Grinding composition
The polishing composition with silica particles, a basic compound, and specific water-soluble polymers addresses defects and scratches on semiconductor substrates by balancing dispersibility and substrate protection, resulting in improved surface quality.
Patent Information
- Application Number
- JP2024511877
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-20
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Existing polishing compositions for semiconductor substrates, such as silicon wafers, fail to adequately reduce defects like LPD-N (Light Point Defect Non-cleanable) and minute scratches (haze lines) despite using silica particles, basic compounds, and water-soluble polymers.
A polishing composition comprising silica particles, a basic compound, a first water-soluble polymer (polyvinyl alcohol-based), a second water-soluble polymer, and water, with a specific zeta potential and etching rate product that balances dispersibility and substrate protection, reducing defects and scratches.
The composition achieves a high-quality polished surface with reduced defects and scratches by optimizing dispersibility and substrate protection performance.
Smart Images

Figure 0007954703000001 
Figure 0007954703000002
Abstract
Description
[Technical Field]
[0001] The present invention relates to an abrasive composition. This application claims priority under Japanese Patent Application No. 2022-58671, filed on 31 March 2022, the entire contents of which are incorporated herein by reference. [Background technology]
[0002] Precision polishing is performed on the surfaces of materials such as metals, metalloids, nonmetals, and their oxides using polishing compositions. For example, the surface of a silicon wafer used as a component of a semiconductor device is generally finished to a high-quality mirror surface through a lapping process (rough polishing process) and a polishing process (precision polishing process). The above polishing process typically includes a preliminary polishing process and a final polishing process. Patent documents 1 to 3 are technical documents relating to polishing compositions mainly used for polishing semiconductor substrates such as silicon wafers. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent No. 6185432 [Patent Document 2] Japanese Patent No. 6348927 [Patent Document 3] Japanese Patent No. 6232243 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] Polishing compositions are used that possess the ability to efficiently polish the object to be polished. For example, in polishing semiconductor substrates such as silicon wafers and other substrates, mechanical polishing action by abrasive grains and chemical polishing action (alkaline etching) by basic compounds are utilized, and high processing power can be achieved through these actions. Polishing compositions with high processing power are preferable because they can improve manufacturing efficiency and cost-effectiveness. In such polishing, by using silica particles as abrasive grains, a polished surface with good quality can be efficiently achieved.
[0005] Furthermore, polishing compositions used for polishing the above-mentioned substrates, such as polishing compositions used in the finishing polishing process (particularly the finishing polishing process for semiconductor substrates such as silicon wafers and other substrates), are required to achieve a high-quality surface after polishing. Improvement of the surface quality of the polished surface can be achieved by methods such as including a water-soluble polymer in the polishing composition and protecting the substrate from alkaline etching with the water-soluble polymer. For example, Patent Documents 1 to 3 disclose polishing compositions containing silica particles, basic compounds, and water-soluble polymers. However, even with such polishing compositions containing abrasive grains, basic compounds, and water-soluble polymers, there was still room for improvement in reducing defects (e.g., LPD-N (Light Point Defect Non-cleanable)) and minute scratches (e.g., haze lines) to improve the surface quality after polishing.
[0006] Therefore, the present invention aims to provide a polishing composition that can achieve a high-quality surface. [Means for solving the problem]
[0007] This specification provides an abrasive composition comprising silica particles (A) as abrasive grains, a basic compound (B), a first water-soluble polymer (C1), a second water-soluble polymer (C2), and water (D). Here, the first water-soluble polymer (C1) is a polyvinyl alcohol-based polymer. The etching rate ER of the abrasive composition is [nm / h The product (ER × ζ) of ] and the zeta potential ζ [mV] of the above polishing composition is -900 pmV / h Above -90 pmV / h The following applies:
[0008] Here, the etching rate ER of the above polishing composition [ nm / h ] is determined based on the following etching rate measurements. [Etching rate measurement] (1) Prepare the above polishing composition as a chemical solution LE for etching rate measurement. (2) Prepare a silicon single crystal substrate (rectangular in shape, 6 cm long, 3 cm wide, and 775 μm thick) by immersing it for 1 minute in a washing solution of NH4OH (29%):H2O2 (31%):deionized water (DIW) = 2:5.3:48 (volume ratio) at 25°C, and then immersing it for 30 seconds in a hydrogen fluoride (HF) aqueous solution (5%) at 25°C, and measure its mass W0. (3) Immerse the silicon single crystal substrate in the above chemical solution LE at 25°C for 48 hours. (4) Remove the silicon single crystal substrate from the above chemical solution LE and wash it for 10 seconds at 25°C with a washing solution of NH4OH (29%):H2O2 (31%):deionized water (DIW) = 1:1:8 (volume ratio). (5) Measure the mass W1 of the silicon single crystal substrate after cleaning. (6) The difference between W0 and W1 and the specific gravity of the silicon single crystal substrate gives the etching rate [ nm / h [As described in ].
[0009] The zeta potential ζ of the polishing composition can serve as an indicator of the dispersibility of the particles contained in the polishing composition. Furthermore, the etching rate ER of the polishing composition can serve as an indicator of the performance of the polishing composition in protecting the surface to be polished from alkaline etching (hereinafter also referred to as "substrate protection performance"). The polishing composition disclosed herein has a product of zeta potential ζ and etching rate ER (ζ × ER) within the above range, so the dispersibility and substrate protection performance of the polishing composition are well controlled in a balanced manner, and it tends to be possible to achieve a high-quality surface with reduced defects (e.g., LPD-N) and minute scratches (e.g., haze lines) after polishing.
[0010] In some embodiments, the first water-soluble polymer (C1) is one or more selected from the group consisting of unmodified polyvinyl alcohol with a degree of saponification of 70% or more; acetalized polyvinyl alcohol polymers; and polyvinyl alcohol polymers containing repeating units derived from alkyl vinyl ethers. When the above polymer is used as the first water-soluble polymer (C1), the surface quality after polishing tends to improve further.
[0011] In some embodiments, the content of the first water-soluble polymer (C1) is 0.5 parts by weight or more and 10 parts by weight or less per 100 parts by weight of the abrasive grains. With such a composition, the effects of the technology disclosed herein can be preferably realized.
[0012] In some embodiments, the second water-soluble polymer (C2) is one or more selected from the group consisting of polyvinyl alcohol-based polymers having a different chemical structure from the first water-soluble polymer (C1); polymers containing nitrogen atoms; and polymers containing (meth)acrylic acid units. When such a second water-soluble polymer (C2) is used together with the first water-soluble polymer (C1), the surface quality after polishing tends to be further improved. In some embodiments, the polymer containing the nitrogen atom is a polymer containing a chain-like amide having an N-(meth)acryloyl group as a monomer unit. When such a polymer is used together with the first water-soluble polymer (C1), the surface quality after polishing tends to be further improved.
[0013] In some embodiments, the content of the second water-soluble polymer (C2) is 0.5 parts by weight or more and 10 parts by weight or less per 100 parts by weight of the abrasive grains. With such a composition, the effects of the technology disclosed herein can be preferably realized.
[0014] In some embodiments, the polishing composition further comprises a surfactant (E). With such a configuration, the surface quality after polishing tends to be further improved. In one preferred embodiment, the surfactant (E) is a nonionic surfactant.
[0015] The polishing compositions disclosed herein can be preferably used for polishing surfaces made of silicon material. By polishing a surface made of silicon material using the above-mentioned polishing compositions, a high-quality surface made of silicon material can be efficiently achieved.
[0016] The polishing compositions disclosed herein may be concentrated liquids. The polishing compositions disclosed herein may be manufactured, distributed, and stored as concentrated liquids. [Modes for carrying out the invention]
[0017] Preferred embodiments of the present invention will be described below. Matters other than those specifically mentioned herein that are necessary for carrying out the present invention can be understood as design matters for those skilled in the art based on the prior art. The present invention can be carried out based on the contents disclosed herein and common technical knowledge in the art.
[0018] <Properties of abrasive compositions> The polishing compositions disclosed herein are characterized by their zeta potential and etching rate. Here, the zeta potential of the polishing composition refers to the zeta potential measured for the polishing composition using a zeta potential measuring device. More specifically, it refers to the zeta potential measured for the particles contained in the polishing composition. The zeta potential of the polishing composition can serve as an indicator of the dispersibility of the particles contained in the polishing composition. For example, a larger absolute value of the zeta potential of a polishing composition with a negative zeta potential means that the electrostatic repulsion of the particles containing abrasive grains in the polishing composition increases, and tends to indicate improved dispersibility of the polishing composition.
[0019] Furthermore, the etching rate of the polishing composition indicates the degree to which the surface of the object to be polished is chemically corroded (etched) by the basic compounds, etc., contained in the polishing composition. Specifically, the etching rate of the polishing composition is determined based on the following etching rate measurement. Here, the water-soluble polymers, etc., contained in the polishing composition tend to adsorb to the surface of the object to be polished and have the effect of protecting the surface of the object to be polished from etching. Therefore, the etching rate of the polishing composition can serve as an indicator of the performance of the polishing composition in suppressing the phenomenon of the surface of the object to be polished being etched by basic compounds, etc., by the water-soluble polymers, etc. contained in the polishing composition, under conditions excluding the effect of mechanical action by abrasive grains, i.e., the performance of the polishing composition in protecting the surface of the object to be polished (hereinafter also referred to as substrate protection performance). In the examples described later, the etching rate of the polishing composition will also be determined based on the following etching rate measurement.
[0020] [Etching rate measurement] (1) Prepare the polishing composition as the etching rate measuring chemical solution LE. (2) Prepare a silicon single crystal substrate (rectangular in shape, 6 cm long, 3 cm wide, and 775 μm thick) by immersing it for 1 minute in a washing solution of NH4OH (29%):H2O2 (31%):deionized water (DIW) = 2:5.3:48 (volume ratio) at 25°C, and then immersing it for 30 seconds in a hydrogen fluoride (HF) aqueous solution (5%) at 25°C, and measure its mass W0. (3) Immerse the silicon single crystal substrate in the above chemical solution LE at 25°C for 48 hours. (4) Remove the silicon single crystal substrate from the above chemical solution LE and wash it for 10 seconds at 25°C with a washing solution of NH4OH (29%):H2O2 (31%):deionized water (DIW) = 1:1:8 (volume ratio). (5) Measure the mass W1 of the silicon single crystal substrate after cleaning. (6) The difference between W0 and W1 and the specific gravity of the silicon single crystal substrate gives the etching rate [ nm / h [As described in ].
[0021] The polishing compositions disclosed herein have a predetermined product of zeta potential and etching rate. The fact that the product of zeta potential and etching rate of the polishing composition is within a predetermined range indicates that the dispersibility of the polishing composition and the substrate protection performance of the polishing composition tend to be controlled and within a predetermined range. Polishing compositions with such a configuration tend to improve the surface quality after polishing.
[0022] According to one aspect of the technology disclosed herein, the zeta potential ζ [mV] of the polishing composition and the etching rate ER [ nm / h The product of ] (ER × ζ) is -900 pmV / h Above -90 pmV / h The following applies: When the product of the zeta potential and etching rate is within the above range, the dispersibility and substrate protection performance of the polishing composition are well-balanced, which tends to result in a high-quality surface with reduced defects (e.g., LPD-N) and minute scratches (e.g., haze lines) after polishing.
[0023] From the perspective of improving surface quality, such as reducing LPD-N and haze lines after polishing, the zeta potential ζ [mV] of the polishing composition and the etching rate ER [ nm / h The product of ] (ER × ζ) is -870 pmV / h It is more preferable that the above is true. pmV / h It may be greater than or equal to -500 pmV / hIt may be greater than or equal to -400 pmV / h Anything above that is also acceptable, -350 pmV / h The above is also acceptable. Similarly, from the viewpoint of improving surface quality, the above ER × ζ is -100 pmV / h The following is also acceptable: -105 pmV / h The following is also acceptable: -115 pmV / h The following is more preferable. In some embodiments, the above ER × ζ is -200 pmV / h It may also be less than -250 pmV / h It may also be less than -300 pmV / h The following is also acceptable: -400 pmV / h The following is also acceptable.
[0024] The zeta potential ζ of the polishing composition is not particularly limited, as long as its product with the etching rate ER is within a specific range. The zeta potential ζ is usually less than 0 mV, and from the viewpoint of the dispersibility of the polishing composition and the surface quality of the polished surface, -5 mV or less is appropriate, preferably -10 mV or less, more preferably -20 mV or less, even more preferably -25 mV or less, and particularly preferably -30 mV or less. In some embodiments, the zeta potential ζ may be -35 mV or less, -38 mV or less, or -45 mV or less. From the viewpoint of improving the polishing rate, it is preferably -80 mV or more, more preferably -70 mV or more, even more preferably -60 mV or more, and may be -45 mV or more. The zeta potential ζ of the polishing composition can be set by the type and content of abrasive grains, the type, molecular weight and content of water-soluble polymers, the type and content of basic compounds, the presence or absence of other additive components (surfactants, etc.), their type and content, pH, etc.
[0025] The zeta potential of the polishing composition can be measured using a known or conventional zeta potential measuring device. Specifically, it can be measured by the method described in the examples below.
[0026] The etching rate ER of the polishing composition is not particularly limited as long as the product with the zeta potential ζ is within a specific range. Based on the above etching rate measurement, the etching rate ER of the polishing composition is usually 25 from the viewpoint of the surface quality of the polished surface, etc. nm / h It is appropriate, preferably 20, to be less than or equal to the following. nm / h More preferably 18 nm / h The following applies. In some embodiments, the etching rate ER is 13 nm / h The following may also be the case: 10 nm / h The following is also acceptable: 8.5 nm / h The following is also acceptable: 5 nm / h The following is also acceptable. From the standpoint of polishing rate, the above etching rate ER is usually 2 nm / h It is appropriate for the above to be the case, preferably 3 nm / h More preferably 4 nm / h That concludes the explanation. In some embodiments, the etching rate ER is 7 nm / h It may be more than 8 nm / h The above is also acceptable, 9 nm / h The above is also acceptable, 10 nm / h The above is also acceptable. The etching rate ER of the polishing composition can be set by the type, molecular weight, and content of the water-soluble polymer, the type and content of the basic compound, the presence or absence of other additives (surfactants, etc.), their type and content, pH, etc.
[0027] <Abrasive grains> The polishing composition disclosed herein contains silica particles as abrasive grains. The silica particles, as abrasive grains, mechanically polish the surface of the object to be polished. By including abrasive grains in the polishing composition, the polishing rate can be improved based on the mechanical polishing action caused by the inclusion of abrasive grains. Furthermore, in polishing compositions that can be used for polishing objects having a silicon surface, such as silicon wafers described later (e.g., finish polishing), the use of silica particles as abrasive grains is particularly significant.
[0028] Specific examples of silica particles include colloidal silica, fumed silica, and precipitated silica. Silica particles can be used individually or in combination of two or more types. Colloidal silica is particularly preferred because it easily yields a polished surface with excellent surface quality after polishing. As colloidal silica, for example, colloidal silica produced from water glass (sodium silicate) by ion exchange or colloidal silica produced by alkoxide method (colloidal silica produced by hydrolysis condensation reaction of alkoxysilane) can be preferably used. Colloidal silica can be used individually or in combination of two or more types.
[0029] The true specific gravity of the silica constituting the silica particles is preferably 1.5 or higher, more preferably 1.6 or higher, and even more preferably 1.7 or higher. There is no particular upper limit to the true specific gravity of silica, but it is typically 2.3 or lower, for example, 2.2 or lower. The true specific gravity of the silica particles can be measured using a liquid displacement method with ethanol as the displacement solution.
[0030] The average primary particle diameter of the abrasive grains (typically silica particles) is not particularly limited, but from the viewpoint of polishing rate, it is preferably 5 nm or more, more preferably 10 nm or more. From the viewpoint of obtaining a higher polishing effect (e.g., effects such as haze reduction and defect removal), the above average primary particle diameter is preferably 15 nm or more, and more preferably 20 nm or more (e.g., greater than 20 nm). Also, from the viewpoint of preventing scratches, the average primary particle diameter of the abrasive grains is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 45 nm or less. From the viewpoint of making it easier to obtain a surface with lower haze, in some embodiments, the average primary particle diameter of the abrasive grains may be 43 nm or less, less than 40 nm, less than 38 nm, less than 35 nm, less than 32 nm, or less than 30 nm.
[0031] In this specification, the average primary particle diameter is calculated from the specific surface area (BET value) measured by the BET method as follows: Average primary particle diameter (nm) = 6000 / (True density (g / cm³) 3) × BET value (m 2 This refers to the particle size (BET particle size) calculated by the formula ( / g). The specific surface area can be measured, for example, using a surface area measuring device manufactured by Micromeritex, product name "Flow Sorb II 2300".
[0032] The average secondary particle diameter of the abrasive grains (typically silica particles) is not particularly limited and can be appropriately selected from a range of, for example, 15 nm to 300 nm. From the viewpoint of improving the polishing rate, the average secondary particle diameter is preferably 30 nm or more, and more preferably 35 nm or more. In some embodiments, the average secondary particle diameter may be, for example, 40 nm or more, 42 nm or more, and preferably 44 nm or more. Also, the average secondary particle diameter is usually advantageous to be 250 nm or less, preferably 200 nm or less, and more preferably 150 nm or less. In some preferred embodiments, the average secondary particle diameter is 120 nm or less, more preferably 100 nm or less, even more preferably 70 nm or less, for example 60 nm or less, or 50 nm or less.
[0033] In this specification, the average secondary particle diameter refers to the particle diameter (volume-average particle diameter) measured by dynamic light scattering. The average secondary particle diameter of abrasive grains can be measured, for example, by dynamic light scattering using the "NanoTrack UPA-UT151" product manufactured by Nikkiso Co., Ltd.
[0034] The shape (outer form) of silica particles may be spherical or non-spherical. Specific examples of non-spherical particles include peanut-shaped (i.e., the shape of a peanut shell), cocoon-shaped, konpeito (sugar candy)-shaped, and rugby ball-shaped particles. For example, silica particles in which most are peanut-shaped or cocoon-shaped may be preferably used.
[0035] While not particularly limited, the average aspect ratio of the major axis to minor axis of the silica particles is, in principle, 1.0 or higher, preferably 1.05 or higher, more preferably 1.1 or higher, and may also be 1.2 or higher. A higher polishing rate can be achieved by increasing the average aspect ratio. Furthermore, from the viewpoint of reducing scratches, the average aspect ratio of the silica particles is preferably 3.0 or lower, more preferably 2.0 or lower, even more preferably 1.5 or lower, and may also be 1.4 or lower.
[0036] The shape (outer shape) and average aspect ratio of silica particles can be determined, for example, by electron microscopy observation. A specific procedure for determining the average aspect ratio is to use a scanning electron microscope (SEM) to draw the smallest rectangle circumscribing each particle image for a predetermined number of silica particles (e.g., 200 particles) whose individual particle shapes can be recognized. Then, for each rectangle drawn for each particle image, the ratio of the major axis to the minor axis (aspect ratio) is calculated by dividing the length of the major side (major axis) by the length of the minor side (minor axis). The average aspect ratio can be obtained by taking the arithmetic mean of the aspect ratios of the predetermined number of particles.
[0037] The polishing compositions disclosed herein may contain abrasive particles other than silica particles (hereinafter also referred to as "non-silica abrasive particles"), to the extent that the effects of the present invention are not significantly hindered. Examples of non-silica abrasive particles include inorganic particles, organic particles, and organic-inorganic composite particles. Specific examples of inorganic particles include oxide particles such as alumina particles, cerium oxide particles, chromium oxide particles, titanium dioxide particles, zirconium oxide particles, magnesium oxide particles, manganese dioxide particles, zinc oxide particles, and red iron oxide particles; nitride particles such as silicon nitride particles and boron nitride particles; carbide particles such as silicon carbide particles and boron carbide particles; diamond particles; and carbonates such as calcium carbonate and barium carbonate. Specific examples of organic particles include polymethyl methacrylate (PMMA) particles and poly(meth)acrylic acid particles (where (meth)acrylic acid comprehensively refers to acrylic acid and methacrylic acid), and polyacrylonitrile particles. Such abrasive particles may be used individually or in combination of two or more types.
[0038] The technology disclosed herein can preferably be implemented in a manner in which substantially only silica particles are used as abrasive grains. From this viewpoint, the proportion of silica particles in the total amount of abrasive grains is suitable to be 90% by weight or more, preferably 95% by weight or more, and more preferably 98% by weight or more (e.g., 99-100% by weight).
[0039] <Basic compounds> The polishing compositions disclosed herein contain basic compounds. In this specification, a basic compound refers to a compound that dissolves in water and increases the pH of the aqueous solution. By including a basic compound in the polishing composition, the object to be polished can be efficiently polished by its chemical polishing action (alkaline etching). Examples of basic compounds include nitrogen-containing organic or inorganic basic compounds, phosphorus-containing basic compounds, alkali metal hydroxides, alkaline earth metal hydroxides, various carbonates and bicarbonates, etc. Examples of nitrogen-containing basic compounds include quaternary ammonium compounds, ammonia, and amines (preferably water-soluble amines). Examples of phosphorus-containing basic compounds include quaternary phosphonium compounds. Such basic compounds can be used individually or in combination of two or more.
[0040] Specific examples of alkali metal hydroxides include potassium hydroxide and sodium hydroxide. Specific examples of carbonates or bicarbonates include ammonium bicarbonate, ammonium carbonate, potassium bicarbonate, potassium carbonate, sodium bicarbonate, and sodium carbonate. Specific examples of amines include methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, monoethanolamine, N-(β-aminoethyl)ethanolamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, anhydrous piperazine, piperazine hexahydrate, 1-(2-aminoethyl)piperazine, N-methylpiperazine, guanidine, and azoles such as imidazole and triazole. Specific examples of quaternary phosphonium compounds include quaternary phosphonium hydroxides such as tetramethylphosphonium hydroxide and tetraethylphosphonium hydroxide.
[0041] As quaternary ammonium compounds, quaternary ammonium salts (typically strong bases) such as tetraalkylammonium salts and hydroxyalkyltrialkylammonium salts can be used. The anionic component in such quaternary ammonium salts is, for example, OH - F- , Cl - , Br - , I - , ClO4 - , BH4 - , and the like. Examples of the quaternary ammonium compound include quaternary ammonium salts in which the anion is OH - , that is, quaternary ammonium hydroxides. Specific examples of quaternary ammonium hydroxides include tetraalkylammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrapentylammonium hydroxide, and tetrahexylammonium hydroxide; hydroxyalkyltrialkylammonium hydroxides such as 2-hydroxyethyltrimethylammonium hydroxide (also referred to as choline); and the like.
[0042] Among these basic compounds, for example, at least one basic compound selected from alkali metal hydroxides, quaternary ammonium hydroxides, and ammonia can be preferably used. Among them, tetraalkylammonium hydroxide (e.g., tetramethylammonium hydroxide) and ammonia are more preferred, and ammonia is particularly preferred.
[0043] <Water-soluble polymer> The polishing composition disclosed herein contains a water-soluble polymer. The water-soluble polymer can be useful for protecting the surface of the object to be polished, improving the wettability of the surface of the object to be polished after polishing, and the like. The polishing composition disclosed herein is characterized by containing at least two types of water-soluble polymers. In other words, the polishing composition disclosed herein contains a first water-soluble polymer and a second water-soluble polymer.
[0044] <First water-soluble polymer> The polishing composition disclosed herein contains a polyvinyl alcohol-based polymer as a first water-soluble polymer. A polishing composition containing a polyvinyl alcohol-based polymer makes it easier to obtain a high-quality polished surface. While not interpreted restrictively, the polyvinyl alcohol-based polymer is thought to protect the substrate surface by acting upon it, thereby contributing to improved polished surface quality (specifically, haze reduction). By using the polyvinyl alcohol-based polymer as the first water-soluble polymer in combination with a second water-soluble polymer, it is possible to effectively achieve high surface quality while enjoying the benefits based on the different actions of each water-soluble polymer.
[0045] In this specification, a polyvinyl alcohol polymer refers to a polymer that contains vinyl alcohol units (hereinafter also referred to as "VA units") as its repeating units. A polyvinyl alcohol polymer may be used alone or in combination of two or more types. A polyvinyl alcohol polymer may contain only VA units as its repeating units, or it may contain VA units in addition to repeating units other than VA units (hereinafter also referred to as "non-VA units"). A polyvinyl alcohol polymer may be a random copolymer containing VA units and non-VA units, a block copolymer, an alternating copolymer, or a graft copolymer. A polyvinyl alcohol polymer may contain only one type of non-VA unit, or it may contain two or more types of non-VA units.
[0046] The above polyvinyl alcohol polymer may be unmodified polyvinyl alcohol (unmodified PVA) or modified polyvinyl alcohol (modified PVA). Here, unmodified PVA refers to a polyvinyl alcohol polymer produced by hydrolysis (saponification) of polyvinyl acetate, which substantially does not contain repeating units other than the vinyl polymerized vinyl acetate structure (-CH2-CH(OCOCH3)-) and VA units. The degree of saponification of the above unmodified PVA may be, for example, 60% or more, and may be 70% or more, 80% or more, or 90% or more from the viewpoint of water solubility. In some embodiments, the degree of saponification of the unmodified PVA may be 98% or more (complete saponification).
[0047] The polyvinyl alcohol polymer may be a modified PVA containing VA units and non-VA units having at least one structure selected from oxyalkylene groups, carboxyl groups, (di)carboxylic acid groups, (di)carboxylic acid ester groups, phenyl groups, naphthyl groups, sulfo groups, amino groups, hydroxyl groups, amide groups, imide groups, nitrile groups, ether groups, ester groups, and salts thereof. The non-VA units that may be included in the modified PVA may, but are not limited to, repeating units derived from N-vinyl type monomers or N-(meth)acryloyl type monomers, repeating units derived from ethylene, repeating units derived from alkyl vinyl ethers, repeating units derived from vinyl esters of monocarboxylic acids having 3 or more carbon atoms, repeating units derived from (di)acetone compounds, etc. A suitable example of the above N-vinyl type monomer is N-vinylpyrrolidone. A suitable example of the above N-(meth)acryloyl type monomer is N-(meth)acryloylmorpholine. The alkyl vinyl ether may be a vinyl ether having an alkyl group with 1 to 10 carbon atoms, such as propyl vinyl ether, butyl vinyl ether, or 2-ethylhexyl vinyl ether. The vinyl ester of a monocarboxylic acid having 3 or more carbon atoms may be a vinyl ester of a monocarboxylic acid having 3 to 7 carbon atoms, such as vinyl propanoate, vinyl butanoate, vinyl pentanoate, or vinyl hexanoate. Preferred examples of the (di)acetone compound include diacetone(meth)acrylamide and acetylacetone.
[0048] Furthermore, in some preferred embodiments, an acetalized polyvinyl alcohol polymer is used as the polyvinyl alcohol polymer. Examples of acetalized polyvinyl alcohol polymers include modified PVA in which some of the VA units contained in the polyvinyl alcohol polymer are acetalized. The above modified PVA in which some of the VA units contained in the polyvinyl alcohol polymer are acetalized (acetalized PVA (ac-PVA)) can be obtained by reacting some of the hydroxyl groups of the polyvinyl alcohol polymer with an aldehyde compound or a ketone compound to acetalize it. Typically, the acetalized polyvinyl alcohol polymer is obtained by an acetalization reaction between the polyvinyl alcohol polymer and an aldehyde compound. In some preferred embodiments, the number of carbon atoms in the aldehyde compound is 1 to 7, more preferably 2 to 7.
[0049] Examples of the above-mentioned aldehyde compounds include formaldehyde; linear or branched alkylaldehydes such as acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, t-butyraldehyde, and hexylaldehyde; and alicyclic or aromatic aldehydes such as cyclohexanecarbaldehyde and benzaldehyde. These may be used individually or in combination of two or more. In addition, except for formaldehyde, one or more hydrogen atoms may be substituted with halogens or the like. Among these, linear or branched alkylaldehydes are preferred due to their high solubility in water and ease of acetalization reaction, and among these, acetaldehyde, n-propylaldehyde, n-butyraldehyde, and n-pentylaldehyde are more preferred.
[0050] In addition to the above, other aldehyde compounds with 8 or more carbon atoms, such as 2-ethylhexylaldehyde, nonylaldehyde, and decylaldehyde, may also be used as aldehyde compounds.
[0051] Acetalized polyvinyl alcohol polymers contain VA units, which are structural parts represented by the following chemical formula: -CH2-CH(OH)-; and acetalized structural units (hereinafter also referred to as "VAC units") represented by the following general formula (1).
[0052] [ka] (In formula (1), R is a hydrogen atom or a linear or branched alkyl group, and the alkyl group may be substituted with a functional group.)
[0053] In some preferred embodiments, R in formula (1) above is a hydrogen atom or a linear or branched alkyl group having 1 to 6 carbon atoms. R may be one of these or a combination of two or more. From the viewpoint of improving haze reduction performance, R is preferably a linear or branched alkyl chain having 1 to 6 carbon atoms.
[0054] From the viewpoint of improving haze reduction performance, the degree of acetalization of the acetalized polyvinyl alcohol-based polymer can be 1 mol% or more, may be 5 mol% or more, preferably 10 mol% or more, more preferably 15 mol% or more, even more preferably 20 mol% or more, and particularly preferably 25 mol% or more (e.g., 27 mol% or more). From the viewpoint of improving hydrophilicity, the degree of acetalization of the acetalized polyvinyl alcohol-based polymer is preferably less than 60 mol%, even more preferably 50 mol% or less, more preferably 40 mol% or less, and particularly preferably 35 mol% or less (e.g., 33 mol% or less). In this specification, "degree of acetalization" refers to the ratio of acetalized structural units (VAC units) to the total repeating units constituting the acetalized polyvinyl alcohol-based polymer.
[0055] Furthermore, as the polyvinyl alcohol polymer, a cation-modified polyvinyl alcohol into which a cationic group such as a quaternary ammonium structure has been introduced may be used. Examples of the above-mentioned cation-modified polyvinyl alcohol include those into which a cationic group derived from a monomer having a cationic group, such as diallyldialkylammonium salt or N-(meth)acryloylaminoalkyl-N,N,N-trialkylammonium salt has been introduced. In addition, as the vinyl alcohol polymer, a non-VA unit with the chemical formula:-CH2-CH(CR 1 (OR 4 )-CR 2 (OR 5 )-R 3 It may have a structural part represented by )-. Here R 1 ~R 3 Each of these independently represents a hydrogen atom or an organic group, and R 4 and R 5 Each is independently a hydrogen atom or R 6 -CO-(wherein, R 6 R indicates an alkyl group. For example, R in the above chemical formula 1 ~R 3 If at least one of the elements is an organic group, the organic group may be a linear or branched alkyl group having 1 to 8 carbon atoms. Also, R in the above chemical formula 6 This can be a linear or branched alkyl group having 1 to 8 carbon atoms.
[0056] In some embodiments, modified PVA having a 1,2-diol structure in the side chain is used as the modified PVA. For example, as the modified PVA, the R 1 ~R 5 Modified PVA (butenediol-vinyl alcohol copolymer (BVOH)) containing non-VA units in which hydrogen atoms can preferably be used.
[0057] The ratio of moles of VA units to the total number of moles of repeating units constituting the polyvinyl alcohol-based polymer may be, for example, 5% or more, 10% or more, 20% or more, or 30% or more. While not particularly limited, in some embodiments, the ratio of moles of VA units may be 50% or more, 65% or more, 75% or more, 80% or more, or 90% or more (e.g., 95% or more, or 98% or more). It is also possible that substantially 100% of the repeating units constituting the polyvinyl alcohol-based polymer are VA units. Here, "substantially 100%" means that the polyvinyl alcohol-based polymer does not contain non-VA units, at least intentionally, and typically includes cases where the ratio of moles of non-VA units to the total number of moles of repeating units is less than 2% (e.g., less than 1%), and 0%. In some other embodiments, the ratio of moles of VA units to the total number of moles of repeating units constituting the polyvinyl alcohol-based polymer may be, for example, 95% or less, 90% or less, 80% or less, or 70% or less.
[0058] The content of VA units (by weight) in the polyvinyl alcohol polymer may be, for example, 5% by weight or more, 10% by weight or more, 20% by weight or more, or 30% by weight or more. Although not particularly limited, in some embodiments, the content of VA units may be 50% by weight or more (e.g., more than 50% by weight), 70% by weight or more, or 80% by weight or more (e.g., 90% by weight or more, or 95% by weight or more, or 98% by weight or more). Substantially 100% by weight of the repeating units constituting the polyvinyl alcohol polymer may be VA units. Here, "substantially 100% by weight" means that, at least intentionally, no non-VA units are included as repeating units constituting the polyvinyl alcohol polymer, and typically means that the content of non-VA units in the polyvinyl alcohol polymer is less than 2% by weight (e.g., less than 1% by weight). In some other embodiments, the VA unit content in the polyvinyl alcohol-based polymer may be, for example, 95% by weight or less, 90% by weight or less, 80% by weight or less, or 70% by weight or less.
[0059] A polyvinyl alcohol-based polymer may contain multiple polymer chains with different VA unit content within the same molecule. Here, a polymer chain refers to a part (segment) that constitutes a portion of a polymer molecule. For example, a polyvinyl alcohol-based polymer may contain polymer chain A, which has a VA unit content higher than 50% by weight, and polymer chain B, which has a VA unit content lower than 50% by weight (i.e., a non-VA unit content higher than 50% by weight), within the same molecule.
[0060] Polymer chain A may contain only VA units as repeating units, or it may contain non-VA units in addition to VA units. The VA unit content in polymer chain A may be 60% by weight or more, 70% by weight or more, 80% by weight or more, or 90% by weight or more. In some embodiments, the VA unit content in polymer chain A may be 95% by weight or more, or 98% by weight or more. Substantially 100% by weight of the repeating units constituting polymer chain A may be VA units.
[0061] Polymer chain B may contain only non-VA units as repeating units, or it may contain VA units in addition to non-VA units. The content of non-VA units in polymer chain B may be 60% by weight or more, 70% by weight or more, 80% by weight or more, or 90% by weight or more. In some embodiments, the content of non-VA units in polymer chain B may be 95% by weight or more, or 98% by weight or more. Substantially 100% by weight of the repeating units constituting polymer chain B may be non-VA units.
[0062] Examples of polyvinyl alcohol-based polymers containing polymer chain A and polymer chain B in the same molecule include block copolymers and graft copolymers containing these polymer chains. The above graft copolymer may be a graft copolymer in which polymer chain B (side chain) is grafted onto polymer chain A (main chain), or a graft copolymer in which polymer chain A (side chain) is grafted onto polymer chain B (main chain). In some embodiments, a polyvinyl alcohol-based polymer in which polymer chain B is grafted onto polymer chain A can be used.
[0063] Examples of polymer chain B include polymer chains whose main repeating unit is a repeating unit derived from an N-vinyl type monomer; polymer chains whose main repeating unit is a repeating unit derived from an N-(meth)acryloyl type monomer; polymer chains whose main repeating unit is a repeating unit derived from vinyl dicarboxylates such as fumaric acid, maleic acid, and maleic anhydride; polymer chains whose main repeating unit is a repeating unit derived from aromatic vinyl monomers such as styrene and vinylnaphthalene; polymer chains whose main repeating unit is an oxyalkylene unit; and so on. In this specification, unless otherwise specified, a main repeating unit refers to a repeating unit that is present in more than 50% by weight.
[0064] A preferred example of polymer chain B is a polymer chain whose main repeating unit is an N-vinyl type monomer, i.e., an N-vinyl polymer chain. The content of repeating units derived from N-vinyl type monomers in the N-vinyl polymer chain is typically more than 50% by weight, may be 70% or more by weight, 85% or more by weight, or 95% or more by weight. Substantially all of polymer chain B may consist of repeating units derived from N-vinyl type monomers.
[0065] In this specification, examples of N-vinyl type monomers include monomers having a nitrogen-containing heterocyclic ring (e.g., a lactam ring) and N-vinyl chain amides. Specific examples of N-vinyl lactam type monomers include N-vinylpyrrolidone, N-vinylpiperidone, N-vinylmorpholinone, N-vinylcaprolactam, N-vinyl-1,3-oxazin-2-one, and N-vinyl-3,5-morpholindione. Specific examples of N-vinyl chain amides include N-vinylacetamide, N-vinylpropionic acid amide, and N-vinylbutyric acid amide. Polymer chain B may be, for example, an N-vinyl polymer chain in which more than 50% by weight (e.g., 70% or more by weight, or 85% or more by weight, or 95% or more by weight) of its repeating units are N-vinylpyrrolidone units. Substantially all of the repeating units constituting polymer chain B may be N-vinylpyrrolidone units.
[0066] Another example of polymer chain B is a polymer chain whose main repeating unit is an N-(meth)acryloyl type monomer, i.e., an N-(meth)acryloyl polymer chain. The content of repeating units derived from N-(meth)acryloyl type monomers in an N-(meth)acryloyl polymer chain is typically more than 50% by weight, may be 70% or more by weight, 85% or more by weight, or 95% or more by weight. It is also possible that substantially all of polymer chain B consists of repeating units derived from N-(meth)acryloyl type monomers.
[0067] In this specification, examples of N-(meth)acryloyl type monomers include chain amides having an N-(meth)acryloyl group and cyclic amides having an N-(meth)acryloyl group. Examples of chain amides having an N-(meth)acryloyl group include (meth)acrylamides; N-alkyl(meth)acrylamides such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and Nn-butyl(meth)acrylamide; and N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, and N,N-di(n-butyl)(meth)acrylamide. Examples of cyclic amides having an N-(meth)acryloyl group include N-(meth)acryloylmorpholine and N-(meth)acryloylpyrrolidine.
[0068] Another example of polymer chain B is a polymer chain containing oxyalkylene units as the main repeating units, i.e., an oxyalkylene polymer chain. The oxyalkylene unit content in the oxyalkylene polymer chain is typically more than 50% by weight, may be 70% or more by weight, 85% or more by weight, or 95% or more by weight. Substantially all of the repeating units in polymer chain B may be oxyalkylene units.
[0069] Examples of oxyalkylene units include oxyethylene units, oxypropylene units, and oxybutylene units. Each of these oxyalkylene units may be repeating units derived from the corresponding alkylene oxide. The oxyalkylene polymer chain may contain one type of oxyalkylene unit or two or more types. For example, it may be an oxyalkylene polymer chain containing a combination of oxyethylene units and oxypropylene units. In an oxyalkylene polymer chain containing two or more types of oxyalkylene units, these oxyalkylene units may be random copolymers of the corresponding alkylene oxides, block copolymers, alternating copolymers, or graft copolymers.
[0070] Further examples of polymer chain B include polymer chains containing repeating units derived from alkyl vinyl ethers (e.g., vinyl ethers having alkyl groups with 1 to 10 carbon atoms), polymer chains containing repeating units derived from monocarboxylate vinyl esters (e.g., vinyl esters of monocarboxylic acids with 3 or more carbon atoms), and polymer chains into which cationic groups (e.g., cationic groups having a quaternary ammonium structure) are introduced.
[0071] In some embodiments of the technology disclosed herein, the polyvinyl alcohol-based polymer as the first water-soluble polymer is preferably a modified polyvinyl alcohol copolymer containing VA units and non-VA units. Furthermore, the degree of saponification of the modified polyvinyl alcohol-based polymer as the first water-soluble polymer is usually 50 mol% or more, preferably 65 mol% or more, more preferably 70 mol% or more, for example 75 mol% or more.
[0072] The weight-average molecular weight (Mw) of the first water-soluble polymer (specifically, a polyvinyl alcohol-based polymer) is, for example, 100 × 10⁻⁶. 4 The following is possible: 60 x 10 4 The following is appropriate. From the viewpoint of concentration efficiency, etc., the above Mw is 30 × 10 4The following may also be included, preferably 20 × 10 4 For example, 10 x 10 4 The following is also acceptable: 8 × 10 4 The following is also acceptable: 5 x 10 4 The following is also acceptable: 3 x 10 4 The following is also acceptable. As the Mw of the polyvinyl alcohol-based polymer decreases, the dispersion stability of the polyvinyl alcohol-based polymer tends to improve. Furthermore, from the viewpoint of suitably protecting the polished surface and maintaining or improving surface quality, the above Mw is, for example, 0.2 × 10 4 It may be greater than or equal to 0.5 × 10 4 The above is preferable. As the Mw of the polyvinyl alcohol-based polymer increases, the effect of protecting the object to be polished and improving wettability tends to increase. From this viewpoint, in some embodiments, the above Mw is 0.8 × 10 4 The above is appropriate, preferably 1.0 × 10 4 That's all. 2 × 10 4 It may be more than 3 × 10 4 The above is also acceptable; for example, 4 x 10 4 The above is also acceptable: 5 x 10 4 That's fine too.
[0073] For water-soluble polymers, the molecular weight (Mw) can be calculated from values based on aqueous gel permeation chromatography (GPC) (aqueous system, polyethylene oxide equivalent). The same applies to the Mw of the first water-soluble polymer and the second water-soluble polymer described later. For the GPC measurement device, the "HLC-8320GPC" model manufactured by Tosoh Corporation is recommended. Measurement can be performed, for example, under the following conditions. The same method is used for the examples described later. [GPC measurement conditions] Sample concentration: 0.1% by weight Column: TSKgel GMPW XL Detector: Differential refractometer Eluent: 100 mM sodium nitrate aqueous solution Flow rate: 1mL / min Measurement temperature: 40℃ Sample injection volume: 200 μL
[0074] While not particularly limited, in some embodiments, the content of the first water-soluble polymer (specifically, a polyvinyl alcohol-based polymer) in the polishing composition can be, for example, 0.01 parts by weight or more per 100 parts by weight of abrasive grains (typically silica particles). From the viewpoint of reducing defects, it is appropriate to have 0.1 parts by weight or more, preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, and may also be 1.5 parts by weight or more, 2 parts by weight or more, 3 parts by weight or more, or 3.5 parts by weight or more. The content of the first water-soluble polymer per 100 parts by weight of abrasive grains may be, for example, 50 parts by weight or less, or 30 parts by weight or less. From the viewpoint of dispersion stability of the polishing composition, in some embodiments, the content of the first water-soluble polymer per 100 parts by weight of abrasive grains is appropriate to be 15 parts by weight or less, preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and may also be less than 3 parts by weight, 2.5 parts by weight or less, or 2 parts by weight or less. By appropriately setting the amount of the first water-soluble polymer (specifically, a polyvinyl alcohol-based polymer) used from the above range, high surface quality after polishing can be achieved.
[0075] <Second water-soluble polymer> The polishing composition disclosed herein comprises a first water-soluble polymer (specifically, a polyvinyl alcohol-based polymer) and a second water-soluble polymer. The second water-soluble polymer is typically a polymer having a different chemical structure from the first water-soluble polymer. The second water-soluble polymer has a zeta potential ζ [mV] of the polishing composition and an etching rate ER [ nm / h Insofar as the specific conditions described above are met with respect to the product of ], various types can be used without particular limitation.
[0076] Examples of the second water-soluble polymer include compounds containing hydroxyl groups, carboxyl groups, acyloxy groups, sulfo groups, amide structures, imide structures, quaternary ammonium structures, heterocyclic structures, vinyl structures, etc., in their molecules. Examples of the second water-soluble polymer include cellulose derivatives, starch derivatives, polymers containing oxyalkylene units, polyvinyl alcohol-based polymers, polymers containing nitrogen atoms, and polymers containing (meth)acrylic acid units. As one embodiment of the polymer containing nitrogen atoms, N-vinyl type polymers and N-(meth)acryloyl type polymers may be used. The second water-soluble polymer may be a polymer derived from a natural product or a synthetic polymer.
[0077] In some embodiments, a polymer derived from a natural product is used as the second water-soluble polymer. Examples of polymers derived from natural products include cellulose derivatives and starch derivatives.
[0078] In some embodiments, a cellulose derivative is used as the second water-soluble polymer. Here, the cellulose derivative is a polymer containing β-glucose units as the main repeating units. Specific examples of cellulose derivatives include hydroxyethylcellulose (HEC), hydroxypropylcellulose, hydroxyethylmethylcellulose, hydroxypropylmethylcellulose, methylcellulose, ethylcellulose, ethylhydroxyethylcellulose, and carboxymethylcellulose. Among these, HEC is preferred.
[0079] In some other embodiments, a starch derivative is used as the second water-soluble polymer. The starch derivative is a polymer containing α-glucose units as the main repeating units, and examples include pregelatinized starch, pullulan, carboxymethyl starch, and cyclodextrin.
[0080] In several other preferred embodiments, a synthetic polymer is used as the second water-soluble polymer. The surface quality improvement effect disclosed herein is preferably exhibited in embodiments in which a synthetic polymer is used as the second water-soluble polymer.
[0081] In some embodiments, a polymer containing oxyalkylene units is used as the second water-soluble polymer. Examples of polymers containing oxyalkylene units include polyethylene oxide (PEO), block copolymers of ethylene oxide (EO) and propylene oxide (PO) or butylene oxide (BO), and random copolymers of EO and PO or BO. Among these, block copolymers of EO and PO or random copolymers of EO and PO are preferred. The block copolymer of EO and PO may be a diblock copolymer or a triblock copolymer containing PEO blocks and polypropylene oxide (PPO) blocks. Examples of the above triblock copolymers include PEO-PPO-PEO type triblock copolymers and PPO-PEO-PPO type triblock copolymers. Generally, PEO-PPO-PEO type triblock copolymers are more preferred.
[0082] In this specification, unless otherwise specified, the term "polymer" comprehensively refers to various types of copolymers, including random copolymers, alternating copolymers, block copolymers, and graft copolymers.
[0083] In block copolymers or random copolymers of EO and PO, the molar ratio (EO / PO) of EO and PO constituting the copolymer is preferably greater than 1, more preferably 2 or more, and even more preferably 3 or more (for example, 5 or more) from the viewpoint of solubility in water and washability.
[0084] In some preferred embodiments, a polyvinyl alcohol-based polymer is used as the second water-soluble polymer. If the polishing composition contains two or more polyvinyl alcohol-based polymers, the one with the smaller Mw is designated as the first water-soluble polymer, and the one with the larger Mw is designated as the second water-soluble polymer.
[0085] In some preferred embodiments, a modified PVA containing repeating units derived from N-vinyl type monomers or N-(meth)acryloyl type monomers as non-VA units can be used as the second water-soluble polymer. In other embodiments where the second water-soluble polymer is a polyvinyl alcohol-based polymer, the second water-soluble polymer can be one of the polyvinyl alcohol-based polymers listed as those that can be preferably used as the first water-soluble polymer. Examples of preferred polymers are omitted to avoid repetition.
[0086] In some other embodiments, N-vinyl polymers may be used as the second water-soluble polymer. Examples of N-vinyl polymers include polymers containing repeating units derived from monomers having nitrogen-containing heterocyclic rings (e.g., lactam rings). Examples of such polymers include homopolymers and copolymers of N-vinyl lactam monomers (e.g., copolymers in which the copolymerization ratio of N-vinyl lactam monomer exceeds 50% by weight), and homopolymers and copolymers of N-vinyl chain amides (e.g., copolymers in which the copolymerization ratio of N-vinyl chain amide exceeds 50% by weight).
[0087] Specific examples of N-vinyllactam monomers (i.e., compounds having a lactam structure and an N-vinyl group within a single molecule) include N-vinylpyrrolidone (VP), N-vinylpiperidone, N-vinylmorpholinone, N-vinylcaprolactam (VC), N-vinyl-1,3-oxazin-2-one, and N-vinyl-3,5-morpholindione. Specific examples of polymers containing N-vinyllactam monomer units include polyvinylpyrrolidone, polyvinylcaprolactam, random copolymers of VP and VC, random copolymers of one or both of VP and VC with other vinyl monomers (e.g., acrylic monomers, vinyl ester monomers, etc.), block copolymers containing polymer chains containing one or both of VP and VC, alternating copolymers, and graft copolymers. Specific examples of N-vinyl chain amides include N-vinylacetamide, N-vinylpropionic acid amide, and N-vinylbutyric acid amide.
[0088] In some other embodiments, an N-(meth)acryloyl polymer may be used as the second water-soluble polymer. Examples of N-(meth)acryloyl polymers include homopolymers and copolymers of N-(meth)acryloyl monomers (typically copolymers in which the copolymerization ratio of N-(meth)acryloyl monomers exceeds 50% by weight). Examples of N-(meth)acryloyl monomers include chain amides having an N-(meth)acryloyl group and cyclic amides having an N-(meth)acryloyl group. In this specification, (meth)acryloyl type refers comprehensively to acryloyl type and methacryloyl type. In this specification, (meth)acryloyl group refers comprehensively to acryloyl group and methacryloyl group.
[0089] Examples of chain amides having an N-(meth)acryloyl group include (meth)acrylamide; N-alkyl(meth)acrylamides such as N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide, and Nn-butyl(meth)acrylamide; and N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, and N,N-di(n-butyl)(meth)acrylamide. Another example is N-hydroxyethylacrylamide (HEAA). Examples of polymers containing chain amides having an N-(meth)acryloyl group as monomer units include homopolymers of N-isopropylacrylamide and copolymers of N-isopropylacrylamide (for example, copolymers in which the copolymerization ratio of N-isopropylacrylamide exceeds 50% by weight). In this specification, (meth)acrylamide refers collectively to acrylamide and methacrylamide.
[0090] Examples of cyclic amides having an N-(meth)acryloyl group include N-acryloylmorpholine, N-acryloylthiomorpholine, N-acryloylpiperidine, N-acryloylpyrrolidine, N-methacryloylmorpholine, N-methacryloylpiperidine, and N-methacryloylpyrrolidine. An example of a polymer containing a cyclic amide having an N-(meth)acryloyl group as a monomer unit is acryloylmorpholine polymer (PACMO). Typical examples of acryloylmorpholine polymers include homopolymers of N-acryloylmorpholine (ACMO) and copolymers of ACMO (for example, copolymers in which the copolymerization ratio of ACMO exceeds 50% by weight). In acryloylmorpholine polymers, the ratio of the number of moles of ACMO units to the total number of moles of repeating units is usually 50% or more, and it is appropriate for it to be 80% or more (for example, 90% or more, typically 95% or more). The entire repeating unit of the second water-soluble polymer may be substantially composed of ACMO units.
[0091] In some embodiments, a carboxylic acid polymer is used as the second water-soluble polymer. Examples of carboxylic acid polymers include polymers containing maleic acid units and polymers containing (meth)acrylic acid units. Examples of polymers containing maleic acid units include styrene-maleic acid copolymer or its salt, styrene-maleic anhydride copolymer, styrene sulfonic acid-maleic acid copolymer or its salt, copolymer of styrene sulfonate and maleic acid, and maleic acid-vinyl acetate copolymer. Examples of polymers containing (meth)acrylic acid units include polyacrylic acid or its salt, styrene-acrylic acid copolymer or its salt, styrene sulfonic acid-acrylic acid copolymer or its salt, copolymer of styrene sulfonate and acrylic acid, acrylic acid-vinyl acetate copolymer, and acrylic acid / sulfonic acid monomer copolymer. In this specification, (meth)acrylic acid refers collectively to acrylic acid and methacrylic acid.
[0092] When the second water-soluble polymer is a polyvinyl alcohol-based polymer, the Mw of the second water-soluble polymer is, for example, 100 × 10 4 The following is possible: 60 x 10 4 The following is appropriate. From the viewpoint of concentration efficiency, etc., the above Mw is 30 × 10 4 The following may also be included, preferably 20 × 10 4 For example, 10 x 10 4 The following is also acceptable: 8 × 10 4 The following is also acceptable: 5 x 10 4 The following is also acceptable: 3 x 10 4 The following is also acceptable. Furthermore, from the viewpoint of suitably protecting the polished surface and maintaining or improving surface quality, the above Mw may be, for example, 0.2 × 10 4 It may be greater than or equal to 0.5 × 10 4 The above is preferable. As the Mw of the polyvinyl alcohol-based polymer increases, the effect of protecting the object to be polished and improving wettability tends to increase. From this viewpoint, in some embodiments, the above Mw is 0.8 × 10 4 The above is appropriate, preferably 1.0 × 10 4 That is all, 1.2 × 10 4 That's fine too.
[0093] When the second water-soluble polymer is a polymer containing a chain-like amide having an N-(meth)acryloyl group as a monomer unit, the Mw of the second water-soluble polymer is, for example, 100 × 10 4 The following can be used: 50 x 10 4 The following is appropriate. From the viewpoint of concentration efficiency, etc., the above Mw is 30 × 10 4 The following is also acceptable: 10 x 10 4 The following is also acceptable: 8 x 10 4 The following is also acceptable: 6 x 10 4 The following is also acceptable. Furthermore, from the viewpoint of improving surface quality, the above Mw can be, for example, 1 × 10 4 It may be more than 2 × 10 4 The above is also acceptable: 3 x 10 4 (For example, 4 x 10) 4The above is also acceptable. High surface quality is easily obtained by using a second water-soluble polymer with a high Mw.
[0094] When the second water-soluble polymer is a polymer containing a cyclic amide having an N-(meth)acryloyl group as a monomer unit, the Mw of the second water-soluble polymer is, for example, 100 × 10 4 The following can be used: 70 x 10 4 The following is appropriate. From the viewpoint of concentration efficiency, etc., the above Mw is 60 × 10 4 The following is also acceptable: 50 x 10 4 The following is also acceptable: 40 x 10 4 The following is also acceptable. Furthermore, from the viewpoint of improving surface quality, the above Mw can be, for example, 1.0 × 10 4 It may be more than 5 × 10 4 The above is also acceptable: 10 x 10 4 (For example, 10 x 10) 4 (Extraordinary) is also acceptable. In some embodiments, the above Mw is 20 × 10 4 The above is appropriate, preferably 25 × 10 4 That is all, more preferably 30 × 10 4 That's all (use 30 x 10) 4 It is extremely high. By using a second water-soluble polymer with high Mw, high surface quality is easily obtained.
[0095] When the second water-soluble polymer is a polymer containing (meth)acrylic acid units, the Mw of the second water-soluble polymer is, for example, 800 × 10 4 The following is possible: 500 x 10 4 The following is appropriate. From the viewpoint of concentration efficiency, etc., the above Mw is 300 × 10 4 The following may also be the case, preferably 200 × 10 4 For example, 175 x 10 4 The following are also acceptable: 150 x 10 4 The following is also acceptable: 140 x 10 4 The following is also acceptable. Furthermore, from the viewpoint of suitably protecting the polished surface and maintaining or improving surface quality, the above Mw is, for example, 20 × 10 4 It may be greater than or equal to 50 x 10 4or more, 100×10 4 or more (for example, 130×10 4 or more) is also acceptable. By using the second water-soluble polymer with a high Mw, high surface quality is easily obtained.
[0096] In the case where the second water-soluble polymer is a polymer containing oxyalkylene units, the Mw of the second water-soluble polymer can be 10×10 4 or less, may be 5×10 4 or less, may be 3×10 4 or less, and may be 2×10 4 or less. The aforementioned Mw can be 1×10 4 or more, may be 1.2×10 4 or more, and may be 1.5×10 4 or more.
[0097] Although not particularly limited, in some embodiments, as the aforementioned second water-soluble polymer, one having an Mw higher than the Mw of the aforementioned first water-soluble polymer can be preferably used. By using the two types of water-soluble polymers having the aforementioned relative Mw, high surface quality after polishing can be favorably achieved.
[0098] Although not particularly limited, in some embodiments, the content of the second water-soluble polymer in the polishing composition can be, for example, 0.01 parts by weight or more relative to 100 parts by weight of abrasive grains (typically silica particles), is suitably 0.1 parts by weight or more from the perspective of haze reduction and the like, preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, and may be 2 parts by weight or more. In addition, the content of the second water-soluble polymer relative to 100 parts by weight of abrasive grains may be, for example, 50 parts by weight or less, or 30 parts by weight or less. From the perspective of dispersion stability and the like of the polishing composition, in some embodiments, the content of the second water-soluble polymer relative to 100 parts by weight of abrasive grains is suitably 15 parts by weight or less, preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and may be, for example, 3.5 parts by weight or less. By appropriately setting the usage amount of the second water-soluble polymer from the aforementioned range, high surface quality can be obtained.
[0099] While not particularly limited, in some embodiments, the ratio of the content of basic compound (B) to the total content of water-soluble polymer (C1+C2) in the polishing composition (B / (C1+C2)) can be, for example, 0.01 or more by weight, and is appropriate to be 0.1 or more from the viewpoint of polishing rate, preferably 0.2 or more, more preferably 0.5 or more, and may also be 0.7 or more. Furthermore, the ratio of the content of basic compound (B) to the total content of water-soluble polymer (C1+C2) in the polishing composition (B / (C1+C2)) may be, for example, 15 or less by weight, and may also be 10 or less. Furthermore, from the viewpoint of suitably protecting the polished surface and maintaining or improving surface quality, the above content ratio is appropriate to be 7 or less, preferably 5 or less, more preferably 2 or less, and may also be, for example, 1 or less. By appropriately setting the ratio of the content of basic compound (B) to the total content of water-soluble polymer (C1+C2) from the above range, high surface quality can be obtained.
[0100] While not particularly limited, in some embodiments, the total content of the water-soluble polymer contained in the polishing composition can be, for example, 0.01 parts by weight or more per 100 parts by weight of abrasive grains (typically silica particles), and from the viewpoint of improving surface quality, it is appropriate to have 0.1 parts by weight or more, preferably 0.5 parts by weight or more, more preferably 1 part by weight or more, even more preferably 2 parts by weight or more, particularly preferably 4 parts by weight or more, and may also be 6 parts by weight or more. Furthermore, the total content of the water-soluble polymer per 100 parts by weight of abrasive grains may be, for example, 50 parts by weight or less, or 30 parts by weight or less. From the viewpoint of dispersion stability of the polishing composition, in some embodiments, the total content of the water-soluble polymer per 100 parts by weight of abrasive grains is appropriate to have 15 parts by weight or less, preferably 12 parts by weight or less, and may also be 10 parts by weight or less (for example, less than 10 parts by weight).
[0101] While not particularly limited, in some embodiments, the ratio of the content W2 of the second water-soluble polymer to the content W1 of the first water-soluble polymer (W2 / W1) is, for example, 0.01 or more by weight, preferably 0.2 or more, may be 0.4 or more, may be 0.6 or more, or may be 0.8 or more. Furthermore, the upper limit of the above ratio (W2 / W1) is, for example, 10 or less by weight, preferably 5 or less, preferably 3 or less, more preferably less than 2, and may be 1 or less (less than 1). By appropriately setting the above ratio (W2 / W1) within the above range, the effects of the technology disclosed herein can be preferably achieved.
[0102] The polishing compositions disclosed herein may contain, as an optional component, water-soluble polymers other than the first and second water-soluble polymers described above (hereinafter also referred to as optional water-soluble polymers), to the extent that the effects of the present invention are not significantly hindered.
[0103] In embodiments in which the polishing composition contains an arbitrary water-soluble polymer, the content ratio of the arbitrary water-soluble polymer to the total amount of water-soluble polymers in the polishing composition is not particularly limited, but from the viewpoint of effectively exerting the effects of the first water-soluble polymer and the second water-soluble polymer, it is appropriate to set it to approximately 50% by weight or less (for example, less than 50% by weight), and may be 30% by weight or less, less than 10% by weight, less than 3% by weight, or less than 1% by weight. The technology disclosed herein can preferably be carried out in embodiments in which the polishing composition does not substantially contain the arbitrary water-soluble polymer.
[0104] <Surfactants> In some embodiments, the polishing composition preferably contains at least one surfactant. Including a surfactant in the polishing composition can reduce haze on the polished surface. According to the techniques disclosed herein, the quality of the polished surface can be further improved with a composition containing the above-mentioned combination of water-soluble polymers and a surfactant. Any surfactant can be used, such as anionic, cationic, nonionic, or amphoteric. Usually, anionic or nonionic surfactants are preferred. Nonionic surfactants are more preferred from the viewpoint of low foaming and ease of pH adjustment. Examples of nonionic surfactants include oxyalkylene polymers such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; polyoxyalkylene derivatives such as polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene alkylamines, polyoxyethylene fatty acid esters, polyoxyethylene glyceryl ether fatty acid esters, and polyoxyethylene sorbitan fatty acid esters (e.g., polyoxyalkylene adducts); and copolymers of multiple types of oxyalkylenes (e.g., diblock copolymers, triblock copolymers, random copolymers, alternating copolymers). Surfactants can be used individually or in combination of two or more types.
[0105] Specific examples of nonionic surfactants include block copolymers of ethylene oxide (EO) and propylene oxide (PO) (diblock copolymers, PEO (polyethylene oxide)-PPO (polypropylene oxide)-PEO type triblock copolymers, PPO-PEO-PPO type triblock copolymers, etc.), random copolymers of EO and PO, polyoxyethylene glycol, polyoxyethylene propyl ether, polyoxyethylene butyl ether, polyoxyethylene pentyl ether, polyoxyethylene hexyl ether, polyoxyethylene octyl ether, polyoxyethylene-2-ethylhexyl ether, polyoxyethylene nonyl ether, polyoxyethylene decyl ether, polyoxyethylene isodecyl ether, polyoxyethylene tridecyl ether, polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene isostearyl ether, polyoxyethylene Examples include layl ether, polyoxyethylene phenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene dodecylphenyl ether, polyoxyethylene styrene phenyl ether, polyoxyethylene laurylamine, polyoxyethylene stearylamine, polyoxyethylene oleylamine, polyoxyethylene monolaurate, polyoxyethylene monostearate, polyoxyethylene distearate, polyoxyethylene monooleate, polyoxyethylene dioleate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopaltimate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan trioleate, polyoxyethylene sorbitan tetraoleate, polyoxyethylene castor oil, and polyoxyethylene hydrogenated castor oil.Among the preferred surfactants are block copolymers of EO and PO (especially PEO-PPO-PEO type triblock copolymers), random copolymers of EO and PO, and polyoxyethylene alkyl ethers (e.g., polyoxyethylene decyl ethers). For polyoxyethylene alkyl ethers, those with an EO addition number of approximately 1 to 10 (e.g., approximately 3 to 8) are preferably used.
[0106] In some embodiments, nonionic surfactants are preferably used. The use of nonionic surfactants tends to further improve haze reduction performance.
[0107] The molecular weight of a surfactant is, for example, 1 × 10⁻⁶ 4 The molecular weight is less than 9500, preferably 9500 or less from the viewpoint of filterability and washing ability, and may be less than 9000, for example. Furthermore, the molecular weight of the surfactant is usually appropriate to be 200 or more from the viewpoint of surface activity, and preferably 250 or more (e.g., 300 or more) from the viewpoint of haze reduction effect. A more preferable range for the molecular weight of the surfactant may also vary depending on the type of surfactant. For example, when polyoxyethylene alkyl ether is used as the surfactant, its molecular weight is preferably less than 2000, more preferably 1900 or less (e.g., less than 1800), even more preferably 1500 or less, and may be 1000 or less (e.g., 500 or less). Furthermore, when a block copolymer of EO and PO is used as the surfactant, its weight-average molecular weight may be, for example, 500 or more, 1000 or more, even 1500 or more, 2000 or more, and even 2500 or more. The upper limit of the above weight-average molecular weight is, for example, 1 × 10 4 It is less than 9500, preferably 9500 or less, for example, it may be less than 9000, less than 7000, or less than 5000.
[0108] The molecular weight of the surfactant may be determined from its chemical formula, or it may be determined by GPC (Gross Propagation) and used as the weight-average molecular weight (water-based, polyethylene glycol equivalent). For example, in the case of polyoxyethylene alkyl ethers, it is preferable to use the molecular weight determined from the chemical formula, and in the case of block copolymers of EO and PO, it is preferable to use the weight-average molecular weight determined by GPC.
[0109] While not particularly limited, in embodiments where the abrasive composition contains a surfactant, the surfactant content is usually appropriate, from the viewpoint of cleaning properties, to be 20 parts by weight or less, preferably 10 parts by weight or less, and more preferably 6 parts by weight or less (e.g., 3 parts by weight or less) per 100 parts by weight of abrasive grains (typically silica particles). From the viewpoint of better demonstrating the effect of the surfactant, the surfactant content per 100 parts by weight of abrasive grains is appropriate at 0.001 parts by weight or more, preferably 0.01 parts by weight or more, more preferably 0.1 parts by weight or more, and may be 0.5 parts by weight or more.
[0110] <Water> The water contained in the polishing composition disclosed herein can preferably be ion-exchanged water (deionized water), pure water, ultrapure water, distilled water, etc. In order to avoid as much as possible the inhibition of the function of other components contained in the polishing composition, the water used should preferably have a total content of transition metal ions of 100 ppb or less. For example, the purity of the water can be increased by operations such as removal of impurity ions with an ion exchange resin, removal of foreign matter with a filter, or distillation. The polishing composition disclosed herein may further contain an organic solvent (lower alcohol, lower ketone, etc.) that can be uniformly mixed with water, if necessary. It is preferable that 90% or more by volume of the solvent contained in the polishing composition is water, and it is more preferable that 95% or more by volume (for example, 99-100% by volume) is water.
[0111] <Other ingredients> The polishing compositions disclosed herein may further contain, as necessary, known additives that can be used in polishing compositions (for example, polishing compositions used in the finishing polishing process of silicon wafers), such as organic acids, organic acid salts, inorganic acids, inorganic acid salts, chelating agents, preservatives, and antifungal agents, to the extent that the effects of the present invention are not significantly hindered.
[0112] Organic acids and their salts, as well as inorganic acids and their salts, can be used individually or in combination of two or more. Examples of organic acids include fatty acids such as formic acid, acetic acid, and propionic acid; aromatic carboxylic acids such as benzoic acid and phthalic acid; itaconic acid, citric acid, oxalic acid, tartaric acid, malic acid, maleic acid, fumaric acid, succinic acid, glycolic acid, malonic acid, gluconic acid, alanine, glycine, lactic acid, organic sulfonic acids such as hydroxyethylidene diphosphate (HEDP) and methanesulfonic acid; and organic phosphonic acids such as nitrilotris (methylene phosphate) (NTMP) and phosphonovutanetricarboxylic acid (PBTC). Examples of organic acid salts include alkali metal salts (sodium salts, potassium salts, etc.) and ammonium salts of organic acids. Examples of inorganic acids include hydrochloric acid, phosphoric acid, sulfuric acid, phosphonic acid, nitric acid, phosphinic acid, boric acid, and carbonic acid. Examples of inorganic acid salts include alkali metal salts (sodium salts, potassium salts, etc.) and ammonium salts of inorganic acids.
[0113] The above chelating agents may be used individually or in combination of two or more. Examples of the above chelating agents include aminocarboxylic acid-based chelating agents and organic phosphonic acid-based chelating agents. Preferred examples of chelating agents include ethylenediaminetetrakis(methylenephosphonic acid), diethylenetriaminepenta(methylenephosphonic acid), and diethylenetriaminepentaacetic acid. Examples of the above preservatives and fungicides include isothiazolinoline compounds, parahydroxybenzoic acid esters, and phenoxyethanol.
[0114] The polishing compositions disclosed herein preferably contain substantially no oxidizing agents. This is because if an oxidizing agent is present in the polishing composition, when the polishing composition is supplied to a substrate (e.g., a silicon wafer), the surface of the substrate may be oxidized, forming an oxide film, which may reduce the polishing rate. Specific examples of oxidizing agents include hydrogen peroxide (H2O2), sodium persulfate, ammonium persulfate, and sodium dichloroisocyanurate. It should be noted that a polishing composition that contains substantially no oxidizing agents means that it does not contain oxidizing agents at least intentionally. Therefore, a polishing composition that inevitably contains trace amounts of oxidizing agents (for example, a molar concentration of oxidizing agents in the polishing composition of 0.001 mol / L or less, preferably 0.0005 mol / L or less, more preferably 0.0001 mol / L or less, even more preferably 0.00005 mol / L or less, particularly preferably 0.00001 mol / L or less) due to raw materials or manufacturing methods may be included in the concept of a polishing composition that contains substantially no oxidizing agents as described herein.
[0115] <ph> The pH of the polishing composition disclosed herein is not particularly limited, and an appropriate pH may be adopted depending on the substrate, etc. In some embodiments, the pH of the polishing composition is suitable at 8.0 or higher, preferably 8.5 or higher, and more preferably 9.0 or higher. As the pH of the polishing composition increases, the polishing rate tends to improve. On the other hand, from the viewpoint of preventing the dissolution of silica particles and suppressing a decrease in mechanical polishing action, the pH of the polishing composition is usually suitable at 12.0 or lower, preferably 11.0 or lower, more preferably 10.8 or lower, and even more preferably 10.5 or lower.
[0116] In the technology disclosed herein, the pH of the polishing composition can be determined by using a pH meter (for example, a glass electrode type hydrogen ion concentration indicator (model number F-72) manufactured by Horiba, Ltd.), performing a three-point calibration using standard buffers (phthalate pH buffer pH: 4.01 (25°C), neutral phosphate pH buffer pH: 6.86 (25°C), carbonate pH buffer pH: 10.01 (25°C)), then placing the glass electrode into the composition to be measured and measuring the value after it has stabilized for two minutes or more.
[0117] <Polishing liquid> The polishing compositions disclosed herein are typically supplied onto the surface of a substrate in the form of a polishing solution containing the polishing composition and used to polish the substrate. The polishing solution may be prepared, for example, by diluting (typically with water) one of the polishing compositions disclosed herein. Alternatively, the polishing composition may be used as is as a polishing solution. Another example of a polishing solution containing one of the polishing compositions disclosed herein is a polishing solution obtained by adjusting the pH of the composition.
[0118] The content of abrasive particles (typically silica particles) in the polishing fluid is not particularly limited, but is preferably 0.005% by weight or more, more preferably 0.01% by weight or more, more preferably 0.03% by weight or more, and even more preferably 0.06% by weight or more. A higher polishing rate can be achieved by increasing the abrasive particle content. The above content is suitable to be 10% by weight or less, preferably 7% by weight or less, more preferably 5% by weight or less, and even more preferably 2% by weight or less, and may be, for example, 1% by weight or less, 0.5% by weight or less, or 0.4% by weight or less. This makes it easier to maintain surface quality.
[0119] The content of basic compounds in the polishing solution is not particularly limited. From the viewpoint of improving the polishing rate, etc., it is usually appropriate to have a content of 0.0005% by weight or more, preferably 0.001% by weight or more, and more preferably 0.003% by weight or more. Furthermore, from the viewpoint of improving surface quality (e.g., reducing haze), etc., it is appropriate to have a content of less than 0.1% by weight, preferably less than 0.05% by weight, and more preferably less than 0.03% by weight (e.g., less than 0.025% by weight, and even more preferably less than 0.01% by weight).
[0120] While not particularly limited, in some embodiments, the content W1 of the first water-soluble polymer (specifically, a polyvinyl alcohol-based polymer) in the polishing solution may be, for example, 0.0001% by weight or more, and is usually appropriate to be 0.0005% by weight or more, preferably 0.001% by weight or more, and may also be, for example, 0.002% by weight or more, or 0.003% by weight or more, from the viewpoint of improving surface quality, etc. The upper limit of the content W1 of the first water-soluble polymer is not particularly limited and can be, for example, 0.05% by weight or less. From the viewpoint of stability in the concentrated solution stage, polishing rate, cleaning ability, etc., in some embodiments, the content W1 of the first water-soluble polymer is preferably 0.03% by weight or less, more preferably 0.015% by weight or less, and even more preferably 0.01% by weight or less. The polishing solution disclosed herein can also be implemented in embodiments in which the content W1 of the first water-soluble polymer is, for example, 0.008% by weight or less, 0.006% by weight or less, or 0.004% by weight or less.
[0121] While not particularly limited, in some embodiments, the content W2 of the second water-soluble polymer in the polishing solution may be, for example, 0.0001% by weight or more, and is usually appropriate to be 0.0005% by weight or more, preferably 0.001% by weight or more, and may also be 0.002% by weight or more, 0.003% by weight or more, or 0.005% by weight or more. The upper limit of the content W2 of the second water-soluble polymer is not particularly limited and can be, for example, 0.1% by weight or less. From the viewpoint of stability in the concentrated solution stage, polishing rate, cleaning ability, etc., in some embodiments, the content W2 of the second water-soluble polymer is preferably 0.05% by weight or less, more preferably 0.02% by weight or less, and even more preferably 0.01% by weight or less.
[0122] The total content of water-soluble polymers in the polishing solution is not particularly limited and, in some embodiments, can be, for example, 0.0001% by weight or more. From the viewpoint of reducing haze, the total content is preferably 0.0005% by weight or more, more preferably 0.001% by weight or more, and even more preferably 0.002% by weight or more, and may be, for example, 0.005% by weight or more. Furthermore, the upper limit of the total content is, for example, 0.5% by weight or less, and from the viewpoint of polishing rate, it is preferably 0.2% by weight or less, more preferably 0.1% by weight or less, and even more preferably 0.05% by weight or less (for example, 0.02% by weight or less, and even more preferably 0.015% by weight or less).
[0123] When a surfactant is included, the amount of surfactant in the polishing solution (the total amount if two or more surfactants are included) is not particularly limited as long as it does not significantly impair the effects of the present invention. Typically, the amount of the surfactant can be, for example, 0.00001% by weight or more from the viewpoint of cleaning performance, etc. From the viewpoint of haze reduction, etc., a preferred amount is 0.0001% by weight or more, more preferably 0.0003% by weight or more, and even more preferably 0.0005% by weight or more. Furthermore, from the viewpoint of polishing rate, etc., it is preferable to have the above amount at 0.1% by weight or less, more preferably 0.01% by weight or less, and even more preferably 0.005% by weight or less (for example, 0.002% by weight or less).
[0124] <Concentrate> The polishing composition disclosed herein may be in a concentrated form (i.e., in the form of a concentrated polishing solution) before being supplied to the substrate. Such a concentrated form of the polishing composition is advantageous in terms of convenience and cost reduction during manufacturing, distribution, and storage. The concentration ratio is not particularly limited and can be, for example, 2 to 100 times by volume, and is usually 5 to 50 times (for example, 10 to 40 times). Such a concentrated solution can be used by diluting it at a desired timing to prepare a polishing solution (working slurry) and supplying the polishing solution to the substrate. The above dilution can be performed, for example, by adding water to the concentrated solution and mixing it.
[0125] When an abrasive composition (i.e., a concentrated solution) is diluted and used for polishing, the abrasive content in the concentrated solution can be, for example, 25% by weight or less. From the viewpoint of dispersion stability and filterability of the abrasive composition, the above content is usually preferably 20% by weight or less, and more preferably 15% by weight or less. In some preferred embodiments, the abrasive content may be 10% by weight or less, or 5% by weight or less. Furthermore, from the viewpoint of convenience and cost reduction during manufacturing, distribution, storage, etc., the abrasive content in the concentrated solution can be, for example, 0.1% by weight or more, preferably 0.5% by weight or more, more preferably 0.7% by weight or more, and even more preferably 1% by weight or more.
[0126] In some embodiments, the content of the basic compound in the concentrate can be, for example, less than 0.25% by weight. From the viewpoint of storage stability, etc., the content is usually preferably 0.15% by weight or less, and more preferably 0.1% by weight or less. Furthermore, from the viewpoint of convenience and cost reduction during manufacturing, distribution, storage, etc., the content of the basic compound in the concentrate can be, for example, 0.005% by weight or more, preferably 0.01% by weight or more, more preferably 0.02% by weight or more, and even more preferably 0.05% by weight or more.
[0127] In some embodiments, the total content of water-soluble polymers in the concentrate can be, for example, 3% by weight or less. From the viewpoint of the filterability and washability of the polishing composition, the content is usually preferably 1% by weight or less, and more preferably 0.5% by weight or less. Furthermore, from the viewpoint of convenience and cost reduction during manufacturing, distribution, storage, etc., the content is usually appropriate to be 0.001% by weight or more, preferably 0.005% by weight or more, and more preferably 0.01% by weight or more.
[0128] In embodiments where the polishing composition contains a surfactant, the surfactant content in the concentrated solution can be, for example, 0.25% by weight or less, preferably 0.15% by weight or less, more preferably 0.1% by weight or less, and may also be 0.05% by weight or less, or 0.025% by weight or less. Alternatively, the surfactant content in the concentrated solution can be, for example, 0.0001% by weight or more, preferably 0.001% by weight or more, more preferably 0.005% by weight or more, and even more preferably 0.01% by weight or more.
[0129] <Preparation of polishing composition> The abrasive compositions used in the technologies disclosed herein may be mono-component, or multi-component, including two-component compositions. For example, the abrasive composition may be configured such that a polishing solution is prepared by mixing part A, which contains at least abrasive grains, and part B, which contains at least a portion of the remaining components, and mixing and diluting these at appropriate times as needed.
[0130] The method for preparing the polishing composition is not particularly limited. For example, the components constituting the polishing composition may be mixed using a well-known mixing device such as a vane-type stirrer, an ultrasonic disperser, or a homomixer. The manner in which these components are mixed is not particularly limited; for example, all components may be mixed at once, or they may be mixed in an order set as appropriate.
[0131] <Application> The polishing compositions disclosed herein can be applied to polishing substrates having various materials and shapes. Substrate materials may include, for example, metals or metalloids such as silicon, aluminum, nickel, tungsten, copper, tantalum, titanium, and stainless steel, or alloys thereof; glassy materials such as quartz glass, aluminosilicate glass, and glassy carbon; ceramic materials such as alumina, silica, sapphire, silicon nitride, tantalum nitride, and titanium carbide; compound semiconductor substrate materials such as silicon carbide, gallium nitride, and gallium arsenide; and resin materials such as polyimide resin. The substrate may also be composed of multiple materials from these. The shape of the substrate is not particularly limited. The polishing compositions disclosed herein can be applied, for example, to polish substrates having flat surfaces, such as plate-shaped or polyhedral substrates, or to polish the edges of substrates (e.g., wafer edge polishing).
[0132] The polishing compositions disclosed herein can be used particularly preferably for polishing surfaces made of silicon materials (typically, for polishing silicon wafers). Specific examples of silicon materials include silicon single crystals, amorphous silicon, and polysilicon. The polishing compositions disclosed herein can be used particularly preferably for polishing surfaces made of silicon single crystals (for example, for polishing silicon wafers).
[0133] The polishing compositions disclosed herein can be preferably applied to a polishing process of a substrate (e.g., a silicon wafer). The substrate may have undergone general treatments that can be applied to the substrate in an upstream process, such as lapping or etching, prior to the polishing process with the polishing compositions disclosed herein.
[0134] The polishing compositions disclosed herein are effective when used in a finishing process of a substrate (e.g., a silicon wafer) or in a polishing process immediately preceding it, and are particularly preferred for use in a finishing polishing process. Here, a finishing polishing process refers to the final polishing process in the manufacturing process of the object (i.e., a process after which no further polishing is performed). The polishing compositions disclosed herein may also be used in polishing processes upstream of finishing polishing (referring to a preliminary polishing process between a rough polishing process and a final polishing process, which typically includes at least a primary polishing process and may further include secondary, tertiary, etc. polishing processes), for example, in a polishing process performed immediately before finishing polishing.
[0135] The polishing compositions disclosed herein are effective, for example, for polishing silicon wafers that have been prepared by an upstream process to a surface roughness of 0.01 nm to 100 nm (typically for finish polishing or polishing immediately preceding it). Application to finish polishing is particularly preferred. The surface roughness Ra of the substrate can be measured, for example, using a laser scanning surface roughness meter "TMS-3000WRC" manufactured by Schmitt Measurement System Inc.
[0136] <Polishing> The polishing compositions disclosed herein can be used for polishing substrates in embodiments including, for example, the following operations. A preferred embodiment of a method for polishing a silicon wafer as a substrate using the polishing compositions disclosed herein will be described below. In other words, a polishing solution containing one of the polishing compositions disclosed herein is prepared. Preparing the polishing solution may involve adjusting the concentration (e.g., dilution) or pH of the polishing composition to prepare the polishing solution. Alternatively, the polishing composition may be used as is as the polishing solution.
[0137] Next, the polishing solution is supplied to the substrate and polished using a conventional method. For example, when performing final polishing of a silicon wafer, typically, the silicon wafer that has undergone the lapping process is set in a general polishing apparatus, and the polishing solution is supplied to the surface of the silicon wafer to be polished through the polishing pad of the apparatus. Typically, while continuously supplying the polishing solution, the polishing pad is pressed against the surface of the silicon wafer to be polished and the two are moved relative to each other (for example, by rotation). Through this polishing process, the polishing of the substrate is completed.
[0138] The polishing pad used in the above polishing process is not particularly limited. For example, polishing pads of foamed polyurethane type, nonwoven fabric type, suede type, etc., can be used. Each polishing pad may or may not contain abrasive grains. Generally, polishing pads that do not contain abrasive grains are preferred.
[0139] A substrate polished using the polishing composition disclosed herein is typically cleaned. Cleaning can be performed using a suitable cleaning solution. The cleaning solution used is not particularly limited, and for example, SC-1 cleaning solution (a mixture of ammonium hydroxide (NH4OH), hydrogen peroxide (H2O2), and water (H2O)), SC-2 cleaning solution (a mixture of HCl, H2O2, and H2O), which are common in fields such as semiconductors, can be used. The temperature of the cleaning solution can be, for example, in the range of room temperature (typically about 15°C to 25°C) or up to about 90°C. From the viewpoint of improving the cleaning effect, a cleaning solution of about 50°C to 85°C can be preferably used.
[0140] As described above, the technologies disclosed herein may include a method for manufacturing a polished product (e.g., a method for manufacturing a silicon wafer) that includes a polishing step (preferably finish polishing) by any of the polishing methods described above, and a polished product (e.g., a silicon wafer) manufactured by said method. [Examples]
[0141] The following describes several embodiments of the present invention, but the present invention is not intended to be limited to those shown in these embodiments. In the following description, "parts" and "%" refer to weight unless otherwise specified.
[0142] <Preparation of polishing composition> (Example 1) A concentrated solution of the polishing composition for each example was prepared by mixing abrasive grains, a basic compound, a water-soluble polymer, a surfactant, and deionized water. Colloidal silica with an average primary particle size of 25 nm was used as the abrasive grain. Ammonia was used as the basic compound. The water-soluble polymer had an Mw of approximately 1.3 × 10⁻⁶. 4 It contains acetalized polyvinyl alcohol (ac-PVA; primary water-soluble polymer, acetalization degree 24 mol%) and vinyl alcohol units and N-vinylpyrrolidone units in a molar ratio of 90:10, with Mw approximately 1.4 × 10⁻⁶. 4 A random copolymer (PVA-r-PVP; second water-soluble polymer) was used. As the surfactant, polyoxyethylene decyl ether (C10EO5) with 5 moles of ethylene oxide added was used. By diluting the concentrated solution of the obtained polishing composition with deionized water at a volume ratio of 40, polishing compositions according to each example were obtained, with a concentration of abrasive grains of 0.08%, a concentration of basic compound of 0.005%, a concentration of ac-PVA of 0.003%, a concentration of PVA-r-PVP of 0.001%, and a concentration of C10EO5 of 0.0006%.
[0143] (Example 2) The second water-soluble polymer has a Mw of approximately 4.9 × 10 4 Poly(N-hydroxyethylacrylamide) (PHEAA) was used. The concentration of PHEAA was set to 0.002%. The polishing composition according to this example was prepared in the same manner as in Example 1.
[0144] (Example 3) As the first water-soluble polymer, alkyl-modified PVA (hydrophobic modified PVA) with an Mw of approximately 6000 is used, and as the second water-soluble polymer, approximately 35 × 10 4 Polyacryloylmorpholine (PACMO) was used. The concentration of PACMO was set to 0.004%. The polishing composition according to this example was prepared in the same manner as in Example 1. The alkyl-modified PVA used in this example is a random copolymer having vinyl alcohol units and n-propyl vinyl ether units in a molar ratio of 85:15.
[0145] (Example 4) The first water-soluble polymer has an Mw of approximately 7.0 × 10 4 Therefore, fully saponified (saponification degree 98% or higher) polyvinyl alcohol (PVA) is used, and the second water-soluble polymer has a Mw of approximately 136 × 10 4 Polyacrylic acid (PAA) was used. The concentration of PVA was set to 0.003% and the concentration of PAA to 0.005%. The polishing composition according to this example was prepared in the same manner as in Example 3.
[0146] (Example 5) The concentration of the basic compound was set to 0.010%. The polishing composition according to this example was prepared in the same manner as in Example 4.
[0147] (Example 6) The concentration of the basic compound was set to 0.015%. The polishing composition according to this example was prepared in the same manner as in Example 4.
[0148] (Comparative Example 1) Poly(vinyl methyl ether) (PVME) was used as the second water-soluble polymer. The concentration of PVME was set to 0.003%. The polishing composition according to this example was prepared in the same manner as in Example 1.
[0149] (Comparative Example 2) As the first water-soluble polymer, a butenediol-vinyl alcohol copolymer (BVOH) with a side chain having a 1,2-diol structure and an Mw of 20,000 is used, and as the second water-soluble polymer, approximately 35 × 10 4 Polyacryloylmorpholine (PACMO) was used. The concentration of BVOH was set to 0.003%, and the concentration of PACMO was set to 0.004%. The polishing composition according to this example was prepared in the same manner as in Example 1. The degree of saponification of the butenediol-vinyl alcohol copolymer was 95% or higher.
[0150] (Comparative Example 3) The first water-soluble polymer has an Mw of approximately 7.0 × 10 4 Therefore, fully saponified (saponification degree of 98% or more) polyvinyl alcohol (PVA) is used, and the second water-soluble polymer has a Mw of approximately 28 × 10 4 Hydroxyethylcellulose (HEC) was used. The concentration of PVA was set to 0.003%, and the concentration of HEC to 0.009%. The concentration of C10EO5 was set to 0.0005%. The polishing composition according to this example was prepared in the same manner as in Example 1.
[0151] <Measuring Zeta Potential> For each polishing composition, the zeta potential ζ [mV] was measured using a zeta potential measuring device under the following conditions. The measuring device used was a Malvern "Zetasizer nano ZSP". The measurement results are shown in the corresponding column of Table 1. [Zeta potential measurement conditions] Dispersion medium: Water Measurement temperature: 25℃ Model: Smoluchowski
[0152] For each polishing composition, the etching rate ER[ nm / h The etching rate was determined based on etching rate measurements. The results are shown in Table 1.
[0153] For each example of polishing composition, the zeta potential ζ [mV] and etching rate ER [ nm / h ] product (ζ×ER)[ pmV / h The value was calculated. The obtained value is shown in the corresponding column of Table 1.
[0154] <Polishing silicon wafers> As the substrate, a commercially available 300mm diameter silicon single crystal wafer (conduction type: P-type, crystal orientation: <100> A silicon wafer was prepared by pre-polishing a COP (Crystal Originated Particle: crystal defect-free) wafer according to the following polishing condition 1. Pre-polishing was performed using a polishing solution containing 0.6% abrasive particles (colloidal silica with an average primary particle size of 35 nm) and 0.08% tetramethylammonium hydroxide (TMAH) in deionized water.
[0155] [Polishing conditions 1] Polishing equipment: Single-wafer polishing machine manufactured by Okamoto Machine Tool Works, model "PNX-332B" Grinding load: 20kPa Plate rotation speed: 20 rpm Head (carrier) rotation speed: 20 rpm Polishing pad: Manufactured by Fujibo Ehime Co., Ltd., product name "FP55" Polishing fluid supply rate: 1.0 L / min Polishing solution temperature: 20℃ Surface plate cooling water temperature: 20℃ Polishing time: 2 min
[0156] The polishing compositions prepared in each of the above examples were used as polishing solutions, and the silicon wafers after the preliminary polishing were polished under the following polishing conditions 2.
[0157] [Polishing conditions 2] Polishing equipment: Single-wafer polishing machine manufactured by Okamoto Machine Tool Works, model "PNX-332B" Grinding load: 20kPa Plate rotation speed: 52 rpm Head (carrier) rotation speed: 50 rpm Polishing pad: Manufactured by Fujibo Ehime Co., Ltd. Product name: "POLYPAS275NX" Polishing fluid supply rate: 1.5 L / min Polishing solution temperature: 20℃ Surface plate cooling water temperature: 20℃ Polishing time: 4 min
[0158] The polished silicon wafer was removed from the polishing apparatus, and cleaned using a cleaning solution of NH4OH (29%):H2O2 (31%):deionized water (DIW) = 2:5.3:48 (volume ratio) (SC-1 cleaning). More specifically, a first cleaning tank equipped with an ultrasonic oscillator was prepared, the cleaning solution was contained in the first cleaning tank and maintained at 70°C, and the polished silicon wafer was immersed in the cleaning tank for 6 minutes. Thereafter, after being immersed for 15 minutes in a second cleaning tank containing deionized water (DIW) at 25°C, the silicon wafer was immersed again in the first cleaning tank for 6 minutes and in the second cleaning tank for 16 minutes, and then the silicon wafer was dried.
[0159] <LPD-N and Haze Line Measurement> The number of LPD-N present on the surface of the cleaned silicon wafer and the haze line were measured using a wafer inspection apparatus manufactured by KLA-Tencor Corporation, trade name "Surfscan SP5", in the DC mode of the apparatus. The measured number of LPD-N is shown in Table 1. In addition, values obtained by converting the measured haze lines into relative values with the haze line of Comparative Example 1 set to 10000 are shown in Table 1. Note that LPD-N refers to Light Point Defect Non-cleanable. Further, the haze line refers to the total area of micro-scratches within the measurement area, which is measured by the above inspection apparatus.
[0160] The summary of each example and the evaluation results are shown in Table 1. In the table, "-" indicates that measurement is impossible or not performed.
[0161] [Table 1]
[0162] As shown in Table 1, in a polishing composition comprising silica particles, a basic compound, and water, the polishing composition contains a polyvinyl alcohol-based polymer as the first water-soluble polymer, and a second water-soluble polymer having a chemical structure different from that of the first water-soluble polymer, and the zeta potential ζ [mV] and the etching rate ER nm / h product (ζ×ER) is -900 pmV / h or more and -90 pmV / h According to the polishing compositions of Examples 1 to 6 below, the above (ζ×ER) is -90 pmV / h Compared to the polishing compositions of Comparative Examples 1-3, which were larger than the above, both the number of LPD-Ns and the haze lines were significantly reduced, resulting in high surface quality.
[0163] Although specific examples of the present invention have been described in detail above, these are merely illustrative and do not limit the scope of the claims. The technologies described in the claims include various modifications and changes to the specific examples illustrated above.< / ph>
Claims
1. It contains silica particles (A) as abrasive grains, a basic compound (B), a first water-soluble polymer (C1), a second water-soluble polymer (C2), and water (D). The first water-soluble polymer (C1) is a polyvinyl alcohol-based polymer, The etching rate measurements below: (1) Prepare the polishing composition as the etching rate measuring chemical solution LE; (2) NH at 25℃ 4 OH (29%): H 2 O 2 A silicon single crystal substrate (rectangular in shape, 6 cm long, 3 cm wide, and 775 μm thick) is prepared by immersing it for 1 minute in a washing solution of (31%):deionized water (DIW) = 2:5.3:48 (volume ratio), and then immersing it for 30 seconds in a 5% aqueous solution of hydrogen fluoride (HF) at 25°C, and its mass W0 is measured; (3) Immerse the silicon single crystal substrate in the chemical solution LE at 25°C for 48 hours; (4) Remove the silicon single crystal substrate from the chemical solution LE and heat it at 25°C in NH 4 OH (29%): H 2 O 2 (31%): Wash for 10 seconds with a washing solution of deionized water (DIW) = 1:1:8 (volume ratio); (5) Measure the mass W1 of the silicon single crystal substrate after cleaning; and (6) Calculate the etching rate [nm / h] from the difference between W0 and W1 and the specific gravity of the silicon single crystal substrate; The etching rate ER [nm / h] of the polishing composition based on the above, The polishing composition wherein the product of the zeta potential ζ [mV] of the polishing composition and (ER × ζ) is -900 pmV / h or more and -90 pmV / h or less.
2. The polishing composition according to claim 1, wherein the first water-soluble polymer (C1) is at least one selected from the group consisting of unmodified polyvinyl alcohol with a degree of saponification of 70% or more; acetalized polyvinyl alcohol-based polymers; and polyvinyl alcohol-based polymers containing repeating units derived from alkyl vinyl ethers.
3. The polishing composition according to claim 1 or 2, wherein the content of the first water-soluble polymer (C1) is 0.5 parts by weight or more and 10 parts by weight or less per 100 parts by weight of the abrasive grains.
4. The polishing composition according to claim 1 or 2, wherein the second water-soluble polymer (C2) is at least one selected from the group consisting of a polyvinyl alcohol-based polymer having a different chemical structure from the first water-soluble polymer (C1); a polymer containing a nitrogen atom; and a polymer containing (meth)acrylic acid units.
5. The polishing composition according to claim 4, wherein the polymer containing the nitrogen atom is a polymer containing a chain-like amide having an N-(meth)acryloyl group as a monomer unit.
6. The polishing composition according to claim 1 or 2, wherein the content of the second water-soluble polymer (C2) is 0.5 parts by weight or more and 10 parts by weight or less per 100 parts by weight of the abrasive grains.
7. The polishing composition according to claim 1 or 2, further comprising a surfactant (E).
8. The polishing composition according to claim 7, wherein the surfactant (E) is a nonionic surfactant.
9. A polishing composition according to claim 1 or 2, used for polishing surfaces made of silicon material.
10. A concentrated solution of the polishing composition according to claim 1 or 2.
Citation Information
Patent Citations
Epoxy resin molding material for encapsulation of semiconductor device
JP1986085432A
JP1987032243A
Panel unconnection detecting system
JP1988048927A
Polishing composition, manufacturing method of polishing composition and kit for manufacturing polishing composition
JP2016166343A
Polishing composition, method for producing polishing composition and kit for preparing polishing composition
JP2019151849A