Composition and method for electrodepositing tin-bismuth alloy onto a metal substrate

The electroplating of a tin-bismuth alloy on metal substrates addresses the electromagnetic susceptibility of composite aircraft structures by providing effective conductivity and compatibility with carbon fiber reinforced plastics, enhancing protection and performance of mechanical fasteners.

JP7954502B2Active Publication Date: 2026-11-20THE BOEING CO
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2019136663
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-07-25
Filing Date
2019-07-25
Publication Date
2026-11-20
Estimated Expiration
2039-07-25

AI Technical Summary

Technical Problem

Composite aircraft structures are susceptible to electromagnetic effects due to their inability to dissipate large currents and electromagnetic forces, necessitating measures to protect mechanical fasteners used in these structures.

Method used

A method involving the electroplating of a tin-bismuth alloy onto metal substrates, utilizing an electrolyte solution containing tin and bismuth salts, acids, and an electroplating system to provide electrical conductivity, lubricity, and galvanic compatibility with carbon fiber reinforced plastics.

Benefits of technology

The tin-bismuth alloy deposition effectively protects mechanical fasteners from electromagnetic effects while ensuring good bonding and compatibility with composite materials, enhancing their electrical conductivity and lubricity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954502000001
    Figure 0007954502000001
  • Figure 0007954502000002
    Figure 0007954502000002
  • Figure 0007954502000003
    Figure 0007954502000003
Patent Text Reader

Abstract

To provide a composition and a method for electrodepositing a tin-bismuth alloy on a metal substrate.SOLUTION: A composition and a method include: (1) a process in which a substrate and an anode are immersed in an electrolytic solution containing at least one of water, tin salt, sulfuric acid, and sulfamic acid, and in which the anode includes tin and optional bismuth; and (2) a process in which a sediment is formed on the substrate by passing an electric current through between the substrate and the anode.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to depositing materials on a substrate, and more specifically, relates to compositions and methods for activating a metal substrate, as well as compositions and methods for electrodepositing a tin-bismuth alloy onto a metal substrate.

[0002] Mechanical fasteners are widely used to join two or more components for structural assemblies. For example, mechanical fasteners are extensively used to join the structural components of aircraft fuselages.

[0003] Aircraft are subject to electromagnetic effects (EME) from various factors such as lightning strikes and precipitation static. Metallic aircraft structures are not relatively sensitive to electromagnetic effects because they are directly electrically conductive. However, aircraft structures made of composite materials (such as carbon fiber reinforced plastics) do not immediately dissipate large currents and electromagnetic forces resulting from electromagnetic effects. For this reason, when mechanical fasteners are used in composite aircraft structures, measures need to be taken to protect against electromagnetic effects.

[0004] Protection against electromagnetic effects can be provided to mechanical fasteners in the form of conductive metal surface deposits (such as metal plating). While various metal surface deposits can provide adequate electrical conductivity to impart protection against electromagnetic effects, other factors such as lubricity and galvanic compatibility with carbon fiber reinforced plastics are also considered for mechanical fasteners intended for the aerospace industry.

[0005] Tin exists in an α phase and a β phase. α-tin is gray in color and forms a powdery pest, while β-tin is white and has a tetragonal crystal structure. When tin is alloyed with bismuth at a concentration of more than 0.4 weight percent bismuth, tin begins to exist as the β phase. Tin-bismuth has been found to be promising as a metal surface deposit suitable for mechanical fasteners due to its electrical conductivity, lubricity, and galvanic compatibility with carbon fiber reinforced plastics.

[0006] Embodiments include the following:

[0007] An electrolyte solution containing water, tin salt, bismuth salt, and acid.

[0008] An electrolyte solution containing water, at least one of tin sulfate, tin chloride, and tin fluoride dissolved in water, at least one of bismuth sulfate, bismuth oxide, bismuth nitrate, bismuth chloride, and bismuth trifluoride dissolved in water, and at least one of sulfuric acid and sulfamic acid dissolved in water.

[0009] An electrolyte solution containing water, tin sulfate, bismuth sulfate, and sulfuric acid.

[0010] An electrolyte solution containing water, at least one of tin sulfate, tin chloride, and tin fluoride dissolved in water at a concentration of approximately 15 grams to approximately 200 grams per liter based on the total volume of the electrolyte solution, at least one of bismuth sulfate, bismuth oxide, bismuth nitrate, bismuth chloride, and bismuth trifluoride dissolved in water at a concentration of approximately 0.25 grams to approximately 10 grams per liter based on the total volume of the electrolyte solution, and at least one of sulfuric acid and sulfamic acid dissolved in water at a concentration of approximately 50 milliliters to approximately 150 milliliters per liter based on the total volume of the electrolyte solution.

[0011] A method for producing an electrolyte solution, (1) A step of mixing at least one of sulfuric acid and sulfamic acid with water to obtain an acidic solution. (2) A step of dissolving a tin salt in an acidic solution, (3) The process of dissolving bismuth salt in an acidic solution. Methods that include...

[0012] It is an electroplating system, A current source having a first terminal and a second terminal, A bath containing an electrolyte solution, wherein the electrolyte solution contains water, tin salt, bismuth salt, and acid. A substrate immersed in an electrolyte solution, which is electrically connected to the first terminal of a current source, and A tin-containing anode, which is immersed in an electrolyte solution and electrically connected to a second terminal of a current source, An electroplating system equipped with this system.

[0013] A method for depositing a tin-bismuth alloy onto a substrate, (1) A step of immersing the substrate and the anode containing tin in an electrolyte solution containing water, a tin salt, a bismuth salt, and an acid, (2) A method comprising the step of passing an electric current between a substrate and an anode to form a deposit on the substrate.

[0014] A method for depositing a tin-bismuth alloy onto a substrate, (1) A step to activate the substrate, (2) A step of strike plating the substrate, (3) A step of immersing the substrate and the tin-containing anode in an electrolyte solution containing water, a tin salt, a bismuth salt, and an acid, (4) A method comprising the step of passing an electric current between a substrate and an anode to form a deposit on the substrate.

[0015] Other aspects of the disclosed compositions and methods for electrodepositing tin-bismuth alloys onto metal substrates will become apparent from the following detailed description, accompanying drawings, and accompanying claims. [Brief explanation of the drawing]

[0016] [Figure 1] This is a flow diagram illustrating the method according to this disclosure for depositing a material onto a substrate. [Figure 2] This is a micrograph of a tin-bismuth alloy deposited on a titanium substrate according to the method shown in Figure 1. [Figure 3]FIG. 1 is a flow diagram illustrating one method according to the present disclosure for activating a substrate (e.g., a titanium substrate) in accordance with the method of the present disclosure. [Figure 4] FIG. 3 schematically illustrates a system for activating a substrate in accordance with the method thereof. [Figure 5] FIG. 1 is a flow diagram illustrating another method according to the present disclosure for activating a substrate (e.g., a titanium substrate) in accordance with the method of the present disclosure. [Figure 6] FIG. 5 schematically illustrates a system for activating a substrate in accordance with the method thereof. [Figure 7] FIG. 1 is a flow diagram illustrating yet another method according to the present disclosure for activating a substrate (e.g., a titanium substrate) in accordance with the method of the present disclosure. [Figure 8] FIG. 7 schematically illustrates a system for activating a substrate in accordance with the method thereof. [Figure 9] FIG. 1 schematically illustrates a system for strike-plating a substrate in accordance with the method thereof. [Figure 10] FIG. 1 is a flow diagram illustrating one method according to the present disclosure for electrodepositing a tin-bismuth alloy on a substrate in accordance with the method of the present disclosure. [Figure 11] FIG. 10 schematically illustrates an electrodeposition system for depositing a tin-bismuth alloy in accordance with the method thereof. [Figure 12] It is a flow diagram of aircraft manufacturing and operation procedures. [Figure 13] It is a block diagram of an aircraft.

[0017] Disclosed herein are compositions, systems, and methods for activating a metal substrate (e.g., a metal fastener or other member / component). Also disclosed are compositions, systems, and methods for depositing a material on a metal substrate (e.g., a metal fastener or other member / component). The compositions, systems, and methods disclosed herein can be used separately or in various combinations to achieve a desired material deposit on a substrate.

[0018] Referring to Figure 1, a method for depositing a material onto a substrate (generally indicated by 10) is disclosed. Although only three general steps are shown, it will be understood by those skilled in the art that various additional steps can be performed before, after, or between the steps presented herein, without departing from the scope of this disclosure.

[0019] The first step of Method 10 (block 12) includes pre-treating the substrate to make it suitable for receiving a material (e.g., a metal deposit, or other metallic / non-metallic material). Various pre-treatments (e.g., cleaning, degreasing, etching, etc.) can be performed. In particular, the pre-treatment step (block 12) may include activating the substrate surface (block 14). For example, in the case of a titanium substrate, the substrate surface activation step (block 14) can remove (or at least substantially reduce) a solid oxide layer known to form on the substrate.

[0020] The intermediate step (block 16) of Method 10 includes strike plating the pre-treated substrate. The strike plating step (block 16) allows for the formation of a thin metal layer on the substrate surface, thereby providing the substrate with a surface more suitable for receiving and bonding with subsequent metal deposits. In certain embodiments, the strike plating step (block 16) can form a thin nickel layer on the substrate surface.

[0021] The final step (block 18) of Method 10 includes electrodeposition onto the strike-plated substrate. The electrodeposition step (block 18) can form a metal deposit on the substrate surface. In certain embodiments, the electrodeposition step (block 18) can deposit a tin-bismuth alloy on the substrate surface.

[0022] Referring to Figure 2, the disclosed method 10 was used to deposit a thin layer of tin-bismuth alloy onto the surface of a titanium alloy (Ti-6Al-4V) substrate. This resulted in excellent bonding between the tin-bismuth alloy deposit and the underlying titanium alloy substrate.

[0023] While this disclosure primarily focuses on titanium substrates (substrates formed from titanium or titanium alloys, e.g., Ti-6Al-4V), the disclosed method 10 and each step of the disclosed method 10 (e.g., the activation step (block 14), the strike plating step (block 16), and / or the electrodeposition step (block 18)) may also be suitable for non-titanium substrates. Examples of non-titanium substrates that may benefit from this disclosure include, but are not limited to, iron alloys, copper alloys, and nickel alloys (e.g., Inconel).

[0024] activation Three activation methods are disclosed, including related compositions and systems. A metal substrate, such as a titanium substrate, can be activated using only one of the disclosed activation methods. Alternatively, a metal substrate, such as a titanium substrate, can be activated using multiple activation methods (e.g., a series of activation methods), which include one or more of the disclosed activation methods.

[0025] Referring to Figures 3 and 4, the first activation method (generally denoted as 100) may begin in block 110 (Figure 3) and include the step of preparing a bath 152 containing the activation solution 154, as shown in Figure 4. The bath 152 and the activation solution 154 may comprise the first activation system 150.

[0026] Bath 152 can be any container suitable for receiving and containing the activation solution 154. Compositionally, the material forming bath 152 must be chemically compatible with the activation solution 154. Of course, bath 152 must be of a size and shape that can accommodate the substrate 156 to be activated by the first activation system 150 within the bath.

[0027] The activation solution 154 contains water (H2O), an ammonium salt dissolved in water, and sulfuric acid (H2SO4) dissolved in water. The activation solution 154 can be maintained at atmospheric pressure (e.g., 1 atm) and at temperatures of approximately 15°C to approximately 50°C (e.g., room temperature (approximately 21°C)). However, without departing from the scope of this disclosure, higher and lower pressures, as well as higher and lower temperatures, may also be used.

[0028] The ammonium salt in activation solution 154 may have a fluorine-containing anion. In one preparation, the ammonium salt in activation solution 154 is ammonium bifluoride (NH4HF2). In another preparation, the ammonium salt in activation solution 154 is ammonium tetrafluoroborate (NH4BF4). In yet another preparation, the ammonium salt in activation solution 154 contains both ammonium bifluoride (NH4HF2) and ammonium tetrafluoroborate (NH4BF4).

[0029] The ammonium salt in the activation solution 154 may be present at concentrations ranging from approximately 10 grams to approximately 150 grams per liter, based on the total volume of the activation solution 154. In one alternative expression, the concentration of the ammonium salt is in the range of approximately 20 grams to approximately 120 grams per liter, based on the total volume of the activation solution 154. In another alternative expression, the concentration of the ammonium salt is in the range of approximately 30 grams to approximately 110 grams per liter, based on the total volume of the activation solution 154. In yet another alternative expression, the concentration of the ammonium salt is in the range of approximately 40 grams to approximately 100 grams per liter, based on the total volume of the activation solution 154. In yet another alternative expression, the concentration of the ammonium salt is in the range of approximately 50 grams to approximately 100 grams per liter, based on the total volume of the activation solution 154. In other words, the concentration of the ammonium salt is in the range of approximately 60 grams to 100 grams per liter, based on the total volume of the activation solution 154. In yet another alternative expression, the concentration of the ammonium salt is in the range of approximately 70 grams to 90 grams per liter, based on the total volume of the activation solution 154. In yet another alternative expression, the concentration of the ammonium salt is approximately 80 grams per liter, based on the total volume of the activation solution 154.

[0030] The sulfuric acid in the activation solution 154 may be present at a concentration ranging from approximately 1 volume percent to approximately 70 volume percent based on the total volume of the activation solution 154. In one alternative expression, the concentration of sulfuric acid is in the range of approximately 2 volume percent to approximately 50 volume percent based on the total volume of the activation solution 154. In another alternative expression, the concentration of sulfuric acid is in the range of approximately 3 volume percent to approximately 40 volume percent based on the total volume of the activation solution 154. In yet another alternative expression, the concentration of sulfuric acid is in the range of approximately 4 volume percent to approximately 30 volume percent based on the total volume of the activation solution 154. In yet another alternative expression, the concentration of sulfuric acid is in the range of approximately 5 volume percent to approximately 25 volume percent based on the total volume of the activation solution 154. In yet another alternative expression, the concentration of sulfuric acid is in the range of approximately 5 volume percent to approximately 15 volume percent based on the total volume of the activation solution 154. In a further alternative expression, the concentration of sulfuric acid is approximately 10 volume percent based on the total volume of the activation solution 154.

[0031] In one specific, non-limiting example, the activation solution 154 contains water, 80 grams of ammonium bifluoride (NH4HF2) per liter, and 10 volume percent sulfuric acid (H2SO4).

[0032] The activating solution 154 can be prepared in a variety of ways, without departing from the scope of this disclosure. In one specific embodiment, the disclosed method for preparing the activating solution 154 includes the following steps: (1) A step of mixing sulfuric acid (for example, 66-degree sulfuric acid from Baume) and water (for example, deionized water) to obtain an acidic solution. (2) A step of dissolving an ammonium salt (e.g., ammonium bifluoride and / or ammonium tetrafluoroborate) in an acidic solution, (3) Adding water if necessary to bring the total volume of the activation solution 154 to the required level.

[0033] In block 120 (Figure 3), the substrate 156 is immersed in the activation solution 154 (e.g., completely immersed). The substrate 156 may remain immersed in the activation solution 154 for a predetermined time, as shown in block 130 (Figure 3), before removing the substrate 156 from the activation solution 154. In the case of a titanium substrate (substrate 156), the predetermined time can be selected so that the activation solution 154 has enough time to reduce / remove the strong oxide layer on the substrate 156 without significantly damaging the oxide layer beneath the titanium / titanium alloy. In one expression, the predetermined time is approximately 5 seconds to approximately 120 seconds. In another expression, the predetermined time is approximately 10 seconds to approximately 100 seconds. In yet another expression, the predetermined time is approximately 20 seconds to approximately 40 seconds. In yet another expression, the predetermined time is approximately 30 seconds.

[0034] In block 140 (Figure 3), the substrate 156 removed from the activation solution 154 can be rinsed with a rinsing fluid. As one example, the rinsing fluid may be water, for example, deionized water.

[0035] Referring to Figures 5 and 6, the second activation method (generally indicated as 200) may begin with block 202 (Figure 5) and include the step of preparing a bath 252 containing the activation solution 254, as shown in Figure 6. The bath 252 and the activation solution 254 may comprise the second activation system 250.

[0036] The bath 252 can be any container suitable for receiving and containing the activation solution 254. Compositionally, the material forming the bath 252 must be chemically compatible with the activation solution 254. Of course, the bath 252 must be of a size and shape that can accommodate the substrate 256 to be activated by the second activation system 250 within the bath.

[0037] The activation solution 254 contains water (H2O), a fluoride salt dissolved in water, hydrofluoric acid (HF) dissolved in water, and sulfuric acid (H2SO4) dissolved in water. The activation solution 254 can be maintained at atmospheric pressure (e.g., 1 atm) and at a temperature of about 15°C to about 50°C (e.g., room temperature (about 21°C)). However, without departing from the scope of this disclosure, higher and lower pressures, as well as higher and lower temperatures, may also be used.

[0038] The fluoride salt in activation solution 254 may have alkali metal cations and / or alkaline earth metal cations. In one preparation, the fluoride salt in activation solution 254 is potassium fluoride (KF). In another preparation, the fluoride salt in activation solution 254 is lithium fluoride (LiF). In another preparation, the fluoride salt in activation solution 254 is sodium fluoride (NaF). In another preparation, the fluoride salt in activation solution 254 is rubidium fluoride (RuF). In another preparation, the fluoride salt in activation solution 254 is barium fluoride (BaF2). In another preparation, the fluoride salt in activation solution 254 is strontium fluoride (SrF2). In yet another preparation, the ammonium salts in the activated solution 254 contain at least two of the following: potassium fluoride (KF), lithium fluoride (LiF), sodium fluoride (NaF), rubidium fluoride (RuF), barium fluoride (BaF2), and strontium fluoride (SrF2).

[0039] The fluoride salt in the activation solution 254 may be present at concentrations ranging from approximately 5 grams to approximately 120 grams per liter, based on the total volume of the activation solution 254. In one alternative expression, the concentration of the fluoride salt is in the range of approximately 10 grams to approximately 100 grams per liter, based on the total volume of the activation solution 254. In another alternative expression, the concentration of the fluoride salt is in the range of approximately 15 grams to approximately 75 grams per liter, based on the total volume of the activation solution 254. In yet another alternative expression, the concentration of the fluoride salt is in the range of approximately 15 grams to approximately 50 grams per liter, based on the total volume of the activation solution 254. In yet another alternative expression, the concentration of the fluoride salt is in the range of approximately 15 grams to approximately 30 grams per liter, based on the total volume of the activation solution 254. In further alternative terms, the concentration of the fluoride salt is approximately 20 grams per liter, based on the total volume of the activated solution 254.

[0040] The hydrofluoric acid in the activation solution 254 may be present at a concentration ranging from approximately 5 milliliters per liter to approximately 250 milliliters per liter, based on the total volume of the activation solution 254. In one alternative expression, the concentration of hydrofluoric acid is in the range of approximately 10 milliliters per liter to approximately 200 milliliters per liter, based on the total volume of the activation solution 254. In another alternative expression, the concentration of hydrofluoric acid is in the range of approximately 15 milliliters per liter to approximately 150 milliliters per liter, based on the total volume of the activation solution 254. In yet another alternative expression, the concentration of hydrofluoric acid is in the range of approximately 20 milliliters per liter to approximately 150 milliliters per liter, based on the total volume of the activation solution 254. In yet another alternative expression, the concentration of hydrofluoric acid is in the range of approximately 30 milliliters per liter to approximately 100 milliliters per liter, based on the total volume of the activation solution 254. In other words, the concentration of hydrofluoric acid is in the range of approximately 40 milliliters to approximately 80 milliliters per liter, based on the total volume of the activation solution 254. In yet another alternative expression, the concentration of hydrofluoric acid is approximately 60 milliliters per liter, based on the total volume of the activation solution 254.

[0041] The sulfuric acid in the activation solution 254 may be present at a concentration ranging from approximately 1 volume percent to approximately 45 volume percent, based on the total volume of the activation solution 254. In one alternative expression, the concentration of sulfuric acid is in the range of approximately 2 volume percent to approximately 35 volume percent, based on the total volume of the activation solution 254. In another alternative expression, the concentration of sulfuric acid is in the range of approximately 2 volume percent to approximately 20 volume percent, based on the total volume of the activation solution 254. In yet another alternative expression, the concentration of sulfuric acid is in the range of approximately 3 volume percent to approximately 15 volume percent, based on the total volume of the activation solution 254. In yet another alternative expression, the concentration of sulfuric acid is in the range of approximately 3 volume percent to approximately 10 volume percent, based on the total volume of the activation solution 254. In a further alternative expression, the concentration of sulfuric acid is approximately 5 volume percent, based on the total volume of the activation solution 254.

[0042] In one specific, non-limiting example, activation solution 254 contains water, 20 grams of potassium fluoride (KF) per liter, 60 milliliters of hydrofluoric acid (HF) per liter, and 5 volume percent of sulfuric acid (H2SO4).

[0043] The activating solution 254 can be prepared in a variety of ways, without departing from the scope of this disclosure. In one specific embodiment, the disclosed method for preparing the activating solution 254 includes the following steps: (1) A step of mixing sulfuric acid (for example, 66-degree sulfuric acid from Baume) and water (for example, deionized water) to obtain a first acidic solution. (2) A step of mixing hydrofluoric acid (for example, 48% by weight in water) with the first acidic solution to obtain a second acidic solution. (3) A step of dissolving a fluoride salt (for example, potassium fluoride) in a second acidic solution, (4) Adding further water, if necessary, to bring the total volume of the activation solution 254 to the required level.

[0044] In block 204 (Figure 5), the substrate 256 is immersed in the activation solution 254 (e.g., completely immersed). The substrate 256 may remain immersed in the activation solution 254 for a predetermined time, as shown in block 206 (Figure 5), before removing the substrate 256 from the activation solution 254. In the case of a titanium substrate (substrate 256), the predetermined time can be selected so that the activation solution 254 has enough time to reduce / remove the strong oxide layer on the substrate 256 without significantly damaging the oxide layer beneath the titanium / titanium alloy. In one expression, the predetermined time is approximately 5 seconds to approximately 120 seconds. In another expression, the predetermined time is approximately 10 seconds to approximately 100 seconds. In yet another expression, the predetermined time is approximately 20 seconds to approximately 40 seconds. In yet another expression, the predetermined time is approximately 30 seconds.

[0045] In block 208 (Figure 5), the substrate 256 removed from the activation solution 254 can be rinsed with a rinsing fluid. As one example, the rinsing fluid may be water, for example, deionized water.

[0046] Referring to Figures 7 and 8, the third activation method (generally indicated as 300) may begin with block 302 (Figure 7) and include the step of preparing a bath 352 containing the activation solution 354, as shown in Figure 8. The bath 352 and the activation solution 354, together with a graphite electrode 358 and a current source 360, may comprise a third activation system 350, which can be used to carry out the anodic sulfuric acid method (third activation method 300) as described herein.

[0047] The bath 352 can be any container suitable for receiving and containing the activation solution 354. Compositionally, the material forming the bath 352 must be chemically compatible with the activation solution 354. Of course, the bath 352 must be of a size and shape that can accommodate the graphite electrode 358 and the substrate 356 to be activated by the third activation system 350.

[0048] The activation solution 354 contains water (H2O) and sulfuric acid (H2SO4) dissolved in water. The activation solution 354 can be maintained at atmospheric pressure (e.g., 1 atm) and at a temperature of approximately 15°C to approximately 50°C (e.g., room temperature (approximately 21°C)). However, without departing from the scope of this disclosure, higher and lower pressures, as well as higher and lower temperatures, may also be used.

[0049] The sulfuric acid in the activation solution 354 may be present at a concentration ranging from approximately 5 volume percent to approximately 45 volume percent, based on the total volume of the activation solution 354. One alternative expression is that the concentration of sulfuric acid is in the range of approximately 5 volume percent to approximately 35 volume percent, based on the total volume of the activation solution 354. Another alternative expression is that the concentration of sulfuric acid is in the range of approximately 5 volume percent to approximately 30 volume percent, based on the total volume of the activation solution 354. Another alternative expression is that the concentration of sulfuric acid is in the range of approximately 5 volume percent to approximately 25 volume percent, based on the total volume of the activation solution 354. Another alternative expression is that the concentration of sulfuric acid is in the range of approximately 10 volume percent to approximately 20 volume percent, based on the total volume of the activation solution 254. A further alternative expression is that the concentration of sulfuric acid is approximately 15 volume percent, based on the total volume of the activation solution 354.

[0050] In one specific, non-limiting example, the activation solution 354 contains water and 15 volume percent sulfuric acid (H2SO4).

[0051] In block 304 (Figure 7), the substrate 356 is immersed in the activation solution 354 (for example, completely immersed). The conductor 368 can electrically connect the immersed substrate 356 to the first terminal 364 of the current source 360.

[0052] In block 306 (Figure 7), the graphite electrode 358 is immersed in the activation solution 354 (for example, completely immersed). The conductor 366 can electrically connect the immersed graphite electrode 358 to the second terminal 362 of the current source 360.

[0053] In block 308 (Figure 7), the current source 360 ​​is activated so that current flows between the substrate 356 and the graphite electrode 358. The current source 360 ​​may be configured such that the substrate 356 is etched by the substrate 356 acting as an anode. In the case of a titanium substrate (substrate 356), the anodic sulfuric acid method (third activation method 300) can reduce / remove a strong oxide layer on the substrate 356 without significantly damaging the oxide layer beneath the titanium / titanium alloy.

[0054] The current-passing process (block 308) can be performed at various current densities, without departing from the scope of this disclosure. Those skilled in the art will appreciate that current density is a controllable parameter and that various factors (among others, for example, the duration of the current-passing process (block 308)) must be considered in order to select an appropriate current density. In one expression, the current passed during the current-passing process (block 308) can have a current density ranging from about 10 amperes per square foot to about 80 amperes per square foot, based on the surface area of ​​the substrate 356. In another expression, the current passed during the current-passing process (block 308) can have a current density ranging from about 20 amperes per square foot to about 60 amperes per square foot, based on the surface area of ​​the substrate 356. In other words, the current passed through during the current-passing process (block 308) can have a current density ranging from approximately 20 amperes per square foot to approximately 40 amperes per square foot, based on the surface area of ​​the substrate 356. In yet another expression, the current passed through during the current-passing process (block 308) can have a current density of approximately 30 amperes per square foot, based on the surface area of ​​the substrate 356.

[0055] The current-passing process (block 308) can be performed for a variety of durations, without departing from the scope of this disclosure. Those skilled in the art will appreciate that current density is a controllable parameter and that various factors (among others, for example, current density) must be considered in order to select an appropriate duration. In one expression, the current-passing process (block 308) can be performed for approximately 5 seconds to approximately 120 seconds. In another expression, the current-passing process (block 308) can be performed for approximately 10 seconds to approximately 100 seconds. In yet another expression, the current-passing process (block 308) can be performed for approximately 10 seconds to approximately 60 seconds. In yet another expression, the current-passing process (block 308) can be performed for approximately 15 seconds to approximately 45 seconds. In yet another expression, the current-passing process (block 308) can be performed for approximately 20 seconds to approximately 30 seconds.

[0056] In block 310 (Figure 7), the substrate 356 is disconnected from the current source 360 ​​and removed from the activation solution 354.

[0057] In block 312 (Figure 7), the substrate 356 can be rinsed with a rinsing fluid. As one example, the rinsing fluid may be water, for example, deionized water.

[0058] Strike Plating Various strike plating processes (including nickel strike plating processes: e.g., Wood bath nickel strike) are known in the art and can be used in Method 10 of Figure 1, without departing from the scope of this disclosure. However, a specific nickel strike plating method has been disclosed that resulted in excellent bonding with the substrate by subsequent plating (see Figure 2).

[0059] Referring to Figure 9, the strike plating system (generally denoted as 450) includes a bath 452, an electrolyte solution 454 received in the bath 452, a nickel anode 458 immersed in the electrolyte solution 454, and a current source 460. The current source 460 may be provided with a first terminal 462 and a second terminal 464. The nickel anode 458 may be electrically connected to the second terminal 464 by a conductor 468.

[0060] The bath 452 can be any container suitable for receiving and containing the electrolyte solution 454. Compositionally, the material forming the bath 452 must be chemically compatible with the electrolyte solution 454. Of course, the bath 452 must be of a size and shape that can accommodate the substrate 456 and the nickel anode 458 in the bath.

[0061] The electrolyte solution 454 contains water (H2O), nickel chloride (NiCl2) dissolved in water, and hydrochloric acid (HCl) dissolved in water. The electrolyte solution 454 can be maintained at atmospheric pressure (e.g., 1 atm) and at temperatures of approximately 15°C to approximately 50°C (e.g., room temperature (approximately 21°C)). However, without departing from the scope of this disclosure, higher and lower pressures, as well as higher and lower temperatures, may also be used.

[0062] Nickel chloride in electrolyte solution 454 may be present at concentrations ranging from approximately 50 grams to approximately 400 grams per liter, based on the total volume of activation solution 354. In one alternative expression, the concentration of nickel chloride is in the range of approximately 75 grams to approximately 350 grams per liter, based on the total volume of activation solution 354. In another alternative expression, the concentration of nickel chloride is in the range of approximately 100 grams to approximately 300 grams per liter, based on the total volume of activation solution 354. In yet another alternative expression, the concentration of nickel chloride is in the range of approximately 125 grams to approximately 275 grams per liter, based on the total volume of activation solution 354. In yet another alternative expression, the concentration of nickel chloride is in the range of approximately 150 grams to approximately 250 grams per liter, based on the total volume of activation solution 354. In other words, the concentration of nickel chloride is in the range of approximately 175 grams to 225 grams per liter, based on the total volume of the activated solution 354.

[0063] The hydrochloric acid in electrolyte solution 454 may be present at a concentration ranging from approximately 25 milliliters per liter to approximately 300 milliliters per liter, based on the total volume of electrolyte solution 454. In one alternative expression, the concentration of hydrochloric acid is in the range of approximately 50 milliliters per liter to approximately 250 milliliters per liter, based on the total volume of electrolyte solution 454. In another alternative expression, the concentration of hydrochloric acid is in the range of approximately 75 milliliters per liter to approximately 225 milliliters per liter, based on the total volume of electrolyte solution 454. In another alternative expression, the concentration of hydrochloric acid is in the range of approximately 100 milliliters per liter to approximately 200 milliliters per liter, based on the total volume of electrolyte solution 454. In another alternative expression, the concentration of hydrochloric acid is in the range of approximately 125 milliliters per liter to approximately 175 milliliters per liter, based on the total volume of electrolyte solution 454.

[0064] In one specific, non-limiting example, electrolyte solution 454 contains water, 200 grams of nickel chloride (NiCl2) per liter, and 150 milliliters of hydrochloric acid (HCl) per liter.

[0065] As shown in Figure 9, the substrate 456 is immersed (for example, completely immersed) in the electrolyte solution 454 in the bath 452. The substrate 456 is electrically connected to the first terminal 462 of the current source 460 by a conductor 466.

[0066] To begin strike plating, the current source 460 is activated so that current passes between the substrate 456 and the nickel anode 458, causing a deposit to form on the substrate 456. Optionally, an anode strike (where the substrate 456 acts as the anode) can be performed to etch the substrate 456 before starting the cathode strike.

[0067] Anode strikes (etching) can be performed at various current densities and durations, without departing from the scope of this disclosure. In one expression, an anode strike can be performed at current densities ranging from approximately 25 amperes per square foot to approximately 75 amperes per square foot, based on the surface area of ​​the substrate 456, for a duration of approximately 1 second to approximately 30 seconds. For example, an anode strike can be performed at a current density of approximately 120 amperes per square foot, based on the surface area of ​​the substrate 456, for approximately 10 seconds.

[0068] Cathode striking (strike plating) can be performed at various current densities and durations, without departing from the scope of this disclosure. In one expression, cathode striking can be performed at current densities ranging from approximately 80 amperes per square foot to approximately 160 amperes per square foot, based on the surface area of ​​the substrate 456, for a duration of approximately 30 seconds to approximately 10 minutes. For example, cathode striking can be performed at a current density of approximately 120 amperes per square foot, based on the surface area of ​​the substrate 456, for approximately 5 minutes.

[0069] Once the current source 460 stops operating, the substrate 456 can be disconnected from the current source 460 and removed from the electrolyte solution 454. Then, the substrate 356 can be rinsed with a rinsing fluid (e.g., deionized water).

[0070] Electroplating Various electrodeposition processes can be used in Method 10 of Figure 1, provided they do not deviate from the scope of this disclosure. However, a specific tin-bismuth electrodeposition method is disclosed, which, when used following any of the activation methods and the disclosed nickel strike plating method, resulted in excellent bonding to the substrate by subsequent plating (see Figure 2).

[0071] Referring to Figures 10 and 11, the disclosed electrodeposition method (generally indicated as 500) may begin with block 502 (Figure 10) and include the step of preparing a bath 552 containing an electrolyte solution 554, as shown in Figure 11. The bath 552 and the activating solution 554, together with an anode 558 and a current source 560, may comprise the disclosed electrodeposition system 550, which can be used to deposit a tin-bismuth alloy onto a substrate 556.

[0072] The base material 556 may be a titanium base material, such as a titanium mechanical fastener. Other metallic base materials 556 (e.g., iron base materials, copper base materials, and nickel base materials (e.g., Inconel)) can also be used by the disclosed electrodeposition method 500 and system 550, without departing from the scope of this disclosure.

[0073] The anode 558 of the disclosed electrodeposition system 550 may be a tin anode (e.g., 99.99 percent pure tin) or a tin-bismuth anode. As one general example, the anode 558 may contain about 2 to 5 weight percent bismuth, with the remainder being substantially tin. As one specific example, the anode 558 may contain about 3 weight percent bismuth, with the remainder being substantially tin.

[0074] The bath 552 can be any container suitable for receiving and containing the electrolyte solution 554. Compositionally, the material forming the bath 552 must be chemically compatible with the activation solution 554. Of course, the bath 552 must be of a size and shape that can accommodate the anode 558 and the substrate 556 in the bath.

[0075] The electrolyte solution 554 contains water (H2O), a tin salt dissolved in water, a bismuth salt dissolved in water, and an acid. The electrolyte solution 554 can be maintained at atmospheric pressure (e.g., 1 atm) and at temperatures of approximately 15°C to approximately 50°C (e.g., room temperature (approximately 21°C)). However, without departing from the scope of this disclosure, higher and lower pressures, as well as higher and lower temperatures, may also be used.

[0076] The tin salt in electrolyte solution 554 is tin(tin(II)) 2+ ) supplies ions. In one preparation, the tin salt in the electrolyte solution 554 is tin sulfate (SnSO4). In another preparation, the tin salt in the electrolyte solution 554 is tin chloride (SnCl2). In yet another preparation, the tin salt in the electrolyte solution 554 is tin fluoride (SnF2). In yet another preparation, the tin salt in the electrolyte solution 554 contains at least two of tin sulfate (SnSO4), tin chloride (SnCl2), and tin fluoride (SnF2).

[0077] The tin salt in the electrolyte solution 554 may be present at a concentration of approximately 15 grams to approximately 200 grams per liter, based on the total volume of the activated solution 554. One alternative expression is that the concentration of the tin salt is in the range of approximately 15 grams to approximately 150 grams per liter, based on the total volume of the electrolyte solution 554. Another alternative expression is that the concentration of the tin salt is in the range of approximately 15 grams to approximately 100 grams per liter, based on the total volume of the electrolyte solution 554. Another alternative expression is that the concentration of the tin salt is in the range of approximately 20 grams to approximately 100 grams per liter, based on the total volume of the electrolyte solution 554. Another alternative expression is that the concentration of the tin salt is in the range of approximately 20 grams to approximately 50 grams per liter, based on the total volume of the electrolyte solution 554. Another alternative way to express this is that the concentration of tin salt is in the range of approximately 25 grams to 35 grams per liter, based on the total volume of electrolyte solution 554.

[0078] The bismuth salt in electrolyte solution 554 is bismuth (Bi 3+ ) supplies ions. In one preparation, the bismuth salt in the electrolyte solution 554 is bismuth sulfate (Bi2(SO4)3). In another preparation, the bismuth salt in the electrolyte solution 554 is bismuth oxide (Bi2O3). In yet another preparation, the bismuth salt in the electrolyte solution 554 is bismuth nitrate (Bi(NO3)3). In yet another preparation, the bismuth salt in the electrolyte solution 554 is bismuth chloride (BiCl3). In yet another preparation, the bismuth salt in the electrolyte solution 554 is bismuth trifluoride (BiF3). In yet another preparation, the bismuth salt in the electrolyte solution 554 contains at least two of the following: bismuth sulfate (Bi2(SO4)3), bismuth oxide (Bi2O3), bismuth nitrate (Bi(NO3)3), bismuth chloride (BiCl3), and bismuth trifluoride (BiF3).

[0079] The bismuth salt in electrolyte solution 554 may be present at a concentration of approximately 0.25 grams to approximately 10 grams per liter, based on the total volume of the activated solution 554. In one alternative expression, the concentration of the bismuth salt is in the range of approximately 0.25 grams to approximately 5 grams per liter, based on the total volume of the electrolyte solution 554. In another alternative expression, the concentration of the bismuth salt is in the range of approximately 0.25 grams to approximately 2.5 grams per liter, based on the total volume of the electrolyte solution 554. In another alternative expression, the concentration of the bismuth salt is in the range of approximately 0.25 grams to approximately 1 gram per liter, based on the total volume of the electrolyte solution 554. In another alternative expression, the concentration of the bismuth salt is in the range of approximately 0.3 grams to approximately 0.8 grams per liter, based on the total volume of the electrolyte solution 554. In other words, the concentration of bismuth salt is in the range of approximately 0.4 grams to approximately 4 grams per liter, based on the total volume of electrolyte solution 554. In yet another alternative expression, the concentration of bismuth salt is in the range of approximately 0.4 grams to approximately 0.7 grams per liter, based on the total volume of electrolyte solution 554.

[0080] The acid lowers the pH of the electrolyte solution 554. In one preparation, the acid in the electrolyte solution 554 is sulfuric acid (H2SO4). In another preparation, the acid in the electrolyte solution 554 is sulfamic acid (H3NSO3). In yet another preparation, the acid in the activation solution 554 contains both sulfuric acid (H2SO4) and sulfamic acid (H3NSO3).

[0081] The acid in electrolyte solution 554 may be present at a concentration ranging from approximately 50 milliliters per liter to approximately 150 milliliters per liter, based on the total volume of electrolyte solution 554. In one alternative expression, the acid concentration is in the range of approximately 60 milliliters per liter to approximately 140 milliliters per liter, based on the total volume of electrolyte solution 554. In another alternative expression, the acid concentration is in the range of approximately 70 milliliters per liter to approximately 130 milliliters per liter, based on the total volume of electrolyte solution 554. In yet another alternative expression, the acid concentration is in the range of approximately 75 milliliters per liter to approximately 125 milliliters per liter, based on the total volume of electrolyte solution 554. In yet another alternative expression, the acid concentration is in the range of approximately 80 milliliters per liter to approximately 120 milliliters per liter, based on the total volume of electrolyte solution 554. Another alternative way to express this is that the acid concentration is in the range of approximately 90 milliliters to 110 milliliters per liter, based on the total volume of the electrolyte solution 554.

[0082] Further components may be included in the electrolyte solution 554, without departing from the scope of this disclosure. Various carriers and / or additives may be included in the electrolyte solution 554. As one specific, non-limiting example, the electrolyte solution 554 may include TIN MAC HT STARTER A (a surfactant protected by intellectual property rights, commercially available from Connecticut's MacDermid of Waterbury). As another specific, non-limiting example, the electrolyte solution 554 may include TIN MAC HT STARTER B (a methacrylic acid source protected by intellectual property rights, commercially available from Connecticut's MacDermid of Waterbury). As yet another specific, non-limiting example, the electrolyte solution 554 may include TIN MAC HT REPLENISHER (a dipropylene glycol methyl ether source and surfactant protected by intellectual property rights, commercially available from Connecticut's MacDermid of Waterbury). In one embodiment, the electrolyte solution further includes at least one of the surfactant, methacrylic acid, and dipropylene glycol methyl ether.

[0083] As one specific, non-limiting example, electrolyte solution 554 contains water, 30 grams of tin sulfate (SnSO4) per liter, 0.58 grams of bismuth sulfate (Bi2(SO4)3) per liter, 105 milliliters of sulfuric acid (H2SO4) per liter, 20 milliliters of TIN MAC HT STARTER A per liter, 5 milliliters of TIN MAC HT STARTER B per liter, and 3 milliliters of TIN MAC HT REPLENISHER per liter.

[0084] The electrolyte solution 554 can be prepared in a variety of ways, without departing from the scope of this disclosure. In one particular embodiment, the method according to this disclosure for preparing the electrolyte solution 554 is as follows: (1) A step of obtaining an acidic solution by mixing an acid (for example, sulfuric acid at 66 degrees Baume) with at least a portion of water (for example, deionized water), (2) A step of dissolving a tin salt (for example, tin sulfate (SnSO4)) in an acid solution. (3) A step of dissolving a bismuth salt (for example, bismuth sulfate (Bi2(SO4)3)) in an acidic solution, (4) Optionally, the step of adding one or more additives / carriers (e.g., TIN MAC HT STARTER A, TIN MAC HT STARTER B, and / or TIN MAC HT REPLENISHER), and (5) Adding water if necessary to bring the total volume of the electrolyte solution 554 to the required level. Includes.

[0085] In block 504 (Figure 10), the substrate 556 is immersed in the electrolyte solution 554 (for example, completely immersed). The conductor 566 can electrically connect the immersed substrate 556 to the first terminal 562 of the current source 560.

[0086] In block 506 (Figure 10), the anode 558 is immersed in the electrolyte solution 554 (for example, completely immersed). The wire 568 can electrically connect the immersed anode 558 to the second terminal 564 of the current source 560.

[0087] In block 508 (Figure 10), the current source 560 is activated so that an electric current passes between the substrate 556 and the anode 558. The electric current causes the tin-bismuth alloy to be deposited on the substrate 556.

[0088] The current-passing process (block 508) can be performed at various current densities, without departing from the scope of this disclosure. Those skilled in the art will appreciate that current density is a controllable parameter and that various factors (among others, for example, the duration of the current-passing process (block 508)) must be considered in order to select an appropriate current density. In one expression, the current passed during the current-passing process (block 508) can have a current density ranging from about 10 amperes per square foot to about 80 amperes per square foot, based on the surface area of ​​the substrate 556. In another expression, the current passed during the current-passing process (block 508) can have a current density ranging from about 10 amperes per square foot to about 50 amperes per square foot, based on the surface area of ​​the substrate 556. In other words, the current passed through during the current-passing process (block 508) can have a current density ranging from approximately 20 amperes per square foot to approximately 40 amperes per square foot, based on the surface area of ​​the substrate 556. In other words, the current passed through during the current-passing process (block 508) can have a current density ranging from approximately 15 amperes per square foot to approximately 30 amperes per square foot, based on the surface area of ​​the substrate 556. In yet another expression, the current passed through during the current-passing process (block 508) can have a current density of approximately 30 amperes per square foot, based on the surface area of ​​the substrate 556.

[0089] The current-passing process (block 508) can be performed for a variety of durations, without departing from the scope of this disclosure. Those skilled in the art will appreciate that current density is a controllable parameter and that various factors (among others, for example, current density) must be considered in order to select an appropriate duration. In one expression, the current-passing process (block 508) can be performed for approximately 5 minutes to approximately 120 minutes. In another expression, the current-passing process (block 508) can be performed for approximately 5 minutes to approximately 60 minutes. In yet another expression, the current-passing process (block 508) can be performed for approximately 10 minutes to approximately 30 minutes. In yet another expression, the current-passing process (block 508) can be performed for approximately 10 minutes to approximately 20 minutes. In yet another expression, the current-passing process (block 508) can be performed for approximately 15 minutes.

[0090] In block 510 (Figure 10), the substrate 556 is disconnected from the current source 560 and removed from the electrolyte solution 554.

[0091] In block 512 (Figure 10), the substrate 556 can be rinsed with a rinsing fluid. As one example, the rinsing fluid may be water, for example, deionized water.

[0092] Examples of this disclosure can be illustrated in reference to the aircraft manufacturing and operation method 1000 shown in Figure 12 and the aircraft 1002 shown in Figure 13. During prefabrication, the aircraft manufacturing and operation method 1000 may include the specification and design 1004 of the aircraft 1002 and the procurement of materials 1006. During manufacturing, the manufacturing of components / subassemblies 1008 and the system integration 1010 of the aircraft 1002 are carried out. The aircraft 1002 is then inspected, transported 1012 and put into operation 1014. While in operation by the customer, the aircraft 1002 is scheduled for periodic maintenance and operation 1016 (which may include deformation, reconstruction, refitting, etc.).

[0093] Each step of Operation Method 1000 may be performed or carried out by a system integrator, a third party, and / or an operator (e.g., a customer). For the purposes of this specification, a system integrator may include, but is not limited to, any number of aircraft manufacturers and subcontractors of key systems; a third party may include, but is not limited to, any number of vendors, subcontractors, and suppliers; and workers may be airlines, leasing companies, military organizations, service organizations, etc.

[0094] As shown in Figure 13, an aircraft 1002 manufactured by exemplary method 1000 may comprise a fuselage 1018 having a plurality of systems 1020 and an interior 1022. Examples of the plurality of systems 1020 may include one or more propulsion systems 1024, an electrical system 1026, a hydraulic system 1028, and one or more environmental systems 1030. One or more other systems may be included.

[0095] The compositions and methods disclosed herein can be used during one or more stages in the aircraft fabrication and operation method 1000. As one example, component or subassembly 1008, corresponding to component / subassembly fabrication, system integration 1010, and / or maintenance and operation 1016 can be fabricated or manufactured using the compositions and methods disclosed herein. As another example, the airframe 1018 may be constructed using the compositions and methods disclosed herein. Also, examples of one or more devices, examples of methods, or combinations thereof can be used during component / subassembly fabrication 1008 and / or system integration 1010, for example, by significantly accelerating the assembly of the aircraft, or by reducing the cost of the aircraft 1002 (e.g., the airframe 1018 and / or interior 1022). Similarly, examples of one or more systems, examples of methods, or combinations thereof can be used while the aircraft 1002 is in operation, for example, for maintenance and operation 1016, but are not limited thereto.

[0096] This disclosure further includes the following descriptive and non-limiting examples, which may or may not be included in the claims.

[0097] Example 1: A method for producing an electrolyte solution, To obtain an acidic solution by mixing at least one of sulfuric acid and sulfamic acid with at least a portion of water. Dissolving tin salt in an acidic solution, and Dissolving bismuth salt in an acidic solution Methods that include...

[0098] Example 2: An electrodeposition system, A current source having a first terminal and a second terminal, A bath containing the electrolyte solution in Example 1, A substrate immersed in an electrolyte solution, which is electrically connected to the first terminal of a current source, and A tin-containing anode, which is immersed in an electrolyte solution and electrically connected to a second terminal of a current source, An electroplating system equipped with this system.

[0099] Example 3: The electrodeposition system according to Example 1 or 2, wherein the anode further comprises bismuth.

[0100] Example 4: The electrodeposition system according to any one of Examples 1 to 3, wherein the anode further contains about 2 to 5 weight percent of bismuth, and the substantial remainder of the anode is tin.

[0101] Example 5: A method for depositing a tin-bismuth alloy onto a substrate, Immerse the substrate and the tin-containing anode in the electrolyte solution of Example 1, and By passing an electric current between the substrate and the anode, deposits are formed on the substrate. Methods that include...

[0102] Example 6: The method according to Example 5, wherein the anode further contains about 2 to about 5 weight percent of bismuth, and the substantial remainder of the anode is tin.

[0103] Example 7: The method according to Example 5 or 6, wherein the current has a current density of approximately 10 amperes per square foot to approximately 50 amperes per square foot, based on the surface area of ​​the substrate.

[0104] Example 8: The method according to Example 7, wherein the current has a current density of approximately 15 amperes per square foot to approximately 30 amperes per square foot, based on the surface area of ​​the substrate.

[0105] Example 9: The method according to Example 8, wherein the current has a current density of approximately 15 amperes per square foot to approximately 30 amperes per square foot, based on the surface area of ​​the substrate.

[0106] Example 10: The method according to any of Examples 5 to 9, wherein an electric current is passed through for a certain duration, the duration being approximately 5 minutes to approximately 120 minutes.

[0107] Example 11: The method according to Example 10, wherein an electric current is passed through for a certain duration, the duration being approximately 10 minutes to approximately 20 minutes.

[0108] Example 12: The method according to any one of Examples 5 to 11, further comprising activating the substrate prior to immersion and current application.

[0109] Example 13: The method according to any one of Examples 5 to 12, wherein activation comprises immersing a substrate in an activation solution for a predetermined time, and the activation solution comprises water, an ammonium salt containing a fluorine-containing anion, and sulfuric acid.

[0110] Example 14: The method according to any one of Examples 5 to 13, wherein activation comprises immersing a substrate in an activation solution for a predetermined time, and the activation solution comprises water, a fluoride salt, hydrofluoric acid, and sulfuric acid.

[0111] Example 15: The method according to any one of Examples 5 to 14, wherein activation includes subjecting the substrate to an anodic sulfuric acid process.

[0112] Example 16: The method according to any one of Examples 5 to 15, further comprising strike plating the substrate prior to immersion and current application.

[0113] Example 17: The method according to any one of Examples 5 to 16, wherein the strike plating includes nickel strike plating.

[0114] Example 18: Strike plating, Immerse the substrate and nickel anode in a strike plating electrolyte solution containing nickel chloride, hydrochloric acid, and water, and Passing an electric current between the substrate and the nickel anode. The method described in any of Examples 5 to 17, including the method described in any of Examples 5 to 17.

[0115] Example 19: Strike plating electrolyte solution, The method according to any one of Examples 5 to 18, comprising approximately 100 grams to approximately 300 grams of nickel chloride per liter based on the total volume of the strike plating electrolyte solution, and approximately 50 milliliters to approximately 250 milliliters of hydrochloric acid per liter based on the total volume of the strike plating electrolyte solution.

[0116] Example 20: An electrolyte solution, An electrolyte solution containing water, a tin salt, a bismuth salt, and at least one of sulfuric acid and sulfamic acid.

[0117] Example 21: The electrolyte solution described in Example 20, wherein the tin salt contains tin sulfate.

[0118] Example 22: The electrolyte solution according to Example 20 or 21, wherein the tin salt is present at a concentration ranging from 20 grams to 100 grams per liter, based on the total volume of the electrolyte solution.

[0119] Example 23: An electrolyte solution according to any of Examples 20 to 22, wherein the bismuth salt contains bismuth sulfate.

[0120] Example 24: An electrolyte solution according to any one of Examples 20 to 23, wherein the bismuth salt is present at a concentration ranging from 0.4 grams to 4 grams per liter, based on the total volume of the electrolyte solution.

[0121] Example 25: An electrolyte solution according to any one of Examples 20 to 24, wherein at least one of sulfuric acid and sulfamic acid is present at a concentration ranging from 75 milliliters per liter to 125 milliliters per liter, based on the total volume of the electrolyte solution.

[0122] Example 26: An electrodeposition system, A current source having a first terminal and a second terminal, Bath containing electrolyte solution in Example 20, A substrate immersed in an electrolyte solution, which is electrically connected to the first terminal of a current source, and A tin-containing anode, which is immersed in an electrolyte solution and electrically connected to a second terminal of a current source, An electroplating system equipped with this system.

[0123] Example 27: The electrodeposition system according to Example 26, wherein the anode further contains bismuth.

[0124] Although the compositions and methods disclosed herein are described in the context of aircraft, those skilled in the art will immediately understand that the disclosed compositions and methods are applicable to a variety of uses. For example, the disclosed compositions and methods can be implemented in various types of vehicles, including, for example, helicopters, passenger ships, automobiles, and marine products (ships, motors, etc.).

[0125] Various embodiments of compositions and methods disclosed for electrodepositing tin-bismuth alloys onto metal substrates have been shown and described, but those skilled in the art who have read this specification may make appropriate modifications. Such modifications are included in this application, and this application is limited only by the claims.

Claims

1. An electrolyte solution, Water and, Tin salt and, Bismuth salt and, Sulfamic acid and, It contains, An electrolyte solution in which the bismuth salt contains bismuth trifluoride, and the bismuth salt is present at a concentration in the range of 0.25 grams per liter to 2.5 grams per liter, based on the total volume of the electrolyte solution.

2. An electrolyte solution, Water and, Tin salt and, Bismuth salt and, Sulfamic acid and, It contains, An electrolyte solution in which the tin salt contains tin fluoride, and the bismuth salt is present at a concentration ranging from 0.25 grams per liter to 2.5 grams per liter, based on the total volume of the electrolyte solution.

3. The electrolyte solution according to claim 1 or 2, wherein the tin salt is present in a concentration ranging from 15 grams per liter to 200 grams per liter, based on the total volume of the electrolyte solution.

4. The electrolyte solution according to claim 1 or 2, comprising tin sulfate, bismuth sulfate, and sulfuric acid.

5. The electrolyte solution according to any one of claims 1 to 4, further comprising at least one of a surfactant, methacrylic acid, and dipropylene glycol methyl ether.

6. It is an electroplating system, A current source having a first terminal and a second terminal, A bath containing the electrolyte solution according to claim 1 or 2, A substrate immersed in the electrolyte solution, which is electrically connected to the first terminal of the current source, and A tin-containing anode, which is immersed in the electrolyte solution and electrically connected to the second terminal of the current source. An electroplating system equipped with this system.

7. The electrodeposition system according to claim 6, wherein the anode further contains 2 to 5 weight percent of bismuth, and the substantial remainder of the anode is tin.

Citation Information

Patent Citations

  • Tin and tin alloy plating bath, and electronic component formed with the plating film

    JP2009185358A

  • Multilayer radial bearing with corrosion-resistant layer

    JP2013534963A

  • Method of electroplating tin films with indium using an alkanesulfonic acid based electrolyte

    US20170321340A1