Lubricant manufacturing method
The method of dispersing particles in ionic liquids by polymerizing monomers within the liquid using light irradiation addresses the challenges of existing dispersion techniques, facilitating stable and efficient production of lubricants with reduced friction and corrosion.
Patent Information
- Application Number
- JP2022152419
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-09-26
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-09-26
AI Technical Summary
Existing methods for dispersing particles in ionic liquids face challenges such as difficulty in selecting appropriate surfactants, complexity in surface modification, presence of impurities, and potential degradation of ionic liquids due to sputtering, which hinder the stable dispersion of small particles.
A method involving the preparation of a monomer mixture with a photopolymerization initiator, dispersing it in an ionic liquid, and irradiating with light to polymerize monomers, generating polymer particles that are dispersed in the ionic liquid, allowing for adjustable particle size and stable dispersion.
This method enables easier production of lubricants with dispersed particles, reducing friction and preventing corrosion by suppressing tribochemical reactions, while maintaining the lubricating properties of the ionic liquid.
Smart Images

Figure 0007954386000007 
Figure 0007954386000008 
Figure 0007954386000009
Abstract
Description
Technical Field
[0001] The present invention relates to a lubricant, and particularly to a lubricant using an ionic liquid.
Background Art
[0002] Ionic liquids, which are salts that are liquid at around normal temperature, have various properties such as electrical conductivity, chemical stability, flame retardancy, and non-volatility. In particular, chemical stability and flame retardancy are properties favorable for lubricants, and non-volatility is a desirable property for lubricants used in high vacuum environments. Accordingly, various proposals have been made to use ionic liquids having such excellent properties as lubricants (see, for example, Non-Patent Document 1).
[0003] Although there are an extremely large number of types of ionic liquids expected to serve as lubricants as described above, most ionic liquids having physical properties suitable for lubricants contain halogens including fluorine. When a halogen-containing ionic liquid is used as a lubricant for a metal member, a tribochemical reaction occurring on the sliding surface (friction surface) causes the halogen derived from the ionic liquid to react with the metal material of the friction surface, which may corrode the metal material in the vicinity of the friction surface. In addition, when an ionic liquid is used as a lubricant for a member formed of a material other than metal, although corrosion or the like does not occur, problems may arise such as decomposition of the ionic liquid leading to deterioration of the properties as a lubricant, or release of decomposition products as outgas.
[0004] Meanwhile, it is known that lubricity can be improved by dispersing particles in an ionic liquid. For example, Non-Patent Document 2 reports that dispersing functional group-modified carbon nanotubes in an ionic liquid improves lubricity. From this, it is expected that dispersing particles in an ionic liquid can suppress tribochemical reactions and realize a lubricant having favorable properties.
Prior Art Documents
Patent Documents
[0005] [Non-Patent Document 1] Y. Kondou, T. Koyama, S. Sasaki, Journal of the Vacuum Society of Japan Vol. 56 (2013), 77 [Non-Patent Document 2] B. Wang, X. Wang, W. Lou, J. Hao, Journal of Physical Chemistry C Vol. 114 (2010), 8749 [Non-Patent Document 3] T. Okabe, D. Moritaka, M. Miyatake, Y. Kondo, S. Sasaki, SYoshimoto, Precision Engineering, Vol. 47 (2017), 97 [Non-Patent Document 4] T. Torimoto, K. Okazaki, T. Kiyama, K. Hirahara, N. Tanaka, S. Kuwabata, Applied Physics Letters Vol. 89 (2006), 243117 [Overview of the Initiative] [Problems that the invention aims to solve]
[0006] However, dispersing particles in an ionic liquid is not always easy. In addition to the method described in Non-Patent Document 2, a known method for dispersing particles in an ionic liquid is to modify the surface of the particles to be dispersed (PTD) with a surfactant (SFT), and then add the SFT-modified PTD particles to the ionic liquid (ILa), as shown in Figure 7(a) (see, for example, Non-Patent Document 3).
[0007] Surfactant SFTs typically consist of a functional group (FNG) with affinity for particle PTDs and a long-chain portion (LCS) with affinity for ionic liquid ILa. However, the chemical properties of ionic liquid ILa vary significantly depending on the cations and anions that constitute it. Therefore, selecting a surfactant SFT with an appropriate long-chain portion (LCS) for each type of ionic liquid ILa is difficult, and in some cases, it becomes necessary to design and synthesize a new surfactant SFT.
[0008] Furthermore, the procedure for surface-modifying the particle PTD is complicated, similar to the method described in Non-Patent Document 2. Moreover, since surfactants such as SFT that were not used for surface modification remain on the surface-modified particle PTD, the lubricant obtained by adding the surface-modified particle PTD to the ionic liquid ILa contains many impurities.
[0009] In addition, since surface modification must be performed outside the ionic liquid ILa, the particle size of the PTD particles cannot be made smaller than a size that allows for handling the PTD particles individually. Therefore, it is not always easy to reduce the particle size of the PTD particles sufficiently and stably disperse them in the ionic liquid ILa.
[0010] Furthermore, as yet another method for dispersing particles in an ionic liquid, it has been proposed to generate particle PTS in the ionic liquid ILb by sputtering, as shown in Figure 7(b) (see, for example, Non-Patent Document 4). The generation of particle PTS by sputtering is Ar + This process involves colliding inert gas ions IIG with the target TGT to detach atomic AMS, and then agglomerating the detached atomic AMS in the ionic liquid ILb. By appropriately setting the sputtering conditions, the particle size of the PTS can be made sufficiently small, allowing the PTS particles to be stably dispersed in the ionic liquid ILb.
[0011] However, when particle PTS is generated by sputtering, collisions between ions IIG and atoms AMS with the ionic liquid ILb may cause the cations and anions constituting the ionic liquid ILb to decompose or change, potentially reducing its lubricating properties.
[0012] This invention was made to solve the aforementioned conventional problems and aims to provide a technology for more easily manufacturing lubricants in which particles are dispersed in an ionic liquid. [Means for solving the problem]
[0013] To achieve at least some of the above objectives, the present invention can be realized in the following forms or applications.
[0014] [Application Example 1] A method for producing a lubricant, comprising: (a) a step of preparing a monomer mixture comprising a liquid raw material monomer containing at least one monomer and a photopolymerization initiator; (b) a step of preparing a monomer-containing ionic liquid by adding the monomer mixture prepared in step (a) to a pre-prepared ionic liquid to disperse or dissolve the monomer mixture in the ionic liquid; and (c) a step of generating polymer particles by irradiating the monomer-containing ionic liquid prepared in step (b) with light of a wavelength in which the photopolymerization initiator is sensitive and which penetrates the ionic liquid to polymerize the raw material monomer.
[0015] According to this application example, by irradiating the monomer-containing ionic liquid with light of a wavelength to which the photopolymerization initiator has sensitivity and which transmits through the ionic liquid, the raw material monomer is polymerized in a state of being dispersed in the ionic liquid, and polymer particles are generated. Therefore, by applying this application example, it becomes possible to more easily produce a lubricant in which particles are dispersed in an ionic liquid. Further, since the particle size of the polymer particles can be adjusted by appropriately setting the wavelength and intensity of the irradiated light and the irradiation time, it becomes easier to maintain the dispersed state of the polymer particles in the ionic liquid.
[0016] [Application Example 2] The method for producing a lubricant according to Application Example 1, wherein the raw material monomer includes two types of monomers.
[0017] According to this application example, the polymerization of the monomers by light irradiation is facilitated, and the influence of the difference in reactivity of each monomer on the polymerization can be reduced, so that the lubricant in which the particles are dispersed in the ionic liquid can be produced even more easily.
[0018] [Application Example 3] The method for producing a lubricant according to Application Example 2, wherein at least one of the two types of monomers is a fluorine-containing monomer.
[0019] According to this application example, since the generated polymer particles are composed of a fluorine-based polymer having a low friction coefficient, the friction coefficient when using the obtained lubricant can be further reduced.
[0020] The present invention can be implemented in various aspects. For example, the present invention can be implemented in aspects such as a method for producing a lubricant, and a lubricant produced by the production method. [Brief Description of the Drawings]
[0021] [Figure 1] A process diagram showing a production process of a lubricant as one embodiment of the present invention. [Figure 2]Structural formula showing an example of the structure of a polymer produced by Monomer A and Monomer B. [Figure 3] Optical micrograph of the solid product produced by the method described in the embodiment. [Figure 4] Schematic diagram showing the state of the friction and wear test conducted as an evaluation of lubricating properties. [Figure 5] Schematic diagram showing the surface state of the test piece after the friction and wear test. [Figure 6] Schematic diagram showing the evaluation result of the surface roughness of the test piece after the friction and wear test. [Figure 7] Schematic diagram showing the prior art for dispersing particles in an ionic liquid. [Mode for Carrying Out the Invention]
[0022] Hereinafter, the modes for carrying out the present invention will be described in the following order. A. Embodiment: B. Examples: B1. Confirmation of formation of polymer particles: B2. Evaluation of lubricating properties: B3. Confirmation of formation of polymer particles under different conditions: C. Modified Examples:
[0023] A. Embodiment: Figure 1 is a process diagram showing the manufacturing process of a lubricant as one embodiment of the present invention. In the present embodiment, first, as shown in Figure 1(a), two types of monomers (raw material monomers) that are liquid near normal temperature (hereinafter simply referred to as "liquid", and similarly those that are solid near normal temperature are simply referred to as "solid"), which are raw materials for forming polymer nanoparticles (described later), are mixed with a photopolymerization initiator to prepare a monomer mixed liquid 10.
[0024] Specifically, the two types of monomers and the photopolymerization initiator are appropriately weighed, and the weighed monomers and photopolymerization initiator are charged into a container. Then, the monomer mixed liquid 10 is obtained by stirring the monomers and the photopolymerization initiator in the container.
[0025] As mentioned above, while a liquid monomer is used, the photopolymerization initiator can be either liquid or solid (powder). When using a powdered photopolymerization initiator, if necessary, after placing the monomer and photopolymerization initiator in a container, heat them in a water bath at a temperature that does not cause polymerization to begin, so that the photopolymerization initiator dissolves in the monomer.
[0026] Of the two monomers to be mixed, the first monomer used is, for example, 1,6-Bis(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane (hereinafter also referred to as "monomer A"), which is represented by the following structural formula. [ka]
[0027] Furthermore, as a second monomer, for example, 1H,1H,2H-Heptadecafluoro-1-decene (hereinafter also referred to as "monomer B"), represented by the following formula, can be used. [ka]
[0028] In this embodiment, monomers A and B described above are used as raw material monomers, but various fluorine-containing monomers having carbon-carbon unsaturated double bonds that are liquid at or near room temperature and capable of radical polymerization can be used as raw material monomers.
[0029] The ratio of the two monomers is set appropriately depending on the monomers used. When monomers A and B are used as raw material monomers, the ratio of monomers A and B is set to, for example, 50% by weight each.
[0030] Various photopolymerization initiators can be used, but for example, acylphosphine oxide-based photopolymerization initiators and alkylphenone-based photopolymerization initiators can be used. An example of an acylphosphine oxide-based photopolymerization initiator is phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (hereinafter also referred to as "initiator A"). This photopolymerization initiator is commercially available as Omnirad 819 (Omnirad is a registered trademark of IGM Resins BV), etc. An example of an alkylphenone-based photopolymerization initiator is 2-Hydroxy-2-methylpropiophenone (hereinafter also referred to as "initiator B"), which is marketed as Omnirad 1173, etc.
[0031] The amount of photopolymerization initiator in the monomer mixture 10 is set appropriately depending on the type of monomer and photopolymerization initiator used. When monomers A and B described above are used as raw material monomers and initiator A described above is used as the photopolymerization initiator, the amount of photopolymerization initiator is set to, for example, 2% by weight of the total weight of the monomer mixture.
[0032] The prepared monomer mixture 10 is added dropwise to the pre-prepared ionic liquid 20, as shown in Figure 1(b). The ionic liquid 20 is a salt that is liquid at or near room temperature, in which at least one of the cations (positive ions) and anions (negative ions) is an organic compound, and is suitable for use as a lubricant due to its excellent chemical stability and flame retardancy. The ionic liquid 20 is also non-volatile and hardly evaporates even in a vacuum, making it particularly suitable for use as a lubricant in high vacuum environments.
[0033] The cation used to constitute the ionic liquid 20 is N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium (DEME: N,N-Diethyl-N-methyl-n-(2-methoxyethyl)ammonium), which is represented by the following formula. [ka]
[0034] Furthermore, the anion used is bis(trifluoromethanesulfonyl)imide (TFSI), which is represented by the following formula. [ka]
[0035] The ionic liquid composed of DEME and TFSI ([DEME][TFSI]) has high thermal stability and relatively low viscosity (67 mPa·s at 25°C), making it suitable for use as a lubricant. However, in addition to ammonium-based ionic liquids such as [DEME][TFSI], various ionic liquids of the imidazolium, choline, sulfonium, pyrazolium, pyridinium, pyrrolidinium, or phosphonium types can be used. It is also possible to mix and use multiple types of ionic liquids. The ionic liquid to be used can be appropriately selected from these various ionic liquids based on the operating environment, such as the temperature range, and physical properties such as the target viscosity.
[0036] The amount of monomer mixture 10 added dropwise to the ionic liquid 20 is set appropriately depending on the type of ionic liquid 20 and the type of monomer used in the monomer mixture 10. When using the above-mentioned [DEME] and [TFSI] as the ionic liquid 20 and monomers A and B as the raw material monomers, for example, 1 part by weight of monomer mixture 10 is added dropwise to 20 parts by weight of ionic liquid 20.
[0037] The ionic liquid 20 to which the monomer mixture 10 is dropped is subjected to physical stirring and ultrasonic stirring (Figure 1(c)). This yields an ionic liquid (monomer-containing ionic liquid) 21 in which the monomer mixture is dispersed or dissolved. In this way, by dispersing or dissolving the monomer mixture 10 in the ionic liquid 20, the raw material monomer and photopolymerization initiator are contained in a nearly uniform manner in the monomer-containing ionic liquid 21.
[0038] The monomer-containing ionic liquid 21 obtained in this way is irradiated with blue light with a wavelength of 470 nm, as shown in Figure 1(d). This causes radicals to be released from the photopolymerization initiator contained in the monomer-containing ionic liquid 21, and the two types of monomers that are the raw material monomers undergo radical copolymerization by the released radicals. Through radical copolymerization of the two types of monomers, fluorine-based polymer particles (polymer nanoparticles) with a particle size of nanoscale (approximately 10 to 100 nm) are generated, and a lubricant 22 is obtained in which the generated polymer nanoparticles are dispersed in the ionic liquid.
[0039] In this embodiment, the monomer-containing ionic liquid 21 is irradiated with blue light having a wavelength of 470 nm. However, the wavelength of the light irradiated onto the monomer-containing ionic liquid 21 can be changed as appropriate, as long as it is a wavelength that is sensitive to the photopolymerization initiator and is not absorbed by the ionic liquid 20. For example, instead of blue light with a wavelength of 470 nm, ultraviolet light with a wavelength of 365 nm can be irradiated onto the monomer-containing ionic liquid 21.
[0040] The irradiation time of the monomer-containing ionic liquid 21 with light is appropriately set according to the intensity and wavelength of the irradiation light, the type of monomer and photopolymerization initiator used, and the particle size of the target polymer particles. When monomers A and B described above are used as raw material monomers and initiator A described above is used as the photopolymerization initiator, if blue light with a wavelength of 470 nm and an intensity of 3 W is irradiated, for example, by setting the irradiation time to 120 seconds, polymer particles with a particle size of nano-size can be produced.
[0041] Thus, according to this embodiment, a lubricant 22 is obtained in which polymer nanoparticles are dispersed in an ionic liquid. By introducing this lubricant 22 to the sliding parts of two sliding members, the polymer nanoparticles dispersed in the ionic liquid penetrate between the sliding surfaces of each sliding member. As a result, a gap is created between the sliding surfaces, and tribochemical reactions occurring near the contact area of the sliding surfaces are suppressed, thereby preventing corrosion and other damage from occurring on the sliding surfaces of each sliding member due to elements (especially halogens such as fluorine) derived from the ionic liquid.
[0042] Furthermore, as mentioned above, by using fluorine-containing monomers as raw materials for polymer nanoparticle production, the resulting polymer nanoparticles are composed of fluorine-based polymers. Generally, fluorine-based polymers have a low coefficient of friction, so the polymer nanoparticles that penetrate between sliding surfaces can suppress the increase in the coefficient of friction between sliding members.
[0043] Figure 2 shows a structural formula illustrating an example of a polymer produced from monomers A and B. As described above, when monomers A and B are used, polymerization reactions occur between the carbon-carbon unsaturated double bonds at both ends of monomer A and the carbon-carbon unsaturated double bonds of monomer B, as shown in the example structure in Figure 2. Therefore, a fluorine-based polymer is produced in which structure A derived from monomer A and structure B derived from monomer B are bonded together.
[0044] Note that while Figure 2 shows an example where structures A and B are bonded alternately, the polymer actually produced does not necessarily have structures A and B bonded alternately as shown in Figure 2. The resulting polymer is a state in which many structures derived from monomer A containing structure A and structures derived from monomer B containing structure B are bonded together. Therefore, it is extremely difficult to identify the structure of the produced polymer, and thus it is not possible to directly identify the polymer properties determined by its structure. Furthermore, because multiple different monomers are used, the properties of the resulting polymer change greatly depending on their proportions and the conditions of the polymerization reaction, making it extremely difficult to express the properties in terms of characteristics.
[0045] B. Examples: B1. Confirmation of polymer particle formation: To confirm that a lubricant can be produced by the method shown in the embodiment, it was confirmed that two types of monomers are photocopolymerized in an ionic liquid to produce polymer particles.
[0046] Specifically, a monomer mixture was prepared with monomers A and B each at 50% by weight, and containing 2% by weight of initiator A. Next, 0.1 g of the monomer mixture was added dropwise to 2 g of [DEME][TFSI] and stirred to prepare a monomer-containing ionic liquid. The prepared monomer-containing ionic liquid was then irradiated with 3 W of blue light (wavelength: 470 nm) to obtain a sample for particle observation. For the preparation of the particle observation sample, the blue light irradiation time was set to 10 minutes so that the generated polymer particles could be observed with an optical microscope. After irradiation with blue light, the obtained particle observation sample was filtered to extract the generated solids (generated solids), and the extracted generated solids were ultrasonically washed with acetone. The washed generated solids were then observed with an optical microscope.
[0047] Figure 3 is an optical microscope image of the solid particles produced in the sample used for particle observation. As shown in Figure 3, the solid particles were spherical white particles with a particle size of approximately 20-50 μm. From these results, it was confirmed that when an ionic liquid containing dispersed monomers is irradiated with blue light, the monomers undergo radical copolymerization, and polymer particles are produced.
[0048] B2. Evaluation of lubrication properties: The lubrication properties of the lubricant prepared by the method described in the embodiment were evaluated. Specifically, a monomer-containing ionic liquid was prepared in the same manner as when preparing the particle observation sample described above, and the prepared monomer-containing ionic liquid was irradiated with 3W blue light (wavelength: 470nm) to obtain the lubricant for the example. In preparing the lubricant for the example, the irradiation time was set to 120 seconds so that the polymer particles would be nano-sized. In addition, the ionic liquids [DEME] and [TFSI] were prepared as lubricants for comparative examples.
[0049] Next, lubrication properties were evaluated by friction and wear tests using lubricant samples as examples and comparative examples. Figure 4 is an explanatory diagram showing the friction and wear tests conducted to evaluate lubrication properties. Figure 4(a) shows the specific method of the friction and wear test, and Figure 4(b) shows the results of the friction and wear test.
[0050] As shown in Figure 4(a), the friction and wear test was performed using a ball-on-disk method, in which a ball BLL placed on a disc-shaped test piece TPC was reciprocated and slid. As the ball BLL, a 10 mm diameter steel ball made of SUJ2, a type of high-carbon chromium bearing steel with high wear resistance, was used, and as the test piece TPC, a steel disc made of SUJ2 with a diameter of 24 mm and a thickness of 7.8 mm was used. Prior to the friction and wear test, the surface of the test piece TPC was buffed with alumina as an abrasive to achieve a mirror finish.
[0051] Then, 30 μl of lubricant was dropped between the ball BLL and the test specimen TPC, and a friction and wear test was performed. The vertical load pressing the ball BLL against the test specimen TPC was 4.5 N, the test sliding distance was 10 mm, and the sliding speed was 3140 mm per minute. The friction and wear test was conducted at room temperature (RT) for 30 minutes (1800 seconds).
[0052] As a result of the friction and wear test, as shown in Figure 4(b), when the lubricant of the comparative example was used, the coefficient of dynamic friction μ was approximately 0.06 to 0.07. On the other hand, when the lubricant of the example was used, the coefficient of dynamic friction μ was higher than that of the comparative example, at approximately 0.07 to 0.09 for the first 300 seconds from the start of the test, but then gradually decreased, finally becoming slightly lower than that of the comparative example, at approximately 0.05 to 0.07. From these results, it was found that the coefficient of dynamic friction μ when using the lubricant was approximately the same for the comparative example without polymer nanoparticles and the example containing polymer nanoparticles.
[0053] Next, the surface condition of the test specimens after the friction and wear test was evaluated. Specifically, the test specimens were ultrasonically cleaned with acetone after the friction and wear test, and the cleaned specimens were observed using an electron microscope and their surface roughness was evaluated.
[0054] Figure 5 is an explanatory diagram showing the surface condition of the test specimen after the friction and wear test. Figures 5(a) and 5(c) show electron microscope images of the test specimen surface when using the lubricants of the comparative example and the example, respectively. Figure 5(b) shows a magnified image of the area within the white frame in Figure 5(a).
[0055] As can be seen in Figure 5(a), when the lubricant used as a comparative example was used, clear wear marks appeared on the surface of the test specimen. In addition to the wear marks, as shown in Figure 5(b), the surface of the test specimen had granular material approximately 10 μm in size and dark-colored areas approximately 2 μm in size. The granular material is thought to be a reaction product of fluorine generated from cations (TFSI) constituting the ionic liquid by a tribochemical reaction and SUJ2, the material of the test specimen. The dark-colored areas are thought to be corrosion marks caused by corrosion by fluorine.
[0056] On the other hand, as can be seen from Figure 5(c), when the lubricant in the example was used, almost no friction marks or corrosion marks appeared on the surface of the test piece. From this result, it was confirmed that by using the lubricant in the example produced by the method shown in the above embodiment, the sliding surface is protected by polymer nanoparticles, and the wear resistance of the sliding members can be improved.
[0057] Figure 6 is an explanatory diagram showing the evaluation results of the surface roughness of the test specimens after the friction and wear test. Figures 6(a) and 6(c) show electron microscope images of the test specimen surface when the lubricants of the comparative example and the example were used, respectively. Figures 6(b) and 6(d) show the evaluation results of the surface roughness along the white lines drawn in Figures 6(a) and 6(c), respectively.
[0058] As shown in Figure 6(b), when the comparative example lubricant was used, it was found that in addition to a height variation of approximately 0.5 μm due to wear marks, there were protrusions exceeding 1 μm, which are thought to be reaction products, and depressions of approximately 2-4 μm, which are thought to be corrosion marks.
[0059] On the other hand, as shown in Figure 6(d), when the lubricant of the example was used, although there was a very small height variation due to wear marks, the surface of the test piece was found to be substantially flat. From this result, it was confirmed that by using the lubricant of the example produced by the method shown in the above embodiment, the sliding surface is protected by polymer nanoparticles and the wear resistance of the sliding members can be improved.
[0060] B3. Confirmation of polymer particle generation under different conditions: As described above, we confirmed that polymer particles are generated by photocopolymerization of monomers in an ionic liquid. We also confirmed that polymer particles are generated in the ionic liquid even when the conditions for polymer particle generation are changed, such as the type of monomer used as the raw material for the polymer particles, the type of photopolymerization initiator, or the wavelength of the irradiation light.
[0061] Specifically, in addition to monomers A and B mentioned above, we prepared a monomer different from these monomers: 1H,1H,2H,2H-heptadecafluorodecyl acrylate (hereinafter also referred to as "monomer C"), represented by the following structural formula. [ka]
[0062] Next, five types of monomer mixtures (monomer mixtures 1 to 5) were prepared in the quantities shown in Table 1. As can be seen from Table 1, the amount of photopolymerization initiator in monomer mixtures 1 to 5 was approximately 3.23% by weight of the total weight of the monomer mixture. [Table 1]
[0063] Five monomer-containing ionic liquids were prepared by adding 0.1 g each of the monomer mixtures 1 to 5, prepared in this manner, dropwise to 2 g of [DEME] and [TFSI] and stirring. Two of each of the five monomer-containing ionic liquids were prepared, resulting in five monomer-containing ionic liquids in two groups.
[0064] Of the two groups of monomer-containing ionic liquids, one group was irradiated with blue light at a wavelength of 470 nm and an intensity of 3 W, while the other group was irradiated with ultraviolet light at a wavelength of 365 nm and an intensity of 3 W. The irradiation time for blue light was 10 minutes, and the irradiation time for ultraviolet light was 5 minutes. After irradiation with blue light or ultraviolet light, the resulting solid was removed and, after washing, observed with an optical microscope, as in the example described above.
[0065] Observation revealed that spherical white particles, similar to those in Figure 3, were observed in all samples. This result confirmed that polymer particles are generated regardless of the type of monomer, the type of photopolymerization initiator, or the wavelength of the irradiation light. Furthermore, the particle size of the polymer particles can be appropriately set by adjusting the irradiation time. Therefore, it was found that lubricants in which polymer nanoparticles are dispersed in an ionic liquid can be produced by changing various types of monomers, photopolymerization initiators, or the wavelength of the irradiation light.
[0066] C. Variant: The present invention is not limited to the above embodiments and examples, and can be implemented in various forms without departing from its spirit, for example, the following modifications are also possible.
[0067] C1. Variation 1: In the above embodiments and examples, two types of fluorine-containing monomers are used as raw material monomers for the polymer particles, but it is sufficient if one of the two monomers is a fluorine-containing monomer. Even in this case, the polymer particles produced are composed of a fluorine-based polymer, so the coefficient of friction of the polymer particles can be reduced. However, it is preferable to use two types of fluorine-containing monomers as raw material monomers in order to further reduce the coefficient of friction of the polymer particles produced.
[0068] Furthermore, the two monomers may be fluorine-free monomers. Even in this case, the polymer nanoparticles that penetrate between the sliding surfaces create gaps between them, suppressing tribochemical reactions that occur near the contact points of the sliding surfaces, thereby preventing corrosion and other damage from occurring on the sliding surfaces of each sliding member. However, in this case, since the generated polymer particles are no longer fluorine-based, there is a possibility that the coefficient of friction between the sliding members may increase due to an increase in the coefficient of friction of the polymer particles.
[0069] C2. Variation 2: In the above embodiments and examples, polymer particles are produced by copolymerization of two monomers. However, polymer particles can also be produced by polymerization of a single monomer, or by copolymerization of three or more monomers. However, it is preferable to produce polymer particles by copolymerization of two or more monomers because photopolymerization is easier. Furthermore, when three or more monomers are used, it becomes difficult to perform copolymerization well due to differences in the reactivity of each monomer. Therefore, it is preferable to produce polymer particles by copolymerization of two monomers.
[0070] C3. Modification 3: In the above embodiments and examples, polymer nanoparticles with nano-sized particle sizes are dispersed in the lubricant 22. However, the particle size of the polymer particles dispersed in the lubricant does not necessarily have to be nano-sized. However, the particle size of the polymer particles is set so that the polymer particles are stably dispersed in the lubricant. Whether or not the polymer particles are stably dispersed can be determined by whether or not the polymer particles have settled after the lubricant has been allowed to stand for a settling time (for example, one week or one month) determined based on actual usage conditions. [Explanation of Symbols]
[0071] 10…Monomer mixture 20…Ionic liquid 21…Monomer-containing ionic liquid 22... Lubricant AMS…Atom BLL...ball FNG…Functional group IIG... Aeon ILa, ILb... Ionic liquids LCS…Long chain part PTD,PTS…particles SFT… Surfactant TGT...Target TPC…Test piece
Claims
1. A method for manufacturing a lubricant, (a) A step of preparing a monomer mixture comprising a liquid raw material monomer containing at least one monomer and a photopolymerization initiator, (b) A step of preparing a monomer-containing ionic liquid by adding the monomer mixture prepared in step (a) to a pre-prepared ionic liquid to disperse or dissolve the monomer mixture in the ionic liquid, (c) A step of generating polymer particles by irradiating the monomer-containing ionic liquid prepared in step (b) with light of a wavelength to which the photopolymerization initiator is sensitive and which penetrates the ionic liquid, thereby polymerizing the raw material monomers. Equipped with, A method for manufacturing lubricants.
2. The method for producing a lubricant according to claim 1, wherein the raw material monomer contains two types of monomers.
3. The method for producing a lubricant according to claim 2, wherein at least one of the two monomers is a fluorine-containing monomer.
Citation Information
Patent Citations
Method of producing copolymer of -olefin and (METH)acrylic acid ester
JP2013043979A