Electrolytic copper foil for current collectors in secondary batteries
The electrolytic copper foil addresses manufacturing challenges and performance issues by offering high strength, elongation, and uniform coating properties, enhancing battery stability and performance.
Patent Information
- Application Number
- JP2024525742
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-29
- Filing Date
- 2022-10-07
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-10-07
AI Technical Summary
Existing electrolytic copper foils for secondary batteries face challenges such as high manufacturing costs, difficulty in producing wide widths, contamination from lubricating oil, uneven surface roughness leading to reduced adhesion with active materials, and adverse effects from volume changes and heat generation during lithium battery operation, which degrade battery performance.
Development of an electrolytic copper foil with specific mechanical properties, including high tensile strength, high elongation rate, uniform surface roughness, and controlled wetting angles on both sides, ensuring good contact with active material coatings and stability under varying temperatures.
The copper foil provides enhanced mechanical strength and elongation, maintains adhesion with active materials, and ensures uniform coating, thereby improving battery performance and lifespan by withstanding volume changes and heat generation.
Smart Images

Figure 0007954713000005 
Figure 0007954713000006 
Figure 0007954713000001
Abstract
Description
[Technical Field]
[0001] This invention relates to electrolytic copper foil, and more particularly to electrolytic copper foil for use in a secondary battery current collector. [Background technology]
[0002] Copper foil is generally used as the current collector in secondary batteries. While rolled copper foil is the most commonly used, it is expensive to manufacture and difficult to produce in wide widths. Furthermore, the rolling process requires the use of lubricating oil, and contamination of the lubricating oil can reduce adhesion to the active material, potentially degrading the battery's charge-discharge cycle characteristics.
[0003] Lithium batteries undergo volume changes and heat generation due to overcharging during charging and discharging. Furthermore, the surface roughness of the copper foil must be low to improve adhesion with the electrode active material and to minimize the impact on the copper foil substrate in relation to the expansion and contraction of the active material layer during the charge-discharge cycle, thereby preventing wrinkles and failures in the copper foil as a current collector. Therefore, a copper foil with high elongation, high strength, and low roughness is required that can withstand the volume changes and heat generation phenomena of lithium batteries and has excellent adhesion with the active material. In addition, when used as a negative electrode current collector for secondary batteries, the electrode active material is coated on both sides of the copper foil. In this case, if the roughness of both sides of the electrolytic copper foil differs, the battery characteristics will differ, so it is necessary to maintain the same or similar level of roughness on both sides of the electrolytic copper foil.
[0004] In the manufacturing process of secondary batteries using electrolytic copper foil, the copper foil is subjected to a vacuum drying stage. However, since vacuum drying is a process carried out at high temperatures for a long time, the adhesive strength and stress between the copper foil and the active material coating surface change during this stage, which can lead to a decrease in battery life or the occurrence of cracks.
[0005] When an electrolytic copper foil is used as a negative electrode current collector for a secondary battery, both surfaces of the copper foil are coated with an electrode active material for use. Therefore, it is preferable that the surface of the electrolytic copper foil provides good contact with the active material. However, conventional approaches for providing good contact with the active material are limited to the level of controlling the surface roughness of the electrolytic copper foil.
[0006] Accordingly, there is a demand for an electrolytic copper foil for a secondary battery current collector that has high mechanical properties in various temperature ranges and can provide good contact characteristics with an active material at the same time. Summary of the Invention Problems to be Solved by the Invention
[0007] In order to solve the problems of the prior art as described above, the present invention aims to provide an electrolytic copper foil that has high mechanical strength and a high elongation rate in a wide temperature range.
[0008] Furthermore, the present invention aims to provide an electrolytic copper foil that has high mechanical strength and a high elongation rate despite the application of a high-temperature drying process.
[0009] Furthermore, the present invention aims to provide an electrolytic copper foil for a secondary battery current collector that can provide good contact performance for an active material coating containing an aqueous binder.
[0010] Furthermore, the present invention aims to provide an electrolytic copper foil for a secondary battery current collector that enables a uniform active material coating on both surfaces of the electrolytic copper foil. Means for Solving the Problems
[0011] To achieve the above technical object, the present invention provides an electrolytic copper foil having an elongation rate relative to room temperature thickness of 1.3 to 2.0% / μm, and a surface wetting angle (θ on the S surface S ) relative to the surface wetting angle (θ on the M surface M ) is 1 or more.
[0012] The electrolytic copper foil of the present invention has a room-temperature tensile strength of 40kgf / mm 2 or more, and the ratio of the surface wetting angle (θ on the M surface to the surface wetting angle (θ on the S surface S ) on the M surface may be 1 or more. At this time, θ M ) may be 1 or more. At this time, θ M is 60° to 70°, and θ S may be 50° to 60°.
[0013] In addition, the surface wetting angle of the electrolytic copper foil of the present invention may satisfy the relationship of 0.7<cosθ M / cosθ S <1.
[0014] In addition, the three-dimensional surface roughness Sz on the M surface of the electrolytic copper foil of the present invention may have a value smaller than the three-dimensional surface roughness Sz on the S surface.
[0015] At this time, the three-dimensional surface roughness Sz on the M surface may be 0.7 to 1.0μm, and the three-dimensional surface roughness Sz on the S surface may be 1.3 to 2.0μm.
[0016] The electrolytic copper foil of the present invention can exhibit the high thickness-specific elongation value as described above in the thickness range of 2 to 12μm.
[0017] In addition, the static friction coefficient of the M surface of the electrolytic copper foil of the present invention may be 0.2 to 0.3, and the static friction coefficient of the S surface may be 0.17 to 0.21.
[0018] In addition, the electrolytic copper foil of the present invention may have a TOC content of 5 to 8ppm.
[0019] In addition, the electrolytic copper foil of the present invention may have a tensile strength of 36kgf / mm after heat treatment at 200°C for 1 hour 2 or more.
[0020] In addition, the electrolytic copper foil of the present invention may have a thickness-specific elongation after heat treatment at 200°C for 1 hour of 1.4% / μm or more. Effects of the Invention
[0021] According to the present invention, it is possible to provide electrolytic copper foil that has high mechanical strength and high elongation over a wide range of temperatures.
[0022] Furthermore, according to the present invention, it is possible to provide a current collector that can provide good contact performance to an active material coating containing a water-based binder.
[0023] Furthermore, according to the present invention, it is possible to provide a secondary battery current collector that enables uniform active material coating on both sides of the electrolytic copper foil. [Brief explanation of the drawing]
[0024] [Figure 1A] Figures 1A and 1B are photographs showing examples of wetting angle measurements on the M and S surfaces of copper foil manufactured according to one embodiment of the present invention, respectively. [Figure 1B] Figures 1A and 1B are photographs showing examples of wetting angle measurements on the M and S surfaces of copper foil manufactured according to one embodiment of the present invention, respectively. [Modes for carrying out the invention]
[0025] The embodiments and configurations shown in the drawings described herein represent only one of the most preferred embodiments of the present invention and do not represent the entire technical concept of the invention. It should be understood that there are various equivalents and modifications that can substitute for them at the time of filing. Embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0026] In the specification of this invention, the S surface is the surface that comes into contact with the drum during the electrolytic copper foil manufacturing process and is usually referred to as the glossy surface, while the M surface is the opposite surface and is referred to as the deposition surface or matte surface. This term does not describe the roughness of the surface, and it goes without saying that the S surface may have a lower gloss or higher surface roughness than the M surface.
[0027] In this invention, the electrolytic copper foil has a tensile strength at room temperature (hereinafter referred to as "room temperature tensile strength") of 40 kgf / mm². 2 It is preferable that the above conditions are met. Furthermore, the electrolytic copper foil has a room-temperature tensile strength of 50 kgf / mm². 2 The following or 45 kgf / mm² 2 The following is preferable:
[0028] The tensile strength of copper foil at room temperature is 40 kgf / mm². 2 If the pressure is less than 50 kgf / mm², in lithium secondary batteries, when the anode active material is rapidly coated onto the copper foil during the anode electrode formation process, there is a high possibility of defects such as wrinkles, distortion, and bending occurring due to plastic deformation. 2 If the value exceeds a certain limit, the occurrence of distortion or wrinkles may decrease, but it is highly likely to cause a high tension imbalance during high-speed coating of the negative electrode active material, which can increase the brittleness of the copper foil itself and cause cracks and tears.
[0029] The electrolytic copper foil of the present invention possesses high tensile strength even after high-temperature heat treatment. The tensile strength of the electrolytic copper foil of the present invention after heat treatment at 200°C for 1 hour (hereinafter referred to as "high-temperature tensile strength") is 36 kgf / mm². 2 It is preferable that the above conditions are met. Furthermore, the electrolytic copper foil has a high-temperature tensile strength of 45 kgf / mm². 2 The following or 42 kgf / mm² 2 The following is preferable:
[0030] In the specification of this invention, the high-temperature tensile strength is a measured value that simulates the process in which high-temperature processes such as coating dry and vacuum dry are applied during the anode electrode formation process of a lithium secondary battery, but the high-temperature tensile strength of copper foil is 36 kgf / mm². 2 If the value is less than 45 kgf / mm², deformation will occur in response to the stress caused by the volume expansion of the negative electrode during charging and discharging of the lithium secondary battery, leading to a reduction in lifespan during charging and discharging. 2If the volume expands beyond a certain point, the deformation due to stress decreases, but the brittleness of the copper foil increases, leading to cracks and electrode detachment due to stress accumulation, and reducing the lifespan of the electrodes. Electrolytic copper foil is required to have a high elongation ratio with appropriate strength.
[0031] In the present invention, the ratio of high-temperature tensile strength to room-temperature tensile strength is preferably 0.9 or higher, and the ratio of tensile strengths is less than 1, preferably less than 0.95. In the present invention, the electrolytic copper foil is characterized in that the deterioration of tensile strength due to high-temperature heat treatment is suppressed as much as possible.
[0032] In the present invention, the electrolytic copper foil has a high elongation ratio compared to electrolytic copper foil. Specifically, the electrolytic copper foil of the present invention exhibits a higher value for the elongation ratio divided by the thickness (hereinafter referred to as "elongation per unit thickness") compared to conventional electrolytic copper foil. For example, the elongation per unit thickness at room temperature (hereinafter referred to as "elongation per unit thickness at room temperature") may be 1.3% / μm or more or 1.5% / μmm or more. Furthermore, the elongation per unit thickness at room temperature may be 2.0% / μm or less, 1.9% / μm or less, or 1.8% / μm or less. In addition, in the present invention, the electrolytic copper foil exhibits a high elongation ratio even after high-temperature heat treatment. The electrolytic copper foil of the present invention may have a thickness-to-stretch ratio (hereinafter referred to as "high-temperature thickness-to-stretch ratio") of 1.4% / μm or more, 1.5% / μm or more, or 1.6% / μm or more after heat treatment at 200°C for 1 hour. Furthermore, the high-temperature thickness-to-stretch ratio of the electrolytic copper foil may have a value of 2.4% / μm or less, 2.2% / μm or less, or 2.0% / μm or less.
[0033] To improve the energy density of lithium secondary batteries, the active material content must be increased, and the thickness of non-active materials such as copper foil, aluminum foil, and separation membranes must be reduced. Therefore, as the energy density of lithium secondary batteries increases, the required thickness of the copper foil becomes thinner. However, as the thickness of the copper foil decreases, the physical energy content of the foil also decreases. Consequently, thinner foils are more susceptible to tearing and cracking even under small external stresses. Therefore, a certain level of elongation ratio per unit thickness is necessary to ensure stable product manufacturing in the copper foil manufacturing process or the manufacturing process of electrodes for secondary batteries using copper foil, and to achieve stable lifespan performance during secondary battery charging and discharging. As described later, the electrolytic copper foil of the present invention has a high elongation ratio per unit thickness even at thin thicknesses.
[0034] If the thickness-to-stretch ratio at room temperature is below the lower limit, tearing and cracking may occur in the copper foil manufacturing process and the secondary battery electrode manufacturing process. If it exceeds the upper limit, excessive deformation may occur, resulting in defects such as wrinkles and distortion. If the thickness-to-stretch ratio at high temperature is below the lower limit, electrode breakage may occur during the charging and discharging of the secondary battery, reducing its lifespan. If it exceeds the upper limit, electrode deformation will cause a decrease in charge and discharge performance. Therefore, an appropriate range of thickness-to-stretch ratio is required.
[0035] In the present invention, the electrolytic copper foil exhibits a high thickness-to-stretch ratio even at thin thicknesses of 2 μm or 4 μm. For example, the thickness range in which the copper foil of the present invention exhibits the aforementioned thickness-to-stretch ratio may be in the range of 2 to 12 μm, 4 to 12 μm, 2 to 10 μm, or 4 to 10 μm.
[0036] Furthermore, in this invention, the thickness-to-stretch ratio of the electrolytic copper thin exhibits a narrow deviation across the thickness range of the copper foil. For example, an electrolytic copper foil with a thickness of 4 μm may have a thickness-to-stretch ratio similar to that of an electrolytic copper foil with a thickness of 12 μm.
[0037] Furthermore, the electrolytic copper foil of the present invention has a ratio of the high-temperature elongation rate to the room-temperature elongation rate (elongation rate ratio) of 1 or more, or 1.05 or more. In addition, the ratio of the high-temperature elongation rate to the room-temperature elongation rate (elongation rate ratio) may be 1.25 or less, or 1.2 or less.
[0038] The electrolytic copper foil of the present invention preferably has an MIT (Mandatory Tension) of 240 or more. For example, the electrolytic copper foil of the present invention may have an MIT of 240 to 300. When a secondary battery is charged and discharged, the copper foil substrate used as a current collector also shrinks and expands along with the shrinkage and expansion. However, the higher the MIT value, the more it can withstand the stress caused by bending. Therefore, copper foil with a high MIT value can improve cycle characteristics and ensure high capacity performance.
[0039] (blank paragraph)
[0040] The M-surface and S-surface of the electrolytic copper thin of the present invention have hydrophilic surfaces to provide good contact characteristics with an active material paste containing a water-based binder. For example, in the present invention, the wetting angle or contact angle of the M-surface and S-surface of the electrolytic copper thin with respect to water is preferably 70° or less, 69° or less, 68° or less, 67° or less, 66° or less, or 65° or less. In addition, in the present invention, the wetting angle of the M-surface and S-surface is preferably 50° or more, 51° or more, 52° or more, 53° or more, 54° or more, or 55° or more.
[0041] According to one embodiment of the present invention, the electrolytic copper foil of the present invention is characterized in that the wetting angle of the M surface is the same as or greater than the wetting angle of the S surface. For example, the wetting angle of the M surface of the electrolytic copper foil may be 60° or more, and the wetting angle of the S surface may be 60° or less.
[0042] Furthermore, in this invention, the two sides of the electrolytic copper sheet have a very small difference in wettability. The difference in wettability (D) between the two sides of the copper foil can be expressed in various ways, but it can be expressed using the wetting angle as follows.
[0043] (mathematical formula 1)
[0044] D = cosθ M / cosθ S
[0045] (Here, θ M θ is the wetting angle on the M surface. S (This refers to the wetting angle on the S surface.)
[0046] (blank paragraph)
[0047] In the electrolytic copper foil of the present invention, the aforementioned wettability difference (D) may be 0.7 or more, 0.75 or more, or 0.8 or more. Alternatively, the wettability difference (D) may be 1 or less, 0.95 or less, 0.90 or less, or 0.85 or less.
[0048] Within the numerical range described above, the electrolytic copper foil of the present invention can guarantee good contact characteristics with the active material paste on the M surface and S surface, while simultaneously providing uniform coating.
[0049] The electrolytic copper foil of the present invention has low surface roughness. For example, the three-dimensional surface roughness (Sz) of the electrolytic copper foil of the present invention may have a value of 2.0 μm or less, 1.5 μm or less, or 1.0 μm or less. Furthermore, it is preferable that the three-dimensional surface roughness (Sz) of the M surface is 1.0 μm or less, and the S surface has a value of 2.0 μm or less.
[0050] When the electrolytic copper foil is used as a current collector for the anode of a secondary battery, if the surface roughness (Sz) of the M surface, which is the deposited surface of the electrolytic copper foil, is flat and 1.0 μm or less, the thickness of the coated electrode is also flat, which can make the distribution of lithium ions in the electrode uniform and improve the performance of the battery. However, if the surface roughness (Sz) value is less than 0.7 μm, the adhesive strength between the interface between the active material and the electrolytic copper foil decreases, which may reduce the performance of the electrode.
[0051] According to one embodiment of the present invention, the M-surface of the electrolytic copper thin has a lower three-dimensional surface roughness (Sz) value compared to the S-surface. For example, while the Sz of the S-surface may be 1.3 to 2.0 μm, the Sz of the M-surface may be 0.7 to 1.0 μm.
[0052] The static friction coefficient of the electrolytic copper thin of the present invention is preferably in the range of 0.2 to 0.3 for the M surface and in the range of 0.17 to 0.21 for the S surface. If the static friction coefficient is below the lower limit mentioned above, the friction coefficient is too low, which may cause a decrease in coating adhesion performance when coating the active material of the secondary battery electrode. If it exceeds the upper limit, the friction coefficient is too high, which may cause a decrease in the uniformity of the coating when coating the active material.
[0053] (blank paragraph)
[0054] In order to achieve high strength and high elongation, minimize changes in mechanical properties between room temperature and high temperature, and minimize differences in surface properties between the M-surface and S-surface, the present invention may be manufactured using an electrolyte containing a combination of additives selected from the following additives A to C.
[0055] (blank paragraph)
[0056] ● Additive A
[0057] Additive A is a thiourea compound, a compound in which a thiol group is linked to a nitrogen-containing heterocycle, or a mixture thereof.
[0058] Here, the thiourea compounds are ethylenethiourea, diethylthiourea, acetylentiolea, dipropylthiourea, dibutylthiourea, N-trifluoroacetylthiourea, N-ethylthiourea, N-cyanoacetylthiourea, N-allylthiourea, o-tolylthiourea, and N,N'-butylenethiourea. The compound may be at least one selected from the group consisting of thiourea, thiazolidinethiol, 4-thiazolinethiol, 4-methyl-2-pyrimidinethiol, and 2-thiouracil, but is not necessarily limited to these, and various thiourea compounds usable as additives in the field of the art may be used.
[0059] The compound in which a thiol group is linked to a nitrogen-containing heterocycle of additive A may be at least one selected from the group consisting of 2-mercapto-5-benzoimidazole sulfonic acid sodium salt, sodium 3-(5-mercapto-1-tetrazolyl)benzene sulfonate, and 2-mercaptobenzothiazole, but is not necessarily limited to these, and various compounds in which a thiol group is linked to a nitrogen-containing heterocycle that can be used as an additive in the field of the art may be used.
[0060] In the present invention, it is preferable that additive A is added to the electrolyte at a concentration of less than 2 ppm. Preferably, additive A is added at a concentration of 0.5 to 1.9 ppm.
[0061] In the present invention, additive A can improve the strength of the electrolytic copper foil. If the content of additive A exceeds 1.9 ppm, the surface roughness of the deposited surface increases, making it difficult to manufacture low-roughness electrolytic copper foil, and the elongation rate may decrease.
[0062] (blank paragraph)
[0063] ● Additive B
[0064] Additive B is a sulfonic acid or a metal salt thereof of a compound containing a sulfur atom.
[0065] For example, sulfonic acids or metal salts thereof of compounds containing sulfur atoms include bis-(3-sulfopropyl)-disulfide disodium salt (SPS), 3-mercapto-1-propanesulfonic acid (MPS), 3-(N,N-dimethylthiocarbamoyl)-thiopropanesulfonate sodium salt (DPS), 3-[(amino-iminomethyl)thio]-1-propanesulfonate sodium salt (UPS), o-ethyldithiocarbonate-S-(3-sulfopropyl)-ester sodium salt (OPX), 3-(benzothiazolyl-2-mercapto)-propylsulfonate sodium salt (ZPS), ethylenedithiodipropylsulfonic acid sodium salt, thioglycolic acid, and thiophosphoric acid-o-ethyl-bis-(ω-sulfopropyl)ester disodium salt. It may be at least one selected from the group consisting of (salt) and thiophosphoric acid-tris-(ω-sulfopropyl)ester trisodium salt, but is not necessarily limited to these, and any sulfonic acid or metal salt thereof of a sulfur atom-containing compound that can be used as an additive in the art is acceptable.
[0066] In the present invention, it is preferable that additive B is added to the electrolyte at a concentration of 5 to 20 ppm.
[0067] In the copper electrolyte, additive B can improve the surface gloss of the electrolytic copper thin. If the content of additive B is less than 5 ppm, the gloss of the electrolytic copper thin may decrease, and if the content of additive B exceeds 20 ppm, the surface roughness of the deposited surface may increase, making it difficult to manufacture low-roughness electrolytic copper foil, and the tensile strength of the electrolytic copper thin may decrease.
[0068] (blank paragraph)
[0069] ● Additive C
[0070] Additive C is a nonionic, water-soluble polymer.
[0071] The aforementioned nonionic water-soluble polymers include polyethylene glycol, polyglycerin, nonylphenol polyglycol ether, octanediol-bis-(polyalkylene glycol ether), octanol polyalkylene glycol ether, oleic acid polyglycol ether, polyethylene propylene glycol, polyethylene glycol dimethyl ether, polyoxypropylene glycol, polyvinyl alcohol, β-naphthol polyglycol ether, stearic acid polyglycol ether, and stearyl alcohol polyglycol ether. It may be at least one selected from the group consisting of ether, but is not necessarily limited to them, and any water-soluble polymer usable as an additive in the field of the art is acceptable. For example, the polyethylene glycol may have a molecular weight of 100 to 20000.
[0072] Furthermore, the nonionic water-soluble polymer may be at least one selected from the group consisting of hydroxyethylcellulose and carboxymethylcellulose, but is not necessarily limited to these.
[0073] Furthermore, the nonionic water-soluble polymer is a water-soluble proteinaceous substance such as gelatin or collagen, and has a structure in which glycine, hydroxylysine, and hydroxyproline are repeated, but there are more than six types, including type I, type II, and type V. A chain in which three types of amino acids are repeated is called an alpha chain, and a triple helix is formed when three alpha chains are wrapped around each other. Generally, the complex structure of collagen is formed by cross-linking these triple helices. The nonionic water-soluble polymer of the present invention may be one or more selected from the group consisting of collagen and gelatin, but is not necessarily limited to them.
[0074] In the present invention, it is preferable that the additive C is added to the electrolyte at a concentration of 5 to 15 ppm. In the copper electrolyte, the additive C can reduce the surface roughness of the electrolytic copper thin and improve the surface gloss. If the content of the additive C is less than 5 ppm, the surface roughness of the deposited surface increases, making it difficult to manufacture low-roughness electrolytic copper foil, and the gloss of the electrolytic copper thin may decrease. If the content of the additive C exceeds 15 ppm, a decrease in high-temperature strength and high-temperature hardness of the electrolytic copper thin may occur.
[0075] In the present invention, the ratios of additives A, B, and C in the electrolyte can be controlled.
[0076] The effects of additives A, B, and C in the electrolyte on the physical properties of the electrolytic copper thin have been explained above, but the above explanation is illustrative. It goes without saying that the type, content, or combination of each additive in this invention may also affect other physical properties of the electrolytic copper thin produced by this invention through unknown mechanisms. [Examples]
[0077] <Electrolytic copper foil production example 1>
[0078] (Examples 1-5)
[0079] In an electrolyte solution containing 200-452 g / L CuSO45H2O, 30-250 g / L sulfuric acid, and a chloride ion concentration of 10-30 ppm, the temperature is 50-60°C and the airflow is 50-70 A / dm². 2 Electroplating was performed at an ASD current density. Additive A consisted of 0.5-1.5 ppm ETU (ethylene thiourea), additive B consisted of 5-20 ppm DPS (3-(N,N-dimethylthiocarbamoyl)-thiopropanesulfonate sodium salt), and additive C consisted of 5-10 ppm PEG (polyethylene glycol, molecular weight Mw: 500-4000). The electrolyte compositions used in each example are shown in Table 1. The thickness of the plated film varied depending on the example.
[0080] (blank paragraph)
[0081] (Comparative Example 1)
[0082] In an electrolyte solution consisting of 100 g / L of Cu, 150 g / L of sulfuric acid, and a chloride ion concentration of 20 ppm, the temperature is 50-60°C and the current is 50-70 A / dm². 2 Electroplating was performed at an ASD current density to produce a plated film with a thickness of 18 μm. The following additives were added to the electrolyte: 2 ppm DET (diethylthiourea) as additive A, 45 ppm SPS (bis-(3-sulfopropyl)-disulfide disodium salt) and 10 ppm ZPS (3-(benzothiazolyl-2-mercapto)-propylsulfonate sodium salt) as additive B, 20 ppm PEG (polyethylene glycol, molecular weight Mw: 500-4000) as additive C, and 3 ppm JGB (Janus Green B) as additive D.
[0083] (blank paragraph)
[0084] (Comparative Example 2)
[0085] In an electrolyte solution consisting of 90 g / L Cu, 120 g / L sulfuric acid, and a chloride ion concentration of 30 ppm, the temperature is 50-60°C and the current is 50-70 A / dm². 2Electroplating was performed at an ASD current density to produce a 4 μm thick plated film. Additive A consisted of 3 ppm DET (diethylthiourea), Additive B consisted of 60 ppm SPS (bis-(3-sulfopropyl)-disulfide disodium salt) and 40 ppm ZPS (3-(benzothiazolyl-2-mercapto)-propylsulfonate sodium salt), Additive C consisted of 20 ppm PEG (polyethylene glycol, molecular weight Mw: 500-4000), 10 ppm PGL (polyglycerin), 375 ppm Zn, and 75 ppm Fe, all added to the electrolyte.
[0086] (blank paragraph)
[0087] (Comparative Example 3)
[0088] In an electrolyte solution consisting of 100 g / L of Cu, 130 g / L of sulfuric acid, and a chloride ion concentration of 30 ppm, the temperature is 50-60°C and the current is 50-70 A / dm². 2 Electroplating was performed at an ASD current density to produce a 6 μm thick plated film. Additive A consisted of 26 ppm DET (diethylthiourea), Additive B consisted of 80 ppm SPS (bis-(3-sulfopropyl)-disulfide disodium salt) and 40 ppm ZPS (3-(benzothiazolyl-2-mercapto)-propylsulfonate sodium salt), and Additive C consisted of 20 ppm PEG (polyethylene glycol, molecular weight Mw: 500-4000) and 10 ppm PGL (polyglycerin).
[0089] (blank paragraph)
[0090] (Comparative Example 4)
[0091] In an electrolyte solution consisting of 80 g / L Cu, 140 g / L sulfuric acid, and a chloride ion concentration of 10 ppm, the temperature is 50-60°C and the current is 50-70 A / dm². 2 Electroplating was performed at the current density (ASD) to produce a 12 μm thick plated film. 5 ppm of MPS (3-mercapto-1-propanesulfonic acid) was added to the electrolyte as additive B, and DDAC (diallyldimethylammonium chloride) was added as additive E.
[0092] (blank paragraph)
[0093] (Comparative Example 5)
[0094] In an electrolyte solution consisting of 80 g / L Cu, 140 g / L sulfuric acid, and a chloride ion concentration of 10 ppm, the temperature is 50-60°C and the current is 50-70 A / dm². 2 Electroplating was performed at the current density (ASD) to produce a 12 μm thick plated film. 5 ppm of MPS (3-mercapto-1-propanesulfonic acid) was added to the electrolyte as additive B, and DDAC (diallyldimethylammonium chloride) was added as additive E.
[0095] The plating solution compositions for each example are shown in Table 1 below.
[0096] (blank paragraph)
[0097] [Table 1]
[0098] (blank paragraph)
[0099] <Evaluation of physical properties>
[0100] The physical properties of each surface-treated cavity foil test specimen produced in the examples and comparative examples were measured and are shown in Tables 1 and 2. The physical property evaluation items and measurement methods are as follows.
[0101] (blank paragraph)
[0102] a. Tensile strength / Elongation
[0103] Tensile test specimens were taken from electrolytic copper foil with a width of 12.7 mm and a gauge length of 50 mm. Tensile tests were then performed at a crosshead speed of 50.8 mm / min according to the IPC-TM-650 2.4.18B standard. The maximum load at which the tensile strength was measured was defined as the tensile strength, and the elongation at the point of failure was defined as the elongation. The tensile strength and elongation were measured for each specimen at room temperature, and then measured again after heat treatment at a high temperature of 200°C for 1 hour. The results are shown in Table 1 below.
[0104] (blank paragraph)
[0105] b. TOC measurement of copper foil
[0106] The TOC content in electrolytic copper foil was analyzed by dissolving the electrolytic copper foil test pieces obtained in the examples and comparative examples in 60 ml of hydrochloric acid (35%) and 40 ml of hydrogen peroxide solution (30%), and then using a Shimadzu TOC-V WP analyzer. The results are shown in Table 2 below.
[0107] (blank paragraph)
[0108] c.3D roughness
[0109] Using a 3D profiler, the NV-2200 from NanoSystems, Inc., the shape of minute steps in an object was measured non-contact, and the three-dimensional roughness was determined. Specifically, the minute distance between the contact light-emitting element and the object being measured was precisely measured using a contact light-emitting element and a photodetector such as a camera. Here, Sz is the roughness of the maximum height of the three-dimensional surface, which is the distance between the highest and lowest points within a single surface, and this parameter is the value of the profile (line roughness) parameter Rz extended to three dimensions. The maximum height Sz is the same as the sum of the height Sp of the maximum peak and the depth Sv of the maximum valley.
[0110] The three-dimensional surface roughness (Sz) was measured at five locations on the manufactured copper foil, and the average values are shown in Table 2 below.
[0111] [Table 2]
[0112] (blank paragraph)
[0113] As shown in Table 2, the electrolytic copper foils of Examples 1 to 5 of the present invention exhibit a low TOC content of 5.1 to 8.
[0114] As listed in Table 2, the test specimens of Examples 1-5 were subjected to a temperature of 40 kgf / mm² at room temperature. 2 It exhibits high strength characteristics, and it can be seen that it maintains high strength even after undergoing high-temperature heat treatment at 200°C.
[0115] Furthermore, as shown in Table 2, Examples 1 to 5 exhibit high thickness-to-stretch ratios of 1.3 to 2.0% / μm at room temperature. Moreover, while Example 1, with a thickness of 4μm, also shows a thickness-to-stretch ratio of 1.3% / μm, the comparative examples show values of 1.2% or less.
[0116] Furthermore, the test specimens of Examples 1 to 5 of the present invention showed a three-dimensional surface roughness (Sz) of 0.73 to 0.82 for the M surface and a three-dimensional surface roughness (Sz) of 1.36 to 1.8 for the S surface, indicating that the deviation in surface roughness between the M surface and the S surface is small.
[0117] (blank paragraph)
[0118] d. Wet corner
[0119] The wetting angle (or contact angle) of water on the surface of copper foil test specimens prepared in the examples and comparative examples was measured. The wetting angle was measured using a Phoenix-300 manufactured by SEO Corporation in accordance with ASTM D5946, and deionized water was used as the water droplet. The measurement conditions were as follows:
[0120] (blank paragraph)
[0121] After taking three test pieces from the manufactured copper foil, the wetting angle of each was measured, and the average value is shown in Table 4 below. Figures 1A and 1B are photographs of examples of wetting angle measurements on the M and S surfaces of the copper foil manufactured according to Example 2 of the present invention, respectively, and Table 3 below shows the measurement data at the time of the measurement.
[0122] [Table 3]
[0123] e. Static friction coefficient
[0124] The test method followed ASTM D1894 (Standard Test Methode for Static and Kinetic Coefficients of Friction of Plastic Film and Sheeting), and the test equipment used was a Shimadzu AGS-X instrument, a general-purpose universal testing machine. The specific measurement conditions are as follows:
[0125] (1) Test speed: 150 mm / min
[0126] (2) Load cell: 29N
[0127] (3) Test environment: (23±2)℃, (45±5)% RH
[0128] (4) Vertical load: 1.96N (200g)
[0129] (5) Average interval: (30~120) mm
[0130] (6) Friction material: SUS (provided by Koptri)
[0131] (blank paragraph)
[0132] The measurement results are shown in Table 4 below.
[0133] [Table 4]
[0134] The electrolytic copper foil according to the embodiments of the present invention has a hydrophilic surface. For example, the copper foil surfaces of Examples 1 to 5 have a wetting angle of 70° or less. This is in contrast to Comparative Examples 1 to 5, in which the M-side or S-side of the copper foil has a wetting angle exceeding 70°.
[0135] Furthermore, the electrolytic copper foil according to the embodiment of the present invention has a wetting angle (θ) on the M surface. M ) is the wetting angle (θ) on the S surface. S It has a value greater than ). In contrast, the electrolytic copper foils of Comparative Examples 1 to 3 have θ M <θ S This shows the relationship. Furthermore, in the embodiment of the present invention, θ M and θ S The difference is smaller than that of Comparative Examples 1-3. Thus, the electrolytic copper foil produced by the embodiment of the present invention exhibits a significant reduction in the wettability deviation between the M-side and the S-side.
[0136] The wettability characteristics of the electrolytic copper foil of the present invention provide good contact performance with active material coatings containing water-based binders, and enable uniform active material coating on both sides of the electrolytic copper foil.
[0137] (blank paragraph)
[0138] Although preferred embodiments of the present invention have been described in detail above, those with ordinary skill in the art to which the present invention pertains will understand that various modifications are possible to the above embodiments without departing from the scope of the present invention. Therefore, the scope of the present invention is not limited to the embodiments described above, but should be defined by the claims and equivalents described below. (Note) This disclosure includes the following aspects: Note 1: The elongation ratio relative to the thickness at room temperature is 1.3-2.0% / μm. Surface wetting angle (θ) on the S surfaceS Surface wetting angle (θ) on the M surface relative to ) M Electrolytic copper foil characterized by having a ratio of ) of 1 or more. Note 2: Room temperature tensile strength is 40 kgf / mm². 2 That's all. Surface wetting angle (θ) on the S surface S Surface wetting angle (θ) on the M surface relative to ) M Electrolytic copper foil characterized by having a ratio of ) of 1 or more. Appendix 3: θ M The electrolytic copper foil described in Appendix 1 or 2, characterized in that the angle is 60° to 70°. Appendix 4: θ S The electrolytic copper foil described in Appendix 3, characterized in that the angle is 50° to 60°. Note 5: 0.7 <cosθ M / cosθ S The electrolytic copper foil described in Appendix 1 or 2, characterized in that <1. Note 6: The electrolytic copper foil according to Note 1 or 2, characterized in that the three-dimensional surface roughness Sz on the M surface is smaller than the three-dimensional surface roughness Sz on the S surface. Note 7: The electrolytic copper foil described in Note 6, characterized in that the three-dimensional surface roughness Sz on the M surface is 0.7 to 1.0 μm. Note 8: The electrolytic copper foil described in Note 6, characterized in that the three-dimensional surface roughness Sz on the S surface is 1.3 to 2.0 μm. Note 9: The electrolytic copper foil described in Note 1 or 2, characterized in that its thickness is 2 to 12 μm. Note 10: The electrolytic copper foil according to Note 1 or 2, characterized in that the static friction coefficient of the M surface is 0.2 to 0.3 and the static friction coefficient of the S surface is 0.17 to 0.21. Note 11: The electrolytic copper foil according to Note 1 or 2, characterized in that the TOC content is 5 to 8 ppm. Note 12: The tensile strength after heat treatment at 200°C for 1 hour is 36 kgf / mm². 2 The electrolytic copper foil described in Appendix 1 or 2, characterized by the above. Note 13: The electrolytic copper foil according to Note 1 or 2, characterized in that the elongation ratio relative to thickness after heat treatment at 200°C for 1 hour is 1.4% / μm or more. [Industrial applicability]
[0139] This invention is applicable to electrolytic copper foil.
Claims
1. The elongation ratio relative to the thickness at room temperature is 1.3 to 2.0% / μm. The thickness-to-stretch ratio after heat treatment at 200°C for 1 hour is 1.4–2.4% / μm. The surface wetting angles on the M surface and S surface are 70° or less. Surface wetting angle (θ) on the S surface S Surface wetting angle (θ) on the M surface relative to ) M The ratio of ) is 1 or more, Electrolytic copper foil characterized in that the surface wetting angle (θ M) on the M surface and the surface wetting angle (θ S) on the S surface are in a relationship of 0.68 ≤ cosθ M / cosθ S < 1.
2. The tensile strength at room temperature is 40-50 kgf / mm². The tensile strength after heat treatment at 200°C for 1 hour is 36-45 kgf / mm². The surface wetting angles on the M surface and S surface are 70° or less. Surface wetting angle (θ) on the S surface S Surface wetting angle (θ) on the M surface relative to ) M The ratio of ) is 1 or more, Electrolytic copper foil characterized in that the surface wetting angle (θ M) on the M surface and the surface wetting angle (θ S) on the S surface are in a relationship of 0.68 ≤ cosθ M / cosθ S < 1.
3. Surface wetting angle (θ) on the M surface M The electrolytic copper foil according to claim 1 or 2, characterized in that the angle is 60° to 70°.
4. Surface wetting angle (θ) on the S surface S The electrolytic copper foil according to claim 3, characterized in that the angle is 50° to 60°.
5. The electrolytic copper foil according to claim 1 or 2, characterized in that the three-dimensional surface roughness Sz on the M surface is smaller than the three-dimensional surface roughness Sz on the S surface.
6. The electrolytic copper foil according to claim 5, characterized in that the three-dimensional surface roughness Sz on the M surface is 0.7 to 1.0 μm.
7. The electrolytic copper foil according to claim 5, characterized in that the three-dimensional surface roughness Sz on the S surface is 1.3 to 2.0 μm.
8. The electrolytic copper foil according to claim 1 or 2, characterized in that its thickness is 2 to 12 μm.
9. The electrolytic copper foil according to claim 1 or 2, characterized in that the static friction coefficient of the M surface is 0.2 to 0.3 and the static friction coefficient of the S surface is 0.17 to 0.
21.
10. The electrolytic copper foil according to claim 1 or 2, characterized in that the TOC content is 5 to 8 ppm.
Citation Information
Patent Citations
Copper foil for current collector of lithium secondary battery
JP2012038700A
Electrolytic copper foil, and electrical component and battery comprising the same
JP2016160503A
Electrolytic copper foil, current collector containing same, negative electrode and lithium battery
JP2017517637A
Roughened copper foil, copper clad laminate and printed wiring board
JP2019218602A
Electrolytic copper foil for secondary batteries and its manufacturing method
JP2019536211A