Method for preparing powder for additive manufacturing

A method for producing cermet and cemented carbide powders for 3D printing by forming a slurry, spray drying, and controlled sintering in a carburizing atmosphere addresses the adhesion and porosity issues, achieving high-quality, spherical granules with excellent fluidity for additive manufacturing.

JP7954173B2Active Publication Date: 2026-11-19SANDVIK MACHINING SOLUTIONS AB
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023580508
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-07-01
Filing Date
2022-06-23
Publication Date
2026-11-19
Estimated Expiration
2042-06-23

AI Technical Summary

Technical Problem

Existing methods for producing cermet and cemented carbide powders for 3D printing result in brittle, porous granules that adhere during sintering, leading to non-spherical shapes and poor fluidity, which affect the quality of the final 3D printed products.

Method used

A method involving the formation of a slurry with a hard component, binder metal, organic binder, and solvent, followed by spray drying to create unsintered granules, which are then sintered in a carburizing atmosphere at controlled temperatures to maintain spherical shape and prevent adhesion, followed by gentle deaggregation.

Benefits of technology

The method produces sintered granules with appropriate porosity and excellent fluidity, maintaining spherical shape and reducing the need for post-sintering cleaning, resulting in high-quality cermet and cemented carbide powders suitable for additive manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954173000005
    Figure 0007954173000005
  • Figure 0007954173000006
    Figure 0007954173000006
  • Figure 0007954173000007
    Figure 0007954173000007
Patent Text Reader

Abstract

The present invention relates to a method for making a ready-to-print cermet or hard metal powder containing sintered granules, comprising sintering the granules in a carburizing atmosphere. Due to the carburizing atmosphere, the granules have less binder phase on the surface, do not sinter together, are easy to deagglomerate and the granules maintain their spherical shape. The present invention also relates to a powder made according to said method and the use of the powder in an additive manufacturing process.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a method for producing a sintered, ready-to-print cermet or cemented carbide powder, and also to a powder produced by such a method. The powder is suitable for additive manufacturing such as 3D printing of cermet and cemented carbide bodies. BACKGROUND ART

[0002] Three-dimensional (3D) printing or additive manufacturing is a promising manufacturing technique that enables printing of three-dimensional bodies. Three-dimensional printing is a promising manufacturing technique because it makes it possible to generate complex structures and objects that cannot be achieved by conventional manufacturing processes.

[0003] The production of cermet or cemented carbide bodies using 3D printing is known in the art. Cermet and cemented carbide materials consist of hard components of carbides and / or nitrides such as WC or TiC in a metallic binder phase of, for example, Co. These materials are useful in very demanding applications due to their high hardness and high wear resistance combined with high toughness. Examples of areas of application are cutting tools for metal cutting, drill bits for rock drilling, and wear parts.

[0004] One of the challenges when producing cermet and cemented carbide materials using 3D printing is to provide an object with a microstructure equivalent to that of cermet and cemented carbide materials produced by conventional methods, i.e., those formed by pressing, namely porosity, minimal Co islands, and the like.

[0005] However, many attempts have been made to find a suitable powder that is easy to manufacture, has suitable properties for 3D printing, and furthermore results in a final sintered cermet or cemented carbide with excellent quality.

[0006] In the conventional production of cemented carbide bodies using crushing, spray drying, pressurization, and sintering, the powder used for pressurization is not sintered. However, for 3D printing, such powder is too brittle and too porous. Therefore, when used for 3D printing, dry powder in granular form is sintered to varying degrees. However, this can cause the granules to adhere to each other because the metal binder on the surface of the granules easily melts together. Thus, sintered powder needs to be crushed or broken using great force in order to be used for 3D printing. This can result in non-spherical granules after the crushing / breaking of sintered granules, which can affect the powder's fluidity.

[0007] One way to prevent granules from sintering together is to use a lower sintering temperature, thus allowing less metal binder to form on the surface of the granules, which results in less dense granules with more pores. If the granules are too porous, the 3D printed cemented carbide may still have pores after final sintering.

[0008] For example, attempts have been made to prevent granules from sintering together by physically hindering contact between them, such as by adding a powder that can act as a barrier. However, such methods also require several post-sintering cleaning steps to remove the barrier powder before the final powder can be used for 3D printing.

[0009] The object of the present invention is to provide a method for producing cermet or cemented carbide powder for additive manufacturing that prevents granules from sintering with each other.

[0010] The object of the present invention is to provide a method for producing cermet or cemented carbide powder for additive manufacturing that is easy and requires few steps.

[0011] The object of the present invention is to obtain a method for producing cermet or cemented carbide powder for additive manufacturing that has appropriate porosity and excellent fluidity. [Brief explanation of the drawing]

[0012] [Figure 1] This is an SEM image of sintered granules prepared according to the present invention. [Figure 2] This is an SEM image of sintered granules prepared according to prior art. [Figure 3] This is a LOM image of a cross-section of a granule. [Figure 4] This diagram shows various steps, in which step A forms unsintered granules, step B places the unsintered granules in a furnace, step C sinters the unsintered granules in a carburizing atmosphere, and step D subjects the sintered granules to a de-aggregation process. [Modes for carrying out the invention]

[0013] The present invention relates to a method for producing powder according to the above. The method is as follows: - A step of forming a slurry containing a hard component, a binder metal, an organic binder, and a solvent. - A process for forming unsintered granules containing hard components, binder metal, and organic binder from a slurry. - The process of placing unsintered granules into a furnace. - To form sintered granules, the mixture is heated in a carburizing atmosphere at 1200°C and T s A process of sintering granules at a temperature between °C, s The binder remains in a solid state for a particular cermet or cemented carbide composition at the maximum temperature of 1200°C and T in a carburizing atmosphere. s A process of sintering granules at a temperature between °C, - A step of subjecting sintered granules to a de-aggregation step, wherein powder of the sintered granules is formed as a result. Includes.

[0014] The slurry comprises a powder that forms a hard component, a binder metal, an organic binder, and a solvent.

[0015] As used herein, the powder forming the hard component means a powder selected from carbides, nitrides or carbonitrides of one or more elements among W, Ta, Ti, Nb, Nb, Cr and V.

[0016] When producing cemented carbide powder, the hard component comprises at least 50 wt% WC granules. The hard component may also comprise carbides or carbonitrides of one or more of Ta, Ti, Nb, Cr, Hf, V, Mo and Zr, such as TiN, TiC and / or TiCN.

[0017] When producing cermet powder, the hard component comprises carbides or carbonitrides of one or more of Ta, Ti, Nb, Cr, Hf, V, Mo and Zr, such as TiN, TiC and / or TiCN.

[0018] As used herein, the metal binder means one or more elements selected from Co, Ni and Fe, preferably the metal binder is Co. The amount of the metal binder in the slurry is suitably between 5 wt% and 14 wt%, preferably between 8 wt% and 14 wt%, based on the weight of the dry powder. The metallic binder phase content is calculated herein excluding the organic binder and the solvent.

[0019] The organic binder is suitably selected from polyethylene glycol (PEG) or wax. The amount of the organic binder may be between 1 wt% and 5 wt% based on the powder weight.

[0020] The solvent may be any solvent suitable for preparing a slurry, preferably a mixture of water and alcohol.

[0021] The formation of unsintered granules is suitably carried out by using spray drying, or any other suitable technique capable of forming spherical granules.

[0022] The unsintered granules are placed on a tray inside a furnace. Preferably, the graphite tray is coated with yttrium oxide to prevent the powder from sticking to the tray.

[0023] The first part of the sintering cycle is a debinding step, in which the organic binder is removed. Suitably, this is performed at a temperature between 200°C and 550°C for a period between 5 minutes and 240 minutes. Debinding can also be carried out in two or more steps, i.e., by increasing the temperature stepwise. The exact debinding process depends on several factors, such as furnace type, batch size, binder type, and the like.

[0024] The second part of sintering, namely solid state sintering, is carried out at a temperature above 1200°C and below T s °C, where T s is the maximum temperature at which the binder is still in the solid state for a particular cermet or cemented carbide composition. This temperature is usually shown as a line called the "solidus line" in the phase diagram for each particular cermet or cemented carbide composition. Solid state sintering is performed for a period between 5 minutes and 60 minutes. Preferably, the sintering is carried out at a temperature between 1250°C and T s °C, more preferably between 1250°C and 1300°C.

[0025] When determining the exact sintering temperature, the particular cermet or cemented carbide composition must be taken into account.

[0026] In one embodiment of the present invention, when the metallic binder is Co, the sintering is carried out at a temperature between 1250°C and 1300°C, preferably between 1260°C and 1290°C.

[0027] A carburizing atmosphere, as used herein, means that carbon is added to the furnace. This can be done in several ways, for example with one or more carbon-containing gases such as CO, CH₄, CO₂. Some carbon contribution can also originate from the furnace if the furnace is a graphite furnace.

[0028] Preferably, the carburizing atmosphere is created by a carbon-containing gas, preferably CO, CO2, and / or CH4. The partial pressure of the carburizing gas should be at least 50 mBar, preferably at least 75 mBar, of the total gas present. The partial pressure of the carburizing gas should be below atmospheric pressure. Other suitable gases that may be present are Ar, H2, etc. The total pressure in the sintering furnace should be below atmospheric pressure.

[0029] After sintering, the granules usually adhere to each other with weak force. To obtain the final powder, only gentle deaggregation is necessary. Deaggregation is preferably carried out by gentle grinding in a ball mill without the use of grinding liquid. If a smaller amount of granules are to be deaggregated, deaggregation can be done by hand using a mortar and pestle.

[0030] Because the granules are not sintered together but instead only weakly adhere to one another, the spherical or rounded shape achieved from the spray drying process can be maintained even after de-aggregation.

[0031] Before using sintered granules for 3D printing, the ready-to-print powder containing the sintered granules may be subjected to one or more sieving steps. This may be done for several purposes, such as removing any larger fragments that have not been deaggregated, as well as to achieve a desired granule size.

[0032] The present invention also relates to a ready-to-print cermet or cemented carbide powder containing sintered granules, prepared according to the method described above.

[0033] In this specification, "ready to print" means that the powder is ready for use in additive manufacturing processes such as 3D printing.

[0034] The powder contains sintered granules having an average diameter (D50) between 15 μm and 30 μm, which include WC and a metal binder, and the sintered granules have a porosity between 0.1 vol% and 5 vol%.

[0035] The porosity of sintered granules can be determined by various methods. One method is to calculate it by first measuring the density of the granules using a specific gravity bottle. The measured density is then compared to the theoretical (or perfect) density for a particular cermet or cemented carbide composition. The perfect density can be determined by calculation using appropriate software such as Thermocalc, or by measuring it for a porosity-free sintered fragment made from powder having the same composition. The difference is presumed to be the pores.

[0036] Another method for measuring porosity is to use image analysis on SEM or LOM images of cross-sections of at least 50 sintered granules. The results are then given in area %, but are estimated to be the same value in vol %.

[0037] Sintered granules produced according to the present invention have a surface region having a metal binder content less than the metal binder content in the inner part of the granule.

[0038] Depletion of the metal binder in the surface region is most easily observed in SEM images of the granules, where the granule surface may be seen to be coated with WC crystals. The metal binder can occasionally be seen at the bottom of larger gaps between WC granules, but not on the actual surface of the granules. See, for example, Figure 1.

[0039] Sintered granules are typically spherical or rounded in shape, which is achieved through the spray drying process. Since the granules do not sinter together during the sintering process, the shape achieved by the spray drying can be maintained.

[0040] In this specification, unsintered granules mean compact particles comprising an organic binder, hard component particles, and a binder metal.

[0041] In this specification, sintered granules refer to compact particles containing hard component particles embedded in a binder metal matrix.

[0042] In this specification, cermet means a material comprising a hard component in a metallic binder phase, wherein the hard component comprises one or more carbides or carbonitrides from Ta, Ti, Nb, Cr, Hf, V, Mo, and Zr, such as TiN, TiC, and / or TiCN.

[0043] As used herein, cemented carbide powder means a material containing a hard component in a metallic binder phase, wherein the hard component comprises at least 50 wt% WC granules. The hard component may also include one or more carbides or carbonitrides from among Ta, Ti, Nb, Cr, Hf, V, Mo, and Zr, such as TiN, TiC, and / or TiCN.

[0044] The present invention also relates to the use of the above-mentioned ready-printable powder for producing cermet or cemented carbide bodies by additive manufacturing such as 3D printing.

[0045] In one embodiment of the present invention, 3D printing is binder jetting. Binder jetting is advantageous in that it is a relatively inexpensive 3D printing method.

[0046] 3D printing of cermet or cemented carbide fragments is well known in the art, and the precise printing parameters are determined by those skilled in the art based on the type of printing technique used. Typically, the printing process is followed by hardening and powder removal, and then a sintering process in which the final cermet or cemented carbide fragment is achieved. [Examples]

[0047] Example 1 (Invention) Ready-to-press (RTP) powders, which are already ground, spray-dried, and contain WC, a metallic binder, and carbides of Cr and, if present, Ta and Nb, were used as raw materials. The composition of the different powders based on elements is shown in Table 1, with the remainder being carbon. The WC granular size (FSSS) in inventions 1 and 2 was 0.80 μm, and in invention 3, the WC granular size (FSSS) was 1.5 μm. In addition to the powder raw materials, the RTP powder also contained 2 wt% PEG, which was not present in the dry powder weight.

[0048] A new slurry was prepared by dissolving the RTP powder in a 78 / 22 ratio of ethanol and water, and adding an additional 2 wt% of PEG. The slurry was spray-dried into small granules with a D50 of approximately 25 μm.

[0049] Unsintered granules were placed in a sintering furnace on a graphite tray coated with yttrium oxide and first subjected to a debindering process in a hydrogen atmosphere, including a stepwise temperature increase to 500°C over 170 minutes. The temperature was then increased to a maximum sintering temperature of 1275°C in an Ar atmosphere (200 mBar partial pressure), where CO and Ar were introduced at a 1:1 flow rate ratio with a partial pressure of 250 mBar. The temperature and CO / Ar atmosphere were maintained for 60 minutes. The granules were then cooled to room temperature by free cooling.

[0050] Sintering yielded a sintered granular cake, which was subjected to deagglomeration in a ball mill using 100 kg of Silpeb with 30 kg of powder. The ball-milled product was dried by running the mill without a grinding solution. The deagglomeration time ranged from 10 to 40 minutes, depending on the sample.

[0051] Next, the powder was sieved through a 63 μm sieve.

[0052] The resulting cemented carbide powder containing sintered granules is referred to as Inventions 1 to 3 in this specification.

[0053] Figure 1 shows an SEM image of the sintered granules of Invention 1. TIFF0007954173000001.tif38170

[0054] The particle size of the sintered granules was measured by laser diffraction of dry granules at intervals of 0.5 μm and 175 μm. The results are shown in Table 2. TIFF0007954173000002.tif38170

[0055] Example 2 The same unsintered granules used in Invention 1 from Example 1 were sintered at different maximum temperatures using the same method as in Example 1, but with a mixture of CO and H2 atmospheres (at a total partial pressure of 250 mBar in a 1:1 ratio) (the same for all three samples). At the end of the cycle, a high pressure of 50 bar (Ar) was applied. The samples are referred to as Inventions 1a-1c.

[0056] Porosity was measured by image analysis of LOM (optical microscope) images (magnification 2000) of granule cross-sections using the software Image J. The average of approximately 50 granules per powder sample was analyzed. Powders sintered at 1300°C were significantly more difficult to deaggregate, and therefore the granules deformed to a greater extent compared to those at 1250°C and 1275°C. TIFF0007954173000003.tif29170

[0057] Example 3 (Comparison) Sintered granules were prepared from powder having the same composition as Invention 1 in Example 1, following the process described in US2017 / 0072469, which uses graphite powder as a physical barrier. After sintering, the graphite powder was removed. SEM images of the sintered granules are shown in Figure 2.

[0058] Example 4 (Printing) A sample cube (15 × 15 × 6 mm) was printed using Invention 2 from Example 1, which consists of sintered granules. The cube was produced by binder jet printing. Printing was performed using ExOne Innovent+ with a layer thickness of 50 μm during printing. Saturation during printing was set to 80%. The cube was then sintered for 90 minutes using a high-pressure sintering cycle with a maximum temperature of 1410 °C. At the end of the cycle, a high pressure of 50 bar was applied. All physical properties were within the standards for this substrate when it is produced by a conventional method, i.e., when compression is used instead of printing as the formation step. TIFF0007954173000004.tif31170

Claims

1. - A step of forming a slurry containing hard components, binder metal, organic binder, and solvent, - A step of forming unsintered granules containing hard components, binder metal, and organic binder from a slurry, - The process of putting unsintered granules into the furnace, - T s However, the binder remains in a solid state at 1200°C and T in a carburizing atmosphere, which is the highest temperature at which the binder remains solid for certain cermet or cemented carbide compositions. s A step of forming sintered granules by sintering granules at a temperature between °C, wherein the sintered granules have a surface region having a metal binder content less than the metal binder content in the inner part of the granules. - A step of subjecting sintered granules to a de-aggregation step, thereby forming powder from the granules. A method for producing a ready-to-print cermet or cemented carbide powder containing sintered granules.

2. Carburizing atmosphere, CO, CO 2 and CH 4 The method according to claim 1, provided by one or more carburizing gases selected from.

3. The method according to claim 2, wherein the carburizing gas is present at a partial pressure of at least 50 mBar.

4. The method according to claim 1, wherein the powder that can be printed immediately is cemented carbide powder, and the hard component comprises at least 50 wt% WC granules.

5. The method according to claim 1, wherein the metal binder is one or more elements selected from Co, Ni, and Fe, and the amount of the metal binder is between 5 wt% and 14 wt% based on the dry powder weight.

6. The method according to claim 1, wherein the sintering temperature is between 1250°C and 1300°C.

7. The method according to claim 1, wherein the metallic binder is Co, and the sintering temperature is between 1260°C and 1290°C.

8. The method according to claim 1, wherein a ready-to-print cermet or cemented carbide powder containing sintered granules is subjected to one or more sieving steps.

9. A ready-printable cermet or cemented carbide powder comprising sintered granules, wherein the sintered granules have an average particle size between 15 μm and 30 μm, the sintered granules contain WC and a metal binder, the sintered granules have a porosity between 0.1 vol% and 5 vol%, and the sintered granules have a surface region having a metal binder content less than the metal binder content in the inner part of the granules.

10. The ready-to-print cermet or cemented carbide powder according to claim 9, wherein the powder is cemented carbide powder.

11. The use of a ready-to-print cermet or cemented carbide powder according to claim 9 in an additive manufacturing process for producing a cermet or cemented carbide body.

12. The use of a ready-to-print cermet or cemented carbide powder according to claim 11, wherein the additive manufacturing process is binder jetting.

Citation Information

Patent Citations

  • JP1975097505A

  • Compacting of gas atomized metal powder to a part

    US20170361378A1

  • Sintered cemented carbide granulate and its use