Block polymer, coating agent, and method for producing block polymer

A block polymer with polyolefin and radically polymerizable monomers, using a macropolymerization initiator, addresses adhesion issues between polyolefin and polar substrates, enhancing bonding stability and efficiency.

JP7954515B2Active Publication Date: 2026-11-20MITSUI CHEMICALS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022057515
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-03-30
Publication Date
2026-11-20
Estimated Expiration
2042-03-30

AI Technical Summary

Technical Problem

Conventional polyolefin adhesive resins exhibit insufficient adhesion to polyolefin base materials, limiting their effectiveness in bonding with polar resin materials.

Method used

A block polymer comprising a polyolefin block and a polymer of radically polymerizable monomers, with iodine atoms, is produced using a macropolymerization initiator, enhancing adhesion to both polyolefin and polar substrates.

Benefits of technology

The block polymer improves adhesion to polyolefin substrates and substrates with different polarities, ensuring stable bonding and reliable production by minimizing unreacted initiators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954515000017
    Figure 0007954515000017
  • Figure 0007954515000001
    Figure 0007954515000001
  • Figure 0007954515000002
    Figure 0007954515000002
Patent Text Reader

Abstract

To provide: a block polymer capable of improving adhesion to a polyolefin base material; a coating agent; and a method for producing a block polymer.SOLUTION: There is provided a block polymer which has a first block comprising a polyolefin, a second block comprising a polymer of a radical polymerizable monomer and iodine atoms and is represented by the following formula. (In the formula, P1 represents a first block and P2 represents a second block, R1 represents any one of hydrogen atoms, an aliphatic group, an aromatic group, an alkoxycarbonyl group and a nitrile group, R2 represents any one of a carbonyloxy group, an alkylene group and a phenylene group.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a block polymer, a coating agent, and a method for producing a block polymer.

Background Art

[0002] Conventionally, as an adhesive layer for bonding a polyolefin base material and a polar resin material (acrylic, PET), a laminate of a layer containing a polyolefin adhesive resin and a layer containing a polar adhesive resin has been proposed (for example, see Patent Document 1.).

[0003] The polyolefin adhesive resin has adhesiveness to a polyolefin base material. The polar adhesive resin has adhesiveness to a polar resin material. As the polyolefin adhesive resin, a maleic anhydride-modified propylene·1-butene copolymer is preferably mentioned.

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0005] The polyolefin adhesive resin described in Patent Document 1 may have insufficient adhesion to a polyolefin base material in some cases.

[0006] The present invention provides a block polymer, a coating agent, and a method for producing a block polymer, which can achieve improved adhesion to a polyolefin base material.

Means for Solving the Problems

[0007] The present invention [1] includes a block polymer represented by the following general formula (1), having a first block made of a polyolefin, a second block made of a polymer of radically polymerizable monomers, and an iodine atom.

[0008] General formula (1):

[0009] [ka]

[0010] (In general formula (1), P1 represents a first block consisting of polyolefins. P2 represents a second block consisting of a polymer of radically polymerizable monomers. 1 R represents one of the following: a hydrogen atom, an aliphatic group, an aromatic group, an alkoxycarbonyl group, or a nitrile group. 2 This represents one of the following groups: carbonyloxy group, alkylene group, and phenylene group. Two R 1 They may be the same or they may be different. n is an integer greater than or equal to 1. The present invention [2] relates to the general formula (1) above, where R 1 is a methyl group, R 2 The above [1] includes a block polymer in which is a carbonyloxy group.

[0011] The present invention [3] comprises the block polymer of [1] or [2] above, wherein the polyolefin is a propylene-1-butene copolymer and the radical polymerizable monomer has an acrylic group or a methacrylic group.

[0012] The present invention [4] comprises a coating agent containing any one of the block polymers described in [1] to [3] above.

[0013] The present invention [5] is a method for producing any one of the block polymers described in [1] to [4] above, comprising polymerizing a radical polymerizable monomer using a macropolymerization initiator represented by the following general formula (2) in the presence of iodine and a catalyst.

[0014] General formula (2):

[0015] [ka]

[0016] (In general formula (1), P1 represents polyolefin. 1 R represents one of the following: a hydrogen atom, an aliphatic group, an aromatic group, an alkoxycarbonyl group, or a nitrile group. 2 This represents one of the following groups: carbonyloxy group, alkylene group, and phenylene group. Two R 1 They may be the same or they may be different. n is an integer greater than or equal to 1. [Effects of the Invention]

[0017] The block polymer of the present invention has a first block made of polyolefin.

[0018] Therefore, it is possible to improve adhesion to polyolefin substrates.

[0019] Furthermore, the second block, which consists of a polymer of radically polymerizable monomers, can improve adhesion even to polymers having a different polarity from the polyolefin substrate.

[0020] As a result, it is possible to improve the adhesion between the polyolefin substrate and a substrate having a different polarity from the polyolefin substrate.

[0021] Furthermore, according to the method for producing block polymers, by polymerizing a radical polymerizable monomer in the presence of iodine using a macropolymerization initiator represented by general formula (2), the radical polymerizable monomer can be reliably reacted with the macropolymerization initiator.

[0022] As a result, block polymers represented by general formula (1) can be stably produced while suppressing the retention of unreacted macropolymerization initiators. [Brief explanation of the drawing]

[0023] [Figure 1] Figure 1 is a graph showing the change in the GPC peak of a block polymer over time during the manufacturing of a block polymer. [Modes for carrying out the invention]

[0024] 1. Macropolymerization initiator Macropolymerization initiators can be used in living radical polymerization. Macropolymerization initiators have a main chain made of polyolefin and have iodine atoms at their terminals as protecting groups. Macropolymerization initiators may also have iodine atoms in the side chains of the polyolefin.

[0025] Specifically, macropolymerization initiators are represented by the following general formula (2). Macropolymerization initiators generate radicals by cleaving the bond between an iodine atom and a carbon atom.

[0026] General formula (2):

[0027] [ka]

[0028] In general formula (2), P1 represents polyolefin.

[0029] Examples of polyolefins include polyethylene, polypropylene, polybutene, polybutadiene, polymethylpentene, α-olefin copolymers, ethylene-propylene-diene copolymers, cyclic olefin copolymers, conjugated diene copolymers, and modified versions thereof.

[0030] Examples of the α-olefin copolymer include an ethylene-propylene copolymer, an ethylene-propylene-1-butene copolymer, and a propylene-1-butene copolymer.

[0031] Examples of the modified product include a graft modified product. Examples of the graft modified product include a maleic anhydride modified product.

[0032] The polyolefin preferably includes polybutadiene and an α-olefin copolymer, and more preferably includes hydrogenated polybutadiene and a propylene-1-butene copolymer.

[0033] In general formula (2), R 1 represents any one of a hydrogen atom, an aliphatic group, an aromatic group, an alkoxycarbonyl group, and a nitrile group.

[0034] Examples of the aliphatic group include a linear alkyl group having 1 to 12 carbon atoms, or a branched alkyl group having 3 to 12 carbon atoms.

[0035] Examples of the linear alkyl group having 1 to 12 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, and an n-dodecyl group.

[0036] Examples of the branched alkyl group having 3 to 12 carbon atoms include an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, and a 2-ethylhexyl group.

[0037] The aliphatic group may be substituted. The aliphatic group is preferably unsubstituted.

[0038] When the aliphatic group is substituted, the number of substituents is not limited. The aliphatic group may have one substituent, or a plurality of substituents.

[0039] Examples of substituents include halogen atoms, linear or branched alkyl groups having 1 to 12 carbon atoms, aromatic hydrocarbon groups, non-aromatic heterocyclic groups, linear or branched alkoxy groups having 1 to 12 carbon atoms, cyano groups, and nitro groups. Alkyl groups, aromatic hydrocarbon groups, and non-aromatic heterocyclic groups as substituents may also be substituted.

[0040] Examples of aromatic groups include aromatic hydrocarbon groups or aromatic heterocyclic groups.

[0041] Examples of aromatic hydrocarbon groups include phenyl, biphenylyl, terphenylyl, naphthyl, binaphthyryl, azulenyl, anthracenyl, and phenantrenyl groups.

[0042] Examples of aromatic heterocyclic groups include furyl, thienyl, pyrrolyl, pyrazolyl, imidazolyl, isoxazolyl, thiazolyl, thiadiazolyl, pyridyl, pyrazinyl, pyrimidinyl, pyridadinyl, benzofuryl, indolyl, quinolyl, isoquinolyl, quinazolinyl, quinoxalinyl, synnolinyl, benzothiazolyl, carbazolyl, phenanthridine, phenazinyl, phenoxazinyl, and phenothiazinyl groups.

[0043] Two R's 1 They may be the same or they may be different from each other. Preferably, two R 1 Both are unsubstituted methyl groups.

[0044] In general formula (2), R 2 This represents one of the following: a carbonyloxy group, an alkylene group, or a phenylene group.

[0045] Examples of alkylene groups include linear alkylene groups having 1 to 12 carbon atoms, branched alkylene groups having 2 to 12 carbon atoms, or cycloalkylene groups having 3 to 12 carbon atoms.

[0046] Examples of linear alkylene groups having 1 to 12 carbon atoms include methylene, 1,2-ethylene, 1,3-propylene, 1,4-butylene, 1,5-pentylene, 1,6-hexylene, 1,7-heptylene, 1,8-octylene, 1,9-nonylene, 1,10-decylene, 1,11-undecylene, and 1,12-dodecylene.

[0047] Examples of branched alkylene groups having 2 to 12 carbon atoms include 1,1-ethylene, 1,1-propylene, 1,2-propylene, 2,2-propylene, 1,1-butylene, 1,2-butylene, 1,3-butylene, 2,2-butylene, and 2,3-butylene.

[0048] Examples of cycloalkylene groups having 4 to 12 carbon atoms include 1,1-cyclopropyl, 1,2-cyclopropyl, 1,1-cyclobutyl, 1,2-cyclobutyl, 1,3-cyclobutyl, 1,1-cyclopentyl, 1,2-cyclopentyl, and 1,3-cyclopentyl groups.

[0049] Preferably, R 2 This is a carbonyloxy group.

[0050] In general formula (2), n is an integer greater than or equal to 1. For example, n is 10 or less, preferably 2 or less.

[0051] 2. Effects of macropolymerization initiators The macropolymerization initiator represented by general formula (2) has a portion consisting of a polyolefin.

[0052] Therefore, by using a macropolymerization initiator, block polymers having blocks made of polyolefin can be easily produced.

[0053] 3. Method for producing macropolymerization initiators Next, we will describe an example of a method for producing a macropolymerization initiator.

[0054] A method for producing a macropolymerization initiator includes a preparation step and an introduction step.

[0055] (1) Preparation process The preparation process involves preparing hydroxypolyolefins. Hydroxypolyolefins are polyolefins that have hydroxyl groups. The preparation process includes a first preparation step, a second preparation step, and a third preparation step. Commercially available hydroxypolyolefins may be purchased for the preparation process.

[0056] (1-1) First preparation process In the first preparation step, a polyolefin is prepared. The polyolefin can be purchased commercially or synthesized. The polyolefin prepared in the first preparation step does not have polar groups or polar bonds. Examples of polar groups include hydroxyl groups, carboxyl groups, and alkoxy groups. Examples of polar bonds include ether bonds and ester bonds.

[0057] To synthesize polyolefins, for example, olefin monomers are polymerized in the presence of a known metallocene catalyst.

[0058] Examples of metallocene catalysts include dimethylmethylene (3-tert-butyl-5-methylcyclopentadienyl)fluorenylzirconium dichloride as the metallocene, and a combination of methylaluminoxane and triisobutylaluminum as co-catalysts.

[0059] Examples of olefin monomers include α-olefins, cyclic olefins, and conjugated dienes.

[0060] Examples of α-olefins include linear or branched α-olefins having 2 to 20 carbon atoms. Examples of linear or branched α-olefins having 2 to 20 carbon atoms include ethylene, propylene, 1-butene, 2-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene.

[0061] Examples of cyclic olefins include cyclic olefins having 4 to 20 carbon atoms. Examples of cyclic olefins having 4 to 20 carbon atoms include cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, and tetracyclododecene.

[0062] Examples of conjugated dienes include aliphatic conjugated dienes having 4 to 20 carbon atoms. Examples of aliphatic conjugated dienes having 4 to 20 carbon atoms include 1,3-butadiene, isoprene, chloroprene, 1,3-cyclohexadiene, 1,3-pentadiene, 4-methyl-1,3-pentadiene, 1,3-hexadiene, and 1,3-octadiene.

[0063] (1-2) Second preparation process In the second preparation step, ethylenically unsaturated groups are introduced into the polyolefin prepared in the first preparation step.

[0064] Methods for introducing ethylenically unsaturated groups include, for example, pyrolysis, high-pressure methods, and polymerization of compounds having ethylenically unsaturated groups using a Ziegler catalyst or a metallocene catalyst.

[0065] Examples of Ziegler catalysts include the magnesium-supported titanium catalysts described in Japanese Patent Publication No. 57-63310, Japanese Patent Publication No. 58-83006, Japanese Patent Publication No. 3-706, Japanese Patent No. 3476793, Japanese Patent Publication No. 4-218508, and Japanese Patent Publication No. 2003-105022.

[0066] Examples of metallocene catalysts include those described in International Publication No. 01 / 53369, International Publication No. 01 / 27124, International Publication No. 2004 / 087775, Japanese Patent Publication No. 3-193796, and Japanese Patent Publication No. 02-41303.

[0067] Preferably, ethylenically unsaturated groups are introduced to the polyolefin by a thermal decomposition method.

[0068] In the pyrolysis method, polyolefins are heated in a pyrolysis apparatus and decomposed. This allows for the introduction of vinylidene groups, an example of ethylenically unsaturated groups, into the polyolefins.

[0069] The heating temperature in the pyrolysis apparatus is, for example, 300°C or higher, preferably 350°C or higher, and for example, 500°C or lower, preferably 450°C or lower.

[0070] The heating time in the pyrolysis apparatus is, for example, 1 hour or more, preferably 3 hours or more, and for example, 8 hours or less, preferably 5 hours or less.

[0071] The functional group equivalent of vinylidene groups can be adjusted by controlling the heating temperature and heating time.

[0072] (1-3) Third preparation process In the third preparation step, the ethylenically unsaturated groups introduced in the second preparation step are replaced with hydroxyl groups.

[0073] To replace ethylenically unsaturated groups introduced into polyolefins with hydroxyl groups, for example, the ethylenically unsaturated groups can be hydroborated and oxidized.

[0074] More specifically, boron is introduced into the polyolefin by reacting an alkylborane with an ethylenically unsaturated group.

[0075] Examples of alkylboranes include 9-borabicyclo[3.3.1]nonane, diciamilborane, texylborane, dicyclohexylborane, catecholborane, pinacolborane, and diisopinocamphaylborane.

[0076] Next, the boron-introduced polyolefin is reacted with hydrogen peroxide in the presence of a base to replace the boron introduced into the polyolefin with a hydroxyl group. This yields a hydroxypolyolefin. Sodium hydroxide can be used as a base, for example.

[0077] In more detail, first, a polyolefin into which ethylenically unsaturated groups have been introduced is dissolved in a solvent, and alkylborane is added to the resulting solution and stirred for, for example, 30 minutes or more, preferably 1 hour or more, for example, 5 hours or less, preferably 3 hours or less.

[0078] As a result, alkylborane reacts with the ethylenically unsaturated groups of the polyolefin, introducing boron into the polyolefin.

[0079] Next, the solution is mixed with a base and hydrogen peroxide, and stirred for, for example, 12 hours or more, preferably 20 hours or more, for example, 48 hours or less, preferably 30 hours or less.

[0080] As a result, the boron introduced into the polyolefin is replaced by a hydroxyl group.

[0081] Afterward, the product is washed to obtain hydroxypolyolefin.

[0082] Furthermore, if necessary, the obtained hydroxypolyolefin may be modified (for example, modified with maleic anhydride).

[0083] (2) Introduction process In the introduction process, the terminal structure shown in the following general formula (3) is introduced into the polyolefin.

[0084] General formula (3):

[0085] [ka]

[0086] In general formula (3), R 1 R in the above general formula (2) is 1 This is the same as. In other words, in general formula (2), R 1 R represents one of the following: a hydrogen atom, an aliphatic group, an aromatic group, an alkoxycarbonyl group, or a nitrile group. 1 They may be the same, or they may be different from one another.

[0087] Specifically, in the introduction step, the hydroxypolyolefin obtained in the preparation step is reacted with the compound represented by the following general formula (4).

[0088] General formula (4):

[0089] [ka]

[0090] In general formula (4), R 1 R in the above general formula (2) is 1 It is the same as. In other words, in general formula (4), R 1 R represents one of the following: a hydrogen atom, an aliphatic group, an aromatic group, an alkoxycarbonyl group, or a nitrile group. 1 They may be the same, or they may be different from one another.

[0091] In general formula (4), R 3 This represents one of the following: a hydroxyl group, an alkoxy group, or a halogen atom.

[0092] In the introduction step, for example, as shown in the reaction equation (A) below, hydroxypolyolefin (P1-OH) is dissolved or suspended in a solvent, and in the presence of a condensing agent, α-iodocarboxylic acid (I-CR) is used. 1 It undergoes a condensation reaction with 2-COOH.

[0093] Reaction equation (A):

[0094] [ka]

[0095] In reaction equation (A), R 1 R in the above general formula (2) is 1 It is the same as this.

[0096] In the introductory step, first, the hydroxypolyolefin is dissolved or suspended in a solvent. Next, α-iodocarboxylic acid and a condensing agent are added to the resulting solution or suspension. If necessary, a nucleophilic compound may be added to the solution or suspension.

[0097] The amount of α-iodocarboxylic acid added is, for example, 1 equivalent or more, for example, 10 equivalents or less, preferably 3 equivalents or less, relative to the hydroxyl groups of the hydroxypolyolefin.

[0098] The amount of condensing agent added is, for example, 1 equivalent or more, for example, 10 equivalents or less, preferably 3 equivalents or less, relative to the hydroxyl groups of the hydroxypolyolefin.

[0099] When adding a nucleophilic compound, the amount of the nucleophilic compound added is, for example, 0.01 equivalents or more, preferably 0.05 equivalents or more, for example 5 equivalents or less, preferably 2 equivalents or less, relative to the hydroxyl groups of the hydroxypolyolefin.

[0100] Next, the solution or suspension is stirred at, for example, -40°C or higher, preferably -20°C or higher, for example 150°C or lower, preferably 100°C or lower, for, for example 5 minutes or more, preferably 15 minutes or more, for, for example 48 hours or less, preferably 24 hours or less.

[0101] This causes a condensation reaction between the hydroxyl group of the hydroxypolyolefin and the carboxyl group of the α-iodocarboxylic acid.

[0102] Examples of condensing agents include carbodiimide, carbodiimidazole, phosgene derivatives, phosphonium, uronium, and triflate reagents.

[0103] Examples of carbodiimides include N,N-dicyclohexylcarbodiimide, N,N-diisopropylcarbodiimide, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide.

[0104] Examples of carbodiimidazoles include carbonyldiimidazole and 1,1'-carbonyldi(1,2,4-triazole).

[0105] Examples of phosgene derivatives include triphosgene, thiophosgene, and di(N-succinimidyl) carbonate.

[0106] Examples of phosphoniums include BOP and BroP.

[0107] Examples of uronium include HATU and TATU.

[0108] Examples of triflate reagents include 4-nitrophenyl trifluoromethanesulfonic acid and trifluoromethanesulfonic acid chloride.

[0109] Furthermore, examples of condensing agents include chloroformate esters, p-toluenesulfonate chloride, 2,4,6-trichlorobenzoate chloride, and 2-chloro-1-methylpyridinium iodide.

[0110] Examples of nucleophilic compounds include pyridine compounds, imidazole compounds, amine compounds, N-hydroxysuccinimide, and 1-hydroxybenzotriazole. Examples of pyridine compounds include pyridine, N,N-dimethyl-4-aminopyridine, and 4-pyrrolidinopyridine. Examples of imidazole compounds include imidazole and 1-methylimidazole. Examples of amine compounds include triethylamine.

[0111] The solvent is not limited as long as it can be used in the condensation reaction. Examples of solvents include halogen solvents, ether solvents, hydrocarbon solvents, and aprotic polar solvents. Examples of halogen solvents include dichloromethane and chloroform. Examples of ether solvents include tetrahydrofuran and diethyl ether. Examples of hydrocarbon solvents include toluene and benzene. Examples of aprotic polar solvents include acetonitrile and dimethylformamide.

[0112] This makes it possible to obtain a macropolymerization initiator.

[0113] In the introduction step, as shown in the following reaction equation (B), hydroxypolyolefin (P1-OH) and α-halogenated carboxylic acid (X-CR) are reacted. 1 The precursor of the macropolymerization initiator (X-CR) is obtained by condensation reaction with 2-COOH. 1 It is also possible to synthesize 2-COO-P1) and then replace the halogen atom (X) of the precursor of the obtained macropolymerization initiator with an iodine atom by a halogen exchange reaction such as the Finkelstein reaction to obtain the macropolymerization initiator.

[0114] Reaction equation (B):

[0115] [ka]

[0116] In reaction equation (B), R1 R in the above general formula (2) is 1 This is the same as the following: X is a halogen atom other than iodine. Examples of halogen atoms include chlorine and bromine.

[0117] Furthermore, in the introduction process, as shown in the following reaction equation (C), hydroxypolyolefin (P1-OH) and α-iodoester (I-CR) are reacted. 1 2-COOR 4 A macropolymerization initiator can also be obtained through a transesterification reaction with ).

[0118] Reaction equation (C):

[0119] [ka]

[0120] In reaction equation (C), R 1 R in the above general formula (2) is 1 It is the same as R 4 It is an alkyl group.

[0121] Furthermore, in the introduction process, as shown in the following reaction equation (D), hydroxypolyolefin (P1-OH) and α-halogenated ester (X-CR) are reacted. 1 2-COOR 4 ) is transesterified to form a precursor of a macropolymerization initiator (X-CR 1 It is also possible to synthesize 2-COO-P1) and then obtain a macropolymerization initiator by substituting the halogen atom (X) of the precursor of the obtained macropolymerization initiator with an iodine atom through a halogen exchange reaction.

[0122] Reaction equation (D):

[0123] [ka]

[0124] In reaction equation (D), R 1 R in the above general formula (2) is 1It is the same as. X is the same as X in the above reaction equation (B). R 4 R in the above reaction equation (C) is 4 It is the same as this.

[0125] Furthermore, in the introduction step, as shown in the following reaction equation (E), hydroxypolyolefin (P1-OH) and α-iodocarboxylic acid halide (I-CR) are reacted. 1 A macropolymerization initiator can also be obtained by reacting it with 2-CO-X'. In this case, a condensing agent is not required.

[0126] Reaction equation (E):

[0127] [ka]

[0128] In reaction equation (E), R 1 R in the above general formula (2) is 1 It is the same as [the given expression]. X' is a halogen atom. Examples of halogen atoms include chlorine and bromine.

[0129] Furthermore, in the introduction process, as shown in the following reaction equation (F), hydroxypolyolefin (P1-OH) and α-halogenated carboxylic acid halide (X-CR) are reacted. 1 The precursor of the macropolymerization initiator (X-CR) is obtained by reacting it with 2-CO-X'. 1 Alternatively, 2-COO-P1) can be synthesized, and the halogen atom (X) of the precursor of the obtained macropolymerization initiator can be replaced with an iodine atom by a halogen exchange reaction to obtain the macropolymerization initiator. In this case as well, a condensing agent is not required.

[0130] Reaction equation (F):

[0131] [ka]

[0132] In reaction equation (F), R 1 R in the above general formula (2) is1 It is the same as above. X is the same as X in reaction equation (B) above. X' is the same as X' in reaction equation (E) above.

[0133] 4. Effects of the method for producing macropolymerization initiators According to the method for producing macropolymerization initiators, a macropolymerization initiator represented by general formula (2) can be easily produced by introducing the terminal structure represented by general formula (3) into a polyolefin.

[0134] 5. Variations of the method for producing macropolymerization initiators R in general formula (2) 2 A macropolymerization initiator whose alkylene group is, for example, produced by reacting the ethylenically unsaturated group of the polyolefin obtained in the second preparation step with hydrogen iodide to iodinate it.

[0135] R in general formula (2) 2 Macropolymerization initiators in which the group is a phenylene group include, for example, first, the R of general formula (2). 2 A macropolymerization initiator, which has an alkylene group, is subjected to a nucleophilic substitution reaction with 4-methylphenylmagnesium bromide.

[0136] Next, the methyl group on the introduced phenyl group can be iodized by methods such as the Wohl-Ziegler reaction to produce the compound.

[0137] 6. Block polymers Next, we will describe block polymers produced using the macropolymerization initiators mentioned above.

[0138] The block polymer comprises a first block (represented by P1 in the general formula (1) below) and a second block (represented by P2 in the general formula (1) below). The first block is made of the polyolefin described above. The second block is made of a polymer of radically polymerizable monomers. The block polymer contains iodine atoms. The block polymer may also have iodine atoms at the ends of the second block.

[0139] Specifically, block polymers are represented by the following general formula (1).

[0140] General formula (1):

[0141] [ka]

[0142] In general formula (1), P1, R 1 , R 2 and n are P1 and R in the general formula (1) above. 1 , R 2 And is the same as n.

[0143] In general formula (1), P2 consists of a polymer of radically polymerizable monomers. Radically polymerizable monomers are monomers that can be radically polymerized. Examples of radically polymerizable monomers include ethylenically unsaturated carboxylic acids, anhydrides of ethylenically unsaturated carboxylic acids, ethylenically unsaturated carboxylic acid esters, aromatic vinyls, and conjugated dienes.

[0144] Examples of ethylenically unsaturated carboxylic acids include monocarboxylic acids and dicarboxylic acids. Examples of monocarboxylic acids include acrylic acid and methacrylic acid. Examples of dicarboxylic acids include fumaric acid, maleic acid and itaconic acid.

[0145] Examples of anhydrides of ethylenically unsaturated carboxylic acids include maleic anhydride and itaconic anhydride.

[0146] Examples of ethylenically unsaturated carboxylic acid esters include acrylic acid esters and methacrylic acid esters.

[0147] Examples of acrylic acid esters include alkyl acrylates. Examples of alkyl acrylates include methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate.

[0148] Examples of methacrylate esters include alkyl methacrylates. Examples of alkyl methacrylate esters include methyl methacrylate, ethyl methacrylate, butyl methacrylate, and 2-ethylhexyl methacrylate.

[0149] Examples of aromatic vinyls include styrene.

[0150] Examples of conjugated dienes include the conjugated dienes mentioned above.

[0151] The radical polymerizable monomers preferably have an acrylic group or a methacrylic group. Examples of radical polymerizable monomers include acrylic acid, methacrylic acid, acrylic acid esters, and methacrylic acid esters.

[0152] The weight-average molecular weight (Mw) of the block polymer is, for example, 1,000 or more, preferably 2,000 or more. The weight-average molecular weight (Mw) of the block polymer is, for example, 2,000,000 or less, preferably 200,000 or less.

[0153] The number-average molecular weight (Mn) of the block polymer is, for example, 1,000 or more, preferably 2,000 or more. The number-average molecular weight (Mn) of the block polymer is, for example, 1,000,000 or less, preferably 100,000 or less.

[0154] The weight-average molecular weight and number-average molecular weight were measured by GPC (gel permeation chromatography) under the conditions described in the examples below, and are polystyrene-equivalent values ​​(PS equivalent values) obtained by a general calibration method.

[0155] The dispersion degree (Mw / Mn) of the block polymer is, for example, 1 or more, preferably 1.05 or more. The dispersion degree (Mw / Mn) of the block polymer is, for example, 5 or less, preferably 2 or less.

[0156] 7. Effects of Block Polymers According to the block polymer represented by general formula (1), it has a first block made of polyolefin.

[0157] Therefore, it is possible to improve adhesion to polyolefin substrates.

[0158] Furthermore, the second block, which consists of a polymer of radically polymerizable monomers, can improve adhesion even to substrates having different polarities from the polyolefin substrate.

[0159] As a result, it is possible to improve the adhesion between the polyolefin substrate and a substrate having a different polarity from the polyolefin substrate.

[0160] 8. Method for producing block polymers Next, we will describe a method for producing block polymers using macropolymerization initiators.

[0161] To produce block polymers, radical polymerizable monomers are polymerized using the macropolymerization initiator described above in the presence of iodine (I2) and a catalyst.

[0162] Polymerization in the presence of iodine can suppress the retention of unreacted macropolymerization initiators.

[0163] The proportion of iodine is, for example, 0.01 moles or more, preferably 0.02 moles or more, and for example, 0.05 moles or less, preferably 0.03 moles or less, per mole of macropolymerization initiator.

[0164] The catalyst does not contain transition metals. Examples of catalysts include tributylmethylphosphonium iodide, tetrabutylammonium iodide, and tetraoctylammonium iodide.

[0165] Specifically, to produce a block polymer, a macropolymerization initiator, a radical polymerizable monomer, a catalyst, iodine, and a reaction solvent are placed in a nitrogen-purged reaction vessel and heated while stirring.

[0166] If necessary, iodine may be removed by known methods as a post-treatment after the reaction is complete.

[0167] As a result, the radical polymerizable monomer polymerizes on the macropolymerization initiator (living radical polymerization), yielding the block polymer shown in the general formula (1) above.

[0168] More specifically, the carbon-iodine bond between the iodine atom and carbon atom of the macropolymerization initiator is cleaved, causing the iodine atom to detach from the macropolymerization initiator and generate a carbon radical. The generated carbon radical reacts with a radical polymerizable monomer to produce a grown species, which is the reaction product of the macropolymerization initiator and the radical polymerizable monomer. A chain reaction occurs with the radical polymerizable monomer on the carbon radical at the end of the grown species, causing P2 (the second block) of the general formula (1) to grow. Here, if an iodine atom is bonded to the carbon radical at the end of the grown species, the grown species becomes inactive. The carbon-iodine bond at the end of the inactive grown species is cleaved, generating another carbon radical at the end of the grown species. A chain reaction occurs with the radical polymerizable monomer on the generated carbon radical, causing P2 (the second block) of the general formula (1) to grow again. This yields the block polymer shown in the general formula (1).

[0169] The heating temperature is, for example, 50°C or higher, preferably 60°C or higher, and for example, 100°C or lower, preferably 90°C or lower.

[0170] The polymerization time is, for example, 8 hours or more, preferably 20 hours or more, and for example, 48 hours or less, preferably 30 hours or less.

[0171] 9. Effects of the Method for Producing Block Polymers According to the method for producing block polymers, by polymerizing a radical polymerizable monomer in the presence of iodine using a macropolymerization initiator represented by general formula (2), the radical polymerizable monomer can be reliably reacted with the macropolymerization initiator.

[0172] As a result, block polymers represented by general formula (1) can be stably produced while suppressing the retention of unreacted macropolymerization initiators.

[0173] 10. Applications of block polymers The block polymer represented by general formula (1) is, for example, incorporated into a coating agent that covers a polyolefin substrate. The coating agent may also be an adhesive layer that bonds the polyolefin substrate to a substrate having a different polarity from the polyolefin substrate. For example, the coating agent can be used as an adhesive layer for decorative films.

[0174] The coating agent contains a block polymer represented by general formula (1) as an essential component.

[0175] The block polymer is blended into the coating agent in an amount equivalent to solid content of, for example, 5% by mass or more, preferably 7% by mass or more, for example, 20% by mass or less, preferably 15% by mass or less.

[0176] The form of the coating agent is not limited. The coating agent may be, for example, a coating liquid, or a film such as a hot melt adhesive film (heat seal film).

[0177] If the coating agent is a coating liquid, the coating agent may contain, as necessary, solvents, surfactants, polar resins, curing agents, curing catalysts, leveling agents, defoamers, antioxidants, heat stabilizers, light stabilizers (such as UV absorbers), plasticizers, pigments (such as rutile titanium dioxide, zinc oxide, and carbon black), thixotropes, thickeners, tackifiers (such as rosin resins and terpene resins), surface modifiers, anti-settlement agents, weathering agents, pigment dispersants, antistatic agents, fillers, organic or inorganic fine particles, fungicides, and silane coupling agents, to the extent that they do not impair the effect.

[0178] When the coating agent is a film, it can be obtained, for example, by printing and coating a varnish containing a block polymer and drying it, or by forming a block polymer into a film. The varnish may be the coating liquid described above. [Examples]

[0179] The present invention will be further described with reference to the following examples, but the present invention is not limited thereto. Specific numerical values ​​such as blending ratios (content), physical properties, and parameters used in the following description may be replaced with the corresponding upper limits (numerical values ​​defined as "less than or equal to" or "less than") or lower limits (numerical values ​​defined as "greater than or equal to" or "greater than or equal to" or "greater than or equal to") of the blending ratios (content), physical properties, and parameters described in the "Modes for Carrying Out the Invention" above. Note that "parts" and "%" refer to mass unless otherwise specified.

[0180] 1. Manufacturing of macropolymerization initiators (1) Preparation process (1-1) Production of polyolefins (first preparation step) 900 ml of dry hexane (solvent), 30 g of 1-butene, and 1.0 mmol of triisobutylaluminum were charged into a nitrogen-purged 2000 ml polymerization apparatus at room temperature.

[0181] Next, the internal temperature of the polymerization apparatus was raised to 70°C, and propylene gas was introduced into the polymerization apparatus so that the internal pressure of the apparatus became 0.7 MPa.

[0182] Next, a toluene solution prepared by contacting 0.002 mmol of dimethylmethylene (3-tert-butyl-5-methylcyclopentadienyl)fluorenyl zirconium dichloride with 0.6 mmol of methylaluminoxane (manufactured by Tosoh Finechem Co., Ltd.) in terms of aluminum was added to the polymerization apparatus, and polymerization was carried out for 30 minutes while maintaining an internal temperature of 62°C and an internal pressure of 0.7 MPa.

[0183] Subsequently, 20 ml of methanol was added to stop the polymerization. This yielded a polymerization solution containing propylene-1-butene copolymer (an example of a polyolefin).

[0184] After depressurizing the polymerization apparatus, the resulting polymerization solution was mixed with 2 L of methanol, and propylene-1-butene copolymer was precipitated from the polymerization solution.

[0185] The precipitated propylene-1-butene copolymer was dried under vacuum at 130°C for 12 hours.

[0186] (1-2) Introduction of vinylidene group (second preparation step) 200g of propylene-1-butene copolymer was placed in a 1.5L stainless steel pyrolysis apparatus equipped with a stirrer, nitrogen inlet pipe, and condenser, and the inside of the pyrolysis apparatus was purged with nitrogen.

[0187] Next, the internal temperature of the pyrolysis apparatus was raised to 380°C while nitrogen was still flowing in, and the propylene-1-butene copolymer was melted.

[0188] Next, stirring was started, and the propylene-1-butene copolymer in the pyrolysis apparatus was heated for 4.5 hours after it reached a predetermined temperature to thermally decompose the propylene-1-butene copolymer.

[0189] The mixture was then cooled to room temperature to obtain a propylene-1-butene copolymer having vinylidene groups at its ends.

[0190] (1-3) Introduction of hydroxyl groups (third preparation step) 20 g (156 mmol) of propylene-1-butene copolymer having vinylidene groups at the ends and 200 g of methylcyclohexane as a solvent were placed in a 1000 mL round-bottom flask that had been purged with nitrogen, and the mixture was heated to 50°C and stirred.

[0191] A propylene-1-butene copolymer having vinylidene groups at its ends was uniformly dissolved in methylcyclohexane and then cooled to room temperature.

[0192] Next, 31 mL (15 mmol, 0.50 mol / L) of a THF solution of 9-borabicyclo[3.3.1]nonane (9-BBN) was added to a round-bottom flask and stirred. This caused 9-borabicyclo[3.3.1]nonane to react with the vinylidene groups at the ends of the propylene·1-butene copolymer (hydroboration reaction), thereby introducing boron to the ends of the propylene·1-butene copolymer.

[0193] After 2 hours, the solution in the eggplant-shaped flask was cooled to 0°C. 15 mL (62 mmol, 4.0 mol / L) of a methanol / water (1 / 4) mixed solution of NaOH and 5.0 mL (52 mmol, 35%) of an aqueous H2O2 solution were added to the eggplant-shaped flask, and after 10 minutes, the temperature was raised to room temperature.

[0194] Subsequently, the mixture was stirred for 24 hours to replace the terminal boron atoms of the propylene-1-butene copolymer with hydroxyl groups (oxidation reaction).

[0195] Next, the obtained reaction product was washed. Specifically, 100 mL of methylcyclohexane and 100 mL of distilled water were added to the solution containing the reaction product, and the mixture was extracted and washed using a separatory funnel. Furthermore, 50 mL of 10% hydrochloric acid was added to the solution containing the reaction product, and the mixture was extracted and washed again with 50 mL of distilled water. Furthermore, 50 mL of saturated sodium bicarbonate aqueous solution was added to the solution containing the reaction product, and the mixture was extracted and washed again with 50 mL of distilled water. Finally, 50 mL of saturated saline solution was added and washed, and the resulting organic layer was dried and then reprecipitationd in methanol.

[0196] This yielded a propylene-1-butene copolymer having hydroxyl groups at its termini (an example of a hydroxypolyolefin, XKP-001).

[0197] (2) Introduction process Manufacturing Example 1-1 A macropolymerization initiator was prepared using a 300 mL four-necked glass flask purged with argon gas, following the steps outlined below.

[0198] First, 25 g of hydroxypolyolefin (XKP-001, number-average molecular weight (Mn): 10260, dispersion (Mw / Mn): 1.95, hydroxyl group count: 3.3 groups / 1000C) was suspended in chlorobenzene to obtain a 140 mL suspension. The hydroxyl group count was measured using the method described in the reference example below.

[0199] While cooling the resulting suspension with ice, 2.35 g (11.0 mmol) of 2-iodoisobutyric acid (an example of a compound represented by the general formula (4) above) and 122 mg (1.0 mmol) of N,N-dimethyl-4-aminopyridine (an example of a nucleophilic compound) were added to the suspension. Furthermore, 10 mL of a chlorobenzene solution of 1.39 g (11.0 mmol) of N,N'-diisopropylcarbodiimide (an example of a bonding agent) was added.

[0200] The mixture was then stirred for 30 minutes while being cooled with ice, and then stirred again at 25°C for 2 hours. This resulted in the synthesis of a condensate of hydroxypolyolefin (XKP-001) and 2-iodoisobutyric acid.

[0201] The synthesized condensate is such that P1 in the above general formula (2) is a propylene-1-butene copolymer, and two R 1 Both are methyl groups, R 2 It is a macropolymerization initiator that has a carbonyloxy group.

[0202] Next, 10 mL of methanol was added to decompose the unreacted N,N'-diisopropylcarbodiimide.

[0203] After addition, the mixture was filtered, the resulting filtration residue was washed with methanol, and then vacuum-dried.

[0204] This yielded 26 g of macropolymerization initiator as a white powder.

[0205] The obtained macropolymerization initiator was pretreated by oxygen flask combustion, and the proportion of iodine in the macropolymerization initiator (iodine content) was measured by ion chromatography. The iodine content was 2.4% by mass.

[0206] Furthermore, the introduction rate (introduced amount / 1000C) of the iodine initiation group (terminal structure shown in the general formula (4) above) of the macropolymerization initiator was determined using a nuclear magnetic resonance spectrometer. 1 The calculation was performed using the ratio of the integrated intensities from 2.2–2.0 ppm to 2.0–0.5 ppm in 1H-NMR measurements. The calculated "introduced amount / 1000C" is shown in Table 1.

[0207] Furthermore, the macropolymerization initiator 1 The 1H-NMR spectrum shows a peak at 2.1 ppm corresponding to the iodine initiator, and the intensity of this peak corresponds to the amount of iodine initiator introduced. Furthermore, the signal intensity from 2.0 to 0.5 ppm corresponds to the main skeleton of the macropolymerization initiator (the part corresponding to P1 in the general formula (2) above).

[0208] Acyclic saturated aliphatic is C n H 2n+1 Since the empirical formula can be written as follows, if n is sufficiently large, the number of carbon atoms in the polymer will be half the number of hydrogen atoms. Therefore, "Amount introduced / 1000C" in Table 1 is calculated from the following formula.

[0209] Formula: Amount introduced / 1000C = (Integrated intensity of 2.2 - 2.0 ppm) / (Integrated intensity of 2.0 - 0.5 ppm) × 2000 / 6 Manufacturing Examples 1-2 to 1-7 A macropolymerization initiator was obtained in the same manner as in Production Example 1-1, except that chlorobenzene was replaced with the solvent shown in Table 1. The "amount introduced / 1000C" of the obtained macropolymerization initiator is shown in Table 1.

[0210] Manufacturing Example 1-8 A macropolymerization initiator was prepared using a Schlenk tube purged with argon gas, following the steps outlined below.

[0211] 21 mg (0.1 mmol) of 2-iodoisobutyric acid (the compound shown in the general formula (4) above) was mixed with 0.5 mL of chlorobenzene and 19 mg (0.1 mmol) of p-toluenesulfonate chloride (an example of a condensing agent), and the mixture was cooled in an ice bath.

[0212] Next, 8 μL (0.1 mmol) of 1-methylimidazole (an example of a nucleophilic compound) was added using a microsyringe, and the mixture was stirred at ice bath temperature for 1 hour to activate 2-iodoisobutyric acid.

[0213] Next, 230 mg of hydroxypolyolefin (XKP-001) and 8 μL (0.1 mmol) of 1-methylimidazole (a nucleophilic compound) were added, and the 2-iodoisobutyric acid and hydroxypolyolefin (XKP-001) were reacted at 25°C for 3 hours. This synthesized a condensate (macropolymerization initiator) of hydroxypolyolefin (XKP-001) and 2-iodoisobutyric acid.

[0214] Unreacted condensing agent (p-toluenesulfonic acid chloride) or activated 2-iodoisobutyric acid was decomposed with 1 mL of methanol and then filtered. The resulting filtration residue was washed with methanol and then vacuum dried. This yielded a macropolymerization initiator. The "amount introduced / 1000C" of the obtained macropolymerization initiator is shown in Table 1.

[0215] Manufacturing Examples 1-9 A macropolymerization initiator was obtained in the same manner as in Production Example 1-8, except that chlorobenzene was replaced with mesitylene. The "amount introduced / 1000C" of the obtained macropolymerization initiator is shown in Table 1.

[0216] Reference example In the reference example, the amount of hydroxyl groups in hydroxypolyolefin (XKP-001) was measured.

[0217] 92 mg of hydroxypolyolefin (XKP-001), 0.5 mL of tetrahydrofuran, and 60 mg (0.6 mmol) of acetic anhydride were mixed in a Schlenk tube while argon gas was flowed through it, and then 12 mg (0.1 mmol) of N,N-dimethyl-4-aminopyridine (nucleophilic compound) was added.

[0218] The resulting slurry solution was heated to 50°C while stirring to dissolve the hydroxypolyolefin in tetrahydrofuran, and the hydroxypolyolefin was reacted with acetic anhydride for 2.5 hours. This resulted in the substitution of hydrogen atoms of the hydroxyl groups in the hydroxypolyolefin with acetyl groups.

[0219] Next, 1 mL of methanol was mixed into the reaction mixture and then filtered to obtain a polyolefin with acetyl groups introduced as the residue. The residue was washed with methanol, and the residue was... 1 The amount of acetyl groups introduced into the polyolefin (introduced amount / 1000C) was calculated from the 1H-NMR spectrum. The results are shown in Table 1.

[0220] By substituting all the hydrogen atoms of the hydroxyl groups in hydroxypolyolefin (XKP-001) with acetyl groups, the amount of acetyl groups introduced can be considered equivalent to the amount of hydroxyl groups in hydroxypolyolefin (XKP-001). Therefore, the amount of acetyl groups introduced corresponds to the amount of hydroxyl groups in hydroxypolyolefin (XKP-001).

[0221] [Table 1]

[0222] The abbreviations in Table 1 are explained below.

[0223] THF: Tetrahydrofuran MCH / MIBK: A mixture of methylcyclohexane (MCH) and methyl isobutyl ketone (MIBK) (volume ratio of methylcyclohexane to methyl isobutyl ketone (MCH / MIBK) = 4 / 1) DIC: N,N'-Diisopropylcarbodiimide DMAP: N,N-dimethyl-4-aminopyridine TsCl:p-toluenesulfonate chloride NMI: 1-methylimidazole Ac2O: Acetic anhydride Manufacturing Example 2-1 A macropolymerization initiator was prepared using a 300 mL four-necked glass flask purged with argon gas, following the steps outlined below.

[0224] 15.4 g (7.2 mmol) of 2-iodoisobutyric acid (the compound shown in general formula (4) above) and 13.4 g (7.0 mmol) of p-toluenesulfonate chloride (a condensing agent) were mixed in 30 mL of methylene chloride and cooled on ice.

[0225] Next, 5.9 g (7.2 mmol) of 1-methylimidazole (nucleophile) in a 5 mL solution of methylene chloride was added over 5 minutes, and the mixture was stirred for 30 minutes after the addition was complete.

[0226] Next, a mixture of 50 mL of methylene chloride and 50 g of hydrogenated polybutadiene glycol (hydroxypolyolefin, manufactured by Nippon Soda Co., Ltd., product name: NISSO PB GI-1000, Mn: 2080, Mw / Mn: 3.58, hydroxyl value (KOH mg / g): 60-75) was added to the reactor. Furthermore, a 5 mL solution of methylene chloride containing 5.9 g (7.2 mmol) of 1-methylimidazole (nucleophilic compound) was added over 5 minutes, and the mixture was stirred for 1 hour while being cooled on ice.

[0227] This resulted in the synthesis of a condensate (macropolymerization initiator) of hydrogenated polybutadiene glycol and 2-iodoisobutyric acid.

[0228] 1 After confirming the completion of the reaction by 1H-NMR, 200 mL of hexane was added to the reaction mixture. The resulting mixture was washed three times with 100 mL of methanol, and then purified by removing the solvent under reduced pressure. This yielded 49 g of a pale yellow to yellow viscous liquid macropolymerization initiator.

[0229] The obtained macropolymerization initiator was pretreated by oxygen flask combustion, and the iodine content of the macropolymerization initiator was measured by ion chromatography of the combustion gas absorption solution. The iodine content was 9.7% by mass.

[0230] Manufacturing Example 2-2 Except for using 36 g of hydrogenated polybutadiene glycol (manufactured by Nippon Soda Co., Ltd., product name: NISSO PB GI-2000, Mn: 2394, Mw / Mn: 1.92, hydroxyl value (KOH mg / g): 40-55) as the hydroxypolyolefin, 35 g of a pale yellow to yellow viscous liquid macropolymerization initiator was obtained in the same manner as in Production Example 2-1. The iodine content of the obtained macropolymerization initiator was 8.0% by mass.

[0231] Manufacturing Example 2-3 Except that 60 g of hydrogenated polybutadiene glycol (manufactured by Nippon Soda Co., Ltd., product name: NISSO PB GI-3000, Mn: 4573, Mw / Mn: 1.32, hydroxyl value (KOHmg / g): 25-35) was used as the hydroxypolyolefin, the same procedure as in Production Example 2-1 was carried out to obtain 58 g of a pale yellow to yellow viscous liquid macro polymerization initiator. The iodine content of the obtained macro polymerization initiator was 5.1% by mass.

[0232] 2. Production of Block Polymer Example 1 After a 100 mL test tube was purged with nitrogen, 2.0 g (20 mmol) of methyl methacrylate, 1.8 g (0.20 mmol) of the macro polymerization initiator, 69 mg (0.20 mmol) of tributylmethylphosphonium iodide, 1.3 mg (0.0050 mmol) of iodine, and 18 g of toluene as an organic solvent were blended, the temperature was raised to 80°C, and heating was performed for 24 hours.

[0233] As a result, methyl methacrylate is polymerized at the terminal of the macro polymerization initiator, and a block polymer of a propylene·1-butene copolymer and polymethyl methacrylate is produced.

[0234] The molecular weight distribution at the time when the internal temperature reached 80°C (polymerization time 0 hour), 1 hour after the internal temperature reached 80°C (polymerization time 1 hour), 8 hours later (polymerization time 8 hours), and 24 hours later (polymerization time 24 hours) was measured by GPC (gel permeation chromatography) under the following measurement conditions. The results are shown in Figure 1.

[0235] <GPC Measurement Conditions> Apparatus: Gel permeation chromatograph Shodex GPC-101 (manufactured by Showa Denko K.K.) Mobile phase: THF (tetrahydrofuran) Columns: GPC KF804L × 3 (manufactured by Showa Denko K.K.) Flow rate: 1.0 mL / min Sample: 0.15 mg / mL THF solution Temperature: 40°C Detector: Differential refractometer RI-71S Calibration curve; commercially available monodisperse standard polystyrene (PS) From Figure 1, since the peak of the block polymer remains monomodal even as the polymerization time progresses, it is considered that no homopolymer of polymethyl methacrylate is formed.

[0236] Thereafter, the reaction solution in the test tube was mixed with 200 g of methanol to precipitate the block polymer. Next, the obtained precipitate was collected by filtration and dried under reduced pressure. Thus, a dried product of the block polymer was obtained.

[0237] Example 2 A block polymer was obtained in the same manner as in Example 1, except that the amount of methyl methacrylate was changed to 1.0 g (10 mmol).

[0238] Example 3 A block polymer was obtained in the same manner as in Example 1, except that the amount of methyl methacrylate was changed to 0.40 g (4.0 mmol).

[0239] Comparative Example A propylene·1-butene copolymer was obtained in the same manner as in "(1-1) Production of polyolefin (first preparation step)" under the above "1. Production of macro polymerization initiator".

[0240] Next, 3 kg of the obtained propylene·1-butene copolymer was added to 10 L of toluene, the temperature was raised to 145°C under a nitrogen atmosphere, and the propylene·1-butene copolymer was dissolved in toluene.

[0241] Next, while stirring, 382 g of maleic anhydride as a monomer and 175 g of di-tert-butyl peroxide as a polymerization initiator were fed into the system over 4 hours.

[0242] Thereafter, the mixture was stirred at 145°C for 2 hours to produce a maleic anhydride-modified propylene·1-butene copolymer.

[0243] After cooling, a large amount of acetone was mixed to precipitate the maleic anhydride-modified propylene-1-butene copolymer. The resulting precipitate was filtered, washed with acetone, and then vacuum-dried.

[0244] 3. Evaluation (1) Preparation of test specimens The block polymers obtained in Examples 1-3 and the maleic anhydride-modified propylene-1-butene copolymer obtained in the Comparative Example were each dissolved in toluene to prepare coating agents with a solid content concentration (specifically, (mass after drying) / (mass before drying) × 100) of 10% by mass.

[0245] Each of the obtained coating agents was applied to a polypropylene plate and a TSOP (Toyota Super Olefin Polymer®: a thermoplastic resin containing PP (polypropylene) and EPDM (ethylene-propylene-diene rubber)) plate, respectively, using a bar coater No. 14.

[0246] Next, the obtained coating film was left to stand at room temperature for 20 minutes, and then left to stand at 120°C for another 20 minutes.

[0247] This resulted in obtaining a test piece having a dried coating film of the coating agent.

[0248] (2) Adhesion to the substrate (substrate adhesion) Adhesion of the dried coating film of a coating agent to a polypropylene board or TSOP board (substrate) was evaluated using the cross-cut method, in accordance with JIS K 5600-5-6 (1999) "General test methods for coatings - Part 5: Mechanical properties of coating films - Section 6: Adhesion (cross-cut method)".

[0249] Specifically, the dried coating on the above test specimen was cross-cut with a utility knife into a 1x1mm grid pattern (100 squares).

[0250] Next, 24mm wide adhesive tape (made by Nichiban) was applied to the grid, and the tape was pressed down so that the dried paint film could be seen through it.

[0251] Subsequently, the adhesive tape was peeled off at a 60° angle to the coating film after 0.5 seconds, and the adhesion was evaluated based on the number of remaining squares. The number of remaining squares is shown in Table 2.

[0252] (3) Topcoat characteristics A UV-curing acrylic topcoat was applied to the dried coating film of the above coating agent using a bar coater No. 14, and allowed to dry at 60°C for 3 minutes.

[0253] Next, 80 mW / cm² of UV-curable acrylic topcoat agent is applied to the coated surface. 2 Using an ultraviolet irradiation device equipped with a high-pressure mercury lamp, the UV-curable acrylic topcoat was cured by irradiating it with ultraviolet light at an irradiation distance of 8.5 cm and a line speed of 1.2 m / min. This formed an acrylic resin layer on top of the dried coating film.

[0254] Next, in accordance with JIS K 5600-5-6 (1999) "General Test Methods for Paints - Part 5: Mechanical Properties of Coating Films - Section 6: Adhesion (Cross-Cut Method)", the adhesion of the dried coating film to the TSOP board (substrate) was evaluated using the cross-cut method (100 squares) with an acrylic resin layer formed on top of the dried coating film. The number of remaining squares is shown in Table 2.

[0255] In the comparative example, all the squares that remained intact in the evaluation of substrate adhesion to TSOP were completely removed in the evaluation of topcoat properties. This is thought to be because the film shrinkage accompanying the curing of the acrylic topcoat agent applied stress to the dried coating film, making the dried coating film more prone to peeling from the substrate.

[0256] In this regard, in each example, more mass remains in the evaluation of the topcoat properties than in the comparative example. Therefore, the block polymers of each example exhibit superior adhesion to the polyolefin substrate, even when an acrylic resin layer is formed on the dried coating film of the coating agent, compared to the maleic anhydride modified product of the comparative example.

[0257] Table 2

Claims

1. A block polymer represented by the following general formula (1), comprising: a first block consisting of a polymer or modified form of at least one olefin monomer selected from linear α-olefins having 2 to 20 carbon atoms, branched α-olefins having 6 to 20 carbon atoms, cyclic olefins having 4 to 20 carbon atoms, and aliphatic conjugated dienes having 6 to 20 carbon atoms; a second block consisting of a polymer of a radically polymerizable monomer; and an iodine atom. General formula (1): 【Chemistry 1】 (In general formula (1), P1 represents the first block. P2 represents the second block consisting of a polymer of radically polymerizable monomers. 1 R represents one of the following: a hydrogen atom, an aliphatic group, an aromatic group, an alkoxycarbonyl group, or a nitrile group. 2 This represents either a carbonyloxy group or a phenylene group. Two R 1 (These two values ​​may be the same or they may be different. n is an integer greater than or equal to 1.)

2. In the above general formula (1), R 1 is a methyl group, R 2 The block polymer according to claim 1, wherein is a carbonyloxy group.

3. The first block is made of a propylene-1-butene copolymer, The block polymer according to claim 1 or 2, wherein the radical polymerizable monomer has an acrylic group or a methacrylic group.

4. A coating agent containing the block polymer described in any one of claims 1 to 3.

5. A method for producing a block polymer according to any one of claims 1 to 4, A method for producing a block polymer, comprising polymerizing the radical polymerizable monomer using a macropolymerization initiator represented by the following general formula (2) in the presence of iodine and a catalyst. General formula (2): 【Chemistry 2】 (In general formula (2), P1 represents a polymer or modified version of at least one olefin monomer selected from linear α-olefins having 2 to 20 carbon atoms, branched α-olefins having 6 to 20 carbon atoms, cyclic olefins having 4 to 20 carbon atoms, and aliphatic conjugated dienes having 6 to 20 carbon atoms. 1 R represents one of the following: a hydrogen atom, an aliphatic group, an aromatic group, a carbonyloxy group, or a nitrile group. 2 This represents either a carbonyloxy group or a phenylene group. Two R 1 (These two values ​​may be the same or they may be different. n is an integer greater than or equal to 1.)

Citation Information

Patent Citations

  • Block copolymer

    JP1991139510A

  • Method for manufacturing olefinic polymer having halogen atom at terminal, method for manufacturing olefinic polymer having group containing metal of the group i, ii or iii at terminal, and method for manufacturing olefinic block copolymer

    JP2002145927A

  • Laminate and formed article including the same

    JP2014008694A

  • Copolymer and manufacturing method therefor, rubber composition and pneumatic tire

    JP2015199834A

  • Preparation of non-polar-polar block copolymers via vinyl-terminated polyolefins

    JP2023552056A