Process for transferring a single-crystal SiC layer to a polycrystalline SiC carrier using a polycrystalline SiC interlayer.
By forming a polycrystalline SiC layer and implanting ions to create a fragile surface, the process addresses bonding challenges between SiC substrates, ensuring defect-free and conductive interfaces for improved power device performance.
Patent Information
- Application Number
- JP2024519335
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-05
- Filing Date
- 2022-10-03
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-10-03
AI Technical Summary
High-quality direct bonding between monocrystalline SiC and polycrystalline SiC substrates is difficult due to surface finish complexity and roughness, leading to bonding defects and reduced electrical conductivity, and existing methods like SAB and ADB generate unstable interfaces.
A process involving forming a polycrystalline SiC layer on a donor substrate, implanting ions to create a fragile surface, and transferring a thin single-crystal SiC layer onto a polycrystalline SiC carrier substrate, ensuring a direct bond without intermediate layers and similar crystal structures for improved adhesion.
This process enhances the reliability and performance of power devices by eliminating bonding defects and maintaining high electrical conductivity at the interface.
Smart Images

Figure 0007954708000001 
Figure 0007954708000002 
Figure 0007954708000003
Abstract
Description
TECHNICAL FIELD
[0001] The field of the invention is that of semiconductor materials for microelectronic components. The present invention relates more particularly to a process for manufacturing a composite structure comprising a thin layer of monocrystalline silicon carbide on a carrier substrate made of polycrystalline silicon carbide. BACKGROUND ART
[0002] Silicon carbide (SiC) is being used more and more widely in power electronics applications to meet the growing range of needs in electronics, such as in electric vehicles in particular. Power devices and integrated power systems based on monocrystalline SiC can indeed manage much higher power densities than their conventional silicon equivalents, and do so in active regions of smaller size.
[0003] Nevertheless, monocrystalline SiC substrates for the microelectronics industry remain expensive and difficult to supply in large sizes. It is therefore preferable to use a layer transfer solution to fabricate composite structures comprising a thin layer of monocrystalline SiC on a typically lower-cost carrier substrate. One well-known thin layer transfer solution is the Smart Cut™ process, which is based on implanting light ions and bonding by direct bonding. Such a process makes it possible to manufacture a composite structure comprising a thin layer made of monocrystalline SiC, taken from a donor substrate made of monocrystalline SiC, in direct contact with a carrier substrate made of polycrystalline SiC, for example.
[0004] Nevertheless, achieving high-quality direct bonding by molecular adhesion between two substrates made of monocrystalline SiC and polycrystalline SiC remains difficult due to the complexity of managing the surface finish and roughness of said substrates.
[0005] The target applications require good thermal and electrical conductivity between thin layers made from single-crystal SiC and carrier substrates made from polycrystalline SiC. Furthermore, the presence of bonding defects at the bonding interface is highly detrimental to the quality of structures fabricated in thin layers made from single-crystal SiC. For example, a lack of adhesion between the two surfaces at a bonding defect can lead to local separation of the thin layer at that location during its transfer from the single-crystal SiC substrate to the polycrystalline SiC substrate.
[0006] Two solutions for achieving bonding of two substrates made from single-crystal SiC and polycrystalline SiC have been reported in the literature, but there is no evidence available today regarding their effectiveness on an industrial scale. Therefore, on the one hand, there is surface-activated bonding (SAB), which typically involves activating the surfaces to be bonded by argon shock, and on the other hand, atomic diffusion bonding (ADB), which involves ultrathin layer sputter deposition and bonding under ultra-high vacuum. These solutions have the disadvantage of generating an unstable layer at the bonding interface that can cause bonding defects and adversely affect electrical conductivity. [Disclosure of the Invention]
[0007] The object of the present invention is to provide a composite structure comprising a thin layer made from very high-quality single-crystal SiC, and in particular to provide a technique for overcoming these drawbacks in order to improve the performance and reliability of power devices intended to be fabricated in said thin layer.
[0008] For this purpose, the present invention provides a process for manufacturing a composite structure comprising a thin layer of single-crystal SiC disposed on a polycrystalline silicon carbide (SiC) carrier substrate, The steps include forming a polycrystalline SiC layer on a donor substrate, at least the surface portion of which is made from single-crystal SiC, Before or after the above-mentioned forming step, a step of implanting ion species into the surface portion of the donor substrate to form a fragile surface that defines the thin single-crystal SiC layer to be transferred, A step of joining a donor substrate and a polycrystalline SiC carrier substrate after the injection step and the forming step, wherein the polycrystalline SiC layer is at the bonding interface, and a step of separating the donor substrate along a fragile surface so as to transfer the polycrystalline SiC layer and a thin single-crystal SiC layer onto the polycrystalline SiC carrier substrate. It provides a process that includes this.
[0009] Specific preferred but non-limiting aspects of this process are as follows: The polycrystalline SiC layer has the same polytype as the carrier substrate. The step of forming a polycrystalline SiC layer includes the deposition of polycrystalline SiC. Polycrystalline SiC is deposited by chemical vapor deposition. Polycrystalline SiC deposition is carried out at temperatures below 1000°C. The step of forming a polycrystalline SiC layer includes depositing an amorphous SiC layer and recrystallization annealing applied to the amorphous SiC layer. The polycrystalline SiC layer deposited on the donor substrate has a thickness between 10 nm and 10 μm. This process includes thinning and / or polishing the surface of the polycrystalline SiC layer intended to be at the bonding interface during the bonding step and / or the surface of the carrier substrate intended to be at the bonding interface during the bonding step. This process further includes forming bonding layers on each of the donor and carrier substrates, wherein the bonding step is performed by direct bonding of the thus formed bonding layers. The bonding layer formed on the donor substrate and the carrier substrate, respectively, is a metal layer, for example, a tungsten layer or a titanium layer. The junction layer formed on the donor substrate and the carrier substrate, respectively, is a layer of silicon, carbon, or silicon carbide. The bonding layer has a melting point below the annealing temperature applied during the bonding step.
[0010] Other aspects, purposes, advantages, and features of the present invention will become more apparent by reading the following detailed description of preferred embodiments, which are given as non-limiting examples and with reference to the accompanying drawings. [Brief explanation of the drawing]
[0011] [Figure 1] This is a schematic cross-sectional view of a single-crystal SiC donor substrate. [Figure 2] This is a schematic cross-sectional view of the deposition of a polycrystalline SiC layer on the surface of a single-crystal SiC donor substrate. [Figure 3] This is a schematic cross-sectional view of the formation of a fragile surface in the donor substrate shown in Figure 1 by implanting ion species, for defining the thin single-crystal SiC layer to be transferred. [Figure 4] Figure 2 is a schematic cross-sectional view of the coupling between the donor substrate and the carrier substrate. [Figure 5] This is a schematic cross-sectional view of the separation along the fragile surface of a donor substrate for transferring a thin single-crystal SiC layer to a carrier substrate. [Modes for carrying out the invention]
[0012] (Detailed disclosure of specific embodiments) The present invention relates to a process for manufacturing a composite structure comprising a thin layer of single-crystal SiC disposed on a polycrystalline SiC carrier substrate. The process includes transferring a thin layer of single-crystal SiC from a donor substrate, whose at least surface portion is made of single-crystal SiC, to a carrier substrate according to the Smart Cut® process.
[0013] The donor substrate may be a bulk substrate of single-crystal SiC. In other embodiments, the donor substrate may be a composite substrate comprising a surface layer of single-crystal SiC and at least one other layer of another material. In this case, the single-crystal SiC layer has a thickness of 0.5 μm or more.
[0014] According to the present invention, preparation for forming a polycrystalline SiC layer on a donor substrate is performed before bonding with a polycrystalline SiC carrier substrate. In this way, the bonding interface is created between materials having the same morphology (i.e., two polycrystalline SiC) instead of the dissimilar crystal structures of the prior art (i.e., single-crystal SiC added to polycrystalline SiC). Accordingly, the drawbacks associated with bonding these dissimilar crystal structures are avoided. In particular, the present invention makes it possible not to create a conduction barrier at the bonding interface and to have a contact area that is not reduced by the formation of voids at this interface.
[0015] Referring to Figure 1, the process according to the present invention starts with the preparation of a donor substrate 10, at least the surface portion of which is made of single-crystal SiC. In the figure, a bulk substrate 10 of single-crystal SiC is shown.
[0016] Referring to Figure 2, the process includes the step of forming a polycrystalline SiC layer 11 on the donor substrate 10. The polycrystalline SiC layer 11 formed on the donor substrate preferably has a thickness between 10 nm and 10 μm, more preferably a thickness of less than 50 nm.
[0017] The grain size of the polycrystalline SiC layer 11 is preferably less than 30 nm, more preferably less than 10 nm, which makes it possible to limit the surface roughness of the layer 11 deposited in this way. Such a reduction in grain size further provides the advantage that the conditions for forming the polycrystalline SiC layer 11 can approach the conditions for an amorphous SiC layer, and the layer 11 thus formed can be a mixture of small grains and a high proportion of amorphous SiC without being detrimental to the effects of the present invention.
[0018] Silicon carbide has various crystal forms (also called polytypes). The most common are the 4H form, 6H form and 3C form. Preferably, the formation of the polycrystalline SiC layer 11 is performed so as to provide the same polytype as that of the carrier substrate 20, generally the 3C polytype.
[0019] In one possible embodiment, the polycrystalline SiC layer is formed by deposition of polycrystalline SiC. Such deposition of the polycrystalline SiC layer may be physical vapor deposition (for example, of the EBPVD [Electron Beam Physical Vapor Deposition] type) or chemical vapor deposition (for example, of the DLI-CVD [Direct Liquid Injection Chemical Vapor Deposition] type). In one possible embodiment, the deposition of the polycrystalline SiC layer is performed at a temperature below 1000°C, preferably below 900°C, more preferably below 850°C. This embodiment has been found to be particularly suitable when the deposition of the polycrystalline SiC layer 11 is performed after the implantation of ionic species described below for forming a weakened plane in the donor substrate. This relatively low temperature makes it possible in particular to limit the growth of cavities present in the weakened plane, which growth, in the absence of a reinforcing effect imparted to the donor substrate, leads to deformation of the layer that directly coincides with the appearance of cavities and blistering phenomena.
[0020] In a variant of one embodiment that may be used particularly when the implantation of the ionic species described below is performed after the formation of the polycrystalline SiC layer 11, the formation of the polycrystalline SiC layer first comprises the deposition of a (completely or partially) amorphous SiC layer, followed by a recrystallization anneal, typically at a temperature above 1100°C, which converts the amorphous SiC layer into the polycrystalline material constituting the polycrystalline SiC layer 11.
[0021] In one possible embodiment, the formation of the polycrystalline SiC layer 11 involves the formation of bonding layers, for example layers of silicon, carbon or silicon carbide, or metal layers such as layers of tungsten or titanium, on the polycrystalline SiC layer 11 and on the carrier substrate respectively. The bonding layer may be formed according to a physical vapor deposition (PVD) process using argon or an argon / nitrogen or argon / propane mixture as the gas for targeted ablation. The bonding layer preferably has a melting point below the temperature of the anneal applied during the bonding step. Thus, for example, a bonding layer made of silicon or titanium is selected when an anneal at a temperature on the order of 1700°C / 1800°C is applied during the bonding step.
[0022] Referring to Figure 3, the process further includes implanting ion species into the donor substrate 10 to form a fragile surface 13 that defines a thin single-crystal SiC layer 12 to be transferred, either before or after the formation of the polycrystalline SiC layer 11. In the figure, the implantation is performed after the deposition of the polycrystalline SiC layer 11.
[0023] The injected species typically contains hydrogen and / or helium. Those skilled in the art can define the required injection dose and energy.
[0024] When the donor substrate is a composite substrate, the injection is performed in such a way that a brittle surface is formed on the surface layer of the single-crystal SiC of the donor substrate.
[0025] Preferably, the thin layer 12 of single-crystal SiC has a thickness of less than 1 μm. Specifically, such a thickness is achievable on an industrial scale using the Smart Cut™ process. In particular, injection devices available in industrial manufacturing lines make it possible to achieve such injection depths.
[0026] Referring to Figure 4, the process includes bonding the donor substrate and the carrier substrate after the injection and formation. The bonding is a direct bond without an intermediate electrical insulating layer, obtained by molecular adhesion of the contacting surfaces. The bonding is typically carried out at ambient temperature. The bonding is preferably carried out under vacuum.
[0027] During this bonding process, the previously formed polycrystalline SiC layer 11 on the donor substrate is located at the bonding interface. The expression "layer at the bonding interface" is understood to mean a layer on the side of the donor substrate that is bonded to the carrier substrate, but does not necessarily imply direct contact between the layer and the carrier substrate. Therefore, the layer may be directly bonded to the carrier substrate or covered by a bonding layer such as the aforementioned bonding layer on which bonding takes place. Bonding by direct contact of polycrystalline layers has the advantage of physically separating the interface between the single-crystal SiC and polycrystalline SiC at the bonding interface.
[0028] Prior to this bonding, operations are typically performed to prepare the surfaces to be bonded, for example, two polycrystalline SiC surfaces in this case, such as precision polishing, wet or dry cleaning, and surface activation. In particular, the process may include thinning and / or polishing of the surface of the polycrystalline SiC layer 11 intended to be at the bonding interface during bonding, and / or the surface of the carrier substrate 20 intended to be at the bonding interface during bonding.
[0029] Referring to Figure 5, the process then includes separating the donor substrate 10 along the fragile surface 13 so as to transfer a polycrystalline SiC layer 11 and a thin single-crystalline SiC layer 12 onto the carrier substrate 20. In known methods, this separation can be caused by heat treatment, mechanical action, or a combination of these means. The remaining 10' of the donor substrate can be preferentially recycled for another use.
[0030] Next, one or more finishing operations can be applied to the transferred single-crystal SiC layer 12. For example, smoothing, cleaning, and even polishing, such as chemical mechanical polishing (CMP) or fine polishing, can be performed to remove defects related to ion species implantation and reduce the roughness of the transferred single-crystal SiC layer 12 (this makes it possible to eliminate the need for preferential chemical etching for certain particle orientations).
Claims
1. A process for manufacturing a composite structure comprising a thin layer (12) of single-crystal SiC disposed on a polycrystalline silicon carbide (SiC) carrier substrate (20), The steps include forming a polycrystalline SiC layer (11) on a donor substrate (10) whose surface portion is made of single-crystal SiC, Before or after the forming step, the step of implanting ion species into the surface portion of the donor substrate (10) to form a fragile surface (13) that defines the thin single-crystal SiC layer (12) to be transferred, A step of joining the donor substrate (10) and the polycrystalline SiC carrier substrate (20) after the injection step and the forming step, wherein the polycrystalline SiC layer (11) is at the joining interface, and a step of separating the donor substrate (10) along the fragile surface (13) so as to transfer the polycrystalline SiC layer (11) and the thin single-crystal SiC layer (12) onto the polycrystalline SiC carrier substrate (20). Includes, A process further comprising forming a bonding layer on each of the donor substrate and the carrier substrate, wherein the bonding step is performed by direct bonding of the thus formed bonding layers.
2. The process according to claim 1, wherein the polycrystalline SiC layer (11) has the same polytype as the carrier substrate (20).
3. The process according to claim 1 or 2, wherein the step of forming the polycrystalline SiC layer (11) includes the deposition of polycrystalline SiC.
4. The process according to claim 3, wherein the deposition of polycrystalline SiC is chemical vapor deposition.
5. The process according to claim 3, wherein the deposition of polycrystalline SiC is carried out at a temperature of less than 1000°C.
6. The process according to claim 1 or 2, wherein the step of forming the polycrystalline SiC layer (11) includes depositing an amorphous SiC layer and recrystallizing annealing applied to the amorphous SiC layer.
7. The process according to claim 1 or 2, wherein the polycrystalline SiC layer (11) formed on the donor substrate has a thickness between 10 nm and 10 μm.
8. The process according to claim 1 or 2, further comprising thinning and / or polishing the surface of the polycrystalline SiC layer (11) intended to be at the bonding interface during the bonding step and / or the surface of the carrier substrate (20) intended to be at the bonding interface during the bonding step.
9. The process according to claim 1 or 2, wherein the bonding layer formed on each of the donor substrate and the carrier substrate is a metal layer.
10. The process according to claim 1 or 2, wherein the bonding layer formed on each of the donor substrate and the carrier substrate is a layer of silicon, carbon, or silicon carbide.
11. The process according to claim 1 or 2, wherein the bonding layer has a melting point below the annealing temperature applied during the bonding step.
Citation Information
Patent Citations
Silicon carbide thin film and production of silicon carbide thin film laminated substrate
JP1997052797A
Method for manufacturing a composite structure comprising a thin layer of monocrystalline sic on a carrier substrate of polycrystalline sic
WO2021019137A1