Manufacturing method of wiring boards

By forming cuts and gaps in a laminated sheet with a carrier, release layer, and metal layer, the method facilitates easy and reliable carrier peeling, addressing the challenges of conventional manufacturing methods.

JP7954601B2Active Publication Date: 2026-11-20MITSUI MINING & SMELTING CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023031748
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-02-04
Filing Date
2023-03-02
Publication Date
2026-11-20
Estimated Expiration
2042-06-15

AI Technical Summary

Technical Problem

Conventional methods for manufacturing wiring boards face challenges in easily and reliably removing carriers due to difficulties related to the thickness of the wiring board, semiconductor elements, and resin-containing layers, often requiring specialized equipment or complex processes.

Method used

A method involving making predetermined cuts in a laminated sheet comprising a carrier, release layer, and metal layer, dividing them into central and peripheral portions, and inserting a thin piece at a specific angle to form a gap between the metal layer and the carrier, allowing for easy and reliable peeling.

Benefits of technology

Enables simple and reliable carrier removal without specialized equipment, suitable for various thicknesses of resin-containing layers, enhancing the manufacturing process's efficiency and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954601000001
    Figure 0007954601000001
  • Figure 0007954601000002
    Figure 0007954601000002
  • Figure 0007954601000003
    Figure 0007954601000003
Patent Text Reader

Abstract

To provide a method for manufacturing a wiring board, which enables a carrier to be peeled off simply and reliably. [Solution] A method for manufacturing a wiring board, comprising the steps of: preparing a laminate sheet having a release layer and a metal layer in that order on a carrier; making an incision in the laminate sheet from the side opposite the carrier so that the incision passes inside the outer edge of the laminate sheet when viewed in plan, and penetrates the metal layer and release layer when viewed in cross section, dividing the metal layer and release layer into a central portion and a peripheral portion using the incision as a boundary; and forming a gap between the metal layer and the carrier from the incision.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a wiring board.

Background Art

[0002] In recent years, in order to increase the mounting density of printed wiring boards and achieve miniaturization, the multilayering of printed wiring boards has been widely carried out. Such multilayer printed wiring boards are used in many portable electronic devices for the purpose of weight reduction and size reduction. Further, these multilayer printed wiring boards are required to have a further reduced thickness of interlayer insulating layers and an even lighter weight as wiring boards.

[0003] As a technique that satisfies such requirements, a method for manufacturing a multilayer printed wiring board using a coreless build-up method has been adopted. The coreless build-up method is a method of forming multiple layers by alternately laminating (building up) insulating layers and wiring layers without using a so-called core substrate. In the coreless build-up method, it has been proposed to use a metal foil with a carrier so that the support and the multilayer printed wiring board can be easily separated. For example, Patent Document 1 (Japanese Unexamined Patent Publication No. 2005-101137) discloses a method including: attaching an insulating resin layer to the carrier surface of a copper foil with a carrier to form a support, forming a first wiring conductor on the ultra-thin copper layer side of the copper foil with a carrier through processes such as photoresist processing, pattern electrolytic copper plating, and resist removal, then forming a build-up wiring layer, peeling off the support substrate with a carrier, and removing the ultra-thin copper layer, for manufacturing a package substrate for mounting a semiconductor element.

[0004] Furthermore, in order to miniaturize embedded circuits as shown in Patent Document 1, a carrier-mounted metal foil with a metal layer thickness of 1 μm or less is desired. Therefore, in order to reduce the thickness of the metal layer, it has been proposed to form the metal layer by a vapor phase method such as sputtering. For example, Patent Document 2 (International Publication No. 2017 / 150283) discloses a carrier-mounted copper foil in which a release layer, an anti-reflective layer, and an ultrathin copper layer (e.g., a film thickness of 300 nm) are formed by sputtering on a carrier such as a glass sheet. Patent Document 3 (International Publication No. 2017 / 150284) also discloses a carrier-mounted copper foil in which an intermediate layer (e.g., an adhesive metal layer and a release assist layer), a release layer, and an ultrathin copper layer (e.g., a film thickness of 300 nm) are formed by sputtering on a carrier such as a glass sheet. Patent documents 2 and 3 teach that interposing an intermediate layer made of a predetermined metal provides excellent stability in the mechanical peel strength of the carrier, and that the anti-reflective layer exhibits a desirable dark color, thereby improving visibility in image inspection (e.g., automated image inspection (AOI)).

[0005] In particular, with the increasing miniaturization and power saving of electronic devices, there is a growing need for higher integration and thinner semiconductor chips and printed circuit boards. To meet these needs, the adoption of FO-WLP (Fan-Out Wafer Level Packaging) and PLP (Panel Level Packaging) has been considered in recent years as next-generation packaging technologies. Furthermore, the adoption of coreless build-up methods is also being considered for FO-WLP and PLP. One such method is called the RDL-First (Redistribution Layer-First) method, in which a wiring layer and, if necessary, a build-up wiring layer are formed on the surface of a coreless support, the chip is mounted and sealed, and then the support is peeled off. For example, Patent Document 4 (Japanese Patent Application Publication No. 2015-35551) discloses a method for manufacturing a semiconductor device, which includes forming a metal delamination layer on the main surface of a support made of glass or a silicon wafer, forming an insulating resin layer thereon, forming a redistribution layer including a build-up layer thereon, mounting and sealing a semiconductor integrated circuit thereon, exposing the delamination layer by removing the support, exposing secondary mounting pads by removing the delamination layer, forming solder bumps on the surface of the secondary mounting pads, and secondary mounting.

[0006] Incidentally, when peeling off a carrier with a wiring layer fabricated using a coreless build-up method or the like, the wiring layer may bend significantly, causing disconnection or peeling, which can reduce the reliability of the wiring layer's connection. Therefore, methods for removing carriers that address this problem have been proposed. For example, Patent Document 5 (Japanese Patent Application Publication No. 2020-119952) discloses a method for removing a carrier from a workpiece (for example, including a wiring layer in contact with the temporary adhesive layer, a plurality of chips bonded to the wiring layer, and a mold layer that seals each chip) that is provided on the surface of the carrier via a temporary adhesive layer. In the method disclosed in Patent Document 5, a stepped portion is formed on the back side of the carrier that the workpiece is provided on, protruding laterally compared to the front side of the carrier. By holding the workpiece from above and applying a downward force to the stepped portion, the carrier can be easily removed from the workpiece. Furthermore, Patent Document 6 (International Publication No. 2018 / 173807) discloses a method for manufacturing a wiring board, in which a composite laminate (including a support, a release layer, and a multilayer wiring board) is brought into close contact with a stage, and the support or multilayer wiring board is peeled off from the release layer to form a predetermined convex curved surface. According to this method, cracks in the support and defects such as cracks and disconnections in the multilayer wiring board can be prevented, and stable peeling is possible. [Prior art documents] [Patent Documents]

[0007] [Patent Document 1] Japanese Patent Publication No. 2005-101137 [Patent Document 2] International Publication No. 2017 / 150283 [Patent Document 3] International Publication No. 2017 / 150284 [Patent Document 4] Japanese Patent Publication No. 2015-35551 [Patent Document 5] Japanese Patent Publication No. 2020-119952 [Patent Document 6] International Publication No. 2018 / 173807 [Overview of the project]

[0008] However, conventional methods for manufacturing wiring boards have limitations, such as difficulty in removing carriers depending on the thickness of the wiring board (e.g., the wiring layer, semiconductor element (chip), and resin-containing layer including the resin layer), or the need for specialized equipment or complex processes for carrier removal. Therefore, there is room for improvement from the perspective of simple and reliable carrier removal.

[0009] The present inventors have now discovered that by making predetermined cuts in a laminated sheet comprising a carrier, a release layer, and a metal layer in that order, dividing the metal layer and the release layer into a central and peripheral portion, and optionally inserting a thin piece at a predetermined angle through these cuts to form a gap between the metal layer and the carrier, it is possible to easily and reliably peel off the carrier and manufacture a wiring board.

[0010] Therefore, the object of the present invention is to provide a method for manufacturing a wiring board that allows for easy and reliable removal of carriers.

[0011] The present invention provides the following embodiments. [Aspect 1] A method for manufacturing a wiring board, A step of preparing a laminated sheet having a release layer and a metal layer arranged in order on a carrier, A step of making an incision from the side of the laminated sheet opposite to the carrier such that when the laminated sheet is viewed in plan, the incision passes inside the outer edge of the laminated sheet, and when the laminated sheet is viewed in cross-section, the incision penetrates the metal layer and the release layer, thereby dividing the metal layer and the release layer into a central part and a peripheral part with the incision as the boundary, A step of inserting a thin slice from the aforementioned cut toward the central part of the metal layer or the release layer as desired, thereby forming a gap between the metal layer and the carrier, wherein, when the laminated sheet is viewed in cross-section, the insertion angle of the thin slice with respect to the main surface of the carrier preferably exceeds 0°. A method for manufacturing a wiring board, including [Aspect 2] A method for manufacturing a wiring board, A step of preparing a laminated sheet having a release layer and a metal layer arranged in order on a carrier, A step of making an incision from the side of the laminated sheet opposite to the carrier such that when the laminated sheet is viewed in plan, the incision passes inside the outer edge of the laminated sheet, and when the laminated sheet is viewed in cross-section, the incision penetrates the metal layer and the release layer, thereby dividing the metal layer and the release layer into a central part and a peripheral part with the incision as the boundary, A step of inserting a thin slice from the aforementioned cut toward the central part of the metal layer or the release layer as desired, thereby forming a gap between the metal layer and the carrier, wherein, when the laminated sheet is viewed in cross-section, the insertion angle of the thin slice with respect to the main surface of the carrier preferably exceeds 0°. Includes, A method for manufacturing a wiring board, wherein the carrier is a single-crystal silicon carrier having a notch or orientation flat on its outer circumference, and in the process of forming the cut, the cut is made such that when the angle θ is defined clockwise starting from a half-line from the center of the single-crystal silicon carrier to the midpoint of the notch or orientation flat, the direction of propagation of the external stress is within the range of 1° < θ < 89°. [Aspect 3] A method for manufacturing a wiring board according to embodiment 1 or 2, further comprising the step of expanding the gap by moving the thin piece along the cut, if desired, starting from the gap formed. [Aspect 4] A method for manufacturing a wiring board according to embodiment 3, further comprising the step of, after widening the gap, applying force to the laminated sheet in a direction that separates the carrier and the metal layer, thereby peeling the metal layer from the carrier using the gap as a starting point. [Aspect 5] The method for manufacturing a wiring board according to any one of embodiments 1 to 4, wherein the notch is formed so that at least a portion of the carrier does not penetrate when the laminated sheet is viewed in cross-section. [Aspect 6] The method for manufacturing a wiring board according to any one of aspects 1 to 5, wherein the width of the cut is 0.01 mm or more and 20 mm or less. [Aspect 7] The method for manufacturing a wiring board according to any one of aspects 1 to 6, wherein the thin piece is a cutting blade, and the cutting blade is any one of a flat blade, a triangular blade, a square blade, a circular blade, and a rotary blade. [Aspect 8] The method for manufacturing a wiring board according to any one of aspects 1 to 7, wherein the cut is formed in a linear pattern such that the peripheral portion surrounds the central portion when the laminated sheet is viewed in plan. [Aspect 9] The method for manufacturing a wiring board according to any one of aspects 3 to 8, wherein the movement of the thin piece is performed over a part or the entire length of the cut. [Aspect 10] The method for manufacturing a wiring board according to any one of aspects 4 to 9, wherein the peeling of the metal layer is performed in a state where the outer edge portion of the carrier or the laminated sheet is gripped or supported. [Aspect 11] The method for manufacturing a wiring board according to any one of aspects 1 to 10, wherein the insertion angle is more than 0.1° and 60° or less. [Aspect 12] The method for manufacturing a wiring board according to any one of aspects 1 to 11, wherein in forming the gap, the insertion width of the thin piece into the laminated sheet is 0.1 mm or more. [Aspect 13] The method for manufacturing a wiring board according to any one of aspects 1 to 12, wherein the thin piece is composed of at least one member selected from the group consisting of ferrous materials, non-ferrous metals, ceramics, and diamond. [Aspect 14] The method for manufacturing a wiring board according to any one of aspects 1 to 13, wherein the laminated sheet further includes a resin-containing layer on a surface of the metal layer opposite to the release layer. [Aspect 15] The method for manufacturing a wiring board according to aspect 14, wherein the resin-containing layer includes at least one selected from the group consisting of a wiring layer, a semiconductor element, and a resin layer. [Aspect 16] A method for manufacturing a wiring board according to embodiment 14 or 15, wherein the thickness of the resin-containing layer is 1000 μm or less. [Aspect 17] A method for manufacturing a wiring board according to any one of embodiments 14 to 16, wherein the insertion of the thin piece in the formation of the gap is performed against the resin-containing layer. [Brief explanation of the drawing]

[0012] [Figure 1A] This is a schematic cross-sectional flow diagram showing an example of a manufacturing method for the wiring board of the present invention, corresponding to the initial steps (steps (i) and (ii)). [Figure 1B] This process flowchart shows the corresponding process as depicted in Figure 1A, in a schematic top view from the side opposite the carrier of the laminated sheet. [Figure 2A] This is a schematic cross-sectional flow diagram showing an example of a manufacturing method for a wiring board according to the present invention, and corresponds to the intermediate steps (steps (iii) and (iv)) following the steps shown in Figure 1A. [Figure 2B] This process flowchart shows the corresponding process as depicted in Figure 2A, in a schematic top view from the side opposite the carrier of the laminated sheet. [Figure 3] This is a schematic cross-sectional flow diagram showing an example of a manufacturing method for the wiring board of the present invention, corresponding to the later steps (steps (v) and (vi)) following the steps shown in Figure 2A. [Figure 4] This schematic cross-sectional flow diagram shows an example of a process in which gaps are formed in a fully molded laminated sheet using a machine tool. [Figure 5] This is a schematic cross-sectional flow diagram showing an example of a conventional wiring board manufacturing method, corresponding to the first half of the process (steps (i) and (ii)). [Figure 6] This is a schematic cross-sectional flow diagram showing an example of a conventional wiring board manufacturing method, corresponding to the later steps (steps (iii) and (iv)) following the steps shown in Figure 5. [Figure 7] This diagram illustrates the diameter, thickness, and angle of the rotating blade. [Figure 8] This is a schematic cross-sectional view showing an example of a carrier detachment method. [Figure 9A] This is a top view flowchart showing a process where, in the case of a silicon wafer with carriers having notches, the direction of propagation of external stress due to the formation of a notch or carrier delamination coincides with the cleavage direction, causing a crack to form in the silicon wafer. This corresponds to the first half of the process (steps (i) and (ii)). [Figure 9B] This is a top view flowchart showing a process where, in the case of a silicon wafer with carriers having notches, the direction of propagation of external stress due to the formation of a notch or delamination of the carriers coincides with the cleavage direction, causing a crack to form in the silicon wafer. This corresponds to the later steps (steps (iii) and (iv)) following the steps shown in Figure 9A. [Figure 10A] This is a top view flowchart showing a process in which, when the carrier is a silicon wafer with notches, the direction of propagation of external stress due to the formation of a notch or carrier delamination does not match the cleavage direction, and cracks in the silicon wafer are suppressed. This corresponds to the first half of the process (steps (i) and (ii)). [Figure 10B] This is a top view flowchart showing a case where, in the case of a silicon wafer with carriers having notches, the direction of propagation of external stress due to the formation of notches or carrier delamination does not match the cleavage direction, and cracks in the silicon wafer are suppressed. This corresponds to the later steps (steps (iii) and (iv)) following the steps shown in Figure 10A. [Figure 11] This figure shows the carrier cleavage orientation when the carrier is on a silicon wafer with an orientation flat. [Modes for carrying out the invention]

[0013] Manufacturing method of wiring boards The present invention relates to a method for manufacturing a wiring board. The method of the present invention includes the steps of (1) preparing a laminated sheet, (2) forming cuts, (3) forming gaps, (4) optionally enlarging the gaps, and (5) optionally peeling off carriers.

[0014] The following explains each of the steps (1) to (5) with reference to the diagrams.

[0015] (1) Preparation of laminated sheets An example of a method for manufacturing a wiring board according to the present invention is shown in Figures 1 to 3. First, as shown in Figure 1A(i), a laminated sheet 10 is prepared, in which a release layer 15 and a metal layer 16 are provided in order on a carrier 12. The release layer 15 is provided on the carrier 12 and is a layer that contributes to the separation of the carrier 12 from the metal layer 16. The metal layer 16 is a layer made of metal provided on the release layer 15.

[0016] The laminated sheet 10 may further have an intermediate layer 14 between the carrier 12 and the release layer 15. Each of the intermediate layer 14, the release layer 15, and the metal layer 16 may be a single layer consisting of one layer, or a multilayer consisting of two or more layers.

[0017] The carrier 12 may be composed of glass, ceramics, silicon, resin, or metal, but is preferably a silicon-containing substrate or a glass substrate. Any substrate containing Si as an element can be used as the silicon-containing substrate, such as an SiO2 substrate, SiN substrate, Si single-crystal substrate, or Si polycrystalline substrate. More preferably, it is a glass carrier, a single-crystal silicon substrate, or a polycrystalline silicon substrate. According to a preferred embodiment of the present invention, the carrier 12 is disc-shaped with a diameter of 100 mm or more, and more preferably disc-shaped with a diameter of 200 mm to 450 mm. According to another preferred embodiment of the present invention, the carrier 12 is rectangular with a short side of 100 mm or more, and more preferably with a short side of 150 mm to 650 mm. The rectangular carrier 12 may be roll-shaped with a long side sufficiently longer than its short side, but preferably with a long side of 200 mm to 650 mm.

[0018] As shown in Figures 1A(i) and 1B(i), the laminated sheet 10 may further include a resin-containing layer 20 on the side of the metal layer 16 opposite to the release layer 15. The resin-containing layer 20 preferably includes at least one selected from the group consisting of a wiring layer, a semiconductor element, and a resin layer (molded resin layer). For example, the resin-containing layer 20 may include at least a resin layer. More preferably, the resin-containing layer 20 includes a wiring layer, a semiconductor element provided on the wiring layer, and a resin layer surrounding at least the semiconductor element. The resin layer may have a structure that surrounds only the semiconductor element (flange mold structure), or it may have a structure that surrounds both the semiconductor element and the wiring layer (full mold structure). In any case, the resin-containing layer 20 can be formed in the same way as conventional wiring substrate manufacturing methods. The above-mentioned semiconductor element includes those equipped with device functions such as integrated circuits and sensors.

[0019] The thickness of the resin-containing layer 20 is preferably 1000 μm or less, more preferably 10 μm to 500 μm, even more preferably 50 μm to 400 μm, and particularly preferably 70 μm to 300 μm. This allows for miniaturization and weight reduction of the wiring board while also providing excellent heat dissipation performance of the resin-containing layer 20. Furthermore, even when the resin-containing layer 20 is this thin, the present invention ensures reliable peeling of the carrier 12.

[0020] The laminated sheet 10 can be prepared, for example, as follows. First, a carrier-mounted metal foil 18 is prepared on a carrier 12, comprising an optional intermediate layer 14 (i.e., any layer), a release layer 15, and a metal layer 16. Next, a first wiring layer is formed on the surface of the metal layer 16. After that, a resin-containing layer 20 is constructed based on the first wiring layer. The formation of the first wiring layer and the construction of the resin-containing layer 20 can be carried out by known methods, and for example, the coreless build-up method described above can be preferably employed. In addition, a semiconductor element 120b may be mounted on the first wiring layer (or on a wiring layer 120a constructed based on the first wiring layer) as needed (see Figure 5(i)). The electrodes of the semiconductor element 120b are joined to the wiring of the wiring layer 120a, thereby electrically connecting the semiconductor element 120b to the wiring layer 120a. It is preferable that the semiconductor element 120b is covered with a resin layer 120c after being mounted on the wiring layer 120a. In this specification, the carrier 12, the intermediate layer 14 (if present), the release layer 15, and the metal layer 16 may be collectively referred to as "metal foil with carrier 18". Preferred embodiments of the metal foil with carrier 18 will be described later.

[0021] (2) Formation of cuts An incision S is made in the prepared laminated sheet 10 from the side opposite to the carrier 12. As shown in Figure 1B(ii), this incision S is made so that, when the laminated sheet 10 is viewed from above, it passes inside the outer edge of the laminated sheet 10. At this time, as shown in Figure 1A(ii), when the laminated sheet 10 is viewed in cross-section, the incision S penetrates the metal layer 16, the release layer 15, and the intermediate layer 14 (if present). By making such an incision S in the laminated sheet 10, the metal layer 16, the release layer 15, and the intermediate layer 14 (if present) are divided into a central part C and a peripheral part P with the incision S as the boundary (see Figures 1A(ii) and 1B(ii)). This makes it possible to form a gap from the incision S, as described later, and allows for easy and reliable peeling of the carrier 12 (peeling off the metal layer 16).

[0022] The method for forming the notch S is not particularly limited and can be any known method. For example, the notch S can be formed in the laminated sheet 10 using a cutting tool such as a cutter CT as shown in Figure 1A(ii), or a machine tool such as a cutting blade. When forming the notch S using a machine tool, it is preferable to align the notch S by visually inspecting the laminated sheet 10 from the horizontal direction with a camera or the like. Here, Figure 4 shows an example of processing a laminated sheet 10 with a full mold structure (a structure in which the resin layer constituting the resin-containing layer 20 surrounds both the semiconductor element and the wiring layer) using a machine tool. As shown in Figures 4(i) to (iii), when forming a notch S and a gap G described later on a laminated sheet 10 with a full mold structure using a machine tool, it is desirable to determine the processing position (distance from the side edge of the resin layer) by visually inspecting the laminated sheet 10 from the horizontal direction with a camera (not shown) (see Figure 4(i)), and then form the notch S and gap G at the determined processing position using a machine tool (e.g., a rotary blade RC) (see Figures 4(ii) and (iii)). Furthermore, when processing a laminated sheet 10 with a flange mold structure (a structure in which the resin layer constituting the resin-containing layer 20 surrounds only the semiconductor element), it is desirable to visually inspect the vicinity of the side edge of the resin layer with a camera and form a cut S along this side edge of the resin layer (see Figure 1A(ii)).

[0023] As shown in Figure 1A(ii), it is preferable that the notch S is formed so that at least a portion of the carrier 12 does not penetrate when the laminated sheet 10 is viewed in cross-section. This makes it possible to insert and move the thin slice using the carrier 12 as a guide in the gap formation and enlargement process described later, and makes the peeling of the carrier 12 (peeling off the metal layer 16) even simpler and more reliable.

[0024] The width of the notch S (the width of the laminated sheet 10 in the surface direction) is preferably 0.01 mm to 20 mm, more preferably 0.05 mm to 15 mm, and even more preferably 0.2 mm to 10 mm. By setting it within this range, in the gap formation and enlargement process described later, for example, thin pieces can be inserted more accurately into the intended location between the release layer 15 and the metal layer 16, and the subsequent peeling process can be carried out smoothly. Furthermore, it has the effect of preventing unnecessary scratches from occurring on the release layer 15, the metal layer 16, etc. The notch S is preferably formed in a direction substantially perpendicular to the main surface of the carrier 12 (in the thickness direction of the laminated sheet 10). That is, it is desirable to insert the blade of a cutting tool or the like into the side of the laminated sheet 10 opposite to the carrier 12 so that it is substantially perpendicular to the main surface of the carrier 12 (for example, within the range of 90° ± 5°).

[0025] Preferably, the notches S are formed in a linear pattern such that the peripheral portion P surrounds the central portion C when the laminated sheet 10 is viewed from above. This linear pattern may also be formed in a curved shape; for example, if the laminated sheet 10 is disc-shaped, it is also possible to form the notches S in a circular pattern. The example shown in Figure 1B(ii) shows that the notches S are formed in a rectangular pattern (a linear pattern on four sides) by processing at a certain distance from the outer edge (four sides) of a rectangular laminated sheet 10. However, when using a rectangular laminated sheet 10, it is not always necessary to form the notches S in the linear pattern on four sides as described above; for example, the notches S may be formed in a linear pattern on one to three sides, as long as a gap sufficient for inserting a thin slice can be formed.

[0026] In the process of forming the notch, if the carrier is a single-crystal silicon carrier, it is preferable to pay attention to the direction of the progression of the notch S. Here, the process of forming the notch and / or the carrier peeling process described later, when the carrier 12 of the carrier-attached metal foil 18 is a single-crystal silicon carrier, is shown in Figures 9A, 9B, 10A, and 10B, respectively. In the process shown in Figures 9A to 10B, a carrier-attached metal foil 18 in which the carrier 12 is a single-crystal silicon carrier is prepared (Figures 9A(i) and 10A(i)), a resin-containing layer 20 is formed on the metal layer 16 of the carrier-attached metal foil 18 (Figures 9A(ii) and 10A(ii)), and then the notch S is formed and / or the carrier 12 is peeled off (Figures 9B(iii) and (iv) and 10B(iii) and (iv)). A single-crystal silicon carrier typically has a notch N, as shown in Figures 9A(i) and 10A(i), or an orientation flat OF (also called an orientation flat), as shown in Figure 11, on its outer circumference to indicate a reference point for crystal orientation. Generally, an orientation flat is formed when the diameter of a single-crystal silicon is 200 mm or less, and a notch is formed when the diameter is 200 mm or more. Hereinafter, this notch N and orientation flat OF may be collectively referred to as "notch, etc."

[0027] As shown in Figures 9B(iii) and (iv), if a notch S is formed in a direction in which the direction of propagation of the external stress ST coincides with the cleavage direction CL, there is a possibility that the silicon carrier may be fractured, such as by the generation of a crack CR along the cleavage direction CL, starting from the point where the external stress ST was first applied. To suppress such fracture due to cleavage of the silicon carrier, when the carrier 12 is a single-crystal silicon carrier, it is preferable to apply the external stress ST in such a way as shown in Figures 10B(iii) and (iv) that it does not coincide with either the direction of the cleavage direction CL on the x-axis (left-right direction in the figure) or the y-axis (up-down direction in the figure) on the silicon carrier, thereby forming a notch S in the carrier 12.

[0028] Therefore, according to a preferred embodiment of the present invention, the carrier 12 is a single-crystal silicon carrier having a notch or the like on its outer circumference, and in the process of forming the notch S, when the angle θ is defined clockwise starting from a half-line L from the center of the single-crystal silicon carrier to the notch or the like, the notch is made such that the direction of external stress propagation is within the range of 1° < θ < 89°.

[0029] Let's explain in more detail. As shown in Figures 9A(i) and 10(i), if we define the angle θ clockwise starting from the half-line L from the center of the carrier 12 to the midpoint of the notch N or orientation flat OF, then θ = 0°, 90°, 180°, and 270° correspond to the cleavage orientation CL. Therefore, regarding the direction of propagation θr of the external stress ST due to the cut, as shown in Figure 9B(iii), it is preferable to perform the cut while maintaining the direction of propagation of the external stress ST so that θr is within the range of 1° < θr < 89°, and more preferably within the range of 5° < θr < 85°. By introducing a cut that satisfies such a range of θr, it is possible to suppress the fracture of the carrier 12 made of silicon wafer. Particularly preferred ranges of θr during this cut are within 45±5°, within 135±5°, within 225±5°, and within 315±5°, clockwise from the half-line L. These angles correspond to the crystal orientation of the silicon wafer. <100> Because the wafer is least likely to cleave in these directions, propagating external stress at these angles allows for the formation of cuts S while effectively suppressing wafer fracture.

[0030] (3) Formation of gaps A thin slice T is inserted from the cut S into the laminated sheet 10 toward the central part C of the resin-containing layer 20 (if present), metal layer 16, release layer 15, or intermediate layer 14 (if present) as desired (Figures 2A(iii) and 2B(iii)). At this time, as shown in Figure 2A(iii), when the laminated sheet 10 is viewed in cross-section, the insertion angle θ of the thin slice T with respect to the main surface of the carrier 12 is preferably greater than 0°. By doing so, a gap G can be formed between the metal layer 16 and the carrier 12 from the cut S (Figure 2A(iv)), and this gap G can be used as a starting point to easily and reliably peel off the carrier 12.

[0031] In recent years, in order to further thin semiconductor packages, the resin-containing layer has been thinned by polishing the resin layer (molding resin), etc. However, conventional carrier peeling methods, such as the one disclosed in Patent Document 5, require a step of holding the highly rigid resin-containing layer from above with a holding unit, and are not adequately suited to such thinning, i.e., resin-containing layers with reduced rigidity. Here, Figures 5 and 6 show an example of a conventional wiring substrate manufacturing method. In the conventional process shown in Figures 5 and 6, first, a laminated sheet 110 is prepared in which a resin-containing layer 120 is provided on a carrier-attached metal foil 118 (Figure 5(i)). In this example, the carrier-attached metal foil 118 has an intermediate layer 114, a peeling layer 115, and a metal layer 116 in that order on a carrier 112. The resin-containing layer 120 also includes a wiring layer 120a, a semiconductor element 120b, and a resin layer 120c. Next, using blade B, an incision is made from the resin-containing layer 120 side of the prepared laminated sheet 110, reaching the metal foil 118 with the carrier, and the outer edge portion outside the incision in the resin-containing layer 120 is removed to form an extended portion E (Figure 5(ii)). Then, with the resin-containing layer 120 fixed by the suction jig SJ, a force is applied to the formed extended portion E in a direction that separates the carrier 112 from the resin-containing layer 120 (Figure 6(iii)). In this way, the carrier 112 and the intermediate layer 114 are peeled off from the resin-containing layer 120 at the position of the release layer 115 (Figure 6(iv)).

[0032] However, according to the inventors' findings, it has been found that with such conventional methods, when the resin-containing layer 120 is thin, less than 300 μm, peeling of the carrier 112 can be difficult. One of the reasons for this is as follows: In the carrier peeling method shown in Figures 5 and 6, when the thickness of the resin-containing layer 120 is greater than 300 μm, the residual stress at the interface between the resin-containing layer 120 and the carrier-attached metal foil 118 is large, and it is thought that this residual stress promotes the peeling of the carrier 112, etc. On the other hand, when the thickness of the resin-containing layer 120 is small, less than 300 μm, the residual stress at the interface between the resin-containing layer 120 and the carrier-attached metal foil 118 is small, and as a result, it is thought that the peeling of the carrier 112, etc. is less likely to be promoted.

[0033] In contrast, the present invention creates a gap G between the metal layer 16 and the carrier 12 (typically in or near the release layer 15), which triggers the reliable delamination of the carrier 12 (peeling off the metal layer 16). Specifically, in the manufacturing of semiconductor packages, the gap between the metal layer 16 and the carrier 12 has a certain level of delamination strength to prevent unintended delamination of the carrier 12 as a support. In this regard, by creating a gap G where the metal layer 16 and the carrier 12 are partially delaminated, a stress concentration area that serves as the starting point for delamination can be formed between the metal layer 16 and the carrier 12 in the subsequent delamination process. This makes it possible to reliably delaminate the carrier 12, which has fulfilled its role as a support, regardless of the thickness of the resin-containing layer 20. Furthermore, the method of the present invention allows for the delamination of the carrier 12 by a simple method of forming an incision S and a gap G, without requiring a dedicated device or complex process. In this way, a predetermined cut S is made in a laminated sheet 10 having a carrier 12, a release layer 15, and a metal layer 16 in that order, dividing the metal layer 16 and the release layer 15 into a central part C and a peripheral part P. A thin piece T is optionally inserted through this cut S at a predetermined angle θ to form a gap G between the metal layer 16 and the carrier 12, thereby enabling the simple and reliable peeling off of the carrier 12 and the manufacture of a wiring board.

[0034] The insertion angle θ of the thin film T with respect to the main surface of the carrier 12 is defined as the angle between the tip of the thin film T and the surface of the carrier 12 at the point where the tip of the thin film T (or a virtual line passing through the tip) touches the surface of the carrier 12 when the laminated sheet 10 is viewed in cross-section, as shown in Figure 2A(iii). The reason for this definition is that the thin film T does not behave as a rigid body but may bend like an elastic body. This insertion angle θ is preferably greater than 0°, more preferably greater than 0.1° and 60° or less, even more preferably 1° or more and 58° or less, even more preferably 2° or more and 55° or less, particularly preferably 3° or more and 50° or less, and most preferably 5° or more and 45° or less. By inserting the thin film T into the laminated sheet 10 at such an angle, the thin film T is inserted into the area of ​​the laminated sheet 10 where the adhesion force is weakest (typically the release layer 15 or its vicinity), and a gap G is efficiently formed. Furthermore, it is preferable to apply vertical stress to the delamination layer 15 or its vicinity when inserting the thin piece T (for example, by prying the area around the delamination layer 15 with the thin piece T), which allows for even more efficient formation of the gap G.

[0035] In forming the gap G, the insertion width of the thin piece T into the laminated sheet 10 is preferably 0.1 mm or more, more preferably 0.5 mm or more, and even more preferably 1 mm or more. In this specification, the insertion width means the distance from the cut S to the innermost part of the gap G (which can also be called the depth of the gap G). With such an insertion width, the peeling of the carrier 12 by the gap G can be further promoted. The upper limit of the insertion width can be appropriately determined according to the size of the laminated sheet 10 and is not particularly limited, but 20 mm can be given as a guideline for the upper limit.

[0036] If the laminated sheet 10 further comprises a resin-containing layer 20, the insertion of the thin piece T (e.g., a rotary blade RC) in forming the gap G may be performed against the resin-containing layer 20 (the central part C side, see Figure 4(ii)). Typically, the peel strength between the metal layer 16 and the resin-containing layer 20 is greater than the peel strength between the carrier 12 and the metal layer 16. Therefore, by inserting the thin piece T against the resin-containing layer 20, the metal layer 16 is lifted together with the resin-containing layer 20 and partially separated from the carrier 12, as shown in Figure 4(iii). As a result, a gap G can be formed between the metal layer 16 and the carrier 12.

[0037] From the viewpoint of gap G formation, the thickness of the thin section T is typically 2 mm or less, and more typically between 0.1 mm and 1 mm. Furthermore, the spring limit value Kb of the thin section T is measured by repeated deflection tests in accordance with JIS H3130-2012. 0.1 is 100 N / mm 2 More than 1500N / mm 2 Preferably, it is 200 N / mm 2 More than 1000N / mm 2 It is more preferable that it be less than 300 N / mm 2 More than 800N / mm 2 It is even more preferable that the following conditions are met. Furthermore, the static modulus of the thin sheet T, as measured in accordance with JIS R1602-1995, is preferably 30 GPa or more and 800 GPa or less, more preferably 80 GPa or more and 300 GPa or less, and even more preferably 100 GPa or more and 200 GPa or less. Using a thin sheet T with such rigidity makes it easier to form the gap G. The thin sheet T may be the same as or different from the cutting tool or machine tool used to form the cut as described above.

[0038] The thin flake T is preferably composed of at least one material from the group consisting of ferrous materials, non-ferrous metals, ceramics, and diamond, and more preferably tungsten or stainless steel. Preferred examples of ferrous materials include stainless steel, carbon tool steel (such as SK120 as specified in JIS G4401-2009), alloy tool steel (such as SKS7 as specified in JIS G4404-2015, which is carbon tool steel with small amounts of tungsten, chromium, vanadium, etc. added), and high-speed tool steel (such as SKH51 as specified in JIS G4403-2015, which is carbon tool steel with large amounts of tungsten, chromium, vanadium, molybdenum, etc. added). Preferred examples of non-ferrous metals include tungsten and cemented carbide (alloys made by sintering powder of hard metal carbides such as tungsten carbide). A preferred example of ceramics is zirconium oxide.

[0039] The thin slice T is preferably a cutting blade because it facilitates the formation of a gap G. The shape of this cutting blade may be a flat blade, a triangular blade, a square blade, a circular blade, or a rotary blade, but of these, a cutting blade with a circular or curved tip is more preferable, and a rotary blade is particularly preferable. By using a rotary blade (sometimes called a rotary cutter, slit cutter, or round knife), it becomes easier to insert the blade into the laminated sheet 10 at a constant insertion angle θ, and by inserting the blade into the laminated sheet 10 while rotating and pressing, a gap G can be smoothly formed, effectively suppressing damage to the resin-containing layer 20.

[0040] A schematic diagram of the rotating blade is shown in Figure 7. As shown in Figure 7, it is preferable from the viewpoint of gap formation ease for the rotating blade to have a diameter d, blade thickness t, and blade angle a within a predetermined range. Specifically, the diameter d of the rotating blade is preferably 5 mm to 150 mm, more preferably 10 mm to 100 mm, and even more preferably 18 mm to 60 mm. The blade thickness t of the rotating blade is preferably 0.1 mm to 5 mm, more preferably 0.2 mm to 3 mm, and even more preferably 0.3 mm to 1 mm. The blade angle a of the rotating blade is preferably 10° to 50°, more preferably 15° to 40°, and even more preferably 20° to 30°.

[0041] (4) Gap expansion (optional process) If desired, the gap G can be expanded by moving, for example, a thin section T along the cut S, starting from the formed gap G (Figure 2B(iv)). By expanding the gap G in this way, the carrier 12 can be peeled off even more smoothly.

[0042] The movement of the thin film T is preferably carried out along a part or the entire length of the cut S, and more preferably along the entire length of the cut S. For example, when the cut S is formed in the rectangular pattern (linear pattern on four sides) described above, gaps G can be formed on each side by moving the thin film T along the rectangular pattern. In particular, when the laminated sheet 10 has a polygonal shape, it is preferable to form gaps G including the corner portions (folded portions) of the cut S, from the viewpoint that the peeling process can be carried out smoothly by stress concentration in the gaps G in the subsequent peeling process. Furthermore, when the carrier is a single-crystal silicon carrier in this gap expansion process, it is preferable to pay attention to the direction of progression of the cut S.

[0043] The insertion angle of the thin slice T relative to the main surface of the carrier 12 during the movement of the thin slice T is not particularly limited, but it is typically within the range of θ±10° (where θ±10°>0°) when the insertion angle of the thin slice T is formed in the gap G. In addition, when moving the thin slice T, the gap G may be enlarged while tilting the thin slice T in the direction of movement.

[0044] (5) Carrier detachment (optional step) If desired, after expanding the gap G, a force is applied to the laminated sheet 10 in a direction that separates the carrier 12 and the metal layer 16 (on the central C side) (Figure 3(v)). In this way, the gap G can be used as a starting point to peel the metal layer 16 (and the resin-containing layer 20, if present) from the carrier 12 (Figure 3(vi)). In other words, as described above, the formation and expansion of the gap G creates a stress concentration point that serves as the starting point for peeling between the metal layer 16 and the carrier 12 in the peeling process, thus facilitating the peeling of the metal layer 16.

[0045] The peeling of the metal layer 16 is preferably performed while the outer edge of the carrier 12 or laminated sheet 10 is, for example, gripped or supported. Here, "support" includes a method of fixing at least a part of the carrier. For example, as shown in Figure 3(v), the metal layer 16 and resin-containing layer 20 can be peeled off by attaching the adhesive member AM to the metal layer 16 or resin-containing layer 20 (on the central part C side) while the carrier 12 is gripped or supported, and pulling in the direction away from the carrier 12 (in the direction of the arrow in the figure). Alternatively, the metal layer 16 may be peeled off by using wind pressure or water pressure by spraying wind or water at a predetermined pressure into the gap G while the carrier 12 is gripped or supported. Alternatively, as shown in Figures 8(i) and (ii), the metal layer 16 or resin-containing layer 20 may be peeled off by using a suction jig SJ or the like to suck the central part C side of the metal layer 16 or resin-containing layer 20, and then using a pressing member PM or the like to push the peripheral part P side of the metal layer 16 or resin-containing layer 20 in the direction opposite to the suction direction.

[0046] In this delamination process, if the carrier is a single-crystal silicon carrier, it is preferable to pay attention to the direction of delamination propagation. That is, as shown in Figures 9B(iii) and (iv), if delamination is performed in a direction in which the direction of propagation of the external stress ST coincides with the cleavage orientation CL, there is a possibility that the silicon carrier may be fractured, such as by the generation of a crack CR along the cleavage orientation CL, starting from the point where the external stress ST was applied due to the initial delamination. To suppress such fracture due to cleavage of the silicon carrier, when the carrier 12 is a single-crystal silicon carrier, it is preferable to apply the external stress ST to delaminate the carrier 12 in such a way that it does not coincide with either the x-axis (left-right direction in the figure) or y-axis (up-down direction in the figure) cleavage orientation CL on the silicon carrier, as shown in Figures 10B(iii) and (iv).

[0047] Therefore, according to a preferred embodiment of the present invention, the carrier 12 is a single-crystal silicon carrier having a notch or the like on its outer circumference, and in the carrier peeling step, when the angle θ is defined clockwise starting from a half-line from the center of the single-crystal silicon carrier to the notch or the like, the peeling is performed such that the direction of external stress propagation is within the range of 1° < θ < 89°.

[0048] Let's explain in more detail. As shown in Figures 9A(i) and 10(i), if we define the angle θ clockwise starting from the half-line L from the center of the carrier 12 to the midpoint of the notch N or orientation flat OF, then θ = 0°, 90°, 180°, and 270° correspond to the cleavage orientation CL. Therefore, regarding the direction of propagation θr of the external stress ST due to delamination, as shown in Figure 10B(iii), it is preferable to perform delamination while maintaining the direction of propagation of the external stress ST so that θr is within the range of 1° < θr < 89°, and more preferably within the range of 5° < θr < 85°. By using a delamination method that satisfies such a range of θr, it is possible to suppress the fracture of the carrier 12 made of silicon wafer. Particularly preferred ranges of θr during this delamination are θr = 45±5°, 135±5°, 225±5°, and 315±5° clockwise starting from the half-line L. These angles correspond to the crystal orientation of the silicon wafer. <100> Since the wafer is least likely to cleave in this direction, propagating external stress at these angles makes it possible to remove carriers while effectively suppressing wafer fracture. When carrier delamination is performed by attaching an adhesive member AM to the metal layer 16 or resin-containing layer 20 and pulling it in the direction away from the carrier 12 (see Figure 3(v)), it is preferable to keep the propagation direction of the tensile stress by the adhesive member AM within the range of θr. Alternatively, when carrier delamination is performed by using a pressing member PM or the like to push the peripheral edge P side of the metal layer 16 or resin-containing layer 20 in the direction opposite to the suction direction (see Figures 8(i) and (ii)), it is preferable to keep the propagation direction of the stress in the pushing direction by the pressing member PM or the like within the range of θr.

[0049] If the laminated sheet 10 has a resin-containing layer 20, the exposed metal layer 16 after peeling off the carrier 12 may be removed by etching. This exposes the wiring (embedded wiring) formed on the surface of the metal layer 16, making it more suitable for forming further circuits on it using a photolithography process. The etching of the metal layer 16 can be carried out using known methods and is not particularly limited.

[0050] Metal foil with carrier As described above with reference to Figure 1A, the carrier-attached metal foil 18 optionally used in the method of the present invention comprises, in order, a carrier 12, optionally an intermediate layer 14, a release layer 15, and a metal layer 16.

[0051] As described above, the material of the carrier 12 may be glass, ceramics, silicon, resin, or metal. Preferably, the carrier 12 is composed of glass, polycrystalline silicon, monocrystalline silicon, or ceramics. The form of the carrier 12 may be a sheet, film, or plate. Alternatively, the carrier 12 may be a laminate of these sheets, films, plates, etc. For example, the carrier 12 may function as a rigid support such as a glass plate, ceramic plate, silicon wafer, or metal plate, or it may be in a form that does not have rigidity, such as a metal foil or resin film. Preferred examples of metals that constitute the carrier 12 include copper, titanium, nickel, stainless steel, and aluminum. Preferred examples of ceramics include alumina, zirconia, silicon nitride, aluminum nitride, and various other fine ceramics. Preferred resins include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyamide, polyimide, nylon, liquid crystal polymer, polyether ether ketone (PEEK®), polyamide imide, polyether sulfone, polyphenylene sulfide, polytetrafluoroethylene (PTFE), and ethylene tetrafluoroethylene (ETFE). More preferably, from the viewpoint of preventing warping of the coreless support due to heating when mounting semiconductor elements, the material has a coefficient of thermal expansion (CTE) of less than 25 ppm / K (typically 1.0 ppm / K to 23 ppm / K). Examples of such materials include the various resins mentioned above (especially low thermal expansion resins such as polyimide and liquid crystal polymer), glass, silicon, and ceramics. Furthermore, from the viewpoint of handling and ensuring flatness during chip mounting, the carrier 12 preferably has a Vickers hardness of 100 HV or more, and more preferably 150 HV to 2500 HV. As a material that satisfies these characteristics, the carrier 12 is preferably composed of glass, silicon, or ceramics, more preferably of glass or ceramics, and particularly preferably of glass. An example of a carrier 12 made of glass is a glass plate.When glass is used as the carrier 12, it has advantages such as being lightweight, having a low coefficient of thermal expansion, high insulating properties, and being rigid and having a flat surface, which allows for an extremely smooth surface on the metal layer 16. Furthermore, when the carrier 12 is glass, it has advantages such as having surface flatness (coplanarity) that is advantageous for forming fine circuits, having chemical resistance in desmear and various plating processes in the wiring manufacturing process, and being able to employ a chemical separation method when peeling the carrier 12 from the carrier-attached metal foil 18. Preferred examples of glass constituting the carrier 12 include quartz glass, borosilicate glass, alkali-free glass, soda-lime glass, aluminosilicate glass, and combinations thereof, more preferably alkali-free glass, soda-lime glass, and combinations thereof, and particularly preferably alkali-free glass. Alkali-free glass is a glass that is substantially free of alkali metals, with silicon dioxide, aluminum oxide, boron oxide, and alkaline earth metal oxides such as calcium oxide and barium oxide as its main components, and further containing boric acid. This alkali-free glass has the advantage of minimizing glass warping during heating processes because its thermal expansion coefficient is low and stable in the range of 3 ppm / K to 5 ppm / K over a wide temperature range from 0°C to 350°C. The thickness of the carrier 12 is preferably 100 μm to 2000 μm, more preferably 300 μm to 1800 μm, and even more preferably 400 μm to 1100 μm. When the carrier 12 has a thickness within this range, it is possible to achieve thinner wiring and reduced warping that occurs when mounting electronic components while ensuring appropriate strength that does not hinder handling.

[0052] The optional intermediate layer 14 may consist of one layer or two or more layers. If the intermediate layer 14 consists of two or more layers, it includes a first intermediate layer provided directly above the carrier 12 and a second intermediate layer provided adjacent to the release layer 15. The first intermediate layer is preferably composed of at least one metal selected from the group consisting of Ti, Cr, Al, and Ni, in order to ensure adhesion with the carrier 12. The first intermediate layer may be a pure metal or an alloy. The thickness of the first intermediate layer is preferably 5 nm to 500 nm, more preferably 10 nm to 300 nm, even more preferably 18 nm to 200 nm, and particularly preferably 20 nm to 100 nm. The second intermediate layer is preferably composed of Cu, in order to control the peel strength with respect to the release layer 15 to a desired value. The thickness of the second intermediate layer is preferably 5 nm to 500 nm, more preferably 10 nm to 400 nm, even more preferably 15 nm to 300 nm, and particularly preferably 20 nm to 200 nm. Another intervening layer may exist between the first intermediate layer and the second intermediate layer. Examples of materials for the intervening layer include alloys of Cu with at least one metal selected from the group consisting of Ti, Cr, Mo, Mn, W, and Ni. On the other hand, if the intermediate layer 14 is a single layer, the first intermediate layer described above may be used as the intermediate layer as is, or the first and second intermediate layers may be replaced with a single intermediate alloy layer. This intermediate alloy layer is preferably composed of a copper alloy having a content of 1.0 at% or more of at least one metal selected from the group consisting of Ti, Cr, Mo, Mn, W, Al, and Ni, and a Cu content of 30 at% or more. The thickness of the intermediate alloy layer is preferably 5 nm to 500 nm, more preferably 10 nm to 400 nm, even more preferably 15 nm to 300 nm, and particularly preferably 20 nm to 200 nm. The thickness of each layer described above is measured by analyzing the cross-section of the layer with an energy-dispersive X-ray spectrometer (TEM-EDX) on a transmission electron microscope. The metal constituting the intermediate layer 14 may contain unavoidable impurities resulting from the raw material components or the film formation process.Furthermore, if the intermediate layer 14 is exposed to the atmosphere after film formation, the presence of oxygen introduced as a result is acceptable. The intermediate layer 14 may be manufactured by any method, but it is particularly preferable that it be formed by magnetron sputtering using a metal target, as this ensures uniformity of the film thickness distribution.

[0053] The release layer 15 is a layer that enables or facilitates the release of the carrier 12 and, if present, the intermediate layer 14. The release layer 15 may be removable by applying physical force, or it may be removable by a laser (laser lift-off, LLO). If the release layer 15 is made of a material that can be removed by laser lift-off, the release layer 15 may be made of a resin whose interfacial adhesion strength decreases upon laser irradiation after curing, or it may be a layer of silicon, silicon carbide, metal oxide, etc. that is modified by laser irradiation. Furthermore, the release layer 15 may be either an organic release layer or an inorganic release layer. Examples of organic components used in the organic release layer include nitrogen-containing organic compounds, sulfur-containing organic compounds, carboxylic acids, etc. Examples of nitrogen-containing organic compounds include triazole compounds, imidazole compounds, etc. On the other hand, examples of inorganic components used in the inorganic release layer include metal oxides or metal oxynitrides containing at least one of Cu, Ti, Al, Nb, Zr, Cr, W, Ta, Co, Ag, Ni, In, Sn, Zn, Ga, Mo, or carbon. Among these, the release layer 15 is preferably a layer mainly composed of carbon from the viewpoint of ease of release and layer formation, more preferably a layer mainly composed of carbon or hydrocarbons, and even more preferably a layer made of amorphous carbon, which is a hard carbon film. In this case, the carbon concentration of the release layer 15 (i.e., the carbon-containing layer) as measured by XPS is preferably 60 atomic% or more, more preferably 70 atomic% or more, even more preferably 80 atomic% or more, and particularly preferably 85 atomic% or more. The upper limit of the carbon concentration is not particularly limited and may be 100 atomic%, but 98 atomic% or less is more practical. The release layer 15 may contain unavoidable impurities (e.g., oxygen, carbon, hydrogen, etc. originating from the surrounding environment such as the atmosphere). Furthermore, due to the film formation method used for the metal layer 16 and other layers that are later laminated, metal atoms of types other than the metal contained in the release layer 15 may be mixed into the release layer 15.When a carbon-containing layer is used as the release layer 15, the interdiffusion and reactivity with carriers are low, and even when subjected to press working at temperatures exceeding 300°C, interdiffusion of metal elements due to high-temperature heating between the metal layer and the bonding interface can be prevented, maintaining a state where carrier peeling and removal is easy. It is preferable that the release layer 15 is formed by a vapor phase method such as sputtering, in terms of suppressing excessive impurities in the release layer 15 and ensuring the continuous productivity of other layers. When a carbon-containing layer is used as the release layer 15, the thickness is preferably 1 nm to 20 nm, and more preferably 1 nm to 10 nm. This thickness is measured by analyzing the cross-section of the layer with an energy-dispersive X-ray spectrometer (TEM-EDX) on a transmission electron microscope.

[0054] The release layer 15 may include a metal oxide layer and a carbon-containing layer, or it may be a layer containing both metal oxide and carbon. In particular, when the carrier-attached metal foil 18 includes an intermediate layer 14, the carbon-containing layer contributes to the stable release of the carrier 12, and the metal oxide layer more effectively suppresses the diffusion of metal elements originating from the intermediate layer 14 and the metal layer 16 during heating. As a result, stable release properties can be maintained even after heating at high temperatures, such as 350°C or higher. The metal oxide layer is preferably a layer containing an oxide of a metal composed of Cu, Ti, Al, Nb, Zr, Cr, W, Ta, Co, Ag, Ni, In, Sn, Zn, Ga, Mo, and combinations thereof. The metal oxide layer is preferably formed by a reactive sputtering method using a metal target and sputtering in an oxidizing atmosphere, as the film thickness can be easily controlled by adjusting the film formation time. The thickness of the metal oxide layer is preferably 0.1 nm to 100 nm. The upper limit of the thickness of the metal oxide layer is more preferably 60 nm or less, even more preferably 30 nm or less, and particularly preferably 10 nm or less. This thickness is measured by analyzing the cross-section of the layer with an energy-dispersive X-ray spectrometer (TEM-EDX) on a transmission electron microscope. In this case, the order in which the metal oxide layer and the carbon layer are stacked as the release layer 15 is not particularly limited. Furthermore, the release layer 15 may exist in a multiphase state (i.e., a layer containing both metal oxide and carbon) where the boundary between the metal oxide layer and the carbon-containing layer is not clearly defined.

[0055] Similarly, from the viewpoint of maintaining stable release properties even after heat treatment at high temperatures, the release layer 15 may be a metal-containing layer whose surface adjacent to the metal layer 16 is a fluorinated surface and / or a nitrided surface. Preferably, the metal-containing layer has a region (hereinafter referred to as the "(F+N) region") over a thickness of 10 nm or more in which the sum of the fluorine content and nitrogen content is 1.0 atomic% or more, and the (F+N) region is preferably located on the metal layer 16 side of the metal-containing layer. The thickness of the (F+N) region (in terms of SiO2) is determined by performing depth-direction elemental analysis of the carrier-attached metal foil 18 using XPS. The fluorinated surface or nitrided surface can preferably be formed by reactive ion etching (RIE) or reactive sputtering. On the other hand, it is preferable that the metal elements contained in the metal-containing layer have a negative standard electrode potential. Preferred examples of metal elements included in the metal-containing layer include Cu, Ag, Sn, Zn, Ti, Al, Nb, Zr, W, Ta, Mo, and combinations thereof (e.g., alloys and intermetallic compounds). The metal element content in the metal-containing layer is preferably 50 atomic% to 100 atomic%. The metal-containing layer may be a single layer or a multilayer composed of two or more layers. The overall thickness of the metal-containing layer is preferably 10 nm to 1000 nm, more preferably 30 nm to 500 nm, even more preferably 50 nm to 400 nm, and particularly preferably 100 nm to 300 nm. The thickness of the metal-containing layer itself is measured by analyzing the cross-section of the layer with an energy-dispersive X-ray spectrometer (TEM-EDX) on a transmission electron microscope.

[0056] Alternatively, the release layer 15 may be a metal oxynitride-containing layer instead of a carbon layer or the like. The surface of the metal oxynitride-containing layer opposite to the carrier 12 (i.e., the metal layer 16 side) preferably contains at least one metal oxynitride selected from the group consisting of TaON, NiON, TiON, NiWON, and MoON. Furthermore, in order to ensure adhesion between the carrier 12 and the metal layer 16, the surface of the metal oxynitride-containing layer on the carrier 12 side preferably contains at least one selected from the group consisting of Cu, Ti, Ta, Cr, Ni, Al, Mo, Zn, W, TiN, and TaN. This suppresses the number of foreign particles on the surface of the metal layer 16, improves circuit formation, and makes it possible to maintain stable release strength even after heating at high temperatures for a long time. The thickness of the metal oxynitride-containing layer is preferably 5 nm to 500 nm, more preferably 10 nm to 400 nm, even more preferably 20 nm to 200 nm, and particularly preferably 30 nm to 100 nm. This thickness is determined by analyzing the layer cross-section using an energy-dispersive X-ray spectrometer (TEM-EDX) on a transmission electron microscope.

[0057] The metal layer 16 is a layer made of metal. The metal layer 16 may be a single layer or a layer of two or more. When the metal layer 16 is made up of two or more layers, the metal layer 16 can be configured such that each metal layer from the first metal layer to the mth metal layer (where m is an integer of 2 or more) is sequentially stacked on the side of the release layer 15 opposite to the carrier 12. The total thickness of the metal layer 16 is preferably 1 nm to 2000 nm, more preferably 100 nm to 1500 nm, more preferably 200 nm to 1000 nm, even more preferably 300 nm to 800 nm, and particularly preferably 350 nm to 500 nm. The thickness of the metal layer 16 is measured by analyzing the cross-section of the layer with an energy-dispersive X-ray spectrometer (TEM-EDX) on a transmission electron microscope. Below, an example in which the metal layer 16 is made up of two layers, a first metal layer and a second metal layer, will be described.

[0058] The first metal layer preferably provides the carrier-attached metal foil 18 with desired functions such as etching stopper function and anti-reflective function. Preferred examples of metals constituting the first metal layer include Ti, Al, Nb, Zr, Cr, W, Ta, Co, Ag, Ni, Mo and combinations thereof, more preferably Ti, Zr, Al, Cr, W, Ni, Mo and combinations thereof, even more preferably Ti, Al, Cr, Ni, Mo and combinations thereof, and particularly preferably Ti, Mo and combinations thereof. These elements have the property of not dissolving in flash etching solutions (e.g., copper flash etching solutions), and as a result, they can exhibit excellent chemical resistance to flash etching solutions. Therefore, the first metal layer is less susceptible to etching by flash etching solutions than the second metal layer described later, and thus can function as an etching stopper layer. Furthermore, since the above-mentioned metals constituting the first metal layer also have the function of preventing light reflection, the first metal layer can also function as an anti-reflective layer to improve visibility in image inspection (e.g., automated image inspection (AOI)). The first metal layer may be a pure metal or an alloy. The metal constituting the first metal layer may contain unavoidable impurities resulting from the raw material components or the film formation process. Furthermore, there is no particular upper limit to the metal content, and it may be 100 atomic percent. The first metal layer is preferably formed by physical vapor deposition (PVD), and more preferably by sputtering. The thickness of the first metal layer is preferably 1 nm to 500 nm, more preferably 10 nm to 400 nm, even more preferably 30 nm to 300 nm, and particularly preferably 50 nm to 200 nm.

[0059] Preferred examples of metals constituting the second metal layer include transition elements of Groups 4, 5, 6, 9, 10, and 11, Al, and combinations thereof (e.g., alloys and intermetallic compounds). More preferably, transition elements of Groups 4 and 11, Al, Nb, Co, Ni, Mo, and combinations thereof. Even more preferably, transition elements of Group 11, Ti, Al, Mo, and combinations thereof. Particularly preferred are Cu, Ti, Mo, and combinations thereof. Most preferably, Cu. The second metal layer may be manufactured by any method, for example, a metal foil formed by wet deposition methods such as electroless metal plating and electrolytic metal plating, physical vapor deposition (PVD) methods such as sputtering and vacuum deposition, chemical vapor deposition, or a combination thereof. A particularly preferred second metal layer is a metal layer formed by physical vapor deposition (PVD) methods such as sputtering or vacuum deposition, from the viewpoint of easily accommodating fine pitch reduction through ultrathinning, and most preferably, a metal layer manufactured by sputtering. Furthermore, while it is preferable that the second metal layer is a metal layer that has not undergone roughening treatment, it may also be a metal layer that has undergone secondary roughening treatment by preliminary roughening treatment, soft etching treatment, cleaning treatment, or oxidation-reduction treatment, as long as it does not interfere with the formation of the wiring pattern. From the viewpoint of supporting fine pitch, the thickness of the second metal layer is preferably 10 nm to 1000 nm, more preferably 20 nm to 900 nm, even more preferably 30 nm to 700 nm, even more preferably 50 nm to 600 nm, particularly preferably 70 nm to 500 nm, and most preferably 100 nm to 400 nm. Metal layers with thicknesses within this range are preferably manufactured by sputtering in terms of in-plane uniformity of film thickness and productivity in sheet or roll form.

[0060] When the metal layer 16 has a single-layer structure, it is preferable to use the second metal layer described above as the metal layer 16. On the other hand, when the metal layer 16 has an n-layer structure (where n is an integer of 3 or more), it is preferable to have the first metal layer to the (n-1)th metal layer of the metal layer 16 have the configuration of the first metal layer described above, and the outermost layer of the metal layer 16, i.e., the nth metal layer, have the configuration of the second metal layer described above.

[0061] It is preferable that the metal layer 16, optionally an intermediate layer 14, and optionally a release layer 15 (i.e., at least the metal layer 16, for example, the metal layer 16 and the intermediate layer 14) extend to the end face of the carrier 12 so that the end face is covered. In other words, it is preferable that not only the surface of the carrier 12 but also the end face is covered with at least the metal layer 16. By covering the end face as well, it is possible to prevent chemical solutions from penetrating the carrier 12 during the manufacturing process of the wiring board, and it is also possible to firmly prevent chipping due to peeling at the side edges when handling the carrier-attached metal foil 18 or laminated sheet 10, i.e., chipping of the film on the release layer 15 (i.e., the metal layer 16). The covered area on the end face of the carrier 12 is preferably an area of ​​0.1 mm or more, more preferably an area of ​​0.2 mm or more, and even more preferably extends over the entire end face of the carrier 12 in the thickness direction (i.e., the direction perpendicular to the carrier surface) from the surface of the carrier 12. [Examples]

[0062] The present invention will be further described in detail by the following examples.

[0063] Example 1 (1) Preparation of laminated sheets A glass substrate (material: soda-lime glass) measuring 320 mm x 320 mm with a thickness of 1.1 mm was prepared as carrier 12. On this carrier 12, a titanium layer (thickness 50 nm) and a copper layer (thickness 200 nm) as an intermediate layer 14, an amorphous carbon layer (thickness 6 nm) as a release layer 15, and a titanium layer (thickness 100 nm) and a copper layer (thickness 300 nm) as a metal layer 16 were deposited in this order by sputtering to obtain a carrier-attached metal foil 18. On the metal layer 16 of this carrier-attached metal foil 18, a resin layer (material: epoxy resin) measuring 300 mm x 300 mm with a thickness of 300 μm was formed to form a resin-containing layer 20. In this way, a laminated sheet 10 was fabricated with carrier 12, intermediate layer 14, release layer 15, metal layer 16, and resin-containing layer 20 in this order (see Figures 1A(i) and 1B(i)).

[0064] (2) Formation of cuts A notch S (width 0.5 mm) was formed by inserting the blade (material: tungsten) of a cutter CT perpendicular to the main surface of the carrier 12 from the surface of the metal layer 16 of the laminated sheet 10. When the laminated sheet 10 is viewed from above, this notch S forms a rectangular pattern (linear pattern on four sides) surrounding the resin-containing layer 20 (see Figure 1B(ii)). Furthermore, when the laminated sheet 10 is viewed in cross-section, this notch S penetrates the metal layer 16, the release layer 15, and the intermediate layer 14, but does not penetrate the carrier 12 (see Figure 1A(ii)). In this way, the metal layer 16, the release layer 15, and the intermediate layer 14 are divided into a central part C and a peripheral part P with the notch S as the boundary.

[0065] (3) Formation of gaps A rotary blade RC (diameter 45 mm, blade thickness 0.3 mm, blade angle 21°, material: tungsten) was inserted from the corner of the cut S toward the center of the metal layer 16, the release layer 15, and the intermediate layer 14 (see Figures 2A(iii) and 2B(iii)). At this time, the insertion angle θ of the rotary blade RC with respect to the main surface of the carrier 12 when the laminated sheet 10 is viewed in cross-section was set to 45°. The insertion width of the rotary blade RC into the laminated sheet 10 was set to 2 mm. In this way, a gap G was formed between the metal layer 16 and the carrier 12.

[0066] (4) Widening of the gap Starting from the gap G that was formed, the rotary blade RC was moved along the cut S (see Figures 2A(iv) and 2B(iv)). By moving the rotary blade RC along the rectangular pattern of the cut S in this way, the gap G was enlarged on each side.

[0067] (5) Carrier detachment With the peripheral edge P of the laminated sheet 10 supported, a commercially available adhesive tape AT was attached to the corner of the resin-containing layer 20, and by pulling it up in a direction away from the carrier 12, the resin-containing layer 20 and the metal layer 16 were peeled off from the carrier 12 (see Figures 3(v) and (vi)).

Claims

1. A method for manufacturing a wiring board, A process of preparing a laminated sheet having a release layer and a metal layer arranged in order on a carrier, A step of making an incision from the side of the laminated sheet opposite to the carrier such that when the laminated sheet is viewed in plan, the incision passes inside the outer edge of the laminated sheet, and when the laminated sheet is viewed in cross-section, the incision penetrates the metal layer and the release layer, thereby dividing the metal layer and the release layer into a central part and a peripheral part with the incision as the boundary, The steps include inserting a thin slice from the aforementioned cut toward the central part to form a gap between the metal layer and the carrier, A method for manufacturing a wiring board, including the method described above.

2. A method for manufacturing a wiring board, A process of preparing a laminated sheet having a release layer and a metal layer arranged in order on a carrier, A step of making an incision from the side of the laminated sheet opposite to the carrier such that when the laminated sheet is viewed in plan, the incision passes inside the outer edge of the laminated sheet, and when the laminated sheet is viewed in cross-section, the incision penetrates the metal layer and the release layer, thereby dividing the metal layer and the release layer into a central part and a peripheral part with the incision as the boundary, The steps include inserting a thin slice from the aforementioned cut toward the central part to form a gap between the metal layer and the carrier, Includes, A method for manufacturing a wiring board, wherein the carrier is a single-crystal silicon carrier having a notch or orientation flat on its outer circumference, and in the process of forming the cut, the cut is made such that when an angle θ is defined clockwise starting from a half-line from the center of the single-crystal silicon carrier to the midpoint of the notch or orientation flat, the direction of external stress propagation is within the range of 1° < θ < 89°.

3. A method for manufacturing a wiring board according to claim 1 or 2, further comprising the step of expanding the gap starting from the gap that has been formed.

4. The method for manufacturing a wiring board according to claim 3, further comprising the step of, after widening the gap, applying force to the laminated sheet in a direction that separates the carrier and the metal layer, thereby peeling the metal layer from the carrier using the gap as a starting point.

5. The method for manufacturing a wiring board according to claim 1 or 2, wherein the notch is formed so that at least a portion of the carrier does not penetrate when the laminated sheet is viewed in cross-section.

6. The method for manufacturing a wiring board according to claim 1 or 2, wherein the width of the cut is 0.01 mm or more and 20 mm or less.

7. The method for manufacturing a wiring board according to claim 1 or 2, wherein the notches are formed in a linear pattern such that, when the laminated sheet is viewed in plan view, the peripheral portion surrounds the central portion.

8. The method for manufacturing a wiring board according to claim 4, wherein the peeling off of the metal layer is performed while gripping or supporting the outer edge of the carrier or the laminated sheet.

9. The method for manufacturing a wiring board according to claim 1 or 2, wherein the laminated sheet further comprises a resin-containing layer on the side of the metal layer opposite to the release layer.

10. The method for manufacturing a wiring substrate according to claim 9, wherein the resin-containing layer includes at least one selected from the group consisting of a wiring layer, a semiconductor element, and a resin layer.

11. The method for manufacturing a wiring board according to claim 9, wherein the thickness of the resin-containing layer is 1,000 μm or less.

Citation Information

Patent Citations

  • Thin film forming device and forming method for thin film

    JP1990125440A

  • Semiconductor device and method for manufacturing the same

    JP2002164479A

  • Substrate for supporting circuit formation, and substrate for packaging semiconductor element and its manufacturing method

    JP2005101137A

  • Electroconductive ink composition

    JP2009062523A

  • Protective tape separation method and apparatus using the same

    JP2009094132A