Method for manufacturing barrier articles based on inorganic fibers or naturally derived organic fibers

A sizing composition of oxidized lignin and nonpolymeric polycarboxylic acid addresses the issues of toxicity and cost in traditional binders, achieving superior mechanical properties in barrier articles by uniformly bonding inorganic and natural organic fibers.

JP7954718B2Active Publication Date: 2026-11-20ISOVER SAINT GOBAIN SA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024535671
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-17
Filing Date
2022-12-15
Publication Date
2026-11-20
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

Existing barrier article production methods using thermosetting resins like resol-based phenolic resins release formaldehyde and urea, which are harmful and unstable, while polyisocyanate-based binders are toxic and expensive, and current alternatives for binding both inorganic and natural organic fibers lack reactivity and stability.

Method used

A sizing composition comprising potentially oxidized lignin and nonpolymeric organic polycarboxylic acid is used to bond inorganic and natural organic fibers, providing a low-toxicity, cost-effective binder that crosslinks efficiently under heating.

Benefits of technology

The method produces barrier articles with mechanical properties comparable to or better than those using traditional binders, without formaldehyde release and at lower cost, using a binder that is uniformly dispersed and stable during processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954718000005
    Figure 0007954718000005
  • Figure 0007954718000006
    Figure 0007954718000006
  • Figure 0007954718000001
    Figure 0007954718000001
Patent Text Reader

Abstract

The present invention relates to a method for making an insulation article comprising inorganic or natural organic fibers bound by an organic binder, the method comprising the steps of: (a) applying a sizing composition to the inorganic fibers or the natural organic fibers; (b) forming an aggregate of said inorganic fibers or said natural organic fibers; (c) heating the collection of inorganic fibers or natural organic fibers until the sizing composition cures; 5, wherein the sizing composition comprises: at least one lignin, which is potentially oxidized; and at least one non-polymeric organic polycarboxylic acid, The present invention is characterized by comprising: The invention also relates to insulation articles obtainable by such a method.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for producing a barrier article comprising inorganic or natural organic fibers bound together by an organic binder obtained by curing or crosslinking a sizing composition containing potentially oxidized lignin and a nonpolymeric polycarboxylic acid organic acid. The present invention also relates to a barrier article obtained by such a method. [Background technology]

[0002] The production of barrier articles based on inorganic fibers, particularly mineral wool, generally involves a process of producing glass fibers or rock fibers via a centrifugal separation process. In their paths between the centrifugal separator and the fiber collection belt, an aqueous sizing composition, also called an aqueous binder composition, is sprayed onto the fibers while they are still hot, and the composition then undergoes a polymerization reaction, generally at a temperature above 100°C.

[0003] For several years, the use of various thermosetting resins as binders in sizing compositions has made it possible to bond inorganic fibers and improve the mechanical performance of the resulting barrier articles. The thermosetting resins most commonly used in the manufacture of barrier articles based on mineral wool are resol-type phenolic resins. In addition to their good crosslinking ability under the aforementioned thermal conditions, these resins are water-soluble, have good affinity with inorganic fibers, especially thanks to the presence of silane, and are relatively inexpensive.

[0004] The most common resols are obtained by the condensation of phenol and formaldehyde in the presence of a basic catalyst. Ultimately, these resols contain a certain proportion of unreacted monomers, particularly formaldehyde, whose presence is undesirable from the standpoint of known adverse effects.

[0005] For this reason, resol-based resins are generally treated with urea, which reacts with free formaldehyde and captures it in the form of a non-volatile urea-formaldehyde condensate. Furthermore, the presence of urea in the resin offers certain economic advantages thanks to its low cost; it can be introduced in relatively large quantities without affecting the quality of use of the resin, and especially without adversely affecting the mechanical performance of the final product, which can significantly reduce the overall cost of the resin.

[0006] Nevertheless, it has been observed that urea-formaldehyde condensates are unstable under the temperature conditions to which the mineral wool layer is exposed to obtain resin crosslinking; they decompose, yielding formaldehyde and urea again, the latter of which decomposes at least partially into ammonia and is released into the factory atmosphere, requiring recovery procedures to reduce its impact on the environment. Therefore, solutions for replacing formaldehyde-based resins in sizing compositions are being developed.

[0007] In their International Publications 2010 / 029266 and 2013 / 014399, the applicant proposed sizing compositions based on hydrides, also known as sugar alcohols, for binding inorganic fibers. These reagents exhibit excellent thermal stability and impart good mechanical properties to the final article.

[0008] Formaldehyde-free binders containing both hydrides and reducing or non-reducing sugars are disclosed in the applicant's International Publications 2013 / 021112 and 2015 / 159012, respectively, for binding inorganic fibers. However, resins based on these sugars have shown little reactivity and stability for binding natural organic fibers.

[0009] To bind natural organic fibers, especially with a density of 250 kg / m³ 3To obtain a barrier article with a molecular weight less than 100%, it is known to use a binder obtained after curing or crosslinking a sizing composition containing polyisocyanate. Among the polyisocyanates most commonly used in the wood fiber industry, poly(methylenediphenyl isocyanate) (pMDI, CAS number 9016-87-9) is a good example, which is a technical grade blend containing 30-80% MDI (methylenediphenyl isocyanate) and the following high molecular weight congener.

[0010] [ka]

[0011] In order to ensure good moisture retention of natural organic fibers by hydrophobic pMDI, it is generally necessary to first dry the fibers, thereby reducing their moisture content to 6% by weight or less, and especially to 2-6% by weight (see International Publication No. 2008 / 144770).

[0012] A relatively recent proposal is an emulsifiable pMDI (EMDI), which is a mixture of pMDI with an unstable, hydrogen-free nonionic surfactant that can react with isocyanate functional groups (see, for example, European Patent Application Publication No. 0516361), or a mixture of pMDI with a low proportion of pMDI functionalized with hydrophilic chains, such as polyethoxylated chains, to stabilize the emulsion.

[0013] Using pMDI in the form of an aqueous emulsion allows for the regular distribution of the binder onto natural organic fibers without pre-drying, which constitutes significant energy savings.

[0014] However, the use of polyisocyanate-based binders, even in the form of aqueous pMDI emulsions, constitutes a significant problem in terms of toxicity in board manufacturing due to the presence of polyisocyanates. Furthermore, polyisocyanates are highly reactive and expensive raw materials. [Overview of the project] [Problems that the invention aims to solve]

[0015] Therefore, the applicant has sought a method for producing both inorganic fiber-based and natural organic fiber-based barrier articles using the same type of organic binder, in other words, the same sizing composition that enables the bonding of both inorganic and natural organic fibers after curing; such a sizing composition should preferably be of biological origin, low toxicity, low cost, have good crosslinking ability, be uniformly dispersed over any of the aforementioned fibers, and enable the production of barrier articles with good mechanical properties. Furthermore, the desired sizing composition should have the advantage of not polymerizing / crosslinking, or hardly polymerizing / crosslinking, before passing through a suitable heating device, and / or rapidly polymerizing / crosslinking once passing through a suitable heating device. [Means for solving the problem]

[0016] In the course of this research, the inventors discovered that sizing compositions comprising the following specific combinations provide the desired advantages or properties: - At least one lignin that is potentially oxidized, and - At least one nonpolymeric organic polycarboxylic acid.

[0017] Therefore, the object of the present invention is, more precisely, a method for manufacturing a barrier article comprising inorganic fibers or natural organic fibers bound together by an organic binder, comprising the following steps: (a) Applying the sizing composition to the inorganic fiber or the natural organic fiber, (b) To form an aggregate of the above-mentioned inorganic fibers or the above-mentioned natural organic fibers, (c) Heat the aggregate of inorganic fibers or natural organic fibers until the sizing composition hardens. The method is characterized by comprising the following sizing composition: - At least one lignin that is potentially oxidized, and, - At least one non-polymeric organic polycarboxylic acid. [BRIEF DESCRIPTION OF THE DRAWINGS]

[0018] [Figure 1] Figure 1 shows a possible structure of native lignin.

[0019] [Figure 2] Figure 2 shows a possible structure of the lignin according to the present invention. [DETAILED DESCRIPTION OF EMBODIMENTS FOR CARRYING OUT THE INVENTION]

[0020] The lignin according to the present invention is a lignin extracted from so-called "native (natural)" lignin, and is a biomolecule belonging to a group of polyphenol polymeric macromolecules (broadly a group of tannins), which is one of the main components of wood together with cellulose and hemicellulose. Figure 1 [Fig.1] shows a possible structure of native lignin. Native lignin has a molar mass of 10,000 g.mol -1Native lignin is a polymer far exceeding [a certain size] and is insoluble in water. It is mainly found in vascular plants and some algae. Its main functions are to provide rigidity, water resistance, and high resistance to degradation. All vascular plants, whether woody or herbaceous, produce lignin. Quantitatively, the native lignin content is 3-5% in leaves, 17-24% in herbaceous stems, and 18-33% in woody stems (18-25% in broad-leaved trees and 27-33% in coniferous trees). It is relatively less abundant in annual plants than in perennial plants, but very abundant in trees. Native lignin is mainly found between cells, but a considerable amount is also present within them. Lignin is a complex three-dimensional hydrophobic network, but its basic unit is essentially a monolignol unit. Following cellulose (which makes up 35-50% of terrestrial plant biomass) and hemicellulose (30-45%), lignin (15-25%) is the third most abundant group of compounds in plants and terrestrial ecosystems, predominantly found in dead or growing plant biomass.

[0021] The lignin according to the present invention is a polymer, and one possible structure thereof is shown in Figure 2 [Fig. 2]. The lignin according to the present invention is extracted by cleaving the β-O-4 ether bond of native lignin, and therefore has a lower molar mass than the native lignin from which it is derived, i.e., 10,000 g·mol -1 An average molar mass of less than 1,000 g·mol, preferably 1,000 g·mol -1 ~9,000 g·mol -1 It has a molar mass of .

[0022] The lignin according to the present invention may be selected from alkaline lignin, lignosulfonates, organic solvent lignin, sodium lignin, lignin from the biorefining process of lignocellulose raw materials, or mixtures thereof, also known as Kraft lignin. The four groups of commercially available lignins are alkaline lignin, or Kraft lignin, lignosulfonates, and organic solvent lignin (extracted lignin and sodium lignin). The fifth group is so-called biorefinery lignin, which differs slightly in that it is described not by the method of extraction but by the origin of the method, for example, biorefining, and therefore may be similar to or different from any other group mentioned. The lignin according to the present invention is preferably alkaline lignin, also known as Kraft lignin.

[0023] Figure 2 [Fig. 2] shows a possible structure of lignin according to the present invention. The reactive functional group that is abundant in typical lignin is the hydroxyl group, which is either an aromatic hydroxyl group or an aliphatic hydroxyl group, and is either a primary alcohol functional group or a secondary alcohol functional group (secondary alcohol functional groups are less reactive than primary alcohol functional groups). The hydroxyl group of lignin can react with crosslinking agents, such as isocyanates or epoxides, amines or aldehydes, and it is known that this can result in crosslinked lignin structures according to various crosslinking mechanisms. However, these crosslinking agents have not received much attention due to their toxicity (isocyanates, amines, formaldehyde) and / or cost (epoxides, amines, aldehydes other than formaldehyde).

[0024] Therefore, the inventors discovered that non-polymeric polycarboxylic acids, which are themselves low in toxicity, can crosslink lignin. Furthermore, they found that these non-polymeric polycarboxylic acids can be used as lignin crosslinking agents to bond both inorganic fibers and natural organic fibers after curing or crosslinking of these components; and that this yields barrier articles with mechanical performance that is as good as, or even relatively better than, that obtained when using other known crosslinking agents, such as formaldehyde or isocyanates.

[0025] In this application, the term "nonpolymeric" organic polycarboxylic acid refers to a polycarboxylic acid linked in a repeating manner by covalent bonds, with a molar mass of 90 g·mol. -1 ~350g·mol -1 This is understood to mean a polycarboxylic acid that is not a polymer composed of monomer aggregates. Therefore, in this application, the sizing composition preferably does not contain polymeric organic polycarboxylic acids. The nonpolymeric organic polycarboxylic acids according to the present invention may be selected from the following: dicarboxylic acids, particularly oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, malic acid, tartaric acid, tartonic acid, aspartic acid, glutamic acid, fumaric acid, itaconic acid, maleic acid, traumuric acid, camphoric acid, phthalic acid and its derivatives, particularly those containing at least one boron or chlorine atom; tetrahydrophthalic acid and its derivatives, particularly those containing at least one chlorine atom; isophthalic acid, terephthalic acid, mesaconic acid and citraconic acid; tricarboxylic acids, particularly citric acid, tricarbaryl acid, 1,2,4-butanetricarboxylic acid, aconitic acid, hemimelitic acid, trimellitic acid and trimesic acid; and tetracarboxylic acids, particularly 1,2,3,4-butanetetracarboxylic acid and pyromellitic acid. More preferably, the nonpolymeric organic polycarboxylic acid is selected from maleic acid, succinic acid, glutaric acid, itaconic acid, and citric acid. Even more preferably, the nonpolymeric organic polycarboxylic acid is a tricarboxylic acid, particularly citric acid.

[0026] In other words, the inventors have surprisingly discovered that lignin, an inexpensive, non-toxic, and low-corrosion bio-derived material, can, in combination with a low-toxicity non-polymeric organic polycarboxylic acid, bond inorganic fibers or natural organic fibers after curing or crosslinking of these components; and that this can enable the manufacture of barrier articles having mechanical properties comparable to, or even better than, those of the known binders described above.

[0027] In one embodiment of the present invention, lignin is diluted with water to adjust the pH to 6.5 to 10.5, preferably 8 to 9, before adding a nonpolymeric organic polycarboxylic acid. This pH range has the advantage of allowing relatively uniform deposition of the sizing composition on the fibers, thereby improving the mechanical properties of the resulting barrier article.

[0028] Preferably, the sizing composition contains at least one lignin in an amount of 25% to 85% by weight, more preferably 40% to 80% by weight, and even more favorably 50% to 75% by weight, based on the total dry weight of the composition.

[0029] Preferably, the sizing composition contains, based on the total dry weight of the composition, at least one nonpolymerizable organic polycarboxylic acid in an amount of 15% to 75% by weight, more preferably 20% to 60% by weight, and even more favorably 25% to 50% by weight.

[0030] In another preferred embodiment of the method of the present invention, the lignin contained in the sizing composition in combination with the non-polymeric organic polycarboxylic acid is oxidized lignin. In this embodiment, the amount of oxidized lignin is 50 wt% to 85 wt%, preferably 55 wt% to 80 wt%, more preferentially 60 wt% to 75 wt%, based on the total dry weight of the sizing composition, and the oxidized lignin comprises a proportion of carboxylic acid functional groups of 2% to 20%, preferably 5% to 15%, and a proportion of primary alcohol functional groups of 2% to 20%, preferably 5% to 15%. The above proportions of the carboxylic acid functional groups and primary alcohol functional groups present on the oxidized lignin are measured by infrared spectroscopy; by calculating the ratio of the peak intensity of the C-O bond of the carboxylic acid functional group (C-OOH) of the oxidized lignin and the peak intensity of the C-O bond of the primary alcohol functional group (C-OH), respectively, relative to the sum of the peak intensities of the C-O bonds of all functional groups present on the oxidized lignin, all peaks being at 1000cm -1~ ~1300cm -1 located. All functional groups present on the oxidized lignin that have C-O bonds are as follows: primary and secondary alcohol functional groups (C-OH); aromatic hydroxyl functional groups (Ar-OH), acid functional groups (C-OOH); aromatic ether functional groups (Ar-OC), aliphatic and cycloaliphatic ether functional groups (C-OC), and methyl ether functional groups (C-OCH3).

[0031] The use of oxidized lignin (compared to non-oxidized lignin) has the advantage of reducing the amount of non-polymeric organic polycarboxylic acid added to the sizing composition for binding inorganic fibers or organic fibers. Therefore, in this particular embodiment, the amount of non-polymeric organic polycarboxylic acid is 15 wt% to 50 wt%, preferably 20 wt% to 45 wt%, more preferentially 25 wt% to 40 wt%, based on the total dry weight of the sizing composition.

[0032] In fact, in a sizing composition comprising a combination of at least one oxidized lignin and at least one nonpolymeric organic polycarboxylic acid, the carboxylic acid groups present on the oxidized lignin obtained by splitting the polymer and then oxidizing the secondary aliphatic hydroxyl groups of the starting lignin will react with some of the aliphatic hydroxyl groups of the oxidized lignin (particularly primary alcohol functional groups) during the heating step of the fiber assembly, thereby initiating the self-crosslinking of the oxidized lignin, and then the remaining aliphatic hydroxyl groups of the oxidized lignin will react with the carboxylic acid groups of the nonpolymeric organic polycarboxylic acid added as a crosslinking agent to complete the crosslinking of the oxidized lignin.

[0033] Furthermore, the sizing composition according to the present invention may be formaldehyde-free. In this application, "formaldehyde-free" is understood to mean that the formaldehyde content in the sizing composition according to the present invention is less than 2000 ppm.

[0034] The sizing composition is an aqueous composition that may have a dry weight content of 0.5% to 50% by weight, preferably 3% to 30% by weight, and more preferably 4% to 20% by weight.

[0035] Next, the aqueous sizing composition is applied to inorganic fibers or natural organic fibers in an amount of 2% to 20% by weight, preferably 5% to 15% by weight, to impart the desired mechanical properties to the barrier article, the above amount being expressed as a dry product based on the weight of the inorganic fibers or natural organic fibers.

[0036] In a preferred embodiment of the method of the present invention, step (a) of applying the sizing composition to an inorganic fiber or a natural organic fiber may be carried out by spraying, particularly by means of a spray nozzle, or by roller coating, or by impregnation.

[0037] According to the present invention, the inorganic fibers are preferably mineral wool, and more preferably glass wool, rock wool, or slag wool, or mixtures thereof. In particular, when the inorganic fibers are mineral wool, they may contain, in weight percent, compositions corresponding to the following formulations: SiO2: 30-50%, preferably 35-45% Na2O: 0-10%, preferably 0.4-7% CaO: 10-35%, preferably 12-25% MgO: 1-15%, preferably 5-13% CaO + MgO: 11-40% total Al2O3: 10-27% K2O: 0-2%, preferably 0-1% Iron oxide: 0.5-15%, preferably 3-12% One or more other oxides: 0-5% in total, preferably less than 3%. The remainder consists of unavoidable impurities.

[0038] The inorganic fibers may be glass fibers or rock fibers, particularly basalt (or wollastonite). More specifically, the inorganic fibers according to the present invention are aluminosilicate glass fibers, particularly aluminosilicate glass fibers containing aluminum oxide (Al2O3) in a proportion of 14% to 28% by weight. In another embodiment, the inorganic fibers may be glass fibers containing, in weight percent, compositions corresponding to the following formulations: SiO2: 50-75%, preferably 60-70% Na2O: 10-25%, preferably 10-20% CaO: 5-15%, preferably 5-10% MgO: 1-10%, preferably 2-5% CaO and MgO together preferably make up 5-20%. B2O3: 0-10%, preferably 2-8% Al2O3: 0-8%, preferably 1-6% K2O: 0-5%, preferably 0.5-2% The combined amount of Na2O and K2O is preferably 12-20%. Iron oxide: 0-3%, preferably less than 2%, more preferably less than 1%, One or more other oxides: 0-5% by weight in total, preferably less than 3% in total. The remainder consists of unavoidable impurities.

[0039] The diameter of the inorganic fibers is advantageously between 0.1 and 25 μm.

[0040] The diameter of the natural organic fibers is advantageously 5 to 100 μm, preferably 10 to 50 μm, and the length of these fibers is particularly 0.1 to 900 mm, more particularly 10 to 120 mm. According to the present invention, the natural organic fibers are advantageously non-thermoplastic fibers, naturally occurring in biomass, and may be mechanically and / or chemically treated. The fibers are derived from plant sources and are advantageously selected from cotton and lignocellulose fibers. Lignocellulose fibers are understood to mean plant-derived fibers based on lignocellulose material, i.e., fibers containing cellulose, hemicellulose, and lignin. Examples of lignocellulose fibers include woody fibers and other plant-derived fibers, such as hemp, flax, sisal, cotton, jute, coconut, raffia, abaca fibers, or even grain straw or rice straw.

[0041] The term "lignocellulose fiber" as used in this application does not include lignocellulose material that has undergone thermomechanical or chemical treatment for the manufacture of paper pulp.

[0042] Therefore, the lignocellulose fibers used in the present invention are those that have undergone mechanical grinding treatment, which is intended simply to reduce and / or control the size of the fibers.

[0043] Lignocellulose fibers are preferably coniferous, particularly pine, fibers obtained by mechanical defibration. Their diameter is advantageously 10–70 μm, preferably 30–50 μm, and their length is in the range of 0.1–100 mm, preferably 0.5–50 mm, particularly 1–10 mm.

[0044] The sizing composition (a) is preferably applied before step (b) of forming an aggregate of inorganic or natural organic fibers, in which case the sized fibers are brought together and then heated continuously or temporarily to cure the sizing composition, thus forming an organic binder that binds the fibers together.

[0045] Therefore, the step (b) of forming an aggregate of inorganic or natural organic fibers may also be called the step of forming a set of fibers, and may be carried out by molding and / or compression. The mold used for molding the article must be made of a material that can withstand the temperature of the heating step. It must also have a structure that allows hot air from the curing furnace to easily penetrate the molded article. The mold may consist, for example, of a box-shaped metal screen. The box of the metal screen is preferably filled with loose fibers in a volume greater than its capacity and closed with a cover of the metal screen. In this way the fibers are more or less compressed depending on the amount of excess filling. This amount of excess filling of the box with fibers is, for example, 10% to 150%, preferably 15% to 100%, and especially 20% to 80%.

[0046] If the method of the present invention is a continuous method, the step of forming a fiber aggregate (b) can be performed, for example, by compression by rollers positioned at the entrance of a curing furnace on a conveyor.

[0047] Furthermore, the fibers can be assembled as follows: - A flexible fiber mat that can be rolled up, compressed, or folded. - A fiberboard or plate that is denser and more rigid than a rollable mat. - Fiber-based molded articles, such as linings for pipes or ducts, - Woven or nonwoven fabrics, such as nonwoven mats made of glass fibers or organic fibers.

[0048] In a particular embodiment of the method according to the present invention, the fibers are natural organic fibers impregnated with an aqueous sizing composition, and the method further includes a fiber drying step between step (a) and step (b), which is aimed at evaporating sufficient moisture to make the sized or unsized fibers substantially non-sticky. In another embodiment, the drying step may be performed before step (a). This drying step may be carried out by heating, for example, in a temperature-controlled ventilated furnace, or by using a steam-heated press. It is important that the drying does not heat the natural organic fibers to an excessively high temperature so as not to soften the dried sizing composition or even initiate crosslinking of the components of the sizing composition. A heating temperature close to the boiling point of water is generally sufficient. Thus, drying of the fibers impregnated with the aqueous sizing composition is preferably carried out by heating to a temperature of 75°C to 150°C for a time of 1 to 10 seconds. The natural organic fibers obtained after the drying step are surrounded by a cover of dried sizing composition.

[0049] Step (c) of heating an aggregate of inorganic fibers or natural organic fibers according to the method of the present invention is preferably carried out in a temperature-controlled container or steam press at a temperature of 100°C to 250°C for a period of 1 to 20 minutes. The temperature-controlled container may be a forced-air furnace or a heating mold having a fluid circulation or resistance heater into which a temperature-controlled high-temperature gas is introduced into one or more compartments. During this step of heating the aggregate of inorganic fibers or natural organic fibers, the components of the sizing composition (according to the present invention) harden / or crosslink / polymerize to form an insoluble organic binder.

[0050] In another specific embodiment of the method according to the present invention, the fibers are inorganic fibers, and after step (c) heating the aggregate of inorganic fibers until the sizing composition hardens, the inorganic fiber aggregate has an ignition loss (LOI) of 1% to 20% by weight, preferably 1% to 15% by weight.

[0051] The present invention also relates to a barrier article that can be obtained by the method described above. The resulting barrier article comprises inorganic or natural organic fibers bound together with a binder obtained by curing or crosslinking a sizing composition (as described above) which optionally contains lignin and a nonpolymeric organic polycarboxylic acid. The resulting barrier article has good mechanical properties. The barrier article has a thickness of 10 to 300 mm, preferably 35 to 240 mm, and a load of 30 to 200 kg / m², as measured according to EN 823:2013. 3 Preferably 35-180 kg / m 3 It may have a density of [value missing]. The resulting barrier material can be used to manufacture exterior barrier panels for buildings. The resulting barrier material may be, in particular, a net of inorganic fibers, especially a net of glass fibers or rock fibers. [Examples]

[0052] Example 1:

[0053] This process generates aqueous sizing compositions containing the components listed in Table 1, each expressed as a weight percentage based on the total dry weight of the respective compositions.

[0054] Composition 1 (i.e., comparative example sample), which is outside the present invention, is produced by mixing Kraft Lignin A with water. Compositions 2 to 4 according to the present invention are produced by mixing a first solution containing lignin A dissolved in water with a second solution containing a specific nonpolymeric organic carboxylic acid dissolved in water. Compositions 5 and 5bis (i.e., comparative example samples), which are outside the present invention, are produced by continuously adding 48 parts by weight of maltitol (as a hydride sugar), 52 parts by weight of citric acid, and 5 parts by weight of sodium hypophosphite (catalyst) to a container while vigorously stirring until the components are completely dissolved.

[0055] All sizing compositions 1-5 and 5bis contain 90% by weight of water and 10% by weight of dry matter. All compositions are used to form glass fiber-based barrier articles.

[0056] Two laminated pieces of glass fiber nonwoven paper (60 mm × 10 mm × 0.250 mm) are impregnated with each aqueous sizing composition, and then the impregnated glass fiber paper is cured at a temperature of 150°C for 4 minutes (for samples 1 to 5) or at a temperature of 210°C for 10 minutes (for sample 5bis).

[0057] The storage modulus of the sample is measured using dynamic mechanical thermal analysis (DMTA) with a TA Instruments RSA-G2 analyzer, employing a three-point bending test during hardening.

[0058] The operating parameters of the measuring device are as follows: Temperature: 25℃, Poisson's ratio: 0.45 Duration of vibrational mechanical stress: 120 seconds. Oscillation frequency: 1.0Hz, Deformation: 0.1% Sample collection rate: 10 points / second.

[0059] Table 1 below shows the preserved modulus of the glass fiber paper obtained after curing each sizing composition. The values ​​for each preserved modulus are the calculated average of 2 to 4 individual measurements.

[0060] result

[0061] [Table 1]

[0062] It can be seen that glass fiber paper produced according to the present invention, i.e., glass fiber paper using sizing compositions 2 to 4 containing a combination of lignin A and a non-polymeric organic polycarboxylic acid, exhibits a higher storage modulus (1.18 GPa to 2.74 GPa) than glass fiber paper produced using sizing composition 1 (0.92 GPa) containing only lignin (i.e., without a crosslinking agent). Furthermore, a relatively high storage modulus is obtained for barrier articles produced using a sizing composition (composition 4) containing lignin A and citric acid. It can also be seen that glass fiber paper (compositions 2 to 4) produced according to the present invention exhibits the following: - A storage modulus higher than that of glass fiber paper obtained using a known thermosetting resin, such as a resin based on hydride sugar (Composition 5, Comparative Example), or - A storage modulus of elasticity equivalent to that of glass fiber paper obtained using a hydrogen-sugar-based resin when the temperature and duration of the curing process are increased (see Comparative Example 5bis).

[0063] Based on the total dry weight of each composition, an aqueous sizing composition is produced containing the components listed in Table 2, each expressed as a weight percentage.

[0064] Composition 6 (Comparative Example) is produced by emulsifying emulsifiable poly(methylenediphenyl isocyanate) (pMDI) with water. Compositions 7 and 8 according to the present invention are produced by mixing a first solution containing lignin A dissolved in water with a second solution containing succinic acid dissolved in water. Composition 9 (Comparative Example) is produced by mixing a first solution containing lignin A dissolved in water with a second solution containing ethylene glycol diglycidyl ether (epoxide) dissolved in water.

[0065] Sizing composition 6 contains 40% by weight of water and 60% by weight of dry matter. Sizing compositions 7 to 9 contain 90% by weight of water and 10% by weight of dry matter.

[0066] For each test, wood fibers are impregnated with an aqueous sizing composition. The amount of aqueous sizing compositions 6, 8, and 9 deposited on the wood fibers is equal to 7% by weight, expressed as dry matter, relative to the weight of the wood fibers. The amount of aqueous sizing composition 7 deposited on the wood fibers is equal to 10% by weight, expressed as dry matter, relative to the weight of the wood fibers.

[0067] Next, the impregnated wood fibers are uniformly deposited in a steel mold having an open cavity measuring 60 mm × 10 mm × 12 mm. A 60 mm × 10 mm × 10 mm steel bar is placed on top of the wood fibers, and the entire assembly is heated in a constant temperature press at 150°C and a pressure of 10 bar for 4 minutes. After the mold has cooled to room temperature, a test specimen (60 mm × 10 mm × 2 mm) of the formed lignocellulose fibers is removed.

[0068] The wood fiber specimens obtained in this way had a density of approximately 180 kg / m². 3 It has a density of .

[0069] The flexural modulus of elasticity (3-point bending) is determined for each sample by dynamic mechanical thermal analysis (DMTA) using a TA Instruments RSA-G2 analyzer. The samples are first dried for several hours in a desiccator under dynamic vacuum (20 mbar). The operating parameters of the measuring instrument are the same as those described above.

[0070] Table 2 below shows the preserved modulus of the wood fiber samples obtained after hardening of each sizing composition. The values ​​for each preserved modulus are the average values ​​calculated from 2 to 4 individual measurements.

[0071] result

[0072] [Table 2]

[0073] According to the present invention, that is, using sizing composition 8 containing a combination of lignin and succinic acid (as a lignin crosslinking agent), it can be seen that wood fiber test specimens produced have a higher storage modulus (50.6 GPa) than wood fiber test specimens produced using sizing composition 9 (comparative example), in which the lignin crosslinking agent is an epoxide rather than a nonpolymeric organic carboxylic acid. Similar storage moduli are obtained for wood fiber test specimens produced using the known sizing composition 6, and for wood fiber test specimens produced using sizing composition 7 according to the present invention, which contains a relatively large amount of the sizing composition on the fibers.

[0074] In conclusion, Tables 1 and 2 show that lignin combined with nonpolymeric organic carboxylic acids can be used to bond both inorganic and natural organic fibers, and can be used to obtain barrier articles with mechanical properties comparable to, or even better than, those obtained using known sizing compositions.

[0075] Example 2:

[0076] Lignin B was collected, and the amount of carboxylic acid functional groups and primary alcohol functional groups present on the lignin was determined by infrared spectroscopy, approximately 1190 cm⁻¹. -1 The intensity of the C-OOH bond peak of the carboxylic acid functional group located at approximately 1040 cm² -1 The intensity of the C-OH bond peak of the primary alcohol functional group located at 1000 cm is measured for all functional groups present on lignin B. -1 ~1300cm -1 It is determined by measuring and comparing it with the sum of the intensities of the CO bond peaks located at [location]. All functionalities present on lignin B that have CO bonds are: primary and secondary alcohol functional groups (C-OH); aromatic hydroxyl functional groups (Ar-OH), acid functional groups (C-OOH); aromatic ether functional groups (Ar-OC), aliphatic and cycloaliphatic ether functional groups (C-OC), and methyl ether functional groups (C-OCH3).

[0077] Next, the same measurement is performed on lignin B, which is first oxidized under the following conditions: in an aqueous solution with pH ≥ 13, using H2O2 + FeCl3 as the oxidizing agent, at 95°C for 120 minutes. In this case, all functional groups present on oxidized lignin B having CO bonds are as follows: primary and secondary alcohol functional groups (C-OH); aromatic hydroxyl functional groups (Ar-OH), acid functional groups (C-OOH); aromatic ether functional groups (Ar-OC), aliphatic and cycloaliphatic ether functional groups (C-OC), and methyl ether functional groups (C-OCH3).

[0078] Next, two sizing compositions 10 and 11 are prepared by mixing lignin B and oxidized lignin B, respectively, dissolved in water with succinic acid, which is dissolved in water. These sizing compositions are deposited onto wood fibers to produce a wood fiberboard specimen according to the method described in Example 1. The flexural retention modulus of the obtained wood fiber specimen is measured by dynamic mechanical thermal analysis (DMTA) as described in Example 1.

[0079] Table 3 shows the results obtained for each sizing composition.

[0080] [Table 3]

[0081] Using oxidized lignin B, which contains more carboxylic acid functional groups than "non-oxidized" lignin B (11% for oxidized lignin compared to less than 1% for "non-oxidized" lignin), can be seen as reducing the amount of succinic acid added to obtain a sizing composition in which the final barrier article has an equivalent storage modulus (37.5% when using oxidized lignin compared to 50% when using "non-oxidized" lignin). This disclosure includes the following aspects: <Aspect 1> A method for manufacturing a barrier article having inorganic fibers or natural organic fibers bound together by an organic binder, comprising the following steps: (a) Applying the sizing composition to the inorganic fiber or the natural organic fiber, (b) To form an aggregate of the inorganic fibers or the natural organic fibers, (c) Heating the aggregate of inorganic fibers or natural organic fibers until the sizing composition hardens to form the organic binder. The sizing composition includes: - At least one lignin that is potentially oxidized, and - At least one nonpolymeric organic polycarboxylic acid, A method characterized by including <Aspect 2> The method according to embodiment 1, wherein the lignin is selected from alkaline lignin, lignosulfonate, organosorb lignin, sodium lignin, lignin from a biorefining process of lignocellulose raw materials, also known as kraft lignin, or a mixture thereof. <Aspect 3> The method according to embodiment 1 or 2, wherein the amount of lignin is 25% to 85% by weight, preferably 40% to 80% by weight, based on the total dry weight of the sizing composition. <Aspect 4> The method according to embodiment 3, wherein the amount of nonpolymeric organic polycarboxylic acid is 15% to 75% by weight, preferably 20% to 60% by weight, based on the total dry weight of the sizing composition. <Aspect 5> The method according to embodiment 1 or 2, wherein the lignin is oxidized lignin, and its amount is 50% to 85% by weight, preferably 55% to 80% by weight, based on the total dry weight of the sizing composition, and the oxidized lignin comprises 2% to 20%, preferably 5% to 15%, of carboxylic acid functional groups and 2% to 20%, preferably 5% to 15%, of primary alcohol functional groups. <Aspect 6> The method according to embodiment 5, wherein the amount of nonpolymeric organic polycarboxylic acid is 15% to 50% by weight, preferably 20% to 45% by weight, based on the total dry weight of the sizing composition. <Aspect 7> The method according to any one of embodiments 1 to 6, wherein the nonpolymerizable organic polycarboxylic acid is selected from dicarboxylic acids, particularly oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, malic acid, tartaric acid, tartonic acid, aspartic acid, glutamic acid, fumaric acid, itaconic acid, maleic acid, traumatic acid, camphoric acid, phthalic acid and its derivatives, particularly those containing at least one boron or chlorine atom, tetrahydrophthalic acid and its derivatives, particularly those containing at least one chlorine atom, isophthalic acid, terephthalic acid, mesaconic acid and citraconic acid, tricarboxylic acids, particularly citric acid, tricarbaryl acid, 1,2,4-butanetricarboxylic acid, aconitic acid, hemimelitic acid, trimellitic acid and trimesic acid; and tetracarboxylic acids, particularly 1,2,3,4-butanetetracarboxylic acid and pyromellitic acid. <Aspect 8> The method according to any one of embodiments 1 to 7, wherein the inorganic fiber is glass fiber, rock fiber, slag fiber, or a mixture thereof. <Pattern 9> The method according to any one of embodiments 1 to 8, wherein the natural organic fiber is selected from wood, hemp, flax, sisal, cotton, jute, coconut, raffia, abaca fiber, or even fiber from grain straw or rice straw. <Aspect 10> The method according to any one of embodiments 1 to 9, wherein the application of the sizing composition in step (a) onto the inorganic fiber or natural organic fiber is carried out by spraying, roller coating, or impregnation. <Aspect 11> The method according to any one of embodiments 1 to 10, wherein the aggregate of inorganic fibers or natural organic fibers in step (b) is a fiber mat, a fiberboard or panel, a fiber-based molded article, or a woven or nonwoven fabric. <Aspect 12> The method according to any one of embodiments 1 to 11, wherein step (c) preferably includes heating the fiber aggregate in a temperature-controlled container or steam press at a temperature of 100°C to 250°C for a period of time of 1 to 20 minutes. <Aspect 13> A blocking article obtained by the method of any one of embodiments 1 to 12, comprising inorganic fibers or natural organic fibers and an organic binder obtained by curing a sizing composition comprising at least one potentially oxidized lignin and a nonpolymeric organic polycarboxylic acid. <Aspect 14> A barrier article according to embodiment 13, which is a net of inorganic fibers.

Claims

1. A method for manufacturing a barrier article having inorganic fibers or natural organic fibers bound together by an organic binder, comprising the following steps: (a) Applying the sizing composition to the inorganic fiber or the natural organic fiber, (b) To form an aggregate of the inorganic fibers or the natural organic fibers, (c) Heating the aggregate of inorganic fibers or natural organic fibers until the sizing composition hardens to form the organic binder. The sizing composition includes: - At least one lignin, and, - At least one nonpolymeric organic polycarboxylic acid, A method characterized by including

2. The method according to claim 1, wherein the lignin is selected from alkaline lignin, lignosulfonate, organosorb lignin, sodium lignin, lignin from a biorefining process of lignocellulose raw materials, also known as kraft lignin, or a mixture thereof.

3. The method according to claim 1 or 2, wherein the amount of lignin is 25% to 85% by weight, based on the total dry weight of the sizing composition.

4. The method according to claim 3, wherein the amount of nonpolymeric organic polycarboxylic acid is 15% to 75% by weight, based on the total dry weight of the sizing composition.

5. The method according to claim 1, wherein the lignin is oxidized lignin.

6. The method according to claim 5, wherein the oxidized lignin is obtained by oxidizing lignin selected from alkali lignin, lignosulfonate, organosorb lignin, sodium lignin, lignin from a biorefining process of lignocellulose raw materials, or a mixture thereof, also known as kraft lignin.

7. The method according to claim 5 or 6, wherein the lignin is oxidized lignin, and its amount is 50% to 85% by weight based on the total dry weight of the sizing composition, and the oxidized lignin comprises 2% to 20% carboxylic acid functional groups and 2% to 20% primary alcohol functional groups.

8. The method according to claim 7, wherein the amount of nonpolymeric organic polycarboxylic acid is 15% to 50% by weight, based on the total dry weight of the sizing composition.

9. The method according to claim 1 or 5, wherein the nonpolymeric organic polycarboxylic acid is selected from dicarboxylic acids, tricarboxylic acids, and tetracarboxylic acids.

10. The method according to claim 9, wherein the nonpolymeric organic polycarboxylic acid is selected from maleic acid, succinic acid, glutaric acid, itaconic acid, and citric acid.

11. The method according to claim 1 or 5, wherein the inorganic fiber is glass fiber, rock fiber, slag fiber, or a mixture thereof.

12. The method according to claim 1 or 5, wherein the natural organic fiber is selected from wood, hemp, flax, sisal, cotton, jute, coconut, raffia, abaca fiber, or even fiber from grain straw or rice straw.

13. The method according to claim 1 or 5, wherein the application of the sizing composition in step (a) onto the inorganic fiber or natural organic fiber is carried out by spraying, roller coating, or impregnation.

14. The method according to claim 1 or 5, wherein the aggregate of inorganic fibers or natural organic fibers in step (b) is a fiber mat, a fiberboard or panel, a fiber-based molded article, or a woven or nonwoven fabric.

15. The method according to claim 1 or 5, wherein step (c) includes heating the fiber aggregate at a temperature of 100°C to 250°C for a period of time of 1 to 20 minutes.

16. A blocking article comprising inorganic fibers or natural organic fibers bound together by an organic binder obtained by curing a sizing composition comprising at least one oxidizable lignin and a nonpolymeric organic polycarboxylic acid.

17. The barrier article according to claim 16, which is a net of inorganic fibers.

Citation Information

Patent Citations

  • Dry papermaking from waste paper

    JP1995026451A

  • Manufacturing method for laminated fiberboard

    JP2008272938A

  • Woody decorative laminate

    JP2011218777A

  • Sizing agent composition for mineral wool containing carbohydrates, organic polycarboxylic acid and reactive silicone, and the resulting insulating product

    JP2012528948A

  • Modified starch based binder

    US20110021101A1