A method for forming a silicon-containing film, and a silicon-containing film formed by this method.

A silicon precursor compound represented by Formula 1 facilitates the deposition of silicon-containing films at high temperatures, addressing deposition rate and substrate complexity issues, resulting in uniform and stable films for advanced electronic devices.

JP7954699B2Active Publication Date: 2026-11-20UP CHEM
View PDF 5 Cites -1 Cited by

Patent Information

Application Number
JP2024501184
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-07-23
Filing Date
2022-07-21
Publication Date
2026-11-20
Estimated Expiration
2042-07-21

AI Technical Summary

Technical Problem

Existing silicon-containing films face challenges in deposition rate, especially for nitride films, and are unsuitable for high-temperature applications and complex substrate shapes, necessitating a composition for forming silicon-containing films with self-regulating film growth characteristics suitable for atomic layer deposition (ALD) at temperatures of 600°C or higher.

Method used

A method using a silicon precursor compound represented by Formula 1, allowing for the deposition of silicon-containing oxide and composite metal oxide films via chemical vapor deposition (CVD) or ALD at high temperatures, achieving precise film thickness control and uniform coverage on complex substrates.

Benefits of technology

Enables the formation of high-quality silicon-containing films with excellent coverage and stability at high temperatures, suitable for memory devices, logic devices, and display devices, with controlled thickness and reduced shrinkage and etching rates.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a method for forming a silicon-containing film, and a silicon-containing film formed by the method. The method for forming a silicon-containing film of the present invention uses a composition for forming a silicon-containing film, which contains a silicon precursor compound having a specific structure, to efficiently form a silicon-containing film, including a silicon-containing oxide film or a silicon-containing composite metal oxide film, at a high temperature of 600°C or higher, to control the silicon-containing film to have a desired film thickness and composition, and to form a silicon-containing film with excellent coverage and uniformity even on a substrate having a complex shape.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for forming a silicon-containing film and a silicon-containing film prepared by the method. More specifically, it relates to a method for forming a silicon-containing film at a high temperature of 600°C or higher using a composition for forming a silicon-containing film comprising a silicon precursor compound having a specific structure, and a silicon-containing film prepared by the method. [Background technology]

[0002] Silicon-containing films are one of the essential thin films for driving semiconductors such as DRAM, flash memory, resistive random-access memory (ReRAM), or phase-change memory (PCRAM), as well as non-semiconductor devices such as logic devices.

[0003] While silicon-containing oxide films have a high deposition rate, silicon-containing nitride films have a slow deposition rate. For various applications, there is a need for silicon-containing films that can be selectively deposited only at desired locations.

[0004] Furthermore, in both the memory and non-memory fields, various products with complex shapes such as high aspect ratios and three-dimensional structures are being developed. As a result, there is a need for a composition for forming silicon-containing films containing silicon precursor compounds that is suitable for process temperatures in various application fields, can overcome the problem of high step ratios, and can be used in atomic layer deposition (ALD).

[0005] In particular, to overcome the step ratio problems that may arise due to the high integration and miniaturization of the device, it is important to exhibit self-regulating film growth characteristics.

[0006] Therefore, there is a need to develop a composition for forming a thin film containing a silicon precursor compound that has self-regulating film growth characteristics at high temperatures of 600°C or higher, is suitable for ALD, can form a uniform and dense film, and has stress resistance, as well as a method for forming a silicon-containing film using this composition. [Prior art documents] [Patent Documents]

[0007] [Patent Document 1] Korean Patent No. 10-0734393 [Disclosure of the Invention] technical challenges

[0008] The object of the present invention is to provide a method for forming a silicon-containing film at a high temperature of 600°C or higher using a composition for forming a silicon-containing film containing a silicon precursor compound having a specific structure, and a silicon-containing film prepared by this method.

[0009] Another object of the present invention is to provide a composition for forming a silicon-containing film, comprising a silicon precursor compound having a specific structure.

[0010] However, the problems to be solved by the present invention are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. Solutions to the problems

[0011] The present invention provides a method for forming a silicon-containing film, comprising depositing a silicon-containing film onto a substrate by chemical vapor deposition (CVD) or atomic layer deposition (ALD) using a composition for forming a silicon-containing film comprising a silicon precursor compound represented by formula 1, wherein the silicon-containing film comprises at least one selected from the group consisting of silicon-containing oxide films and silicon-containing composite metal oxide films, and the deposition is carried out at a temperature of 600°C or higher.

[0012] [ka]

[0013] In formula 1, R 11 and R 12 Each of these is independently selected from the group consisting of hydrogen and linear or branched C1-C4 alkyl groups. R 13 ~R 17 Each is independently selected from the group consisting of hydrogen, a linear or branched C1-C4 alkyl group, and a linear or branched C2-C6 alkenyl group, provided that R 13 and R 14 At least one of them is not hydrogen, R 15 ~R 17 At least one of them is not hydrogen.

[0014] Furthermore, the present invention provides a composition for forming a silicon-containing film, which comprises a silicon precursor compound represented by the above formula 1 and is used to deposit a silicon-containing film by chemical vapor deposition (CVD) or atomic layer deposition (ALD) at a temperature of 600°C or higher, wherein the silicon-containing film comprises at least one selected from the group consisting of silicon-containing oxide films and silicon-containing composite metal oxide films.

[0015] Furthermore, the present invention provides a silicon-containing film formed by a method for forming a silicon-containing film. Advantageous effects of the invention

[0016] A method for forming a silicon-containing film according to an embodiment of the present invention allows for the efficient formation of a silicon-containing film comprising at least one selected from the group consisting of silicon-containing oxide films and silicon-containing composite metal oxide films, at a high temperature of 600°C or higher, using a composition for forming a silicon-containing film comprising a silicon precursor compound having a specific structure. This method allows for precise control of the desired film thickness and composition, and enables the formation of a uniform silicon-containing film with excellent coverage, even on substrates with complex shapes.

[0017] In particular, the method for forming silicon-containing films according to the present invention can be applied to various fields, such as memory devices, logic devices, display devices, and moisture penetration barriers for organic light-emitting diode (OLED) devices. Since films with a desired thickness can be obtained at high temperatures of 600°C or higher during film deposition, it can be used very effectively in electronic devices that require excellent film properties and coverage. [Brief explanation of the drawing]

[0018] [Figure 1] This graph shows the deposition characteristics of silicon-containing oxide films at temperatures ranging from 600°C to 850°C, when silicon-containing films are deposited using compositions for forming silicon-containing films, each containing the silicon precursor compounds of Examples 1 to 5 and 8 of the present invention, as well as Comparative Example 1. [Figure 2] This graph shows the results of secondary ion mass spectrometry (SIMS) of silicon-containing oxide films deposited at a temperature of 750°C using compositions for forming silicon-containing films, each containing the silicon precursor compounds of Examples 1 to 5 and Comparative Example 1 of the present invention. [Figure 3] This is a transmission electron microscope (TEM) image confirming step coverage achieved by depositing a silicon-containing film onto a patterned wafer at 750°C using a composition for forming a silicon-containing film, each containing the silicon precursor compound of Example 2 and Comparative Example 1 of the present invention, respectively. [Best Mode for Carrying Out the Invention]

[0019] The present invention is described in detail below.

[0020] The advantages and characteristics of the present invention, as well as methods for achieving them, will become apparent by referring to the embodiments described below. However, the present invention is not limited to the embodiments described below and can be embodied in a variety of different forms. These embodiments are provided so as to ensure that the disclosure of the present invention is thorough and comprehensive and that the scope of this disclosure is fully conveyed to those skilled in the art. The present invention is defined solely by the claims.

[0021] Further, in the present specification, when an element is referred to as being formed "on" another element, it means not only that the element is formed directly "on" the other element, but also that other element(s) may be interposed therebetween.

[0022] In the present specification, unless otherwise specified, when a part is referred to as "comprising" an element, it should be understood that the part does not exclude other elements, and may also include other parts.

[0023] Unless otherwise specified, all numbers and expressions relating to quantities of components, reaction conditions and the like used herein should be understood as being modified by the term "about".

[0024] In the present specification, unless otherwise specified, each of the terms "film" and "thin film" denotes both a film and a thin film.

[0025] In the present specification, the term "alkyl" or "alkyl group" includes within its scope linear or branched alkyl groups and all possible isomers thereof. For example, the alkyl or alkyl group includes a methyl group (Me), an ethyl group (Et), a normal propyl group( n Pr), an isopropyl group( i Pr), a normal butyl group( n Bu), an isobutyl group( i Bu), a tert-butyl group (tert-Bu, t Bu) and a sec-butyl group( sec Bu) and the like, as well as isomers thereof and the like, but the alkyl or alkyl group is not limited thereto.

[0026] [Method for Forming Silicon-Containing Film] According to embodiments of the present invention, a method for forming a silicon-containing film is provided, comprising the step of depositing a silicon-containing film onto a substrate by chemical vapor deposition (CVD) or atomic layer deposition (ALD) using a composition for forming a silicon-containing film comprising a silicon precursor compound represented by Formula 1, wherein the silicon-containing film comprises at least one selected from the group consisting of silicon-containing oxide films and silicon-containing composite metal oxide films, and the deposition is carried out at a temperature of 600°C or higher.

[0027] [ka]

[0028] In formula 1, R 11 and R 12 Each of these is independently selected from the group consisting of hydrogen and linear or branched C1-C4 alkyl groups. R 13 ~R 17 Each is independently selected from the group consisting of hydrogen, a linear or branched C1-C4 alkyl group, and a linear or branched C2-C6 alkenyl group, provided that R 13 and R 14 At least one of them is not hydrogen, R 15 ~R 17 At least one of them is not hydrogen.

[0029] According to the method for forming a silicon-containing film according to an embodiment of the present invention, a silicon-containing film comprising at least one selected from the group consisting of silicon-containing oxide films and silicon-containing composite metal oxide films can be efficiently formed at a high temperature of 600°C or higher using a composition for forming a silicon-containing film comprising a silicon precursor compound having a specific structure represented by Formula 1. This method allows for precise control of the desired film thickness and composition, and enables the formation of a uniform silicon-containing film with excellent coverage even on substrates with complex shapes.

[0030] In particular, the method for forming a silicon-containing film according to the present invention can be applied to various fields such as memory devices, logic devices, display devices, and moisture penetration barriers for organic light-emitting diode (OLED) devices, and has technical significance in that a film of a desired thickness can be obtained at a high temperature of 600°C or higher during film deposition.

[0031] More specifically, a method for forming a silicon-containing film may include the step of depositing a silicon-containing film onto a substrate using a composition for forming a silicon-containing film that comprises a silicon precursor compound represented by Formula 1.

[0032] The substrate may be, but is not limited to, a silicon semiconductor wafer, a compound semiconductor wafer, or a plastic substrate (PI, PET, or PES). Furthermore, a substrate having holes or grooves may be used, as may a porous substrate having a large surface area.

[0033] In particular, silicon-containing films having a thickness of several nanometers (nm) to several micrometers (μm) can be uniformly formed on substrates having patterns (grooves) on their surface, on porous substrates, or on plastic substrates at temperatures of 600°C or higher, more specifically in the temperature range of 600°C to 850°C. Forming a silicon-containing film with a uniform thickness on a substrate produces excellent effects, such as covering the deepest surface of fine patterns (grooves) and the upper surface of fine irregularities (grooves) having an aspect ratio of 1 or more, for example, about 1 to 50 or more, and a width of 1 μm or less, for example, about 1 μm to 10 nm or less. For example, a silicon-containing film can be formed on a substrate having at least one irregularity with an aspect ratio of 1 or more and a width of 1 μm or less.

[0034] The silicon-containing film can be deposited using any method and equipment known in the art to which the present invention belongs, and if necessary, one or more additional reactant gases may be used.

[0035] The silicon-containing film may be deposited by CVD, for example, metal-organic vapor deposition (MOCVD) or ALD. MOCVD or ALD can be carried out using deposition equipment, deposition conditions, and reactive gases known in the art.

[0036] In detail, the substrate is placed in a reaction chamber, and then a composition for forming a silicon-containing film, which includes a silicon precursor compound, is conveyed onto the substrate using a transport gas or diluent gas, and the silicon-containing film is deposited at a deposition temperature of 600°C or higher, specifically 600°C to 850°C.

[0037] Here, the deposition temperature range described above makes it applicable to memory devices, logic devices, and display devices. Because the process temperature is broad, it can be applied to various fields. In particular, because a composition for forming a silicon-containing film containing a silicon precursor compound that is stress-resistant and can form a dense film at high temperatures is used, deposition can be easily carried out within the above deposition temperature range.

[0038] Furthermore, it is preferable to use at least one mixed gas selected from the group consisting of argon (Ar), nitrogen (N2), helium (He), and hydrogen (H2) as the transport gas or diluent gas.

[0039] Furthermore, the method for delivering the silicon precursor compound to the reaction chamber may be at least one method selected from the group consisting of a bubbling method, which forcibly volatilizes a composition for forming a silicon-containing film containing the silicon precursor compound using a carrier gas or diluent gas; a liquid delivery system (LDS) method, which supplies the composition to the liquid phase at room temperature and volatilizes it through an evaporator; a vapor flow control (VFC) method, which directly supplies the precursor using vapor pressure; and a bypass method, which volatilizes it by heating.

[0040] For example, if the vapor pressure is high, a vapor flow control method may be used. If the vapor pressure is low, a bypass method, in which the silicon precursor compound is vaporized by heating the container, or a bubbling method using argon (Ar) or nitrogen (N2) gas may be used to supply the composition for forming a silicon-containing film to the reaction chamber.

[0041] More specifically, the delivery method includes a bubbling method or a bypass method, the bubbling method may be carried out using a carrier gas or diluent gas in a temperature range of room temperature to 150°C and at a pressure of 0.1 Torr to 10 Torr, and the bypass method may be carried out using a vapor pressure of 0.1 Torr to 1.5 Torr in a temperature range of room temperature to 100°C. For example, the supply of a composition for forming a silicon-containing film, which includes a silicon precursor compound, to the reaction chamber may be carried out using a carrier gas or diluent gas in a temperature range of room temperature to 100°C and at a pressure of 0.1 Torr to 10 Torr.

[0042] Furthermore, to volatilize the composition for forming a silicon-containing film containing a silicon precursor compound, for example, argon (Ar) or nitrogen (N2) gas may be used for transport, thermal energy or plasma may be used during deposition, and a bias may be applied to the substrate.

[0043] On the other hand, according to the method for forming a silicon-containing film, in order to deposit at least one silicon-containing film selected from the group consisting of a silicon-containing oxide film or a silicon-containing composite metal oxide film, at least one selected from the group consisting of water vapor (H2O), oxygen (O2), oxygen plasma (O2 plasma), nitrogen oxide (NO, N2O), nitrogen oxide plasma (N2O plasma), oxygen nitrate (N2O2), hydrogen peroxide (H2O2), and ozone (O3), at least one can be used during deposition.

[0044] At least one silicon-containing film selected from the group consisting of silicon-containing oxide films or silicon-containing composite metal oxide films is, for example, HfSiO x , ZrSiO x , SiO x, HfAlO x ZrAlSiO x TiAlSiO x ZrHfSiO x ZrHfAlSiO x It may include, but is not limited to, at least one selected from the group consisting of SiC, SiCO, and SiON. Here, x can be 1 to 3.

[0045] Furthermore, at least one silicon-containing film selected from the group consisting of silicon-containing nitride films or silicon-containing composite metal nitride films can be formed by using a composition for forming a silicon-containing film that contains a silicon precursor compound represented by Formula 1.

[0046] In detail, in order to deposit a silicon-containing nitride film or a silicon-containing composite metal nitride film, at least one selected from the group consisting of ammonia (NH3), ammonia plasma (HN3 plasma), hydrazine (N2H4), and nitrogen plasma (N2 plasma) may be used during the deposition process.

[0047] Silicon-containing nitride films or silicon-containing composite metal nitride films include, for example, HfSiN x ZrSiN x TiSiN x AlSiN x HfAlSiN x ZrAlSiN x TiAlSiN x HfZrAlSiN x HfZrTiSiN x TiAlSiN x It may include, but is not limited to, at least one selected from the group consisting of SiCN, SiOCN, and SiBN. Here, x can be 1 to 3.

[0048] A composition for forming a silicon-containing film, comprising a silicon precursor compound represented by the above formula 1, is described in detail below.

[0049] [Composition for forming a silicon-containing film] The present invention provides a composition for forming a silicon-containing film, comprising a silicon precursor compound represented by formula 1.

[0050] More specifically, the composition for forming a silicon-containing oxide film comprises a silicon precursor compound represented by the above formula 1, and can be used to deposit a silicon-containing film by chemical vapor deposition (CVD) or atomic layer deposition (ALD) at a temperature of 600°C or higher, wherein the silicon-containing film comprises at least one selected from the group consisting of silicon-containing oxide films and silicon-containing composite metal oxide films.

[0051] The composition for forming a silicon-containing film according to embodiments of the present invention contains a silicon precursor compound having a specific structure represented by Formula 1, and therefore can form a uniform silicon-containing film, more specifically a silicon-containing oxide film, with excellent coverage even on substrates with complex shapes.

[0052] In particular, Formula 1 above is a structure in which various types of amines and alkyl groups are bonded to Si, and especially R among the various types of bonds. 13 -Si-R 14 In R 13 and R 14 Since at least one of the components has a structure that is not hydrogen, it is very advantageous for forming stable films even at high temperatures of 600°C to 850°C.

[0053] In other words, in the silicon precursor compound represented by formula 1, firstly, the -NR in the above structure 11 R 12 The amine represented by has excellent surface reactivity and is advantageous for forming silicon-containing oxide films. Secondly, in the above structure, R 13 -Si-R 14 The part represented by R 13 and R 14 At least one of them is not hydrogen, i.e., R 13 and R 14 At least one of them preferably has an alkyl group or an alkenyl group, R13 and R 14 The presence of at least one alkyl group allows for a thermally stable bond between Si and C, preventing the silicon precursor from rapidly decomposing at high temperatures and enabling the formation of a stable film. This makes it suitable for three-dimensional NAND flash memory processes that require silicon-containing film properties at high temperatures. Thirdly, the structure contains three Si elements, and in SiO2ALD, it has a significantly larger GPC than conventionally known silicon precursor compounds, thus enabling the formation of a dense SiO2 film at high temperatures, making it suitable for three-dimensional NAND flash memory processes.

[0054] In detail, in Equation 1, R 11 and R 12 Each is independently selected from the group consisting of hydrogen and linear or branched C1-C4 alkyl groups, R 13 ~R 17 Each is independently selected from the group consisting of hydrogen, a linear or branched C1-C4 alkyl group, and a linear or branched C2-C6 alkenyl group, provided that R 13 and R 14 At least one of them is not hydrogen, R 15 ~R 17 At least one of them is not hydrogen.

[0055] The silicon precursor compound may include at least one compound selected from the group consisting of compounds represented by the following formulas 1-1 to 1-25.

[0056] [ka]

[0057] [ka]

[0058] [ka]

[0059]

change

[0060]

change

[0061]

change

[0062]

change

[0063]

change

[0064]

change

[0065]

change

[0066]

change

[0067]

change

[0068]

change

[0069]

change

[0070]

change

[0071]

change

[0072]

change

[0073]

change

[0074]

change

[0075]

change

[0076]

change

[0077]

change

[0078]

change

[0079]

change

[0080]

change

[0081] According to another embodiment of the present invention, the silicon precursor compound included in the composition for forming a silicon-containing oxide film may be a compound represented by formula 1-a.

[0082] [ka]

[0083] In formula 1-a, R 11 and R 12 Each of these is independently a linear or branched C1-C4 alkyl group. R 13 ~R 17 Each of these is independently selected from the group consisting of hydrogen, a linear or branched C1-C4 alkyl group, and a linear or branched C2-C6 alkenyl group. However, R 11 and R 12 At least one of them is not a methyl group, R 13 and R 14 At least one of them is not hydrogen, R 15 ~R 17 At least one of them is not hydrogen.

[0084] More specifically, the silicon precursor compound may include at least one selected from the group consisting of compounds represented by formulas 1-2 to 1-5, 1-7, 1-8, 1-10, 1-11, 1-13 to 1-20, and 1-22 to 1-25.

[0085] In other words, the silicon precursor compound may include at least one selected from the group consisting of compounds represented by the following formula.

[0086] [ka]

[0087] [ka]

[0088] [ka]

[0089] [ka]

[0090] [ka]

[0091] [ka]

[0092] [ka]

[0093] [ka]

[0094] [ka]

[0095] [ka]

[0096] According to embodiments of the present invention, when deposition is carried out by ALD using a composition for forming a silicon-containing film, the deposition rate (growth per cycle) (GPC) may be 1.5 to 3.0 Å / cycle with an ALD gas supply in the temperature range of 600°C to 850°C.

[0097] In detail, when deposition is carried out by ALD using a composition for forming a silicon-containing film, deposition rate (GPC) values ​​for ALD gas supply of, for example, 1.5–2.5 Å / cycle, 1.7–2.5 Å / cycle, or 1.75–2.25 Å / cycle can be achieved in the temperature range of 600°C to 850°C, for example at 800°C.

[0098] When a silicon-containing film is formed using a composition for forming a silicon-containing film according to an embodiment of the present invention, the composition can be controlled to achieve a desired film thickness and silicon content, and to form a film with excellent coverage and uniform thickness even on substrates having patterns (grooves) on the surface, porous substrates, plastic substrates, or substrates having complex shapes with three-dimensional structures, thereby providing a high-quality silicon-containing film.

[0099] Furthermore, in addition to silicon-containing films comprising at least one selected from the group consisting of silicon-containing oxide films and silicon-containing composite metal oxide films, at least one selected from the group consisting of silicon-containing nitride films, silicon-containing carbide films, and silicon-containing composite metal films can be efficiently formed on a substrate by CVD or ALD using a composition for forming silicon-containing films.

[0100] In particular, according to embodiments of the present invention, when a silicon-containing film comprising at least one selected from the group consisting of silicon-containing oxide films and silicon-containing composite metal oxide films is formed on a substrate by ALD using a composition for forming a silicon-containing film, there is a great advantage in that a film having a desired thickness can be obtained with a uniform thickness at high temperatures of 600°C or higher, the film shrinkage rate and etching rate at high temperatures are small, and a high-quality, pure silicon-containing film with few impurities can be formed.

[0101] [Method for preparing silicon precursor compounds] On the other hand, silicon precursor compounds represented by formula 1 can be prepared by various methods.

[0102] A method for preparing a silicon precursor compound (Formula 1) according to an embodiment of the present invention comprises subjecting an alkyldisilazane metal salt represented by Formula A to a halogen-amine substitution reaction with a dihalide silicon precursor compound represented by Formula B and a dialkylamine or dialkylamine metal salt represented by Formula C.

[0103] [ka]

[0104] In reaction scheme 1, M3 is an alkali metal and either Li or Na. R 15 ~R 17 Each is independently selected from the group consisting of hydrogen, a linear or branched C1-C4 alkyl group, and a linear or branched C2-C6 alkenyl group, provided that R 15 ~R 17 At least one of them is not hydrogen, X3 and X2 are, independently, a halogen element and Cl, Br, or I, respectively. R 13 and R 14 Each is independently selected from the group consisting of hydrogen, a linear or branched C1-C4 alkyl group, and a linear or branched C2-C6 alkenyl group, provided that R 13 and R 14 At least one of them is not hydrogen, R 11 and R 12 Each of these is independently hydrogen or a linear or branched C1-C4 alkyl group. M4 is selected from the group consisting of hydrogen, lithium, and sodium.

[0105] Referring to reaction scheme 1 above, 0.5 to 2 moles of silicon dihalide precursor compound (formula B) are added to an alkyldisilazane metal salt (formula A) at a low temperature (approximately -30°C to -5°C), and the silicon precursor compound (formula 1) is subjected to a first substitution reaction between the halide and the amine. Subsequently, 1 to 3 moles of dialkylamine or dialkylamine metal salt (formula C) are added to the resulting mixture at a low temperature (approximately -30°C to -5°C) to carry out a second substitution reaction between the halide and the amine. Next, the reaction by-products in the form of metal halide salts or dialkylamine halide salts contained in the reaction product are removed through filter paper (the obtained product may be purified) to obtain the silicon precursor compound represented by formula 1.

[0106] Here, R in reaction scheme 1 13 -Si-R 14 In the structure, R 13 and R 14 When both elements are alkyl groups, the rate of substitution reactions between the halide and the amine can be relatively slow. In such cases, a higher reaction temperature may be more advantageous, as the substitution reaction may proceed more easily.

[0107] The first and second halide-amine substitution reactions can be carried out at 0°C to 30°C, more specifically 20°C to 30°C, in a solvent at room temperature, for example, over a period of 2 to 30 hours.

[0108] Furthermore, the solvent may include one or more selected from the group consisting of alkanes having 5 to 8 carbon atoms, toluene, ethers, tetrahydrofuran, and mono-tetra-ethylene glycol dimethyl ether.

[0109] According to embodiments of the present invention, a composition for forming a silicon-containing film comprising a silicon precursor compound can be obtained using a silicon precursor compound.

[0110] [Silicon-containing film] According to embodiments of the present invention, a silicon-containing film is provided, which is formed by a method for forming a silicon-containing film.

[0111] Silicon-containing films may have a thickness ranging from several nanometers (nm) to several micrometers (μm), and can be applied in various ways depending on the intended purpose. Specifically, silicon-containing films can be formed within a thickness range of 1 nm to 500 nm.

[0112] A silicon-containing film can be formed on a substrate.

[0113] The base material is as described above.

[0114] The silicon-containing film may include at least one selected from the group consisting of silicon-containing oxide films and silicon-containing composite metal oxide films.

[0115] Furthermore, in addition to silicon-containing films comprising at least one selected from the group consisting of silicon-containing oxide films and silicon-containing composite metal oxide films, at least one selected from the group consisting of silicon-containing nitride films, silicon-containing carbide films, and silicon-containing composite metal films can be efficiently formed using a composition for forming silicon-containing films comprising a silicon precursor compound represented by Formula 1.

[0116] Furthermore, since the silicon-containing film is prepared by using a composition for forming a silicon-containing film that contains a silicon precursor compound having excellent thermal stability, the silicon-containing film is characterized by having a small shrinkage rate and a low wet etching rate (Å / s) even at high temperatures of 600°C or higher, for example, 600°C to 850°C.

[0117] In detail, the silicon-containing film has a shrinkage rate of 5.0% or less (S) as expressed by the following formula 1. 750 ) may have. Contraction rate (S 750 ,%)=(AB) / A×100 (Equation 1)

[0118] In Formula 1, A is the initial thickness (Å) of the silicon-containing film formed by ALD at 750°C, and B is the thickness (Å) of the silicon-containing film formed by ALD at 750°C and then left to stand for 60 minutes at 750°C in an argon (Ar) atmosphere.

[0119] The shrinkage rate (S of the silicon-containing film represented by Formula 1 750 ) may be, for example, 4.8% or less, 4.5% or less, 4.4% or less, 4.0% or less, 3.9% or less, 3.8% or less, 3.5% or less, 3.3% or less, 3.2% or less, 3.0% or less, 2.5% or less, 2.0% or less, 1.5% or less, or 1.0% or less.

[0120] When the silicon-containing film has a shrinkage rate (S that satisfies the above range 750 ), it may be advantageous for forming a uniform and dense silicon-containing film.

[0121] On the other hand, when the silicon-containing film is formed to a thickness of 500 Å by deposition at 750°C, and when the thickness of the silicon-containing film is measured using an ellipsometer before and after the silicon-containing film is exposed to an etching solution of 1% diluted hydrofluoric acid, represented by the following Formula 2 Silicon-containing film the wet etching rate (Å / s) may be 4.0 Å / s or less. Wet etching rate (Å / s) = Etching thickness change (ΔE, Å) / 30 s (Formula 2)

[0122] The etching thickness change (ΔE) may be represented by the following Formula 2-1. Etching thickness change (ΔE, Å) = E A - E B (Formula 2-1)

[0123] In Formula 2-1, E A is the initial thickness (Å) of the silicon-containing film formed by ALD at 750°C, and E B is the thickness (Å) of the silicon-containing film formed by ALD at 750°C after being etched for 30 seconds in a 1% diluted HF solution.

[0124] In equation 2, "s" means seconds.

[0125] The wet etching rate (Å / s) of the silicon-containing film represented by Equation 2 may be, for example, 3.8 Å / s or less, 3.5 Å / s or less, 3.2 Å / s or less, 3.0 Å / s or less, 2.8 Å / s or less, 2.5 Å / s or less, 2.45 Å / s or less, 2.4 Å / s or less, 2.2 Å / s or less, 2.1 Å / s or less, 2.0 Å / s or less, 1.5 Å / s or less, 1.0 Å / s or less, 0.5 Å / s or less, 0.1 Å / s or less, 0.05 Å / s or less, or 0.03 Å / s or less. More specifically, the wet etching rate (Å / s) of the silicon-containing film represented by Equation 2 can be 3.8 Å / s ~ 0.5 Å / s, 3.5 Å / s ~ 0.5 Å / s, 3.0 Å / s ~ 1.0 Å / s, 2.5 Å / s ~ 1.0 Å / s, or 2.1 Å / s ~ 1.0 Å / s.

[0126] If the silicon-containing film has a wet etching rate (Å / s) that satisfies the above range, it may be advantageous for forming a uniform and dense silicon-containing film.

[0127] Furthermore, silicon-containing films can exhibit excellent step coverage.

[0128] In detail, when a silicon-containing film is deposited on a substrate having a stepped hole pattern as shown in Figure 3, and then analyzed using a transmission electron microscope (TEM), the silicon-containing film has a step coverage (%) of, for example, 80% or more, 82% or more, 85% or more, 90% or more, 92% or more, 93% or more, 95% or more, or 96% or more.

[0129] When a silicon-containing film has a step coverage (%) that satisfies the above range, a high step ratio and precise thickness control are possible, and it can be advantageously used to manufacture various semiconductor devices, such as DRAM and 3D NAND flash memory. [Examples]

[0130] The present invention will be described in detail below with reference to examples. The following examples are for illustrative purposes only and the scope of the present invention is not limited thereto.

[0131] <Example 1> Dimethylamino-(tetramethyldisilyl)aminodimethylsilane ([{(CH3)2N}Si(CH3)2{N(SiHMe2)2}]) and preparation of a composition for forming a silicone-containing film containing the same. [ka]

[0132] Approximately 118.69 g (2.5 M, approximately 0.426 mol) of n-butyllithium hexane solution (n-BuLi in n-hexane) was mixed with approximately 1,000 ml of anhydrous hexane in a 2-liter round-bottom flask. Approximately 61.99 g (approximately 0.465 mol) of tetramethyldisilazane (1,1,3,3-tetramethyldisilazane) was added to the reaction system at approximately -20°C, and the temperature was then gradually raised to room temperature while stirring, followed by stirring for 4 hours. To the lithium (1,1,3,3-tetramethyldisilazane) salt thus formed at -20°C to -10°C, approximately 50 g (approximately 0.387 mol) of dichlorodimethylsilane was slowly added, and the temperature was then gradually raised to room temperature while stirring, followed by stirring for 4 hours. After 4 hours, approximately 41.91 g (approximately 0.930 mol) of dimethylamine was added to the reaction system at approximately -20°C. The temperature was then gradually raised to room temperature while stirring, and the mixture was stirred for 17 hours. Once the reaction was complete, the salt formed during the reaction was removed by filtration, and the solvent and volatile by-reactants were removed under reduced pressure to obtain 59.97 g (yield approximately 66%) of dimethylamino-(tetramethyldisilyl)aminodimethylsilane [{(CH3)2N}Si(CH3)2{N(SiHMe2)2}] as a colorless liquid compound represented by formula 1-1, which was used in a composition for film formation.

[0133] Boiling point: 72°C at 10 Torr (194.5°C at 760 Torr) 1H-NMR (C6D6): δ 0.221 (Si-CH * 3, s, 6H), δ 0.249, 0.241 (N-Si-CH * 3, d, 12H), δ 2.424 (N-CH * 3, s, 6H), δ 4.700 (N-Si-H * , m, 2H)

[0134] <Example 2> Preparation of ethylmethylamino-(tetramethyldisilyl)amino-dimethylsilane ([{(CH3CH2)(CH3)N}Si(CH3)2{N(SiHMe2)2}]) and a composition for forming a silicone-containing film comprising the same

Chemical Formula

[0135] About 62.6 g (yield about 65%) of ethylmethylamino-(tetramethyldisilyl)amino-dimethylsilane [{(CH3CH2)(CH3)N}Si(CH3)2{N(SiHMe2)2}] was obtained as a colorless liquid compound represented by Formula 1-2 in the same manner as in Example 1, except that ethylmethylamine was used instead of dimethylamine, and this was used in a composition for film formation.

[0136] Boiling point: 76°C at 10 Torr (199.4°C at 760 Torr) 1 H-NMR (C6D6): δ 0.235 (Si-CH * 3, s, 6H), δ 0.257, 0.248 (N-Si-CH * 3, d, 12H), δ 0.981 (N-CH2-CH * 3, t, 3H) δ 2.425 (N-CH * 3, s, 3H), δ 2.774, 2.756 (N-CH * 2-CH3, q, 2H), δ 4.722 (N-Si-H * , m, 2H)

[0137] <Example 3> Preparation of ethylmethylamino-(hexamethyldisilyl)aminodimethylsilane ([{(CH3CH2)(CH3)N}Si(CH3)2{N(SiMe3)2}]) and a composition for forming a silicone-containing film containing the same. [ka]

[0138] Approximately 71.81 g (yield approximately 67%) of ethylmethylamino-(hexamethyldisilyl)aminodimethylsilane [{(CH3CH2)(CH3)N}Si(CH3)2{N(SiMe3)2}] was obtained in the same manner as in Example 1, except that hexamethyldisilazane (1,1,1,3,3,3-hexamethyldisilazane) was used instead of tetramethyldisilazane (1,1,3,3-tetramethyldisilazane) as the colorless liquid compound represented by formula 1-4, and ethylmethylamine was used instead of dimethylamine. This was then used in a composition for film formation.

[0139] Boiling point: 35°C at 0.3 Torr (216.3°C at 760 Torr) 1 H-NMR (C6D6):δ0.236(Si-CH * 3,s,6H),δ0.273(N-Si-CH * 3,s,18H),δ0.968(N-CH2-CH * 3,t,3H),δ2.366(N-CH * 3,s,3H),δ2.722,2.704(N-CH * 2-CH3,q,2H)

[0140] <Example 4> Preparation of a composition for forming a silicone-containing film containing diethylamino-(hexamethyldisilyl)aminodimethylsilane ([{(CH3CH2)2N}Si(CH3)2{N(SiMe3)2}]) and the silicone-containing film containing the same. [ka]

[0141] 118.69 g (2.5 M, 0.426 mol) of n-butyllithium hexane solution (n-BuLi in n-hexane) was mixed with approximately 500 ml of anhydrous hexane in a 3 liter round-bottom flask. Approximately 75.03 g (approximately 0.465 mol) of hexamethyldisilazane (1,1,1,3,3,3-hexamethyldisilazane) was added to the reaction system at approximately -20°C, and the temperature was then gradually raised to room temperature while stirring, followed by stirring for 4 hours. Approximately 50 g (approximately 0.387 mol) of dichlorodimethylsilane was slowly added to the lithium (1,1,1,3,3,3-hexamethyldisilazane) salt solution thus formed at -20°C to -10°C, and the temperature was then gradually raised to room temperature while stirring, followed by stirring for 17 hours.

[0142] Approximately 118.69 g (2.5 M, approximately 0.426 mol) of n-butyllithium hexane solution (n-BuLi in n-hexane) was mixed with approximately 500 ml of anhydrous hexane in a 1 liter round-bottom flask. Approximately 34 g (approximately 0.465 mol) of diethylamine was added to the reaction system at approximately -20°C, and the temperature was then gradually raised to room temperature while stirring, followed by stirring for 4 hours. The lithium (diethylamine) salt solution thus formed was added to a 3 liter round-bottom flask at approximately -20°C, and the temperature was then gradually raised to room temperature while stirring, followed by stirring for 17 hours. After the reaction was complete, the salt formed during the reaction was removed by filtration, and the solvent and volatile by-reactants were removed under reduced pressure to obtain approximately 79.95 g (yield approximately 71%) of diethylamino-(hexamethyldisilyl)aminodimethylsilane [{(CH3CH2)2N}Si(CH3)2{N(SiMe3)2}] as a colorless liquid compound represented by formula 1-5, which was used in a composition for forming a film.

[0143] Boiling point: 45°C at 0.3 Torr (230.4°C at 760 Torr) 1 H-NMR (C6D6):δ0.262(Si-CH * 3,s,6H),δ0.283(N-Si-CH * 3,s,18H),δ0.976(N-CH2-CH *3,t,6H),δ2.806,2.788(N-CH * 2-CH3,q,4H)

[0144] <Example 5> Preparation of N,N-bis(dimethylsilyl)-1,1-dimethylsilanediamine ([(H2N)Si(CH3)2{N(SiHMe2)2}]) and a composition for forming a silicone-containing film containing the same. [ka]

[0145] Approximately 118.69 g (2.5 M, approximately 0.426 mol) of n-butyllithium hexane solution (n-BuLi in n-hexane) was mixed with approximately 1,000 ml of anhydrous hexane in a 3-liter round-bottom flask. Approximately 61.99 g (approximately 0.465 mol) of tetramethyldisilazane (1,1,3,3-tetramethyldisilazane) was added to the reaction system at approximately -20°C, and the temperature was then gradually raised to room temperature while stirring, followed by stirring for 4 hours. To the lithium (1,1,3,3-tetramethyldisilazane) salt thus formed at -20°C to -10°C, approximately 50 g (approximately 0.387 mol) of dichlorodimethylsilane was slowly added, and the temperature was then gradually raised to room temperature while stirring, followed by stirring for 4 hours. After 4 hours, approximately 32.99 g (approximately 1.937 moles) of ammonia gas was added to the reaction system at approximately -78°C. The temperature was then gradually raised to room temperature while stirring, and the mixture was stirred for 17 hours. Once the reaction was complete, the salt formed during the reaction was removed by filtration, and the solvent and volatile by-reactants were removed under reduced pressure to obtain 62.40 g (yield approximately 78%) of N,N-bis(dimethylsilyl)-1,1-dimethylsilanediamine [(H2N)Si(CH3)2{N(SiHMe2)2}] as a colorless liquid compound represented by formula 1-12, which was used in a composition for film formation.

[0146] Boiling point: 54°C at 10 Torr (172.3°C at 760 Torr) 1 H-NMR (C6D6):δ 0.202 (Si-CH *3,s,6H),δ0.269,0.261(N-Si-CH * 3,d,12H),δ0.373(NH * 2,m,2H),δ4.768(N-Si-H * ,m,2H)

[0147] Comparative Example 1 Tris(dimethylamide)silane (3DMAS or TDMAS) [SiH(NMe2)3] (manufactured by UP Chemical Co., Ltd.) was used.

[0148] Test Examples <Test Example 1> Analysis of deposition characteristics of a composition for forming a silicon-containing film, including a silicon precursor compound, at high temperatures. A silicon-containing film was formed by ALD using a composition for forming a silicon-containing film, each containing the silicon precursor compound of the example and comparative example, and ozone (O3) as the reaction gas.

[0149] First, the silicon substrate was immersed for 10 minutes in a piranha solution, which is a mixture of sulfuric acid (H2SO4) and hydrogen peroxide (H2O2) in a 4:1 ratio, and then removed. Next, it was immersed for 2 minutes in a diluted aqueous HF solution to form a new surface. Then, a silicon-containing oxide film was formed on the silicon substrate by ALD.

[0150] A composition for forming a silicon-containing film, including a silicon precursor compound, was placed in a stainless steel container. The composition for film formation was supplied in gaseous form to a reaction chamber at room temperature by flowing argon (Ar) carrier gas at a flow rate of approximately 200 sccm, while the reactor process pressure was set to 4 Torr.

[0151] To confirm the deposition characteristics of each silicon-containing oxide film, the gas supply cycle was repeated 100 times. In this cycle, the composition for film formation was supplied in gaseous form for approximately 3 seconds; argon (Ar) gas was supplied for approximately 10 seconds to remove any remaining composition (gas) in the reactor; ozone (O3) was supplied as a reaction gas for approximately 5 seconds; and argon (Ar) gas was supplied for approximately 10 seconds to remove any remaining ozone (O3) in the reactor.

[0152] The thickness of each oxide film formed using the silicon-containing films prepared by the methods of the examples and comparative examples was measured using an elliptic polarimeter (M-2000, JAWoollam).

[0153] Subsequently, the measured thickness was divided by the number of gas supply cycles (100) to calculate the ALD gas supply deposition rate (GPC).

[0154] In detail, the deposition rate (GPC) of ALD gas supply was measured for temperatures ranging from 600°C to 850°C (process temperature). The results are shown in Figure 1 and Table 1.

[0155] [Table 1]

[0156] As can be seen from Table 1 and Figure 1, when ALD was performed at high temperatures of 600°C or higher, the GPC was constant at relatively high temperatures of 600°C to 850°C compared to when a composition for forming a silicone-containing film containing the silicone compound of Comparative Example 1 was used.

[0157] In detail, when using the composition for forming a silicon-containing film, which contains the silicon compound of Comparative Example 1, the film deposition rate (GPC) with ALD gas supply increased from approximately 700°C. In contrast, when using the compositions for forming a silicon-containing film, which contain the respective silicon compounds of Examples 1, 2, 3, 4, and 5, the film deposition rate (GPC) with ALD gas supply remained constant even at high temperatures of 800°C to 850°C. From the above, it was confirmed that the compositions for forming a silicon-containing film, which contain the silicone compounds of the examples of the present invention, achieve a constant GPC at high temperatures of 600°C to 850°C, exhibit self-regulating film growth characteristics, and are therefore suitable precursors for ALD processes at high temperatures.

[0158] <Test Example 2> Analysis of the physical properties of silicon-containing oxide films deposited at high temperatures. Using compositions for forming silicon-containing films, each containing the silicon compound of Examples 1, 2, 3, 4, and 5 and Comparative Example 1, SiO2 films of the same thickness were formed on a flat wafer at 750°C while adjusting the ALD gas supply cycle. Their physical and chemical properties were analyzed.

[0159] In detail, the shrinkage rate and wet etching rate (WER, Å / s) of the SiO2 film were measured. The thickness of the SiO2 film was measured using an elliptic polarimeter (M-2000, JAWoollam).

[0160] As shown in Table 2, by adjusting the ALD gas supply cycle, the thickness of a silicon-containing film (SiO2 film) with an initial thickness of approximately 100 Å formed on a flat wafer at 750°C was compared with the thickness of a silicon-containing film (SiO2 film) annealed in an argon (Ar) atmosphere at 750°C for 60 minutes, and the shrinkage rate was calculated using Equation 1. Contraction rate (S 750 ,%)=(AB) / A×100 (Equation 1)

[0161] In Equation 1, A is the initial thickness (Å) of the silicon-containing film formed by ALD at 750°C, and B is the thickness (Å) of the silicon-containing film after it has been formed by ALD at 750°C and left to stand in an argon (Ar) atmosphere at 750°C for 60 minutes.

[0162] The results are shown in Table 2.

[0163] [Table 2]

[0164] As can be seen from Table 2 above, the shrinkage rates of the silicon-containing oxide films (SiO2 films) deposited using the silicon-containing film-forming compositions of Examples 1, 2, 3, 4, and 5 were 3.87%, 3.39%, 2.71%, 4.40%, and 3.98%, respectively. In contrast, the shrinkage rate of the silicon-containing oxide film deposited using the silicon-containing film-forming composition of Comparative Example 1 was 6.40%. Thus, the silicon-containing oxide films deposited using the silicon-containing film-forming compositions of Examples 1, 2, 3, 4, and 5 had smaller shrinkage rates than the silicon-containing oxide film deposited using the silicon-containing film-forming composition of Comparative Example 1.

[0165] On the other hand, by adjusting the ALD gas supply cycle shown in Table 4 below, a silicon-containing film (SiO2 film) with an initial thickness of approximately 500 Å, formed on a flat wafer at 750°C, was etched in a 1% diluted HF solution for 30 seconds. The change in thickness was measured, and the wet etching rate (WER, Å / s) was calculated using Equation 2. Wet etching rate (Å / s) = Etching thickness change (ΔE, Å) / 30s (Equation 2)

[0166] The change in etching thickness (ΔE) can be expressed by equation 2-1. Etching thickness change (ΔE, Å) = E A -E B (Formula 2-1)

[0167] In formula 2-1, E A This is the initial thickness (Å) of the silicon-containing film formed by ALD at 750°C, and E B This is the thickness (Å) of the silicon-containing film after it has been formed by ALD at 750°C and etched in a 1% diluted HF solution for 30 seconds.

[0168] In equation 2, "s" means seconds.

[0169] The results are shown in Table 3.

[0170] [Table 3]

[0171] As can be seen from Table 3 above, the wet etching rates of the silicon-containing oxide films (SiO2 films) deposited using the silicon-containing film formation compositions of Examples 2, 3, and 4 were 2.45 Å / s, 2.45 Å / s, and 2.07 Å / s, respectively. In contrast, the wet etching rate of the silicon-containing oxide film deposited using the silicon-containing film formation composition of Comparative Example 1 was 2.90 Å / s. The silicon-containing oxide films deposited using the silicon-containing film formation compositions of Examples 2, 3, and 4 were reduced in thickness.

[0172] Meanwhile, to identify impurities within the silicon-containing oxide layer, secondary ion mass spectrometry (SIMS) was performed on the silicon-containing oxide film.

[0173] Figure 2 is a graph showing the results of secondary ion mass spectrometry (SIMS) of silicon-containing oxide films deposited at a temperature of 750°C using the compositions for forming silicon-containing films of Examples 1, 2, 3, 4, and 5 of the present invention and Comparative Example 1.

[0174] To confirm impurities in the silicon-containing oxide layer deposited using the compositions for forming the respective silicon-containing films of Examples 1, 2, 3, 4 and 5 and Comparative Example 1, the silicon-containing oxide film deposited to a thickness of about 100 Å was analyzed for carbon (C) content by SIMS.

[0175] As a result, the carbon content was reduced by about 80% in Example 1, about 81% in Example 2, about 76% in Example 3, about 81% in Example 4, and about 83% in Example 5, as compared with Comparative Example 1, indicating that a pure silicon-containing oxide film having a carbon content of less than 100 counts was formed.

[0176] Figure 3 is a transmission electron microscope (TEM) image of a silicon-containing oxide film formed on a wafer having a deep pattern by ALD using ozone and the compositions for depositing the respective silicon-containing films of Example 2 of the present invention and Comparative Example 1 at 750°C. Table 4 shows the thickness of the silicon-containing oxide film measured at the portion shown in Figure 3.

[0177] [Table 4]

[0178] As can be seen from Table 4, when the compositions for forming the respective silicon-containing films of Example 2 and Comparative Example 1 were deposited on a stepped substrate and then analyzed using TEM, the step coverage of the silicon-containing oxide film deposited using the composition for forming the silicon-containing film of Example 2 was 93.4%, while the step coverage of the silicon-containing oxide film deposited using the composition for forming the silicon-containing film of Comparative Example 1 was 78.1%. The silicon-containing oxide film deposited using the composition for forming the silicon-containing film of Example 2 had significantly superior step coverage as compared with the silicon-containing oxide film deposited using the composition for forming the silicon-containing film of Comparative Example 1.

[0179] In short, according to the method for forming a silicon-containing film using a composition for forming a silicon-containing film containing a silicon precursor compound according to an embodiment of the present invention, it was possible to easily deposit a silicon-containing film by ALD, accurately control the film thickness and composition, and form a uniform film with excellent coverage even on a substrate with a complex shape.

[0180] In particular, according to the method for forming a silicon-containing film using a composition for forming a silicon-containing film containing a silicon precursor compound according to the present invention, a film of a desired thickness can be obtained even at high temperatures of 600°C to 850°C during deposition. The silicon-containing oxide film obtained in this way had significantly improved physical properties, such as step coverage, shrinkage rate, and wet etching rate, compared to the silicon-containing oxide film obtained using the composition for forming a silicon-containing film containing a silicon precursor compound in Comparative Example 1.

Claims

1. A method for forming a silicon-containing film, comprising depositing a silicon-containing film onto a substrate by chemical vapor deposition (CVD) or atomic layer deposition (ALD) using a composition for forming a silicon-containing film comprising a silicon precursor compound represented by formula 1, A method for forming a silicon-containing film, wherein the silicon-containing film comprises at least one selected from the group consisting of a silicon-containing oxide film and a silicon-containing composite metal oxide film, and the deposition is carried out at a temperature of 600°C or higher. 【Chemistry 1】 [In formula 1, R 11 and R 12 These are, independently, hydrogen and linear or branched carbon atoms. 1 ~C 4 Selected from the group consisting of alkyl groups, R 13 to R 17 each independently represent hydrogen, a linear or branched C 1 to C 4 alkyl group, and a linear or branched C 2 to C 6 alkenyl group selected from the group consisting of, provided that at least one of R 13 and R 14 is not hydrogen, and at least one of R 15 to R 17 is not hydrogen.]

2. A method for forming a silicon-containing film according to claim 1, wherein the silicon precursor compound comprises at least one selected from the group consisting of compounds represented by the following formula. 【Chemistry 2】 【Transformation 3】 【Chemistry 4】 【Transformation 5】 【Transformation 6】 【Transformation 7】 【Transformation 8】 【Chemistry 9】 【Chemistry 10】 【Chemistry 11】 【Chemistry 12】 【Chemistry 13】 【Chemistry 14】

3. A method for forming a silicon-containing film according to claim 1, wherein the deposition is carried out in a temperature range of 600°C to 850°C.

4. A method for forming a silicon-containing film according to claim 1, wherein the deposition is carried out by atomic layer deposition (ALD) using the composition for forming a silicon-containing film, and the deposition rate (GPC) is 1.5 to 3.0 Å / cycle with an ALD gas supply in the temperature range of 600°C to 850°C.

5. In the aforementioned deposit, water vapor (H 2 O), oxygen (O 2 ), oxygen plasma (O 2 Plasma), Nitrogen oxide (NO, N) 2 O), Nitrogen oxide plasma ( 2 O plasma), nitrate oxygen ( 2 O 2 ), hydrogen peroxide (H 2 O 2 ), and ozone (O 3 A method for forming a silicon-containing film according to claim 1, wherein at least one selected from the group consisting of ) is used.

6. A method for forming a silicon-containing film according to claim 1, wherein the silicon-containing film is formed within a thickness range of 1 nm to 500 nm.

7. A method for forming a silicon-containing film according to claim 1, wherein the silicon-containing film is formed on a substrate having at least one surface irregularity having an aspect ratio of 1 or more and a width of 1 μm or less.

8. A method for forming a silicon-containing film according to claim 1, comprising supplying the silicon precursor compound to a reaction chamber using at least one method selected from the group consisting of a bubbling method, a liquid delivery system (LDS) method, a vapor flow control (VFC) method, and a bypass method.

9. A method for forming a silicon-containing film according to claim 8, wherein the silicon precursor compound is supplied to the reaction chamber using a carrier gas or diluent gas at a temperature range of room temperature to 150°C and at a rate of 0.1 to 10 Torr.

10. A method for forming a silicon-containing film according to claim 1, wherein thermal energy or plasma is used during the deposition, or a bias is applied to the substrate.

11. A method for forming a silicon-containing film according to claim 1, wherein the shrinkage rate (S 750) of the silicon-containing film, represented by the following formula 1, is 5.0% or less. Shrinkage rate (S 750, %) = (A - B) / A × 100 (Equation 1) [In Equation 1, A is the initial thickness (Å) of the silicon-containing film formed by ALD at 750°C, and B is the thickness (Å) of the silicon-containing film after it has been formed by ALD at 750°C and left to stand in an argon (Ar) atmosphere at 750°C for 60 minutes.]

12. A method for forming a silicon-containing film according to Claim 1, wherein the silicon-containing film is formed to a thickness of 500 Å by deposition at 750°C, and when the thickness of the silicon-containing film is measured using an elliptic polarimeter before and after exposure to a 1% diluted hydrofluoric acid etching solution, the wet etching rate (Å / s) of the silicon-containing film, represented by the following formula 2, is 4.0 Å / s or less. Wet etching rate (Å / s) = Etching thickness change (ΔE, Å) / 30 s (Equation 2) [In Equation 2, the change in etching thickness (ΔE) is expressed by Equation 2-1 below.] Etching thickness change (ΔE, Å) = E A - E B (Equation 2-1) [In Equation 2-1, E A is the initial thickness (Å) of the silicon-containing film formed by ALD at 750°C, and E B is the thickness (Å) of the silicon-containing film after it has been formed by ALD at 750°C and etched in a 1% diluted HF solution for 30 seconds.]

13. A composition for forming a silicon-containing film, comprising a silicon precursor compound represented by formula 1, It is used to deposit silicon-containing films by chemical vapor deposition (CVD) or atomic layer deposition (ALD) at temperatures of 600°C or higher. A composition wherein the silicon-containing film comprises at least one selected from the group consisting of a silicon-containing oxide film and a silicon-containing composite metal oxide film. 【Chemistry 15】 [In formula 1, R 11 and R 12 These are, independently, hydrogen and linear or branched carbon atoms. 1 ~C 4 Selected from the group consisting of alkyl groups, R 13 ~R 17 Each of these independently consists of hydrogen, a linear or branched carbon atom. 1 ~C 4 Alkyl groups, and linear or branched C molecules. 2 ~C 6 Selected from the group consisting of alkenyl groups, where R 13 and R 14 At least one of them is not hydrogen, R 15 ~R 17 At least one of them is not hydrogen.

14. The composition for forming a silicon-containing film according to claim 13, wherein the silicon precursor compound comprises at least one selected from the group consisting of compounds represented by the following formula. 【Chemistry 16】 【Chemistry 17】 [Chemistry 18] 【Chemistry 19】 【Chemistry 20】 【Chemistry 21】 【Chemistry 22】 【Chemistry 23】 【Chemistry 24】 【Chemistry 25】

Citation Information

Patent Citations

  • High temperature atomic layer deposition of silicon oxide thin films

    JP2013236073A

  • Amine-substituted trisilylamine compound and tridisilylamine compound

    JP2016537305A

  • Novel aminosilylamine compound and method for producing an insulating film containing a Si-N bond using an atomic layer deposition method

    JP2017518286A

  • Compositions and methods of using same for deposition of silicon-containing films

    JP2017533589A

  • method for forming silicon film by Atomic Layer Deposition

    KR100734393B1