Method for manufacturing electrical contact grease, electrical contact grease, method for manufacturing electrical components, and electrical components

By removing low molecular weight components from perfluoropolyether raw material oil and adding polytetrafluoroethylene particles, the electrical contact grease maintains stable electrical contact and sliding durability through reduced viscosity during lead-free soldering processes.

JP7954402B2Active Publication Date: 2026-11-20ALPS ALPINE CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022174779
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2026-11-20
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

The use of perfluoropolyether-based grease in lead-free soldering processes leads to increased viscosity due to vaporization, causing unstable electrical contacts, while using high molecular weight base oils results in decreased electrical contact and sliding durability at low temperatures.

Method used

A method involving the removal of low molecular weight components from perfluoropolyether raw material oil to produce a modified base oil, followed by adding a filler, specifically polytetrafluoroethylene particles, to create electrical contact grease with a weight-average molecular weight of 4,200 to 4,800, which suppresses viscosity increase during reflow processes.

Benefits of technology

The solution maintains stable electrical contact and sliding durability by preventing viscosity increase, ensuring good electrical contact characteristics even after high-temperature reflow processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954402000001
    Figure 0007954402000001
  • Figure 0007954402000002
    Figure 0007954402000002
  • Figure 0007954402000003
    Figure 0007954402000003
Patent Text Reader

Abstract

To provide a grease for electrical contact, which can stably maintain good electrical contact of the electrical contact after a reflow process, and has good characteristics such as the electrical contact at low temperature and sliding durability.SOLUTION: A production method of a grease for electrical contact comprises: a first step S11 of producing a modified base oil by heating or decompressing a raw oil composed of a polymer having a broad molecular weight distribution to evaporate low molecular weight components; and a second step S12 of producing a grease by adding a filler to the modified base oil.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing grease for electrical contacts used for lubricating sliding contacts in electronic devices, the grease for electrical contacts, a method for producing an electrical component provided with a solder portion, and the electrical component provided with a solder portion.

Background Art

[0002] Greases using silicone oil as a base oil are used for the purpose of lubricating sliding contacts such as switches, and are excellent in that they exhibit stable properties. However, in circuits where arcing occurs, there is a problem that low-molecular-weight components of silicone evaporate and oxidize to generate silica (SiO₂), which is an insulator, and this may cause contact failure. For this reason, silicone-free grease for electrical contacts that does not contain silicone is demanded.

[0003] For example, Patent Document 1 describes a lubricant (grease) for contacts obtained by mixing fluororesin fine particles such as polytetrafluoroethylene and perfluoropolyether oil. This document describes that, in order to improve the electrical conductivity and sliding durability of connectors by applying grease, a perfluoropolyether (A) having no functional group and a fluoropolyether compound (B) having at least one functional group at a terminal are used.

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0005] However, in recent years, in response to environmental concerns, there has been a shift towards lead-free soldering, and lead-free solder with a higher melting point than conventional leaded solder is now used for soldering electrical components to circuit boards. As a result, the temperature of the reflow soldering (vapor deposition soldering) process has become higher than before, and the perfluoropolyether used as the base oil of the grease in the reflow soldering process (hereinafter referred to as the reflow process as appropriate) is more likely to vaporize. When the proportion of filler increases due to the vaporization of the base oil, the viscosity of the grease increases, leading to the problem of unstable electrical contact at the contact points. On the other hand, if a base oil with a high weight-average molecular weight is used to suppress the vaporization of the base oil in the reflow process, there is a problem that the electrical contact and sliding durability at low temperatures will decrease. The present invention aims to provide an electrical contact grease that can stably maintain good electrical contact of electrical contacts after the reflow process, and that has good characteristics such as electrical contact and sliding durability at low temperatures. [Means for solving the problem]

[0006] The present invention provides the following configuration as a means for solving the above-mentioned problems. A method for producing electrical contact grease, comprising: a first step of heating or reducing the pressure of a raw material oil consisting of a polymer with a wide molecular weight distribution to vaporize low molecular weight components and produce a modified base oil; and a second step of adding a filler to the modified base oil to produce grease. By performing a second step in which fillers are added to the modified base oil after the first step in which low molecular weight components are removed from the raw material oil to create a modified base oil, it is possible to manufacture grease with less viscosity increase due to the reflow process.

[0007] The raw material oil is a perfluoropolyether with a weight-average molecular weight of 4,100 or less, and the reformed base oil may be a perfluoropolyether with a weight-average molecular weight of 4,200 to 4,800.

[0008] An electrical contact grease characterized by containing a modified base oil consisting of a perfluoropolyether having a weight-average molecular weight of 4,200 to 4,800, and a filler.

[0009] A method for manufacturing an electrical product having soldered parts, comprising: a coating step of applying an electrical contact grease, which consists of a modified base oil made of a perfluoropolyether having a weight-average molecular weight of 4,200 to 4,800 and a filler added to the modified base oil, to the electrical contact parts of an electrical component; and a reflow step of placing the electrical component in a reflow oven and heating it to a temperature above the melting point of solder.

[0010] An electrical component having a soldered portion, characterized in that an electrical contact grease consisting of a modified base oil made of a perfluoropolyether with a weight-average molecular weight of 4,200 to 4,800 and a filler added to the modified base oil is applied to the electrical contact portion.

[0011] By using perfluoropolyethers with a weight-average molecular weight of 4,100 or less as the raw material oil, an electrical contact grease with good properties such as electrical contact and sliding durability at low temperatures can be produced. Furthermore, by using perfluoropolyethers with a weight-average molecular weight of 4,200 to 4,800 as the modified base oil, vaporization of the perfluoropolyether during the reflow process can be suppressed. This prevents a decrease in the properties of the electrical contact grease due to an increase in viscosity.

[0012] In the above-mentioned method for manufacturing electrical contact grease, the above-mentioned electrical contact grease, the above-mentioned method for manufacturing electrical components, and the above-mentioned electrical components, it is preferable that the molecular weight range of the perfluoropolyether is 2,000 to 13,000, and that the weight loss rate when heated to 260°C is 10% or less. These configurations suppress the vaporization of perfluoropolyether during the reflow process, resulting in an electrical contact grease with excellent properties.

[0013] In the method for manufacturing the electrical contact grease described above and the electrical contact grease described above, the filler may be fine particles made of polytetrafluoroethylene. The dispersion and adhesion of polytetrafluoroethylene reduces the coefficient of friction at metal contacts, resulting in an electrical contact grease with excellent properties. [Effects of the Invention]

[0014] According to the present invention, by adding a filler to a modified base oil from which low molecular weight components have been removed from the raw material oil, the increase in viscosity of the grease due to the vaporization of the raw material oil during the reflow process can be suppressed. Therefore, it is possible to provide a sliding contact grease in which the lubrication function of the sliding contacts is well maintained even after the reflow process. [Brief explanation of the drawing]

[0015] [Figure 1] This is a flowchart of a method for manufacturing electrical contact grease according to an embodiment of the present invention. [Figure 2] This is a flowchart of a method for manufacturing an electrical product according to an embodiment of the present invention. [Figure 3] This is a block diagram of an electrical product according to an embodiment of the present invention. [Figure 4] This graph shows the difference between the weight-average molecular weight of the base oil and the change in the weight of the base oil due to heating. [Figure 5] This graph shows the change in the molecular weight range of the base oil due to distillation. [Figure 6] This graph shows the difference in the weight change of the base oil with and without distillation and with heating. [Figure 7A] This graph shows the stability of the switch's return force at room temperature for the grease in Example 1. [Figure 7B] This graph shows the stability of the switch's return force at 85°C for the grease in Example 1. [Figure 8A] This graph shows the stability of the switch's return force at room temperature for the grease in Reference Example 1. [Figure 8B] This is a graph showing the restoring force stability of the switch at 85°C for the grease of Reference Example 1. [Mode for Carrying Out the Invention]

[0016] <Method for Producing Grease for Electrical Contacts> An embodiment in which the present invention is implemented as a method for producing a grease for electrical contacts (hereinafter appropriately referred to as grease) will be described below. As shown in Figure 1, the method for producing the grease of the present embodiment includes a first step S11 of removing low-molecular-weight components from a raw material oil to obtain a modified base oil, and a second step S12 of adding a filler to the modified base oil to produce the grease.

[0017] The first step S11 is a step of vaporizing low-molecular-weight components from the raw material oil to obtain the modified base oil. The production method of the present embodiment is provided with the first step S11 of converting the raw material oil into the modified base oil in advance before the second step S12. By removing the low-molecular-weight components in the raw material oil in advance through the first step S11 to prepare the modified base oil, the vaporization amount of the base oil when the grease is exposed to high temperatures in the subsequent reflow step can be suppressed. This can prevent the viscosity of the grease from increasing due to the reflow step and the lubricating function of the grease from deteriorating.

[0018] The first step S11 for vaporizing the low-molecular-weight components in the raw material oil is performed by heating or reducing the pressure of the raw material oil. That is, by applying heat to the raw material oil or lowering the pressure inside the container holding the raw material oil, at least a part of the low-molecular-weight components in the raw material oil is vaporized and removed from the raw material oil. By vaporizing the low-molecular-weight components in the raw material oil, it is possible to suppress the deterioration of the lubricating function of the grease caused by exposure to high temperatures in the subsequent steps.

[0019] Low molecular weight components in the raw material oil refer to components with relatively small molecular weights in a raw material oil with a wide molecular weight distribution. The components in the raw material oil removed as low molecular weight components in the first step S11 are preferably components with a molecular weight of 1,500 or less, more preferably components with a molecular weight of 1,800 or less, and even more preferably components with a molecular weight of 2,000 or less. By removing low molecular weight components contained in the base oil, the amount of vaporization of the base oil in the reflow process can be reduced, thereby suppressing an increase in the viscosity of the grease.

[0020] The raw material oil is a base oil for grease made of a polymer with a wide molecular weight distribution, and perfluoropolyether is preferred. Perfluoropolyether is a compound having a perfluoropolyether structure in its main chain, and may have functional groups or not. Alternatively, a mixture of perfluoropolyether without functional groups and perfluoropolyether with functional groups may be used as the raw material oil.

[0021] From the viewpoint of improving the performance of the grease at low temperatures and suppressing noise generation, the weight-average molecular weight of the perfluoropolyether used as the raw material oil is preferably 4,100 or less, and more preferably 4,000 or less.

[0022] Furthermore, from the viewpoint of preventing contact failure due to silica and suppressing viscosity increase due to the reflow process S22 to produce a grease with excellent electrical contact characteristics, the modified base oil obtained in the first step is preferably a perfluoropolyether. Also from the same viewpoint, the weight-average molecular weight of the perfluoropolyether is preferably 4,200 to 4,800, more preferably 4,300 to 4,700, and even more preferably 4,400 to 4,600. The molecular weight range of the perfluoropolyether is preferably 2,000 to 13,000. In this specification, the numerical range A to B means the range from A to B.

[0023] The polydispersity of the modified base oil, i.e., the ratio of weight-average molecular weight Mw to number-average molecular weight Mn, Mw / Mn, is preferably 1.5 or less.

[0024] From the viewpoint of producing a grease with minimal viscosity increase due to the reflow process S22 and excellent electrical contact characteristics, the weight loss rate of the modified base oil when the modified base oil is heated to 260°C is preferably 15% or less, more preferably 10% or less, and even more preferably 8% or less.

[0025] From a similar viewpoint, the weight loss rate of the grease when heated to 260°C is preferably 10% or less, more preferably 8% or less, and even more preferably 6% or less.

[0026] The weight loss of the modified base oil or grease due to heating is determined by first measuring the weight of the modified base oil or grease before heating, and then measuring the weight of the modified base oil again after heating it to 260°C. The weight loss rate is defined as the percentage of the weight loss of the modified base oil or grease due to heating, with the weight of the modified base oil or grease before heating being set to 100%. In measuring the weight loss rate, the conditions for heating and cooling the modified base oil or grease are the same as those in the examples described later.

[0027] The second step S12 is a process of manufacturing grease by adding a filler to the modified base oil produced in the first step S11 described above. The filler functions as a thickener to adjust the viscosity of the grease. A preferred filler is, for example, fine particles made of polytetrafluoroethylene (PTFE). The dispersion and adhesion of these polytetrafluoroethylene particles to the electrical contact joints reduces the coefficient of friction at the joints. In this invention, fine particles refer to particles with an average particle size (D50, median diameter) of 30 to 100 nm. From the viewpoint of reducing the coefficient of friction at the joints and stabilizing the electrical connection, the average particle size of the polytetrafluoroethylene is preferably 50 to 80 nm, and more preferably 60 to 70 nm. For example, commercially available polytetrafluoroethylene can be used as the filler.

[0028] From the viewpoint of imparting an appropriate viscosity to the grease, the filler content per 100% by weight of grease is preferably 9 to 19% by weight, more preferably 11 to 17% by weight, and even more preferably 13 to 15% by weight.

[0029] The manufacturing method according to this embodiment makes it possible to produce an electrical contact grease containing a modified base oil made of a perfluoropolyether having a weight-average molecular weight of 4,200 to 4,800, and a filler.

[0030] From the viewpoint of stably maintaining good electrical contact characteristics, the viscosity of the electrical contact grease in this embodiment is preferably 20 Pa·s or less, more preferably 18 Pa·s or less, and even more preferably 15 Pa·s or less, under the conditions of 20°C and 1 rpm. Furthermore, the viscosity of the electrical contact grease is preferably 5 Pa·s or less, more preferably 4 Pa·s or less, and even more preferably 3 Pa·s or less, under the conditions of 20°C and 5 rpm.

[0031] Electrical contact grease may contain other components besides the modified base oil and filler, such as solvents and antioxidants, to the extent that it does not impair its performance.

[0032] The manufacturing method of the present invention described above makes it possible to produce an electrical contact grease that can maintain good electrical contact even after the reflow process. Furthermore, this electrical contact grease can be used to manufacture electrical components having soldered parts.

[0033] <Method for manufacturing grease for electrical contacts> Figure 2 is a flowchart of the manufacturing method of an electrical product according to this embodiment. As shown in the figure, the manufacturing method of an electrical component according to this embodiment includes an application step S21 in which electrical contact grease is applied to the electrical contact portion of the electrical component, and a reflow step S22.

[0034] The coating step S21 is a step of applying the electrical contact grease of this embodiment, which consists of a modified base oil made of a perfluoropolyether with a weight-average molecular weight of 4,200 to 4,800 and a filler added to the modified base oil, to the electrical contact area.

[0035] The reflow process S22 is a process in which electrical components are placed in a reflow oven and heated to a temperature above the melting point of the solder. The temperature during the reflow process is approximately 220-230°C for leaded solder and approximately 260-280°C for lead-free solder.

[0036] As described above, the electrical contact grease of this embodiment contains a modified base oil in which low molecular weight components in the raw material oil have been vaporized. By removing at least a portion of the low molecular weight components that are easily vaporized under high temperature conditions in advance, the vaporization of the base oil during the reflow process and the resulting increase in the viscosity of the grease can be suppressed. As a result, electrical products with good properties such as electrical contact and sliding durability of electrical contacts can be manufactured.

[0037] Figure 3 is a block diagram of an electrical component 1 manufactured by the manufacturing method described above. As shown in the figure, the electrical component 1 comprises an electrical contact portion 2 coated with grease 3 and a soldering portion 4. The grease 3 for the electrical contact consists of a modified base oil made of perfluoropolyether with a weight-average molecular weight of 4,200 to 4,800 and a filler added to the modified base oil. As a result, the electrical component 1 has good electrical contact characteristics, as the performance degradation of the grease 3 due to the vaporization of the modified base oil as a base oil and the resulting increase in viscosity, which occurs when the soldering portion 4 is soldered during the reflow process, is suppressed. [Examples]

[0038] [Consideration of base oil] To investigate the effect of the reflow process on fluorine oil, the following base oils were heated, and the change in weight associated with heating was measured. The perfluoropolyethers used as the base oil for the grease are listed below. Each perfluoropolyether is indicated using the following abbreviations as appropriate. • M03 (Fonbrin® M Lubricant, manufactured by SOLVAY) Weight average molecular weight 3,900 • M07 (Fonbrin® M Lubricant, manufactured by SOLVAY) Weight average molecular weight 5,400 • M15 (Fonbrin® M Lubricant, manufactured by SOLVAY) Weight average molecular weight 9,700 • M30 (Fonbrin® M Lubricant, manufactured by SOLVAY) Weight average molecular weight 16,000

[0039] Figure 4 is a graph showing the weight change of the base oil during heating, illustrating the change in the weight of the base oil as it heats up. In this figure, the weight before heating is set to 100%, and the change is shown as the ratio of the weight of the base oil after the components contained in the base oil have vaporized during heating to the weight before heating. As shown in the figure, among the perfluoropolyether (raw material oils) M03, M07, M15, and M30, M03, which has the smallest weight-average molecular weight, suffered the greatest loss due to vaporization when exposed to high temperatures of around 260°C. Therefore, if M03 is used as the base oil for grease as is, it is thought that the low molecular weight components in M03 will vaporize during the reflow process, increasing the viscosity of the grease and thus degrading the performance of the grease.

[0040] Therefore, M03 distillate (modified base oil) was produced by removing low molecular weight components from M03. Then, the molecular weight range and weight-average molecular weight of both M03 (raw material oil) and M03 distillate (modified base oil) were measured using a gel permeation column.

[0041] Figure 5 is a graph showing the results of measurements using a gel permeation column under the following conditions for M03 (raw material oil) and M03 distillate (modified base oil). Column: Agilent Plgel MIXED-B + MIXED-C Temperature: 23℃ Mobile phase: Asahi Clean AK-225 Sample concentration: 0.2 wt% Injection amount: 0.2ml Standard molecular weight sample: Polymethyl methacrylate (PMMA) Detector: RI (Differential Refraction)

[0042] Measurements using a gel permeation column revealed that the M03 distillate had low molecular weight components (less than 2,000) removed from M03. The molecular weights of M03 and M03 distillate, obtained by measurement using a gel permeation column, are shown below. M03 (raw material oil) Weight average molecular weight: 3,800 Molecular weight range: 500-13,000 M03 Distillate (Modified Base Oil) Weight average molecular weight: 4,500 Molecular weight range: 2,000~13,000

[0043] Figure 6 is a graph showing the weight change of the base oil with heating, illustrating the change in the weight of the raw material oil as it heats up. This figure shows the measurement results of M03 before distillation and the M03 distillate, which are perfluoropolyethers as shown in Figure 4. As shown in Figure 6, M03 experiences significant evaporation losses at around 260°C, the temperature required for the reflow process, resulting in a weight reduction of approximately 30%. Consequently, the proportion of filler in the grease increases during the reflow process, leading to an increase in the grease's viscosity. This increase in grease viscosity reduces the stability of electrical contacts during sliding.

[0044] In contrast, the M03 distillate showed almost no loss due to evaporation at around 260°C. Therefore, by using the M03 distillate as the base oil, the increase in the proportion of filler contained in the grease and the resulting increase in viscosity during the reflow process can be suppressed. By suppressing the increase in viscosity, the stability of electrical contact at electrical contacts during sliding is improved. Consequently, it is possible to manufacture a grease that can maintain stable electrical contact after the reflow process.

[0045] [Example 1] Grease was manufactured using the following base oil and filler. • Raw material oil: M03 distillate (Fonbrin® M lubricant, manufactured by SOLVAY) • Filler: PTFE

[0046] [Comparative Example 1] Grease was manufactured in the same manner as in Example 1, except that undiluted M03 was used as the raw material oil instead of the M03 distillate used in Example 1.

[0047] The grease from Example 1 and the grease from Comparative Example 1 were heated under the following conditions, and the weight loss rate due to M03 being exposed to 260°C, corresponding to the reflow process, was measured. The results were as follows. Conditions: The weight loss of the grease was measured when it reached 260°C during heating to 300°C, with a heating rate of 10°C / min. weight loss rate Example 1: 5% Comparative Example 1: 19%

[0048] The viscosity of the greases in the examples and comparative examples after exposure to 260°C was measured using a rotational viscometer DV-2T (cone type R12mm) manufactured by Eiko Seiki, and the results are shown below. Example 1 20℃ 1rpm 14Pa·s 20℃ 5rpm 3Pa·s Comparative Example 1 20℃ 1rpm 39Pa·s 20℃ 5rpm 9Pa·s

[0049] [Comparative Example 2] Instead of the M03 distillate used in Example 1, M15, which has the following characteristics, was used as the raw material oil to produce grease. M15 Weight average molecular weight: 1.2×10 4 Molecular weight range: 4,000~60,000

[0050] [Reference example 1] A silicone oil-based lubricant containing the following components and having a viscosity of 60-120 Pa·s (6,000-12,000 CP) at 20°C and 1 rpm was evaluated as Reference Example 1. Base oil: Dimethyl silicone Thickener: Silica 2-5% by weight, Extreme pressure agent

[0051] (life characteristics) When the output waveform was measured using a HiCorder with an Alps Alpine switch and a 0.1V pull-up resistor of 10Ω, the grease in Example 1 showed life characteristics equivalent to those of Reference Example 1.

[0052] The output waveform was measured using a HiCorder after 200,000 tests of CW360-CCW360° on an Alps Alpine encoder with a 5V power supply and a 5kΩ pull-up resistor. The lifespan characteristics of the grease in Example 1 were superior to those of the grease in Comparative Example 2 and equivalent to those of Reference Example 1. The grease in Comparative Example 2 generated more noise and less wear at the metal contacts than Reference Example 1. This suggests that the high proportion of fluid lubrication with fewer metal contacts in the grease in Comparative Example 2 is the cause of the noise generation. Therefore, it is believed that the lifespan characteristics of the grease in Example 1 were improved as a result of increased friction coefficient by using a low-viscosity base oil and a mixed lubrication with a high proportion of metal contacts, thereby improving contact stability.

[0053] (Operates at low temperatures) The output waveform when the switch is ON was measured using a HiCorder with an Alps Alpine switch connected with a 0.1V pull-up resistor of 10Ω. The performance of the greases in Example 1, Comparative Example 2, and Reference Example 1 was evaluated at room temperature, -20°C, and -40°C. The grease of Example 1 showed output stability equivalent to that of the grease of Reference Example 1 at room temperature, -20°C, and -40°C. The grease in Comparative Example 2 exhibited more noise and inferior output stability compared to the grease in Reference Example 1 at room temperature, -20°C, and -40°C. Thus, the fluorine-based lubricant in Comparative Example 2 had the problem of generating electrical noise during low-temperature tests and life tests. Therefore, as in Example 1, it was found that using a modified base oil from which low molecular weight components were removed from the raw material oil with a small weight-average molecular weight resulted in a grease with excellent output stability.

[0054] (Switch recovery stability) Figures 7A, 7B, 8A, and 8B show the results of torque measurements of the repulsive force when switching an Alps Alpine switch ON and OFF at room temperature and 85°C, respectively, for Example 1 and Reference Example 1. In these figures, the vertical axis represents torque, and the horizontal axis represents the switch position. In each graph, the upper lines show the measured reaction force (torque) when the switch is ON, i.e., when the electrical contacts are pushed from the OFF position (0 mm on the horizontal axis) to the ON position (approximately 1.9 mm on the horizontal axis), and the lower lines show the measured reaction force (torque) when the switch is OFF, i.e., when the electrical contacts are released from the ON position to the OFF position.

[0055] A measurement result of 0g on the lower side indicates a defective product where there is no reaction force when the switch is released, and the knob remains pressed down and does not return to its original position. One reason for the occurrence of such defective products is that the lubricating effect of the grease decreases under high-temperature conditions.

[0056] The grease of Example 1, shown in Figures 7A and 7B, did not experience a decrease in lubricant effect at 85°C and exhibited better restorative force stability than the grease of Reference Example 1 under both room temperature and 85°C conditions. Specifically, the grease of Example 1 showed similar reaction force (torque) when the switch was released in the range of 0.4 to 1.8 mm on the horizontal axis in both Figure 7A and Figure 7B, and maintained a lubricating effect at 85°C equivalent to that at room temperature. In contrast, the grease of Comparative Example 1, shown in Figures 8A and 8B, exhibited a reaction force (torque) in the range of 0.4 to 1.8 mm on the horizontal axis when the switch was released. Figure 8B showed a slightly smaller reaction force (torque) than Figure 8A, indicating that the lubrication effect at 85°C was slightly lower than at room temperature.

[0057] From the above results, it was found that the grease of the present invention according to Example 1 has lifespan characteristics equivalent to those of the grease in Reference Example 1, and that the switch return characteristics are superior to those of the grease in Reference Example 1. [Industrial applicability]

[0058] The present invention is useful for electrical contact grease and a method for manufacturing the same, as well as for electrical components having soldered parts and a method for manufacturing the same, which have excellent operating force characteristics over a wide temperature range, good contact stability even when exposed to high temperatures in a lead-free reflow soldering process, and excellent properties for electrical contacts with currents ranging from minute currents to several amperes. [Explanation of Symbols]

[0059] 1. Electrical components 2. Electrical contact points 3. Grease 4. Soldering section

Claims

1. The first step involves heating or reducing the pressure of a raw material oil consisting of a polymer with a wide molecular weight distribution to vaporize the low molecular weight components and produce a modified base oil. The process includes a second step of adding a filler to the modified base oil to produce grease, The aforementioned raw material oil is a perfluoropolyether with a weight-average molecular weight of 4,100 or less. The modified base oil is a perfluoropolyether with a weight-average molecular weight of 4,200 to 4,800. A method for producing electrical contact grease, characterized in that the molecular weight range of the perfluoropolyether constituting the modified base oil is 2,000 or more.

2. The method for producing electrical contact grease according to claim 1, wherein the molecular weight range of the perfluoropolyether constituting the modified base oil is 13,000 or less.

3. A method for manufacturing electrical contact grease according to claim 1, wherein the electrical contact grease has a weight loss rate of 10% or less when heated to 260°C.

4. The method for producing electrical contact grease according to claim 1, wherein the filler is fine particles made of polytetrafluoroethylene.

5. A modified base oil consisting of a perfluoropolyether with a weight-average molecular weight of 4,200 to 4,800, Filler and, It contains, An electrical contact grease characterized in that the molecular weight range of the perfluoropolyether is 2,000 or more.

6. The electrical contact grease according to claim 5, wherein the molecular weight range of the perfluoropolyether is 13,000 or less.

7. The electrical contact grease according to claim 5, wherein the weight loss rate when heated to 260°C is 10% or less.

8. The electrical contact grease according to claim 5, wherein the filler is made of fine particles of polytetrafluoroethylene.

9. In a method for manufacturing an electrical product having a soldered part, A coating step of applying an electrical contact grease, which consists of a modified base oil made of a perfluoropolyether with a weight-average molecular weight of 4,200 to 4,800 and a filler added to the modified base oil, to the electrical contact parts of an electrical component, The process includes a reflow step in which the electrical components are placed in a reflow oven and heated to a temperature above the melting point of the solder, A method for manufacturing electrical components, characterized in that the molecular weight range of the perfluoropolyether constituting the modified base oil is 2,000 or more.

10. The method for manufacturing an electrical component according to claim 9, wherein the molecular weight range of the perfluoropolyether is 13,000 or less.

11. The method for manufacturing an electrical component according to claim 9, wherein the electrical contact grease before the reflow process has a weight reduction rate of 10% or less when heated to 260°C.

12. In an electrical component having a soldered portion, An electrical contact grease consisting of a modified base oil made of a perfluoropolyether with a weight-average molecular weight of 4,200 to 4,800 and a filler added to the modified base oil is applied to the electrical contact area. The molecular weight range of the perfluoropolyether constituting the reformed base oil is 2,000 or more. An electrical component characterized by the following features.

13. The electrical component according to claim 12, wherein the molecular weight range of the perfluoropolyether is 13,000 or less.

14. The electrical component according to claim 12, wherein the grease for electrical contacts has a weight loss rate of 10% or less when heated to 260°C.

15. A first step of producing a modified base oil by heating or reducing the pressure of a raw material oil consisting of a polymer with a wide molecular weight distribution to vaporize low molecular weight components, The process includes a second step of adding a filler to the modified base oil to produce grease, The aforementioned raw material oil is a perfluoropolyether with a weight-average molecular weight of 4,100 or less. The molecular weight of the low molecular weight component to be vaporized is 2,000 or less. A method for producing electrical contact grease, characterized in that the modified base oil is a perfluoropolyether having a weight-average molecular weight of 4,200 to 4,800.

Citation Information

Patent Citations

  • Lubricant and use thereof

    JP2019019278A

  • Grease composition

    WO2007052522A1