Wafer processing method and wafer processing apparatus

The method addresses device damage during wafer grinding by forming a frustoconical separation layer and ensuring complete removal of excess material, enhancing the grinding process's efficiency and reducing damage.

JP7954548B2Active Publication Date: 2026-11-20DISCO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022161592
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-06
Publication Date
2026-11-20
Estimated Expiration
2042-10-06

AI Technical Summary

Technical Problem

Existing wafer processing methods result in damage to devices during grinding due to the formation of knife edges and excess material removal, leading to potential collisions and damage to the annular modified layer and polishing pad.

Method used

A method involving a separation layer formation using a laser beam to create a frustoconical structure, followed by grinding and detection steps to ensure complete removal of the excess peripheral region, with optional external force application if necessary.

Benefits of technology

The method effectively removes the excess peripheral region while minimizing device damage, preventing collisions and maintaining the integrity of the polishing pad.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954548000001
    Figure 0007954548000001
  • Figure 0007954548000002
    Figure 0007954548000002
  • Figure 0007954548000003
    Figure 0007954548000003
Patent Text Reader

Abstract

To provide a wafer processing method and a wafer processing apparatus that remove an excess outer region while suppressing device damage in a grinding process of a bonded wafer.SOLUTION: A wafer processing method includes a bonded wafer forming step 1 of bonding one side of a first wafer, which has a device area and an outer peripheral surplus area on one side and a chamfered outer peripheral edge, to a second wafer to form a bonded wafer, a separation layer forming step 2 of forming a separation layer shaped along the side surface of a truncated cone having an inclination from one surface side to the other surface side by irradiating a region a predetermined distance inside the outer periphery of the first wafer with a laser beam in such a way that the focal point of the laser beam is positioned closer to one surface as it approaches the outer periphery, a grinding step 3 of grinding the first wafer from the other side to be thinned to a predetermined thickness, and a detection step 4 of detecting whether the outer peripheral surplus area has been removed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a wafer processing method and a wafer processing apparatus.

Background Art

[0002] With the recent trend toward lower profile and higher integration of device chips, development of three-dimensionally stacked semiconductor wafers is progressing. For example, a TSV (Through-Silicon Via) wafer allows electrodes of two chips to be connected by bonding the two chips together through through-electrodes.

[0003] Such a wafer is ground and thinned in a state where it is bonded to a supporting wafer serving as a base (made of silicon, glass, ceramics, or the like). Normally, since the outer peripheral edge of a wafer is chamfered, when the wafer is ground to an extremely thin thickness, the outer peripheral edge becomes a so-called knife edge, and chipping of the edge is likely to occur during grinding. As a result, the chipping may extend to the device, leading to breakage of the device.

[0004] As a countermeasure against the knife edge problem, an edge trimming method has also been devised in which after wafers are bonded together, a laser beam is irradiated along the outer peripheral edge of a device region to form an annular modified layer, thereby suppressing the edge chipping of the wafer that occurs during grinding from extending to the device (see Patent Document 1).

Prior Art Documents

Patent Documents

[0005]

Patent Document 1

Summary of Invention

Problems to be Solved by the Invention

[0006] However, the method described in Patent Document 1 may result in the remaining material from the excess outer region to be removed during grinding not peeling off, potentially causing the outer and inner regions of the annular modified layer to collide with each other and be damaged, or damaging the polishing pad in the subsequent polishing process.

[0007] The present invention has been made in view of the above problems, and its objective is to provide a wafer processing method and a wafer processing apparatus that can remove excess outer peripheral region while suppressing device damage during the grinding process of bonded wafers. [Means for solving the problem]

[0008] To solve the above-mentioned problems and achieve the objective, the wafer processing method of the present invention comprises a device region on one surface on which a device is formed, and an outer peripheral excess region surrounding the device region, and a bonded wafer forming step of bonding one surface of a first wafer, whose outer peripheral edge is chamfered, to one surface of a second wafer to form a bonded wafer, and positioning the focal point of a laser beam in a region a predetermined distance inward from the outer peripheral edge of the first wafer, such that the closer the focal point is to the outer peripheral edge, the closer it is to the one surface of the first wafer. The process includes: a separation layer formation step of irradiating the first wafer with a laser beam in such a way that a separation layer is formed along the side surface of a frustoconical structure that slopes from one side to the other side of the first wafer; a grinding step of grinding the first wafer of the bonded wafer from the other side after the separation layer formation step to thin it to a predetermined thickness; and a detection step of detecting whether the excess peripheral region on the peripheral edge side of the separation layer has been removed during or after the grinding step. If the detection step detects that the excess outer region has not been removed, the process includes an external force application step to apply an external force to the excess outer region to remove it. It is further characterized by having the following features. Furthermore, the wafer processing method of the present invention comprises a device region on one surface on which a device is formed, and an outer peripheral excess region surrounding the device region, and a bonded wafer forming step of bonding one surface of a first wafer, whose outer peripheral edge is beveled, to one surface of a second wafer to form a bonded wafer, and irradiating a region a predetermined distance inward from the outer peripheral edge of the first wafer with a laser beam such that the focal point of the laser beam is positioned closer to the one surface of the first wafer as it approaches the outer peripheral edge, thereby enabling the processing of the wafer from the one surface side of the first wafer to the other side The method comprises: a separation layer forming step, which is shaped to follow the side surface of a frustum having an inclination toward one side, and separates the device region from the outer peripheral excess region; and a grinding step, after performing the separation layer forming step, which thins the first wafer of the bonded wafer by grinding it from the other side to a predetermined thickness, and further comprises a detection step, which detects whether the outer peripheral excess region on the outer peripheral edge side of the separation layer has been peeled off and removed from the first wafer on the device region side of the separation layer, during or after the grinding step.

[0009] Furthermore, in the wafer processing method of the present invention, it is preferable that the detection step be performed after the grinding step has been carried out. Furthermore, in the wafer processing method of the present invention, in the detection step, measurement light may be irradiated onto the outer peripheral excess region on the outer peripheral edge side of the separation layer, and whether or not the outer peripheral excess region on the outer peripheral edge side of the separation layer has been removed may be detected by receiving at least one of the measurement light reflected from the outer peripheral excess region and the measurement light reflected from the separation layer. Furthermore, in the wafer processing method of the present invention, in the detection step, measurement light may be irradiated onto the outer peripheral excess region on the outer peripheral edge side of the separation layer, and it may be detected whether or not the outer peripheral excess region on the outer peripheral edge side of the separation layer has been removed based on the direction in which the reflected light of the measurement light is reflected.

[0010] Furthermore, if the wafer processing method of the present invention detects in the detection step that the excess outer peripheral region has not been removed, it may further include an external force application step in which an external force is applied to the excess outer peripheral region to remove the excess outer peripheral region.

[0011] Furthermore, the wafer processing apparatus of the present invention comprises a device region on one side on which a device is formed, and an outer peripheral surplus region surrounding the device region, wherein in the region a predetermined distance inward from the outer peripheral edge of the wafer, which has a chamfered outer peripheral edge, there is a shape that follows the side surface of a frustoconical shape having a slope that becomes closer to the outer peripheral edge and closer to the outer surface as it moves from one side to the other side of the wafer. and separate the device region from the outer peripheral excess region. A holding table that holds a wafer on which a separation layer is formed with the other side exposed; a light source that irradiates the excess outer peripheral region of the wafer held on the holding table with measurement light; a light receiving unit that receives at least one of the measurement light irradiated from the light source and reflected from the excess outer peripheral region and the measurement light reflected from the separation layer; and based on the measurement light received by the light receiving unit, the excess outer peripheral region of the wafer starting from the separation layer. From the isolation layer on the device region side from Peel off The invention is characterized by comprising a determination unit that determines whether or not it has been removed.

[0012] Furthermore, the wafer processing apparatus of the present invention further comprises a grinding unit that grinds the other side of the wafer held on the holding table to thin it to a predetermined thickness. The determination unit determines whether the excess outer peripheral region has been peeled off and removed from the wafer due to the grinding load by the grinding unit. That's fine. [Effects of the Invention]

[0013] The present invention can remove the outer peripheral surplus region while suppressing damage to devices in the grinding step of a bonded wafer. [Brief Description of the Drawings]

[0014] [Figure 1] Figure 1 is a flowchart showing the flow of the wafer processing method according to the embodiment. [Figure 2] Figure 2 is a perspective view showing one state of the bonded wafer forming step shown in Figure 1. [Figure 3] Figure 3 is a cross-sectional view showing the bonded wafer after the bonded wafer forming step shown in Figure 1. [Figure 4] Figure 4 is a perspective view showing one state of the separation layer forming step shown in Figure 1. [Figure 5] Figure 5 is an enlarged cross-sectional view showing a part of the bonded wafer after the separation layer forming step shown in Figure 1. [Figure 6] Figure 6 is a plan view showing the bonded wafer after the separation layer forming step shown in Figure 1. [Figure 7] Figure 7 is a side view partially in cross section showing the grinding step shown in Figure 1. [Figure 8] Figure 8 is a side view partially in cross section showing the state after Figure 7 of the grinding step shown in Figure 1. [Figure 9] Figure 9 is a side view partially in cross section showing an example of the detection step shown in Figure 1. [Figure 10] Figure 10 is a plan view showing an example of the detection step shown in Figure 1. [Figure 11] Figure 11 is a side view partially in cross section showing an example of the external force applying step shown in Figure 1. [Figure 12] Figure 12 is a side view partially in cross section showing another example of the external force applying step shown in Figure 1. [Mode for Carrying Out the Invention]

[0015] Embodiments for carrying out the present invention will be described in detail with reference to the drawings. The present invention is not limited to the contents described in the following embodiments. Furthermore, the components described below include those that can be easily imagined by those skilled in the art, and those that are substantially the same. Moreover, the components described below can be combined as appropriate. Furthermore, various omissions, substitutions, or modifications of the components can be made without departing from the spirit of the present invention.

[0016] [Embodiment] A wafer processing method for wafer 10 (see Figure 2) and a wafer processing apparatus 30 according to an embodiment of the present invention will be described based on the drawings. The wafer processing method of the embodiment involves bonding a pair of wafers 10 together and thinning one of the wafers 10 (first wafer 10-1) to a predetermined thickness.

[0017] In the following description, when distinguishing between the wafers 10 of a pair, one wafer 10 will be referred to as the first wafer 10-1, and the other wafer 10 as the second wafer 10-2 (see Figure 2). If they are not distinguished, they will simply be referred to as wafer 10. The second wafer 10-2, which is not thinned, will be described as a TSV wafer similar to the first wafer 10-1 in this embodiment, but in the present invention, it may also be a simple substrate wafer without a pattern.

[0018] Figure 1 is a flowchart showing the flow of the wafer 10 processing method according to the embodiment. As shown in Figure 1, the wafer 10 processing method of the embodiment comprises a bonded wafer formation step 1, a separation layer formation step 2, a grinding step 3, a detection step 4, and an external force application step 5.

[0019] (Laminated wafer formation step 1) Figure 2 is a perspective view showing one state of the bonded wafer formation step 1 shown in Figure 1. Figure 3 is a cross-sectional view showing the bonded wafer 20 after the bonded wafer formation step 1 shown in Figure 1. The bonded wafer formation step 1 is a step in which one side of the first wafer 10-1 is bonded to one side of the second wafer 10-2 to form the bonded wafer 20.

[0020] First, the structure of the wafer 10 to be processed (the first wafer 10-1 and the second wafer 10-2) will be described. The wafer 10 shown in Figures 2 and 3 is a disc-shaped semiconductor wafer, optical device wafer, etc., with a substrate 11 made of silicon (Si), sapphire (Al2O3), gallium arsenide (GaAs), or silicon carbide (SiC), and in this embodiment, it is a silicon wafer. As shown in Figure 3, the outer edge 12 of the wafer 10 is chamfered so that the center in the thickness direction protrudes most towards the outer edge, and the cross-section is arc-shaped from the surface 13 to the back surface 14 of the substrate 11.

[0021] As shown in Figure 2, the wafer 10 comprises a device region 15 and an outer peripheral surplus region 16 surrounding the device region 15. The device region 15 has a plurality of division lines 17 arranged in a grid pattern on the surface 13 of the substrate 11, and devices 18 formed in each region partitioned by the division lines 17. The outer peripheral surplus region 16 surrounds the device region 15 around its entire circumference and is a region where no devices 18 are formed.

[0022] In this embodiment, device 18 constitutes a 3D NAND flash memory and includes electrode pads and through electrodes connected to the electrode pads. The through electrodes penetrate to the back surface 14 of the substrate 11 when the substrate 11 is thinned and the device 18 is individually separated from the wafer 10. That is, the wafer 10 in this embodiment is a so-called TSV wafer in which the individually separated devices 18 have through electrodes. However, the wafer 10 of this invention is not limited to a TSV wafer having through electrodes as in this embodiment, and may be a device wafer without through electrodes.

[0023] In the bonded wafer formation step 1 of the embodiment, one of the surfaces to be bonded is the surface 13. In the bonded wafer formation step 1, first, as shown in Figure 2, a bonding layer 19 is laminated to one of the surfaces 13 of the first wafer 10-1 and the second wafer 10-2. In the embodiment, the bonding layer 19 is laminated to the surface 13 of the second wafer 10-2. In the embodiment, the bonding layer 19 is a double-sided tape in which adhesive layers are laminated on the front and back surfaces of a base material layer, but the present invention is not limited to a double-sided tape, and may be an oxide film, or formed by applying an adhesive containing resin, etc. Alternatively, the first wafer 10-1 and the second wafer 10-2 may be directly bonded without using the bonding layer 19.

[0024] In the first bonded wafer formation step, as shown in Figure 2, the surface 13 of the first wafer 10-1 and the bonding layer 19 laminated on the surface 13 side of the second wafer 10-2 are placed opposite each other with a gap between them. Next, as shown in Figure 3, the surface 13 of the first wafer 10-1 and the surface 13 of the second wafer 10-2 are bonded together via the bonding layer 19. This forms a bonded wafer 20.

[0025] (Wafer processing device 30) In this embodiment, the separation layer formation step 2, the grinding step 3, and the detection step 4 are performed by the wafer processing apparatus 30. The wafer processing apparatus 30 includes a holding table 31 (see Figures 4, 7, 8, and 9), a laser beam irradiation unit 40 (see Figure 4), a grinding unit 50 (see Figures 7 and 8), a light source 60 (see Figures 9 and 10), light receiving units 62 and 63 (see Figures 9 and 10), and a determination unit 65 (see Figure 9). The wafer processing apparatus 30 further includes a moving unit (not shown) that moves the laser beam irradiation unit 40, the grinding unit 50, the light source 60, and the light receiving units 62 and 63 relative to the holding table 31, and an imaging unit (not shown) that images the wafer 10 held on the holding table 31.

[0026] The holding table 31 shown in Figures 4, 7, 8, and 9 holds the wafer 10 on its holding surface (top surface). The holding surface is a disc shape formed from, for example, porous ceramic. In this embodiment, the holding surface is a plane parallel to the horizontal direction. The holding surface is connected to a vacuum suction source, for example, via a vacuum suction path. The holding table 31 holds the wafer 10 placed on the holding surface by suction.

[0027] The laser beam irradiation unit 40 shown in Figure 4 is a unit that irradiates a wafer 10 held on the holding surface of the holding table 31 with a laser beam 41. The laser beam irradiation unit 40 includes, for example, an oscillator that emits a laser beam 41 and a focuser that focuses and irradiates the laser beam 41 emitted from the oscillator. The laser beam 41 includes, for example, a laser beam with a wavelength that penetrates the wafer 10.

[0028] The grinding unit 50 shown in Figures 7 and 8 is a unit that grinds a wafer 10 held on a holding table 31 to thin it to a predetermined thickness. The grinding unit 50 comprises a spindle 51 which is a rotating shaft member, a grinding wheel 52 attached to the lower end of the spindle 51, and a grinding wheel 53 mounted on the lower surface of the grinding wheel 52. The grinding wheel 52 rotates on a rotation axis parallel to the axis of the holding table 31. The grinding wheel 53 faces the upper surface of the wafer 10 held on the holding table 31. The grinding unit 50 further includes a grinding fluid supply unit (not shown) that supplies grinding water to the processing point.

[0029] The light source 60 shown in Figures 9 and 10 irradiates the outer peripheral excess region 16 of the wafer 10 held on the holding table 31 with measurement light 61. The measurement light 61 is reflected off the other surface (grinding surface) of the outer peripheral excess region 16 if the outer peripheral excess region 16 on the outer peripheral edge 12 side of the separation layer 23 (described later) has not been removed. The measurement light 61 is also reflected off the exposed separation layer 23 when the outer peripheral excess region 16 on the outer peripheral edge 12 side of the separation layer 23 (described later) has been removed.

[0030] The light receiving unit 62 shown in Figures 9 and 10 receives measurement light 61 that is irradiated from the light source 60 and reflected from the other surface (grinding surface) of the outer peripheral excess region 16. The light receiving unit 62 includes a light-receiving element such as a photodiode. The light receiving unit 62 converts the intensity of the received light into an electrical signal and outputs it to the judgment unit 65. The light receiving unit 62 is configured so that the direction in which it can receive light can be adjusted. The light receiving unit 62 is also movable relative to the holding table 31. The position of the light receiving unit 62 may be fixed to the main body of the wafer processing apparatus 30.

[0031] The light receiving unit 63 shown in Figures 9 and 10 is irradiated from the light source 60 and receives the measurement light 61 reflected from the exposed separation layer 23 when the outer peripheral excess region 16 on the outer peripheral edge 12 side of the separation layer 23 (described later) has been removed. The light receiving unit 63 includes, for example, a light-receiving element such as a photodiode. The light receiving unit 63 converts the intensity of the received light into an electrical signal and outputs it to the judgment unit 65. The light receiving unit 63 is configured so that the direction in which it can receive light can be adjusted. The light receiving unit 63 is also movable relative to the holding table 31. The position of the light receiving unit 63 may be fixed to the main body of the wafer processing apparatus 30.

[0032] The determination unit 65 shown in Figure 9 is implemented, for example, by a control device that controls each part of the wafer processing device 30. The control device is a computer that includes an arithmetic processing unit as an arithmetic means, a storage device as a storage means, and an input / output interface device as a communication means. The arithmetic processing unit includes, for example, a microprocessor such as a CPU (Central Processing Unit). The storage device has memory such as an HDD (Hard Disk Drive), ROM (Read Only Memory), or RAM (Random Access Memory). The arithmetic processing unit performs various calculations based on a predetermined program stored in the storage device. The arithmetic processing unit outputs various control signals to the above-mentioned components via the input / output interface device according to the calculation results.

[0033] The determination unit 65 determines, based on the measurement light 61 received by the light receiving units 62 and 63, whether or not the outer peripheral excess region 16 has been removed from the wafer 10 (first wafer 10-1) with respect to the separation layer 23 described later. For example, if the measurement light 61 is reflected off the other surface (back surface 14) of the outer peripheral excess region 16, it enters the light receiving unit 62. Also, if the measurement light 61 is reflected off the exposed separation layer 23, it enters the light receiving unit 63.

[0034] The determination unit 65 determines that the outer peripheral excess region 16 has not been removed from the wafer 10 (first wafer 10-1) if the light receiving unit 62 receives the measurement light 61 and the light receiving unit 63 does not receive the measurement light 61. The determination unit 65 also determines that the outer peripheral excess region 16 has been removed from the wafer 10 (first wafer 10-1) if the light receiving unit 63 receives the measurement light 61 and the light receiving unit 63 does not receive the measurement light 61.

[0035] (Separation layer formation step 2) Figure 4 is a perspective view showing one state of separation layer formation step 2 shown in Figure 1. Figure 5 is an enlarged cross-sectional view showing a part of the bonded wafer 20 after separation layer formation step 2 shown in Figure 1. Figure 6 is a plan view showing the bonded wafer 20 after separation layer formation step 2 shown in Figure 1. Separation layer formation step 2 is a step in which a separation layer 23 is formed along the side surface of a frustocone at a predetermined distance inward from the outer peripheral edge 12 of the first wafer 10-1. In separation layer formation step 2, the separation layer 23 is formed inside the first wafer 10-1 by stealth dicing using the laser beam irradiation unit 40 of the wafer processing apparatus 30.

[0036] In separation layer formation step 2, a laser beam 41 is irradiated onto a region a predetermined distance inward from the outer edge 12 of the first wafer 10-1, such that the focal point 42 of the laser beam 41 is positioned closer to one of the surfaces as it approaches the outer edge 12, thereby forming a separation layer 23 that follows the shape of the frustoconical side surface of the first wafer 10-1, which slopes from one surface to the other. In this embodiment, one surface is the front surface 13 and the other surface is the back surface 14.

[0037] In separation layer formation step 2, first, the back surface 14 side of the second wafer 10-2 is held by suction to the holding surface (upper surface) of the holding table 31 of the wafer processing apparatus 30. Next, the first wafer 10-1 and the focuser of the laser beam irradiation unit 40 are aligned. Specifically, the holding table 31 is moved to the irradiation area below the laser beam irradiation unit 40 by a moving unit (not shown). Next, the first wafer 10-1 is photographed and aligned with an imaging unit (not shown) to position the irradiation part of the laser beam irradiation unit 40 vertically opposite to the first wafer 10-1 at a predetermined distance inward from the outer edge 12, and then the focusing point 42 of the laser beam 41 is set inside the first wafer 10-1.

[0038] In separation layer formation step 2, the holding table 31 is rotated around a vertical axis while a laser beam 41 is irradiated from the laser beam irradiation unit 40 from the back surface 14 side of the first wafer 10-1. That is, the laser beam 41 is irradiated along a position a predetermined distance inward from the outer peripheral edge 12 of the first wafer 10-1 to form an annular modified layer 21.

[0039] The modified layer 21 refers to a region whose density, refractive index, mechanical strength, or other physical properties differ from those of the surrounding area due to irradiation with the laser beam 41. The modified layer 21 may include, for example, a melted region, a cracked region, a dielectric breakdown region, a refractive index change region, or a region where these regions are mixed. The modified layer 21 has lower mechanical strength, etc., than other parts of the first wafer 10-1.

[0040] In separation layer formation step 2, the laser beam 41 is irradiated multiple times, or a laser beam 41 having multiple focus points 42 is irradiated, by changing the position of the focal point 42 of the laser beam 41 so that it is positioned closer to one of the surfaces as it approaches the outer edge 12. As a result, multiple modified layers 21 are formed along the side surface of the first wafer 10-1, which is sloped from the surface 13 to the back surface 14. Cracks 22 extend in the modified layers 21, and the connection between the modified layers 21 and the cracks 22 forms a separation layer 23 that is shaped along the side surface of the frustoconical structure, which is sloped from the surface 13 to the back surface 14.

[0041] As shown in Figure 6, in the separation layer formation step 2 of the embodiment, an auxiliary separation layer 24 may be formed to further divide the outer peripheral excess region 16, which is the region of the first wafer 10-1 closer to the outer peripheral edge 12 than the separation layer 23, into at least two or more sections. In the separation layer formation step 2, for example, the auxiliary separation layer 24 is formed radially between the inner peripheral edge and the outer peripheral edge 12 of the outer peripheral excess region 16 at a predetermined position in the circumferential direction of the outer peripheral excess region 16 of the first wafer 10-1.

[0042] In this case, the holding table 31 is moved so that the focal point 42 of the laser beam 41 moves radially outward from the first wafer 10-1. That is, by irradiating the outer peripheral excess region 16 with the laser beam 41 in the radial direction, an auxiliary separation layer 24 is formed along the radial direction. Alternatively, the laser beam 41 may be irradiated while moving the holding table 31 so that the focal point 42 moves radially outward from the first wafer 10-1 to the radial inward. In this case, the irradiation of the laser beam 41 is stopped when the focal point 42 reaches the separation layer 23.

[0043] In addition, the auxiliary separation layer 24 shown in Figure 6 divides the outer peripheral excess region 16 into eight sections in the circumferential direction. However, in the present invention, for example, it may be further divided into 16 sections, or an annular auxiliary separation layer 24 that divides in the radial direction may be included. The number of divisions may be set appropriately according to the diameter of the first wafer 10-1 and the width of the outer peripheral excess region 16.

[0044] Furthermore, when forming the auxiliary separation layer 24, similar to the separation layer 23, the laser beam 41 may be irradiated multiple times by changing the height of the focal point 42 of the laser beam 41, or multiple modified layers 21 may be formed in the thickness direction of the first wafer 10-1 by irradiating with a laser beam 41 having multiple focal points 42 that are separated in the thickness direction of the first wafer 10-1.

[0045] (Grinding step 3) Figure 7 is a side view showing a partial cross-section of grinding step 3 shown in Figure 1. Figure 8 is a side view showing a partial cross-section of grinding step 3 shown in Figure 1 after Figure 7. Grinding step 3 is performed after the separation layer formation step 2 is carried out. Grinding step 3 is a step in which the first wafer 10-1 of the bonded wafer 20 is ground from the other side to thin it to a predetermined thickness. In grinding step 3 of the embodiment, the back surface 14 side of the first wafer 10-1 is ground by the grinding unit 50 of the wafer processing apparatus 30 to thin it to a predetermined finished thickness.

[0046] In grinding step 3, first, the holding table 31, which holds the bonded wafer 20, is transported to below the grinding unit 50. Next, with the holding table 31 rotating around its axis, the grinding wheel 52 is rotated around its axis. Grinding fluid is supplied to the processing point by a grinding fluid supply unit (not shown), and the grinding wheel 53 of the grinding wheel 52 is brought closer to the holding table 31 at a predetermined feed rate, thereby grinding the back surface 14 of the first wafer 10-1 with the grinding wheel 53 and thinning it to a predetermined thickness as shown in Figure 8.

[0047] The excess outer peripheral region 16 on the outer peripheral edge 12 side of the separation layer 23 in the first wafer 10-1 is removed by grinding. That is, the first wafer 10-1 has the separation layer 23 exposed on its outer peripheral surface and forms a frustoconical shape with the separation layer 23 as its side surface. In this case, there is a possibility that the scrap material of the excess outer peripheral region 16 may remain without being peeled off. Whether or not the excess outer peripheral region 16 has been removed in grinding step 3 is detected in detection step 4.

[0048] (Detection step 4) Figure 9 is a side view showing a partial cross-section of an example of the detection step 4 shown in Figure 1. Figure 10 is a plan view showing an example of the detection step 4 shown in Figure 1. The detection step 4 is performed during or after the grinding step 3. In this embodiment, the detection step 4 is performed after the grinding step 3. The detection step 4 is a step to detect whether or not the outer peripheral excess region 16 on the outer peripheral edge 12 side of the separation layer 23 has been removed. In this embodiment, the detection step 4 is performed by the light source 60, light receiving units 62, 63, and judgment unit 65 of the wafer processing apparatus 30.

[0049] In detection step 4, first, the holding table 31 holding the bonded wafer 20 is transported to below the light source 60 and the light receiving units 62 and 63. Here, the light source 60 is positioned so that the measurement light 61 emitted from the light source 60 is irradiated onto the ground surface of the outer peripheral excess region 16 of the first wafer 10-1 of the bonded wafer 20 on the holding table 31, or onto the separation layer 23 that is exposed after the outer peripheral excess region 16 has been removed.

[0050] Furthermore, the position and angle of the light receiving unit 62 are adjusted so that when the measurement light 61 irradiated from the light source 60 is reflected in the outer peripheral excess region 16, the reflected light is incident on it. Similarly, the position and angle of the light receiving unit 63 are adjusted so that when the measurement light 61 irradiated from the light source 60 is reflected in the separation layer 23 that is exposed after the outer peripheral excess region 16 has been removed, the reflected light is incident on it. If the positions of the light receiving units 62 and 63 are fixed to the main body of the wafer processing apparatus 30, their positions are adjusted by moving the holding table 31.

[0051] In detection step 4, after aligning each component as described above, measurement light 61 is then irradiated from the light source 60 onto the outer peripheral excess region 16 on the outer peripheral edge 12 side of the separation layer 23. The measurement light 61 is reflected by the first wafer 10-1, and the reflected light enters the light receiving unit 62 or light receiving unit 63.

[0052] If the excess outer peripheral region 16 on the outer peripheral edge 12 side of the separation layer 23 has not been removed, the measurement light 61 is reflected off the grinding surface of the excess outer peripheral region 16 of the first wafer 10-1, and the reflected light is incident on the light receiving unit 62. The light receiving unit 62 converts the intensity of the received light into an electrical signal and outputs it to the judgment unit 65.

[0053] If the outer peripheral excess region 16 on the outer peripheral edge 12 side of the separation layer 23 has been removed, the measurement light 61 is reflected by the exposed separation layer 23 of the first wafer 10-1, and the reflected light is incident on the light receiving unit 63. The light receiving unit 63 converts the intensity of the received light into an electrical signal and outputs it to the judgment unit 65.

[0054] The determination unit 65 detects whether the outer peripheral excess region 16 on the outer peripheral edge 12 side of the separation layer 23 of the first wafer 10-1 has been removed, based on the reception status of the measurement light 61 by the light receiving units 62 and 63. The determination unit 65 determines that the outer peripheral excess region 16 has not been removed from the first wafer 10-1 if the light receiving unit 62 receives the measurement light 61 and the light receiving unit 63 does not receive the measurement light 61. The determination unit 65 also determines that the outer peripheral excess region 16 has been removed from the first wafer 10-1 if the light receiving unit 63 receives the measurement light 61 and the light receiving unit 62 does not receive the measurement light 61.

[0055] (External force application step 5) Figure 11 is a side view showing a partial cross-section of an example of the external force application step 5 shown in Figure 1. The external force application step 5 is a step in which, if detection step 4 detects that the outer peripheral excess region 16 has not been removed, an external force is applied to the outer peripheral excess region 16 to remove it. In the example shown in Figure 11, the external force application step 5 removes the outer peripheral excess region 16 by applying a shear force in the thickness direction of the first wafer 10-1 with the pressing member 70.

[0056] The pressing member 70 is movable in the vertical direction and applies an external force by pressing against the first wafer 10-1 of the bonded wafer 20 from above. In the external force application step 5 shown in Figure 11, the pressing member 70 is lowered downward while facing the outer peripheral excess area 16 of the first wafer 10-1 in a vertical direction, and the pressing member 70 is pressed against the outer peripheral excess area 16 of the first wafer 10-1.

[0057] As a result, the pressing member 70 applies a downward external force to the outer peripheral excess region 16. Then, starting from the separation layer 23 (and auxiliary separation layer 24; see Figure 6), the device region 15 and the outer peripheral excess region 16 are separated, and the outer peripheral excess region 16 of the first wafer 10-1 is removed.

[0058] Figure 12 is a side view showing a partial cross-section of another example of the external force application step 5 shown in Figure 1. In the example shown in Figure 12, the external force application step 5 removes the outer peripheral excess region 16 of the first wafer 10-1 by applying ultrasound to the outer peripheral excess region 16 with an ultrasound application unit 80 and applying an external force through vibration caused by the ultrasound.

[0059] The ultrasonic application unit 80 includes, for example, an ultrasonic transducer that expands and contracts when alternating current is applied to generate ultrasonic vibrations on the grinding surface of the first wafer 10-1, a power supply that applies alternating current to the ultrasonic transducer, and a liquid supply unit 81. In the external force application step 5 shown in Figure 12, first, with the ultrasonic transducer facing the outer peripheral excess region 16 of the first wafer 10-1 in a vertical direction, liquid is supplied from the liquid supply unit 81 between the ultrasonic transducer and the grinding surface. The liquid is, for example, pure water.

[0060] In the external force application step 5, AC power is applied to the ultrasonic transducer of the ultrasonic application unit 80 for a predetermined time while the opposing surface of the ultrasonic transducer is immersed in the liquid, causing the opposing surface to vibrate ultrasonically. As a result, when ultrasonic vibration is applied to the outer peripheral excess region 16 through the liquid, the cracks 22 in the separation layer 23 extend, separating the device region 15 from the outer peripheral excess region 16 starting from the separation layer 23, and the outer peripheral excess region 16 of the first wafer 10-1 is removed.

[0061] The method of applying external force in the external force application step 5 is not limited to the method of applying external force in the shear direction by pressing the outer periphery excess region 16 from above as shown in Figure 11, or the method of applying external force to the outer periphery excess region 16 by ultrasonic vibration as shown in Figure 12. For example, it may also be a method of crushing by rolling a roller over the outer periphery excess region 16, or a method of applying external force in the shear direction by inserting a claw below the outer periphery excess region 16 and lifting it. Alternatively, grinding step 3 may be performed again, and the grinding load may be continued until the outer periphery excess region 16 is separated.

[0062] As described above, in the wafer 10 processing method according to the embodiment, a laser beam 41 is irradiated onto the bonded wafer 20 such that an annular separation layer 23 formed at a predetermined distance inward from the outer peripheral edge 12 of the first wafer 10-1 has an inclination. As a result, on the bonding layer 19 side (surface 13 side) where the wafer 10 is bonded, the crack 22 extends toward the outer peripheral edge 12 side from the bonding layer 19, thereby suppressing the retention of the scrap material of the outer peripheral excess region 16 while bonded to the second wafer 10-2 via the bonding layer 19.

[0063] Furthermore, during or after grinding, a measuring light 61 is shone onto the outer peripheral excess area 16, and the direction in which the reflected light is reflected is used to detect whether or not the outer peripheral excess area 16 has been removed. By confirming in this way, only the material from which the outer peripheral excess area 16 scraps have been removed can be sent to the subsequent polishing process, thus avoiding the possibility of damaging the polishing pad.

[0064] It should be noted that the present invention is not limited to the embodiments described above. That is, it can be implemented with various modifications without departing from the core principles of the present invention.

[0065] For example, the wafer processing apparatus 30 does not necessarily have to include a laser beam irradiation unit 40. That is, after performing the separation layer formation step 2 in a separate laser processing apparatus, the bonded wafer 20 on which the modified layer 21 has been formed on the first wafer 10-1 may be transported to the wafer processing apparatus 30 and the grinding step 3 and detection step 4 may be performed. Furthermore, the wafer processing apparatus 30 does not necessarily have to include a grinding unit 50. That is, after performing the grinding step 3 in a separate grinding apparatus, the bonded wafer 20 on which the first wafer 10-1 has been ground to a predetermined thickness may be transported to the wafer processing apparatus 30 and the detection step 4 may be performed. Also, the light receiving units 62 and 63 that perform the detection step 4 only need to include at least one of them.

[0066] Furthermore, the separation layer formation step 2 may be performed before the bonded wafer formation step 1, and it is sufficient that the bonded wafer 20 and the separation layer 23 are formed at least before the grinding step 3 is performed. [Explanation of Symbols]

[0067] 10 wafers 10-1 First Wafer 10-2 Second wafer 11 circuit boards 12 Outer edge 13 Surface 14 Back side 15 Device Area 16. Peripheral surplus area 17 planned division lines 18 devices 19 Bonding layer 20 Laminated wafers 21 Modified layer 22 Cracks 23 Separation layer 24 Auxiliary separation layer 30 Wafer processing equipment 31 Holding Table 40 Laser beam irradiation unit 41 Laser beam 42 Focusing points 50 grinding units 60 light source 61 Measuring light 62, 63 Light receiving unit 65 Judgment Department

Claims

1. A method for processing wafers, A bonded wafer forming step comprising: bonding one surface of a first wafer, which has a device region on one surface and an outer peripheral excess region surrounding the device region, and whose outer peripheral edge is beveled, to one surface of a second wafer to form a bonded wafer; A separation layer formation step involves irradiating a region a predetermined distance inward from the outer edge of the first wafer with a laser beam such that the focal point of the laser beam is positioned closer to one of the surfaces of the first wafer as it approaches the outer edge, thereby forming a separation layer that follows the shape of a frustoconical surface of the first wafer, which slopes from one surface to the other. The process includes, after performing the separation layer formation step, a grinding step in which the first wafer of the bonded wafer is ground from the other side to thin it to a predetermined thickness, A detection step to detect whether the excess outer peripheral region on the outer peripheral edge side of the separation layer has been removed during or after the grinding step, If the detection step detects that the excess outer perimeter region has not been removed, the process includes an external force application step to apply an external force to the excess outer perimeter region to remove it, It also has A method for processing wafers, characterized by the following features.

2. A method for processing wafers, A bonded wafer forming step comprising: bonding one surface of a first wafer, which has a device region on one surface and an outer peripheral excess region surrounding the device region, and whose outer peripheral edge is beveled, to one surface of a second wafer to form a bonded wafer; A separation layer formation step involves irradiating a region a predetermined distance inward from the outer edge of the first wafer with a laser beam such that the focal point of the laser beam is positioned closer to one of the faces of the first wafer as it approaches the outer edge, thereby forming a separation layer that separates the device region from the outer edge of the first wafer and has a shape along the side surface of a frustum that slopes from one face to the other of the first wafer. The process includes, after performing the separation layer formation step, a grinding step in which the first wafer of the bonded wafer is ground from the other side to thin it to a predetermined thickness, The method further includes a detection step for detecting whether, during or after the grinding step, the excess peripheral region on the peripheral edge side of the separation layer has been peeled off and removed from the device region side of the first wafer relative to the separation layer. A method for processing wafers, characterized by the following features.

3. The detection step is performed after the grinding step has been performed. The wafer processing method according to claim 2, characterized in that

4. In this detection step, By irradiating the excess peripheral region on the outer edge side of the separation layer with measurement light, and receiving at least one of the measurement light reflected from the excess peripheral region and the measurement light reflected from the separation layer, it is detected whether or not the excess peripheral region on the outer edge side of the separation layer has been removed. The wafer processing method according to claim 2, characterized in that

5. In the detection step, A measurement light is shone onto the excess peripheral region on the outer edge side of the separation layer, and based on the direction in which the reflected measurement light is reflected, it is detected whether or not the excess peripheral region on the outer edge side of the separation layer has been removed. The wafer processing method according to claim 2, characterized in that

6. If the detection step detects that the excess outer region has not been removed, The method further includes an external force application step of applying an external force to the excess outer peripheral region to remove the excess outer peripheral region. A wafer processing method according to any one of claims 2 to 5, characterized in that

7. A wafer processing device, A holding table holds a wafer with the other side exposed, the wafer comprising a device region on one side on which a device is formed, and an outer peripheral excess region surrounding the device region, wherein a separation layer is formed in a region a predetermined distance inward from the outer peripheral edge of the wafer, which has a shape that follows the side surface of a frustoconical shape having a slope that becomes closer to the one side as it approaches the outer peripheral edge from the one side of the wafer to the other side, and which separates the device region from the outer peripheral excess region, the wafer being held with the other side exposed, A light source that irradiates the excess outer region of the wafer held on the holding table with measurement light, A light receiving unit that receives at least one of the measurement light irradiated from the light source and reflected in the outer peripheral excess region, and the measurement light reflected in the separation layer, The system includes a determination unit that determines, based on the measurement light received by the light receiving unit, whether or not the excess outer peripheral region has been peeled off and removed from the wafer from the device region side relative to the separation layer, starting from the separation layer. A wafer processing apparatus characterized by the following:

8. The system further includes a grinding unit that grinds the other side of the wafer held on the holding table to thin it to a predetermined thickness. The determination unit determines whether or not the excess outer peripheral region has been peeled off and removed from the wafer due to the grinding load by the grinding unit. The wafer processing apparatus according to claim 7, characterized in that

Citation Information

Patent Citations

  • Method and apparatus for measuring the thickness of the substrate edge during polishing.

    JP2011519735A

  • Processing method of wafer

    JP2020057709A

  • Wafer processing method

    JP2021129037A

  • Laser machining device and laser machining method

    WO2022014107A1