Laminate

The laminate structure with varying matrix element content and diffusion suppression layers addresses thermal conductivity challenges in phase change materials, ensuring smooth conductivity changes and efficient temperature control.

JP7954722B2Active Publication Date: 2026-11-20SUMITOMO ELECTRIC INDUSTRIES LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024546703
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-14
Filing Date
2023-05-10
Publication Date
2026-11-20
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

Solid phase change materials with sharp thermal conductivity changes at certain temperatures pose challenges for applications in thermal control devices.

Method used

A laminate structure composed of multiple material layers with varying content of a first and second matrix element, separated by diffusion suppression layers, to smooth thermal conductivity changes with ambient temperature.

Benefits of technology

Enables efficient temperature control in devices by minimizing abrupt thermal conductivity changes, enhancing reliability and durability through suppressed atomic diffusion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007954722000003
    Figure 0007954722000003
  • Figure 0007954722000004
    Figure 0007954722000004
  • Figure 0007954722000005
    Figure 0007954722000005
Patent Text Reader

Abstract

This laminate comprises a plurality of material layers configured from a solid phase changing material that includes: a first base material element; and a second base material element different from the first base material element. The plurality of material layers include: a first material layer in which the content ratio of the first base material element is the largest; and a second material layer in which the content ratio of the first base material element is the smallest. A difference in the content ratios obtained by subtracting the content ratio of the first base material element in the second material layer from the content ratio of the first base material element in the first material layer is 10 at% or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to laminates. This application claims priority under Japanese application No. 2022-146482 filed on 14 September 2022, and incorporates all the provisions of the said Japanese application. [Background technology]

[0002] A silver chalcogenide material whose thermal conductivity changes with temperature has been disclosed (for example, Non-Patent Document 1). [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] Keisuke Hirata et al., “High-Performance Solid-State Thermal Diode Consisting of Ag2(S,Se,Te)”, Journal of ELECTRONIC MATERIALS 49,2895(2020) [Overview of the Initiative]

[0004] A laminate according to this disclosure includes a plurality of material layers composed of a solid phase-change material containing a first matrix element and a second matrix element different from the first matrix element. The plurality of material layers include a first material layer having the highest content of the first matrix element and a second material layer having the lowest content of the first matrix element. The difference in content between the first matrix element in the first material layer and the first matrix element in the second material layer is 10 at% or more. [Brief explanation of the drawing]

[0005] [Figure 1] Figure 1 is a schematic side view showing the structure of the laminate according to Embodiment 1. [Figure 2] Figure 2 is a magnified view of a portion of the laminate shown in Figure 1. [Figure 3] FIG. 3 is a schematic perspective view of the laminate shown in FIG. 1. [Figure 4] FIG. 4 is a schematic side view showing the structure of the laminate according to Embodiment 2. [Figure 5] FIG. 5 is a schematic side view showing the structure of the laminate according to Embodiment 3. [Figure 6] FIG. 6 is a phase diagram of the solid phase change material in the aforementioned silver chalcogenide-based material. [Figure 7] FIG. 7 is a graph schematically showing the relationship between temperature and thermal conductivity when the composition ratio is in region R1 and region R3. [Figure 8] FIG. 8 is a graph schematically showing the relationship between temperature and thermal conductivity when the composition ratio is in region R2. [Figure 9] FIG. 9 is a graph showing the relationship between temperature and thermal conductivity in Sample 1 to Sample 6. [Figure 10] FIG. 10 is a graph showing the relationship between temperature and thermal conductivity in Sample 7 to Sample 12. [Modes for Carrying Out the Invention]

[0006] [Problems to be Solved by the Present Disclosure] As disclosed in Non-Patent Document 1, a solid phase change material such as a silver chalcogenide material has a thermal conductivity that changes sharply at a certain temperature as a boundary. For this reason, it is difficult to apply such a solid phase change material to devices involving thermal control such as thermoelectric conversion.

[0007] Accordingly, one of the objects is to provide a laminate that can be easily applied to devices involving thermal control.

[0008] [Advantages of the Present Disclosure] The above-described laminate facilitates application to devices involving thermal control.

[0009] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described. The laminate according to the present disclosure includes a plurality of material layers composed of a solid phase change material containing a first matrix element and a second matrix element different from the first matrix element. The plurality of material layers include a first material layer having the highest content of the first matrix element and a second material layer having the lowest content of the first matrix element. The difference in content between the content of the first matrix element in the first material layer and the content of the first matrix element in the second material layer is 10 at% or more.

[0010] Some devices, such as lasers, require temperature control functions, such as maintaining a constant temperature. Temperature control is achieved through heating and cooling using heaters and cooling elements, or by enhancing heat insulation and heat dissipation with insulating materials and heat sinks. The inventors of this invention focused on solid phase-change materials that exhibit different thermal conductivity depending on temperature. By combining these materials with elements, heating and cooling can be performed efficiently. However, because the change in thermal conductivity with respect to temperature is steep, these materials are difficult to use for temperature control in devices. Therefore, the inventors sought to improve this drawback and arrived at the present invention.

[0011] The laminate relating to this disclosure is (1) The material comprises multiple material layers composed of a solid phase-change material containing a first base material element and a second base material element different from the first base material element. The multiple material layers include a first material layer having the highest content of the first base material element and a second material layer having the lowest content of the first base material element. The inventors have found that when a phase transformation occurs in a solid phase-change material, the carrier concentration in the phase changes, and as a result, the thermal conductivity changes. Therefore, in a uniform thermal control material, i.e., a thermal control material as a bulk material, in order to avoid abrupt changes in the thermal conductivity of the thermal control material when the ambient temperature changes, a multilayer structure composed of multiple material layers is adopted, and a difference in the content of the first base material element is made between the first material layer and the second material layer. By doing so, it is thought that a difference in the degree of phase transformation is made between the first material layer and the second material layer, creating a difference in thermal conductivity, and thus abrupt changes in thermal conductivity at a certain temperature can be avoided. Furthermore, the inventors conducted further intensive studies and discovered that by setting the difference in content between the first material layer and the second material layer, after subtracting the content of the first base material element, to 10 at% or more, the change in thermal conductivity in a laminate used as a thermal control material during changes in ambient temperature can be made smoother. With such a laminate, even in situations where the ambient temperature changes, the thermal conductivity can be smoothly changed in accordance with the ambient temperature, enabling efficient temperature control of the device. Therefore, such a laminate is easily applicable to devices that require thermal control. In this disclosure, the laminate refers to a laminate in which multiple layers having the characteristic of changing thermal conductivity due to temperature, external voltage, etc., are stacked.

[0012] (2) In (1) above, a diffusion suppression layer may be further provided, which is disposed between the first material layer and the second material layer to suppress the diffusion of atoms contained in each material layer to the other material layer. By doing so, the diffusion of atoms contained in each material layer to the other material layer during phase transformation is suppressed, specifically the diffusion of atoms contained in the first material layer to the second material layer and the diffusion of atoms contained in the second material layer to the first material layer, thereby reducing the risk of changes in the composition of the first material layer and the composition of the second material layer. In other words, by providing such a diffusion suppression layer, reactions between material layers and reactions with other materials can be suppressed, and deterioration due to phase transformation during repeated use can be prevented.

[0013] (3) In (1) or (2) above, the solid phase change material may include a silver chalcogenide-based material. Such materials are easily applicable to devices that require thermal control.

[0014] (4) In (3) above, the first base material element and the second base material element may each be an element selected from the group consisting of sulfur, selenium, and tellurium. The solid phase change material is Ag2S x Se 1-x Ag2S x Te 1-x or Ag2Se x Te 1-x It may also be expressed as follows. x may have the relationship 0 ≤ x ≤ 1. A laminate containing multiple material layers composed of such solid phase change materials can smoothly change its thermal conductivity even when the ambient temperature changes, enabling efficient temperature control of the device.

[0015] (5) In any of (1) to (4) above, the thickness of each of the multiple material layers may be 10 μm or more and 5 mm or less. By making the thickness of the material layer 10 μm or more, when the diffusion suppression layer comes into contact with the material layer, the material layer can be made thick enough to ensure that a phase transformation is unlikely to occur from the contacting diffusion suppression layer. Furthermore, by making the thickness of the material layer 5 mm or less, the deposition of elements within a single material layer due to ion conduction when a temperature difference is applied can be suppressed, thereby improving reliability.

[0016] (6) In (2) above, the diffusion suppression layer may be composed of at least one of SiO2, SiN, SiON, and epoxy resin. A diffusion suppression layer composed of such a material can more reliably suppress the diffusion of atoms contained in each material layer to other material layers.

[0017] (7) In (2) above, the thickness of the diffusion suppression layer is 10 nm or more, and may be thinner than the thickest material layer among the multiple material layers. By making the thickness of the diffusion suppression layer 10 nm or more, the diffusion of atoms between each layer can be reliably suppressed. Furthermore, by making the thickness of the diffusion suppression layer thinner than the thickest material layer, the influence of the diffusion suppression layer on the thermal conductivity of the laminate can be reduced.

[0018] (8) In any of (1) to (7) above, the plurality of material layers may further include a third material layer composed of a solid phase change material containing a first base material element and a second base material element. The plurality of material layers may be arranged in the order of the first material layer, the third material layer, and the second material layer in the thickness direction. By doing so, the content ratio of the first base material element in the laminate can be gradually changed, making the change in thermal conductivity between each material layer smoother. Therefore, the temperature control of the device can be performed more efficiently.

[0019] (9) The above (8) may further include diffusion suppression layers disposed between the first material layer and the third material layer and between the third material layer and the second material layer, respectively, to suppress the diffusion of atoms contained in each material layer to the other material layers. In this way, the diffusion of atoms between the first material layer and the third material layer and the diffusion of atoms between the third material layer and the second material layer can be efficiently suppressed. That is, the diffusion of atoms contained in the first material layer to the third material layer, the diffusion of atoms contained in the third material layer to the first material layer, the diffusion of atoms contained in the third material layer to the second material layer, and the diffusion of atoms contained in the second material layer to the third material layer can be efficiently suppressed.

[0020] (10) In any of (1) to (7) above, the plurality of material layers may further include a third material layer composed of a solid phase change material containing a first base material element and a second base material element. The plurality of material layers may be arranged in the order of the first material layer, the second material layer, and the third material layer in the thickness direction. In this way, even if the third material layer is located in a portion other than between the first material layer and the second material layer, the change in thermal conductivity in the first material layer and the second material layer when the ambient temperature changes can be smoothed out. Therefore, the temperature control of the device can be performed more efficiently.

[0021] (11) The above (10) may further include a diffusion suppression layer disposed between the second material layer and the third material layer to suppress the diffusion of atoms contained in each material layer to the other material layer. By doing so, the diffusion of atoms between the second material layer and the third material layer can be efficiently suppressed. That is, the diffusion of atoms contained in the second material layer to the third material layer and the diffusion of atoms contained in the third material layer to the second material layer can be efficiently suppressed.

[0022] [Details of the embodiments of this disclosure] Next, embodiments of the laminates of this disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are denoted by the same reference numerals, and their descriptions will not be repeated.

[0023] (Embodiment 1) Embodiment 1, which is one embodiment of the laminate according to this disclosure, will be described with reference to Figure 1. Figure 1 is a schematic side view showing the structure of the laminate according to Embodiment 1. In Figure 1, the thickness of each layer is exaggerated to facilitate understanding. Figure 2 is a magnified view of a part of the laminate shown in Figure 1. Figure 3 is a schematic perspective view of the laminate shown in Figure 1. In Figure 1 and the following figures, the thickness direction of the laminate is indicated as the Z direction. The X and Y directions are perpendicular to the Z direction. The XY plane is a plane perpendicular to the Z direction.

[0024] Referring to Figures 1, 2, and 3, the laminate 10a according to Embodiment 1 is block-shaped and composed of multiple material layers. In this embodiment, the number of material layers included in the laminate 10a is 10. The laminate 10a includes material layer 11a, material layer 11b, material layer 11c, material layer 11d, material layer 11e, material layer 11f, material layer 11g, material layer 11h, material layer 11i, and material layer 11j. Material layers 11a to 11j are each arranged in the thickness direction. In the Z direction, material layers 11a to 11j are arranged in the order of material layer 11a, material layer 11b, material layer 11c, material layer 11d, material layer 11e, material layer 11f, material layer 11g, material layer 11h, material layer 11i, and material layer 11j. In this embodiment, the first surface 12a located on one side of the thickness direction of material layer 11a and the second surface 13j located on the other side of the thickness direction of material layer 11j are exposed to the outside. That is, material layers 11b to 11i are arranged in order between material layer 11a and material layer 11j. Also, material layer 11a and material layer 11j are arranged at both ends of the laminate 10a in the thickness direction. In terms of the arrangement relationship between the first material layer, the second material layer and the third material layer, in the Z direction which is the thickness direction of the multiple material layers 11a to 11j, for example, the first material layer 11a, the third material layer 11b, and the second material layer 11j are arranged in that order. Such a laminate 10a can be configured, for example, by attaching a first electrode to material layer 11a and a second electrode to material layer 11j, and applying thermal energy (temperature difference) between material layer 11a and material layer 11j to obtain electrical energy between the first electrode and the second electrode. Of the multiple material layers, the material layer with the highest content of the first base material element is the first material layer 11a, and the material layer with the lowest content of the first base material element is the second material layer 11j.

[0025] When viewed from the Z direction, the external shapes of material layers 11a to 11j are the same. In this embodiment, when viewed from the Z direction, the external shapes of material layers 11a to 11j are all rectangular. However, the external shape of the laminate 10a when viewed from the Z direction is not limited to a rectangular shape; for example, it may be round, elliptical, or a polygon such as a triangle or hexagon.

[0026] In this embodiment, the thicknesses of material layers 11a to 11j are the same. The thickness T1 of material layer 11a, that is, the distance between the first surface 12a located on one side in the thickness direction of material layer 11a and the second surface 13a located on the other side in the thickness direction, is 10 μm or more and 5 mm or less. In this embodiment, the thickness T1 of material layer 11a is 100 μm.

[0027] The laminate 10a includes a plurality of diffusion suppression layers 21a, 21b, 21c, 21d, 21e, 21f, 21g, 21h, and 21a. In this embodiment, the laminate 10a includes nine diffusion suppression layers 21a to 21i. Each diffusion suppression layer 21a to 21i is positioned between material layers 11a to 11j in the Z direction. Specifically, diffusion suppression layer 21a is positioned between material layer 11a and material layer 11b. Diffusion suppression layer 21b is positioned between material layer 11b and material layer 11c. Diffusion suppression layer 21c is positioned between material layer 11c and material layer 11d. Diffusion suppression layer 21d is positioned between material layer 11d and material layer 11e. Diffusion suppression layer 21e is positioned between material layer 11e and material layer 11f. Diffusion suppression layer 21f is positioned between material layer 11f and material layer 11g. A diffusion suppression layer 21g is placed between material layer 11g and material layer 11h. A diffusion suppression layer 21h is placed between material layer 11h and material layer 11i. A diffusion suppression layer 21i is placed between material layer 11i and material layer 11j. In other words, diffusion suppression layers 21a to 21i are sandwiched between material layers 11a to 11j, respectively. Furthermore, a diffusion suppression layer is placed between material layer 11a and material layer 11b, and a diffusion suppression layer is also placed between material layer 11b and material layer 11c. Each of the diffusion suppression layers 21a to 21i suppresses the diffusion of atoms contained in each material layer 11a to 11j to the other material layers 11a to 11j. Specifically, diffusion suppression layer 21a suppresses the diffusion of atoms contained in material layer 11a to material layer 11b and the diffusion of atoms contained in material layer 11b to material layer 11a. The diffusion suppression layer 21b suppresses the diffusion of atoms contained in material layer 11b to material layer 11c and the diffusion of atoms contained in material layer 11c to material layer 11b. The diffusion suppression layer 21c suppresses the diffusion of atoms contained in material layer 11c to material layer 11d and the diffusion of atoms contained in material layer 11d to material layer 11c. The diffusion suppression layer 21d suppresses the diffusion of atoms contained in material layer 11d to material layer 11e and the diffusion of atoms contained in material layer 11e to material layer 11d. The diffusion suppression layer 21e suppresses the diffusion of atoms contained in material layer 11e to material layer 11f and the diffusion of atoms contained in material layer 11f to material layer 11e.The diffusion-suppressing layer 21f suppresses the diffusion of atoms contained in material layer 11f to material layer 11g and the diffusion of atoms contained in material layer 11g to material layer 11f. The diffusion-suppressing layer 21g suppresses the diffusion of atoms contained in material layer 11g to material layer 11h and the diffusion of atoms contained in material layer 11h to material layer 11g. The diffusion-suppressing layer 21h suppresses the diffusion of atoms contained in material layer 11h to material layer 11i and the diffusion of atoms contained in material layer 11i to material layer 11h. The diffusion-suppressing layer 21i suppresses the diffusion of atoms contained in material layer 11i to material layer 11j and the diffusion of atoms contained in material layer 11j to material layer 11i.

[0028] In this embodiment, the thicknesses of each diffusion suppression layer 21a to 21i are the same. The thickness T2 of the diffusion suppression layer 21a, that is, the distance between the first surface 22a located on one side in the thickness direction of the diffusion suppression layer 21a and the second surface 23a located on the other side in the thickness direction, is 10 nm or more. Furthermore, the thickness T2 of the diffusion suppression layer 21a is thinner than the thickest material layer among the material layers 11a to 11j. In this embodiment, the thickness T2 of the diffusion suppression layer 21a is 10 μm.

[0029] Each of the diffusion-suppressing layers 21a to 21i is formed from the same material. In this embodiment, each of the diffusion-suppressing layers 21a to 21i is composed of SiO2 (silicon dioxide). Because the diffusion-suppressing layers 21a to 21i, which are composed of such materials, have high insulating properties, they can more reliably suppress the diffusion of atoms contained in each material layer 11a to 11j to the other material layers 11a to 11j.

[0030] Each material layer 11a to 11j is composed of a solid phase change material containing a first and a second matrix element. That is, the laminate 10a according to this disclosure has a multilayer structure. In this embodiment, the first matrix element is S (sulfur). The second matrix element is Se (selenium). The third matrix element is Ag (silver). Each solid phase change material constituting the material layers 11a to 11j in the laminate 10a of Embodiment 1 contains a silver chalcogenide material. Such materials are easily applied to devices that require thermal control. In this embodiment, the solid phase change material is Ag2S x Se 1-x It is expressed as follows: x has the relationship 0 ≤ x ≤ 1.

[0031] Here, in the laminate 10a of Embodiment 1, the difference in content between the content of the first base material element, S (sulfur), in the first material layer 11a and the content of the first base material element, S, in the second material layer 11j is 10 at% or more. Specifically, the content ratios of the first base material element and the second base material element in each material layer 11a to 11j are as shown in Sample 1 described later.

[0032] With a laminate 10a having this configuration, the thermal conductivity can be smoothly changed in accordance with the ambient temperature, even when the ambient temperature changes, allowing for efficient temperature control of the device. Therefore, such a laminate 10a is easily applicable to devices that require thermal control.

[0033] In this embodiment, diffusion suppression layers 21a to 21i are included, which are positioned between the first material layer 11a and the second material layer 11j to suppress the diffusion of atoms between each material layer 11a to 11j. Therefore, during phase transformation, the diffusion of atoms contained in each material layer 11a to 11j to other material layers is suppressed, reducing the risk of changes in the composition of each material layer 11a to 11j. In other words, by positioning the diffusion suppression layers 21a to 21i in this manner, reactions between the material layers 11a to 11j and reactions with other materials can be suppressed, preventing deterioration due to phase transformation during repeated use.

[0034] In the present embodiment, the first base material element and the second base material element are sulfur and selenium, respectively. The solid phase change material is Ag2S x Se 1-x wherein x satisfies the relation 0≦x≦1. The laminate 10a including the plurality of material layers 11a to 11j composed of such a solid phase change material can smoothly change the thermal conductivity even under circumstances where the environmental temperature changes, and can efficiently perform temperature control of the device.

[0035] In the present embodiment, the thickness of each of the plurality of material layers 11a to 11j is 10 μm or more and 5 mm or less. By setting the thickness of the material layers 11a to 11j to 10 μm or more, the material layers 11a to 11j can secure a thickness equal to or larger than the region where phase transformation hardly occurs from the diffusion suppressing layers 21a to 21i in contact therewith. In addition, by setting the thickness of the material layers 11a to 11j to 5 mm or less, precipitation of elements in a single material layer due to ion conduction when a temperature difference is applied can be suppressed, and reliability can be improved.

[0036] In the present embodiment, the thickness of each of the diffusion suppressing layers 21a to 21i is 10 nm or more, and is thinner than the thickest material layer among the plurality of material layers 11a to 11j. By setting the thickness of the diffusion suppressing layers 21a to 21i to 10 nm or more, diffusion of atoms contained in each of the material layers 11a to 11j into the other material layers 11a to 11j can be reliably suppressed. In addition, by making the thickness of the diffusion suppressing layers 21a to 21i thinner than the thickest material layer 11a to 11j, the influence of the diffusion suppressing layers 21a to 21i on the thermal conductivity of the laminate 10a can be reduced.

[0037] In this embodiment, the multiple material layers 11a to 11j include a third material layer 11c composed of a solid phase change material containing a first base material element and a second base material element. The multiple material layers are arranged in the order of first material layer 11a, third material layer 11b, and second material layer 11j in the thickness direction. Therefore, by gradually changing the content ratio of the first base material element in the laminate 10a, the change in thermal conductivity between each material layer 11a, 11b, and 11j can be made smoother. Consequently, the temperature control of the device can be performed more efficiently.

[0038] In the above embodiment, the content of the first base material element (S) gradually decreases from the bottom layer, material layer 11a, in the thickness direction of the laminate 10a, while the content of the second base material element (Se) gradually increases. However, the opposite may be true; the content of the first base material element (S) may decrease from the top layer, material layer 11j, while the content of the second base material element (Se) may increase. Furthermore, instead of the content of the first and second base material elements gradually changing for each adjacent material layer, material layers with different content ratios may be randomly arranged, as in Sample 6 described later. In other words, the material layer with the highest or lowest content of the first base material element does not have to be located at one end in the thickness direction. The same applies to Embodiments 2 and 3 described later.

[0039] (Embodiment 2) Another embodiment, Embodiment 2, will now be described. Figure 4 is a schematic side view showing the structure of the laminate according to Embodiment 2. The laminate in Embodiment 2 has basically the same configuration as in Embodiment 1 and produces the same effects. However, the laminate in Embodiment 2 differs from that in Embodiment 1 in the number of layers.

[0040] Referring to Figure 4, the laminate 10b includes a first material layer 11a and a second material layer 11b, which are composed of a solid phase-change material containing a first and a second matrix element. That is, the laminate 10b has a two-layer structure. A diffusion-suppressing layer 21a is placed between the first material layer 11a and the second material layer 11b. The content ratio of the first matrix element in the first material layer 11a is greater than the content ratio of the first matrix element in the second material layer 11b. The difference in content ratio obtained by subtracting the content ratio of the first matrix element in the second material layer 11b from the content ratio of the first matrix element in the first material layer 11a is 10 at% or more.

[0041] Thus, the laminate 10b may be composed of two material layers having the above-described relationship and one diffusion-suppressing layer. This also allows for efficient temperature control of the device.

[0042] (Embodiment 3) Another embodiment, Embodiment 3, will now be described. Figure 5 is a schematic side view showing the structure of the laminate according to Embodiment 3. The laminate in Embodiment 3 has basically the same configuration as in Embodiment 1 and produces the same effects. However, the laminate in Embodiment 3 differs from that in Embodiment 1 in the number of layers and composition.

[0043] Referring to Figure 5, the laminate 10c in Embodiment 3 has 11 material layers, unlike in Embodiment 1. That is, the laminate 10c in Embodiment 3 is composed of material layers 11a to 11k. In this embodiment, the second surface 13k of material layer 11k is exposed. A diffusion suppression layer 21j is placed between material layer 11j and material layer 11k. Also, unlike in Embodiment 1, the first base material element is S, the second base material element is Te, and the third base material element is Ag. Each solid phase change material constituting material layers 11a to 11k in the laminate 10c of Embodiment 3 is Ag2S x Te 1-xIt is expressed as follows: x has the relationship 0 ≤ x ≤ 1. Also, the material of each diffusion suppression layer 21a to 21j is SiN (silicon nitride).

[0044] Even with a laminated structure 10c having this configuration, the thermal conductivity can be smoothly changed in accordance with the ambient temperature, even when the ambient temperature changes, allowing for efficient temperature control of the device.

[0045] (Other embodiments) In the above embodiment, the diffusion suppression layer was made of SiO2 or SiN, but it is not limited to these materials. The diffusion suppression layer may be composed of at least one of SiO2, SiN, SiON (silicon oxynitride), epoxy resin, and silicone resin. A diffusion suppression layer made of such materials can more reliably suppress the diffusion of atoms contained in each material layer to other material layers.

[0046] In the above embodiments, examples of 2, 10, or 11 material layers were shown, but the invention is not limited to these. There should be at least 2 material layers, and among these multiple material layers, the material layer with the highest content of the first base material element is designated as the first material layer, and the material layer with the lowest content of the first base material element is designated as the second material layer. The difference in content between the first base material element in the first material layer and the first base material element in the second material layer should be 10 at% or more. The first and second base material elements are selected from the group consisting of S, Se, and Te, respectively.

[0047] Figure 6 is a phase diagram of the solid phase change material in the silver chalcogenide-based material described above. In Figure 6, the horizontal axis shows the content ratio of the atoms represented by x, and the vertical axis shows the temperature (°C). In Figure 6, the hatched regions both represent regions that can become either the α phase or the β phase, as described later. When the temperature is increased, it becomes the α phase, and when the temperature is decreased, it becomes the β phase. That is, it is the region of hysteresis in phase transformation. Referring to Figure 6, the Te-Se-based solid phase change material (Ag2Te) shown in region R1 xSe 1-x ), Se-S system solid phase change material (Ag2Se) shown in region R2 x S 1-x ) and the S-Te-based solid phase change material (Ag2S) shown in region R3 x Te 1-x In this case, when two different elements are selected from S, Se, and Te for the first and second base material elements, and their respective content ratios are changed, a phase transformation occurs between the high-temperature α phase and the low-temperature β phase depending on the temperature. The carrier concentration changes due to the phase transformation, and as a result, the thermal conductivity changes. Point defects (vacancies and excess elements) differ for each composition, and the thermal conductivity κ differs accordingly.

[0048] Figure 7 is a schematic graph showing the relationship between temperature and thermal conductivity when the composition ratios are in regions R1 and R3. Figure 8 is a schematic graph showing the relationship between temperature and thermal conductivity when the composition ratios are in region R2. In Figures 7 and 8, the horizontal axis represents temperature and the vertical axis represents thermal conductivity. Referring to Figure 7, in regions R1 and R3, the thermal conductivity is high at low temperatures and low at high temperatures. Referring to Figure 8, in region R2, the thermal conductivity is low at low temperatures and high at high temperatures. Depending on the composition, that is, the content ratio of the first base material element, the proportions of the high-temperature phase (α phase) and the low-temperature phase (β phase) change, and the thermal conductivity changes accordingly. In the laminate according to this disclosure, the thermal conductivity is changed by changing the composition of this base material element, thereby avoiding abrupt changes in thermal conductivity.

[0049] Furthermore, in the above embodiment, the solid phase change material is Ag2S x Se 1-x It is expressed by such that x has the relationship 0 ≤ x ≤ 1, or Ag 2 S x Te 1-x This is expressed by the equation, where x has the relationship 0 ≤ x ≤ 1, but it is not limited to this; solid phase change materials include Ag2Se x S 1-x Ag2Te x S 1-x or Ag2Sex Te 1-x It may also be expressed by . x may have the relationship 0 ≤ x ≤ 1. Note that Ag2Se x Te 1-x As can be seen from Figure 6, a similar effect is observed. A laminate containing multiple material layers composed of such solid phase-change materials can smoothly change its thermal conductivity in response to ambient temperature changes, enabling efficient temperature control of the device. [Examples]

[0050] Samples 1 to 6 were prepared as shown in Table 1. The first matrix element is sulfur, the second matrix element is selenium, and one material layer is Ag2S x Se 1-x It is represented as shown. In Table 1, the arrangement of material layers corresponds to the upper layer at the top and the lower layer at the bottom.

[0051] (Sample 1) As Sample 1, ten material layers were prepared as shown in Table 1. The content ratio (x) of the first matrix element in the material layers, from bottom to top, is x=0.950, x=0.930, x=0.910, x=0.890, x=0.870, x=0.850, x=0.830, x=0.810, x=0.790, and x=0.770. Of the ten material layers, the layer with the highest content of the first matrix element (S) is the first material layer 11a (material layer L shown in Table 1). 10 The second material layer 11j (material layer L1 shown in Table 1) is the layer with the smallest amount of the first base material element (S). The third material layer 11b is, for example, material layer L9 shown in Table 1. The difference in content between the content of the first base material element S in the first material layer 11a and the content of the first base material element S in the second material layer 11j is 18 at%. This difference in content is shown in the lower column of Table 1.

[0052] The laminate 10a is manufactured as follows. First, Ag2S and Ag2Se powders are prepared as raw materials for the material layer, and SiO2 powder is prepared as a raw material for the diffusion-suppressing layer. Then, each raw material powder is weighed and mixed to achieve the content ratio of each layer, i.e., the elemental ratio specified for each layer. In this way, the powders constituting each layer are prepared. After that, the powders constituting each layer are sealed in a vacuum cylinder and heated at 150K to alloy them. After that, the alloy is removed from the vacuum cylinder and ground into a fine powder by hand milling.

[0053] Next, the powder obtained in this way is sintered. Specifically, a die with a diameter of φ50 mm is prepared, the powder constituting the first material layer is placed inside, and then the SiO2 powder constituting the first diffusion suppression layer is placed on top of it. After that, the powder constituting the next material layer is placed inside, and then the SiO2 powder constituting the diffusion suppression layer is placed on top of it again. In this way, the powder constituting each material layer and the SiO2 powder constituting the diffusion suppression layer are alternately placed inside the die. In this embodiment, the material layers were placed inside the die so that the thickness of the material layer was 1 mm or less and the thickness of the diffusion suppression layer was 0.1 mm or less.

[0054] Subsequently, sintering was performed. For sintering, the temperature was set in the range of 600K to 1500K, and hot pressing was performed under a uniaxial pressure of 10MPa to 100MPa. The holding time was 2 hours, and the process was carried out in an Ar (argon) gas atmosphere. After the sintering process and natural cooling, the sample was removed from the die, and the laminate for sample 1 was obtained. The obtained laminate has the configuration shown in Figure 1. The same configuration was used for samples 2, 3, and 6.

[0055] (Sample 2) For Sample 2, the compositions of 10 material layers were prepared according to Table 1 shown below. Then, a laminate for Sample 2 was obtained using the same manufacturing method as for Sample 1. Of the 10 material layers, the layer with the largest amount of the first matrix element (S) was the first material layer 11a (material layer L shown in Table 1). 10) and the layer with the smallest amount of the first matrix element (S) is the second material layer 11j (material layer L1 shown in Table 1). The third material layer 11b is, for example, material layer L9 shown in Table 1.

[0056] (Sample 3) For Sample 3, the compositions of 10 material layers were prepared according to Table 1 shown below. Then, a laminate for Sample 3 was obtained using the same manufacturing method as for Sample 1. Of the 10 material layers, the layer with the largest amount of the first matrix element (S) was the first material layer 11a (material layer L shown in Table 1). 10 ) and the layer with the smallest amount of the first matrix element (S) is the second material layer 11j (material layer L1 shown in Table 1). The third material layer 11b is, for example, material layer L9 shown in Table 1.

[0057] (Sample 4) For Sample 4, the compositions of two material layers were prepared according to Table 1 shown below. Then, a laminate for Sample 4 was obtained using the same manufacturing method as for Sample 1. The obtained laminate has the configuration shown in Figure 4. The same configuration applies to Sample 10. The first material layer 11a is material layer L1 shown in Table 1, and the second material layer 11b is material layer L2 shown in Table 1.

[0058] (Sample 5) As Sample 5, a material consisting of only one layer of material was prepared according to Table 1 shown below. Then, the material for Sample 5 was obtained using the same manufacturing method as for Sample 1.

[0059] (Sample 6) For Sample 6, the compositions of 10 material layers were prepared according to Table 1 shown below. Then, a laminate 10c for Sample 6 was obtained using the same manufacturing method as for Sample 1. Of the 10 material layers, the layer with the largest amount of the first matrix element (S) was the first material layer 11a (material layer L shown in Table 1). 10 ) and the layer with the smallest amount of the first matrix element (S) is the second material layer 11f (material layer L5 shown in Table 1). The third material layer 11b is, for example, material layer L9 shown in Table 1.

[0060] Samples 7 to 12 were prepared as shown in Table 2. The first matrix element is sulfur, the second matrix element is tellurium, and one material layer is Ag2S x Te 1-x As shown above, the arrangement of material layers in Table 2 corresponds to the upper layer at the top and the lower layer at the bottom.

[0061] (Sample 7) For Sample 7, the compositions of 11 material layers were prepared according to Table 2 shown below. Then, a laminate for Sample 7 was obtained using the same manufacturing method as for Sample 1. The obtained laminate has the configuration shown in Figure 5. The same configuration is used for Samples 8, 9, and 12. Of the 11 material layers, the layer with the largest amount of the first matrix element (S) is the first material layer 11a (material layer L shown in Table 1). 11 ) and the layer with the smallest amount of the first matrix element (S) is the second material layer 11k (material layer L1 shown in Table 1). The third material layer 11b is, for example, material layer L shown in Table 2. 10 That is the case.

[0062] (Sample 8) For Sample 8, the compositions of 11 material layers were prepared according to Table 2 shown below. Then, a laminate for Sample 8 was obtained using the same manufacturing method as for Sample 1. Of the 11 material layers, the layer with the largest amount of the first matrix element (S) was the first material layer 11a (material layer L shown in Table 1). 11 ) and the layer with the smallest amount of the first matrix element (S) is the second material layer 11k (material layer L1 shown in Table 1). The third material layer 11b is, for example, material layer L shown in Table 2. 10 That is the case.

[0063] (Sample 9) For Sample 9, the compositions of 11 material layers were prepared according to Table 2 shown below. Then, a laminate for Sample 9 was obtained using the same manufacturing method as for Sample 1. Of the 11 material layers, the layer with the largest amount of the first matrix element (S) was the first material layer 11a (material layer L shown in Table 1). 11) and the layer with the smallest amount of the first matrix element (S) is the second material layer 11k (material layer L1 shown in Table 1). The third material layer 11b is, for example, material layer L shown in Table 2. 10 That is the case.

[0064] (Sample 10) As Sample 10, the compositions of two material layers were prepared according to Table 2 shown below. Then, a laminate relating to Sample 10 was obtained using the same manufacturing method as for Sample 1. The first material layer 11a is material layer L2 shown in Table 2, and the second material layer 11b is material layer L1 shown in Table 2.

[0065] (Sample 11) As Sample 11, a material consisting of only one layer was prepared according to Table 2 shown below. Then, a laminate relating to Sample 11 was obtained using the same manufacturing method as for Sample 1.

[0066] (Sample 12) For Sample 12, the compositions of 11 material layers were prepared according to Table 2 shown below. Then, a laminate for Sample 12 was obtained using the same manufacturing method as for Sample 1. The first material layer 11a is the material layer L shown in Table 2. 11 The second material layer 11b is material layer L6 shown in Table 2. The third material layer 11b is, for example, material layer L6 shown in Table 2. 10 That is the case.

[0067] [Table 1]

[0068] [Table 2]

[0069] The schematic diagram shows the results of EDX (Energy Dispersive X-ray spectrometry) measurement, specifically the proportion of each element within the material layer. EDX was measured by capturing TEM (Transmission Electron Microscope) images of a portion of the laminate. For TEM imaging, a JEM-2800 (manufactured by JEOL Ltd.) was used, with measurement conditions of an acceleration voltage of 200kV, a probe size of 0.5nm, and a CL aperture of 3. For atomic detection using EDX, an EDX (manufactured by Thermo Fisher Scientific K.K.) was used, with measurement conditions of a spot size of 0.5nm, a CL aperture of 3, mapping analysis mode, and an analysis time of 20 minutes. Quantitative analysis was then performed on the EDX measurement spectrum using the instrument's fitting function.

[0070] For the measurement of thermal conductivity, a GH-1 thermal conductivity measuring device manufactured by Advance Engineering Co., Ltd. was used as a steady-state thermal conductivity measuring device. A high-temperature heater, sample, heat flux meter, and low-temperature heater were prepared, and the sample was set up. For the Ag-S-Se system, the measurement was performed in the range of 100°C to 150°C, and for the Ag-S-Te system, in the range of 60°C to 110°C. Three measurements were performed, and the average value was calculated. The thickness of each material layer and the diffusion suppression layer was determined using an optical microscope or SEM (Scanning Electron Microscope).

[0071] The evaluation results for Samples 1 to 6 are shown in Figure 9. Figure 9 is a graph showing the relationship between temperature and thermal conductivity for Samples 1 to 6. In Figure 9, the horizontal axis represents temperature (°C), and the vertical axis represents thermal conductivity (W / mK). Referring to Figure 9, for Sample 1, where the difference in content is 18 at%, for Sample 2, where the difference in content is 10.8 at%, for Sample 4, where the difference in content is 12 at%, and for Sample 6, where the difference in content is 10 at% or more, the change in thermal conductivity is smooth. Here, a smooth change in thermal conductivity means that when the thermal conductivity changes from the minimum value to the maximum value, the temperature changes by 10°C or more while the change in the difference between the maximum and minimum values ​​changes from 10% to 90%. On the other hand, for Sample 3, where the difference in content is 4 at%, and for Sample 5, a bulk material with a difference in content of 0%, the change in thermal conductivity is steep. This is likely because, in Sample 3 and Sample 5, the difference in the content ratios between each material layer is small, or there is no difference in the content ratios, resulting in similar phase transformation temperatures. Furthermore, as shown in Samples 1 to 3, the order of the material layers may be in the order of the content ratio of the first base material element, and as shown in Sample 6, the order of the material layers may be in any order of the content ratio of the first base material element.

[0072] The evaluation results for samples 7 to 12 are shown in Figure 10. Figure 10 is a graph showing the relationship between temperature and thermal conductivity for samples 7 to 12. In Figure 10, the horizontal axis represents temperature (°C), and the vertical axis represents thermal conductivity (W / mK). Referring to Figure 10, for sample 7, sample 8, sample 10, sample 12, and sample 12, where the difference in content is 20 at%, 10 at%, 10 at%, 10 at%, the difference in content is 10 at%, and the change in thermal conductivity is smooth. On the other hand, for sample 9, where the difference in content is 2 at%, and for sample 11, a bulk material with a difference in content of 0%, the change in thermal conductivity is steep. This is thought to be because, in samples 9 and 11, the difference in content between each material layer is small, or there is no difference in content, so the phase transformation temperatures are close. Furthermore, as shown in Samples 7 to 9, the order of the material layers may be in the order of the content ratio of the first base material element, and as shown in Sample 12, the order of the material layers may be in any order of the content ratio of the first base material element.

[0073] Based on the above, the laminate according to this disclosure enables more efficient temperature control of the device.

[0074] The embodiments disclosed herein should be understood to be illustrative in all respects and not restrictive in any way. The scope of the invention is defined by the claims and not by the foregoing description, and all modifications within the meaning and scope of the claims are intended to be included. [Explanation of Symbols]

[0075] 10a,10b,10c laminate, 11a material layer, 11b material layer, 11c material layer, 11d material layer, 11e material layer, 11f material layer, 11g material layer, 11h material layer, 11i material layer, 11j material layer, 11k material layer, 12a,22a first surface, 13a,13j,13k,23a second surface, 21a diffusion suppression layer, 21b diffusion suppression layer, 21c diffusion suppression layer, 21d diffusion suppression layer, 21e diffusion suppression layer, 21f diffusion suppression layer, 21g diffusion suppression layer, 21h diffusion suppression layer, 21i diffusion suppression layer, 21j diffusion suppression layer, T1,T2 thickness, R1,R2,R3 region

Claims

1. The material comprises a plurality of material layers composed of a solid phase change material containing a first matrix element and a second matrix element different from the first matrix element, The aforementioned multiple material layers are The first material layer having the highest content of the first base material element, The material comprises a second material layer having the smallest content of the first base material element, The difference in content ratio obtained by subtracting the content ratio of the first base material element in the second material layer from the content ratio of the first base material element in the first material layer is 10 at% or more. The aforementioned solid phase change material includes a silver chalcogenide-based material. The first and second base material elements are each elements selected from the group consisting of sulfur, selenium, and tellurium. The aforementioned solid phase change material is represented by Ag₂SxSe₁-x, Ag₂SxTe₁-x, or Ag₂Se₂Te₁-x. x is a laminate that satisfies the relationship 0 ≤ x ≤ 1.

2. The laminate according to claim 1, further comprising a diffusion suppression layer disposed between the first material layer and the second material layer, which suppresses the diffusion of atoms contained in each material layer to the other material layer.

3. The laminate according to claim 1 or claim 2, wherein the thickness of each of the plurality of material layers is 10 μm or more and 5 mm or less.

4. The aforementioned diffusion suppression layer is SiO 2 The laminate according to claim 2, comprising at least one of SiN, SiON, epoxy resin, and silicone resin.

5. The laminate according to claim 2, wherein the thickness of the diffusion suppression layer is 10 nm or more, and is thinner than the thickest material layer among the plurality of material layers.

6. The plurality of material layers further include a third material layer composed of a solid phase change material containing the first and second base material elements, The laminate according to claim 1, wherein the plurality of material layers are arranged in the order of the first material layer, the third material layer, and the second material layer in the thickness direction.

7. The laminate according to claim 6, further comprising diffusion suppression layers disposed between the first material layer and the third material layer and between the third material layer and the second material layer, respectively, which suppress the diffusion of atoms contained in each material layer to the other material layers.

8. The plurality of material layers further include a third material layer composed of a solid phase change material containing the first and second base material elements, The laminate according to claim 1, wherein the plurality of material layers are arranged in the order of the first material layer, the second material layer, and the third material layer in the thickness direction.

9. The laminate according to claim 8, further comprising a diffusion suppression layer disposed between the second material layer and the third material layer, which suppresses the diffusion of atoms contained in each material layer to the other material layer.

Citation Information

Patent Citations

  • Laminate and thermoelectric conversion element

    JP2018167557A

  • Method for preparing metal chalcogenide nanomaterials

    JP2018521943A

  • Phase change substance and thermal control device

    WO2007037332A1