Method for manufacturing a gold nanoparticle carrier

By controlling gas flow and incorporating freeze-drying, the method addresses the challenge of producing gold nanoparticle carriers in large quantities with controlled nanoparticle sizes, suitable for catalysts and adsorbents.

JP7954413B1Active Publication Date: 2026-11-20KYUSHU UNIV +1
4 Cites 0 Cited by

Patent Information

Application Number
JP2025188618
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-11-07
Publication Date
2026-11-20
Estimated Expiration
2045-11-07

AI Technical Summary

Technical Problem

Existing methods for producing gold nanoparticle carriers face limitations in increasing production quantities without coarsening the supported gold nanoparticles beyond 10 nm, hindering industrial-scale production.

Method used

Adjusting the gas flow rate during the calcination process and incorporating a freeze-drying step before calcination to control nanoparticle size, using gold/amino acid complexes and porous carriers.

Benefits of technology

Enables efficient production of gold nanoparticle carriers in large quantities with nanoparticle sizes of 10.0 nm or less, suitable for various applications including catalysts and adsorbents.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a method for efficiently producing gold nanoparticle-supported materials in large quantities. [Solution] A method for producing a gold nanoparticle carrier carrying gold nanoparticles, comprising: an impregnation step of mixing at least one complex selected from the group consisting of gold / amino acid complexes and gold / amino acid analog compound complexes with a porous carrier and water to impregnate the porous carrier with the complex; and a firing step of firing the porous carrier impregnated with the complex in a firing furnace, wherein the firing step is a step of firing while introducing gas into the firing furnace, and when the temperature inside the firing furnace rises to a predetermined temperature, the gas flow rate is reduced and the temperature is further increased to fire.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for producing a gold nanoparticle support in which gold nanoparticles are supported on a porous carrier. [Background technology]

[0002] Precious metal catalysts have long been used in various fields. Gold, a precious metal, was once considered an inert element as a catalyst. However, in the 1980s, with the ability to prepare gold as fine particles of about 5 nm or less, its high catalytic activity was discovered, and research into the application of gold nanoparticle catalysts is now actively underway.

[0003] Methods for manufacturing materials that support fine gold particles on a carrier include precipitation-precipitation, coprecipitation, precipitation-reduction, sol immobilization, solid-phase mixing, gas-phase grafting, and impregnation. Among these, the impregnation method is a simple technique in which the carrier is immersed in a gold dispersion or solution, dried, and then calcined, making it suitable for commercial production.

[0004] For example, Patent Document 1 describes a solution of at least one complex selected from the group consisting of gold / amino acid complexes and gold / amino acid analog compound complexes, the solution being prepared by adding as little water as possible to the complex, and a specific surface area of ​​30 m². 2 / g or more, 400m 2 A method for producing a gold nanoparticle carrier is disclosed, comprising the steps of: mixing a porous carrier of less than / g with at least one complex to impregnate the carrier; and immediately subjecting the carrier to a calcination treatment without drying after complex impregnation. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Patent No. 7005829 [Overview of the project] [Problems that the invention aims to solve]

[0006] However, when the amount of gold nanoparticle support produced per batch was increased using the method described in Patent Document 1, the supported gold nanoparticles became coarser, sometimes exceeding a particle size of 10 nm, making it impossible to obtain the desired gold nanoparticle support. Specifically, the upper limit of the amount produced per batch to obtain the desired gold nanoparticle support remained at around 10 g, making it difficult to increase the production amount further. Therefore, from the perspective of industrialization, a novel method for efficiently producing large quantities of gold nanoparticle support is desired.

[0007] The object of the present invention is to provide a method for producing gold nanoparticle carriers that can efficiently produce gold nanoparticle carriers in large quantities. [Means for solving the problem]

[0008] The present inventors conducted various studies on methods for producing gold nanoparticle carriers and found that the above problem could be solved by adjusting the amount of gas flowing into the calcination furnace during the calcination process after gold complex impregnation, thus completing the present invention. Furthermore, they found that the above problem could also be solved by vacuum freeze-drying the porous carrier impregnated with the gold complex before the calcination treatment, thus completing the present invention.

[0009] [1] An impregnation step of mixing at least one complex selected from the group consisting of gold / amino acid complexes and gold / amino acid analog compound complexes with a porous carrier and water to impregnate the porous carrier with the complex, A firing step in which a porous carrier impregnated with the aforementioned complex is fired in a firing furnace, A method for producing a gold nanoparticle carrier comprising gold nanoparticles, A method for producing a gold nanoparticle carrier, characterized in that the firing step is a step of firing while introducing gas into the firing furnace, wherein when the temperature inside the firing furnace rises to a predetermined temperature, the gas flow rate is reduced and the temperature is further increased to perform firing.

[0010] [2] A method for producing a gold nanoparticle carrier according to [1], characterized by comprising a freeze-drying step of freeze-drying the porous carrier impregnated with the complex before the calcination step after the impregnation step.

[0011] [3] An impregnation step of mixing at least one complex selected from the group consisting of gold / amino acid complexes and gold / amino acid analog compound complexes with a porous carrier and water to impregnate the porous carrier with the complex, A freeze-drying step in which a porous carrier impregnated with the aforementioned complex is freeze-dried, A firing process in which a porous carrier impregnated with the freeze-dried complex is fired in a firing furnace while gas is introduced into the firing furnace, A method for producing a gold nanoparticle carrier comprising gold nanoparticles.

[0012] [4] A method for producing a gold nanoparticle carrier according to [1] or [2] above, characterized in that when the temperature inside the firing furnace rises to a predetermined temperature, the gas flow rate is reduced to 10-50%. [5] A method for producing a gold nanoparticle carrier according to [1] or [4] above, characterized in that the predetermined temperature inside the firing furnace that reduces the gas flow rate is 120 to 180°C.

[0013] [6] A method for producing a gold nanoparticle carrier according to any one of [1] to [5] above, characterized in that the porous carrier is silica with a particle size of 1.0 mm or more. [7] A method for producing a gold nanoparticle carrier according to any one of [1] to [5] above, characterized in that the porous carrier is silica with a particle size of less than 1.0 mm. [8] A method for producing a gold nanoparticle carrier according to any one of [1] to [7] above, characterized in that the particle size of the gold nanoparticles supported on the gold nanoparticle carrier is 10.0 nm or less. [Effects of the Invention]

[0014] According to the present invention, gold nanoparticle carriers can be efficiently manufactured in large quantities. [Modes for carrying out the invention]

[0015] <First Invention> The method for producing a gold fine particle-supported body of the present invention is a method for producing a gold fine particle-supported body supporting gold fine particles, comprising an impregnation step of mixing at least one complex selected from the group consisting of a gold / amino acid complex and a gold / amino acid analog compound complex, a porous carrier, and water to impregnate the porous carrier with the complex, and a calcination step of calcining the porous carrier impregnated with the complex in a calcination furnace, wherein the calcination step is a step of performing calcination while flowing gas into the calcination furnace, characterized in that when the temperature inside the calcination furnace is raised to a predetermined temperature, the gas flow rate is reduced, and the temperature is further raised to perform calcination.

[0016] The gold fine particle-supported body produced by the method for producing a gold fine particle-supported body of the present invention (hereinafter referred to as the gold fine particle-supported body of the present invention) can be used in the same manner as known gold nanoparticle catalysts. For example, gold nanoparticle catalysts are known to catalyze various reactions such as decomposition of harmful components in the environment, fuel cell-related reactions (such as anode reactions), and chemical process reactions such as gas-phase epoxidation of propylene and styrene, and the gold fine particle-supported body of the present invention can be used as a catalyst for various reactions in the same manner as these known gold nanoparticle catalysts.

[0017] In addition, the gold fine particle-supported body of the present invention can be used not only for catalyst applications but also for adsorbents, mechanical materials, optical materials, electromagnetic materials, and the like. For example, gold fine particles are known to have an action of adsorbing sulfur compounds (for example, Japanese Patent No. 5170591), and the gold fine particle-supported body of the present invention can also be used as an adsorbent for sulfur compounds. For example, polysulfides such as dimethyl trisulfide and dimethyl disulfide are main constituents of the stale odor, which is a deterioration odor of sake (Journal of the Brewing Society of Japan, 101, 125-131, 2006), and the gold fine particle-supported body of the present invention can also be used for reducing the stale odor in sake as such an adsorptive remover for polysulfides.

[0018] Furthermore, the gold fine particle support of the present invention can be used not only for adsorptive removal of sulfur compounds from aqueous liquids, but also as an adsorbent for adsorptive removal of sulfur compounds from lipophilic liquids such as liquid fuels like gasoline and organic solvents, similarly to the invention described in Japanese Patent No. 5170591, for example.

[0019] In addition, the gold fine particle support of the present invention can be reused repeatedly by being calcined again after use.

[0020] Hereinafter, each step in the method for producing the gold fine particle support of the present invention will be described in detail. The method for producing the gold fine particle support of the present invention may comprise other steps before, after, or between the impregnation step and the calcination step.

[0021] [Impregnation Step] The impregnation step is a step of mixing at least one complex selected from the group consisting of a gold / amino acid complex and a gold / amino acid analog complex, a porous support, and water, to impregnate the porous support with the complex.

[0022] The method for producing the gold fine particle support of the present invention is an impregnation method that uses, as a gold precursor, a complex in which an amino acid and / or an amino acid analog is coordinated to gold. These gold / amino acid complex and gold / amino acid analog complex have good solubility in water, the preparation of the impregnation liquid is extremely simple by only dissolving the complex in a solvent such as water, the complex itself is also easy to prepare, and the complex can be produced from inexpensive raw materials. In addition, due to the high solubility in water, the amount of solvent used can be kept low, the volume of the impregnation liquid can be reduced, the amount of waste liquid can also be reduced, and mass production can be carried out at low cost. The impregnation liquid is chloride ion-free. Furthermore, since the method for producing the gold fine particle support of the present invention can use even acidic supports that are usually difficult to use, it is possible to prepare ultra-small sized gold fine particle supports using various porous supports without being restricted by the type of support.

[0023] Hereinafter, in this specification, amino acids and amino acid-like compounds may be collectively referred to as "amino acid-based compounds," and in this case, gold / amino acid complexes and gold / amino acid-like compound complexes may be referred to as "gold / amino acid-based compound complexes."

[0024] (Gold / amino acid compound complex) The type of amino acid that can be coordinated to gold is not particularly limited. Amino acids can be compounds that contain both an amino group and a carboxyl group in their molecule, and as per the general definition of amino acids, they also include imino acids, which are cyclic compounds in which a hydrogen atom of the amino group is substituted with another part of the molecule to form a secondary amine. Representative examples of these amino acids include the 20 α-amino acids that make up natural proteins, but the definition is not limited to these, and β-, γ-, and δ-amino acids are also included. Furthermore, amino acids can be D-forms, L-forms, or mixtures of both.

[0025] Specific examples of amino acids include, for instance, arginine, histidine, lysine, aspartic acid, glutamic acid, alanine, glycine, leucine, valine, isoleucine, serine, threonine, phenylalanine, tryptophan, tyrosine, cystine or cysteine, glutamine, asparagine, proline, methionine, β-alanine, γ-aminobutyric acid (4-aminobutyric acid), carnitine, γ-aminolevulinic acid, γ-aminovaleric acid, δ-aminovaleric acid (5-aminovaleric acid), ε-aminocaproic acid (6-aminocaproic acid), and others.

[0026] Amino acid analogs are not particularly limited, as long as they have a structure similar to an amino acid as defined above. Examples of amino acid analogs include compounds in which at least one amino group (e.g., all, one or two, or one) of an amino acid molecule is replaced by a sulfhydryl group; compounds in which at least one alkyl group is bonded to at least one amino group (e.g., all, one or two, or one) of an amino acid molecule (the number of carbon atoms in the alkyl group may be, for example, 1 to 5, 1 to 4, 1 to 3, 1 or 2, or 1); and compounds in which at least one carbon atom (e.g., 1 to 5, or) of the carbon atoms constituting the main chain and side chain of an amino acid molecule is replaced by a sulfhydryl group; Examples include compounds in which 1 to 3 atoms, or 1 or 2 atoms, or 1 atom) are replaced by at least one atom selected from nitrogen, oxygen, and sulfur atoms; and compounds in which at least one carbon atom (e.g., 1 to 5, 1 to 4, 1 to 3, 1 or 2, or 1) constituting the main chain and side chain of an amino acid molecule is bonded to at least one element selected from the group consisting of alkyl groups, hydroxyl groups, and halogen atoms (e.g., the number of carbon atoms in the alkyl group is 1 to 5, 1 to 4, 1 to 3, 1 or 2, or 1).

[0027] Specific examples of amino acid analogs include, for example, thiomalic acid (of aspartic acid -NH). 2 Examples include, but are not limited to, aspartic acid analogs (where the group is replaced by an -SH group), p-chlorophenylalanine (a phenylalanine analog in which the para position of the phenyl group is replaced by a chlorine atom), β-chloroalanine (an alanine analog in which the β carbon is replaced by a chlorine atom), hydroxyproline (hydroxylated proline, a component of collagen), hydroxylysine (hydroxylated lysine, a component of collagen), and sarcosine (N-methylglycine, a glycine analog in which one methyl group is bonded to the amino group of glycine).

[0028] Specific examples of methods for preparing gold / amino acid compound complexes include the methods described below. A gold / amino acid compound complex can be obtained by dissolving an amino acid compound in a basic alcoholic aqueous solvent, adding an alcoholic aqueous solvent of a gold-soluble compound, adding more alcohol to precipitate the complex, recovering it, reprecipitation with alcohol as appropriate, and then washing it. Here, examples of alcohols include lower alcohols such as ethanol, and examples of metal-soluble compounds include chloroauric acid. Further details are described in Japanese Patent No. 7005829.

[0029] (Porous carrier) The type of porous carrier is not particularly limited; any carrier capable of supporting gold nanoparticles on its surface may be used. Furthermore, according to the manufacturing method of the present invention, even acidic carriers that are difficult to use with conventional impregnation methods can be used.

[0030] Specific examples of porous carriers include, for example, silicon materials (silica, silica-alumina, aluminosilicate, etc.), carbon materials (activated carbon and various porous carbon materials, etc.), metal oxides (iron oxide, aluminum oxide, titanium oxide, cobalt oxide, zirconium oxide, cerium oxide, manganese oxide, zinc oxide, nickel oxide, magnesium oxide, tungsten oxide, etc.), clays (bentonite, activated clay, diatomaceous earth, montmorillonite, etc.), synthetic or natural polymers (various synthetic resins, polyvinylpyrrolidone, chitosan, microfibrous cellulose, tannin, agar, gelatin, etc.), carbonates (magnesium carbonate, calcium carbonate, barium carbonate, etc.), porous coordination polymers (PCP, a crystalline polymer structure composed of metal ions and organic ligands that crosslink them, also called a Metal-Organic Framework (MOF)), boron nitride, etc., with silica being particularly preferred.

[0031] The shape of the porous carrier is not particularly limited and can be any shape or form. Specifically, various shapes such as powder, granules, pellets, and honeycomb structures can be used.

[0032] The particle size of the porous carrier is not particularly limited, for example, 0.1 mm or larger. Furthermore, in the firing process of the present invention, gas is introduced into the firing furnace, so in order to suppress the scattering of the porous carrier, it is preferable that the particle size be 1.0 mm or larger, more preferably 1.5 mm or larger, and even more preferably 2.0 mm or larger. On the other hand, there is no particular upper limit, but it is about 8.0 mm. Furthermore, when freeze-drying is performed as described later, the gas flow rate can be reduced, so a thickness of less than 1.0 mm is acceptable. In this invention, the particle size of the porous carrier refers to the particle size determined by classification such as sieving.

[0033] The specific surface area of ​​a porous carrier is not particularly limited, and typically, porous carriers with a large specific surface area (for example, approximately 30 m²) are used. 2 Approximately 1g or more, especially 100m 2 It is preferable to use a quantity of approximately 3000ml or more, and there is no particular upper limit to this quantity, usually 3000ml. 2 It is approximately less than or equal to / g.

[0034] (Mixing and impregnation method) The complex, porous support, and water can be mixed in any way that ensures they are thoroughly mixed. For example, all three can be added and mixed simultaneously, but it is preferable to mix the complex and water first (dissolve the complex in water), and then add the porous support to this solution and mix. The time required for mixing is not particularly limited; for example, 3 to 30 minutes is sufficient. The mixing operation can be carried out in batches or continuously.

[0035] When mixing, it is preferable to add as little water as possible (the minimum necessary amount) in order to suppress the aggregation of gold nanoparticles. By rapidly evaporating the water during the calcination process, the aggregation of gold nanoparticles can be suppressed, and the size of the supported gold nanoparticles can be reduced.

[0036] Furthermore, when mixing, it is preferable to add the porous carrier so that the amount of gold supported in the gold nanoparticle carrier is approximately 0.1 to 5.0% by mass, and more preferably approximately 0.5 to 3.0% by mass.

[0037] [Firing process] The firing process involves firing a porous carrier impregnated with a complex in a firing furnace, and this firing process is carried out in a gas flow while gas is introduced into the firing furnace.

[0038] The firing furnace is not particularly limited as long as it can allow gas to flow in and discharge the steam generated inside the furnace. For example, a tubular container with open ends and a heating means for heating this tubular container is preferred. The firing is preferably carried out while rotating (stirring) the container, as this allows for efficient discharge of steam outside the furnace. The tubular container is preferably arranged horizontally (sideways), but may also be arranged diagonally. This firing operation can be carried out in batches or continuously.

[0039] The type of gas introduced into the firing furnace is not particularly limited; for example, oxygen-containing gases such as air may be used, as may reducing gases such as hydrogen gas or carbon monoxide gas, or inert gases such as nitrogen gas or argon gas.

[0040] The gas flow rate from the start of firing until the firing furnace reaches a predetermined temperature (gas flow rate in the initial stage of firing) is preferably about 0.01 to 1.0 L / min per gram of gold nanoparticle carrier produced, more preferably about 0.05 to 0.8 L / min, even more preferably about 0.1 to 0.6 L / min, and particularly preferably about 0.2 to 0.5 L / min. This allows water vapor generated from the porous carrier impregnated with the complex to be effectively discharged outside the firing furnace.

[0041] During firing, when the firing furnace reaches a predetermined temperature, the gas flow rate is reduced, and the temperature is further increased to the predetermined temperature for firing. The predetermined temperature at which the gas flow rate is reduced is preferably around 120 to 180°C, and more preferably around 130 to 170°C. By performing this operation, water vapor can be discharged in a short time, firing can be completed in a short time, the aggregation of gold nanoparticles can be suppressed, and a large quantity of gold nanoparticle carriers can be efficiently manufactured.

[0042] The degree to which the gas flow rate is reduced when a predetermined temperature is reached is preferably 10-50% of the gas flow rate in the initial firing stage, more preferably 20-45%, and even more preferably 25-40%.

[0043] Furthermore, even after reducing the gas flow rate of the firing furnace, the temperature is raised to the final firing temperature. This final firing temperature is not particularly limited, but is, for example, around 200 to 600°C, with 250 to 400°C being preferred. The firing time at the final firing temperature is not particularly limited, but is from a few minutes to more than ten hours, for example, from 5 minutes to 12 hours. The rate of temperature increase from the start of firing is not particularly limited, but is, for example, 2 to 15°C / min is preferred, with 2 to 10°C / min being more preferred.

[0044] Thus, in the calcination process, by calcining the porous support impregnated with the complex, the amino acid-based compounds contained in the complex disappear, and only the gold nanoparticles are supported. Therefore, there is no concern that unwanted components that would reduce performance such as catalytic activity remain on the support. The gold nanoparticles in the manufactured gold nanoparticle support have suppressed aggregation, and their particle size is 10.0 nm or less, preferably 5.0 nm or less. This particle size is determined by XRD.

[0045] [Lyophilization process] The manufacturing method of the present invention may include a freeze-drying step after the impregnation step and before the calcination step. The freeze-drying step is a step of freeze-drying the porous carrier impregnated with the complex.

[0046] Freeze-drying, also known as refrigerated drying, is a method of rapidly freezing a porous carrier impregnated with a complex, and then drying it by sublimating the water under reduced pressure in a vacuum. Because moisture can be rapidly removed by freeze-drying, aggregation of gold nanoparticles is suppressed, and this reduction in moisture content also reduces the gas flow rate into the sintering furnace during the firing process, thus preventing the scattering of the porous carrier impregnated with the complex. For example, even when using a porous carrier with a small particle size of less than 1.0 mm, it is possible to efficiently manufacture a large quantity of gold nanoparticle carriers.

[0047] <Second Invention> Another method for producing a gold nanoparticle carrier according to the present invention is characterized by comprising: an impregnation step of mixing at least one complex selected from the group consisting of gold / amino acid complexes and gold / amino acid analog compound complexes with a porous carrier and water to impregnate the porous carrier with the complex; a freeze-drying step of freeze-drying the porous carrier impregnated with the complex; and a firing step of firing the freeze-dried porous carrier impregnated with the complex in a firing furnace while introducing gas into the firing furnace. In other words, the method of the present invention, which goes through the freeze-drying step described above, is carried out without necessarily performing an operation to reduce the gas flow rate. Furthermore, as described above, when freeze-drying is performed, the gas flow rate can be reduced, and for example, the gas flow rate after the gas amount reduction in the first invention or a gas flow rate lower than that can be used from the beginning of firing. Specifically, the gas flow rate is preferably about 0.001 to 0.2 L / min per 1 g of gold nanoparticle carrier production, more preferably about 0.005 to 0.18 L / min, and even more preferably about 0.01 to 0.15 L / min.

[0048] Although the present invention has been described above with reference to embodiments, the present invention is not limited in any way to the configurations described in the embodiments described above, and includes other embodiments and modifications that can be considered within the scope of the claims. For example, the scope of the present invention also includes cases where a method for manufacturing a gold nanoparticle carrier of the present invention is constructed by combining some or all of the above embodiments and modifications. [Examples]

[0049] The following are examples of the present invention, but the technical scope of the present invention is not limited thereto.

[0050] [Conventional example] <Production of 20g of silica-supported gold nanoparticles (Au / SiO2) by impregnation method using gold / amino acid complex> Place the gold / β-alanine complex (equivalent to 200 mg of gold) in a container, add 20 mL of water to dissolve it, and then add 19.8 g of SiO2 (Fuji Silicia Chemical, CARiACT Q-15, specific surface area 200 m²). 2 The mixture was added (particle size 1.7 mm to 4.0 mm) and stirred for at least 30 minutes. Immediately thereafter, the mixture was calcined (300°C, 30 minutes) while rotating the container 20 times per minute to support the gold particles on the SiO2.

[0051] The gold particle size determined by XRD was 4.2 nm. Strictly speaking, this is the crystallite size, but since the gold nanoparticles supported by the gold nanoparticle support method of the present invention often consist of a single crystallite, the crystallite size determined by XRD can be considered as the particle size. Therefore, in this invention, the crystallite size of gold determined by XRD is expressed as the gold particle size.

[0052] After performing the above method multiple times, the particle size of the gold supported on SiO2 was consistently 10.0 nm or less. This confirmed that 20 g of silica-supported gold nanoparticles with a particle size of 10.0 nm or less can be stably produced.

[0053] [Comparative Example] <Production of 100g of silica-supported gold nanoparticles by impregnation method using gold / amino acid complexes> Place the gold / β-alanine complex (equivalent to 1000 mg of gold) in a container, add 100 mL of water and dissolve it, then add 99 g of SiO2 (Fuji Silicia Chemical, CARiACT Q-15, specific surface area 200 m²) to the mixture. 2 / g, particle size 1.7 mm to 4.0 mm) was added, and the mixture was stirred and mixed for 30 minutes or longer. Immediately thereafter, while rotating the container 35 times per minute, heating was performed in an air flow of 0.20 L / min to 0.25 L / min per 1 g of production amount, but the calcination was insufficient, the supported gold fine particles were coarsened, and the desired gold fine particle support could not be obtained. Therefore, the air flow was then stopped, heating was continued up to 300°C, and calcination (300°C, 30 minutes to 45 minutes) was performed.

[0054] When the above method was carried out multiple times, results in which the particle diameter of gold supported on SiO₂ exceeded 10.0 nm (maximum 11.1 nm) were obtained, and thus it was confirmed that the above method could not stably produce 100 g of silica-supported gold nanoparticles having a gold particle diameter of 10.0 nm or less.

[0055] [Examples] 〈Stable production of 100 g of silica-supported gold nanoparticles having a gold particle diameter of 10.0 nm or less〉

[0056] (Example 1) Confirmation of effect of reducing gas flow rate during heating A gold / β-alanine complex (equivalent to 1000 mg of gold) was placed in a container, 100 mL of water was added to dissolve the complex, and 99 g of SiO₂ (Fuji Silysia Chemical, CARiACT Q-15, specific surface area 200 m 2 / g, particle size 1.7 mm to 4.0 mm) was added, and the mixture was stirred and mixed for 30 minutes or longer (impregnation step). Immediately thereafter, while rotating the container 35 times per minute, heating was performed in an air flow of 0.25 L / min per 1 g of production amount, and after the temperature exceeded 150°C, the air flow rate was reduced to 0.08 L / min per 1 g of production amount, heating was continued up to 300°C, and calcination (300°C, 45 minutes) was performed (calcination step).

[0057] When the above method was carried out multiple times, the particle diameters of gold supported on SiO₂ were all 10.0 nm or less (maximum 3.7 nm), and thus it was confirmed that the above method can stably produce 100 g of silica-supported gold nanoparticles having a gold particle diameter of 10.0 nm or less.

[0058] (Example 2) Confirmation of the effect of freeze-drying 1 Place the gold / β-alanine complex (equivalent to 500 mg of gold) in a container, add 50 mL of water to dissolve it, and then add 49.5 g of SiO2 (Fuji Silicia Chemical, CARiACT Q-15, specific surface area 200 m²). 2 The mixture (particle size 1.7 mm to 4.0 mm) was added and stirred and mixed for at least 30 minutes (impregnation step).

[0059] After mixing the gold / β-alanine complex solution with SiO2, the mixture was freeze-dried (freeze-drying step), and then calcined in an airflow of 0.16 L / min per gram of production (300°C, 45 minutes) while rotating the container 35 times per minute (calcination step). Since the gold particle size was 4.4 nm, we were able to confirm that 50 g of silica-supported gold nanoparticles with a gold particle size of 10.0 nm or less can be stably produced using the method described above.

[0060] (Example 3) Confirmation of the effect of freeze-drying 2 Place the gold / β-alanine complex (equivalent to 1000 mg of gold) in a container, add 100 mL of water and dissolve it, then add 99 g of SiO2 (Fuji Silicia Chemical, CARiACT Q-15, specific surface area 200 m²) to the mixture. 2 The mixture was mixed with (particle size 1.7 mm to 4.0 mm) at a rate of 1 g / g and stirred for at least 30 minutes (impregnation step). After freeze-drying the mixture (freeze-drying step), it was calcined (300°C, 45 minutes) in an airflow of 0.08 L / min per gram of production while rotating the container 35 times per minute (calcination step). Since the gold particle size was 3.6 nm, we were able to confirm that 100 g of silica-supported gold nanoparticles with a gold particle size of 10.0 nm or less can be stably produced using the method described above.

[0061] (Example 4) Confirmation of the effect of freeze-drying 3 Place the gold / β-alanine complex (equivalent to 800 mg of gold) in a container, add 80 mL of water to dissolve it, and then add 79.2 g of SiO2 (Fuji Silicia Chemical, SYLOPUTE 80, specific surface area 300 m²). 2The mixture was mixed with (particle size 75 μm to 500 μm) at a rate of 1 g / g and stirred for at least 30 minutes (impregnation step). After freeze-drying the mixture (freeze-drying step), it was calcined (300°C, 30 minutes) in an airflow of 0.08 L / min per gram of production while rotating the container 35 times per minute (calcination step). Since the gold particle size was 4.1 nm, we were able to confirm that 80 g of silica-supported gold nanoparticles with a gold particle size of 10.0 nm or less can be stably produced using the method described above.

[0062] As described above, it was confirmed that the production volume of gold nanoparticle-supported materials can be increased by using the method for producing gold nanoparticle-supported materials of the present invention. [Industrial applicability]

[0063] This invention is industrially useful because it enables the efficient production of gold nanoparticle carriers.

Claims

1. An impregnation step involves mixing at least one complex selected from the group consisting of gold / amino acid complexes and gold / amino acid analog compound complexes with a porous support and water to impregnate the porous support with the complex. A firing step in which a porous carrier impregnated with the aforementioned complex is fired in a firing furnace, A method for producing a gold nanoparticle carrier comprising gold nanoparticles, The aforementioned amino acid analog is at least one selected from the group consisting of thiomalic acid, p-chlorophenylalanine, β-chloroalanine, hydroxyproline, hydroxylysine, and sarcosine. The firing process involves firing while introducing oxygen-containing gas into the firing furnace, reducing the gas flow rate when the temperature inside the firing furnace reaches a predetermined temperature of 120 to 180°C, and then further increasing the temperature to continue firing. The gas flow rate until the inside of the firing furnace reaches a predetermined temperature is set to 0.01 to 1.0 L / min per gram of the gold nanoparticle support produced. When the temperature inside the firing furnace rises to a predetermined temperature, the gas flow rate is reduced to 10-50%. Manufacturing a gold nanoparticle support containing gold nanoparticles with a particle size of 10.0 nm or less. A method for producing a gold nanoparticle carrier, characterized by the above.

2. A method for producing a gold nanoparticle carrier according to claim 1, characterized in that it comprises a freeze-drying step of freeze-drying the porous carrier impregnated with the complex before the calcination step after the impregnation step.

3. The method for producing a gold nanoparticle carrier according to claim 1, characterized in that the porous carrier is silica with a particle size of 1.0 mm or more.

Citation Information

Patent Citations

  • Catalyst, production of the catalyst and process for production vinyl acetate by using the catalyst

    JP1999244696A

  • Composite metal colloid and its production as well as catalyst for purification of gas and its production

    JP2000296339A

  • Method for producing late transition metal particle support

    JP7005829B2

  • JPP7005829B