semiconductor element

By employing a first and second semiconductor contact layer with controlled Al compositions and graded layers, the semiconductor device addresses high driving voltage and leakage current issues, enhancing electrical and light-emitting performance.

JP7954330B1Active Publication Date: 2026-11-19ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2026067661
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2026-04-16
Publication Date
2026-11-19
Estimated Expiration
2046-04-16

AI Technical Summary

Technical Problem

Existing semiconductor devices face issues with high driving voltage, forward leakage current, and sudden failure due to lattice relaxation and poor contact resistance between electrodes and semiconductor layers, particularly in ultraviolet light-emitting elements.

Method used

The semiconductor device incorporates a first semiconductor contact layer with a specific Al composition (0.3≤x≤1) and a second semiconductor contact layer with a lower Al composition (0

Benefits of technology

The solution effectively suppresses driving voltage, reduces leakage current, and prevents sudden failure by optimizing layer compositions and structures, improving light output and electrical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954330000001_ABST
    Figure 0007954330000001_ABST
Patent Text Reader

Abstract

The present invention provides a semiconductor device comprising at least a first electrode, a first semiconductor contact layer, a second semiconductor contact layer, and a functional layer. [Solution] A first electrode and Al in contact with the first electrode. x Ga 1-x A first semiconductor contact layer represented by the composition N(0.3≦x≦1), and Al located on one side of the first semiconductor contact layer. y Ga 1-y N(0
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a semiconductor element.

Background Art

[0002] Patent Document 1 describes "A deep ultraviolet light-emitting element sequentially having an n-type semiconductor layer, a light-emitting layer, a p-type electron blocking layer, and a p-type contact layer on a substrate, wherein the p-type contact layer has a first layer made of AlₓGa₁₋ₓN having an Al composition ratio x higher than the Al composition ratio w₀ of the layer that emits deep ultraviolet light in the light-emitting layer, and a second layer made of AlᵧGa₁₋ᵧN having an Al composition ratio y lower than the Al composition ratio x, and has a superlattice structure formed by alternately stacking the first layer and the second layer, and the Al composition ratio w₀, the Al composition ratio x, the Al composition ratio y, and the thickness-average Al composition ratio z of the p-type contact layer satisfy the following formulas [1] and [2]: 0.030<z-w₀<0.20···[1] 0.050≦x-y≦0.47···[2] A deep ultraviolet light-emitting element characterized by satisfying the above. (Claim 1)". Patent Document 2 describes "A semiconductor light-emitting device comprising the following components: an n-type nitride semiconductor layer; an active layer formed on the n-type nitride semiconductor layer; a p-type nitride semiconductor layer formed on the active layer; a contact layer formed on the p-type nitride semiconductor layer, the composition ratio of aluminum (Al) element varying along the thickness direction; and a reflective electrode formed on the contact layer. The contact layer includes first, second, and third regions sequentially formed along the thickness direction from the p-type nitride semiconductor layer to the reflective electrode, the first and third regions contain Al element, and the second region does not contain Al element. (Translation of Claim 1)".

[0003] [Prior Art Documents] [Patent Documents] [Patent Document 1] Japanese Patent No. 6849641 [Patent Document 2] U.S. Patent No. 9012884 [Summary of the Invention] [Means for Solving the Problems]

[0004] In a first aspect of the present invention, there is provided a semiconductor device comprising at least a first electrode, a first semiconductor contact layer, a second semiconductor contact layer, and a functional layer. The first semiconductor contact layer is in contact with the first electrode and contains Al x Ga 1-x N, represented by the composition formula where 0.3≦x≦1. The second semiconductor contact layer is located on one side of the first semiconductor contact layer, and contains Al y Ga 1-y N, represented by the composition formula where 0<y≦1. The functional layer is located on one side of the second semiconductor contact layer, and produces a function as a semiconductor device in which carriers recombine with each other or carriers move. The film thickness T2 (nm) of the second semiconductor contact layer satisfies 0.25<T2<4. The semiconductor device satisfies y<x.

[0005] In the above description, the film thickness T1 (nm) of the first semiconductor contact layer may satisfy 4≦T1≦35.

[0006] In the above description, the semiconductor device may further comprise a first graded layer between the first semiconductor contact layer and the second semiconductor contact layer. The first graded layer contains Al z Ga 1-z N, having a composition where 0<z≦1, and the Al composition ratio between the first semiconductor contact layer and the second semiconductor contact layer may be changed stepwise or continuously.

[0007] In the above description, the sum of the film thickness T3 (nm) of the first graded layer and the film thickness T2 (nm) of the second semiconductor contact layer may satisfy 0.25<T2+T3<4.

[0008] In the above description, the semiconductor device may have an electron blocking layer at a position between the functional layer and the second semiconductor contact layer. The electron blocking layer is a nitride semiconductor, and may have a higher Al composition ratio than the functional layer.

[0009] In the above, the semiconductor element may further include a second gradient layer between the electron blocking layer and the second semiconductor contact layer, which has a composition of AlₚGa₁₋ₚN (0<p≦1) and makes the Al composition ratio between the electron blocking layer and the second semiconductor contact layer change stepwise or continuously. The Al composition ratio p of the second gradient layer may be higher than the Al composition ratio y of the second semiconductor contact layer.

[0010] In the above, the semiconductor element may further include a diffusion prevention layer between the second semiconductor contact layer and the second gradient layer. The diffusion prevention layer may have an Al composition ratio higher than the Al composition ratio at the interface of the second gradient layer on the second semiconductor contact layer side and the Al composition ratio at the interface of the second semiconductor contact layer on the second gradient layer side.

[0011] In the above, the film thickness T4 (nm) of the diffusion prevention layer may satisfy 0.25≦T4≦3.

[0012] In the above, the semiconductor element may have only one combination of the first semiconductor contact layer and the second semiconductor contact layer.

[0013] In the above, the average Mg concentration (number of atoms / cm³) of the first semiconductor contact layer may be 9×10 19 cm -3 or more and 1×10 21 cm -3 or less.

[0014] In the above, the average carbon concentration (number of atoms / cm 3 ) of the first semiconductor contact layer may be 3×10 17 ×x + 2×10 17 cm -3 or more, and 9×10 19 ×x + 5×10 17 cm -3 or less.

[0015] In the above, the average oxygen concentration (number of atoms / cm 3 ) of the first semiconductor contact layer may be exp(5.529×x)×2×10 16 cm-3 or more, and exp(8.503×x)×10 18 cm -3 or less.

[0016] In the above description, the first electrode may contain one or more of Rh, Ru, Ir and Al. The first electrode may have a portion with an oxygen concentration higher than that of the first semiconductor contact layer.

[0017] In the above description, the semiconductor element may further include an n-type nitride semiconductor layer having a composition of Al u Ga 1-u N. The functional layer may be a light-emitting layer located between the n-type nitride semiconductor layer and the second semiconductor contact layer. The light-emitting layer may have a composition of Al a Ga 1-a N (0≦a≦1). The light-emitting layer may emit ultraviolet light having a central emission wavelength of 200 nm or more and less than 300 nm. The relationship a-0.1<x may be satisfied.

[0018] In the above description, the light-emitting layer may have a quantum well structure including one or more combinations of barrier layers and well layers.

[0019] Note that the above summary of the present invention does not enumerate all necessary features of the present invention. Sub-combinations of these groups of features may also constitute an invention. [Brief Description of the Drawings]

[0020] [Figure 1] An example of the layer configuration of the semiconductor element 100 according to the present embodiment is shown. [Figure 2A] An example of the Al composition profile of the semiconductor element 100 according to FIG. 1 is shown. [Figure 2B] An example of the Al composition profile of the semiconductor element 100 that does not include the second semiconductor contact layer 140 is shown. [Figure 3] An example of the layer configuration of the semiconductor element 100 according to the first modification of the present embodiment is shown. [Figure 4]An example of the layer configuration of the semiconductor element 100 in a second modified example of this embodiment is shown. [Figure 5] An example of the layer configuration of the semiconductor element 100 in a third modified example of this embodiment is shown. [Figure 6] An example of EDX (energy-dispersive X-ray analysis) of the upper layer of semiconductor device 100, above the second gradient layer 152, is shown. [Modes for carrying out the invention]

[0021] The present invention will be described below through embodiments, but these embodiments are not intended to limit the invention as defined in the claims. Not all combinations of features described in the embodiments are necessarily essential to the solution of the invention. Furthermore, embodiments will be described with reference to the drawings, but in the drawings, identical or similar parts may be given the same reference numeral to omit redundant descriptions.

[0022] [Configuration of semiconductor element 100] Figure 1 shows an example of the layer configuration of the semiconductor element 100 in this embodiment. The semiconductor element 100 may be a semiconductor element mainly using nitride, and may be, for example, a light-emitting element that emits light of a predetermined frequency (e.g., ultraviolet light).

[0023] The semiconductor element 100 comprises a first electrode 110, a first semiconductor contact layer 120, a first gradient layer 130, a second semiconductor contact layer 140, a diffusion prevention layer 150, a second gradient layer 152, an electron blocking layer 160, a functional layer 170, an n-type nitride semiconductor layer 180, an AlN layer 190, and a substrate 192, all stacked in this order.

[0024] Figure 2A shows an example of the Al composition profile of the semiconductor device 100 shown in Figure 1. The horizontal axis of Figure 2A indicates the stacking position of each layer included in the semiconductor device 100. The left side corresponds to the substrate 192 side and the right side corresponds to the first electrode 110 side. Figure 2A shows the composition of the semiconductor device 100 from the first electrode 110 to the n-type nitride semiconductor layer 180. The vertical axis of Figure 2A shows the proportion of Al composition in each layer.

[0025] The first electrode 110 is an electrode provided on the opposite side of the substrate 192. The first electrode 110 may be a p-type electrode. When the semiconductor element 100 is a light-emitting element, light is extracted from the substrate 192 side (the lower side in Figure 1). In this case, the first electrode 110 functions as a reflective electrode that reflects the light irradiated from the functional layer 170 back to the substrate 192 side.

[0026] The first electrode 110 is made of a conductive material. For example, the first electrode 110 may contain one or more of Rh, Ru, Ir, and Al. This increases the reflectivity of the first electrode 110, thereby improving the light extraction efficiency when the functional layer 170 is an emissive layer.

[0027] The first electrode 110 may have regions with a higher oxygen concentration than the first semiconductor contact layer 120. For example, the surface of the first electrode 110 that contacts the first semiconductor contact layer 120 may have a higher oxygen concentration compared to other parts. This allows the first electrode 110 to improve ohmic contact with the first semiconductor contact layer 120, which has a relatively high Al composition.

[0028] The first semiconductor contact layer 120 is in contact with the first electrode 110. The first semiconductor contact layer 120 may be provided between the first electrode 110 and the first gradient layer 130. The first semiconductor contact layer 120 is made of Al x Ga 1-x It is expressed as the composition of N. x may be 0.3 ≤ x ≤ 1, preferably 0.3 ≤ x ≤ 0.9, and more preferably 0.4 ≤ x ≤ 0.8. A higher value of x increases the transparency of the layer and can increase the light output when the functional layer 170 is the light-emitting layer. The first semiconductor contact layer 120 may further contain impurities such as C, H, F, O, Mg, and Si.

[0029] Average Mg concentration (number of atoms / cm³) of the first semiconductor contact layer 120 3 ) is 9 x 10 19 cm -3 Preferably 2 × 10 20 cm -3The above is acceptable. Average Mg concentration of the first semiconductor contact layer 120 (number of atoms / cm³) 3 ) is 1 × 10 21 cm -3 The following is preferably 8 × 10 20 cm -3 The following is acceptable:

[0030] Average carbon concentration (number of atoms / cm³) of the first semiconductor contact layer 120 3 )teeth, 3 x 10 17 ×x + 2×10 17 cm -3 Preferably, 1 x 10 18 cm -3 That's all.

[0031] Average carbon concentration (number of atoms / cm³) of the first semiconductor contact layer 120 3 )teeth, 9×10 19 ×x + 5×10 17 cm -3 Preferably, 2 x 10 19 cm -3 The following is acceptable:

[0032] Average oxygen concentration (number of atoms / cm³) of the first semiconductor contact layer 120 3 ) is exp(5.0×x)×2×10 16 cm -3 Preferably, exp(5.529×x)×2×10 16 cm -3 The above is acceptable. Average oxygen concentration of the first semiconductor contact layer 120 (number of atoms / cm³) 3 ) is exp(9.0×x)×10 18 cm -3 Preferably, exp(8.503×x)×10 18 cm -3 The following is acceptable:

[0033] When the average Mg concentration, average carbon concentration, and / or average oxygen concentration are equal to or higher than the respective predetermined values as described above, the conductivity of the first semiconductor contact layer 120 can be enhanced, favorable contact with the first electrode 110 can be formed, and the risk of leakage current can be reduced. When the average Mg concentration, average carbon concentration, and / or average oxygen concentration are equal to or lower than the respective predetermined values as described above, the flatness of the layer can be improved.

[0034] The film thickness T1 (nm) of the first semiconductor contact layer 120 may satisfy 4≦T1≦35. Thereby, occurrence of leakage current in the semiconductor element 100 can be prevented. Furthermore, it is possible to suppress absorption of light such as ultraviolet light emitted from the functional layer 170 functioning as a light-emitting layer, increase the light output, and reduce the risk of causing electrical defects.

[0035] The first graded layer 130 is in contact with the first semiconductor contact layer 120. For example, the first graded layer 130 is located between the first semiconductor contact layer 120 and the second semiconductor contact layer 140.

[0036] The first graded layer 130 changes the Al composition ratio between the first semiconductor contact layer 120 and the second semiconductor contact layer 140 stepwise or continuously. The first graded layer 130 is disposed between the first semiconductor contact layer 120 and the second semiconductor contact layer 140, and has Al z Ga 1-z N (0<z≦1). That is, z is not constant, but changes continuously or stepwise depending on the position in the film thickness direction.

[0037] For example, the first graded layer 130 may have the same or closest composition as the first semiconductor contact layer 120 at the interface in contact with the first semiconductor contact layer 120, gradually becomes stepwise or continuously closer to the composition of the second semiconductor contact layer 140 toward the second semiconductor contact layer 140 therefrom, and may have the same or closest composition as the second semiconductor contact layer 140 at the interface in contact with the second semiconductor contact layer 140.

[0038] By providing the first graded layer 130, the first semiconductor contact layer 120 and the second semiconductor contact layer 140 can be formed without causing lattice relaxation.

[0039] The film thickness T3 (nm) of the first graded layer 130 may be 0.25 to 4, preferably 0.5 to 3. By satisfying such a range, lattice relaxation can be prevented without making the film thickness excessively large.

[0040] The second semiconductor contact layer 140 is located on one side of the first semiconductor contact layer 120. For example, the second semiconductor contact layer 140 is located between the first graded layer 130 and the diffusion prevention layer 150. The second semiconductor contact layer 140 is Al y Ga 1-y N in composition. y satisfies 0 < y ≤ 1, and may preferably be 0.1 to 0.7. When y is 0, that is, when the second semiconductor contact layer 140 is GaN, it is not suitable from the viewpoint of sample fabrication, such as the occurrence of lattice relaxation and coverage. For example, when the second semiconductor contact layer 140 made of GaN is fabricated on AlN, since the lattice constant difference between AlN and GaN is large, GaN immediately undergoes lattice relaxation, and the crystallinity of GaN deteriorates. In addition, GaN on AlN has poor coverage, and when viewed in the film thickness direction, a portion where the second semiconductor contact layer 140 is not fabricated is formed, and there exists a portion that cannot fulfill the function of the second semiconductor contact layer 140. For this reason, y needs to be greater than 0.

[0041] As described above, the high x value of the first semiconductor contact layer 120 in contact with the first electrode 110 can increase the light output. On the other hand, when the x value of the first semiconductor contact layer 120 is high, the risk of occurrence of a phenomenon called sudden death, in which the light output suddenly drops or non-lighting occurs abruptly, increases. Furthermore, the turn-on voltage also increases.

[0042] Here, by satisfying y<x, that is, making the Al composition ratio y of the second semiconductor contact layer 140 smaller than the Al composition ratio x of the first semiconductor contact layer 120, holes or electrons can move in the film plane direction due to the effect of a two-dimensional hole gas or a two-dimensional electron gas. This effect increases as the Al composition difference between x and y increases. By satisfying y<x, an electric field in a direction different from that in the case where the second semiconductor contact layer 140 is not present is generated in the first semiconductor contact layer 120. This facilitates electrons or holes to tunnel through the first semiconductor contact layer 120, improves the contact resistance between the first electrode 110 and the first semiconductor contact layer 120, and makes it easier for current to flow in the film thickness direction. This effect increases as the Al composition difference between x and y increases.

[0043] As a result, by satisfying y<x, the driving voltage of the semiconductor element 100 can be suppressed, forward leakage current below the turn-on voltage can be suppressed, and furthermore, sudden death can be prevented.

[0044] x-y only needs to be greater than 0, preferably 0.1 or more, and more preferably 0.2 or more. This makes it easier for current to flow in the horizontal direction and the film thickness direction. x-y is preferably 0.9 or less, more preferably 0.6 or less. This can prevent a voltage rise due to lattice relaxation.

[0045] The film thickness T2 (nm) of the second semiconductor contact layer 140 satisfies 0.25<T2<4. When the film thickness of the second semiconductor contact layer 140 is equal to or greater than a certain value, the above effect of y<x can be ensured. By setting the film thickness of the second semiconductor contact layer 140 to be equal to or less than a certain value, it is possible to prevent the driving voltage of the semiconductor element 100 from becoming excessively high and suppress leakage current. In addition, light absorption in the second semiconductor contact layer 140 can be suppressed, and the light output can be improved.

[0046] The sum of the film thickness T2 (nm) of the second semiconductor contact layer 140 and the film thickness T3 (nm) of the first graded layer 130 may satisfy 0.25 < T2+T3 < 4. This can prevent the composition from changing abruptly in the film thickness direction, thereby making lattice relaxation less likely to occur. In addition, the electrical characteristics of the semiconductor element 100 can be maintained favorably, and absorption of emitted light can be suppressed.

[0047] The semiconductor element 100 may have only one combination of the first semiconductor contact layer 120 and the second semiconductor contact layer 140. In this case, the semiconductor element 100 does not include a repeated layer structure such as a superlattice structure. This can prevent an increase in total film thickness that would cause light absorption. Furthermore, since the number of energy barriers that electrons or holes have to cross is reduced due to the increased total film thickness, the function of the second semiconductor contact layer 140 can be ensured.

[0048] The diffusion preventing layer 150 is located on one side of the second semiconductor contact layer 140. For example, the diffusion preventing layer 150 is located between the second semiconductor contact layer 140 and the second graded layer 152.

[0049] The diffusion preventing layer 150 is represented by the composition Al q Ga 1-q N. The diffusion preventing layer 150 has an Al composition ratio (q) that is higher than the Al composition ratio (p1) at the interface of the second graded layer 152 on the second semiconductor contact layer 140 side and the Al composition ratio (y) at the interface of the second semiconductor contact layer 140 on the second graded layer 152 side.

[0050] For example, q may satisfy 0.35 ≦ q ≦ 1.0, preferably 0.35 ≦ q ≦ 0.9, and more preferably 0.45 to 0.8.

[0051] The film thickness T4 (nm) of the diffusion preventing layer 150 may satisfy 0.25≦T4≦3, and preferably satisfies 0.5≦T4≦2.0. By forming the diffusion preventing layer 150 with a film thickness equal to or greater than a certain value, atomic diffusion of the second semiconductor contact layer 140 can be prevented, and the film thickness controllability and surface flatness of the second semiconductor contact layer 140 can be improved. By keeping the film thickness of the diffusion preventing layer 150 equal to or less than a certain value, the risk that the diffusion preventing layer 150 becomes a potential barrier for electrons and / or holes, and the risk that carrier recombination or the like occurs in the second semiconductor contact layer 140 are reduced.

[0052] The second graded layer 152 is located on one side of the diffusion preventing layer 150. For example, the second graded layer 152 is located between the electron blocking layer 160 and the second semiconductor contact layer 140. The second graded layer 152 contains Al p Ga 1-p N with a composition of (0<p≦1). The second graded layer 152 changes the Al composition ratio stepwise or continuously between the electron blocking layer 160 and the second semiconductor contact layer 140. That is, p is not constant, but changes continuously or stepwise depending on the position in the film thickness direction.

[0053] For example, the second graded layer 152 has the lowest Al composition at the interface in contact with the diffusion preventing layer 150, and gradually approaches the composition of the electron blocking layer 160 stepwise or continuously as it goes toward the electron blocking layer 160, and may have the same or closest composition as the electron blocking layer 160 at the interface in contact with the electron blocking layer 160. In addition, in the second graded layer 152, the Al composition at the interface in contact with the diffusion preventing layer 150 may be higher than the Al composition of the second semiconductor contact layer 140. Thereby, the effect of providing the second semiconductor contact layer 140 can be enhanced.

[0054] The second graded layer 152 may contain impurities such as P, As, Sb, Si, Ge, C, H, F, O, Mg and / or Se. The film thickness T5 (nm) of the second graded layer 152 may be 5 to 110, preferably 15 to 90, and more preferably 20 to 70. Thereby, the optical output can be increased while reducing the driving voltage.

[0055] The electron blocking layer 160 is provided at a position in contact with the second inclined layer 152. For example, the electron blocking layer 160 is located between the functional layer 170 and the second semiconductor contact layer 140.

[0056] The electron blocking layer 160 contains Al b Ga 1-b N composition. For example, b may satisfy 0.6≦b≦1.0, preferably 0.7≦b≦0.9. The electron blocking layer 160 is a nitride semiconductor, and may have an Al composition ratio higher than the Al composition ratio (a) of the functional layer 170. Thereby, the current conduction resistance of the semiconductor element can be increased.

[0057] The film thickness T6 (nm) of the electron blocking layer 160 may be 5 or more and 30 or less, preferably 10 or more and 25 or less. Thereby, it is possible to suppress electron overflow while not inhibiting hole injection into the functional layer 170. In the semiconductor element 100, the portion from the first semiconductor contact layer 120 to the electron blocking layer 160 may correspond to a p-type nitride semiconductor layer corresponding to the n-type nitride semiconductor layer 180.

[0058] The functional layer 170 is located on one side of the second semiconductor contact layer 140. For example, the functional layer 170 may be located between the n-type nitride semiconductor layer 180 and the second semiconductor contact layer 140, particularly between the electron blocking layer 160 and the n-type nitride semiconductor layer 180. In the functional layer 170, carriers combine with each other to produce the function as a semiconductor element.

[0059] The functional layer 170 has Al a Ga 1-a N composition (0≦a≦1). Here, a may satisfy the relationship of a-0.1<x in relation to the Al content ratio x of the first semiconductor contact layer 120.

[0060] The functional layer 170 may be an emissive layer that emits ultraviolet light with a central emission wavelength of 200 nm or more and less than 300 nm. In this case, the emissive layer may be a quantum well structure having one or more combinations of a barrier layer and a well layer. As a result, the semiconductor device 100 functions as a light-emitting element. The film thickness T7 (nm) of the functional layer 170 may be set appropriately according to the function, for example, from 1 to 1000.

[0061] The n-type nitride semiconductor layer 180 is located on one side of the functional layer 170. For example, the n-type nitride semiconductor layer 180 is located between the functional layer 170 and the AlN layer 190.

[0062] A second electrode may be provided in the n-type nitride semiconductor layer 180. For example, the n-type nitride semiconductor layer 180 may have a region where the functional layer 170 is provided and a region where the second electrode is provided. The second electrode may be, for example, an n-type electrode. The second electrode may be made of a conductive material (e.g., gold, platinum, nickel, aluminum, titanium, molybdenum and / or vanadium), and is not particularly limited.

[0063] The n-type nitride semiconductor layer 180 is Al u Ga 1-u It has a composition of N. For example, u is 0.4 ≤ u ≤ 0.9, and preferably 0.5 ≤ u ≤ 0.8. This makes it possible to reduce the contact resistance with the second electrode while increasing the light extraction efficiency.

[0064] The thickness of the n-type nitride semiconductor layer 180 may be 400 nm or more and 1.5 μm or less, preferably 400 nm or more and 1.3 μm or less. A thickness above a certain level suppresses the increase in sheet resistance and reduces the driving voltage, while a thickness below a certain level suppresses lattice relaxation in the underlying AlN layer 190 or substrate 192.

[0065] The AlN layer 190 may be a nitride semiconductor layer grown on the surface of the substrate 192. This results in a smaller lattice constant difference compared to the n-type nitride semiconductor layer 180, and by growing it in a lattice-matched system, the number of threading dislocations can be reduced, and the lattice strain for hole gas generation can be increased.

[0066] The thickness of the AlN layer 190 may be between 0.5 μm and 10 μm. By keeping the thickness within this range, the density of penetrating dislocations can be suppressed, and crack formation can be prevented.

[0067] The substrate 192 serves as a base for forming the AlN layer 190 or the n-type nitride semiconductor layer 180. The substrate 192 may be a single crystal substrate. For example, the substrate 192 may be AlN, sapphire, Si, SiC, MgO, Ga2O3, ZnO, GaN, InN, or a mixed crystal substrate thereof. The substrate 192 may be a single crystal substrate with a nitride semiconductor (e.g., AlN, GaN, AlGaN, etc.) as the bulk material.

[0068] In particular, the substrate 192 is preferably an AlN single crystal substrate. For example, the substrate 192 may be manufactured by sublimation, hydride vapor deposition (HVPE), or flux deposition. The first main surface of the substrate 192 may be a C+ plane, and the second main surface may be a C- plane. The substrate 192 may contain impurities.

[0069] The thickness of the substrate 192 is not particularly limited. Any film thickness may be used depending on the size and strength required for the semiconductor element 100.

[0070] According to the semiconductor element 100 of this embodiment, by providing a first semiconductor contact layer 120 and a second semiconductor contact layer 140, the driving voltage of the semiconductor element 100 can be suppressed, the forward leakage current below the rise voltage can be suppressed, and sudden failure can be prevented.

[0071] Some layers of the semiconductor element 100 may be omitted and / or replaced with other layers. Further layers may be provided.

[0072] Figure 2B shows an example of the Al composition profile of semiconductor element 100' that does not have a second semiconductor contact layer 140, etc. Semiconductor element 100' does not have a second semiconductor contact layer 140, etc. In such a semiconductor element 100', electrons or holes are less likely to tunnel through the first semiconductor contact layer 120, the contact resistance of the first electrode 110 and the first semiconductor contact layer 120 increases, and current is less likely to flow in the film thickness direction. As a result, in semiconductor element 100', the driving voltage is higher compared to semiconductor element 100, leakage current is more likely to occur below the driving voltage, and the risk of sudden failure increases.

[0073] Figure 3 shows an example of the layer configuration of the semiconductor element 100 in the first modified example of this embodiment. As shown in the figure, the semiconductor element 100 may omit the n-type nitride semiconductor layer 180 from the semiconductor element 100 shown in Figure 1.

[0074] Figure 4 shows an example of the layer configuration of the semiconductor element 100 in a second modified example of this embodiment. As shown in the figure, the semiconductor element 100 may omit the first gradient layer 130 and the diffusion prevention layer 150 from the semiconductor element 100 shown in Figure 1.

[0075] Figure 5 shows an example of the layer configuration of the semiconductor element 100 in a third modified example of this embodiment. As shown in the figure, the semiconductor element 100 may omit the first gradient layer 130, the diffusion prevention layer 150, the second gradient layer 152, the electron blocking layer 160, and the n-type nitride semiconductor layer 180 from the semiconductor element 100 shown in Figure 1.

[0076] <Measurement method> (Film thickness measurement) The film thickness of each layer of the ultraviolet light-emitting element in this embodiment can be measured by cutting a predetermined cross section perpendicular to the main surface of the substrate, observing this cross section with a transmission electron microscope (TEM), and using the TEM length measurement function. The measurement method involves first observing a cross section perpendicular to the main surface of the nitride semiconductor element substrate using a TEM. Specifically, for example, the observation width is defined as a range of 2 μm or more in the direction parallel to the main surface of the substrate within the TEM image showing a cross section perpendicular to the main surface of the nitride semiconductor element substrate. Within this observation width range, contrast is observed at the interface between two layers with different compositions, so the thickness up to this interface is observed in a continuous observation area with a width of 200 nm. The film thickness of each layer is obtained by calculating the average value of the thickness of each layer contained within this 200 nm wide observation area from five locations arbitrarily extracted from the observation width of 2 μm or more.

[0077] (composition measurement) One method for measuring the composition of each layer of the ultraviolet light-emitting element in this embodiment is reciprocal space mapping (RSM) using X-ray diffraction (XRD). Specifically, the Al composition can be obtained by analyzing the reciprocal space mapping data near the diffraction peak obtained using an asymmetric plane as the diffraction plane. Examples of such diffraction planes include the (10-15) plane and the (20-24) plane.

[0078] Furthermore, for layers such as quantum well layers and graded layers where sufficient reflectance cannot be obtained by XRD, measurements can be performed using X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray spectroscopy (EDX), and electron energy-loss spectroscopy (EELS).

[0079] EELS analyzes the composition of a sample by measuring the energy lost when an electron beam passes through the sample. Specifically, for example, in a thinned sample used for TEM observation, the energy loss spectrum of the transmitted electron beam intensity is measured and analyzed. By utilizing the fact that the peak position of the peak that appears around 20 eV of energy loss changes according to the composition of each layer, the composition can be determined from the peak position. Similar to the layer thickness calculation method using TEM observation described above, the Al composition of each layer is obtained by calculating the average value of the Al composition in an observation width of 200 nm from five locations arbitrarily extracted from an observation area of ​​2 μm or more.

[0080] In EDX, characteristic X-rays generated by the electron beam in the thinned sample used for TEM observation as described above are measured and analyzed. Similar to the layer thickness calculation method using TEM observation described above, the average value of the Al composition at an observation width of 200 nm is calculated from five locations arbitrarily selected from the observation area of ​​2 μm or more, thereby obtaining the Al composition of each layer.

[0081] XPS allows for depth-direction evaluation by performing XPS measurements while sputter etching using an ion beam. While Ar+ is commonly used as the ion beam, other ion species, such as Ar cluster ions, can be used as long as they can be irradiated by the etching ion gun mounted on the XPS apparatus. The depth-direction distribution of the Al composition in each layer is obtained by measuring and analyzing the XPS peak intensities of Al, Ga, and N. Alternatively, instead of sputter etching, a laser diode can be obliquely polished so that a cross-section perpendicular to the main surface of the substrate is magnified and exposed, and the exposed cross-section can be measured with XPS.

[0082] The composition of each layer can be measured not only using XPS but also using Auger electron spectroscopy (AES). In this case, the composition can be measured by performing Auger electron spectroscopy on a cross-section exposed by sputter etching or oblique polishing. Furthermore, the composition of each layer can also be measured by SEM-EDX measurement on a cross-section exposed by oblique polishing. The number of repeating periods of the multiple quantum well structure of the ultraviolet light-emitting element of this embodiment is defined by the number of quantum well layers and can be measured by TEM observation in the same manner as described above.

[0083] The semiconductor element 100 according to this embodiment can be manufactured by stacking each layer on a substrate 192 using a known film deposition process such as MOCVD. The film thickness and composition ratio of each layer can be adjusted by known methods. For example, desired layers can be formed by adjusting the raw material supply ratio, supply amount, growth temperature, growth pressure, and / or growth time.

[0084] Known materials may be used as raw materials for the film deposition process, such as triethylgallium (TEGa), trimethylaluminum (TMAl), ammonia (NH3), monosilane (SiH4), and biscyclopentadienylmagnesium (Cp2Mg). For example, the Al composition of each layer can be controlled by controlling the supply ratio of triethylgallium (TEGa) and trimethylaluminum (TMAl), and the film thickness can be controlled by changing the growth time. The Si doping concentration can be controlled by adjusting the supply amount of monosilane (SiH4).

[0085] The above mainly describes the case where the semiconductor element 100 is a light-emitting element, but it is not limited to this. The semiconductor element 100 may be a photodiode or solar cell having a light-receiving layer, a field-effect transistor having a channel layer with a two-dimensional electron gas at the layer interface of a HEMT, a laser element having a light-amplifying layer, etc. Even in these cases, it is sufficient that a first semiconductor contact layer 120 and a second semiconductor contact layer 140 are provided in the portion of the semiconductor element 100 that is in contact with the first electrode 110.

[0086] Figure 6 shows an example of EDX (energy-dispersive X-ray analysis) of the layer above the second gradient layer 152 of the semiconductor device 100. The elemental amounts measured by the EDX intensity indicate that the semiconductor device 100 has the same Al composition as shown in Figure 2A.

[0087] [Examples] The present embodiment will be described below using examples.

[0088] [Examples 1-3 and Comparative Examples 1-3] Nitride laminates were formed on AlN substrates using the MOCVD method. Triethylgallium (TEGa), trimethylaluminum (TMAl), ammonia (NH3), monosilane (SiH4), and biscyclopentadienylmagnesium (Cp2Mg) were used as raw materials. The Al composition of each layer was controlled by adjusting the supply ratio of triethylgallium (TEGa) and trimethylaluminum (TMAl), and the film thickness was controlled by varying the growth time. The Si doping concentration was controlled by adjusting the supply amount of monosilane (SiH4). During film formation, the substrate temperature was controlled to 1100°C and the growth pressure to 50 hPa, and the raw material supply ratio (V / III ratio) of Group V raw material NH3 and Group III raw materials (triethylgallium, trimethylaluminum) was controlled.

[0089] First, an n-type nitride semiconductor layer 180 was formed on an AlN substrate. The n-type nitride semiconductor layer 180 had a thickness of 500 nm. 0.7 Ga 0.3 The film consists of N-type nitride semiconductor layers, which were deposited at a growth rate of 0.2 μm / h to 5.5 μm / h and a V / III ratio of 615 to 7500. All layers except for n-type nitride semiconductor layer 180 were deposited at a growth rate of 0.2 μm / h and a V / III ratio of 3000.

[0090] A functional layer 170 was formed on an n-type nitride semiconductor layer 180. The functional layer 170 is made of Al with a thickness of 3 nm. 0.55 Ga 0.45 N layer (well layer) and Al layer with a thickness of 12 nm 0.75 Ga 0.25It has a structure that contains five alternating N-layers (barrier layers).

[0091] A 15nm thick layer of Al is applied on top of the functional layer 170. 0.95 Ga 0.05 An electron blocking layer 160 consisting of an N layer was formed. A second gradient layer 152 was formed on top of the electron blocking layer 160. The thickness of the second gradient layer 152 is 40 nm, and it is a layer in which the Al composition p changes continuously from 0.95 to 0.9 from the electron blocking layer 160 to the diffusion prevention layer 150. The diffusion prevention layer 150 is made of Al with a thickness of 2 nm. 0.93 Ga 0.07 It is an N-layer structure.

[0092] A second semiconductor contact layer 140 and a first semiconductor contact layer 120 were sequentially formed on the diffusion prevention layer 150.

[0093] A first electrode 110 was formed on the first semiconductor contact layer 120. The first electrode 110 was formed by creating a nickel layer (2 nm) and a rhodium layer (100 nm) in that order, and then heat-treated at a temperature of 600°C. As a second electrode in contact with the n-type nitride semiconductor layer 180, a titanium layer (20 nm), an aluminum layer (150 nm), a nickel layer (30 nm), and a gold layer (50 nm) were formed in that order, and then heat-treated at a temperature of 870°C.

[0094] The rise voltage refers to the voltage value when a current of 1 mA is applied, and the leakage current refers to the current value when a forward voltage of 4 V, which is less than or equal to the rise voltage, is applied. Light emission measurements were performed on 10 devices, and the percentage of devices with a light output of 1 mW or less when a current of 500 mA was applied was defined as the failure rate.

[0095] The following table shows the Al composition x and film thickness of the first semiconductor contact layer 120, the Al composition y and film thickness of the second semiconductor contact layer 140, the rise voltage, the leakage current measurement results, and the sudden failure rate (%) for each example and comparative example. The film thickness of each layer was measured by cross-sectional TEM.

[0096] Table 1 shows the effect of the film thickness of the second semiconductor contact layer 140. As shown in Table 1, in the comparative examples where the film thickness of the second semiconductor contact layer 140 is 0.25 or less or 4 or more, the turn-on voltage exceeds 7V, which is significantly higher than that of the examples. In particular, in Comparative Example 3 where the second semiconductor contact layer 140 is absent, the turn-on voltage is extremely high. In Examples 1 to 3, the leakage current was small, whereas a large leakage current was measured in Comparative Examples 1 to 3. Further, while sudden failure did not occur in Examples 1 to 3, the sudden failure rate reached 100% in Comparative Example 3.

[0097] [Table 1]

[0098] [Examples 4 to 15 and Comparative Examples 4 to 12] Table 2 shows the effects of the Al composition x of the first semiconductor contact layer 120 and the Al composition y of the second semiconductor contact layer 140. In Examples 4 to 15 satisfying y<x, the turn-on voltage is less than 7V, while in Comparative Examples 4 to 12 not satisfying y<x, the turn-on voltage is 7V or higher, the leakage current value is high, and the sudden failure rate also exceeds 40%. [Table 2]

[0099] [Examples 16 to 23] Table 3 shows the effect of the film thickness of the first semiconductor contact layer 120. The film thickness of the first semiconductor contact layer 120 was varied within the range of 1.0 to 42 nm. In some of Examples 16, 17, 22, and 23, the leakage current and sudden failure rate were slightly higher, but were lower than those of the comparative examples and fell within the allowable range. It has been demonstrated that setting the film thickness of the first semiconductor contact layer within a certain range provides the additional effect of suppressing leakage current and reducing the sudden failure rate. [Table 3]

[0100] [Example 24] In addition to the layer configuration of Example 20, a first gradient layer 130 was provided, which is AlGaN with a film thickness of 1 nm and an Al composition ratio that changes from 0.5 to 1 from the second semiconductor contact layer 140 to the first semiconductor contact layer 120. In this case, the rise voltage was 6.5V, and the introduction of the first gradient layer 130 provided the additional effect of reducing the rise voltage. [Table 4]

[0101] Although the present invention has been described above using embodiments, the technical scope of the present invention is not limited to the scope described in the above embodiments. It will be apparent to those skilled in the art that various modifications or improvements can be made to the above embodiments. Furthermore, within the scope that does not contradict the technical aspects, matters described for a particular embodiment can be applied to other embodiments. In addition, each component may have the same name but different reference numerals as other components. It will be clear from the claims that such modified or improved forms may also be included within the technical scope of the present invention.

[0102] It should be noted that the execution order of operations, procedures, steps, and stages in the apparatus, systems, programs, and methods shown in the claims, specifications, and drawings is not explicitly stated as "before," "prior to," etc., and can be implemented in any order unless the output of a previous process is used in a later process. Even if the operation flow in the claims, specifications, and drawings is described using phrases such as "first," "next," etc. for convenience, it does not mean that it is essential to perform them in that order. The notation "A and / or B" may mean "A, B, or A and B." The notation "A, B, ... and / or Z" may mean "any one of A, B...Z, or any combination of two or more of these (including all of A to Z)." [Explanation of Symbols]

[0103] 110 1st electrode 120 First semiconductor contact layer 130 1st graded layer 140 Second semiconductor contact layer 150 Diffusion prevention layer 152 2nd graded layer 160 electron block layers 170 Functional Layers 180 n-type nitride semiconductor layer 190 AlN layer 192 circuit boards

Claims

1. First electrode and, In contact with the aforementioned electrode 1, Al x Ga 1-x A first semiconductor contact layer represented by composition N (0.3 ≤ x ≤ 1), Located on one side of the first semiconductor contact layer, Al y Ga 1-y A second semiconductor contact layer represented by composition N (0 < y ≤ 1), The device comprises at least a functional layer located on one side of the second semiconductor contact layer, which provides a function as a semiconductor element in which carriers bond to each other or carriers move, The film thickness T2 (nm) of the second semiconductor contact layer satisfies 0.25 < T2 < 4, Satisfying y < x, The average Mg concentration (number of atoms / cm³) of the first semiconductor contact layer is between 9 × 10¹⁹ cm⁻³ and 1 × 10²¹ cm⁻³. Semiconductor element.

2. The film thickness T1 (nm) of the first semiconductor contact layer satisfies 4 ≤ T1 ≤ 35. The semiconductor device according to claim 1.

3. Between the first semiconductor contact layer and the second semiconductor contact layer, Al z Ga 1-z The present invention further comprises a first gradient layer having a composition of N (0 < z ≤ 1) and which changes the Al composition ratio between the first semiconductor contact layer and the second semiconductor contact layer in a stepwise or continuous manner. The semiconductor device according to claim 1.

4. The sum of the film thickness T3 (nm) of the first gradient layer and the film thickness T2 (nm) of the second semiconductor contact layer is, Satisfying 0.25 < T2 + T3 < 4, The semiconductor device according to claim 3.

5. A nitride semiconductor electron blocking layer is provided between the functional layer and the second semiconductor contact layer, wherein the electron blocking layer has a higher Al composition ratio than the functional layer. The semiconductor device according to claim 1.

6. Between the electron blocking layer and the second semiconductor contact layer, Al p Ga 1-p The present invention further comprises a second gradient layer having a composition of N (0 < p ≤ 1) and having a stepwise or continuous change in the Al composition ratio between the electron block layer and the second semiconductor contact layer, wherein the Al composition ratio p of the second gradient layer is higher than the Al composition ratio y of the second semiconductor contact layer. The semiconductor device according to claim 5.

7. Between the second semiconductor contact layer and the second gradient layer, The invention further comprises a diffusion prevention layer having an Al composition ratio higher than the Al composition ratio at the interface of the second gradient layer on the second semiconductor contact layer side and the Al composition ratio at the interface of the second semiconductor contact layer on the second gradient layer side. The semiconductor element according to claim 6.

8. The thickness T4 (nm) of the diffusion prevention layer satisfies 0.25 ≤ T4 ≤ 3. The semiconductor device according to claim 7.

9. The combination of the first semiconductor contact layer and the second semiconductor contact layer has only one, The semiconductor device according to claim 1.

10. A first electrode and A first semiconductor contact layer, which is in contact with the first electrode and has a composition of Al x Ga 1-x N (0.3 ≤ x ≤ 1), A second semiconductor contact layer located on one side of the first semiconductor contact layer and represented by the composition Al y Ga 1-y N (0 < y ≤ 1), The device comprises at least a functional layer located on one side of the second semiconductor contact layer, which provides a function as a semiconductor element in which carriers bond to each other or carriers move, The film thickness T2 (nm) of the second semiconductor contact layer satisfies 0.25 < T2 < 4, Satisfying y < x, The average carbon concentration (number of atoms / cm³) of the first semiconductor contact layer is, 3 × 10¹⁷ × x + 2 × 10¹⁷ cm - 3 or more, and, 9 × 10¹⁹ × x + 5 × 10¹⁷ cm - 3 is less than or equal to Semiconductor element.

11. The first electrode and A first semiconductor contact layer, which is in contact with the first electrode and has a composition of Al x Ga 1-x N (0.3 ≤ x ≤ 1), A second semiconductor contact layer located on one side of the first semiconductor contact layer and represented by the composition Al y Ga 1-y N (0 < y ≤ 1), The device comprises at least a functional layer located on one side of the second semiconductor contact layer, which provides a function as a semiconductor element in which carriers bond to each other or carriers move, The film thickness T2 (nm) of the second semiconductor contact layer satisfies 0.25 < T2 < 4, Satisfying y < x, The average oxygen concentration (number of atoms / cm³) of the first semiconductor contact layer is, exp(5.529 × x) × 2 × 10¹⁶ cm - 3 or more, and exp(8.503 × x) × 10¹⁸ cm⁻³ is less than or equal to -3. Semiconductor element.

12. The average Mg concentration of the first semiconductor contact layer (atomic number / cm 3 ) is 9×10 19 cm -3 or more and 1×10 21 cm -3 or less, The semiconductor device according to claim 10 or 11.

13. The average carbon concentration (number of atoms / cm³) of the first semiconductor contact layer 3 )but, 3 x 10 17 ×x + 2×10 17 cm -3 In addition, 9 x 10 19 ×x + 5×10 17 cm -3 The following is: The semiconductor device according to claim 1 or 11.

14. The average oxygen concentration (number of atoms / cm³) of the first semiconductor contact layer 3 )but, exp(5.529 × x) × 2 × 10 16 cm -3 The above, and exp(8.503 × x) × 10 18 cm -3 The following is: The semiconductor device according to claim 1 or 10.

15. The first electrode is It includes one or more of Rh, Ru, Ir, and Al, Having a region with a higher oxygen concentration than the first semiconductor contact layer, The semiconductor device according to claim 1, 10, or 11.

16. Al u Ga 1-u The n-type nitride semiconductor layer having composition N is further comprising The aforementioned functional layer is Located between the n-type nitride semiconductor layer and the second semiconductor contact layer, Al a Ga 1-a Having composition N (0 ≤ a ≤ 1), This is an emissive layer that emits ultraviolet light with a central emission wavelength of 200 nm or more and less than 300 nm. a - 0.1 < x Satisfying the relationship, The semiconductor device according to claim 1, 10, or 11.

17. The aforementioned light-emitting layer is This quantum well structure has one or more combinations of barrier layers and well layers. The semiconductor device according to claim 16.

Citation Information

Patent Citations

  • Semiconductor light emitting element

    JP2005244128A

  • Group iii nitride semiconductor light-emitting element

    JP2019004178A

  • Ultraviolet light emission element

    JP2022041740A

  • Ultraviolet semiconductor light-emitting element

    JP2026003241A