylphosphinetriphenylborane; and metal compounds such as tin octylate. When using a curing accelerator, the amount used is preferably 0.02 to 5 parts by mass per 100 parts by mass of the epoxy resin component in the epoxy resin composition of the present invention. By using a curing accelerator, the curing temperature can be lowered and the curing time can be shortened.

[0079] The epoxy resin composition may be used with an organic solvent or reactive diluent to adjust its viscosity.

[0080] Examples of organic solvents include amides such as N,N-dimethylformamide and N,N-dimethylacetamide; ethers such as ethylene glycol monomethyl ether, dimethoxydiethylene glycol, ethylene glycol diethyl ether, diethylene glycol diethyl ether, and triethylene glycol dimethyl ether; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohols such as methanol, ethanol, 1-methoxy-2-propanol, 2-ethyl-1-hexanol, benzyl alcohol, ethylene glycol, propylene glycol, butyl diglycol, and pine oil; and vinegar. Examples of acetate esters such as butyl acid, methoxybutyl acetate, methyl cellosolve acetate, cellosolve acetate, ethyl diglycol acetate, propylene glycol monomethyl ether acetate, carbitol acetate, and benzyl alcohol acetate; benzoic acid esters such as methyl benzoate and ethyl benzoate; cellosolves such as methyl cellosolve, cellosolve, and butyl cellosolve; carbitols such as methyl carbitol, carbitol, and butyl carbitol; aromatic hydrocarbons such as benzene, toluene, and xylene; and dimethyl sulfoxide, acetonitrile, and N-methylpyrrolidone, but are not limited to these.

[0081] Examples of reactive diluents include, but are not limited to, monofunctional glycidyl ethers such as allyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, phenyl glycidyl ether, and tolyl glycidyl ether, as well as monofunctional glycidyl esters such as neodecanoic acid glycidyl ester.

[0082] These organic solvents or reactive diluents are preferably used in the resin composition, either individually or in mixtures of several types, at a non-volatile content of 90% by mass or less, and the appropriate type and amount are selected as appropriate depending on the application. For example, in printed circuit board applications, polar solvents with a boiling point of 160°C or less, such as methyl ethyl ketone, acetone, and 1-methoxy-2-propanol, are preferred, and the amount used in the resin composition is preferably 40 to 80% by mass in terms of non-volatile content. In adhesive film applications, for example, ketones, acetate esters, carbitols, aromatic hydrocarbons, dimethylformamide, dimethylacetamide, and N-methylpyrrolidone are preferred, and the amount used is preferably 30 to 60% by mass in terms of non-volatile content.

[0083] The epoxy resin composition may contain other thermosetting resins or thermoplastic resins to the extent that it does not impair the properties. Examples include, but are not limited to, phenolic resins, benzoxazine resins, bismaleimide resins, bismaleimidotriazine resins, acrylic resins, petroleum resins, indene resins, coumarone indene resins, phenoxy resins, polyurethane resins, polyester resins, polyamide resins, polyimide resins, polyamideimide resins, polyetherimide resins, polyphenylene ether resins, modified polyphenylene ether resins, polyethersulfone resins, polysulfone resins, polyetheretherketone resins, polyphenylene sulfide resins, polyvinyl formal resins, polysiloxane compounds, and alkylene resins containing reactive functional groups such as hydroxyl group-containing polybutadiene.

[0084] Various known flame retardants can be used in the epoxy resin composition to improve the flame retardancy of the resulting cured product. Examples of usable flame retardants include halogen-based flame retardants, phosphorus-based flame retardants, nitrogen-based flame retardants, silicone-based flame retardants, inorganic flame retardants, and organometallic salt-based flame retardants. From an environmental standpoint, halogen-free flame retardants are preferred, and phosphorus-based flame retardants are particularly preferred. These flame retardants may be used individually or in combination of two or more types.

[0085] Phosphorus-based flame retardants can be either inorganic phosphorus compounds or organophosphorus compounds. Examples of inorganic phosphorus compounds include ammonium phosphates such as red phosphorus, monoammonium phosphate, diammonium phosphate, triammonium phosphate, and polyammonium phosphate, as well as inorganic nitrogen-containing phosphorus compounds such as phosphate amides. Examples of organophosphorus compounds include aliphatic phosphate esters, phosphate ester compounds, condensed phosphate esters such as PX-200 (manufactured by Daihachi Chemical Industry Co., Ltd.), phosphazenes, phosphonic acid compounds, phosphinic acid compounds, phosphine oxide compounds, phospholane compounds, and organic nitrogen-containing phosphorus compounds, as well as metal salts of phosphinic acid, cyclic organophosphorus compounds such as 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(2,5-dihydrooxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, and 10-(2,7-dihydrooxynaphthyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, and derivatives obtained by reacting these with compounds such as epoxy resins and phenolic resins, such as phosphorus-containing epoxy resins and phosphorus-containing curing agents.

[0086] The amount of flame retardant added is appropriately selected depending on the type of phosphorus-based flame retardant, the components of the epoxy resin composition, and the desired degree of flame retardancy. For example, the phosphorus content in the organic components (excluding organic solvents) of the epoxy resin composition is preferably 0.2 to 4% by mass, more preferably 0.4 to 3.5% by mass, and even more preferably 0.6 to 3% by mass. If the phosphorus content is too low, it may be difficult to ensure flame retardancy, and if it is too high, it may adversely affect the heat resistance. When using a phosphorus-based flame retardant, a flame retardant aid such as magnesium hydroxide may also be used in combination.

[0087] Fillers may be used in epoxy resin compositions as needed. Specifically, examples include fused silica, crystalline silica, alumina, silicon nitride, aluminum hydroxide, boehmite, magnesium hydroxide, talc, mica, calcium carbonate, calcium silicate, calcium hydroxide, magnesium carbonate, barium carbonate, barium sulfate, boron nitride, carbon, carbon fiber, glass fiber, alumina fiber, silica-alumina fiber, silicon carbide fiber, polyester fiber, cellulose fiber, aramid fiber, ceramic fiber, fine particle rubber, silicone rubber, thermoplastic elastomer, carbon black, and pigments. Generally, the reason for using fillers is to improve impact resistance. In addition, when metal hydroxides such as aluminum hydroxide, boehmite, and magnesium hydroxide are used, they act as flame retardant aids, improving flame retardancy. The amount of these fillers added to the epoxy resin composition is preferably 1 to 150% by mass, and more preferably 10 to 70% by mass. If the amount added is too high, the adhesion required for laminate applications may decrease, and the cured product may become brittle, resulting in insufficient mechanical properties. Furthermore, if the amount of filler used is too small, the intended effects of the filler, such as improved impact resistance of the cured product, may not be realized.

[0088] When epoxy resin compositions are used to form plate-shaped substrates, fibrous materials are preferred as fillers in terms of dimensional stability and flexural strength. More preferably, glass fiber substrates are made by weaving glass fibers into a mesh.

[0089] The epoxy resin composition may further contain various additives as needed, such as silane coupling agents, antioxidants, mold release agents, defoaming agents, emulsifiers, thixotropy-inducing agents, smoothing agents, flame retardants, and pigments. The amount of these additives added is preferably in the range of 0.01 to 20% by mass relative to the epoxy resin composition.

[0090] The epoxy resin composition can be used to create prepregs for use in printed circuit boards and the like by impregnating a fibrous substrate with it. The fibrous substrate can be inorganic fibers such as glass, or woven or nonwoven fabrics of organic fibers such as polyester resin, polyamine resin, polyacrylic resin, polyimide resin, or aromatic polyamide resin, but is not limited to these. The method for producing a prepreg from an epoxy resin composition is not particularly limited, but for example, it can be obtained by immersing the epoxy resin composition in a resin varnish prepared by adjusting the viscosity with an organic solvent, impregnating it, and then heating and drying it to partially cure (B-stage) the resin component. For example, it can be heated and dried at 100 to 200°C for 1 to 40 minutes. Here, the amount of resin in the prepreg is preferably 30 to 80% by mass.

[0091] Furthermore, while the curing method for laminates, commonly used in the manufacture of printed circuit boards, can be used to cure the prepreg, it is not limited to this method. For example, when forming a laminate using a prepreg, one or more prepregs are stacked, metal foil is placed on one or both sides to form a laminate, and this laminate is heated and pressurized to integrate the layers. Here, single, alloy, or composite metal foils of copper, aluminum, brass, nickel, etc., can be used as the metal foil. Then, the prepreg is cured by pressurizing and heating the created laminate to obtain a laminate. At that time, it is preferable to set the heating temperature to 160-220°C, the pressurizing pressure to 5-50 MPa, and the heating and pressurizing time to 40-240 minutes, in order to obtain the desired cured product. If the heating temperature is too low, the curing reaction will not proceed sufficiently, and if it is too high, there is a risk that the epoxy resin composition will begin to decompose. Also, if the pressurizing pressure is too low, air bubbles may remain inside the resulting laminate, which may reduce its electrical properties, and if it is too high, the resin may flow before curing, which may prevent obtaining a cured product of the desired thickness. Furthermore, if the heating and pressurizing time is too short, the curing reaction may not proceed sufficiently, and if it is too long, thermal decomposition of the epoxy resin composition in the prepreg may occur, which is undesirable.

[0092] Epoxy resin compositions can be cured in the same manner as known epoxy resin compositions to obtain a cured epoxy resin product. Methods for obtaining the cured product can be the same as those for known epoxy resin compositions, and methods such as casting, injection, potting, dipping, drip coating, transfer molding, compression molding, etc., or lamination of resin sheets, resin-coated copper foil, prepregs, etc., followed by heating, pressing, and curing to form laminates are preferably used. The curing temperature is typically 100-300°C, and the curing time is typically 1-5 hours.

[0093] The epoxy resin cured product of the present invention can take the form of a laminate, molded product, adhesive product, coating film, film, or the like.

[0094] We prepared epoxy resin compositions and evaluated laminates and cured products by heat curing. As a result, we were able to provide an epoxy-curable resin composition that exhibits excellent low dielectric properties in the cured product. Specifically, the dielectric properties include a relative permittivity of 3.00 or less, more preferably 2.90 or less, and a dielectric loss tangent of 0.015 or less, more preferably 0.011 or less. Furthermore, the glass transition temperature (Tg) of the cured product is 120°C or higher, and it is also possible to raise it to 150°C or higher. [Examples]

[0095] The present invention will be specifically described with reference to examples and comparative examples, but the present invention is not limited to these. Unless otherwise specified, "parts" refers to parts by mass, "%" refers to mass percent, and "ppm" refers to mass ppm. The measurements were performed using the following methods.

[0096] (1) Hydroxyl group equivalent: Measurements were performed in accordance with JIS K0070 standard, and the unit is expressed as "g / eq.". Unless otherwise specified, the hydroxyl group equivalent of phenolic resin refers to the phenolic hydroxyl group equivalent.

[0097] (2) Softening point: Measurements were taken in accordance with the JIS K7234 standard and the ring-sphere method. Specifically, an automatic softening point device (ASP-MG4, manufactured by Maytec Co., Ltd.) was used.

[0098] (3) Epoxy equivalent: Measurements were performed in accordance with JIS K7236 standard, and the unit is expressed as "g / eq.". Specifically, an automatic potentiometric titrator (Hiranuma Sangyo Co., Ltd., COM-1600ST) was used, chloroform was used as the solvent, tetraethylammonium brominated acetate solution was added, and titration was performed with 0.1 mol / L perchloric acid-acetic acid solution.

[0099] (4) Total chlorine content: Measurements were performed in accordance with JIS K7243-3 standard, and the unit was expressed in "ppm". Specifically, diethylene glycol monobutyl ether was used as the solvent, and after adding a 1 mol / L potassium hydroxide 1,2-propanediol solution and heating, the solution was titrated with a 0.01 mol / L silver nitrate solution using an automatic potentiometric titrator (Hiranuma Sangyo Co., Ltd., COM-1700).

[0100] (5) Melt viscosity: The melt viscosity at 150°C was measured using an ICI viscosity analyzer (CV-1S, manufactured by Toa Kogyo Co., Ltd.).

[0101] (6) Relative permittivity and dielectric loss tangent: Measurements were performed in accordance with IPC-TM-650 2.5.5.9. Specifically, the samples were dried in an oven set to 105°C for 2 hours, cooled in a desiccator, and then evaluated by determining the relative permittivity and dielectric loss tangent at a frequency of 1 GHz using the capacitance method with a material analyzer manufactured by AGILENT Technologies.

[0102] (7) Copper foil peel strength and interlayer adhesion: The interlayer adhesion strength was measured by peeling the material between the 7th and 8th layers, in accordance with JIS C6481.

[0103] (8) GPC (Gel Permeation Chromatography) measurement: A system consisting of a main unit (Tosoh Corporation, HLC-8220GPC) and columns (Tosoh Corporation, TSKgelG4000HXL, TSKgelG3000HXL, TSKgelG2000HXL) connected in series was used, with the column temperature set to 40°C. Tetrahydrofuran (THF) was used as the eluent at a flow rate of 1 mL / min, and a differential refractive index detector was used. For the measurement sample, 0.1 g of the sample was dissolved in 10 mL of THF, filtered through a microfilter, and 50 μL of the resulting sample was used. Data processing was performed using Tosoh Corporation's GPC-8020 Model II version 6.00.

[0104] (9) IR (Infrared Absorption Spectrum): Using a Fourier transform infrared spectrophotometer (Perkin Elmer Precisely, Spectrum One FT-IR Spectrumeter 1760X), sodium chloride was used as the cell. The sample, dissolved in chloroform, was coated onto the cell, dried, and then measured at wavenumbers of 450-4000 cm⁻¹. -1 The transmittance was measured.

[0105] (10) ESI-MS: Mass spectrometry was performed using a mass spectrometer (Shimadzu Corporation, LCMS-2020) with acetonitrile and water as the mobile phases, by measuring the sample dissolved in acetonitrile.

[0106] The abbreviations used in the examples and comparative examples are as follows:

[0107] [Epoxy resin] E1: Epoxy resin obtained in Example 7 E2: Epoxy resin obtained in Example 8 E3: Epoxy resin obtained in Example 9 E4: Epoxy resin obtained in Example 10 E5: Epoxy resin obtained in Example 11 E6: Epoxy resin obtained in Example 12 EH1: Epoxy resin obtained in Comparative Example 1 EH2: Phenol-dicyclopentadiene type epoxy resin (manufactured by DIC Corporation, HP-7200H, epoxy equivalent 280, softening point 83°C, melt viscosity at 150°C 0.40 Pa·s)

[0108] [Hardening agent] P1: Polyvalent hydroxy resin obtained in Example 1 P2: Polyvalent hydroxy resin obtained in Example 2 P3: Polyvalent hydroxy resin obtained in Example 3 P4: Polyvalent hydroxy resin obtained in Example 4 P5: Polyvalent hydroxy resin obtained in Example 5 P6: Polyvalent hydroxy resin obtained in Example 6 PH1: Polyvalent hydroxy resin obtained in Synthesis Example 1 PH2: Polyvalent hydroxy resin obtained in Synthesis Example 2 PH3: Polyvalent hydroxy resin obtained in Synthesis Example 3 PH4: Polyvalent hydroxy resin obtained in Synthesis Example 4 PH5: Polyvalent hydroxy resin obtained in Synthesis Example 5 PH6: Phenol novolac resin (manufactured by Aica Kogyo Co., Ltd., Shownol BRG-557, hydroxyl group equivalent 105, softening point 80°C, melt viscosity at 150°C 0.30 Pa·s)

[0109] [Curing accelerator] C1:2E4MZ:2-Ethyl-4-methylimidazole (manufactured by Shikoku Chemicals Co., Ltd., Curesol 2E4MZ)

[0110] Synthesis Example 1 A reaction apparatus consisting of a glass separable flask equipped with a stirrer, thermometer, nitrogen blowing tube, dropping funnel, and condenser was used to add 500 parts of 2,6-xylenol (structural formula below). [ka] 7.1 parts of 47% BF3 ether complex were charged and heated to 100°C while stirring. While maintaining the same temperature, 60.1 parts of dicyclopentadiene (see structural formula below) (0.11 molar ratio to 2,6-xylenol) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 115-125°C for 4 hours. After that, 560 parts of MIBK were added to dissolve the product. 19.0 parts of sodium bicarbonate were added, and 507 parts of 80°C warm water were added and washed, separating and removing the lower aqueous layer. After that, the mixture was heated to 160°C to dehydrate, and then heated to 200°C under reduced pressure of 5 mmHg to evaporate and remove any unreacted raw materials. 1320 parts of MIBK were added to dissolve the product, and 400 parts of 80°C warm water were added and washed, separating and removing the lower aqueous layer. After heating to 120°C and reflux dehydration, the mixture was filtered, and then heated to 160°C under reduced pressure of 5 mmHg to evaporate and remove the MIBK, yielding 164 parts of a reddish-brown polyvalent hydroxy resin (pH 1, in formula (4), R1 is a methyl group and i is 2). [ka] The hydroxyl group equivalent was 195, and the softening point was 73°C. In GPC, Mw was 470, Mn was 440, the m=0 content was 2.8 area%, the m=1 content was 86.2 area%, and the m=2 or more content was 11.0 area%. The melt viscosity at 150°C was 0.05 Pa·s.

[0111] Synthesis Example 2 In a reaction apparatus similar to that used in Synthesis Example 1, 500 parts of the polyvalent hydroxy resin (PH1) obtained in Synthesis Example 1 and 125 parts of MIBK were charged and heated to 100°C while stirring. 5.0 parts of the 47% BF3 ether complex were charged and, while maintaining the same temperature, 75.0 parts of dicyclopentadiene (structural formula below) (0.22 molars relative to the hydroxyl groups of the polyvalent hydroxy resin (PH1)) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 115-125°C for 4 hours. After that, 669 parts of MIBK were added to dissolve the product. 13.3 parts of sodium bicarbonate were added, and 521 parts of 80°C warm water were added to wash the mixture, separating and removing the lower aqueous layer. The mixture was heated to 120°C and refluxed for dehydration, then filtered. MIBK was evaporated off by heating to 160°C under reduced pressure of 5 mmHg to obtain 558 parts of a reddish-brown polyvalent hydroxy resin (pH 2, in formula (10), R1 is a methyl group and i is 2). [ka] In FT-IR measurements, a peak originating from the CH stretching vibration of the olefin moiety of the dicyclopentadiene skeleton, indicating the introduction of a dicyclopentenyl group as the side chain R22, is observed at 30-40 cm². -1 It appeared in the vicinity. The hydroxyl group equivalent was 234, and it was a resin with a softening point of 86°C. In GPC, Mw was 560, Mn was 470, the k1=0 content was 6.2 area%, the k1=1 content was 74.0 area%, and the k1=2 or more content was 19.8 area%. The melt viscosity at 150°C was 0.15 Pa·s.

[0112] Synthesis Example 3 In a reaction apparatus similar to that used in Synthesis Example 1, 500 parts of 2,6-xylenol and 7.3 parts of 47% BF3 ether complex (0.1 molars relative to the initially added dicyclopentadiene) were charged and heated to 100°C with stirring. While maintaining the temperature, 67.6 parts of dicyclopentadiene (0.12 molars relative to 2,6-xylenol) were added dropwise over 1 hour. The reaction was then carried out at 115-125°C for 4 hours. After that, the mixture was heated to 200°C under reduced pressure of 5 mmHg to evaporate and remove any unreacted starting materials, and 46.7 parts of MIBK were added to dissolve the product. 3.3 parts of 47% BF3 ether complex were charged, and the mixture was heated to 100°C. While maintaining the temperature, 56.0 parts of dicyclopentadiene were added dropwise over 1 hour. The reaction was then carried out at 115-125°C for 4 hours, and 5 parts of calcium hydroxide were added. Further, 9 parts of a 10% oxalic acid aqueous solution were added. 320 parts of MIBK were added to dissolve the product, and 110 parts of 80°C hot water were added for washing, separating and removing the lower aqueous layer. The mixture was heated to 120°C and dehydrated under reflux, filtered, and then heated to 160°C under reduced pressure of 5 mmHg to evaporate and remove the MIBK, yielding 240 parts of a reddish-brown polyvalent hydroxy resin (pH 3, in formula (10), R1 is a methyl group and i is 2). [ka] In FT-IR measurements, a peak originating from the CH stretching vibration of the olefin moiety of the dicyclopentadiene skeleton, indicating the introduction of a dicyclopentenyl group as the side chain R22, is observed at 30-40 cm². -1 It appeared in the vicinity. The hydroxyl group equivalent was 276, and it was a resin with a softening point of 94°C. In GPC, Mw was 670, Mn was 490, the k1=0 content was 6.6 area%, the k1=1 content was 70.3 area%, and the k1=2 or more content was 23.1 area%. The melt viscosity at 150°C was 0.41 Pa·s.

[0113] Synthesis Example 4 In a reaction apparatus similar to that used in Synthesis Example 1, 361 parts of ortho-cresol (structural formula below) were added. [ka] 5.9 parts of 47% BF3 ether complex were charged and heated to 100°C while stirring. While maintaining the same temperature, 55.2 parts of dicyclopentadiene (see structural formula below) (0.13 molar ratio to ortho-cresol) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 115-125°C for 4 hours, and 9 parts of calcium hydroxide were added. Further, 16 parts of a 10% oxalic acid aqueous solution were added. After that, the mixture was heated to 160°C to dehydrate it, and then heated to 200°C under reduced pressure of 5 mmHg to evaporate and remove any unreacted raw materials. 970 parts of MIBK were added to dissolve the product, and 290 parts of 80°C warm water were added for washing, and the lower layer of water was separated and removed. Then, the mixture was heated to 160°C under reduced pressure of 5 mmHg to evaporate and remove the MIBK, yielding 137 parts of a reddish-brown polyvalent hydroxy resin (pH 4, in formula (4), R1 is a methyl group and i is 1). [ka] The hydroxyl group equivalent was 184, and the softening point was 78°C. In GPC, Mw was 460, Mn was 410, m=0 content was 0.8 area%, m=1 content was 75.5 area%, and m=2 or more content was 23.7 area%. The melt viscosity at 150°C was 0.07 Pa·s.

[0114] Synthesis Example 5 In a reaction apparatus similar to that used in Synthesis Example 1, 250 parts of the polyvalent hydroxy resin (PH1) obtained in Synthesis Example 1, 2.5 parts of p-toluenesulfonic acid monohydrate, and 62.5 parts of MIBK were charged and heated to 120°C while stirring. While maintaining the same temperature, 150 parts of divinylbenzene (a mixture of the structural formulas shown below) (manufactured by Aldrich, 80% divinylbenzene, 20% ethylvinylbenzene) (0.90 molars relative to the hydroxyl groups of PH1) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 120-130°C for 4 hours. 540 parts of MIBK were added to dissolve the product, neutralized with 3.3 parts of sodium bicarbonate, and washed with 180 parts of 80°C water to separate and remove the lower layer of water. Subsequently, the mixture was heated to 180°C under reduced pressure of 5 mmHg to evaporate and remove the MIBK, yielding 381 parts of a reddish-brown polyvalent hydroxy resin (pH 5, in formula (11), R1 is a methyl group and i is 2). [ka] The hydroxyl group equivalent was 308, and the softening point was 81°C. In GPC, Mw was 1750, Mn was 640, the k2=0 isomer content was 3.8 area%, the k2=1 isomer content was 41.1 area%, and the k2=2 or more isomer content was 55.1 area%.

[0115] Example 1 In a reaction apparatus similar to that used in Synthesis Example 1, 100 parts of the polyvalent hydroxy resin (PH2) obtained in Synthesis Example 2, 1.0 part of p-toluenesulfonic acid monohydrate, and 25 parts of MIBK were charged and heated to 120°C while stirring. While maintaining the same temperature, 20 parts of divinylbenzene (a mixture of the structural formulas shown below) (manufactured by Aldrich, 55% divinylbenzene, 45% ethylvinylbenzene) (0.36 molars relative to the hydroxyl groups of PH2) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 120-130°C for 4 hours. 155 parts of MIBK were added to dissolve the product, neutralized with 1.3 parts of sodium bicarbonate, and washed with 105 parts of 90°C water. The lower layer of water was separated and removed. The mixture was heated to 120°C and refluxed, filtered, and then heated to 180°C under reduced pressure of 5 mmHg to evaporate and remove MIBK, yielding 116 parts of a reddish-brown polyvalent hydroxy resin (P1). The hydroxyl group equivalent was 272, and the softening point was 77°C. Absorption ratio (A 3040 / A 1210The ratio was 0.23. Mass spectroscopy by ESI-MS (negative) revealed M-=375, 507, 629, 639, and 761, confirming that it is a polyvalent hydroxy resin of formula (1) with a structure having a dicyclopentenyl group represented by formula (2a) or formula (2b) and a group derived from divinylbenzene represented by formula (3a) or formula (3b) as substituents. The GPC chart of the obtained polyvalent hydroxy resin (P1) is shown in Figure 1, and the IR chart is shown in Figure 2. In the GPC, Mw was 693, Mn was 472, the content of n1=0 was 10.8 area%, the content of n1=1 was 61.4 area%, and the content of n1=2 or more was 27.8 area%. The melt viscosity at 150°C was 0.11 Pa·s.

[0116] Example 2 In a reaction apparatus similar to that used in Synthesis Example 1, 100 parts of the polyvalent hydroxy resin (PH2) obtained in Synthesis Example 2, 1.0 part of p-toluenesulfonic acid monohydrate, and 25 parts of MIBK were charged and heated to 120°C while stirring. While maintaining the same temperature, 30 parts of divinylbenzene (a mixture of the structural formulas shown below) (manufactured by Aldrich, 55% divinylbenzene, 45% ethylvinylbenzene) (0.54 times the molar ratio to the hydroxyl groups of PH2) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 120-130°C for 4 hours. 170 parts of MIBK were added to dissolve the product, neutralized with 1.3 parts of sodium bicarbonate, and washed with 114 parts of 90°C water. The lower layer of water was separated and removed. The mixture was heated to 120°C and refluxed for dehydration. After filtration, the mixture was heated to 180°C under reduced pressure of 5 mmHg to evaporate and remove the MIBK, yielding 126 parts of a reddish-brown polyvalent hydroxy resin (P2). The hydroxyl group equivalent was 303, and the softening point was 80°C. Mass spectroscopy using ESI-MS (negative) revealed M-=375, 507, 629, 639, and 761, confirming that it is a polyvalent hydroxy resin of formula (1) with a structure having a dicyclopentenyl group represented by formula (2a) or (2b) and a group derived from divinylbenzene represented by formula (3a) or (3b) as substituents. GPC showed Mw was 883, Mn was 519, the content of n1=0 was 7.5 area%, the content of n1=1 was 52.9 area%, and the content of n1=2 or more was 39.6 area. The melt viscosity at 150°C was 0.20 Pa·s.

[0117] Example 3 In a reaction apparatus similar to that used in Synthesis Example 1, 90 parts of the polyvalent hydroxy resin (PH1) obtained in Synthesis Example 1, 1.0 part of p-toluenesulfonic acid monohydrate, and 25 parts of MIBK were charged and heated to 120°C while stirring. While maintaining the same temperature, 40 parts of divinylbenzene (a mixture of the structural formulas shown below) (manufactured by Aldrich, 55% divinylbenzene, 45% ethylvinylbenzene) (0.67 molars relative to the hydroxyl groups of PH1) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 120-130°C for 4 hours. 185 parts MIBK was added to dissolve the product, neutralized with 1.3 parts sodium bicarbonate, and washed with 123 parts 90°C water to separate and remove the lower layer of water. The mixture was heated to 120°C and dehydrated under reflux. The mixture was cooled to 100°C, 0.9 parts of 47% BF3 ether complex were added, and while maintaining the same temperature, 13.5 parts of dicyclopentadiene (structural formula below) (0.22 molars relative to the hydroxyl groups at pH 1) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 115-125°C for 4 hours. Subsequently, 120 parts of MIBK were added to dissolve the product. 2.4 parts of sodium bicarbonate were added, and 94 parts of 80°C warm water were added for washing, separating and removing the lower aqueous layer. The mixture was heated to 120°C and dehydrated under reflux, filtered, and then heated to 180°C under reduced pressure of 5 mmHg to evaporate and remove MIBK, yielding 136 parts of a reddish-brown polyvalent hydroxy resin (P3). The hydroxyl group equivalent was 327, and the softening point was 74°C. Mass spectroscopy using ESI-MS (negative) revealed M-=375, 507, 629, 639, and 761, confirming that it is a polyvalent hydroxy resin of formula (1) with a structure having a dicyclopentenyl group represented by formula (2a) or formula (2b) and a group derived from divinylbenzene represented by formula (3a) or formula (3b) as substituents. GPC showed Mw was 813, Mn was 514, the content of n1=0 was 9.6 area%, the content of n1=1 was 53.1 area%, and the content of n1=2 or more was 37.3 area%. The melt viscosity at 150°C was 0.13 Pa·s.

[0118] Example 4 In a reaction apparatus similar to that used in Synthesis Example 1, 100 parts of the polyvalent hydroxy resin (PH2) obtained in Synthesis Example 2, 1.0 part of p-toluenesulfonic acid monohydrate, and 25 parts of MIBK were charged and heated to 120°C while stirring. While maintaining the same temperature, 30 parts of divinylbenzene (a mixture of the structural formulas shown below) (manufactured by Aldrich, 80% divinylbenzene, 20% ethylvinylbenzene) (0.54 times the molar ratio to the hydroxyl groups of PH2) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 120-130°C for 4 hours. 170 parts of MIBK were added to dissolve the product, neutralized with 1.3 parts of sodium bicarbonate, and washed with 114 parts of 90°C water. The lower layer of water was separated and removed. The mixture was heated to 120°C and refluxed for dehydration. After filtration, the mixture was heated to 180°C under reduced pressure of 5 mmHg to evaporate and remove the MIBK, yielding 126 parts of a reddish-brown polyvalent hydroxy resin (P4). The hydroxyl group equivalent was 307, and the softening point was 80°C. Mass spectroscopy using ESI-MS (negative) revealed M-=375, 507, 629, 639, and 761, confirming that it is a polyvalent hydroxy resin of formula (1) with a structure having a dicyclopentenyl group represented by formula (2a) or formula (2b) and a group derived from divinylbenzene represented by formula (3a) or formula (3b) as substituents. GPC showed Mw to be 965, Mn to be 528, n1=0 content to be 8.7 area%, n1=1 content to be 54.1 area%, and n1=2 or more content to be 37.2 area%. The melt viscosity at 150°C was 0.17 Pa·s.

[0119] Example 5 In a reaction apparatus similar to that used in Synthesis Example 1, 100 parts of the polyvalent hydroxy resin (PH3) obtained in Synthesis Example 3, 1.0 part of p-toluenesulfonic acid monohydrate, and 25 parts of MIBK were charged and heated to 120°C while stirring. While maintaining the same temperature, 20 parts of divinylbenzene (a mixture of the structural formulas shown below) (manufactured by Aldrich, 55% divinylbenzene, 45% ethylvinylbenzene) (0.42 times the molar ratio to the hydroxyl groups of PH3) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 120-130°C for 4 hours. 280 parts of MIBK were added to dissolve the product, neutralized with 1.3 parts of sodium bicarbonate, and washed with 105 parts of 90°C water. The lower layer of water was separated and removed. The mixture was heated to 120°C and refluxed for dehydration. After filtration, the mixture was heated to 180°C under reduced pressure of 5 mmHg to evaporate and remove the MIBK, yielding 116 parts of a reddish-brown polyvalent hydroxy resin (P5). The hydroxyl group equivalent was 304, and the softening point was 87°C. Mass spectroscopy using ESI-MS (negative) revealed M-=375, 507, 629, 639, and 761, confirming that it is a polyvalent hydroxy resin of formula (1) with a structure having a dicyclopentenyl group represented by formula (2a) or formula (2b) and a group derived from divinylbenzene represented by formula (3a) or formula (3b) as substituents. GPC showed Mw of 927, Mn of 551, n1=0 content of 6.4 area%, n1=1 content of 59.0 area%, and n1=2 or more content of 34.6 area%. The melt viscosity at 150°C was 0.38 Pa·s.

[0120] Example 6 In a reaction apparatus similar to that used in Synthesis Example 1, 500 parts of the polyvalent hydroxy resin (PH4) obtained in Synthesis Example 4 and 125 parts of MIBK were charged and heated to 100°C while stirring. 5.0 parts of the 47% BF3 ether complex were charged and, while maintaining the same temperature, 75.0 parts of dicyclopentadiene (structural formula below) (0.21 molars relative to the hydroxyl groups of PH4) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 115-125°C for 4 hours. After that, 669 parts of MIBK were added to dissolve the product. 13.3 parts of sodium bicarbonate were added, and 521 parts of 80°C warm water were added for washing, separating and removing the lower aqueous layer. After heating to 120°C and reflux dehydration, 5.6 parts of p-toluenesulfonic acid monohydrate were charged, and while maintaining the same temperature, 112 parts of divinylbenzene (a mixture of the structural formulas shown below) (Aldrich, 55% divinylbenzene, 45% ethylvinylbenzene) (0.32 molars relative to the hydroxyl groups at pH 4) were added. [ka] The mixture was added dropwise over 1 hour. The reaction was then carried out at a temperature of 120-130°C for 4 hours. 1560 parts of MIBK were added to dissolve the product, neutralized with 7.3 parts of sodium bicarbonate, and washed with 580 parts of 90°C water. The lower layer of water was separated and removed. The mixture was heated to 120°C and refluxed for dehydration. After filtration, MIBK was evaporated off by heating to 180°C under reduced pressure of 5 mmHg to obtain 647 parts of a reddish-brown polyvalent hydroxy resin (P6). M-=347, 479, 587, 611, and 719 were identified, confirming that it is a polyvalent hydroxy resin of formula (1) and has a structure in which both a dicyclopentenyl group represented by formula (2a) or formula (2b) and a group derived from divinylbenzene represented by formula (3a) or formula (3b) are substituents. In the GPC study, Mw was 780, Mn was 500, the content of n1=0 was 3.0 area%, the content of n1=1 was 45.1 area%, and the content of n1=2 or more was 51.9 area. The melt viscosity at 150°C was 0.20 Pa·s.

[0121] Example 7 In a reaction apparatus equipped with a stirrer, thermometer, nitrogen blowing tube, dropping funnel, and condenser, 100 parts of the polyvalent hydroxy resin (P1) obtained in Example 1 and 170.1 parts of epichlorohydrin (structural formula shown below) were added. [ka] Adding 25.5 parts of diethylene glycol dimethyl ether, the mixture was heated to 65°C. Under reduced pressure of 125 mmHg, 25.5 parts of 49% sodium hydroxide aqueous solution were added dropwise over 3 hours while maintaining a temperature of 63-67°C. During this time, the epichlorohydrin was azeotropically mixed with water, and the resulting water was sequentially removed from the system. After the reaction was complete, the epichlorohydrin was recovered under conditions of 5 mmHg and 180°C, and 281 parts of MIBK were added to dissolve the product. Then, 240 parts of water were added to dissolve the by-product sodium chloride, and the mixture was allowed to stand to separate and remove the lower layer of saline solution. After neutralization with phosphoric acid aqueous solution, the resin solution was washed with water until the water wash was neutral, and then filtered. Under reduced pressure of 5 mmHg, the mixture was heated to 180°C, and MIBK was removed by distillation to obtain 117 parts of reddish-brown epoxy resin (E1). The resin had an epoxy equivalent of 354, a total chlorine content of 1362 ppm, and a softening point of 59°C. Mass spectra measured by ESI-MS (negative) revealed M-=487, 619, and 797. The GPC chart of the obtained epoxy resin (E1) is shown in Figure 3, and the IR chart is shown in Figure 4. In the GPC, Mw was 755, Mn was 475, the content of n3=0 was 9.1 area%, the content of n3=1 was 41.1 area%, and the content of n3=2 or more was 49.8 area%. The melt viscosity at 150°C was 0.15 Pa·s.

[0122] Example 8 In a reaction apparatus similar to that of Example 7, 100 parts of the polyvalent hydroxy resin (P2) obtained in Example 2, 152.8 parts of epichlorohydrin, and 22.9 parts of diethylene glycol dimethyl ether were added and heated to 65°C. Under reduced pressure of 125 mmHg, 24.0 parts of 49% sodium hydroxide aqueous solution were added dropwise over 3 hours while maintaining a temperature of 63-67°C. During this time, the epichlorohydrin was azeotropically mixed with water, and the resulting water was sequentially removed from the system. After the reaction was complete, the epichlorohydrin was recovered under conditions of 5 mmHg and 180°C, and the product was dissolved by adding 276 parts of MIBK. Then, 220 parts of water were added to dissolve the by-product sodium chloride, and the mixture was allowed to stand to separate and remove the lower layer of saline solution. After neutralization with phosphoric acid aqueous solution, the resin solution was washed with water until the rinse solution was neutral, and then filtered. Under reduced pressure of 5 mmHg, the mixture was heated to 180°C to remove MIBK, yielding 115 parts of a reddish-brown epoxy resin (E2). The epoxy equivalent was 372, the total chlorine content was 750 ppm, and the softening point was 68°C. Mass spectrometry by ESI-MS (negative) revealed M-=487, 619, and 797. GPC showed Mw of 1192, Mn of 547, n3=0 content of 6.9 area%, n3=1 content of 47.7 area%, and n3=2 or more content of 45.4 area%. The melt viscosity at 150°C was 0.30 Pa·s.

[0123] Example 9 In a reaction apparatus similar to that of Example 7, 100 parts of the polyvalent hydroxy resin (P3) obtained in Example 3, 141.4 parts of epichlorohydrin, and 21.2 parts of diethylene glycol dimethyl ether were added and heated to 65°C. Under reduced pressure of 125 mmHg, 22.0 parts of a 49% sodium hydroxide aqueous solution were added dropwise over 3 hours while maintaining a temperature of 63-67°C. During this time, the epichlorohydrin was azeotropically mixed with water, and the resulting water was sequentially removed from the system. After the reaction was complete, the epichlorohydrin was recovered under conditions of 5 mmHg and 180°C, and 273 parts of MIBK were added to dissolve the product. Then, 199 parts of water were added to dissolve the by-product sodium chloride, and the mixture was allowed to stand to separate and remove the lower layer of saline solution. After neutralization with an aqueous phosphoric acid solution, the resin solution was washed with water until the rinse solution was neutral, and then filtered. Under reduced pressure of 5 mmHg, the mixture was heated to 180°C to remove MIBK, yielding 114 parts of a reddish-brown epoxy resin (E3). The resin had an epoxy equivalent of 397, a total chlorine content of 593 ppm, and a softening point of 62°C. Mass spectrometry by ESI-MS (negative) revealed M-=487, 619, and 797. GPC showed Mw of 1127, Mn of 535, n3=0 content of 8.5 area%, n3=1 content of 48.5 area%, and n3=2 or more content of 43.0 area%. The melt viscosity at 150°C was 0.23 Pa·s.

[0124] Example 10 In a reaction apparatus similar to that of Example 7, 100 parts of the polyvalent hydroxy resin (P4) obtained in Example 4, 150.6 parts of epichlorohydrin, and 22.6 parts of diethylene glycol dimethyl ether were added and heated to 65°C. Under reduced pressure of 125 mmHg, 23.6 parts of 49% sodium hydroxide aqueous solution were added dropwise over 3 hours while maintaining a temperature of 63-67°C. During this time, the epichlorohydrin was azeotropically mixed with water, and the resulting water was sequentially removed from the system. After the reaction was complete, the epichlorohydrin was recovered under conditions of 5 mmHg and 180°C, and the product was dissolved by adding 276 parts of MIBK. Then, 211 parts of water were added to dissolve the by-product sodium chloride, and the mixture was allowed to stand to separate and remove the lower layer of saline solution. After neutralization with phosphoric acid aqueous solution, the resin solution was washed with water until the rinse solution was neutral, and then filtered. Under reduced pressure of 5 mmHg, the mixture was heated to 180°C to remove MIBK, yielding 115 parts of a reddish-brown epoxy resin (E4). The epoxy equivalent was 370, the total chlorine content was 741 ppm, and the softening point was 65°C. Mass spectrometry by ESI-MS (negative) revealed M-=487, 619, and 797. GPC showed Mw of 1408, Mn of 537, n3=0 content of 7.4 area%, n3=1 content of 51.2 area%, and n3=2 or more content of 41.4 area%. The melt viscosity at 150°C was 0.27 Pa·s.

[0125] Example 11 In a reaction apparatus similar to that of Example 7, 100 parts of the polyvalent hydroxy resin (P5) obtained in Example 5, 152.4 parts of epichlorohydrin, and 22.9 parts of diethylene glycol dimethyl ether were added and heated to 65°C. Under reduced pressure of 125 mmHg, 23.8 parts of 49% sodium hydroxide aqueous solution were added dropwise over 3 hours while maintaining a temperature of 63-67°C. During this time, the epichlorohydrin was azeotropically mixed with water, and the resulting water was sequentially removed from the system. After the reaction was complete, the epichlorohydrin was recovered under conditions of 5 mmHg and 180°C, and the product was dissolved by adding 276 parts of MIBK. Then, 216 parts of water were added to dissolve the by-product sodium chloride, and the mixture was allowed to stand to separate and remove the lower layer of saline solution. After neutralization with phosphoric acid aqueous solution, the resin solution was washed with water until the rinse solution was neutral, and then filtered. Under reduced pressure of 5 mmHg, the mixture was heated to 180°C to remove MIBK, yielding 115 parts of a reddish-brown epoxy resin (E5). The epoxy equivalent was 373, the total chlorine content was 645 ppm, and the softening point was 73°C. Mass spectrometry by ESI-MS (negative) revealed M-=487, 563, 619, and 797. GPC showed Mw of 1013, Mn of 561, n3=0 content of 5.3 area%, n3=1 content of 56.7 area%, and n3=2 or more content of 38.0 area%. The melt viscosity at 150°C was 0.41 Pa·s.

[0126] Example 12 In a reaction apparatus similar to that of Example 7, 100 parts of the polyvalent hydroxy resin (P6) obtained in Example 6, 152.4 parts of epichlorohydrin, and 22.9 parts of diethylene glycol dimethyl ether were added and heated to 65°C. Under reduced pressure of 125 mmHg, 23.8 parts of 49% sodium hydroxide aqueous solution were added dropwise over 3 hours while maintaining a temperature of 63-67°C. During this time, the epichlorohydrin was azeotropically mixed with water, and the resulting water was sequentially removed from the system. After the reaction was complete, the epichlorohydrin was recovered under conditions of 5 mmHg and 180°C, and the product was dissolved by adding 276 parts of MIBK. Then, 216 parts of water were added to dissolve the by-product sodium chloride, and the mixture was allowed to stand to separate and remove the lower layer of saline solution. After neutralization with phosphoric acid aqueous solution, the resin solution was washed with water until the rinse solution was neutral, and then filtered. Under reduced pressure of 5 mmHg, the mixture was heated to 180°C to remove MIBK, yielding 115 parts of reddish-brown epoxy resin (E6). M-=459, 591, and 723 were identified. In GPC, Mw was 1013, Mn was 561, the content of n3=0 was 5.3 area%, the content of n3=1 was 56.7 area%, and the content of n3=2 or more was 38.0 area. The melt viscosity at 150°C was 0.41 Pa·s.

[0127] Comparative Example 1 In a reaction apparatus similar to that of Example 7, 100 parts of the polyvalent hydroxy resin (PH1) obtained in Synthesis Example 1, 237.2 parts of epichlorohydrin, and 35.6 parts of diethylene glycol dimethyl ether were added and heated to 65°C. Under reduced pressure of 125 mmHg, 38.1 parts of 49% sodium hydroxide aqueous solution were added dropwise over 3 hours while maintaining a temperature of 63-67°C. During this time, the epichlorohydrin was azeotropically mixed with water, and the resulting water was sequentially removed from the system. After the reaction was complete, the epichlorohydrin was recovered under conditions of 5 mmHg and 180°C, and the product was dissolved by adding 300 parts of MIBK. Then, 336 parts of water were added to dissolve the by-product sodium chloride, and the mixture was allowed to stand to separate and remove the lower layer of saline solution. After neutralization with phosphoric acid aqueous solution, the resin solution was washed with water until the water wash was neutral, and then filtered. Under reduced pressure of 5 mmHg, the mixture was heated to 180°C to remove MIBK by distillation, yielding 125 parts of a reddish-brown dicyclopentadiene-type epoxy resin (EH1). The epoxy equivalent was 261, the total chlorine content was 710 ppm, and the softening point was 55°C. The Mw and Mn values ​​in GPC were 670 and 570 respectively, and the melt viscosity at 150°C was 0.10 Pa·s.

[0128] Example 13 An epoxy resin composition varnish was obtained by mixing 100 parts of epoxy resin (E1) as the epoxy resin, 29.7 parts of phenol novolac resin (PH6) as the curing agent, and 0.40 parts of C1 as the curing accelerator, and dissolving them in a mixed solvent prepared with MEK, propylene glycol monomethyl ether, and N,N-dimethylformamide. The obtained epoxy resin composition varnish was impregnated into glass cloth (manufactured by Nitto Boseki Co., Ltd., WEA 7628 XS13, 0.18 mm thick). The impregnated glass cloth was dried in a hot air circulating oven at 150°C for 9 minutes to obtain a prepreg.

[0129] The obtained prepreg was loosened and sieved to obtain a 100-mesh pass prepreg powder. The obtained prepreg powder was placed in a fluororesin mold and subjected to a 2 MPa vacuum press at a temperature of 130°C for 15 minutes + 190°C for 80 minutes to obtain a 50 mm square x 2 mm thick test specimen. The relative permittivity and dielectric loss tangent of the test specimen are shown in Table 1.

[0130] Furthermore, eight of the obtained prepregs were stacked with copper foil (manufactured by Mitsui Mining & Smelting Co., Ltd., 3EC-III, 35 μm thick) on the top and bottom, and vacuum pressed at 2 MPa under the temperature conditions of 130°C for 15 minutes + 190°C for 80 minutes to obtain a 1.6 mm thick laminate. The results of the copper foil peel strength and interlayer adhesion strength of the laminate are shown in Table 1.

[0131] Examples 14-42 and Comparative Examples 2-12 The mixtures were prepared using the proportions (parts) shown in Tables 1-4, and the same procedure as in Example 13 was followed to obtain laminates and test specimens. The amount of curing accelerator used was sufficient to adjust the varnish gel time to approximately 300 seconds. The same test as in Example 13 was performed, and the results are shown in Tables 1-4.

[0132] [Table 1]

[0133] [Table 2]

[0134] [Table 3]

[0135] [Table 4]

[0136] As is clear from these results, the polyvalent hydroxy resins and epoxy resins obtained in the examples exhibit very good low viscosity, and resin compositions containing them can provide cured resin products that exhibit very good low dielectric properties while maintaining an adhesiveness of 1.0 kN / m or more, which is practically acceptable. [Industrial applicability]

[0137] The polyvalent hydroxy resin, epoxy resin, and resin composition of the present invention are applicable to a wide range of fields, including paints, civil engineering adhesives, casting, electrical and electronic materials, and film materials. In particular, they are useful for printed circuit board applications, which are a type of electrical and electronic material.

Claims

1. A polyvalent hydroxy resin characterized by being represented by the following general formula (1). 【Chemistry 1】 Here, R 1 R independently represents an alkyl group having 1 to 8 carbon atoms. 21 R independently represents a hydrogen atom, a dicyclopentenyl group represented by formula (2a) or formula (2b), a group represented by formula (3a), or a group represented by formula (3b), and at least two of these are, one of which is a dicyclopentenyl group represented by formula (2a) or formula (2b), and the other is a group represented by formula (3a) and formula (3b). 3 '' independently represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms. 'Me' represents a methyl group. 'i' is an integer from 0 to 2. 'n1' indicates the number of repetitions, the average value of which is a number from 0 to 5.

2. The aforementioned R 1 The polyvalent hydroxy resin according to claim 1, wherein is a methyl group and i is 1 or 2.

3. A method for producing a polyvalent hydroxy resin, characterized by reacting a polyvalent hydroxy resin (a) represented by the following general formula (4) with an aromatic vinyl compound (b) represented by the following general formulas (5a) and (5b) and dicyclopentadiene. 【Chemistry 2】 Here, R 1 '' independently represents an alkyl group having 1 to 8 carbon atoms. 'i' is an integer from 0 to 2. 'm' indicates the number of repetitions, with its average value being a number from 0 to 5. 【Transformation 3】 Here, R 3 This represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms.

4. A method for producing a polyvalent hydroxy resin according to claim 3, characterized in that, in the presence of an acid catalyst, 0.05 to 2.0 moles of the aromatic vinyl compound (b) and 0.05 to 2.0 moles of dicyclopentadiene are reacted with 1 mole of phenolic hydroxyl groups of the polyvalent hydroxy resin (a) at a reaction temperature of 50 to 200°C.

5. An epoxy resin characterized by being represented by the following general formula (6). 【Chemistry 4】 Here, R 1 each independently represents an alkyl group having 1 to 8 carbon atoms, R 2 each independently represents a hydrogen atom, a dicyclopentenyl group represented by formula (2a) or formula (2b), a group represented by formula (3a), or a group represented by formula (3c), and among at least two thereof, one is the dicyclopentenyl group represented by formula (2a) or formula (2b), and the other is the group represented by formula (3a) or formula (3c). R 3 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 8 carbon atoms. Me represents a methyl group. i is an integer of 0 to 2. n3 represents the number of repeats, and the average value thereof is a number of 0 to 5.

6. A method for producing epoxy resin, characterized by reacting 1 to 20 moles of epihalohydrin with 1 mole of phenolic hydroxyl groups of a polyvalent hydroxyl resin represented by general formula (1) as described in claim 1, in the presence of an alkali metal hydroxide.

7. An epoxy resin composition comprising an epoxy resin and a curing agent, characterized in that it requires the polyvalent hydroxy resin described in claim 1 and / or the epoxy resin described in claim 5.

8. A prepreg characterized by using the epoxy resin composition described in claim 7.

9. A laminate characterized by using the epoxy resin composition described in claim 7.

10. A printed circuit board characterized by using the epoxy resin composition described in claim 7.

11. A cured product obtained by curing the epoxy resin composition according to claim 7.

Citation Information

Patent Citations

  • Resin for improving rubber tear resistance and preparation method thereof

    CN103665331A

  • epoxy resin composition

    JP1993339341A

  • Synthetic resin composition and its cured molded product

    JP1994116345A

  • Circuit board resin composition used for semiconductor device equipped with grid-like energizing terminal, circuit board for semiconductor device equipped with grid-like energizing terminal and semiconductor device equipped with grid-like energizing terminal

    JP2001240654A

  • Modified polyhydric hydroxy resin, epoxy resin, epoxy resin composition, and cured matter thereof

    JP2016069524A