Microporous membrane for energy storage devices

The microporous film for energy storage devices uses polyolefin with functional groups to form a crosslinked structure within the device, addressing strength and safety issues by enhancing high-temperature resistance and reducing stress-induced deformation.

JP7954244B2Active Publication Date: 2026-11-19ASAHI KASEI BATTERY SEPARATOR CORP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2025109236
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-02-18
Filing Date
2025-06-27
Publication Date
2026-11-19
Estimated Expiration
2040-02-07

AI Technical Summary

Technical Problem

Existing microporous membranes for lithium-ion batteries face challenges in maintaining strength and porosity while achieving high-temperature resistance and safety, particularly due to stress-induced deformation during manufacturing processes and uneven crosslinking structures.

Method used

A microporous film for energy storage devices is developed using polyolefin with functional groups that form a crosslinked structure through condensation reactions within the device, avoiding pre-manufacturing crosslinking methods, ensuring high-temperature resistance and safety without increasing internal stress.

Benefits of technology

The solution enhances film rupture resistance at high temperatures, maintaining strength and porosity, and improves safety in nail penetration tests without requiring energy-intensive crosslinking processes like light irradiation or heating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954244000044
    Figure 0007954244000044
  • Figure 0007954244000045
    Figure 0007954244000045
  • Figure 0007954244000046
    Figure 0007954244000046
Patent Text Reader

Abstract

To improve membrane resistance of a microporous film under high temperature, without sacrifice of strength and openness of the microporous film, and to balance device characteristics of a power storage device including the microporous film and high safety in nail piercing test.SOLUTION: Polyolefin contained in microporous film for power storage device has one kind or more of functional group, MFR of 3.0 g / 10 min or less, Mw / Mn of 15 or less, and density of 0.85 g / cm3 or more. In wide-angle X-ray scattering measurement of the microporous film for power storage device, the orientation ratio MD / TD is 1.3 or more, and after the microporous film for power storage device is received in the power storage device, (1) condensation reaction takes place between the functional groups, (2) the functional group reacts on a chemical material in the power storage device, or (3) the functional group reacts on other kind of functional group, and a bridge structure is formed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to microporous membranes for energy storage devices, etc. [Background technology]

[0002] Microporous membranes are widely used as separation or selective permeable separation membranes and isolation materials for various substances. Examples of their applications include microfiltration membranes, separators for fuel cells and capacitors, or base materials for functional membranes that exhibit new functions by filling the pores with functional materials, and separators for energy storage devices. Among these, polyolefin microporous membranes are particularly suitable for use as separators in lithium-ion batteries, which are widely used in notebook personal computers, mobile phones, digital cameras, and the like.

[0003] To ensure battery safety, it has been proposed to achieve both activation of the shutdown function and improvement of the film rupture temperature by forming a crosslinked structure within the separator (Patent Documents 1-8). For example, Patent Documents 1-6 describe a silane crosslinked structure formed by contact between a silane-modified polyolefin-containing separator and water. Patent Document 7 describes a crosslinked structure formed by ring-opening of norbornene by irradiation with ultraviolet light, electron beams, etc. Patent Document 8 describes that the insulating layer of the separator has a crosslinked structure, such as a (meth)acrylic acid copolymer or a styrene-butadiene rubber binder.

[0004] The components used in lithium-ion batteries include positive electrode materials, negative electrode materials, electrolyte, and separators. Of these components, the separator has been required to be inert to electrochemical reactions and surrounding components due to its suitability as an insulating material. On the other hand, for the negative electrode material of lithium-ion batteries, a technology has been established from the beginning of its development to suppress the decomposition of the electrolyte on the negative electrode surface by forming a solid electrolyte interface (SEI) through a chemical reaction during the initial charge (Non-Patent Literature 1). Furthermore, even when polyolefin resin is used for the separator, oxidation reactions are induced on the positive electrode surface under high voltage, and cases of blackening and surface degradation of the separator have been reported. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-216964 [Patent Document 2] International Publication No. 97 / 44839 [Patent Document 3] Japanese Patent Application Publication No. 11-144700 [Patent Document 4] Japanese Patent Application Publication No. 11-172036 [Patent Document 5] Japanese Patent Publication No. 2001-176484 [Patent Document 6] Japanese Patent Publication No. 2000-319441 [Patent Document 7] Japanese Patent Publication No. 2011-071128 [Patent Document 8] Japanese Patent Publication No. 2014-056843 [Non-patent literature]

[0006] [Non-Patent Document 1] Lithium-ion secondary batteries (2nd edition) Published by Nikkan Kogyo Shimbun Co., Ltd. [Overview of the project] [Problems that the invention aims to solve]

[0007] In recent years, there has been a growing demand for higher power output and higher energy density in lithium-ion secondary batteries for mobile devices and automobiles, while simultaneously requiring smaller battery cells and stable cycle charging / discharging performance during long-term use. Therefore, the manufacture of microporous membranes usable as battery separators requires strength and porosity. Furthermore, battery safety standards have become more stringent than before, and as described in Patent Documents 1 and 2, separators with shutdown functionality and high-temperature rupture properties, as well as stable manufacturing methods thereof, are highly desirable. In this regard, a shutdown temperature lower than 150°C is preferable, while a rupture temperature higher is preferable.

[0008] However, the crosslinking methods described in Patent Documents 1 to 8 are all performed in-process on the microporous film or in batches immediately after the microporous film is manufactured. Therefore, after the formation of the crosslinked structure described in Patent Documents 1 to 8, coating and slitting of the microporous film are required for use as a separator. In the subsequent lamination and winding process with electrodes, internal stress increases, which can cause deformation of the manufactured energy storage device. For example, if a crosslinked structure is formed by heating, the internal stress of the separator having that crosslinked structure may increase at room temperature or ambient temperature. Also, if a crosslinked structure is formed by irradiation of the microporous film with light such as ultraviolet light or electron beams, the light irradiation may be uneven, resulting in a heterogeneous crosslinked structure. This is thought to be because the area around the crystalline portion of the resin constituting the microporous film is easily crosslinked by electron beams.

[0009] In view of the above problems, the present invention aims to improve the resistance of microporous membranes to rupture at high temperatures without impairing their strength and porosity, and to achieve both high device characteristics and high safety in nail penetration tests for energy storage devices using microporous membranes as separators. [Means for solving the problem]

[0010] The above problems can be solved by the following technical means. [1] A microporous film for energy storage devices containing polyolefin, The polyolefin has one or more functional groups, and After being stored in the energy storage device, (1) the functional groups undergo a condensation reaction with each other, (2) the functional groups react with chemical substances inside the energy storage device, or (3) the functional groups react with other types of functional groups to form a crosslinked structure. The aforementioned polyolefin meets the following requirements (A) to (C): (A) The melt flow rate (MFR) measured under conditions of a temperature of 230°C and a mass of 2.16 kg is 3.0 g / 10 min or less; (B) The value obtained by dividing the weight-average molecular weight Mw by the number-average molecular weight Mn (Mw / Mn) is 15 or less; and (C) Density is 0.85 g / cm³ 3 That's all; Satisfying the conditions, and The microporous membrane for the energy storage device meets the following requirement (D): (D) The ratio of the orientation ratio in the width direction (TD) to the machine direction (MD) measured by wide-angle X-ray scattering, MD / TD, is 1.3 or greater; A microporous film for energy storage devices characterized by satisfying the following conditions. [2] The crosslinked structure is (1) a microporous film for an energy storage device as described in item 1, formed by a condensation reaction between the functional groups. [3] The crosslinked structure is (2) a microporous membrane for an energy storage device according to item 1, formed by the functional group reacting with a chemical substance inside the energy storage device. [4] A microporous membrane for an energy storage device according to item 1 or 3, wherein the chemical substance is one of the electrolyte, electrolyte solution, electrode active material, additive, or decomposition products thereof contained in the energy storage device. [5] The crosslinked structure is (3) a microporous film for an energy storage device according to item 1, formed by the reaction of the functional group with another type of functional group. [6] The microporous membrane for the energy storage device is given by the following formula (I): R E’X =E' Z / E' Z0 (I) {where, E' Z This is the storage modulus measured in the temperature range of 160°C to 300°C after the crosslinking reaction of the microporous membrane for the energy storage device has proceeded within the energy storage device, and E' Z0 E' is the storage modulus measured in the temperature range of 160°C to 300°C before the microporous membrane for the energy storage device is incorporated into the energy storage device, and E' is the storage modulus measured in the temperature range of 160°C to 300°C. Z or E' Z0 The measurement conditions for the storage modulus are defined by the following configurations (i) to (iv). (i) Dynamic viscoelasticity measurement under the following conditions: • Atmosphere: Nitrogen • Measuring instrument used: RSA-G2 (manufactured by TA Instruments) • Sample film thickness: 5 μm to 50 μm (Measurements are performed on a single sample regardless of its film thickness) • Measurement temperature range: -50 to 300°C • Heating rate: 10℃ / min ·Measurement frequency: 1Hz • Deformation mode: Sinusoidal tension mode (linear tension) Initial value of static tensile load: 0.5N • Initial gap distance (at 25°C): 25mm • Auto strain adjustment: Enabled (Range: Amplitude value 0.05~25%, sinusoidal load 0.02~5N) It was done there. (ii) Static tensile load refers to the midpoint between the maximum and minimum stresses in each periodic motion, and sinusoidal load refers to the vibrational stress centered on the static tensile load. (iii) The sinusoidal tensile mode refers to measuring vibrational stress while performing periodic motion at a fixed amplitude of 0.2%, in which case the distance between gaps and the static tensile load were varied to measure the vibrational stress such that the difference between the static tensile load and the sinusoidal load was within 20%. When the sinusoidal load was 0.02 N or less, the amplitude value was amplified to measure the vibrational stress such that the sinusoidal load was 5 N or less and the increase in the amplitude value was within 25%. (iv) The obtained relationship between the sinusoidal load and the amplitude value, and the following formula: σ * =σ0·Exp[i(ωt+δ)], ε * =ε0·Exp(iωt), σ * =E * ·ε * E * =E'+iE'' (wherein, σ * : vibrational stress, ε * : strain, i: imaginary unit, ω: angular frequency, t: time, δ: phase difference between vibrational stress and strain, E * : complex elastic modulus, E': storage elastic modulus, E'': loss elastic modulus Vibrational stress: sinusoidal load / initial cross-sectional area Static tensile load: the load at the minimum point of vibrational stress in each cycle (the minimum point of the distance between gaps in each cycle) Sinusoidal load: the difference between the measured vibrational stress and the static tensile load) to calculate the storage elastic modulus.} The mixed storage elastic modulus ratio (R E’x ) defined by is 1.2 times to 20 times, the microporous membrane for electricity storage devices according to any one of items 1 to 5. [7] A microporous membrane for electricity storage devices comprising a polyolefin, wherein the microporous membrane for electricity storage devices has an amorphous part crosslinked structure in which the amorphous part of the polyolefin is crosslinked, The polyolefin satisfies the following requirements (A) to (C): (A) The melt flow rate (MFR) when measured under the conditions of a temperature of 230°C and a mass of 2.16 kg is 3.0 g / 10 min or less; (B) The value obtained by dividing the weight-average molecular weight Mw by the number-average molecular weight Mn (Mw / Mn) is 15 or less; and (C) Density is 0.85 g / cm³ 3 That's all; Satisfying the conditions, and The microporous membrane for the energy storage device meets the following requirement (D): (D) The ratio of the orientation ratio in the width direction (TD) to the machine direction (MD) when measured by wide-angle X-ray scattering is MD / TD, which is 1.3 or greater; A microporous film for energy storage devices characterized by satisfying the following conditions. [8] A microporous film for an energy storage device according to item 7, wherein the amorphous portion is selectively crosslinked. [9] The microporous membrane for the energy storage device is given by the following formula (II): R E’mix =E' / E'0(II) {wherein E' is the storage modulus measured at 160°C to 300°C when the microporous film for the energy storage device has the amorphous crosslinking structure, and E'0 is the storage modulus measured at 160°C to 300°C for a microporous film for energy storage devices that does not have an amorphous crosslinking structure, and the measurement conditions for a storage modulus that is E' or E'0 are defined by the following configurations (i) to (iv). (i) Dynamic viscoelasticity measurement under the following conditions: • Atmosphere: Nitrogen • Measuring instrument used: RSA-G2 (manufactured by TA Instruments) • Sample film thickness: 5 μm to 50 μm (Measurements are performed on a single sample regardless of its film thickness) • Measurement temperature range: -50 to 300°C • Heating rate: 10℃ / min ·Measurement frequency: 1Hz • Deformation mode: Sinusoidal tension mode (linear tension) Initial value of static tensile load: 0.5N • Initial gap distance (at 25°C): 25mm • Auto strain adjustment: Enabled (Range: Amplitude value 0.05~25%, sinusoidal load 0.02~5N) It was done there. (ii) Static tensile load refers to the midpoint between the maximum and minimum stresses in each periodic motion, and sinusoidal load refers to the vibrational stress centered on the static tensile load. (iii) The sinusoidal tensile mode refers to measuring vibration stress while performing periodic motion with a fixed amplitude of 0.2%. In this process, the gap distance and static tensile load were varied so that the difference between the static tensile load and the sinusoidal load was within 20%. When the sinusoidal load fell below 0.02N, the amplitude was amplified so that the sinusoidal load remained within 5N and the increase in amplitude was within 25% before measuring the vibration stress. (iv) Relationship between the obtained sinusoidal load and amplitude value, and the following equation: σ * =σ0·Exp[i(ωt+δ)], ε * =ε0·Exp(iωt), σ * =E * ·ε * E * =E'+iE'' (In the formula, σ * : Vibration stress, ε * : strain, i: imaginary unit, ω: angular frequency, t: time, δ: phase difference between vibrational stress and strain, E * :complex modulus of elasticity, E':storage modulus of elasticity, E'':loss modulus of elasticity Vibration stress: sinusoidal load / initial cross-sectional area Static tensile load: The load at the point of minimum vibration stress in each period (the point of minimum gap distance in each period). Sinusoidal load: (The difference between the measured vibration stress and the static tensile load) The storage modulus is calculated from this. The mixed storage modulus ratio (R) is defined by E’mix A microporous membrane for energy storage devices as described in item 7 or 8, wherein the ratio is 1.2 to 20 times.

[10] The aforementioned polyolefin has an MFR of 0.25 g / 10 min or higher, an Mw / Mn ratio of 4.0 or higher, and a density of 1.1 g / cm³. 3 The following and The orientation ratio MD / TD of the microporous film for the energy storage device is 3.0 or less. A microporous film for energy storage devices as described in any one of items 1 to 9.

[11] A microporous membrane for an energy storage device according to any one of items 1 to 10, wherein the polyolefin is polypropylene.

[12] A microporous film for energy storage devices containing polypropylene, The polypropylene has one or more functional groups and is β-crystalline active. A microporous membrane for an energy storage device in which, after being placed in an energy storage device, (1) the functional groups undergo a condensation reaction, (2) the functional groups react with chemical substances inside the energy storage device, or (3) the functional groups react with other types of functional groups to form a crosslinked structure.

[13] The crosslinked structure is (1) a microporous film for an energy storage device as described in item 12, formed by a condensation reaction between the functional groups.

[14] The crosslinked structure is (2) a microporous membrane for an energy storage device according to item 12, formed by the functional group reacting with a chemical substance inside the energy storage device.

[15] A microporous membrane for an energy storage device according to item 12 or 14, wherein the chemical substance is one of the electrolyte, electrolyte solution, electrode active material, additive, or decomposition products thereof contained in the energy storage device.

[16] The crosslinked structure is (3) a microporous film for an energy storage device according to item 12, formed by the reaction of the functional group with another type of functional group.

[17] The microporous membrane for the energy storage device is given by the following formula (I): R E’X =E' Z / E' Z0 (I) {where, E' Z This is the storage modulus measured in the temperature range of 160°C to 300°C after the crosslinking reaction of the microporous membrane for the energy storage device has proceeded within the energy storage device, and E' Z0 E' is the storage modulus measured in the temperature range of 160°C to 300°C before the porous membrane for the energy storage device is incorporated into the energy storage device, and E' is the storage modulus measured in the temperature range of 160°C to 300°C. Z or E' Z0 The measurement conditions for the storage modulus are defined by the following configurations (i) to (iv). (i) Dynamic viscoelasticity measurement under the following conditions: • Atmosphere: Nitrogen • Measuring instrument used: RSA-G2 (manufactured by TA Instruments) • Sample film thickness: 5 μm to 50 μm (Measurements are performed on a single sample regardless of its film thickness) • Measurement temperature range: -50 to 300°C • Heating rate: 10℃ / min ·Measurement frequency: 1Hz • Deformation mode: Sinusoidal tension mode (linear tension) Initial value of static tensile load: 0.5N • Initial gap distance (at 25°C): 25mm • Auto strain adjustment: Enabled (Range: Amplitude value 0.05~25%, sinusoidal load 0.02~5N) It was done there. (ii) Static tensile load refers to the midpoint between the maximum and minimum stresses in each periodic motion, and sinusoidal load refers to the vibrational stress centered on the static tensile load. (iii) The sinusoidal tensile mode refers to measuring vibration stress while performing periodic motion with a fixed amplitude of 0.2%. In this process, the gap distance and static tensile load were varied so that the difference between the static tensile load and the sinusoidal load was within 20%. When the sinusoidal load fell below 0.02N, the amplitude was amplified so that the sinusoidal load remained within 5N and the increase in amplitude was within 25% before measuring the vibration stress. (iv) Relationship between the obtained sinusoidal load and amplitude value, and the following equation: σ * =σ0·Exp[i(ωt+δ)], ε * =ε0·Exp(iωt), σ* =E * ·ε * E * =E'+iE'' (In the formula, σ * : Vibration stress, ε * : strain, i: imaginary unit, ω: angular frequency, t: time, δ: phase difference between vibrational stress and strain, E * :complex modulus of elasticity, E':storage modulus of elasticity, E'':loss modulus of elasticity Vibration stress: sinusoidal load / initial cross-sectional area Static tensile load: The load at the point of minimum vibration stress in each period (the point of minimum gap distance in each period). Sinusoidal load: (The difference between the measured vibration stress and the static tensile load) The storage modulus is calculated from this. The mixed storage modulus ratio (R) is defined by E’x A microporous film for energy storage devices as described in any one of items 12 to 16, wherein the ratio is 1.2 to 20 times.

[18] A microporous membrane for energy storage devices comprising polypropylene, wherein the polypropylene is β-crystalline active, and the microporous membrane for energy storage devices has an amorphous crosslinking structure in which the amorphous portion of the polypropylene is crosslinked.

[19] A microporous film for an energy storage device according to item 18, wherein the amorphous portion is selectively crosslinked.

[20] The microporous membrane for the energy storage device is given by the following formula (II): R E’mix =E' / E'0(II) {wherein E' is the storage modulus measured at 160°C to 300°C when the microporous film for the energy storage device has the amorphous crosslinking structure, and E'0 is the storage modulus measured at 160°C to 300°C for a microporous film for energy storage devices that does not have an amorphous crosslinking structure, and the measurement conditions for a storage modulus that is E' or E'0 are defined by the following configurations (i) to (iv). (i) Dynamic viscoelasticity measurement under the following conditions: • Atmosphere: Nitrogen • Measuring instrument used: RSA-G2 (manufactured by TA Instruments) • Sample film thickness: 5 μm to 50 μm (Measurements are performed on a single sample regardless of its film thickness) • Measurement temperature range: -50 to 300°C • Heating rate: 10℃ / min ·Measurement frequency: 1Hz • Deformation mode: Sinusoidal tension mode (linear tension) Initial value of static tensile load: 0.5N • Initial gap distance (at 25°C): 25mm • Auto strain adjustment: Enabled (Range: Amplitude value 0.05~25%, sinusoidal load 0.02~5N) It was done there. (ii) Static tensile load refers to the midpoint between the maximum and minimum stresses in each periodic motion, and sinusoidal load refers to the vibrational stress centered on the static tensile load. (iii) The sinusoidal tensile mode refers to measuring vibration stress while performing periodic motion with a fixed amplitude of 0.2%. In this process, the gap distance and static tensile load were varied so that the difference between the static tensile load and the sinusoidal load was within 20%. When the sinusoidal load fell below 0.02N, the amplitude was amplified so that the sinusoidal load remained within 5N and the increase in amplitude was within 25% before measuring the vibration stress. (iv) Relationship between the obtained sinusoidal load and amplitude value, and the following equation: σ * =σ0·Exp[i(ωt+δ)], ε * =ε0·Exp(iωt), σ * =E * ·ε * E * =E'+iE'' (In the formula, σ * : Vibration stress, ε * : strain, i: imaginary unit, ω: angular frequency, t: time, δ: phase difference between vibrational stress and strain, E * :complex modulus of elasticity, E':storage modulus of elasticity, E'':loss modulus of elasticity Vibration stress: sinusoidal load / initial cross-sectional area Static tensile load: The load at the point of minimum vibration stress in each period (the point of minimum gap distance in each period). Sinusoidal load: (The difference between the measured vibration stress and the static tensile load) The storage modulus is calculated from this. The mixed storage modulus ratio (R) is defined by E’mix A microporous membrane for energy storage devices as described in item 18 or 19, wherein the ratio is 1.2 to 20 times. [twenty one] The microporous membrane for the energy storage device is made of polypropylene, The following requirements (P1)~(P3): (P1) The MFR measured under conditions of a temperature of 230°C and a mass of 2.16 kg is 2.5 g / 10 min or less; (P2) The value obtained by dividing the weight-average molecular weight Mw by the number-average molecular weight Mn (Mw / Mn) is 10 or less; and (P3) Density is 0.89 g / cm³ 3 That's all: Homopolypropylene (A) that satisfies the following conditions, Polypropylene (B) that does not satisfy at least one of the above requirements (P1) to (P3) and has a functional group, Microporous membranes for energy storage devices, including any one of items 12 to 20. [twenty two] A microporous membrane for energy storage devices according to item 21, wherein the content of polypropylene (B) is 4% by mass or more and 30% by mass or less. [twenty three] A microporous membrane for an energy storage device according to item 21 or 22, wherein the polypropylene (B) is silane-modified polypropylene. [twenty four] The aforementioned homopolypropylene (A) has an MFR of 0.25 g / 10 min or higher, an Mw / Mn ratio of 4.9 or higher, and a density of 0.96 g / cm³. 3 A microporous film for energy storage devices as described in any one of items 21 to 23 below. [Effects of the Invention]

[0011] According to the present invention, it is possible to improve the film rupture resistance at high temperatures without impairing the strength and porosity of microporous films for energy storage devices, thereby achieving both high battery performance and high safety in nail penetration tests for energy storage devices equipped with microporous films as separators. Furthermore, according to the present invention, it is not necessary to form a crosslinked structure during or immediately after the film formation process, so it is possible to suppress the increase in internal stress of the separator and deformation after the fabrication of the energy storage device, and / or to impart a crosslinked structure to the separator without using relatively high energy such as light irradiation or heating. [Brief explanation of the drawing]

[0012] [Figure 1] Figure 1 is a schematic diagram illustrating a crystalline polymer having a higher-order structure divided into lamellae (crystalline parts), amorphous parts, and intermediate layers between them. [Figure 2] This is a schematic diagram illustrating the crystal growth of polyolefin molecules. [Figure 3] Figure 3 is an example of a graph illustrating the relationship between temperature and storage modulus, comparing the storage moduli of a reference film and a crosslinked film within a temperature range of -50°C to 310°C, and showing the transition temperature between the rubbery flat region and the crystalline melting flow region. [Figure 4] Figure 4 is an example of a graph illustrating the relationship between temperature and loss modulus, comparing the loss modulus of a reference film and a crosslinked film within a temperature range of -50°C to 310°C, and showing the transition temperature between the rubbery flat region and the crystalline melting flow region. [Modes for carrying out the invention]

[0013] The following describes in detail embodiments for carrying out the present invention (hereinafter abbreviated as "embodiments"). It should be noted that the present invention is not limited to the following embodiments, and can be implemented in various modifications within the scope of its essence.

[0014] [Microporous membrane for energy storage devices] A microporous membrane can be formed from one or more types of polyolefin resins, or it can be a composite resin membrane having a polyolefin resin and another resin, and it has a large number of fine pores. A microporous membrane containing polyolefin resin as the main component (hereinafter also referred to as a polyolefin microporous membrane) contains 50% by mass or more of polyolefin resin relative to the mass of the membrane.

[0015] Polyolefin-based microporous membranes are preferably used to form energy storage devices, more preferably as constituent materials for energy storage devices, even more preferably as separators for energy storage devices, and particularly preferably as separators for lithium-ion batteries, from the viewpoint of resistance to oxidation-reduction degradation and a dense, uniform porous structure. In this specification, an energy storage device separator (hereinafter sometimes abbreviated as "separator") refers to a component that is placed between a plurality of electrodes in an energy storage device and has ion permeability and, if necessary, shutdown characteristics. The separator includes a microporous membrane and may further include any functional layer as desired.

[0016] [First and Second Embodiments] The microporous membrane according to the first embodiment comprises a polyolefin having one or more functional groups, and after being housed in an energy storage device, a crosslinked structure is formed by (1) condensation reactions between the functional groups of the polyolefin, (2) reactions between the functional groups of the polyolefin and chemical substances inside the energy storage device, or (3) reactions between the functional groups of the polyolefin and other types of functional groups. In the first embodiment, the microporous membrane can form a crosslinked structure by any of the above reactions (1) to (3), thereby maintaining strength and improving resistance to film breakage at high temperatures of 150°C or higher, and tends to achieve a balance between device characteristics and safety when housed in an energy storage device, for example as a separator.

[0017] Furthermore, in the first embodiment, the polyolefin contained in the microporous membrane meets the following requirements (A) to (C): (A) The melt flow rate (MFR) measured under conditions of a temperature of 230°C and a mass of 2.16 kg is 3.0 g / 10 min or less; (B) The value obtained by dividing the weight-average molecular weight Mw by the number-average molecular weight Mn (Mw / Mn) is 15 or less; and (C) Density is 0.85 g / cm³ 3 That's all; The following conditions must be met, and the microporous membrane must meet the following requirement (D): (D) The ratio of the orientation ratio in the width direction (TD) to the machine direction (MD) measured by wide-angle X-ray scattering, MD / TD, is 1.3 or greater; The following conditions are met. In the first embodiment, when the polyolefin and the microporous membrane satisfy requirements (A) to (D), the strength, film-forming properties, productivity, and porosity of the microporous membrane tend to improve.

[0018] Regarding requirement (A), if the MFR of polyolefin (PO) measured under conditions of a temperature of 230°C and a mass of 2.16 kg is 3.0 g / 10 min or less, the strength of the resulting microporous film is more likely to reach an acceptable level. From a similar viewpoint, the MFR of PO is preferably 0.25 to 2.9 g / 10 min, more preferably 0.3 to 2.7 g / 10 min, and even more preferably 0.4 to 2.5 g / 10 min. The MFR of polyolefin (PO) measured under conditions of a temperature of 230°C and a mass of 2.16 kg may be 0.5 g / 10 min or more, 0.6 g / 10 min or more, 0.7 g / 10 min or more, 0.8 g / 10 min or more, 0.9 g / 10 min or more, or 1.0 g / 10 min or more. Under conditions of a temperature of 230°C and a mass of 2.16 kg, the MFR of polyolefin (PO) may be 2.3 g / 10 min or less, 2.0 g / 10 min or less, 1.8 g / 10 min or less, or 1.5 g / 10 min or less.

[0019] Regarding requirement (B), when the dispersion of PO (Mw / Mn) is 15 or less, it tends to be possible to achieve both good film-forming properties and strength when molding the resulting PO. From the viewpoint of achieving both good film-forming properties and strength, the dispersion of PO (Mw / Mn) is preferably 4.0 to 13, more preferably 4.9 to 11, and even more preferably 5.2 to 9.0. The dispersion of PO (Mw / Mn) may be 5.5 or higher, 5.8 or higher, 6.0 or higher, 6.2 or higher, or 6.5 or higher. The dispersion of PO (Mw / Mn) may be 8.0 or lower, 7.0 or lower, or 6.5 or lower.

[0020] Regarding requirement (C), since the PO density is closely related to the crystallinity of PO, it should be 0.85 g / cm³. 3 At the above PO density, the productivity of microporous membranes is improved, and it is particularly effective for the dry porosity method. From the viewpoint of productivity and porosity, the PO density is 0.85 g / cm³. 3 The above is preferable, 0.88 g / cm³ 3 The above is preferable, or 0.90 g / cm³. 3 The above is preferable. Furthermore, the PO density is 1.1 g / cm³. 3 The following is preferable: 1.0 g / cm³ 3 The following is preferable: 0.98 g / cm³ 3 The following is preferable: 0.97 g / cm³ 3 The following is preferable: 0.96 g / cm³ 3 The following is preferable: 0.95 g / cm³ 3 The following is preferable: 0.94 g / cm³ 3 The following is preferable: 0.93 g / cm³ 3 The following is preferable, or 0.92 g / cm³ 3 Less than is preferable. Examples of PO include polypropylene and polyethylene.

[0021] Regarding requirement (D), when measuring the wide-angle X-ray scattering of a microporous film, if the orientation ratio MD / TD is 1.3 or higher, the microporous properties, crosslinking structure, and ion permeability of the film tend to conform to the desired device characteristics. From the viewpoint of conforming film properties and device characteristics, the lower limit of the orientation ratio MD / TD is preferably 1.4 or higher or 1.5 or higher, and more preferably 1.6 or higher. The upper limit of the orientation ratio MD / TD can be, for example, 4.0 or lower, 3.5 or lower, or 3.1 or lower, depending on the film formation process.

[0022] The microporous film according to the second embodiment comprises β-crystal active polypropylene having one or more functional groups, and after being placed in an energy storage device, a crosslinked structure is formed by (1) condensation reactions between the functional groups of the polypropylene, (2) reactions between the functional groups of the polypropylene and chemical substances inside the energy storage device, or (3) reactions between the functional groups of the polypropylene and other types of functional groups. In the second embodiment, an undrawn sheet having β-crystals is produced by melt extrusion of β-crystal active polypropylene, and the produced undrawn sheet is stretched to undergo a crystal transition to an α-crystal with a relatively high crystal density. Micropores are formed due to the difference in crystal density between the two to obtain a microporous film. The obtained microporous film can form a crosslinked structure by any of the reactions (1) to (3) above, thereby maintaining strength and improving resistance to film breakage at high temperatures of 150°C or higher, and tends to achieve both the device characteristics and safety of the energy storage device. The microporous membrane according to the second embodiment may contain one or more types of polypropylene, and if it contains multiple types of polypropylene, at least one of them has one or more functional groups and β-crystal activity.

[0023] In the first and second embodiments, the functional groups contained in polyolefins such as polypropylene are not incorporated into the crystalline portion of the polyolefin, but are crosslinked in the amorphous portion. Therefore, the microporous membranes according to the first and second embodiments can, after being housed in an energy storage device, form a crosslinked structure using the surrounding environment or chemical substances inside the energy storage device, thereby suppressing an increase in internal stress or deformation of the fabricated energy storage device, and contributing to safety. On the other hand, if a microporous membrane undergoes a cross-linking reaction before being housed in an energy storage device, and then goes through processes such as winding and slitting, the effects of stresses such as tension generated during those processes will remain. In this case, if these stresses are released after the assembly of the energy storage device, it is undesirable because it may cause deformation of the electrode windings or damage due to stress concentration.

[0024] Furthermore, in the first and second embodiments, it is not necessary to form a crosslinked structure during or immediately after the film formation process. Therefore, when using a microporous film as a separator, it is possible to suppress an increase in internal stress and deformation after the fabrication of the energy storage device, and / or contribute to energy saving without using light irradiation or heating to form a crosslinked structure.

[0025] [Third and Fourth Embodiments] The microporous membrane according to the third embodiment contains a polyolefin and has an amorphous crosslinked structure in which the amorphous portion of the polyolefin is crosslinked. In the third embodiment, the amorphous crosslinked structure of the polyolefin can improve the film's resistance to rupture at high temperatures of 150°C or higher, and when the microporous membrane is incorporated into an energy storage device as a separator, it tends to achieve both device characteristics and safety.

[0026] Furthermore, in the third embodiment, the polyolefin contained in the microporous membrane meets the following requirements (A) to (C): (A) The melt flow rate (MFR) measured under conditions of a temperature of 230°C and a mass of 2.16 kg is 3.0 g / 10 min or less; (B) The value obtained by dividing the weight-average molecular weight Mw by the number-average molecular weight Mn (Mw / Mn) is 15 or less; and (C) Density is 0.85 g / cm³ 3 That's all; The following conditions must be met, and the microporous membrane must meet the following requirement (D): (D) The ratio of the orientation ratio in the width direction (TD) to the machine direction (MD) measured by wide-angle X-ray scattering, MD / TD, is 1.3 or greater; The following conditions are met. In the third embodiment, when the polyolefin and the microporous membrane satisfy requirements (A) to (D), the strength, film-forming properties, productivity, porosity, and ion permeability of the microporous membrane, as well as the characteristics of the energy storage device, tend to improve for the same reasons as requirements (A) to (D) described in the first embodiment.

[0027] The microporous film according to the fourth embodiment contains polypropylene having β-crystal activity and has an amorphous crosslinked structure in which the amorphous portion of the polypropylene is crosslinked. In the fourth embodiment, an undrawn sheet having β-crystals is produced by melt extrusion of polypropylene having β-crystal activity, and the produced undrawn sheet is stretched to induce a crystal transition to an α-crystal with a relatively high crystal density. Micropores are formed due to the difference in crystal density between the two to obtain a microporous film. Since the obtained microporous film has an amorphous crosslinked structure, its resistance to film breakage at high temperatures of 150°C or higher can be improved, and it tends to achieve both device characteristics and safety in energy storage devices. The microporous film according to the fourth embodiment may contain one or more types of polypropylene, and if it contains multiple types of polypropylene, at least one of them has β-crystal activity.

[0028] In the third and fourth embodiments, the functional groups contained in polyolefins such as polypropylene are not incorporated into the crystalline portion of the polyolefin, but are crosslinked in the amorphous portion. Therefore, the microporous films according to the third and fourth embodiments can suppress an increase in internal stress or deformation of the fabricated energy storage device while achieving both shutdown function and high-temperature rupture resistance, compared to conventional crosslinked microporous films in which the crystalline portion and its periphery are easily crosslinked, thereby ensuring the safety of the energy storage device. From a similar viewpoint, the amorphous portion of the polyolefin contained in the microporous films according to the third and fourth embodiments is preferably selectively crosslinked, and more preferably significantly more crosslinked than the crystalline portion.

[0029] [Mechanism of crosslinking reaction] In the first, second, third, and fourth embodiments, the crosslinking reaction mechanism and crosslinking structure are not clear, but the inventors consider them to be as follows (a) to (d).

[0030] (a) Crystal structure in polyolefin microporous membranes Polyolefin resins, such as polyethylene, are generally crystalline polymers, as shown in Figure 1. They have a higher-order structure divided into lamellae (crystalline parts), amorphous parts, and intermediate layers between them. In the crystalline parts and the intermediate layers between the crystalline and amorphous parts, the mobility of the polymer chains is low and separation is not possible, but relaxation phenomena can be observed in solid viscoelasticity measurements in the 0°C to 120°C range. On the other hand, the mobility of the polymer chains in the amorphous parts is very high and is observed in solid viscoelasticity measurements in the -150°C to -100°C range. This point is related to radical relaxation or radical transfer reactions, crosslinking reactions, etc., which will be described later.

[0031] Furthermore, the polyolefin molecules that constitute the crystal are not single molecules, but rather, as illustrated in Figure 2, multiple polymer chains form small lamellae, which then aggregate to form a crystal. Such phenomena are difficult to observe directly, and in recent years, they have been scientifically studied and clarified through simulations. In this specification, a crystal refers to the smallest crystal unit measured by X-ray structural analysis, and is the unit that can be calculated as crystallite size. Thus, even within the crystalline portion (inside the lamellae), it is predicted that there are parts of the crystal that are not constrained and have somewhat higher mobility.

[0032] (i) Mechanism of crosslinking reaction by electron beam Next, the reaction mechanism for electron beam crosslinking (hereinafter referred to as EB crosslinking) of polymers is as follows. (i) Irradiation with electron beams ranging from tens of kGy to hundreds of kGy, (ii) Transmission of electron beam into the reactant (polymer) and generation of secondary electrons, (iii) Hydrogen abstraction reaction in polymer chains by secondary electrons and radical generation, (iv) Abstraction of adjacent hydrogens by radicals and movement of active sites, (v) Crosslinking reaction or polyene formation by recombination of radicals. Here, radicals generated in the crystalline region have poor mobility, persist for a long period, and because impurities cannot penetrate the crystal, the probability of reaction and quenching is low. Such radical species are called stable radicals, and they persist for a long period of several months, with their lifetime revealed by ESR measurement. As a result, crosslinking reactions within the crystal are considered to be poor. However, in the unconstrained molecular chains present in small amounts within the crystal, or in the surrounding crystalline-amorphous intermediate layer, the generated radicals have a somewhat longer lifetime. Such radical species are called persistent radicals, and it is thought that crosslinking reactions between molecular chains proceed with a high probability in a mobile environment. On the other hand, because the amorphous region has very high mobility, the generated radical species have a short lifetime, and it is thought that not only crosslinking reactions between molecular chains but also polyene reactions within a single molecular chain proceed with a high probability. As described above, at the microscopic level of the crystal, it can be inferred that the crosslinking reaction by EB crosslinking is localized within or around the crystal.

[0033] (c) Mechanism of crosslinking reaction by chemical reaction As mentioned above, polyolefin resins have both crystalline and amorphous regions. However, the functional groups mentioned above do not exist inside the crystal due to steric hindrance, but are localized in the amorphous region. This is generally known; units such as methyl groups, which are present in small amounts in the polyethylene chain, may be incorporated into the crystal, but grafts that are bulkier than ethyl groups are not incorporated ("Basic Polymer Chemistry," published by Tokyo Kagaku Dojin). For this reason, crosslinking sites resulting from reactions other than electron beam crosslinking are localized only in the amorphous region.

[0034] (e) Relationship between differences in cross-linking structures and their effects To form a crosslinked structure in a microporous membrane, it is preferable to use a combination of functional groups in the polyolefin resin and chemical substances contained in the energy storage device, or to use chemical substances contained in the energy storage device as a catalyst. In crosslinking reactions caused by chemical reactions inside the energy storage device, the morphology of the reaction products differs depending on the raw materials or catalysts used. In the research leading up to the present invention, the following experiments were conducted to elucidate the phenomenon in order to clarify the crosslinked structure and the changes in the physical properties of the microporous membrane accompanying structural changes.

[0035] The behavior of EB-crosslinked or uncrosslinked films and chemically crosslinked films during crystal melting was investigated using fuse / meltdown characteristic tests. The results showed that the EB-crosslinked film exhibited a significantly higher fuse temperature, with the meltdown temperature rising to over 200°C. On the other hand, the chemically crosslinked film showed no change in fuse temperature before and after crosslinking, but its meltdown temperature rose to over 200°C. This suggests that the EB-crosslinked film's fuse characteristics, due to crosslinking around the crystalline region, were affected by the increased melting temperature and decreased melting rate. Conversely, the chemically crosslinked film, lacking a crosslinked structure in the crystalline region, was deemed unaffected by the change in fuse characteristics. Furthermore, in the high-temperature range around 200°C, both films, after crystal melting, possess a crosslinked structure, allowing the entire resin to stabilize in a gel state and achieve good meltdown characteristics.

[0036] The above findings are summarized in Table 1 below. [Table 1]

[0037] In the first and third embodiments, (1) the condensation reaction between functional groups of polyolefins such as polyethylene and polypropylene can be, for example, a reaction via covalent bonding between two or more functional groups A contained in the polyolefin. Also, (3) the reaction between a functional group of polyolefin and another type of functional group can be, for example, a reaction via covalent bonding between functional group A and functional group B contained in the polyolefin.

[0038] In the first and third embodiments, (2) in the reaction between a functional group of a polyolefin such as polyethylene or polypropylene and a chemical substance inside the energy storage device, for example, functional group A contained in the polyolefin can form a covalent bond or coordination bond with any of the electrolyte, electrolyte solution, electrode active material, additive, or decomposition products thereof contained in the energy storage device. Furthermore, according to reaction (2), a cross-linking structure can be formed not only inside the separator but also between the separator and the electrode or between the separator and the solid electrolyte interface (SEI), thereby improving the strength between multiple components of the energy storage device.

[0039] The microporous films according to the first, second, third, and fourth embodiments are formulated using the following formula (I): R E’X =E' Z / E' z0 (I) {where, E' Z This is the storage modulus measured in the temperature range of 160°C to 300°C after the crosslinking reaction of the microporous membrane has proceeded within the energy storage device, and E' z0 This is the storage modulus measured in the temperature range of 160°C to 300°C before the microporous membrane was incorporated into the energy storage device. The mixed storage modulus ratio (R) is defined by E’x ), and / or the following formula (III): R E’’X =E'' Z / E'' Z0 (III) {in formula, E'' Z This is the loss modulus measured in the temperature range of 160°C to 300°C after the crosslinking reaction of the microporous membrane has proceeded within the energy storage device, and E'' Z0 This is the loss modulus measured in the temperature range of 160°C to 300°C before the microporous membrane was incorporated into the energy storage device. The mixed loss modulus ratio (R) is defined by E’’x), preferably 1.2 times to 20 times, more preferably 2.0 times to 18 times, and still more preferably 3.0 times to 16.5 times. In addition, E' Z and E' z0 and E'' Z and E'' z0 are each an average value of the storage elastic modulus or the loss elastic modulus measured within the set temperature range of a measurement apparatus, where the widest temperature range is 160°C to 300°C. In the case of a laminated film, only the polyolefin microporous membrane is removed from the laminated film, and the storage elastic modulus E' Z and E' z0 and the loss elastic modulus E'' Z and E'' z0 are to be measured. The measurement conditions for the elastic modulus that is E' Z , E' z0 , E'' Z or E'' z0 are described in the Examples.

[0040] The separators according to the first, second, third, and fourth embodiments satisfy, from the viewpoints of forming an amorphous part crosslinked structure, achieving both a shutdown function and high-temperature membrane rupture resistance, and the like, the following formula (II): R E’mix =E' / E'₀ (II) {wherein E' is the storage elastic modulus of the microporous membrane having an amorphous part crosslinked structure, measured at 160°C to 300°C, and E'₀ is the storage elastic modulus of the microporous membrane not having an amorphous part crosslinked structure, measured at 160°C to 300°C.} the mixed storage elastic modulus ratio (R E’mix ) defined by, and / or the following formula (IV): R E’’mix =E'' / E''₀ (IV) {wherein E'' is the loss elastic modulus measured at 160°C to 300°C when the microporous membrane has an amorphous part crosslinked structure, and E''₀ is the loss elastic modulus of the microporous membrane not having an amorphous part crosslinked structure, measured at 160°C to 300°C.} the mixed loss elastic modulus ratio (R E’’mixThe storage modulus or loss modulus is preferably 1.2 to 20 times, more preferably 2.0 to 18 times, and even more preferably 3.0 to 17 times. E' and E'0 and E'' and E''0 are the average values ​​of the storage modulus or loss modulus measured within the set temperature range of the measuring device, with the widest temperature range being 160°C to 300°C. In the case of a laminated film, the storage modulus E' and E'0 and the loss modulus E'' and E''0 are measured by removing only the polyolefin-based microporous film from the laminated film. The measurement conditions for the moduli that are E', E'0, E'', or E''0 are described in the examples.

[0041] The components of the microporous membrane according to the first, second, third, and fourth embodiments are described below.

[0042] [Polyolefins] The polyolefin constituting the microporous membrane is not particularly limited, but examples include homopolymers of ethylene or propylene, or copolymers formed from at least two monomers selected from the group consisting of ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, and norbornene. Among these, high-density polyethylene, low-density polyethylene, ultra-high molecular weight polyethylene (UHMWPE), polypropylene, polybutene, or combinations thereof are preferred, with polypropylene being more preferred, from the viewpoint of ease of porosity formation in wet or dry processes. Generally, the weight-average molecular weight of UHMWPE is known to be 1,000,000 or more. Note that the polyolefin may be used alone or in combination of two or more types.

[0043] Furthermore, the weight-average molecular weight (Mw) of the polyolefin can be arbitrarily determined such that the degree of dispersion (Mw / Mn) of requirement (B) described above is 15 or less, and from the viewpoint of the thermal shrinkability of the microporous membrane and the safety of the energy storage device, it is preferably 10,000 to 2,000,000, more preferably 20,000 to 1,500,000, and even more preferably 30,000 to 1,000,000. From a similar viewpoint, the microporous membrane preferably contains 3 to 25% by mass, more preferably 5 to 20% by mass, of the polyolefin having an Mw of 10,000 to 2,000,000, relative to the total amount of raw material polyolefin.

[0044] [Polyolefins having one or more functional groups] The microporous membrane preferably contains a functionally modified polyolefin or a polyolefin copolymerized with monomers having functional groups, as a polyolefin having one or more functional groups, from the viewpoint of forming a crosslinked structure, resistance to oxidation-reduction degradation, and a dense and uniform porous structure. In this specification, a functionally modified polyolefin refers to a polyolefin to which functional groups have been bonded after its production. The functional groups are those that can be bonded to the polyolefin skeleton or introduced into the comonomer, and preferably are those that participate in the selective crosslinking of the amorphous portion of the polyolefin. For example, they can be at least one selected from the group consisting of carboxyl groups, hydroxyl groups, carbonyl groups, polymerizable unsaturated hydrocarbon groups, isocyanate groups, epoxy groups, silanol groups, hydrazide groups, carbodiimide groups, oxazoline groups, acetoacetyl groups, aziridine groups, ester groups, active ester groups, carbonate groups, azide groups, linear or cyclic heteroatom-containing hydrocarbon groups, amino groups, sulfhydryl groups, metal chelate groups, and halogen-containing groups.

[0045] [Multiple types of polypropylene] From the viewpoint of strength, ion permeability, resistance to oxidation-reduction degradation, and dense and uniform porous structure of the microporous membrane, it is preferable that the microporous membrane contains both a polyolefin having one or more functional groups and other polyolefins, and more preferably contains both a first polypropylene (A) and a second polypropylene (B) which can be distinguished from polypropylene (A) and has functional groups.

[0046] The first polypropylene (A) meets the following requirements (P1) to (P3) from the viewpoint of strength, film formation, productivity and porosity of microporous films: (P1) The MFR measured under conditions of a temperature of 230°C and a mass of 2.16 kg is 2.5 g / 10 min or less; (P2) The value obtained by dividing the weight-average molecular weight Mw by the number-average molecular weight Mn (Mw / Mn) is 10 or less; and (P3) Density is 0.89 g / cm³ 3 That's all: It is preferable that the homopolypropylene (A) satisfies the following requirements. For requirement (P1) of homopolypropylene (A), the MFR is more preferably 0.25 to 2.4 g / 10 min. For requirement (P2), the dispersion degree (Mw / Mn) of homopolypropylene (A) is more preferably 4.9 to 9.0. For requirement (P3), the density of homopolypropylene (A) is more preferably 0.90 g / cm³. 3 The above and 0.96 g / cm³ 3 The following, or 0.90 g / cm³ 3 The above and 0.93 g / cm³ 3 The following applies:

[0047] On the other hand, the second polypropylene (B) having a functional group is a polypropylene that does not satisfy at least one of the above requirements (P1) to (P3) and has at least one functional group, and may be a homopolymer or a copolymer. The functional group of polypropylene (B) may be at least one selected from the group consisting of, for example, a carboxyl group, a hydroxyl group, a carbonyl group, a polymerizable unsaturated hydrocarbon group, an isocyanate group, an epoxy group, a silanol group, a hydrazide group, a carbodiimide group, an oxazoline group, an acetoacetyl group, an aziridine group, an ester group, an active ester group, a carbonate group, an azide group, a linear or cyclic heteroatom-containing hydrocarbon group, an amino group, a sulfhydryl group, a metal chelate group, and a halogen-containing group, and among these, silane-modified polypropylene is preferred from the viewpoint of forming a crosslinked structure.

[0048] When polypropylene (A) and (B) are used in combination in a microporous membrane, the content of polypropylene (B) in the microporous membrane is preferably 30% by mass or less, more preferably 4 to 25% by mass, and even more preferably 5 to 20% by mass, from the viewpoint of balancing strength and crosslinkability.

[0049] [Crosslinking reaction] The crosslinked structure of the microporous membrane contributes to both the shutdown function and high-temperature film rupture resistance when used as a separator, as well as the safety of energy storage devices, and is preferably formed in the amorphous portion of the polyolefin. The crosslinked structure can be formed, for example, by a reaction via covalent bonds, hydrogen bonds, or coordination bonds. Among these, reactions via covalent bonds are as follows: (I) to (IV): (I) Condensation reaction of multiple identical functional groups (II) Reactions between multiple heterogeneous functional groups (III) Chain condensation reaction between functional groups and electrolyte (IV) Chain condensation reaction between functional groups and additives Preferably, it is at least one selected from the group consisting of the following: Furthermore, the reaction via coordinate bonds is the following reaction (V): (V) Reactions in which multiple identical functional groups crosslink via coordination bonds with eluted metal ions. It is preferable that this be the case.

[0050] Reaction (I) Let A be the first functional group of the microporous membrane. The schematic scheme and specific example of reaction (I) are shown below. [ka] {In the formula, R is an alkyl group or heteroalkyl group having 1 to 20 carbon atoms, which may have substituents.}

[0051] When functional group A for reaction (I) is a silanol group, the polyolefin contained in the microporous membrane is preferably silane graft modified. The silane graft modified polyolefin has a structure in which the main chain is a polyolefin and the main chain has an alkoxysilyl as a graft. Examples of alkoxides substituted for the alkoxysilyl include methoxide, ethoxide, and butoxide. For example, in the above formula, R can be methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, and the like. The main chain and the graft are connected by a covalent bond, and examples of structures include alkyl, ether, glycol, or ester. Considering the manufacturing process of the microporous membrane according to this embodiment, the silane graft modified polyolefin preferably has a silicon-to-carbon ratio (Si / C) of 0.2 to 1.8%, and more preferably 0.5 to 1.7%, before the crosslinking process.

[0052] Reaction (II) Let A be the first functional group and B be the second functional group of the microporous membrane. A schematic scheme and specific example of reaction (II) are shown below. [ka] [ka] [ka] [ka]

[0053] Reactions (I) and (II) can be catalyzed and, for example, catalytically accelerated by chemicals inside an energy storage device in which a microporous membrane is incorporated as a separator. These chemicals may be, for example, electrolytes, electrolyte solutions, electrode active materials, additives, or their decomposition products contained in the energy storage device.

[0054] Reaction (III) The schematic scheme and specific example of reaction (III) are shown below, with A as the first functional group of the microporous membrane and Sol as the electrolyte. [ka] [ka] [ka] [ka]

[0055] Reaction (IV) Let A be the first functional group of the microporous membrane, B be the second functional group which can be incorporated as desired, and Add be the additive. The schematic scheme of reaction (IV) is shown below. [ka]

[0056] Reaction (IV) is preferably a nucleophilic substitution reaction, a nucleophilic addition reaction, or a ring-opening reaction between compound Rx, which constitutes the microporous membrane, and compound Ry, which constitutes the additive (Add), from the viewpoint of forming a covalent bond represented by the dotted line in the scheme above. Compound Rx may be a polyolefin contained in the microporous membrane, such as polyethylene or polypropylene, and preferably the polyolefin is modified by a functional group x, for example, at least one selected from the group consisting of -OH, -NH2, -NH-, -COOH, and -SH.

[0057] Since multiple compounds Rx are crosslinked via compound Ry as an additive, it is preferable that compound Ry has two or more linking reaction units y1. The multiple linking reaction units y1 can be any structure or group, substituted or unsubstituted, heteroatoms or inorganic substances, and may be identical or different from each other, as long as they can undergo nucleophilic substitution, nucleophilic addition, or ring-opening reactions with the functional group x of compound Rx. Furthermore, when compound Ry has a chain structure, each of the multiple linking reaction units y1 can independently be a terminal group, incorporated into the main chain, or a side chain or pendant.

[0058] If reaction (IV) is a nucleophilic substitution reaction, then, as an example, the functional group x of compound Rx will be considered a nucleophilic group and the coupling reaction unit y1 of compound Ry will be considered a leaving group for the explanation below. However, in this embodiment, both the functional group x and the coupling reaction unit y1 can become leaving groups depending on their nucleophilicity.

[0059] From the viewpoint of nucleophilic reagents, the functional group x of compound Rx is preferably an oxygen-based nucleophile, a nitrogen-based nucleophile, or a sulfur-based nucleophile. Examples of oxygen-based nucleophiles include hydroxyl groups, alkoxy groups, ether groups, and carboxyl groups, with -OH and -COOH being particularly preferred. Examples of nitrogen-based nucleophiles include ammonium groups, primary amino groups, and secondary amino groups, with -NH2 and -NH- being particularly preferred. Examples of sulfur-based nucleophiles include -SH and thioether groups, with -SH being particularly preferred.

[0060] If reaction (IV) is a nucleophilic substitution reaction, from the viewpoint of leaving groups, the linking reaction unit y1 of compound Ry can be an alkylsulfonyl group such as CH3SO2-, CH3CH2SO2-; an arylsulfonyl group (-ArSO2-); a haloalkylsulfonyl group such as CF3SO2-, CCl3SO2-; or CH3SO3 - -, CH3CH2SO3 - -Alkyl sulfonate groups such as; aryl sulfonate groups (ArSO3 - -);CF3SO3 - -, CCl3SO3 - Haloalkylsulfonate groups such as - and heterocyclic groups are preferred, and these can be used individually or in combination. Examples of heteroatoms included in the heterocycle include nitrogen, oxygen, and sulfur atoms, and among these, nitrogen atoms are preferred from the viewpoint of leaving group properties. Examples of leaving groups containing a nitrogen atom in the heterocycle are shown in the following formulas (y1-1) to (y1-6): [ka] {In the formula, X is a hydrogen atom or a monovalent substituent.} [ka] {In the formula, X is a hydrogen atom or a monovalent substituent.} [ka] {In the formula, X is a hydrogen atom or a monovalent substituent.} [ka] {In the formula, X is a hydrogen atom or a monovalent substituent.} [ka] {In the formula, X is a hydrogen atom or a monovalent substituent.} [ka] {In the formula, X is a hydrogen atom or a monovalent substituent.} A monovalent group represented by is preferred.

[0061] In formulas (y1-1) to (y1-6), X is a hydrogen atom or a monovalent substituent. Examples of monovalent substituents include alkyl groups, haloalkyl groups, alkoxyl groups, and halogen atoms.

[0062] If reaction (IV) is a nucleophilic substitution reaction and compound Ry has a chain-like structure, compound Ry, in addition to the linking reaction unit y1, is used as a chain-like unit y2, as shown in the following formulas (y2-1) to (y2-6): [ka] {In the formula, m is an integer between 0 and 20, and n is an integer between 1 and 20.} [ka] {In the formula, n is an integer between 1 and 20.} [ka] {In the formula, n is an integer between 1 and 20.} [ka] {In the formula, n is an integer between 1 and 20.} [ka] {In the formula, X is an alkylene group or arylene group having 1 to 20 carbon atoms, and n is an integer from 1 to 20.} [ka] {In the formula, X is an alkylene group or arylene group having 1 to 20 carbon atoms, and n is an integer from 1 to 20.} It is preferable that the compound Ry has at least one selected from the group consisting of divalent groups represented by . Furthermore, if compound Ry contains multiple chain units y2, they may be identical or different from each other, and their sequence may be block or random.

[0063] In formula (y2-1), m is an integer from 0 to 20, preferably from 1 to 18 from the viewpoint of the crosslinking network. In formulas (y2-1) to (y2-6), n is an integer from 1 to 20, preferably from 2 to 19 or 3 to 16 from the viewpoint of the crosslinking network. In formulas (y2-5) to (y2-6), X is an alkylene group or arylene group having 1 to 20 carbon atoms, preferably a methylene group, ethylene group, n-propylene group, n-butylene group, n-hexylene group, n-heptylene group, n-octylene group, n-dodecylene group, o-phenylene group, m-phenylene group, or p-phenylene group from the viewpoint of the stability of the chain structure.

[0064] For the case where reaction (IV) is a nucleophilic substitution reaction, preferred combinations of the functional group x of compound Rx and the linking reaction unit y1 and chain unit y2 of compound Ry are shown in Tables 2 to 4 below.

[0065] [Table 2]

[0066] [Table 3]

[0067] [Table 4]

[0068] As a specific example of a nucleophilic substitution reaction, the functional group x of the polyolefin is -NH2, the coupling reaction unit y1 of the additive (compound Ry) is a skeleton derived from succinimide, and the chain unit y2 is -(O-C2H5) nThe reaction scheme for the case where - is shown below. [ka]

[0069] As a second specific example of a nucleophilic substitution reaction, the reaction scheme for a polyolefin whose functional group x is -SH and -NH2, whose additive (compound Ry) has a nitrogen-containing cyclic skeleton as its linking reaction unit y1 and a chain unit y2 as o-phenylene is shown below. [ka]

[0070] If reaction (IV) is a nucleophilic addition reaction, the functional group x of compound Rx and the coupling reaction unit y1 of compound Ry can undergo an addition reaction. In a nucleophilic addition reaction, the functional group x of compound Rx is preferably an oxygen-based nucleophile, a nitrogen-based nucleophile, or a sulfur-based nucleophile. Examples of oxygen-based nucleophiles include hydroxyl groups, alkoxy groups, ether groups, and carboxyl groups, with -OH and -COOH being preferred. Examples of nitrogen-based nucleophiles include ammonium groups, primary amino groups, and secondary amino groups, with -NH2 and -NH- being preferred. Examples of sulfur-based nucleophiles include -SH and thioether groups, with -SH being preferred.

[0071] In nucleophilic addition reactions, the coupling reaction unit y1 of compound Ry is defined by the following formulas (Ay1-1) to (Ay1-6) from the viewpoint of addition reactivity or the availability of starting materials: [ka] [ka] [ka] [ka] {In the formula, R is a hydrogen atom or a monovalent organic group.} [ka] [ka] Preferably, it is at least one selected from the group consisting of groups represented by .

[0072] In formula (Ay1-4), R is a hydrogen atom or a monovalent organic group, preferably a hydrogen atom and C 1~20 The group is an alkyl group, an alicyclic group, or an aromatic group, more preferably a hydrogen atom, a methyl group, an ethyl group, a cyclohexyl group, or a phenyl group.

[0073] For the case where reaction (IV) is a nucleophilic addition reaction, preferred combinations of the functional group x of compound Rx and the coupling reaction unit y1 of compound Ry are shown in Tables 5 and 6 below.

[0074] [Table 5]

[0075] [Table 6]

[0076] As a specific example of a nucleophilic addition reaction, the reaction scheme when the functional group x of the microporous membrane is -OH and the coupling reaction unit y1 of the additive (compound Ry) is -NCO is shown below. [ka]

[0077] If reaction (IV) is a ring-opening reaction, the functional group x of compound Rx and the linking reaction unit y1 of compound Ry can undergo a ring-opening reaction, and from the viewpoint of the availability of raw materials, it is preferable that the cyclic structure on the linking reaction unit y1 side opens. From a similar viewpoint, it is more preferable that the linking reaction unit y1 is an epoxy group, it is even more preferable that compound Ry has at least two epoxy groups, and even more preferably that it is a diepoxy compound.

[0078] If reaction (IV) is a ring-opening reaction, the functional group x of compound Rx is preferably at least one selected from the group consisting of -OH, -NH2, -NH-, -COOH and -SH, and / or the coupling reaction unit y1 of compound Ry is of the following formula (ROy1-1): [ka] {In the formula, each of the multiple X's is independently either a hydrogen atom or a monovalent substituent.} Preferably, there are at least two groups represented by formula (ROy1-1). In formula (ROy1-1), each of the X's is independently a hydrogen atom or a monovalent substituent, preferably a hydrogen atom, C 1~20 The functional group is an alkyl group, an alicyclic group, or an aromatic group, and more preferably a hydrogen atom, a methyl group, an ethyl group, a cyclohexyl group, or a phenyl group. For the epoxy ring-opening reaction, preferred combinations of the functional group x of compound Rx and the coupling reaction unit y1 of compound Ry are shown in Table 7 below.

[0079] [Table 7]

[0080] Reaction (V) The first functional group of the microporous membrane is A, and the metal ion is M. n+ A schematic scheme of reaction (V) and an example of functional group A are shown below. [ka]

[0081] In the above scheme, metal ion M n+ is preferably one eluted from the electricity storage device (hereinafter also referred to as eluted metal ion), and examples thereof include Zn 2+ , Mn 2+ , Co 3+ , Ni 2+ and Li + , and may be at least one selected from the group consisting of these. The coordination bond when the functional group A is -COO - is exemplified below. [Chemical Formula]

[0082] A specific scheme of reaction (V) when the functional group A is -COOH and the eluted metal ion is Zn 2+ is shown below. [Chemical Formula]

[0083] In the above scheme, hydrofluoric acid (HF) can be derived from, for example, any of the electrolyte, electrolytic solution, electrode active material, additive, or decomposition products or water-absorbed products thereof contained in the electricity storage device, depending on the charge-discharge cycles of the electricity storage device.

[0084] (Other Contained Components) If desired, the microporous membrane may contain, in addition to polyolefin, known additives such as dehydration condensation catalysts, metal soaps such as calcium stearate or zinc stearate, ultraviolet absorbers, light stabilizers, antistatic agents, anti-fogging agents, and color pigments.

[0085] [Properties of Microporous Membrane] The following properties of the microporous membrane are described for the case where the microporous membrane for electricity storage devices is a flat membrane, but when the microporous membrane for electricity storage devices is in the form of a laminated membrane, the properties can be measured after removing layers other than the microporous membrane from the laminated membrane.

[0086] The porosity of the microporous membrane is preferably 20% or more, more preferably 30% or more, and even more preferably 39% or more or 42% or more. When the porosity of the microporous membrane is 20% or more, it tends to improve the ability to follow the rapid movement of lithium ions when used as a separator in a lithium-ion energy storage device. On the other hand, the porosity of the microporous membrane is preferably 90% or less, more preferably 80% or less, and even more preferably 50% or less. When the porosity of the microporous membrane is 90% or less, the membrane strength tends to improve and self-discharge tends to be further suppressed.

[0087] The air permeability resistance of the microporous membrane is preferably 1 second or more, more preferably 50 seconds or more, even more preferably 100 seconds or more, and even more preferably 150 seconds or more or 200 seconds or more per 100 ml of membrane volume. When the air permeability resistance of the microporous membrane is 1 second or more, the balance between film thickness, porosity, and average pore size tends to improve. Furthermore, the air permeability resistance of the microporous membrane is preferably 450 seconds or less, and more preferably 420 seconds or less. When the air permeability resistance of the microporous membrane is 450 seconds or less, the ion permeability tends to improve.

[0088] The tensile strength of the microporous membrane is, in relation to the orientation ratio MD / TD of requirement (D) described above, preferably 900 to 3000 kg / cm² for MD. 2 More preferably 1000-2500 kg / cm² 2 More preferably 1210-2270 kg / cm² 2 The load is preferably 100-1500 kg / cm² in the TD direction (perpendicular to the MD direction, in the film width direction). 2 More preferably 129-1310 kg / cm² 2 That is the case.

[0089] The thickness of the microporous membrane is preferably 1.0 μm or more, more preferably 2.0 μm or more, and even more preferably 3.0 μm or more, 4.0 μm or more, or 5.5 μm or more. A thickness of 1.0 μm or more tends to improve the film strength. Alternatively, the thickness of the microporous membrane is preferably 500 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less, 22 μm or less, or 19 μm or less. A thickness of 500 μm or less tends to improve ion permeability. When the microporous membrane is used as a separator for lithium-ion secondary batteries, the thickness of the microporous membrane is preferably 1.0 to 25 μm, more preferably 3.0 to 22 μm, and even more preferably 13 to 18 μm.

[0090] The puncture strength of the microporous membrane is preferably 200 to 500 gf, more preferably 218 to 481 gf or 227 to 450 gf, from the viewpoint of balancing film rupture resistance and device safety.

[0091] [Method for manufacturing microporous membranes] The method for manufacturing a microporous membrane is as follows: Process for forming polyolefin resin compositions; and Pore ​​opening process for polyolefin resin compositions; Heat treatment process for open oxides; This may include... The case of a microporous membrane (flat membrane) will be explained below, but this is not intended to exclude other forms.

[0092] Polyolefin resin compositions can be manufactured using polyolefin resin and other materials by a melt-kneading method in a single-screw or twin-screw extruder.

[0093] The materials mixed in the mixing process can be determined according to the subsequent porosity-opening process, since the porosity-opening process can be carried out by known dry and / or wet methods.

[0094] Dry methods include methods that involve stretching and extracting an unstretched sheet containing incompatible particles such as inorganic particles and polyolefins to separate the interface between dissimilar materials and form pores, as well as lamellar pore opening methods and β-crystal pore opening methods.

[0095] The lamellar porosity opening method is a method for obtaining an unstretched sheet having a crystalline lamellar structure by controlling the melt crystallization conditions during sheet formation by melt extrusion of resin, and then forming pores by stretching the obtained unstretched sheet to crack the lamellar interface. In the lamellar porosity opening method, for example, the circular die extrusion method can be used. In the circular die extrusion method, for example, a highly crystalline MD-oriented raw material can be obtained by blowing up a molten kneaded polypropylene resin composition mainly to MD from an annular die.

[0096] The β-crystal pore opening method is a method in which an undrawn sheet having a relatively low crystal density β-crystal is produced during the melt extrusion of polypropylene (PP), and the produced undrawn sheet is drawn to induce a crystal transition to a relatively high crystal density α-crystal, thereby forming pores due to the difference in crystal density between the two. As a β-crystal nucleating agent, for example, 1:2,6-naphthalenedicarboxylic acid dicyclohexylamide can be used, and preferably, a β-crystal nucleating agent and an antioxidant are used in combination. In the second and fourth embodiments, the β-crystal pore opening method is preferred because β-crystal activated PP can be used.

[0097] As a wet method, one can use a kneader to knead polyolefin with other resins as desired and a plasticizer or inorganic material to form a sheet, stretch it as needed, and then extract the pore-forming material from the sheet. Another method can be used to dissolve the polyolefin resin composition and then immerse it in a poor solvent for the polyolefin to solidify the polyolefin while simultaneously removing the solvent.

[0098] The plasticizer is not particularly limited, and examples thereof include organic compounds capable of forming a uniform solution with a polyolefin at a temperature not higher than the boiling point. More specific examples include decalin, xylene, dioctyl phthalate, dibutyl phthalate, stearyl alcohol, oleyl alcohol, decyl alcohol, nonyl alcohol, diphenyl ether, n-decane, n-dodecane, paraffin oil and the like. Among these, paraffin oil and dioctyl phthalate are preferred. The plasticizer may be used alone or in combination of two or more kinds.

[0099] Regardless of whether a dry method or a wet method is used, from the viewpoint of maintaining the crosslinkability of the microporous membrane until it is housed in an electricity storage device, the method for producing a microporous membrane preferably does not include a step of bringing the latent crosslinkable polyolefin into contact with a crosslinking agent, other reactive compounds, functional groups of other compounds, a crosslinking acceleration catalyst and the like. In addition, as long as the crosslinkability of the microporous membrane is maintained, the polyolefin resin composition may contain, as additives, for example, a fluorine-based flow modifier, waxes, crystal nucleating materials, antioxidants, metal soaps such as aliphatic carboxylic acid metal salts, ultraviolet absorbers, light stabilizers, antistatic agents, antifogging agents, color pigments and the like.

[0100] The heat treatment step for the pore-opened product can be performed for the purpose of heat setting after the stretching step or after pore formation, in order to suppress shrinkage of the microporous membrane. Examples of the heat treatment include a stretching operation performed at a predetermined temperature atmosphere and a predetermined stretch ratio for the purpose of adjusting physical properties, and / or a relaxation operation performed at a predetermined temperature atmosphere and a predetermined relaxation ratio for the purpose of reducing stretching stress. The relaxation operation may be performed after the stretching operation. These heat treatments can be performed using a tenter or a roll stretching machine.

[0101] [Electricity Storage Device] Microporous membranes according to the first, second, third, and fourth embodiments can be used in energy storage devices. Generally, an energy storage device comprises an outer casing, a positive electrode, a negative electrode, a separator placed between the positive and negative electrodes, and an electrolyte. When the microporous membranes according to these embodiments are housed in the device casing, the functional group-modified polyolefin or functional group-graft copolymerized polyolefin formed during the manufacturing process of the microporous membrane reacts with chemical substances contained in the electrolyte or additives to form a crosslinked structure, and the resulting energy storage device has a crosslinked structure. From the viewpoint of maintaining the crosslinkability of the microporous membrane until it is housed in the energy storage device and then improving the safety of the energy storage device, it is preferable to place the microporous membrane as a separator between the positive and negative electrodes. When the microporous membrane is housed in the energy storage device as a separator, a crosslinked structure is formed, so it is possible to improve the safety of the energy storage device by undergoing a crosslinking reaction after device manufacturing while being compatible with the conventional energy storage device manufacturing process.

[0102] Examples of energy storage devices include lithium batteries, lithium secondary batteries, lithium-ion secondary batteries, sodium secondary batteries, sodium-ion secondary batteries, magnesium secondary batteries, magnesium-ion secondary batteries, calcium secondary batteries, calcium-ion secondary batteries, aluminum secondary batteries, aluminum-ion secondary batteries, nickel-metal hydride batteries, nickel-cadmium batteries, electric double-layer capacitors, lithium-ion capacitors, redox flow batteries, lithium-sulfur batteries, lithium-air batteries, and zinc-air batteries. Among these, from the viewpoint of practicality, lithium batteries, lithium secondary batteries, lithium-ion secondary batteries, nickel-metal hydride batteries, or lithium-ion capacitors are preferred, and lithium batteries or lithium-ion secondary batteries are more preferred.

[0103] [Lithium-ion rechargeable battery] A lithium-ion secondary battery is a rechargeable battery that uses a lithium transition metal oxide such as lithium cobalt oxide or lithium cobalt composite oxide as the positive electrode, a carbon material such as graphite or graphite as the negative electrode, and an organic solvent containing a lithium salt such as LiPF6 as the electrolyte. During charging and discharging of a lithium-ion secondary battery, ionized lithium moves back and forth between the electrodes. Furthermore, because it is necessary for the ionized lithium to move between the electrodes at a relatively high speed while suppressing contact between the electrodes, a separator is placed between the electrodes. [Examples]

[0104] The present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to the following examples unless it exceeds the gist of the invention. The raw materials used and the methods for evaluating the various properties of the microporous membrane are as follows.

[0105] [Measuring Melt Flow Rate (MFR)] The melt flow rate (MFR) is expressed as the value measured for polypropylene resin at 230°C and 2.16 kg in accordance with JIS K 7210 (unit: g / 10 min).

[0106] [GPC (Gel Permission Chromatography) Measurement] Using the Agilent PL-GPC220, standard polystyrene was measured under the following conditions to create a calibration curve. Similarly, chromatographic measurements were taken of each of the polymers listed below under the same conditions, and based on the calibration curve, the weight-average molecular weight Mw of each polymer was calculated by dividing it by the number-average molecular weight Mn using the method described below. Column: TSKgel GMHHR-H(20) HT (7.8mm I.D. × 30 cm) 2 tubes Mobile phase: 1,2,4-trichlorobenzene Detector: RI Column temperature: 160℃ Sample concentration: 1 mg / ml Calibration curve: Polystyrene

[0107] [Measurement of wide-angle X-ray scattering] A Rigaku Ultima-IV detector was used for the measurements. Cu-Kα radiation was incident on the separator sample, and the diffracted light was detected by a D / tex Uitra detector. The measurement conditions were a distance of 285 mm between the sample and the detector, an excitation voltage of 40 kV, and a current of 40 mA. A focusing optical system was employed, with slit conditions of DS = 1 / 2°, SS = open, and a vertical slit of 10 mm. The MD / TD orientation ratio was calculated by dividing the measured MD orientation ratio by the TD orientation ratio.

[0108] [Thickness (μm)] The thickness of the porous film was measured at room temperature (23±2°C) using a Mitutoyo IDC112 digital indicator.

[0109] [Porosity (%)] A 5cm x 5cm square sample was cut from the porous film, and the porosity was calculated from the volume and mass of the sample using the following formula. Porosity (%) = (volume (cm³) 3 )- Mass (g) / Density of resin composition (g / cm³) 3 )) / Volume (cm³ 3 ) × 100

[0110] [Air permeability resistance (sec / 100ml)] The air permeability resistance of the microporous membrane was measured using a Gurley type air permeability meter compliant with JIS P-8117.

[0111] [Piercing strength] A needle with a hemispherical tip with a radius of 0.5 mm was prepared, and a microporous membrane was sandwiched between two plates with an opening of 11 mm in diameter (dia.), and the needle, microporous membrane, and plates were set up. Using an IMADA Corporation "MX2-50N" puncture test was performed under the conditions of a needle tip radius of curvature of 0.5 mm, an opening diameter of 11 mm for the microporous membrane holding plate, and a puncture speed of 25 mm / min, bringing the needle and microporous membrane into contact and measuring the maximum puncture load (i.e., puncture strength (gf)).

[0112] [Measurement of storage modulus, loss modulus, and transition temperature] The dynamic viscoelasticity of the separator was measured using a dynamic viscoelasticity measuring device, and the storage modulus (E'), loss modulus (E''), and transition temperature between the rubbery flat region and the crystalline melting flow region were calculated. The storage modulus change ratio (R E’X ) is given by the following formula (I), mixed storage modulus ratio (R E’mix ) is calculated according to the following formula (II), and the loss modulus ratio (R E’’X ) is calculated according to the following formula (III), and the mixed loss modulus ratio (R E’’mix The following formulas (IV) were used to calculate the values. The measurement conditions were as follows (i) to (iv). (i) Dynamic viscoelasticity measurement under the following conditions: • Atmosphere: Nitrogen • Measuring instrument used: RSA-G2 (manufactured by TA Instruments) • Sample film thickness: 5 μm to 50 μm (Measurements are performed on a single sample regardless of its film thickness) • Measurement temperature range: -50 to 300°C • Heating rate: 10℃ / min ·Measurement frequency: 1Hz • Deformation mode: Sinusoidal tension mode (linear tension) Initial value of static tensile load: 0.5N • Initial gap distance (at 25°C): 25mm • Auto strain adjustment: Enabled (Range: Amplitude value 0.05~25%, sinusoidal load 0.02~5N) It was done there. (ii) Static tensile load refers to the midpoint between the maximum and minimum stresses in each periodic motion, and sinusoidal load refers to the vibrational stress centered on the static tensile load. (iii) The sinusoidal tensile mode refers to measuring vibration stress while performing periodic motion with a fixed amplitude of 0.2%. In this process, the gap distance and static tensile load were varied so that the difference between the static tensile load and the sinusoidal load was within 20%. When the sinusoidal load fell below 0.02N, the amplitude was amplified so that the sinusoidal load remained within 5N and the increase in amplitude was within 25% before measuring the vibration stress. (iv) Relationship between the obtained sinusoidal load and amplitude value, and the following equation: σ * =σ0·Exp[i(ωt+δ)], ε * =ε0·Exp(iωt), σ * =E * ·ε * E * =E'+iE'' {where, σ * : Vibration stress, ε * : strain, i: imaginary unit, ω: angular frequency, t: time, δ: phase difference between vibrational stress and strain, E * :complex modulus of elasticity, E':storage modulus of elasticity, E'':loss modulus of elasticity Vibration stress: sinusoidal load / initial cross-sectional area Static tensile load: The load at the point of minimum vibration stress in each period (the point of minimum gap distance in each period). Sinusoidal load: The difference between the measured vibration stress and the static tensile load. The storage modulus and loss modulus were calculated from this data. E' Z and E' Z0 and E'' Z and E'' Z0 E' and E'0, and E'' and E''0, are the average values ​​of each storage modulus or loss modulus in the dynamic viscoelasticity measurement data between 160°C and 300°C. R E’X =E' Z / E' Z0 (I) Comparison before and after input into the cell R E’mix =E' / E'0(II) Comparison of presence or absence of amorphous cross-linking structure R E’’X =E'' Z / E'' Z0 (III) Comparison before and after input into the cell R E’’mix =E'' / E''0(IV) Comparison of presence or absence of amorphous cross-linking structure

[0113] Figure 3 shows an example of a graph illustrating the relationship between temperature and storage modulus. As shown in Figure 3, the storage modulus of a reference film (a separator for energy storage devices without an amorphous crosslinking structure) and a crosslinked film are compared within a temperature range of -50°C to 310°C, and the transition temperature between the rubbery flat region and the crystalline melting flow region can be confirmed in Figure 3. The transition temperature is defined as the temperature at the intersection of a straight line extending from the high-temperature baseline to the low-temperature side and a tangent line drawn at the inflection point of the curve representing the crystalline melting change. Figure 4 shows an example of a graph illustrating the relationship between temperature and loss modulus. Figure 4 compares the loss modulus of a reference film (a separator for energy storage devices that does not contain silane-grafted modified polyolefins) and a crosslinked film within a temperature range of -50°C to 310°C, and shows the transition temperature determined by the same method as in Figure 3. In this technical field, the storage modulus and loss modulus are given by the following formula: tanδ = E'' / E' {In the formula, tanδ represents the loss tangent, E' represents the storage modulus, and E'' represents the loss modulus.} It is compatible according to the following. Note that the mixed storage modulus ratio (R E’mix ) or mixed loss modulus ratio (R E’’mix In the measurement of ), a silane-unmodified polyolefin-based microporous membrane with a gelation degree of approximately 0% was used as a separator for energy storage devices that does not have an amorphous crosslinking structure. 0、 For E'' and E''0, if no fracture (abrupt decrease in elastic modulus) of the sample was observed between 160°C and 300°C, the values ​​were calculated from the average value between 160°C and 300°C. If fracture was observed in the sample between 160°C and 300°C, the values ​​were calculated from the average value from 160°C to the temperature of the fracture point. In this specification, a separator for energy storage devices that does not have an amorphous crosslinking structure may be a separator manufactured by mixing any one type selected from the group consisting of polyethylene:X (viscosity average molecular weight 100,000 to 400,000), ultra-high molecular weight PE:Y (viscosity average molecular weight 400,000 to 800,000), and ultra-high molecular weight PE:Z (viscosity average molecular weight 800,000 to 9,000,000), or two or three types selected from the group consisting of X, Y, and Z, in any proportion. Furthermore, polyolefins composed solely of a hydrocarbon backbone, such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polypropylene (PP), and olefin-based thermoplastic elastomers, may be added to the mixed composition. More specifically, a separator for energy storage devices that does not have an amorphous crosslinking structure may mean a polyolefin-based microporous membrane in which the rate of change in solid content before and after heating at 160°C in a decalin solution (hereinafter referred to as "degree of gelation") is 10% or less. Furthermore, when measuring the degree of gelation, the solid content refers only to the resin and does not include other materials such as inorganic substances. On the other hand, the degree of gelation of polyolefin-based microporous membranes having amorphous crosslinking structures such as silane crosslinking structures is preferably 30% or more, more preferably 70% or more.

[0114] [Tensile test] The tensile strengths in the MD and TD directions were measured using an Instron Model 4201 according to the ASTM-882 procedure and determined as the fracture strength.

[0115] [Fuse / Meltdown (F / MD) Characteristics] a. Fabrication of the positive electrode A slurry was prepared by dispersing 92.2% by mass of lithium cobalt composite oxide (LiCoO2) as the positive electrode active material, 2.3% by mass each of flake graphite and acetylene black as conductive materials, and 3.2% by mass of polyvinylidene fluoride (PVDF) as a binder in N-methylpyrrolidone (NMP). This slurry was applied to one side of a 20 μm thick aluminum foil, which would serve as the positive electrode current collector, using a die coater. After drying at 130°C for 3 minutes, it was compressed and molded using a roll press. At this time, the amount of active material applied to the positive electrode was 250 g / m². 2The bulk density of the active material is 3.00 g / cm³. 3 I adjusted it so that it would work.

[0116] b. Fabrication of the negative electrode A slurry was prepared by dispersing 96.9% by mass of artificial graphite as the negative electrode active material and 1.4% by mass of ammonium salt of carboxymethylcellulose and 1.7% by mass of styrene-butadiene copolymer latex as binders in purified water. This slurry was applied to one side of a 12 μm thick copper foil, which would serve as the negative electrode current collector, using a die coater. After drying at 120°C for 3 minutes, it was compressed and molded using a roll press. At this time, the amount of active material applied to the negative electrode was 106 g / m². 2 The bulk density of the active material is 1.35 g / cm³. 3 I adjusted it so that it would work.

[0117] c. Preparation of non-aqueous electrolyte A mixed solvent of ethylene carbonate and ethyl methyl carbonate in a 1:2 volume ratio was prepared by dissolving LiPF6 as a solute to a concentration of 1.0 mol / L. A positive electrode, separator, and negative electrode were cut out in a 200 mm diameter circular shape from aluminum foil, with a resistance measuring wire attached to the back with conductive silver paste. These were then overlapped, and the resulting laminate was coated with the electrolyte solution containing the electrolyte, which was then spread throughout. The laminate was placed in the center between circular aluminum heaters with a diameter of 600 mm, and the aluminum heaters were pressurized to 0.5 MPa from above and below using hydraulic jacks to complete the preparation for measurement. The resistance (Ω) between the electrodes was measured while heating the laminate with the aluminum heaters at a heating rate of 2 °C / min. The temperature at which the resistance between the electrodes increased along with the fuse of the separator and first exceeded 1000 Ω was defined as the fuse temperature (shutdown temperature). Further heating was continued, and the temperature at which the resistance dropped below 1000 Ω was defined as the meltdown temperature (rupture temperature).

[0118] [Example 1] <Method for producing silane-grafted polyolefins> The raw material polyolefin used for silane graft-modified polyolefins may have a viscosity-average molecular weight (Mv) of 100,000 or more and 1,000,000 or less, a weight-average molecular weight (Mw) of 30,000 or more and 920,000 or less, and a number-average molecular weight of 10,000 or more and 150,000 or less, and may be a propylene or butene copolymer α-olefin. While melt-kneading the raw material polyolefin in an extruder, an organic peroxide (di-t-butyl peroxide) is added to generate radicals in the α-olefin polymer chain. Then, a trimethoxyalkoxide-substituted vinylsilane is injected, and an addition reaction introduces alkoxysilyl groups into the α-olefin polymer, forming a silane graft structure. At the same time, an appropriate amount of antioxidant (pentaerythritol tetrakis[3-(3,5-di-tetra-butyl-4-hydroxyphenyl)propionate]) is added to adjust the radical concentration in the system and suppress the chain reaction (gelation) within the α-olefin. The obtained silane-grafted polyolefin molten resin is cooled in water, processed into pellets, and then heated and dried at 80°C for two days to remove moisture or unreacted trimethoxyalkoxide-substituted vinylsilane. The residual concentration of unreacted trimethoxyalkoxide-substituted vinylsilane in the pellets is approximately 1000-1500 ppm. The silane-grafted polyolefin obtained by the above manufacturing method will be referred to as "silane-modified polypropylene" in the following examples and Table 1.

[0119] <Fabrication of microporous membranes (monolayer)> High molecular weight polypropylene resin (PP, MFR=0.25) and the above-mentioned silane-modified polypropylene were dry-blended in a mass ratio of PP:silane-modified polypropylene = 95:5 (mass%), then melted in a 2.5-inch extruder and supplied to an annular die using a gear pump. The die temperature was set to 230°C, and the molten polymer was cooled by blown air before being wound onto a roll. The extruded precursor (raw film) had a thickness of 15 μm, and the raw film was then annealed at 130°C for 15 minutes. The annealed film was then cold-stretched to 21% at room temperature, then hot-stretched to 158% at 123°C, and relaxed to 128% at 126°C to form micropores and obtain a microporous film. After the above stretching and porosization, the physical properties of the microporous film were measured. The results are shown in Table 8.

[0120] [Examples 2-6, 8-10, Comparative Examples 1, 2, 4] A microporous membrane was obtained using the same method as in Example 1, except that the raw materials were changed as shown in Table 8, and the obtained microporous membrane was evaluated.

[0121] [Example 7] Polypropylene with an MFR of 2.4 was mixed with 0.2% by mass of 1:2,6-naphthalenedicarboxylic acid dicyclohexylamide as a β-nucleating agent and 0.1% by mass of an antioxidant. The mixture was fed into a coaxial twin-screw extruder and melt-kneaded at a set temperature of 270°C. The resulting strand was cooled and solidified in a water bath, cut with a pelletizer, and pellets were produced. The obtained β-crystalline activated polypropylene pellets and the silane-modified polypropylene were dry-blended in a mass ratio of β-crystalline activated polypropylene:silane-modified polypropylene = 95:5 (mass%), then melted in a 2.5-inch extruder and supplied to an annular die using a gear pump. The die temperature was set to 230°C, and the molten polymer was cooled by blown air before being wound onto a roll. The extruded precursor (raw film) had a thickness of 15 μm, and the raw film was then annealed at 130°C for 15 minutes. The annealed film was then cold-stretched to 21% at room temperature, then hot-stretched to 158% at 123°C, and relaxed to 128% at 126°C to form micropores and obtain a microporous film. After the above stretching and porosization, the physical properties of the microporous film were measured. The results are shown in Table 8.

[0122] [Comparative Example 3] A microporous membrane was obtained according to the same method as in Example 7, except that the raw materials were changed as shown in Table 8, and the obtained microporous membrane was evaluated.

[0123] [Table 8]

Claims

1. A microporous membrane for an energy storage device comprising polypropylene, wherein the microporous membrane for an energy storage device comprises a β-nucleating agent and has an amorphous crosslinking structure in which the amorphous portion of the polypropylene is selectively crosslinked.

2. The microporous membrane for an energy storage device according to claim 1, wherein the β-nucleating agent is 1:2,6-naphthalenedicarboxylic acid dicyclohexylamide.

3. The microporous membrane for the energy storage device is given by the following formula (II): 10 E’mix H' / H' 0 (10) {In the formula, E' is the storage modulus measured at 160°C to 300°C when the microporous film for the energy storage device has the amorphous crosslinking structure, and E' 0 This is the storage modulus measured at 160°C to 300°C for a microporous film for energy storage devices that does not have an amorphous crosslinking structure, and is E' or E'. 0 The measurement conditions for the storage modulus are defined by the following configurations (i) to (iv). (i) Dynamic viscoelasticity measurement under the following conditions: • Atmosphere: Nitrogen • Measurement device used: RSA-G2 (manufactured by TA Instruments) • Sample film thickness: 5 μm to 50 μm (Measurements are performed on a single sample regardless of its film thickness) • Measurement temperature range: -50 to 300°C • Heating rate: 10°C / min ・Measurement frequency: 1Hz • Modification mode: Linear tension mode Initial value of static tensile load: 0.5 N Initial gap distance (at 25°C): 25 mm Auto Strain Adjustment: Enabled (Range: Amplitude value 0.05–25%, sinusoidal load 0.02–5N) It was done there. (ii) Static tensile load refers to the midpoint between the maximum and minimum stresses in each periodic motion, and sinusoidal load refers to the vibrational stress centered on the static tensile load. (iii) The sinusoidal tensile mode refers to measuring vibration stress while performing periodic motion with a fixed amplitude of 0.2%. In this process, the gap distance and static tensile load were varied so that the difference between the static tensile load and the sinusoidal load was within 20%. When the sinusoidal load fell below 0.02 N, the amplitude was amplified so that the sinusoidal load remained within 5 N and the increase in amplitude was within 25% before measuring the vibration stress. (iv) Relationship between the obtained sinusoidal load and amplitude value, and the following equation: s * =s 0 ・Exp[i(ωt+d)], e * =e 0 ・Exp(iot) s * =E * ・e * E * =E'++E'' (In the formula, σ * : Vibration stress, ε * : strain, i: imaginary unit, ω: angular frequency, t: time, δ: phase difference between vibrational stress and strain, E * : Complex modulus of elasticity, E': Storage modulus of elasticity, E'': Loss modulus of elasticity Vibration stress: sinusoidal load / initial cross-sectional area Static tensile load: The load at the point of minimum vibration stress in each period (the point of minimum gap distance in each period). Sinusoidal load: The difference between the measured vibration stress and the static tensile load. The storage modulus is calculated from this. The mixed storage modulus ratio (R) is defined by E’mix A microporous film for an energy storage device according to claim 1 or 2, wherein the ratio is 1.2 to 20 times.

4. The microporous membrane for the energy storage device is made of polypropylene, The following requirements (P1) to (P3): (P1) The MFR measured under conditions of a temperature of 230°C and a mass of 2.16 kg is 2.5 g / 10 min or less; (P2) The value obtained by dividing the weight-average molecular weight Mw by the number-average molecular weight Mn (Mw / Mn) is 10 or less; and (P3) Density is 0.89 g / cm³ 3 That's all: Homopolypropylene (A) that satisfies the following conditions, Polypropylene (B) that does not satisfy at least one of the above requirements (P1) to (P3) and has a functional group, A microporous film for an energy storage device according to any one of claims 1 to 3, including the above.

5. The microporous membrane for energy storage devices according to claim 4, wherein the content of the polypropylene (B) is 4% by mass or more and 30% by mass or less.

6. The microporous membrane for an energy storage device according to claim 4 or 5, wherein the polypropylene (B) is silane-modified polypropylene.

7. The homopolypropylene (A) has an MFR of 0.25 g / 10 min or more, an Mw / Mn of 4.9 or more, and a density of 0.96 g / cm³. 3 The following is a microporous film for an energy storage device according to any one of claims 4 to 6.

Citation Information

Patent Citations

  • Porous film, and separator for cell and cell using the same

    JP1997216964A

  • Porous membrane, battery separator comprising porous membrane, and manufacture thereof

    JP1999144700A

  • Porous film, battery separator comprising porous film, and its production

    JP1999172036A

  • Production of microporous resin film

    JP2000319441A

  • Porous film

    JP2001176484A