Photonic crystal surface-emitting laser and method for manufacturing the same
By designing photonic crystal surface-emitting lasers with voids that allow faster semiconductor growth to close quickly, dislocations are suppressed, enhancing the laser's performance and reliability.
Patent Information
- Application Number
- JP2024536782
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-07-29
- Filing Date
- 2023-04-25
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-04-25
AI Technical Summary
Dislocations in the semiconductor layer of photonic crystal surface-emitting lasers (PCSELs) due to voids in the photonic crystal layer degrade the laser's characteristics.
The photonic crystal layer is designed with voids that extend from one surface to the other, where the length of the voids in one direction is shorter than in the other, allowing the semiconductor layer to grow faster and quickly close the voids, thereby suppressing dislocations.
This design suppresses dislocation-related degradation, improving the laser's properties such as reducing threshold current, increasing output power, and enhancing long-term reliability.
Smart Images

Figure 0007954720000001 
Figure 0007954720000002 
Figure 0007954720000003
Abstract
Description
Technical Field
[0001] The present disclosure relates to a photonic crystal surface emitting laser and a method for manufacturing the same. The present disclosure claims priority based on Japanese Application No. 2022-121596 filed on July 29, 2022, and the entire contents described in the aforementioned Japanese application are incorporated herein by reference.
Background Art
[0002] Photonic-crystal surface emitting lasers (PCSELs), in which a photonic crystal and an active layer having optical gain are stacked, are in use (e.g., Patent Documents 1 to 3). A photonic crystal includes a periodic structure having a refractive index different from that of a base material. By diffracting light within the plane of the photonic crystal, light oscillates at a wavelength based on the period and is emitted in the direction normal to the plane. Since the resonator extends in the plane, PCSELs are superior in single-mode operation and high output compared to edge-emitting lasers.
Prior Art Documents
Patent Documents
[0003]
Patent Document 1
Patent Document 2
Patent Document 3
Summary of the Invention
[0004] The photonic crystal surface-emitting laser according to this disclosure comprises an active layer, a photonic crystal layer, and a first semiconductor layer, wherein the photonic crystal layer has a base material and a plurality of vacancies periodically arranged in the base material, the vacancies extending from one surface of the photonic crystal layer to the opposite surface of the photonic crystal layer, and the first semiconductor layer is provided on the one surface of the photonic crystal layer. <110> The length of the vacancies in the direction is smaller than the length of the vacancies in the <1-10> direction of the photonic crystal layer.
[0005] A method for manufacturing a photonic crystal surface-emitting laser according to this disclosure comprises the steps of forming a plurality of periodically arranged voids in a base material of a photonic crystal layer, extending from one surface of the photonic crystal layer to the opposite surface, forming a first semiconductor layer on the one surface of the photonic crystal layer, and forming an active layer, wherein the photonic crystal layer <110> The length of the vacancies in the direction is smaller than the length of the vacancies in the <1-10> direction of the photonic crystal layer. [Brief explanation of the drawing]
[0006] [Figure 1] Figure 1 is a cross-sectional view illustrating a photonic crystal surface-emitting laser according to the first embodiment. [Figure 2A] Figure 2A is a top view illustrating a photonic crystal surface-emitting laser. [Figure 2B] Figure 2B is a bottom view illustrating a photonic crystal surface-emitting laser. [Figure 3] Figure 3 is a magnified cross-sectional view of a photonic crystal surface-emitting laser. [Figure 4A] Figure 4A is a plan view of the photonic crystal layer. [Figure 4B] Figure 4B is a magnified view of the photonic crystal layer. [Figure 5A] Figure 5A is a cross-sectional view illustrating a method for manufacturing a photonic crystal surface-emitting laser. [Figure 5B] Figure 5B is a cross-sectional view illustrating a method for manufacturing a photonic crystal surface-emitting laser. [Figure 6A] Figure 6A is a cross-sectional view illustrating a method for manufacturing a photonic crystal surface-emitting laser. [Figure 6B] Figure 6B is a cross-sectional view illustrating a method for manufacturing a photonic crystal surface-emitting laser. [Figure 7A] Figure 7A is a cross-sectional view illustrating a method for manufacturing a photonic crystal surface-emitting laser. [Figure 7B] Figure 7B is a cross-sectional view illustrating a method for manufacturing a photonic crystal surface-emitting laser. [Figure 8A] Figure 8A is a plan view illustrating a photonic crystal surface-emitting laser according to Comparative Example 1. [Figure 8B] Figure 8B is a plan view illustrating a photonic crystal surface-emitting laser according to Comparative Example 2. [Figure 9] Figure 9 is a cross-sectional view illustrating a modified photonic crystal surface-emitting laser. [Figure 10] Figure 10 is a plan view illustrating a photonic crystal surface-emitting laser according to the second embodiment. [Figure 11] Figure 11 is a plan view illustrating a photonic crystal surface-emitting laser according to the third embodiment. [Figure 12] Figure 12 is a plan view illustrating a photonic crystal surface-emitting laser according to the fourth embodiment. [Figure 13] Figure 13 is a plan view illustrating a photonic crystal surface-emitting laser according to the fifth embodiment. [Figure 14] Figure 14 is a plan view illustrating a photonic crystal surface-emitting laser according to the sixth embodiment. [Modes for carrying out the invention]
[0007] [Issues this disclosure aims to address] Voids are provided in the base material of the photonic crystal layer. Since the refractive index of the voids differs from the refractive index of the base material, light diffraction is possible. However, dislocations occur in the semiconductor layer provided over the photonic crystal layer having the voids. The dislocations degrade the crystallinity of the semiconductor layer, leading to deterioration of the characteristics of the PCSEL. Accordingly, an object is to provide a photonic crystal surface-emitting laser capable of suppressing dislocations in a semiconductor layer, and a method for manufacturing the same.
[0008] [Advantages of the Present Disclosure] According to the present disclosure, it is possible to provide a photonic crystal surface-emitting laser capable of suppressing characteristic deterioration, and a method for manufacturing the same.
[0009] [Description of Embodiments of the Present Disclosure] First, the contents of the embodiments of the present disclosure will be listed and described.
[0010] One aspect of the present disclosure is a photonic crystal surface-emitting laser comprising: an active layer, a photonic crystal layer, and a first semiconductor layer, wherein the photonic crystal layer has a base material and a plurality of voids periodically arranged in the base material, the voids extend from one surface of the photonic crystal layer to the opposite surface of the photonic crystal layer, the first semiconductor layer is provided on the one surface of the photonic crystal layer, and the length of the voids in the <110> direction of the photonic crystal layer is smaller than the length of the voids in the <1-10> direction of the photonic crystal layer. The growth rate of the first semiconductor layer in the <110> direction is higher than the growth rate in the <1-10> direction. The first semiconductor layer grows faster in the <110> direction, so that the voids are closed quickly. Closing the voids suppresses dislocations. Deterioration of the characteristics of the photonic crystal surface-emitting laser is suppressed. (2) In the above (1), the planar shape of the void has a first symmetry axis and a second symmetry axis, the length of the void in the direction of the first symmetry axis may be smaller than the length of the void in the direction of the second symmetry axis, and the angle formed by the first symmetry axis and the <110> direction of the photonic crystal layer may be 30° or less. Since the angle between the first symmetry axis and the <110> direction is 30°, the void is shortened in the <110> direction. The first semiconductor layer grows fast in the <110> direction. Since the void is closed quickly, dislocations are suppressed, and deterioration of the characteristics of the photonic crystal surface-emitting laser is suppressed. (3) In the above (1) or (2), the first symmetry axis may be parallel to the <110> direction. The void is shortened in the <110> direction. The first semiconductor layer grows fast in the <110> direction. Since the void is closed quickly, dislocations are suppressed, and deterioration of the characteristics of the photonic crystal surface-emitting laser is suppressed. (4) In any one of the above (1) to (3), the planar shape of the void is elliptical, and the minor axis of the void is aligned with the <110> direction may be parallel to. The void is shortened in the <110> direction. The first semiconductor layer grows fast in the <110> direction. Since the void is closed quickly, dislocations are suppressed, and deterioration of the characteristics of the photonic crystal surface-emitting laser is suppressed. (5) In any one of the above (1) to (4), the photonic crystal layer, the first semiconductor layer, and The active layer may be stacked this in order on the circuit board . The void is closed by the first semiconductor layer. The first semiconductor layer can be made thin, and the active layer can be brought close to the photonic crystal layer. Optical coupling between the active layer and the photonic crystal layer becomes stronger. Diffraction of light facilitates laser oscillation at a desired wavelength. (6) In any one of the above (1) to (4), the active layer, The first semiconductor layer and the photonic crystal layer may be stacked this in order on the circuit board . Deterioration of the characteristics of the photonic crystal surface-emitting laser is suppressed. (7) In any of (1) to (6) above, the plurality of vacancies are arranged in a square lattice in the plane of the photonic crystal layer, and the area of the vacancies relative to the area of the square lattice is Area The percentage can be between 3% and 30%. This suppresses the degradation of the properties of the photonic crystal surface-emitting laser. (8) In any of (1) to (7) above, the photonic crystal layer has a plurality of first vacancies and a plurality of second vacancies, the plurality of first vacancies and the plurality of second vacancies are periodically arranged in the base material, and in at least one of the first vacancies and the second vacancies, the photonic crystal layer <110> The length in the direction may be smaller than the length of the photonic crystal layer in the <1-10> direction. The first semiconductor layer is <110> It grows rapidly in the direction of the crystal. Because at least one of the first and second vacancies closes quickly, dislocations are suppressed, and the degradation of the properties of the photonic crystal surface-emitting laser is suppressed. (9) In any of (1) to (8) above, the photonic crystal layer may contain indium gallium arsenide phosphide or aluminum indium gallium arsenide, and the first semiconductor layer may contain indium phosphide. A vacancy is provided in the indium gallium arsenide phosphide. The first semiconductor layer of indium phosphide is <110> Growth is rapid in the direction, and vacancies are closed. Degradation of the properties of photonic crystal surface-emitting lasers is suppressed. (10) The photonic crystal layer comprises the steps of forming a plurality of vacancies periodically arranged in a base material of the photonic crystal layer and extending from one face of the photonic crystal layer to the opposite face, forming a first semiconductor layer on the one face of the photonic crystal layer, and forming an active layer, wherein the photonic crystal layer <110> The method for manufacturing a photonic crystal surface-emitting laser is such that the length of the vacancies in the direction is smaller than the length of the vacancies in the <1-10> direction of the photonic crystal layer. <110> The growth rate in the direction is higher than the growth rate in the <1-10> direction. The first semiconductor layer is <110> Rapid growth in a specific direction leads to faster closure of vacancies. This closure of vacancies suppresses dislocations, thereby reducing the degradation of the properties of photonic crystal surface-emitting lasers.
[0011] [Details of the embodiments of this disclosure] Specific examples of photonic crystal surface-emitting lasers and methods for manufacturing the same according to the embodiments of this disclosure will be described below with reference to the drawings. However, this disclosure is not limited to these examples and is intended to include all changes within the meaning and scope of the claims, as indicated by the claims.
[0012] <First Embodiment> (Photonic crystal surface-emitting laser) Figure 1 is a cross-sectional view illustrating a photonic crystal surface-emitting laser 100 according to the first embodiment. Figure 2A is a top view illustrating the photonic crystal surface-emitting laser 100, and Figure 2B is a bottom view.
[0013] As shown in Figure 1, the photonic crystal surface-emitting laser (PCSEL) 100 comprises a substrate 10, a cladding layer 12, a photonic crystal layer 14, a cladding layer 16 (first semiconductor layer), an active layer 18, a cladding layer 20, and a contact layer 22.
[0014] Semiconductor layers are stacked along the Z-axis. On the substrate 10, a cladding layer 12, a photonic crystal layer 14, a cladding layer 16, an active layer 18, a cladding layer 20, and a contact layer 22 are stacked in this order. The surface of each layer extends parallel to the XY plane. The X, Y, and Z axes are orthogonal to each other.
[0015] Grooves 23 are provided in the contact layer 22 and the cladding layer 20. The grooves 23 extend from the upper surface of the contact layer 22 to partway down the cladding layer 20. The bottom surface of the grooves 23 is recessed compared to the upper surfaces of the contact layer 22 and the cladding layer 20. As shown in Figure 2A, the planar shape of the grooves 23 is, for example, annular.
[0016] As shown in Figure 1, an insulating film 24 is provided on the upper surface of the contact layer 22. The insulating film 24 covers the upper surface of the contact layer 22 and is also provided inside the groove 23. The insulating film 24 is formed of an insulator such as silicon nitride (SiN) or silicon oxide (SiO2). The insulating film 24 has openings 24a and 24b. The contact layer 22 is exposed through openings 24a and 24b. As shown in Figure 2A, the planar shape of opening 24a is, for example, annular. Opening 24a is located outside the groove 23. The planar shape of opening 24b is, for example, circular. Opening 24b is located inside the groove 23.
[0017] As shown in Figure 1, an electrode 26 is provided on the insulating film 24. The electrode 26 is a p-type electrode and may be made of, for example, titanium (Ti), platinum (Pt), and gold (Au), or of other metals. The electrode 26 is provided across the entire upper surface of the insulating film 24 and contacts the upper surface of the contact layer 22 inside the opening 24a. That is, the electrode 26 is electrically connected to the contact layer 22. As shown in Figures 1 and 2A, the end (outer circumference) of the electrode 26 is located at the same position as the end of the opening 24a.
[0018] An electrode 28 is provided on the side of the substrate 10 opposite to the side on which the cladding layer 12 is provided. The electrode 28 is an n-type electrode and may be made of, for example, gold (Au), germanium (Ge), nickel (Ni), or other metals. The electrode 28 has an opening 28a in the center in the XY plane. As shown in Figure 2B, the planar shape of the opening 28a is, for example, circular. The substrate 10 is exposed through the opening 28a. The opening 28a functions as a light-emitting portion (aperture).
[0019] The substrate 10 and cladding layers 12 and 16 are formed of, for example, n-type indium phosphide (n-InP). The n-type dopant is, for example, silicon (Si). The thickness of cladding layer 12 is, for example, 500 nm. The thickness of cladding layer 16 is, for example, 100 nm.
[0020] The cladding layer 20 is formed of, for example, p-type indium phosphide (p-InP). The contact layer 22 is formed of, for example, p-type indium gallium arsenide (p-InGaAs). Dopant For example, zinc (Zn) is used. The thickness of the cladding layer 20 is, for example, 3 μm. The thickness of the contact layer 22 is, for example, 300 nm.
[0021] The photonic crystal layer 14 is formed of, for example, n-type indium gallium arsenide phosphate (InGaAsP) or aluminum indium gallium arsenide (AlInGaAs). The thickness of the photonic crystal layer 14 is, for example, 300 nm.
[0022] The active layer 18 includes multiple well layers and barrier layers, and has a multi-quantum well (MQW) structure. The well layers and barrier layers are formed of, for example, undoped indium gallium arsenide phosphate (InGaAsP) or aluminum gallium indium arsenide (AlGaInAs). The above materials are examples, and each layer may be formed of other materials, or of a combination of the above materials and other materials.
[0023] The refractive index of the active layer 18 is, for example, 3.5. The refractive indices of the cladding layers 12, 16, and 20 are, for example, 3.2. The refractive index of InGaAsP, the base material of the photonic crystal layer 14, is higher than that of the cladding layers 12, 16, and 20, for example, 3.4.
[0024] Figure 3 is an enlarged cross-sectional view of the photonic crystal surface-emitting laser 100, showing from cladding layer 12 to cladding layer 20. As shown in Figure 3, the photonic crystal layer 14 has a plurality of voids 30. The voids 30 extend from the surface of the photonic crystal layer 14 where the cladding layer 16 is provided (the top surface in Figure 3) toward the opposite surface of the photonic crystal layer 14 (the bottom surface in Figure 3), extending, for example, partway through the photonic crystal layer 14. The inside of the voids 30 is filled with air. The refractive index of the voids 30 is different from the refractive index of the base material of the photonic crystal layer 14.
[0025] Figures 4A and 4B are plan views of the photonic crystal layer 14. Figure 4A shows a plane containing multiple vacancies. Figure 4B shows a single vacancy. In Figures 4A and 4B, the photonic crystal layer 14 <110> The direction is upward. <1-10> The direction is to the right. <100> The direction is, <110> It is tilted at 45° with respect to the direction and the <1-10> direction.
[0026] As shown in Figure 4A, the multiple vacancies 30 are arranged periodically on the upper surface of the photonic crystal layer 14. The multiple vacancies 30 are arranged in a square lattice. In Figure 4A, the square lattice is shown by a dotted line. The edges of the square lattice are, <110> It is tilted at 45° with respect to the direction and the <1-10> direction, <100> Oriented in that direction. The void 30 and the square grid are <100> They are arranged periodically in a directional pattern. The number of voids 30 is, for example, several tens or several hundred.
[0027] The distance (period) a between the centers of adjacent vacancies 30 is equal to the length of the edge of one square grid. The distance a is determined according to the oscillation wavelength. For example, if the oscillation wavelength is 1300 nm, the distance a is approximately 400 nm.
[0028] As shown in Figure 4B, the void 30 is elliptical and has a minor axis 32 (first axis of symmetry) and a major axis 34 (second axis of symmetry). The void 30 is symmetric with respect to the minor axis 32 and symmetric with respect to the major axis 34. The minor axis 32 is <110> It is parallel to the direction. The major axis 34 is parallel to the <1-10> direction. The minor axis 32 and the major axis 34 are <100> It is tilted at a 45° angle from that direction.
[0029] The length L1 of the minor axis 32 is smaller than the length L2 of the major axis 34. The length L1 of the minor axis 32 is, for example, between 60 nm and 150 nm, and is, for example, 120 nm. The length L2 of the major axis 34 is, for example, between 100 nm and 355 nm, and is, for example, 280 nm.
[0030] Area a of one square lattice 2 The ratio of the area occupied by one void 30 to the total area (area filling rate) is, for example, 3% or more and 30% or less.
[0031] A voltage is applied to the photonic crystal surface-emitting laser 100 from electrodes 26 and 28. The active layer 18 has optical gain and generates light when carriers are injected. The photonic crystal layer 14 consists of multiple periodically arranged layers. sky Because of the presence of holes 30, the refractive index also changes periodically. Light undergoes Bragg diffraction within the plane of the photonic crystal layer 14. Light having a wavelength corresponding to the period of the holes 30 is amplified and laser oscillation occurs. The laser light is emitted in the direction normal to the photonic crystal layer 14 (Z-axis direction). In the example in Figure 1, the lower surface of the electrode 26 is mirror-finished and reflects light. The opening 28a of the electrode 28 becomes the light emission part (aperture), and light is emitted from the aperture.
[0032] (Manufacturing method) Figures 5A to 7B are cross-sectional views illustrating a method for manufacturing a photonic crystal surface-emitting laser 100. As shown in Figure 5A, for example, a cladding layer 12 and a photonic crystal layer 14 are epitaxially grown on a substrate 10 in that order by metal oxide chemical vapor deposition (MOCVD). In this process, the base material (InGaAsP) of the photonic crystal layer 14 is formed, but no voids 30 are formed.
[0033] Figures 5B to 6B are enlarged views of Figure 3. As shown in Figure 5B, a mask 31 is provided on the upper surface of the photonic crystal layer 14. The mask 31 is made of an insulator such as SiN. An insulating film is formed on the upper surface of the photonic crystal layer 14. A resist pattern is formed by an electron beam or the like, and the mask 31 is formed by transferring the resist pattern to the insulating film. The mask 31 has a plurality of openings 31a. The upper surface of the photonic crystal layer 14 is exposed through the openings 31a. The planar shape of the openings 31a is an ellipse corresponding to the void 30. The minor axis of the openings 31a is <110> It faces in a specific direction. The major axis faces in the <1-10> direction.
[0034] As shown in Figure 6A, multiple vacancies 30 are formed in the photonic crystal layer 14 by methods such as reactive ion etching (RIE). The etching proceeds, for example, partway through the photonic crystal layer 14, but not to the bottom surface of the photonic crystal layer 14. The vacancies 30 take the shape of ellipses corresponding to the openings 31a (see Figures 4A and 4B). After the etching is complete, the mask 31 is removed.
[0035] As shown in Figure 6B, a cladding layer 16, an active layer 18, a cladding layer 20, and a contact layer 22 are epitaxially grown on the photonic crystal layer 14. The voids 30 are closed by the cladding layer 16. The inside of the voids 30 is not filled by the cladding layer 16 and remains a cavity.
[0036] <110> The growth rate of cladding layer 16 in the direction is, <100> The growth rate in the direction and the growth rate in the <1-10> direction are greater. As shown in Figure 4B, the short axis 32 of the void 30 is <110> It is parallel to the direction. The cladding layer 16 grows rapidly in the direction of the minor axis 32 of the void 30. <110> The cladding layer 16, which has grown in the direction, closes the upper side of the void 30. The active layer 18, cladding layer 20, and contact layer 22 grow on top of the cladding layer 16.
[0037] As shown in Figure 7A, the insulating film 24 is formed, for example, by plasma CVD. Grooves 23 are provided in the insulating film 24 by resist patterning (resist pattern not shown) and etching.
[0038] As shown in Figure 7B, for example, an electrode 26 is provided on the contact layer 22 by vacuum deposition and lift-off. An electrode 28 is provided on the lower surface of the substrate 10. The photonic crystal surface-emitting laser 100 is formed by these steps.
[0039] Figure 8A is a plan view illustrating a photonic crystal surface-emitting laser according to Comparative Example 1, showing a portion of the photonic crystal layer 14 that includes one vacancy 30R1. As shown in Figure 8A, the long axis 34 of the vacancy 30R1 is <100> It faces in the direction. In other words, the void 30R1 is in the figure. 4 It faces a direction rotated 45° to the left from vacancy 30 of B. As in the examples in Figures 4A and 4B, the vacancies 30 are assumed to be arranged in a square grid with sides of 400 nm. <110> The length L3 in the direction is 170 nm, which is greater than the length L1 of the minor axis 32 of the void 30 in Figure 4B.
[0040] Figure 8B is a plan view illustrating a photonic crystal surface-emitting laser according to Comparative Example 2, and shows a portion of the photonic crystal layer 14 that includes one vacancy 30R2. As shown in Figure 8B, vacancy 30R 2 The long axis 34 is <110> It faces in the direction. In other words, the void 30R2 is in the figure. 4 The direction is rotated 90° to the left from vacancy 30 B. As in the examples in Figures 4A and 4B, the vacancies 30 are assumed to be arranged in a square grid with sides of 400 nm. <110> The length L4 in the direction is equal to the length of the major axis 34, for example, 280 nm, and is greater than the length L1 of the minor axis 32 of the void 30 in Figure 4B.
[0041] Crystal growth in semiconductor layers on vacancies proceeds from the edge of the vacancy towards the top of the vacancy, sealing the vacancy. In III-V semiconductors such as InP-based and GaAs-based semiconductors, due to the relationship of the atomic structure, the growth rate is low in the <1-10> direction. <110> It has a high growth rate in the direction. When growing a GaAs-based semiconductor layer on a vacancy with a shape having a long axis and a short axis, if there is a difference in the growth rate between the long axis and the short axis, crystal defects (dislocations) are likely to occur. When growing a GaAs-based semiconductor on a vacancy 30R1, the difference between the growth rate with respect to the long axis and the growth rate with respect to the short axis is small. Therefore, a cladding layer with few dislocations can be grown. In other words, the vacancy 30R1 can be closed with a good GaAs-based semiconductor layer with few dislocations. However, the inventors have found that in semiconductor layers other than GaAs-based, the crystal growth pattern differs due to the difference in materials. For example, in InP-based semiconductors, closing the vacancy in a short time is more effective in suppressing crystal defects in the cladding layer than reducing the difference between the growth rate with respect to the long axis and the growth rate with respect to the short axis. For example, the InP cladding layer 16 has a low growth rate in the <1-10> direction, <110> It has a high growth rate in that direction. (See example in Figure 8A) <110> The length L3 in the direction is shown in Figure 4. B It is greater than the length L1 in the example in Figure 8B. <110> The length L4 in the direction is greater than the length L1. It takes a long time for the vacancy to close. In experiments using InP-based semiconductors, there is a possibility that dislocations have occurred in the cladding layer 16 on vacancy 30R1 and the cladding layer 16 on vacancy 30R2. Dislocations in the cladding layer 16 may degrade the properties of the photonic crystal surface-emitting laser.
[0042] According to the first embodiment, the photonic crystal layer 14 has a plurality of voids 30. <110> The length L1 in the <1-10> direction is smaller than the length L2 in the <1-10> direction. <110> The growth rate of cladding layer 16 in the direction is, <100> The growth rate in the direction and the growth rate in the <1-10> direction are higher. Cladding layer 16 <110> By growing rapidly in the direction, the vacancies 30 are quickly closed by the cladding layer 16. The closure of the vacancies 30 makes it less likely for dislocations to occur in the cladding layer 16. This suppresses the degradation of the photonic crystal surface-emitting laser 100's properties caused by dislocations. The suppression of dislocations improves the crystallinity of the cladding layer 16 and the layers above it (such as the active layer 18). This improves the properties of the photonic crystal surface-emitting laser 100. For example, it allows for a reduction in threshold current and an increase in output power. Long-term reliability also improves.
[0043] As shown in Figure 4B, the planar shape of the void 30 is elliptical and has two axes of symmetry (minor axis 32 and major axis 34). The length L1 of the void 30 in the direction of the minor axis 32 is smaller than the length L2 of the void 30 in the direction of the major axis 34. The minor axis 32 is <110> The direction is parallel. Because the direction in which the growth rate of the cladding layer 16 is high is parallel to the direction of the short axis 32 of the vacancies 30, the cladding layer 16 grows faster in the direction of the short axis 32 compared to other directions. The vacancies 30 are closed quickly by the cladding layer 16. This suppresses dislocations in the semiconductor layer, such as the cladding layer 16. By suppressing dislocations, the characteristics of the photonic crystal surface-emitting laser 100 are improved.
[0044] As shown in Figure 1, the photonic crystal layer 14, the cladding layer 16, and the active layer 18 are stacked in this order. The voids 30 in the photonic crystal layer 14 are closed by the cladding layer 16. The active layer 18 grows on top of the cladding layer 16. Because the voids 30 are closed quickly, dislocations are less likely to occur in the cladding layer 16 and the active layer 18 on top of the photonic crystal layer 14. The surface of the cladding layer 16 is flatter than the surface of the photonic crystal layer 14. Since the active layer 18 grows on a flat surface, it has high crystallinity.
[0045] The cladding layer 16 grows rapidly and closes the vacancies 30, thereby suppressing the generation of dislocations in the cladding layer 16. Even if the cladding layer 16 is thinned to, for example, 50 nm or more and 200 nm or less, the generation of dislocations is suppressed. By thinning the cladding layer 16, the distance between the active layer 18 and the photonic crystal layer 14 decreases. The coupling of light between the active layer 18 and the photonic crystal layer 14 becomes stronger. The light generated in the active layer 18 is strongly influenced by the photonic crystal layer 14. The diffraction of light makes it easier to oscillate at the desired wavelength. In other words, the output of the laser light increases.
[0046] As shown in Figure 4A, multiple voids 30 are arranged in a square grid. The ratio of the area of the voids 30 to the area of one square grid is 5% or more and 20% or less. Laser oscillation is possible by diffracting light. The ratio of the area of the voids 30 may also be, for example, 3% or more, 10% or more, 15% or less, or 30% or less.
[0047] When the resonant wavelength is 1300 nm, the length of one side a of the square lattice is 400 nm. The length L1 of the minor axis 32 of the vacancy 30 is 60 nm or more and 150 nm or less. The length L2 of the major axis 34 is 100 nm or more and 355 nm or less. The length L1 of the minor axis 32 is within the above range and is smaller than the length L2. The above dimensions may be changed depending on the resonant wavelength.
[0048] The photonic crystal layer 14 is formed of, for example, InGaAsP or AlInGaAs. The photonic crystal layer 14 is a semiconductor layer containing the compound semiconductor described above. The cladding layer 16 contains InP and is formed of, for example, n-type InP. The growth rate varies depending on the crystal orientation. The cladding layer 16 is <110> It has a high growth rate in the direction. The short axis 32 of the void 30 <110> By orienting it in that direction, the void 30 can be quickly closed by the cladding layer 16. <110> By growing a semiconductor with a high growth rate in the direction, such as InP, on the photonic crystal layer 14, the vacancies 30 can be closed quickly.
[0049] The void 30 is shown in the figure.3 As shown, the material may be stretched partway through the photonic crystal layer 14, or it may be stretched through the photonic crystal layer 14 to the cladding layer 12.
[0050] (modified version) Figure 9 is a cross-sectional view illustrating a modified photonic crystal surface-emitting laser 110. The same configuration as in the first embodiment will not be described. As shown in Figure 9, the substrate 10, cladding layer 12, active layer 18, cladding layer 16, photonic crystal layer 14, and cladding layer 20 are stacked in this order. The active layer 18 is provided between the cladding layer 12 and the photonic crystal layer 14.
[0051] The photonic crystal layer 14 has elliptical pores 30, as shown in Figures 4A and 4B. The minor axis 32 is <110> The orientation is correct. Because the vacancies 30 can be closed quickly, the generation of dislocations is suppressed. The properties of the photonic crystal surface-emitting laser 110 are improved.
[0052] <Second Embodiment> Figure 10 is a plan view illustrating a photonic crystal surface-emitting laser according to the second embodiment, showing a magnified view of the vacancies 30 in the photonic crystal layer 14. The same configuration as in the first embodiment will not be described. The vacancies 30 and square lattice in Figure 10 are located at a position rotated to the left by an angle θ from the vacancies 30 and square lattice in Figure 4B. The short axis 32 of the vacancies 30 is <110> It is inclined with respect to the direction. The minor axis is 32 and <110> The angle θ between the direction is, for example, 30° or less.
[0053] Similar to the examples in Figures 4A and 4B, the voids 30 are arranged in a square grid with sides of 400 nm. <110> The length L5 in the <1-10> direction is 139 nm, which is smaller than the length L6 in the <1-10> direction.
[0054] According to the second embodiment, the void 30 <110> The length L5 in the direction is smaller than the length L6 in the <1-10> direction. Cladding layer 16 <110> Rapid growth in the direction closes the vacancies 30. Closing the vacancies 30 makes it less likely for dislocations to occur in the cladding layer 16. This suppresses the degradation of the properties of the photonic crystal surface-emitting laser.
[0055] Short axis 32 and <110> The angle θ between the direction is, for example, 30° or less. By setting the angle θ to 30° or less, the length L5 becomes smaller. The cladding layer 16 can close the void 30 quickly. The angle θ may also be, for example, 35° or less, 20° or less, 10° or less, or 5° or less. The smaller the angle θ, the shorter the minor axis 32 <110> It approaches the direction. The smaller the angle θ, the smaller the length L5 shown in Figure 10. If the angle θ is 0°, the minor axis 32 is as shown in Figure 4B. <110> It is parallel to the direction. At θ=0°, length L5 is equal to length L1 in Figure 4B. The smaller length L5, the faster the void 30 can be closed.
[0056] The shape of the void 30 is determined by the shape of the opening 31a of the mask 31 used for etching. By making the opening 31a elliptical, the void 30 also becomes elliptical. The minor axis of the opening 31a is <110> By making it parallel to the direction, the minor axis 32 of the void 30 is also as shown in Figure 4B. <110> It becomes parallel to the direction. The minor axis of the opening 31a <110> When tilted at an angle θ from the direction, the minor axis 32 of the void 30 also changes as shown in Figure 10. <110> It is tilted at an angle θ from the direction.
[0057] In the example in Figure 10, the minor axis 32 is, <110> It faces the direction rotated counterclockwise by an angle θ from the original direction. The minor axis 32 is, <110> It is also acceptable to face a direction that is rotated clockwise by an angle θ from the original direction.
[0058] <Third Embodiment> Figure 11 is a plan view illustrating a photonic crystal surface-emitting laser according to the third embodiment, illustrating one square lattice of the photonic crystal layer 14. The same configuration as in the first embodiment will not be described. Two vacancies 30 (first vacancy) and 36 (second vacancy) are provided in one square lattice. The planar shapes of vacancies 30 and 36 are elliptical.
[0059] The void 36 is smaller than the void 30 and similar to the void 30. The minor axis 32 of the void 30 and the minor axis 37 of the void 36 are <110> The major axes 34 of the void 30 and 38 of the void 36 are parallel to the <1-10> direction. The void 30 has the same shape as, for example, the example in Figure 4B. The minor axis 37 of the void 36 is shorter than the minor axis 32 of the void 30. The major axis 38 of the void 36 is shorter than the major axis 34 of the void 30.
[0060] According to the third embodiment, the short axes of the voids 30 and 36 are <110> It is parallel to the direction. The cladding layer 16 is <110> It has a high growth rate in the direction. Vacancies 30 and 36 are quickly closed by the cladding layer 16. Dislocations are suppressed, and the degradation of the properties of the photonic crystal surface-emitting laser is suppressed.
[0061] The photonic crystal layer 14 has two vacancies 30 and 36 in one square lattice. The number of vacancies in one square lattice may be two or more, for example, three or more, or four or more. In at least one vacancy, <110> The length in the <1-10> direction is smaller than the length in the <1-10> direction. For example, let the planar shape of at least one of the multiple voids be an ellipse. The minor axis of the void on the ellipse is, <110> Direct it to a range of angles less than or equal to θ from the direction.
[0062] In Figure 11, both of the two voids 30 and 36 are elliptical. One or both of the two voids 30 and 36 may have a shape other than an ellipse. A shape other than an ellipse would be a polygon, as shown in the fourth to sixth embodiments.
[0063] <Fourth Embodiment> Figure 12 is a plan view illustrating a photonic crystal surface-emitting laser according to the fourth embodiment, showing one of the square lattices in the photonic crystal layer 14. The same configuration as in the first embodiment will not be described.
[0064] A void 40 is provided in the photonic crystal layer 14. The planar shape of the void 40 is rectangular. The void 40 has a minor axis 41 and a major axis 42. The minor axis 41 is shorter than the major axis 42. The minor axis 41 is <110> It is parallel to the direction. The major axis 42 is parallel to the <1-10> direction.
[0065] According to the fourth embodiment, the short axis 41 of the void 40 is <110> It is parallel to the direction. Cladding layer 16 <110> By growing rapidly in the direction, the vacancies 40 are quickly closed by the cladding layer 16. As the vacancies 40 are closed, dislocations are less likely to occur in the cladding layer 16. By suppressing dislocations, the degradation of the properties of the photonic crystal surface-emitting laser is suppressed.
[0066] <Fifth Embodiment> Figure 13 is a plan view illustrating a photonic crystal surface-emitting laser according to the fifth embodiment, showing one square lattice of the photonic crystal layer 14. The same configuration as in the first embodiment will not be described.
[0067] A void 44 is provided in the photonic crystal layer 14. The planar shape of the void 44 is rhombic. The void 44 has a minor axis 45 and a major axis 46. The minor axis 45 is shorter than the major axis 46. The minor axis 45 is <110> It is parallel to the direction. The major axis 46 is parallel to the <1-10> direction.
[0068] According to the fifth embodiment, the short axis 45 of the void 44 is <110> It is parallel to the direction. Cladding layer 16 <110> By growing rapidly in the direction, the vacancies 44 are quickly closed by the cladding layer 16. As the vacancies 44 are closed, dislocations are less likely to occur in the cladding layer 16. By suppressing dislocations, the degradation of the properties of the photonic crystal surface-emitting laser is suppressed.
[0069] In the first to fifth embodiments, the void has two axes of symmetry. With respect to each of the two axes of symmetry, the void is line-symmetric. The void may be strictly line-symmetric, or it may deviate from line symmetry within the range of manufacturing tolerances, for example. The shape of the void is determined by the etching precision, etc. Depending on the etching precision, etc., the void may deviate slightly from line symmetry.
[0070] <Sixth Embodiment> Figure 14 is a plan view illustrating a photonic crystal surface-emitting laser according to the sixth embodiment, showing one square lattice of the photonic crystal layer 14. The same configuration as in the first embodiment will not be described.
[0071] A void 50 is provided in the photonic crystal layer 14. The planar shape of the void 50 is triangular. One side 51 of the void 50 is <110> It is parallel to the direction. Of the vertices of the hole 50, let vertex 52 be the vertex opposite side 51. Let line segment 53 be the line segment that passes through vertex 52 and bisects side 51. Line segment 53 is parallel to the <1-10> direction. Side 51 is shorter than line segment 53.
[0072] According to the sixth embodiment, the side 51 of the void 50 is <110> It is parallel to the direction and shorter than line segment 53 in the <1-10> direction. Cladding layer 16 <110> By growing rapidly in the direction, the vacancies 50 are quickly closed by the cladding layer 16. As the vacancies 50 are closed, dislocations are less likely to occur in the cladding layer 16. By suppressing dislocations, the degradation of the properties of the photonic crystal surface-emitting laser is suppressed.
[0073] As shown in the first embodiment, the planar shape of the void may be elliptical. As shown in the fourth to sixth embodiments, the planar shape of the void may be polygonal. The vertices of the polygon may include curves.
[0074] While embodiments of this disclosure have been described in detail above, this disclosure is not limited to these specific embodiments, and various modifications and changes are possible within the scope of the gist of this disclosure as described in the claims. [Explanation of symbols]
[0075] 10 circuit boards 12, 16, 20 Cladding layers 14 Photonic crystal layer 18 Active layer 22 Contact Layer 23 Groove 24 Insulating film 24a, 24b, 28a, 31a opening 26, 28 electrodes 31 masks 30, 30R1, 30R2, 36, 40, 50 holes 32, 37, 45 short axis 34, 38, 46 long axis 51 sides 52 vertices 53 line segments 100, 110 Photonic crystal surface-emitting lasers
Claims
1. The active layer, Photonic crystal layer and A first semiconductor layer and a first semiconductor layer are provided, The photonic crystal layer has a base material and a plurality of voids periodically arranged in the base material. The void extends from one surface of the photonic crystal layer to the opposite surface of the photonic crystal layer. The first semiconductor layer is provided on one surface of the photonic crystal layer, The length of the vacancy in the <110> direction of the photonic crystal layer is smaller than the length of the vacancy in the <1-10> direction of the photonic crystal layer. The aforementioned photonic crystal layer contains indium gallium arsenide phosphorus or aluminum indium gallium arsenide. The first semiconductor layer is a photonic crystal surface-emitting laser containing indium phosphide.
2. The planar shape of the aforementioned void has a first axis of symmetry and a second axis of symmetry. The length of the void in the direction of the first axis of symmetry is smaller than the length of the void in the direction of the second axis of symmetry. The photonic crystal surface emitting laser according to claim 1, wherein the angle between the first axis of symmetry and the <110> direction of the photonic crystal layer is 30° or less.
3. The photonic crystal surface emitting laser according to claim 2, wherein the first axis of symmetry is parallel to the <110> direction.
4. The planar shape of the aforementioned void is elliptical. The photonic crystal surface emitting laser according to claim 3, wherein the short axis of the void is parallel to the <110> direction.
5. The photonic crystal surface emitting laser according to claim 1 or claim 2, wherein the photonic crystal layer, the first semiconductor layer, and the active layer are stacked on a substrate in this order.
6. The photonic crystal surface emitting laser according to claim 1 or claim 2, wherein the active layer, the first semiconductor layer, and the photonic crystal layer are stacked on a substrate in this order.
7. The plurality of voids are arranged to form a square lattice in the plane of the photonic crystal layer. The photonic crystal surface emitting laser according to claim 1 or claim 2, wherein the ratio of the area of the vacancies to the area of the square lattice is 3% or more and 30% or less.
8. The photonic crystal layer has a plurality of first vacancies and a plurality of second vacancies, The plurality of first voids and the plurality of second voids are periodically arranged in the base material. The photonic crystal surface emitting laser according to claim 1 or claim 2, wherein in at least one of the first vacancy and the second vacancy, the length of the photonic crystal layer in the <110> direction is smaller than the length of the photonic crystal layer in the <1-10> direction.
9. A step of forming a plurality of voids in a base material of a photonic crystal layer, which are periodically arranged and extend from one surface of the photonic crystal layer to the opposite surface, A step of forming a first semiconductor layer on one surface of the photonic crystal layer, The process includes a step of forming an active layer, The length of the vacancy in the <110> direction of the photonic crystal layer is smaller than the length of the vacancy in the <1-10> direction of the photonic crystal layer. The aforementioned photonic crystal layer contains indium gallium arsenide phosphorus or aluminum indium gallium arsenide. The first semiconductor layer is a method for manufacturing a photonic crystal surface-emitting laser containing indium phosphide.
Citation Information
Patent Citations
Two-dimensional photonic crystal face emitting laser array and two-dimensional photonic crystal face emitting laser
JP2003273460A
Semiconductor light emitting device and its manufacturing method
JP2004253811A
2-dimensional photonic crystal surface emitting laser light source
JP2007073571A
Two-dimensional photonic crystal surface light emitting laser light source
JP2007180120A
Two-dimensional photonic crystalline surface emitting laser
JP2008243962A