Phase difference film, polarizing plate, and image display device
A high-strength, solvent-resistant stretched retardation film with nx>nz>ny anisotropy and specific thermal properties minimizes cracks during solvent exposure, addressing the vulnerability of cyclic polyolefin films in image display devices.
Patent Information
- Application Number
- JP2025154797
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-09-18
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2041-06-25
AI Technical Summary
Stretched retardation films made of cyclic polyolefins are prone to edge cracks during solvent resistance tests, particularly when exposed to hydrocarbon solvents like hexane, due to high molecular orientation and low solvent resistance.
A stretched retardation film with a glass transition temperature of 145°C or higher, a heat dimensional change rate of 0.40% or less at 95°C, and a tensile strength of 10 to 20 N/10 mm perpendicular to the stretching direction, combined with a refractive index anisotropy of nx>nz>ny, is developed to enhance solvent resistance.
The film effectively suppresses crack formation during solvent resistance tests by maintaining high tensile strength and low dimensional change, even when exposed to hydrocarbon solvents, ensuring durability in image display device manufacturing.
Smart Images

Figure 0007954787000001 
Figure 0007954787000002
Abstract
Description
[Technical Field]
[0001] The present invention relates to a phase difference film, a polarizing plate, and an image display device. [Background technology]
[0002] Phase difference films are used in displays such as liquid crystal displays for optical compensation such as improving contrast and expanding the viewing angle, as well as for shielding (anti-reflection) of external light reflected by metal electrodes. Phase difference films using non-liquid crystal polymers are given optical anisotropy by stretching the polymer film in at least one direction. Many polymers have positive intrinsic birefringence, and the refractive index increases in the stretching direction.
[0003] The phase difference film is classified into positive A plates (nx>ny=nz), negative A plates (nz=nx>ny), and positive C plates (nx=ny) based on the relative magnitudes of the refractive indices nx in the slow phase axis direction, ny in the fast phase axis direction, and nz in the thickness direction.<nz)、ネガティブCプレート(nx=ny> They are classified into uniaxial films such as nz, and biaxial films such as positive B plates (nz>nx>ny), negative B plates (nx>ny>nz), and Z plates (nx>nz>ny).
[0004] When a polymer film is stretched longitudinally (uniaxial stretching at the free end), the polymer molecular chains become oriented in the longitudinal direction (stretching direction) as the film is stretched, while shrinkage occurs in the width and thickness directions. When a polymer film with a positive intrinsic refractive index is stretched longitudinally, the refractive index in the longitudinal direction (nx) increases, while the refractive index in the width direction (ny) and the refractive index in the thickness direction (nz) decrease. As a result, a positive A plate with refractive index anisotropy nx > ny = nz is obtained.
[0005] When a polymer film is stretched longitudinally with a heat-shrinkable film laminated to at least one side, the shrinkage in the width direction becomes larger than in the case of normal free-end uniaxial stretching due to the influence of the shrinkage force of the heat-shrinkable film. Therefore, in the case of a polymer having positive intrinsic birefringence, the refractive index ny in the phase-advancing axis direction becomes smaller, and the refractive index nz in the thickness direction becomes relatively larger, resulting in a phase difference film with refractive index anisotropy nx>nz>ny (see, for example, Patent Document 1).
[0006] Phase difference films are generally used in combination with polarizers. An image display panel is formed by laminating a polarizing plate, which consists of a polarizer and a phase difference film, onto an image display cell such as a liquid crystal cell or an organic EL cell. The image display panel is connected to a drive circuit, and if necessary, a cover glass, backlight, etc., are combined and housed in a casing to form an image display device. [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] Japanese Patent Publication No. 2006-72309 [Overview of the Initiative] [Problems that the invention aims to solve]
[0008] In the assembly of image display devices, adhesive is used to bond the cover glass to the surface of the polarizing plate, and the edges of the film may be exposed to the solvent contained in the adhesive. Furthermore, solvent-based cleaning may be performed during the assembly of image display devices. Therefore, solvent resistance is required for the phase difference film.
[0009] Cyclic polyolefins are excellent in transparency and heat resistance, as well as in chemical resistance, and are suitable as optical film materials for displays. However, when a stretched retardation film made of cyclic polyolefin is incorporated into an image display panel and a solvent resistance test is performed, fine cracks may occur at the end face of the film when a hydrocarbon solvent such as hexane is used. In particular, in stretched films having a refractive index anisotropy of nx>nz>ny, the occurrence of cracks in the solvent resistance test is significant.
[0010] In view of the above, an object of the present invention is to provide a stretched retardation film in which edge cracks are less likely to occur even in a solvent resistance test using a hydrocarbon solvent such as hexane. [MEANS FOR SOLVING THE PROBLEMS]
[0011] A retardation film according to one embodiment of the present invention is a stretched film of a cyclic polyolefin-based resin. The glass transition temperature of the retardation film is preferably 145°C or higher. The retardation film may have a heat dimensional change rate of 0.40% or less at a temperature of 95°C.
[0012] After applying hexane to the retardation film, the tensile strength when a tensile test is performed in a direction perpendicular to the stretching direction is preferably 10 to 20 N / 10 mm. The tensile strength (per unit area) of the retardation film after applying hexane may be 16 to 31 kPa.
[0013] The tensile strength in the direction perpendicular to the stretching direction of the retardation film (not coated with hexane) may be 40 N / 10 mm or more, and the tensile strength per unit area may be 60 kPa or more.
[0014] The front retardation of the retardation film may be 200 nm or more. The thickness of the retardation film may be 10 to 300 μm. The in-plane birefringence Δn=nx-ny of the retardation film is 1.0×10 -3 or more. The retardation film may have a refractive index anisotropy of nx>nz>ny.
[0015] nx is the refractive index in the slow phase axis direction within the plane of the phase difference film, ny is the refractive index in the fast phase axis direction within the plane of the phase difference film, and nz is the refractive index in the thickness direction of the phase difference film.
[0016] By laminating and integrating the above-mentioned phase difference film with a polarizer, a polarizing plate incorporating the phase difference film is obtained. This polarizing plate is suitably used in the formation of image display devices such as liquid crystal displays and organic EL displays. [Effects of the Invention]
[0017] The above-mentioned phase difference film suppresses crack formation even when it comes into contact with solvents during the manufacturing process of image display devices, such as during heating or washing. [Modes for carrying out the invention]
[0018] The phase difference film of the present invention is a stretched phase difference film obtained by stretching a cyclic polyolefin film. A cyclic polyolefin is a polymer that contains an alicyclic structure in the repeating units of its main chain.
[0019] Examples of cyclic polyolefin resins include those described in Japanese Patent Publication No. 1-240517, Japanese Patent Publication No. 3-14882, and Japanese Patent Publication No. 3-122137. Specific examples include ring-opening (co)polymers of cyclic olefins, addition polymers of cyclic olefins, copolymers of cyclic olefins with α-olefins such as ethylene and propylene (typically random copolymers), and graft polymers and hydrides obtained by modifying these with unsaturated carboxylic acids or their derivatives. Commercially available cyclic polyolefin resins include "Zeonor" and "Zeonex" from Nippon Zeon, "Arton" from JSR, "Appel" from Mitsui Chemicals, and "Topas" from TOPAS ADVANCEDPOLYMERS.
[0020] The cyclic polyolefin film preferably contains 50% by weight or more of the cyclic polyolefin resin. The content of the cyclic polyolefin resin in the cyclic polyolefin film is more preferably 70% by weight or more, even more preferably 80% by weight or more, and may be 90% by weight or more or 95% by weight or more.
[0021] Known methods such as solution casting and melt extrusion can be used to manufacture cyclic polyolefin films. The film thickness is not particularly limited, but is generally around 5 μm to 300 μm. The film may contain additives such as UV absorbers, stabilizers, lubricants, and plasticizers.
[0022] A phase difference film can be obtained by stretching a polymer film to increase its molecular orientation in a specific direction. Stretching methods include longitudinal uniaxial stretching, transverse uniaxial stretching, sequential longitudinal and transverse biaxial stretching, and simultaneous longitudinal and transverse biaxial stretching. Any suitable stretching machine can be used, such as a roll stretcher, tenter stretcher, or pantograph or linear motor type biaxial stretcher.
[0023] With a heat-shrinkable film laminated on at least one surface of a polymer film, the film is stretched in one direction while utilizing the shrinkage force of the heat-shrinkable film to shrink the film in a direction perpendicular to the stretching direction. This results in a stretched phase difference film having a refractive index anisotropy of nx>nz>ny, where nx is the refractive index in the in-plane slow phase axis direction (stretching direction), ny is the refractive index in the in-plane fast phase axis direction, and nz is the refractive index in the thickness direction.
[0024] The heat-shrinkable film is not particularly limited as long as it shrinks in a direction perpendicular to the stretching direction when laminated to the polymer film and stretched. The heat-shrinkable film may have an anisotropic shrinkage rate. For example, when stretching a laminate of a polymer film and a heat-shrinkable film, stretching it in the width direction and shrinking it in the length direction, a heat-shrinkable film may be used in which the amount of shrinkage in the length direction is greater than the amount of shrinkage in the width direction. As an example, when making a heat-shrinkable film (during stretching), by gripping both ends of the film with tenter clips, etc., and moving the clips so that the distance between the clips in the length direction increases while maintaining the distance between the clips in the width direction, a heat-shrinkable film that shrinks easily in the length direction can be obtained.
[0025] The heat-shrinkable film is not particularly limited as long as it has biaxial orientation and shrinks in a direction perpendicular to the stretching direction when laminated to the polymer film and stretched. The heat-shrinkable film may have different shrinkage rates in the stretching direction and the shrinking direction during the stretching process. For example, when stretching a laminate of a polymer film and a heat-shrinkable film, stretching it in the width direction and shrinking it in the longitudinal direction, a heat-shrinkable film with a large amount of shrinkage in the longitudinal direction may be used. As an example, when manufacturing a heat-shrinkable film, by gripping both ends of the film with tenter clips, etc., and moving the clips so that the tenter clip spacing in the longitudinal direction increases while maintaining the distance between clips in the width direction, a heat-shrinkable film that shrinks easily in the longitudinal direction can be obtained.
[0026] The materials constituting the heat-shrinkable film are not particularly limited, but those that shrink at around the stretching temperature of the cyclic polyolefin film are preferred. Due to their versatility and low cost, polyolefins such as polyethylene and polypropylene, and polyesters are preferably used as materials for heat-shrinkable films.
[0027] The front retardation Re of the phase difference film is, for example, around 15 nm to 400 nm, and may be 100 nm or more, or 150 nm or more. The phase difference film may have an NZ coefficient defined as NZ = (nx-nz) / (nx-ny) of around 0 to 3. The NZ coefficient may be 1.5 or less, 1.0 or less, or 0.1 to 0.9, 0.2 to 0.8, or 0.3 to 0.7. The front retardation and NZ coefficient of the phase difference film are set appropriately according to the application of the phase difference film and the optical design of the image display device. Applications of phase difference films with an NZ coefficient less than 1 include optical compensation in liquid crystal display devices and circular polarizers for shielding reflected light in organic EL display devices.
[0028] For example, in IPS type liquid crystal display devices, when viewed from an oblique direction at an angle of 45 degrees with respect to the absorption axis of the polarizer (azimuth angles of 45, 135, 225, and 315 degrees), significant light leakage in black displays occurs, easily leading to a decrease in contrast and color shift. By placing a phase difference film between the liquid crystal cell and the polarizer, where the frontal retardation is 1 / 2 of the wavelength λ and the NZ coefficient is 0.5, the black brightness in oblique directions can be reduced and contrast can be improved.
[0029] In organic EL display devices, a circular polarizer is placed on the viewing side of the organic EL cell to prevent light from being reflected by metal electrodes and the reflected light from being visible from the outside as if it were a mirror. The circular polarizer has a configuration in which a λ / 4 plate, whose frontal retardation is 1 / 4 of the wavelength λ, is placed on one side of the polarizer (the side facing the organic EL cell). A phase difference film with refractive index anisotropy nx>nz>ny exhibits little change in retardation depending on the viewing angle. Therefore, by using a phase difference film with refractive index anisotropy nx>nz>ny as the λ / 4 plate of the circular polarizer, the shielding of light not only in the front (normal direction) of the display device but also in oblique directions can be improved.
[0030] The thickness of the phase difference film is not particularly limited, but from the viewpoint of strength and workability such as handling, 5 to 300 μm is preferred. To increase the frontal retardation, the thickness of the phase difference film is preferably 10 μm or more, more preferably 20 μm or more, and may be 30 μm or more, 40 μm or more, or 50 μm or more. The thickness of the phase difference film may be 250 μm or less or 200 μm or less.
[0031] The in-plane birefringence Δn of the phase difference film is 1.0 × 10⁻⁶. -3 The above is also acceptable. The in-plane birefringence Δn = nx - ny is the difference between the refractive index nx in the slow phase axis direction and the refractive index ny in the fast phase axis direction, and is the value obtained by dividing the frontal retardation Re by the thickness. In stretched phase difference films, Δn tends to increase as the stretching ratio increases, and the larger Δn, the greater the frontal retardation that can be achieved with a small thickness. The Δn of a phase difference film is 1.3 × 10⁻⁶. -3 The above, or 1.5 × 10 -3 That's fine too.
[0032] The glass transition temperature (Tg) of the phase difference film is preferably 145°C or higher, and may be 147°C or higher. The higher the Tg of the phase difference film, the less likely it is to undergo retardation due to heating. The dimensional change rate of the phase difference film at 95°C is preferably 0.40% or less. The dimensional change rate at 95°C is measured by thermomechanical analysis (TMA). There is a tendency for the dimensional change rate at 95°C to be smaller as the Tg increases.
[0033] In the manufacturing process of image display devices, heating may be performed after a polarizing plate is bonded to the surface of the image display cell, in order to adjust the moisture content of the polarizer. Also, during lighting tests, the panel temperature may rise to around 80-100°C. The higher the Tg of the phase difference film and the smaller the dimensional change rate at 95°C, the more likely it is that cracks will occur in the phase difference film when a solvent resistance test is performed after heating the image display panel.
[0034] From the viewpoint of suppressing crack formation during solvent resistance testing, it is preferable that the tensile strength of the phase difference film after hexane application is 10 N / 10 mm or higher. The tensile strength is the test force at which the sample begins to break or undergo plastic deformation when a tensile test is performed in accordance with JIS K7161 using a 10 mm wide test specimen with the longer side (tensile direction) perpendicular to the stretching direction. The tensile strength per unit area, obtained by dividing this test force by the cross-sectional area of the sample, is preferably 16 kPa or higher.
[0035] In addition to the high glass transition temperature of the phase difference film, the high tensile strength after hexane coating tends to suppress the occurrence of cracks at the edges of the phase difference film during solvent resistance tests.
[0036] The occurrence of cracks at the edges of phase difference films in solvent resistance tests is thought to be due to the strain of the stretched phase difference film and the effects of local dissolution in organic solvents. In stretched phase difference films, the polymer chains are oriented in the stretching direction, and generally, cracks tend to occur along the stretching direction. In particular, cyclic polyolefins have a small intrinsic birefringence, so the in-plane birefringence Δn is large, and a high stretching ratio is necessary to obtain a phase difference film with a large frontal retardation. Furthermore, stretched films with refractive index anisotropy nx>nz>ny are stretched in the stretching direction (slow phase axis direction) and simultaneously contracted highly in the direction perpendicular to the stretching direction (advancing phase axis direction), resulting in a high degree of orientation of the polymer chains in the stretching direction, making them prone to cracking.
[0037] In an image display panel, the phase difference film is bonded and fixed to other components such as a polarizing plate (polarizer) and an image display cell. When heating to adjust the moisture content of the polarizer or a lighting test is performed in this state, the temperature of the image display panel rises to about 80-100°C. While the image display cell undergoes only a slight dimensional change even when heated to about 100°C, resin materials such as the phase difference film expand when heated.
[0038] When a phase difference film is bonded to an image display cell or the like, the force of expansion due to heating accumulates as stress within the film. When the edge of the film comes into contact with a solvent while a large amount of stress has accumulated, the stress is locally relieved at the solvent contact point, but conversely, the stress concentrates in the surrounding areas, which is thought to cause crack formation. Films with a low glass transition temperature and large dimensional changes due to heating are thought to be prone to cracking due to contact with solvents because the stress accumulated inside when bonded to an image display cell or the like is large. In particular, films with high molecular chain orientation, such as stretched phase difference films with refractive index anisotropy nx>nz>ny, are prone to cracking due to the high molecular orientation, and the large stress generated by heating is also thought to be a factor in the likelihood of crack formation.
[0039] In this invention, because the glass transition temperature of the film is high, dimensional changes during heating are small, and stress accumulated within the film in the image display device is reduced. Furthermore, because the tensile strength after hexane coating is high, that is, because the film maintains a certain strength even after contact with hexane, local stress relaxation due to contact with the solvent and stress concentration in the surrounding area are less likely to occur, and it is believed that crack formation is suppressed even when the molecular chains are highly oriented, such as in a stretched film exhibiting refractive index anisotropy nx>nz>ny.
[0040] To maintain high tensile strength even after hexane coating, it is preferable that the cyclic polyolefin resin constituting the phase difference film has low solubility in hexane. The solubility of a polymer in a solvent can be evaluated based on the distance Ra between the polymer's coordinate and the solvent's coordinate in the Hansen solubility parameter coordinate space.
[0041] The Hansen solubility parameter (HSP) is calculated by subtracting the dispersion term δ from the Hildebrand solubility parameter δ. d , polarity term δ p , and hydrogen bond term δ h It is divided into three components and represented in a three-dimensional coordinate space, δ 2 =δd 2 +δ p 2 +δ h 2 relationship holds. The dispersion term δ d represents the effect due to dispersion force, the polar term δ p represents the effect due to dipole-dipole force, and the hydrogen bonding term δ h represents the effect due to hydrogen bonding force. The distance Ra between the HSPs of two substances is derived from the difference Δδ in the dispersion terms between the two substances d , the difference Δδ in the polar terms p , and the difference Δδ in the hydrogen bonding terms h as Ra={4Δδ d 2 +Δδ p 2 +Δδ h 2} 1 / 2 , where a smaller Ra indicates higher compatibility, and a larger Ra indicates lower compatibility.
[0042] The solubility of a specific polymer in a solvent can be predicted from the HSP (δ d , δ p , δ h ) and interaction radius Ro of the polymer, as well as the HSP of the solvent. The interaction radius Ro is also referred to as the "radius of the dissolution sphere", and the ratio Ra / Ro of the HSP distance Ra to the interaction radius Ro is called the relative energy difference (RED). Assuming a sphere (dissolution sphere) with radius Ro centered on the HSP coordinates of the polymer, when the HSP coordinates of the solvent are inside the dissolution sphere of the polymer (that is, when Ra / Ro < 1), the polymer is soluble in the solvent; when the HSP coordinates of the solvent are outside the dissolution sphere of the polymer (that is, when Ra / Ro > 1), the polymer is predicted to be insoluble in the solvent. When the HSP coordinates of the solvent are on the surface of the dissolution sphere of the polymer (that is, when Ra / Ro = 1), the polymer is predicted to be partially soluble in the solvent.
[0043] Details of Hansen solubility parameters are described in Hansen Solubility Parameters: A User's Handbook (CRC Press, 2007) by Charles M. Hansen. HSP values of various organic solvents are known. The HSP and Ra of a polymer can be calculated by the Sphere program of the computer software Hansen Solubility Parameters in Practice (HSPiP) based on the results of solubility tests in solvents.
[0044] The HSP and Ro of the polymer are calculated by performing dissolution tests using toluene, hexane, methanol, trichlorobenzene, and γ-butyrolactone as solvents, as well as mixed solvents of toluene and hexane, mixed solvent of toluene and methanol, mixed solvent of toluene and trichlorobenzene, and mixed solvent of toluene and γ-butyrolactone, assigning "1" to dissolved samples and "0" to undissolved samples, and inputting the results into the above program. When the retardation film contains a plurality of polymers, a dissolution test may be performed on the retardation film to calculate the HSP and Ro using the above program.
[0045] It is preferable that the interaction radius Ro in the HSP space of the retardation film (cyclic polyolefin-based resin) and the distance Ra between the HSP coordinates of the retardation film and the HSP coordinates of hexane in the HSP space satisfy 1<Ra / Ro. If Ra / Ro is greater than 1, the decrease in tensile strength due to contact with hexane is small, and the occurrence of cracks in the solvent resistance test tends to be suppressed. The HSP of hexane is known, and is expressed as (δ d ,δ p ,δ h )=(14.9,0,0). Therefore, if the HSP of the retardation film (cyclic polyolefin-based resin) is determined, the distance Ra between coordinates in the HSP space is Ra={4Δδ d 2 +Δδ p 2 +Δδ h 2} 1 / 2It can be calculated.
[0046] The Ra / Ro ratio of the phase difference film is preferably 1.03 or higher, and may be 1.05 or higher or 1.07 or higher. The Ra / Ro ratio of the phase difference film is preferably less than 2, and may be 1.8 or lower, 1.6 or lower or 1.5 or lower.
[0047] As described above, the tensile strength in the direction perpendicular to the stretching direction after coating the phase difference film with hexane is preferably 10 N / 10 mm or more, and the tensile strength per unit area in the direction perpendicular to the stretching direction after coating with hexane is preferably 16 kPa or more. The tensile strength after coating with hexane may be 40 N / 10 mm or less, and the tensile strength per unit area after coating with hexane may be 40 kPa or less.
[0048] The tensile strength of the phase difference film (without hexane coating) in the direction perpendicular to the stretching direction is preferably 40 N / 10 mm or higher, and the tensile strength per unit area in the direction perpendicular to the stretching direction is preferably 60 kPa or higher. The higher the tensile strength (initial value), the more likely it is that crack formation in solvent resistance tests will be suppressed.
[0049] The phase difference film of the present invention may be laminated and integrated with a polarizer to form a polarizing plate. A polarizing plate can be obtained by laminating the phase difference film to one main surface of the polarizer via an appropriate adhesive layer or tack layer. Another film may be laminated between the polarizer and the phase difference film.
[0050] Examples of polarizers include hydrophilic polymer films such as polyvinyl alcohol-based films, partially formalized polyvinyl alcohol-based films, and partially saponified ethylene-vinyl acetate copolymer films, which are uniaxially stretched after adsorbing dichroic substances such as iodine or dichroic dyes; and polyene-based oriented films such as dehydrated polyvinyl alcohol or dehydrochlorinated polyvinyl chloride.
[0051] Among these, polyvinyl alcohol (PVA) polarizers are preferred because they have a high degree of polarization. These polarizers are made by adsorbing dichroic substances such as iodine or dichroic dyes onto a polyvinyl alcohol-based film, such as polyvinyl alcohol or partially formalized polyvinyl alcohol, and oriented in a predetermined direction. For example, a PVA polarizer can be obtained by iodine dyeing and stretching a polyvinyl alcohol-based film.
[0052] As a PVA-based polarizer, a thin polarizer with a thickness of 10 μm or less can also be used. Examples of thin polarizers include the thin polarizing films described in Japanese Patent Publication No. 51-069644, Japanese Patent Publication No. 2000-338329, WO2010 / 100917, Japanese Patent Specification No. 4691205, and Japanese Patent Specification No. 4751481. Such thin polarizers can be obtained, for example, by stretching a laminate of a PVA-based resin layer and a stretchable resin substrate and then staining it with iodine.
[0053] The arrangement angle of the polarizer and the phase difference film is not particularly limited. For example, when using a phase difference film for optical compensation to suppress light loss when viewing a liquid crystal display device from an oblique direction, it is preferable to arrange them so that the absorption axis direction of the polarizer and the slow phase axis direction of the phase difference film are parallel or perpendicular. When forming a circular polarizer by laminating the polarizer and the phase difference film, it is preferable to arrange them so that the angle between the absorption axis direction of the polarizer and the slow phase axis direction of the phase difference film is 45°. Note that the arrangement angle does not need to be strictly within the above range and may include an error of about ±2°.
[0054] A transparent film serving as a polarizer protective film may be laminated to the other side of the polarizer via an appropriate adhesive or tack layer. Optical films other than the phase difference film and polarizer protective film may be laminated onto the polarizing plate. An adhesive or tack layer may be laminated onto the polarizing plate for bonding with an image display cell or the like.
[0055] Phase difference films and polarizing plates can be used as optical films for image display devices. For example, an image display panel can be obtained by bonding a polarizing plate equipped with a phase difference film to the surface of an image display cell using an appropriate adhesive. If the image display cell is a liquid crystal cell, a liquid crystal display device can be formed by further combining it with a backlight as a light source.
[0056] After a polarizing plate is bonded to the surface of the image display cell, heating may be performed to adjust the moisture content of the polarizer, etc. Also, during lighting tests, the panel reaches a high temperature of about 80 to 100°C. In this invention, because the glass transition temperature of the phase difference film is high, even when the temperature rises due to heating or lighting tests, the stress accumulated inside or at the interface of the phase difference film is small. Furthermore, the resin material constituting the phase difference film has low solubility in hydrocarbon solvents such as hexane and maintains a certain strength even after contact with the solvent, so even if the edge of the phase difference film comes into contact with an organic solvent after heating, the occurrence of cracks on the edge of the phase difference film is suppressed. [Examples]
[0057] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0058] [Synthesis Example 1] In a nitrogen-purged reaction vessel, add 21 parts by weight of dicyclopentadiene as a monomer, and 8-methyl-8-carboxymethyltetracyclo[4.4.0.1 2,5 .1 7,1078 parts by weight of ]-3-dodecene, 1 part by weight of 2-norbornene, 14.7 parts by weight of 1-hexene as a molecular weight modifier, and 150 parts by weight of toluene as a solvent were added and heated to 107°C. To this solution, 0.4 parts by weight of ethylaluminum toluene solution (0.6 mol / l) and 1.8 parts by weight of methanol-modified tungsten hexachloride toluene solution (0.025 mol / l) were added and the mixture was reacted at 107°C for 1 hour to obtain a ring-opening polymer. To 360 parts by weight of the obtained ring-opening polymer solution, 0.04 parts by weight of Ru[4-CH3(CH2)4C6H4CO2]H(CO)[P(C6H5)3] was added as a hydrogenation reaction catalyst, the hydrogen gas pressure was set to 9-10 MPa, and the mixture was reacted at a temperature of 160-165°C for 3 hours. After the reaction was complete, the resulting product (hydrogenated material) was precipitated in methanol and vacuum-dried to obtain a cyclic polyolefin resin (weight-average molecular weight: 46,000, glass transition temperature: 148°C). Using a twin-screw extruder, the obtained resin was melt-kneaded, extruded into strands, and after water cooling, passed through a feeder-lubricator to obtain pellets.
[0059] [Comparative Example 1] An unstretched film with a thickness of 135 μm was prepared using cyclic polyolefin resin pellets (JSR's "ARTON R5000") by melt extrusion. This film was then uniaxially stretched at the free end (longitudinal stretching) at a temperature of 150°C and a magnification of 1.5 to obtain a stretched phase difference film.
[0060] [Example 1] Using the cyclic polyolefin resin pellets obtained in Synthesis Example 1 described above, an unstretched film with a thickness of 60 μm was prepared by melt extrusion. This film was longitudinally stretched under the conditions shown in Table 1 to obtain a stretched phase difference film.
[0061] [Comparative Example 2] An unstretched film with a thickness of 135 μm was prepared using cyclic polyolefin resin pellets (JSR's "ARTON R5000") by melt extrusion. A laminate was obtained by laminating a heat-shrinkable biaxially oriented propylene film (Toray's "Trefan") to both sides of this film using an adhesive. This laminate was longitudinally stretched at a temperature of 150°C and a magnification of 1.3 times, after which the heat-shrinkable films laminated to both sides were peeled off to obtain a stretched phase difference film (hereinafter, this stretching method will be referred to as "Z-stretching").
[0062] [Comparative Examples 3, 4, Example 2] Unstretched films were prepared by changing the type of cyclic polyolefin resin and the film thickness as shown in Table 1, and Z-stretching was performed under the conditions shown in Table 1. Otherwise, a stretched phase difference film was obtained in the same manner as in Comparative Example 2.
[0063] [Comparative Example 5] A commercially available cyclic polyolefin film (Zeonor Film ZF16, manufactured by Nippon Zeon Co., Ltd.) was subjected to Z-stretching under the conditions shown in Table 1 to obtain a stretched phase difference film.
[0064] [Reference example 3] A cyclic olefin polymer (COP) resin pellet (JSR's "ARTON R5000") was dissolved in methylene chloride, and an unstretched film with a thickness of 100 μm was prepared by solution deposition. Z-stretching was then performed under the conditions shown in Table 1 to obtain a stretched phase difference film.
[0065] [evaluation] <Hansen Solubility Parameter (HSP)> Under conditions of 25°C, approximately 10 g of resin pellets (or film pieces in the case of Zeonor film in Comparative Example 5) were dissolved in 50 mL of solvent, and the degree of dissolution was visually confirmed. The solvents used in the dissolution test were toluene, hexane, methanol, trichlorobenzene, γ-butyllactone, a mixed solvent of toluene and hexane, a mixed solvent of toluene and methanol, a mixed solvent of toluene and trichlorobenzene, and a mixed solvent of toluene and γ-butyllactone. The mixing ratio of the mixed solvents was changed in five or more steps within the range of 10:90 to 90:10, and the dissolution test was performed for each mixed solvent.
[0066] The values of dissolved material ("1") and undissolved material ("0") are entered into the Sphere program of the Hansen Solubility Parameters in Practice (HSPiP) computer software, and the Hansen solubility parameter (HSP) δ of the resin pellet (polymer) is calculated. d , δ p , and δ h Furthermore, the radius Ro of the molten sphere was calculated.
[0067] <Phase difference characteristics> A phase difference film was cut to a size of 50 mm x 50 mm, and frontal retardation at a measurement wavelength of 550 nm and retardation with the sample tilted 40° around the slow phase axis were measured using a polarization and phase difference measurement system (Axometrics "AxoScan"). From these measurements, the frontal retardation at a wavelength of 550 nm: Re = (nx - ny) × d and the NZ coefficient: NZ = (nx - nz) / (nx - ny) were calculated. nx is the refractive index in the slow phase axis direction in the plane, ny is the refractive index in the fast phase axis direction in the plane, nz is the refractive index in the thickness direction, and d is the thickness. For the calculation of the NZ coefficient, the average refractive index of the film measured with an Abbe refractometer manufactured by Atago was used.
[0068] <Tensile strength> The stretched phase difference film was cut into 10 mm x 100 mm strips with the longer side perpendicular to the stretching direction. Tensile tests were performed using a tensile testing machine (Shimadzu Corporation "Autograph AG-IS") in accordance with JIS K7161, at a tensile speed of 50 mm / min. The tensile strength was defined as the test force at the point where the sample fractured or plastic deformation began. After chucking the test piece in the tensile testing machine, one drop of hexane was dropped into the center of the test piece using a dropper and spread over the entire piece. A tensile test was then performed immediately to measure the tensile strength of the sample after hexane application.
[0069] <Glass transition temperature> A differential thermal analysis of the stretched phase difference film was performed using a differential scanning calorimetry analyzer (SII "DSC6200") under the following conditions, and the inflection point of the obtained DSC curve was defined as the glass transition temperature. Sample amount: 7-9 mg Reference: Aluminum pan Introduced gas: Nitrogen Temperature range: Room temperature to 230℃ Heating rate: 10°C / min
[0070] <Temperature change rate during heating> The stretched phase difference film was cut into strips measuring 16 mm x 4 mm with the stretching direction as the longer side, and thermomechanical analysis of the stretched phase difference film was performed using a thermomechanical analyzer (Hitachi High-Tech Science "TMA7100") under the following conditions. From the obtained TMA curve, the dimensional change rate (%) at 95°C (L0) was calculated based on the sample length L0 at room temperature and the sample length L at 95°C, resulting in 100 × (L - L0) / L0. Introduced gas: Nitrogen Load: 0.0196N Temperature range: Room temperature to 100℃ Heating rate: 10°C / min
[0071] <Solvent resistance test> Phase contrast film was cut to a size of 50 mm x 50 mm and attached to an adhesive glass plate. This sample was heated at 95°C for 3 hours, cooled at room temperature for 20 minutes, and then hexane was dropped onto all four edges of the film for visual inspection. Films with cracks at the edges were classified as NG (Not Good), and those without cracks were classified as OK (Good).
[0072] HSP(δ) of the polymers used in the examples, reference examples, and comparative examples d ,δ p ,δ h The values of ), Ro, Ra, and Ra / Ro are shown in Table 1. The conditions for producing the stretched phase difference films of the examples and comparative examples, and the evaluation results are shown in Table 2. The Ra / Ro values of the resins used to produce the films are also shown in Table 2.
[0073] [Table 1]
[0074] [Table 2]
[0075] The uniaxially oriented phase difference film of Example 1 showed no crack formation even after solvent resistance testing using hexane. The same was true for Example 2, which underwent Z-stretching.
[0076] The Z-oriented film of Comparative Example 5, which had low tensile strength after hexane coating, developed cracks after the solvent resistance test. In Comparative Example 5, the Ra / Ro ratio of the resin was less than 1, and it is thought that the film's strength decreased due to the application of hexane because of its high swelling properties in response to hexane.
[0077] In Comparative Examples 1-4, the tensile strength after hexane coating was equivalent to or greater than that of Example 1, but cracks occurred after the solvent resistance test. It is presumed that the lower glass transition temperature and larger dimensional change during heating in Comparative Examples 1-4 compared to Examples 1 and 2 were the causes of crack formation.
Claims
1. A phase difference film made of a stretched film of a cyclic polyolefin resin, The glass transition temperature is 145°C or higher. The tensile strength in the direction perpendicular to the stretching direction after hexane coating is 10-20 N / 10 mm. Phase difference film.
2. The phase difference film according to claim 1, wherein the tensile strength per unit area in a direction perpendicular to the stretching direction after coating with hexane is 16 to 31 kPa.
3. The phase difference film according to claim 1 or 2, wherein the tensile strength in the direction perpendicular to the stretching direction is 40 N / 10 mm or more.
4. A phase difference film according to any one of claims 1 to 3, wherein the tensile strength per unit area in a direction perpendicular to the stretching direction is 60 kPa or more.
5. A phase difference film according to any one of claims 1 to 4, wherein the frontal retardation is 200 nm or more.
6. A phase difference film according to any one of claims 1 to 5, having a thickness of 10 to 300 μm.
7. The in-plane birefringence Δn, which is the difference between the refractive index nx in the slow-speed axis direction and the refractive index ny in the fast-speed axis direction, is 1.0 × 10⁻⁶. -3 The phase difference film according to any one of claims 1 to 6.
8. A phase difference film according to any one of claims 1 to 7, wherein the refractive index nx in the slow phase axis direction in the plane, the refractive index ny in the fast phase axis direction in the plane, and the refractive index nz in the thickness direction satisfy nx > nz > ny.
9. A phase difference film according to any one of claims 1 to 8, wherein the dimensional change rate when heated at a temperature of 95°C is 0.40% or less.
10. The phase difference film according to any one of claims 1 to 9, wherein the interaction radius Ro of the phase difference film in the Hansen solubility parameter space and the distance Ra between the coordinate of the phase difference film in the Hansen solubility parameter space and the coordinate of hexane in the Hansen solubility parameter space satisfy 1 < Ra / Ro.
11. A polarizing plate in which a phase difference film according to any one of claims 1 to 10 is laminated on one surface of the polarizer.
12. An image display device comprising an image display cell and a polarizing plate according to claim 11.
Citation Information
Patent Citations
Retardation film, process for producing same, optical film, image display device, liquid crystal panel, and liquid crystal display device
JP2006072309A
Retardation film, polarizing plate using the same, and liquid crystal display device
JP2008309997A
Laminate and liquid crystal display device
JP2016218304A
Polarization plate set
JP2020086125A
Retardation film, polarizing plate and image display device
JP2023003920A