Solid electrolyte materials and batteries

A halide solid electrolyte with a crystallite size of 40 nm or larger addresses the need for improved output characteristics in batteries by enhancing ionic conductivity and safety through reduced interfaces and hydrogen sulfide gas generation.

JP7954369B2Active Publication Date: 2026-11-20PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023524039
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-26
Filing Date
2022-03-23
Publication Date
2026-11-20
Estimated Expiration
2042-03-23

AI Technical Summary

Technical Problem

Existing solid electrolyte materials containing halogen elements in batteries require improvement in output characteristics.

Method used

Incorporating a halide solid electrolyte with specific compositional elements and a crystallite size of 40 nm or larger, which enhances ionic conductivity and reduces interface number, thereby improving battery output characteristics.

Benefits of technology

The proposed halide solid electrolyte material with a crystallite size of 40 nm or larger significantly enhances battery output characteristics and prevents the generation of hydrogen sulfide gas, leading to improved safety and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954369000003
    Figure 0007954369000003
  • Figure 0007954369000004
    Figure 0007954369000004
  • Figure 0007954369000005
    Figure 0007954369000005
Patent Text Reader

Abstract

This solid electrolyte material includes a halide solid electrolyte. The halide solid electrolyte contains: Li; at least one element selected from the group consisting of semimetal elements and metal elements other than L1; and at least one element selected from the group consisting of F, Cl, Br and I. The halide solid electrolyte has a crystallite size of at least 40nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a solid electrolyte material and a battery.

Background Art

[0002] In recent years, solid electrolyte materials containing a halogen element have attracted attention as electrolyte materials for batteries. Patent Document 1 discloses a battery in which a solid electrolyte sandwiched between a positive electrode layer and a negative electrode layer contains indium as a cation and a halogen element as an anion.

Prior Art Documents

Patent Documents

[0003]

Patent Document 1

Summary of the Invention

[0004] In the prior art, further improvement in the output characteristics of batteries using solid electrolyte materials containing a halogen element is desired.

[0005] A solid electrolyte material according to one aspect of the present disclosure is comprising a halide solid electrolyte, wherein the halide solid electrolyte contains Li, at least one selected from the group consisting of metal elements and metalloid elements other than Li, and at least one selected from the group consisting of F, Cl, Br and I. The halide solid electrolyte has a crystallite size of 40 nm or more.

[0006] According to the present disclosure, the output characteristics of a battery using a solid electrolyte material containing a halogen element can be improved.

Brief Description of the Drawings

[0007] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic configuration of a battery according to Embodiment 2. [Figure 2] Figure 2 is a diagram illustrating the manufacturing method of a battery according to Embodiment 2. [Figure 3] Figure 3 is a cross-sectional view showing the schematic configuration of a battery according to Embodiment 3. [Figure 4] Figure 4 is a graph showing the powder X-ray diffraction patterns of the compacted powders of Example 1 and Comparative Example 1. [Figure 5] Figure 5 is a graph showing the crystallinity of the compacted powders of Examples 1 and 2 and Comparative Example 1. [Modes for carrying out the invention]

[0008] The inventors diligently studied how to improve the output characteristics of batteries using solid electrolyte materials containing halogen elements. As a result, they found that in solid electrolyte materials containing halogen elements, the output characteristics of the battery can be improved by adjusting the crystallite size of the solid electrolyte containing halogen elements, i.e., the halide solid electrolyte.

[0009] Embodiments of the present disclosure will be described below with reference to the drawings.

[0010] (Summary of one aspect of this disclosure) The solid electrolyte material relating to the first aspect of this disclosure is It contains a halogen solid electrolyte, The halide solid electrolyte comprises Li, at least one selected from the group consisting of metal elements other than Li and metalloid elements, and at least one selected from the group consisting of F, Cl, Br, and I. The aforementioned halide solid electrolyte has a crystallite size of 40 nm or larger.

[0011] According to the first embodiment, the effect of improving the output characteristics of the battery is fully realized by including a halide solid electrolyte having high ionic conductivity in the solid electrolyte material. Furthermore, the output characteristics of the battery are further improved if the halide solid electrolyte has a crystallite size of 40 nm or larger.

[0012] In a second aspect of this disclosure, for example, in the solid electrolyte material according to the first aspect, the halide solid electrolyte may not contain sulfur.

[0013] According to the second embodiment, the generation of hydrogen sulfide gas can be prevented. Therefore, it becomes possible to realize a battery with improved safety.

[0014] In a third aspect of this disclosure, for example, in a solid electrolyte material according to the first or second aspect, the halide solid electrolyte may be represented by the following compositional formula (1).

[0015] Li α1 M1 β1 X1 γ1 ...Equation (1) α1, β1, and γ1 are each greater than 0. M1 is at least one selected from the group consisting of metallic elements and metalloid elements other than Li. X1 is at least one selected from the group consisting of F, Cl, Br, and I.

[0016] According to the third embodiment, the output characteristics of the battery can be further improved.

[0017] In a fourth aspect of this disclosure, for example, in the solid electrolyte material according to the third aspect, the composition formula (1) may satisfy 2 ≤ γ1 / α1 ≤ 2.4.

[0018] According to the fourth embodiment, the output characteristics of the battery can be further improved.

[0019] In a fifth aspect of this disclosure, for example, a solid electrolyte material according to the third or fourth aspect may satisfy the following conditions in composition formula (1): 2.5 ≤ α1 ≤ 3, 1 ≤ β1 ≤ 1.1, and γ1 = 6.

[0020] According to the fifth embodiment, the output characteristics of the battery can be further improved.

[0021] In a sixth aspect of this disclosure, for example, in a solid electrolyte material according to any one of the third to fifth aspects, M1 in the composition formula (1) may contain yttrium.

[0022] According to the sixth embodiment, the output characteristics of the battery can be further improved.

[0023] The battery relating to the seventh aspect of this disclosure is The positive electrode, electrolyte layer, and negative electrode are provided in this order. At least one selected from the group consisting of the positive electrode, the electrolyte layer, and the negative electrode includes a solid electrolyte material according to any one of the first to sixth embodiments.

[0024] According to the seventh embodiment, the output characteristics of the battery are further improved.

[0025] In the eighth aspect of this disclosure, for example, in the battery according to the seventh aspect, the positive electrode may contain a positive electrode active material, and the positive electrode active material may contain lithium nickel cobalt manganese oxide.

[0026] According to the eighth embodiment, the energy density of the battery can be further improved.

[0027] (Embodiment 1) The solid electrolyte material according to Embodiment 1 includes a halide solid electrolyte. The halide solid electrolyte includes Li, at least one selected from the group consisting of metal elements other than Li and metalloid elements, and at least one selected from the group consisting of F, Cl, Br, and I. The halide solid electrolyte has a crystallite size of 40 nm or larger.

[0028] With the above configuration, the effect of improving the battery's output characteristics is fully realized by including a halide solid electrolyte material with high ionic conductivity. Furthermore, the battery's output characteristics are further improved if the halide solid electrolyte has a crystallite size of 40 nm or larger. In this embodiment, ion conduction occurs well within the crystallites of the halide solid electrolyte. On the other hand, the ionic conductivity decreases at the crystallite interface of the halide solid electrolyte in this embodiment. By adjusting the crystallite size to 40 nm or larger, the number of interfaces can be reduced. This makes it possible to improve ionic conductivity.

[0029] In this disclosure, “metalloid elements” refers to B, Si, Ge, As, Sb, and Te. “Metallic elements” refers to all elements in groups 1 through 12 of the periodic table, excluding hydrogen, and all elements in groups 13 through 16 of the periodic table, excluding B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se. In other words, “metalloid elements” or “metallic elements” are the group of elements that can become cations when forming inorganic compounds with halogen elements.

[0030] The crystallite size of a halide solid electrolyte can be calculated by the following method. First, powder X-ray diffraction measurement is performed on the halide solid electrolyte. From the intensity of a specific X-ray diffraction peak in the measured X-ray diffraction spectrum, the crystallite size D (nm) of the halide solid electrolyte is calculated using the following equations (1) and (2). For example, if the halide solid electrolyte is Li3YBr2Cl4, the X-ray diffraction peak originating from the (002) plane of Li3YBr2Cl4 is 28.6°. In this disclosure, "the halide solid electrolyte has a crystallite size of 40 nm or more" means that a halide solid electrolyte with a crystallite size of 40 nm or more can be collected from at least one arbitrary region of a battery component (e.g., the electrolyte layer).

[0031] D = Kλ / (B·cosθ) ···Equation (1) B=(B obs 2 -b 2 )1 / 2 ...Formula (2) Formula (2) is the Scherrer equation. In Formula (1), K represents the Scherrer constant. In the present embodiment, K is 0.94. λ represents the wavelength of the X-ray source. In the present embodiment, the X-ray source is CuKα radiation, and λ is 0.15406 nm. θ represents the Bragg angle. In Formula (2), B obs represents the full width at half maximum of a specific peak in the X-ray diffraction spectrum of the halide solid electrolyte. b represents the full width at half maximum of the standard sample. As the standard sample, standard Si powder (SRM640 series) distributed by the National Institute of Standards and Technology NIST of the United States is used. The full width at half maximum is the full width at half maximum of the X-ray diffraction peak (2θ = about 28.4°) derived from the Si(111) plane.

[0032] The halide solid electrolyte may have a crystallite size of 45 nm or more, may have a crystallite size of 60 nm or more, or may have a crystallite size of 75 nm or more.

[0033] The upper limit of the crystallite size of the halide solid electrolyte is not particularly limited. The halide solid electrolyte may, for example, have a crystallite size of 250 nm or less, may have a crystallite size of 200 nm or less, or may have a crystallite size of 150 nm or less.

[0034] The halide solid electrolyte does not need to contain sulfur. According to the above configuration, generation of hydrogen sulfide gas can be prevented. Therefore, it is possible to realize a battery with improved safety.

[0035] The halide solid electrolyte may be represented by the following compositional formula (1).

[0036] Li α1 M1 β1 X1 γ1 ...Formula (1) α1, β1, and γ1 are each greater than 0. M1 is at least one selected from the group consisting of metal elements and metalloid elements other than Li. X1 is at least one selected from the group consisting of F, Cl, Br, and I. With the above configuration, the ionic conductivity of the solid electrolyte material can be improved. This can further improve the output characteristics of the battery.

[0037] In compositional formula (1), the condition 2 ≤ γ1 / α1 ≤ 2.4 may also be satisfied. With the above configuration, the ionic conductivity of the solid electrolyte material can be further improved. This can further improve the output characteristics of the battery.

[0038] In compositional formula (1), the following conditions may be met: 2.5 ≤ α1 ≤ 3, 1 ≤ β1 ≤ 1.1, and γ1 = 6. With this configuration, the ionic conductivity of the solid electrolyte material can be further improved. This, in turn, can improve the output characteristics of the battery.

[0039] In compositional formula (1), M1 may contain yttrium (i.e., Y). That is, the halide solid electrolyte may contain Y as a metallic element. With the above configuration, the ionic conductivity of the solid electrolyte material can be further improved. This can further improve the output characteristics of the battery.

[0040] A halogenated solid electrolyte containing Y is, for example, Li a Me b Y c The compound may be represented by the compositional formula X16, where a + mb + 3c = 6 and c > 0. Me is at least one selected from the group consisting of metallic and metalloid elements excluding Li and Y. m is the valence of element Me. X1 is at least one selected from the group consisting of F, Cl, Br, and I. With the above configuration, the ionic conductivity of the solid electrolyte material can be further improved. This can further improve the output characteristics of the battery.

[0041] Me may be at least one selected from the group consisting of, for example, Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta and Nb. According to the above configuration, the ionic conductivity of the solid electrolyte material can be further improved. As a result, the output characteristics of the battery can be further improved.

[0042] As the halide solid electrolyte, for example, the following materials can be used. According to the following configuration, the ionic conductivity of the solid electrolyte material can be further improved. As a result, the output characteristics of the battery can be further improved.

[0043] The halide solid electrolyte may be a material represented by the following composition formula (A1).

[0044] Li 6-3d Y d X16···Formula (A1) In the composition formula (A1), X1 is at least one selected from the group consisting of F, Cl, Br and I.

[0045] In the composition formula (A1), 0<d<2 is satisfied.

[0046] The halide solid electrolyte may be a material represented by the following composition formula (A2).

[0047] Li3YX16···Formula (A2) In the composition formula (A2), X1 is at least one selected from the group consisting of F, Cl, Br and I.

[0048] The halide solid electrolyte may be a material represented by the following composition formula (A3).

[0049] Li 3-3δ Y 1+δ Cl6···Formula (A3) In the composition formula (A3), 0<δ≦0.15 is satisfied.

[0050] The halide solid electrolyte may be a material represented by the following composition formula (A4).

[0051] Li 3-3δ Y 1+δ Br6···Formula (A4) In the composition formula (A4), 0<δ≦0.25 is satisfied.

[0052] The halide solid electrolyte may be a material represented by the following composition formula (A5).

[0053] Li 3-3δ+a Y 1+δ-a Me a Cl 6-x Br x ···Formula (A5) In the composition formula (A5), Me is at least one selected from the group consisting of Mg, Ca, Sr, Ba and Zn.

[0054] In the composition formula (A5), -1<δ<2, 0<a<3, 0<(3-3δ+a), 0<(1+δ-a), and 0≦x≦6 are satisfied.

[0055] The halide solid electrolyte may be a material represented by the following composition formula (A6).

[0056] Li 3-3δ Y 1+δ-a Me a Cl 6-x Br x ···Formula (A6) In the composition formula (A6), Me is at least one selected from the group consisting of Al, Sc, Ga and Bi.

[0057] In the composition formula (A6), -1<δ<1, 0<a<2, 0<(1+δ-a), and 0≦x≦6 are satisfied.

[0058] The halide solid electrolyte may be a material represented by the following composition formula (A7).

[0059] Li 3-3δ-a Y 1+δ-a Me a Cl 6-x Br x ···Formula (A7) In the compositional formula (A7), Me is at least one selected from the group consisting of Zr, Hf and Ti.

[0060] In the compositional formula (A7), -1<δ<1, 0<a<1.5, 0<(3-3δ-a), 0<(1+δ-a), and 0≦x≦6 are satisfied.

[0061] The halide solid electrolyte may be a material represented by the following compositional formula (A8).

[0062] Li 3-3δ-2a Y 1+δ-a Me a Cl 6-x Br x ···Formula (A8) In the compositional formula (A8), Me is at least one selected from the group consisting of Ta and Nb.

[0063] In the compositional formula (A8), -1<δ<1, 0<a<1.2, 0<(3-3δ-2a), 0<(1+δ-a), and 0≦x≦6 are satisfied.

[0064] More specifically, as the halide solid electrolyte, for example, Li3YX16, Li2MgX14, Li2FeX14, Li(Al,Ga,In)X14, Li3(Al,Ga,In)X16 and the like can be used. Here, X1 is at least one selected from the group consisting of F, Cl, Br and I.

[0065] In the present disclosure, "(Al,Ga,In)" indicates at least one element selected from the element group in the parentheses. That is, "(Al,Ga,In)" is synonymous with "at least one selected from the group consisting of Al, Ga and In". The same applies to other elements.

[0066] (Embodiment 2) Embodiment 2 will be described below. Descriptions that overlap with Embodiment 1 will be omitted as appropriate.

[0067] Figure 1 is a cross-sectional view showing the schematic configuration of the battery 10 according to Embodiment 2.

[0068] The battery 10 comprises a positive electrode 201, an electrolyte layer 100, and a negative electrode 202 in this order. The positive electrode 201, the electrolyte layer 100, and the negative electrode 202 are stacked in this order. The electrolyte layer 100 is positioned between the positive electrode 201 and the negative electrode 202. At least one selected from the group consisting of the positive electrode 201, the electrolyte layer 100, and the negative electrode 202 includes the solid electrolyte material according to Embodiment 1. That is, the solid electrolyte material includes a halide solid electrolyte. The halide solid electrolyte includes Li, at least one selected from the group consisting of metal elements other than Li and metalloid elements, and at least one selected from the group consisting of F, Cl, Br, and I. The halide solid electrolyte has a crystallite size of 40 nm or larger.

[0069] With the above configuration, the halide solid electrolyte having high ionic conductivity fully enhances the output characteristics of the battery 10. Furthermore, the output characteristics of the battery 10 are further improved by having a crystallite size of 40 nm or larger for the halide solid electrolyte. In this embodiment, ion conduction is good within the crystallites of the halide solid electrolyte. On the other hand, ionic conductivity decreases at the crystallite interface of the halide solid electrolyte in this embodiment. By adjusting the crystallite size to 40 nm or larger, the number of interfaces can be reduced, thereby improving ionic conductivity.

[0070] According to the mechanism described above, the desired effect can be obtained regardless of whether the halide solid electrolyte having a crystallite size of 40 nm or larger is included in any of the layers of the positive electrode 201, electrolyte layer 100, or negative electrode 202.

[0071] A halide solid electrolyte having a crystallite size of 40 nm or larger may be included in two selected components from the group consisting of a positive electrode 201, an electrolyte layer 100, and a negative electrode 202, in only one component, or in all of them.

[0072] In this embodiment, the electrolyte layer 100 is in contact with the positive electrode 201 and the negative electrode 202.

[0073] The average thickness of the electrolyte layer 100 may be 1 μm or more and 300 μm or less. If the average thickness of the electrolyte layer 100 is 1 μm or more, short circuits between the positive electrode 201 and the negative electrode 202 become less likely. If the average thickness of the electrolyte layer 100 is 300 μm or less, the battery 10 can operate at high output.

[0074] The average thickness of the electrolyte layer 100 can be measured by the following method: Observe a cross-section of the electrolyte layer 100 using a scanning electron microscope (SEM). The cross-section is parallel to the stacking direction of each layer and includes the centroid of the electrolyte layer 100 in a plan view. Select any three points in the obtained cross-sectional SEM image. Measure the thickness of the electrolyte layer at the three arbitrarily selected points. The average of these measurements is considered to be the average thickness.

[0075] The electrolyte layer 100 may also contain a solid electrolyte material including the halide solid electrolyte described above. The output characteristics of the battery 10 are further improved when the electrolyte layer 100 contains a halide solid electrolyte.

[0076] The electrolyte layer 100 may contain 100% by mass of a halide solid electrolyte in terms of mass relative to the total electrolyte layer 100, excluding impurities that are unavoidable to be present. In other words, the electrolyte layer 100 may be composed substantially of only a halide solid electrolyte.

[0077] The electrolyte layer 100 mainly contains a halide solid electrolyte, and may also contain unavoidable impurities, or starting materials, by-products, and decomposition products used in the synthesis of the halide solid electrolyte. The ratio of the mass of the halide solid electrolyte to the mass of the electrolyte layer 100 may be, for example, 50% by mass or more, or 70% by mass or more.

[0078] The positive electrode 201 includes, for example, a material having the property of intercalating and releasing metal ions (e.g., lithium ions) as the positive electrode active material. Examples of positive electrode active materials include lithium-containing transition metal oxides, transition metal fluorides, polyanionic materials, fluorinated polyanionic materials, transition metal sulfides, transition metal oxysulfides, and transition metal oxynitrides. Examples of lithium-containing transition metal oxides include Li(Ni,Co,Al)O2, Li(Ni,Co,Mn)O2, and LiCoO2. In particular, when a lithium-containing transition metal oxide is used as the positive electrode active material, manufacturing costs can be reduced and the average discharge voltage can be increased.

[0079] The positive electrode active material may contain lithium nickel-cobalt-manganate. For example, the positive electrode active material may contain Li(Ni,Co,Mn)O2. With the above configuration, the energy density of the battery 10 can be further improved. The positive electrode active material may also be Li(Ni,Co,Mn)O2.

[0080] The positive electrode 201 may contain an electrolyte material, for example, a solid electrolyte material. The solid electrolyte material contained in the positive electrode 201 may contain a halide solid electrolyte. As the halide solid electrolyte contained in the positive electrode 201, the halide solid electrolyte exemplified in Embodiment 1 can be used. With the above configuration, the output characteristics of the battery 10 can be further improved.

[0081] In addition to the halide solid electrolyte exemplified in Embodiment 1, other solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, polymer solid electrolytes, and complex hydride solid electrolytes can be used as the solid electrolyte contained in the positive electrode 201. The output characteristics of the battery 10 can also be further improved with the above configuration.

[0082] Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, and Li 3.25 Ge 0.25 P 0.75 S4, Li 10 GeP2S 12 These include LiX, Li2O, and MO. q Li p MO q The following may be added. Here, X is at least one selected from the group consisting of F, Cl, Br, and I. Also, M is at least one selected from the group consisting of P, Si, Ge, B, Al, Ga, In, Fe, and Zn. p and q are natural numbers, respectively. One or more sulfide solid electrolytes selected from the above materials may be used.

[0083] Examples of oxide solid electrolytes include NASICON-type solid electrolytes, such as LiTi2(PO4)3 and its elemental substitutions, and (LaLi)TiO3-based perovskite-type solid electrolytes, Li 14 ZnGe4O 16 , LISICON-type solid electrolytes such as Li4SiO4, LiGeO4 and their elemental substitutions, Li7La3Zr2O 12 Garnet-type solid electrolytes, such as those represented by elemental substitutions thereof, Li-BO compounds such as Li3PO4 and its N-substituted counterparts, and glass or glass ceramics with Li2SO4, Li2CO3, etc. added as a base may be used. One or more oxide solid electrolytes selected from the above materials may be used.

[0084] As a polymeric solid electrolyte, for example, a compound of a polymer and a lithium salt can be used. The polymer may have an ethylene oxide structure. Polymeric compounds having an ethylene oxide structure can contain a large amount of lithium salt. Therefore, the ionic conductivity can be further increased. Examples of lithium salts that can be used include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2F)2, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), and LiC(SO2CF3)3. A single lithium salt may be used, or two or more may be used in combination.

[0085] Examples of complex hydride solid electrolytes that can be used include LiBH4-LiI and LiBH4-P2S5.

[0086] The shape of the solid electrolyte contained in the battery 10 is not limited. The shape of the solid electrolyte may be, for example, needle-shaped, spherical, or ellipsoidal. The shape of the solid electrolyte may also be, for example, particulate.

[0087] If the solid electrolyte contained in the positive electrode 201 is particulate (for example, spherical), the median diameter of the solid electrolyte contained in the positive electrode 201 may be 100 μm or less. When the median diameter of the solid electrolyte is 100 μm or less, the positive electrode active material and the solid electrolyte can form a good dispersion state in the positive electrode 201. This improves the charge and discharge characteristics of the battery 10.

[0088] If the solid electrolyte contained in the positive electrode 201 is particulate (for example, spherical), the median diameter of the solid electrolyte contained in the positive electrode 201 may be 10 μm or less. When the median diameter of the solid electrolyte is 10 μm or less, the positive electrode active material and the solid electrolyte can form a better dispersion state in the positive electrode 201.

[0089] The median diameter of the solid electrolyte contained in the positive electrode 201 may be smaller than the median diameter of the positive electrode active material. This allows the positive electrode active material and the solid electrolyte to form a good dispersion state in the positive electrode 201.

[0090] The median diameter of the positive electrode active material may be 0.1 μm or more and 100 μm or less. When the median diameter of the positive electrode active material is 0.1 μm or more, the positive electrode active material and the solid electrolyte can form a good dispersion state in the positive electrode 201. This improves the charge and discharge characteristics of the battery 10. When the median diameter of the positive electrode active material is 100 μm or less, the lithium diffusion rate within the positive electrode active material becomes faster. This allows the battery 10 to operate at high power.

[0091] In this specification, the median diameter of the positive electrode active material and solid electrolyte refers to the particle size (d50) corresponding to 50% of the volume cumulative, determined from the particle size distribution measured on a volume basis by laser diffraction scattering. The particle size distribution can also be measured, for example, using an image analysis device. The same applies to other materials.

[0092] The volume ratio "v1:100-v1" of the positive electrode active material and solid electrolyte contained in the positive electrode 201 may satisfy the condition 30≦v1≦95. Here, v1 represents the volume ratio of the positive electrode active material when the total volume of the positive electrode active material and solid electrolyte contained in the positive electrode 201 is set to 100. If 30≦v1 is satisfied, a sufficient energy density of the battery can be secured. If v1≦95 is satisfied, the battery 10 can operate at high power.

[0093] The average thickness of the positive electrode 201 may be 10 μm or more and 500 μm or less. If the average thickness of the positive electrode 201 is 10 μm or more, sufficient energy density of the battery can be ensured. If the average thickness of the positive electrode 201 is 500 μm or less, the battery 10 can operate at high power.

[0094] The method described for measuring the average thickness of the positive electrode 201 can be applied to the average thickness of the electrolyte layer 100. The same method can be applied to the average thickness of the negative electrode 202.

[0095] The negative electrode 202 includes, for example, a material having the property of intercalating and releasing metal ions (e.g., lithium ions) as the negative electrode active material. The negative electrode active material can be a metallic material, a carbon material, an oxide, a nitride, a tin compound, or a silicon compound. The metallic material may be a pure metal. The metallic material may be an alloy. Examples of metallic materials include lithium metal and lithium alloys. Examples of carbon materials include natural graphite, coke, carbon in the process of graphitization, carbon fibers, spheroidal carbon, artificial graphite, and amorphous carbon. The capacity density can be improved by using silicon (Si), tin (Sn), silicon compounds, and tin compounds. An example of an oxide is Li4Ti5O 12 Examples include LiTi2O4 and TiO2.

[0096] The negative electrode 202 may contain an electrolyte material, for example, a solid electrolyte material. The solid electrolyte material contained in the negative electrode 202 may contain a halide solid electrolyte. The above-mentioned halide solid electrolyte can be used as the halide solid electrolyte contained in the negative electrode 202. With the above configuration, the output characteristics of the battery 10 can be further improved.

[0097] If the solid electrolyte contained in the negative electrode 202 is particulate (for example, spherical), the median diameter of the solid electrolyte contained in the negative electrode 202 may be 100 μm or less. When the median diameter of the solid electrolyte is 100 μm or less, the negative electrode active material and the solid electrolyte can form a good dispersion state in the negative electrode 202. This improves the charge and discharge characteristics of the battery 10.

[0098] If the solid electrolyte contained in the negative electrode 202 is particulate (for example, spherical), the median diameter of the solid electrolyte contained in the negative electrode 202 may be 10 μm or less. When the median diameter of the solid electrolyte is 10 μm or less, the negative electrode active material and the solid electrolyte can form a better dispersion state in the negative electrode 202.

[0099] The median diameter of the solid electrolyte contained in the negative electrode 202 may be smaller than the median diameter of the negative electrode active material. This allows the negative electrode active material and the solid electrolyte to form a good dispersion state in the negative electrode 202.

[0100] The median diameter of the negative electrode active material may be 0.1 μm or more and 100 μm or less. When the median diameter of the negative electrode active material is 0.1 μm or more, the negative electrode active material and the solid electrolyte can form a good dispersion state in the negative electrode 202. This improves the charge and discharge characteristics of the battery 10. When the median diameter of the negative electrode active material is 100 μm or less, the lithium diffusion rate within the negative electrode active material becomes faster. Therefore, the battery 10 can operate at high power.

[0101] The volume ratio "v2:100-v2" of the negative electrode active material and solid electrolyte contained in the negative electrode 202 may satisfy the condition 30 ≤ v2 ≤ 95. Here, v2 represents the volume ratio of the negative electrode active material when the total volume of the negative electrode active material and solid electrolyte contained in the negative electrode 202 is set to 100. If 30 ≤ v2 is satisfied, a sufficient energy density of the battery can be secured. If v2 ≤ 95 is satisfied, the battery 10 can operate at high power.

[0102] The average thickness of the negative electrode 202 may be 10 μm or more and 500 μm or less. If the average thickness of the negative electrode 202 is 10 μm or more, sufficient energy density of the battery can be ensured. If the average thickness of the negative electrode 202 is 500 μm or less, the battery 10 can operate at high power.

[0103] The positive electrode active material and the negative electrode active material may be coated with a coating material to reduce the interfacial resistance between each active material and the solid electrolyte. A material with low electronic conductivity may be used as the coating material. Examples of coating materials include sulfide solid electrolytes, oxide solid electrolytes, halide solid electrolytes, polymer solid electrolytes, and complex hydride solid electrolytes.

[0104] The coating material may also be an oxide solid electrolyte.

[0105] Examples of oxide solid electrolytes that can be used as coating materials include Li-Nb-O compounds such as LiNbO3, Li-BO compounds such as LiBO2 and Li3BO3, Li-Al-O compounds such as LiAlO2, Li-Si-O compounds such as Li4SiO4, Li2SO4, and Li4Ti5O 12 Examples include Li-Ti-O compounds such as Li2ZrO3, Li-Zr-O compounds such as Li2MoO3, Li-Mo-O compounds such as LiV2O5, and Li-WO compounds such as Li2WO4. Oxide solid electrolytes have high ionic conductivity. Oxide solid electrolytes have excellent high potential stability. Therefore, by using an oxide solid electrolyte as a coating material, the charge and discharge efficiency of the battery 10 can be further improved.

[0106] The electrolyte layer 100 may contain at least one selected from the group consisting of sulfide solid electrolytes, oxide solid electrolytes, polymer solid electrolytes, and complex hydride solid electrolytes. The materials exemplified as solid electrolytes included in the positive electrode 201 can be used as sulfide solid electrolytes, oxide solid electrolytes, polymer solid electrolytes, and complex hydride solid electrolytes. This configuration facilitates the transfer of lithium ions, thereby further improving the output characteristics of the battery 10.

[0107] At least one selected from the group consisting of the positive electrode 201, the electrolyte layer 100, and the negative electrode 202 may contain a non-aqueous electrolyte, a gel electrolyte, or an ionic liquid. With this configuration, the transfer of lithium ions is facilitated. This makes it possible to further improve the output characteristics of the battery 10.

[0108] Non-aqueous electrolytes contain a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. Non-aqueous solvents that can be used include cyclic carbonate solvents, linear carbonate solvents, cyclic ether solvents, linear ether solvents, cyclic ester solvents, linear ester solvents, and fluorine solvents. Examples of cyclic carbonate solvents include ethylene carbonate, propylene carbonate, and butylene carbonate. Examples of linear carbonate solvents include dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate. Examples of cyclic ether solvents include tetrahydrofuran, 1,4-dioxane, and 1,3-dioxolane. Examples of linear ether solvents include 1,2-dimethoxyethane and 1,2-diethoxyethane. Examples of cyclic ester solvents include γ-butyrolactone. Examples of linear ester solvents include methyl acetate. Examples of fluorinated solvents include fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, fluoroethyl methyl carbonate, and fluorodimethylene carbonate. As the non-aqueous solvent, one non-aqueous solvent selected from these may be used alone, or a mixture of two or more non-aqueous solvents selected from these may be used.

[0109] The non-aqueous electrolyte may contain at least one fluorine solvent selected from the group consisting of fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, fluoroethyl methyl carbonate, and fluorodimethylene carbonate.

[0110] Examples of lithium salts that can be used include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2F)2, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), and LiC(SO2CF3)3. One lithium salt selected from these may be used alone, or a mixture of two or more lithium salts selected from these may be used. The concentration of the lithium salt is, for example, in the range of 0.5 mol / liter to 2 mol / liter.

[0111] As the gel electrolyte, polymer materials impregnated with a non-aqueous electrolyte can be used. Examples of polymer materials include polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, and polymers having ethylene oxide bonds.

[0112] The cations constituting the ionic liquid may include aliphatic quaternary salts such as tetraalkylammonium and tetraalkylphosphonium, aliphatic cyclic ammonium compounds such as pyrrolidiniums, morpholiniums, imidazoliniums, tetrahydropyrimidiniums, piperadiniums, and piperidiniums, and nitrogen-containing heterocyclic aromatic cations such as pyridiniums and imidazoliums. The anions constituting the ionic liquid are PF6. - BF4 - SbF6 - AsF6 - , SO3CF3 - , N(SO2F)2 - , N(SO2CF3)2 - , N(SO2C2F5)2 - , N(SO2CF3)(SO2C4F9) - , C(SO2CF3)3 - Other examples are also acceptable. The ionic liquid may contain a lithium salt.

[0113] At least one selected from the group consisting of a positive electrode 201, an electrolyte layer 100, and a negative electrode 202 may contain a binder for the purpose of improving the adhesion between particles. The binder is used to improve the bonding properties of the materials constituting the electrode. Examples of binders include polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polyacrylate methyl ester, polyacrylate ethyl ester, polyacrylate hexyl ester, polymethacrylic acid, polymethacrylate methyl ester, polymethacrylate ethyl ester, polymethacrylate hexyl ester, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene-butadiene rubber, and carboxymethylcellulose. Copolymers of two or more materials selected from the group consisting of tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene can also be used as binders. A mixture of two or more materials selected from the above materials may also be used as a binder.

[0114] At least one of the positive electrode 201 and the negative electrode 202 may contain a conductive additive for the purpose of enhancing electronic conductivity. Examples of conductive additives include graphites such as natural graphite and artificial graphite, carbon blacks such as acetylene black and Ketjenblack, conductive fibers such as carbon fibers and metal fibers, metal powders such as carbon fluoride and aluminum, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and conductive polymer compounds such as polyaniline, polypyrrole, and polythiophene. When a carbon conductive additive is used as the conductive additive, costs can be reduced.

[0115] The shape of the battery 10 can be, for example, coin-shaped, cylindrical, rectangular, sheet-shaped, button-shaped, flat, or stacked.

[0116] A battery 10, comprising a positive electrode 201, an electrolyte layer 100, and a negative electrode 202, may be stacked in multiple configurations via a current collector. The battery voltage can be increased by electrically connecting multiple batteries in series. The battery capacity can be increased by electrically connecting multiple batteries in parallel. Both the battery voltage and capacity can be increased by electrically connecting multiple batteries in series and parallel.

[0117] <Method for manufacturing solid electrolyte materials> In this embodiment, the halide solid electrolyte represented by composition formula (1), which is used as the solid electrolyte material, can be manufactured, for example, by the following method.

[0118] First, several types of raw material powders for binary halides are prepared according to the desired composition. A binary halide is a compound consisting of two elements, including a halogen element. For example, to produce Li3YCl6, raw material powders LiCl and YCl3 are prepared in a molar ratio of 3:1. At this time, the elements of "M1" and "X1" in composition formula (1) are determined by selecting the type of raw material powder. Furthermore, the values ​​of "α1", "β1", and "γ1" in composition formula (1) are determined by adjusting the type of raw material powder, the mixing ratio of the raw material powders, and the synthesis process.

[0119] After mixing and grinding the raw material powders, the powders are reacted with each other using a mechanochemical milling method. Alternatively, after mixing and grinding the raw material powders, they may be sintered in a vacuum or an inert atmosphere. For example, firing can be performed at a temperature between 100°C and 400°C for at least one hour. By these methods, a halogen solid electrolyte represented by compositional formula (1) can be obtained.

[0120] <Battery manufacturing method> A battery 10 using the halide solid electrolyte manufactured above as the solid electrolyte material can be manufactured, for example, by the following method (dry method).

[0121] Figure 2 illustrates the manufacturing method of the battery 10. As shown in Figure 2, the lower die 1 is inserted into the insulating tube 3. Solid electrolyte material powder is placed inside the insulating tube 3. The upper die 2 is inserted into the insulating tube 3, and the solid electrolyte material powder is pressurized to form the electrolyte layer 100. The upper die 2 is removed, and the positive electrode material powder is placed inside the insulating tube 3. The upper die 2 is reinserted into the insulating tube 3, and the positive electrode material powder is pressurized to form the positive electrode 201 on top of the electrolyte layer 100. The positive electrode material may contain a halogen solid electrolyte.

[0122] After forming the positive electrode 201, the lower die 1 is removed and the negative electrode material powder is placed into the insulating tube 3. The lower die 1 is reinserted, and the negative electrode material powder is pressurized to form the negative electrode 202. This forms the power generation element 9. The negative electrode material may contain a halogen solid electrolyte.

[0123] Next, the material is pressure-molded at a temperature of 100°C or higher. This produces a laminate comprising a positive electrode 201, an electrolyte layer 100, and a negative electrode 202. Pressure molding is preferably performed at a temperature of 120°C. Note that the pressure molding temperature refers to the surface temperature of the mold used for pressure molding.

[0124] In the above example, the positive electrode 201, electrolyte layer 100, and negative electrode 202 are all stacked and then heated and pressurized at a temperature of 100°C or higher. However, the timing of heating and pressurizing is not limited to the above case. For example, when forming the electrolyte layer 100, the powder of the solid electrolyte material may be heated and pressurized. When forming the positive electrode 201, the powder of the positive electrode material may be heated and pressurized. When forming the negative electrode 202, the powder of the negative electrode material may be heated and pressurized. After heating and pressurizing each of the electrolyte layer 100, positive electrode 201, and negative electrode 202, the positive electrode 201, electrolyte layer 100, and negative electrode 202 are all stacked and then heated and pressurized again.

[0125] Stainless steel current collectors are placed above and below the laminate, and current collector leads are attached to the current collectors. Finally, an insulating ferrule is used to isolate and seal the inside of the insulating tube 3 from the outside atmosphere. The lower die 1 and upper die 2 are fixed with insulating tube 4, bolts 5 and nuts 6. This completes the battery 10.

[0126] The battery 10 comprises a positive electrode 201, an electrolyte layer 100, and a negative electrode 202, all obtained by pressure molding at a temperature of 100°C or higher. With this configuration, the crystallite size of the halide solid electrolyte can be adjusted so that it has a crystallite size of 40 nm or larger. This makes it possible to realize a battery 10 with particularly improved output characteristics.

[0127] A battery 10 using the halide solid electrolyte manufactured above as the solid electrolyte material can also be manufactured by a wet method. In the wet method, for example, a positive electrode slurry containing a positive electrode active material and a solid electrolyte is applied to a current collector to form a coating film. Next, the coating film is passed through a roll or flat plate press heated to a temperature of 120°C or higher and pressurized. This yields a positive electrode 201. The electrolyte layer 100 and the negative electrode 202 are manufactured by a similar method. Next, the positive electrode 201, the electrolyte layer 100, and the negative electrode 202 are stacked in this order and press-molded at a temperature of 100°C or higher. This allows the crystallite size of the halide solid electrolyte to be adjusted so that it has a crystallite size of 40 nm or larger.

[0128] (Embodiment 3) Embodiment 3 will be described below. Descriptions that overlap with Embodiments 1 and 2 will be omitted as appropriate.

[0129] Figure 3 is a cross-sectional view showing the schematic configuration of the battery 20 according to Embodiment 3.

[0130] The battery 20 comprises a positive electrode 201, a first electrolyte layer 101, a second electrolyte layer 102, and a negative electrode 202 in this order. The positive electrode 201, the first electrolyte layer 101, the second electrolyte layer 102, and the negative electrode 202 are stacked in this order. The electrolyte layer 100 includes the first electrolyte layer 101 and the second electrolyte layer 102. The electrolyte layer 100 is located between the positive electrode 201 and the negative electrode 202. The first electrolyte layer 101 contains a first solid electrolyte material. The second electrolyte layer 102 contains a second solid electrolyte material. The first solid electrolyte material and the second solid electrolyte material contain a halide solid electrolyte. The halide solid electrolyte contained in the first solid electrolyte material has a different composition from the halide solid electrolyte contained in the second solid electrolyte material. At least one selected from the group consisting of a halide solid electrolyte contained in the first solid electrolyte material and a halide solid electrolyte contained in the second solid electrolyte material has a crystallite size of 40 nm or larger. The halide solid electrolytes exemplified in Embodiment 1 can be used as the halide solid electrolytes contained in the first solid electrolyte material and the second solid electrolyte material.

[0131] Even with the above configuration, the effect of improving the output characteristics of the battery 20 is fully realized by the halide solid electrolyte having high ionic conductivity. Furthermore, the output characteristics of the battery 20 are further improved if at least one selected from the group consisting of the halide solid electrolyte contained in the first solid electrolyte material and the halide solid electrolyte contained in the second solid electrolyte material has a crystallite size of 40 nm or larger.

[0132] Both the halide solid electrolyte contained in the first solid electrolyte material and the halide solid electrolyte contained in the second solid electrolyte material may have a crystallite size of 40 nm or larger. Either the halide solid electrolyte contained in the first solid electrolyte material or the halide solid electrolyte contained in the second solid electrolyte material may have a crystallite size of 40 nm or larger.

[0133] If the halide solid electrolyte contained in the second solid electrolyte material contains iodine (i.e., I), the halide solid electrolyte contained in the first solid electrolyte material does not need to contain iodine. When iodine is contained as a halogen element in the solid electrolyte, an oxidative decomposition layer with poor lithium-ion conductivity is formed between the positive electrode active material and the solid electrolyte due to the oxidation reaction of iodine during charging. This oxidative decomposition layer functions as a large interfacial resistance in the electrode reaction of the positive electrode. However, with the above configuration, the positive electrode 201 and the second electrolyte layer 102 containing I are separated by the first electrolyte layer 101, so direct contact is prevented. Therefore, the oxidative decomposition layer is less likely to form during charging. This makes it possible to realize a battery 20 with further improved output characteristics.

[0134] The halide solid electrolytes contained in the first and second solid electrolyte materials do not necessarily have to contain sulfur. With this configuration, the generation of hydrogen sulfide gas is prevented.

[0135] In this embodiment, the electrolyte layer 100 is in contact with the positive electrode 201 and the negative electrode 202. More specifically, the first electrolyte layer 101 is in contact with the positive electrode 201. The second electrolyte layer 102 is in contact with the negative electrode 202. The first electrolyte layer 101 is in contact with the second electrolyte layer 102.

[0136] The second electrolyte layer 102 does not necessarily have to be in contact with the positive electrode 201. Solid electrolytes containing iodine as a halogen element have excellent ion conductivity but poor oxidation stability. Therefore, with the above configuration, even if the second electrolyte layer 102 contains a halogen solid electrolyte containing iodine, an oxidative decomposition layer is less likely to form during charging. Thus, the output characteristics of the battery 20 can be further improved.

[0137] The halide solid electrolyte contained in the second solid electrolyte material may be represented by the following compositional formula (2).

[0138] Li α2 M2 β2 X2γ2 ...Equation (2) α2, β2, and γ2 are each greater than 0. M2 includes at least one element selected from the group consisting of metal elements and metalloid elements other than Li. X2 includes at least one element selected from the group consisting of F, Cl, and Br, and I. A halide solid electrolyte containing I has better ion conductivity than a halide solid electrolyte that does not contain I. Therefore, with the above configuration, the ion conductivity of the second solid electrolyte material can be improved. This can further improve the output characteristics of the battery 20.

[0139] In compositional formula (2), the following conditions may be met: 2.7 ≤ α2 ≤ 3, 1 ≤ β2 ≤ 1.1, and γ2 = 6. With the above configuration, the ionic conductivity of the second solid electrolyte material can be further improved. This allows for further improvement of the output characteristics of the battery 20.

[0140] In compositional formula (2), M2 may contain yttrium (i.e., Y). That is, the halide solid electrolyte may contain Y as a metallic element. With the above configuration, the ionic conductivity of the second solid electrolyte material can be further improved. This can further improve the output characteristics of the battery 20.

[0141] A halogenated solid electrolyte containing Y is, for example, Li a Me b Y c The compound may be represented by the compositional formula X26, where a + mb + 3c = 6 and c > 0. Me is at least one selected from the group consisting of metallic and metalloid elements excluding Li and Y. m is the valence of element Me. X2 includes at least one selected from the group consisting of F, Cl and Br, and I. With the above configuration, the ionic conductivity of the second solid electrolyte material can be further improved. This can further improve the output characteristics of the battery 20.

[0142] Me may be, for example, at least one selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta and Nb. According to the above configuration, the ionic conductivity of the second solid electrolyte material can be further improved. Thereby, the output characteristics of the battery 20 can be further improved.

[0143] As the halide solid electrolyte contained in the second solid electrolyte material, for example, the following materials may be used. According to the following configuration, the ionic conductivity of the second solid electrolyte material can be further improved. Thereby, the output characteristics of the battery 20 can be further improved.

[0144] The halide solid electrolyte may be a material represented by the following composition formula (B1).

[0145] Li 6-3d Y d X26···Formula (B1) In the composition formula (B1), X2 includes at least one selected from the group consisting of F, Cl and Br, and I.

[0146] In the composition formula (B1), 0<d<2 is satisfied.

[0147] The halide solid electrolyte may be a material represented by the following composition formula (B2).

[0148] Li3YX26···Formula (B2) In the composition formula (B2), X2 includes at least one selected from the group consisting of F, Cl and Br, and I.

[0149] The halide solid electrolyte may be a material represented by the following composition formula (B3).

[0150] Li 3-3δ+a Y 1+δ-a Me a Cl 6-x-y Br x I y... Formula (B3) In the composition formula (B3), Me is at least one selected from the group consisting of Mg, Ca, Sr, Ba and Zn.

[0151] In the composition formula (B3), -1<δ<2, 0<a<3, 0<(3-3δ+a), 0<(1+δ-a), 0≦x<6, 0<y≦6, and (x+y)<6 are satisfied.

[0152] The halide solid electrolyte may be a material represented by the following composition formula (B4).

[0153] Li 3-3δ Y 1+δ-a Me a Cl 6-x-y Br x I y ... Formula (B4) In the composition formula (B4), Me is at least one selected from the group consisting of Al, Sc, Ga and Bi.

[0154] In the composition formula (B4), -1<δ<1, 0<a<2, 0<(1+δ-a), 0≦x<6, 0<y≦6, and (x+y)<6 are satisfied.

[0155] The halide solid electrolyte may be a material represented by the following composition formula (B5).

[0156] Li 3-3δ-a Y 1+δ-a Me a Cl 6-x-y Br x I y ... Formula (B5) In the composition formula (B5), Me is at least one selected from the group consisting of Zr, Hf and Ti.

[0157] In the composition formula (B5), -1<δ<1, 0<a<1.5, 0<(3-3δ-a), 0<(1+δ-a), 0≦x<6, 0<y≦6, and (x+y)<6 are satisfied.

[0158] The halide solid electrolyte may be a material represented by the following composition formula (B6).

[0159] Li 3-3δ-2a Y 1+δ-a Me a Cl 6-x-y Br x I y ···Formula (B6) In the composition formula (B6), Me is at least one selected from the group consisting of Ta and Nb.

[0160] In the composition formula (B6), -1<δ<1, 0<a<1.2, 0<(3-3δ-2a), 0<(1+δ-a), 0≦x<6, 0<y≦6, and (x+y)<6 are satisfied.

[0161] More specifically, for example, Li₃YX₂₆, Li₂MgX₂₄, Li₂FeX₂₄, Li(Al,Ga,In)X₂₄, Li₃(Al,Ga,In)X₂₆ and the like can be used as the halide solid electrolyte. Here, X₂ includes at least one selected from the group consisting of F, Cl and Br, and I.

[0162] The average thickness of the first electrolyte layer 101 and the average thickness of the second electrolyte layer 102 may be 1 μm or more and 300 μm or less. When the average thickness of each of the first electrolyte layer 101 and the second electrolyte layer 102 is 1 μm or more, short circuit between the positive electrode 201 and the negative electrode 202 is less likely to occur. When the average thickness of each of the first electrolyte layer 101 and the second electrolyte layer 102 is 300 μm or less, the battery 10 can operate at high output. The average thickness of the first electrolyte layer 101 and the average thickness of the second electrolyte layer 102 may be equal to or different from each other.

[0163] As the method for measuring the average thickness of the first electrolyte layer 101 and the second electrolyte layer 102, the method described for the average thickness of the electrolyte layer 100 in Embodiment 1 can be applied.

[0164] The first electrolyte layer 101 may contain 100% by mass of a halide solid electrolyte in terms of mass relative to the entire first electrolyte layer 101, excluding impurities that are unavoidable to be present. That is, the first electrolyte layer 101 may be composed substantially solely of a halide solid electrolyte. The second electrolyte layer 102 may contain 100% by mass of a halide solid electrolyte in terms of mass relative to the entire second electrolyte layer 102, excluding impurities that are unavoidable to be present. That is, the second electrolyte layer 102 may be composed substantially solely of a halide solid electrolyte.

[0165] The first electrolyte layer 101 mainly contains a halide solid electrolyte and may further contain unavoidable impurities, or starting materials, by-products, and decomposition products used in the synthesis of the halide solid electrolyte. The second electrolyte layer 102 mainly contains a halide solid electrolyte and may further contain unavoidable impurities, or starting materials, by-products, and decomposition products used in the synthesis of the halide solid electrolyte. The ratio of the mass of the halide solid electrolyte to the mass of the first electrolyte layer 101 may be, for example, 50% by mass or more, or 70% by mass or more. The ratio of the mass of the halide solid electrolyte to the mass of the second electrolyte layer 102 may be, for example, 50% by mass or more, or 70% by mass or more.

[0166] At least one selected from the group consisting of the first electrolyte layer 101 and the second electrolyte layer 102 may include at least one selected from the group consisting of sulfide solid electrolytes, oxide solid electrolytes, polymer solid electrolytes, and complex hydride solid electrolytes. The materials exemplified as solid electrolytes included in the positive electrode 201 can be used as sulfide solid electrolytes, oxide solid electrolytes, polymer solid electrolytes, and complex hydride solid electrolytes. With this configuration, the transfer of lithium ions becomes easier. This allows for further improvement of the output characteristics of the battery 20.

[0167] At least one selected from the group consisting of the positive electrode 201, the first electrolyte layer 101, the second electrolyte layer 102, and the negative electrode 202 may contain a non-aqueous electrolyte, a gel electrolyte, or an ionic liquid. This configuration facilitates the transfer of lithium ions, thereby further improving the output characteristics of the battery 10. The non-aqueous electrolyte, gel electrolyte, and ionic liquid exemplified in Embodiment 2 can be used.

[0168] At least one selected from the group consisting of the positive electrode 201, the first electrolyte layer 101, the second electrolyte layer 102, and the negative electrode 202 may contain a binder for the purpose of improving the adhesion between particles. The binder exemplified in Embodiment 2 may be used.

[0169] The shape of the battery 20 can be, for example, coin-shaped, cylindrical, rectangular, sheet-shaped, button-shaped, flat, or stacked.

[0170] A battery 20, comprising a positive electrode 201, a first electrolyte layer 101, a second electrolyte layer 102, and a negative electrode 202, may be stacked in multiple configurations via a current collector. The voltage of the battery can be increased by electrically connecting multiple batteries in series. The capacity of the battery can be increased by electrically connecting multiple batteries in parallel. The voltage and capacity of the battery 20 can be increased by electrically connecting multiple batteries in series and parallel.

[0171] <Method for manufacturing the first solid electrolyte material> In this embodiment, the method described for the halide solid electrolyte of Embodiment 1 can be applied as the method for producing the first solid electrolyte material, which is a halide solid electrolyte represented by composition formula (1).

[0172] <Method for manufacturing the second solid electrolyte material> In this embodiment, the second solid electrolyte material, a halide solid electrolyte represented by composition formula (2), can be manufactured, for example, by the following method.

[0173] First, several types of ternary halide raw material powders are prepared according to the desired composition. A ternary halide is a compound consisting of three elements, including a halogen element. For example, to produce Li3YBr2Cl2I2, raw material powders LiBr, LiCl, LiI, YCl3, and YBr3 are prepared in a molar ratio of 1:1:4:1:1. At this time, the elements of "M2" and "X2" in composition formula (2) are determined by selecting the type of raw material powder. Furthermore, the values ​​of "α2", "β2", and "γ2" in composition formula (2) are determined by adjusting the type of raw material powder, the mixing ratio of the raw material powders, and the synthesis process.

[0174] After mixing and grinding the raw material powders, the powders are reacted with each other using a mechanochemical milling method. Alternatively, after mixing and grinding the raw material powders, they may be sintered in a vacuum or an inert atmosphere. For example, firing can be performed at a temperature between 100°C and 400°C for at least one hour. These methods yield a halogen solid electrolyte represented by compositional formula (2).

[0175] <Battery manufacturing method> A battery using the first solid electrolyte material and the second solid electrolyte material manufactured as described above can be manufactured, for example, by the method (dry method) described with reference to Figure 2 in Embodiment 2.

[0176] In this embodiment, the second electrolyte layer 102 is formed by adding powder of the second solid electrolyte material to the insulating tube 3 and pressurizing it, and then the first electrolyte layer 101 is formed on top of the second electrolyte layer 102 by adding powder of the first solid electrolyte material and pressurizing it. [Examples]

[0177] The details of this disclosure will be explained below using examples and comparative examples according to Embodiments 1 and 2 described above.

[0178] [Fabrication of Solid Electrolyte Materials] In a glove box under an argon atmosphere with a dew point of -60°C or lower, the raw material powders LiBr, YBr3, LiCl, and YCl3 were weighed in a molar ratio of LiBr:YBr3:LiCl:YCl3 = 1:1:5:1. These raw material powders were mixed in an agate mortar to obtain a mixture. Next, the obtained mixture was milled using a planetary ball mill (Fritsch, P-7 type) for 25 hours at 600 rpm. This yielded a powder of the compound represented by the chemical formula Li3YBr2Cl4.

[0179] [Compacted powder] Example 1 In a glove box under an argon atmosphere with a dew point of -60°C or lower, Li3YBr2Cl4 and Al2O3 prepared according to the method described above were weighed in a volume ratio of Li3YBr2Cl4:Al2O3 = 30:70. These raw material powders were mixed in an agate mortar. The resulting mixture was compressed at a temperature of 120°C and a pressure of 720 MPa for 30 minutes to obtain the compacted powder of Example 1. Al2O3 was added as a substitute for hard oxides such as positive electrode active materials. This allows for the simulation of the environment inside an actual electrode.

[0180] Example 2 The compacted material of Example 2 was obtained by the same method as the compacted material of Example 1, except that the pressure molding was performed at a temperature of 220°C.

[0181] ≪Comparative Example 1≫ The compacted material of Comparative Example 1 was obtained using the same method as the compacted material of Example 1, except that heating was not performed during the pressure molding process. Specifically, in Comparative Example 1, the pressure molding was performed at room temperature (RT).

[0182] (Calculation of crystallite size) The crystallite size of Li3YBr2Cl4 was calculated using the compacts from Example 1 and Comparative Example 1. The crystallite size was calculated from the intensity of the X-ray diffraction peaks of the compacts measured using a powder X-ray diffractometer (MiniFlex600, Rigaku Corporation) using the above formulas (1) and (2). Specifically, the crystallite size was calculated using the above formulas (1) and (2) based on the full width at half maximum (FWHM) of the X-ray diffraction peak (2θ = approximately 28.4°) originating from the (111) plane of the standard Si sample. The measurement conditions for the X-ray diffraction peaks are as follows.

[0183] X-ray source: CuKα radiation (wavelength: 0.15406nm) Measurement range: 2θ = 10° to 80° Sampling step size: 0.01° Scan speed: 10° / min Figure 4 is a graph showing the powder X-ray diffraction patterns of the compacted powders of Example 1 and Comparative Example 1. In Figure 4, the vertical axis represents the number of diffracted X-rays captured by the powder X-ray diffractometer per second, i.e., the diffracted X-ray intensity. The horizontal axis represents the diffraction angle (2θ).

[0184] From the obtained powder X-ray diffraction pattern, the diffraction peaks were specified as follows, and the diffraction peaks were separated accordingly.

[0185] [Specify diffraction peaks] X-ray diffraction peak originating from the (002) plane of Li3YBr2Cl4: 28.6° [Diffraction peak separation] Profile shape function: Pseudo-Voigt Based on the above, the crystallite size of Li3YBr2Cl4 in the compacted powders of Example 1 and Comparative Example 1 was calculated. The results are shown in Table 1 below.

[0186] [Table 1]

[0187] (Evaluation of crystallinity) Crystallinity was evaluated using the compacted powders of Examples 1 and 2 and Comparative Example 1. The full width at half maximum (FWHM) of the X-ray diffraction peak was measured for Example 2 using the same method as for Example 1 and Comparative Example 1. A smaller FWHM indicates higher crystallinity. The FWHMs for Examples 1 and 2 and Comparative Example 1 were 0.270, 0.194, and 0.414, respectively. The results are shown in Figure 5.

[0188] Figure 5 is a graph showing the crystallinity of the compacts of Examples 1 and 2 and Comparative Example 1. In Figure 5, the vertical axis represents the X-ray diffraction peak full width at half maximum (FWHM), and the horizontal axis represents temperature.

[0189] Example 3 [Positive electrode material] Li(Ni,Co,Mn)O2 (hereinafter referred to as NCM) was used as the positive electrode active material. Li3YBr2Cl4, prepared according to the method described above, was used as the solid electrolyte. In a glove box with an argon atmosphere and a dew point of -60°C or lower, Li3YBr2Cl4 and NCM were weighed in a volume ratio of Li3YBr2Cl4:NCM = 30:70. The positive electrode material was obtained by mixing these raw material powders in an agate mortar.

[0190] [Negative electrode material] As the negative electrode active material, Li4Ti5O 12 (Hereinafter referred to as LTO) was used. As the solid electrolyte, Li3YBr2Cl4 prepared according to the method described above was used. In a glove box with an argon atmosphere and a dew point of -60°C or lower, Li3YBr2Cl4 and LTO were weighed in a volume ratio of Li3YBr2Cl4:NCM = 40:60. These raw material powders were mixed in an agate mortar to obtain the negative electrode material.

[0191] [Manufacturing of secondary batteries] The following process was carried out using the Li3YBr2Cl4 powder, cathode material, and anode material described above.

[0192] First, the lower die 1 was inserted into the insulating tube 3 as shown in Figure 2. 120 mg of Li3YBr2Cl4 powder and 19.3 mg of positive electrode material were then added to the insulating tube 3. The upper die 2 was then inserted into the insulating tube 3, and the positive electrode 201 was formed on top of the electrolyte layer 100 made of Li3YBr2Cl4 by pressurizing and molding at a pressure of 360 MPa.

[0193] After forming the positive electrode 201, the lower die 1 was removed and 32.1 mg of negative electrode material was added. The lower die 1 was reinserted, and the negative electrode 202 was formed by pressure molding at a pressure of 720 MPa. This formed the power generation element 9.

[0194] A laminate consisting of a positive electrode 201, an electrolyte layer 100, and a negative electrode 202 was fabricated by pressure molding the power generation element 9 at a temperature of 120°C and a pressure of 720 MPa for 30 minutes.

[0195] Next, stainless steel current collectors were placed above and below the laminate, and current collection leads were attached to the current collectors.

[0196] Finally, the battery 10 of Example 3 was fabricated by using an insulating ferrule to isolate and seal the inside of the insulating tube 3 from the outside atmosphere.

[0197] ≪Comparative Example 2≫ [Manufacturing of secondary batteries] The battery of Comparative Example 2 was manufactured using the same method as the battery of Example 3, except that after forming the power generation element 9, it was not pressure-molded at a temperature of 120°C and a pressure of 720 MPa.

[0198] (Charge / Discharge Test) Charge and discharge tests were performed using the batteries of Example 3 and Comparative Example 2 under the following conditions.

[0199] The battery was placed in a constant temperature bath at 25°C.

[0200] The battery was charged at a current value corresponding to a 2C rate (0.5-hour rate) relative to its theoretical capacity, and charging was terminated when the voltage reached 2.75V.

[0201] Next, the battery was discharged at a current value corresponding to the 2C rate, and the discharge was terminated at a voltage of 1.95V.

[0202] The results of the charge-discharge test are shown in Table 2 below.

[0203] [Table 2]

[0204] ≪Consideration≫ The compacted material of Comparative Example 1 was obtained without heating during pressurization. The compacted material of Example 1 was obtained by pressurizing while heating. Pressurizing while heating increased the crystallite size of the halide solid electrolyte. In the compacted material of Example 1, the crystallite size of the halide solid electrolyte exceeded 45 nm.

[0205] Furthermore, as shown in Figure 5, Examples 1 and 2, where the heating temperature during pressurization was 100°C or higher, showed improved crystallinity compared to Comparative Example 1. Comparing Example 1 and Example 2, crystallinity improved as the temperature during pressurization increased.

[0206] The battery of Comparative Example 2 was obtained without heating during pressurization. The pressurization conditions for the battery of Comparative Example 2 were the same as the pressurization conditions for the compacted powder of Comparative Example 1. Therefore, it can be concluded that the state of the solid electrolyte material in the battery of Comparative Example 2 is the same as the state of the solid electrolyte material in the compacted powder of Comparative Example 1. The battery of Example 3 was obtained by pressurizing while heating. The pressurization conditions for the battery of Example 3 were the same as the pressurization conditions for the compacted powder of Example 1. Therefore, it can be concluded that the state of the solid electrolyte material in the battery of Example 3 is the same as the state of the solid electrolyte material in the compacted powder of Example 1.

[0207] As shown in Table 2, the discharge capacity of the battery in Example 3 exceeded that of the battery in Comparative Example 2. The discharge capacity increased by 22.8 mAh / g. In other words, the output characteristics of the battery also improved significantly as the crystallinity of the halide solid electrolyte improved through the heating and pressurizing process. [Industrial applicability]

[0208] The battery described herein can be used, for example, as an all-solid-state lithium-ion secondary battery. [Explanation of Symbols]

[0209] 1 Lower D 2 Upper D 3. Insulating tube 4. Insulating tube 5 volts 6 nuts 9 Power generation elements 10 batteries 201 Positive electrode 202 Negative electrode 100 electrolyte layer 101 First electrolyte layer 102 Second electrolyte layer

Claims

1. It contains a halogen solid electrolyte, The aforementioned halogen solid electrolyte is Li₃YBr₂Cl₄, The aforementioned halide solid electrolyte has a crystallite size of 40 nm or more. Solid electrolyte material.

2. The crystallite size is calculated by Scherrer's equation using the X-ray diffraction peaks originating from the (002) plane of the halide solid electrolyte Li3YBr2Cl4. The solid electrolyte material according to claim 1.

3. The halide solid electrolyte has a crystallite size of 45 nm or more. The solid electrolyte material according to claim 1.

4. The positive electrode, electrolyte layer, and negative electrode are provided in this order. At least one selected from the group consisting of the positive electrode, the electrolyte layer, and the negative electrode includes the solid electrolyte material described in any one of claims 1 to 3. battery.

5. The positive electrode includes a positive electrode active material. The positive electrode active material includes lithium nickel cobalt manganese oxide. The battery according to claim 4.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery and method for manufacturing the same

    JP2002298846A

  • All-solid lithium secondary battery

    JP2006244734A

  • Lithium-containing composite oxide and production method of the same

    JP2016026981A

  • Positive electrode active material for nonaqueous electrolyte secondary battery, electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

    JP2018073751A

  • Positive electrode layer material for all-solid battery, electrode laminate for all-solid battery, and all-solid battery