Ink and colored solar modules
The integration of infrared reflective powder and color-developing toner in a colored solar module structure addresses the issues of efficiency and temperature, ensuring aesthetic variety and prolonged module lifespan.
Patent Information
- Application Number
- JP2024565359
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-01-29
- Filing Date
- 2023-04-07
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-04-07
AI Technical Summary
Solar modules installed on buildings face challenges in achieving diverse aesthetic colors without reducing efficiency and are prone to high operating temperatures due to inadequate heat dissipation, leading to decreased power output and shortened lifespan.
Incorporation of an ink comprising infrared reflective powder and color-developing toner, which includes a stacked dielectric and metal film configuration, applied in a colored solar module structure to enhance infrared reflectivity and improve heat dissipation.
The solution maintains high efficiency while providing color diversity and reduces operating temperatures, thereby extending the lifespan of solar modules.
Smart Images

Figure 0007954732000002 
Figure 0007954732000003 
Figure 0007954732000004
Abstract
Description
TECHNICAL FIELD
[0001] (CROSS-REFERENCE TO RELATED APPLICATIONS) This application claims priority to Chinese patent applications filed with the China National Intellectual Property Administration on May 16, 2022, with application number 202210529641.0 and titled "Ink and Colored Solar Module", the entire content of which is incorporated into this application by reference. This application also claims priority to Chinese patent applications filed with the China National Intellectual Property Administration on January 29, 2023, with application number 202310078270.3 and titled "Ink and Colored Solar Module", the entire content of which is incorporated into this application by reference.
[0002] The present application pertains to the technical field of solar cells, and specifically relates to an ink and a colored solar module. BACKGROUND ART
[0003] Solar modules, as a means of capturing and converting light energy, have undergone long-term technological innovation and generational changes, and are now highly efficient and widely applied in large-scale ground-based power plants. As the number of photovoltaic devices installed increases, the use of ground surface area is becoming saturated, and the large area of buildings has become an optimal choice for installing photovoltaic devices as a surface for receiving sunlight. By installing photovoltaic devices on buildings, energy revenue is increased while the energy consumption of the building is reduced, and the building can use electricity generated by itself, reducing losses due to long-distance transmission of electricity. However, photovoltaic cells are generally monotonous in color, either dark blue or black, and cannot meet the diverse demands for aesthetics in buildings. Photovoltaic cell technologies include thin-film cell technologies such as cadmium telluride and copper indium gallium selenide, but many of these technologies have low efficiency. Crystalline silicon, as a mature photovoltaic power generation technology, has already reached a mass production efficiency of over 24%, making it a suitable technology for building-integrated solar power generation. One method to meet the demand for diversified solar module colors is to use colored adhesive films in which inorganic or organic dyes are added to the adhesive film. However, this method significantly reduces the efficiency of the solar module due to light absorption by the dye, and there is a risk of fading, making it not a suitable choice for coloring solar modules. Furthermore, a method of applying a colored plating layer to the surface of the battery cell can also be considered, but with this method, it is difficult to control the thickness of the plating layer, making it difficult to achieve uniform color and significantly impairing the appearance. Therefore, a more suitable means of imparting color is needed.
[0004] On the other hand, when a solar module is in operation, it receives sunlight, and some of the light energy at certain wavelengths (380-1100 nm) is absorbed by the silicon solar cell and converted into electrical and thermal energy. However, some of the other light energy, especially infrared light energy with wavelengths above 1100 nm, cannot be converted into electrical energy by the cell and is instead absorbed and converted into thermal energy. This energy above 1100 nm accounts for about 30% of the total energy in the spectrum, and when absorbed by the solar module, it generates a large amount of thermal energy, causing the solar module's temperature to rise. When the operating temperature of a solar module rises, not only does its power output decrease, but the activity of the polymer material increases at high temperatures, making degradation and attenuation more likely. When a solar module is operating in a large-scale power plant, both its front and back surfaces are exposed to sunlight, resulting in a high heat transfer coefficient and allowing the generated thermal energy to be quickly dissipated. In such an environment, its operating temperature is not excessively high and generally does not exceed 70°C. However, when solar modules are applied to buildings, the back side is typically a solid wall, insulation, etc., which hinders airflow. The lack of a heat dissipation channel on the back side significantly increases the operating temperature of the solar module, sometimes exceeding 90°C. Such high temperatures drastically shorten the module's lifespan. Therefore, it is necessary to optimize the conventional design or materials to reduce the module's operating temperature. [Overview of the Initiative]
[0005] This application provides an ink and a colored solar module to address the problems that existed in the prior art.
[0006] Specifically, this application relates to the following aspects:
[0007] An ink comprising infrared reflective powder and a color-developing toner, wherein the mass ratio of the infrared reflective powder is 0.1% to 30%, preferably 5% to 15%, and the mass ratio of the color-developing toner is 0.1% to 20%, preferably 1% to 5%.
[0008] Selectively, the infrared reflective powder has high transmittance to light with wavelengths of 300 nm to 1100 nm and high reflectance to infrared light with wavelengths of 1100 nm to 5000 nm.
[0009] Selectively, the infrared reflective powder is a transparent or translucent sheet with a thickness of 0.5 μm to 5 μm, and the color-developing toner is a transparent or translucent sheet with a thickness of 0.5 μm to 5 μm.
[0010] Selectively, the infrared reflective powder includes a first dielectric film layer, a metal film layer, and a second dielectric film layer arranged in a sequential stacked configuration, wherein the thickness of the first dielectric film layer is 10 nm to 100 nm, the thickness of the metal film layer is 3 nm to 30 nm, and the thickness of the second dielectric film layer is 10 nm to 100 nm.
[0011] Selectively, the infrared reflecting powder is one or more selected from ZnS / Ag / ZnS, SiO2 / Ag / TiO2, Al2O3 / Ag / Al2O3, and ZnO / Ag / ZnS, preferably ZnS / Ag / ZnS.
[0012] Selectively, the ink is a high-temperature ink composed of infrared reflective powder, color-developing toner, glass powder, and organic solvent.
[0013] Selectively, in the high-temperature ink, the mass ratio of infrared reflective powder is 0.1% to 30%, preferably 5% to 15%, the mass ratio of the color-developing toner is 0.1% to 20%, preferably 1% to 5%, the mass ratio of glass powder is 30% to 70%, and the mass ratio of organic solvent is 10% to 40%.
[0014] Selectively, the ink is a low-temperature ink composed of infrared reflective powder, a color-developing toner, and an organic solvent.
[0015] Selectively, in the low-temperature ink, the mass ratio of infrared reflective powder is 0.1% to 30%, preferably 5% to 15%, the mass ratio of the color-developing toner is 0.1% to 20%, preferably 1% to 5%, and the mass ratio of organic solvent is 70% to 99.9%.
[0016] A colored solar module comprising sequentially stacked colored glass layers, a battery chip layer, a first lower flexible adhesive film layer, a reinforcing adhesive film layer, a second lower flexible adhesive film layer, and a back glass layer.
[0017] Selectively, the colored glass layer includes a surface glass layer, a color glaze layer, and an upper adhesive film layer arranged in a sequential stacked configuration, wherein the upper adhesive film layer is closer to the battery chip layer than the surface glass layer and the color glaze layer.
[0018] Selectively, the color glaze layer comprises infrared reflective powder and color-developing toner, wherein the mass ratio of the infrared reflective powder in the color glaze layer is 0.1% to 30%, preferably 5% to 15%, and the mass ratio of the color-developing toner is 0.1% to 20%, preferably 1% to 5%.
[0019] The thickness of the color glaze layer is selectable to be 5 μm to 100 μm, preferably 10 μm to 30 μm.
[0020] The color glaze layer is optionally formed with the ink described in any one of the above.
[0021] Selectively, the colored glass layer includes a surface glass layer and an upper adhesive film layer arranged in a sequential stacking configuration, wherein the upper adhesive film layer is closer to the battery chip layer than the surface glass layer. The upper adhesive film layer contains infrared reflective powder and color-developing toner, wherein the mass ratio of the infrared reflective powder in the upper adhesive film layer is 0.1% to 30%, preferably 5% to 15%, and the mass ratio of the color-developing toner is 0.1% to 20%, preferably 1% to 5%.
[0022] Optionally, the infrared reflective powder has high transmittance for light with a wavelength of 300 nm to 1100 nm, and has high reflectivity for infrared light with a wavelength of 1100 nm to 5000 nm.
[0023] Optionally, the infrared reflective powder is a transparent or translucent sheet with a thickness of 0.5 μm to 5 μm, and the color developing toner is a transparent or translucent sheet with a thickness of 0.5 μm to 5 μm.
[0024] Optionally, the infrared reflective powder includes a first dielectric film layer, a metal film layer and a second dielectric film layer which are sequentially stacked, the thickness of the first dielectric film layer is 10 nm to 100 nm, the thickness of the metal film layer is 3 nm to 30 nm, and the thickness of the second dielectric film layer is 10 nm to 100 nm.
[0025] Optionally, the infrared reflective powder is one or more selected from ZnS / Ag / ZnS, SiO₂ / Ag / TiO₂, Al₂O₃ / Ag / Al₂O₃, and ZnO / Ag / ZnS, preferably ZnS / Ag / ZnS.
[0026] A colored solar module, comprising a surface glass layer, an upper adhesive film layer, a battery chip layer, a lower adhesive film layer and a back panel which are sequentially stacked, wherein the infrared reflective powder and the color developing toner are included on or in the front radiation receiving side.
[0027] Optionally, the colored solar module has high transmittance for light with a wavelength of 300 nm to 1100 nm, and has high reflectivity for infrared light with a wavelength of 1100 nm to 5000 nm.
[0028] Optionally, the infrared reflective powder is a transparent or translucent sheet with a thickness of 0.5 μm to 5 μm, and the color developing toner is a transparent or translucent sheet with a thickness of 0.5 μm to 5 μm.
[0029] Optionally, the infrared reflective powder includes a first dielectric film layer, a metal film layer and a second dielectric film layer which are sequentially stacked, wherein the thickness of the first dielectric film layer is 10 nm to 100 nm, the thickness of the metal film layer is 3 nm to 30 nm, and the thickness of the second dielectric film layer is 10 nm to 100 nm.
[0030] Optionally, the infrared reflective powder is one or more selected from ZnS / Ag / ZnS, SiO₂ / Ag / TiO₂, Al₂O₃ / Ag / Al₂O₃, and ZnO / Ag / ZnS, preferably ZnS / Ag / ZnS.
[0031] Optionally, the colored solar module includes a color glaze layer disposed between the surface glass layer and the upper adhesive film layer, or on the air side of the surface glass layer, and the color glaze layer includes an infrared reflective powder and a color developing toner.
[0032] Optionally, the color glaze layer is formed by the ink according to any one of the above descriptions.
[0033] Optionally, the upper adhesive film layer includes an infrared reflective powder and a color developing toner.
[0034] Optionally, in the upper adhesive film layer, the mass ratio of the infrared reflective powder is 0.1% to 30%, preferably 5% to 15%, and the mass ratio of the color developing toner is 0.1% to 20%, preferably 1% to 5%.
[0035] Optionally, the lower adhesive film layer includes a first lower flexible adhesive film layer, a reinforcing adhesive film layer and a second lower flexible adhesive film layer which are sequentially stacked.
[0036] This application optimizes the coloring means to ensure that the module has high efficiency while simultaneously providing color. Furthermore, by adding infrared reflective toner, the reflectivity of the module's front panel glass to infrared rays is increased, contributing to a decrease in the module's operating temperature, improving power generation, and extending the module's lifespan.
[0037] The above is merely a general description of the technical solution of the present invention. In order to provide a clearer understanding of the technical means of the present invention and to enable implementation based on the contents of the specification, and to make the above and other objectives, features and advantages of the present invention easier to understand, specific embodiments of the present invention are provided below. [Brief explanation of the drawing]
[0038] To more clearly illustrate embodiments of the present invention or technical means in the prior art, the drawings used in describing the embodiments or the prior art will now be briefly described. Clearly, the drawings described below are some embodiments of the present invention, and those skilled in the art can obtain other drawings based on these without any creative work.
[0039] [Figure 1] This is a schematic diagram of the colored solar module for which this application was filed. [Figure 2] This is a graph of the surface reflectance of the solar module manufactured in Example 1. [Figure 3] This is another schematic diagram of the colored solar module of this application. [Figure 4] This is another schematic diagram of the colored solar module of this application. [Modes for carrying out the invention]
[0040] To further clarify the object, technical means, and advantages of the embodiments of the present invention, the technical means in the embodiments of the present invention will be clearly and completely described below with reference to the drawings of the embodiments of this application. However, it should be noted that the embodiments described are only a part of the embodiments of the present invention, not all embodiments. Any other embodiments that a person skilled in the art could obtain without creative work based on the embodiments of the present invention shall be within the scope of protection of this application.
[0041] Next, the present application will be further described with reference to examples, which are not intended to limit the present application but are merely for the purpose of further describing and explaining the present application.
[0042] Unless otherwise specified, technical and scientific terms in this specification have the same meaning as those generally understood by those skilled in the art. Materials and methods are described below, but similar or identical methods and materials may be used in experiments or practical applications. In case of any inconsistency, the definitions included herein shall prevail. Furthermore, materials, methods, and examples are for illustrative purposes only and are not restrictive. The application will be further described below with specific examples, but this will not limit the scope of the application.
[0043] This application provides an ink. The ink comprises an infrared reflective powder and a color-developing toner, wherein the mass ratio of the infrared reflective powder in the ink is 0.1% to 30%, and may be, for example, 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, or 30%, and is preferably 5% to 15%. The mass ratio of the color-developing toner is 0.1% to 20%, and may be, for example, 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%, and is preferably 1% to 5%.
[0044] The infrared reflective powder is a powder capable of reflecting infrared light, and preferably has high transmittance to light with wavelengths of 300 nm to 1100 nm and high reflectance to infrared light with wavelengths of 1100 nm to 5000 nm.
[0045] In a specific embodiment, an infrared reflective powder having high transmittance to light with wavelengths of 300 nm to 1100 nm means that the transmittance to light with wavelengths of 300 nm to 1100 nm is at least 50%, for example, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, This means that percentages such as 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% are also acceptable.
[0046] In a specific embodiment, the statement that an infrared reflective powder has a high reflectivity for infrared light with wavelengths of 1100 nm to 5000 nm means that the reflectivity for infrared light with wavelengths of 1100 nm to 5000 nm is at least 40%, and may be, for example, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, etc.
[0047] The infrared reflective powder is a transparent or translucent sheet, with a thickness of 0.5 μm to 5 μm, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4.0 μm, 4.5 μm, or 5 μm. Since the infrared reflective powder itself is a transparent or translucent sheet, it does not cause a decrease in the transmittance of incident light due to its extremely low shielding and absorption of incident light.
[0048] In a specific embodiment, the infrared reflective powder has a three-layer structure including a first dielectric film layer, a metal film layer, and a second dielectric film layer arranged in a sequential stacked configuration. The thickness of the first dielectric film layer is 10 nm to 100 nm, and may be, for example, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, or 100 nm. The thickness of the metal film layer is 3 nm to 30 nm, and may be, for example, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, or 30 nm. The thickness of the second dielectric film layer is 10 nm to 100 nm, and may be, for example, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, or 100 nm.
[0049] The materials for the first and second dielectric film layers may be selected from ZnS, ZnO, ZnSe, Bi2O3, NbO5, and CeO2. The materials for the first and second dielectric film layers may be the same or different. The material for the metal film layer may be selected from Ag, Au, Cu, Mo, and Al. The infrared reflective powder's reflection and transmission of light in different wavelength ranges can be adjusted by changing the materials and thicknesses of the dielectric film layers and metal film layers.
[0050] In a specific embodiment, the infrared reflective powder is one or more selected from ZnS / Ag / ZnS, SiO2 / Ag / TiO2, Al2O3 / Ag / Al2O3, and ZnO / Ag / ZnS, preferably ZnS / Ag / ZnS. Taking ZnS / Ag / ZnS as an example, ZnS / Ag / ZnS includes a first dielectric film layer, a metal film layer, and a second dielectric film layer arranged in a sequential stacked configuration, where the first and second dielectric film layers are ZnS and the metal film layer is Ag. The thickness of the ZnS layer is 10 nm to 100 nm, and the thickness of the Ag layer is 3 nm to 30 nm.
[0051] In specific embodiments, the infrared reflective powder may be, for example, an infrared reflective powder manufactured based on the above structure, or a commercially available product. For example, ZnS / Ag / ZnS infrared reflective powder can be manufactured by the following method: Using a single-sided polished Si(111) wafer and a 2 mm thick K9 glass plate as a base, ZnS is deposited by electron beam deposition using a box-type vacuum coater. After the deposition of the first layer of ZnS, a thin Ag film layer is manufactured by resistance thermal deposition in a box-type vacuum coater using high-purity silver particles as a deposition source. Subsequently, a third layer of ZnS film is manufactured in the same manner as the first layer of ZnS. After manufacturing, the multilayer film is peeled from the base and crushed to obtain infrared reflective powder.
[0052] The color-developing toner may be any color-developing toner available in this field. For example, it may be a multilayer oxide composed of metal oxides such as titanium, aluminum, silicon, tin, zirconium, and zinc; it may be a multilayer structure formed by adding natural or synthetic mica to a metal oxide such as TiO2, which expresses different colors through optical interference; or it may be a multilayer oxide having the characteristics of a micro-nano structure. The color-developing toner is a transparent or translucent sheet, with a sheet thickness of 0.5 μm to 5 μm, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4.0 μm, 4.5 μm, or 5 μm. The transparent or translucent sheet does not reduce the light transmittance of the surface. Furthermore, when infrared reflective powder and colored toner are placed on or within the front-radiation receiving side of the solar module, the infrared reflective powder disperses in the ink to form multiple optical scattering centers. Working in cooperation with the colored toner, it increases the secondary reflection of light, thereby increasing the transmittance of incident light and improving power generation efficiency. In addition, light scattering reduces flip-flop defects and improves the overall aesthetics of the module.
[0053] In specific embodiments, the color-developing toner may be a substance obtained by any means that expresses different colors through optical interference. For example, it may be a commercially available or self-manufactured blue pearl powder or a red multilayer oxide nanotoner.
[0054] For example, red multilayer oxide nanotoner can be manufactured by the following method: Using K9 glass as a base, a release agent is applied to the surface of the glass, and TiO2 and SiO2 materials are deposited in that order in a film-like manner on the base by electron beam deposition using a vacuum coater, thereby forming a multilayer oxide film. After the deposition is complete, the red multilayer oxide nanotoner can be obtained by demolding and pulverization.
[0055] The ink of this application may be a high-temperature ink or a low-temperature ink. If it is a high-temperature ink, the ink of this application consists of infrared reflective powder, a color-developing toner, glass powder, and an organic solvent. The glass powder is formed by smelting and grinding a mixture of silicon oxide, bismuth oxide, boron oxide, zinc oxide, potassium carbonate, titanium oxide, zirconium oxide, aluminum oxide, calcium oxide, strontium oxide, glass strengthening agents, glass clarifying agents, decolorizing agents, etc.
[0056] In the high-temperature ink, the mass ratio of infrared reflective powder is 0.1% to 30%, and may be, for example, 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, or 30%, preferably 5% to 15%. The mass ratio of the color-developing toner is 0.1% to 20%, and may be, for example, 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%, preferably 1% to 5%. The mass ratio of the glass powder is 30% to 70%, and may be, for example, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, or 70%. The mass ratio of the organic solvent is 10% to 40%, and may be, for example, 10%, 15%, 20%, 25%, 30%, 35%, or 40%.
[0057] The organic solvent is selected from hexanediol acrylate, functional acrylates, coupling agents, photocatalysts, and other resins. The materials for the infrared reflective powder and colored toner are as described above.
[0058] If the ink is a low-temperature ink, it consists of infrared reflective powder, a color-developing toner, and an organic solvent. The materials for the infrared reflective powder, color-developing toner, and organic solvent are as described above.
[0059] In the low-temperature ink, the mass ratio of infrared reflective powder is 0.1% to 30%, and may be, for example, 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, or 30%, preferably 5% to 15%. The mass ratio of the color-developing toner is 0.1% to 20%, and may be, for example, 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%, preferably 1% to 5%. The mass ratio of the organic solvent is 70% to 99.9%.
[0060] This application further provides a colored solar module. The colored solar module includes a sequentially stacked colored glass layer, a battery chip layer, a first lower flexible adhesive film layer, a reinforcing adhesive film layer, a second lower flexible adhesive film layer, and a back glass layer.
[0061] The colored glass layer contains infrared reflective powder and color-developing toner. The infrared reflective powder and color-developing toner are those specified above for the ink.
[0062] In a specific embodiment, the infrared reflective powder has a three-layer structure including a first dielectric film layer, a metal film layer, and a second dielectric film layer arranged in a sequential stacked configuration. The thickness of the first dielectric film layer is 10 nm to 100 nm, the thickness of the metal film layer is 3 nm to 30 nm, and the thickness of the second dielectric film layer is 10 nm to 100 nm.
[0063] In a specific embodiment, the infrared reflecting powder is one or more selected from ZnS / Ag / ZnS, SiO2 / Ag / TiO2, Al2O3 / Ag / Al2O3, and ZnO / Ag / ZnS, and is preferably ZnS / Ag / ZnS.
[0064] The colored glass layer may have two types of structures. The first type includes a surface glass layer, a color glaze layer, and an upper adhesive film layer arranged in a sequential stacked configuration, wherein the upper adhesive film layer is closer to the battery chip layer than to the surface glass layer and the color glaze layer. The color glaze layer includes infrared reflective powder and a color developing toner, and the mass ratio of the infrared reflective powder in the color glaze layer is 0.1% to 30%, and may be, for example, 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, or 30%, preferably 5% to 15%. The mass ratio of the color-developing toner is 0.1% to 20%, and may be, for example, 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%, and is preferably 1% to 5%.
[0065] As shown in Figure 1, a colored solar module with this structure includes a surface glass layer 1, a color glaze layer 2, an upper adhesive film layer 3, a battery chip layer 4, a first lower flexible adhesive film layer 5, a reinforcing adhesive film layer 6, a second lower flexible adhesive film layer 7, and a back glass layer 8, all arranged in a sequential stacked configuration.
[0066] The surface glass layer 1 may be selected differently depending on the application. When used in the field of curtain walls for buildings, low-iron float glass is preferred, and its thickness may be selected from 2 mm to 16 mm depending on the design requirements. In addition, an anti-reflective coating may be applied to the surface of the glass depending on the actual requirements. When used as decorative roofing material, low-iron patterned glass or low-iron float glass of 1 to 5 mm thickness may be selected. In addition, an anti-reflective coating may be applied to the surface of the glass depending on the actual requirements.
[0067] The color glaze layer 2 adheres to the surface glass layer 1 and can be obtained by screen printing or spray coating an ink containing infrared reflective powder and color-developing toner onto the glass, and then sintering it at a temperature range of 500 to 800°C. The ink may be the high-temperature ink or low-temperature ink described in this application.
[0068] In a specific embodiment, the thickness of the color glaze layer is 5 μm to 100 μm, and may be, for example, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, or 100 μm, and preferably 10 μm to 30 μm.
[0069] The upper adhesive film layer 2 may be colorless and transparent, or it may be a colored adhesive film to which the infrared reflective powder and color-developing toner of this application have been added. That is, a colored adhesive film can be obtained by adding the infrared reflective powder and color-developing toner to a colorless and transparent adhesive film. The material of the upper adhesive film layer 2 may be EVA, POE, PVB, SGP, etc.
[0070] As a second type of colored glass layer, the colored glass layer includes a surface glass layer and an upper adhesive film layer arranged in a sequential stacked configuration, the upper adhesive film layer being closer to the battery chip layer than the surface glass layer, and the upper adhesive film layer containing infrared reflective powder and a color-developing toner, i.e., the upper adhesive film layer being a colored adhesive film. In such a colored glass layer, the reflective effect may be adjusted by adjusting the concentration of the toner in the upper adhesive film layer, or by adjusting the thickness of the upper adhesive film layer within a predetermined range. In the upper adhesive film layer, the mass ratio of the infrared reflective powder is 0.1% to 30%, preferably 5% to 15%, and the mass ratio of the color-developing toner is 0.1% to 20%, preferably 1% to 5%. The thickness of the upper adhesive film layer may be 0.1 mm to 0.7 mm, for example, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, or 0.7 mm.
[0071] By incorporating infrared reflective powder and color-developing toner into the colored glass layer, the temperature of the solar module can be reduced while simultaneously allowing the solar module to display various colors. This ensures that the solar module maintains high efficiency while adding color to it.
[0072] In this application, the battery chip layer may include a plurality of battery chips arranged sequentially in an array at equal intervals. The battery chips may be general single-crystal or polycrystalline battery chips, or other types of battery chips. The number of grid lines of the battery chips may be any number from 2 to 30. Furthermore, the battery chips may be back-contact type battery chips, roof-plate-like overlapping structure battery chips, or metal-wrap-through structure battery chips and corresponding connection structures.
[0073] In this application, the first lower flexible adhesive film layer and the second lower flexible adhesive film layer are both selected from among an EVA film layer, a POE film layer, a PVB film layer, or an SGP film layer.
[0074] Specifically, the first lower flexible adhesive film layer and the second lower flexible adhesive film layer may be similar or different film layers.
[0075] In this application, the reinforcing adhesive film layer is one of the following: a PET film layer, a PU film layer, a nylon layer, or a metal screen layer.
[0076] The back glass layer may be transparent glass, have its inner surface coated with a black glaze layer, or have a mesh-like black glaze layer printed in the gaps between the battery cells by screen printing. The thickness of the back glass layer may be 1 to 16 mm.
[0077] Furthermore, the colored solar module described in this application may further include ribbons, busbars, junction boxes, and cables for mounting the module, etc., for connecting the battery cells to each other and conducting current.
[0078] This application further provides a colored solar module comprising any one of the above-described infrared reflective powders and a color-developing toner. Specifically, as shown in Figures 3 and 4, the colored solar module comprises a sequentially stacked surface glass layer 1, an upper adhesive film layer 3, a battery chip layer 4, a lower adhesive film layer 9, and a back panel 10, wherein the solar module includes the infrared reflective powder and color-developing toner on or within the front radiation receiving side.
[0079] In this application, the pre-radiation receiving side refers to the region above the receiving side of the battery chip layer, and "including infrared reflective powder and color-developing toner on or within the pre-radiation receiving side" includes various cases in which the infrared reflective powder and color-developing toner are located on the air side of the surface glass layer (i.e., the side of the surface glass layer away from the battery chip layer), the non-air side of the surface glass layer (i.e., the side of the surface glass layer closer to the battery chip layer), on both sides of the upper adhesive film layer, within the upper adhesive film layer, etc.
[0080] In a specific embodiment, the colored solar module has high transmittance to light with wavelengths of 300 nm to 1100 nm and high reflectance to infrared light with wavelengths of 1100 nm to 5000 nm.
[0081] In a specific embodiment, a colored solar module having high transmittance to light with wavelengths of 300 nm to 1100 nm means that the transmittance to light with wavelengths of 300 nm to 1100 nm is at least 50%, for example, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%. This means that percentages such as %, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% are also acceptable.
[0082] In a specific embodiment, a colored solar module having high reflectivity to infrared light with wavelengths of 1100 nm to 5000 nm means that the reflectivity to infrared light with wavelengths of 1100 nm to 5000 nm is at least 25%, and may be, for example, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, etc.
[0083] As those skilled in the art will understand, under all other conditions, there is a positive correlation between the amount of infrared reflective powder in a colored solar module and its reflectivity to infrared light with wavelengths of 1100nm to 5000nm. By adjusting the amount of infrared reflective powder contained in the solar module, the reflectivity to infrared light with wavelengths of 1100nm to 5000nm can be adjusted to meet different actual demands.
[0084] In a specific embodiment, the colored solar module includes, as shown in Figure 3, a sequentially stacked surface glass layer 1, a color glaze layer 2, an upper adhesive film layer 3, a battery chip layer 4, a lower adhesive film layer 9, and a back panel 10. The color glaze layer 2 contains infrared reflective powder and a color-developing toner, i.e., the infrared reflective powder and the color-developing toner are located within the color glaze layer 2.
[0085] In a specific embodiment, the colored solar module includes sequentially stacked color glaze layers 2, a surface glass layer 1, an upper adhesive film layer 3, a battery chip layer 4, a lower adhesive film layer 9, and a back panel 10. The color glaze layer 2 includes infrared reflective powder and a color-developing toner, i.e., the infrared reflective powder and the color-developing toner are located within the color glaze layer 2.
[0086] The color glaze layer 2 may further contain other components, such as glass powder.
[0087] In a specific embodiment, the color glaze layer 2 is attached to both sides of the surface glass layer 1 (which may be the air side or the non-air side of the surface glass layer) and is formed with any one of the high-temperature or low-temperature inks described in this application. The color glaze layer 2 can be obtained, for example, by screen printing or spray coating a high-temperature or low-temperature ink containing infrared reflective powder and a color-developing toner onto the glass, and then sintering it at a temperature range of 500 to 800°C.
[0088] The lower adhesive film layer 9 may be any type of adhesive film layer known in the art. For example, it may be a single-layer flexible adhesive film layer. For example, it may be any one of the following: an EVA film layer, a POE film layer, a PVB film layer, or an SGP film layer. As described above, as shown in Figure 1, it may also include a first lower flexible adhesive film layer 5, a reinforcing adhesive film layer 6, and a second lower flexible adhesive film layer 7 that are sequentially laminated.
[0089] The back panel 10 may be any type of back panel known in the art. For example, it may be a back panel made of glass material, i.e., the glass layer shown in Figure 1 above. It may also be a back panel made of polymer material.
[0090] In a specific embodiment, the colored solar module includes a sequentially stacked surface glass layer 1, an upper adhesive film layer 3, a battery chip layer 4, a lower adhesive film layer 9, and a back panel 10, as shown in Figure 4. The upper adhesive film layer 3 contains infrared reflective powder and a color-developing toner, i.e., the infrared reflective powder and the color-developing toner are located within the upper adhesive film layer 3. The infrared reflective powder and the color-developing toner are added to the upper adhesive film layer 3 by methods known in the art.
[0091] In such colored solar modules, the reflective effect may be adjusted by adjusting the content of infrared reflective powder in the upper adhesive film layer 3. Alternatively, the reflective effect may be adjusted by adjusting the thickness of the upper adhesive film layer 3 within a predetermined range. Furthermore, to ensure uniformity of the reflective powder and color-developing toner, the upper adhesive film 3 may have a two-layer structure. One layer is a layer containing infrared reflective powder and color-developing toner, and may have a thickness of 0.05 to 0.3 mm. The other layer is a transparent layer that does not contain reflective powder and color-developing toner, in order to satisfy the requirements of sealing and insulation, and may have a thickness of 0.2 to 1 mm. These two layers are formed by co-extrusion to create the upper adhesive film.
[0092] In a specific embodiment, in the upper adhesive film layer 3, the mass ratio of the infrared reflective powder is 0.1% to 30%, preferably 5% to 15%, and the mass ratio of the color-developing toner is 0.1% to 20%, preferably 1% to 5%.
[0093] In a specific embodiment, the thickness of the upper adhesive film layer 3 may be 0.1 mm to 0.7 mm, for example, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, or 0.7 mm.
[0094] Examples Example 1 High-temperature ink was produced by thoroughly stirring and mixing 10g of ZnS(38nm) / Ag(10nm) / ZnS(40nm), 3g of commercially available blue pearl powder, 67g of commercially available glass powder, and 20g of organic solvent varnish, and then further mixing them uniformly using a three-roll mixing machine.
[0095] The ZnS / Ag / ZnS infrared reflective powder was manufactured by the following method. Using a single-sided polished Si(111) wafer and a 2 mm thick K9 glass plate as a base, ZnS was deposited by electron beam deposition using a box-type vacuum coater. After the deposition of the first layer of ZnS, a thin Ag film layer was manufactured by resistance thermal deposition in a box-type vacuum coater using high-purity silver particles as the deposition source. Subsequently, a third layer of ZnS film was manufactured in the same manner as the first layer of ZnS. After manufacturing, the multilayer film was peeled from the base and pulverized to obtain the infrared reflective powder.
[0096] A mixed high-temperature ink was printed onto the inner surface of low-iron glass by screen printing, spray coating, or roll coating, and then baked in an infrared heated tunnel furnace at 150-250°C to form a color glaze layer on the inner layer of the low-iron glass. The thickness of the low-iron glass was 3.2 mm, and the thickness of the color glaze layer was 20 μm. After baking, transparent colored glass was obtained by strengthening in a strengthening furnace.
[0097] Colored solar modules were manufactured by laminating colored glass, a welded battery cell matrix, adhesive films such as EVA, black PET, and POE, and back glass, and then laminating them in a laminator at 140-150°C for approximately 20 minutes.
[0098] The reflectance graph obtained by measuring the manufactured colored solar modules is shown in Figure 2. In the blue wavelength range, the reflectance is approximately 30%, in the infrared wavelength range above 1100 nm, the average reflectance is 53%, and in the infrared wavelength range above 1700 nm, the average reflectance is over 80%. Because the amount of infrared light received by the modules is reduced, it was found that the operating temperature of the measured modules was 3 to 10°C lower than that of typical modules in a similar environment.
[0099] Examples 2-4 In Examples 2-4, colored solar modules were manufactured in the same manner as in Example 1, except that the mass of the infrared reflective powder differed.
[0100] Specifically, in Example 2, the mass of the infrared reflective powder was 5 g. In Example 3, the mass of the infrared reflective powder was 15 g. In Example 4, the mass of the infrared reflective powder was 3 g.
[0101] Examples 5-6 In Examples 5 and 6, colored solar modules were manufactured in the same manner as in Example 1, except that the type of infrared reflective powder was different.
[0102] Specifically, in Example 5, the infrared reflective powder was SiO2 (38 nm) / Ag (10 nm) / TiO2 (40 nm). In Example 6, the infrared reflective powder was Al2O3 (38 nm) / Ag (10 nm) / Al2O3 (40 nm).
[0103] Example 7 Low-temperature ink was produced by thoroughly stirring and mixing 9g of ZnS(38nm) / Ag(10nm) / ZnS(40nm), 1g of red multilayer oxide nanotoner, 90g of n-butyl acrylate, and a thermal initiator (azobisisobutyronitrile).
[0104] The red multilayer oxide nanotoner was manufactured by the following method: Using K9 glass as a base, a release agent was applied to the surface of the glass, and TiO2 and SiO2 materials were deposited in that order in a film-like manner on the base using electron beam deposition with a vacuum coater to form a multilayer oxide film. After the deposition was complete, the red multilayer oxide nanotoner was obtained by demolding and pulverization.
[0105] A mixed low-temperature ink was printed onto the inner surface of low-iron glass by screen printing, spray coating, or roll coating, and then baked in an infrared-heated tunnel furnace at 150-250°C to form a color glaze layer on the inner layer of the low-iron glass. The thickness of the low-iron glass was 2 mm, and the thickness of the color glaze layer was 25 μm. After baking, strengthening was performed using a strengthening furnace, and then heat-cured in an infrared-heated tunnel furnace to obtain transparent colored glass.
[0106] Colored solar modules were manufactured by laminating colored glass, a welded battery cell matrix, adhesive films such as EVA, black PET, and POE, and back glass, and then laminating them in a laminator at 140-150°C for approximately 20 minutes.
[0107] Example 8 In Example 8, a colored solar module was manufactured in the same manner as in Example 7, except that the mass of the infrared reflective powder was different.
[0108] Specifically, in Example 8, the mass of the infrared reflective powder was set to 4 g.
[0109] Examples 9-10 In Examples 9 and 10, colored solar modules were manufactured in the same manner as in Example 7, except that the type of infrared reflective powder was different.
[0110] Specifically, in Example 9, the infrared reflective powder was SiO2 (38 nm) / Ag (10 nm) / TiO2 (40 nm). In Example 10, the infrared reflective powder was Al2O3 (38 nm) / Ag (10 nm) / Al2O3 (40 nm).
[0111] Example 11 Example 11 differs from Example 1 in that the ZnS / Ag / ZnS and blue pearl powder are located in the upper adhesive layer rather than as a color glaze layer, and the amount of blue pearl powder is different.
[0112] Specifically, 10 g of ZnS / Ag / ZnS, 5 g of commercially available blue pearl powder, and 85 g of EVA particles and additives were mixed, heated and melted, then uniformly stirred to extrude a 0.1 mm thick colored EVA adhesive film layer. The colored adhesive film layer and a 0.4 mm thick transparent EVA adhesive film layer were co-extruded to form the upper adhesive film layer (the thickness is the same as the 0.5 mm EVA upper adhesive film layer in Examples 1 to 10).
[0113] Comparative Example 1 Comparative Example 1 differs from Example 1 in that the high-temperature ink produced does not contain infrared reflective powder.
[0114] Specifically, high-temperature ink was produced by thoroughly stirring and mixing 3g of blue pearl powder, 67g of glass powder, and 30g of organic solvent varnish, and then further uniformly mixing them using a three-roll mixing machine.
[0115] Table 1 shows the specific ink recipes for the above examples and comparative examples, as well as the operating temperature and average infrared reflectance at 1100 nm and above for the colored solar modules manufactured in each example and comparative example.
[0116] [Table 1]
[0117] The specification described herein provides a great deal of detail. However, it can be understood that the embodiments of the present invention can be implemented without these details. There are also known methods, structures, and techniques that are not described in detail here, so as not to cause confusion in understanding this specification.
[0118] In the claims, symbols in parentheses should not be understood as limitations on the claims. The term "includes" does not exclude the existence of elements or processes not described in the claims. The terms "one" or "one" preceding an element do not exclude the existence of multiple such elements. The present invention can be realized by hardware and a computer appropriately programmed to include multiple different elements. In claims describing multiple units of a device, some of these devices may be specifically realized by the same hardware. Terms such as "first," "second," "third," etc., are not used to indicate any order. These terms may be interpreted as names.
[0119] Finally, it should be noted that the above embodiments are merely for illustrating the technical means of the present invention and do not limit them. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art will understand that it is possible to modify the technical means described in each of the above embodiments or to substitute some of the technical features, and that the essence of the corresponding technical means will not deviate from the spirit and scope of the technical means of each embodiment of the present invention through such modifications or substitutions. [Explanation of Symbols]
[0120] 1. Surface glass layer 2. Color glaze layer 3 Upper adhesive film layer 4. Battery chip layer 5 First lower flexible adhesive film layer 6 Reinforced adhesive film layer 7 Second lower flexible adhesive film layer 8. Back glass layer 9 Lower adhesive film layer 10 Back Panel
Claims
1. An ink applied to a colored solar module, comprising infrared reflective powder and a color-developing toner, wherein the mass ratio of the infrared reflective powder is 5% to 15%, and the mass ratio of the color-developing toner is 1% to 5%. The infrared reflective powder comprises a first dielectric film layer, a metal film layer, and a second dielectric film layer arranged in a sequential stacked configuration, wherein the thickness of the first dielectric film layer is 10 nm to 100 nm, the thickness of the metal film layer is 3 nm to 30 nm, and the thickness of the second dielectric film layer is 10 nm to 100 nm. The aforementioned infrared reflective powder is characterized by being ZnS / Ag / ZnS, and is an ink.
2. The ink according to claim 1, wherein the infrared reflective powder has high transmittance to light with wavelengths of 300 nm to 1100 nm and high reflectance to infrared light with wavelengths of 1100 nm to 5000 nm, wherein the high transmittance is defined as the transmittance to light with wavelengths of 300 nm to 1100 nm being at least 50%, and the high reflectance is defined as the reflectance to infrared light with wavelengths of 1100 nm to 5000 nm being at least 40%.
3. The ink according to claim 1, characterized in that the infrared reflective powder is a transparent or translucent sheet with a thickness of 0.5 μm to 5 μm, and the color-developing toner is a transparent or translucent sheet with a thickness of 0.5 μm to 5 μm.
4. The ink according to claim 1, characterized in that the ink is a high-temperature ink composed of infrared reflective powder, a color-developing toner, glass powder, and an organic solvent.
5. The ink according to claim 4, characterized in that the mass ratio of the infrared reflective powder is 5% to 15%, the mass ratio of the color-developing toner is 1% to 5%, the mass ratio of the glass powder is 30% to 70%, and the mass ratio of the organic solvent is 10% to 40%.
6. The ink according to claim 1, characterized in that the ink is a low-temperature ink composed of infrared reflective powder, a color-developing toner, and an organic solvent.
7. The ink according to claim 6, characterized in that the mass ratio of the infrared reflective powder is 5% to 15%, the mass ratio of the color-developing toner is 1% to 5%, and the mass ratio of the organic solvent is 70% to 99.9%.
8. Colored solar modules, It includes a surface glass layer, an upper adhesive film layer, a battery chip layer, a lower adhesive film layer, and a back panel arranged in a sequential stacked configuration, and includes infrared reflective powder and color-developing toner on or within the front radiation receiving side. The colored solar module includes a color glaze layer between the surface glass layer and the upper adhesive film layer, or provided on the air side of the surface glass layer, and the color glaze layer includes infrared reflective powder and color developing toner. A colored solar module characterized in that the color glaze layer is formed with the ink described in any one of claims 1 to 7.
9. A colored solar module according to claim 8, characterized in that it has high transmittance to light with wavelengths of 300 nm to 1100 nm and high reflectance to infrared light with wavelengths of 1100 nm to 5000 nm, wherein the high transmittance is at least 50% for light with wavelengths of 300 nm to 1100 nm and the high reflectance is at least 40% for infrared light with wavelengths of 1100 nm to 5000 nm.
10. The colored solar module according to claim 8, characterized in that the infrared reflective powder is a transparent or translucent sheet with a thickness of 0.5 μm to 5 μm, and the color developing toner is a transparent or translucent sheet with a thickness of 0.5 μm to 5 μm.
11. The infrared reflective powder comprises a first dielectric film layer, a metal film layer, and a second dielectric film layer arranged in a sequential stacked configuration, wherein the thickness of the first dielectric film layer is 10 nm to 100 nm, the thickness of the metal film layer is 3 nm to 30 nm, and the thickness of the second dielectric film layer is 10 nm to 100 nm, characterized in that the colored solar module is as described in claim 8.
12. The colored solar module according to claim 11, characterized in that the infrared reflective powder is ZnS / Ag / ZnS.
13. The colored solar module according to claim 8, characterized in that the upper adhesive film layer contains infrared reflective powder and a color-developing toner.
14. The colored solar module according to claim 13, characterized in that, in the upper adhesive film layer, the mass ratio of the infrared reflective powder is 5% to 15%, and the mass ratio of the color-developing toner is 1% to 5%.
15. The colored solar module according to claim 8, characterized in that the lower adhesive film layer includes a first lower flexible adhesive film layer, a reinforcing adhesive film layer, and a second lower flexible adhesive film layer arranged in a sequential stacked configuration.
Citation Information
Patent Citations
Composite UV curing screen anti-counterfeiting ink and manufacturing method thereof
CN110105807A
Ink composition for forming infrared reflection pattern, method for forming infrared reflection pattern, and infrared reflector
JP2017043660A
Back sheet and encapsulant for solar cells, and solar cell module comprising the same
JP2019201211A
Transparent member and item
JP2022040749A
Photovoltaic devices
US20220149213A1