Polyolefin microporous membrane, separator for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery

A polyolefin microporous membrane with controlled indentation modulus and manufacturing parameters addresses the challenge of balancing puncture strength and shutdown temperature, enhancing battery safety and performance.

JP7954503B2Active Publication Date: 2026-11-20TORAY INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020153531
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-14
Publication Date
2026-11-20
Estimated Expiration
2040-09-14

AI Technical Summary

Technical Problem

Existing polyolefin microporous membranes face challenges in balancing puncture strength and shutdown temperature, making it difficult to enhance battery safety while maintaining high capacity and cycle characteristics.

Method used

The polyolefin microporous membrane is designed with specific indentation modulus, terminal vinyl group concentration, and manufacturing process parameters to achieve high puncture strength, low shutdown temperature, and optimal porosity, ensuring excellent rate and cycle characteristics.

Benefits of technology

The membrane provides enhanced battery safety, foreign matter resistance, and improved cycle and rate characteristics by effectively closing pores at high temperatures, thus improving battery performance and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954503000001
    Figure 0007954503000001
Patent Text Reader

Abstract

To provide a polyolefin microporous film capable of imparting safety and impact resistance to a battery, which is suitable as a separator for a non-aqueous electrolyte type secondary battery.SOLUTION: In a polyolefin microporous film, a diamond Berkovich indenter is applied vertically at a rate of 16.67 μN / sec up to 500 μN and held for 30 seconds, and the indentation modulus when unloaded at a rate of 16.67 μN / sec is 280 MPa or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a polyolefin microporous membrane, a separator for a non-aqueous electrolyte secondary battery, and a non-aqueous electrolyte secondary battery. [Background technology]

[0002] Microporous membranes are used in various fields, including filters, battery separators, and electrolytic capacitor separators. Among these, polyolefin microporous membranes, which use polyolefin as the main raw material, are widely used as battery separators because they have excellent chemical resistance, insulation properties, and mechanical strength, and are particularly safe due to their shutdown characteristics.

[0003] Secondary batteries, such as lithium-ion secondary batteries, have a high energy density and are widely used in personal computers, mobile phones, and other devices. In recent years, they have also been used as power sources for motors in electric and hybrid vehicles. In particular, large, high-capacity lithium-ion secondary batteries for automotive use require not only good rate characteristics, which represent the battery's charge and discharge performance, and cycle characteristics, which indicate the capacity retention rate during long-term use, but also high safety features that prevent smoke or fire even when the battery is exposed to high temperatures or when abnormal heat is generated inside the battery.

[0004] Patent Document 1 discloses that a battery using a separator for a non-aqueous electrolyte secondary battery in which the ratio of the displacement amount in the 10th load-unload cycle to the displacement amount in the 50th load-unload cycle, which corresponds to the degree of deformation of the separator when subjected to long-term charge-discharge cycles, is within a specific range, exhibits excellent cycle characteristics.

[0005] Patent Document 2 discloses a method for manufacturing a polyolefin microporous membrane, which allows for easy adjustment of the mechanical strength and other properties of the polyolefin microporous membrane.

[0006] Patent Document 3 discloses a polyolefin microporous membrane that has high puncture strength, low electrical resistance factor, low pore closure temperature, and low thermal shrinkage at the pore closure temperature, as well as a method for producing the same.

[0007] Patent Document 4 discloses a polyolefin laminated microporous film consisting of two or more layers that has excellent battery characteristics and safety. [Prior art documents] [Patent Documents]

[0008] [Patent Document 1] Japanese Patent Publication No. 2018-147886 [Patent Document 2] Special Publication No. 2013-530261 [Patent Document 3] Japanese Patent Publication No. 2003-020357 [Patent Document 4] Japanese Patent Publication No. 2015-208893 [Overview of the Initiative] [Problems that the invention aims to solve]

[0009] In recent years, with the increasing capacity of batteries, there is a growing demand for further improvements in the safety of polyolefin microporous membranes. To enhance battery safety, one method is to lower the shutdown temperature, which is the temperature at which the pores of the microporous membrane close. Known methods for achieving this include lowering the molecular weight and melting point of the polyolefin, which is the main component of the microporous membrane. Furthermore, from the perspective of preventing short circuits caused by battery winding or foreign matter inside the battery, there is a need to increase the puncture strength of the microporous membrane. Known methods for achieving this include controlling the orientation by increasing the stretch ratio and using ultra-high molecular weight polyolefins.

[0010] However, if stretching conditions are set to apply high stress to molecular chains during stretching in order to increase the puncture strength of the microporous membrane, the pores of the microporous membrane become less likely to melt, which raises the shutdown temperature of the separator. Therefore, it has hitherto been difficult to reduce the shutdown temperature while increasing the puncture strength of the microporous membrane.

[0011] Furthermore, when sorting wound bodies composed of separators and electrodes through a voltage withstand test (hipot test) in the battery manufacturing process, the pass rate of the voltage withstand test can be improved by enhancing the puncture strength of the separators. Since wound bodies that fail the voltage withstand test cannot be used in batteries, improving the puncture strength of the separators also leads to an increased yield during battery production.

[0012] Patent Document 1 discloses that, for a microregion of a separator, the smaller the increase rate of the compressive deformation amount when repeated deformation is applied in the film thickness direction, the more excellent battery cycle characteristics can be obtained, but the shutdown temperature is not disclosed. Although Patent Document 2 achieves high puncture strength, the shutdown temperature is not disclosed, and Patent Documents 3 and 4 are inferior in puncture strength.

[0013] In view of the above circumstances, the present invention aims to provide a polyolefin microporous membrane suitable as a separator for non-aqueous electrolyte secondary batteries, which has excellent rate characteristics and cycle characteristics of the battery, foreign matter resistance during battery winding, and excellent safety with pores easily closed when the battery is exposed to high temperatures. [MEANS FOR SOLVING THE PROBLEM]

[0014] The present inventors have found that by setting the indentation elastic modulus of the polyolefin microporous membrane to a specific value, the present inven In the battery using the microporous membrane of the present invention, the rate characteristics and cycle characteristics are improved, and the foreign matter resistant voltage withstand characteristics and battery safety are enhanced. That is, the present invention is as follows. ​(1) When a diamond Berkovich (triangular pyramidal) indenter is subjected to a load of up to 500 μN at a rate of 16.67 μN / sec in the vertical direction and held for 30 seconds, and then unloaded at a rate of 16.67 μN / sec, the indentation modulus is 280 MPa or higher, the SD temperature is less than 140°C, and the basis weight equivalent puncture strength is 0.80 N / (g / m 2 A polyolefin microporous membrane mainly composed of polyethylene resin having a density of ) or more, wherein the concentration of terminal vinyl groups per 10,000 carbon atoms of the polyolefin resin contained in the polyolefin microporous membrane is 1.9 or less, for use as a separator for a non-aqueous electrolyte secondary battery. (2) A polyolefin microporous membrane having a film thickness of 5 to 12 μm as described in (1). (3) A separator for a non-aqueous electrolyte secondary battery using the polyolefin microporous membrane described in (1) or (2) above. (4) A non-aqueous electrolyte secondary battery using the battery separator described in (3) above. [Effects of the Invention]

[0015] The present invention provides a polyolefin microporous membrane that offers excellent battery cycle characteristics, rate characteristics, and foreign matter resistance, and can provide battery safety. [Modes for carrying out the invention]

[0016] [film thickness] The film thickness of the polyolefin microporous membrane is not particularly limited, but a thinner film is preferable from the viewpoint of increasing battery capacity. Preferably, it is 16 μm or less, more preferably 12 μm or less, and even more preferably 10 μm or less. On the other hand, the lower limit of the film thickness is not particularly limited, but from the viewpoint of battery safety, it is preferably 4 μm or more, more preferably 6 μm or more. When the film thickness is within the above range, it is possible to achieve practical puncture strength and pore-closing function, and it is also suitable for the demand for further increases in battery capacity.

[0017] [Air permeability resistance] From the perspective of battery cycle characteristics, the upper limit of the air permeability resistance of the polyolefin microporous membrane is preferably less than 300 sec. / 100cc, more preferably less than 250 sec. / 100cc, and still more preferably 200 sec. / 100cc or less. On the other hand, from the perspective of battery safety, the lower limit of the air permeability resistance is preferably 80 sec. / 100cc or more, more preferably 100 sec. / 100cc or more, and still more preferably 120 sec. / 100cc or more. When the lower limit of the air permeability resistance is within the aforementioned range, abnormal large current is less likely to flow inside the battery, which contributes to improving the safety of the battery.

[0018] [Porosity] From the perspective of battery rate characteristics and cycle characteristics, the lower limit of the porosity of the polyolefin microporous membrane is preferably 30% or more, more preferably 33% or more, and still more preferably 35% or more. The upper limit of the porosity is not particularly limited, but from the perspective of battery safety, it is preferably 55% or less, more preferably 50% or less, and still more preferably 45% or less. By setting the porosity within the above range, it is possible to ensure battery safety while obtaining favorable battery rate characteristics and cycle characteristics.

[0019] [Basis Weight] From the perspective of battery safety, the lower limit of the basis weight of the polyolefin microporous membrane is preferably 4.0 g / m 2 or more, more preferably 4.5 g / m 2 or more, and still more preferably 5.0 g / m 2 or more. The upper limit of the basis weight is not particularly limited, but from the perspective of the rate characteristics and cycle characteristics of the battery, it is 7.0 g / m 2 or less.

[0020] [Basis Weight-Converted Puncture Strength] From the perspective of improving the foreign matter resistance of the microporous membrane, the basis weight-converted puncture strength of the polyolefin microporous membrane is preferably 0.70 N / (g / m 2 ) or more, more preferably 0.80 N / (g / m 2 ) or more, and still more preferably 0.85 N / (g / m 2 ) or more. The upper limit of the basis weight-converted puncture strength is not particularly limited, but is, for example, 0.90 N / (g / m 2) is less than the above range. Because the puncture strength is within the above range, when used as a separator for a secondary battery, it can have excellent resistance to electrode protrusions and foreign matter, as well as good shutdown characteristics.

[0021] [Indentation modulus] The indentation modulus of the polyolefin microporous membrane is preferably 280 MPa or higher, more preferably 350 MPa or higher, and even more preferably 400 MPa or higher. An indentation modulus of 280 MPa or higher has the effect of improving the voltage withstand characteristics of the battery, and an indentation modulus of 350 MPa or higher improves the cycle characteristics because the microporous membrane can more easily follow the expansion and contraction of the electrodes when the battery is repeatedly charged and discharged. There is no particular upper limit to the indentation modulus, but from the viewpoint of transport stability in the microporous membrane production process and the battery production process, it is 600 MPa or lower.

[0022] [Shutdown (SD) Temperature] The shutdown temperature of the polyolefin microporous membrane is preferably 140°C or lower, more preferably 139°C or lower, and even more preferably 138°C or lower, from the viewpoint of battery safety. The lower limit of the shutdown temperature is not particularly limited, but from the viewpoint of obtaining good strength for the polyolefin microporous membrane, it is 130°C or higher.

[0023] Next, the method for producing the polyolefin microporous membrane of this embodiment will be described. Note that the following description is an example of a manufacturing method and is not limited to this method. The method for producing the polyolefin microporous membrane of this embodiment preferably includes the following steps. (a) A step of preparing a polyolefin resin composition by melt-kneading a polyolefin and a plasticizer. (b) A step of extruding a polyolefin resin composition from a die to form a sheet-like polyolefin resin composition. (c) A step of stretching the sheet-like polyolefin resin composition obtained in step (b) to obtain a film. (d) A step of extracting a plasticizer from the film obtained in step (c) and drying it. (e) A step in which the microporous film obtained in step (d) is heat-fixed, stretched, and heat-relaxed in the width direction, if necessary.

[0024] (a) Preparation of polyolefin resin composition A polyolefin resin composition is prepared by melt-kneading a polyolefin resin and a plasticizer as raw materials. As a melt-kneading method, for example, a method using a twin-screw extruder as described in the specifications of Japanese Patent No. 2132327 and Japanese Patent No. 3347835 can be used.

[0025] The resin constituting the polyolefin microporous membrane mainly consists of polyethylene resin. The proportion of polyethylene resin is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 100%, when the total polyethylene microporous membrane is considered to be 100% by mass. When the proportion of polyethylene resin contained in the polyolefin microporous membrane is within the above range, practical permeability and puncture strength can be obtained.

[0026] In this embodiment, in order to set the indentation modulus and shutdown temperature of the polyolefin microporous membrane to specific values, it is necessary to use polyethylene resin with a terminal vinyl group concentration of 2.0 or more per 10,000 carbon atoms as the raw material. From the viewpoint of obtaining a good value for the indentation modulus of the microporous membrane, the lower limit of the polyethylene resin content should preferably be 20% or more, more preferably 30% or more, and even more preferably 40% or more when the entire polyolefin microporous membrane is considered as 100% by mass. Furthermore, from the viewpoint of maintaining the strength and permeability of the microporous membrane, the upper limit should be 60% or less when the entire polyolefin microporous membrane is considered as 100% by mass.

[0027] Furthermore, the polyolefin microporous membrane may contain resins other than polyethylene resin, as long as the effects of the present invention are not impaired. Examples include homopolymers, two-step polymers, copolymers, or mixtures thereof obtained by polymerizing ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, etc. In particular, the addition of polypropylene is known to improve the temperature at which the microporous membrane can maintain its shape when exposed to high temperatures (meltdown temperature).

[0028] (b) Step of forming a sheet-like polyolefin resin composition Next, the polyolefin resin composition prepared in step (a) is fed from the extruder to the die and extruded into a sheet. The extruded resin composition is brought into contact with a cooling roll to form a sheet-like polyolefin resin composition. Cooling is preferably carried out to 90°C, which is below the crystal dispersion temperature (Tcd) of the polyolefin resin, more preferably to 50°C or below, and even more preferably to 40°C or below. Cooling allows the microphase of the polyolefin that was separated by the plasticizer to be immobilized. If the cooling rate is within the above range, the degree of crystallinity is kept within an appropriate range, resulting in a sheet suitable for stretching. As a cooling method, methods such as contact with a refrigerant such as cold air or cooling water, or contact with a cooling roll can be used, but it is preferable to cool by contact with a roll cooled with a refrigerant. As a method for forming a sheet-like polyolefin resin composition, for example, the method disclosed in Japanese Patent No. 2132327 and Japanese Patent No. 3347835 can be used.

[0029] (c) A step of stretching a sheet-like polyolefin resin composition. Next, the sheet-like polyolefin resin composition is stretched. In this embodiment, the stretching method involves performing MD uniaxial stretching using a roll stretcher, followed by TD uniaxial stretching using a tenter. The lower limit of the stretching ratio when performing MD uniaxial stretching is preferably 3 times or more, more preferably 4 times or more, and even more preferably 5 times or more, from the viewpoint of film thickness and uniformity of physical properties. There is no particular upper limit for the MD uniaxial stretching ratio, but setting the stretching ratio too high will cause film breakage during stretching, so 10 times or less is preferable.

[0030] When performing uniaxial stretching of polyolefins (MD), the stretching temperature is preferably within the range of the dispersion temperature (Tcd) of the polyolefin and below its melting point. For example, in the case of polyethylene resin, it is 80 to 130°C, and more preferably 100 to 125°C. After stretching, the material is cooled to below these temperatures. The melting point of the polyolefin refers to the melting point of the polyolefin in the sheet-like polyolefin resin composition. When the stretching temperature is below the melting point of the polyolefin, the melting of the polyolefin in the sheet-like polyolefin resin composition is suppressed, and the molecular chains can be efficiently oriented by stretching. Furthermore, when the stretching temperature is above the dispersion temperature (Tcd) of the polyolefin, the polyolefin in the sheet-like polyolefin resin composition is sufficiently softened, and the stretching tension can be reduced, resulting in good film-forming properties, suppression of film breakage during stretching, and enabling stretching at high magnification.

[0031] After MD uniaxial stretching, the material is guided to a tenter and then TD uniaxial stretching is performed. The stretching ratio at this time is preferably 5 times or more, more preferably 6 times or more, and even more preferably 7 times or more. From the viewpoint of making the tensile strength of the microporous film isotropic, it is necessary to set the stretching ratio higher than the total stretching ratio of the MD uniaxial stretching described above. The stretching temperature when performing TD uniaxial stretching after MD uniaxial stretching is preferably within the range of the crystalline dispersion temperature (Tcd) of the polyolefin and below the melting point of the polyolefin. For example, in the case of polyethylene resin, it is 100 to 135°C, more preferably 110 to 130°C, and it is necessary to set the stretching temperature higher than that of the MD uniaxial stretching described above.

[0032] (d) Steps to extract and dry the plasticizer. A microporous membrane is obtained by extracting and removing the plasticizer from the polyolefin resin composition film obtained in step (c). The plasticizer is removed by washing with a washing solvent. Since the polyolefin phase is phase-separated from the plasticizer phase, when the plasticizer is removed, a porous membrane is obtained consisting of fibrils that form a fine three-dimensional network structure and has irregularly interconnected pores (voids) in three dimensions. The washing solvent and the method of removing the plasticizer using it are well known, so their explanation is omitted. For example, the methods disclosed in Japanese Patent No. 2132327 and Japanese Patent Publication No. 2002-256099 can be used.

[0033] Next, the microporous film from which the plasticizer has been removed is dried by heat drying or air drying. The drying temperature is preferably below the crystalline dispersion temperature (Tcd) of the polyolefin, and is particularly preferably 5°C or more lower than Tcd. Drying is preferably carried out until the residual washing solvent is 3% by mass or less, and more preferably until it is 1% by mass or less, with the microporous film being 100% by mass (dry weight). When the residual washing solvent is within the above range, the porosity of the polyolefin microporous film is maintained, and deterioration of permeability is suppressed.

[0034] (e) Process of heat setting, stretching, and heat relaxation. If necessary, the microporous film may be heat-fixed, stretched in the width direction, and heat-relaxed after drying. By performing heat-fixing and heat-relaxing treatments, the crystals are stabilized and the lamellar layer is made uniform, making it possible to produce a microporous film with excellent strength and thermal shrinkage rate.

[0035] The heat-fixing temperature is set within a temperature range from above the crystal dispersion temperature of the polyolefin microporous film to below its melting point, and can be achieved by a tenter, roll, or rolling method.

[0036] The stretching and thermal relaxation temperatures should be within a temperature range from above the crystal dispersion temperature of the polyolefin microporous film to below its melting point. The stretching ratio should preferably be 1 to 2 times, and the subsequent relaxation ratio should preferably be 1% to 30%, and more preferably 1% to 20% from the viewpoint of thermal shrinkage ratio and the planarity of the microporous film. If the relaxation ratio is higher than 20%, the microporous film will sag in the width direction, which can cause interference with the equipment and lead to film rupture. [Examples]

[0037] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these examples.

[0038] [Terminal vinyl group concentration] The concentration of terminal vinyl groups in polyethylene resin contained in a polyolefin microporous membrane can be determined by infrared spectroscopy. Specifically, a Fourier transform infrared spectrophotometer (model number: FREEXACT-II, manufactured by Horiba, Ltd.) can be used to measure the 910 cm² of the microporous membrane. -1 By measuring the absorbance of the absorption peak at [A=log(I0 / I) (where A represents absorbance, I0 represents the transmitted light intensity of the blank cell, and I represents the transmitted light intensity of the sample cell)], the number of terminal vinyl groups per 10,000 carbon atoms in the polyolefin resin (copies / 10,000C) can be calculated using the following formula.

[0039] Formula: End vinyl group concentration (number / 10,000C) = (11.4 × absorbance A) / (density of polyethylene (g / cm³)) 3 ) × Sample thickness (mm)] [film thickness] A 50mm x 50mm sample was cut from the microporous membrane, and the film thickness at five points within that area was measured using a contact thickness gauge (Mitutoyo Lightmatic, contact pressure 0.01N, 10.5mmφ probe). The average value was calculated and determined as the film thickness of the microporous membrane.

[0040] [Air permeability resistance] Ten 50mm x 50mm samples were cut from the microporous membrane, and the air permeability resistance (sec / 100cm) was measured at the center of each sample in accordance with JIS P-8117:2009 using an air permeability resistance meter (EGO-1T, manufactured by Asahi Seiko Co., Ltd.). 3 The following measurements were taken: The measurement point was set to a single point in the center of the sample, and the measured value was taken as the air permeability resistance of the sample. The same measurement was performed on 10 test pieces taken from arbitrary positions, and the average of the measured values ​​was taken as the air permeability resistance (sec / 100ml) of the microporous membrane.

[0041] [Porosity] A polyolefin microporous membrane was cut to a size of 50 mm x 50 mm, and its volume (mm³) 3 Calculate the ) and weight (g), and then compare them with the membrane density (g / cm³). 3 The calculation was performed using the following formula. Formula: Porosity = ((Volume - Weight / Membrane Density) / Volume) × 100 Here, the film density was assumed to be 0.99. The previously measured thickness [film thickness] was used to calculate the volume.

[0042] [Inspector] The polyolefin microporous membrane was cut into 50mm x 50mm pieces, its weight was determined, and the calculation was performed using the following formula. Formula: Basis = Weight / 0.050 / 0.050 [Piercing strength] Five 50mm x 50mm samples were cut from the microporous membrane. The maximum load L1 (N) was measured when the microporous membrane was punctured at a speed of 2mm / second using a 1mm diameter needle with a spherical tip (radius of curvature R: 0.5mm). The puncture strength per unit thickness was then determined by L1 / T1 (N / μm).

[0043] [Puncture strength equivalent to base weight] Using the aforementioned weight and puncture strength, the weight-equivalent puncture strength was calculated from the following formula.

[0044] Formula: Puncture strength equivalent to base weight = Puncture strength / Base weight [Indentation modulus] The indentation modulus of a microporous membrane, cut to a width of approximately 30-40 mm and a length of approximately 150 mm, was measured using an Anton Paar UNHT3 indenter. The microporous membrane was fixed to a mirror-finished stainless steel base with a radius of curvature of 300 mm, ensuring that no wrinkles formed. Next, a diamond Berkovich (triangular pyramidal) indenter was applied to the fixed microporous membrane in the vertical direction at a speed of 16.67 μN / sec up to 500 μN, held for 30 seconds, and then unloaded at a speed of 16.67 μN / sec to measure the indentation modulus. During this process, the indentation modulus was measured at a total of 25 points: 5 points at 100 μm intervals in the MD direction and 5 points at 50 μm intervals in the TD direction. The average value of the 21 points obtained by excluding the top and bottom two points was taken as the indentation modulus of the microporous membrane.

[0045] [Shutdown (SD) Temperature] The shutdown temperature of the microporous membrane was measured by the method disclosed in International Publication No. 2007 / 052663. According to this method, a polyolefin microporous membrane was exposed to a 30°C atmosphere and heated at a rate of 5°C / min, during which the membrane's air permeability was measured. The air permeability of the microporous membrane was initially 100,000 seconds / 100cm. 3 The temperature exceeding a certain threshold was defined as the shutdown temperature of the microporous membrane. The air permeability resistance of the microporous membrane was measured using an air permeability meter (EGO-1T, manufactured by Asahi Seiko Co., Ltd.) in accordance with JIS P8117:2009.

[0046] <Creation of cylindrical batteries for evaluation> I created a cylindrical battery following the steps below.

[0047] <Fabrication of the positive electrode> A slurry was prepared by dispersing 92.2% by mass of lithium cobalt composite oxide (LiCoO2) as the active material, 2.3% by mass each of flake graphite and acetylene black as conductive agents, and 3.2% by mass of polyvinylidene fluoride (PVDF) as a binder in N-methylpyrrolidone (NMP). This slurry was then applied at an active material coating rate of 250 g / m². 2 Active material bulk density: 3.00 g / cm³ 3Next, a 20 μm thick aluminum foil, which would serve as the positive electrode current collector, was coated with a die coater on one side. It was then dried at 130°C for 3 minutes, compressed and molded using a roll press, and then cut into strips approximately 57 mm wide.

[0048] <Fabrication of the negative electrode> A slurry was prepared by dispersing 96.9% by mass of artificial graphite as the active material and 1.4% by mass of ammonium salt of carboxymethylcellulose and 1.7% by mass of styrene-butadiene copolymer latex as binders in purified water. This slurry was then applied at an active material coating rate of 106 g / m². 2 , active material bulk density 1.55g / cm 3 With this high packing density, the material was applied to one side of a 12 μm thick copper foil, which would serve as the negative electrode current collector, using a die coater. It was then dried at 120°C for 3 minutes, compressed and molded using a roll press, and then cut into strips approximately 58 mm wide.

[0049] <Preparation of non-aqueous electrolyte> A solution was prepared by dissolving LiPF6 as a solute in a mixed solvent of ethylene carbonate / ethyl methyl carbonate = 1 / 2 (by volume) to a concentration of 1.0 mol / L.

[0050] <Separator> The polyolefin microporous membranes obtained in the examples and comparative examples were slit into strips 60 mm wide.

[0051] <Battery Assembly> A laminate of electrode plates was fabricated by stacking a strip-shaped negative electrode, a separator, a strip-shaped positive electrode, and a separator in that order, and winding them multiple times in a spiral shape with a winding tension of 250 gf. This laminate of electrode plates was placed in a stainless steel container with an outer diameter of 18 mm and a height of 65 mm. An aluminum tab leading from the positive electrode current collector was welded to the container lid terminal, and a nickel tab leading from the negative electrode current collector was welded to the container wall. After drying at 80°C under vacuum for 12 hours, the above-mentioned non-aqueous electrolyte was injected into the container in an argon box, and the container was sealed to create a cylindrical battery.

[0052] [Battery withstand voltage test] In the aforementioned process of creating evaluation cylindrical batteries, 10 batteries were prepared before electrolyte injection. A voltage withstand test was performed using the IMP-1090 manufactured by Japan Technart Co., Ltd. Batteries that experienced even one short circuit were rated as "fail," while those that did not experience a short circuit were rated as "excellent."

[0053] [Rate Characteristics] The cylindrical evaluation battery prepared as described above was charged with a constant current of 1.0C until the battery voltage reached 4.2V, then charged with a constant voltage of 0.05C until the battery voltage reached 4.2V, and then discharged (constant current discharge) with a current of 0.2C until the battery voltage reached 3.0V, and the discharge capacity was measured. Subsequently, the battery was charged again to 4.2V using the procedure described above, and then discharged (constant current discharge) with a current of 5C until the battery voltage reached 3.0V, and the discharge capacity was measured. The discharge capacity ratio was calculated using the following formula, and batteries with a discharge capacity ratio of 90% or more were evaluated as excellent, those with a ratio of 80% or more but less than 90% were evaluated as good, and those with a ratio less than 80% were evaluated as poor. Formula: Discharge capacity ratio = Discharge capacity at 5C × 100 / Discharge capacity at 0.2C [Cycle Characteristics] The cylindrical evaluation battery prepared as described above was charged with a constant current of 1.0C until the battery voltage reached 4.2V, and then charged with a constant voltage until the current was 0.05C at 4.2V. After a 10-minute pause, the battery was discharged with a constant current of 1.0C until the battery voltage reached 3.0V, followed by a 10-minute pause. This charge-discharge cycle was considered one cycle, and this was repeated 500 times. The remaining capacity ratio was calculated using the following formula, and batteries with a remaining capacity ratio of 90% or more were evaluated as excellent, those with a ratio between 80% and 90% were evaluated as good, and those with a ratio below 80% were evaluated as poor. Formula: Remaining capacity ratio = Discharge capacity at 500th cycle × 100 / Discharge capacity at 1st cycle [Safety Evaluation] The cylindrical evaluation batteries prepared as described above were charged with a constant current of 500mA. After the battery voltage reached 4.20V, they were charged at a constant voltage until the current value was 10mA or less, resulting in a fully charged battery. Next, the fully charged cylindrical batteries were placed with their long sides facing horizontal, and a rod with a mass of 9.1kg and a diameter of 15.8mm was dropped from a height of 61cm onto the flat central surface of the battery to impart an impact. Ten batteries were evaluated, and those that caught fire or emitted smoke were evaluated as defective (×), while those that did not catch fire or emit smoke were evaluated as good (○).

[0054] (Example 1) Weight-average molecular weight (Mw) is 2.4 × 10⁻⁶ 6 It is 40% by mass of ultra-high molecular weight polyethylene (UHMwPE), with a terminal vinyl group concentration of 6.5 per 10,000 carbon atoms, and Mw is 3.0 × 10 5 A mixture was obtained by dry blending 60% by mass of high-density polyethylene (HDPE) containing long-chain branching. 25% by mass of the obtained mixture was melt-kneaded with 75% by mass of liquid paraffin in a twin-screw extruder to prepare a polyethylene resin composition. This polyethylene resin composition was fed from the twin-screw extruder to a T-die and extruded to obtain a molded body, which was then cooled while being taken up by a cooling roll to form a sheet-like polyethylene resin composition. The sheet-like polyethylene resin composition was stretched 7.0 times at 113°C using a roll stretcher, then guided to a tenter and TD-stretched 7.0 times at 123°C. After that, it was washed in a methylene chloride washing tank to remove the liquid paraffin and dried. The dried film was TD-stretched 1.59 times at 132.5°C in a tenter, and then relaxed by 4.3% at 132.5°C and heat-set to obtain a polyethylene microporous film with a thickness of 9.4 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. The battery performed excellently in all tests, including foreign object resistance tests, rate tests, cycle tests, and safety tests.

[0055] (Example 2) A sheet-like polyethylene resin composition was formed using the same method as in Example 1. After stretching to 7.0 times its original size at 113°C using a roll stretcher, it was guided to a tenter and TD stretched to 7.0 times its original size at 122.5°C. Subsequently, it was washed in a methylene chloride washing tank to remove liquid paraffin and dried. The dried film was TD stretched to 1.60 times its original size at 132.1°C in a tenter, and then heat-set by relaxing by 4.2% at 132.1°C to obtain a polyethylene microporous film with a thickness of 8.8 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. Foreign matter resistance tests, rate tests, cycle tests, and safety tests of batteries were performed, and all showed excellent results.

[0056] (Example 3) A sheet-like polyethylene resin composition was formed using the same method as in Example 1. After being stretched 7.6 times at 113°C using a roll stretcher, it was guided to a tenter and TD stretched 7.6 times at 125°C.

[0057] Subsequently, the film was washed in a methylene chloride washing tank to remove the liquid paraffin and then dried. The dried film was then TD-stretched 1.60 times at 131.9°C in a tenter, followed by 4.2% relaxation at 131.9°C and heat-fixed to obtain a polyethylene microporous film with a thickness of 9.0 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. Foreign matter resistance tests, rate tests, cycle tests, and safety tests were performed on the battery, and all results were excellent.

[0058] (Example 4) A sheet-like polyethylene resin composition was formed using the same method as in Example 1. After being stretched 5.5 times at 111°C using a roll stretcher, it was guided to a tenter and TD stretched 8.9 times at 125°C.

[0059] Subsequently, the film was washed in a methylene chloride washing tank to remove the liquid paraffin and then dried. The dried film was then TD-stretched to 1.67 times its original size at 130.5°C in a tenter, followed by 3.8% relaxation at 130.5°C and heat-fixed to obtain a polyethylene microporous film with a thickness of 9.0 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. Foreign matter resistance tests, rate tests, cycle tests, and safety tests were performed on the battery, and all results were excellent.

[0060] (Example 5) A sheet-like polyethylene resin composition was formed using the same method as in Example 1. After being stretched 5.5 times at 111°C using a roll stretcher, it was guided to a tenter and TD stretched 9.0 times at 125°C. Subsequently, the film was washed in a methylene chloride washing tank to remove the liquid paraffin and then dried. The dried film was then TD-stretched 1.50 times at 130.0°C in a tenter, followed by a 5.6% relaxation at 130.0°C and heat-fixed treatment to obtain a polyethylene microporous film with a thickness of 9.4 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. Foreign matter resistance tests, rate tests, cycle tests, and safety tests were performed on the battery, and all results were excellent.

[0061] (Example 6) Mw is 2.4 × 10 6 It is 40% by mass of ultra-high molecular weight polyethylene (UHMwPE), with a terminal vinyl group concentration of 6.5 per 10,000 carbon atoms, and Mw is 3.0 × 10 5 A mixture was obtained by dry blending 60% by mass of high-density polyethylene (HDPE) containing long-chain branching. 23% by mass of the obtained mixture was melt-kneaded with 77% by mass of liquid paraffin in a twin-screw extruder to prepare a polyethylene resin composition. A molded body obtained by feeding this polyethylene resin composition from the twin-screw extruder to a T-die and extruding it was cooled while being taken up by a cooling roll to form a sheet-like polyethylene resin composition. The sheet-like polyethylene resin composition was stretched 6.1 times at 110°C using a roll stretcher, and then guided to a tenter and TD-stretched 9.1 times at 125°C.

[0062] Subsequently, the film was washed in a methylene chloride washing tank to remove the liquid paraffin and then dried. The dried film was then TD-stretched 1.56 times at 130.0°C in a tenter, followed by 5.6% relaxation at 130.0°C and heat-fixed to obtain a polyethylene microporous film with a thickness of 9.5 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. Foreign matter resistance tests, rate tests, cycle tests, and safety tests were performed on the battery, and all results were excellent.

[0063] (Example 7) Mw is 1.5 × 10 6 It is 40% by mass of ultra-high molecular weight polyethylene (UHMwPE), with a terminal vinyl group concentration of 6.5 per 10,000 carbon atoms, and Mw is 3.0 × 10 5 A mixture was obtained by dry blending 60% by mass of high-density polyethylene (HDPE) containing long-chain branching. 25% by mass of the obtained mixture was melt-kneaded with 75% by mass of liquid paraffin in a twin-screw extruder to prepare a polyethylene resin composition. This polyethylene resin composition was fed from the twin-screw extruder to a T-die and extruded to obtain a molded body, which was then cooled while being taken up by a cooling roll to form a sheet-like polyethylene resin composition. The sheet-like polyethylene resin composition was stretched 5.8 times at 111°C using a roll stretcher, then guided to a tenter and TD-stretched 8.4 times at 125°C. After that, it was washed in a methylene chloride washing tank to remove the liquid paraffin and dried. The dried film was TD-stretched 1.53 times at 132.0°C in a tenter, and then relaxed by 5.6% at 132.0°C and heat-set to obtain a polyethylene microporous film with a thickness of 9.6 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. The battery performed excellently in all tests, including foreign object resistance tests, rate tests, cycle tests, and safety tests.

[0064] (Comparative Example 1) Mw is 2.4 × 10 6 40% by mass of ultra-high molecular weight polyethylene (UHMwPE), and Mw is 2.8 × 10 5A mixture was obtained by dry blending 60% by mass of high-density polyethylene (HDPE). 25% by mass of the obtained mixture and 75% by mass of liquid paraffin were melt-kneaded in a twin-screw extruder to prepare a polyethylene resin composition. This polyethylene resin composition was fed from the twin-screw extruder to a T-die and extruded to obtain a molded body, which was then cooled while being taken up by a cooling roll to form a sheet-like polyethylene resin composition. The sheet-like polyethylene resin composition was stretched 7.0 times at 113°C using a roll stretcher, then guided to a tenter and TD-stretched 7.0 times at 123°C. After that, it was washed in a methylene chloride washing tank to remove the liquid paraffin and dried. The dried film was TD-stretched 1.47 times at 134.8°C in a tenter, and then relaxed by 4.4% at 134.8°C and heat-set to obtain a polyethylene microporous film with a thickness of 9.0 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. Although the battery performed well in foreign object resistance tests, rate tests, and cycle tests, it failed safety tests because its shutdown temperature exceeded 139°C.

[0065] (Comparative Example 2) A sheet-like polyethylene resin composition was formed using the same method as in Comparative Example 1. It was then stretched 7.0 times using a roll stretcher at 113°C, followed by TD stretching at 118°C to 7.0 times the original length. Afterward, it was washed in a methylene chloride washing tank to remove liquid paraffin and dried. The dried film was then TD stretched 1.47 times at 134.3°C in a tenter, followed by 4.4% relaxation at 134.3°C and heat-fixed to obtain a polyethylene microporous film with a thickness of 9.3 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. While the battery performed well in foreign matter resistance tests, rate tests, and cycle tests, it failed safety tests because the shutdown temperature exceeded 139°C.

[0066] (Comparative Example 3) A sheet-like polyethylene resin composition was formed using the same method as in Comparative Example 1. It was then stretched 7.0 times in a roll stretcher at 113°C, followed by TD stretching at 123°C to 7.0 times in a tenter. Afterward, it was washed in a methylene chloride washing tank to remove liquid paraffin and dried. The dried film was then TD stretched 1.47 times in a tenter at 135.7°C, followed by 4.4% relaxation at 135.7°C and heat-fixed to obtain a polyethylene microporous film with a thickness of 9.3 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. While the battery performed well in foreign matter resistance tests, rate tests, and cycle tests, its safety was compromised because the shutdown temperature exceeded 139°C.

[0067] (Comparative Example 4) Mw is 2.4 × 10 6 30% by mass of ultra-high molecular weight polyethylene (UHMwPE), and Mw is 2.8 × 10 5 A mixture was obtained by dry blending 70% by mass of high-density polyethylene (HDPE). 29% by mass of the obtained mixture and 71% by mass of liquid paraffin were melt-kneaded in a twin-screw extruder to prepare a polyethylene resin composition. This polyethylene resin composition was supplied from the twin-screw extruder to a T-die and extruded to obtain a molded body, which was then cooled while being taken up by a cooling roll to form a sheet-like polyethylene resin composition. The sheet-like polyethylene resin composition was stretched 5.8 times at 116°C using a roll stretcher, then guided to a tenter and TD-stretched 7.0 times at 124°C. After that, it was washed in a methylene chloride washing tank to remove the liquid paraffin and dried. The dried film was TD-stretched 1.40 times at 133.2°C in a tenter, then relaxed by 3.8% at 133.2°C and heat-set to obtain a polyethylene microporous film with a thickness of 10.0 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. Although the battery performed well in rate characteristics and safety tests, its indentation modulus was below 280 MPa, resulting in poor cycle characteristics and resistance to foreign matter.

[0068] (Comparative Example 5) A sheet-like polyethylene resin composition was formed in the same manner as in Comparative Example 4, stretched 5.1 times at 114°C using a roll stretcher, then guided to a tenter and TD-stretched 7.5 times at 122°C. After that, it was washed in a methylene chloride washing tank to remove liquid paraffin and dried. The dried film was TD-stretched 1.40 times at 129.7°C in a tenter, and then heat-set by relaxing by 5.8% at 129.7°C to obtain a polyethylene microporous film with a thickness of 9.8 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. Although it performed well in battery rate characteristics and safety tests, its indentation modulus was below 280 MPa, resulting in poor cycle characteristics and resistance to foreign matter.

[0069] (Comparative Example 6) A sheet-like polyethylene resin composition was formed in the same manner as in Comparative Example 4, stretched 7.5 times at 124°C using a roll stretcher, then guided into a tenter and stretched 9.8 times at 124.5°C using a TD stretcher. After that, it was washed in a methylene chloride washing tank to remove liquid paraffin and dried. The dried film was stretched 1.62 times in a TD stretcher at 132.4°C, then relaxed by 5.6% at 132.4°C and heat-set to obtain a polyethylene microporous film with a thickness of 11.8 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. Although it performed well in battery rate characteristics and safety tests, its indentation modulus was below 280 MPa, resulting in poor cycle characteristics and resistance to foreign matter.

[0070] (Comparative Example 7) Mw is 2.4 × 10 6 40% by mass of ultra-high molecular weight polyethylene (UHMwPE), and Mw is 2.8 × 10 5A mixture was obtained by dry blending 60% by mass of high-density polyethylene (HDPE). 25% by mass of the obtained mixture and 75% by mass of liquid paraffin were melt-kneaded in a twin-screw extruder to prepare a polyethylene resin composition. This polyethylene resin composition was fed from the twin-screw extruder to a T-die and extruded to obtain a molded body, which was then cooled while being taken up by a cooling roll to form a sheet-like polyethylene resin composition. The sheet-like polyethylene resin composition was stretched 7.0 times at 116°C using a roll stretcher, then guided to a tenter and TD-stretched 12.6 times at 123°C. After that, it was washed in a methylene chloride washing tank to remove the liquid paraffin and dried. The dried film was TD-stretched 1.70 times at 131.0°C in a tenter, then relaxed by 3.0% at 131.0°C and heat-set to obtain a polyethylene microporous film with a thickness of 11.2 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. Although the battery's rate characteristics and cycle characteristics were excellent, its indentation modulus was below 280 MPa, resulting in poor resistance to foreign matter. Furthermore, its shutdown temperature exceeded 139°C, leading to poor safety.

[0071] (Comparative Example 8) Mw is 2.4 × 10 6 30% by mass of ultra-high molecular weight polyethylene (UHMwPE), and Mw is 2.8 × 10 5A mixture was obtained by dry blending 70% by mass of high-density polyethylene (HDPE). 29% by mass of the obtained mixture and 71% by mass of liquid paraffin were melt-kneaded in a twin-screw extruder to prepare a polyethylene resin composition. This polyethylene resin composition was supplied from the twin-screw extruder to a T-die and extruded to obtain a molded body, which was then cooled while being taken up by a cooling roll to form a sheet-like polyethylene resin composition. The sheet-like polyethylene resin composition was simultaneously biaxially stretched 5 × 5 times at a temperature of 120°C using a tenter. After that, it was washed in a methylene chloride washing tank to remove the liquid paraffin and dried. The dried film was TD-stretched 1.40 times at 128.6°C in a tenter, and then heat-set by relaxing by 3.6% at 128.6°C to obtain a polyethylene microporous film with a thickness of 15.0 μm. Table 1 shows the physical properties of the obtained polyolefin microporous film. Although the battery rate characteristics and safety were excellent, the resistance to foreign matter was poor.

[0072] [Table 1] [Industrial applicability]

[0073] The polyolefin microporous membrane of the present invention has excellent indentation modulus and shutdown temperature, making it suitable for use as a separator for non-aqueous electrolyte secondary batteries.

Claims

1. When a diamond Berkovich (triangular pyramidal) indenter is subjected to a vertical load of up to 500 μN at a rate of 16.67 μN / sec and held for 30 seconds, and then unloaded at a rate of 16.67 μN / sec, the indentation modulus is 280 MPa or higher, the SD temperature is less than 140°C, and the basis weight equivalent puncture strength is 0.80 N / (g / m²). 2 A polyolefin microporous membrane mainly composed of polyethylene resin having a density of ) or more, wherein the concentration of terminal vinyl groups per 10,000 carbon atoms of the polyolefin resin contained in the polyolefin microporous membrane is 1.9 or less, for use as a separator for a non-aqueous electrolyte secondary battery.

2. The polyolefin microporous membrane according to claim 1, wherein the film thickness is 5 to 12 μm.

3. A separator for a non-aqueous electrolyte secondary battery using a polyolefin microporous membrane according to claim 1 or 2.

4. A non-aqueous electrolyte secondary battery using the battery separator described in claim 3.

Citation Information

Patent Citations

  • Microporous polyolefin membrane and manufacturing method therefor

    JP2003020357A

  • A method for producing polyolefin microporous membranes with excellent productivity and easily controllable physical properties.

    JP2013530261A

  • Polyolefin-made laminated microporous film

    JP2015208893A

  • Separator for nonaqueous electrolyte secondary battery

    JP2018147886A

  • Polyolefin microporous film

    WO2007015416A1