Polarizing plates and image display devices

The polarizing plate design with a specific bonding layer and cured liquid crystal compounds addresses peeling issues, ensuring durability and preventing damage to phase difference layers during substrate removal.

JP7954637B2Active Publication Date: 2026-11-20SUMITOMO CHEM CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023156028
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-09-21
Publication Date
2026-11-20
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

Phase difference layers in polarizing plates containing cured liquid crystal compounds are prone to peeling damage during substrate peeling due to insufficient durability against peeling forces.

Method used

A polarizing plate design with a first bonding layer having a tensile modulus of 1.0 × 10⁻⁶ Pa or less, combined with phase difference layers containing cured liquid crystal compounds, ensures high durability against peeling forces by maintaining the integrity of the phase difference layers.

Benefits of technology

The design enhances the polarizing plate's durability during substrate peeling, preventing damage to the phase difference layers and improving overall structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954637000024
    Figure 0007954637000024
  • Figure 0007954637000025
    Figure 0007954637000025
  • Figure 0007954637000026
    Figure 0007954637000026
Patent Text Reader

Abstract

To provide a polarizer including a retardation plate having a plurality of retardation layers each containing a cured product of a liquid crystal compound, the polarizer having excellent durability against peeling force applied when a base material is peeled.SOLUTION: A polarizer is formed by laminating a linear polarizer, a first bonding layer and a retardation plate in this order. The retardation plate includes a first retardation layer and a second retardation layer, where the first retardation layer and the second retardation layer each contains a cured product of a liquid crystal compound and has a puncture modulus of elasticity of 70 g / mm or more. The first bonding layer has a tensile modulus of elasticity of 1.0×108 Pa or less at 23°C and 55% relative humidity.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to polarizing plates and image display devices. [Background technology]

[0002] Conventionally, in image display devices, a method has been employed in which a circular polarizer is placed on the viewing side of the image display panel to suppress the reduction in visibility due to the reflection of external light.

[0003] A circular polarizer has a structure in which a linear polarizer and a phase difference plate are stacked. In a circular polarizer, external light directed toward the image display panel is converted to linear polarization by the linear polarizer, and then converted to circular polarization by the subsequent phase difference plate. The circularly polarized external light is reflected by the surface of the image display panel, but during this reflection, the direction of rotation of the polarization plane is reversed, and it is converted to linear polarization by the phase difference plate and then blocked by the subsequent linear polarizer. As a result, the emission of external light to the outside is significantly suppressed.

[0004] In phase difference plates, a configuration having a phase difference layer containing a cured liquid crystal compound is known (for example, Patent Documents 1 and 2). With such a configuration, the phase difference plate can be made thinner. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2015-163935 [Patent Document 2] Japanese Patent Publication No. 2019-91030 [Overview of the Initiative] [Problems that the invention aims to solve]

[0006] In phase difference plates having multiple phase difference layers containing cured liquid crystal compounds, prioritizing thinning sometimes resulted in a problem where the phase difference layers, particularly those closest to the substrate being peeled off, were damaged by the peeling force applied during substrate peeling.

[0007] The present invention aims to provide a polarizing plate having a plurality of phase difference layers containing a cured liquid crystal compound, which exhibits excellent durability against peeling forces applied during substrate peeling. [Means for solving the problem]

[0008] The present invention provides the following polarizing plates. [1] A polarizing plate comprising a linear polarizing plate, a first bonding layer, and a phase difference plate, laminated in this order, The phase difference plate is It has a first phase difference layer and a second phase difference layer, The first phase difference layer and the second phase difference layer contain a cured liquid crystal compound. The puncture modulus is 70 g / mm or higher. The first laminated layer has a tensile modulus of 1.0 × 10 at a temperature of 23°C and a relative humidity of 55%. 8 A polarizing plate with a Pa rating of less than or equal to Pa. [2] The polarizing plate according to [1], wherein the product of the thickness (m) of the first laminated layer and the tensile modulus (Pa) is 500 or less. [3] The polarizing plate according to [1] or [2], wherein the phase difference plate has only an alignment film between the first phase difference layer and the second phase difference layer, or has no other intervening layer. [4] The linear polarizing plate has a polarizer, The polarizer is a polarizing plate described in item 1, with a thickness of 15 μm or less, and is one of the offsets in [1] to [3]. [5] The linear polarizing plate has a protective film provided on the surface of the polarizer opposite to the first bonding layer, The protective film is a polarizing plate as described in [4], wherein the thickness is 30 μm or less. [6] The polarizer according to any one of [1] to [5], wherein the first phase difference layer is an inversely dispersed λ / 4 layer. [7] The polarizing plate according to any one of [1] to [6], wherein the second phase difference layer is a positive C plate. [Effects of the Invention]

[0009] According to the present invention, it is possible to provide a polarizing plate that has excellent durability against the peeling force applied when peeling off a substrate. [Brief explanation of the drawing]

[0010] [Figure 1] This is a schematic cross-sectional view illustrating an example of a polarizing plate according to this embodiment. [Figure 2] This is a schematic cross-sectional view illustrating a specific example of a phase difference plate. [Figure 3] This is a schematic cross-sectional view illustrating a specific example of a phase difference plate. [Figure 4] This is a schematic cross-sectional view illustrating an example of an image display device according to this embodiment. [Modes for carrying out the invention]

[0011] Embodiments of the present invention will be described below with reference to the drawings, but the present invention is not limited to the following embodiments. In all the following drawings, the scale has been adjusted as appropriate to make each component easier to understand, and the scale of each component shown in the drawings does not necessarily match the scale of the actual component.

[0012] [Polarizing plate] Figure 1 is a schematic cross-sectional view illustrating an example of a polarizing plate according to this embodiment. As shown in Figure 1, the polarizing plate 1 is constructed by laminating a linear polarizing plate 10, a first bonding layer 21, and a phase difference plate 30 in that order from the front side. The phase difference plate 30 has a first phase difference layer 31 and a second phase difference layer 32. The polarizing plate 1 may also be a circular polarizing plate. In this specification, the term polarizing plate also includes circular polarizing plates.

[0013] The phase difference plate 30 has a puncture modulus of 70 g / mm or more. The puncture modulus is the value measured by the method described in the examples. The puncture modulus of the phase difference plate 30 is preferably 140 g / mm or less, more preferably 120 g / mm or less, and may be 110 g / mm or less. The phase difference plate 30 may or may not contain a substrate intended to be peeled off from the polarizing plate, and the puncture modulus of the phase difference plate 30 as referred to herein means the puncture modulus of the layer structure of the portion of the phase difference plate 30 that does not contain a substrate intended to be peeled off from the polarizing plate. In the phase difference plate 30, there may or may not be other interposed layers between the first phase difference layer 31 and the second phase difference layer 32.

[0014] In the phase difference plate 30, when the first phase difference layer 31 and the second phase difference layer 32 are bonded together via a bonding layer (hereinafter referred to as the "third bonding layer"), the puncture modulus depends on the hardness of the third bonding layer. However, if the third bonding layer is made of an adhesive, the puncture modulus tends to be low, and may be less than 70 g / mm. On the other hand, if the third bonding layer is made of an adhesive, the puncture modulus tends to be high, and may be 70 g / mm or more. In the phase difference plate 30, when the first phase difference layer 31 and the second phase difference layer 32 are laminated without a bonding layer interposed between them, the puncture modulus of the phase difference plate 30 is high. The density tends to be such that it is usually 70 g / mm or more. In the phase difference plate 30, a configuration in which the first phase difference layer 31 and the second phase difference layer 32 are laminated without a bonding layer includes a configuration in which there is only an alignment film between the first phase difference layer 31 and the second phase difference layer 32, or no other intervening layer.

[0015] The inventors have found that polarizing plates using phase difference plates with a high puncture modulus have low durability against the peeling force applied when the substrate is peeled off. On the other hand, if the puncture modulus of the phase difference plate is lowered, the peeling force of the substrate becomes lighter, which tends to cause the substrate to lift easily. The inventors have further diligently conducted research and found that even with polarizing plates using phase difference plates with a puncture modulus of 70 g / mm or more, the tensile modulus of the first laminated layer 21 interposed between the linear polarizing plate 10 and the phase difference plate 30 is 1.0 × 10 at a temperature of 23°C and a relative humidity of 55%. 8 The present invention was developed based on the finding that by using an adhesive with a tensile modulus of Pa or less, a polarizing plate with excellent durability against peeling forces applied during substrate removal can be made. Furthermore, this configuration of the present invention can suppress the occurrence of cracks caused by heat shock and polishing. The tensile modulus of the adhesive forming the first bonding layer 21 at a temperature of 23°C and a relative humidity of 55% is preferably 1.0 × 10⁻⁶. 7 It is less than or equal to Pa, and more preferably 1.0 × 10⁻⁶ 6 It is less than or equal to Pa, preferably 1.0 × 10⁻⁶ 3 Pa or higher, more preferably 1.0 × 10⁻⁶ 5 The tensile modulus is Pa or higher. Furthermore, the product of the thickness (m) of the adhesive forming the first bonding layer 21 and its tensile modulus (Pa) is preferably 500 or less, more preferably 50 or less, and even more preferably 5 or less. The product of the thickness (m) of the adhesive forming the first bonding layer 21 and its tensile modulus (Pa) is preferably 0.005 or more, and more preferably 0.5 or more. By setting the numerical range to this, the durability against peeling force can be improved.

[0016] The polarizing plate according to the present invention has high durability against the peeling force applied when peeling off the substrate, and more specifically, it can suppress damage to the phase difference layer of the phase difference plate when peeling off the substrate from a polarizing plate having a phase difference plate equipped with a substrate. The phase difference layer of the phase difference plate is thin when it is a layer containing a cured liquid crystal compound and is easily damaged when peeling off the substrate, and the phase difference layer closer to the substrate is particularly susceptible to damage, but such damage can be suppressed in the polarizing plate according to the present invention. Examples of substrates include substrates used in the manufacturing process of the phase difference plate.

[0017] The tensile modulus of the adhesive forming the first lamination layer 21 at a temperature of 23°C and a relative humidity of 55% can be measured by the following procedure. The adhesive composition is applied to the release-treated surface of a release-treated polyethylene terephthalate film (hereinafter sometimes referred to as "PET film") using an applicator. Then, it is pre-dried by leaving it in a room temperature atmosphere for 30 minutes, and then fully dried by leaving it in a 100°C environment for 5 minutes to allow the solvent contained in the adhesive composition applied to the PET film to evaporate completely. Finally, a predetermined curing treatment (such as heat treatment or ultraviolet irradiation treatment) is performed to create a lamination layer on the PET film, and the tensile modulus of the lamination layer obtained by peeling off the PET film can be measured as a sample using the method described in the examples below.

[0018] [First lamination layer] The first bonding layer 21 is responsible for bonding the linear polarizing plate 10 and the phase difference plate 30. The tensile modulus at a temperature of 23°C and a relative humidity of 55% is 1.0 × 10⁻⁶. 8 Examples of adhesives with a viscosity of Pa or less include adhesives and tacks. Preferably, an adhesive is used as the first bonding layer 21.

[0019] The specific adhesive used in the first bonding layer 21 can be composed of, for example, acrylic polymers, silicone polymers, polyesters, polyurethanes, polyethers, etc., as base polymers. Among these, acrylic polymers are particularly good because they have excellent optical transparency, maintain appropriate wettability and cohesive strength, and have excellent adhesion to the substrate, and further It is preferable to select and use a polymer that has weather resistance and heat resistance, and does not cause peeling problems such as lifting or detachment under heating or humidification conditions. In the case of acrylic polymers, an acrylic copolymer with a weight-average molecular weight of 100,000 or more is useful as a base polymer, which is obtained by blending an alkyl ester of acrylic acid having an alkyl group with 20 or fewer carbon atoms, such as a methyl group, ethyl group, or butyl group, with a functional group-containing acrylic monomer consisting of (meth)acrylic acid or hydroxyethyl (meth)acrylate, etc., so that the glass transition temperature is preferably 25°C or lower, and more preferably 0°C or lower.

[0020] While not particularly limited, acrylic polymers such as butyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, or copolymer-based polymers using two or more of these (meth)acrylate esters, are preferably used. Furthermore, polar monomers may be copolymerized into these base polymers. Examples of polar monomers include monomers having polar functional groups such as carboxyl groups, hydroxyl groups, amide groups, amino groups, and epoxy groups, such as (meth)acrylic acid, 2-hydroxypropyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, (meth)acrylamide, 2-N,N-dimethylaminoethyl (meth)acrylate, and glycidyl (meth)acrylate.

[0021] These acrylic polymers can be used as adhesives on their own, but adhesives typically contain crosslinking agents. Examples of crosslinking agents include divalent or polyvalent metal ions that form metal carboxylate salts with carboxyl groups, polyamine compounds that form amide bonds with carboxyl groups, polyepoxy compounds and polyol compounds that form ester bonds with carboxyl groups, and polyisocyanate compounds that form amide bonds with carboxyl groups. Among these, polyisocyanate compounds are widely used as organic crosslinking agents.

[0022] In this embodiment, there are no particular limitations on the means for adjusting the tensile modulus of the adhesive forming the first bonding layer, but for example, a method of compounding an oligomer, specifically a urethane acrylate-based oligomer, with the above-mentioned adhesive components is preferred. Furthermore, an adhesive compounded with such a urethane acrylate-based oligomer may be cured by irradiation with energy rays. Adhesives compounded with urethane acrylate-based oligomers, or adhesives with separators obtained by coating such an adhesive onto a support film (separator) and curing it with ultraviolet light, are well known and can be obtained from adhesive manufacturers.

[0023] In addition to the base polymer, crosslinking agent, and oligomer mentioned above, adhesives may also contain appropriate additives, such as natural or synthetic resins, tackifying resins, antioxidants, UV absorbers, dyes, pigments, defoamers, corrosion inhibitors, and photopolymerization initiators, to adjust the adhesive strength, cohesive force, viscosity, modulus of elasticity, and glass transition temperature of the adhesive, as needed. Examples of UV absorbers include salicylate ester compounds, benzophenone compounds, benzotriazole compounds, cyanoacrylate compounds, and nickel complex salt compounds.

[0024] The thickness of the first bonding layer 21 is determined according to its adhesive strength, but is usually in the range of 1 to 40 μm. A thickness of 3 to 25 μm or 20 μm or less for the adhesive layer is preferable because it maintains good processability and exhibits high durability. Furthermore, a thickness within the above range can further improve durability against peeling forces.

[0025] Specific adhesives used in the first bonding layer 21 include adhesives other than pressure-sensitive adhesives (tacks), such as water-based adhesives and active energy ray-curing adhesives.

[0026] Examples of water-based adhesives include adhesives in which polyvinyl alcohol-based resin is dissolved or dispersed in water. There are no particular limitations on the drying method when using water-based adhesives, but methods such as using a hot air dryer or an infrared dryer can be employed.

[0027] Examples of active energy ray curing adhesives include solvent-free active energy ray curing adhesives containing curable compounds that harden upon irradiation with active energy rays such as ultraviolet light, visible light, electron beams, and X-rays. By using a solvent-free active energy ray curing adhesive, the adhesion between layers can be improved.

[0028] As an active energy ray curable adhesive, it is preferable to include either a cationic curable compound, a radical curable compound, or both, as these exhibit good adhesion. The active energy ray curable adhesive may further contain a cationic polymerization initiator, such as a photocationic polymerization initiator, or a radical polymerization initiator for initiating the curing reaction of the above-mentioned curable compound.

[0029] Examples of cationically polymerizable curable compounds include epoxy compounds such as alicyclic epoxy compounds having epoxy groups bonded to an alicyclic ring, polyfunctional aliphatic epoxy compounds having two or more epoxy groups but no aromatic ring, monofunctional epoxy groups having one epoxy group (excluding those included in alicyclic epoxy compounds), and polyfunctional aromatic epoxy compounds having two or more epoxy groups and an aromatic ring; oxetane compounds having one or more oxetane rings in the molecule; and combinations thereof.

[0030] Examples of radically polymerizable curable compounds include (meth)acrylic compounds (compounds having one or more (meth)acryloyloxy groups in the molecule), other vinyl compounds having radically polymerizable double bonds, or combinations thereof.

[0031] Active energy ray curing adhesives may contain sensitizers, such as photosensitizers, as needed. Using sensitizers improves reactivity and further enhances the mechanical strength and adhesive strength of the adhesive layer. Known sensitizers can be appropriately applied. When sensitizers are included, the amount is preferably in the range of 0.1 to 20 parts by mass per 100 parts by mass of the total amount of the active energy ray curing adhesive.

[0032] Active energy ray curing adhesives may contain additives such as ion trapping agents, antioxidants, chain transfer agents, tackifiers, thermoplastic resins, fillers, flow regulators, plasticizers, defoamers, antistatic agents, leveling agents, and solvents, as needed.

[0033] When using an active energy ray curing adhesive, the adhesive coating layer can be cured by irradiating it with active energy rays such as ultraviolet light, visible light, electron beams, or X-rays to form an adhesive layer. Ultraviolet light is preferred as the active energy ray, and in this case, low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, chemical lamps, black light lamps, microwave-excited mercury lamps, metal halide lamps, etc., can be used as light sources.

[0034] When the adhesive is used as the first bonding layer 21, its thickness is determined according to its adhesive strength and other factors, but it is usually in the range of 0.02 to 10 μm. A thickness of 1 to 4 μm for the adhesive layer is preferable from the viewpoint of further improving durability against external forces.

[0035] [Linear polarizing plate] The linear polarizing plate 10 can be any film having a polarizing function that obtains linearly polarized light from transmitted light. This film may be a stretched film on which a dye having absorption anisotropy is adsorbed, or an absorbent film. Examples include films containing a film coated with an anisotropic dye as a polarizer. Examples of dyes with absorption anisotropy include dichroic dyes. Examples of films coated with an absorption anisotropic dye used as a polarizer include stretched films on which an absorption anisotropic dye is adsorbed, or films having a liquid phase layer obtained by coating a composition containing a liquid crystalline dichroic dye or a composition containing a dichroic dye and a polymerizable liquid crystal.

[0036] <Linear polarizer equipped with stretched film as a polarizer> This section describes a linear polarizing plate equipped with a stretched film on which an absorption-anisotropic dye is adsorbed as a polarizer. The stretched film on which an absorption-anisotropic dye is adsorbed, which serves as the polarizer, is typically manufactured by a process that includes uniaxial stretching of a polyvinyl alcohol-based resin film, a process of dyeing the polyvinyl alcohol-based resin film with a dichroic dye to adsorb the dichroic dye, a process of treating the polyvinyl alcohol-based resin film on which the dichroic dye has been adsorbed with a boric acid aqueous solution, and a process of washing with water after treatment with the boric acid aqueous solution. Such a polarizer may be used as a linear polarizing plate as is, or a linear polarizing plate in which a transparent protective film is laminated to at least one side of such a polarizer may be used.

[0037] The thickness of the polarizer obtained by uniaxial stretching, dyeing with a dichroic dye, boric acid treatment, water washing, and drying of the polyvinyl alcohol-based resin film is preferably 5 to 40 μm, more preferably 15 μm or less, and even more preferably 10 μm or less.

[0038] The material of the protective film laminated to one or both sides of the polarizer is not particularly limited, but examples of films known in this field include cyclic polyolefin resin films, cellulose acetate resin films made from resins such as triacetylcellulose and diacetylcellulose, polyester resin films made from resins such as polyethylene terephthalate, polyethylene naphthalate and polybutylene terephthalate, polycarbonate resin films, (meth)acrylic resin films, and polypropylene resin films. From the viewpoint of thinning, the thickness of the protective film is usually 300 μm or less, preferably 200 μm or less, more preferably 30 μm or less, and usually 5 μm or more, but may be 10 μm or more. If the thickness of the protective film is 30 μm or less, or if the tensile modulus of elasticity at a temperature of 23°C is 2000 MPa or more, the protective film does not function well as a force-relieving layer applied when peeling off the substrate, so the durability against substrate peeling decreases, and problems such as damage to the phase difference layer close to the peeled substrate are likely to occur. Furthermore, the protective film on the viewing side may or may not have a phase difference.

[0039] The protective film can be bonded to one or both sides of the polarizer via a bonding layer (hereinafter referred to as the "second bonding layer").

[0040] <Linear polarizer equipped with a film having a liquid crystal layer as a polarizer> A linear polarizing plate equipped with a film having a liquid crystal layer as a polarizer will be described. Examples of films coated with an absorption anisotropy dye used as a polarizer include a film obtained by coating a composition containing a liquid crystal dichroic dye, or a film obtained by coating a composition containing a dichroic dye and a liquid crystal compound. The film may be used as a linear polarizing plate on its own, or it may be used as a linear polarizing plate in a configuration in which a protective film is attached to one or both sides thereof. The protective film may be the same as that used in the linear polarizing plate equipped with the stretched film as a polarizer described above. The protective film can be bonded to one or both sides of the polarizer via a second bonding layer.

[0041] A film coated with an absorption-anisotropic dye is preferable to be thin, but if it is too thin, its strength will be compromised. The quality tends to decrease, resulting in poor processability. The thickness of the film is usually 20 μm or less, preferably 15 μm or less, more preferably 5 μm or less, and even more preferably 0.5 μm or more and 3 μm or less.

[0042] Specific examples of films coated with the aforementioned absorption anisotropy dye include the film described in Japanese Patent Publication No. 2013-33249, etc.

[0043] One embodiment of a linear polarizing plate is a configuration in which a protective film is provided on the surface of the linear polarizing plate opposite to the first bonding layer.

[0044] <Frontmost layer> The linear polarizing plate 10 may have an anti-reflective layer on its front surface. The anti-reflective layer has the function of preventing the reflected light of external light on or inside the linear polarizing plate 10 from being visible, and can be formed by conventional methods for forming anti-reflective layers, such as coating, sputtering, or vacuum deposition. The anti-reflective layer may be formed in advance on the front side of a protective film provided on the front side of the linear polarizing plate 10, thereby constructing a linear polarizing plate with an anti-reflective layer using such a protective film, or it may be provided separately from the protective film.

[0045] The linear polarizing plate 10 may have a surface treatment layer other than the anti-reflective layer on its frontmost surface. Examples of such surface treatment layers include a hard coat layer, an anti-sticking layer, an anti-glare layer, and a diffusion layer.

[0046] [Phase plate] The phase difference plate 30 has a first phase difference layer 31 and a second phase difference layer 32, and the first phase difference layer 31 and the second phase difference layer 32 contain a cured liquid crystal compound, and are not limited as long as their puncture modulus is 70 g / mm or more. The phase difference plate 30 may also have a third phase difference layer. The first phase difference layer, the second phase difference layer, and the third phase difference layer may each consist of two or more layers. The phase difference plate 30 may have a substrate on the surface opposite to the linear polarizing plate 10 side. The substrate may be a substrate for forming the phase difference layer and may be peelable from the phase difference layer.

[0047] The phase difference plate 30 preferably has optical properties represented by formulas (1) and (2). In order for the phase difference plate 30 to have such optical properties, the first phase difference layer 31, the second phase difference layer 32, or the third phase difference layer may have optical properties represented by formulas (1) and (2), or at least two selected from the first phase difference layer 31, the second phase difference layer 32, and the third phase difference layer may be combined to exhibit the optical properties represented by formulas (1) and (2). Re(450) / Re(550)≦1.00 (1) 1.00 ≤ Re(650) / Re(550) (2)

[0048] In this specification, Re(450) represents the in-plane phase difference value at a wavelength of 450 nm, Re(550) represents the in-plane phase difference value at a wavelength of 550 nm, and Re(650) represents the in-plane phase difference value at a wavelength of 650 nm.

[0049] <Retardation layer> Examples of phase difference layers include layers formed by polymerizing polymerizable liquid crystals and stretched films. The optical properties of the phase difference layer can be adjusted by the orientation state of the polymerizable liquid crystal or the stretching method of the stretched film. Layers formed by polymerizing polymerizable liquid crystals include cured liquid crystal compounds. In the phase difference plate 30, from the viewpoint of thinning, at least the first phase difference layer 31 and the second phase difference layer 32 are layers containing cured liquid crystal compounds.

[0050] (A layer formed by polymerizing polymerizable liquid crystals) In this specification, a polymerizable liquid crystal whose optical axis is oriented horizontally to the substrate plane is defined as horizontal orientation, and a polymerizable liquid crystal whose optical axis is oriented perpendicularly to the substrate plane is defined as vertical orientation. The optical axis refers to the direction in which the cross-section cut perpendicular to the optical axis of the refractive index ellipsoid formed by the orientation of the polymerizable liquid crystal is a circle, that is, the direction in which the refractive indices in all three directions are equal.

[0051] Examples of polymerizable liquid crystals include rod-shaped polymerizable liquid crystals and disc-shaped polymerizable liquid crystals. When a rod-shaped polymerizable liquid crystal is oriented horizontally or vertically with respect to a substrate, the optical axis of the polymerizable liquid crystal coincides with the long axis of the polymerizable liquid crystal. When a disc-shaped polymerizable liquid crystal is oriented, the optical axis of the polymerizable liquid crystal exists in a direction perpendicular to the disc surface of the polymerizable liquid crystal.

[0052] The slow axis direction of a stretched film varies depending on the stretching method. The slow axis and optical axis are determined according to the stretching method, such as uniaxial, biaxial, or oblique stretching.

[0053] For a layer formed by polymerizing polymerizable liquid crystals to exhibit an in-plane phase difference, the polymerizable liquid crystals should be oriented in a suitable direction. When the polymerizable liquid crystal is rod-shaped, an in-plane phase difference is exhibited by oriented the optical axis of the polymerizable liquid crystal horizontally to the substrate plane; in this case, the optical axis direction and the slow phase axis direction coincide. When the polymerizable liquid crystal is disc-shaped, an in-plane phase difference is exhibited by oriented the optical axis of the polymerizable liquid crystal horizontally to the substrate plane; in this case, the optical axis and the slow phase axis are orthogonal. The orientation state of the polymerizable liquid crystal can be adjusted by combining an alignment film and the polymerizable liquid crystal.

[0054] The in-plane phase difference value of the phase difference layer can be adjusted by the thickness of the phase difference layer. Since the in-plane phase difference value is determined by equation (10), to obtain the desired in-plane phase difference value (Re(λ)), one should adjust Δn(λ) and the film thickness d. Re(λ)=d×Δn(λ) (10) In the formula, Re(λ) represents the in-plane phase difference value at wavelength λnm, d represents the film thickness, and Δn(λ) represents the birefringence at wavelength λnm.

[0055] The birefringence Δn(λ) is obtained by measuring the in-plane phase difference value and dividing it by the thickness of the phase difference layer. In a specific measurement method, the characteristics of the phase difference layer can be measured by measuring a film deposited on a substrate that does not have an in-plane phase difference itself, such as a glass substrate.

[0056] In this specification, the refractive indices in three directions in a refractive index ellipsoid formed by the orientation of polymerizable liquid crystals or the stretching of a film are represented as nx, ny, and nz. nx represents the principal refractive index in the direction parallel to the film plane in the refractive index ellipsoid formed by the phase difference layer. ny represents the phase In the refractive index ellipsoid formed by the difference layer, nx represents the refractive index in a direction parallel to the film plane and perpendicular to the direction of nx. nz represents the refractive index in a direction perpendicular to the film plane in the refractive index ellipsoid formed by the phase difference layer.

[0057] When the optical axis of a rod-like polymerizable liquid crystal is aligned horizontally with respect to the flat surface of a substrate, the resulting retardation layer has a refractive index relationship of nx>ny≈nz (positive A plate), and in the refractive index ellipsoid , the axis in the nx direction coincides with the slow axis.

[0058] Further, when the optical axis of a disc-like polymerizable liquid crystal is aligned horizontally with respect to the flat surface of a substrate, the resulting retardation layer has a refractive index relationship of nx<ny≈nz (negative A plate), and in the refractive index ellipsoid , the axis in the ny direction coincides with the slow axis.

[0059] In order for a layer formed by polymerizing a polymerizable liquid crystal to exhibit thickness-direction retardation, the polymerizable liquid crystal only needs to be aligned in an appropriate direction. In the present invention, "exhibiting thickness-direction retardation" is defined as indicating a characteristic in which Rth (the retardation value in the thickness direction) is negative in formula (20). Rth can be calculated from the retardation value (R 40 ) measured by tilting 40 degrees with the in-plane fast axis as the tilt axis, and the in-plane retardation value (Re). That is, Rth can be calculated from Re, R 40 , d (the thickness of the retardation layer), and n0 (the average refractive index of the retardation layer), by determining nx, ny and nz using the following formulas (21) to (23), and substituting these into formula (20) . Rth=[(nx+ny) / 2-nz]×d (20) Re =(nx-ny)×d (21) R 40 =(nx-ny')×d / cos(φ) (22) (nx+ny+nz) / 3=n0 (23) Here, φ=sin -1 〔sin(40°) / n0〕 ny'=ny×nz / 〔ny 2 ×sin 2 (φ)+nz 2 ×cos 2 (φ)〕 1 / 2 Further, nx, ny and nz are the same as defined above.

[0060] When the polymerizable liquid crystal is in a rod shape, the optical axis of the polymerizable liquid crystal is aligned perpendicular to the substrate plane, whereby retardation in the thickness direction is developed. When the polymerizable liquid crystal is in a discotic shape, the optical axis of the polymerizable liquid crystal is aligned parallel to the substrate plane, whereby retardation in the thickness direction is developed. In the case of a discotic polymerizable liquid crystal, since the optical axis of the polymerizable liquid crystal is parallel to the substrate plane, Re is determined and the thickness is fixed, so Rth is uniquely determined. Meanwhile, in the case of a rod-shaped polymerizable liquid crystal, since the optical axis of the polymerizable liquid crystal is perpendicular to the substrate plane, Rth can be adjusted by adjusting the thickness of the retardation layer without changing Re.

[0061] When the optical axis of the rod-shaped polymerizable liquid crystal is aligned perpendicular to the substrate plane, the resulting retardation layer has a refractive index relationship of nx≈ny<nz (positive C plate), and in the refractive index ellipsoid the axis in the nz direction coincides with the slow axis direction.

[0062] Further, when the optical axis of the discotic polymerizable liquid crystal is aligned parallel to the substrate plane, the resulting retardation layer has a refractive index relationship of nx<ny≈nz (negative A plate), and the refractive index ellipsoid the axis in the ny direction in the body coincides with the slow axis direction.

[0063] <Polymerizable Liquid Crystal> A polymerizable liquid crystal is a compound that has polymerizable groups and liquid crystalline properties. A polymerizable group is a group that participates in polymerization reactions, and it is preferably a photopolymerizable group. Here, a photopolymerizable group is a group that can participate in polymerization reactions by active radicals or acids generated from photopolymerization initiators, which will be described later. Examples of polymerizable groups include vinyl groups, vinyloxy groups, 1-chlorovinyl groups, isopropenyl groups, 4-vinylphenyl groups, acryloyloxy groups, methacryloyloxy groups, oxyranyl groups, and oxetanyl groups. Among these, acryloyloxy groups, methacryloyloxy groups, vinyloxy groups, oxyranyl groups, and oxetanyl groups are preferred, and acryloyloxy groups are more preferred. The liquid crystalline properties of a polymerizable liquid crystal may be either thermotropic or lyotropic, and if thermotropic liquid crystals are classified by their degree of order, they may be either nematic or smectic.

[0064] Examples of rod-shaped polymerizable liquid crystals include compounds represented by the following formula (A) and compounds containing a group represented by the following formula (X). From the viewpoint of exhibiting wavelength dispersibility, liquid crystals having a T-shaped or H-shaped mesogenic structure that is oriented perpendicular to the molecular axis and also birefringent are preferred as rod-shaped polymerizable liquid crystals, and T-shaped liquid crystals are more preferred from the viewpoint of obtaining stronger dispersion. Specifically, examples of the structure of T-shaped liquid crystals include compounds represented by the following formula (A). It can be done.

[0065] (The compound represented by formula (A)) Formula (A) is as follows. Hereinafter, compounds represented by formula (A) may be referred to as polymerizable liquid crystal (A). [ka]

[0066] In formula (A), Ar represents a divalent aromatic group which may have substituents. Preferably, the divalent aromatic group contains at least one of a nitrogen atom, an oxygen atom, or a sulfur atom. If the divalent group Ar contains two or more aromatic groups, the two or more aromatic groups may be bonded to each other by single bonds, divalent bonding groups such as -CO-O-, and -O-. G 1 and G 2 Each of these independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group. Here, the hydrogen atoms contained in the divalent aromatic group or divalent alicyclic hydrocarbon group may be substituted with halogen atoms, C1-C4 alkyl groups, C1-C4 fluoroalkyl groups, C1-C4 alkoxy groups, cyano groups, or nitro groups, and the carbon atoms constituting the divalent aromatic group or divalent alicyclic hydrocarbon group may be substituted with oxygen atoms, sulfur atoms, or nitrogen atoms. L 1 , L 2 、 B 1 and B 2 Each of these is independently a single bond or a divalent linking group. k and l each represent integers from 0 to 3 independently, satisfying the relationship 1 ≤ k + l. Here, if 2 ≤ k + l, then B 1 and B 2 , G 1 and G 2 These elements may be identical to each other, or they may be different. E 1 and E 2 Each of these independently represents an alkanediyl group having 1 to 17 carbon atoms, where the hydrogen atoms in the alkanediyl group may be substituted with halogen atoms, and the -CH2- groups in the alkanediyl group may be substituted with -O-, -S-, or -COO-, and if there are multiple -O-, -S-, or -COO- groups, they are not adjacent to each other. 1 and P 2 Each of these independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group.

[0067] G 1 and G 2Each of these is independently preferably a 1,4-phenylenediyl group which may be substituted with at least one substituent selected from the group consisting of a halogen atom and an alkyl group having 1 to 4 carbon atoms, or a 1,4-cyclohexanediyl group which may be substituted with at least one substituent selected from the group consisting of a halogen atom and an alkyl group having 1 to 4 carbon atoms, more preferably a methyl-substituted 1,4-phenylenediyl group, an unsubstituted 1,4-phenylenediyl group, or an unsubstituted 1,4-trans-cyclohexanediyl group, and particularly preferably an unsubstituted 1,4-phenylenediyl group or an unsubstituted 1,4-trans-cyclohexandiyl group. Also, there are multiple G 1 and G 2 Preferably, at least one of them is a divalent alicyclic hydrocarbon group, and L 1 or L 2 G that joins 1 and G 2 It is more preferable that at least one of these is a divalent alicyclic hydrocarbon group.

[0068] L 1 and L 2 Each of these is independently, preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a1 Ure a2 -, -R a3 COOR a4 -, -R a5 OCOR a6 -, R a7 OC=OOR a8 -, -N=N-, -CR c =CR d -, or C≡C-. Here, R a1 ~R a8 Each of these independently represents a single bond or an alkylene group with 1 to 4 carbon atoms, R c and R d L represents an alkyl group with 1 to 4 carbon atoms or a hydrogen atom. 1 and L 2 Each is independently, more preferably a single bond, -OR a2-1 -, -CH2-, -CH2CH2-, -COOR a4-1 -, or OCORa6-1 - is the case here R a2-1 , R a4-1 , R a6-1 Each of these can independently be a single bond, -CH2-, or -CH2CH2-. Represents L 1 and L 2 Each of these is independently, and more preferably, a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, or OCO-.

[0069] B 1 and B 2 Each of these is independently, preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a9 Ure a10 -, -R a11 COOR a12 -, -R a13 OCOR a14 -, or R a15 OC=OOR a16 - is the case here R a9 ~R a16 Each of these independently represents a single bond or an alkylene group with 1 to 4 carbon atoms. 1 and B 2 Each is independently, more preferably a single bond, -OR a10-1 -, -CH2-, -CH2CH2-, -COOR a12-1 -, or OCOR a14-1 - is the case here R a10-1 , R a12-1 , R a14-1 Each of these independently represents either a single bond, -CH2-, or -CH2CH2-. 1 and B 2 Each of these is independently, and more preferably, a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, -OCO-, or OCOCH2CH2-.

[0070] From the viewpoint of exhibiting inverse wavelength dispersion, k and l are preferably in the range of 2 ≤ k + l ≤ 6, preferably k + l = 4, and more preferably k = 2 and l = 2. A symmetric structure is preferred when k = 2 and l = 2.

[0071] E 1 and E 2 each independently are preferably an alkanediyl group having 1 to 17 carbon atoms, more preferably an alkanediyl group having 4 to 12 carbon atoms.

[0072] P 1 or P 2 Examples of the polymerizable group represented by include an epoxy group, a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group and an oxetanyl group are preferable, and an acryloyloxy group is more preferable.

[0073] Ar preferably has at least one selected from an aromatic hydrocarbon ring which may have a substituent, an aromatic heterocyclic ring which may have a substituent, and an electron-withdrawing group. Examples of the aromatic hydrocarbon ring include a benzene ring, a naphthalene ring, an anthracene ring and the like, and a benzene ring and a naphthalene ring are preferable. Examples of the aromatic heterocyclic ring include a furan ring, a benzofuran ring, a pyrrole ring, an indole ring, a thiophene ring, a benzothiophene ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, a triazole ring, a triazine ring, a pyrroline ring, an imidazole ring, a pyrazole ring, a thiazole ring, a benzothiazole ring, a thienothiazole ring, an oxazole ring, a benzoxazole ring, a phenanthroline ring and the like. Among them, it preferably has a thiazole ring, a benzothiazole ring or a benzofuran ring, and more preferably has a benzothiazolyl group. When Ar contains a nitrogen atom, the nitrogen atom preferably has a π electron.

[0074] In formula (A), the total number N of π electrons contained in the divalent aromatic group represented by Ar π is preferably 8 or more, more preferably 10 or more, still more preferably 14 or more, and particularly preferably 16 or more. Further, it is preferably 30 or less, more preferably 26 or less, and still more preferably 24 or less.

[0075] Preferable examples of the aromatic group represented by Ar include the following groups.

[0076]

Chemical Formula

[0077] In formula (Ar-1) to formula (Ar-23), the * mark represents a linking moiety, and Z 0 , Z 1 and Z 2 each independently represent a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, an alkylsulfinyl group having 1 to 12 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, a carboxyl group, a fluoroalkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkylthio group having 1 to 12 carbon atoms, an N-alkylamino group having 1 to 12 carbon atoms, an N,N-dialkylamino group having 2 to 12 carbon atoms, an N-alkylsulfamoyl group having 1 to 12 carbon atoms, or an N,N-dialkylsulfamoyl group having 2 to 12 carbon atoms.

[0078] Q 1 , Q 2 and Q 3 each independently represent -CR 2’ R 3’ -, -S-, -NH-, -NR 2’ -, -CO- or -O-, and R 2’ and R 3’ each independently represent a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.

[0079] J 1 , and J 2 each independently represent a carbon atom or a nitrogen atom.

[0080] Y 1 , Y 2 and Y 3 each independently represent an optionally substituted aromatic hydrocarbon group or aromatic heterocyclic group.

[0081] W1 and W 2 Each of these independently represents a hydrogen atom, a cyano group, a methyl group, or a halogen atom, and m represents an integer from 0 to 6.

[0082] Y 1 , Y 2 and Y 3 Examples of aromatic hydrocarbon groups in this context include C6-C20 aromatic hydrocarbon groups such as phenyl, naphthyl, anthuryl, phenanthuryl, and biphenyl groups, with phenyl and naphthyl groups being preferred and phenyl groups being more preferred. Examples of aromatic heterocyclic groups include C4-C20 aromatic heterocyclic groups containing at least one heteroatom such as a nitrogen atom, oxygen atom, or sulfur atom, such as furyl, pyrrolyl, thienyl, pyridinyl, thiazolyl, and benzothiazolyl groups, with furyl, thienyl, pyridinyl, thiazolyl, and benzothiazolyl groups being preferred.

[0083] Y 1 , Y 2 and Y 3 Each of these may independently be a substituted polycyclic aromatic hydrocarbon group or a polycyclic aromatic heterocyclic group. A polycyclic aromatic hydrocarbon group refers to a fused polycyclic aromatic hydrocarbon group or a group derived from an aromatic ring assembly. A polycyclic aromatic heterocyclic group refers to a fused polycyclic aromatic heterocyclic group or a group derived from an aromatic ring assembly.

[0084] Z 0 , Z 1 and Z 2 Each of these is preferably independently a hydrogen atom, a halogen atom, a C1-C12 alkyl group, a cyano group, a nitro group, or a C1-C12 alkoxy group, Z 0 A hydrogen atom, an alkyl group having 1 to 12 carbon atoms, and a cyano group are more preferably Z 1 and Z 2 Hydrogen atoms, fluorine atoms, chlorine atoms, methyl groups, and cyano groups are more preferred.

[0085] Q 1 Q 2 and Q 3 -NH-, -S-, -NR2’ -, -O- is preferred, R 2’ A hydrogen atom is preferred. Among these, -S-, -O-, and -NH- are particularly preferred.

[0086] Among formulas (Ar-1) to (Ar-23), formulas (Ar-6) and (Ar-7) are preferred from the viewpoint of molecular stability. In equations (Ar-16) to (Ar-23), Y 1 This is the nitrogen atom and Z to which it is bonded. 0 It may also form an aromatic heterocyclic group. Examples of aromatic heterocyclic groups that Ar may have include those mentioned above, such as a pyrrole ring, imidazole ring, pyrroline ring, pyridine ring, pyrazine ring, pyrimidine ring, indole ring, quinoline ring, isoquinoline ring, purine ring, pyrrolidine ring, etc. This aromatic heterocyclic group may have substituents. Also, Y 1 This is the nitrogen atom and Z to which it is bonded. 0 In addition, the aforementioned substituted polycyclic aromatic hydrocarbon groups or polycyclic aromatic heterocyclic groups may also be used. Examples include benzofuran rings, benzothiazole rings, and benzoxazole rings.

[0087] (Compounds containing a group represented by formula (X)) Formula (X) is as follows. Hereinafter, compounds containing the group represented by formula (X) are sometimes referred to as polymerizable liquid crystals (B). P11-B11-E11-B12-A11-B13- (X)

[0088] [In formula (X), P11 represents a polymerizable group. A11 represents a divalent alicyclic hydrocarbon group or a divalent aromatic hydrocarbon group. The hydrogen atoms in the divalent alicyclic hydrocarbon group and the divalent aromatic hydrocarbon group are substituted with halogen atoms, C1-C6 alkyl groups, C1-C6 alkoxy groups, cyano groups, or nitro groups. It is also possible that the C1-C6 alkyl group and the C1-C6 alkoxy group may be substituted with fluorine atoms. B11 is -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, -CO-NR 16 -, -NR 16 -CO-, -CO-, -CS-, or single bond. 16 This represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. B12 and B13 are independently -C≡C-, -CH=CH-, -CH2-CH2-, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -OC(=O)-O-, -CH=N-, -N=CH-, -N=N-, -C(=O)-NR 16 -, -NR 16 -C(=O)-, -OCH2-, -OCF2-, -CH2O-, -CF2O-, -CH=CH-C(=O)-O-, -OC(=O)-CH=CH-, or a single bond. E11 represents an alkanediyl group having 1 to 12 carbon atoms. The hydrogen atoms in the alkanediyl group may be substituted with an alkoxy group having 1 to 5 carbon atoms, and the hydrogen atoms in the alkoxy group may be substituted with a halogen atom. Furthermore, the -CH2- group constituting the alkanediyl group may be replaced with -O- or -CO-.

[0089] The number of carbon atoms in the aromatic hydrocarbon group and alicyclic hydrocarbon group of A11 is preferably in the range of 3 to 18, more preferably in the range of 5 to 12, and particularly preferably 5 or 6. As A11, cyclohexane-1,4-diyl group and 1,4-phenylene group are preferred.

[0090] As E11, a linear alkanediyl group having 1 to 12 carbon atoms is preferred. The -CH2- group constituting the alkanediyl group may be replaced with -O-. Specifically, examples include linear alkanediyl groups having 1 to 12 carbon atoms, such as methylene group, ethylene group, propane-1,3-diyl group, butane-1,4-diyl group, pentane-1,5-diyl group, hexane-1,6-diyl group, heptane-1,7-diyl group, octane-1,8-diyl group, nonane-1,9-diyl group, decane-1,10-diyl group, undecane-1,11-diyl group, and dodecane-1,12-diyl group; and -CH2-CH2-O-CH2-CH2-, -CH2-CH2-O-CH2-CH2-O-CH2-CH2-, and -CH2-CH2-O-CH2-CH2-O-CH2-CH2-. For B11, -O-, -S-, -CO-O-, and -O-CO- are preferred, with -CO-O- being the most preferred among them. For B12 and B13, independently, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, and -OC(=O)-O- are preferred, with -O- or -OC(=O)-O- being more preferred.

[0091] As for the polymerizable group represented by P11, radical polymerizable groups or cationic polymerizable groups are preferred in terms of high polymerization reactivity, particularly photopolymerization reactivity, and are easy to handle, as well as the liquid crystal compound itself is easy to manufacture. Therefore, the polymerizable group is preferably a group represented by the following formulas (P-11) to (P-15).

[0092] [ka] [In formulas (P-11) to (P-15), R 17 ~R 21 Each of these independently represents an alkyl group or hydrogen atom having 1 to 6 carbon atoms.

[0093] Specific examples of the groups represented by equations (P-11) to (P-15) include the groups represented by equations (P-16) to (P-20) below.

[0094] [ka]

[0095] P11 is preferably a group represented by formulas (P-14) to (P-20), and more preferably a vinyl group, a p-stilbene group, an epoxy group, or an oxetanyl group. It is even more preferable that the group represented by P11-B11- is an acryloyloxy group or a methacryloyloxy group.

[0096] Polymerizable liquid crystals (B) include compounds represented by formulas (I), (II), (III), (IV), (V), or (VI). P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-B16-E12-B17-P12 (I) P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-F11 (II) P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-E12-B17-P12 (III) P11-B11-E11-B12-A11-B13-A12-B14-A13-F11 (IV) P11-B11-E11-B12-A11-B13-A12-B14-E12-B17-P12 (V) P11-B11-E11-B12-A11-B13-A12-F11 (VI) (In the formula, A12 to A14 are each independently synonymous with A11, B14 to B16 are each independently synonymous with B12, B17 is synonymous with B11, and E12 is synonymous with E11. F11 represents a hydrogen atom, a C1-C13 alkyl group, a C1-C13 alkoxy group, a cyano group, a nitro group, a trifluoromethyl group, a dimethylamino group, a hydroxyl group, a methylol group, a formyl group, a sulfo group (-SO3H), a carboxyl group, a C1-C10 alkoxycarbonyl group, or a halogen atom, and the -CH2- group constituting the alkyl and alkoxy groups may be replaced with -O-.

[0097] Specific examples of polymerizable liquid crystals (B) include compounds having polymerizable groups among the compounds described in "3.8.6 Network (Fully Crosslinked Type)" and "6.5.1 Liquid Crystal Materials b. Polymerizable Nematic Liquid Crystal Materials" of the Liquid Crystal Handbook (edited by the Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 2000), as well as polymerizable liquid crystals described in Japanese Patent Publication No. 2010-31223, Japanese Patent Publication No. 2010-270108, Japanese Patent Publication No. 2011-6360, and Japanese Patent Publication No. 2011-207765.

[0098] Specific examples of polymerizable liquid crystals (B) include compounds represented by the following formulas (I-1) to (I-4), (II-1) to (II-4), (III-1) to (III-26), (IV-1) to (IV-26), (V-1) to (V-2), and (VI-1) to (VI-6). In the following formulas, k1 and k2 are independently 2- Represents the integer 12. These polymerizable liquid crystals (B) are preferred in terms of their ease of synthesis or availability.

[0099] [ka]

[0100] [ka]

[0101] [ka]

[0102] [ka]

[0103] [ka]

[0104] [ka]

[0105] [ka]

[0106] [ka]

[0107] [ka]

[0108] Examples of disc-shaped polymerizable liquid crystals include compounds containing a group represented by formula (W) (hereinafter sometimes referred to as polymerizable liquid crystal (C)).

[0109] [ka] [In formula (W), R 40 This represents the following equations (W-1) to (W-5).

[0110] [ka]

[0111] X 40 and Z 40 This represents an alkanediyl group having 1 to 12 carbon atoms, and the hydrogen atoms in the alkanediyl group may be substituted with an alkoxy group having 1 to 5 carbon atoms, or the hydrogen atoms in the alkoxy group may be substituted with a halogen atom. Furthermore, the -CH2- constituting the alkanediyl group may be replaced with -O- or -CO-. .

[0112] A specific example of polymerizable liquid crystal (C) is found in "6.5.1 Liquid Crystal Materials b. Polymerizable Nematic Liquid Crystal Materials" in the Liquid Crystal Handbook (edited by the Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 2000). Examples include the compounds described in "Figure 6.21", and the polymerizable liquid crystals described in Japanese Patent Publication No. 7-258170, Japanese Patent Publication No. 7-30637, Japanese Patent Publication No. 7-309807, and Japanese Patent Publication No. 8-231470.

[0113] A phase difference plate 30 having optical properties represented by formulas (1) and (2) can be obtained by polymerizing a polymerizable liquid crystal having a specific structure, stretching a polymer film having a specific structure, or by combining a layer having optical properties represented by formulas (4), (6), and (7) with a layer having optical properties represented by formulas (5), (6), and (7) in a specific slow axis relationship. Re(450) / Re(550)≦1.00 (1) 1.00 ≤ Re(650) / Re(550) (2) 100nm <Re(550)<160nm (4) 200nm <Re(550)<320nm (5) Re(450) / Re(550)≧1.00 (6) 1.00 ≥ Re(650) / Re(550) (7)

[0114] The phase difference plate 30 preferably has optical properties represented by formulas (1) and (2). When the phase difference plate 30 has optical properties represented by formulas (1) and (2), uniform polarization conversion characteristics can be obtained for light of each wavelength in the visible light range, and light leakage can be suppressed when displaying black in a display device such as an organic EL display device.

[0115] Examples of the polymerizable liquid crystal having the specific structure include the aforementioned polymerizable liquid crystal (A). By aligning the polymerizable liquid crystal (A) such that its optical axis is horizontal with respect to the flat surface of the substrate, a retardation layer having the optical properties represented by formula (1) and formula (2) is obtained, and further, by adjusting the film thickness in accordance with the aforementioned formula (10), a retardation layer having a desired in-plane retardation value such as the optical property represented by formula (4) can be obtained. 100nm<Re(550)<160nm (4)

[0116] Examples of the method of combining the layer having the optical properties represented by formulae (4), (6) and (7) and the layer having the optical properties represented by formulae (5), (6) and (7) in a specific slow axis relationship include well-known methods. For example, JP-A 2001-4837, JP-A 2001-21720 and JP-A 2000-206331 disclose retardation films having at least two retardation layers composed of liquid crystal compounds.

[0117] The retardation layer having the optical properties represented by the aforementioned formulae (6) and (7) can be obtained by a well-known method. That is, retardation layers obtained by methods other than the method for obtaining the retardation layer having the optical properties represented by the aforementioned formulae (1) and (2) generally have the optical properties represented by formulae (6) and (7).

[0118] (First Retardation Layer) The first retardation layer 31 preferably has the optical property represented by formula (4) (in the present specification, a retardation layer satisfying the optical property represented by formula (4) is also referred to as a "λ / 4 layer"), and more preferably has the optical property represented by formula (4-1). The in-plane retardation value Re(550) can be adjusted by the same method as the aforementioned method for adjusting the in-plane retardation value of the retardation layer. 100nm<Re(550)<160nm (4) 130nm<Re(550)<150nm (4-1)

[0119] Furthermore, the first phase difference layer preferably has optical properties represented by formulas (1) and (2) (in this specification, the optical properties represented by formulas (1) and (2) are also referred to as "reverse dispersion"). Such optical properties can be obtained in the same manner as the phase difference layer described above. Re(450) / Re(550)≦1.00 (1) 1.00 ≤ Re(650) / Re(550) (2)

[0120] Furthermore, the first phase difference layer preferably comprises layer A having optical properties represented by formulas (4), (6), and (7), and layer B having optical properties represented by formulas (5), (6), and (7). Such optical properties can be obtained in the same manner as the phase difference layer described above. 100nm <Re(550)<160nm (4) 200nm <Re(550)<320nm (5) Re(450) / Re(550)≧1.00 (6) 1.00 ≥ Re(650) / Re(550) (7) Layer A is preferably a layer having optical properties represented by formula (4-1), and layer B is preferably a layer having optical properties represented by formula (5-1). 130nm <Re(550)<150nm (4-1) 265nm <Re(550)<285nm (5-1)

[0121] Furthermore, if the phase difference plate has a third phase difference layer, the first phase difference layer preferably has optical properties represented by formulas (6) and (7). Such optical properties can be obtained in the same way as the phase difference layer described above. Re(450) / Re(550)≧1.00 (6) 1.00 ≥ Re(650) / Re(550) (7)

[0122] The first phase difference layer is a coating layer formed by polymerizing one or more polymerizable liquid crystals. When the first phase difference layer consists of one phase difference layer and has optical properties represented by formulas (1) and (2), it is preferable that such a phase difference layer is a coating layer formed by polymerizing polymerizable liquid crystal (A). When the second phase difference layer has optical properties represented by formulas (6) and (7), it is preferable that such a phase difference layer is a coating layer formed by polymerizing polymerizable liquid crystal (B).

[0123] Layer A is a coating layer preferably formed by polymerizing polymerizable liquid crystal (B). Layer B is a coating layer preferably formed by polymerizing polymerizable liquid crystal (C).

[0124] The first phase difference layer is a layer formed by polymerizing polymerizable liquid crystal, and its thickness is usually 20 μm or less, preferably 5 μm or less, and more preferably 0.5 μm to 3 μm. The thickness of the first phase difference layer can be determined by measurement using an interferometer, laser microscope, or stylus-type film thickness gauge.

[0125] (Second retardation layer) The second phase difference layer 32 preferably has optical properties represented by formula (3) (positive C plate). nx≒ny <nz (3)

[0126] The in-plane phase difference value Re(550) of the second phase difference layer is typically in the range of 0 to 10 nm, preferably in the range of 0 to 5 nm. The phase difference value Rth in the thickness direction is typically in the range of -10 to -300 nm, preferably in the range of -20 to -200 nm. 550) and the phase difference value Rth in the thickness direction can be adjusted in the same way as the phase difference layer described above.

[0127] The second phase difference layer is a coating layer formed by polymerizing one or more polymerizable liquid crystals. More preferably, it is a coating layer formed by polymerizing polymerizable liquid crystal (B).

[0128] The second phase difference layer is a layer formed by polymerizing polymerizable liquid crystal, and its thickness is usually 10 μm or less, preferably 5 μm or less, and more preferably 0.3 μm to 3 μm. The thickness of the second phase difference layer can be determined by the same method as for the first phase difference layer. Furthermore, it is preferable that the thicknesses of both the first and second phase difference layers be 5 μm or less.

[0129] (Third retardation layer) The third phase difference layer preferably has optical properties represented by formula (5), and more preferably has optical properties represented by formula (5-1). The in-plane phase difference value Re(550) can be adjusted in the same manner as the method for adjusting the in-plane phase difference value of the above-mentioned phase difference layer. 200nm <Re(550)<320nm (5) 265nm <Re(550)<285nm (5-1)

[0130] Furthermore, the third phase difference layer preferably has optical properties represented by formulas (6) and (7). Such optical properties can be obtained in the same manner as the phase difference layer described above. Re(450) / Re(550)≧1.00 (6) 1.00 ≥ Re(650) / Re(550) (7)

[0131] The third phase difference layer is preferably a coating layer formed by polymerizing one or more polymerizable liquid crystals. More preferably, it is a coating layer formed by polymerizing polymerizable liquid crystal (B) or (C).

[0132] The third phase difference layer may be a stretched film. In the case of a stretched film, its thickness is usually 300 μm or less, preferably 5 μm to 100 μm, and more preferably 10 μm to 50 μm. If the third phase difference layer is a layer formed by polymerizing polymerizable liquid crystal, its thickness is usually 10 μm or less, preferably 5 μm or less, and more preferably 0.5 μm to 5 μm. The thickness of the third phase difference layer can be determined by the same method as for the first phase difference layer.

[0133] (base material) The phase difference plate 30 may have a base material. The base material is usually a transparent base material. A transparent base material means a base material that has transparency that can transmit light, especially visible light, and transparency refers to the characteristic that the transmittance for light rays with wavelengths of 380 to 780 nm is 80% or more. Specific transparent base materials include translucent resin base materials. Resins that constitute translucent resin base materials include polyolefins such as polyethylene and polypropylene; cyclic olefin resins such as norbornene polymers; polyvinyl alcohol; polyethylene terephthalate; polymethacrylate esters; polyacrylic acid esters; cellulose esters such as triacetylcellulose, diacetylcellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyethersulfone; polyetherketone; polyphenylene sulfide and polyphenylene oxide. From the viewpoint of availability and transparency, polyethylene terephthalate, polymethacrylate esters, cellulose esters, cyclic olefin resins, or polycarbonate are preferred.

[0134] The surface of the substrate on which the alignment film, first phase difference layer, second phase difference layer, and third phase difference layer are formed may be surface-treated before the alignment film or phase difference layer is formed. Examples of surface treatment methods include treating the substrate surface with corona or plasma under vacuum or atmospheric pressure, laser treatment of the substrate surface, ozone treatment of the substrate surface, saponification treatment of the substrate surface, or flame treatment of the substrate surface, primer treatment by applying a coupling agent to the substrate surface, and graft polymerization, in which reactive monomers or reactive polymers are attached to the substrate surface and then reacted by irradiation with radiation, plasma, or ultraviolet light. Among these, the method of treating the substrate surface with corona or plasma under vacuum or atmospheric pressure is preferred.

[0135] Methods for surface treatment of a substrate using corona or plasma include: placing the substrate between opposing electrodes under pressure near atmospheric pressure and generating corona or plasma to perform surface treatment on the substrate; flowing gas between opposing electrodes, plasmaizing the gas between the electrodes, and blowing the plasmaized gas onto the substrate; and generating glow discharge plasma under low pressure conditions to perform surface treatment on the substrate.

[0136] In particular, a preferred method involves placing a substrate between opposing electrodes under pressure near atmospheric pressure and generating corona or plasma to perform surface treatment on the substrate, or a preferred method involves flowing gas between opposing electrodes, converting the gas into plasma between the electrodes, and blowing the plasma-converted gas onto the substrate. Such surface treatment using corona or plasma is usually performed using commercially available surface treatment equipment.

[0137] A substrate with a small phase difference is preferred. Examples of substrates with a small phase difference include cellulose ester films that do not have a phase difference, such as ZeroTack (registered trademark) (Konica Minolta Opto, Inc.) and Z-Tack (Fujifilm Corporation). Unstretched cyclic olefin resin substrates are also preferred.

[0138] Furthermore, the surfaces of the substrate on which the alignment film, first phase difference layer, second phase difference layer, and third phase difference layer are not formed may be treated with a hard coat, antistatic treatment, etc. In addition, additives such as ultraviolet absorbers may be included to the extent that they do not affect the performance.

[0139] The thickness of the substrate is usually 5 to 300 μm, preferably 10 to 200 μm, because if it is too thin, the strength decreases and the processability tends to be poor.

[0140] (Polymerizable liquid crystal composition) A layer formed by polymerizing polymerizable liquid crystals (phase difference layer) is typically formed by applying a composition containing one or more polymerizable liquid crystals (hereinafter sometimes referred to as a polymerizable liquid crystal composition) onto a substrate, alignment film, protective layer, or phase difference layer, and polymerizing the polymerizable liquid crystals in the resulting coating film.

[0141] Polymerizable liquid crystal compositions typically contain a solvent, and the solvent is preferably one that can dissolve the polymerizable liquid crystal and is inert to the polymerization reaction of the polymerizable liquid crystal. Specific examples of solvents include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, propylene glycol monomethyl ether, and phenol; ester solvents such as ethyl acetate and butyl acetate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, cycloheptanone, methyl amyl ketone, methyl isobutyl ketone, and N-methyl-2-pyrrolidinone; non-chlorinated aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; non-chlorinated aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as propylene glycol monomethyl ether, tetrahydrofuran, and dimethoxyethane; and chlorinated hydrocarbon solvents such as chloroform and chlorobenzene. These other solvents may be used individually or in combination.

[0142] The solvent content in a polymerizable liquid crystal composition is usually preferably 10 to 10,000 parts by mass, and more preferably 50 to 5,000 parts by mass, per 100 parts by mass of solids. Solids refer to the total amount of components in the polymerizable liquid crystal composition excluding the solvent.

[0143] Polymerizable liquid crystal compositions are typically applied by known methods such as spin coating, extrusion, gravure coating, die coating, slit coating, bar coating, and applicator coating, as well as printing methods such as flexographic coating. After application, a dry film is usually formed by removing the solvent under conditions that prevent polymerization of the polymerizable liquid crystals contained in the resulting coating film. Drying methods include natural drying, forced-air drying, heat drying, and reduced-pressure drying.

[0144] (Orientation film) In this specification, an alignment film is a film that has an alignment-regulating force that causes polymerizable liquid crystals to be liquid crystal oriented in a desired direction. Preferably, the alignment film has solvent resistance that prevents dissolution by coating with polymerizable liquid crystal compositions, and also has heat resistance for solvent removal and heat treatment for alignment of polymerizable liquid crystals. Examples of such alignment films include alignment films containing aligning polymers, photoalignment films, and groove alignment films that form uneven patterns or multiple grooves on their surface for alignment.

[0145] Examples of oriented polymers include polyamides and gelatins having amide bonds in their molecules, polyimides having imide bonds in their molecules and their hydrolysates such as polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among these, polyvinyl alcohol is preferred. Two or more oriented polymers may be used in combination.

[0146] Orientation films containing oriented polymers are typically obtained by applying a composition in which the oriented polymer is dissolved in a solvent (hereinafter sometimes referred to as the oriented polymer composition) to a substrate and removing the solvent, or by applying the oriented polymer composition to a substrate, removing the solvent, and then rubbing (rubbing method).

[0147] Examples of the aforementioned solvents include water, methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; and chlorinated hydrocarbon solvents such as chloroform and chlorobenzene. These solvents may be used individually or in combination of two or more.

[0148] The concentration of the oriented polymer in the oriented polymer composition should be within a range in which the oriented polymer material can be completely dissolved in the solvent, but it is preferably 0.1 to 20% in terms of solid content relative to the solution, and more preferably 0.1 to 10%.

[0149] As the oriented polymer composition, commercially available orientation film materials may be used as is. Examples of commercially available orientation film materials include SunEver (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark). Examples include trademarks (manufactured by JSR Corporation).

[0150] Methods for applying an oriented polymer composition to a substrate include known methods such as spin coating, extrusion, gravure coating, die coating, slit coating, bar coating, and applicator coating, as well as printing methods such as flexographic coating. When this optical film is manufactured by the continuous Roll-to-Roll manufacturing method described later, the application method typically employs gravure coating, die coating, or printing methods such as flexographic coating.

[0151] Methods for removing solvents contained in oriented polymer compositions include natural drying, forced-air drying, heat drying, and reduced-pressure drying.

[0152] To impart orientation-regulating force to the orientation film, rubbing can be performed as needed (rubbing method).

[0153] One method for imparting orientation-regulating force by the rubbing method involves wrapping a rubbing cloth around a rotating rubbing roll and bringing into contact with the oriented polymer film formed on the substrate surface by applying an oriented polymer composition to the substrate and annealing it.

[0154] To impart alignment-regulating force to the alignment film, photo-alignment can be performed as needed (photo-alignment method).

[0155] Photoalignment films are typically obtained by applying a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter sometimes referred to as a "photoalignment film forming composition") to a substrate and irradiating it with light (preferably polarized UV). Photoalignment films are more preferable in that the direction of the alignment restricting force can be arbitrarily controlled by selecting the polarization direction of the irradiated light.

[0156] A photoreactive group is a group that generates liquid crystal alignment ability upon light irradiation. Specifically, this includes groups involved in photoreactions that are the origin of liquid crystal alignment ability, such as molecular orientation induction or isomerization reactions, dimerization reactions, photocrosslinking reactions, or photodegradation reactions, which are induced by light irradiation. Among these, groups involved in dimerization reactions or photocrosslinking reactions are preferred because they exhibit excellent orientation properties. As a photoreactive group, groups having unsaturated bonds, especially double bonds, are preferred, and groups having at least one selected from the group consisting of carbon-carbon double bonds (C=C bonds), carbon-nitrogen double bonds (C=N bonds), nitrogen-nitrogen double bonds (N=N bonds), and carbon-oxygen double bonds (C=O bonds) are particularly preferred.

[0157] Photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazole groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having an azoxybenzene structure. Photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, allyl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.

[0158] Among these, photoreactive groups involved in the photodimerization reaction are preferred, and cinnamoyl groups and chalcone groups are preferred because they require a relatively small amount of polarized irradiation for photo-orientation, and it is easy to obtain a photo-orientation film with excellent thermal stability and chronological stability. Examples of polymers having photoreactive groups include: Particularly preferred are polymers having cinnamoyl groups such that the terminal portion of the polymer side chain has a cinnamic acid structure.

[0159] A photo-alignment film-forming composition can be applied to a substrate to form a photo-alignment-inducing layer on the substrate. The solvent included in the composition is similar to that included in the above-mentioned aligning polymer composition, and can be appropriately selected depending on the solubility of the polymer or monomer having photoreactive groups.

[0160] The content of photo-alignment film-forming polymers or monomers having photoreactive groups in the photo-alignment film-forming composition can be appropriately adjusted depending on the type of polymer or monomer and the desired thickness of the photo-alignment film, but it is preferably at least 0.2% by mass, and more preferably in the range of 0.3 to 10% by mass. The photo-alignment film-forming composition may also contain polymer materials such as polyvinyl alcohol or polyimide, or photosensitizers, as long as the properties of the photo-alignment film are not significantly impaired.

[0161] Methods for applying the photo-alignment film-forming composition to a substrate include those similar to those for applying an oriented polymer composition to a substrate. Methods for removing the solvent from the applied photo-alignment film-forming composition include, for example, those similar to those for removing the solvent from an oriented polymer composition.

[0162] To irradiate with polarized light, the polarized UV light may be directly irradiated onto a photo-alignment film-forming composition coated on a substrate from which the solvent has been removed, or polarized light may be irradiated from the substrate side and transmitted through to the surface. Furthermore, it is particularly preferable that the polarized light is substantially parallel light. The wavelength of the polarized light to be irradiated should be in the wavelength range in which the photoreactive groups of the polymer or monomer having photoreactive groups can absorb light energy. Specifically, UV (ultraviolet) light in the wavelength range of 250 to 400 nm is particularly preferred. Examples of light sources used for this polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, and ultraviolet light lasers such as KrF and ArF, with high-pressure mercury lamps, ultra-high-pressure mercury lamps and metal halide lamps being more preferred. These lamps are preferred because they have a high emission intensity of ultraviolet light at a wavelength of 313 nm. Polarized UV light can be irradiated by passing the light from the light source through a suitable polarizer. Such polarizers can include polarizing filters, polarizing prisms such as Grant-Thomson and Grant-Teller, and wire grid type polarizers.

[0163] Furthermore, by applying masking during rubbing or polarized irradiation, it is possible to form multiple regions (patterns) with different liquid crystal orientation directions.

[0164] Glue-aligned films are films in which liquid crystal alignment is achieved through a surface pattern of irregularities or multiple grooves. HV Kennel et al. reported that when liquid crystal molecules are placed on a substrate having multiple equally spaced linear grooves, the liquid crystal molecules align in the direction along the grooves (Physical Review A24(5), p. 2713, 1981).

[0165] Specific examples of obtaining a groove-aligned film include a method of exposing a photosensitive polyimide surface through an exposure mask having a periodic pattern of slits, followed by development and rinsing to remove the unwanted polyimide film and form an uneven pattern; a method of forming a UV-curable resin layer on a plate-shaped master disc having grooves on its surface, transferring the resin layer to a substrate film, and then curing it; and a method of transporting a substrate film on which a UV-curable resin layer has been formed, pressing a roll-shaped master disc having multiple grooves against the surface of the UV-curable resin layer to form unevenness, and then curing it. Methods such as those described in Japanese Patent Publication No. 6-34976 and Japanese Patent Publication No. 2011-242743 can be used.

[0166] Among the above methods, the method of pressing a roll-shaped master plate having multiple grooves against the surface of a UV-curable resin layer to form irregularities and then curing is preferred. From the viewpoint of durability, stainless steel (SUS) can be used as the roll-shaped master plate.

[0167] As the UV-curing resin, polymers of monofunctional acrylates, polymers of polyfunctional acrylates, or polymers of mixtures thereof can be used. A monofunctional acrylate is a compound that has one group selected from the group consisting of acryloyloxy groups (CH2=CH-COO-) and methacryloyloxy groups (CH2=C(CH3)-COO-) (hereinafter sometimes referred to as a (meth)acryloyloxy group) in its molecule.

[0168] Examples of monofunctional acrylates having one (meth)acryloyloxy group include C4 to C16 alkyl (meth)acrylates, C2 to C14 β-carboxyalkyl (meth)acrylates, C2 to C14 alkylated phenyl (meth)acrylates, methoxypolyethylene glycol (meth)acrylates, phenoxypolyethylene glycol (meth)acrylates, and isobonyl (meth)acrylates.

[0169] Polyfunctional acrylates are typically compounds that have two to six (meth)acryloyloxy groups in their molecule.

[0170] Examples of difunctional acrylates having two (meth)acryloyloxy groups include 1,3-butanediol di(meth)acrylate; 1,3-butanediol (meth)acrylate; 1,6-hexanediol di(meth)acrylate; ethylene glycol di(meth)acrylate; diethylene glycol di(meth)acrylate; neopentyl glycol di(meth)acrylate; triethylene glycol di(meth)acrylate; tetraethylene glycol di(meth)acrylate; polyethylene glycol diacrylate; bis(acryloyloxyethyl) ether of bisphenol A; ethoxylated bisphenol A di(meth)acrylate; propoxylated neopentyl glycol di(meth)acrylate; ethoxylated neopentyl glycol di(meth)acrylate and 3-methylpentanediol di(meth)acrylate.

[0171] Polyfunctional acrylates having 3 to 6 (meth)acryloyloxy groups include: trimethylolpropane tri(meth)acrylate; pentaerythritol tri(meth)acrylate; tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate; ethoxylated trimethylolpropane tri(meth)acrylate; propoxylated trimethylolpropane tri(meth)acrylate; pentaerythritol tetra(meth)acrylate; dipentaerythritol penta(meth)acrylate; dipentaerythritol hexa(meth)acrylate; tripentaerythritol tetra(meth)acrylate; tripentaerythritol penta(meth)acrylate; tripentaerythritol hexa(meth)acrylate; tripentaerythritol hepta(meth)acrylate; tripentaerythritol octa(meth)acrylate Reactates; reaction products of pentaerythritol tri(meth)acrylate and acid anhydrides; reaction products of dipentaerythritol penta(meth)acrylate and acid anhydrides; reaction products of tripentaerythritol hepta(meth)acrylate and acid anhydrides; caprolactone-modified trimethylolpropane tri(meth)acrylate; caprolactone-modified pentaerythritol tri(meth)acrylate; caprolactone-modified tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate; caprolactone-modified pentaerythritol tetra(meth)acrylate; caprolactone-modified dipentaerythritol penta(meth)acrylate; caprolactone-modified dipentaerythritol hexa(meth)acrylate; caprolactone-modified tripentaerythritol tetra(meth)acrylate; caprolactone-modified tripentaerythritol penta( Examples include meth)acrylate; caprolactone-modified tripentaerythritol hexa(meth)acrylate; caprolactone-modified tripentaerythritol hepta(meth)acrylate; caprolactone-modified tripentaerythritol octa(meth)acrylate; reaction products of caprolactone-modified pentaerythritol tri(meth)acrylate and acid anhydrides; reaction products of caprolactone-modified dipentaerythritol penta(meth)acrylate and acid anhydrides; and caprolactone-modified tripentaerythritol hepta(meth)acrylate and acid anhydrides. In the specific examples of polyfunctional acrylates shown herein, (meth)acrylate means acrylate or methacrylate. Furthermore, caprolactone-modified means that an open-ring form or polymer of caprolactone is introduced between the alcohol-derived part of the (meth)acrylate compound and the (meth)acryloyloxy group.

[0172] Commercially available polyfunctional acrylates can also be used. Examples of such commercially available products include A-DOD-N, A-HD-N, A-NOD-N, APG-100, APG-200, APG-400, A-GLY-9E, A-GLY-20E, A-TMM-3, A-TMPT, AD-TMP, ATM-35E, A-TMMT, A-9550, A-DPH, HD-N, NOD-N, NPG, TMPT (manufactured by Shin-Nakamura Chemical Co., Ltd.), "ARONIX M-220", "M-325", "M-240", "M-270", "M-309", "M-310", "M-321", "M-350", "M-360", and "M Examples include -305”, M-306, M-450, M-451, M-408, M-400, M-402, M-403, M-404, M-405, M-406 (manufactured by Toagosei Co., Ltd.), EBECRYL11, EBECRYL145, EBECRYL150, EBECRYL140, EBECRYL180

[0173] The groove alignment film preferably has a convex width of 0.05 to 5 μm, a concave width of 0.1 to 5 μm, and a step depth of 2 μm or less, preferably 0.01 to 1 μm or less. Within this range, a liquid crystal alignment with minimal orientation disorder can be obtained.

[0174] The thickness of the orientation film is typically in the range of 10 nm to 10,000 nm, preferably in the range of 10 nm to 1,000 nm, more preferably 500 nm or less, and even more preferably in the range of 10 nm to 500 nm.

[0175] The liquid crystal orientation of polymerizable liquid crystals is controlled by the properties of the alignment film and the polymerizable liquid crystal. For example, if the alignment film is made of a material that exhibits a horizontal alignment restricting force, the polymerizable liquid crystal can form a horizontal or hybrid alignment. If the material exhibits a vertical alignment restricting force, the polymerizable liquid crystal can form a vertical or tilted alignment. The alignment restricting force can be arbitrarily adjusted by the surface state and rubbing conditions if the alignment film is made of an alignment polymer, and by polarization irradiation conditions, etc., if it is made of a photo-aligning polymer. Furthermore, the liquid crystal orientation can also be controlled by selecting physical properties such as surface tension and liquid crystalline properties of the polymerizable liquid crystal.

[0176] Polymerization of polymerizable liquid crystals can be carried out by known methods for polymerizing compounds having polymerizable functional groups. Specifically, thermal polymerization and photopolymerization are mentioned, and photopolymerization is preferred from the viewpoint of ease of polymerization. When polymerizing polymerizable liquid crystals by photopolymerization, it is preferable to apply a polymerizable liquid crystal composition containing a photopolymerization initiator, dry the resulting dried film to bring the polymerizable liquid crystal in the liquid crystal phase state, and then perform photopolymerization while maintaining the liquid crystal state.

[0177] Photopolymerization is usually carried out by irradiating a dried coating film with light. The light to be irradiated is appropriately selected according to the type of photopolymerization initiator contained in the dried coating film, the type of polymerizable liquid crystal (particularly, the type of photopolymerizable group possessed by the polymerizable liquid crystal), and the amount thereof, and specific examples thereof include light selected from the group consisting of visible light, ultraviolet light, and laser light, as well as active electron beams. Among these, ultraviolet light is preferred from the viewpoints that the progress of the polymerization reaction is easy to control, and that apparatuses widely used in the art as photopolymerization apparatuses can be used, and it is preferable to select the types of the polymerizable liquid crystal and the photopolymerization initiator such that photopolymerization can be performed with ultraviolet light. Further, during polymerization, the polymerization temperature can also be controlled by performing light irradiation while cooling the dried coating film with an appropriate cooling means. By employing such a cooling means and carrying out the polymerization of the polymerizable liquid crystal at a lower temperature, the retardation layer can be appropriately formed even when a substrate having relatively low heat resistance is used. During photopolymerization, a patterned retardation layer can also be obtained by performing masking, development, or the like.

[0178] The polymerizable liquid crystal composition may contain a reactive additive. As the reactive additive, those having a carbon-carbon unsaturated bond and an active hydrogen-reactive group in the molecule are preferable. The term "active hydrogen-reactive group" as used herein means a group having reactivity with a group having active hydrogen, such as a carboxyl group (-COOH), a hydroxyl group (-OH), and an amino group (-NH2), and representative examples thereof include a glycidyl group, an oxazoline group, a carbodiimide group, an aziridine group, an imide group, an isocyanate group, a thioisocyanate group, and a maleic anhydride group. The number of each of the carbon-carbon unsaturated bonds and the active hydrogen-reactive groups contained in the reactive additive is usually 1 to 20, and preferably 1 to 10.

[0179] In the reactive additive, it is preferable that at least two active hydrogen-reactive groups are present, and in this case, the plurality of active hydrogen-reactive groups may be the same or different.

[0180] The carbon-carbon unsaturated bond possessed by the reactive additive may be a carbon-carbon double bond, a carbon-carbon triple bond, or a combination thereof, and is preferably a carbon-carbon double bond. Above all, the reactive additive preferably contains a carbon-carbon unsaturated bond as a vinyl group and / or a (meth)acryl group. Further, the active hydrogen-reactive group is preferably at least one selected from the group consisting of an epoxy group, a glycidyl group and an isocyanate group, and a reactive additive having an acryl group and an isocyanate group is particularly preferred.

[0181] Specific examples of the reactive additive include compounds having a (meth)acryl group and an epoxy group, such as methacryloxyglycidyl ether and acryloxyglycidyl ether; compounds having a (meth)acryl group and an oxetane group, such as oxetane acrylate and oxetane methacrylate; compounds having a (meth)acryl group and a lactone group, such as lactone acrylate and lactone methacrylate; compounds having a vinyl group and an oxazoline group, such as vinyloxazoline and isopropenyloxazoline; and oligomers of compounds having a (meth)acryl group and an isocyanate group, such as isocyanatomethyl acrylate, isocyanatomethyl methacrylate, 2-isocyanatoethyl acrylate and 2-isocyanatoethyl methacrylate. Further, compounds having a vinyl group or vinylene group and an acid anhydride, such as methacrylic anhydride, acrylic anhydride, maleic anhydride and vinyl maleic anhydride, may be mentioned. Among these, methacryloxyglycidyl ether, acryloxyglycidyl ether, isocyanatomethyl acrylate, isocyanatomethyl methacrylate, vinyloxazoline, 2-isocyanatoethyl acrylate, 2-isocyanatoethyl methacrylate and the aforementioned oligomers are preferred, and isocyanatomethyl acrylate, 2-isocyanatoethyl acrylate and the aforementioned oligomers are particularly preferred.

[0182] Specifically, a compound represented by the following formula (Y) is preferred.

Chemical Formula

[0183] Among the reactive additives represented by the above formula (Y), the compound represented by the following formula (YY) (hereinafter sometimes referred to as compound (YY)) is particularly preferred (where n has the same meaning as above).

[0184] [ka] Compound (YY) can be used as is from a commercially available product or purified as needed. An example of a commercially available product is Laromer® LR-9000 (manufactured by BASF).

[0185] If the polymerizable liquid crystal composition contains a reactive additive, its content is usually 0.1 to 30 parts by mass, preferably 0.1 to 5 parts by mass, per 100 parts by mass of polymerizable liquid crystal.

[0186] The polymerizable liquid crystal composition preferably contains one or more leveling agents. The leveling agents have the function of adjusting the fluidity of the polymerizable liquid crystal composition and making the coated film obtained by applying the polymerizable liquid crystal composition flatter, and specifically include surfactants. The leveling agent is preferably at least one selected from the group consisting of leveling agents mainly composed of polyacrylate compounds and leveling agents mainly composed of fluorine atom-containing compounds.

[0187] Leveling agents mainly composed of polyacrylate compounds include "BYK-350", "BYK-352", "BYK-353", "BYK-354", "BYK-355", "BYK-358N", "BYK-361N", "BYK-380", and "BYK-381 Examples include "BYK-392" [BYK Chemie].

[0188] Leveling agents mainly composed of fluorine atom-containing compounds include "Megafac® R-08", "R-30", "R-90", "F-410", "F-411", "F-443", "F-445", "F-470", "F-471", "F-477", "F-479", "F-482", and "F-483" [DIC Corporation]; "Surflon® S-381", "S-3 Examples include 82”, S-383”, S-393”, SC-101”, SC-105”, KH-40 and SA-100 [AGC Seimi Chemical Co., Ltd.]; E1830, E5844 [Daikin Fine Chemical Laboratories, Inc.]; F-Top EF301, F-Top EF303, F-Top EF351 and F-Top EF352 [Mitsubishi Materials Electronic Chemicals Co., Ltd.].

[0189] When the polymerizable liquid crystal composition contains a leveling agent, its content is preferably 0.01 parts by mass or more and 5 parts by mass or less, more preferably 0.05 parts by mass or more and 5 parts by mass or less, and even more preferably 0.05 parts by mass or more and 3 parts by mass or less, per 100 parts by mass of polymerizable liquid crystal. When the content of the leveling agent is within the above range, it is easy to orient the polymerizable liquid crystal horizontally, and the resulting polarized layer tends to be smoother. When the content of the leveling agent relative to the polymerizable liquid crystal is within the above range, unevenness tends to occur less in the resulting phase difference layer.

[0190] The polymerizable liquid crystal composition preferably contains one or more polymerization initiators. The polymerization initiator is a compound that can initiate the polymerization reaction of the polymerizable liquid crystal, and photopolymerization initiators are preferred because they can initiate the polymerization reaction under lower temperature conditions. Specifically, photopolymerization initiators that can generate active radicals or acids upon the action of light are mentioned, and among these, photopolymerization initiators that generate radicals upon the action of light are preferred.

[0191] Polymerization initiators include benzoin compounds, benzophenone compounds, alkylphenone compounds, acylphosphine oxide compounds, triazine compounds, iodonium salts, and sulfonium salts.

[0192] Examples of benzoin compounds include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether.

[0193] Examples of benzophenone compounds include benzophenone, o-methyl benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.

[0194] Examples of alkylphenone compounds include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1,2-diphenyl-2,2-dimethoxyethane-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexylphenyl ketone, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.

[0195] Examples of acylphosphine oxide compounds include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenyl Phosphine oxides are one example.

[0196] Examples of triazine compounds include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)ethenyl] Examples include -1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine.

[0197] Commercially available polymerization initiators can be used. Examples of commercially available polymerization initiators include "Irgacure (registered trademark) 907", "Irgacure (registered trademark) 184", "Irgacure (registered trademark) 651", "Irgacure (registered trademark) 819", "Irgacure (registered trademark) 250", "Irgacure (registered trademark) 369" (Chiba Japan Co., Ltd.); "Seiquall (registered trademark) BZ", "Seiquall (registered trademark) Z", and "Seiquall (registered trademark) Examples include the trademarks "BEE" (Seiko Chemicals Co., Ltd.), "Kayacure (registered trademark) BP100" (Nippon Kayaku Co., Ltd.), "Kayacure (registered trademark) UVI-6992" (manufactured by Dow Corporation), "ADEKA Optomer SP-152", "ADEKA Optomer SP-170" (ADEKA Corporation), "TAZ-A", "TAZ-PP" (Nippon Siber Hegner Ltd.), and "TAZ-104" (Sanwa Chemical Co., Ltd.).

[0198] When the polymerizable liquid crystal composition contains a polymerization initiator, the content thereof can be appropriately adjusted according to the type and amount of the polymerizable liquid crystal contained in the composition, and is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, still more preferably 0.5 to 8 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal. When the content of the polymerization initiator is within this range, the polymerizable liquid crystal can be polymerized without disturbing the alignment thereof.

[0199] When the polymerizable liquid crystal composition contains a photopolymerization initiator, the composition may further contain a photosensitizer. Examples of the photosensitizer include xanthone compounds such as xanthone and thioxanthone (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.); anthracene compounds such as anthracene and alkoxy group-containing anthracene (e.g., dibutoxyanthracene, etc.); phenothiazine and rubrene.

[0200] When the polymerizable liquid crystal composition contains a photopolymerization initiator and a photosensitizer, the polymerization reaction of the polymerizable liquid crystal contained in the composition can be further accelerated. The usage amount of the photosensitizer can be appropriately adjusted according to the types and amounts of the photopolymerization initiator and the polymerizable liquid crystal, and is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, still more preferably 0.5 to 8 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal.

[0201] In order to allow the polymerization reaction of the polymerizable liquid crystal to proceed more stably, the polymerizable liquid crystal composition may contain an appropriate amount of a polymerization inhibitor, which makes it easy to control the progress degree of the polymerization reaction of the polymerizable liquid crystal.

[0202] Examples of the polymerization inhibitor include radical scavengers such as hydroquinone, alkoxy group-containing hydroquinone, alkoxy group-containing catechol (e.g., butylcatechol, etc.), pyrogallol, and 2,2,6,6-tetramethyl-1-piperidinyloxy radical; thiophenols; β-naphthylamines and β-naphthols.

[0203] When a polymerizable liquid crystal composition contains a polymerization inhibitor, its content can be appropriately adjusted depending on the type and amount of polymerizable liquid crystal, as well as the amount of photosensitizer used. However, 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass per 100 parts by mass of polymerizable liquid crystal are preferred. Within this range, polymerization can be carried out without disrupting the orientation of the polymerizable liquid crystal.

[0204] [Manufacturing method for phase difference plates] When manufacturing a phase difference plate, the order in which the first phase difference layer, the second phase difference layer, and the third phase difference layer are formed is arbitrary. Furthermore, the order in which layers A and B are formed in the first phase difference layer is also arbitrary.

[0205] A layer A may be formed on a substrate with or without an orientation film, a layer B may be formed on layer A with or without an orientation film, and a second phase difference layer may be formed on layer B with or without an orientation film. A layer B may be formed on the substrate with or without an orientation film, a layer A may be formed on layer B with or without an orientation film, and a second phase difference layer may be formed on layer A with or without an orientation film. A second phase difference layer may be formed on the substrate with or without an alignment film, layer A may be formed on the second phase difference layer with or without an alignment film, and layer B may be formed on layer A with or without an alignment film. A second phase difference layer is formed on the substrate with or without an alignment film, a layer B is formed on the second phase difference layer with or without an alignment film, and a layer B is formed on the layer B with an alignment film Layer A may be formed with or without intermediary. A layer A may be formed on one side of the substrate with or without an alignment film, a layer B may be formed on layer A with or without an alignment film, and a second phase difference layer may be formed on the other side of the substrate with or without an alignment film. A layer B may be formed on one side of the substrate with or without an orientation film, a layer A may be formed on layer B with or without an orientation film, and a second phase difference layer may be formed on the other side of the substrate with or without an orientation film.

[0206] If layer B is formed on layer A with or without an alignment film in between, or if layer A is formed on layer B with or without an alignment film in between, a protective layer may be present between layer A and layer B. Also, if layer A is formed on a second phase difference layer with or without an alignment film in between, if layer A is formed on a second phase difference layer with or without an alignment film in between, if a second phase difference layer is formed on layer A with or without an alignment film in between, or if a second phase difference layer is formed on layer B with or without an alignment film in between, a protective layer may be present between the second phase difference layer and layer A or layer B.

[0207] A first phase difference layer may be formed on a substrate with or without an alignment film, a second phase difference layer may be formed on the first phase difference layer with or without an alignment film, and a third phase difference layer may be formed on the second phase difference layer with or without an alignment film. A third phase difference layer may be formed on the substrate with or without an alignment film, a second phase difference layer may be formed on the third phase difference layer with or without an alignment film, and a first phase difference layer may be formed on the second phase difference layer with or without an alignment film. Alternatively, a first phase difference layer may be formed on one side of the substrate with or without an alignment film, a second phase difference layer may be formed on the first phase difference layer with or without an alignment film, and a third phase difference layer may be formed on the other side of the substrate with or without an alignment film. A second phase difference layer may be formed on one surface of the substrate with or without an alignment film, a first phase difference layer may be formed on the second phase difference layer with or without an alignment film, and a third phase difference layer may be formed on the other surface of the substrate with or without an alignment film. A third phase difference layer may be formed on one surface of the substrate with or without an alignment film, a second phase difference layer may be formed on the third phase difference layer with or without an alignment film, and a first phase difference layer may be formed on the other surface of the substrate with or without an alignment film. A second phase difference layer may be formed on one surface of the substrate with or without an alignment film, a third phase difference layer may be formed on the second phase difference layer with or without an alignment film, and a first phase difference layer may be formed on the other surface of the substrate with or without an alignment film.

[0208] A first phase difference layer may be formed on the substrate with or without an orientation film, and a second phase difference layer may be formed on the first phase difference layer with or without an orientation film. A second phase difference layer may be formed on one surface of the substrate with or without an alignment film, and a first phase difference layer may be formed on the second phase difference layer with or without an alignment film. A second phase difference layer may be formed on one surface of the substrate with or without an alignment film, and a first phase difference layer may be formed on the other surface of the substrate with or without an alignment film.

[0209] If a second phase difference layer is formed on the first phase difference layer with or without an alignment film, or if a first phase difference layer is formed on the second phase difference layer with or without an alignment film, a protective layer may be provided between the first phase difference layer and the second phase difference layer. Furthermore, if a third phase difference layer is formed on the second phase difference layer with or without an alignment film, or if a second phase difference layer is formed on the third phase difference layer with or without an alignment film, a protective layer may be provided between the second phase difference layer and the third phase difference layer.

[0210] (protective layer) The protective layer is preferably formed from a protective layer-forming composition containing an acrylic oligomer or polymer, such as polyfunctional acrylate (methacrylate), urethane acrylate, polyester acrylate, or epoxy acrylate; a water-soluble polymer, such as polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyvinylpyrrolidone, starches, methylcellulose, carboxymethylcellulose, or sodium alginate; and a solvent.

[0211] The solvents contained in the protective layer-forming composition are the same as those described above, and among them, at least one solvent selected from the group consisting of water, alcohol solvents, and ether solvents is preferred because it does not dissolve the layer forming the protective layer. Examples of alcohol solvents include methanol, ethanol, butanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether. Examples of ether solvents include ethylene glycol monomethyl ether acetate and propylene glycol monomethyl ether acetate. Among these, ethanol, isopropyl alcohol, propylene glycol monomethyl ether, and propylene glycol monomethyl ether acetate are preferred.

[0212] The thickness of the protective layer is usually 20 μm or less. Preferably, the thickness of the protective layer is 0.5 μm to 10 μm, and more preferably 1 μm to 5 μm. The thickness of the protective layer can usually be determined by measurement using an interferometer, laser microscope, or stylus-type film thickness gauge.

[0213] Next, a method for continuously manufacturing phase difference plates will be described. A suitable method for continuously manufacturing this optical film is the Roll-to-Roll method. Here, a method for manufacturing a phase difference layer formed by polymerizing polymerizable liquid crystal will be described, but a phase difference layer made of a stretched film may be used instead of a phase difference layer formed by polymerizing polymerizable liquid crystal. In this case, "coating a polymerizable liquid crystal composition" in the manufacturing process below should be read as "laminating a stretched film". Furthermore, while the manufacturing methods for typical configurations are illustrated below, other configurations may be manufactured in accordance with the methods described below.

[0214] (1) A process of preparing a roll in which the base material is wound onto a core, (2) A process of continuously feeding the substrate from the roll, (3) A step of continuously forming an orientation film on the substrate, (4) A step of applying a polymerizable liquid crystal composition onto the alignment film to continuously form a first phase difference layer; (5) A step of continuously forming a protective layer on the first phase difference layer obtained in (4); (6) A step of continuously forming an alignment film on the protective layer obtained in (5) above, (7) A step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (6) above to continuously form a second phase difference layer. (8) A method is to sequentially carry out the steps of winding the continuously obtained optical film onto a second core to obtain a second roll. Steps (3), (5), and (6) may be omitted as necessary, in which case "on the alignment film" in step (4) shall be read as "on the substrate", "the protective layer obtained in (5)" in step (6) shall be read as "the first phase difference layer", and "the alignment film obtained in (6)" in step (7) shall be read as "the first phase difference layer" or "the protective layer obtained in (5)". In addition, a protective film may be laminated during film transport in each step in order to suppress wrinkles and curls during transport.

[0215] Also, (1a) A step of preparing a roll in which the base material is wound onto a core, (2a) A step of continuously feeding the substrate from the roll, (3a) A step of continuously forming an orientation film on the substrate, (4a) A step of applying a polymerizable liquid crystal composition onto the alignment film to continuously form a second phase difference layer. (5a) A step of continuously forming a protective layer on the second phase difference layer obtained in (4a), (6a) A step of continuously forming an alignment film on the protective layer obtained in (5a), (7a) A step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (6a) above to continuously form a first phase difference layer. (8a) Another method involves sequentially winding the continuously obtained optical film onto a second core to obtain a second roll. Steps (3a), (5a), and (6a) may be omitted as needed, in which case "on the alignment film" in step (4a) shall be read as "on the substrate", "the protective layer obtained in (5a)" in step (6a) shall be read as "the second phase difference layer", and "the alignment film obtained in (6a)" in step (7a) shall be read as "the second phase difference layer" or "the protective layer obtained in (5a)". Furthermore, in order to suppress wrinkles and curls during transport, a protective film may be laminated during film transport in each step.

[0216] Also, (1b) A step of preparing a roll in which the base material is wound onto a core, (2b) A step of continuously feeding the substrate from the roll, (3b) A step of continuously forming an orientation film on the substrate, (4b) A step of applying a polymerizable liquid crystal composition onto the alignment film to continuously form a first phase difference layer. (5b) A step of continuously forming an orientation film on the substrate surface opposite to the first phase difference layer obtained in (4b), (6b) A step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (5b) above to continuously form a second phase difference layer. (7b) A method is also to sequentially perform the steps of (7b) winding the continuously obtained optical film onto a second core to obtain a second roll. Steps (3b) and (5b) may be omitted as needed, in which case "on the orientation film" in step (4b) will be replaced with "on the substrate", and step In (6b), "on the orientation film obtained in (5b)" shall be read as "the substrate surface opposite to the first phase difference layer obtained in (4b)". In addition, to suppress wrinkles and curls during transport, a protective film may be laminated during film transport in each process.

[0217] Also, (1c) A step of preparing a roll in which a transparent substrate is wound onto a core, (2c) A step of continuously feeding the transparent substrate from the roll, (3c) A step of continuously forming an orientation film on the transparent substrate, (4c) A step of applying a polymerizable liquid crystal composition onto the alignment film to continuously form a second phase difference layer. (5c) A step of continuously forming an orientation film on the substrate surface opposite to the second phase difference layer obtained in (4c), (6c) A step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (5c) above to continuously form a first phase difference layer. (7c) A method is also to sequentially perform the steps of (7c) winding the continuously obtained optical film onto a second core to obtain a second roll. Steps (3c) and (5c) may be omitted as necessary, in which case "on the orientation film" in step (4c) shall be read as "on the substrate," and "on the orientation film obtained in (5c)" in step (6c) shall be read as "the substrate surface opposite to the second phase difference layer obtained in (4c)." In addition, a protective film may be laminated to the film during film transport in each step in order to suppress wrinkles and curls during transport.

[0218] Also, (1d) A step of preparing a roll in which the base material is wound onto a core, (2d) A step of continuously feeding the substrate from the roll, (3d) A step of continuously forming an orientation film on the substrate, (4d) A step of applying a polymerizable liquid crystal composition onto the alignment film to continuously form layer A, (5d) A step of continuously forming a protective layer on the layer A obtained in (4d), (6d) A step of continuously forming an alignment film on the protective layer obtained in (5d), (7d) A step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (6d) above to continuously form layer B, (8d) A step of continuously forming a protective layer on the layer B obtained in (7d), (9d) A step of continuously forming an alignment film on the protective layer obtained in (8d), (10d) A step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (9d) above to continuously form a second phase difference layer. (11d) A method is to sequentially carry out the steps of winding the continuously obtained optical film onto a second core to obtain a second roll. Steps (3d), (5d), (6d), (8d), and (9d) may be omitted as necessary, in which case "on the alignment film" in step (4d) shall be read as "on the substrate", "the protective layer obtained in (5d)" in step (6d) shall be read as "the layer A", "the alignment film obtained in (6d)" in step (7d) shall be read as "the layer A" or "the protective layer obtained in (5d)", "the protective layer obtained in (8d)" in step (9d) shall be read as "the layer B", and "the alignment film obtained in (9d)" in step (10d) shall be read as "the layer B" or "the protective layer obtained in (9d)". In addition, a protective film may be laminated during film transport in each step in order to suppress wrinkles and curls during transport.

[0219] Also, (1e) A step of preparing a roll in which the base material is wound onto a core, (2e) A step of continuously feeding the substrate from the roll, (3e) A step of continuously forming an orientation film on the substrate, (4e) A step of applying a polymerizable liquid crystal composition onto the alignment film to continuously form a first phase difference layer. , (5e) A step of continuously forming a protective layer on the first phase difference layer obtained in (4e), (6e) A step of continuously forming an alignment film on the protective layer obtained in (5e), (7e) A step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (6e) above to continuously form a second phase difference layer. (8e) A step of continuously forming an orientation film on the substrate surface opposite to the first phase difference layer obtained in (4e), (9e) A step of applying a polymerizable liquid crystal composition onto the alignment film obtained in (8e) above to continuously form a third phase difference layer. (10e) Another method involves sequentially winding the continuously obtained optical film onto a second core to obtain a second roll. Steps (3e), (5e), ​​and (8e) may be omitted as necessary, in which case "on the orientation film" in step (4e) shall be read as "on the substrate", "the protective layer obtained in (5e)" in step (6e) shall be read as "the first phase difference layer obtained in (4e)", and "on the orientation film obtained in (8e)" in step (9e) shall be read as "the substrate surface opposite to the first phase difference layer obtained in (4e)". Furthermore, in order to suppress wrinkles and curls during transport, a protective film may be laminated during film transport in each step. Furthermore, in order to suppress wrinkles and curls during transport, a protective film may be laminated during film transport in each step.

[0220] Figure 2 is a schematic cross-sectional view illustrating a specific example of the phase difference plate 30. Figure 2(a) shows a phase difference plate 30 in which a first phase difference layer 31 and a second phase difference layer 32 are laminated. Figure 2(b) shows a phase difference plate 30 in which the base material 33, the first phase difference layer 31, and the second phase difference layer 32 are laminated in this order. Figure 2(c) shows a phase difference plate 30 in which the base material 33, the second phase difference layer 32, and the first phase difference layer 31 are laminated in this order. Figure 2(d) shows a phase difference plate 30 in which the first phase difference layer 31, the base material 33, and the second phase difference layer are laminated in this order.

[0221] By removing the base material 33 from the phase difference plate 30 having the base material 33, a phase difference plate 30 without a base material (Figure 2(a)) can be obtained.

[0222] Furthermore, the phase difference plate 30 can also be manufactured by bonding a substrate 33 having a first phase difference layer 31 to a substrate 33' having a second phase difference layer 32. Specific examples are shown in Figures 2(e), 2(f), and 2(g). A bonding layer (hereinafter, the bonding layer used for bonding between layers within the phase difference plate 30 will also be referred to as the "third bonding layer") can be used for bonding.

[0223] Figure 3 is a schematic cross-sectional view illustrating specific examples of a phase difference plate 30 when the first phase difference layer is composed of layers A and B, or when it has a third phase difference layer. Figure 3(a) shows a phase difference plate 30 in which layers A34, B35, and the second phase difference layer 32 are laminated in this order. Figure 3(b) shows a phase difference plate 30 in which layers B35, A34, and the second phase difference layer 32 are laminated in this order. Figure 3(c) shows a phase difference plate 30 in which the base material 33, layer A34, layer B35, and the second phase difference layer 32 are laminated in this order. Figure 3(d) shows a phase difference plate 30 in which the base material 33, the first phase difference layer 31, the second phase difference layer 32, and the third phase difference layer 38 are laminated in this order. Figure 3(e) shows a phase difference plate 30 in which the base material 33, layer B35, layer A34, and the second phase difference layer 32 are laminated in this order. Figure 3(f) shows a phase difference plate 30 in which the base material 33, third phase difference layer 38, second phase difference 32, and first phase difference layer 31 are laminated in this order. Figure 3(g) shows a phase difference plate 30 in which the base material 33, second phase difference 32, layer B35, and layer A34 are laminated in this order. Figure 3(h) shows a phase difference plate 30 in which the base material 33, second phase difference 32, layer A34, and layer B35 are laminated in this order. A phase difference plate 30 without a base material 33 (Figures 3(a), (b)) can also be obtained by peeling off the base material 33 from a phase difference plate 30 having a base material 33.

[0224] In the case of a configuration including a first phase difference layer 31, layer A34 and layer B35, or if a third phase difference layer 33 is present, each layer may be laminated on both sides of the base material 33. As a specific example, for example, Figure 3(i) shows a phase difference plate 30 in which a second phase difference layer 32, base material 33, layer A34 and layer B35 are laminated in this order. Figure 3(j) shows a phase difference plate 30 in which a second phase difference layer 32, base material 33, layer B35 and layer A34 are laminated in this order. Figure 3(k) shows a phase difference plate 30 in which a first phase difference layer 31, base material 33, third phase difference layer 38 and second phase difference layer 32 are laminated in this order. Figure 3(l) shows a phase difference plate 30 in which a first phase difference layer 31, base material 33, second phase difference layer 32 and third phase difference layer 38 are laminated in this order. Figure 3(m) shows a phase difference plate 30 in which the third phase difference layer 38, base material 33, first phase difference layer 31, and second phase difference layer 32 are laminated in this order. Figure 3(n) shows a phase difference plate 30 in which the third phase difference layer 38, base material 33, second phase difference layer 32, and first phase difference layer 31 are laminated in this order. The second phase difference layer 32, layer A34, and layer B35 may be formed by direct coating on each layer, the layers may be bonded together after manufacturing, or the layers may be laminated sequentially by transfer.

[0225] The phase difference plate 30 may have a configuration in which other layers are interposed between the first phase difference layer 31 and the second phase difference layer 32, or it may have a configuration in which other layers are not interposed. Examples of other interposed layers include the base material 33, the protective layer described above, the orientation film described above, and the third bonding layer. In configurations in which the phase difference plate 30 has only an orientation film as the other interposed layer between the first phase difference layer 31 and the second phase difference layer 32, or in configurations in which there are no other interposed layers, the puncture modulus tends to be 35 g / mm or more. In this specification, the layer interposed between the first phase difference layer 31 and the second phase difference layer 32 means the layer interposed between the outermost surface of the first phase difference layer 31 on the second phase difference layer 32 side and the outermost surface of the second phase difference layer 32 on the first phase difference layer 31 side. Therefore, when the first phase difference layer 31 is composed of layer A and layer B, the layer interposed between layer A and layer B is not considered to be the layer interposed between the first phase difference layer 31 and the second phase difference layer 32.

[0226] [Second lamination layer, third lamination layer] The second bonding layer is used to bond layers together within the linear polarizing plate 10, and the third bonding layer is used to bond layers together within the phase difference plate 30. Hereafter, the term "bonding layer" includes both the second and third bonding layers.

[0227] The bonding layer is an adhesive layer formed using an adhesive composition, or an adhesive layer formed using an adhesive composition. The second and third bonding layers are preferably adhesive layers from the viewpoint of suppressing thermal shrinkage behavior when heat is applied.

[0228] When the bonding layer is an adhesive layer, the adhesive composition used to form the adhesive layer is not particularly limited as long as it can satisfy the above-mentioned moisture permeability requirements. For example, the adhesive composition may contain polymers such as rubber polymers, (meth)acrylic polymers, urethane polymers, polyester polymers, silicone polymers, polyvinyl ether polymers, polyvinyl alcohol polymers, polyolefin polymers, vinyl alkyl ether polymers, polyvinylpyrrolidone polymers, poly(meth)acrylamide polymers, and cellulose polymers as its main component. In this specification, the main component refers to a component that accounts for 50% by mass or more of the total solid content of the adhesive composition. The adhesive composition may be of the active energy ray curing type or the thermosetting type. Rubber polymers are preferred as the adhesive composition. Note that "(meth)acrylic" above means "at least one of acrylic and methacrylic". The same applies to notations such as "(meth)acrylate".

[0229] Rubber polymers include natural rubber; polyisobutylene rubber (PIB), isoprene rubber (IR), isobutylene-isoprene rubber (IIR), n-butylene-isobutylene Examples of synthetic rubbers include styrene-butadiene rubber (BR), chloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), styrene-butadiene rubber (SBR), styrene-isoprene rubber (SIR), styrene-isoprene-styrene block copolymer rubber (SIBS), styrene-ethylene-butylene-styrene block copolymer rubber (SEBS), styrene-ethylene-propylene-styrene block copolymer rubber (SEPS), styrene-butadiene-styrene block copolymer rubber (SBS), and styrene-ethylene-propylene block copolymer rubber (SEP). Preferred rubber polymers include polyisobutylene rubber (PIB), isobutylene-isoprene rubber (IIR), and n-butylene-isobutylene copolymer rubber, with polyisobutylene rubber (PIB) being more preferred.

[0230] As the (meth)acrylic polymer, polymers or copolymers using one or more (meth)acrylic acid esters such as butyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate as monomers are preferably used. It is preferable to copolymerize a polar monomer as the base polymer. Examples of polar monomers include monomers having carboxyl groups, hydroxyl groups, amide groups, amino groups, epoxy groups, etc., such as (meth)acrylic acid, 2-hydroxypropyl (meth)acrylate, hydroxyethyl (meth)acrylate, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, and glycidyl (meth)acrylate.

[0231] An active energy ray curable adhesive composition is an adhesive composition that has the property of curing when irradiated with active energy rays such as ultraviolet rays or electron beams. It can adhere to a substrate such as a film even before irradiation with active energy rays, and the adhesion strength can be adjusted by curing with irradiation with active energy rays. The active energy ray curable adhesive composition is preferably ultraviolet curable. In addition to a base polymer and a crosslinking agent, the active energy ray curable adhesive composition further contains an active energy ray polymerizable compound. Furthermore, it may also contain a photopolymerization initiator and a photosensitizer as needed.

[0232] The adhesive composition may include, in addition to the polymer, a solvent; additives such as tackifiers, softeners, fillers (metal powders or other inorganic powders, etc.), antioxidants, UV absorbers, dyes, pigments, colorants, defoamers, corrosion inhibitors, and photopolymerization initiators. When an active energy ray curable adhesive composition is used, a cured product with a desired degree of curing can be obtained by irradiating the formed adhesive layer with active energy rays.

[0233] The adhesive layer can be formed by applying a diluted solution of the adhesive composition with an organic solvent onto a substrate and allowing it to dry.

[0234] When the bonding layer is an adhesive layer, the adhesive composition used to form the adhesive layer is not particularly limited as long as it can satisfy the above-mentioned moisture permeability requirements. Examples of adhesive compositions include water-based adhesives, active energy ray-curing adhesives, natural rubber adhesives, α-olefin-based adhesives, urethane resin-based adhesives, ethylene-vinyl acetate resin emulsion adhesives, ethylene-vinyl acetate resin-based hot melt adhesives, epoxy resin-based adhesives, vinyl chloride resin solvent-based adhesives, chloroprene rubber-based adhesives, cyanoacrylate-based adhesives, silicone-based adhesives, styrene-butadiene rubber solvent-based adhesives, nitrile rubber-based adhesives, nitrocellulose-based adhesives, reactive hot melt adhesives, phenol resin-based adhesives, modified silicone-based adhesives, polyester-based hot melt adhesives, polyamide resin hot melt adhesives, polyimide-based adhesives, polyurethane resin hot melt adhesives, polyolefin resin hot melt adhesives, polyvinyl acetate resin solvent-based adhesives, polystyrene resin solvent-based adhesives, polyvinyl alcohol-based adhesives, polyvinylpyrrolidone resin-based adhesives, and polyvinyl butyral-based adhesives. Examples include adhesives, polybenzimidazole adhesives, polymethacrylate resin solvent-based adhesives, melamine resin-based adhesives, urea resin-based adhesives, and resorcinol-based adhesives. Such adhesives can be used individually or in combination of two or more types.

[0235] Examples of water-based adhesives include aqueous solutions of polyvinyl alcohol-based resins and two-component water-based urethane emulsion adhesives. Active energy ray curing adhesives are adhesives that cure by irradiation with active energy rays such as ultraviolet light, and examples include those containing polymerizable compounds and photopolymerization initiators, those containing photoreactive resins, and those containing binder resins and photoreactive crosslinking agents. Examples of polymerizable compounds include photopolymerizable monomers such as photocurable epoxy monomers, photocurable (meth)acrylic monomers, and photocurable urethane monomers, as well as oligomers derived from these monomers. Examples of photopolymerization initiators include substances that generate active species such as neutral radicals, anionic radicals, and cationic radicals when irradiated with active energy rays such as ultraviolet light.

[0236] The thickness of the laminated layer is not particularly limited, but if the laminated layer is an adhesive layer, it is preferably 5 μm or more, may be 15 μm or more, may be 20 μm or more, may be 25 μm or more, is usually 200 μm or less, may be 100 μm or less, or may be 50 μm or less. If the laminated layer is an adhesive layer, the thickness of the laminated layer is preferably 0.01 μm or more, may be 0.05 μm or more, may be 0.5 μm or more, and is preferably 5 μm or less, may be 3 μm or less, or may be 2 μm or less.

[0237] [Manufacturing method for polarizing plates] The polarizing plate of this embodiment can be obtained by bonding the phase difference plate and the linear polarizing plate using a first bonding layer. When the first phase difference layer of the phase difference plate consists of only one layer and there is only one slow axis, it is preferable to set the transmission axis of the linear polarizing plate to substantially 45° with respect to the slow axis (optical axis) of the first phase difference layer of the phase difference plate. Substantially 45° is usually in the range of 45 ± 5°. In such an angular arrangement, the polarizing plate can function as a circular polarizing plate.

[0238] Methods for laminating a phase difference plate without a substrate to a linear polarizing plate include laminating a phase difference plate from which the substrate has been removed (peeled) to the linear polarizing plate using a first lamination layer, and laminating the phase difference plate to the linear polarizing plate using a first lamination layer and then removing (peeling) the substrate. In this embodiment, the form in which the substrate is removed after laminating the phase difference plate to the linear polarizing plate is preferred. According to the present invention, even in this form, damage to the phase difference layer of the phase difference plate can be suppressed when removing the substrate.

[0239] The first bonding layer may be formed directly by applying adhesive to the phase difference layer side of the phase difference plate, or by applying adhesive to the linear polarizing plate side, or by interposing a first bonding layer that has been previously formed on another substrate between the linear polarizing plate and the phase difference plate. If there is an alignment film between the substrate and the phase difference layer, the alignment film may be removed along with the substrate.

[0240] Substrates having functional groups on their surface that form chemical bonds with the phase difference layer or orientation film tend to become difficult to remove due to the chemical bonding with the phase difference layer or orientation film. Therefore, when removing the substrate by peeling it off, a substrate with fewer functional groups on its surface is preferred, and a substrate that has not undergone surface treatment to form functional groups on its surface is also preferred.

[0241] Furthermore, the alignment film having functional groups that form a chemical bond with the substrate has a strong adhesion between the substrate and the alignment film. Because they tend to grow larger, when peeling off and removing the substrate, an orientation film with fewer functional groups that form chemical bonds with the substrate is preferred. Furthermore, it is preferable that the product does not contain reagents that crosslink the substrate and the orientation film, and it is also preferable that the solution, such as the orientation polymer composition and the photo-alignment film forming composition, does not contain components such as solvents that dissolve the substrate.

[0242] Furthermore, orientation films having functional groups that form chemical bonds with the phase difference layer tend to have greater adhesion between the phase difference layer and the orientation film. Therefore, when removing the orientation film together with the substrate, an orientation film with fewer functional groups that form chemical bonds with the phase difference layer is preferable. In addition, it is preferable that the phase difference layer and the orientation film do not contain reagents that crosslink the phase difference layer and the orientation film.

[0243] Furthermore, a phase difference layer having functional groups that form chemical bonds with the alignment film tends to have greater adhesion between the alignment film and the phase difference layer. Therefore, when removing the substrate or when removing the alignment film together with the substrate, a phase difference layer with fewer functional groups that form chemical bonds with the substrate or alignment film is preferable. Also, the polymerizable liquid crystal composition preferably does not contain reagents that crosslink the substrate or alignment film with the phase difference layer.

[0244] For example, a polarizing plate with the configuration shown in Figure 1 can be manufactured by attaching a first bonding layer 21 to the surface of the first phase difference layer 31 of a phase difference plate 30 in which a base material, a second phase difference layer 32, and a first phase difference layer 31 are laminated in this order, bonding a linear polarizing plate 10 to it, and then removing the base material of the phase difference plate 30, thereby manufacturing a polarizing plate with the linear polarizing plate 10, a first bonding layer 21, a first phase difference layer 31, and a second phase difference layer 32 laminated in this order. Alternatively, a polarizing plate with the linear polarizing plate, a second phase difference layer, and a first phase difference layer laminated in this order can be manufactured by attaching a first bonding layer to the surface of the second phase difference layer of a phase difference plate in which a base material, a first phase difference layer, and a second phase difference layer are laminated in this order, bonding a linear polarizing plate to it, and then removing the base material of the phase difference plate. From the viewpoint of thinning, it is preferable to peel off the base material.

[0245] If the first phase difference layer includes layers A and B, or if it includes a third phase difference layer, there are restrictions on the stacking direction of each layer. Specifically, when stacking layer A, which has a phase difference of λ / 4, and layer B, which has a phase difference of λ / 2, layer B is first formed with respect to the absorption axis of the linear polarizer such that the slow axis of layer B is 75°, and then layer A is formed such that the slow axis of layer A is 15°. Furthermore, when there is a first phase difference layer having a phase difference of λ / 4 and a third phase difference layer having a phase difference of λ / 2, the third phase difference layer is first formed with respect to the absorption axis of the linear polarizer such that the lagging axis of the third phase difference layer is 75°, and then the first phase difference layer is formed such that the lagging axis of the first phase difference layer is 15°. There are no restrictions on the position of the second phase difference layer, but the linear polarizer, layer B and layer A must be stacked in this order, or the linear polarizer, third phase difference layer and first phase difference layer must be stacked in this order. By stacking in this way, the resulting polarizer can function as a broadband circular polarizer. Here, there are no restrictions on the axial angles forming layers A and B. For example, as described in Japanese Patent Publication No. 2004-126538, it is known that even if the slow axis angles of layers A and B are 30° and -30° or 45° and -45° with respect to the absorption axis of the polarizer, the function as a broadband λ / 4 plate can be achieved. Therefore, it is possible to laminate the layers in any desired manner.

[0246] [Image display device] Figure 4 is a schematic cross-sectional view illustrating an example of the image display device of this embodiment. As shown in Figure 4, the image display device 2 has, from the front, the polarizing plate 1 and the image display panel 40 shown in Figure 1, in that order. In the image display device 2, the polarizing plate 1 is arranged such that the linear polarizing plate 10 side is in front of the phase difference plate 30.

[0247] When polarizing plate 1 is a circular polarizing plate, in the image display device 2, incident light from the outside is polarized. There is light reflected by plate 1 and light transmitted through polarizing plate 1. Polarizing plate 1 may have an anti-reflective layer on its front surface, and by providing an anti-reflective layer, the light reflected from the surface of polarizing plate 1 (hereinafter also referred to as "external reflected light") can be reduced. The light transmitted through polarizing plate 1 is reflected by the image display panel 40 and becomes reflected light (hereinafter also referred to as "internal reflected light"), which is absorbed by polarizing plate 1. It is desirable that all of the internal reflected light is absorbed by polarizing plate 1, but some is emitted from the front surface (hereinafter, such light is also referred to as "emitted internal reflected light").

[0248] The polarizing plate 1 may be configured as a polarizing plate with an adhesive layer, having an adhesive layer on its rear surface that can be used to bond the polarizing plate 1 to the image display panel 40.

[0249] <Other layers that the image display device may have> The image display device 2 may have layers other than those described above. Examples of other layers that the image display device 2 may have are given below.

[0250] (Touch sensor panel) A touch sensor panel is a device (sensor) that detects (senses) fingers or other objects touching the screen of an image display device, and is used as an input means to detect the position of the finger on the screen and input it to the image display device. The touch sensor panel may be placed between the polarizing plate 1 and the image display panel 40, or it may be placed on the front side of the polarizing plate 1. As long as the sensor can detect the position of the touch, the detection method is not limited, and examples of touch sensor panels include resistive film type, capacitive coupling type, optical sensor type, ultrasonic type, electromagnetic induction coupling type, surface acoustic wave type, and infrared type touch sensor panels. Due to their low cost, resistive film type and capacitive coupling type touch sensor panels are preferably used.

[0251] An example of a resistive touch sensor panel consists of a pair of substrates positioned opposite each other, an insulating spacer sandwiched between the two substrates, a transparent conductive film provided as a resistive film on the inner front surface of each substrate, and a touch position detection circuit. In an image display device equipped with a resistive touch sensor panel, when the surface of the front panel is touched, the opposing resistive films short-circuit, and current flows through the resistive films. The touch position detection circuit detects the change in voltage at this time, and the touched position is detected.

[0252] An example of a capacitively coupled touch sensor panel consists of a substrate, transparent electrodes for position detection provided across the entire surface of the substrate, and a touch position detection circuit. In an image display device equipped with a capacitively coupled touch sensor panel, when the surface of the front panel is touched, the transparent electrodes are grounded at the touched point via the capacitance of the human body. The touch position detection circuit detects the grounding of the transparent electrodes and detects the touched position. A capacitive touch sensor panel is divided into an active area and an inactive area located on the outer periphery of the active area. The active area corresponds to the area on the display panel where the screen is displayed (display area) and is the area where the user's touch is detected, while the inactive area corresponds to the area on the display device where the screen is not displayed (non-display area).

[0253] The thickness of the touch sensor panel may be, for example, 5 μm or more and 2,000 μm or less, or 5 μm or more and 100 μm or less.

[0254] <Flexible Image Display Device> The image display device may be a flexible image display device. A flexible image display device is a foldable image display device. The flexible image display device incorporates an optical fingerprint authentication system and comprises a foldable image display element and a polarizing plate of the present invention. The foldable image display element is, for example, an organic EL display panel. The polarizing plate of the present invention is positioned on the viewing side of the organic EL display panel and is configured to be foldable. The polarizing plate for the blue image display device may further include a front panel and a touch sensor panel. It is preferable that the front panel, the polarizing plate of the present invention, and the touch sensor panel are stacked in this order from the viewing side, or that the front panel, the touch sensor panel, and the polarizing plate of the present invention are stacked in this order from the viewing side. If the polarizer is located on the viewing side of the touch sensor panel, the pattern of the touch sensor panel becomes difficult to see, and as a result the visibility of the displayed image improves. Therefore, it is even more preferable to have the polarizing plate of the present invention on the viewing side of the touch sensor panel, i.e., to have the front panel, the polarizing plate of the present invention, and the touch sensor panel in this order. Each component can be stacked using an adhesive, glue, etc. Furthermore, a light-shielding pattern can be formed on at least one surface of any of the layers of the front panel, polarizing plate, or touch sensor panel.

[0255] In a flexible image display device comprising a front panel, a polarizing plate of the present invention, and a foldable image display panel, the front panel and the polarizing plate of the present invention constitute a polarizing plate with a front panel, comprising a polarizing plate and a front panel. In this polarizing plate with a front panel, the front panel is usually placed on the viewing side of the polarizing plate and is laminated with the polarizing plate, for example, by an adhesive or bonding agent. In a flexible image display device comprising a touch sensor panel, a polarizing plate of the present invention, and a foldable image display panel, the touch sensor panel and the polarizing plate of the present invention constitute a polarizing plate with a touch sensor panel, comprising a polarizing plate and a touch sensor panel. Furthermore, in a flexible image display device comprising a polarizing plate of the present invention, a touch sensor panel, and a foldable image display element, the touch sensor panel and the polarizing plate of the present invention constitute a polarizing plate with a touch sensor panel, comprising a polarizing plate and a touch sensor panel. In this polarizing plate with a touch sensor panel, the touch sensor panel may be positioned on the back side (opposite side from the viewing side) of the polarizing plate, or on the viewing side of the polarizing plate. The touch sensor panel and the polarizing plate are laminated together, for example, with an adhesive or glue.

[0256] The polarizing plate of the present invention can also be used as a polarizing plate with a front plate by laminating a front plate on its viewing side. The polarizing plate with a front plate comprises the polarizing plate of the present invention and a front plate positioned on its viewing side.

[0257] (Front plate) Examples of front panels include glass and resin films with a hard coat layer on at least one surface. For example, high-transparency glass or tempered glass can be used as the glass. Chemically strengthened glass is preferred, especially when using a thin transparent surface material. The thickness of the glass can be, for example, 100 μm to 5 mm.

[0258] A front panel comprising a resin film with a hard coat layer on at least one surface can have flexible properties rather than being rigid like existing glass. The thickness of the hard coat layer is not particularly limited and may be, for example, 5 μm to 100 μm.

[0259] Examples of resin films include cycloolefin derivatives having monomer units containing cycloolefins such as norbornene and polycyclic norbornene monomers, cellulose (diacetylcellulose, triacetylcellulose, acetylcellulose butyrate, isobutyl ester cellulose, propionylcellulose, butyrylcellulose, acetylpropionylcellulose) ethylene-vinyl acetate copolymer, polycycloolefin, polyester, polystyrene, polyamide, polyetherimide, polyacrylic, polyimide, polyamideimide, polyethersulfone, polysulfone, polyethylene, polypropylene, polymethylpentene, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl acetal, polyether ketone, polyetherether ketone, polyethersulfone, polymethyl methacrylate, polyethylene terephthalate, polybutylene The film may be made of polymers such as reflatate, polyethylene naphthalate, polycarbonate, polyurethane, or epoxy. These polymers can be used individually or in combination of two or more. The resin film may be an unstretched film or a stretched film, such as a uniaxially oriented film or a biaxially oriented film. Preferred resin films include polyamide-imide films, polyimide films, uniaxially oriented polyester films, and biaxially oriented polyester films due to their excellent transparency and heat resistance. Cycloolefin derivative films and polymethyl methacrylate films are preferred because they offer excellent transparency and heat resistance, and can accommodate larger film sizes. Triacetylcellulose and isobutyl ester cellulose films are preferred because they offer good transparency and are relatively readily available as resin films without optical anisotropy. The thickness of the resin film is typically 5 to 200 μm, preferably 20 to 100 μm.

[0260] (Light-blocking pattern) The light-shielding pattern is a component also called a bezel and can be formed on the display element side of the front panel. By providing a light-shielding pattern, the wiring constituting the display device can be hidden and not visible to the user. The color and material of the light-shielding pattern are not particularly limited and can be formed from a resin material having various colors such as black, white, and gold. In one embodiment, the thickness of the light-shielding pattern may be 2 μm to 50 μm, preferably 4 μm to 30 μm, and more preferably in the range of 6 μm to 15 μm. Furthermore, a shape can be given to the light-shielding pattern to suppress the inclusion of air bubbles due to the step between the light-shielding pattern and the display part and to suppress the visibility of the boundary. [Examples]

[0261] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. Unless otherwise specified, the proportions expressed as "%" and "parts" in the examples and comparative examples are mass%, and parts by mass.

[0262] [Evaluation of circular polarizing plates (durability against substrate delamination)] An adhesive layer was laminated onto the protective film on the outermost surface of the linear polarizer of the circular polarizer. This was cut to create a test specimen measuring 25 mm wide x approximately 150 mm long. The adhesive layer of the test specimen was bonded to a glass plate. A release tape (25 mm wide x approximately 180 mm long) was attached to the surface (one side of the 25 mm width) of the outermost substrate of the phase difference element of the circular polarizer (the substrate used to form the second phase difference layer). One end of the release tape was grasped, and the substrate layer was peeled off using a tensile testing machine. Peeling speeds of 300 mm / min and 15000 mm / min were used. The peeling angle was 180°. If damage occurred to the phase difference layer on the side closer to the substrate during peeling, it was judged as zipping occurred (evaluation C); if this phenomenon was not observed, it was judged as no zipping (evaluation A); and if this phenomenon was slightly observed, it was judged as slight zipping (evaluation B).

[0263] [Measurement of the puncture modulus of a phase difference plate] A needle was attached to a handheld compression testing machine, the "NDG5 puncture tester, needle penetration force measurement specification," manufactured by Kato Tech Co., Ltd. The needle was punctured perpendicularly to the surface of the second phase difference layer side of the phase difference body, which had been peeled from the outermost surface of the substrate. The stress F (g) and the strain S (mm) at the moment just before the puncture test sample fractured were calculated, and the puncture modulus (g / mm) was calculated using the formula stress F (g) / strain S (mm). This procedure was performed for each of the five test samples, and the average value was taken as the puncture modulus. The needle used had a tip diameter of 1 mmφ and a radius of 0.5R. The needle puncture speed was set to 0.33 cm / second. The measurements were performed in a room temperature environment of 23°C and 55% relative humidity. The above method was used to produce the circular polarizing plates described later in Examples 1-6, Comparative Examples 1-2, and Reference Example 1. The puncture modulus of phase difference plates A, B, and C was measured. The measurement results are shown in Table 1.

[0264] [Measurement of the tensile modulus of the first laminated layer] The adhesive to be used as the first bonding layer was applied to one side of the release paper using a coating machine (bar coater, manufactured by Daiichi Rika Co., Ltd.), and another layer of release paper was laminated on top of the adhesive layer. The laminate was then heat-treated at 90°C for 1 minute and cured for 7 days under conditions of 23°C and 55% relative humidity. The laminate was cut to a size of 100 mm in MD length and 50 mm in TD length, and the release paper on both sides was peeled off to obtain an adhesive layer film consisting only of the adhesive layer. The adhesive layer was also cured using a predetermined curing method to obtain a film consisting only of the adhesive layer.

[0265] In accordance with JIS K7161:1994 and JIS K7127:1999, the tensile fracture strain was defined as the fracture elongation if the test specimen did not have a yield point, and the tensile fracture elongation strain was defined as the fracture elongation if the specimen had a yield point, and the fracture elongation was measured. The adhesive layer film obtained as described above was clamped at both ends in the MD length direction of the measurement sample with the upper and lower grips of a tensile testing machine [Autograph AG-Xplus testing machine manufactured by Shimadzu Corporation] so that the distance between the grips was 5 cm, and the measurement sample was pulled in the MD length direction at a tensile speed of 300 mm / min in an environment with a temperature of 23°C and a relative humidity of 55%, and the tensile modulus of elasticity [Pa] in the MD length direction at a temperature of 23°C and a relative humidity of 55% was calculated.

[0266] [Manufacturing Example 1: Fabrication of a laminate including a first phase difference layer] (i) Preparation of composition for forming photo-alignment film Five parts of a photo-aligning material with the structure shown below (weight-average molecular weight: 30,000) and 95 parts of cyclopentanone (solvent) were mixed. The resulting mixture was stirred at 80°C for 1 hour to obtain a composition for forming photo-aligned films.

[0267] [ka]

[0268] (ii) Preparation of the composition for forming the first phase difference layer Polymerizable liquid crystal compound A and polymerizable liquid crystal compound B, shown below, were mixed in a mass ratio of 90:10. To 100 parts of this mixture, 1.0 part of a leveling agent (F-556; manufactured by DIC Corporation) and 6 parts of a polymerization initiator, 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one ("Irg369," manufactured by BASF Japan Ltd.), were added.

[0269] Furthermore, N-methyl-2-pyrrolidone (NMP) was added to achieve a solid content concentration of 13%, and the mixture was stirred at 80°C for 1 hour to obtain a composition for forming the first phase difference layer.

[0270] Polymerizable liquid crystal compound A was produced by the method described in Japanese Patent Publication No. 2010-31223. Polymerizable liquid crystal compound B was produced according to the method described in Japanese Patent Publication No. 2009-173893. The molecular structures of each compound are shown below.

[0271] (Polymerizable liquid crystal compound A) [ka]

[0272] (Polymerizable liquid crystal compound B) [ka]

[0273] (iii) Preparation of the phase difference layer substrate A cycloolefin resin film with a thickness of 50 μm (ZF-14-50, manufactured by Nippon Zeon Co., Ltd.) was subjected to corona treatment to create a phase difference layer substrate. The corona treatment was performed using a TEC-4AX manufactured by Ushio Inc. The corona treatment was performed once under the conditions of an output of 0.78 kW and a processing speed of 10 m / min.

[0274] (iv) Formation of photoalignment film A photo-alignment film-forming composition was applied to a phase difference layer substrate using a bar coater. The coated film was dried at 80°C for 1 minute, and then exposed to 100 mJ / cm² of polarized UV light using a polarized UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.). 2 Polarized UV exposure was performed with the integrated light intensity. The thickness of the resulting horizontally aligned film was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and was found to be 100 nm.

[0275] (v) Formation of the first phase difference layer Next, under conditions of 25°C room temperature and 30% relative humidity, the first phase difference layer forming composition was passed through a PTFE membrane filter with a pore size of 0.2 μm (manufactured by Advantec Toyo Co., Ltd., part number: T300A025A) and coated onto an alignment film substrate film, which had been kept warm at 25°C, using a bar coater. After drying the coating film at 120°C for 1 minute, ultraviolet light was irradiated using a high-pressure mercury lamp (UniCure VB-15201BY-A, manufactured by Ushio Inc.) (under a nitrogen atmosphere, wavelength: 365 nm, integrated light intensity at 365 nm: 1000 mJ / cm²). 2 The thickness of the resulting coating film was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 2 μm. When the phase difference values ​​of the obtained first phase difference layer were measured, Re(450)=121nm, Re(550)=139nm, and Re(650)=146nm. The relationship between the in-plane phase difference values ​​at each wavelength was as follows: Re(450) / Re(550)=0.87 Re(650) / Re(550)=1.05

[0276] [Manufacturing Example 2: Fabrication of a laminate including a second phase difference layer] (i) Preparation of oriented polymer composition (1) An oriented polymer composition (1) was obtained by mixing 1 part of SunEver SE-610 (manufactured by Nissan Chemical Corporation) and 99 parts of 2-butoxyethanol.

[0277] (ii) Preparation of the composition for forming the second phase difference layer A mixture of 19.2 parts of polymerizable liquid crystal (BASF, LC242), 0.1 part of a leveling agent (BYK-361N, BIC Chemie Japan), 0.5 parts of a polymerization initiator (BASF Japan, Irgacure 907), 1.1 parts of a reaction additive (BASF Japan, Laromaer LR-9000), and 79.1 parts of propylene glycol 1-monomethyl ether 2-acetate was prepared. The mixture was stirred at 80°C for 1 hour to obtain a composition for forming the second phase difference layer.

[0278] [ka]

[0279] (iii) Preparation of the phase difference layer substrate A cycloolefin resin film with a thickness of 50 μm (ZF-14-50, manufactured by Nippon Zeon Co., Ltd.) was subjected to corona treatment to create a phase difference layer substrate. The corona treatment was performed using a TEC-4AX manufactured by Ushio Inc. The corona treatment was performed once under the conditions of an output of 0.78 kW and a processing speed of 10 m / min.

[0280] (iv) Formation of oriented polymer film An oriented polymer composition (1) was applied to a phase difference layer substrate using a bar coater and dried at 90°C for 1 minute to obtain an oriented film. The thickness of the obtained oriented film was measured with a laser microscope and found to be 34 nm.

[0281] (v) Formation of the second phase difference layer Next, the composition for forming the second phase difference layer is applied to the alignment film using a bar coater, dried at 90°C for 1 minute, and then irradiated with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, temperature: 25°C, integrated light intensity at wavelength 365 nm: 1000 mJ / cm²). 2A second phase difference layer was obtained by ). The thickness of the obtained second phase difference layer was measured with a laser microscope and found to be 450 nm. Furthermore, the phase difference value of the obtained phase difference film (2) at a wavelength of 550 nm was measured and found to be Re(550) = 1 nm and Rth(550) = -70 nm. In other words, the second phase difference layer had the optical properties represented by the following equation (3). Note that the phase difference value of COP at a wavelength of 550 nm is approximately 0 and therefore does not affect the optical properties. nx≒ny <nz (3)

[0282] [Manufacturing Example 3: Fabrication of Phase Difference Plate A] A laminate containing the first phase difference layer obtained in Manufacturing Example 1 and a laminate containing the second phase difference layer obtained in Manufacturing Example 2 were bonded together using the following active energy ray curable adhesive A, such that the respective phase difference layer surfaces (the surfaces opposite to the substrate side) became the bonding surfaces. Next, the active energy ray curable adhesive A was cured by irradiation with ultraviolet light. In this way, a phase difference plate A containing two phase difference layers, the first phase difference layer and the second phase difference layer, was fabricated.

[0283] <Activated energy ray curing adhesive A> After mixing the following components and then removing the foam, an active energy ray-curing adhesive A was prepared. · 3',4'-Epoxycyclohexylmethyl 3,4-Epoxycyclohexanecarboxylate (Trade name: CEL2021P, manufactured by Daicel Corporation): 70 parts by mass • Neopentyl glycol diglycidyl ether (product name: EX-211, manufactured by Nagase ChemteX Corporation): 20 parts by mass • 2-Ethylhexylglycidyl ether (product name: EX-121, manufactured by Nagase ChemteX Corporation): 10 parts by mass • Cationic polymerization initiator (product name: CPI-100_50% solution, manufactured by Sunapro Co., Ltd.): 4.5 parts by mass (actual solid content 2.25 parts by mass) • 1,4-Diethoxynaphthalene: 2 parts by mass

[0284] [Manufacturing Example 4: Fabrication of Phase Difference Plate B] A phase difference plate B was fabricated as follows, in which the substrate / orientation layer / second phase difference layer (positive C plate) / orientation layer / first phase difference layer (λ / 4 layer) were laminated in this order.

[0285] (base material) As a base material, a cycloolefin polymer film (COP) (ZF-14 manufactured by Zeon Corporation) was prepared.

[0286] (Corona treatment) The corona treatment device used was the AGF-B10 manufactured by Kasuga Electric Co., Ltd. Corona treatment was performed once using the above corona treatment device under the conditions of an output of 0.3 kW and a processing speed of 3 m / min.

[0287] (High-pressure mercury lamp) For the high-pressure mercury lamp, we used the UniCure VB-15201BY-A manufactured by Ushio Inc.

[0288] The oriented polymer composition (1) prepared in the fabrication of phase difference plate A was applied to the surface of a corona-treated substrate using a bar coater and dried at 90°C for 1 minute. The film thickness was measured with a laser microscope and found to be 34 nm. Next, the second phase difference layer forming composition prepared in the fabrication of phase difference plate A was applied to the alignment film using a bar coater, dried at 90°C for 1 minute, and then irradiated with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light intensity at a wavelength of 365 nm: 1000 mJ / cm²). 2 A second phase difference layer (positive C plate) was formed by ) and a second phase difference film having the second phase difference layer was obtained. When the thickness of the obtained second phase difference layer was measured with a laser microscope, the thickness was 450 nm. Furthermore, when the phase difference value of the obtained second phase difference film at a wavelength of 550 nm was measured, Re(550) = 1 nm and Rth(550) = -70 nm. That is, the second phase difference layer is given by the following equation (3): nx≒ny <nz (3) The material possessed the optical properties represented by [the specified formula]. Note that the phase difference value at a wavelength of 550 nm of the substrate is approximately 0, and therefore does not affect these optical properties.

[0289] Next, the following oriented polymer composition (2) was applied to the second phase difference layer of the second phase difference film using a bar coater and dried at 100°C for 1 minute. The thickness of the resulting oriented film was measured with a laser microscope (LEXT, manufactured by Olympus Corporation) and was found to be 100 nm. Subsequently, the oriented film was rubbed and the first phase difference layer forming composition prepared in the fabrication of phase difference plate A was applied to the treated surface using a bar coater and dried at 120°C for 1 minute. The coating film was irradiated with ultraviolet light using a high-pressure mercury lamp (under a nitrogen atmosphere, integrated light intensity at a wavelength of 365 nm: 1000 mJ / cm²). 2 By doing so, a first phase difference layer was formed on the second phase difference layer to obtain a phase difference plate B. The thickness of the obtained first phase difference layer was measured using a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 2 μm. The phase difference values ​​of the obtained phase difference plate B were measured and found to be Re(450)=121 nm, Re(550)=139 nm, and Re(650)=146 nm. The relationship between the in-plane phase difference values ​​at each wavelength was as follows: Re(450) / Re(550)=0.87 Re(650) / Re(550)=1.05 In other words, the obtained phase difference plate B had the optical properties represented by the above-mentioned equations (1), (2), and (4).

[0290] (Oriented polymer composition (2)) Commercially available polyvinyl alcohol (Polyvinyl Alcohol 1000 Fully Saponified Type, Wako Pure Chemical Industries) (Manufactured by Kogyo Co., Ltd.), add water and heat at 100°C for 1 hour, solid content 2% by mass (solvent concentration 9 An oriented polymer composition (2) with a concentration of 8% by mass was obtained.

[0291] [Manufacturing Example 5: Fabrication of Phase Difference Plate C] Phase difference plate C was fabricated in the same manner as phase difference plate A, except that, in the fabrication of phase difference plate A, an adhesive layer 3 (a sheet-like acrylic adhesive with a thickness of 5 μm) was used instead of an active energy ray-curable adhesive A to bond the laminate containing the first phase difference layer to the laminate containing the second phase difference layer.

[0292] [Manufacturing Example 6: Polarizer Fabrication] A polyvinyl alcohol film with a thickness of 20 μm, a degree of polymerization of 2,400, and a degree of saponification of 99.9% or higher was uniaxially stretched to a stretching ratio of 4.5 times by dry process, and while maintaining tension, was immersed for 60 seconds in a staining bath at 28°C containing 0.05 parts by weight of iodine and 5 parts by weight of potassium iodide per 100 parts by weight of water.

[0293] Next, the polarizer was immersed for 110 seconds in a 64°C boric acid aqueous solution 1 containing 5.5 parts by weight of boric acid and 15 parts by weight of potassium iodide per 100 parts by weight of water. Then, it was immersed for 30 seconds in a 67°C boric acid aqueous solution 2 containing 5.5 parts by weight of boric acid and 15 parts by weight of potassium iodide per 100 parts by weight of water. After that, it was washed with 3°C pure water and dried to obtain a polarizer with a thickness of 8 μm.

[0294] [Manufacturing Example 7: Fabrication of Linear Polarizing Plates] I prepared the following protective film. Protective film: 13μm thick norbornene-based resin film [Manufactured by Zeon Corporation, product name "ZEONOR"] The protective film described above was laminated to one side of the polarizer prepared as described above using a roll laminating machine via a water-based adhesive. After lamination, it was dried at 80°C for 3 minutes. A linear polarizing plate was obtained in which the protective film was laminated only on one side of the polarizer. The linear polarizing plate consisted of the polarizer, adhesive layer, and protective film laminated in this order.

[0295] [Manufacturing Example 8: Preparation of Adhesive Layer 1] A reaction vessel equipped with a condenser, nitrogen inlet, thermometer, and stirrer was charged with a mixed solution of 81.8 parts ethyl acetate, 90.0 parts butyl acrylate, 5.0 parts methyl acrylate, and 5.0 parts acrylic acid. The internal temperature was raised to 55°C while replacing the air in the apparatus with nitrogen gas to eliminate oxygen. Subsequently, the entirety of a solution of 0.15 parts azobisisobutyronitrile (polymerization initiator) dissolved in 10 parts ethyl acetate was added. After adding the polymerization initiator, the mixture was maintained at this temperature for 1 hour, and then ethyl acetate was added at a rate of 17.3 parts / hr while maintaining the internal temperature at 54-56°C. The ethyl acetate was continuously added to the container, and the addition was stopped when the concentration of the (meth)acrylic resin reached 35% by mass. The temperature was then maintained at this level for 6 hours from the start of the ethyl acetate addition. Finally, ethyl acetate was added to adjust the concentration of the (meth)acrylic resin to 20% by mass, and acrylic resin solution 1 was prepared. The obtained acrylic resin had a weight-average molecular weight Mw of 1.6 million and a molecular weight distribution Mw / Mn of 4.5. Note that Mw and Mn are G Two "TSKgel GMHHR-H(S)" columns manufactured by Tosoh Corporation were connected in series and placed in the PC instrument, and tetrahydrofuran was used as the eluate, with a sample concentration of 2 mg / Measurements were taken using standard polystyrene equivalents under the following conditions: mL, sample introduction volume 100 μL, temperature 40°C, flow rate 1 mL / min.

[0296] To 100 parts of the solid content of the above acrylic resin solution 1, 0.15 parts on an active ingredient basis of a crosslinking agent (manufactured by Tosoh Corporation: trade name "Coronate L" (ethyl acetate solution of trimethylolpropane adduct of tolylene diisocyanate (solid content concentration 75% by mass)) and 0.2 parts of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name "KBM-403") were added, and then ethyl acetate was added to bring the solid content concentration to 13% to obtain adhesive composition 1.

[0297] Adhesive composition 1 was applied using an applicator to the release-treated surface of a separator film made of polyethylene terephthalate film with a release treatment [PLR-382190 obtained from Lintec Corporation] to a thickness of 25 μm after drying, and dried at 100°C for 1 minute to produce an adhesive layer (adhesive sheet). Next, the surface of the obtained adhesive layer opposite to the separator film was laminated to the release-treated surface of a separator film made of polyethylene terephthalate film with a release treatment [PET-251130 obtained from Lintec Corporation] to produce adhesive layer 1.

[0298] [Manufacturing Example 9: Preparation of Adhesive Layer 2] A reaction vessel equipped with a condenser, nitrogen inlet, thermometer, and stirrer was charged with a mixed solution of 100 parts ethyl acetate, 99.0 parts butyl acrylate, 0.5 parts 2-hydroxyethyl acrylate, and 0.5 parts acrylic acid. The internal temperature was raised to 55°C while replacing the air in the apparatus with nitrogen gas to eliminate oxygen. Subsequently, the entirety of a solution of 0.12 parts azobisisobutyronitrile (polymerization initiator) dissolved in 10 parts ethyl acetate was added. After adding the polymerization initiator, the mixture was maintained at this temperature for 1 hour, and then ethyl acetate was added at a rate of 17.3 while maintaining the internal temperature at 54-56°C. The ethyl acetate was continuously added to the reaction vessel at a rate of parts / hr, and the addition of ethyl acetate was stopped when the concentration of the (meth)acrylic resin reached 35% by mass. The temperature was then maintained at this level for 6 hours from the start of ethyl acetate addition. Finally, ethyl acetate was added to adjust the concentration of the (meth)acrylic resin to 20% by mass, and acrylic resin solution 2 was prepared. The obtained acrylic resin had a weight-average molecular weight Mw of 1.7 million and a molecular weight distribution Mw / Mn of 3.9. Mn was measured using two TSKgel GMHHR-H(S) columns manufactured by Tosoh Corporation, connected in series, as columns in a GPC instrument, with tetrahydrofuran as the eluent, under the conditions of a sample concentration of 2 mg / mL, sample introduction volume of 100 μL, temperature of 40°C, and flow rate of 1 mL / min, in terms of standard polystyrene equivalent.

[0299] To 80 parts of the solid content of the acrylic resin solution 2, 20 parts (solid content) of a difunctional acrylate (obtained from Shin-Nakamura Chemical Co., Ltd.; product number "A-DOG"), 2.5 parts based on the active ingredient of a crosslinking agent (manufactured by Tosoh Corporation: trade name "Coronate L" (an ethyl acetate solution of the trimethylolpropane adduct of tolylene diisocyanate, with a solid content concentration of 75 mass%)), 1.5 parts of a photopolymerization initiator (manufactured by Ciba Specialty Chemicals Inc.: trade name "Irgacure 500"), and 0.3 parts of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name "KBM-403") were added, and ethyl acetate was further added so that the solid content concentration became 13%, to obtain pressure-sensitive adhesive composition 2. A-DOG is a diacrylate of an acetal compound of hydroxypivalaldehyde and trimethylolpropane, and has a structure represented by the following formula.

[0300]

Chemical Formula

[0301] Pressure-sensitive adhesive composition 2 was applied onto the release-treated surface of a separate film composed of a release-treated polyethylene terephthalate film ("PLZ-383030" obtained from Lintec Corporation) using an applicator so that the thickness after drying would be 15 μm, and dried at 100°C for 1 minute to produce a pressure-sensitive adhesive layer (pressure-sensitive adhesive sheet). Subsequently, the surface of the obtained pressure-sensitive adhesive layer on the side opposite to the separator film was laminated to the release-treated surface of a separate film composed of a release-treated polyethylene terephthalate film ("PLR-381031" obtained from Lintec Corporation). Subsequently, ultraviolet rays were irradiated under the following conditions to fabricate pressure-sensitive adhesive layer 2. <UV Irradiation Conditions> · Using an H bulb of Fusion UV lamp system (manufactured by Fusion UV Systems Inc.) · Integrated light quantity in the UVA wavelength region of 250 mJ / cm 2 (Measured value by UV Power Puck II manufactured by Fusion UV Inc.)

[0302] [Production Example 10: Fabrication of Pressure-Sensitive Adhesive Layer 3] The adhesive layer 3 was prepared in the same manner as in Production Example 9, except that the adhesive composition 2 was applied so that its thickness after drying was 5 μm.

[0303] [Example 1] The laminate (circular polarizer) of Example 1 was fabricated as follows. An adhesive layer 1 (a sheet-like acrylic adhesive with a thickness of 25 μm) was laminated onto the polarizer of the linear polarizer fabricated above. The tensile modulus of adhesive layer 1 measured by the above method is shown in Table 1. The substrate used to form the first phase difference layer was peeled off from the phase difference plate A fabricated in Manufacturing Example 3. The exposed horizontal alignment film and the adhesive layer (first bonding layer) were bonded together to fabricate a laminate (circular polarizer) in which the linear polarizer, the first bonding layer, and the phase difference plate A were laminated in this order. The angle between the absorption axis of the polarizer and the slow axis of the first phase difference layer was 45°.

[0304] [Example 2] Except for using adhesive layer 2 (a sheet-like acrylic adhesive with a thickness of 15 μm) instead of adhesive layer 1 used in the preparation of the laminate (circular polarizer) of Example 1, a laminate (circular polarizer) was obtained in the same manner as in Example 1, in which a linear polarizer, a first bonding layer, and a phase difference plate A were laminated in that order. The tensile modulus of adhesive layer 2 measured by the above method is shown in Table 1.

[0305] [Example 3] Except for using adhesive layer 3 (a 5 μm thick sheet of acrylic adhesive) instead of adhesive layer 1 used in the preparation of the laminate (circular polarizer) of Example 1, a laminate (circular polarizer) was obtained in the same manner as in Example 1, in which a linear polarizer, a first bonding layer, and a phase difference plate A were laminated in that order. The tensile modulus of adhesive layer 3 measured by the above method is shown in Table 1.

[0306] [Example 4] Except for using phase difference plate B, which was prepared in Manufacturing Example 4, instead of phase difference plate A, which was used in the preparation of the laminate (circular polarizer) in Example 1, and bonding adhesive layer 1 (first bonding layer) to the first phase difference layer of phase difference plate B, a laminate (circular polarizer) was obtained in the same manner as in Example 1, in which a linear polarizer, the first bonding layer, and phase difference plate B were laminated in this order.

[0307] [Example 5] Except for using phase difference plate B, which was prepared in Manufacturing Example 4, instead of phase difference plate A, which was used in the preparation of the laminate (circular polarizer) in Example 2, and bonding the adhesive layer 2 (first bonding layer) to the first phase difference layer of phase difference plate B, a laminate (circular polarizer) was obtained in the same manner as in Example 2, in which a linear polarizer, the first bonding layer, and phase difference plate B were laminated in this order.

[0308] [Example 6] Except for using adhesive layer 3 (a sheet-like adhesive with a thickness of 5 μm) instead of adhesive layer 1 used in the preparation of the laminate (circular polarizer) of Example 4, a laminate (circular polarizer) was obtained in the same manner as in Example 4, in which a linear polarizer, a first bonding layer, and a phase difference plate B were laminated in this order.

[0309] [Comparative Example 1] Except for using adhesive layer A (thickness 1.5 μm after drying) formed with the above-described active energy ray curing adhesive A instead of adhesive layer 1 used in the preparation of the laminate (circular polarizer) of Example 1, a laminate (circular polarizer) was obtained in the same manner as in Example 1, in which a linear polarizer, a first bonding layer, and a phase difference plate A were laminated in this order. The tensile modulus of adhesive layer A measured by the above method is shown in Table 1.

[0310] [Comparative Example 2] Except for using adhesive layer A (thickness 1.5 μm after drying) formed with the above-mentioned active energy ray curable adhesive A instead of adhesive layer 1 used in the preparation of the laminate (circular polarizer) of Example 4, a laminate (circular polarizer) was obtained in the same manner as in Example 4, in which a linear polarizer, a first bonding layer, and a phase difference plate B were laminated in this order.

[0311] [Reference example 1] Except for using phase difference plate C, which was made in Manufacturing Example 5, instead of phase difference plate A, which was used in the fabrication of the laminate (circular polarizer) in Example 3, a laminate (circular polarizer) was obtained in the same manner as in Example 3, in which a linear polarizer, a first bonding layer, and a phase difference plate were laminated in this order.

[0312] [evaluation] The durability of the circular polarizing plates of Examples 1-6, Comparative Examples 1-2, and Reference Example 1 after peeling off the substrate used to form the second phase difference layer was evaluated according to the method described above. The evaluation results are shown in Table 1.

[0313] [Table 1] [Explanation of Symbols]

[0314] 1 Polarizing plate, 2 Image display device, 10 Linear polarizing plate, 21 First bonding layer, 30 Phase difference plate, 31 First phase difference layer, 32 Second phase difference layer, 40 Image display panel.

Claims

1. A polarizing plate comprising a linear polarizing plate, a first bonding layer, and a phase difference plate, laminated in this order, The aforementioned linear polarizing plate has a protective film laminated on only one side of the polarizer. The first laminated layer is laminated on the polarizer side of the linear polarizing plate. The phase difference plate is It has a first phase difference layer and a second phase difference layer, Furthermore, the surface opposite to the first laminated layer has a substrate, The first phase difference layer and the second phase difference layer contain a cured liquid crystal compound. The puncture modulus is 70 g / mm or more. The first laminated layer has a tensile modulus of 1.3 × 10 at a temperature of 23°C and a relative humidity of 55%. 5 The pressure is between Pa and 1.0 × 10⁷ Pa. A polarizing plate used by peeling off the aforementioned substrate and then laminating it onto an image display panel.

2. The polarizing plate according to claim 1, wherein the product of the thickness (m) of the first laminated layer and the tensile modulus (Pa) is 500 or less.

3. The polarizing plate according to claim 1 or 2, wherein the phase difference plate has only an alignment film between the first phase difference layer and the second phase difference layer, or has no other intervening layer.

4. The linear polarizing plate has a polarizer, The polarizer is a polarizing plate according to claim 1 or 2, wherein the polarizer has a thickness of 15 μm or less.

5. The linear polarizing plate has a protective film provided on the surface of the polarizer opposite to the first lamination layer, The polarizing plate according to claim 4, wherein the protective film has a thickness of 30 μm or less.

6. The polarizer according to claim 1 or 2, wherein the first phase difference layer is an inversely dispersed λ / 4 layer.

7. The polarizing plate according to claim 1 or 2, wherein the second phase difference layer is a positive C plate.

Citation Information

Patent Citations

  • Polarizing plate with adherent type optical compensating layer and image display device

    JP2004264333A

  • Adhesive mass and adhesive sheet using the same

    JP2014196376A

  • Optical film

    JP2015163935A

  • Adhesive composition, adhesive layer and optical member with adhesive layer

    JP2016094592A

  • Polarizing plate and image display device

    JP2017204003A