Display system, optical laminate, and method for manufacturing the display system

The display system enhances VR goggles with high-definition image display by utilizing a specific optical configuration of polarizing and phase difference members, addressing the need for improved resolution and clarity.

JP7954600B2Active Publication Date: 2026-11-20NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023030337
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-02-28
Publication Date
2026-11-20
Estimated Expiration
2043-02-28

AI Technical Summary

Technical Problem

Existing VR goggles lack the necessary high definition for effective image display, particularly in applications requiring enhanced resolution and clarity.

Method used

A display system comprising a display element, a reflective polarizing member, a first lens portion, a half mirror, and phase difference members (λ/4 members) with specific optical configurations and angles to manage light polarization, ensuring high-definition image display.

Benefits of technology

The system achieves high resolution and reduces light depolarization, preventing display defects and improving image clarity in VR goggles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954600000002
    Figure 0007954600000002
  • Figure 0007954600000003
    Figure 0007954600000003
  • Figure 0007954600000004
    Figure 0007954600000004
Patent Text Reader

Abstract

To provide a display system that can achieve improvement in definition of a VR goggle.SOLUTION: A display system displays an image for a user, and the display system comprises: a display device having a display surface emitting light showing an image frontward through a polarization member; a reflection type polarization member arranged in front of the display device, and reflecting light emitted from the display device; a first lens part arranged on an optical path between the display device and the reflection type polarization member; a semitransparent mirror arranged between the display device and the first lens part, transmitting light emitted from the display device, and reflecting light reflected by the reflection type polarization member toward the reflection type polarization member; a first λ / 4 member arranged on an optical path between the display device and the semitransparent mirror; and a second λ / 4 member arranged on an optical path between the semitransparent mirror and the reflection type polarization member.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a display system, an optical laminate, and a method for manufacturing a display system.

Background Art

[0002] Image display devices typified by liquid crystal display devices and electroluminescent (EL) display devices (e.g., organic EL display devices) are rapidly becoming widespread. In image display devices, optical members such as polarizing members and retardation members are generally used to achieve image display and enhance image display performance (see, for example, Patent Document 1).

[0003] In recent years, new applications for image display devices have been developed. For example, goggles with a display (VR goggles) for realizing Virtual Reality (VR) have begun to be commercialized. Since VR goggles are being considered for use in various scenarios, higher definition and the like are desired for them.

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0005] In view of the above, the main object of the present invention is to provide a display system capable of realizing higher definition of VR goggles.

Means for Solving the Problems

[0006] [1] According to one aspect of the present invention, a display system for displaying an image to a user, comprising: a display element having a display surface that emits light representing an image forward via a polarizing member; a reflective polarizing member disposed in front of the display element and reflecting the light emitted from the display element; a first lens portion disposed in the optical path between the display element and the reflective polarizing member; a half mirror disposed between the display element and the first lens portion, which transmits the light emitted from the display element and reflects the light reflected by the reflective polarizing member toward the reflective polarizing member; and a first λ / 4 portion disposed in the optical path between the display element and the half mirror. A display system is provided comprising a material and a second λ / 4 member disposed in the optical path between the half mirror and the reflective polarizing member, wherein the first λ / 4 member has a Re(550) of 100 nm to 190 nm and a Re(450) / Re(550) of 0.75 or more and less than 1, the second λ / 4 member has a Re(550) of 100 nm to 190 nm and a Re(450) / Re(550) of 0.75 or more and less than 1, the light emitted through the polarizing member is linearly polarized, and the angle between the polarization direction of the linearly polarized light and the reflection axis of the reflective polarizing member is 87.5° to 92.5° or 0° to 2.5°. [2] In the display system described in [1] above, the angle between the slow axis of the second λ / 4 member and the reflection axis of the reflective polarizing member may be 42.5° to 47.5°. [3] In the display system described in [1] or [2] above, the angle between the absorption axis of the polarizing member included in the display element and the slow axis of the first λ / 4 member may be 40° to 50°, the angle between the slow axis of the first λ / 4 member and the slow axis of the second λ / 4 member may be 0° to 10°, and the angle between the polarization direction of the linearly polarized light and the reflection axis of the reflective polarizing member may be 87.5° to 92.5°. [4] In the display system described in [1] or [2] above, the angle between the absorption axis of the polarizing member included in the display element and the slow axis of the first λ / 4 member may be 40° to 50°, the angle between the slow axis of the first λ / 4 member and the slow axis of the second λ / 4 member may be 80° to 100°, and the angle between the polarization direction of the linearly polarized light and the reflection axis of the reflective polarizing member may be 0° to 2.5°. [5] In the display system described in any of [1] to [4] above, the first λ / 4 member may satisfy all of the following conditions: Re(400) / Re(550)<0.85, Re(650) / Re(550)>1.03, and Re(750) / Re(550)>1.05. [6] In the display system described in any of [1] to [5] above, the second λ / 4 member may satisfy all of the following conditions: Re(400) / Re(550)<0.85, Re(650) / Re(550)>1.03, and Re(750) / Re(550)>1.05. [7]According to another aspect of the present invention, there is an optical laminate used in any of the display systems described in [1] to [6] above, comprising the second λ / 4 member and the reflective polarizing member, wherein the angle between the slow axis of the second λ / 4 member and the reflection axis of the reflective polarizing member is 42.5° to 47.5°. [8] In another aspect of the present invention, a manufacturing method is provided for manufacturing a display system as described in any of [1] to [6] above, comprising slitting a long first film member including the second λ / 4 member along the longitudinal direction to obtain a second film member, wherein the variation in the lagging axis of the second λ / 4 member in the width direction is 1° or less in the second film member. [9]According to another aspect of the present invention, a manufacturing method for manufacturing a display system according to any one of [1] to [6] above is provided, comprising slitting a long first film member including the reflective polarizing member along the longitudinal direction to obtain a second film member, wherein the variation in the reflection axis of the reflective polarizing member in the width direction of the second film member is 1° or less. [Effects of the Invention]

[0007] According to the display system of the embodiment of the present invention, it is possible to achieve high resolution for VR goggles. [Brief explanation of the drawing]

[0008] [Figure 1] This is a schematic diagram showing the general configuration of a display system according to one embodiment of the present invention. [Figure 2] (a) is a schematic diagram illustrating the propagation of light in an example of the display system shown in Figure 1, and (b) is a schematic diagram illustrating the change in the polarization state of light in the display system shown in (a). [Figure 3] (a) is a schematic diagram illustrating the propagation of light in an example of the display system shown in Figure 1, and (b) is a schematic diagram illustrating the change in the polarization state of light in the display system shown in (a). [Figure 4] Figure 1 is a schematic cross-sectional view showing an example of the details of the lens section of the display system. [Figure 5] This is a schematic perspective view showing an example of a multilayer structure contained in a reflective polarizing film. [Figure 6A] This is a schematic diagram illustrating an example of a method for manufacturing a display system according to one embodiment of the present invention. [Figure 6B] This is a schematic diagram illustrating an example of a method for manufacturing a display system according to one embodiment of the present invention. [Figure 7] This graph shows the average reflectance values ​​measured for the measurement samples in the examples and comparative examples. [Modes for carrying out the invention]

[0009] Embodiments of the present invention will be described below with reference to the drawings, but the present invention is not limited to these embodiments. While the drawings may schematically represent the width, thickness, shape, etc., of each part compared to the embodiments in order to clarify the explanation, these are merely examples and do not limit the interpretation of the present invention. Furthermore, in the drawings, the same or equivalent elements are denoted by the same reference numerals, and redundant explanations may be omitted.

[0010] (Definitions of terms and symbols) The definitions of terms and symbols used in this specification are as follows: (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction where the refractive index is maximum in the plane (i.e., the slow phase axis direction), "ny" is the refractive index in the direction perpendicular to the slow phase axis in the plane (i.e., the fast phase axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane phase difference measured with light of wavelength λnm at 23°C. For example, "Re(550)" is the in-plane phase difference measured with light of wavelength 550nm at 23°C. Re(λ) can be calculated using the formula: Re(λ) = (nx - ny) × d, where d (nm) is the thickness of the layer (film). (3) Phase difference in the thickness direction (Rth) "Rth(λ)" is the phase difference in the thickness direction measured with light of wavelength λnm at 23°C. For example, "Rth(550)" is the phase difference in the thickness direction measured with light of wavelength 550nm at 23°C. Rth(λ) can be calculated using the formula: Rth(λ) = (nx - nz) × d, where d (nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated using the formula Nz = Rth / Re. (5)Angle When an angle is referred to in this specification, unless otherwise specified, the relevant angle includes both clockwise and counterclockwise directions relative to the reference direction. Therefore, for example, "45°" means ±45°. Further, in this specification, "substantially parallel" includes a range of 0°±10°, preferably within a range of 0°±5°, more preferably within a range of 0°±3°, and still more preferably within a range of 0°±1°. "Substantially orthogonal" includes a range of 90°±10°, preferably within a range of 90°±5°, more preferably within a range of 90°±3°, and still more preferably within a range of 90°±1°.

[0011] A. Display System Figure 1 is a schematic diagram showing a schematic configuration of a display system according to one embodiment of the present invention. In Figure 1, the arrangement, shape and the like of each component of the display system 2 are schematically illustrated. The display system 2 includes a display element 12, a reflective polarizing member 14, a first lens portion 16, a half mirror 18, a first phase difference member 20, a second phase difference member 22, and a second lens portion 24. The reflective polarizing member 14 is disposed in front of the display element 12 on the side of the display surface 12a, and can reflect light emitted from the display element 12. The first lens portion 16 is disposed on the optical path between the display element 12 and the reflective polarizing member 14, and the half mirror 18 is disposed between the display element 12 and the first lens portion 16. The first phase difference member 20 is disposed on the optical path between the display element 12 and the half mirror 18, and the second phase difference member 22 is disposed on the optical path between the half mirror 18 and the reflective polarizing member 14.

[0012] The half mirror, or the components disposed forward from the first lens portion (in the illustrated example, the half mirror 18, the first lens portion 16, the second phase difference member 22, the reflective polarizing member 14 and the second lens portion 24) may be collectively referred to as a lens portion (lens portion 4).

[0013] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12a for displaying an image. Light emitted from the display surface 12a passes through a polarizing member (typically a polarizing film) that may be included in the display element 12, and is emitted as first linearly polarized light.

[0014] The first phase difference member 20 includes a first λ / 4 member capable of converting a first linearly polarized light incident on the first phase difference member 20 into a first circularly polarized light. If the first phase difference member does not include any members other than the first λ / 4 member, the first phase difference member may correspond to the first λ / 4 member. The first phase difference member 20 may be provided integrally with the display element 12.

[0015] The half mirror 18 transmits light emitted from the display element 12 and reflects the light reflected by the reflective polarizing member 14 back towards the reflective polarizing member 14. The half mirror 18 is integrally provided with the first lens portion 16.

[0016] The second phase difference member 22 includes a second λ / 4 member that can transmit light reflected by the reflective polarizing member 14 and the half mirror 18 through the reflective polarizing member 14. If the second phase difference member does not include any members other than the second λ / 4 member, the second phase difference member may correspond to the second λ / 4 member. The second phase difference member 22 may be provided integrally with the first lens portion 16.

[0017] The first circularly polarized light emitted from the first λ / 4 member included in the first phase difference member 20 passes through the half mirror 18 and the first lens portion 16 and is converted into a second linearly polarized light by the second λ / 4 member included in the second phase difference member 22. The second linearly polarized light emitted from the second λ / 4 member is reflected towards the half mirror 18 without passing through the reflective polarizing member 14. At this time, the polarization direction of the second linearly polarized light incident on the reflective polarizing member 14 is in the same direction as the reflection axis of the reflective polarizing member 14. Therefore, the second linearly polarized light incident on the reflective polarizing member 14 is reflected by the reflective polarizing member 14.

[0018] The second linearly polarized light reflected by the reflective polarizing member 14 is converted into a second circularly polarized light by the second λ / 4 member included in the second phase difference member 22. The second circularly polarized light emitted from the second λ / 4 member passes through the first lens portion 16 and is reflected by the half mirror 18. The circularly polarized light reflected by the half mirror 18 passes through the first lens portion 16 and is converted into a third linearly polarized light by the second λ / 4 member included in the second phase difference member 22. The third linearly polarized light is transmitted through the reflective polarizing member 14. At this time, the polarization direction of the third linearly polarized light incident on the reflective polarizing member 14 is in the same direction as the transmission axis of the reflective polarizing member 14. Therefore, the third linearly polarized light incident on the reflective polarizing member 14 is transmitted through the reflective polarizing member 14.

[0019] Light that has passed through the reflective polarizing member 14 passes through the second lens portion 24 and enters the user's eye 26.

[0020] The in-plane phase difference Re(550) of the first λ / 4 member is, for example, 100 nm to 190 nm, but may also be 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. Preferably, the first λ / 4 member exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measured light. The Re(450) / Re(550) of the first λ / 4 member is, for example, 0.75 or more and less than 1, but may also be 0.8 or more and less than 1, or 0.8 or more and 0.95 or less.

[0021] In one embodiment, the first λ / 4 member satisfies all of Re(400) / Re(550)<0.85, Re(650) / Re(550)>1.03, and Re(750) / Re(550)>1.05. The first λ / 4 member preferably satisfies at least one selected from 0.65<Re(400) / Re(550)<0.80 (preferably 0.7<Re(400) / Re(550)<0.75), 1.0<Re(650) / Re(550)<1.25 (preferably 1.05<Re(650) / Re(550)<1.20), and 1.05<Re(750) / Re(550)<1.40 (preferably 1.08<Re(750) / Re(550)<1.36), more preferably satisfies at least two, and even more preferably satisfies all. The first λ / 4 member having such wavelength dispersion characteristics can maintain the polarization state of transmitted light more uniformly over the entire visible light range.

[0022] The in-plane retardation Re(550) of the second λ / 4 member is, for example, 100 nm to 190 nm, may be 110 nm to 180 nm, may be 130 nm to 160 nm, or may be 135 nm to 155 nm. The second λ / 4 member preferably exhibits reverse dispersion wavelength characteristics in which the retardation value increases in accordance with the wavelength of the measurement light. Re(450) / Re(550) of the second λ / 4 member is, for example, 0.75 or more and less than 1, and may be 0.8 or more and less than 1, or 0.8 or more and 0.95 or less.

[0023] In one embodiment, the second λ / 4 member satisfies all of Re(400) / Re(550)<0.85, Re(650) / Re(550)>1.03, and Re(750) / Re(550)>1.05. The second λ / 4 member preferably satisfies at least one selected from 0.65<Re(400) / Re(550)<0.80 (preferably 0.7<Re(400) / Re(550)<0.75), 1.0<Re(650) / Re(550)<1.25 (preferably 1.05<Re(650) / Re(550)<1.20), and 1.05<Re(750) / Re(550)<1.40 (preferably 1.08<Re(750) / Re(550)<1.36), more preferably satisfies at least two, and even more preferably satisfies all. The second λ / 4 member having such wavelength dispersion characteristics can maintain the polarization state of transmitted light more uniformly over the entire visible light range.

[0024] Figure 2 is a schematic diagram illustrating the propagation of light and the change in polarization state in an example of the display system shown in Figure 1. Specifically, Figure 2(a) is a schematic diagram illustrating an example of the propagation of light in the display system, and Figure 2(b) is a schematic diagram illustrating an example of the change in the polarization state of light caused by transmission through each member or reflection by each member in the display system. In Figure 2, the solid line arrow and the dashed line arrow attached to the display element 12 respectively indicate the absorption axis direction and the transmission axis direction of the polarizing member included in the display element 12, the arrows attached to the first retardation member 20 and the second retardation member 22 respectively indicate the slow axis direction of the first λ / 4 member and the second λ / 4 member, and the solid line arrow and the dashed line arrow attached to the reflective polarizing member 14 respectively indicate the reflection axis direction and the transmission axis direction.

[0025] In the display system shown in Figure 2, the angle between the polarization direction of the first linearly polarized light emitted forward through the polarizing member included in the display element 12 and the reflection axis of the reflective polarizing member 14 is approximately orthogonal, for example, 87.5° to 92.5°, preferably 88° to 92°, more preferably 89° to 91°, and even more preferably about 90°. Therefore, the polarizing member included in the display element 12 and the reflective polarizing member 14 can be arranged such that the angle between the absorption axis of the polarizing member and the reflection axis of the reflective polarizing member 14 is approximately parallel, for example, 0° to 2.5°, preferably 0° to 2°, more preferably 0° to 1°, and even more preferably about 0°. The angle between the polarization direction of the first linearly polarized light and the slow axis of the first λ / 4 member is, for example, 40° to 50°, preferably 42° to 48°, more preferably 44° to 46°, and even more preferably about 45°. Therefore, the polarizing member and the first λ / 4 member included in the display element 12 can be arranged such that the angle between the absorption axis of the polarizing member and the slow axis of the first λ / 4 member is, for example, 40° to 50°, preferably 42° to 48°, more preferably 44° to 46°, and even more preferably about 45°. The angle between the phase-lagging axis of the first λ / 4 member and the phase-lagging axis of the second λ / 4 member is, for example, 0° to 10°, preferably 0° to 5°, more preferably 0° to 3°, even more preferably 0° to 1°, and even more preferably about 0°. The angle between the slow axis of the second λ / 4 plate and the reflection axis of the reflective polarizing member 14 is, for example, 42.5° to 47.5°, preferably 43° to 47°, more preferably 44° to 46°, and even more preferably about 45°.

[0026] Light L emitted from the display element 12 as first linearly polarized light via the polarizing member is converted into first circularly polarized light by the first λ / 4 member included in the first phase difference member 20. The first circularly polarized light passes through the half mirror 18 and the first lens portion 16 (not shown) and is converted into second linearly polarized light whose polarization direction is orthogonal to that of the first linearly polarized light by the second λ / 4 member included in the second phase difference member 22. The polarization direction of the second linearly polarized light is in the same direction as (approximately parallel to) the reflection axis of the reflective polarizing member 14. Therefore, the second linearly polarized light incident on the reflective polarizing member 14 is reflected by the reflective polarizing member 14 toward the half mirror 18.

[0027] The second linearly polarized light reflected by the reflective polarizing member 14 is converted into a second circularly polarized light by the second λ / 4 member. The rotation direction of the second circularly polarized light is the same as the rotation direction of the first circularly polarized light. The second circularly polarized light emitted from the second λ / 4 member passes through the first lens portion 16 and is reflected by the half mirror 18, converting it into a third circularly polarized light that rotates in the opposite direction to the second circularly polarized light. The third circularly polarized light reflected by the half mirror 18 passes through the first lens portion 16 and is converted into a third linearly polarized light by the second λ / 4 member. The polarization direction of the third linearly polarized light is perpendicular to the polarization direction of the second linearly polarized light and is in the same direction (approximately parallel) to the transmission axis of the reflective polarizing member 14. Therefore, the third linearly polarized light can be transmitted through the reflective polarizing member 14. The light transmitted through the reflective polarizing member 14 passes through the second lens portion 24 and is incident on the user's eye 26.

[0028] In Figure 2, when viewed from the display element 12 side, the slow-motion axes of the first λ / 4 member and the second λ / 4 member are both arranged at an angle of approximately 45° counterclockwise with respect to the absorption axis of the polarizing member included in the display element 12. However, the same explanation can be applied even if they are arranged at an angle of approximately 45° clockwise.

[0029] Figure 3 is a schematic diagram illustrating the propagation of light and changes in polarization state in another example of the display system shown in Figure 1. Specifically, Figure 3(a) is a schematic diagram illustrating an example of the propagation of light in the display system, and Figure 3(b) is a schematic diagram illustrating an example of changes in the polarization state of light due to transmission through or reflection by each component in the display system. In Figure 3, the solid and dashed arrows attached to the display element 12 indicate the absorption axis direction and transmission axis direction of the polarizing member included in the display element 12, respectively; the arrows attached to the first phase difference member 20 and the second phase difference member 22 indicate the slow phase axis direction of the first λ / 4 member and the second λ / 4 member, respectively; and the solid and dashed arrows attached to the reflective polarizing member 14 indicate the reflection axis direction and transmission axis direction, respectively.

[0030] In the display system shown in Figure 3, the angle between the polarization direction of the first linearly polarized light emitted forward through the polarizing member included in the display element 12 and the reflection axis of the reflective polarizing member 14 is approximately parallel, for example, 0° to 2.5°, preferably 0° to 2°, more preferably 0° to 1°, and even more preferably about 0°. Therefore, the polarizing member included in the display element 12 and the reflective polarizing member 14 can be arranged such that the angle between the absorption axis of the polarizing member and the reflection axis of the reflective polarizing member 14 is approximately orthogonal, for example, 87.5° to 92.5°, preferably 88° to 92°, more preferably 89° to 91°, and even more preferably about 90°. The angle between the polarization direction of the first linearly polarized light and the slow axis of the first λ / 4 member is, for example, 40° to 50°, preferably 42° to 48°, more preferably 44° to 46°, and even more preferably about 45°. Therefore, the polarizing member and the first λ / 4 member included in the display element 12 can be arranged such that the angle between the absorption axis of the polarizing member and the slow axis of the first λ / 4 member is, for example, 40° to 50°, preferably 42° to 48°, more preferably 44° to 46°, and even more preferably about 45°. The angle between the phase-lagging axis of the first λ / 4 member and the phase-lagging axis of the second λ / 4 member is, for example, 80° to 100°, preferably 85° to 95°, more preferably 87° to 93°, even more preferably 89° to 91°, and even more preferably about 90°. The angle between the slow axis of the second λ / 4 plate and the reflection axis of the reflective polarizing member 14 is, for example, 42.5° to 47.5°, preferably 43° to 47°, more preferably 44° to 46°, and even more preferably about 45°.

[0031] Light L emitted from the display element 12 as first linearly polarized light via the polarizing member is converted into first circularly polarized light by the first λ / 4 member included in the first phase difference member 20. The first circularly polarized light passes through the half mirror 18 and the first lens portion 16 (not shown) and is converted into second linearly polarized light whose polarization direction is parallel to that of the first linearly polarized light by the second λ / 4 member included in the second phase difference member 22. The polarization direction of the second linearly polarized light is in the same direction as (approximately parallel to) the reflection axis of the reflective polarizing member 14. Therefore, the second linearly polarized light incident on the reflective polarizing member 14 is reflected by the reflective polarizing member 14 toward the half mirror 18.

[0032] The second linearly polarized light reflected by the reflective polarizing member 14 is converted into a second circularly polarized light by the second λ / 4 member. The rotation direction of the second circularly polarized light is the same as the rotation direction of the first circularly polarized light. The second circularly polarized light emitted from the second λ / 4 member passes through the first lens portion 16 and is reflected by the half mirror 18, converting it into a third circularly polarized light that rotates in the opposite direction to the second circularly polarized light. The third circularly polarized light reflected by the half mirror 18 passes through the first lens portion 16 and is converted into a third linearly polarized light by the second λ / 4 member. The polarization direction of the third linearly polarized light is perpendicular to the polarization direction of the second linearly polarized light and is in the same direction (approximately parallel) to the transmission axis of the reflective polarizing member 14. Therefore, the third linearly polarized light can be transmitted through the reflective polarizing member 14. The light transmitted through the reflective polarizing member 14 passes through the second lens portion 24 and is incident on the user's eye 26.

[0033] In Figure 3, when viewed from the display element 12 side, the slow-phase axes of the first λ / 4 member and the second λ / 4 member are arranged to form angles of approximately 45° counterclockwise and approximately 45° clockwise with respect to the absorption axis of the polarizing member included in the display element 12, respectively. However, the same explanation can be applied even when they are arranged to form angles of approximately 45° clockwise and approximately 45° counterclockwise.

[0034] In the display systems shown in Figures 2 and 3, first linearly polarized light emitted from the display element 12 via a polarizing member is reflected by a reflective polarizer after passing through a first λ / 4 member and a second λ / 4 member. In such a display system, partial depolarization occurs as the linearly polarized light passes through the λ / 4 member twice, which can reduce the reflectivity of the reflective polarizer 14. When the reflectivity decreases, light that should be reflected is transmitted, which can result in display defects, uneven display, etc. In contrast, according to the display system of the embodiment of the present invention, by using a λ / 4 member having inverse wavelength dispersion characteristics and strictly controlling the angle between the polarization direction of the first linearly polarized light and the reflection axis direction of the reflective polarizer 14 to be within the range of 90°±2.5° or 0°±2.5°, the decrease in reflectivity can be suitably prevented. Furthermore, by adjusting the angle between the slow axis of the second λ / 4 plate and the reflection axis of the reflective polarizing member 14 to within the range of 45° ± 2.5°, the angle between the polarization direction of the first linearly polarized light and the reflection axis direction of the reflective polarizing member 14 can be suitably controlled.

[0035] B. Lens section and optical laminate In the lens section 4 of the display system shown in Figure 1, a space may be formed between the first lens section 16 and the second lens section 24. In this case, it is preferable that the member placed between the first lens section 16 and the second lens section 24 is integrally provided with either the first lens section 16 or the second lens section 24. For example, it is preferable that the member placed between the first lens section 16 and the second lens section 24 is integrated with either the first lens section 16 or the second lens section 24 via an adhesive layer. With such a configuration, for example, the handling of each member can be improved. The adhesive layer may be formed of an adhesive or a tack. Specifically, the adhesive layer may be an adhesive layer or a tack layer. The thickness of the adhesive layer is, for example, 0.05 μm to 30 μm.

[0036] Figure 4 is a schematic cross-sectional view showing an example of the details of the lens portion 4. Specifically, Figure 4 shows the first lens portion, the second lens portion, and a member positioned between them. The lens portion 4 comprises the first lens portion 16, the first laminated portion 100 provided adjacent to the first lens portion 16, and the second lens portion 24. The first laminated portion 100 and the second lens portion 24 are spaced apart.

[0037] The first laminated portion 100 includes a second phase difference member 22, which includes a second λ / 4 member 22a, and a reflective polarizing member 14. The first laminated portion 100 further includes an adhesive layer (e.g., an adhesive layer) 40 disposed between the first lens portion 16 and the second phase difference member 22, and is integrally provided with the first lens portion 16 by the adhesive layer 40. The first laminated portion 100 further includes an absorptive polarizing member 28 and a protective member 30 in front of the reflective polarizing member 14, in that order. Visibility can be improved by arranging the absorptive polarizing member 28 between the reflective polarizing member 14 and the second lens portion 24. The reflection axis of the reflective polarizing member 14 and the absorption axis of the absorptive polarizing member 28 may be arranged substantially parallel to each other, and the transmission axis of the reflective polarizing member 14 and the transmission axis of the absorptive polarizing member 28 may be arranged substantially parallel to each other. In the first laminated portion 100, the angle between the slow axis of the second λ / 4 member 22a and the reflection axis of the reflective polarizing member 14 is, for example, within the range of 45°±2.5°, preferably within the range of 45°±2°, more preferably within the range of 45°±1°, and even more preferably within the range of about 45°.

[0038] In the example shown in Figure 4, the second phase difference member 22 includes, in addition to the second λ / 4 member 22a, a member (a so-called positive C plate) 22b whose refractive index characteristics can exhibit the relationship nz>nx=ny. The second phase difference member 22 has a laminated structure of the second λ / 4 member 22a and the positive C plate 22b. By using the positive C plate, light leakage (for example, light leakage in an oblique direction) can be prevented. As shown in Figure 4, it is preferable that in the second phase difference member 22, the second λ / 4 member 22a is positioned in front of the positive C plate 22b.

[0039] Although not illustrated, a third retardation member may be disposed between the absorptive polarizing member 28 and the protective member 30. The third retardation member includes, for example, a third λ / 4 member. The angle formed by the absorption axis of the absorptive polarizing member 28 and the slow axis of the third λ / 4 member included in the third retardation member is, for example, 40° to 50°, may be 42° to 48°, or may be about 45°. By providing such a member, for example, reflection of external light from the second lens portion 24 side can be prevented. When the third retardation member does not include any member other than the third λ / 4 member, the third retardation member can correspond to the third λ / 4 member.

[0040] In one embodiment, the first laminated portion 100 is produced as the optical laminate having the above configuration, and is bonded to the first lens portion 16 by the adhesive layer 40. The optical laminate can be produced, for example, by bonding the respective members via an adhesive layer.

[0041] <Second λ / 4 Member> The in-plane retardation Re(550) and wavelength dispersion characteristic of the second λ / 4 member are as described in section A. The second λ / 4 member preferably exhibits a refractive index characteristic satisfying a relationship of nx>ny≧nz. Here, "ny=nz" encompasses not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, within a range that does not impair the effects of the present invention, ny may be smaller than nz. The Nz coefficient of the second λ / 4 member is preferably 0.9 to 3, more preferably 0.9 to 2.5, still more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.

[0042] The second λ / 4 member is formed of any appropriate material that can satisfy the above characteristics. The second λ / 4 member can be, for example, a stretched film of a resin film or an oriented solidified layer of a liquid crystal compound.

[0043] Examples of resins included in the above-mentioned resin film include polycarbonate resins, polyester carbonate resins, polyester resins, polyvinyl acetal resins, polyarylate resins, cyclic olefin resins, cellulose resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyether resins, polystyrene resins, and acrylic resins. These resins may be used individually or in combination. Methods of combination include blending and copolymerization. When the second λ / 4 member exhibits inverse dispersion wavelength characteristics, a resin film containing a polycarbonate resin or a polyester carbonate resin (hereinafter sometimes simply referred to as a polycarbonate resin) can be suitably used.

[0044] Any suitable polycarbonate resin can be used as the above-mentioned polycarbonate resin. For example, the polycarbonate resin includes structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, and structural units derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic dimethanol, di, tri, or polyethylene glycol, and alkylene glycol or spiroglycol. Preferably, the polycarbonate resin includes structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, structural units derived from alicyclic dimethanol, and / or structural units derived from di, tri, or polyethylene glycol; more preferably, it includes structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, and structural units derived from di, tri, or polyethylene glycol. The polycarbonate resin may optionally include structural units derived from other dihydroxy compounds. Further details regarding polycarbonate resins suitably used for the second λ / 4 member and methods for forming the second λ / 4 member are described, for example, in Japanese Patent Publication Nos. 2014-10291, 2014-26266, 2015-212816, 2015-212817, and 2015-212818, and the descriptions in these publications are incorporated herein by reference.

[0045] The thickness of the second λ / 4 member, which is composed of a stretched resin film, is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 20 μm to 60 μm.

[0046] The orientation-solidified layer of the above-mentioned liquid crystal compound is a layer in which the liquid crystal compound is oriented in a predetermined direction within the layer, and this orientation state is fixed. Note that the term "orientation-solidified layer" is a concept that includes the orientation-cured layer obtained by curing liquid crystal monomers, as described later. In the second λ / 4 member, typically, rod-shaped liquid crystal compounds are oriented in a state where they are aligned along the slow axis direction of the second λ / 4 member (homogenous orientation). Examples of rod-shaped liquid crystal compounds include liquid crystal polymers and liquid crystal monomers. Preferably, the liquid crystal compound is polymerizable. If the liquid crystal compound is polymerizable, the orientation state of the liquid crystal compound can be fixed by polymerizing it after orientation.

[0047] The above-mentioned oriented solidified layer of liquid crystal compound (liquid crystal oriented solidified layer) can be formed by applying an orientation treatment to the surface of a predetermined substrate, coating the surface with a coating liquid containing the liquid crystal compound to orient the liquid crystal compound in the direction corresponding to the orientation treatment, and fixing the orientation state. Any appropriate orientation treatment can be used as the orientation treatment. Specifically, these include mechanical orientation treatment, physical orientation treatment, and chemical orientation treatment. Specific examples of mechanical orientation treatment include rubbing treatment and stretching treatment. Specific examples of physical orientation treatment include magnetic field orientation treatment and electric field orientation treatment. Specific examples of chemical orientation treatment include oblique deposition and photo-orientation treatment. Any appropriate conditions can be adopted for each orientation treatment depending on the purpose.

[0048] The orientation of liquid crystal compounds is achieved by treating them at a temperature that exhibits the liquid crystal phase, depending on the type of liquid crystal compound. This temperature treatment causes the liquid crystal compound to enter a liquid crystal state, and it then orients according to the orientation treatment direction on the substrate surface.

[0049] In one embodiment, the orientation state is fixed by cooling the liquid crystal compound oriented as described above. If the liquid crystal compound is polymerizable or crosslinkable, the orientation state is fixed by subjecting the liquid crystal compound oriented as described above to a polymerization treatment or a crosslinking treatment.

[0050] As the above-mentioned liquid crystal compound, any suitable liquid crystal polymer and / or liquid crystal monomer can be used. The liquid crystal polymer and liquid crystal monomer may be used individually or in combination. Specific examples of liquid crystal compounds and methods for producing liquid crystal alignment solidified layers are described, for example, in Japanese Patent Publication No. 2006-163343, Japanese Patent Publication No. 2006-178389, and International Publication No. 2018 / 123551. The descriptions in these publications are incorporated herein by reference.

[0051] The thickness of the second λ / 4 member, which is composed of a liquid crystal alignment solidification layer, is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and even more preferably 1 μm to 4 μm.

[0052] <Positive C-plate> The phase difference Rth(550) in the thickness direction of the positive C plate described above is preferably -50nm to -300nm, more preferably -70nm to -250nm, even more preferably -90nm to -200nm, and particularly preferably -100nm to -180nm. Here, "nx=ny" includes not only the case where nx and ny are exactly equal, but also the case where nx and ny are substantially equal. The in-plane phase difference Re(550) of the positive C plate is, for example, less than 10nm.

[0053] The positive C plate can be formed from any suitable material, but preferably it is composed of a film containing a liquid crystal material fixed in a homeotropic orientation. The liquid crystal material (liquid crystal compound) that can be homeotropically oriented may be a liquid crystal monomer or a liquid crystal polymer. Specific examples of methods for forming such liquid crystal compounds and positive C plates include the liquid crystal compound and the method for forming the phase difference layer described in paragraphs

[0020] to

[0028] of Japanese Patent Application Publication No. 2002-333642. In this case, the thickness of the positive C plate is preferably 0.5 μm to 5 μm.

[0054] <Reflective polarizing material> The above-described reflective polarizing member transmits polarized light parallel to its transmission axis (typically linearly polarized light) while maintaining its polarization state, and reflects light in other polarization states. Typically, the reflective polarizing member is composed of a multilayer film (sometimes referred to as a reflective polarizing film). In this case, the thickness of the reflective polarizing member is, for example, 10 μm to 150 μm, preferably 20 μm to 100 μm, and more preferably 30 μm to 60 μm.

[0055] Figure 5 is a schematic perspective view showing an example of a multilayer structure included in a reflective polarizing film. The multilayer structure 14a alternates between layers A, which have birefringence, and layers B, which have substantially no birefringence. The total number of layers constituting the multilayer structure may be 50 to 1000. For example, the refractive index nx in the x-axis direction of layer A is greater than the refractive index ny in the y-axis direction, and the refractive index nx in the x-axis direction and the refractive index ny in the y-axis direction of layer B are substantially the same, so the refractive index difference between layer A and layer B is large in the x-axis direction and substantially zero in the y-axis direction. As a result, the x-axis direction can be the reflection axis and the y-axis direction can be the transmission axis. The refractive index difference between layer A and layer B in the x-axis direction is preferably 0.2 to 0.3.

[0056] The above-mentioned layer A is typically composed of a material that exhibits birefringence upon stretching. Examples of such materials include naphthalenedicarboxylic acid polyester (e.g., polyethylene naphthalate), polycarbonate, and acrylic resins (e.g., polymethyl methacrylate). The above-mentioned layer B is typically composed of a material that does not substantially exhibit birefringence upon stretching. Examples of such materials include a copolyester of naphthalenedicarboxylic acid and terephthalic acid. The above multilayer structure can be formed by a combination of co-extrusion and stretching. For example, the materials constituting layer A and layer B are extruded and then multilayered (e.g., using a multiplier). The resulting multilayer laminate is then stretched. The x-axis direction in the illustrated example may correspond to the stretching direction.

[0057] Examples of commercially available reflective polarizing films include the product names "DBEF" and "APF" from 3M Corporation, and "APCF" from Nitto Denko Corporation.

[0058] The orthogonal transmittance (Tc) of the reflective polarizing member (reflective polarizing film) may be, for example, 0.01% to 3%. The single-element transmittance (Ts) of the reflective polarizing member (reflective polarizing film) may be, for example, 43% to 49%, preferably 45% to 47%. The degree of polarization (P) of the reflective polarizing member (reflective polarizing film) may be, for example, 92% to 99.99%.

[0059] The above orthogonal transmittance, single-element transmittance, and polarization degree can be measured, for example, using a UV-Vis spectrophotometer. The polarization degree P can be calculated using a UV-Vis spectrophotometer to measure the single-element transmittance Ts, parallel transmittance Tp, and orthogonal transmittance Tc, and then calculated from the obtained Tp and Tc using the following formula. Note that Ts, Tp, and Tc are Y values ​​measured using a 2-degree field of view (C light source) according to JIS Z 8701 and corrected for luminous efficiency. Polarization degree P(%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0060] <Absorbing polarizing material> The above-mentioned absorption-type polarizing member may typically include a resin film containing a dichroic substance (sometimes referred to as an absorption-type polarizing film). The thickness of the absorption-type polarizing film is, for example, 1 μm or more and 20 μm or less, but may also be 2 μm or more and 15 μm or less, 12 μm or less, 10 μm or less, 8 μm or less, or 5 μm or less.

[0061] The above-mentioned absorption polarizing film may be made from a single layer of resin film, or it may be made using a laminate of two or more layers.

[0062] When manufactured from a single layer of resin film, for example, an absorption polarizing film can be obtained by subjecting a hydrophilic polymer film, such as a polyvinyl alcohol (PVA) film, a partially formalized PVA film, or a partially saponified ethylene-vinyl acetate copolymer film, to dyeing treatment with a dichroic substance such as iodine or a dichroic dye, and stretching treatment. Among these, an absorption polarizing film obtained by dyeing a PVA film with iodine and uniaxially stretching it is preferred.

[0063] The above iodine staining is carried out, for example, by immersing the PVA-based film in an iodine aqueous solution. The stretching ratio for the above uniaxial stretching is preferably 3 to 7 times. Stretching may be performed after the staining treatment, or during the staining process. Alternatively, staining may be performed after stretching. If necessary, the PVA-based film may be subjected to swelling, crosslinking, washing, drying, etc.

[0064] When using the above-mentioned laminate of two or more layers, examples of laminates include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a laminate of a resin substrate and a PVA-based resin layer coated and formed on the resin substrate. An absorption polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer coated and formed on the resin substrate can be produced, for example, by applying a PVA-based resin solution to a resin substrate, drying it to form a PVA-based resin layer on the resin substrate, and obtaining a laminate of a resin substrate and a PVA-based resin layer; or by stretching and dyeing the laminate to make the PVA-based resin layer an absorption polarizing film. In this embodiment, preferably, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is formed on one side of the resin substrate. Stretching typically includes immersing the laminate in an aqueous boric acid solution and stretching it. Furthermore, stretching may, if necessary, further include air-stretching the laminate at a high temperature (e.g., 95°C or higher) before stretching in the aqueous boric acid solution. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which it shrinks by 2% or more in the width direction by heating while being transported in the longitudinal direction. Typically, the manufacturing method of this embodiment includes applying an air-assisted stretching treatment, a dyeing treatment, a water-based stretching treatment, and a drying shrinkage treatment to the laminate in this order. By introducing auxiliary stretching, it is possible to increase the crystallinity of PVA even when PVA is coated on a thermoplastic resin, making it possible to achieve high optical properties. At the same time, by increasing the orientation of PVA in advance, it is possible to prevent problems such as a decrease in the orientation of PVA and dissolution when immersed in water in the subsequent dyeing and stretching processes, making it possible to achieve high optical properties. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of polyvinyl alcohol molecules and the decrease in orientation can be suppressed compared to when the PVA-based resin layer does not contain halides. As a result, the optical properties of the absorption polarizing film obtained through processing steps in which the laminate is immersed in a liquid, such as dyeing and water-based stretching, can be improved. Furthermore, by shrinking the laminate in the width direction through a drying shrinkage treatment, the optical properties can be improved.The resulting resin substrate / absorbent polarizing film laminate may be used as is (i.e., the resin substrate may be used as a protective layer for the absorbent polarizing film), or an appropriate protective layer may be laminated on the peeled surface obtained by removing the resin substrate from the resin substrate / absorbent polarizing film laminate, or on the surface opposite to the peeled surface, depending on the purpose. Details of such a method for manufacturing an absorbent polarizing film are described, for example, in Japanese Patent Application Publication No. 2012-73580 and Japanese Patent No. 6470455. The entire contents of these publications are incorporated herein by reference.

[0065] The orthogonal transmittance (Tc) of the absorbing polarizing member (absorbing polarizing film) is preferably 0.5% or less, more preferably 0.1% or less, and even more preferably 0.05% or less. The single-layer transmittance (Ts) of the absorbing polarizing member (absorbing polarizing film) is, for example, 41.0% to 45.0%, and preferably 42.0% or more. The degree of polarization (P) of the absorbing polarizing member (absorbing polarizing film) is, for example, 99.0% to 99.997%, and preferably 99.9% or more.

[0066] <Third λ / 4 member> The in-plane phase difference Re(550) of the third λ / 4 member described above is, for example, 100 nm to 190 nm, but may also be 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The third λ / 4 member preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measured light. The Re(450) / Re(550) of the third λ / 4 member is, for example, 0.75 or more and less than 1, and may also be 0.8 or more and 0.95 or less. The third λ / 4 member preferably exhibits a refractive index characteristic in which nx > ny ≥ nz. The Nz coefficient of the third λ / 4 member is preferably 0.9 to 3, more preferably 0.9 to 2.5, even more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.

[0067] The third λ / 4 member is formed from any suitable material that can satisfy the above characteristics. The third λ / 4 member may be, for example, a stretched resin film or an oriented solidified layer of a liquid crystal compound. The same description as for the second λ / 4 member can be applied to the third λ / 4 member which is composed of a stretched resin film or an oriented solidified layer of a liquid crystal compound. The second λ / 4 member and the third λ / 4 member may be the same in composition (e.g., forming material, thickness, optical properties, etc.) or they may be different in composition.

[0068] <Protective material> The protective member described above typically includes a base material. The thickness of the base material is preferably 5 μm to 80 μm, more preferably 10 μm to 50 μm, and even more preferably 15 μm to 40 μm. The base material can be composed of any suitable film. Examples of materials that make up the film of the base material include cellulosic resins such as triacetylcellulose (TAC), polyester, polyvinyl alcohol, polycarbonate, polyamide, polyimide, polyethersulfone, polysulfone, polystyrene, cycloolefins such as polynorbornene, polyolefins, (meth)acrylic, and acetate resins. Here, (meth)acrylic refers to acrylic and / or methacrylic.

[0069] The protective member preferably comprises a substrate and a surface treatment layer formed on the substrate. The protective member having the surface treatment layer may be arranged such that the surface treatment layer is located on the front side. Specifically, the surface treatment layer may be located on the outermost surface of the first laminated portion. The surface treatment layer may have any suitable function. The surface treatment layer preferably has an anti-reflective function, for example, from the viewpoint of improving visibility. The thickness of the surface treatment layer is preferably 0.5 μm to 10 μm, more preferably 1 μm to 7 μm, and even more preferably 2 μm to 5 μm.

[0070] <Variation> In another example of the lens portion 4, a space may be formed between the second phase difference member and the reflective polarizing member. In this case, the second phase difference member may be integrated with the first lens portion 16 via an adhesive layer, and a protective member may be integrally provided on the outermost surface on the space side via an adhesive layer. Members positioned in front of the second phase difference member (reflective polarizing member, absorbing polarizing member, third phase difference member, etc.) may be integrated with the second lens portion 24 via an adhesive layer, and a protective member may be integrally provided on the outermost surface on the space side via an adhesive layer. In the lens portion having the above configuration, the angle between the slow axis of the second λ / 4 member and the reflection axis of the reflective polarizing member is, for example, within the range of 45°±2.5°, preferably within the range of 45°±2°, more preferably within the range of 45°±1°, and even more preferably within the range of about 45°.

[0071] C. Manufacturing method of the display system The display system described in Section A is manufactured by any suitable method. For example, the display system may be manufactured by arranging adjacent components in a predetermined positional relationship, such as by integrating them via an adhesive layer or by arranging them with space between them.

[0072] C-1. Embodiment I In Embodiment I, the manufacturing method of the display system includes obtaining a second film member A2 by slitting a long first film member A1, which includes a second λ / 4 member, along the longitudinal direction, as shown in Figure 6A. As shown in Figure 6B, if necessary, in addition to slitting along the longitudinal direction, slitting along the width direction may also be performed to obtain the second film member A2. In one embodiment, the second film member A2 is long. A wide second λ / 4 member may have variations in the lagging axis angle in the width direction, but by slitting the wide first film member A1 along the longitudinal direction, a narrow second film member A2 in which such variations in the lagging axis angle are suppressed can be efficiently obtained.

[0073] In this specification, "long-length" means an elongated shape in which the length is sufficiently longer than the width, and includes, for example, an elongated shape in which the length is 10 times or more, preferably 20 times or more, than the width. The length of the long-length film member may be, for example, 50 m or more, and may also be, for example, 100 m to 2000 m. The long-length film member may be wound in a roll.

[0074] The manufacturing method for the above display system may further include cutting the second film member A2 into a predetermined shape to obtain a single-sheet third film member A3. By cutting the second film member A2, which has small variation in the lagging axis angle in the width direction of the second λ / 4 member, into a predetermined shape, a single-sheet third film member A3 with small variation in the lagging axis angle can be efficiently obtained. The cutting may be performed by punching.

[0075] In the second film member A2 and the third film member A3 described above, the variation in the lagging axis angle of the second λ / 4 member is small. Therefore, by manufacturing the display system using the second film member A2 or the third film member A3, the lagging axis angle of the second λ / 4 member in the display system can be easily controlled.

[0076] The width of the first film member A1 is, for example, 500mm to 2000mm, and may be 900mm to 1500mm.

[0077] The variation in the lagging axis angle in the width direction of the second λ / 4 member in the first film member A1 is, for example, 0.5° or more, and may be between 1.0° and 5.0°. The variation in the axis angle (lagging axis, reflection axis, etc.) in the width direction of the film member can be determined by measuring the axis angle at multiple locations (for example, 10 or more locations) at intervals of 30 mm to 150 mm in the width direction of the film member, and taking the difference between the maximum and minimum values.

[0078] The width of the second film member A2 (in other words, the slit width) is, for example, 40 mm to 1500 mm, may be 45 mm to 1300 mm, or may be 50 mm to 1250 mm.

[0079] The variation in the lagging axis angle in the width direction of the second λ / 4 member in the second film member A2 is, for example, 5° or less, preferably 4° or less, more preferably 3° or less, even more preferably 2° or less, even more preferably 1° or less, and may be, for example, 0.8° or less, or for example, 0.5° or less.

[0080] The first film member A1 includes a second λ / 4 member and may further include other members as needed. Examples of other members include adhesive layers (tack layer, adhesive layer), positive C plate, protective member, etc.

[0081] In one embodiment, the first film member A1 includes an adhesive layer, a second λ / 4 member, and a protective member in that order. Depending on the purpose, the first film member A1 may further include a positive C plate between the adhesive layer and the second λ / 4 member or between the second λ / 4 member and the protective member. By slitting the first film member A1 having such a configuration along its longitudinal direction to obtain a long second film member A2; by continuously punching out the second film member A2 in its longitudinal direction to obtain a third film member A3 having a shape corresponding to the first lens portion; and by bonding the third film member A3 to the first lens portion with the adhesive layer, a display system with excellent accuracy in the lagging axis angle of the second λ / 4 member can be efficiently obtained.

[0082] C-2. Embodiment II In Embodiment II, the manufacturing method of the display system includes slitting a long first film member B1 containing a reflective polarizing member along its longitudinal direction to obtain a second film member B2. If necessary, in addition to slitting along the longitudinal direction, slitting along the width direction may also be performed to obtain the second film member B2. In one embodiment, the second film member B2 is long. A wide reflective polarizing member may have variations in the reflection axis angle in the width direction, but by slitting the wide first film member B1 along its longitudinal direction, a narrow second film member B2 with suppressed variations in the reflection axis angle can be efficiently obtained.

[0083] The manufacturing method for the above display system may further include cutting the second film member B2 into a predetermined shape to obtain a single-sheet third film member B3. By cutting the second film member B2, which has small variation in the reflection axis angle in the width direction of the reflective polarizing member, into a predetermined shape, a single-sheet third film member B3 with small variation in the reflection axis angle can be efficiently obtained. The cutting may be performed by punching.

[0084] In the second film member B2 and the third film member B3 described above, the variation in the reflection axis angle of the reflective polarizing member is small. Therefore, by manufacturing the display system using the second film member B2 or the third film member B3, the reflection axis angle of the reflective polarizing member in the display system can be easily controlled.

[0085] The width of the first film member B1 is, for example, 300mm to 1500mm, and may be 400mm to 1200mm.

[0086] The variation in the reflection axis angle in the width direction of the reflective polarizing member in the first film member B1 is, for example, 1.0° or more, and may be between 1.5° and 5.0°.

[0087] The width of the second film member B2 (in other words, the slit width) is, for example, 40 mm to 1500 mm, may be 45 mm to 1300 mm, or may be 50 mm to 1250 mm.

[0088] The variation in the reflection axis angle in the width direction of the reflective polarizing member in the second film member B2 is, for example, 1° or less, preferably 0.8° or less, and more preferably 0.5° or less.

[0089] The first film member B1 includes a reflective polarizing member and may further include other members as needed.

[0090] In one embodiment, a long laminated film member can be easily obtained by laminating a second film member B2, which is elongated and includes a reflective polarizing member having a reflection axis parallel to the longitudinal direction, and a film member, which is elongated and includes an absorptive polarizing member having an absorption axis parallel to the longitudinal direction, with their longitudinal directions aligned. This laminated film member is laminated so that the reflection axis of the reflective polarizing member and the absorption axis of the absorptive polarizing member are parallel. Alternatively, a rectangular third film member B3 can be made by cutting the long second film member B2, and laminating it with an absorptive polarizing member of substantially the same shape, with their edges aligned. This laminated film member is laminated so that the reflection axis of the reflective polarizing member and the absorption axis of the absorptive polarizing member form a desired angle (specifically, substantially parallel). By arranging such a laminated film member behind the second lens portion, a display system with excellent accuracy in the reflection axis angle of the reflective polarizing member, and furthermore, in the absorption axis angle of the absorptive polarizing member, can be efficiently obtained.

[0091] Embodiments I and II described above can be combined as needed. For example, a single-sheet laminated film member can be easily obtained by punching out a rectangular third film member A3 from a second film member A2 which includes a second λ / 4 member that is elongated and has a slow axis parallel to the width direction, such that the side direction is at an angle of 45° with respect to the width direction; punching out a rectangular third film member B3 from a second film member B2 which includes a reflective polarizing member that is elongated and has a reflection axis parallel to the elongated direction, such that the side direction is parallel to the elongated direction; and bonding the third film member A3 and the third film member B3 together with their corresponding sides aligned; thereby laminating the second λ / 4 member and the reflection axis of the reflective polarizing member at a desired angle (e.g., 45° ± 2.5°). Such a laminated film member is useful, for example, for the fabrication of the optical laminate described in Section B. [Examples]

[0092] The present invention will be specifically described below with reference to examples, but the present invention is not limited in any way to these examples. The test and evaluation methods in the examples are as follows. When "parts" is written, it means "parts by weight" unless otherwise specified, and when "%" is written, it means "percent by weight" unless otherwise specified.

[0093] (1) Thickness Thicknesses of 10 μm or less were measured using a scanning electron microscope (JEOL Ltd., product name "JSM-7100F"). Thicknesses exceeding 10 μm were measured using a digital micrometer (Anritsu Corporation, product name "KC-351C"). (2) In-plane phase difference Re(λ) The phase difference values ​​at each wavelength at 23°C were measured using a phase difference measuring device (KOBRA, manufactured by Oji Instruments Co., Ltd.).

[0094] [Manufacturing Example 1: Fabrication of λ / 4 component A] A batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and reflux condensers controlled to 100°C was used to prepare the reactor. The mixture contained 29.60 parts by weight (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by weight (0.200 mol) of isosorbide (ISB), 42.28 parts by weight (0.139 mol) of spiroglycol (SPG), 63.77 parts by weight (0.298 mol) of diphenyl carbonate (DPC), and 1.19 × 10⁻¹⁶ calcium acetate monohydrate as a catalyst. -2 Weight part (6.78×10 -5 A mol (mol) of polymer was added. After purging the reactor with reduced pressure using nitrogen, the reactor was heated with a heat transfer medium, and stirring was started when the internal temperature reached 100°C. Forty minutes after the start of heating, the internal temperature was raised to 220°C, and while controlling the pressure to maintain this temperature, the pressure was reduced to 13.3 kPa 90 minutes after reaching 220°C. The phenol vapor produced as a by-product of the polymerization reaction was directed to a reflux condenser at 100°C, and the monomer components contained in the phenol vapor were returned to the reactor. The uncondensed phenol vapor was directed to a condenser at 45°C and recovered. Nitrogen was introduced into the first reactor to restore the pressure to atmospheric pressure, and then the oligomerized reaction mixture in the first reactor was transferred to the second reactor. Next, heating and depressurization in the second reactor were started, and the internal temperature reached 240°C and the pressure 0.2 kPa in 50 minutes. Polymerization was then allowed to proceed until the predetermined stirring power was reached. Once the predetermined power level was reached, nitrogen was introduced into the reactor to restore pressure, and the resulting polyester carbonate resin was extruded into water. The strands were then cut to obtain pellets. The obtained polyester carbonate resin (pellets) was vacuum-dried at 80°C for 5 hours. Then, a long resin film with a thickness of 130 μm was produced using a film-making apparatus equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200 mm, setting temperature: 250°C), a chill roll (setting temperature: 120~130°C), and a winding machine. The obtained long resin film was stretched in the width direction at a stretching temperature of 140°C and a stretching ratio of 2.7 times. Thus, a λ / 4 member A with a thickness of 47 μm, a Re(590) of 143 nm, and an Nz coefficient of 1.2 was obtained. The Re(450) / Re(550) of the obtained λ / 4 member A was 0.856. Furthermore, the Re(400) / Re(550) of λ / 4 member A was 0.734, the Re(650) / Re(550) was 1.058, and the Re(750) / Re(550) was 1.088.

[0095] [Manufacturing Example 2: Preparation of Adhesive Layer A] A monomer mixture containing 91.5 parts butyl acrylate, 3 parts acrylic acid, 0.5 parts 4-hydroxybutyl acrylate, and 5 parts acryloylmorpholine was charged into a four-necked flask equipped with a stirring blade, thermometer, nitrogen gas inlet tube, and condenser. Furthermore, 0.1 parts 2,2'-azobisisobutyronitrile was added to 100 parts of this monomer mixture as a polymerization initiator along with 100 parts ethyl acetate. After introducing nitrogen gas to purge the flask with nitrogen while gently stirring, the polymerization reaction was carried out for 8 hours while maintaining the liquid temperature in the flask at approximately 55°C. Next, ethyl acetate was added to the resulting reaction solution to adjust the solid content to 12% by weight, preparing a solution of an acrylic polymer with a weight-average molecular weight (Mw) of 2.5 million. To 100 parts of the solid content of the obtained acrylic polymer solution, an adhesive composition was prepared by blending 0.3 parts of the peroxide-based crosslinking agent benzoyl peroxide (trade name: Niper BMT, manufactured by Nippon Oil & Fats Co., Ltd.), 0.2 parts of trimethylolpropane / tolylene diisocyanate adduct (trade name: Coronate L, manufactured by Tosoh Corporation), and 0.2 parts of a silane coupling agent (trade name: KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.). The obtained adhesive composition was applied to the release surface of a release liner, which is a PET film treated with a mold release agent on its release surface, and dried to form an adhesive layer A with a thickness of 5 μm.

[0096] [Example 1] An acrylic film (Re(550) ≈ 0 nm, thickness 40 μm) was bonded to one side of the above-mentioned λ / 4 member A (hereinafter referred to as the first λ / 4 member A) via an adhesive layer A, and another λ / 4 member A (hereinafter referred to as the second λ / 4 member A) was bonded to the other side via an adhesive layer A. Next, a reflective polarizing member (manufactured by Nitto Denko Corporation, "APCF") was bonded onto the second λ / 4 member A via an adhesive layer A. This resulted in a laminate having the configuration of [acrylic film / first λ / 4 member A / second λ / 4 member A / reflective polarizing member]. In the obtained laminate, the angle between the slow axis of the first λ / 4 member A and the slow axis of the second λ / 4 member A was 0°, and the angle between the slow axis of the second λ / 4 member A and the reflection axis of the reflective polarizing member was 45°.

[0097] [Example 2] A laminate was obtained in the same manner as in Example 1, except that the angle between the slow axis of the second λ / 4 member A and the reflection axis of the reflective polarizing member was set to 46°.

[0098] [Example 3] A laminate was obtained in the same manner as in Example 1, except that the angle between the slow axis of the second λ / 4 member A and the reflection axis of the reflective polarizing member was set to 47°.

[0099] [Comparative Example 1-1] A laminate was obtained in the same manner as in Example 1, except that the angle between the slow axis of the second λ / 4 member A and the reflection axis of the reflective polarizing member was set to 48°.

[0100] [Comparative Example 1-2] A laminate was obtained in the same manner as in Example 1, except that the angle between the slow axis of the second λ / 4 member A and the reflection axis of the reflective polarizing member was set to 49°.

[0101] [Comparative Example 2] An acrylic film (Re(550) ≈ 0 nm, thickness 40 μm) was bonded to one side of a reflective polarizing member (manufactured by Nitto Denko Corporation, "APCF") via an adhesive layer A. This resulted in a laminate having the configuration of [acrylic film / reflective polarizing member].

[0102] <Reflectance measurement> A blackboard was attached to the reflective polarizing member side of the laminate obtained in the above examples and comparative examples via a transparent adhesive layer to obtain a measurement sample. The reflectance of the acrylic film side surface of the measurement sample was determined under the following conditions when linearly polarized light was incident on the surface. ·Measuring device: Spectrophotometer (manufactured by Hitachi, product name "U-4100") • Measurement conditions: Total internal reflection measurement, incident angle 10°, measurement angle 10° ·Light source: D65 light source • Method for calculating reflectance: Reflected light intensity / Incident light intensity × 100 (%)

[0103] The average reflectance values ​​measured for the three measurement samples are shown in Table 1 and Figure 7. Table 1 also shows the angles of the reflection axis of the reflective polarizing member and the lagging axis of the first λ / 4 member A and the second λ / 4 member A, with the polarization direction of the incident light as the reference (0°), when the measurement sample is viewed from the acrylic film side ("+" indicates a clockwise angle, and "-" indicates a counterclockwise angle). For Comparative Examples 2-1 to 2-5, measurements were performed using the laminate obtained in Comparative Example 2, by shifting the direction in which the laminate was installed by 1° each time. [Table 1]

[0104] The laminate fabricated in the example is a simplified evaluation model of the display system according to an embodiment of the present invention. Specifically, the reflectance measured for the above laminate can correspond to the reflectance when linearly polarized light emitted from a display element via a polarizing member passes through a first phase difference member including a first λ / 4 member and a second phase difference member including a second λ / 4 member, and is reflected by a reflective polarizing member in the display system according to an embodiment of the present invention.

[0105] In the laminate configuration of Comparative Example 2, incident linearly polarized light is reflected by the reflective polarizing member without passing through the λ / 4 member. As shown in Table 1 and Figure 7, in this configuration, even if there is an axial misalignment of about 4° with respect to the polarization direction of the incident light, there is almost no decrease in the reflection characteristics. On the other hand, in the laminate configurations of Examples 1-3 and Comparative Examples 1-1-1-2, incident linearly polarized light is reflected by the reflective polarizing member after passing through the first λ / 4 member A and the second λ / 4 member A. In this configuration, the reflectivity decreases as the axial misalignment of the reflective polarizing member increases. This decrease in reflectivity is presumed to be because partial depolarization occurs when the linearly polarized light passes through the λ / 4 member twice, and this depolarization affects the decrease in the reflective properties due to the axial misalignment of the reflective polarizing member. However, by setting the angle between the polarization direction of the incident light to the laminate and the reflection axis of the reflective polarizing member to 87.5° to 92.5°, the decrease in reflectivity compared to the corresponding Comparative Examples 2-1-2-5 can be suppressed to less than 2%.

[0106] The present invention is not limited to the embodiments described above, and various modifications are possible. For example, the configurations shown in the embodiments above can be replaced with configurations that are substantially the same, configurations that produce the same effects, or configurations that can achieve the same purpose. [Industrial applicability]

[0107] The display system according to an embodiment of the present invention can be used, for example, in a display device such as VR goggles. [Explanation of symbols]

[0108] 2 Display System 12 Display elements 14 Reflective polarizing member 16 First lens section 18 Half Mirror 20 First phase difference member 22 Second phase difference member 24 Second lens section

Claims

1. A display system that displays images to the user, A display element having a display surface that emits light representing an image forward via a polarizing member, A reflective polarizing member is positioned in front of the display element and reflects light emitted from the display element, A first lens portion is arranged in the optical path between the display element and the reflective polarizing member, A half-mirror is disposed between the display element and the first lens portion, which transmits light emitted from the display element and reflects the light reflected by the reflective polarizing member toward the reflective polarizing member, A first λ / 4 member is arranged in the optical path between the display element and the half mirror, A second λ / 4 member is positioned in the optical path between the half mirror and the reflective polarizing member, Equipped with, The first λ / 4 member has a Re(550) of 100 nm to 190 nm and satisfies all of the following: 0.75 ≤ Re(450) / Re(550) < 1, Re(400) / Re(550) < 0.85, Re(650) / Re(550) > 1.03, and Re(750) / Re(550) > 1.

05. The second λ / 4 member has a Re(550) of 100 nm to 190 nm and satisfies all of the following: 0.75 ≤ Re(450) / Re(550) < 1, Re(400) / Re(550) < 0.85, Re(650) / Re(550) > 1.03, and Re(750) / Re(550) > 1.

05. The light emitted through the polarizing member is linearly polarized. The angle between the polarization direction of the linearly polarized light and the reflection axis of the reflective polarizing member is 87.5° to 92.5° or 0° to 2.5°. Display system.

2. The display system according to claim 1, wherein the angle between the slow axis of the second λ / 4 member and the reflection axis of the reflective polarizing member is 42.5° to 47.5°.

3. The angle between the absorption axis of the polarizing member included in the display element and the lagging axis of the first λ / 4 member is 40° to 50°. The angle between the slow axis of the first λ / 4 member and the slow axis of the second λ / 4 member is between 0° and 10°. The angle between the polarization direction of the linearly polarized light and the reflection axis of the reflective polarizing member is 87.5° to 92.5°. The display system according to claim 1.

4. The angle between the absorption axis of the polarizing member included in the display element and the lagging axis of the first λ / 4 member is 40° to 50°. The angle between the slow axis of the first λ / 4 member and the slow axis of the second λ / 4 member is 80° to 100°. The angle between the polarization direction of the linearly polarized light and the reflection axis of the reflective polarizing member is between 0° and 2.5°. The display system according to claim 1.

5. An optical laminate used in a display system according to any one of claims 1 to 4, The second λ / 4 member and the reflective polarizing member are included, The angle between the slow axis of the second λ / 4 member and the reflection axis of the reflective polarizing member is 42.5° to 47.5°. The second λ / 4 member is an optical laminate in which Re(550) is 100 nm to 190 nm and satisfies all of the following conditions: 0.75 ≤ Re(450) / Re(550) < 1, Re(400) / Re(550) < 0.85, Re(650) / Re(550) > 1.03, and Re(750) / Re(550) > 1.

05.

6. A manufacturing method for manufacturing a display system according to any one of claims 1 to 4, The method includes slitting a long first film member, which includes the second λ / 4 member and has a width of 500 mm to 2000 mm, along its longitudinal direction to obtain a second film member having a width of 40 mm to 1250 mm, A manufacturing method in which the second film member has a variation in the lagging axis of the second λ / 4 member in the width direction of 1° or less.

7. A manufacturing method for manufacturing a display system according to any one of claims 1 to 4, The method includes slitting a long first film member, which includes the reflective polarizing member and has a width of 300 mm to 1500 mm, along its longitudinal direction to obtain a second film member having a width of 40 mm to 1250 mm. A manufacturing method for the second film member, wherein the variation in the reflection axis of the reflective polarizing member in the width direction is 1° or less.

Citation Information

Patent Citations

  • Optical film roll

    JP2013218317A

  • Laminate for organic el displays and circular polarizing plate used therefor

    JP2021103286A

  • Image display device

    JP2021124540A