Method and system for precipitating solid carbon
The method and system optimize the composition ratios in a three-step process to enhance solid carbon recovery and minimize methane generation, addressing inefficiencies in existing carbon dioxide fixation technologies.
Patent Information
- Application Number
- JP2023057631
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing carbon dioxide fixation technologies do not adequately consider the composition ratio of the raw material gas, leading to inefficient recovery of solid carbon and excessive generation of methane as a by-product.
A method and system involving a three-step process: first, a methanation reaction to convert carbon dioxide and hydrogen into methane, followed by a dry reforming reaction to convert methane into carbon monoxide, and finally a solid carbon precipitation reaction to produce solid carbon, with controlled molar ratios and concentrations to optimize the process.
Improves the recovery rate of solid carbon and reduces the generation of methane and unreacted methane, achieving efficient and cost-effective carbon dioxide conversion.
Smart Images

Figure 0007954614000003 
Figure 0007954614000004 
Figure 0007954614000005
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a solid carbon deposition method and a solid carbon deposition system. BACKGROUND ART
[0002] At present, the reduction and fixation of carbon dioxide, which exerts adverse environmental effects as a greenhouse gas, is an urgent global task. In response, various technologies including CO2 emission reduction technologies, CO2 separation and recovery technologies, CO2 conversion to useful resources technologies, and CO2 fixation technologies are being researched and developed toward practical implementation in various fields.
[0003] As a method for effectively utilizing carbon dioxide, for example, it is known that methane can be synthesized via a methanation reaction by flowing a mixed gas of carbon dioxide and hydrogen in the presence of a catalyst heated to 250 to 500°C (see Patent Document 1). Technologies for depositing solid carbon by subjecting methane to high-temperature pyrolysis are also known (see Patent Documents 2 to 5).
[0004] Patent Document 2 discloses a continuous carbon removal system in which a first reactor that causes a methanation reaction without using a catalyst and a second reactor that decomposes methane under a temperature condition of 1200°C or higher are connected in series.
[0005] Patent Document 3 discloses a carbon dioxide fixation method comprising a first reaction step of reacting carbon dioxide and hydrogen in the presence of a catalyst to generate a mixed gas containing methane and water, and a second reaction step of using the methane gas obtained in the first reaction step as a raw material to produce at least one carbon product selected from the group consisting of carbon, graphite, carbon nanotubes and diamond.
[0006] Patent Document 4 discloses a carbon dioxide fixation system that includes a methanation reactor that brings a raw material gas containing carbon dioxide and hydrogen into contact with a catalyst that activates a methanation reaction to produce methane and hydrogen from the raw material gas, and a methane pyrolysis reactor that heats the methane produced in the methanation reactor to decompose the methane into solid carbon and hydrogen.
[0007] Patent Document 5 discloses a technique in which a mixed gas of carbon dioxide and methane in a ratio of 7:3 is flowed into a pre-reaction vessel filled with a 30 wt% Ni / SiO2 catalyst, and reacted in a heating furnace at a reaction temperature of 550°C for a certain period of time to convert it into a mixed gas of carbon dioxide, methane, hydrogen, and carbon monoxide. Subsequently, this mixture is flowed into a main reaction vessel filled with a 50 wt% Fe / SiO2 catalyst, which is mainly composed of iron, and carbon is precipitated by a catalytic reduction reaction of carbon dioxide with hydrogen in a heating furnace at a low temperature of 400°C. [Prior art documents] [Patent Documents]
[0008] [Patent Document 1] Japanese Patent Publication No. 2019-172595 [Patent Document 2] Japanese Patent Application Publication No. 8-133200 [Patent Document 3] Japanese Patent Publication No. 2005-60137 [Patent Document 4] Japanese Patent Publication No. 2015-196619 [Patent Document 5] Japanese Patent Publication No. 2003-48708 [Overview of the Initiative] [Problems that the invention aims to solve]
[0009] Incidentally, the above-mentioned Patent Documents 2-4 do not describe the composition ratio of the raw material gas supplied to the reactor that produces the methanation reaction. Furthermore, while Patent Document 5 discloses the composition ratio of the raw material gas, it only states that the ratio of carbon dioxide to methane is 7:3. Therefore, the composition ratio of the raw material gas has not been sufficiently considered, and there is still room for improvement.
[0010] This invention has been made in view of these circumstances, and aims to provide a method and system for precipitation of solid carbon that improve the recovery rate of solid carbon precipitated from raw material gas in CO2 fixation, and suppress the generation of methane as a by-product associated with the solid carbon precipitation reaction and the residue of unreacted methane. [Means for solving the problem]
[0011] (1) To achieve the above objective, the present invention provides a method for precipitating solid carbon, comprising: a first step of contacting a raw material gas containing carbon dioxide and hydrogen with a catalyst that activates a methanation reaction to produce methane and water from the raw material gas; a second step of heating the produced methane in contact with a catalyst that activates a dry reforming reaction to convert the produced methane into carbon monoxide; and a third step of contacting the converted carbon monoxide with a catalyst that activates a solid carbon precipitation reaction to precipitate solid carbon from the converted carbon monoxide, wherein the CO2 / CH4 molar ratio in the gas produced in the first step is 0.9 or more and 2.1 or less, the carbon monoxide concentration in the gas produced in the second step is 30 vol% or more, and the CO / (CH4+CO2+CO) molar ratio is 0.80 or more.
[0012] (2) The present invention also relates to a solid carbon deposition system for precipitating solid carbon from a raw material gas containing carbon dioxide and hydrogen, comprising: a first reactor that brings the raw material gas into contact with a catalyst that activates a methanation reaction to produce methane and water from the raw material gas; a second reactor that converts the produced methane into carbon monoxide by heating it in contact with a catalyst that activates a dry reforming reaction; and a second reactor that brings the converted carbon monoxide into contact with a catalyst that activates a solid carbon deposition reaction to produce solid carbon from the carbon monoxide. The system includes a third reactor for precipitating elements, a first exhaust gas measuring device for measuring the composition of the gas discharged from the first reactor, a second exhaust gas measuring device for measuring the composition of the gas discharged from the second reactor, and a control unit that controls the composition ratio of the gases discharged from each reactor based on the measurement results of each exhaust gas measuring device, wherein the control unit controls the CO2 / CH4 molar ratio in the gas discharged from the first reactor and the carbon monoxide concentration and CO / (CH4+CO2+CO) molar ratio in the gas discharged from the second reactor to be within a specified range. [Effects of the Invention]
[0013] According to the present invention, it is possible to improve the recovery rate of solid carbon precipitated from the raw material gas during CO2 fixation, and to suppress the generation of methane, a by-product of the solid carbon precipitation reaction, as well as the residue of unreacted methane. [Brief explanation of the drawing]
[0014] [Figure 1] This is a schematic diagram showing the configuration of the solid carbon deposition apparatus according to the present invention. [Figure 2] This is a schematic diagram showing the configuration of the solid carbon deposition system according to the present invention. [Figure 3] This is a schematic diagram showing a spiral-shaped catalyst. [Modes for carrying out the invention]
[0015] [principle] As reactions for precipitating solid carbon from each of carbon dioxide, methane, and carbon monoxide, the following reaction equations are conceivable. CO2→C+O2 ΔH=395kJ / mol...(Equation 1) CH4→C+2H2 ΔH=75kJ / mol...(Equation 2) 2CO→C+CO2 ΔH=-172kJ / mol...(Equation 3) CO+H2→C+2H2O ΔH=-131kJ / mol...(Equation 4) CO2+2H2→C+H2O ΔH=-90kJ / mol...(Equation 5)
[0016] As shown in Equation 1, the Gibbs free energy of the direct decomposition reaction of carbon dioxide is 395 kJ / mol, which requires a large amount of energy. In contrast, as shown in Equation 2, it is possible to precipitate solid carbon by thermally decomposing methane at a high temperature. At this time, carbon dioxide is converted to methane, and the methane is thermally decomposed. However, for Equation 2 as well, the Gibbs free energy is 75 kJ / mol, and since it is an endothermic reaction, a large amount of energy is required. In Equation 1 and Equation 2, when energy is supplied from the outside as thermal energy, a high temperature of 1000°C or higher is required, which incurs significant costs.
[0017] In contrast, when precipitating solid carbon from carbon monoxide, the reaction is exothermic with -172 kJ / mol in Equation 3 and -131 kJ / mol in Equation 4. Therefore, there is no need to supply a large amount of energy to the reactor, making it possible to precipitate solid carbon at reduced cost. In addition, since Equation 5 is an exothermic reaction of -90 kJ / mol, solid carbon can be similarly precipitated at reduced cost even when solid carbon is precipitated from carbon dioxide and hydrogen.
[0018] Therefore, it is considered that carbon dioxide can be converted to solid carbon at low cost by converting carbon dioxide to carbon monoxide and then precipitating solid carbon, or by precipitating solid carbon from carbon dioxide and hydrogen.
[0019] Based on the above, the present invention precipitates solid carbon from a raw material gas containing carbon dioxide and hydrogen by the following reaction equation. First reaction: CO2 + 4H2 → CH4 + 2H2O ΔH = -165 kJ / mol…(Equation 6) Second reaction: CO2+CH4→2CO+2H2ΔH=248kJ / mol…(Equation 7) Third reaction: 2CO → C + CO2 ΔH = -172 kJ / mol…(Equation 8)
[0020] As described above, in this invention, a methanation reaction is first carried out to convert carbon dioxide and hydrogen into methane, as shown in Equation 6. Next, a dry reforming reaction is carried out to convert carbon dioxide and methane into carbon monoxide, as shown in Equation 7. Then, solid carbon is precipitated from carbon monoxide by a solid carbon precipitation reaction including a boudoir reaction, as shown in Equation 8. By combining the dry reforming reaction and the solid carbon precipitation reaction, the reaction can proceed at a relatively low temperature, and the energy required to precipitate solid carbon from carbon dioxide can be kept low.
[0021] Next, we will explain the changes in the raw material gas when a raw material gas consisting of carbon dioxide and hydrogen is reacted continuously from the first to the third reaction.
[0022] In the first reaction, methane and water vapor are typically produced from 1 mole of carbon dioxide and 4 moles of hydrogen via a catalyst. Even if the molar ratio of H2 / CO2 is the theoretical value of 4, not all of the carbon dioxide and hydrogen react to produce 1 mole of methane. In other words, the raw material gas containing carbon dioxide and hydrogen becomes a mixed gas consisting of methane synthesized in the first reaction, unreacted carbon dioxide, hydrogen, and water vapor. Although the raw material gas after the first reaction contains water vapor, it is preferable to remove the water vapor from the raw material gas before proceeding to the second reaction, as water vapor may reduce the conversion rate of methane in the second reaction.
[0023] In the second reaction, 2 moles of carbon monoxide and 2 moles of hydrogen are produced from 1 mole of methane and 1 mole of carbon dioxide synthesized in the first reaction, via a catalyst. The raw material gas after the second reaction is a mixed gas containing hydrogen, methane, carbon dioxide, and carbon monoxide.
[0024] In the third reaction, 2 moles of carbon monoxide are converted to 1 mole of solid carbon and 1 mole of carbon dioxide via a catalyst. Since the solid carbon precipitates on the surface of the catalyst, the catalyst is recovered along with the precipitated solid carbon. In the third reaction, various reaction systems are competing with each other. Therefore, the raw material gas after the third reaction becomes a mixed gas containing hydrogen, methane, carbon dioxide, carbon monoxide, and water vapor.
[0025] [Configuration of a solid carbon deposition apparatus] Embodiments of the present invention will be described below. Figure 1 shows a solid carbon deposition apparatus according to the present invention. The solid carbon deposition apparatus 1 is a device that precipitates solid carbon from process exhaust gas containing carbon dioxide. Process exhaust gas refers to exhaust gas containing carbon dioxide emitted from cement clinker firing processes, quicklime production processes, thermal power plants, waste incineration facilities, firing equipment for ceramics and other products, steel mills, and chemical plants.
[0026] As shown in Figure 1, the solid carbon deposition apparatus 1 has three reactors in which different reactions occur, and the three reactors are connected in series. When the reactor to which the raw material gas is supplied is designated as the first reactor 10, the reactions proceed in the order of the first reactor 10, the second reactor 20, and the third reactor 30, and solid carbon is deposited in the third reactor 30.
[0027] The solid carbon deposition apparatus 1 includes, in addition to the three reactors, a hydrogen supply unit 3, a hydrogen flow meter 4, a first gas mixer 5, a second gas mixer 6, a third gas mixer 7, a first gas separator 8, a second gas separator 9, steam removal equipment 41-43 installed at the outlets of each reactor, exhaust gas measuring instruments 45-47, and a flow meter 50. Furthermore, it is preferable that the solid carbon deposition apparatus 1 also includes equipment 61 for removing sulfur oxides that cause catalyst degradation, carbon dioxide concentration equipment 62, and equipment 70 for reusing the mixed gas discharged from the third reactor 30. In addition, since the absolute amount of raw material gas increases if nitrogen or oxygen is contained in the process exhaust gas, equipment for removing nitrogen and oxygen from the process exhaust gas may be further provided upstream of the first reactor.
[0028] The exhaust gas measuring devices 45-47 are installed at the outlets of each reactor, preferably at the gas flow section after the separation of water vapor, and measure the composition of the mixed gas discharged from each reactor. The exhaust gas measuring devices 45-47 only need to be capable of determining the component ratios of at least hydrogen, methane, carbon dioxide, and carbon monoxide, and examples include sensors and gas property analyzers. The first exhaust gas measuring device 45 measures the composition of the mixed gas discharged from the first reactor 10. The second exhaust gas measuring device 46 measures the composition of the mixed gas discharged from the second reactor 20. The third exhaust gas measuring device 47 measures the composition of the mixed gas discharged from the third reactor 30. The third exhaust gas measuring device 47 is not essential for the solid carbon deposition apparatus 1, but it is preferable that it measures the composition ratio of the exhaust gas in each reactor.
[0029] Gas mixers 5 to 7 adjust the mixed gas supplied to each reactor by mixing multiple gases. It is preferable that each of the gas mixers 5 to 7 is equipped with a flow meter to measure the flow rate of the mixed gas. The first gas mixer 5 adjusts the raw material gas supplied to the first reactor 10, the second gas mixer 6 adjusts the mixed gas supplied to the second reactor 20, and the third gas mixer 7 adjusts the mixed gas supplied to the third reactor 30. The second gas mixer 6 and the third gas mixer 7 are not essential to the solid carbon deposition apparatus 1, but the mixed gas discharged from each reactor may not have a composition ratio suitable for the next reaction. Therefore, it is preferable that the mixed gas discharged from each reactor be adjusted by the second gas mixer 6 and the third gas mixer 7 to remove part of the mixed gas or add other gases.
[0030] The first gas mixer 5 mixes hydrogen supplied from the hydrogen supply equipment 3 with process exhaust gas containing carbon dioxide to produce a raw material gas to be supplied to the first reactor 10. Preferably, the process exhaust gas is supplied to the first gas mixer 5 after sulfur oxides are removed by the sulfur oxide removal equipment 61 and the carbon dioxide concentration is increased by the carbon dioxide concentration equipment 62. If there is also equipment 70 for recycling the mixed gas discharged from the third reactor 30, the mixed gas discharged from the third reactor 30 may be mixed with the raw material gas.
[0031] The first reactor 10 brings the raw material gas supplied from the first gas mixer 5 into contact with a catalyst that activates the methanation reaction, producing methane and water from the raw material gas as shown in Equation 6. Preferably, the raw material gas is supplied to the first reactor 10 so that the space velocity is 2000 to 20000 / h. The first reactor 10 comprises a gas flow reaction tube filled with a catalyst that activates the methanation reaction, and a heating furnace capable of heating the gas flow reaction tube to 300 to 550°C. Since the gas flow path is not blocked by solid products, for example, an atmospheric pressure flow reactor with a fixed gas flow tube is used in the first reactor 10.
[0032] Catalysts that activate the methanation reaction include, for example, Ni, Ru, Pt, and Rh. Various oxides and aluminosilicates such as CeO2, ZrO2, Y2O3, and Al2O3 can be used as supports. The catalyst can be in any shape as long as a predetermined space velocity is achieved, but a helical shape is preferred because it requires less catalyst volume. When the catalyst is helical, it is made by forming a metal plate member such as aluminum into a helical shape and applying a paste-like catalyst to it.
[0033] The first exhaust gas measuring device 45 measures the composition of the mixed gas discharged from the first reactor 10. At this time, the solid carbon deposition device 1 is controlled so that the CO2 / CH4 molar ratio in the mixed gas discharged from the first reactor 10 is measured to be between 0.9 and 2.1. When the CO2 / CH4 molar ratio in the mixed gas discharged from the first reactor 10 is between 0.9 and 2.1, catalyst degradation due to solid carbon deposition in the second reactor can be suppressed, and the residue of unreacted CO2 can be suppressed.
[0034] The second reactor 20 converts methane to carbon monoxide as shown in Equation 7 by heating a mixed gas containing methane supplied from the first reactor 10 in contact with a catalyst that promotes the dry reforming reaction. Preferably, the mixed gas supplied to the second reactor 20 is supplied so that the space velocity is 1300 to 15000 / h. The second reactor 20 comprises a gas flow reaction tube filled with a catalyst that activates the dry reforming reaction, and a heating furnace capable of heating the gas flow reaction tube to 700 to 900°C. Since there is little concern that the gas flow path in the reactor will be blocked by solid products, for example, an atmospheric pressure flow reactor with a fixed gas flow side tube is used in the second reactor 20.
[0035] Catalysts that activate the dry reforming reaction include, for example, Ni and Rh. Various oxides and aluminosilicates such as CeO2, ZrO2, Y2O3, and Al2O3 can be used as supports, but γ-Al2O3 is preferred. The catalyst can be in any shape as long as a predetermined space velocity is achieved, but a helical shape is preferred because it requires less catalyst volume. When the catalyst is helical, it is made by forming a metal plate member such as stainless steel into a helical shape and applying a paste-like catalyst to it.
[0036] The second exhaust gas measuring device 46 measures the composition of the mixed gas discharged from the second reactor 20. At this time, the solid carbon deposition device 1 is controlled so that the carbon monoxide concentration in the mixed gas discharged from the second reactor 20 is measured to be 30 vol% or higher, and the CO / (CH4+CO2+CO) molar ratio is measured to be 0.80 or higher. When the carbon monoxide concentration in the mixed gas discharged from the second reactor 20 is 30 vol% or higher, and the CO / (CH4+CO2+CO) molar ratio is 0.80 or higher, the recovery rate of solid carbon can be improved.
[0037] The third reactor 30 brings a mixed gas containing carbon monoxide supplied from the second reactor 20 into contact with a catalyst that activates the solid carbon deposition reaction, and precipitates solid carbon from carbon monoxide as shown in Equation 8. The mixed gas supplied to the third reactor 30 is preferably supplied so that the space velocity is a maximum of 2000 / h. The third reactor 30 comprises a gas flow reaction tube filled with the catalyst that activates the solid carbon deposition reaction, and a heating furnace capable of heating the gas flow reaction tube to 400-500°C. The third reactor 30 is preferably capable of continuously discharging the catalyst on which solid carbon has precipitated, and also capable of continuously supplying new catalyst into the reactor. For example, a fluidized bed, a moving bed, or a rotary kiln are preferred.
[0038] Catalysts that activate the solid carbon deposition reaction include Ni, Fe, Mn, Co, Cu, and Zn, but iron-based catalysts are preferred from an environmental perspective. Various oxides and aluminosilicates such as CeO2, ZrO2, Y2O3, and Al2O3 can be used as supports. The catalyst can be in any shape as long as a predetermined space velocity is achieved, but a helical shape is preferred because it requires less catalyst volume. When a catalyst is made into a helical shape, it is manufactured by forming a metal plate member such as stainless steel into a helical shape and applying a paste-like catalyst to it.
[0039] Furthermore, Figure 1 shows that steam removal equipment 41-43 is provided at the outlet of each reactor. Steam removal equipment 41-43 concentrates the steam by cooling the gas discharged from the outlet of the target reactor and discharges it as factory wastewater.
[0040] In the methanation reaction in the first reactor 10, water vapor is generated. Actively removing the generated water vapor increases the reaction rate of the forward reaction in Equation 6, improving the conversion rate of CO2 to methane. Therefore, it is preferable to install a first water vapor removal facility 41 at the outlet of the first reactor 10 to actively remove the water vapor. On the other hand, the dry reforming reaction in the second reactor 20 does not basically generate water vapor. Therefore, it is not necessary to install a second water vapor removal facility 42 at the outlet of the second reactor 20. However, considering that various reaction systems compete within the second reactor 20, and that water vapor may be generated when the type of catalyst or temperature conditions are changed, it may be preferable to install one. Furthermore, although the solid carbon deposition reaction is dominant in the third reactor 30, it is conceivable that some reactions that generate water vapor may occur. Therefore, it is preferable to install a third water vapor removal facility 43 at the outlet of the third reactor 30.
[0041] Furthermore, as described above, the solid carbon deposition apparatus 1 preferably has equipment 70 that allows for the recycling and reuse of the mixed gas discharged from the third reactor 30. The equipment 70 that allows for the recycling and reuse of the mixed gas discharged from the third reactor 30 may include equipment that supplies the mixed gas discharged from the third reactor 30 to each reactor. Since the mixed gas discharged from the third reactor 30 contains carbon dioxide, carbon dioxide emissions can be prevented by using the mixed gas as a raw material for the raw material gas instead of discharging it. The equipment 70 that allows for the recycling and reuse of the mixed gas discharged from the third reactor 30 may also allow for the recycling and reuse of a portion of the mixed gas discharged not only from the third reactor 30, but also from the first reactor 10 and the second reactor 20. In this case, it is preferable to adjust the composition ratio of the mixed gas using gas mixers 5 to 7 before supplying it to each reactor, rather than supplying the discharged mixed gas directly to each reactor.
[0042] To adjust the composition ratio of the mixed gas, it is preferable that sensors for measuring the composition ratio of the gases supplied to gas mixers 5-7, valves capable of adjusting the flow rate of each mixed gas, and gas mixers 5-7 are installed. The sensors only need to be capable of determining the component ratios of at least hydrogen, methane, carbon dioxide, and carbon monoxide, and it is preferable that the valves capable of adjusting the flow rate of each mixed gas are installed not only at the outlet from which process exhaust gas is discharged and the hydrogen supply equipment 3, but also when the mixed gas discharged from the first reactor 10 and the second reactor 20, and the mixed gas discharged from the third reactor 30 are circulated and reused in each gas mixer.
[0043] Furthermore, in the solid carbon deposition apparatus 1, the reactions in the first reactor 10 and the third reactor 30 are exothermic, while the reaction in the second reactor 20 is an endothermic reaction. Therefore, it is preferable to recover the sensible heat of the mixed gas discharged from the first reactor 10 and the third reactor 30 using a heat exchanger and use it as an energy source for the second reactor 20.
[0044] [Solid carbon deposition system] Next, the solid carbon deposition system will be described. Figure 2 is a schematic diagram showing the configuration of the solid carbon deposition system. The solid carbon deposition system 500 controls the composition ratio of the mixed gas discharged from each reactor in the solid carbon deposition apparatus 1 to a specified range. The specification may be made by the user, but may also be made by pre-setting, setting by automatic calculation, or by instruction via the network.
[0045] The solid carbon deposition system 500 comprises a solid carbon deposition apparatus 1 and a gas composition ratio control device 100. The gas composition ratio control device has a storage unit 110, an operation unit 120, and a control unit 130. The storage unit 110 records values measured in the solid carbon deposition apparatus 1. The values measured in the solid carbon deposition apparatus 1 include, for example, the composition ratio of the mixed gas discharged from each reactor, the composition ratio of the process exhaust gas, and the composition ratio of the gas supplied to the gas mixers 5-7.
[0046] The control unit 120 is a device that the user can use to input data as desired, such as a keyboard, mouse, or touch panel. The user can input any range of composition ratios for the mixed gases discharged from each reactor via the control unit 120.
[0047] The control unit 130 controls the solid carbon deposition apparatus 1 so that the mixed gas discharged from each reactor falls within a specified range, based on data recorded in the storage unit 110, including the measurement results from the exhaust gas measuring instruments 45 to 47. Specifically, it controls the composition ratio and flow rate of the mixed gas supplied to each reactor, as well as the temperature and pressure in each reactor, according to the measurement results from the exhaust gas measuring instruments 45 to 47. The composition ratio of the mixed gas supplied to each reactor may be adjusted by partially removing the mixed gas or adding other gases, or, if there is equipment 70 for circulating the mixed gas discharged from the third reactor 30, the mixed gas discharged from the third reactor 30 may be mixed in and adjusted. By recognizing the gas flow rate from each piece of equipment and controlling the valves supplying the gas to the gas mixers 5 to 7, the composition ratio of the mixed gas can be controlled in the gas mixers 5 to 7.
[0048] In this embodiment, we have described an example in which the composition ratio of the mixed gas discharged from all reactors can be controlled. However, it is sufficient that at least the CO2 / CH4 molar ratio in the gas discharged from the first reactor 10 and the carbon monoxide concentration and CO / (CH4+CO2+CO) molar ratio in the mixed gas discharged from the second reactor 20 can be controlled within a specified range, and it is not necessary to be able to control the composition ratio of the mixed gas discharged from the third reactor 30.
[0049] [Method for precipitating solid carbon] Next, we will explain the method for precipitating solid carbon. First, the raw material gas supplied to the first reactor 10 is prepared. The raw material gas is produced by mixing hydrogen supplied from the hydrogen supply equipment 3 with process exhaust gas containing carbon dioxide.
[0050] Next, the raw material gas is supplied to the first reactor 10, and the raw material gas is circulated through the gas flow reaction tube of the first reactor 10. The gas flow reaction tube is filled with a catalyst heated to 300-500°C by a heating furnace, and the catalyst, which activates the methanation reaction, comes into contact with the raw material gas, producing methane from the raw material gas. At this time, the CO2 / CH4 molar ratio in the mixed gas discharged from the first reactor 10 is adjusted to be between 0.9 and 2.1.
[0051] Next, the mixed gas discharged from the first reactor 10 is supplied to the second reactor 20, and the mixed gas is circulated through the gas flow reaction tube of the second reactor 20. The gas flow reaction tube is filled with a catalyst heated to approximately 800°C by a heating furnace, and the catalyst, which activates the dry reforming reaction, comes into contact with the mixed gas, converting methane into carbon monoxide. At this time, the carbon monoxide concentration in the mixed gas discharged from the second reactor 20 is adjusted to be 30 vol% or more, and the CO / (CH4+CO2+CO) molar ratio is adjusted to be 0.80 or more.
[0052] Next, the mixed gas discharged from the second reactor 20 is supplied to the third reactor 30, and the mixed gas is circulated through the gas flow reaction tube of the third reactor 30. The gas flow reaction tube is filled with a catalyst heated to approximately 450°C by a heating furnace. The catalyst, which activates the solid carbon deposition reaction, comes into contact with the mixed gas, and carbon monoxide is converted into solid carbon, which is deposited on the surface of the catalyst. Solid carbon can then be recovered by recovering the catalyst on which the solid carbon has been deposited.
[0053] From the above, in the method for precipitating solid carbon according to the present invention, the reaction can be carried out continuously from the time the raw material gas is supplied to the first reactor until solid carbon is precipitated in the third reactor. This makes the process more efficient compared to when each reaction is carried out independently. Since the carbon monoxide concentration in the mixed gas discharged from the second reactor 20 is 30 vol% or more, the solid carbon recovery rate is improved.
[0054] [Examples] (Example 1) The heating furnace in the first reactor was a single-zone electric furnace with temperature control (a ceramic electric tubular furnace manufactured by Asahi Rika Seisakusho, with an effective length of 300 mm), and the atmospheric pressure flow-through reaction tube was a quartz tube with an inner diameter of 8 mmφ and a length of 600 mm. Two catalysts, each coated with 10 wt% Ni / CeO2 on the surface of a spiral structure as shown in Figure 3, were installed inside the atmospheric pressure flow-through reaction tube at the position of the thermocouple for temperature control of the heating furnace, to activate the methanation reaction.
[0055] The catalyst used to activate the methanation reaction was CeO2 (reagent manufactured by Kanto Chemical Co., Ltd.), on which 10 wt% of Ni(NO3)2·6H2O (98% Wako Pure Chemical Industries) was supported by evaporation to dryness. After support, the material was calcined at 500°C for 2 hours in an air atmosphere to separate the nitric acid component. After cooling the calcined material, distilled water was added and the mixture was ground using a mortar to prepare a Ni / CeO2 paste.
[0056] In addition to the Ni / CeO2 paste, a spirally twisted aluminum plate (JIS A1100 H14, 7 mm wide x 50 mm long, 1.5 mm thick), as shown in Figure 3, was surface-treated with a 0.8 mol NaOH aqueous solution and a 3.0 mol hydrochloric acid solution. The plate was then repeatedly dried with cold air and immersed until a sufficient amount of Ni / CeO2 catalyst was supported on the spirally twisted aluminum plate to achieve the desired methanation.
[0057] The second reactor was prepared in the same manner as the first reactor, except that a catalyst for activating the dry reforming reaction was used instead of a catalyst for activating the methanation reaction. The catalyst for activating the dry reforming reaction was prepared by supporting 10 wt% of Ni(NO3)2·6H2O (Wako Pure Chemical Industries 98%) on a commercially available γ-Al2O3 (C20, manufactured by Nippon Light Metal Co., Ltd.) support by evaporation to dryness. It was prepared in the same manner as the catalyst for activating the methanation reaction, except that a Ni / γ-Al2O3 paste was applied to a spirally twisted stainless steel plate (SUS304, 7 mm wide x 50 mm long, 0.5 mm thick) as shown in Figure 3.
[0058] The third reactor was prepared in the same manner as the first reactor, except that a quartz tube with an inner diameter of 21 mm and a length of 600 mm was used as the atmospheric pressure flow-through reaction tube, and instead of a catalyst to activate the methanation reaction, eight catalysts to activate the solid carbon deposition reaction were placed inside the atmospheric pressure flow-through reaction tube (four catalysts bundled together, with two bundles arranged in series). The catalyst to activate the solid carbon deposition reaction was magnetite (Fe3O4 reagent: Wako Pure Chemical Industries 98%), and distilled water was added to the magnetite to make a paste. It was prepared in the same manner as the catalyst to activate the methanation reaction, except that the paste-like magnetite was applied to a spirally twisted stainless steel plate (SUS304, 7 mm wide x 50 mm long, 0.5 mm thick) as shown in Figure 3.
[0059] After preparing each reactor, hydrogen was flowed at 200 ml / min while maintaining a temperature of 500°C for 1 hour to reduce the catalyst in each reactor. Next, the control temperature of the first reactor was set to 350°C, the control temperature of the second reactor to 800°C, and the control temperature of the third reactor to 450°C. Once all reactors reached the predetermined temperatures, a hydrogen standard gas cylinder was used as hydrogen supply equipment 3, and a carbon dioxide standard gas cylinder was used instead of process exhaust gas. The raw material gas was supplied to the first reactor via a mass flow controller and a first gas mixer.
[0060] At this time, solid carbon was recovered for 4 hours with a molar ratio of H2 / CO2 in the raw material gas set to 2.6. Specifically, the hydrogen flow rate was set to 180 ml / min and the carbon dioxide flow rate to 70 ml / min using a mass flow controller, and the total flow rate of the raw material gas was set to 250 ml / min and supplied to the first reactor.
[0061] Each reactor outlet was equipped with a steam removal system and a sampling port. Thirty minutes after the indicated temperature of each reactor reached the set temperature, samples were taken from the sampling port using a syringe, and hydrogen, nitrogen, oxygen, methane, carbon monoxide, and carbon dioxide were quantitatively analyzed using a gas chromatograph GC-2014 (Shimadzu Corporation).
[0062] Furthermore, a wet gas meter was installed at the outlet of the third reactor to measure the gas flow rate. The mixed gas discharged from the third reactor was not recycled but discharged into an outdoor pollution control facility. After the third reactor had cooled sufficiently, the catalyst was removed from the atmospheric pressure flow-type reaction tube, the weight of the precipitated solid carbon was measured, and the solid carbon recovery rate was calculated using Equation 9 below. Solid carbon recovery rate (%) = (moles of precipitated solid carbon) / (moles of carbon supplied to the solid carbon precipitation apparatus) × 100 ... (Equation 9)
[0063] (Example 2) The procedure was carried out in the same manner as in Example 1, except that the hydrogen flow rate was set to 170 ml / min, the carbon dioxide flow rate to 80 ml / min, and the molar ratio of H2 / CO2 in the source gas was set to 2.1.
[0064] (Example 3) The procedure was carried out in the same manner as in Example 1, except that the hydrogen flow rate was set to 160 ml / min, the carbon dioxide flow rate to 90 ml / min, and the molar ratio of H2 / CO2 in the source gas was set to 1.8.
[0065] (Comparative Example 1) The procedure was carried out in the same manner as in Example 1, except that the hydrogen flow rate was set to 200 ml / min, the carbon dioxide flow rate to 50 ml / min, and the molar ratio of H2 / CO2 in the source gas was set to 4.0.
[0066] (Comparative Example 2) The procedure was carried out in the same manner as in Example 1, except that the hydrogen flow rate was set to 190 ml / min, the carbon dioxide flow rate to 60 ml / min, and the molar ratio of H2 / CO2 in the source gas was set to 3.2.
[0067] (Comparative Example 3) The procedure was carried out in the same manner as in Example 1, except that the hydrogen flow rate was set to 150 ml / min, the carbon dioxide flow rate to 100 ml / min, and the molar ratio of H2 / CO2 in the source gas was set to 1.5.
[0068] (Experimental results) The experimental results for Examples 1-3 and Comparative Examples 1-3 are shown in Tables 1 and 2 below. Table 1 shows the molar ratio of H2 / CO2 in the raw material gas, the gas concentrations of hydrogen, methane, carbon dioxide, and carbon monoxide in the mixed gas sampled from a sampling hole at the outlet of the first reactor, the CO2 conversion rate, and the CO2 / CH4 molar ratio. The CO2 conversion rate was calculated from the amount of carbon dioxide reacted in the first reactor / the amount of carbon dioxide supplied. [Table 1]
[0069] Table 2 shows the molar ratio of H2 / CO2 in the raw material gas, the gas concentrations of hydrogen, methane, carbon dioxide, and carbon monoxide in the mixed gas sampled from a sampling hole at the outlet of the second reactor, the molar ratio of H2 / CO2, the molar ratio of CO / (CH4+CO2+CO), and the solid carbon recovery rate. [Table 2]
[0070] As shown in Tables 1 and 2, in Examples 1 to 3, the solid carbon recovery rate was high at 20% or more, and the methane gas concentration in the mixed gas discharged from the second reactor 20 was less than 5%. In contrast, in Comparative Examples 1 to 3, which satisfied at least one of the following conditions: the CO2 / CH4 molar ratio in the mixed gas discharged from the first reactor was less than 0.9, the carbon monoxide concentration in the mixed gas discharged from the second reactor was less than 30%, and the CO / (CH4+CO2+CO) molar ratio was less than 0.80, the solid carbon recovery rate was less than 20% or the methane gas concentration in the mixed gas discharged from the second reactor was 5% or more. From this, it was confirmed that by setting the CO2 / CH4 molar ratio in the mixed gas discharged from the first reactor to 0.9 to 2.1, the carbon monoxide concentration in the mixed gas discharged from the second reactor to 30 vol% or higher, and the CO / (CH4+CO2+CO) molar ratio to 0.80 or higher, the solid carbon recovery rate is improved, and the generation of methane, a by-product of the solid carbon precipitation reaction, and the residue of unreacted methane are suppressed. [Explanation of Symbols]
[0071] 1. Solid carbon deposition apparatus 3. Hydrogen supply facilities 4. Hydrogen flow meter 5. First gas mixer 6. Second gas mixer 7. Third gas mixer 8. First gas separator 9. Second gas separator 10 First Reactor 20 Second Reactor 30 Third Reactor 41. First Steam Removal Equipment 42 Second Steam Removal Equipment 43. Third Steam Removal Equipment 45. First exhaust gas measuring instrument 46. Second exhaust gas measuring instrument 47 Third exhaust gas measuring instrument 50 flow meter 61 Equipment for removing sulfur oxides 62. Carbon dioxide concentration equipment 70 Equipment for circulating and utilizing mixed gases 100 Gas composition ratio control device 110 Storage section 120 Operation section 130 Control Unit 500 Solid Carbon Deposition System
Claims
1. A first step involves contacting a raw material gas containing carbon dioxide and hydrogen with a catalyst that activates a methanation reaction to produce a gas containing methane and water vapor from the raw material gas. A water vapor removal step, which removes at least a portion of the water vapor from the gas generated in the first step, A second step involves heating the methane contained in the gas from which at least some of the water vapor has been removed in the water vapor removal step, in contact with a catalyst that activates the dry reforming reaction, thereby converting the methane contained in the gas from which at least some of the water vapor has been removed into carbon monoxide. The third step involves contacting the converted carbon monoxide with a catalyst that activates a solid carbon deposition reaction, thereby precipitating solid carbon from the converted carbon monoxide. CO in the gas from which at least some of the water vapor has been removed in the water vapor removal step from the gas generated in the first step. 2 / CH 4 The molar ratio is between 0.9 and 2.
1. The carbon monoxide concentration in the gas produced in the second step is 30 vol% or higher, and CO / (CH 4 +CO 2 A method for precipitating solid carbon, characterized in that the molar ratio of +CO is 0.80 or higher.
2. A solid carbon deposition system for precipitating solid carbon from a raw material gas containing carbon dioxide and hydrogen, A first reactor that brings the aforementioned raw material gas into contact with a catalyst that activates the methanation reaction to produce a gas containing methane and water vapor from the raw material gas, A steam removal device that removes at least some of the steam from the gas produced in the first reactor, A second reactor converts the methane contained in the gas from which at least some of the water vapor has been removed by the water vapor removal equipment, which is produced in the first reactor, into carbon monoxide by heating the gas in contact with a catalyst that activates the dry reforming reaction. A third reactor is provided in which the converted carbon monoxide is brought into contact with a catalyst that activates the solid carbon deposition reaction, and the solid carbon is deposited from the converted carbon monoxide. A first exhaust gas measuring instrument for measuring the composition of the gas from which at least some of the water vapor has been removed by the water vapor removal equipment from the gas produced in the first reactor, A second exhaust gas measuring instrument for measuring the composition of the gas discharged from the second reactor, The system includes a control unit that controls the composition ratio of the gases discharged from each reactor based on the measurement results of each exhaust gas measuring device, The control unit controls the CO2 in the gas from which at least some of the water vapor has been removed by the water vapor removal equipment from the gas generated in the first reactor. 2 / CH 4 The molar ratio, the carbon monoxide concentration in the gas discharged from the second reactor, and CO / (CH 4 +CO 2 A solid carbon precipitation system characterized by controlling the molar ratio of +CO to fall within a specified range.
Citation Information
Patent Citations
Continuous carbon removing system
JP1996133200A
Device for manufacturing carbon
JP2003048708A
Method for immobilizing carbon dioxide and its system
JP2005060137A
Carbon dioxide fixation system
JP2015196619A
Method and apparatus for manufacturing methane
JP2018135283A