Multilayer ceramic capacitors and circuit boards

The multilayer ceramic capacitor addresses dielectric breakdown and structural issues by optimizing continuity ratios in internal electrode regions, improving reliability and insulation resistance through enhanced adhesion and reduced stress concentration.

JP7954512B2Active Publication Date: 2026-11-20TAIYO YUDEN KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022044811
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-03-22
Publication Date
2026-11-20
Estimated Expiration
2042-03-22

AI Technical Summary

Technical Problem

Existing multilayer ceramic capacitors face issues with dielectric breakdown due to electric field concentration at the margin edges of internal electrodes, leading to potential delamination, cracking, and reduced insulation resistance, especially in high-reliability applications like electric vehicles and medical equipment.

Method used

A multilayer ceramic capacitor design with specific continuity ratios in different regions of the internal electrodes, where the continuity rate is higher along the margin edges to suppress spheroidization and lower in other regions to improve adhesion, thereby reducing dielectric breakdown and structural defects.

Benefits of technology

The design enhances the reliability of the capacitor by suppressing dielectric breakdown, delamination, and cracking, maintaining high insulation resistance and capacitance, while also reducing manufacturing costs and stress concentration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954512000002
    Figure 0007954512000002
  • Figure 0007954512000003
    Figure 0007954512000003
  • Figure 0007954512000004
    Figure 0007954512000004
Patent Text Reader

Abstract

To provide a multilayer ceramic capacitor having a high reliability and provide a circuit board mounting them.SOLUTION: A multilayer ceramic capacitor comprises a ceramic element body, and first and second external electrodes. The ceramic element body includes: a capacity formation part including first and second internal electrodes and a ceramic layer; and a margin part including an end margin part and a side margin part. Each of the first and second internal electrodes includes: an end part constructed by a leading end part coming into contact with the first or second external electrode, and a margin end part coming into contact with the margin part; a first region where a continuous rate of a conductive component in a plan view from a second axial direction is a first continuous rate, and which is arranged along the margin end part; and a second region where the continuous rate of the conductive component in the plan view is a second conductive rate lower than the first conductive rate, and which is arranged in an inner side in a first axial direction and a third axial direction from the first region.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a multilayer ceramic capacitor and a circuit board on which the same is mounted.

Background Art

[0002] A multilayer ceramic capacitor includes, for example, a ceramic body having internal electrodes alternately led out to a pair of end faces and stacked, and ceramic layers disposed between the internal electrodes, and a pair of external electrodes respectively covering the pair of end faces and connected to the internal electrodes (see Patent Documents 1 and 2). In the internal electrodes, ends other than the lead-out end portions connected to the external electrodes are covered with margin portions made of ceramic.

[0003] The end portion of the internal electrode covered by the margin portion may be located at the periphery of the region facing the adjacent internal electrode in the stacking direction. For this reason, it is known that the electric field formed between the adjacent internal electrodes concentrates at the end portion, and dielectric breakdown is likely to occur. For example, Patent Document 1 discloses a technique for alleviating electric field concentration at the end portion of the internal electrode by making the thickness of the ceramic layer at the peripheral portion of the internal electrode pattern larger than the thickness of the ceramic layer at the central portion. For example, Patent Document 2 discloses that by setting the porosity in a region 20 times the thickness of the internal electrode from the outer peripheral edge of the internal electrode to be in the range of 5% to 15%, the occurrence of cracks at the outer peripheral edge of the internal electrode and the decrease in withstand voltage are suppressed. This configuration is realized by moving the common material composed of ceramic powder contained in the internal electrode from the central portion of the internal electrode to the outer peripheral edge thereof.

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Patent Document 2

Summary of Invention

[0005] However, in the technology described in Patent Document 1, the central part of the laminate is pressed more strongly than the peripheral part, which reduces the adhesion of the peripheral part of the laminate, including the margin, raising concerns about delamination and cracking. In the technology described in Patent Document 2, the porosity in the central part of the internal electrode may be low. This raises concerns about delamination due to reduced adhesion between the ceramic layer and the internal electrode, and cracking due to the difference in shrinkage rate during firing between the central part of the internal electrode and the ceramic layer.

[0006] Furthermore, in recent years, multilayer ceramic capacitors have been incorporated into electronic devices that require particularly high reliability, such as electric vehicles and medical equipment. Therefore, there is a demand for highly reliable multilayer ceramic capacitors that can effectively suppress the decrease in insulation resistance.

[0007] In view of the above circumstances, the object of the present invention is to provide a multilayer ceramic capacitor with high reliability and a circuit board on which it is mounted. [Means for solving the problem]

[0008] To achieve the above objective, a multilayer ceramic capacitor according to one embodiment of the present invention comprises a ceramic body and first and second external electrodes. The ceramic body has first and second end faces perpendicular to the first axial direction, a volume-forming portion, and a margin portion. The capacitance forming portion includes a first internal electrode drawn out from the first end face, a second internal electrode drawn out from the second end face and facing the first internal electrode in a second axial direction perpendicular to the first axis, and a ceramic layer disposed between the first and second internal electrodes. The margin portion includes a first end margin portion disposed between the first end face and the second internal electrode, a second end margin portion disposed between the second end face and the first internal electrode, and first and second side margin portions disposed on both sides of the third axial direction perpendicular to the first and second axes of the capacitance forming portion. The first and second external electrodes cover the first and second end faces, respectively. The first and second internal electrodes are, respectively, An end comprising a lead-out end in contact with the first or second external electrode and a margin end in contact with the margin portion, The continuity rate of the conductive component in a plan view from the second axial direction is the first continuity rate, and the first region is arranged along the margin end, The second region is located inward from the first region in the first axial direction and the third axial direction, and the continuity rate of the conductive component in the plan view is a second continuity rate that is lower than the first continuity rate. Where a is the value obtained by subjecting the first continuity ratio to omega transformation, and b is the value obtained by subjecting the second continuity ratio to omega transformation, 0 < a - b ≤ 6.8 is satisfied.

[0009] In the above configuration, the first continuity ratio of the first region, which is positioned along the margin edge of the internal electrode, is higher than the second continuity ratio of the second region. This suppresses the spheroidization of conductive components at and near the margin edge, thereby suppressing dielectric breakdown due to electric field concentration. Furthermore, by relatively lowering the second continuity ratio of the second region, the adhesion between the ceramic layer and the second region is improved, and their sintering behavior can be made more similar. This suppresses delamination and cracking of the ceramic body, and also suppresses leakage current associated with these structural defects. Therefore, the above configuration can suppress the decrease in insulation resistance of the multilayer ceramic capacitor and improve its reliability. Further, by setting a - b ≤ 6.8, the difference in sintering behavior between the first and second regions caused by the difference in continuity ratio can be reduced, and the occurrence of stress at the interface with the ceramic layer and the occurrence of cracks and the like caused thereby can be suppressed. Therefore, the reliability of the multilayer ceramic capacitor can be more reliably improved.

[0010] For example, the margin end includes a pair of side ends that are in contact with the first and second side margin portions, and an end end that is in contact with the first or second end margin portion. The first region is, From each of the pair of side ends, a pair of side regions located within 10% of the width dimension in the third axial direction of each of the first and second internal electrodes, Includes an end region located within 10% of the length dimension of the first and second internal electrodes in the first axial direction from the end end, The second region may occupy the region of each of the first and second internal electrodes excluding the first region. This design allows the region where the electric field is particularly prone to concentration to be designated as the first region, effectively suppressing dielectric breakdown associated with electric field concentration. Furthermore, by having the second region occupy a wide area of ​​the internal electrodes, the effect of suppressing structural defects such as delamination and cracks in the ceramic body can be enhanced. Therefore, the above configuration can more effectively improve the reliability of the multilayer ceramic capacitor.

[0011] In this case, the first continuity rate may be a value measured in the end region and / or the side region of the first region.

[0012] For example, the second consecutive rate may be 70% or higher. This makes it possible to obtain a multilayer ceramic capacitor that has sufficient capacitance and good frequency characteristics such as impedance and Q value.

[0013] The continuity rate of the conductive component may gradually decrease from the first region to the second region. This can alleviate stress concentration and further improve the reliability of multilayer ceramic capacitors.

[0015] For example, the first and second consecutive rates are, After the ceramic body is immersed in an etching solution that dissolves ceramics but does not dissolve the conductive component, it may be calculated as the ratio of the area of the undissolved conductive component per unit area in each of the first and second regions. Thereby, the first and second continuity ratios of the conductive component in a plan view can be clearly and easily calculated.

[0016] For example, the conductive component may include nickel, copper, palladium, platinum, silver, gold, tin, or an alloy thereof.

[0017] Further, the first region may contain at least one of silver, chromium, iridium, magnesium, molybdenum, osmium, palladium, platinum, rhenium, rhodium, ruthenium, yttrium, and tungsten as an additive.

[0018] For example, the thickness of the second region in the second axial direction may be 0.2 μm or more and 0.85 μm or less.

[0019] For example, the dimension of the multilayer ceramic capacitor in the first axial direction is 0.4 mm or less, The dimension of the multilayer ceramic capacitor in the third axial direction may be 0.2 mm or less.

[0020] For example, the dimension of each of the first and second side margin portions in the third axial direction may be 30 μm or less. For example, the dimension of each of the first and second end margin portions in the first axial direction may be 30 μm or less.

[0021] For example, the thickness of the ceramic layer may be 0.2 μm or more and 0.5 μm or less.

[0022] For example, the dimension of the multilayer ceramic capacitor in the second axial direction may be larger than at least one of the dimensions of the multilayer ceramic capacitor in the first axial direction or the dimensions of the multilayer ceramic capacitor in the third axial direction. According to the present invention, even with multilayer ceramic capacitors having large dimensions in the second axial direction, structural defects in the ceramic body can be suppressed, thereby improving reliability.

[0023] Another embodiment of the present invention comprises a ceramic capacitor and a mounting substrate on which the multilayer ceramic capacitor is mounted. The multilayer ceramic capacitor comprises a ceramic body and first and second external electrodes. The ceramic body has first and second end faces perpendicular to the first axial direction, a volume-forming portion, and a margin portion. The capacitance forming portion includes a first internal electrode drawn out from the first end face, a second internal electrode drawn out from the second end face and facing the first internal electrode in a second axial direction perpendicular to the first axis, and a ceramic layer disposed between the first and second internal electrodes. The margin portion includes a first end margin portion disposed between the first end face and the second internal electrode, a second end margin portion disposed between the second end face and the first internal electrode, and first and second side margin portions disposed on both sides of the third axial direction perpendicular to the first and second axes of the capacitance forming portion. The first and second external electrodes cover the first and second end faces, respectively, and are connected to the mounting substrate. The first and second internal electrodes are, respectively, An end comprising a lead-out end in contact with the first or second external electrode and a margin end in contact with the margin portion, The continuity rate of the conductive component in a plan view from the second axial direction is the first continuity rate, and the first region is arranged along the margin end, The second region is located inward from the first region in the first axial direction and the third axial direction, and the continuity rate of the conductive component in the plan view is a second continuity rate that is lower than the first continuity rate. Where a is the value obtained by subjecting the first continuity ratio to omega transformation, and b is the value obtained by subjecting the second continuity ratio to omega transformation, 0 < a - b ≤ 6.8 is satisfied. [Effects of the Invention]

[0024] As described above, the present invention provides a highly reliable multilayer ceramic capacitor and a circuit board on which it is mounted. [Brief explanation of the drawing]

[0025] Figure 1 This is a perspective view of a multilayer ceramic capacitor according to one embodiment of the present invention. Figure 2 This is a cross-sectional view of the multilayer ceramic capacitor shown above, along the line A-A' in Figure 1. Figure 3 This is a cross-sectional view of the multilayer ceramic capacitor shown above, along the line B-B' in Figure 1. Figure 4 This is a cross-sectional view of the ceramic body of the multilayer ceramic capacitor described above, showing a cross-section taken parallel to the X-axis direction (second axis direction) and the Y-axis direction (third axis direction) at the position of the first internal electrode. Figure 5 This is a cross-sectional view of the ceramic body of the multilayer ceramic capacitor described above, showing a cross-section taken parallel to the X-axis direction (second axis direction) and the Y-axis direction (third axis direction) at the position of the second internal electrode. Figure 6 This is a cross-sectional view of a circuit board on which the above-mentioned multilayer ceramic capacitor is mounted. Figure 7 This flowchart shows the manufacturing method for the multilayer ceramic capacitor described above. Figure 8 This is a plan view showing the manufacturing process of the multilayer ceramic capacitor described above. Figure 9 This is a perspective view showing the manufacturing process of the multilayer ceramic capacitor described above. Figure 10The graph shows the results of analyzing the relationship between the difference (ab) between the omega-converted value (a) of the continuity rate A of the first region of the internal electrode and the omega-converted value (b) of the continuity rate B of the second region, and the dielectric breakdown voltage (BDV) for the examples and comparative examples of the above embodiment, using the Weibull distribution method. A shows the result of Weibull α, a parameter of the Weibull distribution, and B shows the result of Weibull β, another parameter of the Weibull distribution. [Modes for carrying out the invention]

[0026] Embodiments of the present invention will be described below with reference to the drawings. The drawings show mutually orthogonal X, Y, and Z axes as appropriate. The X, Y, and Z axes define a fixed coordinate system fixed to the multilayer ceramic capacitor 10.

[0027] [Overall configuration of a multilayer ceramic capacitor] Figures 1-3 show a multilayer ceramic capacitor 10 according to one embodiment of the present invention. Figure 1 is a perspective view of the multilayer ceramic capacitor 10. Figure 2 is a cross-sectional view of the multilayer ceramic capacitor 10 along the line A-A' in Figure 1. Figure 3 is a cross-sectional view of the multilayer ceramic capacitor 10 along the line B-B' in Figure 1.

[0028] The multilayer ceramic capacitor 10 comprises a ceramic body 11, a first external electrode 14a, and a second external electrode 14b.

[0029] The ceramic body 11 is constructed as a rectangular parallelepiped having a first end face 11a and a second end face 11b perpendicular to the X-axis, a first side face 11c and a second side face 11d perpendicular to the Y-axis, and a first main face 11e and a second main face 11f perpendicular to the Z-axis. Note that "rectangular parallelepiped" means that it is substantially rectangular in shape, and for example, the edges connecting each face of the ceramic body 11 may be rounded.

[0030] The main surfaces 11e, 11f, end surfaces 11a, 11b, and side surfaces 11c, 11d of the ceramic body 11 are all configured as flat surfaces. In this embodiment, a flat surface does not have to be strictly planar as long as it is perceived as flat when viewed as a whole, and includes, for example, surfaces having minute irregularities on the surface or gently curved shapes within a predetermined range.

[0031] The multilayer ceramic capacitor 10 of this embodiment has, for example, the following dimensions. The dimensions of the multilayer ceramic capacitor 10 in the X-axis direction are, for example, 0.2 mm or more and 4.8 mm or less, and more preferably 0.4 mm or less. The dimensions of the multilayer ceramic capacitor 10 in the Y-axis direction are, for example, 0.1 mm or more and 3.5 mm or less, and more preferably 0.2 mm or less. The dimensions of the multilayer ceramic capacitor 10 in the Z-axis direction are, for example, 0.1 mm or more and 3.5 mm or less. Specifically, when the size of the multilayer ceramic capacitor 10 is expressed as (dimensions in the X-axis direction) × (dimensions in the Y-axis direction) × (dimensions in the Z-axis direction), it may be 0.25 mm × 0.125 mm × 0.125 mm, 0.4 mm × 0.2 mm × 0.2 mm, etc. Note that the "dimensions" in a certain direction of the multilayer ceramic capacitor 10 refer to the maximum dimensions of the multilayer ceramic capacitor 10 in that direction.

[0032] Furthermore, in the following explanation, "inward in the X-axis direction" refers to the side approaching a virtual YZ plane that divides the multilayer ceramic capacitor 10 in two equal parts in the X-axis direction, and "outward in the X-axis direction" refers to the side moving away from the above virtual YZ plane. "Inward in the Y-axis direction" refers to the side approaching a virtual XZ plane that divides the multilayer ceramic capacitor 10 in two equal parts in the Z-axis direction, and "outward in the Z-axis direction" refers to the side moving away from the above virtual XZ plane.

[0033] The external electrodes 14a and 14b cover both ends of the ceramic body 11 in the X-axis direction. For example, the first external electrode 14a shown in Figures 1 and 2 extends from the first end face 11a of the ceramic body 11 to both main faces 11e and 11f and both side faces 11c and 11d. The second external electrode 14b shown in Figure 1 extends from the second end face 11b of the ceramic body 11 to both main faces 11e and 11f and both side faces 11c and 11d. However, the shape of the external electrodes 14a and 14b is not limited to these.

[0034] The ceramic body 11 includes a volume forming portion 15, a first cover portion 16a, a second cover portion 16b, a first side margin portion 17a, a second side margin portion 17b, a first end margin portion 18a, and a second end margin portion 18b. In this embodiment, the first and second side margin portions 17a, 17b and the first and second end margin portions 18a, 18b constitute the margin portion M of the ceramic body 11 (see Figures 4 and 5).

[0035] The first and second cover portions 16a and 16b face each other in the Z-axis direction with the volume forming portion 15 in between, and constitute the main surfaces 11e and 11f of the ceramic body 11.

[0036] The first and second side margin portions 17a and 17b are respectively located on both sides of the volume forming portion 15 in the Y-axis direction. In other words, the first and second side margin portions 17a and 17b face each other in the Y-axis direction with the volume forming portion 15 in between. Each side margin portion 17a and 17b is also referred to as the side margin portion 17.

[0037] The dimensions of each side margin portion 17 in the Y-axis direction may be, for example, 30 μm or less and 20 μm or less, in order to achieve miniaturization and increased capacity of the ceramic body 11. The dimensions of each side margin portion 17 in the Y-axis direction may be, for example, 5 μm or more, in order to ensure insulation.

[0038] The first end margin portion 18a is positioned between the first end face 11a and the second internal electrode 13. The second end margin portion 18b is positioned between the second end face 11b and the first internal electrode 12. Each of the end margin portions 18a and 18b is also referred to as the end margin portion 18.

[0039] The dimensions of each end margin portion 18 in the X-axis direction may be, for example, 30 μm or less and 20 μm or less, in order to achieve miniaturization and increased capacity of the ceramic body 11. The dimensions of each end margin portion 18 in the X-axis direction may be, for example, 10 μm or more, in order to ensure insulation.

[0040] The capacitance forming section 15 includes a ceramic layer 19 and first and second internal electrodes 12 and 13 positioned between the ceramic layer 19. The first internal electrode 12 is drawn out to a first end face 11a. The second internal electrode 13 is drawn out to a second end face 11b and faces the first internal electrode 12 in the Z-axis direction. The ceramic layer 19 is positioned between the first and second internal electrodes 12 and 13. In other words, the first and second internal electrodes 12 and 13 are alternately stacked in the Z-axis direction via the ceramic layer 19. In this embodiment, both the ceramic layer 19 and the internal electrodes 12 and 13 are configured as sheets extending along the XY plane.

[0041] The internal electrodes 12 and 13 mainly contain a conductive component. Typical conductive components include nickel (Ni), but other examples include copper (Cu), palladium (Pd), platinum (Pt), silver (Ag), gold (Au), tin (Sn), and alloys thereof.

[0042] The first internal electrode 12 is connected to the first external electrode 14a at its first end face 11a. The second end face 11b side of the first internal electrode 12 is insulated from the second external electrode 14b by the second end margin portion 18b. The second internal electrode 13 is connected to the second external electrode 14b at its second end face 11b. The first end face 11a side of the second internal electrode 13 is insulated from the first external electrode 14a by the first end margin portion 18a.

[0043] With this configuration, when a voltage is applied between the external electrodes 14a and 14b of the multilayer ceramic capacitor 10, a voltage is applied to multiple ceramic layers 19 between the internal electrodes 12 and 13. As a result, the multilayer ceramic capacitor 10 stores a charge corresponding to the voltage between the external electrodes 14a and 14b.

[0044] The ceramic layer 19 mainly contains dielectric ceramics. The dielectric ceramics contained in the ceramic layer 19 have a perovskite structure represented by the general formula ABO3, for example. Examples of dielectric ceramics having a perovskite structure include materials containing barium (Ba) and titanium (Ti), such as barium titanate (BaTiO3).

[0045] Specifically, dielectric ceramics may be composed of other materials besides barium titanate, such as strontium titanate (SrTiO3), calcium titanate (CaTiO3), magnesium titanate (MgTiO3), calcium zirconate (CaZrO3), calcium zirconate titanate (Ca(Ti,Zr,Ti)O3), barium calcium zirconate titanate ((Ba,Ca)(Ti,Zr)O3), barium zirconate (BaZrO3), and titanium dioxide (TiO2).

[0046] The compositions of the ceramic layer 19, cover portions 16a and 16b, side margin portion 17, and end margin portion 18 may be the same or different. From the viewpoint of mitigating stress caused by differences in physical properties between the capacitance forming portion 15 and its surroundings, it is preferable that the cover portions 16a and 16b, side margin portion 17, and end margin portion 18 contain dielectric ceramics of the same composition system as the ceramic layer 19.

[0047] The thickness of each ceramic layer 19 in the Z-axis direction can be, for example, 0.2 μm to 20 μm, preferably 0.2 μm to 0.5 μm. This makes it possible to make the thickness of each ceramic layer 19 in the Z-axis direction greater than or equal to the grain size of the dielectric ceramic crystals, and to increase the capacitance. The thickness of the ceramic layer 19 is the average value of the thickness measured at multiple locations on the ceramic layer 19. As an example, a cross-section parallel to the Z-axis direction of the ceramic body 11 is observed using an SEM (scanning electron microscope) or TEM (transmission electron microscope). Six layers are selected from the ceramic layers 19 in the field of view, and the thickness is measured at five equally spaced locations in each layer. The average value of the obtained 30 thicknesses is then taken as the thickness of the ceramic layer 19.

[0048] [Internal electrode configuration] Figures 4 and 5 are cross-sectional views of the ceramic body 11. Figure 4 shows a cross-section parallel to the XY plane at the position of the first internal electrode 12, and Figure 5 shows a cross-section parallel to the XY plane at the position of the second internal electrode 13. In Figures 4 and 5, the internal electrodes 12 and 13 are represented by hatching, and the margin area M is represented by a dot pattern.

[0049] As shown in Figures 4 and 5, each internal electrode 12, 13 has an end portion E. The end portion E constitutes the peripheral edge of the internal electrodes 12, 13 in the X-axis and Y-axis directions. The end portion E is composed of a lead-out end portion E1 that contacts the first external electrode 14a or the second external electrode 14b, and a margin end portion E2 that contacts the margin portion M.

[0050] The lead-out end E1 is the portion of the internal electrodes 12 and 13 in the X-axis direction that is in contact with the external electrodes 14a and 14b. The lead-out end E1 of the first internal electrode 12 is located on the first end face 11a. The lead-out end E1 of the second internal electrode 13 is located on the second end face 11b. The margin end E2 is the portion of end E excluding the lead-out end E1.

[0051] In this embodiment, the margin end E2 further includes a side end E21 that contacts the side margin portion 17 and an end end E22 that contacts the end margin portion 18. In Figures 4 and 5, the boundary between the side end E21 and the end end E22 is curved, but is not limited to this and may be angular.

[0052] The margin edge E2 is located at the periphery of the region where the internal electrodes 12 and 13 face each other. As a result, the electric field formed between the internal electrodes 12 and 13 is concentrated, making dielectric breakdown likely. In particular, as the thickness of the ceramic layer 19 decreases due to the miniaturization of the multilayer ceramic capacitor 10, dielectric breakdown due to electric field concentration becomes even more likely.

[0053] The concentration of the electric field at the margin edge E2 is thought to be promoted by the spheroidization of conductive components such as Ni in the internal electrodes 12 and 13. Spheroidization of the conductive components occurs due to excessive sintering and shrinkage of the conductive components and the ceramics in the internal electrodes 12 and 13. When the conductive components spheroidize at the margin edge E2, the spheroidized portion becomes convex, and the local thickness of the ceramic layer 19 may become thinner than the surrounding area. This makes dielectric breakdown more likely. In addition, some of the spheroidized conductive components may become sharp, causing the electric field to concentrate in that area and leading to dielectric breakdown. Furthermore, dielectric breakdown due to such electric field concentration is more likely to occur as the ceramic layer 19 becomes thinner.

[0054] On the other hand, in regions where the continuity of the conductive component is high, spheroidization of the conductive component is less likely to occur. Therefore, in this embodiment, the continuity of the conductive component is locally increased along the margin edge E2.

[0055] Specifically, in this embodiment, each internal electrode 12, 13 has a first region R1 positioned along the margin end E2, and a second region R2 positioned inward from the first region R1 in the X-axis and Y-axis directions. In Figures 4 and 5, the first region R1 is represented by dense hatching, and the second region R2 is represented by sparse hatching.

[0056] In the first region R1, the continuity rate of the conductive component in a plan view is the first continuity rate A. On the other hand, in the second region R2, the continuity rate of the conductive component in a plan view is the second continuity rate B, which is smaller than the first continuity rate A. Note that "plan view" refers to the plan view when the planes of the internal electrodes 12 and 13 extending along the XY plane are viewed from the Z-axis direction.

[0057] In this configuration, the continuity of the conductive component in the first region R1 along the margin edge E2 becomes relatively high, and the spheroidization of the conductive component in the first region R1 can be suppressed. Therefore, dielectric breakdown at the margin edge E2 can be suppressed, and the reliability of the multilayer ceramic capacitor 10 can be improved.

[0058] Furthermore, in the second region R2, which is located inside the first region R1 in the X and Y directions, the continuity of the conductive component becomes relatively low. As a result, ceramics can penetrate into the gaps in the conductive component of the second region R2, improving the adhesion between the ceramic layer 19 and the second region R2. Therefore, delamination at the interface between the internal electrodes 12, 13 and the ceramic layer 19 can be suppressed.

[0059] Furthermore, during firing, stress may be generated due to the difference in shrinkage behavior between the ceramic layer 19 and the internal electrodes 12 and 13 containing conductive components. In this embodiment, the proportion of ceramics in the second region R2, which occupies the central part of the internal electrodes 12 and 13, can be relatively increased, bringing the shrinkage behavior of the second region R2 during firing closer to that of the ceramic layer 19. As a result, the stress generated at the interface between the internal electrodes 12 and 13 and the ceramic layer 19 during sintering can be alleviated, and cracks caused by such stress can be suppressed.

[0060] Thus, in this embodiment, leakage current due to structural defects such as delamination and cracks in the ceramic element 11 can also be suppressed. Therefore, in the multilayer ceramic capacitor 10, the decrease in insulation resistance associated with such leakage current can also be suppressed.

[0061] Furthermore, by relatively lowering the continuity rate of the conductive component in the second region R2, the material cost related to the conductive component can be reduced compared to the case where the overall continuity rate of the internal electrodes 12 and 13 is increased. Also, as will be described later, the internal electrodes 12 and 13 in this embodiment can be realized by improving the application of the conductive paste and the firing conditions, thereby suppressing an increase in man-hours and an increase in manufacturing costs.

[0062] Furthermore, in this embodiment, the continuity rates A and B in a plan view from the Z-axis direction are used as the continuity rates of the conductive components of the internal electrodes 12 and 13. In other words, these continuity rates A and B represent the continuity rates of the internal electrodes 12 and 13 in the XY plane. By using the continuity rates in the XY plane, the effect of suppressing dielectric breakdown in the first region R1 and the effect of suppressing stress at the interface with the ceramic layer 19 in the second region R2 can be accurately evaluated.

[0063] An example of how to calculate the continuity rates A and B in this embodiment will be described. First, the ceramic body 11 is immersed in an etching solution that dissolves the ceramics but not the conductive components. The etching solution is, for example, a hydrofluoric acid solution. The concentration of the hydrofluoric acid solution is preferably, for example, 2 to 20%. The immersion time is preferably 12 to 48 hours. As a result, the ceramics of the multilayer ceramic capacitor 10 dissolve, leaving the conductive components behind. In other words, the ceramics of the same material contained within the internal electrodes 12 and 13 also dissolve and disappear. The remaining conductive components of the internal electrodes 12 and 13 are in a state where voids are dispersed.

[0064] Next, the internal electrodes are removed from the immersed ceramic body 11. Then, for the removed internal electrodes, the ratio of the area of ​​the undissolved conductive component per unit area in the first region R1 and the second region R2 is calculated as continuity ratios A and B. For example, the processed internal electrodes are imaged by SEM at a magnification of 200 to 2000 times. Subsequently, the ratio of the area of ​​the conductive component to the area of ​​the first region R1 and the second region R2 is calculated by image processing, and these values ​​are defined as continuity ratios A and B. The areas of the first region R1 and the second region R2 include the area of ​​voids, while the area of ​​the conductive component is the area of ​​only the portion consisting of the conductive component excluding the voids.

[0065] The continuity rate A of the first region R1 may be measured in the end region R12 and the side region R11, as described later, or it may be measured in either the end region R12 or the side region R11.

[0066] In this way, by calculating the continuity ratios A and B by melting the ceramics, the continuity ratios A and B of the conductive components in a plan view of the internal electrodes 12 and 13 can be calculated clearly and simply. In addition to the above method, an XY cross section exposing the internal electrodes 12 and 13 may be cut out from the multilayer ceramic capacitor 10, and this cross section may be magnified and imaged using a SEM or the like. In this method, the continuity ratios A and B can be calculated from the visual difference between the conductive component and other components. 。

[0067] Furthermore, in this embodiment, the second continuity rate B of the second region R2 is preferably 70% or more. This makes it possible to obtain a multilayer ceramic capacitor 10 that has high reliability, sufficient capacitance, and good frequency characteristics such as impedance and Q value.

[0068] Furthermore, in this embodiment, it is preferable that the first continuity ratio A of the first region R1 is 95% or less. This makes it possible to suppress the burden of applying conductive paste to increase the first continuity ratio A and to suppress an increase in the thickness of the first region R1.

[0069] On the other hand, the margin end E2 includes a side end E21 that is in contact with the first and second side margin portions 17a and 17b, and an end end E22 that is in contact with the end margin portion 18. The side end E21 is the end of the margin end E2 that extends, for example, in the X-axis direction. The end end E22 is the end of the margin end E2 that extends, for example, in the Y-axis direction.

[0070] For example, the first region R1 may include a side region R11 that occupies a range within 10% of the width dimension W1 in the Y-axis direction of the internal electrodes 12 and 13, starting from the side end E21, and an end region R12 that occupies a range within 10% of the length dimension L1 in the X-axis direction of the internal electrodes 12 and 13, starting from the end end E22. In this example, the dimension W2 in the Y-axis direction of each side region R11 is 10% of the width dimension W1 of the internal electrodes 12 and 13. The dimension L2 in the X-axis direction of the end region R12 is 10% of the length dimension L2 of the internal electrodes 12 and 13. Note that the width dimension W1 and length dimension L1 of the internal electrodes 12 and 13 are the maximum dimensions in the Y-axis direction and X-axis direction of the internal electrodes 12 and 13, respectively.

[0071] In this example, the second region R2 occupies the area of ​​the internal electrodes 12 and 13 excluding the first region R1. That is, the second region R is located in the center of the internal electrodes 12 and 13 in the Y-axis direction, and its dimension W3 in the Y-axis direction is 80% of the width dimension W1 of the internal electrodes 12 and 13. The dimension L3 of the second region R2 in the X-axis direction is 90% of the length dimension L1 of the internal electrodes 12 and 13.

[0072] By setting the range of the first region R1 in this manner, it is possible to reliably increase the continuity ratio of the region where electric field concentration is likely to occur. Thereby, dielectric breakdown occurring between the side region R11 and / or the end region R12 and the respective opposing external electrodes can be suppressed. In addition, by setting the range of the second region R2 in this manner, the second region R2 occupies a wide range of the internal electrodes 12, 13. As a result, the effect of reducing the difference in sintering behavior between the internal electrodes 12, 13 and the ceramic layer 19 and the effect of enhancing adhesion can be sufficiently obtained, and leakage current caused by delamination and cracks can be effectively suppressed. Therefore, with this configuration, the reliability of the multilayer ceramic capacitor 10 can be further improved.

[0073] Furthermore, in the present embodiment, when a value obtained by omega-transforming the first continuity ratio A of the first region R1 is defined as a, and a value obtained by omega-transforming the second continuity ratio B of the second region R2 is defined as b, it is preferable to satisfy 0 < a - b ≤ 6.8. The omega-transformed values a and b are expressed by the following formulas using the continuity ratios A and B. The unit of A and B is %, and the unit of a and b is db (decibels). a=10×log(A / (100-A)) b=10×log(B / (100-B))

[0074] By evaluating the difference a - b between the values a and b obtained by omega-transforming the continuity ratios A and B, the difference between the continuity ratios A and B can be evaluated on a scale that takes the values of the continuity ratios A and B into consideration. That is, the value of a - b can serve as an index that reflects practical effects more than the value of A - B.

[0075] By making a - b larger than 0, the continuity ratio A can be made larger than the continuity ratio B, and as described above, the reliability of the multilayer ceramic capacitor 10 can be improved. In addition, by setting a - b to 6.8 or less, it is possible to suppress the occurrence of cracks and the like at the interface with the ceramic layer 19 due to a large difference in sintering behavior between the first region R1 and the second region R2. As a result, as shown in the examples described later, the dielectric breakdown voltage (BDV) can be stably increased, and the reliability can be improved.

[0076] Furthermore, by setting ab to between 2.0 and 6.8, the effect of stably increasing BDV can be obtained more reliably, further improving the reliability of the multilayer ceramic capacitor 10.

[0077] Furthermore, if the continuity rate gradually decreases from the first region R1 to the second region R2, stress concentration can be alleviated, further improving the reliability of the multilayer ceramic capacitor 10.

[0078] Furthermore, for example, the thickness of each internal electrode 12, 13 in the second region R2 can be set to, for example, 0.2 μm or more and 0.4 μm or less. This makes it possible to reduce the thickness of the internal electrodes 12, 13 while maintaining the second continuity ratio B of the second region R2 at, for example, 70% or more, thereby enabling miniaturization and increased capacitance of the multilayer ceramic capacitor 10.

[0079] In this embodiment, the thickness of each internal electrode 12, 13 in the first region R1 can be, for example, 1.05 times or more and 1.2 times or less the thickness in the second region R2. By making the thickness in the first region R1 slightly thicker than the thickness in the second region R2, the first continuity ratio A in the first region R1 can be made relatively higher while suppressing distortion of the ceramic body 11 due to thickness imbalance within the internal electrodes 12, 13. Therefore, cracks and the like caused by distortion of the ceramic body 11 can be suppressed, and reliability can be improved more reliably.

[0080] Furthermore, in order to relatively increase the first continuity ratio A of the first region R1, in addition to adjusting the thickness of the first region R1 as described above, the firing conditions may be adjusted, or other methods may be used. The firing conditions will be described later.

[0081] The thickness of the first region R1 and the second region R2 of each internal electrode 12, 13 is the average of the thicknesses measured in the Z-axis direction at multiple locations in each region. As an example, the internal electrodes 12, 13 in a cross-section parallel to the Z-axis direction of the ceramic body 11 are observed using SEM or TEM. A field of view containing six or more layers of the first region R1 and a field of view containing six or more layers of the second region R2 are selected. Six layers are selected from the internal electrodes 12, 13 in each field of view, and the thickness is measured at five evenly spaced locations in each layer. The average of the 30 thicknesses obtained from one field of view is then taken as the thickness of the region included in that field of view. Alternatively, if the dimensions of the multilayer ceramic capacitor 10 in the X-axis direction are, for example, 1 mm or more and easy to handle, the internal electrodes can be removed from the ceramic body 11 after immersion in etching solution and measured with a contact-type thickness gauge. In this case as well, the method for calculating the thickness is the same as above: six layers are selected from the internal electrodes 12, 13, the thickness is measured at five evenly spaced locations in each layer, and the average of the 30 thicknesses obtained is taken as the thickness of the target region.

[0082] [Circuit board configuration] The multilayer ceramic capacitor 10 with the above configuration is mounted, for example, on a circuit board 100. Figure 6 is a cross-sectional view of the circuit board 100 according to this embodiment.

[0083] The circuit board 100 includes a multilayer ceramic capacitor 10 and a mounting board 110 on which the multilayer ceramic capacitor 10 is mounted. The mounting board 110 has a mounting surface 111 that includes lands (connection electrodes) 111a. The external electrodes 14a and 14b of the multilayer ceramic capacitor 10 are connected to the lands 111a, for example, by solder H. As a result, the multilayer ceramic capacitor 10 is mounted on the mounting board 110 with its second main surface 11f facing the mounting surface 111 in the Z-axis direction.

[0084] In such a circuit board 100, a voltage is applied from the mounting board 110 to the external electrodes 14a and 14b. As described above, the multilayer ceramic capacitor 10 of this embodiment can suppress the decrease in insulation resistance, thus improving the reliability of the circuit board 100.

[0085] [Manufacturing method for multilayer ceramic capacitors] Figure 7 is a flowchart showing the manufacturing method of the multilayer ceramic capacitor 10. Figures 8 and 9 show the manufacturing process of the multilayer ceramic capacitor 10. The manufacturing method of the multilayer ceramic capacitor 10 will be described below with reference to these figures.

[0086] (Step S01: Prepare the ceramic sheet) In this step, referring to Figures 8 and 9, a first ceramic sheet 101 and a second ceramic sheet 102 for forming the volume forming section 15, and a third ceramic sheet 103 for forming the cover sections 16a and 16b are formed.

[0087] In this step, the ceramic sheets 101, 102, and 103 are composed of unfired ceramic green sheets without internal electrodes or the like formed on them. First, the materials for the ceramic green sheets are mixed to obtain a slurry. This slurry contains dielectric ceramic powder, binder resin, and organic solvent. The slurry obtained by crushing and mixing these materials is formed into a sheet using a doctor blade method, die coater method, gravure coater method, or the like.

[0088] The thicknesses of the first and second ceramic sheets 101 and 102 are adjusted according to the thickness of the ceramic layer 19 after firing. The thickness of the third ceramic sheet 103 is adjusted as appropriate according to the thickness of the cover portions 16a and 16b after firing.

[0089] (Step S02: Internal electrode pattern formation) In this step, referring to Figure 8, internal electrode patterns 112 and 113 are formed on the first and second ceramic sheets 101 and 102 for forming the capacitance forming section 15.

[0090] The internal electrode patterns 112 and 113 are formed by applying conductive paste to the ceramic sheets 101 and 102. The first internal electrode pattern 112 corresponds to the first internal electrode 12 and is formed on the first ceramic sheet 101. The second internal electrode pattern 113 corresponds to the second internal electrode 13 and is formed on the second ceramic sheet 102.

[0091] The conductive paste used in the internal electrode patterns 112 and 113 includes, for example, conductive powder, a binder resin, and an organic solvent. The conductive powder consists of nickel (Ni), copper (Cu), palladium (Pd), platinum (Pt), silver (Ag), gold (Au), and mixtures or alloys thereof. Furthermore, it is preferable that the conductive paste contains a ceramic material as a co-material. The ceramic material is, for example, a dielectric ceramic powder.

[0092] The ceramic sheets 101, 102, and 103 shown in Figure 8 have cut lines Lx and Ly for separating the ceramic body 11 into individual pieces. Each internal electrode pattern 112 and 113 is configured in a rectangular shape, for example, extending across a single cut line Ly. The second internal electrode pattern 113 is formed offset from the first internal electrode pattern 112 by one chip in the X-axis or Y-axis direction.

[0093] In this embodiment, it is preferable to form the peripheral region Ru1 along the ends of the internal electrode patterns 112 and 113 in the X-axis and Y-axis directions to be thicker than the inner region Ru2 in the X-axis and Y-axis directions. The peripheral region Ru1 corresponds to the first region R1, and the inner region Ru2 corresponds to the second region R2. Specifically, for example, conductive paste may be applied to the peripheral region Ru1 multiple times.

[0094] For example, the thickness of the peripheral region Ru1 in the Z-axis direction can be set to 1.05 times or more and 1.2 times or less the thickness of the inner region Ru2 in the Z-axis direction. This makes it easier to relatively increase the first continuity ratio A in the first region R1 after firing.

[0095] (Step S03: Lamination) In this step, as shown in Figure 9, ceramic sheets 101, 102, and 103 are laminated to create a laminated sheet 104.

[0096] In the laminated sheet 104 shown in Figure 9, ceramic sheets 101 and 102 that form the volume-forming section 15 are stacked alternately, and a third ceramic sheet 103 is stacked above and below them in the Z-axis direction. These ceramic sheets 101, 102, and 103 are integrated by being pressed together. Note that the number of ceramic sheets 101, 102, and 103 is not limited to the example shown in Figure 9.

[0097] (Step S04: Cutting) In this step, an unfired ceramic body 11 is produced by cutting the laminated sheet 104 along the cut lines Lx and Ly. Methods such as push cutting and blade dicing can be used for cutting.

[0098] (Step S05: Firing) In this step, the unfired ceramic body 11 is sintered. This produces the ceramic body 11 shown in Figures 1-3.

[0099] The firing temperature can be determined based on the sintering temperature of the ceramic body 11. For example, when using a barium titanate (BaTiO3)-based material, the firing temperature can be set to approximately 1000-1350°C. Furthermore, firing can be carried out, for example, under a reducing atmosphere or a low oxygen partial pressure atmosphere.

[0100] In this embodiment, in addition to increasing the thickness of the peripheral region Ru1 as described above, a first region R1 with relatively high continuity can be formed by adjusting the firing conditions as follows. Specifically, during the heating process, it is preferable to maintain a low temperature range (e.g., 800°C or below) where shrinkage of the internal electrodes does not begin for a long period of time (e.g., 95 minutes or more). This allows for sufficient removal of organic matter from the conductive paste. Furthermore, in the high temperature range (e.g., 800-1350°C) where shrinkage of the internal electrodes begins and sintering progresses, it is preferable to shorten the firing time. It is also preferable to use a stronger reducing atmosphere in the high temperature range than in the low temperature range. By making such adjustments in the high temperature range, spheroidization in the first region R1 of the internal electrodes 12 and 13 can be suppressed.

[0101] (Step S06: External electrode formation) In this step, a multilayer ceramic capacitor 10, as shown in Figures 1-3, is fabricated by forming external electrodes 14a and 14b on both ends of the ceramic body 11 in the X-axis direction after firing. The method for forming the external electrodes 14a and 14b in this step can be arbitrarily selected from known methods. For example, a conductive paste is applied to both ends of the ceramic body 11 in the X-axis direction and fired to form a base film. Subsequently, one or more plating films are formed on this base film.

[0102] Through the above steps, the multilayer ceramic capacitor 10 shown in Figures 1 to 3 is manufactured. Note that the manufacturing method in this embodiment is not limited to the example described above. For example, the application of the conductive paste in step 06 may be performed before the firing process in step S05. This allows for the formation of the undercoat of the external electrodes simultaneously with the firing of the ceramic body 11.

[0103] [Examples and Comparative Examples] Examples and comparative examples of the above embodiments will now be described. In Examples 1 to 6, samples of multilayer ceramic capacitors were prepared under the condition that the continuity ratio A of the first region of the internal electrode was greater than the continuity ratio B of the second region. In Comparative Example 1, a sample of a multilayer ceramic capacitor was prepared under the condition that the continuity ratio A of the first region of the internal electrode was smaller than the continuity ratio B of the second region. The continuity ratios A and B were adjusted by the thickness of the peripheral region of the internal electrode pattern and the firing conditions.

[0104] In Examples 1-6 and Comparative Example 1, the size of the multilayer ceramic capacitor sample was 0.4 mm × 0.2 mm × 0.2 mm. Furthermore, in Examples 1-6 and Comparative Example 1, the configuration of the multilayer ceramic capacitor sample was substantially the same except for the continuity ratios A and B.

[0105] The continuity rates A and B for Examples 1-6 and Comparative Example 1 were calculated using the method of immersing the multilayer ceramic capacitor in hydrofluoric acid (etching solution) as described in the above embodiment. The calculated continuity rates A and B were then converted to omega values ​​to obtain a and b. The values ​​for Examples 1-6 and Comparative Example 1 are shown in Table 1.

[0106] [Table 1]

[0107] (Evaluation of dielectric breakdown voltage) Next, the dielectric breakdown voltage (BDV) was measured using 20 samples each from Examples 1-6 and Comparative Example 1. The BDV was measured by applying a DC voltage at a rate of 10V / second. The relationship between ab and BDV for each of Examples 1-6 and Comparative Example 1 was analyzed using the Weibull distribution method. Then, for each of Examples 1-6 and Comparative Example 1, the Weibull distribution parameters, Weibull α and Weibull β, were calculated. These results are shown in Table 1 and Figure 10. Weibull-α represents the quantile at which the cumulative failure rate is 63.2%. Weibull-β is a value that determines how the hazard (instantaneous failure rate) changes over time.

[0108] As shown in Table 1 and Figure 10, the Weibull α of Comparative Example 1, where the continuity rate A of the first region was smaller than the continuity rate B of the second region and ab was -1.1, was 289V. In contrast, the Weibull α of Examples 1 to 6, where the continuity rate A of the first region was larger than the continuity rate B of the second region, was 294V or higher. This indicates that the samples of Examples 1 to 6 tended to have a higher BDV than the sample of Comparative Example 1.

[0109] As shown in Table 1 and Figure 10, the Weibull β of Comparative Example 1, where the continuity A of the first region was smaller than the continuity B of the second region and ab was -1.1, was 6.1. In contrast, the Weibull β of Examples 1 to 6, where the continuity A of the first region was larger than the continuity B of the second region, was 7.8 or higher. Since a larger Weibull β results in smaller BDV variability, the above results indicate that the samples of Examples 1 to 6 exhibited smaller BDV variability and were more likely to yield a stable BDV than the sample of Comparative Example 1.

[0110] Furthermore, in Examples 3-5, where ab was between 2.0 and 6.8, the Weibull β was 15 or higher in all cases, indicating that the variability in BDV can be further reduced.

[0111] These results indicate that the samples in Examples 1-6 exhibited less reduction in insulation resistance and improved reliability compared to the sample in Comparative Example 1.

[0112] [Other embodiments] Although embodiments of the present invention have been described above, the present invention is not limited to the embodiments described above, and various modifications can be made without departing from the spirit of the present invention.

[0113] For example, the dimension of the multilayer ceramic capacitor in the Z-axis direction may be larger than at least one of the dimensions of the multilayer ceramic capacitor in the X-axis direction or the Y-axis direction. In other words, the multilayer ceramic capacitor according to the present invention may be a tall type, with a larger ratio of the dimension in the Z-axis direction than the size exemplified in the above embodiment.

[0114] In such tall-profile multilayer ceramic capacitors, the capacitance-forming portion, including the internal electrodes, becomes thicker in the Z-axis direction, making it prone to significant stress due to differences in sintering behavior between the internal electrodes and the surrounding ceramic portion. Furthermore, in the above configuration, the number of internal electrode layers increases, making the cost of the conductive material used for the internal electrodes a more significant factor.

[0115] Therefore, in the above configuration, by making the first continuity ratio A of the first region of the internal electrode higher than the second continuity ratio B of the second region, dielectric breakdown in the first region can be suppressed. Furthermore, by relatively lowering the second continuity ratio B of the second region, cracks and the like associated with the above stress can be suppressed, leakage current can be suppressed, and the cost of conductive materials can be reduced.

[0116] Furthermore, while increasing the thickness of the first region R1 and adjusting the firing conditions were mentioned as methods to relatively increase the continuity ratio A of the first region R1, the method is not limited to this. For example, conductive pastes with different amounts of ceramic material in the first region R1 and the second region R2 may be used. In this case, for example, the amount of ceramic material in the conductive paste for forming the first region R1 (peripheral region Ru1) can be made less than the amount of ceramic material in the conductive paste for forming the second region R2 (inner region Ru2). For example, when the main material of the conductive paste for forming the first region R1 (peripheral region Ru1) and the second region R2 (inner region Ru2) is Ni, at least one of the following additives may be added only to the first region R1 (peripheral region Ru1): silver (Ag), chromium (Cr), iridium (Ir), magnesium (Mg), molybdenum (Mo), osmium (Os), palladium (Pd), platinum (Pt), rhenium (Re), rhodium (Rh), ruthenium (Ru), yttrium (Y), or tungsten (W). Alternatively, the above additives may be added to both the first region R1 (peripheral region Ru1) and the second region R2 (inner region Ru2). In this case, the content of the above additives in the first region R1 may be adjusted to be greater than that in the second region R2. [Explanation of Symbols]

[0117] 10 Multilayer ceramic capacitors 11a,11b end face 12,13 Internal electrode 14a,14b External electrode 15 Capacity forming part 16a, 16b Cover section 17, 17a, 17b Side margin section 18, 18a, 18b End margin section M Margin Section 19 Ceramic layer E end E1 Drawer end E2 Margin End E21 Side End E22 End section R1 1st area R11 Side Area R12 End Region R2 2nd area

Claims

1. First and second end faces perpendicular to the first axial direction, A capacitance forming section comprising: a first internal electrode drawn out from the first end face; a second internal electrode drawn out from the second end face and facing the first internal electrode in a second axial direction perpendicular to the first axis; and a ceramic layer disposed between the first and second internal electrodes. A margin portion including a first end margin portion disposed between the first end face and the second internal electrode, a second end margin portion disposed between the second end face and the first internal electrode, and first and second side margin portions disposed on both sides of the capacitance forming portion in the third axial direction perpendicular to the first and second axes, A ceramic body having, First and second external electrodes covering the first and second end faces, respectively, It is equipped with, The first and second internal electrodes are, respectively, An end comprising a lead-out end in contact with the first or second external electrode and a margin end in contact with the margin portion, The continuity rate of the conductive component in a plan view from the second axial direction is the first continuity rate, and the first region is arranged along the margin end, The continuous rate of the conductive component in the plan view is a second continuous rate which is lower than the first continuous rate, and the second region is located inward from the first region in the first axial direction and the third axial direction, Let a be the value obtained by omega transformation of the first continuity rate, and b be the value obtained by omega transformation of the second continuity rate, then satisfy 0 < a - b ≤ 6.

8. Multilayer ceramic capacitor.

2. A multilayer ceramic capacitor according to claim 1, The margin end includes a pair of side ends that are in contact with the first and second side margin portions, and an end end that is in contact with the first or second end margin portion. The first region is, From each of the pair of side ends, a pair of side regions located within 10% of the width dimension in the third axial direction of each of the first and second internal electrodes, The end region includes, located within 10% of the length dimension of the first and second internal electrodes in the first axial direction from the end end, The second region occupies the region of each of the first and second internal electrodes excluding the first region. Multilayer ceramic capacitor.

3. A multilayer ceramic capacitor according to claim 2, The first continuity rate is a value measured in the end region and / or the side region of the first region. Multilayer ceramic capacitor.

4. A multilayer ceramic capacitor according to any one of claims 1 to 3, The aforementioned second consecutive rate is 70% or higher. Multilayer ceramic capacitor.

5. A multilayer ceramic capacitor according to any one of claims 1 to 4, The first and second consecutive rates are, respectively, This is calculated as the ratio of the area of ​​the undissolved conductive component per unit area in each of the first and second regions after immersing the ceramic body in an etching solution that dissolves the ceramics but does not dissolve the conductive component. Multilayer ceramic capacitor.

6. A multilayer ceramic capacitor according to any one of claims 1 to 5, The conductive component includes nickel, copper, palladium, platinum, silver, gold, tin, or alloys thereof. Multilayer ceramic capacitor.

7. A multilayer ceramic capacitor according to claim 6, The first region contains, as an additive, at least one of the following: silver, chromium, iridium, magnesium, molybdenum, osmium, palladium, platinum, rhenium, rhodium, ruthenium, yttrium, and tungsten. Multilayer ceramic capacitor.

8. A multilayer ceramic capacitor according to any one of claims 1 to 7, The thickness of the second region in the second axial direction is 0.2 μm or more and 0.4 μm or less. Multilayer ceramic capacitor.

9. A multilayer ceramic capacitor according to any one of claims 1 to 8, The dimension of the multilayer ceramic capacitor in the first axial direction is 0.4 mm or less. The dimension of the multilayer ceramic capacitor in the third axial direction is 0.2 mm or less. Multilayer ceramic capacitor.

10. A multilayer ceramic capacitor according to any one of claims 1 to 9, The dimensions of each of the first and second side margin portions in the third axial direction are 30 μm or less. Multilayer ceramic capacitor.

11. A multilayer ceramic capacitor according to any one of claims 1 to 10, The dimensions of the first and second end margin portions in the first axial direction are 30 μm or less. Multilayer ceramic capacitor.

12. A multilayer ceramic capacitor according to any one of claims 1 to 11, The thickness of the ceramic layer is 0.2 μm or more and 0.5 μm or less. Multilayer ceramic capacitor.

13. A multilayer ceramic capacitor according to any one of claims 1 to 12, The dimension of the multilayer ceramic capacitor in the second axial direction is greater than at least one of the dimensions of the multilayer ceramic capacitor in the first axial direction or the dimensions of the multilayer ceramic capacitor in the third axial direction. Multilayer ceramic capacitor.

14. Multilayer ceramic capacitors, A mounting substrate on which the multilayer ceramic capacitor is mounted, It is equipped with, The aforementioned multilayer ceramic capacitor is First and second end faces perpendicular to the first axial direction, A capacitance forming section comprising: a first internal electrode drawn out from the first end face; a second internal electrode drawn out from the second end face and facing the first internal electrode in a second axial direction perpendicular to the first axis; and a ceramic layer disposed between the first and second internal electrodes. A margin portion including a first end margin portion disposed between the first end face and the second internal electrode, a second end margin portion disposed between the second end face and the first internal electrode, and first and second side margin portions disposed on both sides of the capacitance forming portion in the third axial direction perpendicular to the first and second axes, A ceramic body having, The first and second end faces are covered, respectively, and the first and second external electrodes are connected to the mounting substrate, It has, The first and second internal electrodes are, respectively, An end comprising a lead-out end in contact with the first or second external electrode and a margin end in contact with the margin portion, The continuity rate of the conductive component in a plan view from the second axial direction is the first continuity rate, and the first region is arranged along the margin end, The continuous rate of the conductive component in the plan view is a second continuous rate which is lower than the first continuous rate, and the second region is located inward from the first region in the first axial direction and the third axial direction, Let a be the value obtained by omega transformation of the first continuity rate, and b be the value obtained by omega transformation of the second continuity rate, then satisfy 0 < a - b ≤ 6.

8. Circuit board.

Citation Information

Patent Citations

  • Multilayer ceramic chip capacitor and manufacture thereof

    JP1991133115A

  • Multilayer ceramic capacitor

    JP1993275271A

  • Laminated ceramic electronic component and its manufacturing method

    JP2002359140A

  • Stacked type ceramic capacitor and its manufacturing method

    JP2004111489A

  • Laminated electronic component and its manufacturing method

    JP2004179349A