Method and composition
A washcoat composition with alumina-silica support and platinum group metal impregnation enhances catalyst stability and sulfur resistance, addressing deactivation and poisoning issues in natural gas-fueled engines and turbines.
Patent Information
- Application Number
- JP2023530299
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-09
- Filing Date
- 2022-01-07
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-01-07
AI Technical Summary
Existing catalysts for treating CO and formaldehyde emissions from natural gas-fueled engines and turbines suffer from deactivation over time and are susceptible to catalyst poisoning, particularly from sulfur in the exhaust stream.
A method involving a washcoat composition prepared with a support material comprising alumina and silica or zirconia, impregnated with a platinum group metal component, and a metal oxide sol, applied to a substrate and calcined, enhancing CO and formaldehyde oxidation stability and resistance to sulfur poisoning.
The method provides improved CO and formaldehyde oxidation stability and resistance to catalyst poisons, maintaining activity over time while using lower amounts of platinum group metals.
Smart Images

Figure 0007954650000001 
Figure 0007954650000002 
Figure 0007954650000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for preparing catalytic articles for treating exhaust gases generated by power generation devices such as engines or turbines, particularly engines and turbines that use natural gas as fuel. The present invention further relates to a washcoat composition suitable for use in such a method. [Background technology]
[0002] Under normal operation, natural gas-fueled turbines and engines produce significant amounts of carbon dioxide (CO2), water, carbon monoxide (CO), volatile organic compounds (VOCs) such as formaldehyde, and nitrogen oxides (NOx) as part of the combustion process.
[0003] Recent environmental regulations emphasize the importance of reducing the levels of partially burned fuel components in the exhaust of such turbines and engines. These regulated exhaust emissions include carbon monoxide (CO) and formaldehyde (CH2O).
[0004] A catalytic converter can be used to treat emissions from such engines. The catalytic converter converts these emissions in the exhaust gas into less harmful substances before they are released into the atmosphere. A catalytic converter typically includes a suitable substrate coated with a catalytically active material.
[0005] In the production of coated catalysts, compositions known as “washcoats” are applied to a substrate (e.g., a ceramic monolith). The washcoat may take the form of a solution, slurry, or suspension of the catalyst material in a liquid medium. Once coated onto the substrate, the washcoat typically undergoes a calcination process to remove the liquid medium and fix the catalytic activator to the substrate.
[0006] Known catalysts suitable for catalyzing the oxidation of CO and formaldehyde typically employ one or more platinum group metals (PGM) supported on a suitable catalyst carrier. The catalyst carrier may be a high-surface-area refractory metal oxide such as alumina or silica. However, known oxidation catalysts may deactivate over time. Furthermore, certain components present in fuel or lubricating oil may cause catalyst poisoning. For example, in the operation of two-stroke engines, sulfur in the exhaust stream derived from engine oil is a major cause of catalyst poisoning.
[0007] There remains a need for improved oxidation catalysts, particularly for use in treating CO and formaldehyde emissions from natural gas-fueled engines and turbines. SUMMARY OF THE INVENTION
[0008] According to aspects of the present disclosure, there is provided a method of preparing a catalytic article, the method comprising: (a) preparing a washcoat composition by combining at least the following components: ● a support material comprising a mixed oxide, a mixture of oxides, or a molecular sieve, wherein the mixed oxide or mixture of oxides comprises (i) alumina and (ii) silica and / or zirconia, ● a metal oxide sol comprising at least one of titania, silica, or zirconia, ● a liquid medium; (b) applying the washcoat composition to a substrate to form a washcoat coating; (c) drying and / or calcining the washcoat coating; wherein the method further comprises the step of impregnating the support material with a platinum group metal component.
[0009] According to further aspects of the present disclosure, ● a support material comprising a mixed oxide, a mixture of oxides, or a molecular sieve, wherein the mixed oxide or mixture of oxides comprises (i) alumina and (ii) silica and / or zirconia, and wherein the support material is optionally impregnated with a platinum group metal component; ● A metal oxide sol comprising at least one of titania, silica or zirconia, and ● a liquid medium. A washcoat composition is provided.
[0010] Advantageously, it has been found that catalysts prepared according to the above methods can provide improved CO and / or formaldehyde oxidation stability (i.e., activity maintained over time). Furthermore, improved and / or equivalent oxidation activity can be achieved compared to known catalysts while using a lower amount of PGM. In addition, improved resistance to catalyst poisons, particularly improved sulfur resistance, can be achieved.
[0011] Furthermore, catalysts prepared according to the methods described herein may find use in other stationary emission control applications, for example, in the treatment of exhaust gases from industrial processes or in indoor air treatment systems. In particular, the catalytic articles prepared according to the methods of the present invention may be useful for the decomposition of ozone (O3) present in a gas stream. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] [Figure 1] FIG. 2 is a graph showing the CO oxidation activity achieved by a catalytic article prepared according to the method of the present disclosure, in comparison with that achieved by a prior art catalyst. [Figure 2] FIG. 3 is a graph showing the CO oxidation activity achieved by a comparative catalytic article. [Figure 3] FIG. 4 is a graph showing the CO oxidation activity achieved by a catalytic article prepared according to the method of the present disclosure. DETAILED DESCRIPTION OF EMBODIMENTS OF THE INVENTION
[0013] The present disclosure will now be further described. Different aspects / embodiments of the present disclosure are defined in more detail in the following sections. Each of the aspects / embodiments defined in this way may be combined with any other aspects / embodiments or aspects / embodiments unless otherwise expressly indicated. In particular, any feature indicated as preferred or advantageous may be combined with any other or more features indicated as preferred or advantageous.
[0014] Furthermore, as used herein, the term “comprising” may be interchanged with the definitions “consisting essentially of” or “consisting of.” The term “comprising” is intended to mean that the specified elements are essential, but other elements may be added and still form a configuration within the scope of the claim. The term “consisting essentially of” limits the scope of the claim to the specified materials or processes, and to those that do not substantially affect the basic and novel characteristics of the claimed invention. The term “consisting of” closes the claim to the inclusion of materials other than those enumerated, except for impurities that are usually associated with them.
[0015] Wash coat compositions can be prepared by combining the necessary components and optional additives. The combination of components may be carried out by mixing, for example, by stirring. Preferably, the components are mixed so that the wash coat composition is substantially homogeneous, i.e., homogeneous, that is, the distribution of components throughout the wash coat is substantially uniform.
[0016] The carrier material includes a mixed oxide, a mixture of oxides, or a molecular sieve containing (i) alumina and (ii) silica and / or zirconia. Preferably, the carrier material is a mixed oxide. As used herein, the term "mixed oxide" refers to a mixture of oxides in a single phase. For example, the mixed oxide material may be a silica-alumina mixed oxide or a zirconia-alumina mixed oxide. Alternatively, the carrier material may be an aluminosilicate molecular sieve (zeolite).
[0017] Preferably, the carrier material is a silica-alumina mixed oxide. The silica-alumina mixed oxide may have a silica content in the range of 1-40% by weight, 2-35% by weight, 5-35% by weight, or 5-30% by weight. For example, the silica-alumina mixed oxide may have a silica content in the range of 2-10% by weight, for example, about 5% by weight. Alternatively, the silica-alumina mixed oxide may have a silica content in the range of 25-40% by weight, for example, about 30% by weight.
[0018] Generally, the carrier material used in the present invention is particulate. The carrier material may have a D90 particle size of ≤50 μm, ≤30 μm, ≤20 μm, or ≤10 μm. The particles can be obtained by grinding.
[0019] As used herein, the term "D90 particle size" refers to the particle size distribution. The D90 particle size value corresponds to the particle size value at which 90% by volume of the total particles in a particular sample are present. The D90 particle size can be determined using laser diffraction (for example, using a Malvern Mastersizer 2000).
[0020] The amount of carrier material present in the wash coat composition is 0.5 to 4 g / in. 3 Preferably 1-2 g / in 3 It may be selected to provide the amount of support material in the final catalyst article. This is within the capabilities of those skilled in the art.
[0021] As used herein, the term "loaded amount" conventionally defines the concentration of a component present in the catalyst layer on a substrate. The unit of loaded amount is generally g / ft 3 or g / in 3 This is expressed as and relates to the volume of the base material used.
[0022] The step of impregnating the carrier material with a platinum group metal component may be performed before combining the carrier material with the other components of the wash coat (i.e., before step (a) of the method described herein). For example, impregnation may be performed by contacting the carrier material with an impregnation solution containing a platinum group metal component. The impregnated carrier material may be dried and / or calcined before combining it with the other components of the wash coat composition.
[0023] Alternatively, the carrier material may be impregnated with a platinum group metal component after step (a) and before step (b). For example, the wash coat composition prepared in step (a) may be blended with the impregnation solution before being applied to the substrate in step (b).
[0024] Alternatively, after step (c) of the present method, the carrier material may be impregnated with a PGM component, and the impregnation may be carried out by bringing the substrate into contact with an impregnation solution containing a platinum group metal component. Contact between the wash-coated substrate and the impregnation solution can be achieved by applying the impregnation solution to the substrate (for example, on top of a dried and / or fired wash coating) to form a second coating. Thus, the present method may further include (d) a step of applying an impregnation solution containing a platinum group metal component to the substrate to form a second coating, and (e) a step of drying and / or firing the second coating.
[0025] The impregnation solution may be an aqueous solution of a platinum group metal component.
[0026] The platinum group metal component may be a salt of a platinum group metal (PGM). In particular, the platinum group metal component may be a nitrate of PGM, an acetate of PGM, or a carboxylate of PGM. The PGM may be ruthenium (Ru), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), platinum (Pt), or a mixture thereof. Preferably, the PGM is platinum, palladium, or a mixture of platinum or palladium. More preferably, the PGM is platinum. Suitable platinum group metal components include platinum nitrate or platinum acetate, such as tetraammineplatinum acetate.
[0027] The amount of the platinum group metal component used is such that the final catalyst layer formed on the substrate has 1 to 100 g / ft 3 , for example 4 to 90 g / ft 3 , 8 to 50 g / ft 3 , or 20 to 35 g / ft 3 can be selected to include a platinum group metal loading in the range of.
[0028] The above drying step may be carried out at a temperature below 120°C, for example at a temperature of about 100°C. The calcination step may be carried out at a temperature of 550°C or less, preferably in the range of 450 to 550°C, for a period of 3 hours or less, preferably 30 minutes to 2 hours.
[0029] The metal oxide sol comprises at least one of titania, silica or zirconia. As used herein, the term "metal oxide sol" refers to a colloid comprising particulate metal oxide having a BET surface area of at least 100 m 2 / g dispersed in a continuous liquid medium. Preferably, the metal oxide sol is a titania sol (i.e., a colloid comprising particulate titania having a specific surface area of at least 100 m 2 / g dispersed in a continuous liquid medium).
[0030] The liquid medium of the metal oxide sol may be aqueous.
[0031] The metal oxide of the metal oxide sol has ≧100 m 2 / g, ≥150m 2 / g, ≥200m 2 / g, ≥250m 2 / g or ≥300m 2 It may have a BET surface area of / g.
[0032] Metal oxide sols contain titania ≥ 250 m 2 / g or ≥300m 2 It may also be a titania sol having a BET surface area of / g.
[0033] The metal oxide sol may be acidic or basic. Preferably, the metal oxide sol is acidic. For example, the metal oxide sol may have a pH in the range of 0.5 to 5, for example, 0.5 to 3 or 0.5 to 2.
[0034] The metal oxide particles in the sol may have a D50 particle size of ≤1 micron, for example, ≤0.5 micron or ≤0.2 micron. The metal oxide particles in the sol may have a D90 particle size of ≤5 micron, for example, ≤2 micron, ≤1 micron or ≤0.5 micron.
[0035] As used herein, the term "D50 particle size" refers to the particle size distribution. The D50 particle size value corresponds to the particle size value at which 50% by volume of the total particles in a particular sample are present. The D50 particle size can be determined using laser diffraction (for example, using a Malvern Mastersizer 2000).
[0036] The amount of metal oxide sol used is 2.5 g / in for the final catalyst layer formed on the substrate. 3 For example, ≤2g / in 3 ≤1g / in 3 ≤0.5g / in 3 or ≤0.2 g / in 3 The amount of metal oxide supported can be selected to include the amount of metal oxide supported.
[0037] The washcoat composition further comprises a liquid medium in which other components are suspended or solvated. The liquid medium may be aqueous; for example, the liquid medium may be water. Preferably, the liquid medium consists essentially of water. That is, the liquid medium contains water but may also contain trace amounts of non-aqueous (e.g., organic or inorganic) impurities. The water may be deionized water or desalinated water.
[0038] The wash coat composition may have a solid content of 50% by weight or less. "Solid content" refers to the proportion of solid material present in the composition based on the total weight of the wash coat composition. The solid content of the wash coat composition is preferably in the range of 20 to 40% by weight, more preferably in the range of 30 to 35% by weight.
[0039] The washcoat composition may have an acidic pH. For example, the pH of the washcoat may be <7 or ≤5. For example, the washcoat composition may have a pH of about 3.
[0040] The wash coat composition may have a viscosity in the range of 100 to 1000 centipoise.
[0041] The washcoat composition may further contain organic additives such as rheological modifiers, dispersants, and / or other additives.
[0042] The relative amounts of each component used in the wash coat composition can be selected so that the wash coat has a desired solid content.
[0043] A preferred substrate includes a flow-through monolith having a so-called honeycomb shape, which contains multiple adjacent parallel channels that are open at both ends and often extend from the inlet to the outlet surface of the substrate, resulting in a high surface area-to-volume ratio. The catalyst composition is coated onto the walls of the channels so that, during use, the exhaust gas comes into contact with the catalyst as it flows through the channels.
[0044] The monolithic substrate may be an inert substrate. The substrate may be composed of a ceramic material or a metallic material. For example, the substrate may be made of or composed of cordierite (SiO2-Al2O3-MgO), silicon carbide (SiC), Fe-Cr-Al alloy, Ni-Cr-Al alloy, aluminum titanate, or stainless steel alloy.
[0045] The shape, size, and cell density of the honeycomb substrate are typically selected to optimize the exposure of the catalytic activator in the catalytic article to exhaust gases during use. For example, if the intended use of the catalytic article is the treatment of emissions from an internal combustion engine fueled by natural gas (e.g., a two-stroke reciprocating engine), the substrate may be cylindrical or substantially cylindrical in shape with a diameter ranging from 20 to 40 inches. The cell density may range from 100 to 400 cpsi (cells / square inch) or 200 to 400 cpsi, for example, about 300 cells / square inch.
[0046] Alternatively, if the intended use of the catalyst article is the treatment of emissions from a gas turbine, the substrate may have a square or rectangular cross-section. Typically, in such applications, multiple wash-coated substrates are stacked in a grid pattern to fill flue ducts. Such substrates may have a cross-sectional area of approximately 24 × 24 inches and a depth of approximately 3.5 inches. The cell density may range from 100 to 400 cpsi, for example, 200 to 300 cpsi.
[0047] One method for applying a wash coating to a honeycomb substrate involves positioning the substrate so that the channels are substantially vertically oriented, applying the wash coat composition to a first surface (e.g., the top surface) of the substrate, and subjecting the opposite second surface (e.g., the bottom surface) of the substrate to at least partial vacuum to achieve movement of the wash coat composition through the channels. Monolithic substrates can be coated in a single dose, and the wash coat can be applied to the substrate in a single step while the substrate remains in a single orientation. Alternatively, the substrate can be coated in two injections. For example, in the first dose, the monolithic substrate is in a first orientation with the first surface at the top and the second surface at the bottom. The coating is applied to the first surface, coating a length portion of the substrate. The substrate is then inverted so that the second surface is at the top. Next, the coating is applied to the second surface to coat the portion of the substrate that was not coated by the first injection. International Publication No. 99 / 47260 describes a general method for coating monolithic substrates.
[0048] Other methods for coating the substrate include immersing the substrate in a washcoat composition or passing the substrate through a curtain or waterfall of the washcoat composition. Compressed air can be used to blow the fluid into the substrate and pass it through to ensure that the cells are coated and that there are no or substantially no blocked cells.
[0049] If the method further includes steps (d) and (e) as defined above, the application of the impregnation solution to the substrate for forming the second coating may be carried out in a manner similar to the application of the wash coating in step (b).
[0050] This disclosure further provides catalyst articles obtained or obtainable by the methods described above or using the wash-coat compositions described above. In particular, such catalyst articles include a substrate having a layer of catalyst material coated thereon. The catalyst material is a carrier material impregnated with PGM components, comprising a carrier material comprising a mixed oxide, a mixture of oxides or a molecular sieve containing (i) alumina and (ii) silica and / or zirconia, and at least 100 m 2 / g, at least 150m 2 / g, at least 200m 2 / g, at least 250m 2 / g or at least 300m 2 A metal oxide having a BET surface area of 1 / g, which may include at least one of titania, silica, or zirconia. Preferably, the carrier material is a silica-alumina mixed oxide, and the metal oxide is titania.
[0051] The catalyst articles obtained by the above process can be used to treat exhaust gases from internal combustion engines (such as diesel engines or internal combustion engines that use natural gas or methanol as fuel) or gas turbines. In particular, the catalyst articles can be used to reduce formaldehyde and / or carbon monoxide emissions from internal combustion engines that use natural gas or turbines that use natural gas as fuel. In addition, the catalyst articles may be used to decompose ozone (O3) present in exhaust gases or airflows. [Examples]
[0052] The present invention will be further described with reference to the following examples, which are illustrative and not intended to limit the present invention.
[0053] ●Comparative Example 1 Alumina powder was slurryed in water and ground to a d50 < 10 microns. The slurry had a solid content of ≤ 50% and a pH of ≤ 7. The slurry was applied as a washcoat to a 200 cells / square inch (cpsi) metal honeycomb monolith substrate. The coated substrate was dried and then calcined at a temperature of 525°C. An impregnation solution was prepared using platinum tetraamine acetate. The impregnation solution was coated onto the washcoated metal substrate and dried. Next, the impregnated coated substrate was calcined at 525°C. The resulting catalyst was 8.25 g ft -3 It contained a total PGM load of Pt. The alumina load was 1.6 g / in -3 That was the case.
[0054] ●Example 2 Alumina-silica (70% alumina, 30% silica) mixed oxide powder was slurryed in water and ground to a d50 < 10 microns. The slurry had a solid content of less than 50% and a pH of less than 7. ≥ 300m 2 A titania sol having a surface area of / g, a pH of approximately 1, D50 and D90 particle sizes of <0.2 microns and <0.5 microns, respectively, and a TiO2 content of approximately 20% by weight, was added to the washcoat and mixed in a high-shear mixer for 1 hour. The resulting slurry was then applied as a washcoat to a 200 cpsi metal honeycomb monolith substrate and dried. An impregnation solution containing platinum nitrate in an acidic solution was prepared. The impregnation solution was applied to the washcoated metal substrate and dried. Next, the impregnated coated substrate was calcined at 525°C. The resulting catalyst was 8.25 g ft -3 The total PGM load on the Pt was 1.6 g / in. -3 The titania load is 0.178 g / in -3 That was the case.
[0055] ●Comparative Example 3 Alumina-silica (70% alumina, 30% silica) mixed oxide powder was slurryed in water and pulverized to a d50 < 10 microns. The slurry had a solid content of less than 50% and a pH of less than 7. The obtained slurry was then applied as a washcoat to a 200 cpsi metal honeycomb monolith substrate and dried. An impregnation solution containing platinum nitrate in an acidic solution was prepared. The impregnation solution was applied to the washcoated metal substrate and dried. Next, the impregnated coated substrate was calcined at 525°C. The resulting catalyst had a total PGM load of 8.25 g ft-3 Pt. The alumina-silica load was 0.8 g / in-3.
[0056] ●Example 4 Alumina-silica (70% alumina, 30% silica) mixed oxide powder was slurryed in water and ground to a d50 < 10 microns. The slurry had a solid content of less than 50% and a pH of less than 7. ≥ 300m 2 A titania sol having a surface area of approximately 1 / g, a pH of approximately 1, D50 and D90 particle sizes of <0.2 microns and <0.5 microns, respectively, and a TiO2 content of approximately 20% by weight was added to the washcoat and mixed in a high-shear mixer for 1 hour. The resulting slurry was then applied as a washcoat to a 200 cpsi metal honeycomb monolith substrate and dried. An impregnation solution containing platinum nitrate in an acidic solution was prepared. The impregnation solution was applied to the washcoated metal substrate and dried. Next, the impregnated coated substrate was calcined at 525°C. The resulting catalyst had a total PGM load of 4 g ft-3 Pt. The alumina-silica load was 1.6 g / in-3, and the titania load was 0.178 g / in-3.
[0057] ● Carbon monoxide oxidation activity Core samples of the same volume (1.0 × 3.5 inches) were taken from the catalyst articles prepared in each of the above examples and tested in a synthetic catalytic activity test (SCAT) apparatus at a selected inlet temperature in a GHSV for 200,000 hr-1 using the following inlet gas mixture: 50 ppm CO, 20 ppm NO, 15 ppm C1 propene, 15% O2, 8% H2O, 3% CO2, and the remainder N2. Catalyst samples were tested both under fresh conditions and after hydrothermal sulfur aging (25 ppm SO2, 15% O2, 8% H2O, 3% CO2, and the remainder N2, at 250°C for 24 hours).
[0058] The results for Comparative Example 1 and Example 2 are shown in Figure 1. Figure 1 compares the CO conversion rates achieved by the catalyst articles of Examples 1 and 2 at the selected inlet temperature.
[0059] The results for Comparative Example 3 and Example 4 are shown in Figures 2 and 3. Figure 2 compares the CO conversion rates achieved by the catalyst article of Comparative Example 3 at the selected inlet temperature. Figure 3 compares the CO conversion rates achieved by the catalyst article of Example 4 at the selected inlet temperature.
[0060] As demonstrated by the data shown in Figure 1, both catalyst articles achieve comparable CO oxidation rates under fresh conditions; however, after sulfur aging, the CO oxidation activity of the catalyst article prepared in Example 2 is significantly improved compared to that of the catalyst article in Example 1.
[0061] As demonstrated by the data shown in Figures 2 and 3, under both fresh and aged conditions, the catalyst article of Example 4 provides a CO oxidation rate equivalent to or better than that of the catalyst article of Comparative Example 3, despite a significantly reduced PGM load.
[0062] Further aspects and embodiments of this disclosure are described in the following numbered clauses.
[0063] Clauses: 1. A method for preparing a catalyst article, (a) At least the following components: ● A carrier material comprising a mixed oxide, a mixture of oxides, or a molecular sieve containing (i) alumina and (ii) silica and / or zirconia. ● A metal oxide sol containing at least one of titania, silica, or zirconia. ●A process of preparing a wash coat composition by combining liquid media, (b) A step of applying the wash coat composition to a substrate to form a wash coating, (c) a step of drying and / or firing the wash coating, A method further comprising the step of impregnating a carrier material with a platinum group metal component. 2. The method specified in Clause 1, wherein step (a) includes mixing the components together by stirring. 3. A method specified in Clause 1 or 2, wherein the carrier material includes mixed oxides. 4. The method specified in Clause 1 or 2, wherein the carrier material is a silica-alumina mixed oxide, a zirconia-alumina mixed oxide, or an aluminosilicate molecular sieve. 5. A method specified in any one of clauses 1 to 4, wherein the carrier material is a silica-alumina mixed oxide. 6. The method specified in Clause 5, wherein the silica-alumina mixed oxide has a silica content in the range of 1-40% by weight, 2-35% by weight, 5-35% by weight, or 5-30% by weight. 7. A method according to any one of clauses 1 to 5, wherein the silica-alumina mixed oxide has a silica content in the range of 2 to 10% by weight. 8. The silica-alumina mixed oxide having a silica content of approximately 5% by weight, as specified in Clause 7. 9. A method according to any one of clauses 1 to 5, wherein the silica-alumina mixed oxide has a silica content in the range of 25 to 40% by weight. 10. The method specified in Clause 9, wherein the silica-alumina mixed oxide has a silica content of approximately 30% by weight. 11. A method according to any one of the clauses 1 to 10, wherein the carrier material has a D90 particle size of ≤50 μm or ≤30 μm. 12. The prepared catalyst article contains 0.5-4 g / in 3 Preferably 1-2 g / in 3 A method specified in any one of clauses 1 to 11, wherein the amount of carrier material used in step (a) is selected to include a carrier material load within the range of the specified amount. 13. A method according to any one of clauses 1 to 12, wherein the carrier material is impregnated with the PGM component prior to step (a) by contacting the carrier material with the impregnation solution, and the impregnation solution contains the PGM component. 14. A method according to any one of clauses 1 to 13, wherein the wash coat composition formed in step (a) is blended with an impregnation solution containing the PGM component, thereby impregnating the carrier material with the PGM component after step (a) and before step (b). 15. A method, as specified in any one of Clauses 1 to 13, wherein, after step (c), the carrier material is impregnated with a platinum group metal component by contacting the substrate with the impregnation solution, and the impregnation solution contains a platinum group metal component. 16. After step (c), the carrier material is impregnated with platinum group metal components. (d) Applying an impregnation solution containing PGM components to the substrate to form a second coating, (e) A method provided for in any one of clauses 1 to 13, further comprising drying and / or firing the second coating. 17. A method as prescribed in any one of Clauses 1 to 16, wherein the platinum group metal component comprises platinum, palladium, or a mixture of platinum and palladium. 18. A method as defined in Clause 17, wherein the platinum group metal component includes platinum. 19. The method specified in Clause 18, wherein the platinum group metal component is platinum nitrate or platinum acetate. 20. A method specified in any one of clauses 13 to 16, or any one of clauses 17 to 19 as applicable to any one of clauses 13 to 16, wherein the impregnation solution is an aqueous solution of a platinum group metal component. 21. The prepared catalyst material is 1-100 g / ft3 , 4-90g / ft 3 8-50g / ft 3 Or 20-35g / ft 3 A method as specified in any one of Clauses 1 to 20, wherein the amount of platinum group metal used in the impregnation process is selected to include a platinum group metal loading within the range of . 22. In step (c), the wash coating is dried at a temperature below 120°C, as specified in any one of clauses 1 to 21. 23. In step (c), the wash coating is fired at a temperature in the range of 450 to 550°C, as specified in any one of clauses 1 to 22. 24. In step (e), the second coating is dried at a temperature below 120°C, using the method specified in Clause 16 or any one of Clauses 17 to 23 if dependent on Clause 16. 25. In step (e), the second coating is fired at a temperature in the range of 450 to 550°C, using the method specified in Clause 16 or any one of Clauses 17 to 24 if dependent on Clause 16. 26. A method specified in any one of clauses 1 to 25, wherein the metal oxide sol is a titania sol. 27. The metal oxide in the metal oxide sol is ≥100m 2 / g, ≥150m 2 / g, ≥200m 2 / g, ≥250m 2 / g or ≥300m 2 A method having a BET surface area of / g as specified in any one of clauses 1 to 26. 28. A method according to any one of clauses 1 to 27, wherein the metal oxide sol has a D50 particle size of ≤1 μm, ≤0.5 μm, or ≤0.2 μm. 29. A method according to any one of Clauses 1 to 28, wherein the metal oxide sol has a D90 particle size of ≤5 μm, ≤2 μm, ≤1 μm, or ≤0.5 μm. 30. The prepared catalyst article is ≤2.5 g / in 3 ≤2g / in 3 ≤1g / in 3 ≤0.5g / in 3 or ≤0.2 g / in3 A method as specified in any one of Clauses 1 to 29, wherein the amount of metal oxide sol used in step (a) is selected so as to have a metal oxide loading amount. 31. A method specified in any one of the clauses 1 to 30, wherein the liquid medium is water. 32. The method according to any one of the clauses 1 to 31, wherein the wash coat composition prepared in step (a) has a solid content of 50% by weight or less. 33. The method specified in Clause 32, wherein the wash coat composition prepared in step (a) has a solid content in the range of 20-40% by weight or 30-35% by weight. 34. The wash coat composition prepared in step (a) has a pH of <7, ≤5, or about 3, as specified in any one of the clauses 1 to 33. 35. The method according to any one of the clauses 1 to 34, wherein the wash coat composition prepared in step (a) has a viscosity in the range of 100 to 1000 centipoise. 36. A method specified in any one of clauses 1 to 35, wherein the substrate is a flow-through monolith substrate. 37. The method specified in Clause 36, wherein the substrate is substantially cylindrical in shape and has a diameter in the range of 20 to 40 inches and a cell density in the range of 200 to 400 cpsi. 38. The method specified in Clause 36, wherein the substrate has a substantially square or rectangular cross-section. 39. ●A carrier material comprising a mixed oxide, a mixture of oxides, or a molecular sieve containing (i) alumina and (ii) silica and / or zirconia, ● A metal oxide sol containing at least one of titania, silica, or zirconia, A wash coat composition comprising a liquid medium. 40. A wash coat composition as defined in Clause 38, wherein the carrier material comprises a mixed oxide. 41. A wash coat composition as specified in Clause 38 or 39, wherein the carrier material is a silica-alumina mixed oxide, a zirconia-alumina mixed oxide, or an aluminosilicate molecular sieve. 42. A wash coat composition as defined in Clause 40 or 41, wherein the carrier material is a silica-alumina mixed oxide. 43. A wash coat composition as defined in Clause 42, wherein the silica-alumina mixed oxide has a silica content in the range of 1-40% by weight, 2-35% by weight, 5-35% by weight, or 5-30% by weight. 44. A wash coat composition as defined in any one of clauses 38 to 42, wherein the silica-alumina mixed oxide has a silica content in the range of 2 to 10% by weight. 45. A wash coat composition as defined in Clause 44, wherein the silica-alumina mixed oxide has a silica content of approximately 5% by weight. 46. A wash coat composition as defined in any one of clauses 38 to 42, wherein the silica-alumina mixed oxide has a silica content in the range of 25 to 40% by weight. 47. A wash coat composition as defined in Clause 46, wherein the silica-alumina mixed oxide has a silica content of approximately 30% by weight. 48. A wash coat composition as specified in any one of clauses 38 to 47, wherein the carrier material has a D90 particle size of ≤50 μm or ≤30 μm. 49. A wash coat composition as defined in any one of clauses 38 to 48, wherein a carrier material is impregnated with a platinum group metal component. 50. A wash coat composition as defined in Clause 49, wherein the platinum group metal component comprises platinum, palladium, or a mixture of platinum and palladium. 51. A wash coat composition as defined in Clause 50, wherein the platinum group metal component includes platinum. 52. A wash coat composition as defined in Clause 51, wherein the platinum group metal component is platinum nitrate or platinum acetate. 53. A wash coat composition as defined in any one of clauses 38 to 52, wherein the metal oxide sol is titania sol. 54. Metal oxide sols, ≥100 m 2 / g, ≥150m 2 / g, ≥200m 2 / g, ≥250m 2 / g or ≥300m 2A wash coat composition having a BET surface area of 1 / g as defined in any one of clauses 38 to 53. 55. A method according to any one of the clauses 38 to 54, wherein the metal oxide sol has a D50 particle size of ≤1 μm, ≤0.5 μm, or ≤0.2 μm. 56. A method according to any one of clauses 38 to 55, wherein the metal oxide sol has a D90 particle size of ≤5 μm, ≤2 μm, ≤1 μm, or ≤0.5 μm. 57. A wash coat composition as defined in any one of clauses 38 to 56, wherein the liquid medium is water. A wash coat composition as defined in any one of clauses 38 to 57, having a solid content of 58.50% by weight or less. A wash coat composition as defined in Clause 58, having a solid content in the range of 59.20-40% by weight or 30-35% by weight. 60. A wash coat composition as defined in any one of clauses 38 to 59, having a pH of <7, ≤5, or about 3. 61. A wash coat composition as defined in any one of clauses 38 to 60, having a viscosity in the range of 100 to 1000 centipoise. 62. A wash coat composition as defined in any one of clauses 38 to 61, further comprising an organic additive.
Claims
1. A method for preparing a catalyst article used to treat carbon monoxide and / or formaldehyde emissions from an internal combustion engine or a turbine that uses natural gas as fuel, (a) at least the following components: ● Carrier material that is a silica-alumina mixed oxide, a zirconia-alumina mixed oxide, or an aluminosilicate molecular sieve. ● Metal oxide sols containing titania, ●A process of preparing a wash coat composition by combining liquid media, (b) A step of applying the wash coat composition to a substrate to form a wash coating, (c) a step of drying and / or firing the wash coating, The process further includes impregnating the carrier material with a platinum group metal component. The metal oxide in the aforementioned metal oxide sol is ≥ 300 m 2 A method having a BET surface area of 1 / g.
2. The method according to claim 1, wherein the carrier material is a silica-alumina mixed oxide.
3. The method according to claim 2, wherein the carrier material is a silica-alumina mixed oxide having a silica content in the range of 1 to 40% by weight.
4. The method according to any one of claims 1 to 3, wherein the carrier material has a D90 particle size of ≤ 50 μm.
5. The method according to any one of claims 1 to 4, wherein, prior to step (a), the carrier material is impregnated with a platinum group metal component by contacting the carrier material with an impregnation solution, and the impregnation solution contains the platinum group metal component.
6. The method according to any one of claims 1 to 4, wherein the wash coat composition formed in step (a) is blended with an impregnation solution containing a platinum group metal component, thereby impregnating the carrier material with the platinum group metal component after step (a) and before step (b).
7. After step (c), the carrier material is impregnated with a platinum group metal component. (d) Applying the impregnation solution containing the platinum group metal component to the substrate to form a second coating, (e) The method according to any one of claims 1 to 4, further comprising drying and / or firing the second coating.
8. The method according to any one of claims 1 to 7, wherein the platinum group metal component comprises platinum, palladium, or a mixture of platinum and palladium.
9. The method according to any one of claims 1 to 8, wherein the platinum group metal component is platinum nitrate or platinum acetate.
10. The method according to any one of claims 1 to 9, wherein the metal oxide sol has a D50 particle size of ≤ 1 μm.
11. A washcoat composition used in a method for preparing a catalyst article for treating carbon monoxide and / or formaldehyde emissions from an internal combustion engine or a turbine fueled by natural gas, ● A carrier material which is a silica-alumina mixed oxide, a zirconia-alumina mixed oxide, or an aluminosilicate molecular sieve, ●A metal oxide sol containing titania, ●Includes a liquid medium, The metal oxide in the aforementioned metal oxide sol is ≥ 300 m 2 Having a BET surface area of / g, A wash coat composition in which the carrier material is impregnated with a salt of a platinum group metal selected from ruthenium, rhodium, palladium, osnium, platinum, or a mixture thereof.
12. The wash coat composition according to claim 11, wherein the carrier material is a silica-alumina mixed oxide and the metal oxide sol is a titania sol.
Citation Information
Patent Citations
Exhaust gas purifying catalyst
JP1995155613A
Catalyst for purification of exhaust gas and its production
JP1996150335A
Purifyication of waste gas
JP1999128687A
Carbon monoxide selective oxidation catalyst and selective removal method for carbon monoxide
JP2001224965A
Exhaust gas treatment catalyst and its manufacturing method