Packaging materials for secondary batteries

A laminated structure with a heat-resistant resin film, metal foil gas barrier, and thermoplastic polyolefin inner layer with specific thermal properties addresses thermal and mechanical challenges in secondary battery packaging, enhancing heat-sealability and stability.

JP7954712B2Active Publication Date: 2026-11-20LOTTE CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024525312
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-11-05
Filing Date
2022-09-27
Publication Date
2026-11-20
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

Existing secondary battery packaging materials face issues with thermal stability, shape stability, and susceptibility to damage due to exposure of aluminum layers, leading to potential corrosion and leakage, especially in high-temperature environments.

Method used

A laminated structure comprising a heat-resistant resin film outer layer, a metal foil gas barrier layer, and an inner layer made of a thermoplastic polyolefin composition with specific thermal characteristics, including at least three endothermic peaks between 90 to 180°C, and a composition containing acid-modified polypropylene for improved heat resistance and dimensional stability.

Benefits of technology

The packaging material exhibits improved heat-sealability, heat resistance, and shape stability, reducing the risk of corrosion and leakage, even in high-temperature conditions, while maintaining mechanical integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954712000002
    Figure 0007954712000002
  • Figure 0007954712000003
    Figure 0007954712000003
  • Figure 0007954712000004
    Figure 0007954712000004
Patent Text Reader

Abstract

The present invention provides a packaging material for secondary batteries having a laminated structure of an outer layer made of a heat-resistant resin film, a metal foil gas barrier layer, and an inner layer made of a composition containing a thermoplastic polyolefin, which can be heat-sewn under low heat-sewn temperature conditions and exhibits improved heat resistance and shape stability in a high-temperature environment.The present invention provides a packaging material for secondary batteries having a laminated structure of an outer layer made of a heat-resistant resin film, a metal foil gas barrier layer, and an inner layer made of a composition containing a thermoplastic polyolefin, which is characterized in that the composition constituting the inner layer has at least three endothermic peaks in a temperature-calorie curve when measured by a thermal fractionation analysis method (Successive Self-nucleation and Annealing (SSA) using a Differential Scanning Calorimetry (DSC)), and the endothermic peaks appear in the range of 90 to 180°C.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a packaging material for secondary batteries, and more specifically, to a packaging material for secondary batteries having a structure in which an outer layer, a metal foil gas barrier layer, and an inner layer are laminated.

[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2021-0151769 filed on November 5, 2021, the entire content of which is incorporated herein by reference. BACKGROUND ART

[0003] Secondary batteries generally refer to lithium secondary batteries, which are batteries used in portable terminal devices such as notebook computers, smartphones, tablet PCs and video cameras, electric vehicles including hybrid vehicles, smart grids for energy storage, and the like, and research is being carried out to achieve miniaturization, weight reduction and thinning, as well as to overcome various environmental factors such as severe thermal environments and mechanical impacts.

[0004] Unlike conventional can-type packaging materials, rechargeable battery pouches are used as outer packaging materials for lithium batteries because they have the advantage of being able to freely change the shape of the battery. These pouches consist of a multilayer structure (for example, an internal resin layer, an aluminum layer, and an external resin layer). Typically used rechargeable battery pouch films are composed of a multilayer film structure consisting of an internal resin layer made of polyolefins such as polyethylene (PE), casted polypropylene (cPP), and polypropylene (PP), or copolymers thereof, which have heat-adhesive properties and act as a sealant; an aluminum layer, which is a metal foil that maintains mechanical strength and acts as a barrier layer against moisture and oxygen; and an external resin layer formed by a functional polymer film such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), nylon, or liquid crystal polymer (LCP) to protect the battery cells from external impacts.

[0005] Traditionally, packaging materials made from metal, particularly aluminum, pressed and shaped into cylinders or parallelepipeds were primarily used. However, with such metal can packaging materials, the outer wall of the container is rigid, and the shape of the battery itself is determined by the shape of the metal can packaging material, which presents a limitation.

[0006] To overcome these constraints, technologies for packaging materials made of multilayer plastic films have been developed. For example, Patent Document 1 discloses a cell pouch consisting of a base layer, an adhesive layer, a barrier layer, a dry lamination layer, and a sealant layer, in which the sealant layer is composed of a low-flow polypropylene layer and a high-flow polypropylene layer. Patent Document 2 discloses a cell pouch laminated using biaxially oriented nylon, polyethylene terephthalate (PET), and polyolefin resin for the base film and surface protective layer, as well as a technology for coating the base film with a fluorine-based, silicone-based, or acrylic resin as a secondary processing step.

[0007] Pouch-type rechargeable batteries offer flexibility in form and have the advantage of realizing rechargeable batteries of the same capacity in a smaller volume and mass. However, unlike can-type batteries, pouch-type batteries use a soft pouch as a container, which can be damaged for various reasons during various processes. For example, during the process of housing the electrode assembly inside the pouch, protruding parts such as electrode tabs and electrode leads can cause damage such as cracks in the PP or cPP layers inside the pouch. If the aluminum layer is exposed due to such damage, side reactions can occur due to its reactivity with the electrolyte. The aluminum layer exposed to the electrolyte in this way can corrode as it chemically reacts with oxygen or moisture in the electrolyte that has penetrated or diffused into the battery. This can lead to the problem of swelling, where corrosive gases are generated and the inside of the battery expands. Specifically, lithium hexafluoride phosphate (LIPF6) reacts with water and oxygen to produce hydrofluoric acid (HF), a corrosive gas. Such hydrofluoric acid can react with aluminum to cause a rapid exothermic reaction. In a secondary reaction, it can be adsorbed onto the aluminum surface and penetrate into the tissue, increasing the brittleness of the tissue. This can lead to cracks in the pouch film even with minor impacts, and leakage of the electrolyte can cause lithium to react with the atmosphere, potentially leading to ignition.

[0008] Patent Document 3 describes a polymer film for cell packaging containing 1 to 30% by weight of low-density polyethylene (LDPE), 50 to 98% by weight of polypropylene (PP), and 1 to 20% by weight of a crosslinked resin. It states that LDPE is used to reduce the penetration rate of the electrolyte, PP is used to complement the heat resistance, and a crosslinked resin is used to improve the compatibility of LDPE and PP. However, it does not go into detail about changes in physical properties due to molecular weight, density, melting point, degree of crystallinity, comonomer content, etc.

[0009] Patent Document 4 discloses a battery packaging material consisting of a laminate in which a base layer, a metal layer, and a sealant layer are sequentially laminated, wherein the sealant layer contains multiple types of fatty acid amide lubricants, and at least one of the fatty acid amide lubricants is a saturated fatty acid amide. However, when using an extrusion lamination process, the fatty acid amide may volatilize, potentially causing the loss of sleep characteristics.

[0010] Patent Document 5 discloses a resin composition for a sealant layer of a battery packaging material in which the first sealant layer is formed by an acid-modified polyolefin and the second sealant layer is a polyolefin resin having an isotactic fraction (mm) of 99% or less. However, since the isotactic fraction of commercially available or synthesizable polyolefin resins cannot exceed 99%, it is difficult to specifically identify the category of polyolefin resins having an isotactic fraction (mm) of 99% or less. [Prior art documents] [Patent Documents]

[0011] [Patent Document 1] Korean Published Patent No. 2003-0029141 [Patent Document 2] Korean Published Patent No. 2002-0030737 [Patent Document 3] Korean Registered Patent No. 1499740 [Patent Document 4] Japanese Registered Patent No. 6808966 [Patent Document 5] Japanese Registered Patent No. 5761278 [Overview of the Initiative] [Problems that the invention aims to solve]

[0012] The present invention aims to provide a secondary battery packaging material comprising a laminated structure including an outer layer made of a heat-resistant resin film, a metal foil gas barrier layer, and an inner layer made of a composition containing a thermoplastic polyolefin, which allows for thermal suturing at low thermal suturing temperature conditions and exhibits improved heat resistance and dimensional stability in high-temperature environments. [Means for solving the problem]

[0013] To solve the aforementioned problems, the present invention provides a packaging material for secondary batteries comprising a laminated structure including an outer layer made of a heat-resistant resin film, a metal foil gas barrier layer, and an inner layer made of a composition containing a thermoplastic polyolefin, wherein the composition forming the inner layer has at least three endothermic peaks in the temperature-calorimetry curve when measured using a thermal fractionation analysis method (Successive Self-nucleation and Annealing, SSA) with a differential scanning calorimetry (DSC), and the endothermic peaks appear in the range of 90 to 180°C.

[0014] Furthermore, the inner layer composition is characterized in that, when analyzed by the thermal fractionation analysis method, the region containing endothermic peaks below 100°C does not exceed 10%, and the region containing endothermic peaks above 150°C exceeds 20% but is less than 90%.

[0015] Furthermore, the present invention provides a packaging material for secondary batteries characterized in that the composition forming the inner layer contains at least one type of acid-modified polypropylene.

[0016] Furthermore, the acid-modified polypropylene is a modified polypropylene grafted with maleic anhydride at a content of 1 to 10% by weight, so as to provide a packaging material for secondary batteries.

[0017] Furthermore, the heat-resistant resin is a polyamide-based resin or a polyester-based resin, so as to provide a packaging material for secondary batteries.

[0018] Furthermore, the metal foil contains one or more metals selected from the group consisting of aluminum (Al), iron (Fe), copper (Cu), nickel (Ni), tin (Sn), zinc (Zn), indium (In), and tungsten (W), so as to provide a packaging material for secondary batteries.

[0019] Furthermore, the thickness of the outer layer is 15 to 30 μm, the thickness of the metal foil gas barrier layer is 25 to 45 μm, and the thickness of the inner layer is 25 to 120 μm, so as to provide a packaging material for secondary batteries. [Effects of the Invention]

[0020] According to the present invention, in a packaging material for secondary batteries comprising a laminated structure of an outer layer made of a heat-resistant resin film, a metal foil gas barrier layer, and an inner layer made of a composition containing a thermoplastic polyolefin, by exhibiting specific thermal characteristics when the thermal fractionation analysis method using a differential scanning calorimeter is performed on the composition forming the inner layer, it is possible to provide a packaging material for secondary batteries that can be heat-sealed under low heat-sealing temperature conditions, and exhibits improved heat resistance and shape stability in a high-temperature environment. [Brief Description of the Drawings]

[0021] [Figure 1] This is a graph exemplarily showing a case that does not exhibit triple or more melting behavior in the measurement result of the thermal fractionation analysis method (SSA) using a differential scanning calorimeter (DSC). [Figure 2] This is a graph exemplarily showing the heat treatment process in the thermal fractionation analysis method (SSA) using a differential scanning calorimeter (DSC). [Figure 3]This is a graph exemplarily showing cases that exhibit melting behavior of three or more peaks in the measurement results of the thermal fractionation analysis method (SSA) using a differential scanning calorimeter (DSC). [Figure 4] This is a graph showing the measurement results of the thermal fractionation analysis method (SSA) using a differential scanning calorimeter (DSC) for the inner layer in Example 1. [Figure 5] This is a graph showing the measurement results of the thermal fractionation analysis method (SSA) using a differential scanning calorimeter (DSC) for the inner layer in Example 2. [Figure 6] This is a graph showing the measurement results of the thermal fractionation analysis method (SSA) using a differential scanning calorimeter (DSC) for the inner layer in Example 3. [Figure 7] This is a graph showing the measurement results of the thermal fractionation analysis method (SSA) using a differential scanning calorimeter (DSC) for the inner layer in Example 4. [Figure 8] This is a graph showing the measurement results of the thermal fractionation analysis method (SSA) using a differential scanning calorimeter (DSC) for the inner layer in Comparative Example 1. [Figure 9] This is a graph showing the measurement results of the thermal fractionation analysis method (SSA) using a differential scanning calorimeter (DSC) for the inner layer in Comparative Example 2. [Modes for Carrying Out the Invention]

[0022] Hereinafter, the present invention will be described in detail through preferred examples. Before that, the terms and words used in this specification and the claims must not be construed as limited to their ordinary or dictionary meanings. Based on the principle that the inventor may appropriately define the concept of terms to describe their invention in the best way, they should be construed with the meaning and concept consistent with the technical idea of the present invention. Therefore, the configurations of the examples described in this specification are merely the most preferred embodiment of the present invention, and do not represent the entire technical idea of the present invention. Thus, it should be understood that various equivalents and modifications that may replace these may exist at the time of filing of the present application.

[0023] The present invention discloses a packaging material for lithium secondary batteries, characterized in that it has a structure in which an outer layer made of a heat-resistant resin film, a metal foil gas barrier layer, and an inner layer made of a composition containing a thermoplastic polyolefin are laminated, and the temperature-caloric curve measured for the composition constituting the inner layer by thermal fractionation analysis (SSA) using nucleation / annealing with a differential scanning calorimeter (DSC) has at least three endothermic peaks, the endothermic peaks appear in the range of 90 to 180°C.

[0024] The inner layer is a layer made of a composition containing a thermoplastic polyolefin that is the innermost layer of the secondary battery packaging material and comes into contact with the electrolyte of the battery, and is thermally bonded for the purpose of sealing the lithium secondary battery.

[0025] The composition containing the thermoplastic polyolefin as the inner layer of the lithium secondary battery packaging material according to the present invention is characterized by having at least three endothermic peaks in the temperature-calorimetry curve when measured by thermal fractionation analysis (SSA) using a differential scanning calorimeter (DSC). In other words, in the lithium secondary battery packaging material according to the present invention, the composition containing the thermoplastic polyolefin as the inner layer exhibits melting behavior at three or more peaks, which can be observed with a DSC instrument.

[0026] In this case, it is preferable that the composition forming the inner layer has a region containing endothermic peaks below 100°C that does not exceed 10% of the total peak area, and a region containing endothermic peaks above 150°C that exceeds 20% but is less than 90%.

[0027] For example, in the SSA measurement results shown in Figure 1, no more than three types of melting behavior are observed, and the region containing an endothermic peak above 150°C accounts for more than 90% of the total peak area in the temperature-caloric curve. However, using an inner layer made of a composition that exhibits such SSA measurement results makes it difficult to realize the improved heat-sealability, heat resistance, and morphological stability of secondary battery packaging materials that the present invention aims to solve.

[0028] Here, the temperature-caloric curve obtained by thermal fractionation analysis using differential scanning calorimeter shows the results obtained by repeatedly heating and cooling the thermoplastic resin to be analyzed from room temperature to a sufficiently high temperature, for example, approximately 200°C, at a rate of 10°C per minute, using DSC, and holding it for a certain period of time at specific temperatures, for example, 180, 170, and 160°C at 10°C intervals, to induce self-nucleation and annealing, thereby obtaining more precise determination information (see Figures 2 and 3). In other words, when a thermoplastic resin is heated and completely melted, and then cooled to a specific temperature (T) and gradually annealed, lamellae that are not stable at that temperature (T) remain melted, and only stable lamellae crystallize. In this case, the stability at that temperature (T) depends on the thickness of the lamellar, and the thickness of the lamellar depends on the chain structure. Therefore, by performing such heat treatment in steps, the thickness of the lamellae due to the polymer chain structure and its distribution map can be quantitatively measured, and thereby the distribution of each melted peak area can be measured.

[0029] In this invention, a secondary battery packaging material includes a laminated structure comprising an outer layer made of a heat-resistant resin film, a metal foil gas barrier layer, and an inner layer made of a composition containing thermoplastic polyolefin. The inner layer is separated separately and subjected to thermal fractionation analysis using DSC. However, since the inner layer contains not only the crystalline structure due to the chemical composition of the composition containing thermoplastic polyolefin itself, but also the crystalline structure resulting from the molding and heat treatment of the resin, thermal annealing heat treatment is performed at a sufficiently high temperature above the melting point at room temperature to remove the history of molding and heat treatment of the resin. The thermoplastic resin is maintained at a high temperature below the melting point for a sufficient amount of time, for example, 3 to 60 minutes. After such thermal annealing, the thermoplastic resin is cooled to room temperature at the same rate as the heating, and heat treatment is performed. However, the temperature in the maintenance period is lowered at specific temperature intervals until it reaches room temperature to induce self-nucleation and annealing.

[0030] After such heat treatment, the composition forming the inner layer changes from exhibiting an endothermic peak only at the melting point to exhibiting a thermoplastic resin with multiple melting behavior, showing an endothermic phase transition at a phase transition temperature lower than the melting point (see Figure 3).

[0031] This indicates that, in the case of the inner layer composition of the present invention, thermal bonding becomes possible below the melting point by confirming the endothermic phase transition peak that occurs at a temperature lower than the inherent melting point of the resin. It also indicates that it possesses multiple endothermic phase transitions in the range of 90 to 180°C, enabling bonding under a wide range of bonding temperature conditions. Furthermore, the region containing the endothermic peak above 150°C accounts for more than 20% but less than 90%, and excellent thermal bonding strength is exhibited after the inner layer is thermally bonded, with imparted mechanical rigidity and heat resistance.

[0032] On the other hand, the composition containing the thermoplastic polyolefin that constitutes the inner layer in the present invention is composed of multiple layers, preferably two or three layers.

[0033] In the present invention, the composition forming the inner layer contains at least one type of acid-modified polypropylene, and may include modified polypropylene grafted with maleic anhydride in an amount of 1 to 10% by weight, preferably 3 to 5% by weight, as the active group of the acid-modifying group. If the maleic anhydride content is less than 1% by weight, adhesion to the metal foil gas barrier layer may decrease, and if it exceeds 10% by weight, fish eyes (F / E) and low molecular weights may be generated due to the large amount of polar active groups, which may reduce the surface tension after corona surface treatment and decrease the adhesion to the metal foil gas barrier layer. Preferably, it can be configured as a two- or three-layer structure with layers abutting against the metal foil gas barrier layer.

[0034] The inner layer may have a thickness of approximately 25 to 120 μm for sufficient thermal bonding properties, but is not limited to this. It may have an appropriate thickness depending on the intended use of the cell pouch, for example, a thin-film cell pouch with a total thickness of approximately 88 μm, a general-purpose cell pouch with a total thickness of approximately 113 μm, or a medium-to-large cell pouch with a total thickness of approximately 153 μm.

[0035] The outer layer is the outermost layer of a packaging material for lithium secondary batteries, provided on top of a metal foil gas barrier layer and exposed to the outside. It is preferable that the outer layer be formed using a material that has abrasion resistance, as well as heat resistance, cold resistance, pinhole resistance, insulation, chemical resistance, and moldability, so as to protect the metal foil gas barrier layer. Such an outer layer made of a heat-resistant resin film may include a polyamide-based resin or a polypropylene-based resin. The polyamide-based resin may be nylon, which has a high elongation rate and is advantageous for molding, and the polyester-based resin may be polybutylene terephthalate (PBT) or polyethylene terephthalate (PET), which can embody high chemical resistance, pinhole resistance, insulation, and mechanical strength.

[0036] The outer layer may have a thickness of approximately 15 to 30 μm, taking into consideration sufficient abrasion resistance, heat resistance, pinhole resistance, chemical resistance, moldability, and insulation properties. If the outer layer is too thin, the moldability of the secondary battery packaging material may decrease due to insufficient strength of the outer layer. On the other hand, if it is too thick, the inner layer and metal foil gas barrier layer provided below the outer layer must be made relatively thin, which may cause problems such as a decrease in thermal adhesion strength and a decrease in interlayer peel strength in the secondary battery packaging material. However, the thickness of the outer layer is not limited to the above range, and may have an appropriate thickness depending on the intended use of the cell pouch, for example, a thin-film cell pouch with a total thickness of approximately 88 μm, a general-purpose cell pouch with a total thickness of approximately 113 μm, or a medium-to-large cell pouch with a total thickness of approximately 153 μm.

[0037] In the present invention, a first adhesive resin layer may be further formed to bond the outer layer and the metal foil gas barrier layer.

[0038] The first adhesive resin layer is formed by an adhesive capable of bonding the outer layer and the metal foil gas barrier layer. The adhesive used to form the first adhesive resin layer may be a two-component curing adhesive or a one-component curing adhesive. Furthermore, the adhesive device used to form the first adhesive resin layer is not particularly limited and can be selected from chemical reaction type, solvent evaporation type, heat melting type, hot pressure type, etc.

[0039] Examples of adhesive resin components that can be used to form the first adhesive resin layer include polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, polycarbonate, and copolymerized polyester; polyether adhesives; polyurethane adhesives; epoxy resins; phenolic resins; polyamide resins such as nylon 6, nylon 66, nylon 12, and copolymerized polyamide; polyolefin resins such as polyolefins, acid-modified polyolefins, and metal-modified polyolefins; polyvinyl acetate resins; cellulose adhesives; (meth)acrylate resins; polyimide resins; amino resins such as urea resin and melamine resin; rubbers such as chloroprene rubber, nitrile rubber, and styrene-butadiene rubber; silicone resins; and fluoroethylene propylene copolymers. These adhesive components may be used individually or in combination of two or more. The modification patterns of the two or more adhesive components are not particularly limited, but examples of adhesive components include mixed resins of amide and acid-modified polyolefin, mixed resins of polyamide and metal-modified polyolefin, mixed resins of polyamide and polyester, mixed resins of polyester and acid-modified polyolefin, and mixed resins of polyester and metal-modified polyolefin. Among these, polyurethane-based two-component curable adhesives, polyamides, polyesters, or mixed resins of these with modified polyolefins are preferred from the viewpoint of excelling in stretchability, durability and adaptability under high humidity conditions, and thermal degradation suppression during heat suturing, and effectively suppressing the occurrence of delamination by suppressing the decrease in lamination strength between the outer layer and the metal foil gas barrier layer.

[0040] On the other hand, the thickness of the first adhesive resin layer may be, for example, 2 to 10 μm.

[0041] The metal foil gas barrier layer is intended to block the entry and exit of moisture and air from the outside, and gases generated from the inside, and may be in contact with the inner layer. The metal foil gas barrier layer contains a metal having gas barrier and moisture barrier properties, and may contain one or more selected from the group consisting of aluminum (Al), iron (Fe), copper (Cu), nickel (Ni), tin (Sn), zinc (Zn), indium (In), tungsten (W), etc. (a single metal or a mixture of single metals), or two or more alloys selected from these. As a preferred example, the metal foil gas barrier layer may contain aluminum (Al) or an aluminum alloy (Al alloy), taking into consideration moisture barrier properties, gas barrier properties, and formability. The metal foil gas barrier layer may have a thickness of about 25 to 45 μm for sufficient gas barrier and moisture barrier properties. However, the thickness of the metal foil gas barrier layer is not limited to this, and the appropriate thickness can be determined by the intended use of the cell pouch, that is, generally, a thin-film cell pouch with a total thickness of approximately 88 μm, a general-purpose cell pouch with a total thickness of approximately 113 μm, or a medium-to-large cell pouch with a total thickness of approximately 153 μm.

[0042] The metal foil gas barrier layer is preferably treated with a chemical conversion treatment on at least one surface, preferably at least the inner layer side, and more preferably both surfaces, to stabilize adhesion and prevent dissolution and corrosion. Here, the chemical conversion treatment is a treatment that forms an acid-resistant film on the surface of the metal foil gas barrier layer. Examples of chemical conversion treatments include chromate treatment using chromic acid compounds such as chromium nitrate, chromium fluoride, chromium sulfate, chromium acetate, chromium oxalate, chromium biphosphate, acetylacetic acid chromate, chromium chloride, and calcium chromium sulfate; chromate treatment using phosphorylated substances such as sodium phosphate, potassium phosphate, ammonium phosphate, and polyphosphate; and chromate treatment using amination phenol polymers.

[0043] One method for chemical treatment to impart corrosion resistance to a metal foil gas barrier layer involves coating the metal foil gas barrier layer with a mixture of metal oxides such as aluminum oxide, titanium oxide, cerium oxide, and tin oxide, or fine particles of barium sulfate dispersed in phosphoric acid, and then baking it at 150°C or higher to form a corrosion-resistant treatment layer on the surface of the metal foil gas barrier layer. Furthermore, a resin layer can be formed on the corrosion-resistant treatment layer by crosslinking a positively charged polymer with a crosslinking agent. Examples of positively charged polymers include polyethyleneimine, ionic polymer complexes consisting of polyethyleneimine and carboxyl acid, primary amine-grafted acrylic resins in which a primary amine is grafted onto the main acrylic skeleton, polyallylamine or its derivatives, and aminophenol. These positively charged polymers may be used individually or in combination of two or more. Examples of crosslinking agents include compounds having at least one functional group selected from the group consisting of isocyanate, glycidyl, carboxyl, and oxazoline groups, and silane coupling agents. These crosslinking agents may be used individually or in combination of two or more.

[0044] The aforementioned chemical treatment may be performed using one chemical treatment alone, or using a combination of two or more chemical treatments. Furthermore, the aforementioned chemical treatment may be performed using one compound alone, or using a combination of two or more compounds. Among these, chromate treatment is preferred, and more preferably, chromate treatment combining a chromate compound, a phosphoric acid compound, and an aminophenol polymer is used.

[0045] The chemical conversion treatment is carried out by applying a solution containing compounds used to form an acid-resistant coating to the surface of the gas barrier layer of the metal foil using methods such as bar coating, roll coating, Bravia coating, or immersion, and then heating the metal foil to a temperature of approximately 70 to 200°C.

[0046] In the present invention, a second adhesive resin layer may be further formed to bond the metal foil gas barrier layer and the inner layer.

[0047] The second adhesive resin layer may be formed by an adhesive capable of bonding the inner layer and the metal foil gas barrier layer. The adhesive used to form the second adhesive resin layer may be a two-component curing adhesive or a one-component curing adhesive. Furthermore, the adhesive device used to form the second adhesive resin layer is not particularly limited and can be selected from among chemical reaction type, solvent evaporation type, heat melting type, hot pressure type, etc.

[0048] Examples of adhesive resin components that can be used to form the second adhesive resin layer include polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, polycarbonate, and copolymerized polyester; polyether adhesives; polyurethane adhesives; epoxy resins; phenolic resins; polyamide resins such as nylon 6, nylon 66, nylon 12, and copolymerized polyamide; polyolefin resins such as polyolefins, acid-modified polyolefins, and metal-modified polyolefins; polyvinyl acetate resins; cellulose adhesives; (meth)acrylic resins; polyimide resins; amino resins such as urea resins and melamine resins; rubbers such as chloroprene rubber, nitrile rubber, and styrene-butadiene; silicone resins; and fluoroethylene propylene copolymers. These adhesive components may be used individually or in combination of two or more. The deformation pattern of two or more adhesive components is not particularly limited, but examples of adhesive components include mixed resins of polyamide and acid-modified polyolefin, mixed resins of polyamide and metal-modified polyolefin, mixed resins of polyamide and polyester, mixed resins of polyester and acid-modified polyolefin, and mixed resins of polyester and metal-modified polyolefin. Among these, polyurethane-based two-component curable adhesives, polyolefin resins, or mixed resins of these with modified polyolefins are preferred from the viewpoint of being excellent in stretchability, durability and deformation suppression under high humidity conditions, and thermal degradation suppression during heat suturing, and effectively suppressing the occurrence of delamination by suppressing the decrease in lamination strength between the inner layer and the metal foil gas barrier layer.

[0049] On the other hand, the thickness of the second adhesive resin layer may be, for example, 2 to 60 μm.

[0050] The method for manufacturing the packaging material for secondary batteries according to the present invention is not particularly limited as long as a laminate is obtained by stacking layers of a predetermined composition, but the following methods are examples.

[0051] First, a laminate (laminated laminate A) is formed by sequentially laminating an outer layer, a first adhesive resin layer, and a metal foil gas barrier layer. More specifically, laminate A can be formed by a dry lamination method in which the adhesive used to form the metal foil gas barrier layer and the first adhesive resin layer is applied to a barrier layer whose surface has been chemically treated, using coating methods such as extrusion, gravure coating, or roll coating, and then the outer layer is laminated and the first adhesive resin layer is cured.

[0052] Next, the inner layer is laminated on top of the metal foil gas barrier layer of laminate A. When a second adhesive resin layer is provided between the metal foil gas barrier layer and the inner layer, for example, the following methods may be used: (1) a method in which an adhesive for forming the second adhesive resin layer is solution coated onto the metal foil of laminate A and then laminated by a drying method at high temperature, and the inner layer, which has been previously formed into a sheet of two or three layers, is laminated onto this second adhesive resin layer by a thermal lamination method (dry lamination method); (2) a method in which the inner layer consisting of two or three layers is co-extruded onto the metal foil gas barrier layer of laminate A (co-extrusion lamination method); or (3) a method in which the laminate A and the inner layer are joined via the second adhesive resin layer by pouring the molten second adhesive resin layer between the metal foil of laminate A and the sealant layer, which has been previously formed into a sheet of two or three layers (sandwich lamination method). [Examples]

[0053] The present invention will be described in more detail below with reference to specific examples and comparative examples.

[0054] [Example 1] A stretched polyamide film (25 μm thick) is used as the outer layer, and a thin aluminum film (30 μm thick) with chromate phosphate coatings on both sides is used as the metal foil gas barrier layer. These are joined by dry lamination using an adhesive (polyurethane-based two-component curing adhesive, 3 μm thick). The inner layer is formed by T-die casting. The inner layer (40 μm thick), consisting of the aforementioned outer layer, metal foil gas barrier layer bonding film, and a composition containing thermoplastic polyolefin, is joined by dry lamination to obtain a packaging material for lithium secondary batteries.

[0055] The inner layer, composed of a thermoplastic polyolefin, consists of maleic anhydride (4% by weight), modified polypropylene (1% by weight), homopolypropylene (54% by weight), ethylene-containing propylene copolymer (25% by weight), and amorphous propylene rubber (20% by weight). When thermal fractionation analysis (SSA) was performed using differential scanning calorimeter (DSC), the temperature-calorimetry curve showed 12 endothermic peaks in the range of 90 to 180°C. Based on the total peak area, 0.12% of the region contained endothermic peaks below 100°C, and 77.5% contained endothermic peaks above 150°C (see Figure 4).

[0056] [Example 2] A stretched polyamide film (25 μm thick) is used as the outer layer, and a thin aluminum film (30 μm thick) with chromate phosphate coatings on both sides is used as a metal foil gas barrier layer. These are joined together by dry lamination using an adhesive (polyurethane-based two-component curing adhesive, 3 μm thick). The inner layer (40 μm thick) consists of three layers and is joined to the film using a T-die casting method to obtain a packaging material for lithium secondary batteries.

[0057] The inner layer, composed of a thermoplastic polyolefin, consists of maleic anhydride (4% by weight), modified polypropylene (5% by weight), homopolypropylene (5% by weight), ethylene-containing propylene copolymer (35% by weight), ethylene and butene-containing propylene ternary copolymer (25% by weight), low-density polyethylene (12% by weight), and amorphous propylene rubber (18% by weight). When thermal fractionation analysis (SSA) was performed using differential scanning calorimeter (DSC), the temperature-caloric curve showed 13 endothermic peaks in the range of 90 to 180°C. Based on the total peak area, 0.59% of the region contained endothermic peaks below 100°C, and 33% contained endothermic peaks above 150°C (see Figure 5).

[0058] [Example 3] A stretched polyamide film (25 μm thick) is used as the outer layer, and a thin aluminum film (30 μm thick) with chromate phosphate coatings on both sides is used as the metal foil gas barrier layer. These are joined by dry lamination using an adhesive (polyurethane-based two-component curing adhesive, 3 μm thick). The inner layer consists of three layers and is formed by T-die casting. The inner layer (40 μm thick), which is made of the aforementioned outer layer, metal foil gas barrier layer bonding film, and thermoplastic polyolefin composition, is joined by dry lamination to obtain a packaging material for lithium secondary batteries.

[0059] The inner layer, composed of a thermoplastic polyolefin, consists of maleic anhydride (4% by weight), modified polypropylene (1% by weight), homopolypropylene (44% by weight), linear low-density polyethylene (20% by weight), and amorphous propylene rubber (35% by weight). When thermal fractionation analysis (SSA) was performed using differential scanning calorimeter (DSC), the temperature-calorimetry curve showed 18 endothermic peaks in the range of 90 to 180°C. Based on the total peak area, 1.21% of the region contained endothermic peaks below 100°C, and 87% contained endothermic peaks above 150°C (see Figure 6).

[0060] [Example 4] A stretched polyamide film (25 μm thick) is used as the outer layer, and a thin aluminum film (30 μm thick) with chromate phosphate coatings on both sides is used as the metal foil gas barrier layer. These are joined by dry lamination using an adhesive (polyurethane-based two-component curing adhesive, 3 μm thick). The inner layer consists of three layers and is formed by T-die casting. The inner layer (40 μm thick), which is made of the aforementioned outer layer, metal foil gas barrier layer bonding film, and thermoplastic polyolefin composition, is joined by dry lamination to obtain a packaging material for lithium secondary batteries.

[0061] The inner layer, composed of a thermoplastic polyolefin, consists of maleic anhydride (4% by weight), modified polypropylene (1% by weight), homopolypropylene (29% by weight), ethylene-containing propylene copolymer (35% by weight), low-density polyethylene (20% by weight), and amorphous propylene rubber (15% by weight). When thermal fractionation analysis (SSA) was performed using differential scanning calorimeter (DSC), the temperature-calorimetry curve showed 12 endothermic peaks in the range of 90 to 180°C. Based on the total peak area, 0.83% of the region contained endothermic peaks below 100°C, and 22.3% contained endothermic peaks above 150°C (see Figure 7).

[0062] [Comparative Example 1] A stretched polyamide film (25 μm thick) is used as the outer layer, and a thin aluminum film (30 μm thick) with chromate phosphate coatings on both sides is used as a metal foil gas barrier layer. These are joined together by dry lamination using an adhesive (polyurethane-based two-component curing adhesive, 3 μm thick). The inner layer (40 μm thick) consists of three layers and is joined to the film using a T-die casting method to obtain a packaging material for lithium secondary batteries.

[0063] The inner layer, which consists of a composition containing thermoplastic polyolefin, does not contain maleic anhydride-modified polypropylene and is composed of 85% by weight of homopolypropylene and 15% by weight of amorphous propylene rubber. When thermal fractionation analysis (SSA) was performed using differential scanning calorimeter (DSC), the temperature-calorimetry curve showed one endothermic peak. Based on the total peak area, the region containing the endothermic peak below 100°C was 0%, and the region containing the endothermic peak above 150°C was measured to be 91.2% (see Figure 8).

[0064] [Comparative Example 2] A stretched polyamide film (25 μm thick) is used as the outer layer, and a thin aluminum film (30 μm thick) with chromate phosphate coatings on both sides is used as a metal foil gas barrier layer. These are joined together by dry lamination using an adhesive (polyurethane-based two-component curing adhesive, 3 μm thick). The inner layer (40 μm thick) consists of three layers and is joined to the film using a T-die casting method to obtain a packaging material for lithium secondary batteries.

[0065] The inner layer, which consists of a composition containing thermoplastic polyolefin, does not contain maleic anhydride-modified polypropylene and is composed of 90% by weight of ethylene and butene-containing propylene terpolymer and 10% by weight of amorphous propylene rubber. When thermal fractionation analysis (SSA) was performed using differential scanning calorimeter (DSC), the temperature-caloric curve showed six endothermic peaks, and based on the sum of the total peak areas, the region containing endothermic peaks below 100°C was measured to be 0%, and the region containing endothermic peaks above 150°C was also measured to be 0% (see Figure 9).

[0066] [Example Test] Using the aforementioned manufactured packaging material, test specimens were prepared, and their physical properties were measured or evaluated by the following method. The results are shown in Table 1 below.

[0067] [Methods for measuring or evaluating physical properties] (1) Peel strength of aluminum The manufactured material was cured at 50°C for 14 days, then cut into strips 15 mm wide, and the peel strength was measured at a peel angle of 180° with a peel rate of 50 mm / min at 23°C. (2) Thermal adhesive strength The manufactured material was placed in contact with the inner layer film, heat-bonded at 200°C with a pressure of 2 kgf and 1 s, then cut to 15 mm, and the peel strength was measured at 23°C with a peeling speed of 100 mm / min at peeling angles of 180° and 160°. (3) Electrolyte resistance The specimens used to measure the thermal adhesion strength were immersed in an 85°C electrolyte for 75 hours, and then the peel strength was measured using the same method as the thermal adhesion strength measurement method. If the peel strength after immersion in the electrolyte was maintained at 90% or more of the peel strength before immersion in the electrolyte, it was indicated as "◎", if it was 70% or more but less than 90%, it was indicated as "△", and if it was less than 70%, it was indicated as "×". The electrolyte composition was [EC / DEC / DMC=1 / 1 / 1(v / v%)+LiPF6(1 mol / L)+H2O300ppm], where EC is ethylene carbonate, DEC is diethyl carbonate, and DMC is dimethyl carbonate. (4) Forming performance The manufactured packaging material was placed on a frame-shaped metal mold (10cm x 10cm) with the outer layer touching the edge of the mold. The inner layer film surface was pressed with a square pyramid, and the drawing process was performed five times to a minimum depth of 6mm. If there was no tearing at the corners of the packaging material, it was indicated as "◎", if there was one to three tears it was indicated as "△", and if there were four or more tears it was indicated as "×".

[0068] [Table 1]

[0069] Referring to Table 1, it can be confirmed that the present invention provides excellent thermal bonding performance and excellent peel strength between the materials of each layer (peel strength of aluminum, electrolyte resistance) if the inner layer, which is made of a thermoplastic polyolefin composition for lithium secondary battery packaging, contains at least one type of acid-modified polypropylene, and when measured by thermal fractionation analysis, the temperature-caloric curve has at least three endothermic peaks in the range of 90 to 180°C, and the region containing endothermic peaks below 100°C does not exceed 10% of the total peak area, and the region containing endothermic peaks exceeding 150°C exceeds 20% but is less than 90%.

[0070] In contrast, Comparative Example 1 exhibits a relatively high endothermic phase transition at a higher temperature than the Example. This indicates that the thermal annealing region of the thermoplastic polyolefin constituting the inner layer decreases at a relatively low thermal sealing temperature, confirming that thermal bonding is not sufficiently occurring. Furthermore, it can be confirmed that the peel strength and electrolyte resistance of the aluminum are reduced because maleic anhydride-modified polypropylene is not included, resulting in insufficient adhesion to the metal. Additionally, the region exhibiting an endothermic phase transition at high temperatures has a high degree of crystallinity of the thermoplastic polyolefin. While this high crystallinity results in good mechanical rigidity, it can be confirmed that the forming performance is reduced.

[0071] In Comparative Example 2, the region between 100 and 140°C exhibits 100% endothermic phase transition, allowing for adhesion in a relatively low temperature range. However, the region exhibiting endothermic phase transition is in a lower temperature range compared to the Examples, indicating a relatively lower degree of crystallinity of the thermoplastic polyolefin. This results in insufficient mechanical rigidity due to the absence of an endothermic peak in the region above 150°C, which also affects the low peel strength after thermal bonding. Furthermore, similar to Comparative Example 1, the absence of maleic anhydride-modified polypropylene and insufficient adhesion to the metal led to a decrease in the peel strength and electrolyte resistance of the aluminum. However, due to the relatively low degree of crystallinity, the forming performance in the amorphous region was improved compared to Comparative Example 1.

[0072] Preferred embodiments of the present invention have been described in detail. The description of the present invention is illustrative, and a person with ordinary skill in the art to which the present invention belongs should understand that it can be easily modified into other specific forms without changing the technical idea or essential features of the present invention.

[0073] Therefore, the scope of the present invention is indicated by the claims described below rather than by the detailed description above, and all modified or altered forms derived from the meaning, scope, and equivalent concepts of the claims should be interpreted as being included within the scope of the present invention.

Claims

1. A packaging material for secondary batteries having a laminated structure comprising an outer layer made of a heat-resistant resin film, a metal foil gas barrier layer, and an inner layer made of a composition containing a thermoplastic polyolefin, The composition forming the inner layer, when measured using a Successive Self-Nucleation and Annealing (SSA) method with a Differential Scanning Calorimetry (DSC), has at least three endothermic peaks in the temperature-calorimetry curve, and these at least three endothermic peaks appear in the range of 90 to 180°C. The composition forming the inner layer, when analyzed by the thermal fractionation analysis method, has a total area of ​​endothermic peaks below 100°C that does not exceed 10%, and a total area of ​​endothermic peaks above 150°C that exceeds 20% but is less than 90%. The composition forming the inner layer comprises at least one type of acid-modified polypropylene. The acid-modified polypropylene is a modified polypropylene grafted with maleic anhydride in a content of 1 to 10% by weight, and is a packaging material for secondary batteries.

2. The packaging material for secondary batteries according to claim 1, characterized in that the heat-resistant resin is a polyamide resin or a polyester resin.

3. The packaging material for secondary batteries according to claim 1, characterized in that the metal foil contains one or more metals selected from the group consisting of aluminum (Al), iron (Fe), copper (Cu), nickel (Ni), tin (Sn), zinc (Zn), indium (In), and tungsten (W).

4. The packaging material for secondary batteries according to claim 1, characterized in that the thickness of the outer layer is 15 to 30 μm, the thickness of the metal foil gas barrier layer is 25 to 45 μm, and the thickness of the inner layer is 25 to 120 μm.

Citation Information

Patent Citations

  • Slide conductor and method of manufacturing same

    JP1982061278A

  • Polyolefin composition, laminate, and packaging material for electrochemical cell

    JP2019178255A

  • Battery Packaging Materials

    JP6808966B2

  • Polymer film for cell packing material and cell packing material containing same

    KR101499740B1

  • Packing Material for Lithium Secondary Batteries

    KR1020140067521A