Compound for forming metal-containing films, composition for forming metal-containing films, and pattern forming method
A metal-containing film-forming compound with Ti, Zr, or Hf, and a cyclic ether structure addresses pattern collapse and etching resistance issues in multilayer resist methods, enhancing adhesion and precision in semiconductor manufacturing.
Patent Information
- Application Number
- JP2023139356
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-08-29
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-08-29
AI Technical Summary
The miniaturization of semiconductor patterns leads to decreased photoresist film resolution and aspect ratio issues, resulting in pattern collapse and inadequate dry etching selectivity, necessitating improved adhesion and etching resistance in multilayer resist methods.
A metal-containing film-forming compound comprising Ti, Zr, or Hf, and a polydentate ligand with a cyclic ether structure is used to enhance adhesion to the resist upper layer, preventing pattern collapse and providing high refractive index and etching resistance under ArF immersion and high NA exposure conditions.
The compound forms a metal-containing film with excellent adhesion to the resist upper layer, suppressing pattern collapse and ensuring high-precision pattern transfer in multilayer resist processes, with improved anti-reflective effects and etching resistance.
Smart Images

Figure 0007954634000065 
Figure 0007954634000066 
Figure 0007954634000067
Abstract
Description
[Technical Field]
[0001] The present invention relates to a metal-containing film-forming compound that can be used for fine patterning by a multilayer resist method in the semiconductor device manufacturing process, a metal-containing film-forming composition using the compound, and a pattern-forming method using the composition. [Background technology]
[0002] With the increasing integration and speed of LSIs, the miniaturization of pattern dimensions is progressing rapidly. Lithography technology has achieved the formation of fine patterns in line with this miniaturization by shortening the wavelength of the light source and appropriately selecting the resist composition. At the heart of this is the single-layer positive photoresist composition. This single-layer positive photoresist composition has a framework in the resist resin that is resistant to dry etching with chlorine-based or fluorine-based gas plasma, and also has a switching mechanism that causes the exposed area to dissolve, thereby forming a pattern by dissolving the exposed area, and the remaining resist pattern is used as an etching mask to dry etch the substrate to be processed.
[0003] However, when the thickness of the photoresist film used was kept the same while miniaturization was achieved, i.e., the pattern width was reduced, the resolution performance of the photoresist film decreased. Furthermore, when attempting to develop the photoresist film using a developer, the aspect ratio became too large, resulting in pattern collapse. For this reason, as patterns became smaller, the photoresist film was made thinner.
[0004] On the other hand, the processing of substrates typically involves using a photoresist film with a pattern formed on it as an etching mask and processing the substrate by dry etching. However, in reality, there is no dry etching method that can achieve complete etching selectivity between the photoresist film and the substrate. As a result, the photoresist film is damaged and disintegrates during substrate processing, making it impossible to accurately transfer the resist pattern to the substrate. Therefore, with the miniaturization of patterns, high dry etching resistance has been required for the resist composition. However, at the same time, in order to improve resolution, resins with low light absorption at the exposure wavelength have been required for the resins used in the photoresist composition. Therefore, as the exposure light has become shorter in wavelength, from i-line to KrF and ArF, the resins have also changed to novolac resins, polyhydroxystyrene, and resins with aliphatic polycyclic skeletons. However, in reality, the etching rate under dry etching conditions during substrate processing has become fast, and recent photoresist compositions with high resolution tend to have weaker etching resistance.
[0005] This necessitates dry etching of substrates using thinner photoresist films with weaker etching resistance, making the securing of materials and processes for this manufacturing stage a matter of urgency.
[0006] One way to solve these problems is the multilayer resist method. In this method, a photoresist film (i.e., a resist upper layer) and a resist interlayer with different etching selectivity are interposed between the resist upper layer and the substrate to be processed. After obtaining a pattern on the resist upper layer, the resist upper layer pattern is used as a dry etching mask to transfer the pattern to the resist interlayer by dry etching, and then the resist interlayer is used as a dry etching mask to transfer the pattern to the substrate to be processed by dry etching.
[0007] One multilayer resist method is the three-layer resist method, which can be performed using the same resist compositions as those used in the single-layer resist method. In this three-layer resist method, for example, an organic film made of novolac resin or the like is deposited on the substrate to be processed as the resist underlayer, a silicon-containing resist interlayer is deposited on top of that as the resist interlayer, and a normal organic photoresist film is formed on top of that as the resist upper layer. When dry etching is performed using a fluorine-based gas plasma, the organic resist upper layer has a good etching selectivity ratio compared to the silicon-containing resist interlayer, so the resist upper layer pattern can be transferred to the silicon-containing resist interlayer by dry etching with a fluorine-based gas plasma. With this method, even if a resist composition that does not have sufficient thickness to form a pattern for direct processing of the substrate or a resist composition that does not have sufficient dry etching resistance for substrate processing is used, the pattern can be transferred to the silicon-containing resist interlayer (resist interlayer), and then by performing pattern transfer by dry etching with an oxygen-based or hydrogen-based gas plasma, a pattern of an organic film (resist underlayer) made of novolac resin or the like with sufficient dry etching resistance for substrate processing can be obtained. Many types of resist underlayer films, such as those described in Patent Document 1, are already known.
[0008] As silicon-containing resist interlayers used in the three-layer resist method described above, silicon-containing inorganic films produced by CVD, such as SiO2 films (e.g., Patent Document 2) and SiON films (e.g., Patent Document 3), and films that can be obtained by rotary coating, such as SOG (spin-on glass) films (e.g., Patent Document 4, Non-Patent Document 1) and crosslinkable silsesquioxane films (e.g., Patent Document 5), are used, and polysilane films (e.g., Patent Document 6) may also be usable. Among these, SiO2 films and SiON films have high performance as dry etching masks when dry etching the underlying organic film, but require special equipment for film formation. In contrast, SOG films, crosslinkable silsesquioxane films, and polysilane films can be formed by rotary coating and heating alone, and are considered to have high process efficiency.
[0009] The silicon-containing films conventionally used in such multilayer resist methods have several problems. For example, when attempting to form a resist pattern by photolithography, it is well known that exposure light is reflected by the substrate and interferes with the incident light, causing the so-called standing wave problem. To obtain fine patterns without edge roughness in the resist film under state-of-the-art ArF immersion and high NA exposure conditions, an anti-reflective function is essential for the interlayer. Furthermore, in the state-of-the-art semiconductor processes described above, the thinning of photoresists is progressing even further, so thinning of the interlayer is also required, and in next-generation exposure processes, it is required to impart an anti-reflective effect with a film thickness of 30 nm or less. In addition, the dry etching rate for oxygen gas plasma, which is commonly used when processing the resist underlayer, is preferably lower in order to increase the etching selectivity ratio between the interlayer and the underlayer, and improvement in dry etching resistance is required for the interlayer in line with the trend towards thinner films.
[0010] To meet the requirements for anti-reflective properties and dry etching characteristics, metal hard mask films containing Ti or Zr are attracting attention as resist interlayers, replacing conventional silicon-containing films. TiO2 and ZrO2 are known as high refractive index materials, and including them in the film makes it possible to improve the anti-reflective effect under high NA exposure conditions. Furthermore, the inclusion of metal-oxygen bonds is expected to provide excellent dry etching resistance to oxygen gas.
[0011] Furthermore, since the metal hard mask film exhibits excellent dry etching resistance not only to oxygen gas but also to fluorine gas, a two-layer resist method is also promising, in which the metal hard mask film is deposited as a resist underlayer on the substrate to be processed, and a resist upper layer is formed on top of it.
[0012] On the other hand, when such a metal hard mask film is used directly beneath the resist upper layer, improving adhesion with the resist pattern becomes a challenge. The cured metal hard mask film has a much higher surface energy (or a lower water contact angle) than the subsequently applied photoresist. This mismatch in surface energy causes poor adhesion between the metal hard mask film and the subsequently applied photoresist, leading to pattern collapse.
[0013] To suppress the collapse of photoresist patterns on a metal hard mask film, surface modification of the metal hard mask film is necessary. For example, Patent Document 7 reports a metal hard mask containing a surface-modified organic polymer. It has been reported that by utilizing the difference in free energy between the organic polymer and the metal compound and unevenly distributing the organic polymer on the surface, adhesion to the resist pattern is improved. To suppress pattern collapse, organic polymers containing surface-treated portions selected from hydroxyl, protected hydroxyl, protected carboxyl, and mixtures thereof are used. However, in the current situation where finer pattern formation is required, these materials do not have sufficient pattern collapse suppression performance. Furthermore, since the inclusion of organic polymers may degrade the dry etching resistance to oxygen gas, there is a need for the development of metal-containing film-forming compounds with excellent adhesion to the resist upper layer film.
[0014] Recently, it has been recognized that the interaction at the interface between the resist upper layer and the lower layer directly beneath it in fine patterns affects the sensitivity of the resist, the shape of the pattern (rectangularity and space residue), and from these perspectives, there is a need for performance improvement in the lower layer directly beneath the resist upper layer (Non-Patent Literature 2). [Prior art documents] [Patent Documents]
[0015] [Patent Document 1] Japanese Patent Publication No. 2004-205685 [Patent Document 2] Japanese Patent Application Publication No. 7-183194 [Patent Document 3] Japanese Patent Application Publication No. 7-181688 [Patent Document 4] Japanese Patent Application Publication No. 5-291208 [Patent Document 5] Special Publication No. 2005-520354 [Patent Document 6] Japanese Patent Application Publication No. 11-60735 [Patent Document 7] Patent Publication No. 6463600 [Non-patent literature]
[0016] [Non-Patent Document 1] J.Appl.Polym. Sci.,Vol.88,636-640(2003) [Non-Patent Document 2] Proc. SPIE Vol. 7273,72731J(2009) [Overview of the Initiative] [Problems that the invention aims to solve]
[0017] The present invention has been made in view of the above circumstances, and aims to provide a metal-containing film forming compound that provides a metal-containing film that yields a good pattern shape and has high adhesion to the resist upper layer film, thereby suppressing the collapse of the fine pattern in a fine patterning process in the semiconductor device manufacturing process, a metal-containing film forming composition using the compound, and a pattern forming method using the composition. [Means for solving the problem]
[0018] In order to solve the above problems, the present invention provides: The present invention provides a metal-containing film-forming compound, wherein the metal-containing film-forming compound comprises at least one metal atom selected from the group consisting of Ti, Zr, and Hf, and a polydentate ligand containing a cyclic ether structure having 2 to 13 carbon atoms that coordinates to the metal atom.
[0019] When such a metal-containing film-forming compound is used in a resist underlayer film-forming composition, it exhibits high adhesion to the resist upper layer film, prevents the deformation of fine patterns, and forms a metal-containing film that provides a good pattern shape. Furthermore, because the resulting metal-containing film exhibits a high refractive index, it can demonstrate a high anti-reflective effect under ArF immersion and high NA exposure conditions.
[0020] Furthermore, it is preferable that the polydentate ligand has a structure represented by the following general formulas (1-A) to (1-D). [ka] (In the above general formulas (1-A) to (1-D), R1 to R4 are monovalent organic groups having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms; R5 to R6 are monovalent organic groups having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms; and R7 to R 10 R is a monovalent organic group having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms. 11 R is a monovalent organic group having 1 to 20 carbon atoms, which may contain a cyclic ether structure having 2 to 13 carbon atoms, and Y is a divalent organic group having 1 to 10 carbon atoms. The compounds of the above general formulas (1-A) to (1-D) contain at least one cyclic ether structure having 2 to 13 carbon atoms. In the above general formula (1-A), R2 and R3 may be bonded to each other to form a cyclic ether structure having 2 to 13 carbon atoms. In the above general formula (1-B), adjacent R5 and R6 may be bonded to each other to form an unsaturated or saturated ring structure. In the above general formula (1-C), adjacent R8 and R9 may be bonded to each other to form a cyclic ether structure having 2 to 13 carbon atoms, or an unsaturated or saturated ring structure.
[0021] When a metal-containing film-forming compound has a polydentate ligand with such a structure, using it in a resist underlayer film-forming composition results in higher adhesion to the resist upper layer film, making it even more effective in preventing the deformation of fine patterns.
[0022] In this case, it is preferable that the polydentate ligand has the structure shown by formula (1-A) or (1-B) above.
[0023] Such polydentate ligands can provide metal-containing film-forming compounds with excellent stability.
[0024] Furthermore, it is preferable that the cyclic ether structure is one of the structures represented by the following formulas (a-1) to (a-2). [ka] (In the formula, R a (where * represents a hydrogen atom or an organic group with 1 to 10 carbon atoms, and * indicates a bond.)
[0025] The presence of such a cyclic ether structure causes the epoxy or oxetane structure to undergo a ring-opening reaction during heat deposition, leading to film hardening. Furthermore, the hydroxyl groups generated by this ring-opening reaction also contribute to improved adhesion to the resist upper layer film.
[0026] Furthermore, it is preferable that the metal-containing film-forming compound is a reaction product of a metal-containing compound comprising a metal compound represented by the following formula (2), a hydrolysate or condensate of the metal compound represented by the following formula (2), or a hydrolysate condensate, and a polydentate ligand having the structure represented by the above general formulas (1-A) to (1-D). [ka] (In the formula, M is one of Ti, Zr, and Hf; L is a monodentate ligand and / or polydentate ligand having 1 to 30 carbon atoms; X is a halogen atom, an alkoxy group, a carboxylate group, an acyloxy group, or -NR) a R b It is a hydrolyzable group selected from among the following. a and R b Each of these is independently a hydrogen atom or a monovalent organic group with 1 to 20 carbon atoms. a + b = 4, where a and b are integers between 0 and 4.
[0027] By using such a compound for forming a metal-containing film, it is possible to form a metal-containing film having more excellent dry etching resistance against oxygen gas.
[0028] At this time, the metal compound represented by the aforementioned formula (2) preferably has the structure of the following formula (3).
Chemical Formula
[0029] The compound for forming a metal-containing film having such a structure is preferable from the viewpoints of productivity and availability of raw materials.
[0030] Further, it is preferable that the compound for forming a metal-containing film further contains a ligand derived from a silicon compound represented by the following general formula (4).
Chemical Formula
Chemical Formula
[0031] By containing such a ligand, the stability of the compound for forming a metal-containing film can be further improved.
[0032] Further, in the present invention, there is provided a composition for forming a metal-containing film, which is (A) The above-mentioned metal-containing film-forming compound, and (B) Organic solvents The present invention provides a metal-containing film-forming composition containing the following:
[0033] Such a metal-containing film-forming composition provides high adhesion to the resist upper layer, prevents distortion of fine patterns, and forms a metal-containing film that gives a good pattern shape. Furthermore, because the resulting metal-containing film exhibits a high refractive index, it can exhibit a high anti-reflective effect under ArF immersion and high NA exposure conditions.
[0034] Furthermore, the composition may contain one or more of (C) a thermal acid generator and (D) a photoacid generator.
[0035] A metal-containing film-forming composition containing the above-mentioned additives will be a metal-containing film-forming composition with superior coatability and adhesion to the resist upper layer.
[0036] Furthermore, the composition may also contain one or more of (E) crosslinking agents and (F) surfactants.
[0037] A metal-containing film-forming composition containing the above-mentioned additives will be a metal-containing film-forming composition with superior coatability, dry etching resistance, and embedding and / or planarization properties.
[0038] Furthermore, it is preferable that the (B) organic solvent is a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher.
[0039] By imparting fluidity to the above-mentioned metal-containing film-forming compound through the addition of a high-boiling-point solvent, the occurrence of coating defects caused by drying of the metal-containing film-forming composition can be suppressed.
[0040] Furthermore, the present invention provides a method for forming a pattern on a substrate to be processed, (I-1) A step of forming a metal-containing film by applying the above-mentioned metal-containing film-forming composition onto a substrate to be processed and then heat-treating it. (I-2) A step of forming a resist upper layer film on the metal-containing film using a photoresist material, (I-3) After pattern exposure of the resist upper layer film, develop it with a developer to form a pattern on the resist upper layer film. (I-4) A step of transferring the pattern to the metal-containing film by dry etching using the resist upper layer film on which the pattern is formed as a mask, and (I-5) A step of processing the workpiece substrate using the metal-containing film on which the pattern is formed as a mask to form a pattern on the workpiece substrate. The present invention provides a pattern forming method having the following characteristics.
[0041] Furthermore, the present invention provides a method for forming a pattern on a substrate to be processed, (II-1) A step of forming a resist underlayer film on a substrate to be processed, (II-2) A step of forming a metal-containing film by applying the above-mentioned metal-containing film-forming composition onto the resist underlayer film and then heat-treating it. (II-3) A step of forming a resist upper layer film on the metal-containing film using a photoresist material, (II-4) After pattern exposure of the resist upper layer film, develop it with a developer to form a pattern on the resist upper layer film. (II-5) A step of transferring the pattern to the metal-containing film by dry etching, using the resist upper layer film on which the pattern is formed as a mask. (II-6) A step of transferring the pattern to the resist underlayer film by dry etching, using the metal-containing film on which the pattern has been transferred as a mask. (II-7) A step of processing the substrate to be processed using the resist underlayer film on which the pattern is formed as a mask to form a pattern on the substrate to be processed, The present invention provides a pattern forming method having the following characteristics.
[0042] As described above, the metal-containing film-forming compound of the present invention is, for example, a metal-containing film-forming compound containing a cyclic ether structure selected from formula (a-1) or (a-2) above. When this is used in a metal-containing film-forming composition, a metal-containing film with excellent adhesion to the resist upper layer can be formed, making it suitable for use in various pattern formation methods such as two-layer resist processes and three-layer resist processes. With these pattern formation methods, the metal-containing film provided by the present invention can effectively suppress pattern collapse, making it suitable for photolithography of the resist upper layer and enabling high-precision transfer of the resist upper layer pattern to the substrate to be processed. [Effects of the Invention]
[0043] As described above, the present invention provides a metal-containing film-forming compound that has high adhesion to a resist upper layer film and has an effect of suppressing the collapse of fine patterns, a metal-containing film-forming composition using the compound, and a pattern-forming method using the composition.
[0044] In resist underlayer films formed using conventional metal-containing film-forming compounds, the surface energy (or water contact angle) is significantly higher than that of the subsequently applied photoresist. This mismatch in surface energy causes poor adhesion between the metal-containing film and the subsequently applied photoresist, leading to pattern collapse. Furthermore, when organic polymers are mixed as surface modifiers, the dry etching resistance during processing of the organic underlayer film becomes insufficient, potentially inducing poor pattern transfer.
[0045] In contrast, the metal-containing film-forming compound of the present invention contains a cyclic ether structure, and when used in a metal-containing film-forming composition, it can form a metal-containing film with excellent adhesion to the resist upper layer film. Therefore, it has an effect of suppressing the collapse of fine patterns and imparts a highly rectangular pattern shape to the resist upper layer film on the substrate, making it extremely useful in multilayer resist processes. Furthermore, the metal-containing film-forming compound using the multidentate ligand of the present invention can form a resist underlayer film with a higher proportion of metal atoms compared to the metal-containing film-forming compound using the monodentate ligand. Therefore, it has excellent resistance to dry etching using oxygen gas and fluorine gas, respectively, and can form fine patterns on the substrate with high precision in various pattern formation methods such as two-layer resist processes and three-layer resist processes. [Brief explanation of the drawing]
[0046] [Figure 1] This is an explanatory diagram of an example of the pattern formation method of the present invention (a 3-layer resist process). [Figure 2] This is an explanatory diagram of an example of the pattern formation method of the present invention (two-layer resist process). [Figure 3] This is an explanatory diagram for the calculation of reflectance in the pattern formation method. [Modes for carrying out the invention]
[0047] As described above, in the fine patterning process of semiconductor device manufacturing, there has been a need for the development of a metal-containing film forming compound that provides a metal-containing film that yields a good pattern shape and has high adhesion to the resist upper layer film, thereby suppressing the collapse of the fine pattern, as well as a metal-containing film forming composition using the compound, and a pattern forming method using the composition.
[0048] As a result of diligent research into the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by a metal-containing film-forming compound containing a ligand of a specific structure, a metal-containing film-forming composition using the compound, and a pattern-forming method using the composition, and have completed the present invention.
[0049] In other words, the present invention relates to a metal-containing film-forming compound, wherein the metal-containing film-forming compound comprises at least one metal atom selected from the group consisting of Ti, Zr, and Hf, and a polydentate ligand containing a cyclic ether structure having 2 to 13 carbon atoms that coordinates to the metal atom.
[0050] The present invention will be described in detail below, but the present invention is not limited to these descriptions.
[0051] <Compounds for forming metal-containing films> The present invention relates to a metal-containing film-forming compound that can be used in a metal-containing film-forming composition, characterized in that the metal-containing film-forming compound has at least one metal atom selected from the group consisting of Ti, Zr, and Hf, and a polydentate ligand containing a cyclic ether structure having 2 to 13 carbon atoms that coordinates to the metal atom.
[0052] When such a metal-containing film-forming compound is used in a resist underlayer film-forming composition, it exhibits high adhesion to the resist upper layer film, prevents the deformation of fine patterns, and forms a metal-containing film that provides a good pattern shape. Furthermore, because the resulting metal-containing film exhibits a high refractive index, it can demonstrate a high anti-reflective effect under ArF immersion and high NA exposure conditions.
[0053] The polydentate ligand is preferably one of the structures shown by the following general formulas (1-A) to (1-D). [ka] (In the above general formulas (1-A) to (1-D), R1 to R4 are monovalent organic groups having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms; R5 to R6 are monovalent organic groups having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms; and R7 to R 10 R is a monovalent organic group having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms. 11 R is a monovalent organic group having 1 to 20 carbon atoms, which may contain a cyclic ether structure having 2 to 13 carbon atoms, and Y is a divalent organic group having 1 to 10 carbon atoms. The compounds of the above general formulas (1-A) to (1-D) contain at least one cyclic ether structure having 2 to 13 carbon atoms. In the above general formula (1-A), R2 and R3 may be bonded to each other to form a cyclic ether structure having 2 to 13 carbon atoms. In the above general formula (1-B), adjacent R5 and R6 may be bonded to each other to form an unsaturated or saturated ring structure. In the above general formula (1-C), adjacent R8 and R9 may be bonded to each other to form a cyclic ether structure having 2 to 13 carbon atoms, or an unsaturated or saturated ring structure.
[0054] The compounds of formulas (1-A) to (1-D) above contain at least one cyclic ether structure having 2 to 13 carbon atoms, preferably 2 to 10 carbon atoms. It is more preferable that the molecule contains one or two of the cyclic ether structures, and even more preferable that it contains one.
[0055] In the above formula (1-A), R1 and R4 are monovalent organic groups having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms. Preferably, R1 and R4 are a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted allyl group having 2 to 10 carbon atoms, a substituted or unsubstituted ethynyl group having 2 to 10 carbon atoms, or a monovalent organic group having 1 to 20 carbon atoms containing a cyclic ether structure having 2 to 13 carbon atoms. More preferably, R1 and R4 are a methyl group, a methoxy group, or an ethoxy group.
[0056] R2 and R3 are monovalent organic groups having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms. Preferably, R2 is a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted allyl group having 2 to 10 carbon atoms, a substituted or unsubstituted ethynyl group having 2 to 10 carbon atoms, or a monovalent organic group having 1 to 20 carbon atoms containing a cyclic ether structure having 2 to 13 carbon atoms. More preferably, R2 is a hydrogen atom, a methyl group, an ethyl group, a phenyl group, an allyloxy group, a propargyloxy group, or a monovalent organic group having 1 to 20 carbon atoms containing a cyclic ether structure having 2 to 13 carbon atoms. Furthermore, R2 and R3 may bond to each other to form a cyclic ether structure having 2 to 13 carbon atoms. If R2 has substituents other than a hydrogen atom, R3 is preferably a hydrogen atom. Preferably, at least one of R2 and R3 is a hydrogen atom. If R2 and R3 do not contain a cyclic ether structure with 2 to 13 carbon atoms, it is preferable that both R2 and R3 are hydrogen atoms.
[0057] In the above formula (1-B), R5 and R6 are a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, which may contain a cyclic ether structure having 2 to 13 carbon atoms. Preferably, R5 and R6 are a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, a substituted or unsubstituted allyl group having 2 to 10 carbon atoms, a substituted or unsubstituted ethynyl group having 2 to 10 carbon atoms, or a monovalent organic group having 1 to 20 carbon atoms containing a cyclic ether structure having 2 to 13 carbon atoms. If a cyclic ether structure having 2 to 13 carbon atoms is not included, R5 and R6 are preferably hydrogen atoms. R5 and R6 may be bonded to each other, forming an unsaturated or saturated ring structure.
[0058] In the above formula (1-C), R7 and R 10 This is a monovalent organic group having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms. It is preferably a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, and more preferably a hydrogen atom.
[0059] In the above formula (1-C), R8 is a monovalent organic group having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms, and is more preferably a monovalent organic group having 1 to 20 carbon atoms, which may contain a cyclic ether structure having 2 to 13 carbon atoms. R9 is a monovalent organic group having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms, and is more preferably a hydrogen atom or an alkyl or aryl group having 1 to 10 carbon atoms, and even more preferably a hydrogen atom. Furthermore, R8 and R9 may bond to each other to form a cyclic ether structure having 2 to 13 carbon atoms, or an unsaturated or saturated ring structure.
[0060] In the above equation (1-D), R 11 It is preferable that is a divalent organic group having 1 to 20 carbon atoms, including a cyclic ether structure having 2 to 13 carbon atoms. Y is a divalent organic group having 1 to 10 carbon atoms, preferably a divalent hydrocarbon group having 1 to 10 carbon atoms, more preferably a hydrocarbon group having 1 to 5 carbon atoms from the viewpoint of raw material availability, even more preferably a methylene group or an ethylene group, and particularly preferably an ethylene group.
[0061] When a metal-containing film-forming compound has such a multidentate ligand, using it in a resist underlayer film-forming composition results in higher adhesion to the resist upper layer film, making it even more effective in preventing the deformation of fine patterns.
[0062] The cyclic ether structure (cyclic ether structure having 2 to 13 carbon atoms) is preferably one of the structures shown by the following formulas (a-1) to (a-2). [ka] (In the formula, R a (where * represents a hydrogen atom or an organic group with 1 to 10 carbon atoms, and * indicates a bond.)
[0063] With such metal-containing film-forming compounds, the epoxy or oxetane structure undergoes a ring-opening reaction during heating for film formation, causing the film to harden. Furthermore, the hydroxyl groups generated by this ring-opening reaction also contribute to improved adhesion to the resist upper layer.
[0064] R in (a-2) above a The atom is preferably a hydrogen atom, a methyl group, or an ethyl group, with the ethyl group being more preferred.
[0065] The following compounds are examples of ligand structures derived from formulas (1-A) to (1-D), but the present invention is not limited to these.
[0066] [ka] (R1, R4, R above) a (This is the same as above, and n represents 1 to 10.)
[0067] From the viewpoint of productivity and stability of metal-containing film-forming compounds, the cyclic ether structure is more preferably the structure shown in formula (a-2).
[0068] It is more preferable that the polydentate ligand has the structure represented by formula (1-A) or (1-B) above.
[0069] Such polydentate ligands can provide metal-containing film-forming compounds with excellent stability.
[0070] Furthermore, it is preferable that the metal-containing film-forming compound is a reaction product of (a) a metal-containing compound which includes a metal compound represented by the following formula (2), a hydrolysate or condensate of the metal compound represented by the following formula (2), or a hydrolysate condensate, and a polydentate ligand having the structure represented by the above general formulas (1-A) to (1-D). [ka] (In the formula, M is one of Ti, Zr, and Hf; L is a monodentate ligand and / or polydentate ligand having 1 to 30 carbon atoms; X is a halogen atom, an alkoxy group, a carboxylate group, an acyloxy group, or -NR) a R b It is a hydrolyzable group selected from among the following. a and R b Each of these is independently a hydrogen atom or a monovalent organic group with 1 to 20 carbon atoms. a + b = 4, where a and b are integers between 0 and 4.
[0071] When such a metal-containing film-forming compound is used in a metal-containing film-forming composition, it is possible to form a metal-containing film with excellent dry etching resistance to oxygen gas.
[0072] [(a) Metal-containing compounds] (hydrolyzable group) Examples of hydrolyzable groups X in formula (2) above include halogen atoms, alkoxy groups, carboxylate groups, acyloxy groups, and -NR groups. a R b R is one example. a and R b Each of these is preferably a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.
[0073] Examples of the halogen atoms mentioned above include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms.
[0074] Examples of the alkoxy groups mentioned above include methoxy groups, ethoxy groups, and n-p groups. B Examples include the poxy group, i-propoxy group, n-butoxy group, and t-butoxy group.
[0075] Examples of the carboxylate groups mentioned above include acetate groups, propionate groups, butyrate groups, n-hexanecarboxylate groups, and n-octanecarboxylate groups.
[0076] Examples of the above-mentioned acyloxy groups include acetoxy group, ethylyloxy group, propionyloxy group, butyryloxy group, t-butyryloxy group, t-amiryloxy group, n-hexanecarbonyloxy group, and n-octanecarbonyloxy group.
[0077] The above -NR a R b Examples of such groups include unsubstituted amino groups, methylamino groups, dimethylamino groups, diethylamino groups, and dipropylamino groups.
[0078] The hydrolyzable group X is preferably an alkoxy group, and more preferably an i-propoxy group, an n-butoxy group, or a t-butoxy group.
[0079] (monodentate ligand) Examples of monodentate ligands L in formula (2) above include hydroxo ligands, carboxyl ligands, amide ligands, amine ligands, ammonia ligands, olefin ligands, and the like.
[0080] Examples of the above-mentioned amide ligands include unsubstituted amide ligands (NH2), methylamide ligands (NHMe), dimethylamide ligands (NMe2), diethylamide ligands (NEt2), and dipropylamide ligands (NPr2).
[0081] Examples of the amine ligands mentioned above include pyridine, trimethylamine ligand, and piperidine ligand.
[0082] Examples of olefin ligands include chain olefins such as ethylene and propylene, and cyclic olefins such as cyclopentene, cyclohexene, and norbornene.
[0083] (polydentate ligand) Examples of the polydentate ligand L in formula (2) above include ligands derived from hydroxy acid esters, ligands derived from β-diketones, ligands derived from β-ketoesters, ligands derived from α,α-dicarboxylic acid esters, hydrocarbons having π bonds, diphosphines, and the like.
[0084] Examples of the hydroxy acid esters mentioned above include glycolic acid esters, lactate esters, 2-hydroxycyclohexane-1-carboxylic acid esters, salicylic acid esters, and the like.
[0085] Examples of the above-mentioned β-diketones include acetoacetate esters, α-alkyl-substituted acetoacetate esters, β-ketopentanoate esters, benzoyl acetate esters, and 1,3-acetonedicarboxylic acid esters.
[0086] Examples of the α,α-dicarboxylic acid esters mentioned above include malonic acid diesters, α-alkyl-substituted malonic acid diesters, α-cycloalkyl-substituted malonic acid diesters, and α-aryl-substituted malonic acid diesters.
[0087] Examples of hydrocarbons having the π bond mentioned above include linear dienes such as butadiene and isoprene, cyclic dienes such as cyclopentadiene, methylcyclopentadiene, pentamethylcyclopentadiene, cyclohexadiene, and norbornadiene, and aromatic hydrocarbons such as benzene, toluene, xylene, hexamethylbenzene, naphthalene, and indene.
[0088] Examples of the above-mentioned diphosphines include 1,1-bis(diphenylphosphino)methane, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 2,2'-bis(diphenylphosphino)-1,1'-binaphthyl, and 1,1'-bis(diphenylphosphino)ferrocene.
[0089] In the general formula (2) above, a + b = 4, and a and b are integers from 0 to 4. For a, 0 to 3 is preferred, 0 to 2 is more preferred, 1 to 2 is even more preferred, and 2 is particularly preferred. For b, 2 to 4 is preferred, 2 or 3 is more preferred, and 2 is even more preferred. By setting a and b within the above ranges, the stability of the (A) metal compound can be increased.
[0090] Examples of the above (a) metal-containing compounds include titanium-containing compounds such as diisopropoxybis(2,4-pentanedione)titanium(IV), tetra-n-butoxytitanium(IV), tetra-n-propoxytitanium(IV), tri-n-butoxymonostearatetitanium(IV), titanium(IV) butoxide oligomer, aminopropyltrimethoxytitanium(IV), triethoxymono(2,4-pentanedione)titanium(IV), and tri-n-propoxymono(2,4-pentanedione) Examples include titanium(IV), triisopropoxymono(2,4-pentanedione)titanium, di-n-butoxybis(2,4-pentanedione)titanium(IV), and zirconium-containing compounds such as dibutoxybis(ethylacetate)zirconium(IV), di-n-butoxybis(2,4-pentanedione)zirconium(IV), tetra-n-butoxyzirconium(IV), tetra-n-propoxyzirconium(IV), and tetraisopropoxyzirconium(IV). V), aminopropyltriethoxyzirconium(IV), 2-(3,4-epoxycyclohexyl)ethyltrimethoxyzirconium(IV), γ-glycidoxypropyltrimethoxyzirconium(IV), 3-isocyanopropyltrimethoxyzirconium(IV), triethoxymono(2,4-pentanedione)zirconium(IV), trin-propoxymono(2,4-pentanedione)zirconium(IV), triisopropoxymono(2,4-pentanedione) Examples of hafnium-containing compounds include zirconium(IV), tri(3-methacryloxypropyl)methoxyzirconium(IV), tri(3-acryloxypropyl)methoxyzirconium(IV), and hafnium-containing compounds include diisopropoxybis(2,4-pentanedione)hafnium(IV), tetrabutoxyhafnium(IV), tetraisopropoxyhafnium(IV), tetraethoxyhafnium(IV), and dichlorobis(cyclopentadienyl)hafnium(IV).
[0091] From the viewpoint of obtaining good raw materials, it is preferable that the metal compound represented by formula (2) has the structure of formula (3) below. [ka] (In the formula, M is Ti, Zr, or Hf, and R 1A (It is a monovalent organic group with 1 to 20 carbon atoms.)
[0092] In the above equation (3), R 1A The group is a monovalent organic group having 1 to 20 carbon atoms, preferably a methyl group, ethyl group, n-propyl group, i-propyl group, n-butyl group, or t-butyl group, and more preferably an isopropyl group, n-butyl group, or t-butyl group.
[0093] [(b) Ligand-forming compound] In the synthesis reaction of a metal-containing film-forming compound, in addition to (a) a metal-containing compound and a polydentate ligand containing a cyclic ether structure with 2 to 13 carbon atoms, a compound that can become a monodentate or polydentate ligand in the metal-containing film-forming compound (hereinafter referred to as (b) ligand-forming compound) may also be added.
[0094] As for the ligand-forming compounds in (b) above, in addition to organic compounds derived from hydroxyl ligands, carboxyl ligands, amide ligands, amine ligands, ammonia ligands, olefin ligands, etc., as listed as L in formula (2) above, organic compounds derived from hydroxy acid esters, β-diketone ligands, β-ketoester ligands, α,α-dicarboxylic acid ester ligands, etc., compounds having multiple hydroxyl groups things etc. These are some examples.
[0095] Furthermore, (b) the ligand-forming compound may be an organic compound having 1 to 30 carbon atoms that contains at least one bridging group represented by any of the following general formulas (c-1) to (c-4), (d-1) to (d-4), and (e-1) to (e-3).
[0096] [ka] (In the above general formulas (c-1) to (c-4), R c (where is a hydrogen atom or a monovalent organic group with 1 to 10 carbon atoms, q represents 0 or 1, and * represents a bond.) [ka] (In the above general formula, R d1 R is a hydrogen atom or a methyl group, and in the same formula they may be the same or different from each other. d2 (where * represents a hydrogen atom, a substituted or unsubstituted saturated or unsaturated monovalent organic group having 1 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms, and * represents a bond.) [ka] (In the above general formulas (e-1) to (e-3), Y e R is a divalent organic group having 1 to 31 carbon atoms, preferably 1 to 20 carbon atoms, e2 R is a hydrogen atom, a substituted or unsubstituted monovalent organic group having 1 to 20 carbon atoms in a saturated state or 2 to 20 carbon atoms in an unsaturated state, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms. e1 This refers to an organic group represented by the following general formula (e-4) in which a protecting group is removed by the action of either an acid, heat, or both, generating one or more hydroxyl groups or carboxyl groups, where * represents a bond. [ka] (In the above general formula (e-4), R e3 * is an organic group whose protecting group is removed by the action of acid, heat, or both, and * is Y e (This represents the connection point.)
[0097] (b) The ligand-forming compound contains at least one crosslinking group as indicated in (c-1) to (c-4), (d-1) to (d-4), and (e-1) to (e-3) above, so that sufficient thermal fluidity can be obtained during film formation, and when used in a metal-containing film-forming composition, a metal-containing film with excellent flatness can be formed.
[0098] From the viewpoint of productivity and stability of metal-containing film-forming compounds, the above (b) ligand-forming compounds are compounds derived from carboxyl ligands, compounds derived from β-diketone ligands, and compounds having multiple hydroxyl groups. things More preferable. These can be used individually or in combination of two or more.
[0099] Examples of compounds derived from carboxyl ligands include the compound shown in formula (5) below. [ka] (In the above general formula (5), p is either 0 or 1. If p is 1, X 1 is a divalent organic group having 2 to 20 carbon atoms, and W is an alkoxy group having 1 to 10 carbon atoms, one of the following general formulas (5-A) or (d-1) to (d-4). When p is 0, X 1 This is a monovalent organic group having 8 to 30 carbon atoms that contains a bridging group and an aromatic ring, as shown in any of the general formulas (c-2) to (c-4) above. [ka] (In the above general formula (5-A), Y is a divalent organic group having 1 to 20 carbon atoms and saturated or 2 to 20 carbon atoms and unsaturated, R A (c-1) represents one of the structures shown in the general formulas (c-1) to (c-4) above, where h represents 1 to 6, and * represents the bond with the carbonyl atom.)
[0100] If the compound is derived from a carboxyl ligand with such a structure, the thermosetting properties of the metal-containing film-forming compound are improved, and a metal-containing film with excellent mixing resistance with the resist upper layer can be formed.
[0101] In the above general formula (5), it is preferable that p is 1 and W has the structure shown in the following general formula (5-B). [ka] (In the above general formula (5-B), R A1This is the structure shown by the general formula (c-1) above, and R A2 is one of the structures represented by the above general formula (c-2) or (c-3), Z is either an oxygen atom or a secondary amine, and L 1 R is a divalent hydrocarbon group having 1 to 10 carbon atoms. A3 (where is a monovalent organic group with 1 to 20 carbon atoms, saturated or unsaturated with 2 to 20 carbon atoms; t is 1 to 6, s is 0 to 5, t+s is 1 to 6, r is 1 to 10, u is 0 or 1, m is 0 or 1, and * represents the bond with the carbon atom of the carbonyl group.)
[0102] If the compound is derived from a carboxyl ligand with this structure, the heat resistance of the metal-containing film-forming compound is improved, resulting in a metal-containing film that exhibits excellent film-forming properties. Furthermore, the generation of sublimation during heat curing is suppressed, preventing contamination of the equipment.
[0103] In the above general formula (5), p is 1, W is an alkoxy group having 1 to 10 carbon atoms, and X 1 It is preferable that the structure is one of those represented by the following general formula (5-C).
[0104] [ka] (In the formula, * represents a connection.)
[0105] If the compound is derived from a carboxyl ligand with this structure, the heat resistance of the metal-containing film-forming compound is improved, resulting in a metal-containing film that exhibits excellent film-forming properties. Furthermore, the generation of sublimation during heat curing is suppressed, preventing contamination of the equipment.
[0106] Alternatively, in the general formula (5) above, p is 0 and X 1 It is preferable that the structure is one of those represented by the following general formula (5-D).
[0107] [ka] (In the above general formula (5-D), Rf This is the same as Rc in the general formula (c-2) or (c-3) above, and * represents the bond with the carbonyl atom.
[0108] Examples of compounds derived from carboxyl ligands include the compound shown in formula (6) below. [ka] (In the above general formula (6), X 2 R is a divalent organic group having 1 to 31 carbon atoms. 6A (This is one of the general formulas (e-1) to (e-3) above.)
[0109] In the above general formula (6), X 2 The group is a divalent organic group having 1 to 31 carbon atoms, and from the viewpoint of thermosetting properties, it is more preferable to be a saturated hydrocarbon having 1 to 20 carbon atoms or an unsaturated hydrocarbon having 2 to 20 carbon atoms.
[0110] In the above general formulas (e-1) to (e-3), Y e Y is a substituted or unsubstituted saturated or unsaturated divalent organic group having 1 to 20 carbon atoms, a substituted or unsubstituted aryl group having 6 to 30 carbon atoms, or a substituted or unsubstituted arylalkyl group having 7 to 31 carbon atoms. e It is preferable that the hydrocarbon is a saturated hydrocarbon having 1 to 20 carbon atoms or an unsaturated hydrocarbon having 2 to 20 carbon atoms.
[0111] In the above general formulas (e-1) to (e-3), Y e If the hydrocarbon is a saturated hydrocarbon with 1 to 20 carbon atoms or an unsaturated hydrocarbon with 2 to 20 carbon atoms, the thermosetting properties of the metal-containing film-forming compound can be further improved. This is also preferable from the standpoint of raw material availability.
[0112] Y e The following structures are examples of this, but are not limited to these. [ka] (*1 is a bond with an oxygen atom or nitrogen atom, and *2 is Re1 (This represents the connection point.)
[0113] In the above general formula (e-4), R e3 Protecting groups (thermally acid-unstable groups) are affected by either acid, heat, or both. ) organic that detaches Based The group is preferably a tertiary hydrocarbyl group or a group that forms an acetal structure with an adjacent oxygen atom, with the tertiary hydrocarbyl group being particularly preferred. The tertiary hydrocarbyl group is preferably one having 4 to 20 carbon atoms, and among these, one with fewer carbon atoms is more preferred.
[0114] Examples of compounds derived from β-diketone ligands include the compound shown in formula (7). [ka] (In the above general formula, R 7A ~R 7c This is a monovalent organic group having 1 to 20 carbon atoms, which may contain a hydrogen atom or a bridging group represented by any of the general formulas (c-1) to (c-4) and (d-1) to (d-4) above.
[0115] The compound of general formula (7) above preferably contains at least one crosslinking group represented by any of the general formulas (c-1) to (c-4) and (d-1) to (d-4). Such a compound is preferable because it can further improve the thermosetting properties of the metal-containing film-forming compound.
[0116] Examples of compounds having multiple hydroxyl groups include dihydric alcohols represented by any of the formulas (7-A) to (7-C). [ka] (In the above general formula, R 7a ~R 7b R is a monovalent organic group having 1 to 20 carbon atoms, which may contain a hydrogen atom or a bridging group represented by any of the above general formulas (c-1) to (c-4), 7c ~R7f is a hydrogen atom or the above A monovalent organic group having 1 to 20 carbon atoms, which may contain a bridging group represented by any of the general formulas (c-1) to (c-4) and (d-1) to (d-4), Y 2 R is a divalent organic group having 1 to 10 carbon atoms. In the general formula (7-A) above, adjacent R 7a and R 7b These elements may bond to each other, forming unsaturated or saturated ring structures.
[0117] The compounds of the above general formulas (7-A) to (7-C) preferably contain at least one crosslinking group represented by any of the above general formulas (c-1) to (c-4) and (d-1) to (d-4). Such compounds are preferable because they can further improve the thermosetting properties of the metal-containing film-forming compound.
[0118] (b) In the metal-containing film-forming compound, the content of polydentate ligands including a cyclic ether structure having 2 to 13 carbon atoms is preferably 10 mol% to 100 mol%, more preferably 20 mol% to 90 mol%, and even more preferably 25 mol% to 75 mol% of the total amount of ligands coordinating to the metal atom. (b) The content of ligands derived from the ligand-forming compound is preferably 0 mol% to 50 mol%, more preferably 0 mol% to 25 mol% of the total amount of ligands coordinating to the metal atom. (b) Ligands other than those derived from the ligand-forming compound, for example, ligands derived from alkoxy groups having 1 to 10 carbon atoms, are preferably 0 mol% to 90 mol%, more preferably 0 mol% to 75 mol% of the total amount of ligands coordinating to the metal atom.
[0119] [(c) Silicon-containing compound] Furthermore, in the synthesis reaction of the metal-containing film-forming compound, (c) a silicon-containing compound may be added in addition to the polydentate ligand containing a cyclic ether structure with 2 to 13 carbon atoms.
[0120] (a) By substituting the hydrolyzable groups of the metal-containing compound with a silicon-containing compound, the stability of the metal-containing film-forming compound in the metal-containing film-forming composition can be improved.
[0121] Examples of silicon-containing compounds include structures represented by the following general formula (4). [ka] (In the above general formula (4), R 3A , R 3B and R 3C This is one of the following organic groups selected from a C1-C30 organic group having a bridging group in any of the structures shown in the general formulas (b-1) to (b-3) below, a substituted or unsubstituted C1-C20 alkyl group, and a C1-C20 aryl group. [ka] (In the general formulas (b-1) to (b-3) above, R3 is hydrogen or a monovalent organic group having 1 to 10 carbon atoms, q represents 0 or 1, and * represents a bond.)
[0122] As for the silicon-containing compound, any of the following groups is more preferred, and trimethylsilanol is more preferred from the viewpoint of productivity. [ka] (In the above formula, * represents the bond with the metal atom.)
[0123] When the metal-containing film-forming compound contains a polydentate ligand having a cyclic ether structure with 2 to 13 carbon atoms and a ligand derived from (c) a silicon-containing compound, the content of the polydentate ligand having a cyclic ether structure with 2 to 13 carbon atoms in the metal-containing film-forming compound is preferably 10 mol% to 100 mol%, more preferably 20 mol% to 80 mol%, and even more preferably 25 mol% to 75 mol% of the total amount of ligands coordinating to the metal atom. (c) Silicon-containing compound thingLigands derived from (c) are preferably present in an amount of 10 mol% to 90 mol%, more preferably 20 mol% to 80 mol%, and even more preferably 25 mol% to 75 mol% of the total amount of ligands coordinating to the metal atom. Polydentate ligands containing cyclic ether structures having 2 to 13 carbon atoms and ligands other than silicon-containing compounds, such as ligands derived from alkoxy groups having 1 to 10 carbon atoms, are preferably present in an amount of 0 mol% to 90 mol%, and more preferably 0 mol% to 75 mol% of the total amount of ligands coordinating to the metal atom.
[0124] [Synthesis method] When synthesizing the metal-containing film-forming compound of the present invention, the synthesis method is not particularly limited as long as the metal-containing film-forming compound contains a polydentate ligand containing a cyclic ether structure having 2 to 13 carbon atoms. For example, (a) a metal alkoxide or metal acetylacetonate (acac) can be used as the metal-containing compound, and it can be obtained by reacting the alkoxy or acac metal with a polydentate ligand containing a cyclic ether structure having 2 to 13 carbon atoms. (a) The metal-containing compound may be hydrolyzed and condensed before being reacted with a polydentate ligand containing a cyclic ether structure having 2 to 13 carbon atoms, or (a) the metal-containing compound may be reacted with a polydentate ligand containing a cyclic ether structure having 2 to 13 carbon atoms before hydrolyzation and condensation. If it is difficult to control the hydrolysis and condensation, the reaction may be carried out in a non-aqueous environment with a polydentate ligand containing a cyclic ether structure having 2 to 13 carbon atoms. These are preferably adjusted as appropriate according to the properties required for the metal-containing film-forming compound and the metal-containing film. (c) When a silicon-containing compound is to be used as a ligand with a polydentate ligand containing a cyclic ether structure having 2 to 13 carbon atoms, it is preferable to react (a) the metal-containing compound with (c) the silicon-containing compound first, and then react with the polydentate ligand containing a cyclic ether structure having 2 to 13 carbon atoms.
[0125] (a) A method for carrying out a hydrolysis condensation reaction using a metal-containing compound is, for example, to carry out a hydrolysis condensation reaction of the metal-containing compound in a solvent containing water. In this case, other compounds having hydrolyzable groups may be added as needed. Also, an acid such as acetic acid may be added as a catalyst for the hydrolysis condensation reaction. The lower limit of the amount of water used in this hydrolysis condensation reaction is preferably 0.2 moles, more preferably 1 mole, and even more preferably 3 moles, relative to the hydrolyzable groups of the metal-containing compound, etc. The upper limit of the amount of water is preferably 20 moles, more preferably 15 moles, and even more preferably 10 moles.
[0126] The solvent used in the synthesis reaction of the metal-containing film-forming compound is not particularly limited, and for example, solvents similar to those exemplified as (B) organic solvents described later can be used. Typical solvents and solvent mixtures include those containing ester, ether, or alcohol functional groups, for example, a mixture of 70 / 30 by volume of propylene glycol monomethyl ether acetate (PGMEA) and propylene glycol monomethyl ether (PGME). Examples of other solvents that can be used include butanediol monomethyl ether, ethylene glycol monomethyl ether, butanediol monoethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, butanediol monopropyl ether, propylene glycol monopropyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, propylene glycol monobutyl ether, 1-butanol, 2-butanol, 2-methyl-1-propanol, 4-methyl-2- PeExamples include ethanol, acetone, tetrahydrofuran, toluene, hexane, ethyl acetate, cyclohexanone, methyl amyl ketone, propylene glycol dimethyl ether, diethylene glycol dimethyl ether, diamyl ether, isoamyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, t-butyl acetate, t-butyl propionate, propylene glycol mono-t-butyl ether acetate, γ-butyrolactone, methyl isobutyl ketone, and cyclopentyl methyl ether.
[0127] <Metal-containing film forming composition> Furthermore, the present invention provides a metal-containing film-forming composition that contains (A) the metal-containing film-forming compound of the present invention and (B) an organic solvent.
[0128] <(A) Metal-containing film-forming compound> Component (A) in the metal-containing film-forming composition of the present invention is the metal-containing film-forming compound of the present invention described above. The amount of component (A) in the composition is not particularly limited, but for example, it can be 1 to 20 parts by mass, preferably 1 to 10 parts by mass, and more preferably 1 to 5 parts by mass, per 100 parts by mass of the total amount of the composition.
[0129] <(B) Organic solvents> The (B) organic solvent that can be used in the metal-containing film-forming composition of the present invention is not particularly limited as long as it dissolves the (A) metal-containing film-forming compound described above, as well as the (C) thermal acid generator, (D) photoacid generator, (E) crosslinking agent, (F) surfactant, and other additives described below, if included.
[0130] Specifically, for example, organic solvents described in paragraphs
[0091] to
[0092] of Japanese Patent Publication No. 2007-199653 can be added. More specifically, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, 2-heptanone, cyclopentanone, cyclohexanone, and γ-butyrolactone, or a mixture containing one or more of these, are preferably used.
[0131] The amount of organic solvent blended is preferably 200 to 10,000 parts, and more preferably 250 to 5,000 parts, per 100 parts by mass of (A) the metal-containing film-forming compound.
[0132] <High boiling point solvents> In the metal-containing film-forming composition of the present invention, the (B) organic solvent may include a high-boiling point organic solvent. The high-boiling point organic solvent may be one or more organic solvents with a boiling point of 180 degrees (°C) or higher.
[0133] For example, (B) may be a mixture of one or more organic solvents with a boiling point of less than 180°C and one or more organic solvents with a boiling point of 180°C or higher (high-boiling point solvents).
[0134] As for high-boiling point solvents, there are no particular restrictions on hydrocarbons, alcohols, ketones, esters, ethers, chlorinated solvents, etc., as long as they can dissolve each component of the metal-containing film-forming composition of the present invention. Specific examples include 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, 1-undecanol, ethylene glycol, 1,2-propylene glycol, 1,3-butylene glycol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 2,4-heptanediol, 2-ethyl-1,3-Hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerin, n-nonyl acetate, monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, diethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol monoisobutyl ether, diethylene glycol monohexyl ether, diethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, triethylene glycol monomethyl ether, triethylene glycol-n-butyl ether, triethylene glycol Dibutyl methyl ether, tetraethylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tripropylene glycol mono-n-propyl ether, tripropylene glycol mono-n-butyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, triacetin, propylene glycol diacetate, dipropylene glycol methyl-n-propyl ether, dipropylene glycol methyl ether acetate, 1,4-butanediol diacetate, 1,3-butylene glycol diacetate, 1,Examples include 6-hexanediol diacetate, triethylene glycol diacetate, γ-butyrolactone, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, dihexyl malonate, diethyl succinate, dipropyl succinate, dibutyl succinate, dihexyl succinate, dimethyl adipate, diethyl adipate, and dibutyl adipate, which may be used individually or in combination.
[0135] The high-boiling point solvent can be appropriately selected from the above, for example, according to the temperature at which the metal-containing film-forming composition of the present invention is heat-treated. The boiling point of the high-boiling point solvent is preferably 180°C to 300°C, and more preferably 200°C to 300°C. With such a boiling point, there is no risk of excessive volatilization during baking (heat treatment), thus suppressing the occurrence of defects caused by drying during film formation. Furthermore, with such a boiling point, the solvent does not remain in the film without volatilizing after baking, so there is no risk of adversely affecting film properties such as etching resistance.
[0136] Furthermore, when using a high-boiling-point solvent, the blending amount is preferably 1 to 30 parts by mass per 100 parts by mass of an organic solvent with a boiling point of less than 180°C. This blending amount is preferable because it provides sufficient thermal fluidity during baking, does not remain in the film, and does not lead to deterioration of film properties such as etching resistance.
[0137] <Other ingredients> If the metal-containing film-forming composition is a metal-containing film-forming composition that can be used as a resist underlayer film in a multilayer resist method, it only needs to contain one or more of the above-mentioned (A) metal-containing film-forming compounds and (B) organic solvents, and may optionally contain at least one of (C) a thermal acid generator, (D) a photoacid generator, (E) a crosslinking agent, and (F) a surfactant.
[0138] The following describes components that may be included in the metal-containing film-forming composition of the present invention, other than (A) the metal-containing film-forming compound and (B) the organic solvent mentioned above.
[0139] [(C) Thermal acid generator] In the metal-containing film-forming composition of the present invention, it is preferable to add (C) a thermal acid generator to promote the crosslinking reaction by heat.
[0140] Examples of thermal acid generators (C) that can be used in the metal-containing film-forming composition of the present invention include the following general formula (7).
[0141] [ka] (In the formula, X A - R represents a non-nucleophilic counterion. 70 , R 71 , R 72 , and R 73 Each represents a hydrogen atom or a linear, branched, or cyclic alkyl, alkenyl, oxoalkyl, or oxoalkenyl group having 1 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl or aryloxoalkyl group having 7 to 12 carbon atoms, and some or all of the hydrogen atoms of these groups may be substituted with alkoxy groups, etc. Also, R 70 and R 71 , or R 70 , R 71 and R 72 It may form a ring, and if a ring is formed, R 70 and R 71 , or R 70 , R 71 and R 72 This represents an alkylene group having 3 to 10 carbon atoms, or a heteroaromatic ring containing the nitrogen atom in the formula within the ring.
[0142] The above, R 70 , R 71 , R 72 , and R 73These groups may be the same or different from each other. Specifically, examples of alkyl groups include methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, octyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclopropylmethyl, 4-methylcyclohexyl, cyclohexylmethyl, norbornyl, and adamantyl groups.
[0143] Examples of alkenyl groups include vinyl, allyl, propenyl, butenyl, hexenyl, and cyclohexenyl groups.
[0144] Examples of oxoalkyl groups include 2-oxocyclopentyl group, 2-oxocyclohexyl group, 2-oxopropyl group, 2-cyclopentyl-2-oxoethyl group, 2-cyclohexyl-2-oxoethyl group, and 2-(4-methylcyclohexyl)-2-oxoethyl group.
[0145] Examples of oxoalkenyl groups include the 2-oxo-4-cyclohexenyl group and the 2-oxo-4-propenyl group.
[0146] Examples of aryl groups include phenyl groups, naphthyl groups, alkoxyphenyl groups such as p-methoxyphenyl, m-methoxyphenyl, o-methoxyphenyl, ethoxyphenyl, p-tert-butoxyphenyl, and m-tert-butoxyphenyl, alkylphenyl groups such as 2-methylphenyl, 3-methylphenyl, 4-methylphenyl, ethylphenyl, 4-tert-butylphenyl, 4-butylphenyl, and dimethylphenyl, alkylnaphthyl groups such as methylnaphthyl and ethylnaphthyl, alkoxynaphthyl groups such as methoxynaphthyl and ethoxynaphthyl, dialkylnaphthyl groups such as dimethylnaphthyl and diethylnaphthyl, and dialkoxynaphthyl groups such as dimethoxynaphthyl and diethoxynaphthyl.
[0147] Examples of the aralkyl group include a benzyl group, a phenylethyl group, a phenethyl group, and the like.
[0148] Examples of the aryloxyalkyl group include 2-aryl-2-oxoethyl groups such as 2-phenyl-2-oxoethyl group, 2-(1-naphthyl)-2-oxoethyl group, 2-(2-naphthyl)-2-oxoethyl group, and the like.
[0149] Further, R 70 and R 71 , or R 70 , R 71 and R 72When the nitrogen atom in the formula forms a heteroaromatic ring within the ring, the derivatives include imidazole derivatives (e.g., imidazole, 4-methylimidazole, 4-methyl-2-phenylimidazole, etc.), pyrazole derivatives, furazan derivatives, pyrroline derivatives (e.g., pyrroline, 2-methyl-1-pyrroline, etc.), pyrrolidine derivatives (e.g., pyrrolidine, N-methylpyrrolidine, pyrrolidinone, N-methylpyrrolidone, etc.), imidazoline derivatives, imidazolidine derivatives, and pyridine derivatives (e.g., pyridine, methylpyridine, ethylpyridine, propylpyridine, butylpyridine, 4-(1-butylpentyl)pyridine, dimethylpyridine, trimethylpyridine, triethylpyridine, phenylpyridine, 3-methyl-2-phenylpyridine, 4-tert-butylpyridine, diphenylpyridine, benzylpyridine, methoxypyridine, butoxypyridine, dimethoxypyridine, 1-methyl-2-phenyl Examples include lidone, 4-pyrrolidinopyridine, 1-methyl-4-phenylpyridine, 2-(1-ethylpropyl)pyridine, aminopyridine, dimethylaminopyridine, etc., pyridazine derivatives, pyrimidine derivatives, pyrazine derivatives, pyrazoline derivatives, pyrazolidine derivatives, piperidine derivatives, piperazine derivatives, morpholine derivatives, indole derivatives, isoindole derivatives, 1H-indazole derivatives, indoline derivatives, quinoline derivatives (e.g., quinoline, 3-quinoline carbonitride, etc.), isoquinoline derivatives, sinnoline derivatives, quinazoline derivatives, quinoxaline derivatives, phthalazine derivatives, purine derivatives, pteridine derivatives, carbazole derivatives, phenanthridine derivatives, acridine derivatives, phenazine derivatives, 1,10-phenanthroline derivatives, adenine derivatives, adenosine derivatives, guanine derivatives, guanosine derivatives, uracil derivatives, uridine derivatives, etc.
[0150] The above, X A -Examples of the non-nucleophilic counter ion include halide ions such as chloride ion and bromide ion, fluoroalkylsulfonates such as triflate, 1,1,1-trifluoroethanesulfonate, and nonafluorobutanesulfonate, arylsulfonates such as tosylate, benzenesulfonate, 4-fluorobenzenesulfonate, and 1,2,3,4,5-pentafluorobenzenesulfonate, alkylsulfonates such as mesylate and butanesulfonate, imidic acids such as bis(trifluoromethylsulfonyl)imide, bis(perfluoroethylsulfonyl)imide, and bis(perfluorobutylsulfonyl)imide, methide acids such as tris(trifluoromethylsulfonyl)methide and tris(perfluoroethylsulfonyl)methide, as well as sulfonates with fluorine substitution at the α-position represented by the following general formula (8), and sulfonates with fluorine substitution at the α and β positions represented by the following general formula (9).
[0151]
Chemical Formula
[0152] In the above general formula (8), R 81 is a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 23 carbon atoms, an acyl group, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aryloxy group. In the above general formula (9), R 91 is a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms.
[0153] Specific examples of the above thermal acid generator include, but are not limited to, the following compounds.
[0154]
Chemical Formula
[0155] The (C) thermal acid generator contained in the metal-containing film-forming composition of the present invention can be used alone or in combination of two or more types. The amount of thermal acid generator added is preferably 0.05 to 30 parts, more preferably 0.1 to 10 parts, per 100 parts of the (A) metal-containing film-forming compound. If the amount is 0.05 parts or more, the amount of acid generated and the crosslinking reaction will be sufficient, and if it is 30 parts or less, there is little risk of mixing occurring due to the migration of acid to the upper resist layer.
[0156] [(D) Photoacid Generator] The metal-containing film-forming composition of the present invention may contain (D) a photoacid generator to appropriately adjust the pattern shape, exposure sensitivity, etc., of the resist upper layer film. One type of photoacid generator may be used alone or in combination of two or more types.
[0157] As the photoacid generator, for example, the one described in paragraphs
[0160] to
[0179] of Japanese Patent Publication No. 2009-126940 can be used. The amount of photoacid generator added is preferably 0.05 to 30 parts, more preferably 0.1 to 10 parts, per 100 parts of the above (A) metal-containing film-forming compound. If the amount of photoacid generator added is within the above range, the resolution will be good and there will be no risk of foreign matter problems occurring after resist development or during peeling.
[0158] [(E) Crosslinking agent] Furthermore, the metal-containing film-forming composition of the present invention may also contain (E) a crosslinking agent in order to enhance curability and further suppress intermixing with the resist upper layer film.
[0159] The crosslinking agent is not particularly limited, and a wide variety of known crosslinking agents can be used. Examples include melamine-based crosslinking agents, glycoluryl-based crosslinking agents, benzoguanamine-based crosslinking agents, urea-based crosslinking agents, β-hydroxyalkylamide-based crosslinking agents, isocyanurate-based crosslinking agents, aziridine-based crosslinking agents, oxazoline-based crosslinking agents, epoxy-based crosslinking agents, and phenol-based crosslinking agents. The above (E) crosslinking agents can be used individually or in combination of two or more. When adding a crosslinking agent, the amount added is preferably 5 to 50 parts, more preferably 10 to 40 parts, per 100 parts of the above (A) metal-containing film-forming compound. If the amount added is 5 parts or more, sufficient curability can be achieved and intermixing with the resist upper layer can be suppressed. On the other hand, if the amount added is 50 parts or less, there is no risk of deterioration of dry etching resistance due to a lower ratio of the (A) metal-containing film-forming compound in the composition.
[0160] Examples of melamine-based crosslinking agents include hexamethoxymethylated melamine, hexasubtoxicmethylated melamine, alkoxy and / or hydroxy-substituted derivatives thereof, and partially self-condensed derivatives thereof.
[0161] Examples of glycoluryl crosslinking agents include tetramethoxymethylated glycoluryl, tetrabutoxymethylated glycoluryl, their alkoxy and / or hydroxy substituted derivatives, and their partial self-condensates.
[0162] Examples of benzoguanamine-based crosslinking agents include tetramethoxymethylated benzoguanamine, tetrabutoxymethylated benzoguanamine, their alkoxy and / or hydroxy-substituted derivatives, and their partial self-condensed derivatives.
[0163] Examples of urea-based crosslinking agents include dimethoxymethylated dimethoxyethyleneurea, its alkoxy and / or hydroxy-substituted derivatives, and partially self-condensed derivatives thereof.
[0164] A specific example of a β-hydroxyalkylamide crosslinking agent is N,N,N',N'-tetra(2-hydroxyethyl)adipamide.
[0165] Examples of isocyanurate-based crosslinking agents include triglycidyl isocyanurate and triallyl isocyanurate.
[0166] Examples of aziridine-based crosslinking agents include 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane and 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate].
[0167] Examples of oxazoline-based crosslinking agents include 2,2'-isopropylidenebis(4-benzyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-methylenebis-4,5-diphenyl-2-oxazoline, 2,2'-methylenebis-4-phenyl-2-oxazoline, 2,2'-methylenebis-4-tertbutyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylenebis(2-oxazoline), 1,4-phenylenebis(2-oxazoline), and 2-isopropenyloxazoline copolymers.
[0168] Examples of epoxy crosslinking agents include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether.
[0169] Examples of phenolic crosslinking agents include compounds represented by the following general formula (10). [ka] (In the formula, Q is a single bond or q having 1 to 20 carbon atoms) 1 It is a valence hydrocarbon group. 16 is a hydrogen atom, or an alkyl group having 1 to 20 carbon atoms. q 1 (This is an integer between 1 and 5.)
[0170] Q is a single bond, or a q with 1 to 20 carbon atoms. 1 It is a valence hydrocarbon group. 1 R is an integer from 1 to 5, and is more preferably 2 or 3. Examples of Q include methane, ethane, propane, butane, isobutane, pentane, cyclopentane, hexane, cyclohexane, methylpentane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, benzene, toluene, xylene, ethylbenzene, ethylisopropylbenzene, diisopropylbenzene, methylnaphthalene, ethylnaphthalene, and eicosane. 16 The C1-C20 alkyl group is either a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Specific examples of alkyl groups having 1 to 20 carbon atoms include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, pentyl, isopentyl, hexyl, octyl, ethylhexyl, decyl, and eicosanyl groups, with hydrogen atoms or methyl groups being preferred.
[0171] As examples of compounds represented by the above general formula (10), the following compounds can be specifically cited. Among these, triphenolmethane, triphenolethane, 1,1,1-tris(4-hydroxyphenyl)ethane, and hexamethoxymethylated tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene are preferred from the viewpoint of improving the curability and uniformity of the adhesion film.
[0172] [ka]
[0173] [ka] (In the formula, R 16 (As stated above.)
[0174] [(F) Surfactants] The metal-containing film-forming composition of the present invention may contain (F) surfactants to improve the coatability in spin coating. One surfactant may be used alone or in combination of two or more surfactants.
[0175] As the surfactant, for example, those described in paragraphs
[0142] to
[0147] of Japanese Patent Publication No. 2009-269953 can be used. When adding a surfactant, the amount to add is preferably 0.001 to 20 parts, more preferably 0.01 to 10 parts, per 100 parts of the above (A) metal-containing film-forming compound. Within this range, the coatability is reliably improved, and a thin, uniform, and adhesive film can be formed.
[0176] [Plasticizer] Furthermore, a plasticizer may be added to the metal-containing film-forming composition of the present invention. The plasticizer is not particularly limited, and various known types of plasticizers can be widely used. Examples include low molecular weight compounds such as phthalates, adipicates, phosphates, trimelliticates, and citrates, as well as polymers such as polyethers, polyesters, and polyacetal polymers described in Japanese Patent Application Publication No. 2013-253227. The amount of plasticizer to be added is preferably 1% to 500% by mass per 100 parts of the metal-containing film-forming compound (A). When the amount added is within this range, excellent pattern embedding and averaging are achieved.
[0177] <Metal-containing film formation method> In the present invention, by using the above-described metal-containing film-forming composition, a metal-containing film can be formed, for example, as a resist underlayer for a multilayer resist film used in lithography.
[0178] In the method for forming a resist underlayer film using the metal-containing film-forming composition of the present invention, the aforementioned metal-containing film-forming composition is coated onto a substrate to be processed by a spin coating method or the like. After spin coating, the solvent is evaporated, and baking (heat treatment) is performed to prevent mixing with the resist upper layer film and to accelerate the crosslinking reaction. The baking is preferably performed at a temperature of 100°C to 450°C for 10 to 600 seconds, more preferably at 200°C to 300°C for 10 to 300 seconds. Considering the effects on device damage and wafer deformation, the upper limit of the heating temperature in the lithography wafer process is preferably 450°C or lower, more preferably 300°C or lower.
[0179] Further, in the method for forming a resist underlayer film using the metal-containing film-forming composition of the present invention, the metal-containing film-forming composition of the present invention is coated onto a substrate to be processed by a spin coating method or the like as described above, and the metal-containing film-forming composition is fired and cured in an atmosphere having an oxygen concentration of 0.1% by volume to 21% by volume, whereby a metal-containing film can also be formed.
[0180] By firing the metal-containing film-forming composition of the present invention in such an oxygen atmosphere, a sufficiently cured film can be obtained. The atmosphere during baking may be air, but enclosing an inert gas such as N₂, Ar, or He to reduce oxygen is preferable for preventing oxidation of the metal-containing film. To prevent oxidation, it is necessary to control the oxygen concentration, which is preferably 1000 ppm or less, more preferably 100 ppm or less (by volume). Preventing oxidation of the metal-containing film during baking is preferable because it does not cause an increase in absorption or a decrease in etching resistance.
[0181] Alternatively, using the aforementioned metal-containing film-forming composition, for example, a metal-containing film as an intermediate film of a multilayer resist film used in lithography can also be formed.
[0182] <Pattern Forming Method Using Metal-Containing Film-Forming Composition> Furthermore, the present invention provides a method for forming a pattern on a workpiece substrate using a two-layer resist process with the metal-containing film-forming composition of the present invention, (I-1) A step of forming a metal-containing film by applying the metal-containing film-forming composition of the present invention onto a substrate to be processed, and then heat-treating it. (I-2) A step of forming a resist upper layer film on the metal-containing film using a photoresist material, (I-3) After pattern exposure of the resist upper layer film, develop it with a developer to form a pattern on the resist upper layer film. (I-4) A step of transferring the pattern to the metal-containing film by dry etching using the resist upper layer film on which the pattern is formed as a mask, and (I-5) A step of processing the workpiece substrate using the metal-containing film on which the pattern is formed as a mask to form a pattern on the workpiece substrate. The present invention provides a pattern forming method characterized by having the following features.
[0183] Since the resist upper layer of the above two-layer resist process exhibits etching resistance to chlorine-based gases, it is preferable to perform dry etching of the metal-containing film using the resist upper layer as a mask in the above two-layer resist process using an etching gas mainly composed of chlorine-based gases. Since the metal-containing film exhibits etching resistance to fluorine-based gases, it is preferable to perform dry etching of the substrate to be processed using the metal-containing film as a mask using an etching gas mainly composed of fluorine-based gases.
[0184] Furthermore, the present invention provides a method for forming a pattern on a workpiece substrate using a three-layer resist process with the metal-containing film-forming composition of the present invention, (II-1) A step of forming a resist underlayer film on a substrate to be processed, (II-2) A step of forming a metal-containing film by applying the metal-containing film-forming composition of the present invention onto the resist underlayer film and then heat-treating it, (II-3) A step of forming a resist upper layer film on the metal-containing film using a photoresist material, (II-4) After pattern exposure of the resist upper layer film, develop it with a developer to form a pattern on the resist upper layer film. (II-5) A step of transferring the pattern to the metal-containing film by dry etching, using the resist upper layer film on which the pattern is formed as a mask. (II-6) A step of transferring the pattern to the resist underlayer film by dry etching, using the metal-containing film on which the pattern has been transferred as a mask. (II-7) A step of processing the substrate to be processed using the resist underlayer film on which the pattern is formed as a mask to form a pattern on the substrate to be processed, The present invention provides a pattern forming method characterized by having the following features.
[0185] Since the metal-containing film formed by the metal-containing film-forming composition of the present invention and used as an intermediate film in the above three-layer resist process exhibits etching resistance to oxygen-based gases, it is preferable to perform dry etching of the organic resist underlayer film, which is carried out using the metal-containing film as a mask, with an etching gas mainly composed of oxygen-based gases in the above three-layer resist process. Since the organic underlayer film exhibits etching resistance to fluorine-based gases, it is preferable to perform dry etching of the substrate to be processed, which is carried out using the organic underlayer film as a mask, with an etching gas mainly composed of fluorine-based gases.
[0186] In the pattern formation method described above, the resist upper layer film can be either positive or negative, and the same photoresist composition as commonly used can be used. When forming the resist upper layer film with the above photoresist composition, a spin coating method is preferred.
[0187] When forming a resist upper layer film using a photoresist composition by spin coating, pre-baking is performed after resist coating, preferably at 60-180°C for 10-300 seconds. Subsequently, exposure is performed according to a conventional method, followed by post-exposure baking (PEB) and development to obtain the resist pattern. The thickness of the resist upper layer film is not particularly limited, but 10-500 nm, and especially 20-400 nm, is preferred.
[0188] Examples of exposure light include high-energy rays with wavelengths of 300 nm or less, specifically far ultraviolet light, KrF excimer laser light (248 nm), ArF excimer laser light (193 nm), F2 laser light (157 nm), Kr2 laser light (146 nm), Ar2 laser light (126 nm), soft X-rays (EUV) in the 3-20 nm range, electron beams (EB), ion beams, and X-rays.
[0189] As a method for forming the pattern of the resist upper layer film described above, it is preferable to use photolithography with a wavelength of 5 nm to 300 nm, direct writing with an electron beam, nanoimprinting, or a combination thereof to form the pattern.
[0190] Furthermore, it is preferable that the development method in the pattern formation method be alkaline development or development with an organic solvent.
[0191] Next, etching is performed using the obtained resist pattern as a mask. For example, in a two-layer resist process, etching of the metal-containing film is performed using a chlorine-based gas with the upper resist pattern as a mask. This forms the metal-containing film pattern. Then, etching of the substrate to be processed is performed using the obtained metal-containing film pattern as a mask. Etching of the workpiece can be performed by conventional methods; for example, if the workpiece is SiO2, SiN, or a silica-based low-dielectric-constant insulating film, etching is performed mainly using a fluorocarbon-based gas.
[0192] The metal-containing films obtained using the metal-containing film-forming composition of the present invention have excellent etching resistance when these workpieces are etched.
[0193] Examples of organic resist underlayer materials that can be used for the above-mentioned resist underlayer include those already known as underlayers for the 3-layer resist method or the 2-layer resist method using a silicon resist composition. For example, see Japanese Patent Publication No. 2012-1687, Japanese Patent Publication No. 2012-77295, Japanese Patent Publication No. 2004-264710, Japanese Patent Publication No. 2005-043471, Japanese Patent Publication No. 2005-250434, Japanese Patent Publication No. 2007-293294, Japanese Patent Publication No. 2008-65303, and Japanese Patent Publication No. 2004-205 Japanese Patent Publication No. 685, Japanese Patent Publication No. 2007-171895, Japanese Patent Publication No. 2009-14816, Japanese Patent Publication No. 2007-199653, Japanese Patent Publication No. 2008-274250, Japanese Patent Publication No. 2010-122656, Japanese Patent Publication No. 2012-214720, Japanese Patent Publication No. 2014-29435, International Publication WO Examples of resins and compositions can be found in Japanese Patent Publication No. 2012 / 077640, International Publication No. WO2010 / 147155, International Publication No. WO2012 / 077640, International Publication No. WO2010 / 147155, International Publication No. WO2012 / 176767, Japanese Patent Publication No. 2005-128509, Japanese Patent Publication No. 2006-259249, Japanese Patent Publication No. 2006-259482, Japanese Patent Publication No. 2006-293298, Japanese Patent Publication No. 2007-316282, Japanese Patent Publication No. 2012-145897, Japanese Patent Publication No. 2017-119671, Japanese Patent Publication No. 2019-44022, and others.
[0194] The above-mentioned resist underlayer film can be formed on a substrate by a spin coating method or the like, similar to the photoresist composition, using, for example, a composition solution containing the above-mentioned organic resist underlayer film material. After forming the organic resist underlayer film by a spin coating method or the like, it is desirable to bake the film to evaporate the organic solvent. The bake temperature is preferably in the range of 100 to 600°C, and the bake time is preferably in the range of 10 to 300 seconds.
[0195] It is also possible to apply an organic hard mask formed by a CVD method or an ALD method instead of the above organic resist underlayer film material.
[0196] In the case of a three-layer resist process, dry etching of the metal-containing film is performed, for example, using a chlorine-based gas with the upper resist pattern as a mask. Thereby, a metal-containing film pattern is formed. Next, using the obtained metal-containing film pattern as a mask, the resist underlayer film is etched using an oxygen-based gas. Thereby, a resist underlayer film pattern is formed. Next, using the obtained organic resist underlayer film pattern as a mask, the substrate to be processed is subjected to etching processing.
[0197] The metal-containing film obtained from the metal-containing film-forming composition of the present invention is characterized by excellent etching resistance during etching of these resist underlayer films.
[0198] Note that the object to be processed (substrate to be processed) is not particularly limited, and substrates such as Si, α-Si, p-Si, SiO₂, SiN, SiON, W, TiN, Al, and those having a layer to be processed deposited on the substrate are used. As the layer to be processed, various Low-k films such as Si, SiO₂, SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si and their stopper films are used, and it can usually be formed to a thickness of 50 to 10,000 nm, particularly 100 to 5,000 nm. When forming the layer to be processed, materials different from each other are used for the substrate and the layer to be processed.
[0199] Here, an example of a pattern formation method using the above three-layer resist process will be explained with reference to Figure 1. In this example, first, as shown in Figure 1(A), an organic resist underlayer film 3 is formed on the workpiece layer 2 of a workpiece substrate 10 consisting of a substrate 1 and a workpiece layer 2 thereon using an organic resist underlayer film material. A metal-containing film 4 is then formed on the organic resist underlayer film 3 using the metal-containing film forming composition of the present invention, and a resist upper layer film 5 is formed on the metal-containing film 4 using a photoresist material. Next, as shown in Figure 1(B), the exposed portion 6 of the resist upper layer film is pattern-exposed. Then, as shown in Figure 1(C), the resist upper layer film is developed with a developer to form a resist upper layer film pattern 5a on the resist upper layer film. Next, as shown in Figure 1(D), the resist upper layer film on which pattern 5a is formed is used as a mask to transfer the pattern to the metal-containing film 4 by dry etching to obtain a metal-containing film pattern 4a. Next, as shown in Figure 1(E), the pattern 4a is transferred to the metal-containing film, which is used as a mask, and the pattern is transferred to the organic resist underlayer film by dry etching to obtain the organic resist underlayer film pattern 3a. Then, as shown in Figure 1(F), the workpiece layer 2 on the substrate 1 is processed using the organic resist underlayer film on which pattern 3a is formed as a mask, and pattern 2a is formed on the workpiece substrate 10.
[0200] Furthermore, an example of a pattern formation method using the above two-layer resist process will be explained with reference to Figure 2. In this example, first, as shown in Figure 2(G), a metal-containing film 4 is formed on the workpiece layer 2 of a workpiece substrate 10 consisting of a substrate 1 and a workpiece layer 2 thereon using the metal-containing film forming composition of the present invention, and a resist upper layer film 5 is formed on the metal-containing film 4 using a photoresist material. Next, as shown in Figure 2(H), the exposed portion 6 of the resist upper layer film is pattern-exposed. Then, as shown in Figure 2(I), the resist upper layer film is developed with a developer to form a resist upper layer film pattern 5a on the resist upper layer film. Next, as shown in Figure 2(J), the resist upper layer film on which pattern 5a is formed is used as a mask to transfer the pattern to the metal-containing film 4 by dry etching to obtain a metal-containing film pattern 4a. Then, as shown in Figure 2(K), the workpiece layer 2 on the substrate 1 is processed using the metal-containing film on which pattern 4a is formed as a mask to form a pattern 2a on the workpiece substrate 10. [Examples]
[0201] The present invention will be described in more detail below with reference to synthesis examples, comparative synthesis examples, examples, and comparative examples, but the present invention is not limited thereto.
[0202] [(A) Examples of synthesis of metal-containing film-forming compounds] In the following synthesis examples, the organic group raw materials G: (G1) to (G15) and the silicon-containing organic group raw materials H: (H1) to (H2) shown below were used.
[0203] The raw material groups G: (G1) to (G15) and H: (H1) to (H2) are shown below.
[0204] [ka]
[0205] [ka]
[0206] The following metal compounds were used as the metal source M. (M1): Titanium tetraisopropoxide (Sigma-Aldrich Corp, 377996) (M2):Hf(OBu)4:Hafnium(IV)n-butoxide (Sigma-Aldrich Corp, 667943) (M3):Zr(OBu)4:Zirconium(IV) tetrabutoxide (80% by mass 1-butanol solution) (Tokyo Chemical Industries, Ltd., Z0016)
[0207] [Synthesis Example 1] Synthesis of Metal-Containing Film-Forming Compound (A-1) Under a nitrogen atmosphere, 28.4 g of titanium tetraisopropoxide (M1) was dissolved in 50.0 g of 2-propanol, and while stirring, a 50.0 g solution of IPA in 2.7 g of deionized water was added dropwise over 2 hours at room temperature. 15.8 g of organic raw material group (G1) was added to the resulting solution and stirred at room temperature for 30 minutes. This solution was concentrated under reduced pressure at 30°C, then heated to 60°C, and continued under reduced pressure until no more distillate was observed. Once no distillate was observed, 120.0 g of PGMEA / PGME (weight ratio 70 / 30) solution was added, and the mixture was heated at 40°C under reduced pressure until no more IPA distilled, yielding a PGMEA / PGME solution of metal-containing film-forming compound (A-1).
[0208] [Synthesis of compounds (A-2) to (A-3)] Compounds (A-2) to (A-3) shown in Table 1 were obtained under the same reaction conditions as in Synthesis Example 1, except that the above-mentioned metal source M and compound group G were used in the amounts shown in Table 1.
[0209] [Table 1]
[0210] [Synthesis Example 2] Synthesis of Metal-Containing Film-Forming Compound (A-4) Under a nitrogen atmosphere, 47.9 g of zirconium(IV) tetrabutoxide (M3) was dissolved in 65.9 g of PGMEA / PGME (weight ratio 70 / 30) solution, and the reaction temperature was raised to 60°C while stirring. A mixture of 18.6 g of compound G4 suspended in 27.5 g of PGMEA / PGME (weight ratio 70 / 30) solution was added to the reaction system, and stirring was continued for 1 hour at a reaction temperature of 60°C. After cooling to room temperature, the resulting reaction solution was filtered through a 0.45 μm PTFE filter to obtain a PGMEA / PGME solution of the metal-containing film-forming compound (A-4).
[0211] [Synthesis of compounds (A-5) to (A-11)] Compounds (A-5) to (A-11) shown in Table 2 were obtained under the same reaction conditions as in Synthesis Example 2, except that the above-mentioned metal source M and compound group G were used in the amounts shown in Table 2.
[0212] [Table 2]
[0213] [Synthesis Example 3] Synthesis of Metal-Containing Film-Forming Compound (A-12) Under a nitrogen atmosphere, 12.0 g of zirconium(IV) tetrabutoxide (M3) was dissolved in 16.5 g of PGMEA / PGME (weight ratio 70 / 30) solution, and the reaction temperature was raised to 50°C while stirring. 6.8 g of compound H1 was then added dropwise to the solution. After the addition, the reaction temperature was increased to 60°C and stirring was continued for 2 hours. Next, a mixture of 5.0 g of compound G3 suspended in 6.8 g of PGMEA / PGME (weight ratio 70 / 30) solution was added to the reaction system, and stirring was continued at a reaction temperature of 60°C for 1 hour. After cooling to room temperature, the resulting reaction solution was filtered through a 0.45 μm PTFE filter to obtain a PGMEA / PGME solution of the metal-containing film-forming compound (A-12).
[0214] [Synthesis of compounds (A-13) to (A-14) and comparative examples (R-1) to (R-4)] Except for using the above-mentioned metal source M, compound group G, and compound group H in the amounts shown in Table 3, the compounds (A-13) to (A-14) and comparative examples (R-1) to (R-4) shown in Table 3 were obtained under the same reaction conditions as in Synthesis Example 3.
[0215] [Table 3]
[0216] Preparation of metal-containing film-forming compositions (MUL-1 to 19, comparative MUL-1 to 4) For the preparation of the metal-containing film-forming compositions, the above-mentioned metal-containing film-forming compounds (A-1) to (A-14), (AG1) as a thermal acid generator, (AG2) as a photoacid generator, (XL1) to (XL2) as a crosslinking agent, and (F1: ethylene glycol dibenzyl ether: boiling point 364°C) as a high-boiling point solvent were used. After dissolving them in organic solvents in the proportions shown in Table 4, the metal-containing film-forming compositions (MUL-1 to 19, comparative MUL-1 to 4) were prepared by filtration through a 0.1 μm fluororesin filter.
[0217] [ka]
[0218] [Table 4]
[0219] [Example 1: Contact Angle Evaluation] The metal-containing film-forming compositions prepared above (MUL-1 to 19, comparative examples MUL-1 to 4) were applied to a silicon substrate and baked at 250°C for 60 seconds to produce metal-containing films with a thickness of 45 nm. The contact angle (CA1) with pure water was measured for each cured film. The results are shown in Table 5 below.
[0220] [Table 5]
[0221] As shown in Table 5, all of the metal-containing film-forming compositions of the present invention (MUL-1 to 19) having a cyclic ether structure form films with a contact angle of more than 60° with respect to pure water, indicating that good adhesion to the resist pattern can be expected. In particular, it was found that the metal-containing film-forming compositions using compounds with epoxy or oxetane structures had high contact angles. Furthermore, it was found that the contact angles of Examples 1-15 and 1-17 to 1-18, which used compositions containing a thermal acid generator (AG1), were also high. Although the effect is not clear, it is presumed that the hardening by ring-opening reaction of the epoxy or oxetane structure was accelerated by the action of the acid generator. On the other hand, the comparative metal-containing film-forming compositions that do not have a cyclic ether structure (Comparative Examples MUL-1 to MUL-4) showed low contact angles, suggesting that their adhesion to the resist pattern is insufficient.
[0222] [Example 2: Evaluation of optical constants (n / k)] Metal-containing film-forming compositions (MUL-2 to 19, comparative examples MUL-1 to 4) were applied to a silicon substrate and fired at 250°C for 60 seconds. The optical constants (refractive index n, extinction coefficient k) at a wavelength of 193 nm were then determined using a variable-angle spectroscopic ellipsometer (VASE) manufactured by JA Woolam, and the results are shown in Table 6.
[0223] [Table 6]
[0224] As shown in Table 6, the metal-containing film-forming compositions of the present invention (MUL-2 to 19) containing hafnium and zirconium all had n values of 1.8 or higher and k values between 0.1 and 0.5. While the optical constants depend on the film thickness, the type of upper film, etc., generally, if the n value is between 1.8 and 2.3 and the k value is between 0.1 and 0.5, even when forming a metal-containing film with a thin film of 20 nm or less, reflected light from the substrate during ArF immersion high-NA exposure can be suppressed to a considerable extent, making it applicable as an underlayer film for photoresist patterning. In the above examples, the optical constants are all within a suitable range, indicating that they are applicable as underlayer films for photoresist patterning. On the other hand, Comparative Examples 2-3 and 2-4 have n values of 1.8 or lower, possibly due to the large amount of organic components in the metal-containing film, suggesting insufficient suppression of reflected light from the substrate during ArF immersion high-NA exposure.
[0225] [Example 3: Etching resistance evaluation] A metal-containing film-forming composition (MUL-1 to 19, and Comparative Examples MUL-1 to 4) was applied to a silicon substrate and heated at 250°C for 60 seconds using a hot plate to form a metal-containing film with a thickness of 50 nm (film thickness a). In Comparative Examples 3-5, the silicon atom-containing resist interlayer material (SOG-1) described below was applied and baked at 220°C for 60 seconds to form a resist interlayer with a thickness of 50 nm.
[0226] As a silicon atom-containing resist interlayer material (SOG-1), a polymer represented by ArF silicon-containing interlayer polymer (SiP1) and a thermal crosslinking catalyst (CAT1) were dissolved in a solvent containing 0.1% by mass of FC-4430 (manufactured by Sumitomo 3M Co., Ltd.) in the proportions shown in Table 7, and the mixture was filtered through a fluororesin filter with a pore size of 0.1 μm to prepare the silicon atom-containing resist interlayer material (SOG-1).
[0227] [Table 7]
[0228] The structural formulas of the ArF silicon-containing interlayer polymer (SiP1) and thermal crosslinking catalyst (CAT1) used are shown below. [ka]
[0229] In Comparative Example 3-6, the following organic resist underlayer material (SOC-1) was applied and baked at 350°C for 60 seconds to form a resist underlayer with a thickness of 50 nm.
[0230] For the organic resist underlayer film material (SOC-1), the polymer represented by organic underlayer film polymer (CP1) was dissolved in a solvent containing 0.1% by mass of FC-4430 (manufactured by Sumitomo 3M Co., Ltd.) in the proportions shown in Table 8, and the mixture was filtered through a fluororesin filter with a pore size of 0.1 μm to prepare the organic resist underlayer film material (SOC-1).
[0231] [Table 8]
[0232] The structural formula of the organic underlayer polymer (CP1) used is shown below. [ka] Mw = 7,000, Mw / Mn = 3.50
[0233] Next, etching was performed using CF4 gas and O2 gas under the following conditions with a ULVAC CE-300I etching system, and the film thickness b was measured. The etching rate (nm / min) was calculated from the film thickness etched per minute (film thickness b - film thickness a) over a specified time using each gas.
[0234] The etching rate for CF4 gas was judged as "A (Excellent)" if it was 20 nm / min or less, "B (Good)" if it was between 20 nm / min and 30 nm / min, and "C (Poor)" if it was 30 nm / min or more. The results are shown in Table 9.
[0235] The etching rate for O2 gas was judged as "A (Excellent)" if it was 20 nm / min or less, "B (Good)" if it was between 20 nm / min and 30 nm / min, and "C (Poor)" if it was 30 nm / min or more. The results are shown in Table 9.
[0236] Dry etching conditions with CF4 gas Pressure: 3 Pa Antenna RF power: 100W Bias RF Power: 15W CF4 gas flow rate: 15 sccm Time: 30sec
[0237] Dry etching conditions using O2 gas Pressure: 3 Pa Antenna RF power: 300W Bias RF Power: 10W O2 gas flow rate: 25 sccm Time: 30sec
[0238] [Table 9]
[0239] As shown in Table 9, the metal-containing film-forming compositions (MUL-1 to MUL-19) of the present invention were found to exhibit excellent etching resistance to CF4 gas and O2 gas. Compared to SOG-1 used in Comparative Example 3-5, O Because it exhibits excellent resistance to etching using two gases, it is suitable for a three-layer resist process in which a resist pattern is transferred to a substrate in combination with an organic resist underlayer film. Compared to SOC-1 used in Comparative Example 3-6, it exhibits superior etching resistance to CF4 gas, making it suitable for a two-layer resist process in which a resist pattern is transferred to a substrate in combination with a photoresist upper layer film.
[0240] [Example 4: Pattern Forming Method] Using the above-mentioned SOC-1 as an organic underlayer on a substrate, a carbon film with a thickness of 60 nm was fabricated by spin coating onto a Si wafer and baking at 350°C for 60 seconds. The carbon ratio of the carbon film was 46 atomic%, and the optical constant (n / k) at a wavelength of 193 nm was 1.42 / 0.50. A composition prepared by diluting a metal-containing film-forming composition (MDL-3 to 19, and comparative examples MDL-1 to 4) with an organic solvent (PGMEA / PGME = 700 / 300 parts by mass) was applied on top of the carbon film, and heated at 250°C for 60 seconds using a hot plate. death, A 15 nm thick resist interlayer was formed. An ArF single-layer resist, which is a resist top layer material, was applied on top of it and baked at 105°C for 60 seconds to form a 100 nm thick photoresist film. An immersion protective film material (TC-1) was applied on top of the photoresist film and baked at 90°C for 60 seconds to form a 50 nm thick protective film.
[0241] The resist upper layer material (single-layer resist for ArF) was prepared by dissolving a polymer (RP1), an acid generator (PAG1), and a basic compound (Amine1) in the proportions shown in Table 10 in a solvent containing 0.1% by mass of the surfactant FC-4430 (manufactured by Sumitomo 3M Co., Ltd.), and filtering the mixture through a 0.1 μm fluororesin filter.
[0242] [Table 10]
[0243] The polymer (RP1), acid generator (PAG1), and basic compound (Amine1) used in the resist upper layer material (single-layer resist for ArF) are shown below. [ka]
[0244] The immersion protective film material (TC-1) was prepared by dissolving the protective film polymer (PP1) in an organic solvent in the proportions shown in Table 11 and filtering it through a 0.1 μm fluororesin filter.
[0245] [Table 11]
[0246] The protective film polymer (PP1) used in the immersion protective film material (TC-1) is shown below. [ka]
[0247] Next, the sample was exposed using an ArF immersion lithography system (Nikon Corporation; NSR-S610C, NA 1.30, σ 0.98 / 0.78, 35-degree dipole s polarized illumination, 6% halftone phase shift mask), baked (PEB) at 100°C for 60 seconds, and developed with a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution for 30 seconds to obtain a 50 nm 1:1 positive-type line-and-space pattern (resist upper layer pattern).
[0248] Reflectance calculations were performed using PROLITH 2020a (Lithotech Japan Co., Ltd.). Figure 3 shows the results of calculating the reflectance for the metal-containing film with a fixed thickness of 10 nm, where n is 1.60 to 2.20 and k is 0.15 to 0.50. Optical constants (n / k) that can reduce reflected light from the substrate during pattern exposure to 1.0% or less are preferred. The pattern cross-section was observed using an S-4700 (Hitachi, Ltd. electron microscope). The results are shown in Table 12.
[0249] Next, a hard mask pattern was formed by dry etching, using the resist upper layer pattern as a mask to etch the resist interlayer. The resulting hard mask pattern was then used as a mask to etch the organic underlayer to form a pattern. Finally, the resulting resist underlayer pattern was used as a mask to etch the SiO2 film. The etching conditions are as follows.
[0250] The pattern cross-section was observed using an S-4700 electron microscope (Hitachi, Ltd.). The results are shown in Table 12.
[0251] Transfer conditions for hard mask patterns to metal-containing films (resist interlayers). Dry etching conditions with Cl2 gas Pressure: 1 Pa Antenna RF power: 320W Bias RF Power: 30W Cl2 gas flow rate: 25 sccm Time: 15sec
[0252] Transfer conditions for resist interlayer patterns to organic underlayers. Dry etching conditions using O2 gas Pressure: 1 Pa Antenna RF power: 300W Bias RF Power: 10W O2 gas flow rate: 25 sccm Time: 20sec
[0253] Transfer conditions for resist underlayer film patterns onto SiO2 film. Dry etching conditions with CF4 gas Pressure: 1 Pa Antenna RF power: 100W Bias RF Power: 15W CF4 gas flow rate: 15 sccm Time: 60sec
[0254] [Table 12]
[0255] As shown in Table 12, all of the metal-containing film-forming compositions of the present invention (MUL-3 to 19) were confirmed to have good pattern shapes after development. It is presumed that the metal-containing film material of the present invention, because it contains a cyclic ether structure, has high adhesion to the resist pattern and has optical constants that can sufficiently reduce substrate reflected light during pattern exposure, thus resulting in a good resist pattern. Furthermore, after etching following substrate transfer, the resist upper layer film pattern was successfully transferred to the substrate, confirming that it is suitable for use in microfabrication using the multilayer resist method. In contrast, the metal-containing film-forming compositions (Comparative Examples MUL-1 to 4), which showed low contact angles in the contact angle evaluation of Example 1, exhibited collapse of the resist upper layer film pattern after development.
[0256] Based on the above, the metal-containing film-forming compound, the composition using the compound, and the pattern-forming method of the present invention have high adhesion to the resist upper layer film pattern and have an effect of suppressing the collapse of fine patterns, and also provide a highly rectangular pattern shape for the resist upper layer film. Therefore, they are particularly suitable for use in multilayer resist processes and are extremely useful in fine patterning for semiconductor device manufacturing.
[0257] This specification includes the following inventions:
[0258] [1]: A metal-containing film-forming compound, characterized in that the metal-containing film-forming compound comprises at least one metal atom selected from the group consisting of Ti, Zr, and Hf, and a polydentate ligand having a cyclic ether structure with 2 to 13 carbon atoms that coordinates to the metal atom.
[0259] [2]: The metal-containing film-forming compound according to [1] above, characterized in that the polydentate ligand has a structure represented by the following general formulas (1-A) to (1-D). [ka] (In the above general formulas (1-A) to (1-D), R1 to R4 are monovalent organic groups having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms; R5 to R6 are monovalent organic groups having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms; and R7 to R 10 R is a monovalent organic group having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms. 11 R is a monovalent organic group having 1 to 20 carbon atoms, which may contain a cyclic ether structure having 2 to 13 carbon atoms, and Y is a divalent organic group having 1 to 10 carbon atoms. The compounds of the above general formulas (1-A) to (1-D) contain at least one cyclic ether structure having 2 to 13 carbon atoms. In the above general formula (1-A), R2 and R3 may be bonded to each other to form a cyclic ether structure having 2 to 13 carbon atoms. In the above general formula (1-B), adjacent R5 and R6 may be bonded to each other to form an unsaturated or saturated ring structure. In the above general formula (1-C), adjacent R8 and R9 may be bonded to each other to form a cyclic ether structure having 2 to 13 carbon atoms, or an unsaturated or saturated ring structure.
[0260] [3]: The metal-containing film-forming compound according to [2] above, characterized in that the polydentate ligand has a structure represented by formula (1-A) or (1-B) above.
[0261] [4]: The metal-containing film-forming compound according to any one of [1] to [3] above, characterized in that the cyclic ether structure is one of the structures shown by the following formulas (a-1) to (a-2). [ka] (In the formula, R a (where * represents a hydrogen atom or an organic group with 1 to 10 carbon atoms, and * indicates a bond.)
[0262] [5]: The metal-containing film-forming compound according to any one of [2] to [4] above, characterized in that the metal-containing film-forming compound is a reaction product of a metal-containing compound comprising a metal compound represented by the following formula (2), a hydrolysate or condensate of a metal compound represented by the following formula (2), or a hydrolysate condensate, and a polydentate ligand having the structure represented by the above general formulas (1-A) to (1-D). [ka] (In the formula, M is one of Ti, Zr, and Hf; L is a monodentate ligand and / or polydentate ligand having 1 to 30 carbon atoms; X is a halogen atom, an alkoxy group, a carboxylate group, an acyloxy group, or -NR) a R b It is a hydrolyzable group selected from among the following. a and R b Each of these is independently a hydrogen atom or a monovalent organic group with 1 to 20 carbon atoms. a + b = 4, where a and b are integers between 0 and 4.
[0263] [6]: The metal-containing film-forming compound according to [5] above, characterized in that the metal compound represented by formula (2) has the structure of formula (3) below. [ka] (In the formula, M is Ti, Zr, or Hf, and R 1A (It is a monovalent organic group with 1 to 20 carbon atoms.)
[0264] [7]: The metal-containing film-forming compound according to any one of [1] to [6] above, characterized in that the metal-containing film-forming compound further contains a ligand derived from a silicon compound represented by the following general formula (4). [ka] (In the above general formula (4), R 3A , R 3B and R 3CThis is one of the following organic groups selected from a C1-C30 organic group having a bridging group in any of the structures shown in the general formulas (b-1) to (b-3) below, a substituted or unsubstituted C1-C20 alkyl group, and a C1-C20 aryl group. [ka] (In the above general formulas (b-1) to (b-3), R3 is a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, q represents 0 or 1, and * represents a bond.)
[0265] [8]: A metal-containing film-forming composition, characterized in that it contains (A) a metal-containing film-forming compound described in any of [1] to [7] above, and (B) an organic solvent.
[0266] [9]: The metal-containing film-forming composition according to [8] above, characterized in that the composition contains one or more of (C) a thermal acid generator and (D) a photoacid generator.
[0267]
[10] : The metal-containing film-forming composition according to [8] or [9] above, characterized in that the composition further contains one or more of (E) a crosslinking agent and (F) a surfactant.
[0268]
[11] : The metal-containing film-forming composition according to any one of [8] to
[10] above, characterized in that the (B) organic solvent is a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher.
[0269]
[12] : A method for forming a pattern on a substrate to be processed, comprising: (I-1) a step of forming a metal-containing film by applying a metal-containing film-forming composition described in any of [8] to
[11] above onto a substrate to be processed and then heat-treating it; (I-2) a step of forming a resist upper layer film on the metal-containing film using a photoresist material; (I-3) a step of pattern exposure of the resist upper layer film and then developing it with a developer to form a pattern on the resist upper layer film; (I-4) a step of transferring a pattern to the metal-containing film by dry etching using the resist upper layer film on which the pattern has been formed as a mask; and (I-5) a step of processing the substrate to be processed using the metal-containing film on which the pattern has been formed as a mask to form a pattern on the substrate to be processed.
[0270]
[13] : A method for forming a pattern on a substrate to be processed, comprising: (II-1) a step of forming a resist underlayer film on a substrate to be processed; (II-2) a step of forming a metal-containing film by applying a metal-containing film-forming composition described in any of [8] to
[11] above onto the resist underlayer film and then heat-treating it; (II-3) a step of forming a resist upper layer film on the metal-containing film using a photoresist material; (II-4) a step of pattern exposure of the resist upper layer film and then developing it with a developer to form a pattern on the resist upper layer film; (II-5) a step of transferring the pattern to the metal-containing film by dry etching using the resist upper layer film on which the pattern has been formed as a mask; (II-6) a step of transferring the pattern to the resist underlayer film by dry etching using the metal-containing film on which the pattern has been transferred as a mask; and (II-7) a step of processing the substrate to be processed using the resist underlayer film on which the pattern has been formed as a mask to form a pattern on the substrate to be processed.
[0271] It should be noted that the present invention is not limited to the embodiments described above. The embodiments described above are illustrative, and any configuration that is substantially identical to the technical idea described in the claims of the present invention and achieves similar effects is included within the technical scope of the present invention. [Explanation of Symbols]
[0272] 1...Substrate, 2...Workpiece layer, 2a...Pattern (pattern formed on the workpiece layer) 3…Organic resist underlayer film, 3a…Organic resist underlayer film pattern, 4…Metal-containing film, 4a...metal-containing film pattern, 5...resist top layer film, 5a...resist top layer film pattern, 6...Exposed part, 10...Substrate to be processed.
Claims
1. A metal-containing film-forming compound, wherein the metal-containing film-forming compound comprises at least one metal atom selected from the group consisting of Zr and Hf, and a polydentate ligand containing a cyclic ether structure having 2 to 13 carbon atoms that coordinates to the metal atom. The aforementioned polydentate ligand has the structure shown by the following general formula (1-A), A metal-containing film-forming compound characterized in that the cyclic ether structure is one of the structures shown in the following formulas (a-1) to (a-2). 【Chemistry 1】 (In the above general formula (1-A), R1 to R4 are monovalent organic groups having 1 to 20 carbon atoms, which may contain a hydrogen atom or a cyclic ether structure having 2 to 13 carbon atoms. The compound of the above general formula (1-A) contains at least one cyclic ether structure having 2 to 13 carbon atoms. In the above general formula (1-A), R2 and R3 may bond to each other to form a cyclic ether structure having 2 to 13 carbon atoms.) 【Chemistry 2】 (In the formula, Ra is a hydrogen atom or an organic group having 1 to 10 carbon atoms, and * indicates a bond.)
2. The metal-containing film-forming compound according to claim 1, characterized in that the metal-containing film-forming compound is a reaction product of a metal-containing compound comprising a metal compound represented by the following formula (2), a hydrolysate or condensate of a metal compound represented by the following formula (2), or a hydrolysate condensate, and a polydentate ligand having the structure represented by the general formula (1-A). 【Transformation 3】 (In the formula, M is either Zr or Hf. L is a monodentate ligand and / or polydentate ligand having 1 to 30 carbon atoms, and X is a halogen atom, an alkoxy group, a carboxylate group, an acyloxy group, or -NR) a R b It is a hydrolyzable group selected from among the following. a and R b Each of these is independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. a + b = 4, where a and b are integers from 0 to 4.
3. The metal-containing film-forming compound according to claim 2, characterized in that the metal compound represented by formula (2) has the structure of formula (3) below. 【Chemistry 4】 (In the formula, M is Zr or Hf, and R 1A (It is a monovalent organic group with 1 to 20 carbon atoms.)
4. The metal-containing film-forming compound according to claim 1, characterized in that the metal-containing film-forming compound further contains a ligand derived from a silicon compound represented by the following general formula (4). 【Transformation 5】 (In the above general formula (4), R 3A , R 3B and R 3C This is one of the following organic groups selected from a C1-C30 organic group having a bridging group in any of the structures shown in the general formulas (b-1) to (b-3) below, a substituted or unsubstituted C1-C20 alkyl group, and a C1-C20 aryl group. 【Transformation 6】 (In the above general formulas (b-1) to (b-3), R 3 is a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, q represents 0 or 1, and * represents a bonding site.)
5. A composition for forming a metal-containing film, (A) A metal-containing film-forming compound according to any one of claims 1 to 4, and (B) Organic solvents A metal-containing film-forming composition characterized by containing the following:
6. The metal-containing film-forming composition according to claim 5, characterized in that the composition contains one or more of (C) a thermal acid generator and (D) a photoacid generator.
7. The metal-containing film-forming composition according to claim 5, characterized in that the composition further contains one or more of (E) a crosslinking agent and (F) a surfactant.
8. The metal-containing film-forming composition according to claim 5, characterized in that the (B) organic solvent is a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher.
9. A method for forming a pattern on a substrate to be processed, (I-1) A step of forming a metal-containing film by applying the metal-containing film-forming composition described in claim 5 onto a substrate to be processed, and then heat-treating it. (I-2) A step of forming a resist upper layer film on the metal-containing film using a photoresist material, (I-3) A step of forming a pattern on the resist upper layer film by pattern exposure followed by development with a developer solution. (I-4) A step of transferring the pattern to the metal-containing film by dry etching using the resist upper layer film on which the pattern is formed as a mask, and (I-5) A step of processing the workpiece substrate using the metal-containing film on which the pattern is formed as a mask to form a pattern on the workpiece substrate. A pattern forming method characterized by having the following features.
10. A method for forming a pattern on a substrate to be processed, (II-1) A step of forming a resist underlayer film on the substrate to be processed, (II-2) A step of forming a metal-containing film by applying the metal-containing film-forming composition described in claim 5 onto the resist underlayer film and then heat-treating it, (II-3) A step of forming a resist upper layer film on the metal-containing film using a photoresist material, (II-4) After pattern exposure of the resist upper layer film, develop it with a developer to form a pattern on the resist upper layer film. (II-5) A step of transferring the pattern to the metal-containing film by dry etching, using the resist upper layer film on which the pattern is formed as a mask. (II-6) A step of transferring the pattern to the resist underlayer film by dry etching, using the metal-containing film on which the pattern has been transferred as a mask. (II-7) A step of processing the substrate to be processed using the resist underlayer film on which the pattern is formed as a mask to form a pattern on the substrate to be processed, A pattern forming method characterized by having the following features.
Citation Information
Patent Citations
New epoxide-containing metal chelates process for their preparation and their use
GB1036574A
Method for purifying vitronectin
JP1989063600A
Ultraviolet absorber and cosmetic containing the same
JP1992185690A
Dry etching method
JP1993291208A
Forming method of multilayer resist pattern
JP1995181688A