Microcrystalline nanoscale silicon particles and their use as anode active material in lithium-ion secondary batteries

Nanoscale amorphous silicon particles with a carbon coating, produced via vapor condensation and heat treatment, address dendrite and SEI issues, enhancing the cycleability and specific capacity of lithium-ion batteries.

JP7954661B2Active Publication Date: 2026-11-20セネート アクティーゼルスカブ
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023558375
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-26
Filing Date
2022-03-25
Publication Date
2026-11-20
Estimated Expiration
2042-03-25

AI Technical Summary

Technical Problem

Existing lithium-ion batteries face challenges with dendrite formation, anisotropic stress leading to fracture and pulverization of silicon anodes, and irreversible capacity loss due to the formation of a solid electrolyte interphase (SEI), which limits their ability to meet the high energy density requirements for electric vehicles.

Method used

The production of nanoscale amorphous silicon particles with a carbon coating, achieved through vapor condensation and controlled heat treatment, maintains an amorphous phase at higher temperatures, reducing crystallization and enhancing Coulomb efficiency, and forms a stable SEI layer, thereby improving cycleability and specific capacity.

Benefits of technology

The nanoscale amorphous silicon particles with controlled microcrystallization and carbon coating exhibit improved cycleability, high specific capacity, and reduced irreversible capacity loss, making them suitable for high-energy density lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954661000006
    Figure 0007954661000006
  • Figure 0007954661000007
    Figure 0007954661000007
  • Figure 0007954661000008
    Figure 0007954661000008
Patent Text Reader

Abstract

The present invention relates to a method for producing microcrystalline nanoscale silicon particles, to the particles produced by this method, and to secondary electrochemical cells using said particles as the active material of the negative electrode of a secondary electrochemical cell, the silicon particles having the formula Si (1-x) M x where 0.005≦x≦0.20 and M is at least one substitution element selected from C, N or mixtures thereof, and the particles are subjected to a heat treatment at 800-900° C. to be converted into a microcrystalline phase having a crystallite size in the range of 1-15 nm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a method for producing nanoscale microcrystalline silicon particles, the produced particles, and a secondary electrochemical cell that utilizes these particles as the active material for the negative electrode of the secondary electrochemical cell. [Background technology]

[0002] In today's society, which is powered by fossil fuels, the use of renewable energy and electricity is rapidly increasing in many sectors, making it necessary to achieve the goals of the Paris Agreement under the United Nations Climate Agreement. A key factor in achieving these goals is access to rechargeable batteries with superior specific energy.

[0003] Lithium is 0.534 g / cm³ 3 It has a relatively very low density, and also half-reacted Li 0 →Li + +e - It has a high standard reduction potential of -3.045V. This makes lithium an attractive candidate for manufacturing electrochemical cells with high energy density. However, secondary (rechargeable) electrochemical cells with metallic lithium anodes have been shown to suffer from a persistent problem of dendrite formation during charging, which tends to short-circuit the electrochemical cell after several charge-discharge cycles.

[0004] The dendrite problem was solved by applying a negative electrode that can store lithium atoms in a releaseable manner through intercalation. Such batteries are known as lithium-ion secondary batteries (LIBs). The electrochemical properties of an LIB are directly influenced by the physical and chemical properties of the negative electrode active material. The selection and preparation of the material, as well as appropriate structural modifications and designs of the active material, both affect battery performance. A key issue in this regard is to reliably and reversibly store lithium atoms at a high volume density when the battery is charged, and then release the lithium into ions (Li) when discharged through a large number of consecutive charge-discharge cycles.+ The goal was, and still is, to find an active material that can be released as )

[0005] Currently, most commercially available lithium-ion batteries (LIBs) use graphite as the active material for the negative electrode. Graphite can accommodate / fill one lithium ion per six carbon atoms through intercalation with minimal shape deformation, and has a theoretical specific energy of 372 mAh / g. Commercial secondary LIBs with graphite anodes typically achieve a specific energy of 100-200 Wh / kg, enabling, for example, a medium-sized long-range electric vehicle battery to weigh several hundred kilograms. This level of specific energy density is likely insufficient to meet the targets of the Paris Agreement.

[0006] One strategy to improve the specific energy of LIBs is to find a material with a higher lithium ion storage capacity than graphite, which is used as the active material for the negative electrode. One candidate that has been studied extensively in this regard is silicon, due to its high ability to store lithium atoms by diffusion and alloying. At typical ambient temperatures, the most lithified phase of silicon has a theoretical specific energy of 3579 mA h / g. 3、75 It is Si [Non-Patent Literature 1]. A silicon negative electrode also has the advantage of being able to provide an attractive operating potential that reduces safety concerns regarding lithium deposition during cell overcharging [Non-Patent Literature 2].

[0007] Li is the most lithium-concentrated state. 3.75In Si, the silicon material has a volume that is about 320% greater than that in the non-lithiated state. Wang et al. (2013) [Non-Patent Document 4] studied the diffusion kinetics of lithium in crystalline silicon, and found that the diffusion rate of lithium in silicon crystals is faster in the <110> direction than in the <100> direction and the <111> direction. This causes anisotropic expansion of silicon crystals during lithiation, and in turn, induces anisotropic stress that may cause fracture and pulverization of the silicon material. This anisotropic stress has been found to be reduced in some anode structures when the silicon material is amorphous compared to crystalline silicon [Non-Patent Document 3], which is probably due to the more isotropic expansion of amorphous silicon. Pulverization of the silicon material leads to rapid capacity fade of the battery due to loss of electrical contact, loss of active material within the electrode, ineffective electron transfer, repeated dynamic formation of the solid electrolyte interphase, and the like [Non-Patent Documents 1 and 2].

[0008] It has been demonstrated that the use of nanoscale particles in electrodes can provide electrodes with outstanding properties resulting from small particle sizes that bring effects such as improved electrical conductivity and improved mechanical and optical properties [Non-Patent Document 1]. Furthermore, since nanosized particles have a very high surface area to volume ratio, a negative electrode with a nanosized active material can provide excellent charge-discharge capacity due to the highly accessible surface for lithium ion adsorption / desorption [Non-Patent Document 1].

[0009] Several challenges in silicon / graphite anodes decrease as the silicon particles are made smaller. When the absolute expansion of each particle is reduced, the mechanical pressure from each surrounding particle decreases, and the diffusion distance of lithium inside the silicon becomes smaller. By increasing the surface area to volume ratio, the current density on the particle surface is reduced, and detrimental overpotential is lowered.

[0010] On the other hand, an increase in surface area introduces new issues such as a portion of Li being trapped at the surface itself in the anode (irreversible loss during the first cycle), as well as an increased risk of self-ignition in air and the potential for greater irreversible first-cycle losses related to silicon oxide formed during atmospheric exposure.

[0011] In LIBs with liquid electrolytes, a solid electrolyte interphase (SEI) is often formed during the initial lithiation. The formation of the SEI layer irreversibly consumes lithium, representing an irreversible capacity loss for the electrochemical cell [Non-Patent Document 1]. Accordingly, it is advantageous to form a stable SEI layer to limit SEI-induced loss of lithium during the initial lithiation / charging of the cell. To avoid direct contact between silicon and the electrolyte, coating the silicon surface with a suitable element can yield a stable SEI layer [Non-Patent Document 1], but it has been demonstrated that unprotected surfaces appear when cracks occur.

[0012] Carbon has been studied and utilized as a coating material and / or a composite material with silicon in LIBs that have nanostructured silicon as the active material in the negative electrode. Many silicon-carbon structures have been reported in the literature, ranging from simple mixtures of silicon to complex morphologies of silicon with graphene or graphite. While these complex structures exhibit excellent cyclability and capacity, they suffer from requiring a large number of charge-discharge cycles to reach high Coulombic efficiency, and require complicated multi-step synthesis processes to be scaled up to commercial production levels [Non-Patent Document 2].

[0013] From Sourice et al. (2016) [Non-Patent Document 2], a method is known for producing nanoscale amorphous silicon particles with a carbon shell / coating via a two-stage laser pyrolysis process, in which a silane gas stream diluted in an inert gas enters a first reaction zone irradiated by a CO₂ laser to decompose the silane gas into amorphous silicon core particles. Ethylene is then added to the gas carrying the formed silicon core particles, and this mixture is passed through a second reaction zone and irradiated by a CO₂ laser to decompose the ethylene into a carbon shell deposited on the silicon core particles. Amorphous silicon particles with a carbon coating have been found to exhibit excellent specific capacity and high charge-discharge cycle performance.

[0014] Patent Document 1 discloses an active material for a negative electrode of a LIB comprising a silicon-containing compound of formula SiC x , where x is 0.05 to 1.5, and the carbon concentration in the material follows the relationship A≦B, where A is the molar concentration ratio of carbon to silicon at the center of the active material, and B is the molar concentration ratio of carbon to silicon on / in the surface region of the active material. This document teaches that carbon may be covalently bonded to silicon, and further that the silicon-containing compound may be in the form of fine particles and have an amorphous molecular structure. Furthermore, paragraph

[0030] of Patent Document 1 describes that if the carbon content in the active material is too low, that is, when x is less than 0.05, the active material may deteriorate due to cracking.

[0015] From Patent Document 2, an active material for a negative electrode of a rechargeable LIB is known, which comprises an amorphous silicon-based compound of formula SiA x H y , where A is any one of carbon, nitrogen, or a combination thereof, and x>0, y>0, and 0.1≦x+y≦1.5. The active material may be in particulate form and coated with a carbon layer. The active material can be produced by a sputtering process using hydrogen gas and Si and C targets, or a plasma method using hydrogen gas, silane gas, and nitrogen gas.

[0016] Patent Document 3 discloses a reactor and method for producing crystalline or amorphous silicon particles by chemically depositing a silicon-containing precursor onto seed particles in a heated and rapidly rotating reactor space. The silicon-containing gas may be diluted in a carrier gas and may be one of SiH4, Si2H6, SiHCl3, or a mixture thereof. The carrier gas may be one of hydrogen, nitrogen, or argon. SiO x SiC x SiN x By introducing a second precursor gas, liquid, or substance containing a combination of C, O, or N with silicon, amorphous carbon, graphite, low-crystalline carbon, or short-range ordered graphene structures, the formed silicon particles can be given an outer layer of a second substance with a lower silicon content than the core material of the particles.

[0017] Wang et al. (2013) [Non-Patent Literature 4] are one of several research groups that have disclosed the formation of secondary particles from silicon nanoparticles and carbon precursors such as pitch, and the use of such particles in Li-ion batteries. Secondary particles reduce the interfacial region between silicon and electrolyte, thereby reducing the formation of a solid electrolyte interface (SEI), which is known to consume both lithium and electrolyte, thereby gradually reducing the battery capacity. The formation of an SEI in the first cycle is quantified by measuring the Coulomb efficiency (CE) of the first lithiumization cycle, and furthermore, the thickness and quality of the SEI can be estimated using XPS. Jeff Dahn (1995) [Non-Patent Literature 5] has demonstrated that the CE of carbon formed from pitch or sugar is improved if carbonization can occur at >500°C, preferably >700°C, more preferably >800°C for at least 2 hours. Escamilla-Perez et al. (2019) [Non-Patent Literature 6] actually performed thermal decomposition at 900°C for 3 hours.

[0018] Patent Document 4 discloses an extremely pure, nanoparticle-like amorphous silicon powder that can optionally be alloyed with an electron donor and / or electron acceptor. Furthermore, a method for producing the silicon powder and the use of a reactor for producing the silicon powder are disclosed. The silicon powder of this invention can preferably be used in the manufacture of semiconductor starting materials, semiconductors, thermocouples for energy recovery from waste heat, and especially thermocouples that are stable at high temperatures.

[0019] Patent Document 5 discloses silicon nanoparticles and a method for producing the same. This document particularly relates to silicon nanoparticles having an amorphous phase, by containing silicon as an active ingredient and having an excess amount of atoms P or B beyond the doping limit inside / outside the nanoparticles, and a method for producing the nanoparticles. The produced silicon nanoparticles have an amorphous secondary phase that acts as a shock absorber for the volume expansion and contraction that occurs during the charging and discharging of silicon, thereby improving the charge-discharge cycle (life) of secondary batteries using silicon nanoparticles as an anode material.

[0020] Therefore, in summary, the optimal silicon-based anode active material has several conflicting requirements. It must contain very small particles to reduce cracking, but not so small that it leads to the formation of excessively high SEI or uncontrolled oxidation during manufacturing. It must have isotropic or near-isotropic expansion, meaning the powder must not be single crystal, but the manufacturing of the final anode material requires temperatures up to about 900°C to improve Coulomb efficiency, which is the temperature at which pure silicon nanoparticles become crystalline. Preferably, it must be possible to charge quickly even on the first charge, maintaining almost all of the high charge capacity of silicon while minimizing the loss of efficiency in the first cycle. [Prior art documents] [Patent Documents]

[0021] [Patent Document 1] U.S. Patent Application Publication No. 2012 / 0107639 [Patent Document 2] European Patent No. 2405509 [Patent Document 3] International Publication No. 2018 / 052318 [Patent Document 4] European Patent Application Publication No. 3025702 [Patent Document 5] Korean Patent Application Publication No. 2016 / 0009807 Specification [Patent Document 6] UK Patent Application Publication No. 2592097 [Non-patent literature]

[0022] [Non-Patent Document 1] Qi et al. (2017), “Nanostructured anode materials for lithium-ion batteries: principles, recent progress and future perspectives”, J.Mater.Chem.A, vol.5, pp.19521-19540 [Non-Patent Document 2] Sourice et al. (2016), “Core-shell amorphous silicon-carbon nanoparticles for high performance anodes in lithium-ion batteries”, Journal of Power Sources, vol. 328, pp. 527-535 [Non-Patent Document 3] Berla,Lucas A.;Lee、Seok Woo;Ryu、Ill;Cui、Yi;Nix,William D.(2014),“Robustness of amorphous silicon during the initial lithiation / delithiation cycle”,Journal of Power Sources 258:253-259,Bibcode:2014JPS...258...253B.doi:10.1016 / j.jpowsour.2014.02.032.

Outdoor Tools 4

Direct Environment 5

Outdoor Configuration6

Direct Environment 7

Outdoor Track 8

Outdoor Tools9

Outdoor Tools 10

Outdoor Content11

[0023] The main object of the present invention is to provide nanoscale silicon-containing particles suitable for use as an active material in the negative electrode of a rechargeable lithium-ion electrochemical cell that satisfies the above requirements, and a method for producing nanoscale silicon-containing particles.

[0024] A further object of the present invention is to provide an anode material containing the silicon-containing particles described above.

[0025] A further object of the present invention is to provide a secondary electrochemical cell having a negative electrode containing nanoscale silicon-containing particles. [Means for solving the problem]

[0026] As described above, we have found that lithium-ion secondary batteries (LIBs) using amorphous silicon particles as electrode active materials have improved cycle capability. This is particularly true for nanoscale amorphous silicon particles having a carbon coating on their surface, which we found to have excellent specific capacity and high charge-discharge cycle capability, as reported in [Non-Patent Document 2].

[0027] The inventors have discovered that by producing nanoscale silicon particles through vapor condensation of a mixture of silicon precursor gas and a relatively small amount of a substitution element precursor gas, silicon-containing particles with a small atomic percent of the substitution element introduced into the silicon structure can be generated. The silicon phase is mainly amorphous and has been shown to be more heat resistant than the amorphous phase of pure silicon. That is, while amorphous pure silicon begins a phase transformation to crystalline silicon at temperatures below 700°C, these mainly amorphous particles, which have a small atomic percent of trace elements in their silicon structure, have been observed to remain in the mainly amorphous phase at temperatures up to approximately 750-820°C, depending on the degree of trace element substitution.

[0028] The increased temperature stability of these primarily amorphous silicon-containing particles is beneficial in that it allows for the formation of carbon coatings on the particle surface and carbon-based structures around the particles at higher temperatures without transforming the particles into a crystalline phase. That is, the beneficial amorphous structure is maintained at higher coating temperatures, which gives silicon particles with improved Coulomb efficiency compared to particles coated or calcined at lower carbonization temperatures, as observed by [Non-Patent Literature 5]. Therefore, electrode active materials containing such primarily amorphous nanoscale silicon-containing particles make it possible to form secondary LIBs with relatively high cycleability, high specific capacity, and high Coulomb effect.

[0029] Another beneficial property of nanoscale amorphous silicon is that the diffusion rate of lithium atoms in the silicon phase is higher compared to crystalline silicon. This results in two advantages: a more uniform distribution of lithium atoms during lithiation (less congestion in the outer regions) and thus a more uniform / isotropic expansion of silicon particles; and a considerable time saving related to the initial lithiation of the negative electrode in the industrial production of batteries.

[0030] Therefore, the applicant has applied for patent protection for these primarily amorphous silicon-containing particles in Patent Document 6, and the entirety of that application is incorporated herein. The primarily amorphous silicon-containing particles described in Patent Document 6 are of the formula Si (1-x) M x The compound consists of, where 0.005 ≤ x < 0.05, and M is at least one substitution element selected from C, N, or a combination thereof, and the particles, when subjected to XRD analysis using non-monochromatic CuKα radiation, exhibit one peak at approximately 28° and one peak at approximately 52°, and both peaks have a full width at half maximum of at least 5° when Gaussian peak fitting is used.

[0031] Patent Document 6 further discloses a negative electrode for a lithium-ion secondary electrochemical cell, comprising at least one particulate active material which is mainly amorphous silicon-containing particles, a particulate conductive filler material, a binder material, and a current collector substrate, wherein at least one particulate active material is embedded in the binder material to form an anode mass which is deposited on the current collector substrate as an anode mass layer.

[0032] Patent Document 6 also discloses composite particles comprising a plurality of primarily amorphous particles and a primarily carbon-containing material produced by the thermal decomposition of a carbon-rich material. Patent Document 6 further discloses a method for producing these primarily amorphous silicon-containing particles, the method comprising forming a homogeneous gas mixture of a first precursor gas of a silicon-containing compound and at least one second precursor gas of a substitution element M-containing compound, injecting the homogeneous gas mixture of the first and second precursor gases into a reactor space, where the precursor gases are heated to a temperature in the range of 700-900°C so that the precursor gases react to form particles, recovering the particles and cooling them to a temperature in the range of ambient temperature to about 350°C, wherein the relative amounts of the first and second precursor gases are adapted so that the formed particles obtain an atomic ratio M:Si in the range of [0.005, 0.05].

[0033] As used herein, the term “primarily amorphous” encompasses silicon materials ranging from those with a 100% amorphous molecular structure to those containing extremely small crystalline domains on an atomic length scale (virtually undetectable by XRD analysis).

[0034] This invention can be considered a further development of the invention described in Patent Document 6, and is based on the further discovery that when these mainly amorphous silicon-containing particles are heated to a temperature at which they crystallize, for example, 800-900°C, significantly smaller microcrystals can be obtained compared to the microcrystal size obtained when pure amorphous silicon particles are heated to the same temperature, depending on the carbon and / or nitrogen content in the silicon structure.

[0035] As shown in Domi et al. (2019) [Non-Patent Literature 7], which studied the effect of microcrystal size on the electrochemical properties of silicon particles of the same size when used as electrode active material in secondary LIBs, smaller microcrystal sizes are preferable to larger microcrystal sizes by significantly improving cycleability, thus making them suitable for such applications. This effect is thought to be due to lithium ions diffusing along crystal boundaries faster than in bulk silicon (see, for example, Buonassisi et al. (2006) [Non-Patent Literature 8]) and the fact that diffusion is faster as the boundary widens. Domi et al. suggested that since grain boundaries between larger microcrystals are usually wider than those between smaller microcrystals, Li in the microcrystals at the grain boundaries... + We hypothesize that the concentration gradient is higher in larger microcrystals compared to smaller microcrystals. This means that the strain from the corresponding volume expansion is less in smaller microcrystals, and they have greater resistance to volume changes associated with charge-discharge cycles. As the concentration gradient decreases, the amount of Li flux decreases, so the Li in the microcrystals + A decrease in the concentration gradient tends to negatively affect velocity performance. On the other hand, this effect is mitigated as the microcrystal size decreases, because the surface area on which Li atoms can enter silicon increases. Domi et al. (2019) [Non-Patent Literature 7] found a decrease in velocity performance when comparing particles with a microcrystal size of 80 nm to particles with a microcrystal size of 30 nm. This may not apply to the small microcrystals of the particles of the present invention, which are 1 to 15 nm in size, because the surface area of ​​the microcrystal becomes considerably larger in such small microcrystals.

[0036] A related but not identical hypothesis, to which the inventors believe there may be a contribution, is based on the same understanding that Li ions move faster along grain boundaries, meaning that the expansion of polycrystalline nanoparticles is more isotropic and amorphous compared to single-crystal or small-crystal nanoparticles. Due to the high-speed ion movement along grain boundaries, polycrystalline nanoparticles rapidly acquire Li ions distributed beyond several internal crystal boundaries during charging. Subsequently, as the ions begin to diffuse into the bulk of each nanocrystal, although their crystal orientations are very small and fluctuating, the overall effect is that the particles themselves expand much more isotropically than single-crystal or small-crystal particles. This would be very beneficial against the mechanical pressure around the nanoparticles. It also reduces the tendency of the outer surface layer of silicon particles to crack compared to the single-crystal state where the outer layer expands strongly by complete lithiation before the inner bulk phase begins to expand. In addition to this, it leads to the fact that the internal diffusion of Li ions actually utilizes a much larger surface area because the inner surface rapidly exchanges ions with the outer surface. Therefore, the overpotential required to drive ion exchange across the particle surface can be reduced, and the risk of ionization of silicon atoms on the surface is similarly reduced, making the surface more stable.

[0037] Furthermore, the relative abundance of microcrystalline boundaries within polycrystalline silicon nanoparticles significantly accelerates the initial lithiumization process of silicon particles compared to single-crystal silicon particles of similar size. This results in substantial cost reductions in the mass production lines of secondary lithium-ion batteries (LIBs).

[0038] The thermodynamically stable state at the temperature at which amorphous silicon-containing particles primarily crystallize is when the C and / or N content of the particles exists as SiC and / or Si3N4 phases, and the remaining Si exists as pure Si crystals. (1-x) C x Phase or Si (1-x) N xC and / or N present in the phase attempt to diffuse from the bulk phase at such temperatures and accumulate at crystal boundaries as either SiC or Si3N4. However, the reaction rate of solid diffusion is considered too slow to achieve complete separation of Si and C or N content during the typical heat treatment time associated with the manufacture of negative electrodes for secondary LIBs. Therefore, the polycrystalline silicon-containing particles obtained by the present invention are pure Si (1-x) M x It is thought to be somewhere between the particles and pure composite particles of Si, SiC, and / or Si3N4. However, the total C and / or N content of the particles will be the same regardless of the degree of phase separation.

[0039] Furthermore, it has been observed that the formation of nanoscale microcrystalline structures is primarily promoted by a slightly higher trace element content compared to the predetermined range for amorphous particles.

[0040] Therefore, in the first embodiment, the present invention relates to silicon-containing particles, Particle size is determined by Brunauer-Emmet-Teller (BET) analysis according to ISO 9277:2010, ranging from 25 to 182 mm. 2 Having a surface area of ​​ / g, Silicon-containing particles are given by the formula Si (1-x) M x It contains the compound, where, 0.0005 ≤x ≤ 0.20, and M is at least one substitution element selected from C, N, or a combination thereof. The silicon-containing particle compound has a microcrystalline size in the range of 1 to 15 nm, as determined by the Rietveld method.

[0041] The determination of microcrystal size by the Rietveld method is well known to those skilled in the art and belongs to general knowledge, as demonstrated, for example, in the text "The Rietveld Method" edited by RA Young [Non-Patent Literature 9]. An example of applying the Rietveld method using XRD data can be described as follows: The microcrystal size τ is determined from the sharp features in the XRD data, i.e., the width of the Bragg peak. Analysis is performed by fitting the XRD data calculated from a crystalline Si model to experimental data using the least squares method, which is known as Rietveld refinement [Non-Patent Literature 10]. Rietveld refinement can be performed using free software such as GSAS-II [Non-Patent Literature 11] or commercially available software such as Topas [Non-Patent Literature 12]. The instrument's contribution to the Bragg peak width is calculated from the instrument's geometry ("fundamental parameter approach" [Non-Patent Literature 13]) or explained by a Thomson-Cox-Hastings pseudo-Voigt function experimentally determined from highly crystalline standards such as NIST SRM 640f silicon [Non-Patent Literature 14]. The instrument's contribution to the Bragg peak remains fixed during Rietveld refinement. All observed additional broadening of the Bragg peak is presumed to be due to small microcrystallization size and to have a Lorentz shape. This broadening of microcrystallization size is modeled by refining the calculated additional contribution β to the Bragg peak width, which varies with the scattering angle.

number

[0042] In exemplary embodiments, the silicon-containing particles according to the first aspect of the present invention are advantageous in that they contain only C and / or N (excluding unavoidable impurities). That is, the silicon-containing particles have a total content of C and / or N of 0.05 to 20 atomic percent, with the remainder being Si and unavoidable impurities.

[0043] The chemical formula used here is Si (i-x) M x ( 0.0005 The expression (≤x ≤ 0.20) should be interpreted and understood in accordance with IUPAC Recommendation 2005 IR-11.3.2 "Phases with Variable Composition" for Inorganic Chemical Nomenclature. That is, the above formula defines a single (phase) compound having a composition that changes, either alone or partially, by isovalent substitution of Si atoms with M atoms by an amount determined by the variable "x". Thus, the term "silicon-containing particles" used herein means that the particles are made from a silicon-dominant phase containing alloying elements dispersed in the molecular structure of the silicon phase. The M atoms are chemically bonded and dispersed as in alloys, and the most adjacent and next-closest adjacent atoms to a typical M atom are Si atoms. Depending on the material history, it may also contain small amounts of separated phase SiC and Si3N4.

[0044] In an exemplary embodiment, the silicon-containing particles according to the first aspect of the present invention are of the formula Si (1-x) M x The compound consists of, where M is at least one substitution element selected from C, N, or a combination thereof, and x is 0.001 ≤ x ≤ 0.15, preferably 0.005 ≤ x ≤ 0.10, more preferably 0.0075 ≤ x ≤ 0.075, more preferably 0.01 ≤ x ≤ 0.05, and most preferably 0.02 ≤ x ≤ 0.03.

[0045] The particles according to the present invention have a density of approximately 2200 kg / m³. 3 We found that these particles have a density of 25-182m. Therefore, assuming that these particles are spherical or quasi-spherical and non-porous, 2 The BET surface area per gram corresponds to the average particle size in the range of 15-110 nm (approximate estimate).

[0046] Furthermore, in an exemplary embodiment of the present invention relating to the first aspect, the silicon-containing particles are 34-136m 2 / g, preferably 39-109mg 2 The range of / g, more preferably 45-91m 2 / g, most preferably 54-68m 2 The BET surface area may be in the range of / g. These BET surface areas correspond to the average particle size in the range of 20-80 nm, preferably 25-70 nm, preferably 30-60 nm, and most preferably 40-50 nm. Determining the BET of particle surface area is well known to those skilled in the art. An example of a standard that can be applied to determine the BET surface area of ​​mainly amorphous silicon-containing particles according to the first and second embodiments of the present invention is ISO 9277:2010.

[0047] Since the microcrystal size is in the range of 1 to 15 nm, which is smaller than the particle size of 15 to 100 nm, the silicon-containing particles according to the first embodiment are polycrystalline nanoscale particles. The polycrystalline structure makes the particles according to the present invention more resistant to charge-discharge cycles than similar nanoscale silicon particles having larger and therefore fewer microcrystals, as observed by Domi et al. (2019) [Non-Patent Literature 7]. In an exemplary embodiment of the present invention according to the first embodiment, the silicon-containing particle compound may have a microcrystal size in the range of 2 to 12 nm, preferably 3 to 10 nm, more preferably 4 to 8 nm, and most preferably 5 to 6 nm, as determined by Rietveld refinement, where the instrument Bragg peak profile was calculated from basic parameters and refined to account for Lorentzian and Gaussian sample spreading due to small particle size, and then the particle size was calculated using Scherrer's formula from the sample's contribution to the total width at half maximum (FWHM) using a shape factor of 0.89.

[0048] In one exemplary embodiment, the silicon-containing particles according to the first aspect of the present invention may further include a carbon coating having a thickness in the range of 0.2 to 10 nm, preferably 1.5 to 8 nm, more preferably 2 to 6 nm, and most preferably 3 to 4 nm.

[0049] In one exemplary embodiment, the silicon-containing particles according to the first aspect of the present invention may further include a surface deactivation film formed by reacting the raw silicon-containing particles with gaseous carbon monoxide (CO). That is, the silicon-containing particles according to the first aspect of the present invention may further include a coating covering at least a portion of the surface of the silicon particles, the coating being a reaction product from the reaction between the silicon surface and gaseous carbon monoxide (CO).

[0050] As used herein, the term “reaction product from the reaction of a silicon surface with gaseous carbon monoxide (CO)” means that the surface film is the result of simply bringing raw silicon particles (particles with a non-oxidized or nearly non-oxidized surface) into contact with gaseous carbon monoxide at partial pressure and temperature at which CO reacts with the silicon surface of the particles to form a protective film. The film is, in fact, a mixture of Si, O, and C atoms.

[0051] XPS analysis of silicon particles indicates that the film formed upon contact with CO is a mixture of reaction products resulting from the gas reacting as both a functional group and a dissociated atom entering the molecular lattice of the silicon phase. XPS analysis shows that the carbon atom bonded to the oxygen atom is silicon carbonyl Si n We demonstrated the formation of CO compounds, showing that when the CO molecule dissociates, the carbon atom bonded to the silicon atom and the oxygen atom bonded to the silicon atom bond to separate Si atoms within the molecular lattice of the silicon phase. Furthermore, XPS data shows that a four-membered ring structure of Si-O-Si-C can be formed on the particle surface.

[0052] XPS results indicate that the molecular structure and composition of the CO-derived coating are a complex mixture of reaction products from both dissociated and non-dissociated gas molecules, making it difficult to define the coating as a compound. However, XPS analysis provides atomic percentages of various elements present in the molecular lattice in the surface region where reflected radiation escapes to the detector. X-rays penetrate the molecular lattice of the silicon particle in each measurement, extracting information from substantially equal depths, and XRD analysis determines the atomic composition of the outermost bulk phase and the surface layer of the particle, which are substantially equal in thickness. The absorption cross-sections of radiation from different atoms may differ, resulting in different signals based on the depth at which different atoms are found. Therefore, some interpretation is necessary and must be performed by a skilled operator with experience with similar materials. This means that if the X-ray and re-emitted signals do not penetrate the entire particle, and the XPS analysis does not include the coating on the shadowed (back) side of the particle, the atomic composition determined by XPS is an indirect measurement of the thickness of the CO-derived coating, regardless of particle size. In practice, this means that XPS analysis is reliable if the diameter of the silicon particle is 10 nm or larger.

[0053] Transmission electron microscopy (TEM) and especially electron energy loss spectroscopy (EELS) measurements can also be used to estimate the thickness and, in particular, the homogeneity of the coating layer. Because TEM images are cross-sectional images of the entire particle, the coating may appear slightly thicker than it actually is due to surface roughness and curvature. Furthermore, EELS may be less suitable than XPS for precise compositional analysis. Therefore, TEM is primarily used for verifying homogeneity, while XPS is used for qualitative and quantitative analysis of the surface coating.

[0054] In exemplary embodiments, the thickness of the coating on silicon-containing particles according to the first aspect of the present invention may be in the range of 0.1 to 3 nm, preferably 0.2 to 2 nm, more preferably 0.3 to 1.5 nm, more preferably 0.4 to 1.0 nm, more preferably 0.5 to 0.8 nm, and most preferably 0.6 to 0.7 nm. This thickness can be determined by high-resolution bright-field transmission electron microscopy (TEM) for visualization of the layer thickness. Scanning transmission electron microscopy using electron energy loss spectroscopy and energy-dispersive X-ray spectroscopy may be used to confirm that both the particles and the observed outer layer have the expected chemical composition.

[0055] As used herein, the term "XPS analysis" refers to X-ray photon spectroscopy (XPS) measurements performed using a spectrometer with monochromatic AlKα radiation at 1486.6 eV, and the data analysis is performed using CasaXPS software with Shirley background subtraction and energy axis calibration using pure Si 2p 3 / 2 = 99.4 eV. It is possible to use spectrometers with other radiation sources at other wavelengths and convert these measurements to be comparable to those obtained using monochromatic AlKα radiation at 1486.6 eV. Such conversions are well known to those skilled in the art.

[0056] The relatively high temperature resistance of silicon-containing particles according to the first aspect of the present invention provides an advantage when the particles are applied to the active material of the negative electrode of a secondary lithium-ion battery (LIB). Therefore, the silicon-containing particles are typically mixed with graphite and a binder, and then thermally decomposed to embed the silicon-containing particles in the carbon matrix constituting the active material.

[0057] In a second embodiment, the present invention relates to a method for producing polycrystalline silicon-containing particles according to a first aspect of the present invention, wherein the method is A step of forming a homogeneous gas mixture of a first precursor gas of a silicon-containing compound and at least one second precursor gas of a substituted element M-containing compound, wherein M is C or N, or a combination thereof. A step of injecting a homogeneous gas mixture of first and second precursor gases into the reactor space, wherein the precursor gases are heated to a temperature in the range of 700 to 900°C, causing the precursor gases to react and form mainly amorphous silicon-containing particles. A process of converting amorphous silicon-containing particles into polycrystalline silicon-containing particles by heat-treating them in an inert atmosphere at a temperature in the range of 800 to 900°C for 0.1 to 4 hours, The process includes a step of cooling and recovering polycrystalline silicon-containing particles. The relative amounts of the first and second precursor gases are adjusted so that the formed particles obtain an atomic ratio M:Si in the range of [0.005, 0.25].

[0058] As used herein, the term “first precursor gas of a silicon-containing compound” means any silicon-containing compound that exists in a gaseous state and reacts at the intended reaction temperature to form Si particles. Examples of preferred first precursor gases include, but are not limited to, silanes (SiH4), disilanes (Si2H6), trichlorosilanes (HCl3Si), or mixtures thereof. Similarly, as used herein, the term “second precursor gas of a substituted element M-containing compound” means any compound containing a substituted element M that exists in a gaseous state, participates in a gas-phase reaction, and, when heated to the intended reaction temperature, incorporates the M atom into the molecular structure of the Si particles formed. Examples of preferred second precursor gases include, but are not limited to, alkanes, alkenes, alkynes, aromatic compounds, or N hydrides, hydrogen cyanide, and mixtures thereof.

[0059] A particularly preferred exemplary embodiment of the precursor gas, i.e., a homogeneous gas mixture of a gaseous silicon-hydrogen compound and a gaseous substitution element M-hydrogen compound, is either silane (SiH4) or disilane (Si2H6) mixed with a hydrocarbon gas selected from one of methane (CH4), ethane (C2H6), propane (C3H8), ethene (C2H4), ethyne (C2H2), and mixtures thereof.

[0060] In an exemplary embodiment of the method according to a second aspect of the present invention, a homogeneous gas mixture of the first and second precursor gases is injected into the reactor space and heated to a temperature in the range of 740 to 850°C, preferably 780 to 830°C, and most preferably 790 to 820°C. Optionally, the homogeneous gas mixture of the first and second precursor gases may be preheated to a temperature in the range of 300 to 500°C before being inserted into the reactor space.

[0061] In an exemplary embodiment of the method according to a second aspect of the present invention, the relative amounts of the first and second precursor gases are adapted to obtain an atomic ratio M:Si of the formed particles in the range of [0.0070, 0.177], preferably in the range of [0.0081, 0.11], preferably in the range of [0.0091, 0.081], and most preferably in the range of [0.01, 0.053].

[0062] In an exemplary embodiment of the method according to a second aspect of the present invention, the homogeneous gas mixture further comprises a noble gas such as hydrogen, nitrogen, helium, neon, argon, or any other gas that does not chemically react with the precursor gas at a particular temperature.

[0063] In an exemplary embodiment of the method according to a second aspect of the present invention, the relative amounts of the first and second precursor gases are adapted to obtain the intended atomic ratio M:Si in the resulting particles by adjusting the flow rates of the first and second precursor gases injected into the reactor, measuring the composition of the exhaust gas from the reactor using a mass spectrometer to determine the rate at which the injected first and second precursor gases are converted into particles, estimating the atomic ratio M:Si in the formed particles using this information, and adjusting the supply rates of the first and second precursor gases.

[0064] The notation for intervals used herein follows the international standard ISO 80000-2, where square brackets "[ ]" and " ]" indicate the boundary of a closed interval, and parentheses "( ]" and " )" indicate the boundary of an open interval. For example, [a, b] is a closed interval containing all real numbers from a (inclusive) to b (inclusive):

number

number

[0065] In exemplary embodiments, the homogeneous gas mixture may include additional inert gases such as hydrogen, nitrogen, argon, neon, helium, or other gases, which can be used to influence heating, cooling, particle formation rate, and mass transport, without leaving chemical impurities in the final particle product. Heating of the precursor gas in the reactor chamber can be achieved by convection, conduction, radiation, laser, mixing with a warmer gas, or any other known method.

[0066] The reaction rate in a gas reaction that forms particles from a precursor gas varies greatly depending on which gases are used as the first and / or second precursor gases and the reaction temperature at which the particles are formed, and the atomic ratio M:Si in the precursor gas may deviate significantly from the atomic ratio M:Si in the produced particles. Therefore, the term used herein, "the relative amounts of the first and second precursor gases are adapted so that the formed particles obtain an atomic ratio M:Si within the range of...", means that the relative amounts of the mixed and homogenized first and second precursor gases are adjusted so that the resulting particles obtain the intended atomic ratio when the mixture of precursor gases is heated to the intended reaction temperature and reacts to form particles.

[0067] Adapting the relative amounts of the first and second precursor gases to form the intended particles is within the ordinary art of those skilled in the art. For example, the adaptation of the relative amounts of the precursor gases for a given first and second precursor gases and intended reaction temperature can be obtained prior to the manufacturing stage by simply performing trial-and-error tests to determine the relative amounts of the precursor gases to be applied to this gas mixture and reaction temperature.

[0068] Alternatively, the atomic ratio M:Si in the formed particles can be monitored / determined by analyzing the exhaust gas from the reactor using a mass spectrometer to determine how much of the supplied first and second precursor gases were reacted / consumed in the reactor, and then indirectly determining the relative amounts of M and Si in the formed particles. For example, the flow rates of the first and second precursor gases injected into the reactor can be adjusted, and the composition of the exhaust gas from the reactor can be measured using a mass spectrometer to determine the rate at which the injected first and second precursor gases are converted into particles. This information can then be used to estimate the atomic ratio M:Si in the formed particles, and the supply rates of the first and second precursor gases can be adjusted to obtain the intended atomic ratio M:Si in the resulting particles.

[0069] A method according to a second aspect of the present invention, in one exemplary embodiment, includes an additional process step, namely, i) A step of placing silicon-containing particles inside the reactor chamber, ii) A step of introducing a precursor gas containing carbon monoxide (CO) into the reactor chamber, iii) A step of maintaining the silicon-containing particles in the reactor chamber for the time until a coating is formed on the silicon particles, This may further include forming a surface passivation layer on the surface of silicon-containing particles.

[0070] In a third embodiment, the present invention relates to a negative electrode for a lithium-ion secondary electrochemical cell, wherein the negative electrode is At least one particulate active material, Binder material and, Including a current collector board, At least one particulate active material is embedded in the binder material to form an anode mass that is deposited on the current collector substrate as an anode mass layer. At least one particulate active material is a silicon-containing particle according to a first aspect of the present invention.

[0071] In a secondary electrochemical cell, the chemical half-cell reactions at the electrodes switch from oxidation to reduction reactions depending on the charging and discharging states of the charge-discharge cycle. As used herein, the term "negative electrode" refers to the electrode in the electrochemical cell where the oxidation side of the chemical reaction occurs during discharge. That is, the negative electrode is the electron-generating electrode when power is extracted from the electrochemical cell. The negative electrode may also be referred to as the anode in the literature. The terms anode and negative electrode are interchangeable as used herein.

[0072] The negative electrode according to a third aspect of the present invention can use any conductive substrate known or conceivable to those skilled in the art that is suitable for use as a current collector in the negative electrode of a lithium-ion secondary electrochemical cell. Examples of suitable conductive substrates include, but are not limited to, graphite, aluminum, or copper foil / sheets.

[0073] The negative electrode according to a third aspect of the present invention may use any binder material known or conceivable to those skilled in the art that is suitable for use as a binder in the negative electrode of a lithium-ion secondary electrochemical cell. Examples of suitable binders include, but are not limited to, styrene-butadiene copolymer (SBR), carboxymethylcellulose (CMC), ethylene-propylene-dienemethylene (EPDM), and polyacrylic acid (PAA).

[0074] In exemplary embodiments, the anode mass may further comprise a particulate conductive filler material mixed with particulate active material and embedded together in a binder material. The anode according to a third aspect of the present invention may use any conductive filler material known or conceivable to those skilled in the art that is suitable for use as a conductive filler for an anode mass for the anode of a lithium-ion secondary electrochemical cell. Suitable examples of particulate conductive fillers include, but are not limited to, carbon isotopes such as graphene, reduced graphene oxide, elastic polymers, carbon-rich materials, carbon black, carbon nanotubes, or materials mainly containing carbon produced by the thermal decomposition of mixtures thereof.

[0075] In a fourth aspect of the present invention, the crystallization of primarily amorphous silicon particles forming polycrystalline silicon-containing particles according to the first aspect of the present invention can be obtained during the thermal decomposition of a carbonaceous material containing a plurality of the primarily amorphous silicon particles of the present invention, thereby forming secondary particles. Each secondary particle may contain 10 to possibly 1 million polycrystalline silicon-containing particles of the present invention and a large amount of carbon formed by the heat treatment of a precursor material containing carbon atoms. This precursor material may be, for example, a large carbon-aggregating molecule such as petroleum or pitch. Alternatively, the precursor material may be a strongly crosslinked material such as resorcinol formaldehyde or melamine formaldehyde, where thermal decomposition can be used to form a nanoporous structure or aerogel primarily containing carbon. The thermal decomposition process can be carried out at >600°C, preferably >700°C, more preferably >800°C. In one exemplary embodiment, the secondary particles may be similar in size to graphite particles used in batteries today, i.e., have an average cross-sectional distance of, for example, 2 to 5 microns.

[0076] In a fifth aspect of the present invention, the crystallization of primarily amorphous silicon particles forming polycrystalline silicon-containing particles according to the first aspect of the present invention can be obtained during the formation of secondary particles having graphene or graphene oxide as a conductive additive and as a protective barrier to the electrolyte. The secondary particles can then be used again as battery electrodes and may contain, for example, 10 to possibly 1 million polycrystalline silicon-containing particles of the present invention and a large amount of graphene or reduced graphene oxide formed by heat treatment of a precursor material containing oxidized graphene or graphene oxide. The reduction process can be carried out at >600°C, preferably >700°C, more preferably >800°C. In one exemplary embodiment, the secondary particles may have a size similar to graphite particles used in batteries today, i.e., an average cross-sectional distance of, for example, 2 to 5 microns. The secondary particles may further contain binders or other components to ensure the geometric stability of the secondary particles in a later manufacturing process.

[0077] In a sixth aspect of the present invention, polycrystalline silicon-containing particles according to the first and second aspects of the present invention may be used to form secondary particles using an elastic binder as a barrier to the electrolyte. The secondary particles may also contain conductive additives. The secondary particles can then be used again as battery electrodes and may contain, for example, 10 to 1 million of the primarily amorphous silicon particles of the present invention. The elastic binder can be any elastic polymer or plastic, including known elastomers such as imides, amides, silicones, styrene-butadiene rubber, and nitrile rubber. In one exemplary embodiment, the secondary particles may have a size similar to graphite particles used in batteries today, i.e., an average cross-sectional distance of, for example, 2 to 5 microns.

[0078] In a seventh aspect of the present invention, the crystallization of primarily amorphous silicon particles forming polycrystalline silicon-containing particles according to the first aspect of the present invention can be obtained during the formation of secondary particles having a primarily carbon-containing substance obtained by thermal decomposition of a carbon-rich substance as a conductive additive and protective barrier to the electrolyte. These secondary particles can then be used again as battery electrodes and may contain 10 to possibly 1 million polycrystalline silicon-containing particles of the present invention and a large amount of the primarily carbon-containing substance produced by thermal decomposition of a carbon-rich substance. The thermal decomposition process can be carried out at >700°C, preferably >800°C. In one exemplary embodiment, the secondary particles may have a size similar to graphite particles used in batteries today, i.e., an average cross-sectional distance of, for example, 2 to 5 microns. The secondary particles may further contain binders or other components to ensure the geometric stability of the secondary particles in a later manufacturing process. [Brief explanation of the drawing]

[0079] [Figure 1] This figure shows the XRD analysis of silicon particles prepared at three different temperatures. [Figure 2] This figure shows the XRD analysis of various samples (samples R11_FA, R11_FB, R11_FC) of SiO.99C0.01 and SiO.98C0.02, which are manufactured at over 800°C using a process very similar to that shown in Figure 1 and remain completely amorphous. [Figure 3] The figures show the XRD analyses of SiO.92C0.08 after heat treatment at 700°C (R18-F2 700) and 800°C (R18-F2 800) for 2 hours, respectively. These curves indicate that SiO.92C0.08 remains amorphous after 2 hours at 700°C and begins crystallization when exposed to 800°C for 2 hours. [Figure 4] This figure shows the microcrystalline size of silicon-containing particles after heat treatment at 800 or 900°C for 2 hours, as a function of the carbon content. [Modes for carrying out the invention]

[0080] The present invention will be described in more detail by exemplary embodiments.

[0081] Comparative Example A homogeneous gas mixture of 33% silane diluted in hydrogen gas was preheated to approximately 400°C. This gas was then introduced into a decomposition reactor, and the silane gas was mixed with preheated hydrogen gas at temperatures of 710°C, 745°C, and 770°C, respectively, to produce three samples of (pure) silicon particles. The residence time in the reactor was approximately 1.5 seconds. The resulting silicon particles were rapidly cooled to below 300°C and recovered by filtration.

[0082] Next, the sample particles were analyzed by XRD to investigate their atomic structure. The particles produced at 710°C (labeled RTF1 in Figure 1) had an XRD curve typical of amorphous silicon, the particles produced at 745°C (labeled RTF2 in Figure 1) had an XRD curve indicating some formation of crystalline silicon, and the particles produced at 770°C (labeled RTF3 in Figure 1) had an XRD curve typical of crystalline silicon.

[0083] Preparation of amorphous precursor particles Polycrystalline silicon particles according to exemplary embodiments of the present invention can be manufactured as follows.

[0084] A homogeneous mixture of silane gas and ethene was preheated to approximately 400°C and introduced into the reactor chamber. This homogeneous mixture was then mixed with an inert gas (nitrogen) preheated to a temperature of 810°C, resulting in the final gas mixture. The relative amounts of each gas in the final mixture were approximately 28 mol% silane, 1.5 mol% ethene, and the remainder (70 mol%) nitrogen. The C:Si atomic ratio in the gas mixture was 0.05. However, the C:Si atomic ratio of the resulting particles was 0.02, meaning the particles were primarily amorphous Si. 0.98 C 0.02 It was composed of [something].

[0085] The residence time in the reactor was approximately 1.0 second. Afterward, the exhaust gas and particles exiting the reactor space were rapidly cooled and collected in a filter. The particles were analyzed by XRD to determine their atomic structure. The results are shown in Figure 2 as a curve labeled R11_FA. This XRD curve is typical of silicon with an amorphous molecular structure.

[0086] Furthermore, three more embodiments of primarily amorphous particles were produced in the same manner, except that the gas mixture contained silane, ethene, ammonia, and nitrogen. These samples were characterized using differential scanning calorimetry, and the crystallization temperature was determined from the energy released during crystallization. Nitrogen content is not as easy to measure as carbon content due to its low content, but the particle composition Si was determined based on linear extrapolation from samples with higher nitrogen content, and by analyzing gas consumption in the reaction. x , C y , N z SiO 0.984 C 0.016 N0, Si 0.992 C 008 N0 and Si 0.976 C 0.012 N 0.012 It was presumed that this was the case.

[0087] All of these samples showed higher crystallization temperatures compared to the pure silicon comparative particles mentioned above, and the estimated composition was Si 0.976 C 0.012 N 0.012 One sample exhibited a maximum crystallization temperature of 794°C. The other two samples showed crystallization temperatures at least 10°C lower, i.e., slightly lower than 784°C.

[0088] Figure 3 shows Si after heat treatment at 700°C (indicated as R18-F2 700 in the figure) and 800°C (indicated as R 18-F2 800 in the figure) for 2 hours, respectively. 0.92 C 0.08 The XRD analysis of the sample is shown. These curves represent Si 0.92 C 0.08This shows that the material remains amorphous even after 2 hours at 700°C, but begins to crystallize when exposed to 800°C for 2 hours.

[0089] Demonstration of the invention A sample set of mainly amorphous particles was prepared in the same manner as shown in the above example. The particles were 34m 2 The particles had a BET of 1 / g (corresponding to a particle size of approximately 80 nm) and a carbon content ranging from C0 to C3.1 wt%, as shown in Table 1. These particles were heat-treated for 2 hours in an inert atmosphere at 700°C, 800°C, or 900°C.

[0090] The crystallinity of the obtained particles was determined by Rietveld refinement using peak fitting, assuming two phases with different particle size ratios. The microcrystal size of the heat-treated particles was taken as the linear average of two different particle size ratios in each phase. The obtained microcrystal size is shown in Figure 4 as a function of carbon content. The carbon content is given in weight percent in the figure. 1.4 wt% of C corresponds to 3.2 atomic percent of C, and when expressed by the chemical formula, it is Si 0.968 C 0.032 This is the result.

[0091] As can be seen from Table 1 and Figure 4, the pure silicon particles, which are mainly amorphous (carbon-free), were converted into a microcrystalline phase having relatively coarse fine particles of 18-22 nm, close to the particle size. However, including a relatively small amount of carbon in the silicon molecular structure has the effect of forming significantly smaller microcrystals during heat treatment. We found that particles with carbon content of 2.5 and 3.1 wt% (5.6 and 7.0 atomic%) developed a microcrystalline structure with a microcrystal size of 10-11 nm after heat treatment at 900°C for 2 hours, and a microcrystalline structure with a microcrystal size of only 2-3 nm after heat treatment at 800°C for 2 hours.

[0092] [Table 1]

[0093] Similar tests were also conducted on mainly amorphous silicon-containing particles that had only N, or N and C atoms, in the amounts shown in Table 2. The particles were heat-treated in an inert atmosphere at 800°C or 900°C for 2 hours, and the crystallinity of the resulting particles was determined by Rietveld refinement. As can be seen from Table 2, the mainly amorphous silicon-containing particles with 1.4 wt% N (no C) were also converted into a microcrystalline phase with microcrystals slightly smaller than those obtained in pure silicon particles. When some C was also included, the resulting microcrystal size was as shown in Table 1. 1-x C x It was comparable to a particle.

[0094] [Table 2]

Claims

1. Silicon-containing particles, The aforementioned particles are determined by Brunauer-Emmet-Teller (BET) analysis according to ISO 9277:2010, ranging from 25 to 182 m². 2 Having a surface area of ​​ / g, The silicon-containing particles are of the formula Si (1-x) M x The compound comprises, where 0.0005 ≤ x ≤ 0.20, and M is at least one substitution element selected from C, N, or a combination thereof. The silicon-containing particle compound is a silicon-containing particle having a microcrystalline size in the range of 1 to 15 nm, determined by the Rietveld method.

2. The silicon-containing particles according to claim 1, wherein the silicon-containing particles consist of a compound of the formula Si(1-x)Mx, where M is at least one substitution element selected from C, N, or a combination thereof, and 0.001 ≤ x ≤ 0.

15.

3. The aforementioned particles are determined by Brunauer-Emmet-Teller (BET) analysis in accordance with ISO 9277:2010, and range from 34 to 136 m. 2 Silicon-containing particles according to claim 1 or 2, having a BET surface area in the range of / g.

4. The silicon-containing particle according to any one of claims 1 to 3, wherein the compound of the silicon-containing particle has a microcrystalline size in the range of 2 to 12 nm, determined by Rietveld refinement, the instrument Bragg peak profile is calculated from basic parameters and refined considering Lorentz and Gaussian sample spreading due to small microcrystalline sizes, and the microcrystalline size is calculated using Scherrer's formula from the sample's contribution to the full width at half maximum (FWHM) using a shape factor of 0.

89.

5. The silicon-containing particles according to any one of claims 1 to 4, wherein the silicon-containing particles further comprise a carbon film having a thickness in the range of 0.2 to 10 nm.

6. The silicon-containing particle according to any one of claims 1 to 4, wherein the particle has a coating covering at least a portion of the surface of the particle, and the coating is a reaction product from the reaction between the surface of the silicon-containing particle and gaseous carbon monoxide (CO).

7. The silicon-containing particles according to claim 6, wherein the thickness of the coating, as determined by high-resolution bright-field transmission electron microscopy (TEM), is in the range of 0.1 to 3 nm, preferably 0.2 to 2 nm, more preferably 0.3 to 1.5 nm, more preferably 0.4 to 1.0 nm, more preferably 0.5 to 0.8 nm, and most preferably 0.6 to 0.7 nm.

8. A method for producing polycrystalline silicon-containing particles according to any one of claims 1 to 7, A step of forming a homogeneous gas mixture of a first precursor gas of a silicon-containing compound and at least one second precursor gas of a substituted element M-containing compound, wherein M is C or N, or a combination thereof. A step of injecting the homogeneous gas mixture of the first and second precursor gases into the reactor space, wherein the precursor gas is heated to a temperature in the range of 700 to 900°C so that the precursor gas reacts to form mainly amorphous silicon-containing particles, A step of converting the aforementioned mainly amorphous silicon-containing particles into polycrystalline silicon-containing particles by heat-treating them in an inert atmosphere at a temperature in the range of 800 to 900°C for 0.1 to 4 hours, The process includes a step of cooling and recovering the polycrystalline silicon-containing particles, The relative amounts of the first and second precursor gases are adapted so that the formed particles obtain an atomic ratio M:Si in the range of [0.005, 0.25], in a method.

9. The first precursor gas is silane (SiH 4 ), disilane (Si 2 H 6 ), trichlorosilane (HCl 3 Si), or a mixture thereof, and the second precursor gas is methane (CH 4 ), ethane (C 2 H 6 ), propane (C 3 H 8 ), ethene (C 2 H 4 ), ethyne (C 2 H 2 ), an alkane, an alkene, an alkyne, a hydride of N, hydrogen cyanide, or a mixture thereof, the method according to claim 8.

10. The method according to claim 8 or 9, wherein the relative amounts of the first and second precursor gases are adapted so that the formed particles obtain an atomic ratio M:Si in the range of [0.0070, 0.177].

11. The method according to any one of claims 8 to 10, wherein the homogeneous gas mixture of the first and second precursor gases is preheated to a temperature in the range of 300 to 500°C before being inserted into the reactor space, and then further heated to a temperature in the range of 740 to 850°C after being injected into the reactor space.

12. The method according to any one of claims 8 to 11, wherein the homogeneous gas mixture further comprises a noble gas such as hydrogen, nitrogen, helium, neon, or argon, or any other gas that does not chemically react with the precursor gas at the specified temperature.

13. The method according to any one of claims 8 to 12, wherein the relative amounts of the first and second precursor gases are adapted to obtain the intended atomic ratio M:Si in the particles being manufactured by adjusting the flow rate of the first and second precursor gases injected into the reactor, measuring the composition of the exhaust gas from the reactor using a mass spectrometer to determine the proportion of the injected first and second precursor gases that are converted into particles, estimating the atomic ratio M:Si in the formed particles using this information, and adjusting the supply rate of the first and second precursor gases.

14. The aforementioned method, i) Place the silicon-containing particles inside the reactor chamber, ii) A precursor gas containing carbon monoxide (CO) is introduced into the reactor chamber. iii) By maintaining the silicon-containing particles in the reactor chamber for the time until a coating is formed on the silicon-containing particles, The method according to any one of claims 8 to 13, further comprising coating the silicon-containing particles.

15. The negative electrode of a lithium-ion secondary electrochemical cell, wherein the negative electrode is At least one type of particulate active material, Binder material and Including a current collector board, The at least one particulate active material is embedded in the binder material to form anode masses that are deposited on the current collector substrate as an anode mass layer. The negative electrode wherein the at least one particulate active material is a silicon-containing particle according to any one of claims 1 to 7.

16. The negative electrode according to claim 15, wherein the current collector substrate is a foil or sheet of graphite, Cu, or Al, and the binder is a styrene-butadiene copolymer (SBR), carboxymethylcellulose (CMC), ethylene-propylene-dienemethylene (EPDM), or polyacrylic acid (PAA).

17. The negative electrode according to claim 15 or 16, wherein the anode mass further comprises a particulate conductive additive material that is mixed with the particulate active material and embedded together in the binder material.

18. The negative electrode according to claim 17, wherein the particulate conductive additive material is carbon black, carbon nanotubes, graphene, or a mixture thereof.

19. A composite particle used in the negative electrode of a lithium-ion secondary electrochemical cell, wherein the composite particle comprises a plurality of silicon-containing particles according to any one of claims 1 to 7, and graphene or reduced graphene oxide.

20. A composite particle used in the negative electrode of a lithium-ion secondary electrochemical cell, wherein the composite particle comprises a plurality of silicon-containing particles according to any one of claims 1 to 7, and a nanoporous structure mainly containing carbon or an aerogel mainly containing carbon.

21. A composite particle used in the negative electrode of a lithium-ion secondary electrochemical cell, wherein the composite particle comprises a plurality of silicon-containing particles according to any one of claims 1 to 7, and a substance mainly containing carbon produced by the thermal decomposition of a carbon-rich substance.

22. The silicon-containing particles according to any one of claims 1 to 7, wherein the total content of C and / or N is 0.05 to 20 atomic percent, and the remainder is Si and unavoidable impurities.

Citation Information

Patent Citations

  • Negative electrode of lithium ionic cell, preparing method and cell thereof

    CN101453013A

  • Negative active material for rechargeable lithium battery and rechargeable lithium battery

    EP2405509A2

  • High purity, amorphous silicon powder, method for preparation of same and use of same

    EP3025702A1

  • Predominantly amorphous silicon particles and use thereof as active anode material in secondary lithium ion batteries

    GB2592097A

  • Negative electrode active material for lithium secondary battery, its manufacturing method, and lithium secondary battery containing it

    JP2004349253A