Method for producing hydrolyzable silyl group-containing polyoxyalkylene

By controlling the water content in monoepoxide polymerization and introducing hydrolyzable silyl groups, the method produces polyoxyalkylene with enhanced modulus and curability, addressing modulus inconsistencies in sealants and adhesives.

JP7954664B2Active Publication Date: 2026-11-20KANEKA CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023563616
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-11-24
Filing Date
2022-11-10
Publication Date
2026-11-20
Estimated Expiration
2042-11-10

AI Technical Summary

Technical Problem

Existing hydrolyzable silyl group-containing polyoxyalkylenes do not adequately adjust modulus for applications requiring high or low flexibility and adhesion, limiting their use in sealants and adhesives due to inconsistent mechanical properties.

Method used

Producing hydrolyzable silyl group-containing polyoxyalkylene by ring-opening polymerization of monoepoxide with a water content of 5 ppm or more and less than 50 ppm, followed by introducing hydrolyzable silyl groups, using specific catalysts and methods to enhance modulus.

Benefits of technology

The method results in polyoxyalkylene with improved modulus and curability, suitable for applications needing high or low flexibility and adhesion, enhancing performance in sealants and adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954664000001
    Figure 0007954664000001
  • Figure 0007954664000002
    Figure 0007954664000002
  • Figure 0007954664000003
    Figure 0007954664000003
Patent Text Reader

Abstract

Provided is a method for producing a hydrolyzable silyl group-containing polyoxyalkylene that can exhibit a higher modulus after curing. A hydroxyl group-containing polyoxyalkylene (A) is obtained by performing ring-opening polymerization of a monoepoxide having a moisture content of at least 5 ppm but less than 50 ppm, and a hydrolyzable silyl group is introduced into (A). The step for introducing the hydrolyzable silyl group may be a step for converting the hydroxyl group of (A) into a carbon-carbon unsaturated bond-containing group and converting the carbon-carbon unsaturated bond-containing group into a hydrolyzable silyl group, or may be a step for causing a urethanization reaction of a hydrolyzable silyl group-containing isocyanate compound with respect to the hydroxyl group of the hydroxyl group-containing polyoxyalkylene (A).
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a method for producing a polyoxyalkylene having a silyl group that has a hydroxyl group or a hydrolyzable group bonded to a silicon atom and is capable of forming a crosslink by forming a siloxane bond (hereinafter also referred to as "hydrolyzable silyl group"). BACKGROUND ART

[0002] As organic polymers having a hydrolyzable silyl group, organic polymers whose main chain skeleton is a polyoxyalkylene polymer have already been industrially produced and are widely used in applications such as sealants, adhesives, and coatings (see, for example, Patent Documents 1 and 2). PRIOR ART DOCUMENTS PATENT DOCUMENTS

[0003] PATENT DOCUMENT 1 Japanese Unexamined Patent Publication No. Sho 52-73998 PATENT DOCUMENT 2 Japanese Unexamined Patent Publication No. Hei 10-245482 SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION

[0004] Hydrolyzable silyl group-containing polyoxyalkylenes and their compositions can form cured products through crosslinking and are therefore used in applications such as sealants, adhesives, and paints. Depending on the application, the cured products require various physical properties such as flexibility, adhesion, and durability. Modulus is an important physical property, but the required modulus range differs depending on the application. For example, for sealant applications, low-modulus types are preferable for applications such as curtain wall joints, where there is relatively large movement, because they have superior resistance to movement and the force applied to the bonded surface is small. On the other hand, high-modulus types are preferable for reinforced concrete exterior walls, where there is little movement in the joints. Furthermore, for adhesive applications, it is desirable that the bonded surface does not move due to external forces, so high-modulus polymers are often required. Against this backdrop, technologies for adjusting modulus and technologies for achieving higher modulus are important.

[0005] In view of the above situation, the present invention aims to provide a method for producing a hydrolyzable silyl group-containing polyoxyalkylene that can exhibit a higher modulus after curing. [Means for solving the problem]

[0006] Hydrolyzable silyl group-containing polyoxyalkylenes are generally produced by ring-opening addition polymerization of a monoepoxide in the presence of a hydroxyl group-containing initiator to obtain a hydroxyl group-containing polyoxyalkylene, and then introducing a hydrolyzable silyl group into the hydroxyl group-containing polyoxyalkylene. The inventors' investigations revealed, surprisingly, that a polyoxyalkylene containing hydrolyzable silyl groups, obtained by polymerizing a monoepoxide with a low water content and then introducing hydrolyzable silyl groups, exhibited improved modulus after curing, leading to the present invention.

[0007] In other words, the present invention relates to a method for producing a hydrolyzable silyl group-containing polyoxyalkylene (B), comprising the steps of obtaining a hydroxyl group-containing polyoxyalkylene (A) by ring-opening polymerization of a monoepoxide with a water content of 5 ppm or more and less than 50 ppm, and introducing a hydrolyzable silyl group into the hydroxyl group-containing polyoxyalkylene (A). Preferably, the step of obtaining the hydroxyl group-containing polyoxyalkylene (A) is carried out in the presence of a complex metal cyanide catalyst. The step of introducing the hydrolyzable silyl group may be a step of converting the hydroxyl group of the hydroxyl group-containing polyoxyalkylene (A) into a carbon-carbon unsaturated bond-containing group, and then converting the carbon-carbon unsaturated bond-containing group into a hydrolyzable silyl group. Furthermore, the step of introducing the hydrolyzable silyl group may be a step of urethane-forming the hydroxyl group of the hydroxyl group-containing polyoxyalkylene (A) with a hydrolyzable silyl group-containing isocyanate compound. The hydroxyl group-containing polyoxyalkylene (A) and the hydrolyzable silyl group-containing polyoxyalkylene (B) may have a branched polymer skeleton. Furthermore, the hydroxyl group-containing polyoxyalkylene (A) and the hydrolyzable silyl group-containing polyoxyalkylene (B) may have a linear polymer skeleton. [Effects of the Invention]

[0008] According to the present invention, it is possible to provide a method for producing a hydrolyzable silyl group-containing polyoxyalkylene that can exhibit a higher modulus after curing. [Modes for carrying out the invention]

[0009] Embodiments of the present invention will be described in detail below. The method for producing the hydrolyzable silyl group-containing polyoxyalkylene (B) according to this embodiment includes the steps of obtaining a hydroxyl group-containing polyoxyalkylene (A) by ring-opening polymerization of a monoepoxide, and introducing a hydrolyzable silyl group into the hydroxyl group-containing polyoxyalkylene (A).

[0010] <<Step to obtain hydroxyl group-containing polyoxyalkylene (A)>> Hydroxyl group-containing polyoxyalkylene (A) can be obtained by conventionally known methods, by ring-opening addition polymerization of a monoepoxide in the presence of a hydroxyl group-containing initiator and a polymerization catalyst.

[0011] The monoepoxide is not particularly limited and examples include ethylene oxide, propylene oxide, butylene oxide (e.g., 1,2-butylene oxide, 2,3-butylene oxide, isobutylene oxide), and styrene oxide. Only one type may be used, or two or more types may be used in combination. From the viewpoint of availability and the physical properties of the resulting polymer, ethylene oxide and propylene oxide are preferred, and propylene oxide is particularly preferred.

[0012] Commercially available monoepoxides generally contain water as an impurity. Surprisingly, it was found that hydrolyzable silyl group-containing polyoxyalkylenes, produced by ring-opening polymerization of a monoepoxide with low water content followed by the introduction of hydrolyzable silyl groups, exhibit a higher modulus after curing compared to hydrolyzable silyl group-containing polyoxyalkylenes produced using the same raw materials and conditions except for the higher water content of the monoepoxide. Furthermore, it was found that physical properties such as curability may be more favorable in this case.

[0013] From the viewpoint of exhibiting a higher modulus after curing, a lower water content in the monoepoxide is preferable. Specifically, in this embodiment, the water content of the monoepoxide is 5 ppm or more and less than 50 ppm. 5 ppm or more and less than 40 ppm is preferred, 5 ppm or more and less than 30 ppm is more preferred, and 5 ppm or more and less than 20 ppm is particularly preferred.

[0014] Because monoepoxides are highly hygroscopic, they can absorb moisture remaining in transport containers and production lines between the time of production and the time they are used to produce hydroxyl group-containing polyoxyalkylene (A). Therefore, it is difficult to keep the moisture content of monoepoxides below 5 ppm.

[0015] The water content of commercially available monoepoxides is sometimes measured and disclosed as an inspection value. In that case, it is preferable to select and use a monoepoxide whose water content falls within the above range. It is also possible to use a monoepoxide whose water content has been reduced to 50 ppm by appropriately performing a known drying or dehydration operation on a monoepoxide having a water content of 50 ppm or more.

[0016] The initiator having a hydroxyl group is not particularly limited, and examples thereof include organic compounds having one or more hydroxyl groups, such as ethylene glycol, propylene glycol, glycerin, pentaerythritol, polyoxypropylene glycol, polyoxypropylene triol, allyl alcohol, polyoxypropylene monoallyl ether, and polyoxypropylene monoalkyl ether, among which those having two or more hydroxyl groups are preferred from the viewpoint of curability.

[0017] When the initiator has two hydroxyl groups, the hydroxyl group-containing polyoxyalkylene (A) and the hydrolyzable silyl group-containing polyoxyalkylene (B) produced using the initiator each have a linear polymer skeleton. On the other hand, when the initiator has three or more hydroxyl groups, the hydroxyl group-containing polyoxyalkylene (A) and the hydrolyzable silyl group-containing polyoxyalkylene (B) each have a branched polymer skeleton.

[0018] The amount of the initiator having a hydroxyl group to be used is not particularly limited, and can be set according to the target molecular weight of the hydroxyl group-containing polyoxyalkylene (A) to be produced. The entire amount of the initiator having a hydroxyl group may be added to the reaction system all at once, or may be added in multiple divided portions.

[0019] Examples of the aforementioned polymerization catalyst include double metal cyanide complexes, alkali metal catalysts, metal porphyrins such as complexes obtained by reacting a transition metal compound such as an organoaluminum compound with porphyrin, and phosphazenes. A double metal cyanide complex is preferred because a polymer with a small molecular weight distribution (Mw / Mn) and low viscosity can be obtained.

[0020] As the aforementioned double metal cyanide complex, conventionally known compounds can be used with no particular limitation. Among them, a double metal cyanide complex having an organic ligand coordinated to the catalyst skeleton is preferred. As the catalyst skeleton, a zinc hexacyanocobaltate complex is preferred. Examples of the organic ligand include tert-butyl alcohol and glyme, and glyme is preferred.

[0021] When carrying out ring-opening addition polymerization of a monoepoxide, it is preferable to perform the polymerization reaction in the presence of an organic solvent. The organic solvent is not particularly limited as long as it is an organic solvent that has no active hydrogen and is inert to the polymerization. Examples thereof include aromatic compounds such as benzene, monochlorobenzene, toluene, ethylbenzene, styrene, o-, m-, and p-xylene, heterocyclic compounds such as tetrahydrofuran, dioxane, furan, and pyran, and polar compounds such as chain ethers such as butyl ethyl ether. The aforementioned organic solvents may be used alone, or two or more thereof may be used in combination. Among them, heterocyclic compounds and chain ethers are preferred, tetrahydrofuran, dioxane, and butyl ethyl ether are more preferred, and tetrahydrofuran is particularly preferred.

[0022] The temperature condition for carrying out the ring-opening addition polymerization of the monoepoxide is not particularly limited, but may be, for example, 70 to 180°C, and is preferably 90 to 160°C.

[0023] In the aforementioned ring-opening addition polymerization, the entire amount of the monoepoxide to be used may be added to the reaction system all at once, or after a part of the monoepoxide is added to initiate the polymerization reaction, the remaining monoepoxide may be additionally added midway to continue the polymerization reaction. Furthermore, the ring-opening addition polymerization is preferably carried out under an inert gas atmosphere such as nitrogen or argon.

[0024] In the hydroxyl group-containing polyoxyalkylene (A) obtained by the polymerization reaction described above, the position where the hydroxyl group is attached to the polymer skeleton is not particularly limited, but it is preferably at the end of the polymer skeleton.

[0025] The hydroxyl group-containing polyoxyalkylene (A) may be a polymer having one polymer skeleton or a polymer having two or more polymer skeletons. Furthermore, the hydroxyl group-containing polyoxyalkylene (A) may consist of only one polymer or may be a mixture containing two or more polymers with different polymer skeletons and molecular weights. The mixture may be a mixture of polymers manufactured individually or a mixture manufactured in the same system to achieve any desired mixed composition.

[0026] The number-average molecular weight of the hydroxyl group-containing polyoxyalkylene (A) is not particularly limited, but is preferably 3,000 to 100,000, more preferably 3,000 to 50,000, and even more preferably 3,000 to 30,000 in terms of polystyrene-based molecular weight in GPC. A number-average molecular weight of 3,000 or more is desirable in terms of manufacturing cost because the relative amount of hydrolyzable silyl groups to the entire polymer is within an appropriate range. Furthermore, a number-average molecular weight of 100,000 or less makes it easier to achieve a desirable viscosity in terms of workability. The number-average molecular weight can be determined in terms of polystyrene-based molecular weight by GPC measurement.

[0027] The molecular weight distribution (Mw / Mn) of hydroxyl group-containing polyoxyalkylene (A) is not particularly limited, but a narrow range is preferred. Specifically, it is preferably less than 2.0, more preferably 1.6 or less, even more preferably 1.5 or less, and particularly preferably 1.4 or less. Furthermore, from the viewpoint of improving mechanical properties such as durability and elongation of the cured product, it is preferably 1.3 or less, and particularly preferably 1.2 or less. The molecular weight distribution (Mw / Mn) can be calculated from the number average molecular weight and weight average molecular weight obtained in polystyrene equivalent by GPC measurement.

[0028] <<Step to obtain hydrolyzable silyl group-containing polyoxyalkylene (B)>> A hydrolyzable silyl group-containing polyoxyalkylene (B) can be produced by introducing a hydrolyzable silyl group into the hydroxyl group-containing polyoxyalkylene (A) through one or more steps. The specific method is not particularly limited, but examples include the following. However, the method for obtaining the hydrolyzable silyl group-containing polyoxyalkylene (B) is not limited to the following embodiments. Embodiment (I): A hydrolyzable silyl group-containing isocyanate compound is used to urethaneize the hydroxyl groups of a hydroxyl group-containing polyoxyalkylene (A). Embodiment (II): The hydroxyl groups of a hydroxyl group-containing polyoxyalkylene (A) are converted to carbon-carbon unsaturated bond-containing groups, and then the carbon-carbon unsaturated bonds are converted to hydrolyzable silyl groups.

[0029] The hydrolyzable silyl group-containing polyoxyalkylene (B) may be a single polymer produced in either embodiment (I) or embodiment (II), or a mixture of two polymers produced in each embodiment.

[0030] [Aspect (I)] <Urethane formation reaction> In this embodiment, a hydrolyzable silyl group-containing polyoxyalkylene (B) is obtained by urethane-forming the hydroxyl groups of a hydroxyl group-containing polyoxyalkylene (A) with the isocyanate groups of a hydrolyzable silyl group-containing isocyanate compound. In the obtained hydrolyzable silyl group-containing polyoxyalkylene (B), the polymer backbone and the hydrolyzable silyl groups are bonded via urethane bonds.

[0031] The hydrolyzable silyl group-containing isocyanate compound is not particularly limited, as long as it is a compound having an isocyanate group and a hydrolyzable silyl group in the same molecule. Examples include (isocyanate methyl)trimethoxysilane, (isocyanate methyl)triethoxysilane, (isocyanate methyl)dimethoxymethylsilane, (isocyanate methyl)diethoxymethylsilane, (3-isocyanate propyl)trimethoxysilane, (3-isocyanate propyl)dimethoxymethylsilane, (3-isocyanate propyl)triethoxysilane, and (3-isocyanate propyl)diethoxymethylsilane. One hydrolyzable silyl group-containing isocyanate compound may be used alone, or two or more may be used in combination.

[0032] The amount of the hydrolyzable silyl group-containing isocyanate compound used can be appropriately determined considering the amount of hydroxyl groups present in the hydroxyl group-containing polyoxyalkylene (A) and the amount of hydrolyzable silyl groups to be introduced, and is not particularly limited. However, it is preferably 0.1 to 10 molar equivalents, more preferably 0.3 to 5 molar equivalents, and even more preferably 0.5 to 3 molar equivalents relative to the hydroxyl groups present in the hydroxyl group-containing polyoxyalkylene (A).

[0033] The urethane reaction may be carried out without a urethane catalyst, but it may also be carried out in the presence of a urethane catalyst to improve the reaction rate or reaction efficiency. Such urethane catalysts include, for example, those listed in *Polyurethanes: Chemistry and Technology, Part I, Table 30, Chapter 4, Saunders and Frisch, Interscience Publishers, New York, 1963*, and other conventionally known urethane catalysts. Specifically, examples include, but are not limited to, organotin compounds, bismuth compounds, and base catalysts such as organic amines.

[0034] As a urethane catalyst, organotin compounds are preferred due to their high activity. Specifically, examples include tin octylate, tin stearate, dibutyltin dioctoate, dibutyltin dioleyl malate, dibutyltin dibutyl malate, dibutyltin dilaurate, 1,1,3,3-tetrabutyl-1,3-dilauryloxycarbonyldistanoxane, dibutyltin diacetate, dibutyltin diacetylacetonate, dibutyltin bis(o-phenylphenoxide), dibutyltin oxide, dibutyltin bis(triethoxysilicate), dibutyltin distearate, dibutyltin bis(isononyl-3-mercaptopropionate), dibutyltin bis(isooctyl mercaptopropionate), dibutyltin bis(isooctyl thioglycolate), dioctyltin oxide, dioctyltin dilaurate, dioctyltin diacetate, and dioctyltin diversate. Furthermore, urethane catalysts with low activity towards hydrolyzable silyl groups are preferred, and from this viewpoint, organotin compounds containing sulfur atoms are preferred, among which dibutylsutunbis(isononyl-3-mercaptopropionate), dibutylsutunbis(isooctyl mercaptopropionate), and dibutylsutunbis(isooctyl thioglycolate) are particularly preferred.

[0035] As a urethane catalyst, an organic bismuth compound is preferred because it exhibits good activity and maintains good stability of the hydrolyzable silyl group-containing polyoxyalkylene (B). Examples of such organic bismuth compounds include bismuth carboxylates such as bismuth (2-ethylhexanoate), bismuth neodecanoate, and bismuth tetramethylheptanedione. Catalysts further containing other metals in addition to bismuth, particularly bismuth-zinc mixed catalysts, can also be suitably used. Examples of commercially available catalysts include, for example, catalysts from Borchers GmbH with trade names Borchi(R) Kat 22, Borchi(R) Kat 24, Borchi(R) Kat 320, Borchi(R) Kat 315EU, Borchi(R) Kat VP 0243, and Borchi(R) Kat VP 0244, and catalysts from Fujifilm Wako Pure Chemical Industries, Ltd. with trade names 2-ethylhexanoate bismuth(III) 2-ethylhexanoic acid solution (Bi:25%); 2-ethylhexanoate bismuth(III), 70-75% in xylenes (~24%Bi) (99.99+%-Bi)PURATREM, but are not particularly limited as long as they promote the urethane reaction.

[0036] The amount of urethane catalyst added can be appropriately determined by those skilled in the art, but from the viewpoint of reaction activity, 1 to 1000 ppm and more preferably 10 to 100 ppm per 100 parts by weight of the hydroxyl group-containing polyoxyalkylene (A) is preferred. Within this range, sufficient reaction activity can be obtained, and the physical properties of the hydrolyzable silyl group-containing polyoxyalkylene (B) produced can be well maintained.

[0037] The urethane formation reaction can be carried out without using a solvent, but an organic solvent may be added to uniformly dissolve the hydroxyl group-containing polyoxyalkylene (A), the hydrolyzable silyl group-containing isocyanate compound, and the urethane formation catalyst, and to facilitate temperature control of the reaction system and addition of the urethane formation catalyst.

[0038] There are no particular limitations on the types of organic solvents that can be used in the urethane reaction, and they can be selected as appropriate. Examples include aliphatic hydrocarbons such as pentane, hexane, heptane, octane, cyclohexane, cyclooctane, cyclodecane, cyclododecane, and petroleum ether; aliphatic halogenated hydrocarbons such as dichloroethane and chloroform; aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, and isopropylbenzene; aromatic halogenated hydrocarbons such as chlorobenzene and chlorotoluene; and ether solvents such as tetrahydrofuran (THF) and tetrahydropyran (THP). One type of organic solvent may be used, or two or more types may be used in combination.

[0039] The temperature during the urethane formation reaction can be set appropriately by those skilled in the art, but it is preferably 50°C to 120°C, and more preferably 70°C to 100°C. The reaction time can also be set appropriately, but it is preferable to adjust the reaction time along with the temperature conditions to prevent unintended condensation reactions between polymers. Specifically, the reaction time is preferably 15 minutes to 5 hours, and more preferably 30 minutes to 3 hours.

[0040] [Aspect (II)] <Aspects including a hydrosilylation reaction> In this embodiment, the hydroxyl groups of hydroxyl group-containing polyoxyalkylene (A) are converted to carbon-carbon unsaturated bond-containing groups, and then the carbon-carbon unsaturated bond-containing groups are converted to hydrolyzable silyl groups to obtain hydrolyzable silyl group-containing polyoxyalkylene (B). The obtained hydrolyzable silyl group-containing polyoxyalkylene (B) usually does not contain urethane bonds.

[0041] More specifically, a polyoxyalkylene (B) containing hydrolyzable silyl groups can be obtained by reacting the hydroxyl groups of a hydroxyl group-containing polyoxyalkylene (A) with an alkali metal salt, then reacting it with a halide containing a carbon-carbon unsaturated bond to convert it into a carbon-carbon unsaturated bond-containing group, and finally hydrosilylation reacting the carbon-carbon unsaturated bond with a hydrolyzable silyl group-containing hydrosilane compound.

[0042] The hydrolyzable silyl group in the hydrolyzable silyl group-containing polyoxyalkylene (B) obtained using embodiment (II) is not particularly limited, but is particularly preferably represented by the following formula (1). -O-(CH2)3-SiR a X 3-a (1) In the above formula, R represents a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms. X represents a hydroxyl group or a hydrolyzable group. a represents 0, 1, or 2, preferably 0 or 1.

[0043] The hydrocarbon group represented by R preferably has 1 to 10 carbon atoms, more preferably 1 to 5, and even more preferably 1 to 3. Specific examples of R include methyl, ethyl, chloromethyl, methoxymethyl, and N,N-diethylaminomethyl groups. Preferably, R is a methyl or ethyl group.

[0044] Examples of X include hydroxyl groups, hydrogen, halogens, alkoxy groups, acyloxy groups, ketoximate groups, amino groups, amide groups, acid amide groups, aminooxy groups, mercapto groups, alkenyloxy groups, etc. Among these, alkoxy groups such as methoxy groups and ethoxy groups are more preferred because they are mildly hydrolyzable and easy to handle, with methoxy groups and ethoxy groups being particularly preferred.

[0045] Specific examples of the hydrolyzable silyl group include trimethoxysilyl group, triethoxysilyl group, tris(2-propenyloxy)silyl group, triacetoxysilyl group, dimethoxymethylsilyl group, diethoxymethylsilyl group, dimethoxyethylsilyl group, (chloromethyl)dimethoxysilyl group, (chloromethyl)diethoxysilyl group, (methoxymethyl)dimethoxysilyl group, (methoxymethyl)diethoxysilyl group, (N,N-diethylaminomethyl)dimethoxysilyl group, (N,N-diethylaminomethyl)diethoxysilyl group, and the like.

[0046] Such silyl groups can be formed by using allyl chloride or the like as the carbon-carbon unsaturated bond-containing halide, and further reacting it with the compounds listed as specific examples as hydrolyzable silyl group-containing hydrosilane compounds.

[0047] (Reaction with alkali metal salts) In converting the hydroxyl groups in a hydroxyl group-containing polyoxyalkylene (A) to carbon-carbon unsaturated bond-containing groups, it is preferable to first react the hydroxyl group-containing polyoxyalkylene (A) with an alkali metal salt to convert the hydroxyl groups in the polymer into metal-oxy groups. Alternatively, a complex metal cyanide catalyst can be used instead of an alkali metal salt. Through these steps, a metal-oxy group-containing polyoxyalkylene is formed.

[0048] The alkali metal salt is not particularly limited, but examples include sodium hydroxide, sodium alkoxide, potassium hydroxide, potassium alkoxide, lithium hydroxide, lithium alkoxide, cesium hydroxide, cesium alkoxide, and the like. Due to their ease of handling and solubility, sodium hydroxide, sodium methoxide, sodium ethoxide, sodium tert-butoxide, potassium hydroxide, potassium methoxide, potassium ethoxide, and potassium tert-butoxide are preferred, with sodium methoxide and sodium tert-butoxide being more preferred. Sodium methoxide is particularly preferred in terms of availability, and sodium tert-butoxide is particularly preferred in terms of reactivity. The alkali metal salt may be subjected to the reaction in a dissolved state in the solvent.

[0049] The amount of alkali metal salt used is not particularly limited, but in order to increase the reaction rate, the molar ratio of the alkali metal salt to the hydroxyl groups of the hydroxyl group-containing polyoxyalkylene (A) is preferably 0.5 or higher, more preferably 0.6 or higher, even more preferably 0.7 or higher, and even more preferably 0.8 or higher. The molar ratio is preferably 1.2 or lower, and more preferably 1.1 or lower.

[0050] To efficiently carry out the reaction that converts the hydroxyl groups of hydroxyl group-containing polyoxyalkylene (A) to metaloxy groups, it is preferable to remove water and any other substances containing hydroxyl groups other than hydroxyl group-containing polyoxyalkylene (A) from the reaction system beforehand. Known methods can be used for this removal, such as heating evaporation, vacuum deflation, spray vaporization, thin-film evaporation, and azeotropic deflation.

[0051] The temperature at which the alkali metal salt is reacted can be appropriately set by those skilled in the art, but is preferably 50°C to 150°C, and more preferably 110°C to 145°C. The duration for which the alkali metal salt is reacted is preferably 10 minutes to 5 hours, and more preferably 30 minutes to 3 hours.

[0052] (Reaction with carbon-carbon unsaturated bond-containing halides) By reacting the metal-oxy group-containing polyoxyalkylene with a carbon-carbon unsaturated bond-containing halide, the metal-oxy groups in the metal-oxy group-containing polyoxyalkylene can be converted into carbon-carbon unsaturated bond-containing groups. The carbon-carbon unsaturated bond-containing halide reacts with the metal-oxy group through a halogen substitution reaction to form an ether bond. This results in the formation of a polyoxyalkylene having a carbon-carbon unsaturated bond.

[0053] Specific examples of carbon-carbon unsaturated bond-containing halides are not limited to vinyl chloride, allyl chloride, methyl chloride, vinyl bromide, allyl bromide, methyl bromide, vinyl iodide, allyl iodide, and methyl iodide. Allyl chloride and methyl chloride are preferred due to their ease of handling.

[0054] There are no particular restrictions on the amount of carbon-carbon unsaturated bond-containing halide added, but the molar ratio of the organic halide to the metaloxy groups of the polyoxyalkylene is preferably 0.7 or higher, and more preferably 1.0 or higher. Furthermore, this molar ratio is preferably 5.0 or lower, and more preferably 2.0 or lower.

[0055] The reaction temperature when reacting a metaloxy group-containing polyoxyalkylene with a carbon-carbon unsaturated bond-containing halide is preferably 50°C to 150°C, and more preferably 110°C to 140°C. The reaction time is preferably 10 minutes to 5 hours, and more preferably 30 minutes to 3 hours.

[0056] Furthermore, a polyoxyalkylene having two or more carbon-carbon unsaturated bonds at one end can also be formed by first reacting the metaloxy group-containing polyoxyalkylene with an epoxy compound having carbon-carbon unsaturated bonds (for example, allyl glycidyl ether), and then reacting it with the aforementioned carbon-carbon unsaturated bond-containing halide.

[0057] (Hydrosilylation reaction) Next, a hydrolyzable silyl group-containing polyoxyalkylene (B) can be obtained by hydrosilylation of the carbon-carbon unsaturated bond of the polyoxyalkylene with a hydrosilane compound containing a hydrolyzable silyl group.

[0058] Specific examples of the hydrolyzable silyl group-containing hydrosilane compounds include halosilanes such as trichlorosilane, dichloromethylsilane, chlorodimethylsilane, dichlorophenylsilane, (chloromethyl)dichlorosilane, (dichloromethyl)dichlorosilane, bis(chloromethyl)chlorosilane, (methoxymethyl)dichlorosilane, (dimethoxymethyl)dichlorosilane, and bis(methoxymethyl)chlorosilane; trimethoxysilane, triethoxysilane, dimethoxymethylsilane, diethoxymethylsilane Lan, dimethoxyphenylsilane, ethyldimethoxysilane, methoxydimethylsilane, ethoxydimethylsilane, (chloromethyl)methylmethoxysilane, (chloromethyl)dimethoxysilane, (chloromethyl)diethoxysilane, bis(chloromethyl)methoxysilane, (methoxymethyl)methylmethoxysilane, (methoxymethyl)dimethoxysilane, bis(methoxymethyl)methoxysilane, (methoxymethyl)diethoxysilane, (ethoxymethyl)diethoxysilane, (3,3,3-trifluor (Propropyl)dimethoxysilane, (N,N-diethylaminomethyl)dimethoxysilane, (N,N-diethylaminomethyl)diethoxysilane, [(chloromethyl)dimethoxysilyloxy]dimethylsilane, [(chloromethyl)diethoxysilyloxy]dimethylsilane, [(methoxymethyl)dimethoxysilyloxy]dimethylsilane, [(methoxymethyl)dimethoxysilyloxy]dimethylsilane, [(diethylaminomethyl)dimethoxysilyloxy]dimethylsilane, [(3,3,3-triph Examples include alkoxysilanes such as [dimethoxysilyloxy]dimethylsilane (orololpropyl); acyloxysilanes such as diacetoxymethylsilane and diacetoxyphenylsilane; ketoximate silanes such as bis(dimethylketoximate)methylsilane and bis(cyclohexylketoximate)methylsilane; and isopropenyloxysilanes (deacetone-free type) such as triisopropenyloxysilane, (chloromethyl)diisopropenyloxysilane, and (methoxymethyl)diisopropenyloxysilane.

[0059] The amount of hydrolyzable silyl group-containing hydrosilane compound used is not particularly limited, but the molar ratio of the hydrosilane compound to the carbon-carbon unsaturated bonds of the polyoxyalkylene is preferably 0.6 or higher, and more preferably 0.8 or higher. Furthermore, this molar ratio is preferably 5.0 or lower, and more preferably 2.0 or lower.

[0060] Hydrosilylation reactions are preferably carried out in the presence of a hydrosilylation catalyst to accelerate the reaction. Suitable hydrosilylation catalysts include metals such as cobalt, nickel, iridium, platinum, palladium, rhodium, and ruthenium, as well as complexes thereof. Specifically, examples include platinum supported on a carrier such as alumina, silica, or carbon black; chloroplatinic acid; chloroplatinic acid complexes consisting of chloroplatinic acid with alcohols, aldehydes, or ketones; platinum-olefin complexes [e.g., Pt(CH2=CH2)2(PPh3), Pt(CH2=CH2)2Cl2]; platinum-vinylsiloxane complexes [e.g., Pt{(vinyl)Me2SiOSiMe2(vinyl)}, Pt{Me(vinyl)SiO}4]; platinum-phosphine complexes [e.g., Ph(PPh3)4, Pt(PBu3)4]; and platinum-phosphine complexes [e.g., Pt{P(OPh)3}4]. From the viewpoint of reaction efficiency, platinum catalysts such as chloroplatinic acid and platinum vinylsiloxane complexes are preferred.

[0061] Although the hydrosilylation reaction can be carried out without a solvent, an organic solvent may be added to ensure uniform dissolution of the polyoxyalkylene having a carbon-carbon unsaturated bond, the hydrolyzable silyl group-containing hydrosilane compound, and the hydrosilylation catalyst, as well as to facilitate temperature control of the reaction system and the addition of the hydrosilylation catalyst.

[0062] The temperature during the hydrosilylation reaction is not particularly limited and can be set appropriately by those skilled in the art, but heating conditions are preferred in order to lower the viscosity of the reaction system and improve reactivity. Specifically, 50°C to 150°C is more preferred, and 70°C to 120°C is even more preferred. The reaction time can also be set appropriately, but it is preferable to adjust the reaction time along with the temperature conditions to prevent unintended condensation reactions between polymers from proceeding. Specifically, the reaction time is preferably 30 minutes to 5 hours, and more preferably 3 hours or less.

[0063] <<Hydrolyzable silyl group-containing polyoxyalkylene (B)>> By the manufacturing method described above, a hydrolyzable silyl group-containing polyoxyalkylene (B) can be produced. Because the water content of the monoepoxide used during polymerization is less than 50 ppm, this hydrolyzable silyl group-containing polyoxyalkylene (B) can exhibit a higher modulus after curing.

[0064] The hydrolyzable silyl groups in polyoxyalkylene (B) are silyl groups that have a hydroxyl group or hydrolyzable group bonded to a silicon atom and can form crosslinks by forming siloxane bonds. Specifically, they can be represented by the following formula. -SiR b X 3-b (2) In the above formula, R represents a substituted or unsubstituted hydrocarbon group having 1 to 20 carbon atoms. X represents a hydroxyl group or a hydrolyzable group. b represents 0, 1, or 2, preferably 0 or 1.

[0065] The hydrocarbon group represented by R preferably has 1 to 10 carbon atoms, more preferably 1 to 5, and even more preferably 1 to 3. Specific examples of R include methyl, ethyl, chloromethyl, methoxymethyl, and N,N-diethylaminomethyl groups. Preferably, R is a methyl or ethyl group.

[0066] Examples of X include hydroxyl groups, hydrogen, halogens, alkoxy groups, acyloxy groups, ketoximate groups, amino groups, amide groups, acid amide groups, aminooxy groups, mercapto groups, alkenyloxy groups, etc. Among these, alkoxy groups such as methoxy groups and ethoxy groups are more preferred because they are mildly hydrolyzable and easy to handle, with methoxy groups and ethoxy groups being particularly preferred.

[0067] Specific examples of the hydrolyzable silyl group include trimethoxysilyl group, triethoxysilyl group, tris(2-propenyloxy)silyl group, triacetoxysilyl group, dimethoxymethylsilyl group, diethoxymethylsilyl group, dimethoxyethylsilyl group, (chloromethyl)dimethoxysilyl group, (chloromethyl)diethoxysilyl group, (methoxymethyl)dimethoxysilyl group, (methoxymethyl)diethoxysilyl group, (N,N-diethylaminomethyl)dimethoxysilyl group, (N,N-diethylaminomethyl)diethoxysilyl group, and the like.

[0068] As described above, hydrolyzable silyl group-containing polyoxyalkylene (B) has either a linear polymer skeleton or a branched polymer skeleton, depending on the number of hydroxyl groups in the initiator. When the hydrolyzable silyl group-containing polyoxyalkylene (B) has a branched polymer skeleton, producing it using a monoepoxide with a low water content according to this embodiment can result in a higher modulus compared to producing it using a monoepoxide with a high water content. This is presumed to be because the polymer produced with water as an initiator has a linear structure, and such linear hydrolyzable silyl group-containing polyoxyalkylenes are less likely to exhibit modulus compared to branched hydrolyzable silyl group-containing polyoxyalkylenes.

[0069] On the other hand, when the hydrolyzable silyl group-containing polyoxyalkylene (B) has a linear polymer skeleton, when it is produced using a monoepoxide with a low water content according to this embodiment, the curability of the hydrolyzable silyl group-containing polyoxyalkylene (B) is better than when it is produced using a monoepoxide with a high water content.

[0070] <<Curable composition containing hydrolyzable silyl group-containing polyoxyalkylene (B)>> The hydrolyzable silyl group-containing polyoxyalkylene (B) produced by this embodiment can be used to make a curable composition containing it. The curable composition may use only one type of hydrolyzable silyl group-containing polyoxyalkylene (B), or two or more types may be used in combination.

[0071] A curable composition containing a hydrolyzable silyl group-containing polyoxyalkylene (B) may also contain a curing catalyst, silicon compound, adhesion promoter, plasticizer, solvent, diluent, silicate, filler, anti-sagging agent, antioxidant, light stabilizer, UV absorber, property modifier, tackifying resin, epoxy group-containing compound, photocurable substance, oxygen-curable substance, surface modifier, epoxy resin, other resin, flame retardant, foaming agent, etc.

[0072] Furthermore, various additives may be added to the curable composition as needed for the purpose of adjusting the physical properties of the composition or the cured product. Examples of such additives include curing modifiers, radical inhibitors, metal deactivators, ozone degradation inhibitors, phosphorus-based peroxide decomposers, lubricants, pigments, and antifungal agents.

[0073] <<Application>> The curable composition can be used as an adhesive, a sealing material for buildings, ships, automobiles, roads, etc., a waterproofing material, a waterproof coating material, a molding material, a vibration damping material, a soundproofing material, a foaming material, a paint, or a spray material. The cured product obtained by curing the composition according to this embodiment has excellent flexibility and adhesion, and can therefore be suitably used as a sealing material or an adhesive.

[0074] Furthermore, the curable composition is used for electrical and electronic component materials such as back-surface sealing materials for solar cells, electrical and electronic component and device insulating coatings such as insulating coatings for wires and cables, acoustic insulating materials, elastic adhesives, binders, contact adhesives, spray sealants, crack repair materials, tile adhesives, asphalt waterproofing adhesives, powder coatings, casting materials, medical rubber materials, medical adhesives, medical adhesive sheets, medical device sealants, dental impression materials, food packaging materials, and joint sealants for exterior materials such as sizing boards. It can be used in a wide variety of applications, including coatings, anti-slip coatings, cushioning materials, primers, conductive materials for electromagnetic shielding, thermally conductive materials, hot-melt materials, potting agents for electrical and electronic applications, films, gaskets, concrete reinforcement materials, temporary adhesives, various molding materials, and liquid sealants used in rust prevention and waterproofing of wired glass and laminated glass edges (cut sections), automobile parts, large vehicle parts such as trucks and buses, train car parts, aircraft parts, ship parts, electrical parts, and various machine parts. Taking automobiles as an example, it can be used in a wide variety of applications, such as adhesive attachment of plastic covers, trims, flanges, bumpers, window mounting, interior components, and exterior components. Furthermore, since it can adhere to a wide range of substrates such as glass, porcelain, wood, metal, and resin molded products, either alone or with the help of a primer, it can also be used as various types of sealing and adhesive compositions. Furthermore, the composition according to this embodiment can be used as an adhesive for interior panels, exterior panels, tile adhesives, stone cladding adhesives, ceiling finishing adhesives, floor finishing adhesives, wall finishing adhesives, vehicle panels, electrical, electronic, and precision equipment assembly adhesives, adhesives for bonding leather, textiles, fabrics, paper, boards, and rubber, reactive crosslinking pressure-sensitive adhesives, direct glazing sealants, double-glazed glass sealants, SSG method sealants, or working joint sealants for buildings, as well as for civil engineering and bridge construction materials. In addition, it can be used as an adhesive material such as adhesive tape or adhesive sheet.

[0075] [Disclosure items] Each of the following items is a disclosure of a preferred embodiment.

[0076] [Item 1] A process to obtain a hydroxyl group-containing polyoxyalkylene (A) by ring-opening polymerization of a monoepoxide with a water content of 5 ppm or more and less than 50 ppm, and A method for producing a hydrolyzable silyl group-containing polyoxyalkylene (B), comprising the step of introducing a hydrolyzable silyl group into the hydroxyl group-containing polyoxyalkylene (A).

[0077] [Item 2] The method for obtaining the hydroxyl group-containing polyoxyalkylene (A) as described in item 1, wherein the step is carried out in the presence of a complex metal cyanide catalyst.

[0078] [Item 3] The manufacturing method according to item 1 or 2, wherein the step of introducing the hydrolyzable silyl group is a step of converting the hydroxyl group of the hydroxyl group-containing polyoxyalkylene (A) into a carbon-carbon unsaturated bond-containing group, and converting the carbon-carbon unsaturated bond-containing group into a hydrolyzable silyl group.

[0079] [Item 4] The manufacturing method according to item 1 or 2, wherein the step of introducing the hydrolyzable silyl group is a step of urethane-forming the hydroxyl group of the hydroxyl group-containing polyoxyalkylene (A) with a hydrolyzable silyl group-containing isocyanate compound.

[0080] [Item 5] The method for producing polyoxyalkylene according to any one of items 1 to 4, wherein the hydroxyl group-containing polyoxyalkylene (A) and the hydrolyzable silyl group-containing polyoxyalkylene (B) have a branched polymer skeleton.

[0081] [Item 6] The method for producing the hydroxyl group-containing polyoxyalkylene (A) and the hydrolyzable silyl group-containing polyoxyalkylene (B) according to any one of items 1 to 4, wherein the hydroxyl group-containing polyoxyalkylene (A) and the hydrolyzable silyl group-containing polyoxyalkylene (B) have a linear polymer skeleton. [Examples]

[0082] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0083] The number-average molecular weight in the examples is the GPC molecular weight measured under the following conditions. Liquid delivery system: Tosoh HLC-8220GPC Column: Tosoh TSK-GEL H type Solvent: THF Molecular weight: Polystyrene equivalent Measurement temperature: 40℃

[0084] The water content of the propylene oxide in the examples was measured using a Karl Fischer moisture meter (model MKH-700) manufactured by Kyoto Electronics Manufacturing Co., Ltd.

[0085] (Example 1) In a stainless steel reactor, 550 g of polyoxypropylene triol with a number-average molecular weight of approximately 4,500, a zinc hexacyanocobaltate-grime complex catalyst, THF, and 70 g of propylene oxide with a pre-measured water content were added as initiators. The mixture was heated to 90°C while stirring with a stirrer to activate the catalyst. After the reactor pressure decreased, an additional 4400 g of propylene oxide with a pre-measured water content was continuously added to the reactor at 135°C to obtain branched polyoxypropylene (A-1) having hydroxyl groups at the ends. The water content of the propylene oxide used was 19 ppm.

[0086] 0.76 molar equivalents of sodium methoxide in a 28% methanol solution were added to the hydroxyl groups of the obtained hydroxyl group-containing polyoxypropylene (A-1). After removing methanol by vacuum distillation, 0.85 molar equivalents of allyl chloride were added to the hydroxyl groups of polymer (A-1) and the reaction was carried out at 130°C for 1 hour, after which the allyl chloride was removed by distillation. Subsequently, 0.47 molar equivalents of sodium methoxide in a 28% methanol solution were added to the hydroxyl groups of polymer (A-1) and the reaction was carried out at 130°C for 2 hours, after which the allyl chloride was removed by distillation. The obtained unpurified allyl-terminated polyoxypropylene was mixed and stirred with n-hexane and water, and the water was removed by centrifugation. The metal salts in the polymer were removed by vacuum distillation of hexane from the obtained hexane solution. Thus, polyoxypropylene (C-1) having a carbon-carbon unsaturated bond (allyl group) was obtained.

[0087] Next, at 90°C, 50 ppm of platinum divinyldisiloxane complex (a solution of isopropanol equivalent to 3% by weight of platinum) and 1.28 parts by weight of dimethoxymethylsilane were added to 100 parts by weight of polymer (C-1) to carry out a hydrosilylation reaction of the allyl groups of polymer (C-1). The reaction was carried out at 90°C until the dimethoxymethylsilane was completely consumed, and then the volatile components were removed by distillation. As a result, branched polyoxypropylene (B-1) having dimethoxymethylsilyl groups at the terminals was obtained.

[0088] (Comparative Example 1) Polymerization, allylation, and hydrosilylation reactions were carried out in exactly the same procedure as in Example 1, except that the water content of the propylene oxide used was 60 ppm. Polymerization yielded branched polyoxypropylene (A-2) having hydroxyl groups at the terminals, followed by allylation to obtain polyoxypropylene (C-2) having carbon-carbon unsaturated bonds (allyl groups), and then hydrosilylation to obtain branched polyoxypropylene (B-2) having dimethoxymethylsilyl groups at the terminals.

[0089] (Dumbbell tensile properties) To 100 parts by weight of polyoxypropylene having dimethoxymethylsilyl groups at the ends, 3 parts by weight of Neostan U-28, 0.5 parts by weight of laurylamine, and 0.6 parts by weight of pure water were mixed and stirred. The mixture was then filled into a mold and cured at 80°C for 20 hours to produce a sheet-like cured material with a thickness of approximately 3 mm. The sheet-like cured material was punched out into a No. 3 dumbbell shape, and a tensile strength test was performed at 23°C and 50% RH to measure the modulus at 50% elongation. The measurement was performed using a Shimadzu Autograph (AGS-J) at a tensile speed of 200 mm / min. The results are shown in Table 1.

[0090] [Table 1]

[0091] Although Example 1 and Comparative Example 1 have the same formulation except for the water content of the propylene oxide used in polymerization, Table 1 shows that the hydrolyzable silyl group-containing polyoxypropylene of Example 1, which has a water content of 5 ppm or more and less than 50 ppm of propylene oxide, exhibits a higher modulus than the hydrolyzable silyl group-containing polyoxypropylene of Comparative Example 1, which has a water content of 50 ppm or more of propylene oxide.

[0092] (Example 2) In a stainless steel reactor, 520 g of polyoxypropylene triol with a number-average molecular weight of approximately 4,500, a zinc hexacyanocobaltate glyme complex catalyst, THF, and 70 g of propylene oxide with a pre-measured water content were added as initiators. The mixture was heated to 90°C while stirring with a stirrer to activate the catalyst. After the reactor pressure decreased, an additional 3800 g of propylene oxide with a pre-measured water content was continuously added to the reactor at 135°C to obtain branched polyoxypropylene (A-3) having hydroxyl groups at the ends. The water content of the propylene oxide used was 15 ppm.

[0093] Next, at 90°C, 30 ppm of bismuth(III) 2-ethylhexanoic acid solution (Bi: 25%) and 2.2 parts by weight of (isocyanate methyl)dimethoxymethylsilane were added to 100 parts by weight of polymer (A-3) to carry out a urethane reaction on the hydroxyl groups of the polymer. As a result, branched polyoxypropylene (B-3) having dimethoxymethylsilyl groups at its terminals was obtained.

[0094] (Comparative Example 2) The polymerization and urethane reaction were carried out in exactly the same procedure as in Example 2, except that the water content of the propylene oxide used was 66 ppm. Branched polyoxypropylene (A-4) with hydroxyl groups at the terminals was obtained by polymerization, and branched polyoxypropylene (B-4) with dimethoxymethylsilyl groups at the terminals was obtained by the subsequent urethane reaction.

[0095] (Dumbbell tensile properties) The modulus at 50% elongation was measured for Example 1 and Comparative Example 1 using the method described above. The results are shown in Table 2.

[0096] [Table 2]

[0097] Although Example 2 and Comparative Example 2 have the same formulation except for the water content of the propylene oxide used in polymerization, Table 2 shows that the hydrolyzable silyl group-containing polyoxypropylene of Example 2, which has a propylene oxide water content of 5 ppm or more and less than 50 ppm, exhibits a higher modulus than the hydrolyzable silyl group-containing polyoxypropylene of Comparative Example 2, which has a propylene oxide water content of 50 ppm or more.

[0098] (Example 3) At 90°C, 30 ppm of a bismuth(III) 2-ethylhexanoic acid solution (Bi: 25%) and 2.5 parts by weight of (3-isocyanatetopropyl)trimethoxysilane were added to 100 parts by weight of polymer (A-3) obtained in Example 2 to carry out a urethane reaction on the hydroxyl groups of the polymer. As a result, branched polyoxypropylene (B-5) having trimethoxysilyl groups at the terminals was obtained.

[0099] (Comparative Example 3) At 90°C, 30 ppm of a bismuth(III) 2-ethylhexanoic acid solution (Bi: 25%) and 2.5 parts by weight of (3-isocyanatetopropyl)trimethoxysilane were added to 100 parts by weight of polymer (A-4) obtained in Comparative Example 2 to carry out a urethane reaction on the hydroxyl groups of the polymer. As a result, branched polyoxypropylene (B-6) having trimethoxysilyl groups at the terminals was obtained.

[0100] (Dumbbell tensile properties) The modulus at 50% elongation was measured for Example 1 and Comparative Example 1 using the method described above. The results are shown in Table 3.

[0101] [Table 3]

[0102] Although Example 3 and Comparative Example 3 have the same formulation except for the water content of the propylene oxide used in polymerization, Table 3 shows that the hydrolyzable silyl group-containing polyoxypropylene of Example 3, which has a water content of 5 ppm or more and less than 50 ppm of propylene oxide, exhibits a higher modulus than the hydrolyzable silyl group-containing polyoxypropylene of Comparative Example 3, which has a water content of 50 ppm or more of propylene oxide.

[0103] (Example 4) In a stainless steel reactor, 740 g of polyoxypropylene glycol with a number-average molecular weight of approximately 6,200, a zinc hexacyanocobaltate-grime complex catalyst, THF, and 50 g of propylene oxide with a pre-measured water content were added as initiators. The mixture was heated to 90°C while stirring with a stirrer to activate the catalyst. After the reactor pressure decreased, an additional 3752 g of propylene oxide with a pre-measured water content was continuously added to the reactor at 135°C to obtain linear polyoxypropylene (A-5) with hydroxyl groups at the ends. The water content of the propylene oxide used was 41 ppm.

[0104] To the hydroxyl groups of the obtained hydroxyl-containing polyoxypropylene (A-5), 1.00 molar equivalent of sodium methoxide was added as a 28% methanol solution. After removing the methanol by vacuum distillation, 1.00 molar equivalent of allyl glycidyl ether was added to the hydroxyl groups of polymer (A-5) and the reaction was carried out at 130°C for 2 hours. Furthermore, 1.30 molar equivalent of allyl chloride was added to the hydroxyl groups of polymer (A-5) and the reaction was carried out at 130°C for 1 hour, after which the allyl chloride was removed by distillation. Subsequently, 0.30 molar equivalent of sodium methoxide was added to the hydroxyl groups of polymer (A-5) as a 28% methanol solution. After removing the methanol by vacuum distillation at 130°C, 0.70 molar equivalent of allyl chloride was added to the hydroxyl groups of polymer (A-5) and the reaction was carried out at 130°C for 2 hours, after which the allyl chloride was removed by distillation. The obtained unpurified allyl-terminated polyoxypropylene was mixed and stirred with n-hexane and water. After removing the water by centrifugation, the hexane was removed from the resulting hexane solution under reduced pressure to remove the metal salts from the polymer. Thus, polyoxypropylene (C-3) having carbon-carbon unsaturated bonds (allyl groups) was obtained.

[0105] Next, at 90°C, 36 ppm of platinum divinyldisiloxane complex (a solution of isopropanol equivalent to 3% by weight of platinum) and 1.83 parts by weight of dimethoxymethylsilane were added to 100 parts by weight of polymer (C-3) to carry out a hydrosilylation reaction of the allyl groups of polymer (C-3). The reaction was carried out at 90°C until the dimethoxymethylsilane was completely consumed, and then the volatile components were removed by distillation. Thus, linear polyoxypropylene (B-7) having dimethoxymethylsilyl groups at its termini was obtained.

[0106] (Comparative Example 4) Polymerization, allylation, and hydrosilylation reactions were carried out in exactly the same procedure as in Example 4, except that the water content of the propylene oxide used was 107 ppm. Polymerization yielded linear polyoxypropylene (A-6) with hydroxyl groups at the terminals, followed by allylation to obtain polyoxypropylene (C-4) with carbon-carbon unsaturated bonds (allyl groups), and then hydrosilylation to obtain linear polyoxypropylene (B-8) with dimethoxymethylsilyl groups at the terminals.

[0107] (Dumbbell tensile properties) The modulus at 50% elongation was measured for Example 1 and Comparative Example 1 using the method described above. The results are shown in Table 4.

[0108] [Table 4]

[0109] Although Example 4 and Comparative Example 4 have the same formulation except for the water content of the propylene oxide used in polymerization, Table 4 shows that the hydrolyzable silyl group-containing polyoxypropylene of Example 4, which has a water content of 5 ppm or more and less than 50 ppm of propylene oxide, exhibits a higher modulus than the hydrolyzable silyl group-containing polyoxypropylene of Comparative Example 4, which has a water content of 50 ppm or more of propylene oxide.

[0110] (Example 5) At 90°C, 30 ppm of a bismuth(III) 2-ethylhexanoic acid solution (Bi: 25%) and 1.85 parts by weight of (3-isocyanatetopropyl)trimethoxysilane were added to 100 parts by weight of the polymer (A-5) obtained in Example 4 to carry out a urethane reaction on the hydroxyl groups of the polymer. As a result, linear polyoxypropylene (B-9) having trimethoxysilyl groups at its termini was obtained.

[0111] (Comparative Example 5) At 90°C, 30 ppm of a bismuth(III) 2-ethylhexanoic acid solution (Bi: 25%) and 1.85 parts by weight of (3-isocyanatetopropyl)trimethoxysilane were added to 100 parts by weight of polymer (A-6) obtained in Comparative Example 4 to carry out a urethane reaction on the hydroxyl groups of the polymer. As a result, linear polyoxypropylene (B-10) having trimethoxysilyl groups at its termini was obtained.

[0112] (Dumbbell tensile properties) The modulus at 50% elongation was measured for Example 1 and Comparative Example 1 using the method described above. The results are shown in Table 5.

[0113] [Table 5]

[0114] Although Example 5 and Comparative Example 5 have the same formulation except for the water content of the propylene oxide used in polymerization, Table 5 shows that the hydrolyzable silyl group-containing polyoxypropylene of Example 5, which has a water content of 5 ppm or more and less than 50 ppm of propylene oxide, exhibits a higher modulus than the hydrolyzable silyl group-containing polyoxypropylene of Comparative Example 5, which has a water content of 50 ppm or more of propylene oxide.

[0115] (Synthesis Example 1) In a stainless steel reactor, 530 g of polyoxypropylene glycol with a number-average molecular weight of approximately 4,500, a zinc hexacyanocobaltate-grime complex catalyst, THF, and 60 g of propylene oxide with a pre-measured water content were added as initiators. The mixture was heated to 90°C while stirring with a stirrer to activate the catalyst. After the reactor pressure decreased, an additional 4400 g of propylene oxide with a pre-measured water content was continuously added to the reactor at 110°C to obtain linear polyoxypropylene (A-7) with hydroxyl groups at the ends. The water content of the propylene oxide used was 16 ppm.

[0116] 0.94 molar equivalents of sodium methoxide in a 28% methanol solution were added to the hydroxyl groups of the obtained hydroxyl group-containing polyoxypropylene (A-7). After removing methanol by vacuum distillation, 1.15 molar equivalents of metharyl chloride were added to the hydroxyl groups of polymer (A-7) and the reaction was carried out at 130°C for 1 hour, after which the metharyl chloride was removed by distillation. Subsequently, 0.42 molar equivalents of sodium methoxide in a 28% methanol solution were added to the hydroxyl groups of polymer (A-7) and the reaction was carried out at 130°C for 1 hour, after which the metharyl chloride was removed by distillation. The obtained unpurified metharyl-terminated polyoxypropylene was mixed and stirred with n-hexane and water, and the water was removed by centrifugation. The metal salts in the polymer were removed by vacuum distillation of hexane from the obtained hexane solution. Thus, polyoxypropylene (C-5) having a carbon-carbon unsaturated bond (methallyl group) was obtained.

[0117] Next, at 90°C, 100 ppm of platinum divinyldisiloxane complex (isopropanol solution equivalent to 3% by weight of platinum), 0.08 ppm of 2,5-di-tert-butyl-1,4-benzoquinone, 100 ppm of 0.25% sulfur / hexane solution, and 1.75 ppm of dimethoxymethylsilane were added to 100 ppm by weight of polymer (C-5) to carry out a hydrosilylation reaction of the methallyl groups of polymer (C-5). The reaction was carried out at 90°C until the methallyl groups were completely consumed, and then the volatile components were removed by distillation. Thus, linear polyoxypropylene (B-11) having dimethoxymethylsilyl groups at its termini was obtained.

[0118] (Synthesis Example 2) Polymerization, methallylation, and hydrosilylation reactions were carried out using the exact same procedure as in Synthesis Example 1, except that the water content of the propylene oxide used was 60 ppm. Polymerization yielded linear polyoxypropylene (A-8) with hydroxyl groups at the terminals, followed by an allylation reaction to obtain polyoxypropylene (C-6) with carbon-carbon unsaturated bonds (allyl groups), and then a subsequent hydrosilylation reaction to obtain linear polyoxypropylene (B-12) with dimethoxymethylsilyl groups at the terminals.

[0119] (Examples 6-7, Comparative Examples 6-7) For every 100 parts by weight of each polymer listed in Table 6, add 90 parts by weight of DINP (J-Plus Co., Ltd.: diisononyl phthalate), 160 parts by weight of Shirotsuya CCR (Shiraishi Calcium Co., Ltd.: precipitated calcium carbonate), 54 parts by weight of Whiten SB (Shiraishi Calcium Co., Ltd.: heavy calcium carbonate), 5 parts by weight of Typeque R820 (Ishihara Sangyo Co., Ltd.: titanium dioxide), 2 parts by weight of Disparon 6500 (Kusumoto Chemical Co., Ltd.: fatty acid amide wax), 1 part by weight of Tinuvin 770 (BASF: bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate), and Tinuvin 326 (BASF: 2-(3-tert-butyl-2-hydroxy- 1 part by weight of 5-methylphenyl)-5-chlorobenzotriazole was mixed, and 2 parts by weight of A-171 (manufactured by Momentive: vinyltrimethoxysilane), 3 parts by weight of A-1120 (manufactured by Momentive: N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane), and 2 parts by weight of Neostan U-220H (manufactured by Nitto Chemical Co., Ltd., dibutyltin diacetoacetonate) were added and mixed to obtain the composition for evaluation.

[0120] (Dumbbell tensile properties) The obtained evaluation composition was filled into a mold and cured at 23°C for 3 days, and then at 50°C for 4 days to produce a sheet-like hardened material with a thickness of approximately 3 mm. The sheet-like hardened material was punched out into a No. 3 dumbbell shape, and a tensile strength test was performed at 23°C and 50% RH to measure the modulus at 50% elongation. The measurement was performed using a Shimadzu Autograph (AGS-J) at a tensile speed of 200 mm / min. The results are shown in Table 6.

[0121] (Leather stretching time) The obtained evaluation composition was filled into a mold approximately 5 mm thick. The time it took to flatten the surface was defined as the curing start time, and the time it took for the evaluation composition to no longer adhere to the spatula after touching the surface was defined as the skinning time. The curing time was measured in Table 6. The results are shown in Table 6.

[0122] [Table 6]

[0123] Table 6 shows that the hydrolyzable silyl group-containing polyoxypropylene of Example 6 or 7, where the propylene oxide water content is 5 ppm or more and less than 50 ppm, exhibits a higher modulus than the hydrolyzable silyl group-containing polyoxypropylene of Comparative Example 6 or 7, where the propylene oxide water content is 50 ppm or more.

[0124] Furthermore, in the case of branched hydrolyzable silyl group-containing polyoxyalkylenes, Comparative Example 7, in which the propylene oxide water content was 50 ppm or more, and Example 7, in which the propylene oxide water content was 5 ppm or more and less than 50 ppm, had equivalent skinning times. On the other hand, in the case of linear hydrolyzable silyl group-containing polyoxyalkylenes, Example 6, in which the propylene oxide water content was 5 ppm or more and less than 50 ppm, had a shorter skinning time and better curing properties compared to Comparative Example 6, in which the propylene oxide water content was 50 ppm or more.

Claims

1. A step of obtaining a hydroxyl group-containing polyoxyalkylene (A) by ring-opening polymerization of a monoepoxide with a water content of 15 ppm or more and less than 50 ppm, and The process includes introducing a hydrolyzable silyl group into the hydroxyl group-containing polyoxyalkylene (A), The process for obtaining the hydroxyl group-containing polyoxyalkylene (A) is carried out in the presence of an initiator having two or more hydroxyl groups and a complex metal cyanide catalyst. A method for producing hydrolyzable silyl group-containing polyoxyalkylene (B), wherein the moisture content is a value measured using a Karl Fischer moisture meter.

2. The manufacturing method according to claim 1, wherein the step of introducing the hydrolyzable silyl group is a step of converting the hydroxyl group of the hydroxyl group-containing polyoxyalkylene (A) into a carbon-carbon unsaturated bond-containing group, and converting the carbon-carbon unsaturated bond-containing group into a hydrolyzable silyl group.

3. The manufacturing method according to claim 1, wherein the step of introducing the hydrolyzable silyl group is a step of urethane-forming the hydroxyl group of the hydroxyl group-containing polyoxyalkylene (A) with a hydrolyzable silyl group-containing isocyanate compound.

4. The method for producing polyoxyalkylene according to any one of claims 1 to 3, wherein the hydroxyl group-containing polyoxyalkylene (A) and the hydrolyzable silyl group-containing polyoxyalkylene (B) have a branched polymer skeleton.

5. The method for producing polyoxyalkylene according to any one of claims 1 to 3, wherein the hydroxyl group-containing polyoxyalkylene (A) and the hydrolyzable silyl group-containing polyoxyalkylene (B) have a linear polymer skeleton.

Citation Information

Patent Citations

  • Water removing reagent and preparation method of water removing reagent as well as method for removing trace water in alkylene oxide

    CN106831660A

  • Room temperature curing compositions

    JP1977073998A

  • Silicone-based resin composition

    JP1998245482A

  • Curable composition

    JP2000109676A

  • Manufacturing method of cyclic ether adduct of alcohol with less smell

    JP2003183383A